Solid-state electrolyte membrane, preparation method therefor, all-solid-state battery and electrical apparatus
By dispersing ceramic fiber materials in the solid electrolyte membrane, improving their fracture toughness and mechanical properties, the short circuit problem during fast charging of all solid state batteries is solved, and the fast charging capability of the battery and the stability of the electrolyte are improved.
Patent Information
- Application Number
- PCT/CN2023/142849
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2023-12-28
- Publication Date
- 2024-12-05
AI Technical Summary
All-solid-state batteries are prone to short-circuit problems during fast charging, and the fracture toughness of the solid electrolyte membrane is insufficient, resulting in lithium dendrites and electrolyte fragmentation.
The ceramic fiber material is uniformly dispersed in the solid electrolyte, and the diameter and length of the ceramic fiber material meet L/D≥2. The solid electrolyte membrane is prepared by dry or wet mixing to improve its fracture toughness and mechanical properties, and inhibit the lithium dendrites. produce.
It significantly improves the fracture toughness and critical current density of the solid-state electrolyte membrane, enhances the fast charging capability of all-solid-state batteries, and reduces the probability of short circuits.
Smart Images

Figure CN2023142849_05122024_PF_FP_ABST
Abstract
Description
Solid electrolyte membrane and preparation method thereof, all-solid-state battery and power-consuming device
[0001] This application refers to Chinese patent application No. 202310294817.3 filed on March 24, 2023, entitled “Solid electrolyte membrane and preparation method thereof, all-solid-state battery and electrical device”, which is incorporated into this application in its entirety by reference. Technical Field
[0002] The present application relates to the technical field of secondary batteries, and in particular to a solid electrolyte membrane and a preparation method thereof, an all-solid-state battery and an electrical device. Background Art
[0003] Lithium-ion batteries are widely used in portable electronic devices, electric vehicles, and other fields. With the development of society, people's requirements for the safety of lithium-ion batteries are becoming increasingly stringent. Advances in battery research have led to the emergence of solid-state batteries, which are non-flammable, non-corrosive, non-volatile, and leak-proof. In recent years, they have been seen as a successor to lithium-ion batteries. Solid-state battery technology replaces liquid electrolytes with solid electrolytes, significantly increasing the battery's energy density.
[0004] However, all-solid-state batteries in related technologies are prone to short circuit problems during fast charging.
[0005] Summary of the Invention
[0006] This application is made in view of the above-mentioned issues, and its purpose includes providing a solid electrolyte membrane and its preparation method, an all-solid-state battery and an electrical device to reduce the probability of short circuit during the fast charging process of the all-solid-state battery and improve the fast charging capability of the all-solid-state battery.
[0007] In order to achieve the above-mentioned object, the first aspect of the present application provides a solid electrolyte membrane, comprising a solid electrolyte and a ceramic fiber material dispersed in the solid electrolyte;
[0008] The solid electrolyte includes an inorganic solid electrolyte;
[0009] The diameter of the ceramic fiber material is recorded as D, and the length of the ceramic fiber material is recorded as L. The diameter of the ceramic fiber material and the length of the ceramic fiber material satisfy: L / D≥2.
[0010] Because ceramic fibers are dispersed within the solid electrolyte, when the solid electrolyte membrane fractures due to stress generated by electrochemical deposition, the ceramic fibers surrounding the crack can pull out or break, absorbing a significant amount of the strain energy of the fracture, significantly increasing the difficulty of crack propagation and improving the fracture toughness of the solid electrolyte membrane to over 0.05 MPa m^(1 / 2). This improves its mechanical properties and inhibits the formation of lithium dendrites. This significantly increases the critical current density of the solid electrolyte membrane, enhancing the fast-charging capability of all-solid-state batteries. Furthermore, an aspect ratio of the ceramic fiber material ≥2 further enhances the toughness of the solid electrolyte membrane.
[0011] In some embodiments, the diameter of the ceramic fiber material and the length of the ceramic fiber material satisfy: L / D ≥ 20; optionally 20 ≤ L / D ≤ 500.
[0012] In some embodiments, the diameter of the ceramic fiber material satisfies: D≤5 μm; optionally 0.5 μm≤D≤2 μm.
[0013] In some embodiments, the length of the ceramic fiber material satisfies: 1 μm≤L≤500 μm; optionally 10 μm≤L≤200 μm.
[0014] In some embodiments, the ceramic fiber material includes one or more of silicon carbide fibers, silicon nitride fibers, boron nitride fibers, alumina fibers, and silica fibers.
[0015] In some embodiments, the ceramic fiber material has at least one of the following features (1)-(2):
[0016] (1) The volume ratio of the ceramic fiber material to the solid electrolyte is (0.01-40):100; optionally (3-7):100;
[0017] (2) The mass ratio of the ceramic fiber material to the solid electrolyte is (0.01-85):100; optionally, (2-15):100.
[0018] In some embodiments, the distribution uniformity of the ceramic fiber material in the solid electrolyte is ≤0.3; alternatively, the distribution uniformity of the ceramic fiber material in the solid electrolyte is ≤0.1.
[0019] In some embodiments, a binder is further distributed in the solid electrolyte;
[0020] Optionally, the binder includes one or more of nitrile rubber, polyvinylidene fluoride, polytetrafluoroethylene, polyacrylic acid, polyvinyl alcohol, polyimide, polyacrylonitrile, polyurethane, polycarboxymethyl cellulose, cyclodextrin, sodium alginate, polysaccharide, nitrile rubber and styrene-butadiene rubber;
[0021] Optionally, the mass ratio of the binder to the solid electrolyte is (0.01-20):100; optionally (0.5-5):100.
[0022] In some embodiments, the solid electrolyte membrane has at least one of the following features (1)-(4):
[0023] (1) The critical current density of the solid electrolyte membrane at 25°C is 0.5 mA / cm 2 -10mA / cm 2 ;
[0024] (2) The fracture toughness of the solid electrolyte membrane is 0.05 MPa m^(1 / 2)-2 MPa m^(1 / 2);
[0025] (3) The ionic conductivity of the solid electrolyte membrane at 25°C is 0.1 mS / cm 2 -10mS / cm 2 ;
[0026] (4) The thickness of the solid electrolyte membrane is 1 μm-1000 μm.
[0027] A second aspect of the present application provides a method for preparing a solid electrolyte membrane, comprising the following steps:
[0028] mixing the ceramic fiber material and the solid electrolyte to prepare a mixture;
[0029] The mixed material is molded to prepare the solid electrolyte membrane.
[0030] In some embodiments, the ceramic fiber material and the solid electrolyte are mixed by dry mixing;
[0031] Optionally, the mixing time is 1 h-24 h.
[0032] In some embodiments, the molding process is a pressurization process; optionally, the pressure of the pressurization process is 200 MPa-600 MPa.
[0033] In some embodiments, the ceramic fiber material and the solid electrolyte are mixed using wet mixing;
[0034] Optionally, the mixing time is 0.5h-12h.
[0035] In some embodiments, the molding process includes coating the mixture into a film and then drying it.
[0036] A third aspect of the present application provides an all-solid-state battery, comprising the solid-state electrolyte membrane of the first aspect.
[0037] The fourth aspect of the present application provides an electrical device comprising the all-solid-state battery of the third aspect.
[0038] The details of one or more embodiments of the present application are set forth in the following drawings and description. Other features, objects, and advantages of the present application will become apparent from the description, drawings, and claims. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to better describe and illustrate the embodiments or examples provided in this application, reference may be made to one or more of the accompanying drawings. The additional details or examples used to describe the accompanying drawings should not be considered as limiting the scope of the disclosed application, the embodiments or examples currently described, and any of the best modes currently understood for these applications. Moreover, the same reference numerals are used throughout the drawings to represent the same components. In the accompanying drawings:
[0040] FIG1 is a cross-sectional SEM image of the solid electrolyte membrane in Example 2 of the present application.
[0041] FIG2 is a schematic diagram of an all-solid-state battery according to an embodiment of the present application.
[0042] FIG3 is an exploded view of the all-solid-state battery according to one embodiment of the present application shown in FIG2 .
[0043] FIG4 is a schematic diagram of an electrical device using an all-solid-state battery as a power source according to an embodiment of the present application.
[0044] Explanation of Reference Numerals: 111, ceramic fiber material; 112, solid electrolyte; 1, all-solid-state battery; 11, housing; 12, electrode assembly; 13, cover plate; 2, power-consuming device. DETAILED DESCRIPTION
[0045] To facilitate understanding of the present application, a more comprehensive description of the present application will be provided below with reference to the accompanying drawings. The accompanying drawings illustrate preferred embodiments of the present application. However, the present application may be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a more thorough and comprehensive understanding of the disclosure of the present application.
[0046] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application pertains. The terms used herein in the specification of this application are for the purpose of describing specific embodiments only and are not intended to limit this application.
[0047] In this application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0048] In this application, when referring to numerical ranges, unless otherwise specified, the numerical ranges are considered continuous and include the minimum and maximum values of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe a feature or characteristic, the ranges can be combined. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges subsumed therein.
[0049] In this application, when referring to a range of units, if only the right endpoint is followed by a unit, it means that the units of the left and right endpoints are the same. For example, 10-1000nm means that the units of the left endpoint "10" and the right endpoint "1000" are both nm (nanometers).
[0050] In this application, references to "multiple," "multiple," and "multiple times," etc., unless otherwise specified, refer to a number greater than or equal to 2. For example, "multiple" means greater than or equal to two. Only some numerical ranges are specifically disclosed herein. However, any lower limit can be combined with any upper limit to form an unspecified range; and any lower limit can be combined with other lower limits to form an unspecified range, and similarly, any upper limit can be combined with any other upper limit to form an unspecified range. In addition, each individually disclosed point or single value can itself be combined as a lower limit or upper limit with any other point or single value, or with other lower limits or upper limits, to form an unspecified range.
[0051] The "ranges" disclosed herein are defined in terms of lower and upper limits. A given range is defined by selecting a lower limit and an upper limit, and the selected lower and upper limits define the boundaries of the particular range. Ranges defined in this manner may be inclusive or exclusive of the end values.
[0052] The temperature parameters in this application, unless otherwise specified, allow for both constant temperature treatment and treatment within a certain temperature range. The constant temperature treatment allows for temperature fluctuations within the precision range of instrument control.
[0053] References to "embodiments" herein mean that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment or implementation of the present application. The appearance of such phrases in various locations in the specification does not necessarily refer to the same embodiment, nor does it necessarily refer to independent or alternative embodiments that are mutually exclusive with other embodiments. It is understood, both explicitly and implicitly, by those skilled in the art that the embodiments described herein may be combined with other embodiments. References to "implementations" herein have a similar understanding.
[0054] It will be appreciated by those skilled in the art that, in the methods of various embodiments or examples, the order in which the steps are written does not imply a strict order of execution and does not constitute any limitation on the implementation process, and the detailed order of execution of each step should be determined by its function and possible inherent logic. Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or steps (a), (c) and (b), or steps (c), (a) and (b), etc.
[0055] In this application, in the open technical features or technical solutions described with words such as "contain", "include", and "include", unless otherwise specified, additional members other than the listed members are not excluded, and it can be regarded as providing both closed features or solutions consisting of the listed members and open features or solutions that also include additional members in addition to the listed members. For example, A includes a1, a2, and a3. Unless otherwise specified, it may also include other members or may not include additional members. It can be regarded as providing both the feature or solution of "A consists of a1, a2, and a3", and the feature or solution of "A includes not only a1, a2, and a3, but also other members". In recent years, with the progress of battery research, the application of solid-state batteries has become more and more extensive. In the related art, all-solid-state batteries are prone to short circuit problems during fast charging. After research, the technical personnel of this application found that during the charging process of all-solid-state batteries, high-rate charging will cause uneven lithium deposition, and the uneven lithium deposition process may induce electrolyte fragmentation and the formation of dendrites; dendrites will penetrate the solid electrolyte and eventually establish an electron path between the positive and negative electrodes, thereby causing short circuit and failure of the all-solid-state battery.
[0056] In addition, solid electrolyte membranes also have the problems of brittleness and low fracture toughness.
[0057] The present application provides a solid electrolyte membrane, comprising a solid electrolyte and a ceramic fiber material dispersed in the solid electrolyte; the solid electrolyte comprises an inorganic solid electrolyte; the diameter of the ceramic fiber material is denoted as D, and the length of the ceramic fiber material is denoted as L, and the diameter of the ceramic fiber material and the length of the ceramic fiber material satisfy: L / D ≥ 2.
[0058] It should be noted that the ceramic fiber material can be uniformly dispersed or randomly dispersed in the solid electrolyte. Preferably, the ceramic fiber material is uniformly dispersed in the solid electrolyte, and the distribution of the ceramic fiber material in the solid electrolyte has no obvious spatial orientation characteristics.
[0059] Understandably, since ceramic fiber materials are dispersed in the solid electrolyte, when the solid electrolyte membrane is fractured by the stress generated by electrochemical deposition, the ceramic fiber materials around the cracks may be pulled out or fractured, absorbing a large amount of strain energy of the fracture, greatly increasing the difficulty of crack propagation, and improving the fracture toughness of the solid electrolyte membrane to a value higher than 0.05MPa m^(1 / 2), thereby improving its mechanical properties and inhibiting the formation of lithium dendrites. At the same time, it greatly increases the critical current density of the solid electrolyte membrane and improves the fast charging capability of the all-solid-state battery. In addition, when the aspect ratio of the ceramic fiber material is ≥2, the fracture toughness of the solid electrolyte membrane can be further improved.
[0060] The length and diameter of the ceramic fiber material mentioned above can be measured by the following method: a uniformly broken cross-section of a solid electrolyte membrane is prepared by an ultrasonic knife and observed by a scanning electron microscope. In the backscattered electron imaging mode of the scanning electron microscope, the ceramic fiber material is distinguished by the contrast of the material, and the length and diameter of the ceramic fiber material are measured.
[0061] In some embodiments, the diameter of the ceramic fiber material and the length of the ceramic fiber material satisfy: L / D ≥ 20; when the diameter and length of the ceramic fiber material satisfy the above relationship, the ceramic fiber material has a high degree of interlacing and can cover most of the volume of the solid electrolyte, thereby improving the toughening effect and reducing the problem of interface ion conduction non-uniformity caused by the continuous exposure area of the ceramic fiber material at the lithium metal solid electrolyte interface.
[0062] In some exemplary embodiments, the diameter and length of the ceramic fiber material satisfy the following ratio: 20≤L / D≤500. For example, the ratio may be 20≤L / D≤450, 20≤L / D≤400, 20≤L / D≤350, 20≤L / D≤300, 20≤L / D≤250, 20≤L / D≤200, 20≤L / D≤150, 20≤L / D≤100, or 20≤L / D≤50. As an example, the ratio of the length to the diameter of the ceramic fiber material may be 20, 50, 100, 150, 200, 250, 300, 350, 400, 450, or 500.
[0063] In some embodiments, the diameter of the ceramic fiber material satisfies: D ≤ 5 μm. By controlling the diameter of the ceramic fiber material within this range, the ceramic fiber's toughening effect can be maintained while further reducing its obstruction to the lithium ion transmission path of the solid electrolyte, thereby reducing the unevenness of ion conduction at the lithium metal solid electrolyte interface. If the diameter of the ceramic fiber material is too large, it will significantly affect the ionic conductivity and uniformity of the ion transmission path of the solid electrolyte membrane.
[0064] In some exemplary embodiments, the diameter of the ceramic fiber material satisfies the following: 0.5 μm ≤ D ≤ 2 μm. For example, the diameter may be 0.6 μm ≤ D ≤ 2 μm, 0.7 μm ≤ D ≤ 1.9 μm, 0.8 μm ≤ D ≤ 1.8 μm, 0.9 μm ≤ D ≤ 1.7 μm, 1.0 μm ≤ D ≤ 1.6 μm, 1.1 μm ≤ D ≤ 1.5 μm, or 1.2 μm ≤ D ≤ 1.4 μm. As an example, the diameter of the ceramic fiber material may be 0.5 μm, 0.8 μm, 1 μm, 1.3 μm, 1.5 μm, 1.7 μm, or 2 μm.
[0065] In some embodiments, the length of the ceramic fiber material satisfies the following conditions: 1 μm ≤ L ≤ 500 μm; for example, 5 μm ≤ L ≤ 450 μm, 5 μm ≤ L ≤ 400 μm, 5 μm ≤ L ≤ 350 μm, 5 μm ≤ L ≤ 300 μm, 5 μm ≤ L ≤ 250 μm, 5 μm ≤ L ≤ 200 μm, 5 μm ≤ L ≤ 150 μm, 5 μm ≤ L ≤ 100 μm, or 5 μm ≤ L ≤ 50 μm, etc., without limitation. By controlling the length of the ceramic fiber material within the above range, the toughening effect of the ceramic fiber material can be maximized to cover all areas of the solid electrolyte, while also reducing or even avoiding obstruction to ion transport pathways in the solid electrolyte. As an example, the length of the ceramic fiber material may include, but is not limited to, 1 μm, 5 μm, 10 μm, 50 μm, 100 μm, 150 μm, 200 μm, 250 μm, 300 μm, 350 μm, 400 μm, 450 μm, or 500 μm.
[0066] In some embodiments, the length of the ceramic fiber material satisfies 10 μm≤L≤200 μm.
[0067] In some embodiments, the ceramic fiber material includes one or more of silicon carbide fiber, silicon nitride fiber, boron nitride fiber, alumina fiber, and silica fiber. Optionally, the ceramic fiber material is selected from alumina; this can enhance the toughening effect of the ceramic fiber material and improve its affinity with lithium metal at the solid electrolyte interface, thereby improving the uniformity of ion conduction.
[0068] In some embodiments, the volume ratio of the ceramic fiber material to the solid electrolyte is (0.01-40):100; for example, it can be (0.1-40):100, (0.5-38):100, (1-35):100, (3-30):100, (3-25):100, (3-20):100, (3-15):100, (3-10):100, or (3-5):100. When the volume ratio of the ceramic fiber material to the solid electrolyte is lower than the above range, the mechanical properties and fracture toughness of the solid electrolyte may not be effectively improved; when the volume ratio of the ceramic fiber material to the solid electrolyte is higher than the above range, the ceramic fiber material may occupy too much volume of the solid electrolyte, reducing the distribution uniformity of the solid electrolyte bulk and interface ion transport channels, thereby inducing local current density hot spots and reducing the critical current density of the solid electrolyte. When the volume ratio of the ceramic fiber material to the solid electrolyte is within the above range, the toughening effect of the ceramic fiber material can be enhanced while ensuring the ionic conductivity of the solid electrolyte, and the critical current density of the solid electrolyte membrane can be increased.
[0069] In some embodiments, the volume ratio of the ceramic fiber material to the solid electrolyte is (3-7):100.
[0070] As an example, the volume ratio of the above-mentioned ceramic fiber material and solid electrolyte can be measured by the following method: an electrolyte disc with a diameter of 10 mm is prepared by an ultrasonic knife or a slicing mold, and observed by a high-resolution X-ray tomography scanner. In the high-resolution X-ray tomography results, the ceramic fiber material and the solid electrolyte material can be distinguished by the grayscale based on the electron density of the material within the pixel, thereby confirming the volume ratio of the ceramic fiber material in the solid electrolyte membrane / sheet.
[0071] In some embodiments, the mass ratio of the ceramic fiber material to the solid electrolyte is (0.01-85):100; for example, it can be (0.1-85):100, (1-80):100, (1-75):100, (1-70):100, (1-65):100, (1-60):100, (1-55):100, (1-50):100, (1-45):100, (1-40):100, (1-35):100, (1-30):100, (1-25):100, (1-20):100, (1-15):100, or (1-10):100, etc., without specific limitation.
[0072] In some exemplary embodiments, the mass ratio of the ceramic fiber material to the solid electrolyte is (2-15):100.
[0073] Taking sulfide electrolyte as an example, the mass ratio of the ceramic fiber material to the solid electrolyte mentioned above can be measured using the following method: Weigh a piece of solid electrolyte membrane / sheet, then dissolve the sulfide solid electrolyte in an excess of deionized water. After the sulfide solid electrolyte is fully dissolved, it is filtered to obtain a ceramic fiber material, which is then fully dried in an 80°C vacuum oven and weighed again. The weight of the weighed ceramic fiber material is divided by the weight of the initial electrolyte membrane / sheet to obtain the mass ratio of the ceramic fiber material in the solid electrolyte membrane / sheet.
[0074] In some embodiments, the distribution uniformity of the ceramic fiber material in the solid electrolyte is ≤0.3; for example, it can be 0.05-0.3, 0.05-0.25, 0.05-0.2, 0.05-0.15 or 0.05-0.1, etc. In some exemplary embodiments, the distribution uniformity of the ceramic fiber material in the solid electrolyte is ≤0.1. The smaller the distribution uniformity of the ceramic fiber material in the solid electrolyte, the more uniform its distribution in the solid electrolyte, which helps to further improve the fracture toughness and mechanical strength of the solid electrolyte, inhibit the fragmentation of the solid electrolyte, and significantly increase the critical current density of the solid electrolyte membrane; at the same time, the ion conduction uniformity at the interface between the lithium metal and the solid electrolyte is better. As an example, the distribution uniformity of the ceramic fiber material in the solid electrolyte can be 0.05, 0.1, 0.15, 0.2, 0.25 or 0.3, etc.
[0075] It should be noted that distribution uniformity is an indicator that describes the degree of uniform distribution of ceramic fiber materials in solid electrolytes. The distribution uniformity between solid phases can generally be measured using methods such as grid counting method, intercept method, area method, zone method, and exclusive circle method.
[0076] The distribution uniformity of the ceramic fiber material mentioned above in the solid electrolyte in this application can be tested by the intercept method: take the solid electrolyte membrane, and prepare a cross-section of the ceramic fiber material and the solid electrolyte with uniform fracture by the ultrasonic knife method, and observe it through a scanning electron microscope. In the backscattered electron imaging mode of the scanning electron microscope, the ceramic fiber material and the solid electrolyte are distinguished according to the contrast of the material, and then the distribution uniformity is calculated based on the image measurement.
[0077] The distance d between the cross sections of the ceramic fiber material was measured by line analysis based on the scanning electron microscope image. i (i=1,2,3,…..N), by d i Find the standard deviation σ between N distances d :
[0078] Among them, A0 represents the distribution uniformity of ceramic fiber material in solid electrolyte, It represents the average value of the distance between N ceramic fiber material sections.
[0079] It should be noted that when measuring the distribution uniformity of the ceramic fiber material in the solid electrolyte, the frozen ion beam polishing method can also be used to prepare a cross-section of the ceramic fiber and the solid electrolyte with uniform fracture.
[0080] In some embodiments, a binder is also distributed in the solid electrolyte membrane.
[0081] In some embodiments, the binder includes one or more of nitrile rubber, polyvinylidene fluoride, polytetrafluoroethylene, polyacrylic acid, polyvinyl alcohol, polyimide, polyacrylonitrile, polyurethane, polycarboxymethyl cellulose, cyclodextrin, sodium alginate, polysaccharide, nitrile rubber and styrene-butadiene rubber.
[0082] In some embodiments, the mass ratio of the binder to the solid electrolyte is (0.01-20):100; for example, it can be (0.1-20):100, (0.3-18):100, (0.3-15):100, (0.3-12):100, (0.3-10):100, (0.3-7):100 or (0.3-5):100, etc., without specific limitation.
[0083] In some exemplary embodiments, the mass ratio of the binder to the solid electrolyte is (0.5-5):100.
[0084] In some embodiments, the inorganic solid electrolyte includes one of a lithium ion solid electrolyte, a sodium ion solid electrolyte, and a potassium ion solid electrolyte.
[0085] As an example, lithium ion solid electrolytes include LISICON type solid electrolytes, NASICON type lithium ion solid electrolytes, Garnet type solid electrolytes, LIPON type solid electrolytes, Perovskite type solid electrolytes, Anti-Perovskite type lithium ion solid electrolytes, Thio-LiSICON type solid electrolytes, Li 10 GeP2S 12One or more of a Garnet-type solid electrolyte, a (100-e)Li2S·e(F2)·f(G2)-type solid electrolyte, an Argyrodite-type solid electrolyte, a Halide-type solid electrolyte, and a Hydride-type lithium-ion solid electrolyte; wherein, in the (100-e)Li2S·e(F2)·f(G2)-type solid electrolyte, 20 ≤ e ≤ 30, 0 ≤ f ≤ 50, F2 includes one or more of B2S3, Al2S3, In2S3, SiS2, GeS2, SnS2, P2S5, As2S3, Sb2S5, Bi2S3, WS2, and MoS2, and G2 includes one or more of B2O3, Al2O3, In2O3, SiO2, GeO2, SnO2, P2O5, Sb2O5, Bi2O3, WO2, WO3, MoO2, MoO3, Fe2O3, ZnO, MgO, CuO, CaO, LiN, Li2O, LiF, LiCl, LiBr, and LiI; the sodium-ion solid electrolyte includes a NASICON-type sodium-ion solid electrolyte, a Na-β-Alumina-type solid electrolyte, a Na3PS4-type solid electrolyte, Na 11 Sn2PS 12 One or more of a type solid electrolyte, an anti-perovskite-type solid electrolyte, and a Hydride-type sodium-ion solid electrolyte; the potassium-ion solid electrolyte includes one or more of a β-Alumina-type potassium-ion solid electrolyte, an Anti-Perovskite-type potassium-ion solid electrolyte, a K2Fe4O7-type solid electrolyte, and a KSi2P3-type solid electrolyte.
[0086] As an example, the Garnet-type solid electrolyte includes Li 7-a La3Zr 2-a (A2) a O 12 ; wherein, 0 ≤ a < 1; A2 includes one or more of Sb, Nb, Ta, Te, and W.
[0087] The Thio-LiSICON-type solid electrolyte includes Li 3+b (B2) c (C2) 1-c (D2) 4-d (E2) d ; wherein, -1 < b < 2, 0 ≤ c ≤ 1, 0 ≤ d ≤ 2; B2 includes one or more of B, Al, In, Si, Ge, Sn, Ti, W, and Mo; C2 includes one or more of P, As, Sb, and Bi; D2 includes one or more of S and Se; E2 includes one or more of F, Cl, Br, and I.
[0088] The argyrodite-type solid electrolyte includes Li 6+g (H2) h (I2) 1-h (J2) 5-i (K2) 1+i ; where, -1 ≤ g ≤ 1, 0 ≤ h ≤ 1, -1 < i ≤ 1; H2 includes one or more of B, Al, In, Si, Ge, Sn, Ti, W, and Mo; I2 includes one or more of P, As, Sb, and Bi; J2 represents one or more of S and Se; K2 includes one or more of F, Cl, Br, and I.
[0089] The LISICON-type solid electrolyte includes γ-Li3PO4.
[0090] The NASICON-type lithium ion solid electrolyte includes Li 1+j (L2) j (M2) 2-j (PO4)3, where 0 ≤ j < 1; L2 includes one or more of Al, Cr, Ba, Fe, Sc, In, Lu, Y, and La; M2 includes one or more of Ti and Ge.
[0091] The Perovskite-type solid electrolyte includes Li 3k (N2) 2 / 3-k (Q2)O3, where 0.04 < k < 0.17; N2 includes one or more of La, Sr, Ba, and Nd; Q2 includes one or more of Al, Ti, and Ge.
[0092] The Anti-Perovskite-type lithium ion solid electrolyte includes Li3OCl.
[0093] Li 10 GeP2S 12 -type solid electrolyte includes Li 10+l (R2) 1+m (S2) 2-m (T2) 12-n (U2) n , where -2 < l < 2, 0 ≤ m ≤ 2, 0 ≤ n ≤ 2, R2 includes one or more of B, Al, In, Si, Ge, Sn, Ti, W, and Mo; S2 includes one or more of P, As, Sb, and Bi; T2 includes one or more of S and Se; U2 includes one or more of F, Cl, Br, and I. <0One or more of those in (W2)4; wherein, V2 includes one or more of Y, Er, In, Sc, and Ga; W2 includes one or more of F, Cl, Br, and I.
[0095] The Hydride type lithium ion solid electrolyte includes LiBH4 and pLi(CB9H 10 ).·(1 - p)Li(CB 11 H 12 ); wherein, 0 < p < 1.
[0096] The LIPON type solid electrolyte includes Li q PO r N s etc.; wherein, when 2r + 3s - q = 5, q≥1, r≥1, s≥0.
[0097] The NASICON type sodium ion solid electrolyte includes Na 1+t+2u Zr 2-u (A3) u P 3-t Si t O 12 ; wherein, 0≤t≤3, 0≤u≤1, A3 includes one or more of Zn, Mg, and Ca.
[0098] The Na-β-Alumina type solid electrolyte includes one or more of Na2O·(5 - 7)Al2O3 and Na2O·(8 - 11)Al2O3.
[0099] The Na3PS4 type solid electrolyte includes Na 3+x (B3) v (C3) 1-v (D3) 4-w (E3) w , where -1 < x < 2, 0≤v≤1, 0≤w≤'2, B3 includes one or more of B, Al, In, Si, Ge, Sn, Ti, W, and Mo; C3 includes one or more of P, As, Sb, and Bi; D3 includes one or more of S and Se; E3 represents one or more of F, Cl, Br, and I.
[0100] Na 11 Sn2PS 12 The type solid electrolyte includes Na 11+(x1) (F3) 2-y (G, where -1 < x1 < 1, 0 ≤ y ≤ 2, 0 ≤ z ≤ 2, F3 includes one or more of B, Al, In, Si, Ge, Sn, Ti, W, and Mo; G3 includes one or more of P, As, Sb, and Bi; H3 includes one or more of S and Se; J3 includes one or more of F, Cl, Br, and I.
[0101] The anti-perovskite type solid electrolyte includes Na3O(K3), where K3 includes one or more of Cl, Br, I, and BH4.
[0102] The Hydride type sodium ion solid electrolyte includes Na2C (b1) B (a1)-(b1) H (b1) and Na(BH4) 0.5 (NH2) 0.5 etc., where a1 = 10 or 12, b1 = 0 or 1.
[0103] The β-alumina type potassium ion solid electrolyte includes K2O·(8 - 11)Al2O3.
[0104] The Anti-Perovskite type potassium ion solid electrolyte includes K3OI.
[0105] The K2Fe4O7 type solid electrolyte includes K2Fe4O7.
[0106] The KSi2P3 type solid electrolyte includes KSi2P3.
[0107] In some embodiments, the critical current density of the solid electrolyte membrane at 25 °C is 0.5 mA / cm 2 - 10 mA / cm 2 .
[0108] It should be noted that the critical current density refers to the lowest current density at which dendrites and short circuits occur when the solid electrolyte membrane is paired with the corresponding alkali metal electrode for electrochemical deposition. That is, when electrochemical deposition occurs at a current density lower than the critical current density, dendrites and short circuits will not occur. The critical current density is a core index for describing the ability of the solid electrolyte membrane to inhibit dendrites and short circuits.
[0109] As an example, the critical current density of the solid electrolyte membrane mentioned above can be measured using the traditional symmetrical battery step-by-step current density cycle method: at 25°C, two 8mm dendrites and 50μm thick lithium metal discs are placed at the symmetrical center of the solid electrolyte membrane on both sides. Mechanical pressure is used to tightly fit the lithium metal discs and the solid electrolyte membrane to form a lithium / solid electrolyte membrane / lithium symmetrical battery; after the symmetrical battery is assembled and packaged, the lithium / solid electrolyte membrane / lithium symmetrical battery is increased from 0.25mA / cm 2 Initially, 1 mAh / cm was deposited and stripped on one side. 2 After lithium, the current was increased to 0.5 mA / cm 2 , maintain 1mAh / cm 2 After the surface capacity deposition and stripping, the 2 The gradient is 0.75 mA / cm 2 , 1.0mA / cm 2 , 1.25mA / cm 2 ...to 10mA / cm 2 The current density at which the voltage suddenly drops sharply is recorded as the critical current density.
[0110] In some embodiments, the fracture toughness of the solid electrolyte membrane is 0.05 MPa m^(1 / 2)-2 MPa m^(1 / 2).
[0111] It should be noted that fracture toughness is a parameter that describes the ability of the solid electrolyte membrane to absorb strain energy before fracture. Higher fracture toughness represents a stronger barrier to crack propagation, and also reflects the solid electrolyte membrane's resistance to cracking and short circuits caused by dendrites.
[0112] As an example, the fracture toughness of the solid electrolyte membrane mentioned above can be obtained by using a Vickers cone indentation test: the surface of the solid electrolyte membrane is polished with sandpaper in an argon atmosphere, from 800 mesh, to 2000 mesh, to 4000 mesh, to 8000 mesh, until the surface of the solid electrolyte membrane presents a mirror surface without obvious defects; then, the polished surface is subjected to an indentation test using a Vickers cone indentation tester; the indentation tester is driven with an appropriate load until radial cracks appear at the four corners of the cone indentation; according to the indentation load S, the extension length L of the radial crack, and the microhardness H V The fracture toughness value K can be calculated by the following formula IC :
[0113] Here, E represents the Young's modulus of the solid electrolyte membrane.
[0114] In some embodiments, the solid electrolyte membrane has an ionic conductivity of 0.1 mS / cm at 25°C. 2 -10mS / cm 2 .
[0115] It should be noted that ionic conductivity is the core indicator for measuring the ability of solid electrolyte membrane to transmit corresponding alkali metal ions.
[0116] The ionic conductivity of the solid electrolyte membrane mentioned above can be measured by the following method: at 25°C, a 10 mm diameter cylindrical stainless steel current collector is used to tightly clamp the solid electrolyte membrane in a battery mold under mechanical pressure, and then the current collector is connected to an electrochemical workstation and the bias voltage is 10 mV and the frequency is 10 6 The electrochemical impedance spectroscopy (EIS) test of the solid electrolyte membrane was performed in the range of 0.1 Hz to 0.1 Hz. The Z' coordinate value of the point closest to the Z' axis from right to left in the low-frequency band of the EIS curve was used as the resistance value R, and the ionic conductivity σ was calculated using the following formula:
[0117] Wherein, D is the thickness of the solid electrolyte membrane, and A is the contact area between the solid electrolyte membrane and the current collector.
[0118] In some embodiments, the solid electrolyte membrane has a thickness of 1 μm to 1000 μm.
[0119] As an example, the thickness of the solid electrolyte membrane mentioned above can be measured by the following method: first calibrate the micrometer, then place the solid electrolyte membrane between the double anvils, gently rotate the sleeve until a sound is heard, and read and record the thickness of the solid electrolyte membrane.
[0120] The present application also provides a method for preparing a solid electrolyte membrane, comprising the following steps: mixing a ceramic fiber material and a solid electrolyte to prepare a mixture; and molding the mixture to prepare a solid electrolyte membrane.
[0121] In some embodiments, the ceramic fiber material and the solid electrolyte are mixed using a dry mixing process. As an example, the mixing time is 1 hour to 24 hours. For example, the mixing time may be 3 hours to 24 hours, 5 hours to 20 hours, 7 hours to 18 hours, 10 hours to 15 hours, or 10 hours to 12 hours, etc., without limitation.
[0122] In some embodiments, the forming process is a pressurization process. In some exemplary embodiments, the pressure of the pressurization process is 200 MPa-600 MPa. For example, the pressure can be 250 MPa-600 MPa, 250 MPa-550 MPa, 300 MPa-500 MPa, 350 MPa-450 MPa, or 400 MPa-450 MPa, etc., without limitation.
[0123] As an example, a method for preparing a solid electrolyte membrane includes: weighing ceramic fiber material powder and solid electrolyte powder respectively, performing dry mixing to prepare a mixture; and using a mold to press the mixture into a sheet under mechanical flat pressing to prepare a solid electrolyte membrane.
[0124] In some embodiments, the ceramic fiber material and the solid electrolyte are mixed using a wet mixing process. In some embodiments, the mixing time is 0.5 hours to 12 hours. For example, the mixing time may be 1 hour to 12 hours, 2 hours to 11 hours, 3 hours to 10 hours, 4 hours to 9 hours, 5 hours to 8 hours, or 6 hours to 7 hours, etc., without limitation.
[0125] In some embodiments, the forming process includes coating the mixed material into a film and then drying it.
[0126] As an example, the preparation method of the solid electrolyte membrane includes: weighing ceramic fiber material powder and solid electrolyte powder separately, adding the ceramic fiber material powder to the solid electrolyte powder, and then adding a solvent and a binder for wet mixing to prepare a mixture; coating the mixture to form a continuous electrolyte film, drying it, and preparing the solid electrolyte membrane.
[0127] The above raw materials, unless otherwise specified, can be obtained commercially.
[0128] The present application also provides an all-solid-state battery, comprising the above-mentioned solid-state electrolyte membrane.
[0129] As a result, the obtained all-solid-state battery has good fast charging performance.
[0130] The all-solid-state battery, battery module, battery pack and electrical device of the present application are described below with appropriate reference to the accompanying drawings.
[0131] In one embodiment of the present application, an all-solid-state battery is provided.
[0132] Typically, an all-solid-state battery consists of a positive electrode, a negative electrode, and a solid electrolyte membrane. During the battery's charge and discharge processes, active ions are embedded in and extracted from the positive and negative electrodes. The solid electrolyte membrane acts as a conductor of ions between the positive and negative electrodes.
[0133] Positive electrode
[0134] The positive electrode sheet includes a positive electrode current collector and a positive electrode film layer provided on at least one surface of the positive electrode current collector, wherein the positive electrode film layer includes a positive electrode active material.
[0135] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive electrode current collector.
[0136] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material base layer. The composite current collector may be formed by forming a metal material on a polymer material substrate. Among them, the metal material includes but is not limited to aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc. The polymer material substrate includes but is not limited to polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.
[0137] In some embodiments, the positive electrode active material may include a positive electrode active material for a battery that is well known in the art. As an example, the positive electrode active material may include at least one of the following materials: a lithium-containing phosphate with an olivine structure, a lithium transition metal oxide, and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM 333 ), LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM 523 ), LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 ), LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM 622 ), LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM 811 ), lithium nickel cobalt aluminum oxide (such as LiNi 0.80 Co 0.15 Al 0.05O2) and its modified compounds. Examples of olivine-structured lithium-containing phosphates may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon. The weight ratio of the positive electrode active material in the positive electrode film layer is 80% to 100% by weight, based on the total weight of the positive electrode film layer.
[0138] In some embodiments, the positive electrode film layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin. The weight ratio of the binder in the positive electrode film layer is 0-20 weight%, based on the total weight of the positive electrode film layer.
[0139] In some embodiments, the positive electrode film layer may further optionally include a conductive agent. For example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. The weight ratio of the conductive agent in the positive electrode film layer is 0-20% by weight, based on the total weight of the positive electrode film layer.
[0140] In some embodiments, the positive electrode film layer may further include an electrolyte. As an example, the electrolyte may include one of a lithium ion solid electrolyte, a sodium ion solid electrolyte, and a potassium ion solid electrolyte.
[0141] In some embodiments, the lithium ion solid electrolyte includes a LISICON type solid electrolyte, a NASICON type lithium ion solid electrolyte, a Garnet type solid electrolyte, a LIPON type solid electrolyte, a Perovskite type solid electrolyte, an Anti-Perovskite type lithium ion solid electrolyte, a Thio-LiSICON type solid electrolyte, a Li 10 GeP2S 12One or more of a (100-e)Li2S·e(F2)·f(G2) type solid electrolyte, a (100-e)Li2S·e(F2)·f(G2) type solid electrolyte, an Argyrodite type solid electrolyte, a Halide type solid electrolyte, and a Hydride type lithium ion solid electrolyte; wherein, in the (100-e)Li2S·e(F2)·f(G2) type solid electrolyte, 20≤e≤30, 0≤f≤50, and F2 includes B2S3, Al2S3, In2S3, SiS2, GeS2, SnS2, P2S5, As2S3, Sb2S5, Bi2S3, WS 2 and MoS2, G2 includes one or more of B2O3, Al2O3, In2O3, SiO2, GeO2, SnO2, P2O5, Sb2O5, Bi2O3, WO2, WO3, MoO2, MoO3, Fe2O3, ZnO, MgO, CuO, CaO, LiN, Li2O, LiF, LiCl, LiBr and LiI; the sodium ion solid electrolyte includes NASICON type sodium ion solid electrolyte, Na-β-Alumina type solid electrolyte, Na3PS4 type solid electrolyte, Na 11 Sn2PS 12 The potassium ion solid electrolyte includes one or more of a β-Alumina type potassium ion solid electrolyte, an anti-Perovskite type potassium ion solid electrolyte, a K2Fe4O7 type solid electrolyte and a KSi2P3 type solid electrolyte.
[0142] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder, the electrolyte and any other components are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry, wherein the positive electrode slurry has a solid content of 40wt%-80wt% and a viscosity at room temperature adjusted to 5000mPa·s-25000mPa·s, the positive electrode slurry is coated on both sides of the positive electrode current collector, and after drying, the positive electrode sheet is formed by cold rolling; the unit surface density of the positive electrode powder coated on one side is 150g / m 2 -350g / m 2 The compaction density of the positive electrode is 1.5g / cm 3 -3.6g / cm 3 , optional 2.5g / cm 3 -3.5g / cm 3 The calculation formula of the compacted density is:
[0143] Compaction density = coating surface density / (thickness of the electrode after extrusion - thickness of the current collector).
[0144] Negative electrode
[0145] The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer provided on at least one surface of the negative electrode current collector, wherein the negative electrode film layer includes a negative electrode active material.
[0146] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.
[0147] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material on a polymer material substrate. Among them, the metal material includes but is not limited to copper, copper alloys, nickel, nickel alloys, titanium, titanium alloys, silver and silver alloys, etc., and the polymer material substrate includes but is not limited to polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE) and other substrates.
[0148] In some embodiments, the negative electrode active material may adopt the negative electrode active material for batteries that is well known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, lithium metal and lithium alloys, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxides, silicon-carbon composites, silicon-nitrogen composites and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxides and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more. The weight ratio of the negative electrode active material in the negative electrode film layer is 70% by weight to 100% by weight, based on the total weight of the negative electrode film layer.
[0149] In some embodiments, the negative electrode film layer may further include a binder. The binder may be selected from at least one of nitrile rubber (NBR), polyvinylidene fluoride (PVDF), styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS). The weight ratio of the binder in the negative electrode film layer is 0-30% by weight, based on the total weight of the negative electrode film layer.
[0150] In some embodiments, the negative electrode film layer may further include a conductive agent. The conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. The weight ratio of the conductive agent in the negative electrode film layer is 0-20% by weight, based on the total weight of the negative electrode film layer.
[0151] In some embodiments, the negative electrode film layer may further include an electrolyte, which may be selected from a lithium ion solid electrolyte, a sodium ion solid electrolyte, and a potassium ion solid electrolyte.
[0152] Optionally, the lithium ion solid electrolyte includes a LISICON type solid electrolyte, a NASICON type lithium ion solid electrolyte, a Garnet type solid electrolyte, a LIPON type solid electrolyte, a Perovskite type solid electrolyte, an Anti-Perovskite type lithium ion solid electrolyte, a Thio-LiSICON type solid electrolyte, a Li 10 GeP2S 12 One or more of a (100-e)Li2S·e(F2)·f(G2) type solid electrolyte, a (100-e)Li2S·e(F2)·f(G2) type solid electrolyte, an Argyrodite type solid electrolyte, a Halide type solid electrolyte, and a Hydride type lithium ion solid electrolyte; wherein, in the (100-e)Li2S·e(F2)·f(G2) type solid electrolyte, 20≤e≤30, 0≤f≤50, and F2 includes B2S3, Al2S3, In2S3, SiS2, GeS2, SnS2, P2S5, As2S3, Sb2S5, Bi2S3, WS 2 and MoS2, G2 includes one or more of B2O3, Al2O3, In2O3, SiO2, GeO2, SnO2, P2O5, Sb2O5, Bi2O3, WO2, WO3, MoO2, MoO3, Fe2O3, ZnO, MgO, CuO, CaO, LiN, Li2O, LiF, LiCl, LiBr and LiI; the sodium ion solid electrolyte includes NASICON type sodium ion solid electrolyte, Na-β-Alumina type solid electrolyte, Na3PS4 type solid electrolyte, Na 11 Sn2PS 12 The potassium ion solid electrolyte includes one or more of a β-Alumina type potassium ion solid electrolyte, an anti-Perovskite type potassium ion solid electrolyte, a K2Fe4O7 type solid electrolyte and a KSi2P3 type solid electrolyte.
[0153] In some embodiments, the negative electrode film layer may further include other additives, such as thickeners. Thickeners may include, but are not limited to, sodium carboxymethyl cellulose (CMC-Na). The weight ratio of other additives in the negative electrode film layer is 0-15% by weight, based on the total weight of the negative electrode film layer.
[0154] In some embodiments, the negative electrode sheet can be prepared by the following method: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder, the electrolyte and any other components are dispersed in a solvent (such as deionized water) to form a negative electrode slurry, wherein the solid content of the negative electrode slurry is 30wt%-70wt%, and the viscosity at room temperature is adjusted to 2000mPa·s-10000mPa·s; the obtained negative electrode slurry is coated on both sides of the negative electrode current collector, and after a drying process, cold pressing, such as rolling, is performed to obtain a negative electrode sheet. The unit surface density of the negative electrode powder coated on one side is 5g / m 2 -220g / m 2 , the compaction density of the negative electrode is 1.2g / m 3 -2.0g / m 3 .
[0155] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the solid electrolyte membrane can be formed into an electrode assembly through a winding process or a lamination process.
[0156] In some embodiments, the all-solid-state battery may include an outer packaging that can be used to encapsulate the electrode assembly and the solid electrolyte membrane.
[0157] In some embodiments, the outer packaging of the all-solid-state battery can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. Alternatively, the outer packaging of the all-solid-state battery can be a soft shell, such as a pouch-type soft shell. The soft shell can be made of plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0158] The present application has no particular restrictions on the shape of the all-solid-state battery, which can be cylindrical, square, or any other shape. For example, FIG2 is an example of an all-solid-state battery 1 with a square structure.
[0159] In some embodiments, referring to FIG3 , the outer packaging may include a housing 11 and a cover 13 . The housing 11 may include a bottom plate and side plates connected to the bottom plate, which together form a receiving cavity. The housing 11 may have an opening communicating with the receiving cavity, and the cover 13 may be positioned over the opening to seal the receiving cavity.
[0160] The positive electrode sheet, the negative electrode sheet, and the solid electrolyte membrane can be wound or laminated to form an electrode assembly 12. The electrode assembly 12 is encapsulated in the housing. The number of electrode assemblies 12 included in the all-solid-state battery 1 can be one or more, and can be adjusted according to needs.
[0161] In some embodiments, all-solid-state batteries can be assembled into battery modules. The battery module can contain multiple all-solid-state batteries, and the specific number can be adjusted according to the application and capacity of the battery module.
[0162] In a battery module, multiple all-solid-state batteries can be arranged in sequence along the length of the battery module. Of course, they can also be arranged in any other manner. Furthermore, the multiple all-solid-state batteries can be fixed using fasteners.
[0163] Optionally, the battery module may further include a housing having a housing space, wherein the plurality of all-solid-state batteries are housed in the housing space.
[0164] In some embodiments, the battery modules described above may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.
[0165] A battery pack may include a battery box and multiple battery modules disposed within the box. The battery box comprises an upper case and a lower case. The upper case can be placed over the lower case to form an enclosed space for accommodating the battery modules. The multiple battery modules can be arranged in any manner within the battery box.
[0166] Electrical devices
[0167] The present application also provides an electrical device, comprising at least one of the aforementioned all-solid-state battery, battery module, or battery pack. The all-solid-state battery, battery module, or battery pack can be used as a power source for the device, or as an energy storage unit for the device. The device may be, but is not limited to, a mobile device, an electric vehicle, an electric train, a ship, a satellite, an energy storage system, etc.; wherein the mobile device may include, but is not limited to, at least one of a mobile phone and a laptop computer; and the electric vehicle may include, but is not limited to, at least one of a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.
[0168] The device can select a secondary battery, a battery module or a battery pack according to its usage requirements.
[0169] Figure 4 shows an example of an electric device 2. The electric device 2 is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the device's requirements for high power and high energy density of secondary batteries, a battery pack or battery module can be used.
[0170] Another example device may be a mobile phone, a tablet computer, a laptop computer, etc. Such a device is usually required to be lightweight and thin, and may use an all-solid-state battery as a power source.
[0171] The beneficial effects of the present application are further illustrated below with reference to the examples.
[0172] In order to make the technical problems, technical solutions and beneficial effects solved by this application clearer, the following will be further described in detail with reference to the embodiments and drawings. Obviously, the described embodiments are only a part of the embodiments of this application, rather than all the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is in no way intended to limit this application and its applications. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0173] If no specific techniques or conditions are specified in the examples, the experiments were carried out according to the techniques or conditions described in the literature in the field or according to the product instructions. All reagents or instruments used without specifying the manufacturer are commercially available conventional products.
[0174] 1. Preparation of solid electrolyte membrane
[0175] Example 1
[0176] Silicon carbide powder (as the ceramic fiber material) and Li6PS5Cl powder (as the solid electrolyte) were weighed and dry-mixed to prepare a mixture. The mixture was then pressed into a sheet using a die and a mechanical flat press to produce a solid electrolyte membrane. The dry-mixing time was 0.5 hours and the pressure was 500 MPa.
[0177] Example 2-23
[0178] The preparation method of the solid electrolyte membrane in Example 2-23 is basically the same as the preparation method of the solid electrolyte membrane in Example 1, and the main difference is: one or more of the type of ceramic fiber material, the diameter of the ceramic fiber material, the aspect ratio of the ceramic fiber material, the volume proportion of the ceramic fiber material in the solid electrolyte membrane, the type of solid electrolyte, the distribution uniformity of the ceramic fiber material in the solid electrolyte membrane, the dry mixing time, and the pressure of the pressurization treatment are different; for details of Example 2-15, please see Table 1-1, and for details of Examples 16-23, please see Table 1-2.
[0179] Example 24
[0180] Weigh silicon carbide (as ceramic fiber material) powder and Li7La3Zr2O 12Silicon carbide powder (as a solid electrolyte) was added to Li6PS5Cl powder, followed by wet mixing with p-xylene (as a solvent) and nitrile rubber (as a binder) to prepare a mixture. The mixture was coated to form a continuous electrolyte film and dried to produce a solid electrolyte membrane. The wet mixing time was 3 hours. See Table 1-2 for details.
[0181] Example 25
[0182] The preparation method of the solid electrolyte membrane in Example 25 is basically the same as the preparation method of the solid electrolyte membrane in Example 24. The main differences are: one or more of the type of ceramic fiber material, the diameter of the ceramic fiber material, the aspect ratio of the ceramic fiber material, the volume proportion of the ceramic fiber material in the solid electrolyte membrane, the type of solid electrolyte, the distribution uniformity of the ceramic fiber material in the solid electrolyte membrane, the wet mixing time, the type of binder, and the mass proportion of the binder in the solid electrolyte membrane. See Table 1-2 for details.
[0183] Comparative Example 1
[0184] In Comparative Example 1, no ceramic fiber material was added, and only Li6PS5Cl powder (as a solid electrolyte) was used. The mixture was pressed into a sheet by a mold under mechanical flat pressing to produce a solid electrolyte membrane. See Table 1-2 for details.
[0185] Comparative Example 2
[0186] The preparation method of the solid electrolyte membrane in Comparative Example 2 is substantially the same as that in Example 2, except that the length and aspect ratio of the ceramic fiber material are different. See Table 1-2 for details.
[0187] [Corrected 28.10.2024 in accordance with Rule 26] Table 1-1
[0188] [Corrected 28.10.2024 in accordance with Rule 26] Table 1-2
[0189] Wherein, D represents the diameter of the ceramic fiber material, L represents the length of the ceramic fiber material, n1 represents the volume ratio of the ceramic fiber material to the solid electrolyte, A0 represents the distribution uniformity of the ceramic fiber material in the solid electrolyte, n2 represents the mass ratio of the binder to the solid electrolyte, and NBR represents styrene-butadiene rubber.
[0190] It should be noted that the diameter and length of the ceramic fiber material mentioned above are measured by the following method: a uniformly broken cross-section of the solid electrolyte membrane is prepared by an ultrasonic knife and observed by a scanning electron microscope. In the backscattered electron imaging mode of the scanning electron microscope, the ceramic fiber material is distinguished by the contrast of the material, and the length and diameter of the ceramic fiber material are measured.
[0191] The volume ratio of the above-mentioned ceramic fiber material and solid electrolyte is measured by the following method: an electrolyte original sheet with a diameter of 10 mm is prepared by an ultrasonic knife or a slicing mold, and observed by a high-resolution X-ray tomography scanner. In the high-resolution X-ray tomography results, the ceramic fiber material and the solid electrolyte material can be distinguished by the grayscale based on the electron density of the material within the pixel, thereby confirming the mentioned proportion of ceramic fiber material in the solid electrolyte membrane / sheet.
[0192] The distribution uniformity of the ceramic fiber material mentioned above in the solid electrolyte is measured by the following method: take the solid electrolyte membrane, and prepare the cross section of the ceramic fiber material and the solid electrolyte by ultrasonic knife method, observe it by scanning electron microscope, and distinguish the ceramic fiber material from the solid electrolyte according to the contrast of the material in the backscattered electron imaging mode of the scanning electron microscope, and then calculate the distribution uniformity based on the image measurement. Based on the scanning electron microscope image, the distance d between the cross sections of the ceramic fiber material is measured by line analysis method. i (i=1,2,3,…..N), by d i Find the standard deviation σ between N distances d :
[0193] Among them, A0 represents the distribution uniformity of ceramic fiber material in solid electrolyte, It represents the average value of the distance between N ceramic fiber material sections.
[0194] The thickness of the solid electrolyte membrane mentioned above is measured by the following method: first calibrate the micrometer, then place the solid electrolyte membrane between the double anvils, gently rotate the sleeve until a sound is heard, and read and record the thickness of the solid electrolyte membrane.
[0195] 2. Solid electrolyte membrane performance measurement
[0196] 1. Critical current density
[0197] At 25°C, two 8mm dendrites and 50μm thick lithium metal discs were placed at the center of the solid electrolyte membrane on both sides. Mechanical pressure was used to make the lithium metal discs and the solid electrolyte membrane tightly fit together to form a lithium / solid electrolyte membrane / lithium symmetrical battery. After the symmetrical battery was assembled and packaged, the lithium / solid electrolyte membrane / lithium symmetrical battery was made to have a flow rate of 0.25mA / cm 2 Initially, 1 mAh / cm was deposited and stripped on one side. 2 After lithium, the current was increased to 0.5 mA / cm 2 , maintain 1mAh / cm 2 After the surface capacity deposition and stripping, the 2 The gradient is 0.75 mA / cm 2 , 1.0mA / cm 2 , 1.25mA / cm 2 ...to 10mA / cm 2 The current density at which the voltage suddenly drops sharply is recorded as the critical current density.
[0198] 2. Fracture toughness
[0199] In an argon atmosphere, the surface of the solid electrolyte membrane is polished with sandpaper from 800 mesh, to 2000 mesh, to 4000 mesh, to 8000 mesh, until the surface of the solid electrolyte membrane presents mirror properties without obvious defects; then, the polished surface is subjected to an indentation test using a Vickers cone indentation tester; the indentation tester is driven with an appropriate load until radial cracks appear at the four corners of the cone indentation; according to the indentation load S, the extension length L of the radial crack, and the microhardness H V The fracture toughness value K can be calculated by the following formula IC :
[0200] Here, E represents the Young's modulus of the solid electrolyte membrane.
[0201] 3. Ionic conductivity
[0202] At 25°C, a 10 mm diameter cylindrical stainless steel current collector was used to clamp the solid electrolyte membrane tightly under mechanical pressure in a battery mold. The current collector was then connected to an electrochemical workstation and operated at a bias voltage of 10 mV and a frequency of 10 6 The electrochemical impedance spectroscopy (EIS) test of the solid electrolyte membrane was performed in the range of 0.1 Hz to 0.1 Hz. The Z' coordinate value of the point closest to the Z' axis from right to left in the low-frequency band of the EIS curve was used as the resistance value R, and the ionic conductivity σ was calculated using the following formula:
[0203] Wherein, D is the thickness of the solid electrolyte membrane, and A is the contact area between the solid electrolyte membrane and the current collector.
[0204] The test results of the critical current density, fracture toughness and ionic conductivity of the solid electrolyte membranes in the above embodiments and comparative examples are shown in Table 2.
[0205] 3. Preparation of all-solid-state batteries
[0206] 1. Preparation of positive electrode sheet
[0207] NCM811 (as the positive electrode active material), nitrile rubber (NBR, as a binder), VGCF (as a conductive agent) and Li6PS5Cl (as an electrolyte) are mixed in a mass ratio of 80:1.5:0.5:18, and p-xylene is added and stirred to form a uniformly dispersed slurry; the slurry is evenly coated on one surface of the aluminum foil, and then transferred to a vacuum drying oven for complete drying; the obtained electrode is rolled and then punched to obtain the positive electrode.
[0208] 2. Preparation of negative electrode sheet
[0209] In Examples 1-11, Examples 16-23, and Comparative Examples 1-2, lithium metal is used as the negative electrode active material, and the preparation method of the negative electrode sheet is as follows:
[0210] The lithium metal foil is rolled and thinned to a thickness of 50 μm, and the lithium metal foil is covered on one surface of the copper foil by rolling again, and then cut to obtain a negative electrode sheet.
[0211] In Examples 12-15 and 24-25, artificial graphite is used as the negative electrode active material, and the preparation method of the negative electrode sheet is as follows:
[0212] Artificial graphite (as the negative electrode active material), conductive carbon black (as the conductive agent), styrene-butadiene rubber (as the binder), and Li6PS5Cl (as the electrolyte) were mixed in a mass ratio of 70:2:2:26. Deionized water was then added and stirred to form a negative electrode slurry. The negative electrode slurry was evenly coated on one side of the copper foil, dried, cold pressed, and slit to produce the negative electrode sheet.
[0213] 3. Solid electrolyte membrane
[0214] The solid electrolyte membranes prepared in the above-mentioned embodiments and comparative examples were respectively used.
[0215] 4. All-solid-state battery performance test
[0216] 1. A cross section of the solid electrolyte membrane in Example 2 was scanned using a scanning electron microscope, as shown in Figure 1. As shown in Figure 1, the ceramic fiber material 111 is uniformly distributed in the solid electrolyte 112.
[0217] 2. Maximum charging current density
[0218] As an example, the maximum charging current density of the all-solid-state battery mentioned above can be measured by cycling the current density in a step-by-step manner until failure: at 25°C, after the all-solid-state battery is assembled and packaged, the full battery is charged from 0.25 mA / cm 2 At the beginning, charge and discharge were performed separately, and the capacity was controlled at 1 mAh / cm 2 To ensure constant test surface capacity during the cycle test, increase the current to 0.5 mA / cm after completing the first cycle. 2 , maintain 1mAh / cm 2 After the surface capacity is charged and discharged for a cycle, the 2 The gradient is 0.75 mA / cm 2 , 1.0mA / cm 2 , 1.25mA / cm 2 ...to 10mA / cm 2 Perform all-solid-state battery cycling and record the current density at which the voltage suddenly drops sharply or exhibits obvious jitter as the maximum charging current density.
[0219] The performance test results of the above embodiments and comparative examples are shown in Table 2 below.
[0220] [Corrected 28.10.2024 in accordance with Rule 26] Table 2
[0221] It can be seen from the results of Examples 1-25 and Comparative Example 1 in Table 2 that by distributing ceramic fiber materials in the solid electrolyte, the fracture toughness and mechanical strength of the solid electrolyte membrane can be improved while ensuring the ionic conductivity of the solid electrolyte. At the same time, the critical current density of the solid electrolyte membrane can be significantly improved, thereby enhancing the fast charging capability of the all-solid-state secondary battery.
[0222] The difference between Example 1 and Example 2 lies in the different mixing times during dry preparation, resulting in different distribution uniformity of the ceramic fiber material in the solid electrolyte. Compared with Example 2, the critical current density and fracture toughness of the solid electrolyte membrane in Example 1, as well as the maximum charge current density of the all-solid-state battery, are all reduced. This indicates that the uniform distribution of the ceramic fiber material in the solid electrolyte helps improve the fracture toughness and mechanical strength of the solid electrolyte, inhibits the fragmentation of the solid electrolyte due to lithium metal deposition stress, and significantly increases the critical current density of the solid electrolyte membrane.
[0223] The main difference between Examples 2-11 lies in the different volume ratios of the ceramic fiber material to the solid electrolyte. The volume ratio of the ceramic fiber material to the solid electrolyte is the smallest in Example 10, while the volume ratio of the ceramic fiber material to the solid electrolyte is the largest in Example 11. Compared with Example 2-9, the fracture toughness of the solid electrolyte membrane in Example 10 is reduced, and the critical current density and ionic conductivity in Example 11 are both reduced. It is speculated that this may be because when the amount of ceramic fiber material added is too small, it cannot effectively improve the mechanical properties and fracture toughness of the solid electrolyte. When the amount of ceramic fiber material added is too large, it may occupy too much volume of the solid electrolyte, reducing the distribution uniformity of the solid electrolyte bulk and interface ion transport channels, thereby inducing local current density hotspots and reducing the critical current density of the solid electrolyte.
[0224] The main difference between Example 2, Examples 16-23 and Comparative Example 2 is that the ratio of the length to the diameter of the ceramic fiber material is different; from the results of Example 2, Examples 16-23 and Comparative Example 2, it can be seen that when the aspect ratio of the ceramic fiber material is ≥2, the fracture toughness and critical current density of the solid electrolyte membrane can be improved, and the fast charging capability of the all-solid-state battery can be improved.
[0225] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0226] The above-described embodiments merely represent several implementation methods of the present application. While the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the patent application. It should be noted that a person of ordinary skill in the art may make various modifications and improvements without departing from the spirit of the present application, and these modifications and improvements fall within the scope of protection of the present application. Therefore, the scope of protection of the present patent application shall be determined by the appended claims.
Claims
1. A solid electrolyte membrane, comprising a solid electrolyte and a ceramic fiber material dispersed in the solid electrolyte; The solid electrolyte includes an inorganic solid electrolyte; The diameter of the ceramic fiber material is denoted as D, and the length of the ceramic fiber material is denoted as L. The diameter of the ceramic fiber material and the length of the ceramic fiber material satisfy: L / D≥2. 2 . The solid electrolyte membrane as claimed in claim 1 , wherein the diameter of the ceramic fiber material and the length of the ceramic fiber material satisfy: L / D ≥ 20; optionally 20 ≤ L / D ≤ 500.
3. The solid electrolyte membrane according to any one of claims 1 to 2, wherein the diameter of the ceramic fiber material satisfies: D≤5 μm; optionally 0.5 μm≤D≤2 μm. 4 . The solid electrolyte membrane according to claim 1 , wherein the length of the ceramic fiber material satisfies: 1 μm ≤ L ≤ 500 μm; optionally 10 μm ≤ L ≤ 200 μm.
5. The solid electrolyte membrane according to any one of claims 1 to 4, wherein the ceramic fiber material comprises one or more of silicon carbide fiber, silicon nitride fiber, boron nitride fiber, alumina fiber and silica fiber.
6. The solid electrolyte membrane according to any one of claims 1 to 5, wherein the ceramic fiber material has at least one of the following (1)-(2) characteristics: (1) The volume ratio of the ceramic fiber material to the solid electrolyte is (0.01-40):100; optionally (3-7):100; (2) The mass ratio of the ceramic fiber material to the solid electrolyte is (0.01-85):100; or can be (2-15):
100.
7. The solid electrolyte membrane according to any one of claims 1 to 6, wherein the distribution uniformity of the ceramic fiber material in the solid electrolyte is ≤0.3; Optionally, the distribution uniformity of the ceramic fiber material in the solid electrolyte is ≤0.
1.
8. The solid electrolyte membrane according to any one of claims 1 to 7, wherein a binder is also distributed in the solid electrolyte; Optionally, the binder includes one or more of nitrile rubber, polyvinylidene fluoride, polytetrafluoroethylene, polyacrylic acid, polyvinyl alcohol, polyimide, polyacrylonitrile, polyurethane, polycarboxymethyl cellulose, cyclodextrin, sodium alginate, polysaccharide, nitrile rubber and styrene-butadiene rubber; Optionally, the mass ratio of the binder to the solid electrolyte is (0.01-20):100; optionally, it is (0.5-5):
100.
9. The solid electrolyte membrane according to any one of claims 1 to 8, wherein the solid electrolyte membrane has at least one of the following features (1) to (4): (1) The critical current density of the solid electrolyte membrane at 25°C is 0.5 mA / cm 2 -10mA / cm 2 ; (2) The fracture toughness of the solid electrolyte membrane is 0.05MPa m^(1 / 2)-2MPa m^(1 / 2); (3) The ionic conductivity of the solid electrolyte membrane at 25°C is 0.1 mS / cm 2 -10mS / cm 2 ; (4) The thickness of the solid electrolyte membrane is 1 μm-1000 μm.
10. A method for preparing a solid electrolyte membrane according to any one of claims 1 to 99, comprising the following steps: Mixing the ceramic fiber material and the solid electrolyte to prepare a mixture; The mixed material is subjected to molding treatment to prepare the solid electrolyte membrane.
11. The method for preparing a solid electrolyte membrane according to claim 10, wherein the ceramic fiber material and the solid electrolyte are mixed by dry mixing; Optionally, the mixing time is 1 h-24 h. 12 . The method for preparing a solid electrolyte membrane according to claim 11 , wherein the molding process is a pressurization process; optionally, the pressure of the pressurization process is 200 MPa-600 MPa.
13. The method for preparing a solid electrolyte membrane according to claim 10, wherein the ceramic fiber material and the solid electrolyte are mixed by wet mixing; Optionally, the mixing time is 0.5h-12h. 14 . The method for preparing a solid electrolyte membrane according to claim 13 , wherein the molding process comprises coating the mixed material into a film and then drying it.
15. An all-solid-state battery comprising the solid electrolyte membrane according to any one of claims 1 to 9.
16. An electrical device comprising the all-solid-state battery according to claim 15.
Citation Information
Cited By
Sulfide solid electrolyte, preparation method thereof, battery and application
CN120767395A