Structural material and method for manufacturing same

The structural material with silicon particles distributed around the periphery of titanium diboride bodies, combined with an impregnation method using molten silicon, addresses the strength reduction issue in titanium diboride at high temperatures by forming a stable SiO2 film, enhancing oxidation resistance and maintaining mechanical strength.

WO2024201915A1PCT designated stage expired Publication Date: 2024-10-03TOHOKU UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/013244
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Titanium diboride structural materials experience significant strength reduction at high temperatures due to oxidation, as the protective boron oxide coating evaporates, and the addition of silicon compounds, while providing oxidation resistance, can embrittle grain boundaries and reduce strength.

Method used

A structural material comprising a sintered titanium diboride body with silicon particles distributed around its periphery, particularly in voids and grain boundaries, and an impregnation method using molten silicon to form a stable SiO2 protective film, maintaining mechanical strength and oxidation resistance.

Benefits of technology

The solution effectively prevents internal oxidation and maintains mechanical strength at high temperatures while achieving oxidation resistance through a stable SiO2 film, preventing grain boundary destruction and maintaining electrical conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023013244_03102024_PF_FP_ABST
    Figure JP2023013244_03102024_PF_FP_ABST
Patent Text Reader

Abstract

A structural material (100) according to the present invention comprises: a sintered body (101) containing titanium diboride as the main component; and a plurality of silicon particles (102) distributed in the outer peripheral part (101A) of the sintered body.
Need to check novelty before this filing date? Find Prior Art

Description

Structural materials and their manufacturing methods

[0001] The present invention relates to a structural material and a method for manufacturing the same.

[0002] Titanium diboride (TiB 2 The structural material of titanium diboride is a type of ultra-high temperature ceramic with a melting point of 3000°C or higher, and is expected to be a high-temperature structural material with electrical conductivity, but it is known to be vulnerable to high-temperature oxidation. The mechanical strength of the structural material of titanium diboride is significantly reduced in the high-temperature range of 1000°C or higher. In the low-temperature range of 700°C to 1000°C, boron oxide (B 2 O 3 ) is formed and functions as a protective coating. However, in high temperature regions, this protective coating evaporates, causing rapid oxidation inside the structural material and resulting in a decrease in strength.

[0003] In order to prevent the deterioration of strength due to oxidation in high temperature regions, silicon compounds (SiC, MoSi 2 In the high temperature range, the surface of the structural material to which silicon compounds are added is covered with SiO, which is stable even at high temperatures. 2 The glass phase formed prevents oxidation inside the structural material. However, it has been found that the addition of this silicon compound causes a decrease in strength due to a mechanism other than oxidation (Non-Patent Document 1). The Si distributed inside the structural material is converted into TiB 2 This is thought to be due to the fact that the grain boundaries are embrittled, inducing grain boundary fracture.

[0004] BR Golla, A. Mukhopadhyay, B. Basu, SK Thimmappa, Prog. Mater. Sci. 111 (2020) 100651

[0005] The present invention has been made in view of the above circumstances, and aims to provide a structural material that has oxidation resistance and is capable of maintaining strength in high-temperature environments, and a method for manufacturing the same.

[0006] In order to solve the above problems, the present invention employs the following means.

[0007] (1) A structural material according to one aspect of the present invention includes a sintered body containing titanium diboride as a main component, and a plurality of silicon particles distributed on the outer periphery of the sintered body.

[0008] (2) In the structural material described in (1) above, some of the silicon particles may be distributed in voids contained in the outer periphery.

[0009] (3) In the structural material according to either (1) or (2) above, another portion of the plurality of silicon particles may be distributed at grain boundaries included in the outer periphery.

[0010] (4) In the structural material according to any one of (1) to (3) above, the number density of the silicon particles may decrease with increasing distance from the surface of the sintered body.

[0011] (5) In the structural material according to any one of (1) to (4) above, the sintered body may contain a boride of a transition metal.

[0012] (6) In the structural material according to any one of (1) to (5) above, the open porosity of the sintered body is preferably 1% or less.

[0013] (7) A method for manufacturing a structural material according to one aspect of the present invention is a method for manufacturing a structural material according to any one of (1) to (6) above, which includes an impregnation step of impregnating the sintered body with molten silicon.

[0014] (8) In the method for manufacturing a structural material described in (7) above, it is preferable that the temperature of the molten silicon in the impregnation treatment step is set to 1420° C. or higher and 3225° C. or lower.

[0015] According to the present invention, it is possible to provide a structural material that has oxidation resistance and is capable of maintaining strength in a high-temperature environment, and a method for manufacturing the same.

[0016] 3A is an enlarged view of a portion of the structural material according to a first embodiment of the present invention; FIG. 1B is an enlarged view of a portion of the structural material according to FIG. 1A in a state in which the structural material according to the embodiment has been subjected to high-temperature oxidation; FIG. 3C is an enlarged view of a portion of the structural material according to the embodiment; FIG. 3D is an enlarged view of the outer periphery of the structural material in the backscattered electron image of FIG. 3A; FIG. 4A is an elemental mapping diagram of the cross section of the structural material according to Example 1; FIG. 4D is an enlarged view of the outer periphery of the structural material in the elemental mapping diagram of FIG. 4A; FIG. 4E is a graph showing the results of isothermal oxidation thermogravimetry performed on the structural materials of Examples 1 to 4 and Comparative Examples 1 and 2; FIG. 5 is a graph showing the results of crystalline phase identification performed by XRD measurement on the structural material of Example 1; FIG. 5F is a graph showing the results of crystalline phase identification performed by XRD measurement on the structural material of Example 2; FIG. 5G is a graph showing the results of crystalline phase identification performed by XRD measurement on the structural material of Example 3; FIG. 5H is a graph showing the results of crystalline phase identification performed by XRD measurement on the structural material of Example 4; FIG. 6 is a graph showing the change in open porosity of the structural materials of Examples 1 to 4.

[0017] A structural material according to an embodiment of the present invention and a manufacturing method thereof will be described in detail below with reference to the drawings. Note that the drawings used in the following description may show characteristic portions enlarged for ease of understanding, and the dimensional proportions of each component element may not necessarily be the same as those in reality. Furthermore, the materials, dimensions, etc. exemplified in the following description are merely examples, and the present invention is not limited thereto. Appropriate modifications may be made within the scope of the present invention.

[0018] 1A is a cross-sectional view of a structural material 100 according to a first embodiment of the present invention. The structural material 100 is mainly made of titanium diboride (TiB 2 ) and a plurality of silicon particles 102 distributed in an outer peripheral portion 101A of the sintered body 101. The shape of the silicon particles in this embodiment is not limited to granular (spherical, etc.) shapes, but also includes shapes extending along voids.

[0019] The sintered body 101 contains titanium diboride as a main component. The shape and size of the sintered body 101 are not particularly limited, but there is a preferred range for the porosity of the sintered body 101. As will be described later, during high-temperature oxidation of the sintered body 101, SiO 2 It is necessary to distribute an amount of silicon particles 102 sufficient to form the phase in the voids (open pores) that are connected to the outside of the sintered body. Hereinafter, the voids that are connected to the outside of the sintered body may be simply referred to as voids.

[0020] The sintered body 101 is obtained by sintering a powder containing titanium diboride as a main component. The sintering method is not particularly limited, but for example, spark plasma sintering may be used. The sintering temperature may be, for example, 1300°C to 2000°C, and the sintering time may be, for example, 5 minutes to 15 minutes. The pressure during sintering may be 50 MPa or more and 60 MPa or less.

[0021] 1B is an enlarged view of a portion P near the surface of the structural material of FIG. 1A. Silicon particles 102 are distributed mainly in voids contained in the outer periphery 101A of the sintered body. These voids are spaces formed between the crystal grains that make up the sintered body 101 when the sintered body 101 is formed.

[0022] The outer periphery 101A of the sintered body, in which the silicon particles 102 are distributed, is a region having a predetermined thickness D extending inward from the surface 101a, in other words, a region having a predetermined thickness D extending inward from the surface (outermost periphery) 101a in any cross section of the sintered body 101. No silicon particles 102 are distributed in the interior (central portion) 101B surrounded by the outer periphery 101A, and the state before the silicon particles 102 were distributed (immediately after sintering) is substantially maintained. The boundary 101b between the outer periphery 101A and the interior 101B of the sintered body can be confirmed using, for example, an electron probe microanalyzer (EPMA) or the like.

[0023] The number density of silicon particles 102 distributed in outer periphery 101A may be high enough to exhibit oxidation resistance at high temperatures, at least on the outermost surface. For example, when formed through an impregnation treatment process described later, the number density of silicon particles 102 distributed in outer periphery 101A tends to decrease with increasing distance from surface 101a of the sintered body, but may be uniform regardless of the distance (depth) from surface 101a of the sintered body, if possible.

[0024] FIG. 1B illustrates an example in which the silicon particles 102 are ideally distributed in voids at a uniform depth from the surface 101 a of the sintered body. However, in reality, the depth at which the silicon particles 102 are distributed often varies due to the random distribution of the voids.

[0025] Most of the silicon particles 102 are distributed in the voids, but some of the silicon particles 102 may be distributed at the grain boundaries (crystal grain boundaries) that make up the sintered body 100. These grain boundaries are contact surfaces between crystal particles that are in close contact with each other within the sintered body 101.

[0026] 1C is an enlarged view of a portion P of the structural material of FIG. 1A in a state where the structural material 100 has been oxidized at high temperature. The outer peripheral portion 101A of the sintered body 101 that has been oxidized at high temperature is made of SiO 2 SiO consisting of crystal grains 103 2 phase (glass phase). 2 The SiO phase can prevent oxidation inside the sintered body and improve the oxidation resistance. 2 The thickness of the phase is comparable to the thickness of the region where the silicon particles were distributed.

[0027] 2 is a diagram illustrating a method for manufacturing the structural material 100. The structural material 100 can be manufactured mainly through an impregnation process in which a sintered body 101 containing titanium diboride as a main component is immersed in molten silicon 105 contained in a predetermined container 104, and the molten silicon 105 is impregnated into the outer peripheral portion 101A of the sintered body 101.

[0028] The sintered body 101 is obtained by heating a powder containing titanium diboride as a main component while applying pressure. The powder to be heated may contain impurities to the extent that they do not significantly affect the physical properties of the sintered body 101, but it must not contain materials such as silicon that cause grain boundary fracture.

[0029] The molten silicon 104 is, for example, single crystal silicon that has been heated to a temperature equal to or higher than its melting point (1420° C.) and melted. During the impregnation treatment step, the temperature of the molten silicon is preferably set to 1420° C. or higher and 3225° C. or lower.

[0030] The heating for melting the single crystal silicon may be carried out before the sintered body 101 is impregnated, or may be carried out after the sintered body 101 is brought into contact with the single crystal silicon and simultaneously with the heating of the sintered body 101 .

[0031] As described above, the structural material 100 of this embodiment achieves both improved oxidation resistance and maintenance of high-temperature strength. In the structural material 100 of this embodiment, silicon particles 102 are distributed in the outer periphery 101A of the sintered body 101. Therefore, when oxidized at high temperature, the outer periphery 101A where the silicon particles 102 are distributed turns into stable SiO 2 This acts as a protective coating to prevent internal oxidation and improve oxidation resistance. Furthermore, in the structural material 100 of this embodiment, silicon particles 102 are not distributed in most of the inner part of the sintered body 101, excluding the outer peripheral portion 101A. This prevents grain boundary fracture originating from the silicon particles 102 during high-temperature oxidation, and allows mechanical strength to be maintained. Furthermore, because the inner part of the sintered body 101 is made of titanium boride, which is a conductive material, higher electrical conductivity can be achieved compared to when silicon particles 102 are distributed.

[0032] Second Embodiment In a structural material according to a second embodiment of the present invention, the sintered body is TiB 2 The transition metal boride contains TiB as the main component and further contains a transition metal boride. 2 It is sufficient if it does not significantly affect the physical properties (melting point, etc.) of the 2 , CrB 2 , TaB2 TiB etc. 2 The ratio of the volume of the boride of the transition metal to the volume of the sintered body is preferably 0 vol % or more and 20 vol % or less, and more preferably about 20 vol %. 2 The structure other than being a composite substrate is the same as that of the structural material 101 of the first embodiment, and the same effects as those of the structural material 101 are achieved.

[0033] The effects of the present invention will be more clearly understood from the following examples. Note that the present invention is not limited to the following examples and can be practiced with appropriate modifications within the scope of the present invention.

[0034] (Example 1) A structural material according to the first embodiment was manufactured. 2 The powder (purity 99%, particle size 2-3 μm) was subjected to discharge plasma treatment at 1600°C for 15 minutes at 60 MPa, and then sintered. This sintered body was cut into multiple pieces using an electric discharge machine and a low-speed saw. The size (volume) of each cut sintered body was approximately 18 mm. 3 In the impregnation process, each cut sintered body (40 mg or more, 100 mg or less) and a small piece of Si (1 g) were placed in a quartz tube for 10 minutes. -4 The quartz tube was sealed with Pa, and the quartz tube was heat-treated at 1450°C for 1 hour using an electric furnace. After the heat treatment, the structural material in which the sintered body was impregnated with Si was taken out from the quartz tube, and its surface was polished to #2000.

[0035] Example 2 A structural material according to the second embodiment was manufactured. 2 powder (purity 99%, particle size 2-3 μm) and ZrB 2 The powder (purity 97%, particle size 5-10 μm) of TiB was mixed with the powder of TiB, and the powder was subjected to a spark plasma treatment at 1800°C for 15 minutes at 60 MPa, and sintered. 2 powder and ZrB 2 The powders were mixed using a tabletop pot mill rotating table at 400 rpm for 24 hours. 2 ZrB relative to the volume2 The amount of powder to be mixed was adjusted so that the volume ratio of was about 20 vol %. The manufacturing conditions other than the selection of the sintered body were the same as in Example 1.

[0036] (Example 3) Another structural material according to the second embodiment was manufactured. 2 powder (purity 99%, particle size 2-3 μm) and CrB 2 The manufacturing conditions were the same as in Example 2, except that a mixed powder of the powders (1) and (2) was used.

[0037] Example 4 Another structural material according to the second embodiment was manufactured. 2 powder (purity 99%, particle size 2-3 μm) and TaB 2 The manufacturing conditions were the same as in Example 2, except that a mixed powder of the powders (1) and (2) was used.

[0038] Comparative Example 1 A structural material was manufactured from a sintered body that had not been subjected to the Si impregnation treatment. The sintered body was manufactured under the same conditions as in Example 1.

[0039] Comparative Example 2 Another structural material was manufactured from a sintered body that had not been subjected to the Si impregnation treatment. The sintered body was manufactured under the same conditions as in Example 2.

[0040] The structural material obtained in Example 1 was subjected to elemental mapping analysis using EPMA. Fig. 3A is a backscattered electron image of a cross section of the structural material. Fig. 3B is a backscattered electron image of a part P of the outer periphery of the structural material in the backscattered electron image of Fig. 3A. 1 4A is an enlarged image of the same cross section as in FIG. 3A. FIG. 4B is an enlarged image of the same outer peripheral portion P as in FIG. 3B in the Si element mapping diagram of FIG. 4A. 1 This is an enlarged view.

[0041] 4A, it can be seen that the structural material is formed with an outer periphery 101A where silicon particles are distributed and an inner portion 101B where silicon particles are not distributed. The thickness of outer periphery 101A, i.e., the width of the region where silicon particles are distributed, is about 0.4 to 1.0 mm as measured from surface 101a.

[0042] As shown in FIG. 3B, the outer peripheral portion 101A of the sintered body is formed of TiB2 It can be seen that voids 106 are formed between the crystal grains. From Fig. 4B, it can be seen that silicon particles are distributed at the positions of these voids 106. It can also be seen that more silicon particles 102 are distributed in the relatively large voids 106, grain boundary triple junctions, etc.

[0043] Thermogravimetry was performed at 1300°C on the structural materials of Examples 1 to 4 and Comparative Examples 1 and 2. Figure 5 is a graph showing the results. The horizontal axis of the graph represents the measurement time (minutes). The left and right vertical axes of the graph represent the temperature (°C) and the oxidation mass gain (%), respectively. The oxidation mass gain is the mass gain due to oxidation normalized by the mass before measurement.

[0044] In the structural materials of Comparative Examples 1 and 2, which were not impregnated with Si, the mass increased rapidly around 100 minutes into the measurement, and continued to increase over time. In contrast, the structural material of Example 1, which was impregnated with Si, did not exhibit the same rapid increase in mass as Comparative Examples 1 and 2, and the mass increase trend was more gradual than in Comparative Examples 1 and 2. In the structural materials of Examples 2 to 4, the mass increase trend was even more gradual (almost constant) than in Example 1. These results demonstrate that the Si impregnation treatment in the structural materials of Examples 1 to 4 suppresses internal oxidation of the structural material, improving oxidation resistance. In particular, it can be seen that oxidation is almost completely suppressed in the structural materials of Examples 2 to 4.

[0045] Crystalline phases were identified by XRD measurement for the structural materials of Examples 1 to 4. Fig. 6 is a graph showing the results for the structural materials of Example 1 and Comparative Example 1. Fig. 7 is a graph showing the results for the structural materials of Example 2 and Comparative Example 2. Fig. 8 is a graph showing the results for the structural material of Example 3. Fig. 9 is a graph showing the results for the structural material of Example 4. The horizontal axis of the graph represents the diffraction angle, and the vertical axis of the graph represents the diffraction intensity.

[0046] On the surface of the structural materials of Comparative Examples 1 and 2, only the transition metal oxides (metal borides, etc.) contained in the sintered body were identified. On the other hand, on the surface of the structural materials of Examples 1 to 4, SiO was identified in addition to the transition metal oxides contained in the sintered body. 2These results suggest that the Si impregnation treatment produces SiO on the surface of the sintered body, which acts as an oxidation-resistant protective film. 2 It is clear that a phase is formed.

[0047] The sintered bodies of Examples 1 to 4 were measured for changes in open porosity before and after the Si impregnation treatment using EPMA. Figure 10 is a graph showing the measurement results. The horizontal axis of the graph indicates the timing of the measurement (before or after the Si impregnation treatment), and the vertical axis of the graph indicates the open porosity (%). The open porosity was 42.0 mm 2 The measurement was carried out in an area of ​​(surface area of ​​a rectangular parallelepiped (3.0 mm x 3.0 mm x 2.0 mm)).

[0048] These results show that before the Si impregnation treatment, there was a large difference in open porosity between Examples 1 to 4, but after the Si impregnation treatment, this difference almost disappeared, falling within 1% in all cases. This is thought to be because the Si impregnation treatment allowed silicon particles to penetrate the sintered compact through the open pores, filling the open pores in the periphery of the sintered compact with silicon particles.

[0049] According to the present invention, it is possible to provide a structural material that has oxidation resistance and is capable of maintaining strength in a high-temperature environment, and a method for manufacturing the same.

[0050] 100 Structural material 101 Sintered body 101A Periphery of sintered body 101B Inside of sintered body 101a Outermost surface of sintered body (structural material) 101b Boundary between the periphery and inside of sintered body 102 Silicon particle 103 SiO 2 Crystal grains 104 Container 105 Molten silicon 106 Voids in sintered body D Thickness of outer periphery P Part of structural material P 1 Part of the outer periphery of the structural material R Average diameter

Claims

1. A structural material comprising a sintered body containing titanium diboride as a main component, and a plurality of silicon particles distributed on the outer periphery of the sintered body.

2. The structural material according to claim 1, characterized in that a portion of the plurality of silicon particles are distributed in voids contained in the outer periphery.

3. A structural material according to claim 1 or 2, characterized in that another portion of the plurality of silicon particles is distributed at grain boundaries contained in the outer periphery.

4. A structural material according to claim 1 or 2, characterized in that the number density of said silicon particles decreases with increasing distance from the surface of said sintered body.

5. The structural material according to claim 1 or 2, characterized in that the sintered body contains a boride of a transition metal.

6. A structural material according to claim 1 or 2, characterized in that the open porosity of said sintered body is 1% or less.

7. A method for manufacturing a structural material according to claim 1 or 2, comprising an impregnation step of impregnating the sintered body with molten silicon.

8. The method for manufacturing a structural material according to claim 7, characterized in that the temperature of the molten silicon in the impregnation process is 1420°C or higher and 3225°C or lower.

Citation Information

Patent Citations

  • Method for preparing titanium-diboride-based ceramic composite material

    CN105084902A

  • Titanium boride-based composite cathode material and preparation method thereof

    CN106278281A

  • Preparation method of low-cost titanium boride ceramic composite material

    CN113582700A

  • Sintered body by electric discharge of titanium diboride

    JP1979090312A

  • Die for sintering, and manufacturing method thereof