Back contact battery with specific arrangement of isolation grooves, and preparation method therefor
By arranging an isolation groove and a conductive composite layer in the back contact battery, the problems of leakage micro-short circuit and large amount of silver paste are solved, the conversion efficiency and yield of the battery are improved, and the cost is reduced.
Patent Information
- Application Number
- PCT/CN2023/119645
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2023-09-19
- Publication Date
- 2024-10-03
AI Technical Summary
The existing back-contact battery structure cannot effectively avoid leakage and micro-short circuits. At the same time, a large amount of silver paste grid electrodes is used, resulting in high costs.
An isolation groove is provided at the Z-axis contact interface between the first semiconductor layer and the second semiconductor layer of the back contact battery, and a conductive composite layer is formed on the conductive film layer and the conductive mask layer. The isolation groove spans the polishing area and texturing area. area, the square resistance of the conductive composite layer is controlled within an appropriate range to improve the insulation resistance and carrier transmission efficiency.
It greatly improves the leakage and micro-short circuit phenomenon, improves battery conversion efficiency and yield, while reducing the amount of silver paste and reducing the cost of metal electrodes.
Smart Images

Figure CN2023119645_03102024_PF_FP_ABST
Abstract
Description
A back contact battery with a specifically configured isolation groove and a method for preparing the same
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This disclosure claims priority to Chinese patent application number 2023103322453 filed with the State Intellectual Property Office of China on March 31, 2023, entitled “A back contact battery with a specific isolation groove arrangement and its preparation method,” the entire contents of which are incorporated by reference into this disclosure. Technical Field
[0003] The present disclosure belongs to the technical field of back-contact batteries, and particularly relates to a back-contact battery with a specifically configured isolation groove and a preparation method thereof. Background Art
[0004] At present, the first semiconductor layer and the second semiconductor layer in the back-contact battery (or back-contact solar cell) are distributed on the back of the battery, and are generally arranged in an interdigitated shape to form two semiconductor regions. An insulating dielectric film is usually set between the first semiconductor layer and the second semiconductor layer stacked up and down to isolate and increase the parallel resistance, and a conductive film layer is set on the second semiconductor layer, and an isolation groove is opened on the conductive film layer between the first semiconductor region and the second semiconductor region. During the preparation, the isolation groove pattern is formed with printed protective ink, and then the printed protective ink is corroded by a chemical solution and cleaned; then, silver paste grid line electrodes (including silver paste fine grid line electrodes and silver paste main grid line electrodes, where the silver paste fine grid line accounts for about 70% of the total silver paste usage) are formed on the first semiconductor region and the second semiconductor region of the silicon substrate, as shown in the structures in CN114068731A and CN115207137A.
[0005] However, in a back-contact cell, a cell structure in which only a layer of intrinsic amorphous silicon (which serves as a passivation layer for the second semiconductor layer) with a thickness of about 10 nm is provided between the first doped silicon crystal layer in the first semiconductor layer and the second doped silicon crystal layer in the second semiconductor layer is insulated has a low parallel resistance and poor insulation effect. When a conductive film layer is deposited on the second semiconductor layer, the conductive film layer on the upper surface of the second doped silicon crystal layer collects carriers from the second semiconductor layer and transmits them to the interface between the first and second semiconductor layers (i.e., the contact interface in the Z-axis direction). The carriers collected by the first semiconductor form a leakage micro-short circuit at the interface between the first and second semiconductor layers. However, the better the conductivity of the two semiconductor layers, the more serious the leakage phenomenon, thereby affecting the cell conversion efficiency.
[0006] To address the aforementioned leakage short-circuit phenomenon, prior art typically employs an insulating dielectric film between the stacked first and second semiconductor layers to increase parallel resistance and effectively reduce leakage micro-short-circuit phenomena. However, to ensure battery conversion efficiency, a low-resistivity silver paste fine gridline electrode is typically positioned on the conductive film layer to increase carrier transport and ensure sufficient carrier transmission, in conjunction with a main gridline electrode. However, back-contact batteries of this structure utilize silver paste gridline electrodes (including both silver paste fine gridline electrodes and silver paste main gridline electrodes), which require a significant amount of silver paste and are therefore costly. The silver paste fine gridline accounts for approximately 70% of the total silver paste usage.
[0007] Summary of the Invention
[0008] The purpose of the present disclosure is to overcome the defects of the back-contact battery structure in the prior art that it cannot effectively avoid the leakage micro-short circuit phenomenon and improve the battery conversion efficiency, and the large amount of silver paste grid electrode is expensive. A back-contact battery with a specific isolation groove setting and a preparation method thereof are provided. The back-contact battery greatly improves the leakage micro-short circuit phenomenon, while improving the battery conversion efficiency and battery yield; and greatly reduces the amount of silver paste used, thereby greatly reducing the cost of metal electrodes.
[0009] In order to achieve the above-mentioned objectives, in a first aspect, the present disclosure provides a back-contact battery with a specifically arranged isolation groove, comprising a silicon substrate having a polishing area and a textured area spaced apart along the X-axis direction of the back side, a first semiconductor layer arranged on the polishing area, and a second semiconductor layer arranged on the textured area, the back-contact battery also comprising a conductive film layer and a conductive mask layer sequentially arranged outward along the Z-axis direction of the back side, the conductive composite layer formed by the conductive mask layer and the conductive film layer being provided with isolation grooves spaced apart along the X-axis direction, the isolation grooves being located above the contact interface between the first semiconductor layer and the second semiconductor layer in the Z-axis direction, and the isolation grooves spanning part of the polishing area and part of the textured area in the X-axis direction, the ratio of the span length Wa1 of the isolation groove on the polishing area to the span length Wa2 on the textured area is 1:0.1-4, preferably 1:0.1-1.
[0010] In some preferred embodiments of the present disclosure, a length Wa of the isolation trench in the X-axis direction is 50-300 μm.
[0011] In some preferred embodiments of the present disclosure, the sheet resistance of the conductive composite layer is no more than 50Ω / □.
[0012] Preferably, in the present disclosure, the thickness ratio of the conductive film layer to the conductive mask layer is 1:10-100.
[0013] In some preferred embodiments of the present disclosure, the conductive film layer includes at least one of tin-doped indium oxide, metallic copper, metallic aluminum, metallic silver, and nickel-copper alloy.
[0014] In some preferred embodiments of the present disclosure, the sheet resistance of the conductive film layer is no greater than 0.7Ω / □, more preferably less than 0.2Ω / □.
[0015] In some preferred embodiments of the present disclosure, the conductive film layer includes a composite film layer formed by a tin-doped indium oxide layer, a metal copper layer, and a nickel-copper alloy layer sequentially arranged outward along the Z-axis direction.
[0016] More preferably, the thickness of the tin-doped indium oxide layer is 50-100 nm, the thickness of the metal copper layer is 200-400 nm, and the thickness of the nickel-copper alloy layer is 50-100 nm.
[0017] In other preferred embodiments of the present disclosure, the conductive film layer comprises a composite film layer comprising a tin-doped indium oxide layer and a metal aluminum layer sequentially disposed outwardly along the Z-axis. More preferably, the tin-doped indium oxide layer has a thickness of 50-100 nm, and the metal aluminum layer has a thickness of 300-600 nm.
[0018] In some preferred embodiments of the present disclosure, the conductive mask layer includes a layer formed of at least one material selected from the group consisting of carbon paste, copper paste, nickel paste, and conductive ink.
[0019] In some preferred embodiments of the present disclosure, the sheet resistance of the conductive mask layer is no more than 50Ω / □.
[0020] In some preferred embodiments of the present disclosure, in the Z-axis direction of the polishing area, a second semiconductor layer is further provided above both side edges of the first semiconductor layer in the X-axis direction, and the first semiconductor layer and the second semiconductor layer distributed up and down are in direct contact.
[0021] In some preferred embodiments of the present disclosure, the first semiconductor layer includes a tunneling oxide layer and a first doped silicon crystal layer, and the second semiconductor layer includes an intrinsic amorphous silicon layer and a second doped silicon crystal layer, wherein one of the first doped silicon crystal layer and the second doped silicon crystal layer is N-type and the other is P-type, and the first doped silicon crystal layer is a doped polycrystalline silicon layer, and the second doped silicon crystal layer is a doped amorphous silicon or microcrystalline silicon layer.
[0022] More preferably, the texturing area forms a second opening area to lay part of the second semiconductor layer. In the Z-axis direction of the polishing area, a second semiconductor layer with a first opening area in the middle is also provided above the first semiconductor layer, and the first opening area is filled with the conductive film layer.
[0023] Further preferably, in the X-axis direction, the span length of the isolation groove in the polishing area and the span length in the texturing area are respectively recorded as Wa1 and Wa2, satisfying: Wa1 / Wg is 5%-100%, Wa2 / W2 is 1%-25%, wherein Wg is the interval between the first opening area and the second opening area, and W2 is the length of the second opening area.
[0024] Further preferably, in the X-axis direction, the length W1 of the first opening area is 100-300 μm, the length W2 of the second opening area is 300-700 μm, and the interval Wg between the first opening area and the second opening area is 50-400 μm.
[0025] More preferably, the tunneling oxide layer is silicon dioxide with a thickness of 0.5-3 nm; the first doped silicon crystal layer is a phosphorus-doped or boron-doped polycrystalline silicon layer with a thickness of 50-300 nm and a resistivity of 1E-4 Ω.cm—1E-2 Ω.cm; the intrinsic amorphous silicon layer has a thickness of 5-15 nm; the second doped silicon crystal layer is a phosphorus-doped or boron-doped amorphous silicon layer or a phosphorus-doped or boron-doped microcrystalline silicon layer with a thickness of 5-30 nm and a resistivity of 1E-1 Ω.cm—1E9 Ω.cm.
[0026] In some preferred embodiments of the present disclosure, the back contact battery further comprises:
[0027] an insulating layer disposed on the surface of the conductive mask layer along the Z-axis direction, with a first portion disposed in the isolation trench and a second portion spaced apart from the outer surface of the conductive mask layer and a side surface of the second portion in contact with the first portion; the second portion of the insulating layer having a thickness of 5-50 μm;
[0028] The main grid lines are extended along the X-axis direction and electrically connect the conductive mask layers located in the Z-axis direction of the first semiconductor layer and the second semiconductor layer in series, and are spaced apart along the Y-axis direction.
[0029] In some preferred embodiments of the present disclosure, the back contact cell further comprises: a front passivation layer and an anti-reflection layer, which are sequentially arranged on the front side of the silicon substrate outward along the Z-axis direction, and the front side of the silicon substrate is a texturing area.
[0030] In a second aspect, the present disclosure provides a method for preparing the back-contact battery according to the first aspect, comprising the following steps:
[0031] S100, providing a solar panel with a first semiconductor layer and a second semiconductor layer on the back side of a silicon substrate, wherein the back side portion where the first semiconductor layer is located is a polishing area, and the back side portion where the second semiconductor layer is located is a texturing area;
[0032] S101, forming a conductive film layer on the back side of the solar panel obtained in S100 to fully cover the back side;
[0033] S102, forming a conductive mask layer on the back side of the solar cell panel obtained in S101, with isolation openings spaced apart along the X-axis direction on the conductive mask layer, the isolation openings being located above the contact interface between the first semiconductor layer and the second semiconductor layer in the Z-axis direction and spanning the polishing area and the texturing area in the X-axis direction;
[0034] S103, etching is performed on the back side of the solar panel obtained in S102 to remove a portion of the conductive film layer below the isolation opening, thereby forming an isolation groove on the conductive composite layer formed by the conductive mask layer and the conductive film layer.
[0035] In some preferred embodiments of the present disclosure, the conductive film layer in S101 is formed by deposition.
[0036] In some preferred embodiments of the present disclosure, the conductive mask layer in S102 is formed by printing or inkjet.
[0037] In some preferred embodiments of the present disclosure, the etching in S103 uses a chemical corrosion solution, and more preferably the chemical corrosion solution is at least one of a sulfuric acid solution, a hydrochloric acid solution, a hydrogen peroxide solution, and a ferric chloride solution.
[0038] In some preferred embodiments of the present disclosure, S100 further includes: providing a front passivation layer and an anti-reflection layer in the front texturing area of the solar panel.
[0039] In some preferred embodiments of the present disclosure, the preparation method further comprises:
[0040] S104, filling the isolation grooves on the back of the solar panel obtained in S103 with an insulating layer material, and simultaneously providing the insulating layer material arranged in intervals on the surface of the conductive mask layer on the back of the solar panel, thereby forming an insulating layer;
[0041] S105 , printing a plurality of busbars on the back of the solar cell panel obtained in S104 , wherein the busbars connect the conductive mask layer on the first semiconductor layer and the second semiconductor layer in series to form a busbar electrode. Beneficial effects:
[0042] The present disclosure specifically arranges the isolation groove above the contact interface of the first semiconductor layer and the second semiconductor layer in the Z-axis direction, and spans a portion of the polishing area and a portion of the texturing area with an appropriate length ratio, and arranges a conductive composite layer of a conductive film layer and a conductive mask layer above the second semiconductor layer. This can enhance the conductivity while significantly improving the leakage micro-short circuit phenomenon, thereby improving the battery conversion efficiency and improving the battery yield; moreover, the conductive composite layer can act as a fine gate electrode, so that silver paste fine grid lines are no longer needed, which greatly reduces the amount of silver paste used, thereby significantly reducing the cost of metal electrodes.
[0043] Specifically, the isolation trench of the present disclosure is configured as described above, which can appropriately increase the carrier transmission distance between the conductive film layer on the upper surface of the second semiconductor layer and the first semiconductor layer, significantly increase the insulation resistance between the first semiconductor layer and the second semiconductor layer, thereby significantly improving the leakage micro-short circuit phenomenon and improving the parallel resistance of the battery. The present disclosure also provides a conductive composite layer of a conductive film layer and a conductive mask layer above the second semiconductor layer (wherein the conductive mask layer can be formed by etching after masking with a cheap conductive paste, which can play the role of Z-axis conductivity and mask etching). The sheet resistance of the conductive composite layer is very low, which can meet the requirements of large-scale carrier transmission. It can serve as a fine gate electrode, which can significantly improve the leakage micro-short circuit phenomenon while enhancing conductivity, thereby improving the battery conversion efficiency. The conductive composite layer can act as a fine gate electrode, eliminating the need for silver paste fine gate, significantly reducing the amount of silver paste used, and thus significantly reducing the cost of metal electrodes. Under the same conditions, if the ratio of the above-mentioned span length is not appropriate, for example, if it is too large, the contact resistance will increase due to the reduction of the contact area between the conductive film layer on the second opening area and the second doped silicon crystal layer, thereby reducing the conversion efficiency of the back contact battery. If it is too small, the distance between the conductive film layer in the second opening area and the first semiconductor layer will be too small, resulting in a significant increase in the risk of micro-short circuit leakage, thereby affecting the battery yield.
[0044] In the preparation method disclosed herein, a conductive mask layer with an isolation opening is first formed and then etched to form an isolation groove, thereby obtaining a fine gate electrode. The widened isolation groove structure significantly improves leakage micro-short circuits and improves battery conversion efficiency. Furthermore, a cheap conductive mask material is used as the fine gate electrode, eliminating the need for silver paste for the fine gate electrode, significantly reducing the silver paste consumption of the metal electrode and thus significantly reducing the cost of the metal electrode. Furthermore, the conductive mask layer can also protect the underlying semiconductor layer during the etching process to form the isolation groove, and after etching the isolation groove, there is no need to remove the protective layer (i.e., the conductive mask layer), thereby simplifying the process. In the prior art, the isolation groove is usually prepared by using printed protective ink to form the isolation groove pattern, followed by chemical solution etching. The printed protective ink then needs to be cleaned, resulting in a relatively complex process.
[0045] Furthermore, the inventors of the present disclosure have discovered that in the combined passivation battery structure, the first doped silicon crystal layer is a doped polycrystalline silicon layer, which has a very low resistivity and is combined with a tunneling oxide layer that is prone to leakage current, and the second doped silicon crystal layer is a doped amorphous silicon or microcrystalline silicon layer, making the overall combined passivation structure more prone to leakage micro-short circuit problems; while in the conventional heterojunction battery structure, the first doped silicon crystal layer and the second doped silicon crystal layer are both amorphous silicon or microcrystalline silicon layers, which have very high resistivity and are both passivated by intrinsic amorphous silicon, and the overall heterojunction passivation structure is not prone to leakage micro-short circuit problems; therefore, compared with the conventional heterojunction battery structure, the combined passivation battery structure is more prone to micro-short circuit leakage. The specific isolation trench widening setting disclosed in the present disclosure is more conducive to reducing the leakage micro-short circuit problems that are more likely to exist in the combined passivation back contact battery structure, further improving the parallel resistance, and at the same time improving the battery conversion efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] In order to more clearly illustrate the technical solutions of the embodiments of the present disclosure, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present disclosure and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other relevant drawings can be obtained based on these drawings without creative work.
[0047] FIG1 is a schematic structural diagram of a back-contact solar panel provided by the present disclosure, in which a front passivation layer and an anti-reflection layer are formed on the front side, and a first semiconductor layer and a second semiconductor layer are formed on the back side;
[0048] FIG2 is a schematic diagram of the structure of depositing a conductive film layer on the back side of the battery in FIG1 according to the present disclosure;
[0049] FIG3 is a schematic structural diagram of a conductive mask layer formed on the back side of the battery in FIG2 according to the present disclosure;
[0050] FIG3 a is a schematic plan view of a conductive mask layer screen of the present invention;
[0051] FIG3 b is a top view of the back side of the battery after a conductive mask layer is formed on the back side of the battery according to FIG3 a ;
[0052] FIG4 is a schematic structural diagram of the present disclosure in FIG3 in which the conductive film layer between the conductive mask layers is etched away by a chemical etching solution;
[0053] FIG5 is a schematic diagram of a structure in which insulating ink is formed on the back of the battery of FIG4 according to the present disclosure;
[0054] FIG5 a is a schematic plan view of the insulating ink screen of the present invention;
[0055] FIG5 b is a top view of the back side of the battery after an insulating ink layer is formed on the back side of the battery according to FIG5 a ;
[0056] FIG6 is a plan view schematically showing a main grid electrode formed on the back side of the battery in FIG5 according to the present disclosure.
[0057] Description of Reference Numerals
[0058] 1. Silicon substrate, 2. Tunneling oxide layer, 3. N-type doped polysilicon layer, 4. Intrinsically doped amorphous silicon layer, 5. P-type doped amorphous silicon layer, 6. Front passivation layer, 7. Anti-reflection layer, 8. Conductive film layer, 9. Conductive mask layer, 10. Insulating layer, 11. Main gate electrode. DETAILED DESCRIPTION
[0059] In the present disclosure, unless otherwise specified, directional words such as “upper, lower, left, right” are generally understood in conjunction with the directions shown in the drawings and actual applications.
[0060] The following describes in detail embodiments of the present disclosure, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended only to explain the present disclosure and are not to be construed as limiting the present disclosure.
[0061] In the description of the present disclosure, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present disclosure and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation to the present disclosure.
[0062] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of the technical features being referred to. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. Throughout the present disclosure, "plurality" means two or more, unless otherwise specifically defined.
[0063] In the present disclosure, unless otherwise expressly specified or limited, when a first feature is "above" or "below" a second feature, it may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Furthermore, when a first feature is "above," "above," or "above" a second feature, it may mean that the first feature is directly above or diagonally above the second feature, or simply means that the first feature is at a higher level than the second feature. When a first feature is "below," "below," or "below" a second feature, it may mean that the first feature is directly below or diagonally below the second feature, or simply means that the first feature is at a lower level than the second feature.
[0064] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein. Among them, the terms "optional" and "optional" all mean that they may be included or not (or may be present or not).
[0065] In this disclosure, the description is based on the X-axis direction (i.e., horizontal direction), Y-axis direction (i.e., direction perpendicular to the X-axis in the horizontal plane), and Z-axis direction (i.e., vertical direction) of the back side, and the direction away from the silicon substrate is considered outward, and the direction close to the silicon substrate is considered inward.
[0066] In a first aspect, the present disclosure provides a back-contact battery with a specific isolation groove arrangement, comprising a silicon substrate with a polishing area and a textured area arranged at intervals along the X-axis direction of the back, a first semiconductor layer arranged on the polishing area, and a second semiconductor layer arranged on the textured area, the back-contact battery further comprising a conductive film layer and a conductive mask layer sequentially arranged outward along the Z-axis direction of the back, a conductive composite layer formed by the conductive mask layer and the conductive film layer having isolation grooves arranged at intervals along the X-axis direction, the isolation grooves being located between the first semiconductor layer and the conductive mask layer. Above the Z-axis contact interface between the body layer and the second semiconductor layer, the isolation groove spans part of the polishing area and part of the texturing area in the X-axis direction, and the ratio of the span length Wa1 of the isolation groove in the polishing area to the span length Wa2 in the texturing area is 1:0.1-4, for example, it can be 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:4, etc.
[0067] The present invention adopts the above-mentioned suitable ratio of the span length of the isolation groove on the polishing area to the span length on the textured area, which can significantly increase the distance between the conductive film layer on the surface of the second semiconductor layer and the first semi-conductive layer, while taking into account the suitable contact area between the conductive film layer on the second opening area where the second semiconductor layer is located and the second doped silicon crystal layer, which is conducive to significantly improving the leakage micro-short circuit phenomenon, improving the parallel resistance of the battery, and at the same time meeting the carrier transmission requirements, which is conducive to reducing the loss in the carrier transmission process and improving the conversion efficiency of the back contact battery. Under the same conditions, if the above-mentioned span length ratio is not suitable, if it is too large, the contact resistance will increase due to the reduction of the contact area between the conductive film layer on the second opening area and the second doped silicon crystal layer, thereby reducing the conversion efficiency of the back contact battery. If it is too small, the risk of micro-short circuit leakage will be significantly increased due to the small distance between the conductive film layer in the second opening area and the first semiconductor layer, thereby affecting the battery yield.
[0068] It is understood in the present disclosure that, in the X-axis direction, the isolation trench extends beyond the edge of the first semiconductor layer, spanning a portion of the polished area and a portion of the textured area, and is located between the first emitter formed by the first semiconductor layer and the second emitter formed by the second semiconductor layer. The isolation trench in the present disclosure extends along the Y-axis direction and extends inwardly along the Z-axis direction to the surface of the second semiconductor layer.
[0069] In some preferred embodiments of the present disclosure, the length Wa of the isolation trench in the X-axis direction is 50-300 μm. In this preferred embodiment, combined with the ratio of the span lengths, the span length Wa2 of the isolation trench in the texturing area is micron-level. The carrier transmission distance between the conductive film layer on the upper surface of the second semiconductor layer and the first semiconductor layer is increased from tens of nanometers in conventional isolation trenches to several microns or tens of microns in the present disclosure, further significantly increasing the insulation resistance between the first semiconductor layer and the second semiconductor layer, thereby significantly improving the leakage micro-short circuit phenomenon while ensuring improved battery conversion efficiency.
[0070] In the present disclosure, the ranges of Wa1 and Wa2 can be adjusted under the condition of satisfying the above-mentioned Wa1 / Wa2 ratio (or the ratio and Wa range). For example, it is preferred that Wa2 is 1-100μm, specifically 1μm, 9μm, 10μm, 20μm, 23μm, 30μm, 33μm, 40μm, 50μm, 60μm, 70μm, 80μm, 90μm, 80μm, 100μm. Wa1 is 1-200μm, specifically 1μm, 10μm, 20μm, 30μm, 40μm, 50μm, 60μm, 70μm, 80μm, 90μm, 100μm, 150μm, 200μm, preferably 20-200μm.
[0071] In some preferred embodiments of the present disclosure, the sheet resistance of the conductive composite layer is no greater than 50Ω / □. This preferred solution is more conducive to improving battery conversion efficiency while significantly reducing leakage and micro-short circuit phenomena.
[0072] In the preferred embodiment of the present disclosure, the thickness ratio of the conductive film layer to the conductive mask layer is 1:10 to 100. In this preferred embodiment, the conductive mask layer can play a role in assisting conduction, which is more conducive to mask etching.
[0073] The conductive film layer disclosed herein may be a transparent conductive film layer, more preferably a composite film layer composed of a transparent conductive film and a metal conductive film. The preferred composite film layer is more conducive to improving the battery conversion efficiency.
[0074] Further preferably, the transparent conductive film can be, for example, indium oxide doped with zinc, tin, tungsten, titanium, or silicon, or zinc oxide doped with aluminum, boron, or gallium. Further preferably, the metal conductive film layer can include at least one of aluminum, copper, silver, a nickel alloy (such as a nickel-copper alloy), or a titanium alloy. It is understood that the conductive film layer can be multiple layers or a single layer, and the material in the same layer can be a single material or a combination of multiple materials; those skilled in the art can select within the above range according to actual needs.
[0075] In some preferred embodiments of the present disclosure, the conductive film layer includes at least one of tin-doped indium oxide, metallic copper, metallic aluminum, metallic silver, and nickel-copper alloy.
[0076] In some preferred embodiments of the present disclosure, the sheet resistance of the conductive film layer is no greater than 0.7Ω / □, more preferably less than 0.2Ω / □. The preferred embodiment of the present disclosure can meet the requirements of carrier transport, further reducing losses during carrier transport and improving battery conversion efficiency.
[0077] In some more preferred embodiments of the present disclosure, the conductive film layer comprises a composite film layer formed by a tin-doped indium oxide layer, a metallic copper layer, and a nickel-copper alloy layer, sequentially arranged outward along the Z-axis. In this preferred embodiment, the metallic copper exhibits low resistivity, high infrared reflectivity, and low material cost, while the nickel-copper alloy resists oxidative corrosion. Consequently, a conductive film layer with low square resistance and high infrared reflectivity is obtained, further improving battery conversion efficiency.
[0078] More preferably, the thickness of the tin-doped indium oxide layer is 50-100 nm, the thickness of the metallic copper layer is 200-400 nm, and the thickness of the nickel-copper alloy layer is 50-100 nm. Under this preferred embodiment, the thickness of each layer is appropriate, which is more conducive to obtaining a conductive film layer with low square resistance and high infrared reflectivity, and is more conducive to improving battery conversion efficiency.
[0079] In other preferred embodiments of the present disclosure, the conductive film layer comprises a composite film layer comprising a tin-doped indium oxide layer and a metal aluminum layer sequentially disposed outwardly along the Z-axis. This preferred solution provides a low-sheet-resistance, low-cost conductive film layer, further reducing the cost of the conductive film layer.
[0080] More preferably, the thickness of the tin-doped indium oxide layer is 50-100 nm, and the thickness of the metal aluminum layer is 300-600 nm.
[0081] In the present disclosure, "conductive mask layer" refers to a mask layer having conductivity. In some preferred embodiments of the present disclosure, the conductive mask layer comprises a layer formed of at least one material selected from carbon paste, copper paste, nickel paste, and conductive ink, more preferably a layer formed of carbon paste.
[0082] In some preferred embodiments of the present disclosure, the sheet resistance of the conductive mask layer is no greater than 50Ω / □. This preferred solution can better assist in conducting electricity and is more conducive to improving battery conversion efficiency.
[0083] In some preferred embodiments of the present disclosure, a second semiconductor layer is disposed above both edges of the first semiconductor layer in the X-axis direction in the polishing region in the Z-axis direction, with the first and second semiconductor layers, disposed one above the other, in direct contact. This significantly reduces leakage micro-short circuits without requiring an additional insulating dielectric film between the first and second semiconductor layers, while maintaining high battery conversion efficiency and yield.
[0084] It can be understood that on the back side of the silicon substrate, along the X-axis direction, the first semiconductor layer and the second semiconductor layer are alternately arranged, and there is a gap between the first opening area and the second opening area, and the first semiconductor layer and the second semiconductor layer are stacked up and down in the gap.
[0085] The first semiconductor layer and the second semiconductor layer disclosed in the present invention can be a conventional heterojunction passivation structure, that is, both are passivated using an intrinsic amorphous silicon layer (such as a doped intrinsic amorphous silicon layer); or they can be a combined passivation structure, that is, the first semiconductor layer includes a tunneling oxide layer and a first doped silicon crystal layer, and the second semiconductor layer includes an intrinsic amorphous silicon layer and a second doped silicon crystal layer.
[0086] In some preferred embodiments of the present disclosure, the first semiconductor layer comprises a tunneling oxide layer and a first doped silicon crystal layer, and the second semiconductor layer comprises an intrinsic amorphous silicon layer and a second doped silicon crystal layer, wherein one of the first doped silicon crystal layer and the second doped silicon crystal layer is N-type and the other is P-type, and the first doped silicon crystal layer is a doped polycrystalline silicon layer, and the second doped silicon crystal layer is a doped amorphous silicon or microcrystalline silicon layer. In this preferred embodiment, the back-contact cell of the present disclosure has a combined passivation structure. The specific isolation trench widening configuration of the present disclosure is more conducive to reducing the micro-short circuit problem that exists in cells with a combined passivation structure, further improving the parallel resistance.
[0087] In some preferred embodiments, the ratio of the isolation groove's span length Wa1 in the polished area to its span length Wa2 in the texturing area is 1:0.1-1, more preferably 1:0.5-1. This preferred solution is more conducive to reducing leakage and micro-short circuit issues in combined passivation structure batteries, further improving parallel resistance, and further enhancing battery conversion efficiency.
[0088] More preferably, the texturing area forms a second opening for laying a portion of the second semiconductor layer. In the Z-axis direction of the polishing area, a second semiconductor layer having a first opening in the middle is further disposed above the first semiconductor layer, and the first opening is filled with the conductive film. It is understood that the first opening is used to expose the underlying first semiconductor layer to facilitate formation of the first emitter.
[0089] Further preferably, in the X-axis direction, the cross-sectional lengths of the isolation groove in the polishing area and in the texturing area are denoted as Wa1 and Wa2, respectively, satisfying the following conditions: Wa1 / Wg is 5%-100%, and Wa2 / W2 is 1%-25%, where Wg is the spacing between the first opening area and the second opening area, and W2 is the length of the second opening area. Under this preferred solution, the spacing between the conductive film layer on the surface of the second semiconductor layer and the first semiconductor layer can be increased, while also ensuring an appropriate contact area between the conductive film layer in the second opening area and the second doped silicon crystal layer, further improving the parallel resistance and conversion efficiency of the battery with the combined passivation structure.
[0090] Wa1 / Wg is 5%-100%, for example, it can be 5%, 10%, 20%, 25%, 30%, 40%, 50%, 60%, 67%, 70%, 77%, 80%, 90%, 91%, 100%, etc.
[0091] Wa2 / W2 is 1%-25%, for example, 1%, 2%, 5%, 6%, 8%, 10%, 13%, 15%, 19%, 20%, 23%, 25%, etc.
[0092] In some preferred embodiments, Wa2 / W2 is 8%-25%. This preferred solution is more conducive to reducing leakage and micro-short circuit problems, further improving parallel resistance and battery yield, and further improving battery conversion efficiency.
[0093] More preferably, the tunneling oxide layer is silicon dioxide with a thickness of 0.5-3 nm; the first doped silicon crystal layer is a phosphorus-doped or boron-doped polycrystalline silicon layer with a thickness of 50-300 nm and a resistivity of 1E-4 Ω.cm—1E-2 Ω.cm; the intrinsic amorphous silicon layer has a thickness of 5-15 nm; the second doped silicon crystal layer is a phosphorus-doped or boron-doped amorphous silicon layer or a phosphorus-doped or boron-doped microcrystalline silicon layer with a thickness of 5-30 nm and a resistivity of 1E-1 Ω.cm—1E9 Ω.cm.
[0094] In the combined passivation structure, the first semiconductor layer has good conductivity, while the second doped silicon crystal layer and its second semiconductor layer have poor conductivity. Therefore, in the present disclosure, the cross-sectional length of the isolation trench Wa2 is expected to be as small as possible while satisfying the insulation effect, and the width of Wa1 has little effect.
[0095] When the second doped silicon crystal layer is an N-type amorphous / microcrystalline silicon layer, the resistivity is approximately 1E-1-1E2Ω.cm; when the second doped silicon crystal layer is a P-type amorphous / microcrystalline silicon layer, the resistivity is approximately 1E4-1E9Ω.cm.
[0096] Further preferably, in the X-axis direction, the length W1 of the first opening area is 100-300 μm.
[0097] Further preferably, in the X-axis direction, the length W2 of the second opening area is 300-700 μm.
[0098] Further preferably, in the X-axis direction, the interval Wg between the first opening area and the second opening area is 50-400 μm.
[0099] In some preferred embodiments of the present disclosure, the back contact battery further comprises:
[0100] an insulating layer disposed on the surface of the conductive mask layer along the Z-axis direction, with a first portion disposed within the isolation trench and a second portion spaced apart from the outer surface of the conductive mask layer and with a side surface of the second portion in contact with the first portion; preferably, the second portion of the insulating layer has a thickness of 5-50 μm;
[0101] The main grid lines are extended along the X-axis direction and electrically connect the conductive mask layers located in the Z-axis direction of the first semiconductor layer and the second semiconductor layer in series, and are spaced apart along the Y-axis direction.
[0102] In some preferred embodiments of the present disclosure, the back contact cell further comprises: a front passivation layer and an anti-reflection layer, which are sequentially arranged on the front side of the silicon substrate outward along the Z-axis direction, and the front side of the silicon substrate is a texturing area.
[0103] Those skilled in the art can select the materials of the front passivation layer and the anti-reflection layer according to needs. For example, the front passivation layer is a silicon dielectric material, specifically, for example, it can be at least one of amorphous silicon, microcrystalline silicon, silicon oxide, and polycrystalline silicon; the anti-reflection layer is a silicon dielectric layer, specifically, for example, it can be at least one of silicon nitride, silicon oxide, and silicon oxynitride. The present disclosure has no restrictions on this.
[0104] In a second aspect, the present disclosure provides a method for preparing the back-contact battery according to the first aspect, comprising the following steps:
[0105] S100, providing a solar panel with a first semiconductor layer and a second semiconductor layer on the back side of a silicon substrate, wherein the back side portion where the first semiconductor layer is located is a polishing area, and the back side portion where the second semiconductor layer is located is a texturing area;
[0106] S101, forming a conductive film layer on the back side of the solar panel obtained in S100 to fully cover the back side;
[0107] S102, forming a conductive mask layer on the back side of the solar cell panel obtained in S101, with isolation openings spaced apart along the X-axis direction on the conductive mask layer, the isolation openings being located above the contact interface between the first semiconductor layer and the second semiconductor layer in the Z-axis direction and spanning the polishing area and the texturing area in the X-axis direction;
[0108] S103, etching is performed on the back side of the solar panel obtained in S102 to remove a portion of the conductive film layer below the isolation opening, thereby forming an isolation groove on the conductive composite layer formed by the conductive mask layer and the conductive film layer.
[0109] The disclosed preparation method first forms a conductive mask layer with an isolation opening, then etches it to form an isolation trench and simultaneously obtain a fine gate electrode. The conductive mask layer provides protection during the etching process, eliminating the need for subsequent removal of the protective layer (conductive mask layer). This significantly reduces leakage and micro-shorts and improves battery conversion efficiency while simplifying the manufacturing process. Conventional methods typically use printed protective ink to form the isolation trench pattern, followed by chemical etching, which then requires cleaning of the printed protective ink, resulting in a relatively complex process.
[0110] In the solar panel of S100 of the present disclosure, preferably, the first semiconductor layer and the second semiconductor layer, which are arranged vertically in the Z-axis direction of the polishing zone, are in direct contact. The present disclosure does not limit the manufacturing method of the solar panel, as long as the desired structure can be formed; for example, the post-texturing method described in CN115312633A, an earlier research study by the applicant of the present disclosure, can be adopted.
[0111] In some preferred embodiments of the present disclosure, the conductive film layer in S101 is formed by deposition.
[0112] In some preferred embodiments of the present disclosure, the conductive mask layer in S102 is formed by printing or inkjet.
[0113] In some preferred embodiments of the present disclosure, the etching in S103 uses a chemical etching solution. The chemical etching solution of the present disclosure preferably has good selectivity for etching the conductive film layer and the second semiconductor layer, and can quickly etch the conductive film layer without damaging the second semiconductor layer. More preferably, the chemical etching solution is at least one of a sulfuric acid solution (with a concentration of, for example, 1-10 wt%), a hydrochloric acid solution (with a concentration of, for example, 5-30 wt%), a hydrogen peroxide solution (with a concentration of, for example, 2-20 wt%), and a ferric chloride solution (with a concentration of, for example, 5-30 wt%).
[0114] In some preferred embodiments of the present disclosure, S100 further includes: providing a front passivation layer and an anti-reflection layer in the front texturing area of the solar panel.
[0115] In some preferred embodiments of the present disclosure, the preparation method further comprises:
[0116] S104, filling the isolation grooves on the back of the solar panel obtained in S103 with an insulating layer material, and simultaneously providing the insulating layer material arranged in intervals on the surface of the conductive mask layer on the back of the solar panel, thereby forming an insulating layer;
[0117] S105 , printing a plurality of busbars on the back of the solar cell panel obtained in S104 , wherein the busbars connect the conductive mask layer on the first semiconductor layer and the second semiconductor layer in series to form a busbar electrode.
[0118] In S104 , those skilled in the art may select a method for forming the insulating layer according to actual needs, for example, the insulating layer may be formed by printing or spraying.
[0119] In S105, while printing the busbars, those skilled in the art can choose whether to print busbar pads according to actual needs. The busbar printing material can be existing silver paste, solder paste, etc., which can be selected by those skilled in the art according to actual needs.
[0120] The present disclosure will be further elaborated below in conjunction with specific embodiments.
[0121] Example 1
[0122] A back contact battery with a specifically configured isolation groove, the preparation method and structure of which are as follows:
[0123] S100. As shown in FIG1 , a back-contact solar panel is provided, wherein a front passivation layer 6 (composed of an intrinsically doped amorphous silicon layer and an N-type microcrystalline silicon layer) and an anti-reflective layer 7 are formed on the front surface of a silicon substrate 1, and a first semiconductor layer and a second semiconductor layer are formed on the back surface. The first semiconductor layer and the second semiconductor layer are in direct contact in the upper and lower overlapping regions. The first semiconductor layer comprises a 1.5 nm thick tunneling oxide layer 2 and a 100 nm thick N-type doped polycrystalline silicon layer 3 (with a resistivity of 1E-3 Ω.cm). The second semiconductor layer comprises a 10 nm thick intrinsically doped amorphous silicon layer 4 and a 20 nm thick P-type doped amorphous silicon layer 5 (with a resistivity of 1E2 Ω.cm). The texturing area forms a second opening area to lay part of the second semiconductor layer; in the Z-axis direction of the polishing area, a second semiconductor layer with a first opening area in the middle is also provided above the first semiconductor layer, and the first opening area is filled with the conductive film layer. In the X-axis direction, the length W1 of the first opening area is 200μm, the length W2 of the second opening area is 400μm, and the interval Wg between the first opening area and the second opening area is 100μm.
[0124] S101. As shown in FIG2 , a conductive film layer 8 is deposited on the back side of the solar panel obtained in S100. The conductive film layer 8 is a composite film layer formed by sequentially disposing a tin-doped indium oxide layer, a metallic copper layer, and a nickel-copper alloy layer along the Z-axis. The tin-doped indium oxide layer (80 nm) + the metallic copper layer (300 nm) + the nickel-copper alloy layer (80 nm) have a sheet resistance of 0.08 Ω / □.
[0125] S102. As shown in FIG3 , a conductive mask layer 9 is formed on the back side of the solar panel obtained in S101. The conductive mask layer 9 has a thickness of 10 μm and a square resistance of 20 Ω / □. The conductive mask layer 9 forms an isolation opening with a gap width Wa at the edge of the first semiconductor layer. The length Wa is 100 μm, and the ratio of the span length Wa1 of Wa in the polishing area to the span length Wa2 of Wa in the texturing area in the X-axis direction is 1:0.5. The ratio Wa1 / Wg is 67%, and the ratio Wa2 / W2 is 8%. The conductive mask layer 9 is made of carbon paste and is formed by printing.
[0126] FIG3 a is a schematic diagram of the pattern of the conductive mask layer 9 screen in this embodiment, and FIG3 b is a schematic diagram of the conductive mask layer 9 formed on the back side of the battery in this embodiment.
[0127] S103, as shown in FIG4, after forming the conductive mask layer, the battery is subjected to a chemical etching solution to etch away the conductive film layer in the gap Wa between the conductive mask layers, thereby forming an isolation trench with a width of Wa. The etching solution is a mixture of 20 wt% hydrochloric acid and 10 wt% hydrogen peroxide.
[0128] S104, as shown in FIG5, insulating ink is printed in the isolation groove Wa on the back of the solar panel obtained in S103, and at the same time, an insulating ink layer with a thickness of 20 μm is formed on the conductive mask layer 9 at intervals to form an insulating layer 10. The insulating ink is formed by printing.
[0129] FIG5 a is a schematic diagram of the insulating ink layer screen in this embodiment, and FIG5 b is a schematic diagram of the insulating ink layer formed on the back of the battery in this embodiment.
[0130] S105 , as shown in FIG6 , printing silver paste busbars on the back of the solar panel obtained in S104 , connecting the conductive mask layers on the first semiconductor and the second semiconductor in series to form a busbar electrode 11 .
[0131] The silver paste consumption, parallel resistance, and battery conversion efficiency used in this embodiment are shown in Table 1 below.
[0132] Example 2
[0133] The method of Example 1 is referred to, except that the sheet resistance of the conductive film layer is 0.3Ω / □.
[0134] The silver paste consumption, parallel resistance, and battery conversion efficiency used in this embodiment are shown in Table 1 below.
[0135] Example 3
[0136] The method of Example 1 is referred to, except that in S105, solder paste is printed instead of silver paste as the main grid line.
[0137] The silver paste consumption, parallel resistance, and battery conversion efficiency used in this embodiment are shown in Table 1 below.
[0138] Example 4
[0139] The method of Example 1 is referred to, except that the conductive film layer is a composite film layer of a tin-doped indium oxide layer and a metal aluminum layer, the thickness ratio of the tin-doped indium oxide layer: the metal aluminum layer is 1:5, the total thickness of the composite film layer is the same as that of Example 1, and the square resistance of the composite film layer is 0.2Ω / □.
[0140] The silver paste consumption, parallel resistance, and battery conversion efficiency used in this embodiment are shown in Table 1 below.
[0141] Example 5
[0142] The method of Example 1 is referred to, except that Wa is adjusted to 300 μm, Wa1 / Wa2 remains unchanged, Wa2 / W2 is 25%, and Wg is adjusted so that Wa1 / Wg is 80%.
[0143] The silver paste consumption, parallel resistance, and battery conversion efficiency used in this embodiment are shown in Table 1 below.
[0144] Example 6
[0145] The method of Example 1 is referred to, except that the ratio of the span length of the isolation groove in the polishing area to the span length in the texturing area is different, and Wa2 is changed so that Wa1 / Wa2=1:0.3. At this time, Wa1 / Wg is 77% and Wa2 / W2 is 6%.
[0146] The silver paste consumption, parallel resistance, and battery conversion efficiency used in this embodiment are shown in Table 1 below.
[0147] Example 7
[0148] The method of Example 1 is referred to, except that the ratio of the span length of the isolation groove in the polishing area to the span length in the texturing area is different, and Wa2 is changed so that Wa1 / Wa2=1:0.1. At this time, Wa1 / Wg is 91% and Wa2 / W2 is 2%.
[0149] The silver paste consumption, parallel resistance, and battery conversion efficiency used in this embodiment are shown in Table 1 below.
[0150] Example 8
[0151] The method of Example 1 was followed, except that Wa1 was changed so that Wa1 / Wg was 10%, and Wa2 was adjusted so that Wa1 / Wa2 was 1:4 and Wa2 / W2 was 10%.
[0152] The silver paste consumption, parallel resistance, and battery conversion efficiency used in this embodiment are shown in Table 1 below.
[0153] Example 9
[0154] The method of Example 1 is referred to, except that Wa2 is changed so that Wa2 / W2 is 20%, Wa remains unchanged, and at this time Wa1 / Wa2 is 1:4, and Wa1 / Wg is 20%.
[0155] The silver paste consumption, parallel resistance, and battery conversion efficiency used in this embodiment are shown in Table 1 below.
[0156] Example 10
[0157] The method of Example 1 is referred to, except that the ratio of the span length of the isolation groove in the polishing area to the span length in the texturing area is different, and Wa2 is changed so that Wa1 / Wa2=1:3, and Wa remains unchanged. At this time, Wa1 / Wg is 25%, and Wa2 / W2 is 19%.
[0158] The silver paste consumption, parallel resistance, and battery conversion efficiency used in this embodiment are shown in Table 1 below.
[0159] Example 11
[0160] The method of Example 1 is referred to, except that the passivation structure is different and conventional heterojunction passivation is adopted. Specifically, the tunneling oxide layer with a thickness of 2 nm in the first semiconductor layer is replaced by an intrinsically doped amorphous silicon layer with a thickness of 10 nm for passivation.
[0161] The silver paste consumption, parallel resistance, and battery conversion efficiency used in this embodiment are shown in Table 1 below.
[0162] Comparative Example 1
[0163] The method of Example 1 is referred to, except that a conductive composite layer of a conductive film layer and a conductive mask layer is not provided, but a transparent conductive film layer is deposited to fully cover the second semiconductor. Then, protective ink is printed on the upper and lower distribution areas of the first semiconductor layer and the second semiconductor layer, and etching and cleaning are performed to form isolation grooves (whose size is the same as in Example 1). After that, the protective ink is cleaned, and then silver paste is printed to form conventional fine grid lines. The other steps (forming the insulating layer and the main grid lines) are exactly the same.
[0164] The silver paste consumption, parallel resistance, and battery conversion efficiency used in this comparative example are shown in Table 1 below.
[0165] Comparative Example 2
[0166] The method of Example 1 is referred to, except that the isolation groove is not arranged above the contact interface between the first semiconductor layer and the second semiconductor layer in the Z-axis direction, but is arranged in the interval Wg area between the first opening area and the second opening area, that is, the isolation groove does not cross to the textured area in the X-axis direction.
[0167] The silver paste consumption, parallel resistance, and battery conversion efficiency used in this comparative example are shown in Table 1 below.
[0168] Comparative Example 3
[0169] The method of Example 1 is referred to, except that the ratio of the span length of the isolation groove on the polishing area to the span length on the texturing area is different, and Wa2 is changed so that Wa1 / Wa2=1:0.02.
[0170] The silver paste consumption, parallel resistance, and battery conversion efficiency used in this comparative example are shown in Table 1 below.
[0171] Table 1
[0172] Note: The size of each piece in mg / piece is M10 silicon wafer.
[0173] The above examples and comparative examples demonstrate that the use of a back-contact battery structure with a specific isolation slot location and an appropriate cross-length ratio significantly improves leakage micro-short circuits, while also improving battery conversion efficiency and yield. This significantly reduces silver paste usage, thereby significantly reducing metal electrode costs. However, comparative examples that do not meet the scope of this disclosure fail to achieve the comprehensive benefits of this disclosure. Furthermore, using comparative examples that do not meet the scope of this disclosure fails to achieve the desired comprehensive benefits, including silver paste consumption, yield, parallel resistance, and battery conversion efficiency.
[0174] Furthermore, according to Example 1, Example 2 and Example 4, it can be seen that the use of the preferred conductive film layer scheme of the present disclosure can further improve the battery conversion efficiency while reducing the silver paste consumption. According to Example 1 and Examples 6-10, it can be seen that the use of the preferred specific structural size scheme of the present disclosure is more conducive to improving the battery yield, while taking into account the improvement of the battery parallel resistance and battery conversion efficiency. According to Example 1 and Example 11, it can be seen that the structure of the isolation groove with a specific position and a suitable cross-length ratio disclosed in the present disclosure can be applied to combined passivation structure batteries and heterojunction batteries, and is more conducive to promoting the battery performance in the combined passivation structure, and can better take into account the comprehensive improvement of the silver paste consumption, yield, parallel resistance and battery conversion efficiency in the combined passivation structure battery.
[0175] The preferred embodiments of the present disclosure are described in detail above, but the present disclosure is not limited thereto. Within the technical concept of the present disclosure, various simple variations of the technical solution of the present disclosure may be made, including combining the various technical features in any other appropriate manner. These simple variations and combinations should also be regarded as disclosed by the present disclosure and fall within the scope of protection of the present disclosure. Industrial Applicability
[0176] The present disclosure provides a back-contact battery with a specifically arranged isolation groove and a preparation method thereof, comprising a silicon substrate having a polishing area and a textured area spaced apart along the X-axis direction of the back, a first semiconductor layer disposed on the polishing area, and a second semiconductor layer disposed on the textured area, the back-contact battery further comprising a conductive film layer and a conductive mask layer sequentially disposed outward along the Z-axis direction of the back, the conductive composite layer formed by the conductive mask layer and the conductive film layer being provided with isolation grooves spaced apart along the X-axis direction, the isolation grooves being located above the contact interface of the first semiconductor layer and the second semiconductor layer in the Z-axis direction, and the isolation grooves spanning part of the polishing area and part of the textured area in the X-axis direction. The present disclosure significantly improves the leakage micro-short circuit phenomenon, while improving the battery conversion efficiency and battery yield; and significantly reduces the amount of silver paste used, thereby significantly reducing the cost of metal electrodes.
[0177] Furthermore, it is understood that the disclosed back-contact cells with a specific isolation trench configuration and the method for making the same are reproducible and can be used in a variety of industrial applications. For example, the disclosed back-contact cells with a specific isolation trench configuration and the method for making the same can be used in the field of back-contact cell technology.
Claims
1. A back contact battery with a specific isolation groove arrangement, comprising a silicon substrate having a polishing area and a texturing area arranged at intervals along the X-axis direction of the back side, a first semiconductor layer arranged on the polishing area, and a second semiconductor layer arranged on the texturing area, characterized in that: The back-contact battery also includes a conductive film layer and a conductive mask layer which are sequentially arranged outward along the Z-axis direction of the back side; the conductive composite layer formed by the conductive mask layer and the conductive film layer is provided with isolation grooves spaced along the X-axis direction; the isolation grooves are located above the contact interface between the first semiconductor layer and the second semiconductor layer in the Z-axis direction, and the isolation grooves span part of the polishing area and part of the texturing area in the X-axis direction; the ratio of the span length Wa1 of the isolation groove in the polishing area to the span length Wa2 in the texturing area is 1:0.1-4.
2. The back contact cell according to claim 1, characterized in that: The ratio of the span length Wa1 of the isolation groove in the polishing area to the span length Wa2 in the texturing area is 1:0.1-1; and / or the length Wa of the isolation groove in the X-axis direction is 50-300 μm.
3. The back contact cell according to claim 1, characterized in that: The sheet resistance of the conductive composite layer is not greater than 50Ω / □, and / or the thickness ratio of the conductive film layer to the conductive mask layer is 1:10-100.
4. The back contact cell according to claim 1, characterized in that: The conductive film layer includes at least one of tin-doped indium oxide, metallic copper, metallic aluminum, metallic silver, and nickel-copper alloy, and / or the sheet resistance of the conductive film layer is not greater than 0.7Ω / □.
5. The back contact cell according to claim 4, characterized in that: The conductive film layer comprises a composite film layer formed by a tin-doped indium oxide layer, a metal copper layer, and a nickel-copper alloy layer which are sequentially arranged outwardly along the Z-axis direction, wherein the thickness of the tin-doped indium oxide layer is 50-100 nm, the thickness of the metal copper layer is 200-400 nm, and the thickness of the nickel-copper alloy layer is 50-100 nm; And / or, the conductive film layer comprises a composite film layer of a tin-doped indium oxide layer and a metal aluminum layer sequentially arranged outwardly along the Z-axis direction, the thickness of the tin-doped indium oxide layer is 50-100 nm, and the thickness of the metal aluminum layer is 300-600 nm.
6. The back contact cell according to claim 1, characterized in that: The conductive mask layer includes a layer formed of at least one material selected from carbon paste, copper paste, nickel paste, and conductive ink, and / or the sheet resistance of the conductive mask layer is not greater than 50Ω / □.
7. The back contact cell according to claim 1, characterized in that: In the Z-axis direction of the polishing area, a second semiconductor layer is further disposed above both side edges of the first semiconductor layer in the X-axis direction, and the first semiconductor layer and the second semiconductor layer distributed up and down are in direct contact with each other.
8. The back contact cell according to claim 1 or 7, characterized in that: The first semiconductor layer includes a tunneling oxide layer and a first doped silicon crystal layer, and the second semiconductor layer includes an intrinsic amorphous silicon layer and a second doped silicon crystal layer, wherein one of the first doped silicon crystal layer and the second doped silicon crystal layer is N-type and the other is P-type, and the first doped silicon crystal layer is a doped polycrystalline silicon layer, and the second doped silicon crystal layer is a doped amorphous silicon or microcrystalline silicon layer; the texturing area forms a second opening area to lay part of the second semiconductor layer, and in the Z-axis direction of the polishing area, a second semiconductor layer with a first opening area in the middle is also arranged above the first semiconductor layer, and the first opening area is filled with the conductive film layer.
9. The back contact cell according to claim 8, characterized in that: In the X-axis direction, the span length of the isolation groove on the polishing area and the span length on the texturing area are respectively recorded as Wa1 and Wa2, satisfying: Wa1 / Wg is 5%-100%, Wa2 / W2 is 1%-25%, wherein Wg is the interval between the first opening area and the second opening area, and W2 is the length of the second opening area; And / or, in the X-axis direction, the length W1 of the first opening area is 100-300 μm, the length W2 of the second opening area is 300-700 μm, and the interval Wg between the first opening area and the second opening area is 50-400 μm.
10. The back contact cell according to claim 8, characterized in that The tunneling oxide layer is silicon dioxide with a thickness of 0.5-3nm; the first doped silicon crystal layer is a phosphorus-doped or boron-doped polycrystalline silicon layer with a thickness of 50-300nm and a resistivity of 1E-4Ω.cm—1E-2Ω.cm; the intrinsic amorphous silicon layer has a thickness of 5-15nm; the second doped silicon crystal layer is a phosphorus-doped or boron-doped amorphous silicon layer or a phosphorus-doped or boron-doped microcrystalline silicon layer with a thickness of 5-30nm and a resistivity of 1E-1Ω.cm—1E9Ω.cm.
11. The back contact cell according to claim 1, characterized in that: The back contact battery further comprises: An insulating layer, which is arranged on the surface of the conductive mask layer along the Z-axis direction, and a first portion of which is arranged in the isolation groove, and a second portion of which is arranged at intervals on the outer surface of the conductive mask layer and a side surface of the second portion is in contact with the first portion; the second portion of the insulating layer has a thickness of 5-50 μm; Main grid lines extending along the X-axis direction and electrically connecting the conductive mask layers located in the Z-axis direction of the first semiconductor layer and the second semiconductor layer in series, and arranged at intervals along the Y-axis direction; The front passivation layer and the anti-reflection layer are sequentially arranged on the front side of the silicon substrate outward along the Z-axis direction, and the front side of the silicon substrate is a texturing area.
12. A method for preparing a back contact battery, characterized in that: The back contact battery is a back contact battery according to any one of claims 1 to 11, and the preparation method comprises the following steps: S100, providing a solar panel with a first semiconductor layer and a second semiconductor layer on the back side of a silicon substrate, wherein the back side portion where the first semiconductor layer is located is a polishing area, and the back side portion where the second semiconductor layer is located is a texturing area; S101, forming a conductive film layer on the back side of the solar panel obtained in S100 to fully cover the back side; S102, forming a conductive mask layer on the back side of the solar panel obtained in S101, and leaving isolation openings spaced apart along the X-axis direction on the conductive mask layer, wherein the isolation openings are located above the contact interface between the first semiconductor layer and the second semiconductor layer in the Z-axis direction and span the polishing area and the texturing area in the X-axis direction; S103, etching is performed on the back side of the solar panel obtained in S102 to remove a portion of the conductive film layer located below the isolation opening, so as to form an isolation groove located on the conductive composite layer formed by the conductive mask layer and the conductive film layer.
13. The preparation method according to claim 12, characterized in that: The conductive film layer in S101 is formed by deposition, and the conductive mask layer in S102 is formed by printing or inkjet; and / or, the etching in S103 uses a chemical corrosion solution, and the chemical corrosion solution is at least one of a sulfuric acid solution, a hydrochloric acid solution, a hydrogen peroxide solution, and a ferric chloride solution.
14. The preparation method according to claim 12, characterized in that: S100 also includes: providing a front passivation layer and an anti-reflection layer in the front texturing area of the solar panel; and / or The preparation method further comprises: S104, filling the isolation groove on the back of the solar panel obtained in S103 with an insulating layer material, and simultaneously arranging the insulating layer material in intervals on the surface of the conductive mask layer on the back of the solar panel, thereby forming an insulating layer; S105, printing a plurality of busbars on the back of the solar panel obtained in S104, wherein the busbars respectively connect the first semiconductor layer and the conductive mask layer on the second semiconductor layer in series to form a busbar electrode.
Citation Information
Patent Citations
Back contact heterojunction solar cell and manufacturing method thereof
CN111477694A
Mask-layer-free joint passivation back contact battery and preparation method thereof
CN115312633A
Double-sided tunneling silicon oxide passivated back contact solar cell and preparation method thereof
CN115621333A
Back contact battery with specifically arranged isolation groove and preparation method thereof
CN116093176A