Process for producing iron chloride from iron phosphate compounds
The process recycles iron from spent lithium iron phosphate and manganese phosphate battery materials by reacting them with alkali or alkaline earth metal chlorides, efficiently producing iron chlorides and a usable residue, addressing the need for alternative iron sources and promoting sustainable battery material reuse.
Patent Information
- Application Number
- PCT/EP2024/057840
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-22
- Publication Date
- 2024-10-03
AI Technical Summary
Current methods for producing iron chlorides primarily start from metallic iron, overlooking iron-containing compounds like lithium iron phosphate (LFP) and lithium iron manganese phosphate (LFMP) after their life cycle, which are attractive sources for iron raw materials due to recycling needs.
A process involving iron phosphate compounds with alkali or alkaline earth metal chlorides at 200-1100°C in an inert gas atmosphere, where iron chloride is derived and isolated from the exhaust gas stream, utilizing a material composition that includes LFP and LFMP with specific elemental proportions and particle sizes, and using a reactor system for efficient separation.
This process effectively recycles iron from spent battery materials, producing high-purity iron chlorides that can be reused in battery production or converted into other forms like iron oxides, while also generating a lithium-depleted residue suitable for agricultural use.
Smart Images

Figure 000001 
Figure 000002 
Figure 000003
Abstract
Description
[0001] P001 01205-A
[0002] Process for the production of iron chloride from iron phosphate compounds
[0003] The invention relates to a process for producing iron chloride from material containing iron phosphate compounds.
[0004] The production of iron chlorides such as Fe(II)Cl2 and Fe(III)Ch usually starts from metallic iron. However, there are increasingly large-volume iron-containing compounds that have not previously been considered as alternative sources for the production of iron chlorides. Examples include lithium iron phosphate (LFP) and lithium iron manganese phosphate (LFMP), as well as their modifications, which may be doped with other elements, particularly metals, which are used as cathode materials – also known as cathode active materials (CAM) – for batteries. These require recycling after their life cycle, making them an attractive source of iron raw materials.
[0005] Synthetic iron phosphate compounds such as LFP and LFMP therefore have in common that they contain iron phosphate compounds, which offer further access to the production of iron chlorides.
[0006] The object of the invention was therefore to provide a corresponding process starting from iron phosphate compounds.
[0007] Surprisingly, a process for the preparation of iron chlorides has now been found, which is characterized in that i) a material containing at least one iron phosphate compound is reacted with at least one alkali metal chloride and / or at least one alkaline earth metal chloride at a temperature of 200 to 1100°C, in an inert gas atmosphere, preferably containing less than 200 ppm, in particular less than 100 ppm of oxygen, and ii) the iron chloride formed is discharged and isolated in the exhaust gas stream.
[0008] Iron phosphate compounds
[0009] Examples of iron phosphate compounds include iron phosphates, in particular iron(II) phosphate, iron(III) phosphate and iron(III) pyrophosphatase, lithium iron phosphates (LFP) such as triphyline or lithium iron manganese phosphates (LFMP), which together have the general formula LiFe(II). X )Mn x PO4, where 0s=x<0.9 is possible. The iron phosphates can be present in anhydrous form or as hydrous iron phosphates, the latter being, for example, vivianite, which can generally be described by the formula FesPO^StW, metavivianite, which can generally be described by the formula Fe2(PO4)2(OH)2'6H2O, strengite, which can generally be described by the formula Fe(PO4)2H2O, kryzhanovskite, which can generally be described by the formula Fe3(OH)s(PO4)2 and phosphoferrite, which can generally be described by the formula Fe3(H2O)s(PO4)2.
[0010] These iron phosphate compounds can of course also be used in any mixtures.
[0011] Preferred iron phosphate compounds are LFP and / or LFMP with the general common formula LiFe(i. X )Mn x PO4, where 0=£x<0.9, in particular 0=£x<0.6.
[0012] material
[0013] The material containing at least one iron phosphate compound can consist of 100% iron phosphate compounds, but usually only contains them in a proportionate amount. The material used preferably contains the iron phosphate compounds in a total amount of 1 to 40 wt.%, preferably 1 to 15 wt.%.
[0014] The material used contains at least one iron phosphate compound selected from the group consisting of iron phosphates, in particular iron(II) phosphate, iron(III) phosphate and iron(III) pyrophosphate, lithium iron phosphate (LFP), lithium iron manganese phosphate (LFMP), in particular LFP and / or LFMP with the general common formula LiFe(II). X )Mn x PO4, where 0 s = x < 0.9, in particular 0 s = x < 0.6, or mixtures thereof.
[0015] A material containing LFP and / or LFMP is preferred. As such, a material containing a proportion of 5 to 100 wt. %, preferably 40 to 99 wt. %, in particular 50 to 99 wt. %, particularly preferably 70 to 99 wt. % of LFP and / or LFMP is used for the process according to the invention.
[0016] Preferably, the description of the composition of the material used is also possible by determining the weight proportion of certain elements in the material used, preferably containing LFP and / or LFMP, in each case based on the amount of material, wherein the material used preferably contains:
[0017] 1 to 36 wt.% Fe, of which preferably 2 to 100 wt.% as iron phosphate compound
[0018] 1 to 20 wt% P, 0 to 35 wt% Mn,
[0019] 1 to 8 wt% Li and
[0020] 1 to 55 wt.%, preferably 1 to 40 wt.%, in particular 1 to 30 wt.% carbon.
[0021] These elemental quantities can be derived from the LFP, the LFMP, or from other components of the material used, such as residual metallic components. The elemental content is preferably determined using classical methods for elemental analysis. The type and quantity of the iron phosphate compound present is preferably determined using the X-ray scattering (XRD) method on a powder in reflection using a Cu-K a Radiation is determined. The resulting reflections are compared with data from, for example, the ICDD (International Centre for Diffraction Data), and the resulting iron phosphate-containing phases are assigned. For lithium iron phosphate, the reflections from JCPDS (International Centre for Powder Diffraction Data Sample) card #83-2092 are used for comparison.
[0022] The material used preferably further contains 1 to 55 wt.%, preferably 1 to 40 wt.%, in particular 1 to 30 wt.% of carbon, in particular graphite and / or carbon black.
[0023] Preferably, the sum of LFP and / or LFMP and carbon in the preferably LFP and / or LFMP-containing material used is more than 70 wt.%, preferably more than 80 wt.%, particularly preferably more than 90 wt.%.
[0024] Typically, the LFP and / or LFPM-containing battery cells are mechanically disassembled as far as possible, and the residue, containing the cathode and anode material, possibly binders, and other components, is crushed into a mass that is black due to the dark LFP / LFMP and the graphite-containing anode material and is therefore called "black mass." Due to incomplete technical separation, the black mass may also contain residues of other battery components, such as metals.
[0025] The material can therefore also be the so-called black mass, with a proportion of iron phosphate compounds of 5 to 90 wt.%.
[0026] The material used may also contain metals, preferably from 0 to 15 wt.%, preferably 0 to 5 wt.%, in particular Al, Cu, Co and Ni may be contained.
[0027] The aluminum content, determined as elemental aluminum, of the material used is preferably less than 10 wt.%, in particular less than 5 wt.%.
[0028] It is preferred that the material used contains less than 10 wt.%, in particular less than 1 wt.%, particularly preferably less than 0.1 wt.% of polymer particles, in particular plastics such as polyethylene and / or polypropylene. It is also preferred if the material used contains less than 5 wt.% of PVDF (polyvinylidene fluoride) and / or other binders such as carboxymethylcellulose or alginates. The content of all binders is preferably less than 5 wt.%.
[0029] The VOC content of the material used is preferably less than 1 wt.%, in particular less than 0.1 wt.%, particularly preferably less than 0.01 wt.%. VOCs (volatile organic compounds) are preferably understood to mean organic compounds with boiling points in the range of 50 to 260°C at a standard pressure of 101.3 kPa.
[0030] The preferred material containing LFP and / or LFMP is black mass from battery shredding.
[0031] The material used preferably has an average particle size of 0.1 μm to 10 mm. Depending on the size, the particle size can be easily determined by sieving or, for smaller particles, by laser diffraction or laser scattering. The most suitable method for each case is known to those skilled in the art.
[0032] The material used, which preferably contains LFP and / or LFMP, can also be a coated material. Carbon, especially graphite, and metal oxides are preferred coating materials.
[0033] Alkali chlorides
[0034] Preferred alkali chlorides are NaCl, KCl, LiCl, and mixtures thereof. NaCl or KCl, or a mixture of NaCl and KCl, is preferred. If NaCl is used in a mixture with other alkali chlorides, especially with KCl, the mixing weight ratio is preferably from 10:1 to 0.1:1, in particular from 5:1 to 0.5:1.
[0035] Alkali chloride is preferably used in an amount of 1 to 5 mol, based on 1 mol of iron present - determined by elemental analysis.
[0036] Alkaline earth chlorides
[0037] Suitable alkaline earth chlorides include MgCl, CaCh, or mixtures thereof. MgCh is preferred.
[0038] Preferably, a mixture of alkaline earth metal chlorides and alkali metal chlorides, in particular MgCh and NaCl and / or KCl, is used in a weight ratio of 4:1 to 0.25:1, in particular of 2:1 to 1:2. Particularly preferably, a mixture of KCl, NaCl and MgCh is used.
[0039] Also particularly preferred is a mixture of MgCh and KCl with a weight ratio of 3 : 1 to 0.5 : 1.
[0040] Miscellaneous
[0041] Particularly preferred is a molar ratio of chlorine from the alkali metal chlorides and alkaline earth chlorides used to phosphate groups contained in the material in the range from 1:1 to 4:1, preferably from 2.3:1 to 3.5:1 mol / mol.
[0042] Proceedings
[0043] The feedstocks, the material, and the alkali metal chloride and / or alkaline earth metal chloride to be used are preferably mixed in dry form in a mixer. A paddle mixer or mills, such as a ball mill, are preferred. The latter have the advantage of achieving better homogenization of the reactants through comminution.
[0044] It is advantageous to carry out the mixing step of the reactants in an inert gas atmosphere, preferably anhydrous, in order to protect the possibly contained hygroscopic components from water absorption, which could have a detrimental effect on the process yield.
[0045] The reaction itself also preferably takes place in the absence of air and water. Preferred inert gases include nitrogen, argon, or carbon dioxide. The inert gas atmosphere preferably contains less than 200 ppm, especially less than 100 ppm, of oxygen.
[0046] The conversion of the iron phosphate compounds can then take place in a fluidized bed, packed bed, or moving bed reactor, in a shaft furnace, or in a preferably gas-tight furnace, which is most easily designed as an indirectly heated tube furnace or rotary kiln. Optionally, the material can also be shaped before being introduced into a furnace, for example by briquetting, extruding, or pelletizing, with subsequent thermal pretreatment at 100 to 199°C if necessary. Auxiliary agents such as layered silicates, particularly bentonites, as well as ligninsulfonate, methylcellulose, waterglass, starch, or others can be used for this purpose. The products formed during the reaction, which are volatile at the reaction temperature, here primarily iron chloride, but also aluminum chlorides and possiblyother heavy metal chlorides are preferably resublimated and collected together in a cold place at temperatures below 150°C or resublimated and collected separately in different cool places.
[0047] Preferred deposition temperatures for FeCh are less than or equal to 700°C, preferably less than or equal to 600°C. In the case of iron(III) chloride, the resublimation temperature can also be less than 307°C.
[0048] Iron(III) chloride and also AlCh, if the material used contains aluminum, can be separated from the exhaust stream and separated from each other, preferably by resublimation on surfaces of different temperatures. If iron(III) chloride is present in the exhaust stream together with AlCh, the respective chlorides can also be fractionally resublimated on different surfaces at different temperatures due to their sufficiently different boiling points, thus allowing them to be separated very cleanly.
[0049] Preferred deposition temperatures for FeCh are less than 700°C, in particular less than 699°C to 307°C, for FeCh less than 307°C, in particular 150°C to 300°C and for AlC less than 150°C, in particular 110°C to 149°C.
[0050] The iron recovered according to the invention in the form of iron(I) chloride and / or iron(II) chloride is already very pure and can be converted into the desired raw material form of iron, for example, for the re-production of LFP and / or LFMP. Examples include iron sulfate, iron nitrate, iron phosphate, or various forms of iron oxide.
[0051] Alternatively, the iron chloride can be introduced directly as a gas stream into an aqueous medium containing sulfuric acid, nitric acid, or phosphoric acid, even without being separated by resublimation, thereby resulting in the formation of the corresponding iron(II) sulfates, nitrates, or phosphates. If necessary, a suitable reducing agent is used in the reaction to obtain iron(II) sulfate, iron(II) nitrate, or iron(II) phosphate.
[0052] However, the preferred method is to separate ferric chloride from the exhaust stream by resublimation. The exhaust stream contains gaseous ferric chloride, such as ferric chloride or ferrous chloride, and possibly also AlCl, if the material used contains aluminum, as well as NaCl and volatile chlorides of other metals, if these metals were present in the black mass.
[0053] The residue after the reaction preferably contains phosphates of the alkali and / or alkaline earth metal group used.
[0054] The lithium ions contained in the residue can be extracted by shaking the dry residue with a suitable non-aqueous solvent. Suitable solvents include alcohols, esters or ethers, ketones or nitriles, or mixtures thereof, optionally also in mixtures with water.
[0055] The residue obtained after extraction, which is preferably lithium-depleted or lithium-free, is preferably treated by adding 0.1 to 5 mol of phosphoric acid per mole of phosphate, preferably 0.2 to 1 mol of phosphoric acid per mole of phosphate, to the residue. The reaction residue can thus be converted into a soluble form, making it suitable for use in agriculture.
[0056] Carbon, if present in the material used, remains as the insoluble residue. The remaining water-soluble components can then be separated and isolated from one another in the form of their sulfides, chlorides, phosphates, fluorides, or other precipitated compounds, if necessary after determining their possible existence using the classic F^S separation process.
[0057] temperature
[0058] The reaction preferably takes place at a temperature of 400 to 900°C. The reaction typically lasts 5 minutes to 10 hours, preferably 2 to 5 hours.
[0059] If the material used has a binder content of greater than 1 wt.%, based on the material, it is preferably dissolved out by treatment with an organic solvent, in particular acetone, ethyl acetate, methyl ethyl ketone, tetrahydrofuran (THF), acetoacetic ester, acetylacetone, dioxane and / or acetic anhydride and mixtures thereof, in order to reduce the content to less than 0.1 wt.%.
[0060] If the material contains a polymer content, particularly plastic, of greater than 1 wt.%, it is advantageous to first subject the material to a thermal treatment at a temperature of 300°C to 600°C, preferably under an inert gas atmosphere, in order to reduce the polymer content to less than 0.1 wt.%. A possible binder content of greater than 1 wt.% can be reduced to less than 0.1 wt.% by leaching with organic solvents, alternatively or additionally by a thermal treatment at a temperature of 300°C to 700°C, preferably under an inert gas atmosphere.
[0061] reactor
[0062] The material to be used in the process according to the invention is preferably introduced into a reactor, which is preferably provided with a layer resistant to the reaction conditions to be established. Preferred reactor materials are nickel- or graphite-coated reactors. Tubular reactors such as rotary tube reactors or other reactors can be used as such. Particular preference is given to reactors that allow movement of the material during the reaction. Fluidized-bed reactors, rotary tube reactors, or a reaction in an extruder device with screw propulsion are preferred.
[0063] In the case of a tubular reactor, the reactor length is preferably 0.2 to 40 m. The residence time in the reactor during the reaction generally depends on the temperature. The residence time in the reactor can range, for example, from one minute to five hours. The process according to the invention can be operated as a batch or continuously.
[0064] Preferably, the reactor has an outlet for the exhaust stream. The exhaust stream contains the gaseous reaction products and volatile components of the material, which can be discharged together from the reaction chamber. The possible separation of solid components such as particulate matter from gaseous components in the exhaust stream can be achieved, for example, using devices such as a cyclone.
[0065] The reaction is preferably completed when the iron content in the residue has reached less than 0.05 wt.%.
[0066] Preferred deposition temperatures for FeCh are less than 700°C, FeC less than or equal to 307°C, in particular 150°C to 300°C, and for AlC less than or equal to 150°C, in particular 110°C to 149°C. The poorly soluble manganese sulfide remaining after a H2S separation process can be converted to manganese sulfate with air and thus recovered and, if necessary, reused for the production of LFMP.
[0067] Examples
[0068] Analytics
[0069] After dissolving the LFF sample LFP or the sublimate with suitable acids, the analysis was carried out in an ICP-OES, after calibration for the respective element using standard solutions.
[0070] X-ray diffraction patterns (XRD) were recorded on powders (flat preparation) between 2Theta angles of 0 and 60° with a wavelength of 0.154 nm.
[0071] Example 1 : LFP NaCI / MgCh
[0072] 5.02 g of lithium iron phosphate (31.7 mmol of phosphate) (lithium iron phosphate, the structure was confirmed by XRD; apart from lithium iron phosphate, no further reflections were detected), with the following analytical data (in percent by weight): Fe 34.6%, phosphate 60.9%, Li 4.6%, C: 1.8%, with an average particle size distribution d10 0.35|jm, d50 0.62|jm, d100 6.7|jm, is thoroughly mixed with 1.83 g of NaCl (31.3 mmol of chloride) and 2.24 g of anhydrous MgCh (47 mmol of chloride), homogenized and placed in a quartz glass tube (diameter: 120 mm) which is located in a tube furnace.
[0073] A stream of dry nitrogen (0.3 liters per minute; oxygen content < 100 ppm v / v) is passed through the reactor, heated to 750°C, and held at that temperature for six hours. A brown precipitate (1.17 g) separates at approximately 160°C on the cooler quartz tube protruding from the furnace. The precipitate consists of 82 wt.% of a mixture of iron(II) chloride and iron(III) chloride, and 15 wt.% of NaCl. The NaCl content can be reduced by lowering the reaction temperature.
[0074] The weight loss of the sample is 34 wt%. The residue contains significantly less iron than the reactant and is therefore lighter in color.
[0075] The residue is taken up with 50 ml of anhydrous ethanol and then filtered. The procedure is repeated twice. The filtrates are combined, and the ethanol is evaporated. The remaining mass contains the lithium compounds.
[0076] The residue remaining after ethanol extraction was first dried and then triturated with concentrated phosphoric acid. The resulting soluble phosphate has a very low iron content and can therefore be used for plant fertilization. Example 2: LFP KCl / MgCh
[0077] 5g lithium iron phosphate (31.7 mmol phosphate) (lithium iron phosphate, the structure was confirmed by XRD, apart from lithium iron phosphate no further reflections were detected), with the following analytical data (in percent by weight): Fe 34.6%, phosphate 60.9%, Li 4.6%, C: 1.8%, with an average particle size distribution d10 0.35pm, d50 0.62pm, d1006.7pm, is thoroughly mixed with 3g (40mmol chloride) KCl and 2g (42 mmol chloride) anhydrous MgCh and homogenized and placed in a quartz glass tube (diameter: 120 mm) which is located in a tube furnace.
[0078] A stream of dry nitrogen (0.3 liters per minute; oxygen content < 100 ppm v / v) is passed through the reactor, heated to 750°C, and held at this temperature for twelve hours. A brown precipitate (3.4 g) forms on the cooler quartz tube protruding from the furnace at approximately 160°C. The precipitate consists of a mixture of iron(II) chloride and iron(III) chloride.
[0079] The weight loss of the sample is 45 wt%, the residue is significantly lighter than the reactant.
[0080] The residue is dissolved in 200 ml of anhydrous ethanol and then filtered. The procedure is repeated twice. The filtrates are combined, and the ethanol is evaporated. The remaining mass contains the lithium compounds.
[0081] The residue remaining after ethanol extraction was first dried and then triturated with concentrated phosphoric acid. The resulting soluble phosphate has a very low iron content and can therefore be used for plant fertilization.
Claims
Patent claims 1. A process for the preparation of iron chloride, characterized in that i) a material containing at least one iron phosphate compound is reacted with at least one alkali metal chloride and / or at least one alkaline earth metal chloride at a temperature of 200 to 1100°C in an inert gas atmosphere and ii) the iron chloride formed is discharged in the exhaust gas stream and isolated.
2. Process according to claim 1, characterized in that the iron chloride is separated from the exhaust gas stream in step ii) by resublimation.
3. Process according to claim 1 or 2, characterized in that the iron chloride is deposited at temperatures of less than 700°C, preferably for FeCh at less than 699°C to 307°C, for FeC at less than 307°C, in particular at 150°C to 300°C.
4. The method according to at least one of claims 1 to 3, characterized in that the material used comprises at least one iron phosphate compound selected from the group consisting of iron phosphates, in particular iron(II) phosphate, iron(III) phosphate and iron(III) pyrophosphate, lithium iron phosphate (LFP), lithium iron manganese phosphate (LFMP), in particular LFP and / or LFMP with the general common formula LiFe(II). X )Mn x PO4, where 0 s=x<0.9, in particular 0 s=x<0.6, or mixtures thereof.
5. Process according to at least one of claims 1 to 4, characterized in that the reaction is carried out with at least one alkali metal chloride and at least one alkaline earth metal chloride.
6. Process according to at least one of claims 1 to 5, characterized in that the reaction is carried out with sodium chloride and magnesium chloride or potassium chloride and magnesium chloride.
7. Process according to at least one of claims 1 to 6, characterized in that a mixture of alkaline earth metal chlorides and alkali metal chlorides is used in a weight ratio of 4:1 to 0.25:1, in particular of 2:1 to 1:
2.
8. Method according to at least one of claims 1 to 7, characterized in that the material used 1 to 36 wt.% Fe, of which preferably 2 to 100 wt.% as iron phosphate compound 1 to 20 wt% P, 0 to 35 wt% Mn, 1 to 8 wt.% Li and Contains 1 to 55 wt.% carbon.
9. Process according to at least one of claims 1 to 8, characterized in that the material used contains from 5 to 100% by weight, preferably from 40 to 99% by weight, in particular from 50 to 99% by weight, particularly preferably from 70 to 99% by weight of at least one iron phosphate compound.
10. Process according to at least one of claims 1 to 9, characterized in that the molar ratio of chlorine from the alkali metal chlorides and alkaline earth chlorides used to phosphate groups contained in the material is in the range from 1:1 to 4:1, preferably from 2.3:1 to 3.5:1 mol / mol.
11. Process according to at least one of claims 1 to 10, characterized in that the reaction takes place at a temperature of 400°C to 1000°C.