Adhesive structure, semiconductor device, motor, flying object, and method for manufacturing adhesive structure
The bonded structure, with a porous epoxy resin thin film impregnated adhesive, addresses the brittleness and low adhesive strength of conventional high-temperature adhesives by providing flexibility and maintaining adhesive strength under thermal stress, ensuring reliable bonding in high-temperature applications.
Patent Information
- Application Number
- PCT/JP2023/013557
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional high-temperature heat-resistant adhesives used in semiconductor devices and motor drive parts are brittle and lack sufficient adhesive strength, leading to issues with thermal stress and cracking due to temperature cycling, especially when using pressure-sensitive adhesives.
A bonded structure featuring a thin film made of epoxy resin with pores impregnated with a high-strength adhesive, utilizing a phase-separable mechanism to create a dimensionally continuous network skeleton, which provides flexibility and maintains adhesive strength under thermal stress.
The adhesive structure effectively relieves thermal stress and maintains excellent adhesive properties, enabling reliable bonding in high-temperature applications and withstanding severe temperature cycles without cracking or peeling, even with differing thermal expansion coefficients.
Smart Images

Figure JP2023013557_03102024_PF_FP_ABST
Abstract
Description
Adhesive structure, semiconductor device, motor, flying object, and method of manufacturing adhesive structure
[0001] The present application relates to a bonded structure, a semiconductor device, a motor, a flying object, and a method for manufacturing a bonded structure.
[0002] In recent years, efforts have been made to improve the high-temperature resistance of semiconductor devices and motor drive parts, and heat resistance is also being demanded of adhesives used to bond these components. Epoxy adhesives are an example of adhesives that have high adhesive strength and can withstand high temperatures. While traditionally used epoxy adhesives have only a heat resistance of around 180°C at most, adhesives with heat resistance of over 200°C have recently begun to appear on the market.
[0003] However, adhesives with high heat resistance generally have issues such as brittle cured products and poor adhesive strength.In addition, when thermal stress is applied due to temperature cycling, the adhesive strength cannot be guaranteed, resulting in cracks or peeling from the adherend.
[0004] In order to sufficiently relieve the thermal stress of the adhesive between a semiconductor element and a wiring circuit board in the application of bonding to a semiconductor device, for example, Patent Document 1 discloses an adhesive sheet having a structure in which adhesive layers are formed on both sides of a sheet-like porous substrate.
[0005] JP 2000-17240 A (paragraph 0010, Figure 1)
[0006] However, the adhesive sheet disclosed in Patent Document 1 has a problem in that it cannot exhibit the strength required for structural adhesion because it uses a pressure-sensitive adhesive in the adhesive layer.
[0007] The present application has been made to solve the above-mentioned problems, and aims to provide an adhesive structure, a semiconductor device, a motor, a flying object, and a method for manufacturing an adhesive structure that can sufficiently relieve thermal stress and has excellent adhesiveness.
[0008] The bonded structure disclosed in the present application is characterized by comprising a thin film made of an epoxy resin in which pores are formed by a porous skeleton, and the pores of the thin film are impregnated with an adhesive.
[0009] The semiconductor device disclosed in the present application is characterized by comprising a semiconductor element provided on the surface of a substrate via the above-mentioned adhesive structure, bonding wires connecting electrodes provided on the surface of the substrate to electrodes provided on the surface of the semiconductor element, and a sealing resin that seals the semiconductor element.
[0010] The motor disclosed in the present application is characterized by comprising a cylindrical steel plate attached to a shaft, and a magnet adhered to the outer periphery of the steel plate via the above-mentioned adhesive structure.
[0011] The flying object disclosed in the present application is a flying object equipped with a compressor, characterized in that the above-described adhesive structure is used to adhere sensors and components used in the compressor.
[0012] The method for manufacturing an adhesive structure disclosed in the present application is characterized by including a step of applying an epoxy resin solution onto a substrate and thermally curing it to form a thin film of a desired thickness, and a step of impregnating the thin film, which has been peeled off from the substrate, with an adhesive.
[0013] According to the present application, the bonded structure not only can sufficiently relieve thermal stress but also has excellent adhesive properties.
[0014] 1 is a cross-sectional view showing the configuration of an adhesive structure according to embodiment 1. FIG. 2 is a cross-sectional view showing a state in which adhesion is performed using the adhesive structure according to embodiment 1. FIG. 3 is a diagram showing the rate of change in adhesive strength of the adhesive structure according to embodiment 1. FIG. 4 is a cross-sectional view showing the configuration of a semiconductor device using the adhesive structure according to embodiment 2. FIG. 5 is a cross-sectional view showing the configuration of an SPM motor using the adhesive structure according to embodiment 3. FIG. 6 is a block diagram showing the configuration of an adhesive structure according to embodiment 4. FIG. 7 is a system flow diagram showing the flow of operation of an aviation system using the adhesive structure according to embodiment 4.
[0015] 1 is a cross-sectional view showing the configuration of an adhesive structure according to embodiment 1 of the present invention. As shown in Fig. 1, an adhesive structure 100 according to embodiment 1 is composed of a porous thin film 11 and an adhesive 13 impregnated in the porous thin film 11.
[0016] The porous thin film 11 is a thin film having a porous skeleton. The porous thin film 11 is composed of a resin that is cured by heating, mainly using an epoxy base resin and an amine-based curing agent. By adding a phase-separable material during curing, a polymerization-induced phase separation mechanism occurs, and parts where cross-linking polymerization occurs and parts where phase separation occurs are randomly formed during curing, making it possible to produce a porous thin film with a three-dimensionally continuous network skeleton and pores.
[0017] The epoxy monomers used herein include aromatic epoxy resins such as bisphenol A epoxy resins, hydrogenated bisphenol A epoxy resins, brominated bisphenol A epoxy resins, bisphenol F epoxy resins, bisphenol E epoxy resins, bisphenol AD epoxy resins, stilbene epoxy resins, biphenyl epoxy resins, bisphenol A novolac epoxy resins, cresol novolac epoxy resins, and epoxy resins containing heteroaromatic rings; and non-aromatic epoxy resins such as aliphatic glycidyl ether epoxy resins, aliphatic glycidyl ester epoxy resins, alicyclic glycidyl ether epoxy resins, and alicyclic glycidyl ester epoxy resins. While the number of epoxy groups in the monomer does not matter, difunctional or tetrafunctional epoxy monomers are preferred. These epoxy monomers may be used alone or in combination. Combinations of these monomers can alter properties such as flexibility, pore size, heat resistance, and strength / elongation.
[0018] Examples of curing agents include aromatic amines such as metaphenylenediamine, diaminodiphenylmethane, diaminodiphenyl sulfone, benzyldimethylamine, and dimethylaminomethylbenzene; aliphatic amines such as ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, iminobispropylamine, bis(hexamethylene)triamine, trimethylhexamethylenediamine, and polyetherdiamine; alicyclic amines such as isophoronediamine, 3,9-bis(3-aminopropyl)2,4,8,10-tetraoxaspiro(5,5)undecane adduct, bis(4-amino-3-methylcyclohexyl)methane, and bis(4-aminocyclohexyl)methane; heteroaromatic ring-containing amines; and modified products thereof. Non-aromatic curing agents such as aliphatic polyamidoamines composed of polyamines and dimer acids are also possible. These curing agents may be used alone or in combination of two or more. Here, the ratio of epoxy monomer to curing agent added is preferably in the range of 40 to 300 parts by weight per 100 parts by weight of uncured epoxy.
[0019] To form pores during thermal curing of a thermosetting resin, a phase-separation pore-forming agent must be selected to cause phase separation. The phase-separation pore-forming agent is selected from those capable of dissolving the uncured monomer (or polymer) and / or curing agent that constitute the epoxy resin. After the monomer (or uncured polymer) and curing agent are polymerized, the uncured monomer (or polymer) and / or curing agent that have phase-separated from the polymer are removed. Examples of phase-separation pore-forming agents include cellosolves such as methyl cellosolve and ethyl cellosolve, esters such as ethylene glycol monomethyl ether acetate and propylene glycol monomethyl ether acetate, glycols such as polyethylene glycol and polypropylene glycol, and ethers such as polyoxyethylene monomethyl ether and polyoxyethylene dimethyl ether. These phase-separation pore-forming agents may be used alone or in combination of two or more. Among these phase-separation pore-forming agents, it is preferable to use diethylene glycol, triethylene glycol, tetraethylene glycol, or polyethylene glycol. The amount of the phase separation pore-forming agent used is preferably 10 to 400 parts by weight per 100 parts by weight of the uncured epoxy / curing agent.
[0020] The adhesive 13 used alone has an adhesive strength of 10 MPa or more between SPCC (Steel Plate Cold Commercial) and SPCC, and exhibits physical properties of a glass transition temperature of 150° C. or more.
[0021] Examples of the adhesive 13 include a mixture of an epoxy resin having a high glass transition temperature, such as 4,4'-methylenebis(N,N-diglycidylaniline), N,N,N',N'-tetraglycidyl-4,4'-diamidodiphenylmethane, N,N,N',N'-tetraglycidyl-m-xylylenediamine, or 2,2'-diallylbisphenol A diallyl ether, and an aromatic amine, such as phenylenediamine, 4,4'-dimethyldiphenylmethane, 3,3'-diaminodiphenylsulfone, diaminocyclohexane, N,N'-diphenyl-1,4-phenylenediamine, or 4,4'-diaminodiphenyl ether. Alternatively, commercially available adhesives, such as Cemedine Y612, Panacol GTH-T, ThreeBond TB2237J, or ADEKA CLS-1194, which have high heat resistance and a higher elastic modulus than the porous thin film 11, can also be used.
[0022] Since the elastic modulus of these adhesives 13 is 2000 to 10,000 MPa, the difference in elastic modulus with the porous thin film 11 is large, and it is desirable that the ratio of the elastic modulus of the porous thin film 11 to the impregnated adhesive 13 be in the range of 2 to 20. If it is lower than 2, the effect of adding a thin film layer is weak, and if it exceeds 20, it is impossible for an organic material to exist. In addition, because the impregnated adhesive 13 is rigid, the adhesive itself has a small elongation rate of approximately 1 to 5%. By combining it with the porous thin film 11, the flexibility of the porous thin film 11 is imparted, preventing sudden cracks on the adhesive surface and dispersing stress, making it more resistant to stresses generated by temperature changes. In this case, the ratio of the elongation rates of the adhesive 13 to the porous thin film 11 is preferably in the range of 2 to 1000, more preferably in the range of 2 to 20. The thicker the porous thin film 11, the more difficult it is for the adhesive 13 to penetrate, so the thickness of the porous thin film 11 is preferably 1 mm or less, and more preferably 0.001 mm to 0.5 mm. A porous thin film 11 thinner than 0.001 mm cannot be produced, and if it exceeds 0.5 mm, the adhesive layer will be too thick during subsequent bonding, making it impractical.
[0023] Next, a method for manufacturing the porous thin film 11 used in the bonded structure 100 according to the first embodiment of the present invention will be described.
[0024] First, a mixed solution of an epoxy base resin, an amine-based curing agent, and a phase separation pore-forming agent is thoroughly stirred with a stirrer. Next, this epoxy solution is thinly applied to a pretreated substrate to obtain the desired thickness, and then thermally cured. Finally, the thermally cured epoxy thin film is peeled off from the substrate to obtain a porous epoxy thin film as the porous thin film 11. If necessary, the thin film can be washed with a solvent to obtain a thin film with a cleaner surface.
[0025] Here, the porous thin film 11 produced is characterized by having an elastic modulus in the range of 0.1 to 3000 MPa. Of these, a porous thin film 11 having an elastic modulus in the range of 10 to 1000 MPa is more preferable for improving adhesive reliability. It is known that the porous thin film 11 in this case has a pore diameter of 0.1 to 100 μm; if the pore diameter is smaller than 0.1 μm, the adhesive cannot be sufficiently impregnated. If the pore diameter is larger than 100 μm, a fine flexible structure cannot be obtained, and the effect is poor. A pore diameter of 0.5 to 10 μm is more preferable.
[0026] Furthermore, the porous thin film 11 produced has been found to have a glass transition temperature of 60 to 200°C. Porous thin films with temperatures below 60°C tend to have significantly reduced heat resistance, and while those above 200°C can be produced, they are rigid resins and therefore cannot ensure structural flexibility. A glass transition temperature of 100 to 140°C is desirable, as this results in good bonding reliability without cracking or peeling. The porous thin film 11 itself is known to be soft, exhibiting an elongation of approximately 3 to 50%. Here, if the elongation ratio with respect to the cured product is less than 2, sufficient curing is not achieved, and if it exceeds 1000, the heat resistance of the flexible structure is low, resulting in an unsuitability for high-heat-resistant applications.
[0027] The produced porous thin film 11 can be impregnated with the adhesive 13 to obtain an adhesive structure 100 having a porous structure. When the adhesive 13 is impregnated, it is possible to sufficiently impregnate the porous thin film 11 by applying a temperature lower than the curing temperature of the adhesive 13 and repeating vacuum degassing. The adhesive 13 used has an adhesive strength between SPCCs of 10 MPa or more after curing of the adherends and a glass transition temperature of 170°C to 300°C that is higher than the glass transition temperature of the porous thin film.
[0028] Although the adhesive structure 100 exhibits a decrease in the initial strength of the adhesive 13 due to the impregnation of the porous thin film 11 with the adhesive 13, the high adhesive strength of the adhesive 13 provides excellent adhesive strength in practical use. On the other hand, the configuration of the adhesive structure 100 allows for stress relaxation effects in environmental changes, enabling it to withstand temperature cycle tests with severe temperature differences, such as -20 to 130°C. Furthermore, when bonding materials with different thermal expansion coefficients, such as magnet / steel plate, aluminum / iron, invar / iron, and engineering plastics (polyether ether ketone, polyacetal, polycarbonate, polyethersulfone polyphenylene sulfide, polyimide, polyetherimide) / metal, there has been a problem of adhesive peeling due to the difference in the thermal expansion coefficients of the adherends during heat curing. However, the use of the adhesive structure 100 can solve this problem.
[0029] Furthermore, when using the bonded structure 100, surface treatments to improve adhesion can be performed, such as polishing the adherend surface with abrasive paper to improve surface roughness and obtain a new surface, air treatment, argon plasma treatment, deep ultraviolet light treatment, and corona discharge treatment, which are physical treatments that can be expected to improve adhesion and adhesive strength.
[0030] Similar effects can also be achieved by applying a silane coupling agent as a chemical treatment. For example, for epoxy adhesives, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldithoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-aminopropyltrimethoxysilane, 3-triethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, N-(phenylbenzyl)-2-aminoethyl-3-aminopropyltrimethoxysilane hydrochloride, or the like may be used as a primer. This not only alleviates stress during thermal curing, making the adhesive more flexible for use in places with large temperature differences, but also enables its use in areas where commercially available adhesives have not previously been used.
[0031] Fig. 2 is a diagram showing a state where bonding is performed using the bonded structure 100 according to the first embodiment of the present application. As shown in Fig. 2, it is the impregnated adhesive 13 that comes into direct contact with the adherend 12. In addition, the thickness of the adhesive 13 is generally also often designed, and the thickness of the bonded structure 100 is preferably 0.5 mm or less in order to satisfy the clearance with other components and the design tolerance.
[0032] Figure 3 shows the rate of change in adhesive strength of the bonded structure 100 according to the first embodiment of the present application. Figure 3 shows the results of a temperature cycle test (○: bonded structure 100, △: commercially available adhesive) in which the bonded structure 100 was bonded to an adherend 12, such as Invar steel, and subjected to 300 cycles at a temperature difference of -15 to 130°C. The results show that the adhesive strength of the commercially available adhesive decreased after the temperature cycle test, whereas the adhesive structure 100 maintained its adhesive strength even after the temperature cycle test. By introducing a more flexible structure into the porous skeleton, the bonded structure 100 achieved effects that could not be achieved with conventional rigid components alone.
[0033] As described above, the adhesive structure 100 according to the first embodiment includes a porous thin film 11 made of an epoxy resin with pores formed by a porous skeleton, and the pores of the porous thin film 11 are impregnated with an adhesive 13. The epoxy porous thin film has flexible mechanical properties and exhibits a stress relaxation effect, thereby easing stresses generated by temperature cycles and the like, making it suitable for use in devices subject to large temperature changes. This allows stress relaxation to occur without lowering the adhesive's glass transition temperature or adhesive strength. Furthermore, while a hard adhesive alone often exhibits interfacial failure and cracks during shear testing, the use of an adhesive-impregnated porous thin film results in at least a partial cohesive failure of the adhesive within the porous thin film, dispersing stress.
[0034] Second Embodiment In a second embodiment, a case where the adhesive structure 100 in the first embodiment is applied to an electronic component will be described.
[0035] 4 is a cross-sectional view showing the configuration of a semiconductor device using an adhesive structure 100 according to embodiment 2 of the present invention. As shown in Fig. 4, the semiconductor device 200 is composed of a substrate 21, a semiconductor element 23 provided on the surface of the substrate 21 via the adhesive structure 100, bonding wires 24 connecting electrodes (not shown) provided on the surface of the substrate 21 to surface electrodes (not shown) provided on the surface of the semiconductor element 23, and a sealing resin 25 that seals the semiconductor element 23.
[0036] Power devices that pass large currents of up to several hundred amperes must withstand high temperatures of around 200°C, and unprecedented heat resistance is required. 2 O 3 Such power semiconductors can operate at temperatures above 300°C, and in order to utilize this capability, the adhesive structure 100 in embodiment 1 can be used as a mounting material for a module that can withstand such high temperatures.
[0037] By using the adhesive structure 100 of the first embodiment in a semiconductor device 200 such as a power device, stresses that occur due to temperature cycles or the like can be alleviated.
[0038] If necessary, a certain thermal conductivity can be imparted by adding an arbitrary amount of powder (flake, spherical, needle-like, or special shape) of a thermally conductive material such as silica, boron nitride, aluminum oxide, aluminum nitride, magnesium oxide, silicon nitride, beryllium oxide, or diamond to the porous thin film 11. In addition, if conductivity is required, conductive powder (flake, spherical, needle-like, or special shape) of a thermally conductive material such as copper, silver, carbon black, or graphite may be added.
[0039] In addition, the substrate used as the mounting material may be a printed wiring board laminated with a glass prepreg material using epoxy, a ceramic substrate formed by laminating and sintering ceramic layers, or a lead frame formed by punching out a thin pure copper plate.
[0040] As described above, the semiconductor device 200 using the adhesive structure 100 of this embodiment 2 includes a semiconductor element 23 provided on the surface of a substrate 21 via the adhesive structure 100 of embodiment 1, bonding wires 24 connecting electrodes provided on the surface of the substrate 21 to electrodes provided on the surface of the semiconductor element 23, and a sealing resin 25 that seals the semiconductor element 23. This not only allows for sufficient relaxation of stresses that occur due to temperature cycles, etc. when bonding the semiconductor element, but also provides excellent adhesion.
[0041] Third Embodiment In a third embodiment, a case where the adhesive structure 100 in the first embodiment is applied to a motor will be described.
[0042] 5 is a cross-sectional view showing the configuration of a motor using an adhesive structure 100 according to embodiment 3 of the present invention. As shown in Fig. 5, the motor 200 is composed of a shaft 34, a cylindrical steel plate 33 attached to the shaft 34, and a magnet 32 adhered to the outer periphery of the steel plate 33 via the adhesive structure 100.
[0043] In an SPM motor (Surface Permanent Magnet Motor), the adhesive structure 100 in embodiment 1 can be used to fix magnets that require high heat resistance, and to fix parts in the engine compartment.
[0044] By using the adhesive structure 100 of the first embodiment in the motor 300 such as an SPM motor, stresses that occur due to temperature cycles and the like can be alleviated.
[0045] The magnets used here can be any type of magnet, including ferrite magnets, neodymium magnets, samarium-cobalt magnets, alnico magnets, and bonded magnets, regardless of their alloy composition. The material bonding the magnets is iron, and the magnets can be in the form of die-cast products or electromagnetic steel sheets made by laminating thin iron plates.
[0046] As described above, the motor 300 using the adhesive structure 100 according to the third embodiment includes a cylindrical steel plate 33 attached to the shaft 34 and a magnet 32 attached to the outer periphery of the steel plate 33 via the adhesive structure 100 according to the first embodiment. This not only fully alleviates stresses that occur due to temperature cycles, etc., when bonding the magnets, but also provides excellent adhesion.
[0047] Fourth Embodiment In a fourth embodiment, a case where the bonded structure 100 in the first embodiment is applied to an aircraft part will be described.
[0048] Fig. 6 is a block diagram showing the configuration of the bonded structure 100 according to the fourth embodiment of the present invention. Fig. 7 is a diagram showing the system flow of an interior air conditioning system using the bonded structure 100 according to the fourth embodiment of the present invention.
[0049] As shown in FIG. 6, first, the jet engine 41 takes in outside air and produces compressed air using a compressor 42 equipped with sensors and components 44 using the adhesive structure 100. The compressed air is then mixed with fuel in a combustion chamber and combusted intermittently (step S701).
[0050] Next, the air coming out of the combustion chamber is cooled to a desired temperature by the heat exchanger 43 using the sensor and the component 45 using the adhesive structure 100 (step S702).
[0051] Next, compressed air is taken from the compressor 42 using the sensors and components 44 using the adhesive structure 100 (step S703) and sent to the aircraft's air conditioning system (step S704).
[0052] Finally, the air is cooled in the air conditioning system (step S705) and then blown into the aircraft (step S706).
[0053] The air outside an aircraft is cold, ranging from 0 to 40°C on the ground and from -40 to 60°C at altitudes of 10,000 m or higher. Therefore, the sensors and components 44 used in the compressor 42 must be able to withstand temperatures ranging from relatively high temperatures of 100 to 200°C to low temperatures of -40 to 60°C.
[0054] By using the adhesive structure 100 in an interior air conditioning system as described above, the system has heat resistance and high toughness to maintain the structure in areas with large temperature differences.
[0055] As described above, in the on-board air conditioning equipment using the adhesive structure 100 of the fourth embodiment, the adhesive structure 100 of the first embodiment is used to bond the sensors and components 44 used in the compressor 42, and therefore not only can the stress generated by temperature cycles and the like in bonding the sensors and components be sufficiently alleviated, but the adhesive properties are also excellent.
[0056] Although various exemplary embodiments and examples are described in this application, the various features, aspects, and functions described in one or more embodiments are not limited to the application of a particular embodiment, but may be applied to the embodiments alone or in various combinations. Therefore, countless variations not illustrated are contemplated within the scope of the technology disclosed in this specification. For example, this includes cases where at least one component is modified, added, or omitted, or where at least one component is extracted and combined with components of another embodiment.
[0057] 11 porous thin film, 13 adhesive, 100 adhesive structure.
Claims
1. An adhesive structure comprising a thin film made of an epoxy resin having pores formed by a porous skeleton, the pores of the thin film being impregnated with an adhesive.
2. The adhesive structure according to claim 1, wherein the ratio of the elastic modulus of the adhesive to that of the thin film is 2 or more and 20 or less.
3. An adhesive structure as described in claim 1 or 2, characterized in that the thin film has a glass transition temperature of 60°C or higher and 200°C or lower, and the glass transition temperature of the impregnated, cured adhesive is higher than the glass transition temperature of the porous thin film.
4. An adhesive structure as described in any one of claims 1 to 3, characterized in that the pores have a diameter of 0.1 μm or more and 100 μm or less.
5. An adhesive structure as described in any one of claims 1 to 4, characterized in that the ratio of the elongation rate of the thin film to that of the adhesive is 2 or more and 1,000 or less.
6. The adhesive structure according to any one of claims 1 to 5, characterized in that the thin film contains a thermally conductive material.
7. The adhesive structure according to any one of claims 1 to 6, characterized in that the thin film contains a conductive material.
8. A semiconductor device comprising: a semiconductor element provided on the surface of a substrate via an adhesive structure described in any one of claims 1 to 7; bonding wires connecting electrodes provided on the surface of the substrate and electrodes provided on the surface of the semiconductor element; and a sealing resin that seals the semiconductor element.
9. A motor comprising a cylindrical steel plate attached to a shaft and a magnet attached to the outer periphery of the steel plate via an adhesive structure as claimed in any one of claims 1 to 7.
10. A flying object equipped with a compressor, characterized in that the adhesive structure according to any one of claims 1 to 7 is used to adhere sensors and parts used in the compressor.
11. A method for producing an adhesive structure, comprising the steps of: applying a solution of an epoxy base agent, an amine-based curing agent, and an added phase separation pore-forming agent onto a substrate, and thermally curing the solution to form a thin film; and impregnating the thin film, which has been peeled off from the substrate, with an adhesive.
Citation Information
Patent Citations
Epoxy foamed structural adhesive film capable of resisting 177 DEG C thermal oxidation for 3000 hours and preparation method thereof
CN112662357A
Method and apparatus for producing thermosetting resin porous sheet, thermosetting resin porous sheet and sheet roll
JP2014005314A
Flexible and adhesive flat formations for structural bonding
JP2018532837A
Foam / adhesive composite and methods of use thereof
US20110212288A1
Process for manufacturing porous epoxy with open pores and porous epoxy made therefrom
US20110269859A1
Cited By
Insulating sheet, method for producing porous resin sheet, stator, hoist, and liquid composition