Extraction process
The chemical extraction process for magnesium hydroxide from asbestos and magnesite sources addresses purity and environmental concerns by using acid leaching and filtration, achieving high-purity magnesium hydroxide while reducing carbon emissions and safely managing hazardous materials.
Patent Information
- Application Number
- PCT/IB2024/052765
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2024-03-22
- Publication Date
- 2024-10-03
AI Technical Summary
Existing methods for extracting magnesium products from asbestos and magnesite sources face challenges in achieving high purity and are environmentally hazardous, with pyrometallurgical processes leading to carbon dioxide emissions and hazardous material leaching into water systems.
A chemical extraction process involving a pre-leach step to create a feedstock, followed by acid leaching in an autoclave, differential precipitation, and filtration to separate impurities and extract magnesium hydroxide, which is then dewatered and purified, with reagents recovered for reuse.
The process achieves high-purity magnesium hydroxide extraction while minimizing environmental impact by reducing carbon emissions and safely managing hazardous materials, offering a commercially viable alternative to traditional pyrometallurgical methods.
Smart Images

Figure IB2024052765_03102024_PF_FP_ABST
Abstract
Description
[0001] EXTRACTION PROCESS
[0002] FIELD OF INVENTION
[0003] The invention relates to an extraction process, and more particularly, to an extraction process from a magnesium silicate (chrysotile asbestos), serpentinite and / or magnesite source.
[0004] BACKGROUND TO THE INVENTION
[0005] Asbestos is a potentially hazardous consisting of fibres. It occurs in many deposits around the world, broadly categorized into blue (crocidolite), brown (amosite) and white (chrysotile) asbestos, blue being the most hazardous and white being the least hazardous.
[0006] Asbestos deposits, many of which contain between 5 and 50 per cent asbestos, are a source of various metals and minerals, including nickel, magnesium, iron, chrome, aluminium, silica, and the like. Some of these, for example various magnesium products, may be useful to extract. Although attempts have been made to extract magnesium products from asbestos mine tailings, high purities have not been obtainable and commercial extraction using hydrochloric acid has been unsuccessful.
[0007] Most asbestos tailings facilities are exposed to the elements, increasing the risk of this potentially hazardous material being leached into local water systems due to rain, and dispersed in the air by wind. Removal of the asbestos and the rehabilitation of the environment are therefore also priorities.
[0008] Furthermore, the production of magnesium products from magnesite has been predominantly pyrometallurgical, resulting in large scale production of carbon dioxide. OBJECT OF THE INVENTION
[0009] It is accordingly an object of the invention to provide an extraction process, which will at least partially overcome the abovementioned disadvantages.
[0010] It is also an object of the invention to provide an extraction process, which will be a useful alternative to existing technologies.
[0011] SUMMARY OF THE INVENTION
[0012] In accordance with the invention, there is provided an extraction process for extracting wanted product from a raw material source, including the steps of: providing the raw material source; subjecting the raw material to a pre-leach process to obtain a suitable feedstock material; adding a leaching agent to the feedstock material in a leaching step to selectively extract a precursor product; selectively adjusting the pH in a first differential precipitation step to precipitate out impurities from the precursor product; separating the precursor product from the precipitated impurities in a first filtration step, wherein the precursor product is contained in a pregnant solution filtrate and the precipitated impurities are contained in a first filter cake; subjecting the filtrate to a second precipitation step to extract the wanted product as a precipitate pulp, while leaving a second filtrate (liquid phase) behind; dewatering the product pulp; separating the extracted wanted product in the form of the product pulp from the liquid phase in a second filtration step, wherein the wanted product is contained in a second filter cake;
[0013] - wherein the wanted product is extracted at a high purity, and
[0014] - wherein the raw material source may be mine tailings or run of mine (ROM).. The raw material may be selected from the group including chrysotile (a magnesium silicate with formula Mg3Si2O5(OH)4), serpentinite, or magnesite ( a magnesium carbonate with formula MgCO3).
[0015] In the instance where the raw material is chrysotile, the tailings may include fibrous fine (FF), fine and course particles. The FF portion may be predominantly chrysotile (asbestos).
[0016] In the instance of the raw material being chrysotile tailings, the pre-leach process may be a wet process, whereby the FF particles may be separated from the fine and course particles.
[0017] The pre-leach process may include the steps of adding water to the chrysotile tailings to form a slurry, allowing the slurry to be subjected to high shear agitation in a tank, passing the slurry over a fine mesh or grid, passing the slurry through one or more spirals and / or one or more sedimentation tanks and / or one or more sedimentation thickeners, to obtain the suitable feedstock material.
[0018] The feedstock material may be a smooth FF slurry from the pre-leach process. The FF slurry may have a specific gravity (SG) of between 1.2 and 1.3 ton / m3. The FF slurry may include fibres and impurities.
[0019] In the instance of the raw material being magnesite tailings or ROM, initial dry processing may be possible, and may include the steps of crushing, screening, magnetic separation, manual separation and milling, followed by the steps of adding water to the magnesite tailings to form a slurry and allowing the slurry to be subjected to high shear agitation in a tank to obtain the suitable feedstock material.
[0020] The feedstock material may be a smooth magnesium carbonate slurry from the preleach process. The magnesium carbonate slurry may have a specific gravity (SG) of between 1.2 and 1.3 ton / m3. The slurry may contain predominantly magnesium carbonate particles. In the case of either raw material, the prepared smooth slurry may be subjected to high shear agitation prior to entering the leach process.
[0021] In the case of either raw material, the leaching agent may be an acid. The acid may be sulphuric acid (H2SO4).
[0022] The leaching step may take place in an enclosed autoclave (reactor) at a controlled optimal temperature of between 60 °C and 65 °C, preferably between 60 °C to 63 °C. The leaching step may require a reaction time of approximately four (4) hours.
[0023] The precursor product may be magnesium sulphate (MgSO4) in solution.
[0024] The pH may be adjusted in the first precipitation step by systematically titrating magnesium oxide (MgO) into the reactor. The MgO systematically may raise the pH to between 6.5 and 7. The MgO may react with and selectively precipitate out the impurities (in the form of metal oxides), whilst the precursor product is maintained in solution. The MgO may also serve to neutralise any unreacted acid.
[0025] The first filter cake may consist of silica and other solid impurities, such as iron, aluminium, nickel, chrome and other trace element metal oxides.
[0026] During the second precipitation step, the precursor product retained in the pregnant filtrate may be converted to the wanted product by the addition of sodium hydroxide (NaOH).
[0027] The wanted product may be magnesium hydroxide (Mg(OH)2). The Mg(OH)2may be formed as a product precipitate pulp.
[0028] The purity of the wanted product may be between 80 and 99.7 per cent.
[0029] The liquid phase, second filtrate may contain sodium sulphate (Na2SO4) in solution. The sodium sulphate may be used to produce calcium sulphate (CaSO4- gypsum) and toregenerate sodium hydroxide (NaOH), a valuable reagent, by the addition of Lime (CaO). The dewatering step of the wanted product pulp may occur via filtration and / or sedimentation of the pulp and periodic siphoning off some of the liquid phase / second filtrate.
[0030] The second filtrate may undergo additional treatment, which may include rinsing, sedimentation, partial or complete dewatering, and / or filtration to retrieve micro- and nano-particle fractions of the wanted product which may have slipped through the initial second filtration process.
[0031] The second filter cake contains the wanted product of pure magnesium hydroxide and waterThe magnesium hydroxide cake may be dried, crushed, and milled to the required particle size and then packaged accordingly.
[0032] The process may further include the step of recovering reagents and / or by-products. In this step, the sodium sulphate from the second filtrate may be treated with lime (CaO) to form sodium hydroxide (NaOH).
[0033] Gypsum may be recovered and filtered out. Further steps of dewatering and a third filtration may follow.
[0034] BRIEF DESCRIPTION OF THE DRAWINGS
[0035] The invention will now be described further by way of non-limiting examples with reference to the accompanying drawing wherein:
[0036] Figure 1 is a schematic representation of the differential chemical leaching process in accordance with the invention, where the raw material utilized is chrysotile (asbestos) tailings.
[0037] Figure 2 is a schematic representation of the differential chemical leaching process in accordance with the invention, where the raw material utilized is magnesite (90% MgCO3) or comparable magnesite tailings. DETAILED DESCRIPTION OF THE INVENTION
[0038] In accordance with the invention, there is provided an extraction process 10 for extracting wanted 20 product from an raw material source, including the steps of providing the raw material source, subjecting the raw material to a pre-leach process to obtain a suitable feedstock material 30, adding a leaching agent 40 to the feedstock material 30 in a leaching step 50a to selectively extract a precursor product, selectively adjusting the pH in a first precipitation step 50b to precipitate out impurities from the precursor product, separating the precursor product from the precipitated impurities in a first filtration step 60, wherein the precursor product is contained in a pregnant solution filtrate and the precipitated impurities is contained in a first filter cake 70, subjecting the filtrate to a second precipitation step 80 to extract the wanted product 20 as a precipitate pulp, while leaving a liquid phase behind, dewatering the product pulp, separating the extracted wanted product in the form of the product pulp from the liquid phase in a second filtration step 90, wherein the wanted product 20 is contained in a second filter cake, wherein the wanted product 20 is extracted at a high purity, and wherein the raw material source is mine tailings or run of mine (ROM).
[0039] The raw material may be selected from the group including chrysotile (a magnesium silicate with formula Mg3Si2O5(OH)4), serpentinite, or magnesite (a magnesium carbonate with formula MgCO3).
[0040] In the instance where the raw material is chrysotile, the tailings include fibrous fine (FF), fine and course particles, with the FF portion being predominantly chrysotile (asbestos), which is a magnesium silicate with formula Mg3Si2O5(OH) The FF particles consist of a long fibre (LF) fraction and a short fibre or dust (SF) fraction. The LF fraction of the FF may be particles between 1-2 mm in size.
[0041] The pre-leach process, applicable to the chrysotile, is a wet process, whereby the FF particles are separated from the fine and course particles. The pre-leach process is a wet process to prevent dust formation of the raw material, which may be potentially hazardous. The pre-leach process includes the steps of adding water to the chrysotile tailings to form a slurry, allowing the slurry to be subjected to high shear agitation in a tank, passing the slurry over a fine mesh or grid, passing the slurry through one or more spirals and / or one or more sedimentation tanks and / or one or more sedimentation thickeners, to obtain the suitable feedstock material 30a.
[0042] The feedstock material 30a is the FF slurry from the pre-leach process. The FF slurry is smooth and preferably has a specific gravity (SG) of between 1.2 and 1.3 ton / m3. The FF slurry includes chrysotile fibres and impurities.
[0043] In the instance of the raw material being magnesite tailings or ROM, initial dry processing is possible, and includes the steps of crushing, screening, magnetic separation, manual separation and milling, followed by the steps of adding water to the magnesite tailings to form a slurry and allowing the slurry to be subjected to high shear agitation in a tank to obtain the suitable feedstock material 30b.
[0044] Magnesite (processed ROM at 90% MgCO3or comparable tailings) consists predominantly of magnesium carbonate, with the chemical formula MgCO3. Particle size is determined by the milling process, with an optimal size being between 75 urn and 150 urn.
[0045] The initial processing of magnesite can be a dry process, as magnesite is not classified as a hazardous material.
[0046] In this case, the feedstock material 30b is a smooth magnesium carbonate slurry from the pre-leach process. The magnesium carbonate slurry has a specific gravity (SG) of between 1 .2 and 1 .3 ton / m3. This slurry contains predominantly magnesium carbonate particles.
[0047] The leaching and other chemical processes for both the prepared chrysotile and magnesite material is the same, however, reagent quantities for the leaching process may differ slightly depending on the type of material being processed. The leaching agent 40 is an acid. The acid is sulphuric acid (H2SO4).
[0048] The leaching step takes place in an enclosed autoclave (reactor) 50a & 50b at an optimal temperature of between 60 °C and 65 °C, preferably between 60 °C and 63 °C. The leaching step requires a reaction time of approximately four (4) hours, give or take 20 minutes on either side.
[0049] The precursor product is magnesium sulphate (MgSO4).
[0050] In the instance of the raw material being leached being magnesite, a specific volume of Carbon Dioxide (CO2) will be released during the acid leach, which can be captured, filtered, scrubbed, compressed, and stored in suitable tanks 100 designed for the purpose of holding and transporting gas.
[0051] The pH is adjusted in the first precipitation step by systematically titrating magnesium oxide (MgO) 110 into the reactor 50. The MgO systematically raises the pH to between 6.5 and 7. The MgO reacts with and selectively precipitates out the impurities (in the form of metal oxides), whilst the precursor product is maintained in solution. The MgO also serves to neutralise any unreacted acid. Each impurity precipitates out at a different pH. Therefore, the respective solid impurities move out of solution as the pH is elevated.
[0052] At this stage, as the precursor product, MgSO4, is retained in solution in the filtrate, and the asbestos / chrysotile / magnesite is decomposed during this first reaction, the link between the source of the elemental magnesium in the asbestos tailings feed stock and the final product has effectively already broken at this stage.
[0053] The first filter cake 70 consists of silica and other solid impurities, such as iron, aluminium, nickel, chrome and other trace element metal oxides.
[0054] This solid phase filter cake 70 can be discarded as safe, neutral, and inert tailings.
[0055] During the second precipitation step 80, the precursor product retained in the pregnant filtrate is converted to the wanted product by the addition of a specific quantity of sodium hydroxide (NaOH) 120. The wanted product 20 is magnesium hydroxide (Mg(OH)2). The Mg(OH)2is formed as a product precipitate pulp.
[0056] The purity of the useful product is between 80 and 99.5 per cent.
[0057] The liquid phase, second filtrate contains sodium sulphate (Na2SO4) in solution. The sodium sulphate is used to produce calcium sulphate (CaSO4- gypsum) 160 and to regenerate sodium hydroxide (NaOH) 120, a valuable reagent, by the addition of Lime (CaO) 140.
[0058] The dewatering step of the wanted product pulp occurs via sedimentation of the pulp and periodic siphoning off some of the liquid phase / second filtrate.
[0059] The second filtrate can undergo additional treatment, which includes rinsing, sedimentation, partial or complete dewatering, and / or filtration to retrieve micro- and nano-particle fractions of the wanted product which could have slipped through the initial second filtration process.
[0060] Further processing may be applied to these fractions retrieved containing micro- and nano- particles, to ensure particle size stability and produce specific types and grades of products.
[0061] The second filter cake contains the wanted product 20 of pure magnesium hydroxide and water. The magnesium hydroxide is of a range of particle sizes large enough to be retained by a filter cloth utilised during this step. The magnesium hydroxide cake can be dried, crushed and milled to the required particle size, and then packaged 20 accordingly.
[0062] The process further includes the step 130 of recovering reagents and / or byproducts. In this step, the sodium sulphate from the second filtrate is treated with lime (CaO) 140 to form sodium hydroxide (NaOH) 120.
[0063] The gypsum 160 can be filtered out 150, dried, crushed and packaged 160. Further steps of rewatering and further filtration can follow. The Gypsum 160 is recovered as a solid filter cake by a third filtration step 150, and is then dried, crushed, and milled, for use in animal feed or fertilizer, or calcined to produce Plaster of Paris to be used as a structural binding or filler in the building industry.
[0064] The retained filtrate which contains Sodium Hydroxide (NaOH) can undergo a further partial dewatering step to be returned to the correct concentration and may be reused as a reagent 120 in the magnesium hydroxide precipitation step 80.
[0065] The unique extraction process described herein, can, therefore be used to produce various useful products from mine tailings or ROM, said products being magnesium hydroxide (Mg(OH)2) 20, carbon dioxide (CO2) 100 - depending on the raw material fed into the process, sodium hydroxide (NAOH) 120, and calcium sulphate dihydrate (gypsum) 160.
[0066] EXAMPLE OF PROCESS FLOW
[0067] FOR CHRYSOTILE
[0068] The process of the present invention demonstrates the removal of chrysotile (asbestos) material from tailings by using a unique approach to materials handling, to provide suitable feed stock material for the chemical part of the process, during which the asbestos is chemically destroyed through an acid leach process and converted into Magnesium Hydroxide Mg(OH)2.
[0069] Resource
[0070] In accordance with an example of the invention, a tailings resource contains approximately 28 million tons of raw asbestos tailings. Approximately 24 % of that is elemental magnesium, from which potentially 11.7 million tons of magnesium hydroxide product can be produced. Testing - material properties
[0071] During tests conducted on a pilot plant, a batch of raw material was characterised as follows:
[0072] • 42 % is a fine fibrous material which comprises predominantly asbestos (chrysotile) fibres, o Approximately 60 % contains fibres 1-2mm in length; and o Approximately 40 % contains light fibrous dust (i.e., ‘short’ fibres).
[0073] • 58 % comprises heavy and medium density material consisting of magnesium silicate in the form of serpentine and olivine, magnesium oxide in the form of brucite and the about 10 % if the total mass consisting of iron pyrite. o 45 % is a course (+2mm) fraction; and o 55 % is a fine (<2mm) fraction.
[0074] The fine fibrous (FF) material was established as a rich source of magnesium for the process of the current invention. However, the FF material was causing wet processing problems, as it formed a sticky fibrous network that captured and held the heavier course and fine particles together.
[0075] Mining and preparation of raw material
[0076] Approximately 263 tons of chrysotile tailings (dry weight) per day is treated. High pressure waterjets are used to break up clumps of material. The resultant slurry is then cleaned of detritus and oversize particles, using a course 20 mm vibrating screen. This results in approximately 850 m3to 900 m3of a course slurry being produced, which is fed through a 6 mm vibrating screen into an agitation tank, where it is subjected to high shear agitation for at least half an hour. The slurry is then passed through a 3 mm screen, to form a smooth slurry. Thereafter, the slurry is partially dewatered using a sedimentation tank, to produce a slurry with an optimal SG of between 1.2 and 1.3. The slurry is then pumped and fed into the pre-leach process at a constant rate of 0.63 m3 / minute (630 litres per minute). Wet processing of FF material
[0077] A wet method, using an array of spirals to remove the fine fibrous material, is preferred. As the FF material is relatively light, it separates readily from the rest of the material when passed over a set of spirals. The FF material is picked up in a tailings outlet. The course, heavier material is picked up in a middle and heavies outlet. Two passes over the spirals removed most of the fine fibrous material.
[0078] From a mining perspective, the inventors believe that this approach is unexpected and novel, for the following reasons:
[0079] During usual mining processes, ore is crushed and milled prior to wet separation using spirals. However, in the process of the present invention, apart from passing through a course screen, the material is sent directly to the spirals for separation.
[0080] During a normal mining process, when using a spiral set for separation, the light material (which ends up in the tailings outlet) is discarded, and the heavy and middle fraction retained and sent for further processing. However, in the process of the present invention, the tailings are retained for further processing and the heavy and middle fractions are not necessarily discarded but are sent to a stockpile for processing at a later stage.
[0081] Pre-leach of chrysotile tailings
[0082] The primary purpose of the pre-leach process is to separate the fine fibrous (FF) component of the ROM from the heavier fine and course fractions. It ensures a constant supply of FF slurry to be fed into the leach process.
[0083] The FF material comprises between 45 and 50% of the total mass of the ROM (i.e., 110 tons per day of FF). This FF material / feedstock material is predominantly magnesium silicate and will be liberated and fed into the leach process. The remaining 50 to 55 % of the ROM is fine and course material, which is to be stockpiled as this contains valuable minerals (including magnesium in silicate and hydroxide form, and iron pyrite). The FF consists of two fractions, namely a long fibre (LF) fraction (1-2 mm fibres) which is about 25 % of the volume of the ROM (or 60 % of the FF material) and then a short fibre (SF) fraction, predominantly asbestos dust, which is 17 % of the ROM (or 40 % of the FF material).
[0084] The LF-FF is easier to remove than the SF-FF, so this portion is washed off first and is easily captured in the tailings runoff of a spiral. Once most of the LF-FF has been removed, the SF-FF is more accessible and can be liberated and collected in a similar fashion.
[0085] Water management is a critical feature of the entire process, therefore, monitoring of the density of slurries is critical, as excessive water in the process can drastically reduce efficiency. Consequently, between each spiral processing cycle, the specific gravity (SG) of both the product and effluent slurries need to be monitored and adjusted using a set of settling or sedimentation tanks.
[0086] A constant supply of FF slurry is made available to be fed into the leach process at an SG of between 1.2 and 1.3 ton / m3, to facilitate the processing of at least 110 tons (dry weight) of FF material per day.
[0087] The pre-leach process consists of the following steps: a) Primary Spiral, b) Sedimentation Tank, c) Secondary Spiral, d) Thickener for slurry feed to leach process, e) Dewatering cyclone to retrieve process water from tailings and f) Tailings management (in this instance the tailings are valuable and will be dry stockpiled in a dedicated tailings stockpile facility).
[0088] In an example of the invention, the Primary Spiral Set accommodates 42 tons of material per hour. At a rate of four (4) tons of material per spiral, the system requires a minimum of 11 spirals. The process might require additional water to be sprayed to facilitate adequate flow and separation, which may add an additional 10- 12m3of water per hour. This effectively increases the required capacity to 62-64 tons per hour, which translates to 16 spirals. A primary spiral assembly consisting of four banks of four spirals sharing a steady head with a large single steady head feeding the four banks would facilitate this requirement.
[0089] In an example of the invention, the sedimentation tanks accommodate about half of the volume of the efferent slurry from the primary spirals or approximately 32 m3per hour. The excess water, which would need to be removed to return the SG back to 1 .2-1.3, will be in the region of about 6 m3. This takes about an hour to settle out, which can be sped up by the addition of a vibration motor at the base of the tank. Once adequate settling has occurred, the supernatant can be siphoned or pumped off. The arrangement of tanks can be set up in such a way that a batch of slurry will be ready for release every 5 minutes, which translates to 12 batches with an input of 2.6 m3of slurry and an output of 2.2 m3of slurry at an SG of 1.2 to 1.3 every 5 minutes, to maintain a continuous rate of 26.4 m3per hour. High density polyethylene (HDPE) tanks of 3 000 litre capacity are used for this purpose. Each tank is equipped with an agitator, weight and volume monitoring systems and is linked to a pump and valve system, linked to a programmable logic controller (PLC) system.
[0090] In an example of the invention, the Secondary Spiral Set accommodates 27 m3per hour of a slurry with a SG of 1.2-1.3, translating to a slurry mass of approximately 36 tons per hour. An additional 8 tons of water is required to be sprayed on the spirals to facilitate adequate flow and separation, bringing the per hour total to 44 tons per hour. Consequently, at a nominal capacity of 4 tons per spiral per hour, the secondary spiral system requires at least 11 spirals. A secondary spiral assembly, consisting of 3 banks of 4 spirals sharing a steady head with a large steady head feeding the 3 banks, would facilitate this requirement.
[0091] In an example of the invention, a multiple sedimentation thickener arrangement is used, with each thickener being large enough to accommodate enough slurry for one full day’s production. A least two, but preferably three thickeners is preferable. 110 tons of Fine Fibrous material is needed per day for the leach process. The ROM FF has a density of 2.6 ton / m3. Therefore, to produce a slurry with an SG of 1.3, from 110 tons of ROM FF, 293 tons of water is required. The resultant slurry has a mass of 403 tons and a volume of 335m3. The volume of thickener will need to equal the maximum expected volume of slurry per day and will be about 10 % larger by volume than the nominal volume of the slurry, i.e., in the region of about 370 m3. A thickener with a diameter of 14 meters and a height of 2.4 meters is suitable for this purpose.
[0092] FOR MAGNESITE
[0093] As there is no hazardous material in magnesite ore, an initial dry pre-leach process can be performed, which consists of the following steps: a) Mining - retrieval of ore \ tailings b) Crushing c) Screening d) Magnetic separation e) Milling f) Addition of water to form a slurry, and g) allowing the slurry to be subjected to high shear agitation in a tank to obtain the suitable feedstock material.
[0094] The feedstock material will be a smooth magnesium carbonate slurry with a specific gravity (SG) of between 1.2 and 1.3 ton / m3.
[0095] FOR CHRYSOTILE AND MAGNESITE
[0096] Leaching
[0097] In accordance with an example of the invention, the process flow depicted in Figures 1 and 2 demonstrates the acid leach and other chemical processes wherein the prepared chrysotile or magnesite tailings (feedstock material 30), either from the asbestos tailings-facility and / or the prepared material from the magnesite tailings or ROM, is transferred from the pre-leach thickener to the rest of the process. During leaching, the feedstock material is chemically broken down and converted into magnesium hydroxide, the wanted product 20.
[0098] The process was developed, tested, and optimised in a pilot plant and encompasses what the inventors believe to be a novel combination of chemical reactions and accompanying process parameters. Notably, five parameters were optimised, namely, pH requirements and rate of acid addition, SG of material at various stages of the process, fraction size of feedstock, temperature, and retention time for the chemical leaching reaction in the reactor.
[0099] Acid leach to produce precursor product
[0100] In accordance with an example of the invention, in this step the prepared feedstock material, i.e., fine fibrous (FF) chrysotile (being a magnesium silicate with formula Mg3Si2O5(OH)4, or magnesite (being a magnesium carbonate with formula MgCO3) is converted to magnesium sulphate and silica using sulphuric acid (H2SO4) as a leaching agent 40. This is represented by the following balanced chemical formulas:
[0101] Mg3Si2O5(OH)4+ 3 H2SO4= 3 MgSO4+ 2 SiO2+ 5 H2O or
[0102] MgCO3+ H2SO4=MgSO4+ CO2+H2O
[0103] The prepared slurry feedstock is a material with a diverse composition, it also contains several impurities which are impossible to remove during the pre-leach process. These impurities can include silicate forms of Al (aluminium), Fe (iron) and other trace element minerals such as nickel and chrome, and in this example comprises about a third of the mass of the dry prepared material.
[0104] The inventors have determined that it is possible to eliminate the chemical effect of these impurities by maintaining an optimal temperature of between 60 °C and 63 °C during the leach process. This temperature range has been established to favour selective conversion of the magnesium alone. At temperatures above this limit, the leaching of aluminium, iron and other trace element impurities takes place. At temperatures below this limit, the leach process is incomplete. Both of these scenarios will adversely impact both the yield and the purity of the final product.
[0105] DETAILED EXAMPLE
[0106] In this example of the invention, a production scale operation utilizing chrysotile (asbestos) tailings as a raw material, processes a total of 110 tons of prepared FF ROM per day. This feedstock material is stored in the pre-leach thickener, suspended in 293 m3of process water, making a total daily volume of 310 m3.
[0107] The acid leach process takes place in one or more 20 000 litre polypropylene or steel epoxy coated autoclaves (reactor vessels), specifically constructed for the process of the invention. These vessels have better insulating properties than the equivalent stainless-steel tanks, rendering power usage far less.
[0108] Time is an important factor of the leaching process. A leach cycle takes 6 hours in total, approximately broken up as follows:
[0109] 20 minutes for preparation and filling,
[0110] 240 minutes (4 hours) for the leach process itself, 100 minutes for emptying and filtration.
[0111] Four leaches per vessel per day is possible. A total of 110 tons of prepared FF ROM is to be processed per day. For 6 leach reactors at 4 leaches per day, each leach vessel processes 4.58 tons of material per cycle, suspended in 12,221 m3of water. This slurry is pumped into the vessel from the pre-leach thickener under the automated control of an integrated PLC system. A total volume of 12.926 m3, with a SG of 1.3 and a mass of 16.804 tons, is pumped / fed into the tank from the thickener. The FF feed from the thickener can be via a dedicated pump or through a gravity feed. The 24 leach cycles per day, are staged or staggered at hourly intervals over a 24-hour period, as illustrated in Table 1 below. TABLE 1
[0112] To start the leach reaction, 3.21 tons of sulphuric acid is pumped in from a storage tank at an SG of 1.8 (equalling 1.782 m3). Each reactor vessel is equipped with an agitator / stirrer, a set of valves, piping linked to a pump system, a steam heating system, as well as monitors for weight, volume, temperature and pH. The steam heating system consists of a boiler which produces steam at about 300 °C. The steam is bubbled through the slurry at a predetermined rate to maintain the desired temperature of between 60 °C to 63 °C.
[0113] The leaching process is an exothermic reaction and produces its own heat. Therefore, the temperature is monitored on a continuous basis and additional heating only is applied when necessary to maintain the optimal temperature range.
[0114] In this instance, to maintain a temperature of between 60 °C to 65 °C, the optimal amount of steam required over a 4-hour leach period will add 463 litres of water to the 14 700 litres.
[0115] Precipitation of impurities via pH control
[0116] This step of the process deals with the interaction between magnesium oxide and magnesium hydroxide in a dilute acid medium to neutralize any unreacted sulphuric acid. The reaction also drives the precipitation of impurities via the addition of sacrificial magnesium oxide. This is represented by the following formula:
[0117] MgO + H2O = Mg(OH)2
[0118] This part of the reaction does not affect the outcome and yield of the magnesium sulphate generated in the previous reaction. However, neutralisation is important in maintaining the magnesium sulphate in solution, while promoting the precipitation of impurities.
[0119] After the leaching reaction, the pH in the reactor vessel is measured and monitored and magnesium oxide is selectively titrated into the vessel, using the pH as an indicator. A potential maximum of 764 kg of MgO is titrated in, in the form of a watery suspension, to neutralise and stabilise the pH at between 6.5 to 7. This can increase the volume of the contents of the vessel by as much as 2 m3.
[0120] This is a key part of the process, as raising the pH will halt any residual reactions and promotes the precipitation of solid impurities. At this point, the elemental magnesium has reacted to form soluble magnesium sulphate, which remains in suspension.
[0121] The pH, prior to adding MgO, is a good indicator of the efficiency of the leach reaction of the previous step. The higher the pH prior to adding MgO, the more efficient the leach process, and less MgO is required to neutralise the acid and stabilise the pH. Once the pH has been stabilised, the leach has completed and the contents of the reactor is ready for filtration.
[0122] First filtration
[0123] In accordance with the invention, it is essential at this point of the process to separate the solid and liquid phases, as the magnesium sulphate precursor product is entirely contained in solution in the liquid phase.
[0124] The filtrate containing magnesium sulphate is retained and placed in a reactor vessel or tank for the next part of the process. The solid phase (filter cake) consists predominantly of silica with precipitated impurities. This can be discarded as safe, neutral, and inert tailings.
[0125] In this example of the invention, after the leach process has ended, the reactor vessel contains a slurry with a volume of approximately 17.2 m3, weighing 22.6 tons and with an SG of 1.32 kg / l, which needs to be filtered. The slurry consists of the following constituents, as per Table 2. TABLE 2
[0126] At this stage, the elemental magnesium has been ‘stripped’ from the chrysotile asbestos, thus destroying its molecular configuration. The magnesium is captured in the magnesium sulphate, which is dissolve in the liquid (water) phase. The remainder of the chrysotile molecule has been converted into a safe and inert solid silica.
[0127] The slurry is filtered to separate the solid phase (SiO2(silica) and other solid impurities) from the liquid phase, which contains the magnesium sulphate.
[0128] A filter press is used for this process, with a capacity to filter, rinse and produce a dry cake from 17.2 m3(22.6 tons) of slurry containing 3.641 tons (16.11 %) of solid material and with an SG of 1.312 in 100 minutes.
[0129] The filtration cycle proceeds as per Table 3.
[0130] TABLE 3 FILTRATION 1 (Filtrate = Magnesium Sulphate || Cake = Silicate)
[0131] In an example of the invention, the time per filtration cycle is 15 to 20 minutes. Approximately 17.28 m3of slurry is processed every 60 to 80 minutes. The filtrate volume liberated from the slurry is 15.744 m3, which is transferred to a reactor vessel (along with all rinse water added during filtration, approximately 13.76 m3).
[0132] The 4 tons of cake produced per filtration cycle drops down to a channel below the filter press onto a conveyor belt system for removal.
[0133] Precipitation of magnesium hydroxide
[0134] In this step of the invention, the magnesium sulphate precursor produced during the first reaction (retained in solution in the captured filtrate), is converted to magnesium hydroxide (Mg(OH)2) by the addition of sodium hydroxide (NaOH).
[0135] This is represented by the following formula:
[0136] MgSO4+ 2 NaOH = Mg(OH)2+ Na2SO4
[0137] The reaction above is a double replacement reaction (not temperature sensitive) where Mg(OH)2is formed as a precipitate and Na2SO4remains in solution.
[0138] In one example of the invention, to convert 3.932 tons of magnesium sulphate dissolved in the filtrate in the second reactor vessel, 2.659 tons of sodium hydroxide (NaOH) in solution is added, by pumping it in from a holding tank. The NaOH is dissolved in a volume of 6.72 m3of water, creating a solution with a volume of 7.4 m3. The volume of magnesium sulphate filtrate is 29.504m3, divided equally between two 20 000 m3vessels (14.752 m3per vessel). Consequently, the NaOH solution needs to be divided equally between the two vessels, i.e., 3.7 m3per vessel, bringing the volume in each vessel to 18.452 m3.
[0139] Whilst the precipitation reaction occurs relatively quickly, the reaction is allowed to continue for 30 minutes with maximum agitation. Approximately 1 .925 tons of magnesium hydroxide is produced as a precipitate pulp during this process (0.963 tons per tank).
[0140] Dewatering of magnesium hydroxide pulp
[0141] This is a very important step, as the system may become overburdened with excess water, which will dilute reagents and drastically increase reaction times, requiring the use of unnecessarily large storage and reaction vessels.
[0142] The first step of dewatering is a sedimentation step. Once the agitators in the vessels are switched off, the reactor vessels are left to stand for 120 minutes, to allow settlement of the precipitate (magnesium hydroxide product).
[0143] The reactors are fitted with a set of pumps designed to periodically siphon off the clear supernatant once adequate settling has occurred. Siphoning is done until approximately half of the volume of liquid in the vessels (9.43 m3from each) is removed this way. This leaves the precipitant laden pulp in the bottom half of the vessels.
[0144] The clear supernatant is a solution of sodium sulphate (Na2SO4) and is treated with lime (CaO) to produce sodium hydroxide (NaOH) and calcium sulphate. This NaOH is returned to the NaOH holding tank. Calcium sulphate (CaSO4- gypsum) is filtered out.
[0145] Further dewatering of the remaining precipitate laden slurry is achieved by pumping the slurry through a hydro-cyclone to increase the SG of the slurry to 1.2.
[0146] The entire dewatering process, in this example of the invention, takes about 150 minutes in total (120 min for sedimentation plus 90 min for hydro-cyclone dewatering).
[0147] The magnesium hydroxide product pulp can now be processed through a filter press. Second filtration
[0148] As with the previous filtration step, this is not a chemical reaction, but is essential, as the precipitated (solid phase) magnesium hydroxide needs to be separated from the liquid phase, which contains sodium sulphate in solution.
[0149] In this instance as much of the filtrate must be rinsed out of the filter cake as possible with fresh, preferably de-ionised, water. This will improve purity and ensure that the highest quality product is achieved. The filtrate is captured and retained in a reactor vessel, as the sodium hydroxide reagent can be reclaimed chemically.
[0150] The filter cake, which essentially consists of pure magnesium hydroxide and water, needs to be dried, crushed to the required particle size and the packaged accordingly.
[0151] In accordance with one example of the invention, 12 m3magnesium hydroxide pulp in the reactor vessel has the following composition, as per Table 4.
[0152] TABLE 4
[0153] An automated tower filter press is used for this process, with a capacity to filter, rinse and produce a dry cake from 12 m3(16.6 tons) of pulp containing 1.925 tons (11.6 %) of magnesium hydroxide precipitate and with an SG of 1.2, in 60 minutes. The filtration cycle proceeds as per Table 5.
[0154] TABLE 5
[0155] FILTRATION 2 (Filtrate = Sodium Sulphate || Cake = Magnesium Hydroxide)
[0156] In an example of the invention, the time per filtration cycle is 36 to 38 minutes, which means that approximately 12.96 m3of pulp is processed every 108 to 114 minutes. The filtrate volume liberated from the slurry is 11 .198 m3(which contains 4.675 tons of sodium sulphate in solution). This is transferred to a reactor vessel along with all rinse water added during the filtration process (approximately 16.8 m3).
[0157] The 2.25 tons of magnesium hydroxide cake produced per filtration cycle drops down onto a conveyor belt below the filter, for removal to an extruding press. In the extruding press, the moist magnesium hydroxide paste is formed into flakes and deposited in an even pattern onto a conveyor which travels through a 10 m long drying tunnel.
[0158] In the drying tunnel, the magnesium hydroxide flakes are exposes to downward laminar flow dry hot air at a temperature of 120 °C for 30 min. This dries the magnesium hydroxide to between 5 % and 7 % moisture.
[0159] The flakes are the deposited in a hopper of a de-agglomerator, which completes the drying process and pulverises the flakes into a fine powder. From there the powdered magnesium hydroxide product is deposited into a ribbon blender and thoroughly blended for 30 minutes. Afterwards, it is analysed and certified as being within the required purity limits. Packaging follows. Recovery and regeneration
[0160] Sodium Hydroxide is a relatively expensive reagent, therefore, it is economically prudent to regenerate as much of it as possible by the addition of a less expensive reagent.
[0161] In an example of the invention, this step of the process enables regeneration of approximately 90 % of the sodium hydroxide. This is done via the addition of lime (CaO) to the filtrate captured during the second filtration step. The sodium hydroxide is produced and retained in solution while calcium sulphate (gypsum) is produced as a precipitate.
[0162] This is represented by the following formula:
[0163] Na2SO4+ CaO + H2O = 2 NaOH + CaSO4
[0164] In this case, to convert 4.675 tons of sodium sulphate dissolved in the filtrate, 1.846 tons of calcium oxide (lime) in suspension is added. The CaO is suspended in a volume of 4.37 m3of water, creating a solution with a volume of 4.83 m3.
[0165] This is a double substitution reaction, wherein the limiting factor is the rate at which the lime (which has limited solubility in an aqueous medium) is able to dissolve and react with the sodium sulphate. The reaction is allowed to proceed for one hour with vigorous agitation.
[0166] The reaction recovers 2.64 tons of sodium hydroxide in solution, as well as 4.48 tons of calcium sulphate (gypsum) as precipitate / pulp.
[0167] Dewatering of calcium sulphate pulp
[0168] Following the regeneration step, the SG of the calcium sulphate pulp is approximately 1.08, due to the excessive volume of the liquid phase. For effective filtration to occur, the SG of the pulp must be raised to at least 1.2, i.e., the liquid phase needs to be reduced. This is achieved in two ways, namely sedimentation and dewatering using a hydro-cyclone.
[0169] As before, the first dewatering step is a sedimentation step, by switching off the reactor vessels and allowing it to stand for 120 minutes. Settlement of the precipitate then occurs. Pumps siphon off the clear supernatant once adequate settling has occurred, leaving the thickened pulp in the bottom half of the vessel.
[0170] The clear supernatant is a solution of Sodium Hydroxide (NaOH), which is returned to a holding tank for use in previous steps of the process.
[0171] Further dewatering of the remaining pulp is achieved by pumping the pulp through a hydro-cyclone system to increase the SG thereof to at least 1.2. The pulp can now be processed through a filter press.
[0172] Third filtration
[0173] In the present example of the invention, the 13.7 m3of calcium sulphate pulp has the following composition, as per Table 6:
[0174] TABLE 6
[0175] An automated tower filter press is used for this process, with the capacity to filter, rinse and produce a dry cake from 13.8 m3(17.22 tons) of pulp containing 4.48 tons The filtration cycle proceeds as follows, as per Table 7.
[0176] TABLE 7
[0177] FILTRATION 3 (Filtrate = Sodium Hydroxide || Cake = Gypsum)
[0178] The filtrate volume liberated from pulp / slurry is 11.198 m3, which contains 2.64 tons of sodium hydroxide in solution. This is transferred to a holding tank along with all rinse water added during the filtration process (approximately 11 .04 m3).
[0179] In this example of the invention, the 4.95 tons of calcium sulphate (gypsum) cake produced per filtration cycle, drops down onto the conveyor belt below. The gypsum is transferred to an extruding press. In the press, the moist gypsum paste is made into flakes and deposited in an even pattern onto a conveyor which travels through a 10 m long drying tunnel.
[0180] In the drying tunnel the gypsum flakes are exposes to downward laminar flow dry hot air at a temperature of 120 °C for 30 minutes. This dries the gypsum to between 5 % and 7 % moisture.
[0181] The flakes are the deposited in a hopper of a de-agglomerator, which completes the drying process and pulverises the flakes into a fine powder. From there the powdered gypsum is deposited into a ribbon blender and thoroughly blended for 30 minutes, after which it is stored.
[0182] Once the calcium sulphate (gypsum) powder has been analysed and certified as being within the required purity limits, a certificate of analysis / compliance is issued to the batch concerned. The recovered product can now be packaged.
[0183] Accordingly, the carbon footprint of extraction of magnesium hydroxide from magnesite using a hydrometallurgical process is considerably less than current methodologies.
[0184] It should also be noted that, whilst this process was primarily developed to deal with asbestos tailings, the process can also be similarly applied to magnesite and magnesite tailings (MgCO3), if so desired. As Magnesite does not present the same health hazard as asbestos, dry processing of this raw material prior to the leach process is possible.
[0185] The inventors believe that the differential leaching process of the invention would be advantageous in that: a) It provides for the rehabilitation of asbestos dumps; b) Magnesium products are obtained using a hydro-metallurgical process instead of the usual pyro-metallurgical processes of the prior-art, which emits an excess of carbon dioxide; c) The process of the invention is commercially viable; d) The process of the invention assists in removing sulphur from the environment (via the use of sulphuric acid); and e) Various useful by-products are obtained in the process of the invention, including fertiliser and animal feeds (magnesium sulphate) and gypsum.
[0186] It will be appreciated that various alternative embodiments are also possible in accordance with the present invention. The above is only an example of the invention and there may be many variations in detail without departing from the spirit and / or scope of the invention. Furthermore, it will be understood that some advantages of the present invention may be attained by selecting some of the features of the present invention without utilizing other features. Accordingly, those skilled in the art will recognize that modifications and adaptations to the present invention may be possible or desirable in certain circumstances and may form part of the present invention.
Claims
CLAIMS1. An extraction process for extracting wanted product from a raw material source, including the steps of providing the raw material source, subjecting the raw material to a pre-leach process to obtain a suitable feedstock material, selectively extracting a precursor product from the feedstock material in a leaching step by adding a leaching agent to the feedstock material, precipitating out impurities from the precursor product in a first differential precipitation step by selectively adjusting the pH, separating the precursor product from the precipitated impurities in a first filtration step, wherein the precursor product is contained in a pregnant solution filtrate and the precipitated impurities are contained in a first filter cake, in a second precipitation step extracting the wanted product from the pregnant solution filtrate as a precipitate pulp, while leaving a liquid phase behind, in a second filtration step separating the wanted product from the liquid phase, the liquid phase now making up a second filtrate, wherein the wanted product is contained in a second filter cake at a high purity, and wherein the raw material source is mine tailings or run of mine (ROM).
2. The extraction process of claim 1 , wherein the raw material is selected from the group including chrysotile, serpentinite, or magnesite.
3. The extraction process of claim 2, wherein, in the instance of the raw material being chrysotile, the chrysotile (asbestos) is predominantly contained in a fibrous fine (FF) portion of the mine tailings, the mine tailing also including fine and course particles.
4. The extraction process of claim 3, wherein the pre-leach process is a wet process, whereby the chrysotile containing FF particles are separated from the fine and course particles.
5. The extraction process of claim 4, wherein the pre-leach process includes the steps of adding water to the chrysotile tailings to form a slurry, allowing the slurry to be subjected to high shear agitation in a tank, passing the slurryover a fine mesh or grid, passing the slurry through one or more spirals and / or one or more sedimentation tanks and / or one or more sedimentation thickeners, to obtain the suitable feedstock material in the form of a smooth FF slurry.
6. The extraction process of claim 5, wherein the feedstock material is the FF slurry from the pre-leach process with a specific gravity (SG) of between 1.2 and 1.3 ton / m3.
7. The extraction process of claim 2, wherein, in the instance of the raw material being magnesite or ROM, initial dry processing is done, including the steps of crushing, screening, magnetic separation, manual separation and milling, followed by the steps of adding water to the magnesite tailings to form a slurry and allowing the slurry to be subjected to high shear agitation in a tank to obtain the suitable feedstock material.
8. The extraction process of claim 7, wherein the feedstock material is a smooth magnesium carbonate slurry from the pre-leach process with a specific gravity (SG) of between 1.2 and 1.3 ton / m3.
9. The extraction process of claim 7, wherein carbon dioxide is released during the leach step, which carbon dioxide is captured, filtered, scrubbed, compressed, and stored in suitable tanks designed for the purpose of holding and transporting gas.
10. The extraction process of any one of the preceding claims, wherein the leaching agent is an acid, selected from the group including sulphuric acid.11 . The extraction process of any one of the preceding claims, wherein the leaching step takes place in an enclosed autoclave reactor at a temperature of between 60 °C and 65 °C, preferably between 60 °C to 63 °C.
12. The extraction process of any one of the preceding claims, wherein the leaching step requires a reaction time of approximately four (4) hours.
13. The extraction process of any one of the preceding claims, wherein the precursor product is magnesium sulphate in solution.
14. The extraction process of any one of the preceding claims, wherein the pH is selectively adjusted in the first precipitation step by systematically titrating magnesium oxide into the reactor, thereby systematically raising the pH to between 6.5 and 7.
15. The extraction process of claim 14, wherein the magnesium oxide reacts with, and selectively precipitate out, the impurities, whilst the precursor product is maintained in solution.
16. The extraction process of claim 14, wherein each impurity precipitates out at a different pH, thereby moving the respective solid impurities out of solution as the pH is elevated.
17. The extraction process of claim 14, wherein the magnesium oxide serves to neutralise any unreacted acid.
18. The extraction process of any one of the preceding claims, wherein the first filter cake consists of silica and other solid impurities, including, but not limited to iron, aluminium, nickel, chrome, and trace element metal oxides.
19. The extraction process of claim 18, wherein this filter cake is suitable to be discarded as safe, neutral, and inert tailings.
20. The extraction process of any one of the preceding claims, wherein the precursor product is converted to the wanted product during the secondprecipitation step by the addition of sodium hydroxide.
21. The extraction process of any one of the preceding claims, wherein the wanted product is magnesium hydroxide.
22. The extraction process of claim 21 , wherein the magnesium hydroxide has a purity of between 80 and 99.7 per cent.
23. The extraction process of any one of the preceding claims, wherein the liquid phase and second filtrate contain sodium sulphate in solution.
24. The extraction process of any one of the preceding claims, wherein the sodium sulphate is used to produce calcium sulphate (gypsum) and to regenerate sodium hydroxide by the addition of calcium oxide (lime).
25. The extraction process of any one of the preceding claims, wherein the wanted product pulp undergoes a dewatering step via filtration and / or sedimentation of the pulp and periodic siphoning off the liquid phase.
26. The extraction process of any one of the preceding claims, wherein the second filtrate undergoes additional treatment, including rinsing, sedimentation, partial or complete dewatering, and / or further filtration to retrieve micro- and nano-particle fractions of the wanted product following the initial second filtration process.
27. The extraction process of any one of the preceding claims, wherein the magnesium hydroxide cake is dried, crushed, and milled to the required particle size and then packaged accordingly.
28. The extraction process of any one of the preceding claims, wherein the process includes the further step of recovering reagents and / or by-products.
29. The extraction process of claim 23 or 28, wherein sodium sulphate from the second filtrate is treated with lime to form sodium hydroxide.
30. The extraction process of claim 29, wherein gypsum is recovered as a sideproduct, dried, crushed, and milled, or calcined to produce Plaster of Paris.
31. The extraction process of claim 1 , substantially as herein described and exemplified and / or described with reference to the accompanying figures.
Citation Information
Patent Citations
Method for leaching magnesium from magnesium hydroxide-containing compositions
CA1181243A
Recovery of metals from metal silicates
CA2340567A1
Production of fine grain magnesium oxide and fibrous amorphous silica from serpentinite mine tailings
CA3149664A1
Leaching method of magnesium-containing ore
CN101760646A
Method for preparing light-magnesium oxide from serpentine tailings
CN1024565C