Low-temperature structural steel for TMCP-state low-cost high heat input welding, and manufacturing method

By not adding Nb to the steel for large thermal energy welding, using oxide metallurgy technology and micro-alloying elements, we designed TMCP low-temperature structural steel with low carbon and high manganese content, which solved the cost of steel for large thermal energy welding in the existing technology. It solves the problem of microstructure coarsening in the welding heat-affected zone and achieves high toughness and low-cost welding performance.

WO2024198101A1PCT designated stage expired Publication Date: 2024-10-03NANJING IRON & STEEL CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/100205
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2023-06-14
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

The cost of existing high-intensity welding steel is high, and the structure of the welding heat-affected zone is excessively coarsened under high heat input conditions, resulting in a decrease in the mechanical properties of the welded joints and failure to meet low-temperature toughness requirements.

Method used

TMCP state low-cost high-heat input welding low-temperature structural steel is used. By not adding Nb to the chemical composition of the steel, oxide metallurgical technology is used to form fine, dispersed and composite oxide particles, combined with V and Ni micro-alloys. Chemical elements are used to design steel with low carbon and high manganese content, and a two-stage rolling process of austenite recrystallization zone and non-recrystallization zone is used to control grain refinement and improve the toughness of the welding heat-affected zone.

Benefits of technology

It achieves high toughness in the heat-affected zone of welding under high heat input conditions, ensures welding strength, reduces production costs, and meets the performance requirements of large linear energy welding without the need for heat treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023100205_03102024_PF_FP_ABST
    Figure CN2023100205_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of steel production. Disclosed are a low-temperature structural steel for TMCP-state low-cost high heat input welding and a manufacturing method. By means of a low-carbon niobium-free component design and a smelting process based on oxide metallurgy technology, the present invention forms fine, dispersed and compound oxide particles in steel, uses the high-temperature thermally-stable fine and dispersed inclusion particles to pin austenite grain boundaries of a heat affected zone in welding under a high heat input condition, so as to refine austenite grains, and uses the oxides as nucleation points of intragranular acicular ferrite (IAF) to form in the heat affected zone in welding IAF tissues having good strength and ductility, thus further remarkably improving the ductility of the heat affected zone in high heat input welding. Producing high-strength shipbuilding steel plates by means of TMCP technology combined with high-temperature low-speed heavy reduction rolling does not require heat treatment, reduces costs, and involves stable production processes.
Need to check novelty before this filing date? Find Prior Art

Description

A TMCP state low-cost high-heat input welding low-temperature structural steel and its manufacturing method Technical Field

[0001] The present invention relates to the technical field of steel production, and in particular to a TMCP state low-cost low-temperature structural steel for high-heat input welding and a manufacturing method thereof. Background Art

[0002] High-heat-input welding steel has a wide range of applications. For example, in strategic oil reserves, shipbuilding, and cryogenic structures, high heat input welding efficiency increases by 2-4 times. Domestic production is unavailable, requiring importation, which is expensive. High-heat-input welding is the most practical way to improve welding efficiency and reduce costs. The "Guidelines for the Scientific and Technological Development of the Chinese Iron and Steel Industry (2006-2020)" states that high-heat-input welding steel is a key development target for my country's steel industry, with broad market prospects.

[0003] When the welding heat input is greater than 50kJ / cm, it is called high-energy input welding. When the welding heat input of traditional steel plates is greater than 50kJ / cm, the mechanical properties of the welded joint will seriously decline due to the excessive coarsening of the structure of the welding heat-affected zone, and may even fall below the standard requirements of the parent steel plate. Research and development of steel that meets high-energy input welding requirements is an effective way to solve the deterioration of low-temperature toughness in the heat-affected zone of high-energy input welding.

[0004] Existing patents for steel plates for high heat input welding, such as CN1946862A, CN1338528A, CN101050502A, and CN101050504A, all contain the alloying element Nb, the main purpose of which is to improve the strength and toughness of the base steel plate, but the cost is high.

[0005] Summary of the Invention

[0006] The present invention addresses the above-mentioned technical problems and overcomes the shortcomings of the prior art. It provides a TMCP state low-cost low-temperature structural steel for high-heat input welding, wherein no Nb is added to the chemical composition of the steel. The chemical composition by weight is as follows: C: 0.05% to 0.12%, Si: 0.15% to 0.30%, Mn: 1.20% to 1.60%, P≤0.015%, S≤0.0030%, V: 0.030% to 0.040%, Alt: 0.005% to 0.050%, Ti: 0.005% to 0.030%, Ca: 0.0005% to 0.0040%, Ni: 0.05% to 0.40%, Mg: 0.0005% to 0.0040%, Ceq: 0.32% to 0.41%, and the remainder is Fe and unavoidable impurities.

[0007] The technical solution further defined in the present invention is:

[0008] The aforementioned TMCP state low-cost low-temperature structural steel for high-heat input welding has the following chemical composition by weight: C: 0.06% to 0.10%, Si: 0.16% to 0.27%, Mn: 1.23% to 1.45%, P≤0.015%, S≤0.0030%, V: 0.033% to 0.037%, Alt: 0.010% to 0.044%, Ti: 0.029% to 0.030%, Ca: 0.0015% to 0.0032%, Ni: 0.24% to 0.27%, Mg: 0.0011% to 0.0014%, Ceq: 0.35% to 0.40%, and the rest is Fe and unavoidable impurities.

[0009] The aforementioned TMCP state low-cost low-temperature structural steel for high-heat input welding has the following chemical composition by weight: C: 0.07% to 0.08%, Si: 0.25% to 0.28%, Mn: 1.47% to 1.56%, P≤0.015%, S≤0.0030%, V: 0.036% to 0.038%, Alt: 0.044% to 0.050%, Ti: 0.017% to 0.020%, Ca: 0.0026% to 0.0033%, Ni: 0.22% to 0.25%, Mg: 0.0032% to 0.0036%, Ceq: 0.36% to 0.40%, and the rest is Fe and unavoidable impurities.

[0010] Another object of the present invention is to provide a method for manufacturing low-cost, high-heat-input welding low-temperature structural steel in a TMCP state, comprising the following steps: hot metal desulfurization pretreatment → converter smelting → LF refining → RH refining → continuous casting → ingot inspection and determination → ingot acceptance → continuous casting ingot heating → descaling → rolling → cooling → flaw detection → cutting and sampling → label printing → storage.

[0011] After desulfurization pretreatment of molten iron, S is controlled to ≤ 0.005%, and P is controlled to ≤ 0.013% in converter smelting. LF refining is carried out to control inclusions and adjust alloy composition. After the Si iron in the LF furnace is adjusted to an appropriate oxygen content, it is added strictly in the order of Ti iron - Al wire - Ca wire - Mg alloy wire, with an interval of no more than 5 minutes. RH refining vacuum treatment is maintained at a high vacuum degree of ≤ 5.0 mbar for ≥ 30 minutes. The continuous casting tundish temperature is controlled at the liquidus line of 8-22°C, and the continuous casting billet stack is slowly cooled for more than 48 hours.

[0012] The continuous casting slab is heated at a temperature of 1150-1250°C, heated for 300-400 minutes, and discharged from the furnace at a temperature of 1130-1230°C. The rolling adopts two-stage rolling in the austenite recrystallization zone and the non-recrystallization zone. The rough rolling adopts a large reduction per pass to crush the austenite grains, the reduction per pass is ≥30mm, the rough rolling start temperature is ≥1050°C, and the intermediate slab is rough rolled into a thickness ≥2.0 times that of the finished product. The rough rolling finish temperature is controlled at 900-1050°C, the finishing rolling start temperature is 780-880°C, and the reduction rate per pass is 10%-15%. After rolling, the cooling is controlled, laminar cooling is adopted, the red-return temperature is 600-700°C, and then air cooling is performed.

[0013] The aforementioned method for manufacturing low-temperature structural steel for high-heat input welding in a TMCP state at low cost produces S355ML grade steel with a thickness of 10 to 80 mm.

[0014] The aforementioned method for manufacturing low-cost low-temperature structural steel for high-line energy welding in a TMCP state has a steel plate yield strength ≥355MPa, a tensile strength ≥470~630MPa, and is suitable for welding line energy of 50-250kJ / cm. Under high-line energy welding conditions, the average impact energy of the HAZ of the steel plate at -50°C is above 150J, and the average impact energy of the HAZ of the steel plate at -50°C is above 27J, without the need for heat treatment.

[0015] The beneficial effects of the present invention are:

[0016] (1) The present invention forms fine, dispersed, and composite oxide particles in steel through a smelting process based on oxide metallurgy technology. These high-temperature thermally stable fine dispersed inclusion particles are used to pin the austenite grain boundaries in the heat-affected zone of the weld under high heat input conditions, thereby refining the austenite grains. At the same time, these oxides are used as nucleation points for intragranular acicular ferrite IAF, thereby forming a strong and tough IAF structure in the heat-affected zone of the weld, thereby improving the toughness of the heat-affected zone of high-input heat welding;

[0017] (2) The present invention uses V and Ni microalloying elements to improve the strength and toughness of steel. The product has a strength of more than 510 MPa while ensuring high-energy-line welding. The production cycle is short and the production pace is fast, which has great economic significance.

[0018] (3) The basic idea of ​​the composition design of the steel for high-heat input welding in the present invention is to not add niobium to ensure weldability, increase the content of manganese and microalloying elements to improve strength, control the content of impurity elements such as phosphorus and sulfur, effectively refine the grains and improve toughness, and improve the atmospheric corrosion resistance of the steel; adopt oxide metallurgy methods to form fine and dispersed microinclusions, inhibit the growth of austenite and control the transformation of the structure during welding, so that the toughness of the coarse-grained zone of the steel for high-heat input welding is maintained at a good level. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] FIG1 is a metallographic image of the HAZ coarse grain zone of the 80 mm thick TMCP state low-cost high input heat welding low-temperature structural steel S355ML in the embodiment. DETAILED DESCRIPTION

[0020] Chemical composition design principle:

[0021] Carbon is the most important element in steel and also one of the cheapest elements. Carbon is a strong interstitial solid solution element. Adding carbon to steel can have a significant interstitial solid solution strengthening effect on the steel, thereby improving the strength of low-alloy high-strength steel and making the greatest contribution to the strength of steel. Carbon combines with microalloying elements (Nb, Ti, V, etc.) in steel to form carbides, especially forming small, dispersed carbide inclusions in austenite, which play a role in grain refinement and precipitation strengthening, thereby improving the hardness and strength of steel. When the carbon content in steel increases, the yield and tensile strength increase, but the plasticity and impact toughness decrease, and its welding performance is also impaired. In order to adapt to large Heat input welding improves the toughness of steel and appropriately reduces the carbon content of low-alloy high-strength steel to improve the low-temperature impact toughness and welding performance of steel plates. The carbon content of low-alloy structural steel used for welding generally does not exceed 0.20%. Reducing the carbon content to below 0.10%, or even lower, can effectively improve the toughness of the heat-affected zone of high-heat input welding and reduce the sensitivity of steel to welding cracks. The use of low-carbon design in low-alloy high-strength steel will inevitably cause strength loss. In order to ensure that steel for high-heat input welding still has high strength under the premise of low carbon, it is necessary to adopt reasonable micro-alloying treatment and improve the strength by adding micro-alloying elements.

[0022] Manganese is a weak carbide-forming element. Except for a small amount dissolved in carburizer, it is almost entirely dissolved in ferrite and austenite, improving the hardness and strength of ferrite and austenite in steel. Manganese content is usually increased to compensate for some of the strength loss caused by reducing carbon content. Manganese can significantly reduce the transformation temperature, strongly lowering the starting transformation temperature of grain boundary ferrite, and promoting the formation of acicular ferrite. Manganese is also a good deoxidizer and desulfurizer. It is often added together with silicon and titanium for composite deoxidation to form composite inclusions with high sulfur capacity, effectively inducing the nucleation of intracrystalline acicular ferrite. Manganese and sulfur form MnS with a higher melting point, which can prevent the formation of FeS and the resulting hot brittleness. In addition, manganese can increase the tendency of steel grain coarsening, temper brittleness sensitivity, and overheating sensitivity.

[0023] Silicon can dissolve in ferrite and austenite, thereby increasing the hardness and strength of steel and compensating for some of the strength loss caused by reducing carbon content. Silicon has a good deoxidizing effect in molten steel and is a good deoxidizer. When using aluminum for deoxidation, adding a certain amount of silicon can significantly improve the deoxidizing ability of aluminum. However, excessive silicon content can promote the nucleation of grain boundary ferrite, inhibit the formation of acicular ferrite, increase the content of MA components, reduce the plasticity and toughness of steel, and reduce the weldability of steel. Therefore, the composition of steel for high-heat input welding should be low in silicon to promote the formation of fine bainite and ferrite structures.

[0024] As a strong oxidant, aluminum has high stability and can generate fine oxides dispersed in the steel. These oxides can serve as inclusion nucleation centers, inducing the attachment and precipitation of nitrides, carbides and sulfides. At the same time, aluminum is also a strong nitrogen fixer, forming nano-scale aluminum nitride precipitates, improving the thermal stability of steel and inhibiting the coarsening of austenite grains during the reheating process. However, the pinning effect of aluminum nitride on austenite grain boundaries is limited to within 1100℃. When austenite decomposes, the aluminum complex Inclusions can effectively induce the nucleation of acicular ferrite, refine grains and improve toughness. When an appropriate amount of aluminum is added to steel, the number of MA islands in the heat-affected zone (HAZ) decreases, their average length decreases, and the amount of retained austenite in MA increases, thereby improving the toughness of the HAZ. When the aluminum content is high, aluminum oxide inclusions cluster to form coarse particles, which are prone to forming crack sources. At the same time, an increase in aluminum concentration can form unfavorable organizational structures in the steel, such as promoting the formation of side lath ferrite organization in the steel, which reduces the toughness of the steel.

[0025] Niobium is a typical precipitation-strengthening element with a strong affinity for carbon and nitrogen. At room temperature, most of the niobium in steel exists in the form of carbides, nitrides, and carbonitrides. An appropriate amount of niobium can form fine, dispersed second-phase particles, which have excellent grain refinement and precipitation strengthening effects during rolling. These fine second-phase particles can also pin austenite grains during welding, inhibiting grain coarsening. Some niobium can be dissolved in the austenite matrix and segregated at austenite grain boundaries. Through the solute drag effect, it inhibits austenite grain boundary movement, limiting grain growth, refining grains, and improving strength and toughness. At the same time, niobium has a significant effect on the microstructure of the heat-affected zone and the morphological characteristics of the MA component. However, niobium can cause the second-phase particles to coarsen, losing their ability to inhibit grain coarsening. It also inhibits ferrite transformation and promotes the formation of granular bainite, resulting in a serious deterioration in toughness.

[0026] Vanadium has a strong affinity with elements such as carbon and nitrogen. It exists in steel mainly in the form of carbides and nitrides. It can improve the strength through precipitation strengthening. VN precipitated in austenite can inhibit the growth of austenite grains. VN precipitated in the ferrite region can increase the nucleation core of ferrite within the grain. These two aspects jointly promote grain refinement and significantly improve the welding performance of low-carbon low-alloy steel. However, during high-energy-input welding, vanadium carbonitrides cannot be fully precipitated.

[0027] Titanium has a strong affinity with oxygen, nitrogen, and carbon. It is a good deoxidizer and an effective element for fixing nitrogen and carbon. Titanium oxide is considered to be the most effective nucleation inclusion in steel and can effectively promote the nucleation of acicular ferrite.

[0028] Magnesium deoxidation and magnesium-titanium synergistic inclusion control technologies solve the problem that TiN coarsening in medium carbon microalloyed steel at conventional cooling rates can significantly increase the titanium nitride content in the steel.

[0029] Nickel is a very important element for improving the low-temperature toughness of steel. It is a pure solid-solution element in steel, which can strengthen the ferrite matrix and significantly reduce the ductile-brittle transition temperature. In liquid or solid state, it is miscible with iron in any proportion, which can inhibit the formation of coarse proeutectoid ferrite, refine ferrite grains, and improve the low-temperature toughness of steel. Nickel is an element that expands the austenite phase region, which can affect the diffusion rate of carbon and alloying elements, prevent the formation of pearlite, improve hardenability, and slow down the tendency of hardening cracking during welding.

[0030] Sulfur is a harmful element in steel. It exists in the form of FeS with a low melting point, which can easily cause hot brittleness in steel and thus cracks. Sulfur in steel easily combines with Mn to form layered segregation with MnS inclusions, which significantly reduces the strength and plasticity in the thickness direction of the plate, causing layered tearing and endangering the performance of the steel. At the same time, under certain conditions, MnS in steel, together with VN and TiN, pins the growth of austenite grains and induces the nucleation of intragranular ferrite, effectively refining the grains and improving toughness.

[0031] Phosphorus is an impurity element. Its biggest harm is severe segregation, which significantly reduces the plasticity and toughness of steel and also has an adverse effect on weldability. When it acts together with copper in steel, it can improve the steel's resistance to atmospheric corrosion.

[0032] Examples 1-3 provide an 80 mm thick TMCP state low-cost high-heat input welding low-temperature structural steel, the manufacturing method of which adopts a low-carbon niobium-free and oxide-free metallurgical process, adds trace elements Ni and V, and adopts controlled rolling and controlled cooling technology.

[0033] Table 1 Main chemical components of the examples (wt%)

[0034] Table 2 Rolling cooling process parameters

[0035] The process includes the following steps: hot metal desulfurization pretreatment → converter smelting → LF refining → RH refining → continuous casting → ingot inspection and judgment → ingot acceptance → continuous casting ingot heating → descaling → rolling → cooling → flaw detection → cutting and sampling → printing identification → storage. The main process points are as follows:

[0036] After molten iron desulfurization pretreatment, the S content is controlled at ≤0.005%, the P content is controlled at ≤0.013% in converter smelting, and inclusions are controlled and alloy composition is adjusted in LF refining. After the Si iron in the LF furnace is adjusted to an appropriate oxygen content, it is added strictly in the order of Ti iron-Al line-Ca-Mg alloy line, with the interval time not exceeding 5 minutes; RH refining vacuum treatment is maintained at high vacuum degree ≤5.0mbar for ≥30 minutes, the continuous casting tundish temperature is controlled at the liquidus line of 8-22℃, and the continuous casting billet stack is slowly cooled for more than 48 hours;

[0037] The continuous casting slab is heated to a temperature of 1150-1250°C for 300-400 minutes and discharged from the furnace at a temperature of 1130-1230°C. The rolling process adopts two-stage rolling in the austenite recrystallization zone and the non-recrystallization zone. The rough rolling adopts a large reduction per pass to crush the austenite grains. The pass reduction is ≥30 mm. The start temperature of the rough rolling is ≥1050°C. The intermediate slab is rough rolled to a thickness ≥2.0 times that of the finished product. The finishing temperature of the rough rolling is controlled at 900-1050°C. The start temperature of the finish rolling is 780-880°C. The reduction rate of each pass is 10-15%. After rolling, controlled cooling is performed using laminar cooling with a red-return temperature of 600-700°C, followed by air cooling. A high-temperature offline slow cooling process is used: the steel plate is placed on a cooling bed for cooling after hot straightening. The offline temperature is 250-500°C and the stack cooling time is 48 hours to obtain 80 mm E40 grade high-strength shipbuilding plate for high heat input welding.

[0038] In this embodiment, the heating temperature is 1220°C, the holding time is 140 minutes, and the furnace temperature is 1200°C; the rough rolling reduction is 35 mm per pass, and the intermediate billet is roughly rolled to a thickness 2.2 times that of the finished product; the finishing rolling start temperature is 820-850°C, and the reduction rate per pass is greater than 10%; the final cooling temperature is 650-680°C; the off-line temperature is 440°C, and the steel plate is pile-cooled after it comes off the line for 48 hours.

[0039] Table 3 Physical properties of the embodiments

[0040] The steel plate has good comprehensive mechanical properties, with a yield strength ≥355MPa and a tensile strength ≥470MPa. It is suitable for TMCP state low-cost high-line energy welding of low-temperature structural steel S355ML with a welding line energy range of 50-250kJ / cm. Under the high-line energy welding conditions of 50 and 250kJ / cm, the average impact energy of the HAZ of the steel plate at -40°C is above 150J, no heat treatment is required, and the production cost is low.

[0041] In addition to the above embodiments, the present invention may also have other implementations. Any technical solution formed by equivalent replacement or equivalent transformation falls within the scope of protection required by the present invention.

Claims

1. A TMCP state low-cost high-energy-input low-temperature structural steel for welding, characterized in that: No Nb is needed to be added to the chemical composition of the steel, and the chemical composition by weight percentage is: C: 0.05% ~ 0.12%, Si: 0.15% ~ 0.30%, Mn: 1.20% ~ 1.60%, P≤0.015%, S≤0.0030%, V: 0.030% ~ 0.040%, Alt: 0.005% ~ 0.050%, Ti: 0.005% ~ 0.030%, Ca: 0.0005% ~ 0.0040%, Ni: 0.05% ~ 0.40%, Mg: 0.0005% ~ 0.0040%, Ceq: 0.32% ~ 0.41%, and the rest is Fe and unavoidable impurities.

2. The TMCP state low-cost high-heat input welding low-temperature structural steel according to claim 1, characterized in that: Its chemical composition by weight percentage is: C: 0.06% ~ 0.10%, Si: 0.16% ~ 0.27%, Mn: 1.23% ~ 1.45%, P ≤ 0.015%, S ≤ 0.0030%, V: 0.033% ~ 0.037%, Alt: 0.010% ~ 0.044%, Ti: 0.029% ~ 0.030%, Ca: 0.0015% ~ 0.0032%, Ni: 0.24% ~ 0.27%, Mg: 0.0011% ~ 0.0014%, Ceq: 0.35% ~ 0.40%, and the rest is Fe and unavoidable impurities.

3. The TMCP state low-cost high-heat input welding low-temperature structural steel according to claim 1, characterized in that: Its chemical composition by weight percentage is: C: 0.07% ~ 0.08%, Si: 0.25% ~ 0.28%, Mn: 1.47% ~ 1.56%, P≤0.015%, S≤0.0030%, V: 0.036% ~ 0.038%, Alt: 0.044% ~ 0.050%, Ti: 0.017% ~ 0.020%, Ca: 0.0026% ~ 0.0033%, Ni: 0.22% ~ 0.25%, Mg: 0.0032% ~ 0.0036%, Ceq: 0.36% ~ 0.40%, and the rest is Fe and unavoidable impurities.

4. A method for manufacturing low-temperature structural steel for TMCP state low-cost high-heat input welding, characterized in that: Applicable to any one of claims 1-3, comprising the following steps: hot metal desulfurization pretreatment → converter smelting → LF refining → RH refining → continuous casting → ingot inspection and determination → ingot acceptance → continuous casting ingot heating → descaling → rolling → cooling → flaw detection → cutting and sampling → printing identification → storage, After the hot metal is desulfurized and pretreated, S is controlled to be ≤0.005%, and P is controlled to be ≤0.013% in converter smelting; LF refining is used to control inclusions and adjust alloy composition. After the Si iron in the LF furnace is adjusted to an appropriate oxygen content, it is added in strict accordance with the order of Ti iron-Al wire-Ca wire-Mg alloy wire, and the interval time does not exceed 5 minutes; RH refining vacuum treatment is maintained for ≥30 minutes under high vacuum degree ≤5.0mbar, and the temperature of the continuous casting ladle is controlled at the liquidus line of 8-22℃, and the continuous casting billet is stacked and slowly cooled for more than 48 hours; The continuous casting billet is heated at 1150-1250°C, the heating time is 300-400min, and the furnace temperature is 1130-1230°C; the rolling adopts two-stage rolling in the austenite recrystallization zone and the non-recrystallization zone, the rough rolling adopts a large pass reduction to crush the austenite grains, the pass reduction is ≥30mm, the rough rolling start temperature is ≥1050°C, the rough rolling is ≥2.0 times the finished product thickness of the intermediate billet, the rough rolling final rolling temperature is controlled at 900-1050°C, the finishing rolling start temperature is 780-880°C, and the reduction rate of each pass is 10%-15%; the cooling after rolling is controlled, laminar cooling is adopted, the red-returning temperature is 600-700°C, and then air cooling is performed.

5. The method for manufacturing low-temperature structural steel for high-heat input welding in TMCP state at low cost according to claim 4, characterized in that: Produce S355ML grade steel with thickness of 10 to 80 mm.

6. The method for manufacturing low-temperature structural steel for high-heat input welding in TMCP state at low cost according to claim 4, characterized in that: The yield strength of the steel plate is ≥355MPa, the tensile strength is ≥470~630MPa, and the suitable welding line energy is 50-250kJ / cm. Under the condition of large line energy welding, the average impact energy of the HAZ of the steel plate at -50℃ is above 150J, and the average impact energy of the HAZ of the steel plate at -50℃ is above 27J, and no heat treatment is required.

Citation Information

Patent Citations

  • Soldering boat deck steel in high intensity by large line energy, and manufacturing method

    CN101050502A

  • Soldering not quenching and tempering steel plate in high intensity by large line energy, and manufacturing method

    CN101050504A

  • Unmodified high-toughness low-temp steel for high-energy line welding and its production method

    CN1338528A

  • Thick high strength steel plate having excellent low temperature toughness in welding heat affected zone caused by high heat input welding

    CN1946862A

  • Steel plate smelting method for improving high heat input welding performance

    CN103215507A