Light-emitting element, display device, and quantum dot adduct
The use of a discontinuous or porous silica adduct around quantum dots addresses the insulating issues of silica coverage, enhancing carrier injection and luminous efficiency in light-emitting devices, resulting in improved performance and longevity.
Patent Information
- Application Number
- PCT/JP2023/012831
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-03
AI Technical Summary
The challenge is to improve carrier injection efficiency into quantum dots covered with silica, as silica's insulating nature inhibits carrier injection, and existing attempts using organic cyclic structures within silica are insufficient.
A light-emitting device configuration featuring quantum dots surrounded by a discontinuous, non-uniform, or porous silica adduct with a thickness of 1 nm or less, allowing for enhanced carrier injection by reducing the distance and barrier for carrier transport.
This configuration significantly improves carrier injection efficiency and luminous efficiency of the light-emitting device, leading to increased brightness and extended service life, with the adduct protecting the quantum dots while allowing efficient carrier passage.
Smart Images

Figure JP2023012831_03102024_PF_FP_ABST
Abstract
Description
Light-emitting device, display device, and quantum dot adduct
[0001] The present disclosure relates to a light-emitting device, a display device, and a quantum dot adduct.
[0002] To improve durability, research is being conducted into covering quantum dots with silica (silicon oxide). Non-Patent Document 1 discloses a structure in which quantum dots are covered with silica having an organic ring structure introduced therein.
[0003] "Blue-Emitting InP / GaP / ZnS Quantum Dots with Enhanced Stability by Siloxane Capping: Implication for Electroluminescent Devices" (ACS Appl. Nano Mater. 2022, 5, 2801-2811)
[0004] Since silica is insulating, covering quantum dots with silica hinders carrier injection into the quantum dots. Non-Patent Document 1 attempts to improve the carrier injection efficiency by introducing an organic ring structure into silica, but carrier injection is still insufficient.
[0005] A light-emitting element according to one aspect of the present disclosure comprises a first electrode and a second electrode facing each other, and a light-emitting layer disposed between the first electrode and the second electrode, the light-emitting layer including quantum dots and an additive located at least partially around the quantum dots, the additive being at least one of a discontinuous film, having a non-uniform thickness, being porous, and having a portion having a thickness of 1 nm or less.
[0006] A quantum dot adduct according to one aspect of the present disclosure includes a quantum dot and an adduct located at least partially around the quantum dot, wherein the adduct is at least one of a discontinuous film, an ununiform thickness, a porous film, and a film having a thickness of 1 nm or less.
[0007] According to the configuration according to one aspect of the present disclosure, the efficiency of carrier injection into quantum dots can be improved.
[0008] 1 is a cross-sectional view showing an example of the configuration of a light-emitting device according to an embodiment of the disclosure. FIG. 1 is a cross-sectional view showing an example of the configuration of the quantum dot-added body shown in FIG. 1. FIG. 2 is a cross-sectional view showing another example of the configuration of the quantum dot-added body shown in FIG. 1. FIG. 3 is a cross-sectional view showing another example of the configuration of the quantum dot-added body shown in FIG. 1. FIG. 4 is a cross-sectional view showing another example of the configuration of the quantum dot-added body shown in FIG. 1. FIG. 5 is a cross-sectional view showing another example of the configuration of the quantum dot-added body shown in FIG. 1. FIG. 6 is a diagram showing a method for manufacturing a quantum dot-added body according to an embodiment of the present disclosure. FIG. 7 is a diagram showing a graph of voltage-luminance characteristics of light-emitting devices according to Example 1 and Comparative Example 1. FIG. 8 is a graph of voltage-current density characteristics of light-emitting devices according to Example 1 and Comparative Example 1. FIG. 9 is a graph of current density-luminance characteristics of light-emitting devices according to Example 1 and Comparative Example 1. FIG. 10 is a graph of current density-EQE characteristics of light-emitting devices according to Example 1 and Comparative Example 1. FIG. 11 is a graph showing luminance and driving voltage over time for the light-emitting device according to Example 1 in a constant current test. FIG. 12 is a graph showing luminance and driving voltage over time for the light-emitting device according to Comparative Example 1 in a constant current test. FIG. 13 is a diagram showing an estimated useful life of the light-emitting device according to Example 1. FIG. 14 is a diagram showing an estimated useful life of the light-emitting device according to Comparative Example 1. Fig. 1 is a diagram showing the results of FTIR of a solution of a quantum dot adduct according to Example 1. Fig. 2 is a diagram showing the results of FTIR of a solution of quantum dots according to Comparative Example 1. Fig. 3 is a cross-sectional view showing an example of the configuration of a display device according to an embodiment of the present disclosure.
[0009] [Embodiment 1] (Configuration of Light-Emitting Device) Fig. 1 is a cross-sectional view showing an example of the configuration of a light-emitting device according to an embodiment of the present disclosure. As shown in Fig. 1, a light-emitting device 10 according to the present disclosure includes a first electrode 12 and a second electrode 16 facing each other, and a light-emitting layer 14 provided between the first electrode 12 and the second electrode 16, the light-emitting layer 14 including quantum dots QDs and an addition 2 located at least partially around the quantum dots QDs, the addition 2 being at least one of a discontinuous film, having a non-uniform thickness, being porous, and having a portion with a thickness of 1 nm or less. The quantum dots QDs and the addition 2 constitute a quantum dot addition product 1.
[0010] In this configuration, the additive 2 does not hinder carrier injection into the quantum dots QD, as compared with the conventional configuration in which the additive covering the periphery of the quantum dots is a continuous film with a uniform thickness and a dense structure, thereby improving the efficiency of carrier injection into the quantum dots QD in the light-emitting element 10 and the luminous efficiency of the light-emitting element 10.
[0011] One of the first electrode 12 and the second electrode 16 is an anode, and the other is a cathode. At least one of the first electrode 12 and the second electrode 16 is a transparent electrode. The light-emitting element 10 may include additional components, such as a substrate 11 on which the first electrode 12 is formed, a sealing film 17 covering the second electrode 16, a charge transport layer 13 located between the first electrode 12 and the light-emitting layer 14, and a charge transport layer 15 located between the second electrode 16 and the light-emitting layer 14.
[0012] The addition 2 is in direct contact with the quantum dots QD. Therefore, the outside of the addition 2 is close to the quantum dots QD, and the efficiency of carrier injection into the quantum dots QD can be improved.
[0013] The band gap of the additive 2 is wider than the band gap of the constituent material of the quantum dot QD. When the quantum dot QD has a core and a shell surrounding the core, the band gap of the additive 2 is wider than the band gap of the constituent material of the shell. Usually, the additive 2 is insulating.
[0014] The additive 2 may be an inorganic material. For example, the additive 2 may be silicon oxide (SiO 2 ), and may further contain silicic acid ([SiO x (OH) 4-2x ] n Additive 2 may contain titanium oxide (TiO 2 The additive 2 may contain aluminum oxide (Al 2 O 3 Adduct 2 may contain zinc chloride (ZnCl 2 The additive 2 may include silicon nitride (Si 3 N 4 Additive 2 may include, for example, boron oxide (B 2 O3 ), phosphorus oxide (P 2 O 5 ), germanium oxide (GeO 2 ), beryllium fluoride (BeF 2 ), arsenic sulfide (As 2 S 3 ), silicon selenide (SiSe 2 ), germanium sulfide (GeS), tellurium oxide (TeO 2 ), bismuth oxide (Bi 2 O 3 ), vanadium oxide (V 2 O 5 ), antimony oxide (Sb 2 O 5 ), lead oxide (PbO), copper oxide (CuO), zirconium fluoride (ZrF 4 ), aluminum fluoride (AlF 3 ), indium fluoride (InF 3 ), and zinc bromide (ZnBr 2 ) may contain one or more selected from the group consisting of. The chemical formulas written in parentheses after the compound names are representative examples. The composition ratios written in the chemical formulas may be stoichiometric, but do not necessarily have to be stoichiometric.
[0015] The additive 2 may include at least one of polycrystalline and amorphous. The maximum thickness of the additive 2 may be 2 nm or more.
[0016] (Structure of Quantum Dot Addendum) FIG. 2 is a cross-sectional view showing an example of the structure of the quantum dot addendum shown in FIG. 1. As shown in FIG. 2, the addendum 2 may be solid or may include a discontinuous film arranged around the quantum dot QD in a cross section passing through the quantum dot QD. The discontinuous film has one or more discontinuous points in the circumferential direction centered on the quantum dot QD. With this structure, the addendum 2 protects the quantum dot QD, and carriers can be injected into the quantum dot QD through the discontinuous points of the addendum 2. "Solid" may mean that there is no region lacking a constituent element of the addendum 2 or that the region is negligibly small, typically meaning that the size of the missing region is 5 nm or less. "Discontinuous points" may be regions lacking one or more constituent elements of the addendum 2, typically having a size of more than 8 nm. The discontinuous points may penetrate the addendum 2 three-dimensionally. Furthermore, when the addendum 2 for one quantum dot is composed of multiple parts that are separated and independent from each other, the discontinuous points may include gaps between the multiple parts. A "solid discontinuous film" may refer to a film that has discontinuities and is solid in areas other than the discontinuities.
[0017] Furthermore, "surrounding" refers to a region extending around an object (here, quantum dots QDs), and the distance from the object is not particularly limited. However, "surrounding" may refer to a region extending outward from the surface of an object to a given width, or may refer to a region from the quantum dots QDs having a width approximately equal to or less than the distance between adjacent quantum dots QDs. Furthermore, "disposed around" does not necessarily mean continuously surrounding an object, but also includes cases where the object is intermittently surrounded, and cases where the object is disposed in only a portion of the region extending around the object.
[0018] FIG. 3 is a cross-sectional view showing another example of the configuration of the quantum dot adduct shown in FIG. 1 . As shown in FIG. 3 , the adduct 2 may be solid and may include a continuous film of non-uniform thickness surrounding the quantum dot QD in a cross section passing through the quantum dot QD. The thickness of the adduct 2 is the size in the radial direction centered on the quantum dot QD. With this configuration, the adduct 2 protects the quantum dot QD, and carriers can be injected into the quantum dot QD through the thin portion of the adduct 2. The minimum thickness of the adduct 2 may be 1 nm or less. By setting the thickness to 1 nm or less, carriers can pass through the thin portion more efficiently, allowing carriers to be injected into the quantum dot QD more efficiently. Furthermore, the entire continuous film may have a thickness of 1 nm or less, allowing carriers to be injected into the quantum dot QD more efficiently. Alternatively, the entire continuous film may be a uniform continuous film with a thickness of 1 nm or less.
[0019] 4 is a cross-sectional view showing another example of the configuration of the quantum dot adduct shown in FIG. 1. As shown in FIG. 4, the adduct 2 may be porous and may include a continuous film surrounding the quantum dot QDs in a cross section passing through the quantum dot QDs. With this configuration, the adduct 2 protects the quantum dot QDs, and carriers can be injected into the quantum dot QDs through the pores of the adduct 2. The porous pores may be regions in which one or more of the constituent elements of the adduct 2 are deficient, and typically have a size of more than 5 nm and not more than 8 nm. The pores may penetrate the adduct 2 three-dimensionally.
[0020] Figure 5 is a cross-sectional view showing another example of the configuration of the quantum dot adduct shown in Figure 1. As shown in Figure 5, the adduct 2 may be porous and may include a discontinuous film arranged around the quantum dot QD in a cross section passing through the quantum dot QD. With this configuration, the adduct 2 protects the quantum dot QD, and carriers can be injected into the quantum dot QD through discontinuities or pores in the adduct 2. A "porous discontinuous film" may mean a film having discontinuities and having porous regions other than the discontinuities.
[0021] 6 is a cross-sectional view showing another example of the configuration of the quantum dot adduct shown in FIG. 6. As shown in FIG. 6, the adduct 2 may be porous and may include a continuous film with a non-uniform thickness that surrounds the quantum dot QD in a cross section passing through the quantum dot QD. With this configuration, the adduct 2 protects the quantum dot QD, and carriers can be injected into the quantum dot QD through the pores of the adduct 2 or through thin portions of the adduct 2. The minimum thickness of the adduct 2 may be 1 nm or less.
[0022] 2 to 6 , the quantum dot adduct 1 according to the present disclosure includes a quantum dot QD and an adduct 2 located at least partially around the quantum dot QD, and the adduct 2 is at least one of a discontinuous film, an uneven thickness, a porous film, and a portion having a thickness of 1 nm or less. The quantum dot adduct 1 may further include an element 6 for passivating surface defects of the quantum dot QD. The element 6 may be a halogen.
[0023] (Manufacturing Method) The manufacturing method of the light-emitting element 10 according to the present disclosure may be any manufacturing method, and the light-emitting element 10 may be manufactured using common materials and common film-forming and sealing processes. For example, an alcohol solution in which the quantum dot adduct 1 is dispersed may be applied by spin coating, slit coating, or the like to form the light-emitting layer 14. For example, the quantum dot adduct 1 may be mixed with a solvent for viscosity control, and an ink containing the quantum dot adduct 1 may be printed by inkjet printing, screen printing, or the like to form the light-emitting layer 14. The printing method is suitable for producing light-emitting panels and display panels because it can uniformly form the light-emitting layer 14 over a large area.
[0024] Example 1 A quantum dot adduct 1 and a light-emitting device 10 according to an example of the present disclosure will be described below. A quantum dot adduct 1 and a light-emitting device 10 were prepared using commercially available red quantum dots as the quantum dots QD and zinc chloride (ZnCl) as the halogen source. 2 ) 0.02 [mol / L] of ethanol (C 2 H 6A solution of tetramethyl orthosilicate (TMOS) was prepared as a precursor for adduct 2. The red quantum dots had a core of ZeSeTe, a shell of ZeS, and an organic ligand. The following chemical formula (1) shows TMOS. Octane (C) was used as a solvent. 8 H 18 ) and N-methylformamide (NMF) were prepared.
[0025] 7 and 8 are diagrams illustrating a method for manufacturing a quantum dot adduct according to one embodiment of the present disclosure. As shown in FIG. 7 , a first liquid L1 containing quantum dots (QDs) dispersed in octane was mixed with a zinc chloride ethanol solution and held at room temperature for approximately one hour. Stirring may be performed using a stirrer or similar device. This process inactivates chlorine in the remaining defects (not deactivated by ligands) on the surface of the quantum dots (QDs). In FIG. 7 , active defects are indicated by crosses, and deactivated defects or chlorine in the defects are indicated by circles. In the first liquid L1, chlorine was coordinated to the quantum dots (QDs) in addition to the organic ligands described above. The first liquid L1 could be used directly in subsequent processes, or the first liquid L1 could be centrifuged to separate the quantum dots (QDs) coordinated with the organic ligands and chlorine. The quantum dots (QDs) could then be dispersed again in pure octane to form a new first liquid L1 for subsequent processes. A second liquid L2 was also prepared by dissolving TMOS in NMF. In the first liquid L1, the quantum dots QD were coordinated with the aforementioned organic ligands. The concentration of TMOS in the second liquid L2 was 0.02 mol / L.
[0026] Next, the first liquid L1 and the second liquid L2 were thoroughly stirred and mixed, as shown in Figure 8. During the stirring process, the halogen also coordinated with the quantum dots QDs, deactivating some of the defects in the quantum dots QDs. The quantum dots QDs also migrated from the first liquid L1 to the second liquid L2.
[0027] A quantum dot adduct 1 was formed in the second liquid L2. TMOS reacted to synthesize silicon oxide. Because the reaction occurred near room temperature, the silicon oxide had a trigonal crystal system. The crystal systems of the ZeS in the quantum dot QD shell and silicon oxide differ, resulting in significantly different lattice constants. Therefore, a large lattice mismatch occurs between the ZeS in the quantum dot QD shell and the silicon oxide grown thereon. Furthermore, the melting point of silicon oxide is 1710°C. For this reason, silicon oxide synthesized in contact with quantum dot QDs at a temperature much lower than the melting point of over 1000°C, such as near room temperature, is difficult to grow into a single crystal and is likely to become polycrystalline, amorphous, or porous. In addition, some silicon elements bond with hydroxyl groups (-OH) and / or some silicon oxide is converted into water (H 2 The inorganic film containing silicon oxide and silicic acid was disposed at least partially around the quantum dots (QDs).
[0028] Subsequently, the solvent was replaced with alcohol. Specifically, the first liquid L1 was removed, and ethyl acetate was added to the second liquid L2 to precipitate and separate the quantum dot adduct 1. The quantum dot adduct 1 was then dispersed in ethanol. Other alcohols such as methanol and IPA may be used instead of ethanol. The alcohol converts silicon oxide and silicic acid into water (H 2 O) to prevent water from corroding the quantum dots QDs.
[0029] The quantum dot adduct 1 was again precipitated and separated with ethyl acetate, and dispersed in alcohol. Because silicon oxide and silicic acid tend to retain water, it is desirable to repeat alcohol dehydration multiple times. In this example, alcohol dehydration was performed twice. Hereinafter, "the quantum dot adduct according to Example 1" refers to the quantum dot adduct 1 after the second alcohol dehydration.
[0030] Next, the quantum dot adduct 1 according to Example 1 was used to manufacture the light emitting device 10 according to Example 1, and the device characteristics and service life of the light emitting device 10 were measured. In addition, a solution of the quantum dot adduct 1 according to Example 1 was analyzed by Fourier transform infrared spectroscopy (FTIR).
[0031] Comparative Example 1 In Comparative Example 1, the commercially available red quantum dots described above were used instead of the quantum dot adduct 1, and otherwise a light-emitting device according to Comparative Example 1 was manufactured in the same manner as the light-emitting device 10 according to Example 1, and the device characteristics and service life were measured. In addition, the commercially available red quantum dots were analyzed by Fourier transform infrared spectroscopy (FTIR). Hereinafter, "quantum dots according to Comparative Example 1" refers to the commercially available red quantum dots.
[0032] 9 to 12 are graphs showing the element characteristics (voltage-luminance characteristics, voltage-current density characteristics, current density-luminance characteristics, and current density-luminous efficiency characteristics) of the light-emitting elements according to Example 1 and Comparative Example 1. In each figure, points for Example 1 and Comparative Example 1 are indicated by triangles and circles, respectively, and the points are connected by solid lines.
[0033] As shown in Figures 9 to 12, compared to Comparative Example 1, the light-emitting device according to Example 1 has a turn-on voltage in the luminance-voltage characteristics (see Figure 9) that is only about 2 V higher, even though the quantum dots QDs are protected by insulating silicon oxide. Furthermore, as with Comparative Example 1, the luminance of the light-emitting device according to Example 1 increases with increasing voltage at voltages higher than the turn-on voltage. This result is thought to indicate that in Example 1, the additive 2 protecting the quantum dots QDs is at least one of a discontinuous film, an uneven thickness, a porous film, and a film having a thickness of 1 nm or less, and therefore no excessive voltage is required for carrier transport to the QDs.
[0034] 13 and 14 are graphs showing the emission luminance and driving voltage over time of the light-emitting elements according to Example 1 and Comparative Example 1 in a constant current test. The horizontal axis in each diagram indicates time from the start of light emission. The left vertical axis indicates relative luminance, with the emission luminance of each light-emitting element at the start of light emission taken as 100%. The right vertical axis indicates relative voltage, with the driving voltage of each light-emitting element at the start of light emission taken as 100%. In each diagram, the relationship between luminance and time is shown by a solid line, and the relationship between voltage and time is shown by a dashed line. In this constant current test, a current of 25 mA / cm was applied to the light-emitting elements. 2A current of 100 cd / m s was applied at 25° C. The luminance at the start of light emission in this constant current test was 341 cd / m s for the light-emitting element 10 according to Example 1. 2 ], and the light emitting device according to Comparative Example 1 had a luminance of 157 [cd / m 2 〕 was the case.
[0035] As shown in Fig. 13, the light-emitting device according to Example 1 exhibited a characteristic in which the luminance increased from the start of light emission until about 91 hours later (so-called "positive aging"). Here, the positive aging time was defined as the time elapsed until the sign of the time differential of the luminance, calculated by least squares approximation, changed from positive (positive aging) to negative (deterioration). This is thought to be due to the improvement in the EQE according to Example 1 due to the application of current. The luminance was approximately 341 [cd / m 2 ] to about 390 [cd / m 2 ], which is a large improvement of about 1.14 times, or equivalent to an EQE of 9% from the initial 8%. Note that the light extraction efficiency of a light-emitting element is determined by the refractive index of each material, and the light extraction efficiency of light-emitting elements using a glass substrate and a general organic carrier transport material, metal oxide, etc. does not exceed 20%. Therefore, in the light-emitting element according to Example 1, the IQE (internal quantum efficiency) after 26 hours of application of electricity exceeds 45%.
[0036] This positive aging is a phenomenon specific to Example 1, and is thought to be the result of the additive 2 gradually inactivating the surface defects of the quantum dots QDs through electrochemical reactions, electrophoresis, or the like.
[0037] 14, the light-emitting device according to Comparative Example 1 does not exhibit positive aging, and the luminance rapidly and monotonically decreases with the passage of current. 2 ] to about 13 [cd / m 2], which is approximately one-twelfth of the original value. This is thought to be because the quantum dots of Comparative Example 1 were only protected by organic ligands, and so degradation progressed rapidly when a current was applied. The degradation may include degradation of the organic ligand itself or dissociation of the organic ligand from the quantum dots. Because the degradation was so rapid, it is thought that practical use in display panels and the like would be difficult.
[0038] For the relationship between luminance and time in Example 1, a fitting function using the least squares method was applied to the measured values from 91 hours to 130 hours so that the application results would form a straight line on a semi-logarithmic graph. According to the reliability test results of this example, slight positive aging was observed in the region up to 91 hours, so the fitting function was applied to the period from 91 hours to 130 hours, where luminance changes with time at a negative slope. For the relationship between luminance and time in Comparative Example 1, a fitting function using the least squares method was applied to the measured values from 20 hours to 130 hours so that the application results would form a straight line on a semi-logarithmic graph. The LT50 and LT95 were calculated from the application results. "LT95" indicates an estimated lifetime (lifetime) until the luminance of the light-emitting element reaches 95% of its initial value, and "LT50" indicates an estimated lifetime until the luminance of the light-emitting element reaches 50% of its initial value.
[0039] 15 and 16 are diagrams showing estimated values of useful life of the light emitting elements according to Example 1 and Comparative Example 1, respectively. Generally, in a nanoLED, the initial value of the light emission luminance is L 0 The lifetime LT(x, P) until the luminance reaches x [%] of the initial value when (P) is reached, and the initial value of the luminance is L 0 (Q) and the lifetime LT(x, Q) until the luminance reaches x [%] of the initial value. 0 (P), L 0 It is known that the following relational expression holds regardless of (Q) and x: This relational expression is called the "reliability calculation formula."
[0040] LT(x, P) × {L 0 (P)} n =LT(x,Q)×{L 0 (Q)} n= constant n is a coefficient that depends on the nanoLED, and n=1.8.
[0041] As shown in FIGS. 15 and 16, when the initial luminance is 100 [cd / m 2 ], the L50 of Comparative Example 1 was about 0.1 hours, whereas the LT50 of Example 1 was about 380,000 hours, achieving reliability more than one million times higher. Therefore, according to Example 1, the efficiency of carrier injection into the quantum dots QDs could be improved, and a light-emitting element 10 with a high EQE and a long service life could be realized.
[0042] In Non-Patent Document 1, quantum dots are completely covered with a dense continuous film of silicon oxide. According to Non-Patent Document 1, reliability is improved compared to light-emitting devices using quantum dots protected only with organic ligands, but only by about three times. In the quantum dot-containing light-emitting device described in Non-Patent Document 1, positive aging due to current flow is thought to be absent because only a small amount of organic ligand is present inside the continuous film and the continuous film is not in direct contact with the quantum dots. Furthermore, since carrier injection into the quantum dots in Non-Patent Document 1 is via the π electrons of organic cyclic molecules mixed into silicon oxide, it is speculated that the actual carriers injected into the quantum dots are insufficient. Furthermore, since carrier injection into the quantum dots in Non-Patent Document 1 is via organic molecules, it is speculated that even cyclic molecules are unable to reduce degradation due to electrochemical reactions.
[0043] 17 and 18 are diagrams showing the results of FTIR (Fourier transform infrared spectroscopy) of the quantum dot adduct according to Example 1 and the quantum dot solution according to Comparative Example 1, respectively. As shown in FIG. 18, in Comparative Example 1, only a peak corresponding to the C-H bond of the organic ligand is observed. On the other hand, as shown in FIG. 17, in Example 1, in addition to the peak corresponding to the C-H bond, a peak corresponding to the Si-O bond of silicon dioxide appears in the range of 1000 to 1200 [cm -1 ], and a broad peak corresponding to the Si-OH bond of silicic acid is observed at 2600 to 3600 [cm -1]. Therefore, it can be seen that the quantum dots in Example 1 are protected by an inorganic film containing silicon dioxide and silicic acid, while the quantum dots in Comparative Example 1 are not protected by an inorganic film. Hereinafter, for the sake of simplicity, the "peak corresponding to the ... bond" will be referred to as the "... peak."
[0044] Silicon oxide naturally (i.e., when only silicon oxide is produced) forms a dense and continuous inorganic film. Silicic acid is insoluble in acid and inhibits the synthesis of silicon oxide. Therefore, an appropriate amount of silicic acid helps form an inorganic film containing silicon oxide and silicic acid so that the inorganic film is at least one of discontinuous, non-uniform in thickness, porous, and / or has portions with a thickness of 1 nm or less. On the other hand, excess silicic acid forms a dense and continuous film with silicon dioxide, covering the quantum dots (QDs). Thus, silicic acid plays an important role in protecting and insulating the quantum dots (QDs). The amount of silicic acid produced can be adjusted by the amount of TMOS.
[0045] In Example 1, the amount of silicic acid is appropriate, and it is presumed that the inorganic film containing silicon oxide and silicic acid is at least one of the following: a discontinuous film, an uneven thickness, a porous film, or a film having a thickness of 1 nm or less. In addition, due to differences in crystal system and lattice constant, silicon oxide is unlikely to form a continuous film on the quantum dot adduct 1 if at least one of the following two conditions is met: one of the two conditions is that the TMOS is less than 0.02 mol / L; and the other is that silicon oxide is synthesized at a low temperature below room temperature.
[0046] In Non-Patent Document 1, the results of FTIR are about 800 to 3200 [cm -1 ] range, but 3200 [cm -1], it is believed that the material in Non-Patent Document 1 does not contain silicic acid. Furthermore, in Non-Patent Document 1, the quantum dots are protected with silicon dioxide, and the intensity of the C-H peak is similar to the intensity of the Si-O peak, indicating the presence of cyclic organic molecules that contribute to carrier injection into the quantum dots. In contrast, in Example 1 of the present disclosure, the intensity of the C-H peak is less than one-tenth of the Si-O peak, and in Comparative Example 2, the intensity of the C-H peak is less than one-half of the Si-O peak. Therefore, it is believed that the inorganic films of Example 1 and Comparative Example 2 do not contain organic cyclic structures or contain only trace amounts, and that cyclic organic molecules do not contribute to carrier injection into the quantum dots. In particular, the C-H peak in Example 1 is very weak, completely different from that in Non-Patent Document 1.
[0047] [Embodiment 2] Another embodiment of the present disclosure will be described below. For ease of explanation, the same reference numerals will be used to designate components having the same functions as those described in the above embodiment, and the description thereof will not be repeated.
[0048] Fig. 19 is a cross-sectional view showing an example of the configuration of a display device according to an embodiment of the present disclosure. As shown in Fig. 19, a display device 100 according to the present disclosure includes a light-emitting element 10 according to an embodiment of the present disclosure. The light-emitting element 10 may be the light-emitting element 10 described in the first embodiment above, or may be an improved or modified version of the light-emitting element 10 described in the first embodiment above.
[0049] The display device 100 may include a display unit 30 including a plurality of sub-pixels X, and a driver circuit 25 that drives the plurality of sub-pixels X. At least one of the plurality of sub-pixels X may include a light-emitting element 10 and a pixel circuit 20.
[0050] The present disclosure is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present disclosure.
[0051] REFERENCE SIGNS LIST 1 quantum dot adduct 2 adduct 10 light emitting element 12 first electrode 14 light emitting layer 16 second electrode 100 display device QD quantum dot
Claims
1. A light-emitting element comprising: a first electrode and a second electrode facing each other; and a light-emitting layer provided between the first electrode and the second electrode, the light-emitting layer including quantum dots and an additive located at least partially around the quantum dots, the additive being at least one of a discontinuous film, having a non-uniform thickness, being porous, and having a portion having a thickness of 1 nm or less.
2. The light-emitting device according to claim 1, wherein the additive is in direct contact with the quantum dot.
3. The light-emitting device according to claim 1 or 2, wherein the band gap of the additive is wider than the band gap of the material constituting the quantum dots.
4. The light-emitting element according to claim 3, wherein the quantum dot has a core and a shell surrounding the core, and the band gap of the additive is wider than the band gap of a material constituting the shell.
5. The light-emitting device according to claim 3 or 4, wherein the attachment is insulating.
6. The light-emitting element according to any one of claims 1 to 5, wherein the additive contains silicon oxide.
7. The light-emitting element according to any one of claims 1 to 5, wherein the additive contains silicic acid.
8. The light-emitting element according to any one of claims 1 to 5, wherein the additive contains titanium oxide.
9. The light-emitting element according to any one of claims 1 to 5, wherein the additive contains aluminum oxide.
10. The light-emitting device according to any one of claims 1 to 5, wherein the additive comprises zinc chloride.
11. The light-emitting device according to any one of claims 1 to 5, wherein the additive comprises silicon nitride.
12. The light-emitting element according to any one of claims 1 to 5, wherein the additive comprises one selected from the group consisting of boron oxide, phosphorus oxide, germanium oxide, beryllium fluoride, arsenic sulfide, silicon selenide, germanium sulfide, tellurium oxide, bismuth oxide, vanadium oxide, antimony oxide, lead oxide, copper oxide, zirconium fluoride, aluminum fluoride, indium fluoride, and zinc bromide.
13. The light-emitting device according to any one of claims 1 to 12, wherein the additive includes at least one of polycrystalline and amorphous.
14. The light-emitting element according to claim 13, wherein the maximum thickness of the additive is 2 nm or more.
15. The light-emitting device according to any one of claims 1 to 14, wherein the additive is porous.
16. The light-emitting device according to claim 15, wherein the appendage comprises a continuous film surrounding the quantum dot at a cross section through the quantum dot.
17. The light-emitting device according to any one of claims 1 to 14, wherein the attachment is solid.
18. The light-emitting device according to claim 15 or 17, wherein the appendage comprises a discontinuous film disposed around the quantum dot in a cross section through the quantum dot.
19. The light-emitting device according to claim 15 or 17, wherein the appendage comprises a continuous film of non-uniform thickness surrounding the quantum dot in a cross section through the quantum dot.
20. The light-emitting element according to claim 19, wherein the minimum thickness of the additive is 1 nm or less.
21. A display device comprising the light-emitting element according to any one of claims 1 to 20.
22. A quantum dot adduct comprising a quantum dot and an adduct located at least partially around the quantum dot, the adduct being at least one of a discontinuous film, having a non-uniform thickness, being porous, and having a portion having a thickness of 1 nm or less.
Citation Information
Patent Citations
Core-shell perovskite quantum dot and preparation method thereof, quantum dot composition and quantum dot device with quantum dot composition
CN112521933A
Semiconductor structures having polymer and insulator coatings, and compositions and methods for forming same
JP2020507801A
Fluorescent particle, with semiconductor nanoparticles dispersed therein, fabricated by the sol-gel process
WO2011081037A1
Light emitting device
WO2020194409A1
Cited By
Light-emitting element and light-emitting device
WO2026159806A1
Light-emitting element and display device
WO2026159807A1