Piezoelectric multilayer body, method for producing piezoelectric multilayer body, and piezoelectric element
The two-stage formation method for KNN films addresses the issue of high film stress in piezoelectric KNN films, achieving high piezoelectric constants and DC stress resistance while maintaining low film stress, thereby enhancing the reliability and performance of piezoelectric elements.
Patent Information
- Application Number
- PCT/JP2023/045474
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2023-12-19
- Publication Date
- 2024-10-03
AI Technical Summary
Piezoelectric KNN films with high piezoelectric constants and DC stress resistance often exhibit high film stress, leading to structural deformation and reduced manufacturing yield in piezoelectric elements, particularly when formed at high temperatures.
A method involving the formation of a KNN film in two stages, where the first layer is formed at a temperature that achieves a high (001) orientation ratio and low film stress, followed by a second layer formed at a higher temperature to enhance piezoelectric constant and DC stress resistance, while maintaining film stress below 150 MPa.
The approach results in a KNN film with a high piezoelectric constant, high DC stress resistance, and low film stress, improving the reliability and performance of piezoelectric elements by suppressing structural deformation and increasing the number of application cycles without dielectric breakdown.
Smart Images

Figure JP2023045474_03102024_PF_FP_ABST
Abstract
Description
Piezoelectric laminate, method for manufacturing piezoelectric laminate, and piezoelectric element
[0001] The present disclosure relates to a piezoelectric laminate, a method for manufacturing a piezoelectric laminate, and a piezoelectric element.
[0002] Piezoelectric materials are widely used in functional electronic components such as sensors and actuators. KNN-based ferroelectric materials containing potassium, sodium, niobium, and oxygen are used as piezoelectric materials, and laminates have been proposed that include piezoelectric films (KNN films) formed using such piezoelectric materials. KNN films are required to have a high piezoelectric constant and be resistant to dielectric breakdown even when a large negative voltage is applied to the KNN film for a long period of time (i.e., high DC stress resistance). Therefore, techniques for increasing the piezoelectric constant of KNN films (see, for example, Patent Document 1) and techniques for increasing the DC stress resistance of KNN films (see, for example, Patent Documents 2 and 3) have been proposed.
[0003] JP 2009-295786 A JP 2017-076730 A JP 2018-207055 A
[0004] However, although the KNN film obtained by the above-mentioned technique has a high piezoelectric constant or high DC stress resistance, it has a large film stress.
[0005] An object of the present disclosure is to provide a piezoelectric stack having a piezoelectric film containing potassium, sodium, niobium, and oxygen, which has a high piezoelectric constant, a high DC stress resistance, and a small film stress.
[0006] According to one aspect of the present disclosure, there is provided a piezoelectric element comprising: a substrate; a lower electrode film formed on the substrate; and a piezoelectric film formed on the lower electrode film and made of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen, wherein the piezoelectric film has a piezoelectric constant e 31 is 10 C / m 2 or more, and when a negative voltage is applied to the upper electrode film so as to generate an electric field of 300 kV / cm between the lower electrode film and an upper electrode film provided on the piezoelectric film at a temperature of 200° C., the leakage current density flowing through the piezoelectric film from the start of application of the negative voltage is 30 mA / cm 2the time until the temperature exceeds 100°C is 5 hours or more, and the film stress of the piezoelectric film is 150 MPa or less.
[0007] According to another aspect of the present disclosure, a method for fabricating a piezoelectric film includes the steps of: forming a lower electrode film on a substrate; and forming a piezoelectric film composed of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen on the lower electrode film, wherein in the step of fabricating the piezoelectric film, first, a first piezoelectric film, which is a part of the piezoelectric film, is formed at a first temperature at which the (001) orientation rate is 95% or more and the film stress is 100 MPa or less, and then, a second piezoelectric film, which is the other part of the piezoelectric film, is formed at a first temperature at which the piezoelectric constant e of the second piezoelectric film is 100 MPa or less. 31 is 10 C / m 2 When a negative voltage is applied to the upper electrode film so as to generate an electric field of 300 kV / cm between the lower electrode film and the upper electrode film formed on the second piezoelectric film, the leakage current density flowing through the second piezoelectric film is 30 mA / cm. 2 The method for producing a piezoelectric laminate includes forming the film at a second temperature at which the time until the temperature exceeds the threshold value is 5 hours or more.
[0008] According to the present disclosure, it is possible to provide a piezoelectric laminate having a piezoelectric film containing potassium, sodium, niobium, and oxygen, which has a high piezoelectric constant, a high DC stress resistance, and a small film stress.
[0009] FIG. 1 is a diagram showing an example of a cross-sectional structure of a piezoelectric laminate according to an embodiment of the present disclosure; FIG. 2 is a diagram showing an example of a structure of a simple piezoelectric element according to an embodiment of the present disclosure; FIG. 3 is a diagram showing an example of a schematic configuration of a piezoelectric element according to an embodiment of the present disclosure; FIG. 4 is a diagram showing an example of a schematic configuration of a piezoelectric device module according to an embodiment of the present disclosure; FIG. 5(a) is a diagram showing an example of a schematic configuration of a simple unimorph cantilever produced using each sample, and FIG. 5(b) is a diagram explaining a method for measuring the piezoelectric constant.
[0010] <Discoveries Obtained by the Inventors> The inventors conducted extensive research to develop a KNN film having both a high piezoelectric constant and high DC stress resistance. As a result, they discovered that by depositing a KNN film at a high temperature on a substrate, such as a silicon (Si) substrate, by sputtering, a KNN film having both a high piezoelectric constant and high DC stress resistance can be achieved. However, depositing a KNN film at a high temperature increases the film stress of the KNN film, although it can increase the piezoelectric constant and DC stress resistance of the KNN film. Furthermore, high temperatures during sputtering deposition tend to increase the film stress induced in the KNN film, resulting in increased tensile stress. If the film stress of the KNN film is high, for example, if the film stress of the KNN film exceeds 150 MPa, significant structural deformation occurs during the fabrication of piezoelectric elements, such as membrane structures and cantilever structures. As a result, the fabricated piezoelectric elements will not function properly. Furthermore, the manufacturing yield of piezoelectric elements and piezoelectric device modules will decrease. For this reason, it is required to keep the film stress of the KNN film low, for example, to keep the film stress of the KNN film at 150 MPa or less.
[0011] The present inventors conducted extensive research to develop a KNN film that simultaneously possesses three previously unrealized characteristics: a high piezoelectric constant, high DC stress resistance, and low film stress. As a result, they obtained the following five findings. (First finding) The film stress of a KNN film obtained by sputtering deposition is significantly dependent on the conditions at the initial stage of deposition. (Second finding) First, a KNN film serving as a first layer (initial layer) is deposited under temperature conditions that reduce film stress (at the initial stage of deposition). Then, a KNN film serving as a second layer is deposited on the first layer under temperature conditions that increase the piezoelectric constant and DC stress resistance. This significantly reduces film stress throughout the entire KNN film (the laminate of the first and second layers), even when the KNN film (second layer) is deposited at a high temperature that would normally result in high film stress. (Third finding) In order to reproducibly obtain a KNN film with a high piezoelectric constant and DC stress resistance, the (001) orientation rate of the KNN film must be increased. To obtain a KNN film with a high (001) orientation, the deposition temperature of the KNN film must generally be within a predetermined range. By depositing a KNN film as the first layer at a temperature that increases the (001) orientation in the initial stage of deposition, and then depositing a KNN film as the second layer on the first layer at a temperature that increases the piezoelectric constant and DC stress resistance, a KNN film with a high (001) orientation can be obtained even when the KNN film (second layer) is deposited at a high temperature that would normally decrease the (001) orientation. The (001) orientation of the KNN film refers to the orientation rate of the crystals constituting the KNN film in the (001) plane direction, as will be described in detail later. (Fourth Finding) To reproducibly obtain a KNN film with a high piezoelectric constant and DC stress resistance, the (001) orientation of the KNN film must be 90% or higher. By depositing the KNN film as the first layer under conditions that result in a (001) orientation rate of 95% or more in the initial stage of deposition, a KNN film with a (001) orientation rate of 90% or more can be obtained even when the KNN film as the second layer is subsequently deposited at a high temperature. (Fifth Finding) By depositing the KNN film as the first layer under conditions that result in a small film stress and a high (001) orientation rate in the initial stage of deposition, and then depositing the KNN film as the second layer on the first layer under temperature conditions that result in a high piezoelectric constant and DC stress resistance, a KNN film with a high piezoelectric constant and DC stress resistance can be realized.
[0012] Based on the above five findings, the inventors have found that by depositing a KNN film as the first layer under temperature conditions in which the film stress is 100 MPa or less and the (001) orientation rate is 95% or more in the early stages of film deposition, and then depositing a KNN film as the second layer under temperature conditions in which the piezoelectric constant and DC stress resistance of the KNN film are high, a KNN film having a high piezoelectric constant and DC stress resistance and a film stress of 150 MPa or less can be obtained.
[0013] The present disclosure has been made based on the above-mentioned problems and findings obtained by the present inventors.
[0014] <One Aspect of the Present Disclosure> Hereinafter, one aspect of the present disclosure will be described with reference to the drawings.
[0015] (1) Configuration of Piezoelectric Laminate As shown in FIG. 1 , a laminate (laminated substrate) 10 (hereinafter also referred to as piezoelectric laminate 10) having a piezoelectric film according to this embodiment includes a substrate 1, a lower electrode film 2 formed on the substrate 1, a piezoelectric film (piezoelectric thin film) 3 formed on the lower electrode film 2, and an upper electrode film 4 formed on the piezoelectric film 3.
[0016] The substrate 1 is a substrate having a surface oxide film (SiO 2 A single crystal silicon (Si) substrate 1a on which a surface oxide film 1b is formed, i.e., a Si substrate having a surface oxide film, can be suitably used. 2 It is also possible to use a Si substrate 1a having an insulating film formed of an insulating material other than the above. Also, as the substrate 1, a Si substrate 1a having an exposed Si(100) face or Si(111) face on the surface, that is, a Si substrate having no surface oxide film 1b or insulating film, can be used. Also, as the substrate 1, an SOI (Silicon On Insulator) substrate, a quartz glass (SiO 2 The thickness of the single crystal Si substrate 1a can be, for example, 300 μm to 1000 μm, and the thickness of the surface oxide film 1b can be, for example, 1 nm to 4000 nm.
[0017] The lower electrode film 2 can be formed using, for example, platinum (Pt). The lower electrode film 2 is a polycrystalline film. Hereinafter, a polycrystalline film formed using Pt will also be referred to as a Pt film. It is preferable that the (111) plane of the Pt film is parallel to the main surface of the substrate 1 (including cases where the (111) plane is inclined at an angle of ±5° or less with respect to the main surface of the substrate 1), i.e., the Pt film is oriented in the (111) plane. Orientation of the Pt film in the (111) plane means that no peaks other than those attributable to the (111) plane are observed in the X-ray diffraction pattern obtained by X-ray diffraction (XRD) measured on the surface of the piezoelectric film 3. Thus, the main surface of the lower electrode film 2 (the surface underlying the piezoelectric film 3) is preferably composed of the Pt (111) plane. The lower electrode film 2 can be formed by a method such as sputtering or vapor deposition. The material of the lower electrode film 2 may be, in addition to Pt, various metals such as gold (Au), ruthenium (Ru), or iridium (Ir), alloys containing these as main components, or strontium ruthenate (SrRuO 3 , abbreviated as SRO) or lanthanum nickelate (LaNiO 3 The lower electrode film 2 may also be formed using a metal oxide such as SiO2 (abbreviated as LNO). When the lower electrode film 2 is formed using a metal oxide, the crystals constituting the lower electrode film 2 preferably have a (001) plane orientation preferentially relative to the surface of the substrate 1. The lower electrode film 2 may be a single layer film formed using the above-mentioned metals, an alloy mainly composed of the above-mentioned metals, or a metal oxide. The lower electrode film 2 may be a laminate of a Pt film and a film mainly composed of SRO provided on the Pt film, or a laminate of a Pt film and a film mainly composed of LNO provided on the Pt film. The thickness of the lower electrode film 2 (when the lower electrode film 2 is a laminate, the total thickness of each layer) may be, for example, 100 nm to 400 nm.
[0018] An adhesion layer 6 may be provided between the substrate 1 and the lower electrode film 2 to enhance adhesion therebetween. The adhesion layer 6 may be, for example, a layer containing zinc (Zn) and oxygen (O) as main components (hereinafter also referred to as a "ZnO layer"). The ZnO layer may be formed using, for example, zinc oxide. The composition ratio of Zn and O constituting the ZnO layer preferably satisfies the relationship Zn:O = 1:1, but is not limited thereto and may vary somewhat. The ZnO layer is a polycrystalline layer. It is preferable that the (0001) plane of the ZnO layer is parallel to the major surface of the substrate 1 (including the case where the (0001) plane is inclined at an angle of ±5° or less with respect to the major surface of the substrate 1), i.e., the ZnO layer is oriented in the (0001) plane direction. The ZnO layer being oriented in the (0001) plane direction means that the intensity of the peak due to the (0002) plane is high in the X-ray diffraction pattern obtained by XRD measured on the surface of the piezoelectric film 3. As such, the main surface of the ZnO layer (the surface that serves as the base of the lower electrode film 2) is preferably configured as the ZnO (0001) plane. The ZnO layer can be formed by a method such as sputtering or vapor deposition. The thickness of the ZnO layer can be, for example, 1 nm or more and 200 nm or less, preferably 10 nm or more and 50 nm or less. The adhesion layer 6 can be formed of, for example, titanium (Ti), tantalum (Ta), titanium oxide (TiO 2 ), nickel (Ni), ruthenium oxide (RuO 2 ), iridium oxide (IrO 2 ) or the like as a main component may be provided. Such an adhesion layer 6 can also be formed by a method such as sputtering or vapor deposition, and the thickness of the adhesion layer 6 can be, for example, 1 nm to 200 nm, preferably 10 nm to 50 nm. In this specification, the adhesion layer 6 provided between the substrate 1 and the lower electrode film 2 is sometimes referred to as a lower adhesion layer 6.
[0019] The piezoelectric film 3 is a film formed of, for example, an alkali niobium oxide containing potassium (K), sodium (Na), niobium (Nb), and oxygen (O). That is, the piezoelectric film 3 is a film whose main component is an alkali niobium oxide containing K, Na, Nb, and O. The piezoelectric film 3 is a film formed of, for example, an alkali niobium oxide containing potassium (K), sodium (Na), niobium (Nb), and oxygen (O).1-x Na x ) NbO 3 The piezoelectric film 3 can be formed using an alkali niobium oxide represented by the formula (I), i.e., potassium sodium niobate (KNN). The coefficient x [= Na / (K+Na)] in the above composition formula can be within the range of 0<x<1, preferably 0.4≦x≦0.8. The piezoelectric film 3 is a KNN polycrystalline film (hereinafter also referred to as the KNN film 3). The crystal structure of KNN is a perovskite structure. That is, the KNN film 3 has a perovskite structure. Preferably, more than half of the crystals constituting the KNN film 3 have a columnar structure. In this specification, the crystal system of KNN is considered to be a tetragonal system. The KNN film 3 can be formed by a sputtering method. The thickness of the KNN film 3 can be, for example, 0.5 μm to 5 μm, preferably 1 μm to 3 μm.
[0020] The crystals constituting the KNN film 3 are preferentially oriented in the (001) plane with respect to the main surface of the substrate 1 (Si substrate 1a when the substrate 1 is, for example, a Si substrate 1a having a surface oxide film 1b or an insulating film, etc.). That is, the main surface of the KNN film 3 (the surface that serves as the base for the upper electrode film 4) is mainly composed of the KNN (001) plane. For example, by directly depositing the KNN film 3 on a Pt film (lower electrode film 2) whose main surface is mainly composed of the Pt (111) plane, a KNN film 3 whose main surface is mainly composed of the KNN (001) plane can be obtained.
[0021] As used herein, the crystals constituting the KNN film 3 being oriented in the (001) plane direction means that the (001) plane of the crystals constituting the KNN film 3 is parallel or approximately parallel to the main surface of the substrate 1. Furthermore, the crystals constituting the KNN film 3 being preferentially oriented in the (001) plane direction means that many of the crystals have their (001) planes parallel or approximately parallel to the main surface of the substrate 1. For example, it is preferred that 90% or more of the crystals constituting the KNN film 3 be oriented in the (001) plane direction relative to the main surface of the substrate 1. That is, the orientation rate of the crystals constituting the KNN film 3 in the (001) plane direction (also referred to herein as the "(001) orientation rate") is preferably 90% or more, and more preferably 95% or more. The "(001) orientation rate" as used herein is a value calculated by the following formula (1) based on the peak intensity of the X-ray diffraction pattern (2θ / θ) obtained by performing XRD measurement on the KNN film 3.
[0022] (001) orientation rate (%)={(001) peak intensity / ((001) peak intensity+(110) peak intensity)}×100 (1)
[0023] The "(001) peak intensity" in the above formula (1) refers to the intensity of a diffraction peak due to crystals oriented in the (001) plane direction (i.e., crystals whose (001) plane is parallel to the main surface of the substrate 1) among the crystals constituting the KNN film 3 in the X-ray diffraction pattern obtained by performing XRD measurement on the KNN film 3, and refers to the intensity of a peak appearing within a 2θ range of 20° to 23°. When multiple peaks appear within a 2θ range of 20° to 23°, the intensity refers to the intensity of the highest peak. The "(110) peak intensity" in the above formula (1) refers to the intensity of a diffraction peak due to crystals oriented in the (110) plane direction (i.e., crystals whose (110) plane is parallel to the main surface of the substrate 1) among the crystals constituting the KNN film 3 in the X-ray diffraction pattern obtained by performing XRD measurement on the KNN film 3, and refers to the intensity of a peak appearing within a 2θ range of 30° to 33°. When multiple peaks appear within the 2θ range of 30° to 33°, the intensity is that of the highest peak.
[0024] The alkali niobium oxide constituting the KNN film 3 may be selected from the group consisting of lithium (Li), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), bismuth (Bi), antimony (Sb), vanadium (V), indium (In), tantalum (Ta), molybdenum (Mo), tungsten (W), chromium (Cr), Ti, zirconium (Zr), hafnium (Hf), scandium (Sc), yttrium (Y), lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), The alkali niobium oxide may further contain at least one element (dopant) selected from the group consisting of samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), lutetium (Lu), copper (Cu), zinc (Zn), silver (Ag), manganese (Mn), iron (Fe), cobalt (Co), Ni, aluminum (Al), Si, germanium (Ge), tin (Sn), and gallium (Ga). The concentration of these elements in the alkali niobium oxide can be, for example, 5 at % or less (when a plurality of the above elements is contained, the total concentration can be 5 at % or less).
[0025] As will be described in detail later, in this embodiment, first, a first KNN film 3a (first piezoelectric film, hereinafter also referred to as "KNN film 3a"), which is a part of the KNN film 3, is deposited at a first temperature at which the (001) orientation rate is 95% or more and the film stress is 100 MPa or less, and then a second KNN film 3b (second piezoelectric film, hereinafter also referred to as "KNN film 3b"), which is the other part of the KNN film 3, is deposited on the KNN film 3a at a second temperature at which the piezoelectric constant and DC stress resistance are increased. As a result, the KNN film 3 in this embodiment (i.e., a laminate of the KNN film 3a and the KNN film 3b) simultaneously has all of the features 1 to 3 described below. Furthermore, the KNN film 3 in this embodiment may further have the feature 4 described below.
[0026] The following describes features 1 to 4 that the KNN film 3 of this embodiment may have.
[0027] (Feature 1) The KNN film 3 has a piezoelectric constant e 31 is 10 C / m2 That is, the KNN film 3 has a feature of having a high piezoelectric constant.
[0028] In this specification, the "piezoelectric constant e 31 " is a value measured under the condition that a negative voltage (e.g., a triangular wave or sine wave voltage) is applied to the upper electrode film 4 while the lower electrode film 2 is grounded so as to generate an electric field of 100 kV / cm between the lower electrode film 2 and the upper electrode film 4 (i.e., the KNN film 3).
[0029] The high piezoelectric constant of the KNN film 3 makes it possible to improve the performance of the piezoelectric element 20 (piezoelectric device module 30) described below, which is obtained by processing the piezoelectric stack 10. As a result, the piezoelectric element 20 (piezoelectric device module 30) can be suitably used as an actuator.
[0030] This feature can be reproducibly (reliably) exhibited by the (001) orientation rate of the KNN film 3 (KNN film 3b) being 90% or more.
[0031] (Feature 2) When a highly accelerated life test (HALT) is performed on the KNN film 3, in which a negative voltage is applied to the upper electrode film 4 (via the KNN film 3) (with the lower electrode film 2 grounded) so as to generate an electric field of 300 kV / cm between the lower electrode film 2 and the upper electrode film 4 (i.e., the KNN film 3) at a temperature of 200° C. (with the piezoelectric stack 10 heated to 200° C.) (hereinafter also referred to as "when a HALT under predetermined conditions is performed at a temperature of 200° C."), the leakage current density flowing through the KNN film 3 from the start of voltage application is 30 mA / cm. 2 Thus, the KNN film 3 has a feature that it has a long life against DC stress, that is, it has a high DC stress resistance.
[0032] Since the KNN film 3 has high DC stress resistance, the KNN film 3 is less susceptible to dielectric breakdown (the time until the KNN film 3 reaches dielectric breakdown becomes longer) even when a high voltage (electric field) is applied to the KNN film 3 via the upper electrode film 4 for a long period of time when the piezoelectric element 20 (piezoelectric device module 30) described below, obtained by processing the piezoelectric laminate 10, is driven (hereinafter, also simply referred to as "driving time"). Note that in this embodiment, the leakage current density flowing through the KNN film 3 is 30 mA / cm 2 When the temperature exceeds this value, it is considered that the KNN film 3 has reached a dielectric breakdown.
[0033] This feature can be reproducibly (reliably) exhibited by the (001) orientation rate of the KNN film 3 (KNN film 3b) being 90% or more.
[0034] (Feature 3) The KNN film 3 further has the feature that "the film stress is 150 MPa or less."
[0035] By keeping the film stress of the KNN film 3 at 150 MPa or less, it is possible to suppress large structural deformation when processing the piezoelectric stack 10 to fabricate piezoelectric elements 20 having a membrane structure, a cantilever structure, or the like, as described below. This allows the piezoelectric elements 20 (piezoelectric device modules 30) obtained by processing the piezoelectric stack 10, as described below, to operate normally.
[0036] (Feature 4) The KNN film 3 may further have the feature that "when a negative (AC) voltage is continuously applied to the upper electrode film 4 (and via it to the KNN film 3) so as to generate a unipolar AC electric field of 300 kV / cm between the lower electrode film 2 and the upper electrode film 4 (i.e., the KNN film 3), the number of voltage application cycles until the piezoelectric displacement of the KNN film 3 decreases to 80% or less of its initial value exceeds 10 million."
[0037] For example, in the case of a piezoelectric laminate 10 having a KNN film 3 with a thickness of 2 μm, when a unipolar triangular or sinusoidal AC voltage having an amplitude in the range of 0 V to −60 V is continuously applied to the KNN film 3 via the upper electrode film 4 at a frequency of 300 Hz with the lower electrode film 2 grounded so that the direction of the electric field applied to the KNN film 3 does not reverse (so that the direction of the electric field is in one direction), the number of voltage application cycles until the piezoelectric displacement of the KNN film 3 decreases to 80% or less of its initial value exceeds 10 million.
[0038] In this specification, the term "unipolar electric field" refers to an electric field that is unidirectional even if the magnitude of the voltage applied to the KNN film 3 via the upper electrode film 4 periodically fluctuates within a range of, for example, 0 V to -60 V. In addition, in this specification, the "number of voltage application cycles until the piezoelectric displacement of the KNN film 3 falls to 80% or less of its initial value when a negative voltage is continuously applied to the upper electrode film 4 so as to generate a unipolar AC electric field of 300 kV / cm in the KNN film 3" is also referred to as the "number of application cycles."
[0039] When an AC voltage is applied to the KNN film 3 via the upper electrode film 4, the KNN film 3 deforms. The higher the applied voltage, the greater the deformation of the KNN film 3. The KNN film 3 in this embodiment can have the characteristic that the amount of piezoelectric displacement is unlikely to decrease even when it is repeatedly deformed by applying a large AC voltage continuously, i.e., has the characteristic of excellent AC stress resistance.
[0040] In the piezoelectric laminate 10 obtained by the above-described novel method, a KNN film 3a having a high (001) orientation rate and low film stress, for example, a KNN film 3a having a (001) orientation rate of 95% or more and a film stress of 100 MPa or less, is interposed between the bottom electrode film 2 and the KNN film 3b. This allows the KNN film 3 (a laminate of the KNN film 3a and the KNN film 3b) in this embodiment to have superior AC stress resistance compared to a laminate without the KNN film 3a. This is believed to be because the interposition of the KNN film 3a significantly improves adhesion between the bottom electrode film 2 and the KNN film 3. The fact that the interposition of the KNN film 3a can increase the number of application cycles to more than 10 million, i.e., improves the AC stress resistance of the KNN film 3, is a novel finding first discovered as a result of extensive research by the present inventors.
[0041] The excellent AC stress resistance of the KNN film 3 makes it possible to improve the reliability of the piezoelectric element 20 (piezoelectric device module 30) obtained by processing the piezoelectric laminate 10, which will be described later.
[0042] The inventors have confirmed that in a piezoelectric laminate 10 having a KNN film 3a with a (001) orientation rate of 95% or more and a film stress of 100 MPa or less interposed between a lower electrode film 2 and a KNN film 3b, when a negative voltage is continuously applied to the KNN film 3 via the upper electrode film 4 so as to generate a unipolar AC electric field of 300 kV / cm in the KNN film 3, the piezoelectric displacement of the KNN film 3 can be maintained at 80% or more of its initial value even after the number of application cycles exceeds 10 million, and even reaches 50 million or more.
[0043] On the other hand, when the KNN film 3a is not interposed, that is, when the KNN film 3 is not configured as a laminate of the KNN film 3a and the KNN film 3b, if a large AC voltage is continuously applied to the KNN film 3 via the upper electrode film 4 and the KNN film 3 is continuously deformed, the KNN film 3 will gradually peel off from the lower electrode film 2. As a result, the amount of piezoelectric displacement of the KNN film 3 will be easily reduced.
[0044] The inventors have confirmed that in a piezoelectric laminate in which the KNN film 3a is not interposed between the lower electrode film 2 and the KNN film 3b, when a negative voltage is continuously applied to the KNN film via the upper electrode film 4 so as to generate a unipolar AC electric field of 300 kV / cm in the KNN film, the piezoelectric displacement of the KNN film falls to less than 80% of its initial value before the number of application cycles reaches 10 million.
[0045] As described above, the KNN film 3 in this embodiment can have all of the above-mentioned features 1 to 3, and preferably all of the above-mentioned features 1 to 4. When the KNN film 3 has all of the above-mentioned features 1 to 3, it becomes possible to suitably apply the piezoelectric element 20 (piezoelectric device module 30) described below, which is obtained by processing the piezoelectric stack 10 having the KNN film 3, to actuator applications. Furthermore, when the KNN film 3 has all of the above-mentioned features 1 to 4, it becomes possible to more suitably apply the piezoelectric element 20 (piezoelectric device module 30) described below to actuator applications.
[0046] In this embodiment, when depositing the KNN film 3, the KNN film 3a is first deposited at a first temperature at which the (001) orientation rate is 95% or more and the film stress is 100 MPa or less, and then the KNN film 3b is deposited on the KNN film 3a at a second temperature at which the piezoelectric constant and DC stress resistance are increased. Therefore, the KNN film 3 in this embodiment has a laminated structure of the KNN film 3a as a first layer (initial layer) deposited at the first temperature and the KNN film 3b as a second layer deposited at the second temperature.
[0047] The KNN film 3a deposited at the first temperature has a low piezoelectric constant and low DC stress resistance. Therefore, as the ratio of the thickness of the KNN film 3a to the total thickness of the KNN film 3 (the total thickness of the KNN film 3a and the KNN film 3b) increases, at least one of the above-mentioned features 1 and 2 tends to be less likely to be realized. Therefore, it is preferable to minimize the thickness of the KNN film 3a so as to reduce the film stress of the KNN film 3 and keep the film stress of the entire KNN film 3 at 150 MPa or less. While the thickness of the KNN film 3a is not strictly limited, it is preferably, for example, 20% or less of the total thickness of the KNN film 3. This ensures that a KNN film 3 having the above-mentioned features 1 and 2 (i.e., a KNN film 3 having a high piezoelectric constant and high DC stress resistance) can be reliably obtained, and preferably, a KNN film 3 having the above-mentioned features 1 and 2 can be reliably obtained with good reproducibility.
[0048] The upper electrode film 4 is mainly composed of various metals such as Pt, Au, Al, Cu, etc., or alloys thereof. The upper electrode film 4 can be formed by a method such as sputtering, vapor deposition, plating, or metal paste. The upper electrode film 4 does not have a significant effect on the crystal structure of the KNN film 3, unlike the lower electrode film 2. Therefore, the material, crystal structure, and film formation method of the upper electrode film 4 are not particularly limited. Note that, for example, RuO may be interposed between the KNN film 3 and the upper electrode film 4 to enhance their adhesion. 2 , IrO 2 , Ti, Ta, TiO 2 An adhesion layer 7 containing, as a main component, Ni or the like may be provided. The thickness of the upper electrode film 4 may be, for example, 50 nm to 5000 nm, preferably 50 nm to 300 nm, and when the adhesion layer 7 is provided, the thickness of the adhesion layer 7 may be, for example, 1 nm to 200 nm, preferably 5 nm to 50 nm. In this specification, the adhesion layer 7 provided between the KNN film 3 and the upper electrode film 4 may also be referred to as the upper adhesion layer 7.
[0049] (2) Methods of Manufacturing the Piezoelectric Laminate, Piezoelectric Element, and Piezoelectric Device Module Methods of manufacturing the above-described piezoelectric laminate 10, piezoelectric element, and piezoelectric device module will now be described.
[0050] (Deposition of Lower Adhesion Layer and Lower Electrode Film) First, a substrate 1 is prepared, and a lower adhesion layer 6 (e.g., a ZnO layer) and a lower electrode film 2 (e.g., a Pt film) are deposited in this order by, for example, sputtering on one of the main surfaces of the substrate 1. Note that a substrate 1 may be prepared on which the lower adhesion layer 6 and the lower electrode film 2 have already been deposited on one of the main surfaces.
[0051] The conditions for depositing the ZnO layer as the lower adhesive layer 6 are exemplified below. The deposition time for the lower adhesive layer 6 is adjusted appropriately depending on the target thickness of the lower adhesive layer 6. Target: ZnO sintered body Temperature (substrate temperature): 200°C or higher and 700°C or lower, preferably 300°C or higher and 700°C or lower, more preferably 500°C or higher and 700°C or lower Discharge power density: 2 W / cm 2 More than 6W / cm 2 Preferably less than 3 W / cm 2 More than 5W / cm 2 The following atmosphere: argon (Ar) gas and oxygen (O 2 ) gas (hereinafter referred to as "Ar / O 2 (also called "mixed gas atmosphere") O 2 The ratio of the partial pressure of Ar gas to the partial pressure of O 2 Gas partial pressure): 5 / 1 to 30 / 1, preferably 7 / 1 to 20 / 1, more preferably 10 / 1 to 15 / 1 Atmospheric pressure: 0.1 Pa or more and 0.5 Pa or less, preferably 0.2 Pa or more and 0.4 Pa or less Thickness: 1 nm or more and 200 nm or less, preferably 10 nm or more and 50 nm or less
[0052] In this specification, when a numerical range is expressed, such as "5 / 1 to 30 / 1," it means that the lower limit and the upper limit are included in the range. The same applies to other numerical ranges.
[0053] The conditions for forming a Ti layer or the like as the lower adhesion layer 6 are exemplified as follows: Target: Ti plate or the like Temperature (substrate temperature): 100°C or higher and 500°C or lower, preferably 200°C or higher and 400°C or lower Atmosphere: Ar gas atmosphere Atmosphere pressure: 0.1 Pa or higher and 0.5 Pa or lower, preferably 0.2 Pa or higher and 0.4 Pa or lower Other conditions can be the same as those for forming a ZnO layer.
[0054] The conditions for depositing a Pt film as the lower electrode film 2 are exemplified below. The deposition time for the lower electrode film 2 is adjusted appropriately depending on the target thickness of the lower electrode film 2. Target: Pt plate Temperature (substrate temperature): 200°C or higher and 600°C or lower, preferably 300°C or higher and 500°C or lower Discharge power density: 1 W / cm 2 More than 5W / cm 2 Preferably 2 W / cm or less 2 More than 4W / cm 2 Atmosphere: Ar gas atmosphere Atmosphere pressure: 0.1 Pa or more and 0.5 Pa or less, preferably 0.2 Pa or more and 0.4 Pa or less Thickness: 100 nm or more and 400 nm or less
[0055] (Deposition of KNN film) After the deposition of the lower adhesive layer 6 and the lower electrode film 2 is completed, the KNN film 3 is deposited on the lower electrode film 2 by a sputtering method such as RF magnetron sputtering. The composition of the KNN film 3 can be adjusted by controlling the composition of the target used during sputter deposition, for example. 2 CO 3 Powder, Na 2 CO 3 powder, Nb 2 O 5 The target can be prepared by mixing powders and firing them. 2 CO 3 Powder, Na 2 CO 3 powder, Nb 2 O 5 This can be controlled by adjusting the mixing ratio of the powders, etc. When depositing the KNN film 3 containing the above elements such as Cu and Mn, a target may be used in which Cu powder (or CuO powder), Mn powder (or MnO powder), etc. are mixed in a predetermined ratio in addition to the above powders.
[0056] The KNN film 3 is formed in two stages by changing the temperature conditions. Specifically, first (at the beginning of the film formation), the KNN film 3a is formed at a first temperature, and then the KNN film 3b is formed at a second temperature.
[0057] The first temperature is a temperature at which the (001) orientation rate of the KNN film 3a becomes 95% or more and the film stress becomes 100 MPa or less. For example, the first temperature is a temperature at which the (001) orientation rate of the KNN film 3a becomes 95% or more when the KNN film 3a is formed to a thickness of 2 μm (±10%) at the first temperature. Furthermore, the first temperature is a temperature at which the film stress of the KNN film 3a becomes 100 MPa or less when the KNN film 3a is formed to a thickness of 2 μm (±10%) at the first temperature.
[0058] The second temperature is the piezoelectric constant e of the KNN film 3b. 31 is 10 C / m 2 The second temperature is the temperature at which the leakage current density flowing through the KNN film 3b from the start of voltage application becomes 30 mA / cm when HALT under predetermined conditions is performed at a temperature of 200°C. 2 is the temperature at which the time required for the temperature to exceed this value is 5 hours or more.
[0059] Although the first and second temperatures depend somewhat on the sputtering deposition apparatus and deposition conditions, in the sputtering deposition of the KNN film 3 in this embodiment, the second temperature is usually higher than the first temperature (first temperature < second temperature). For example, the first temperature can be in the range of 550°C to 600°C, and the second temperature can be in the range of 650°C to 800°C.
[0060] The conditions other than the temperature when depositing the KNN film 3 (KNN film 3a, KNN film 3b) are, for both the deposition at the first temperature and the deposition at the second temperature, as follows: Discharge power density: 2.7 W / cm 2 More than 4.1W / cm 2 Preferably 2.8 W / cm or less 2 More than 3.8W / cm 2 Atmosphere: an atmosphere containing at least Ar gas, preferably Ar / O 2 Mixed gas atmosphere: Atmospheric pressure: 0.03 Pa or more and 0.5 Pa or less, preferably 0.04 Pa or more and 0.4 Pa or less O relative to Ar gas 2 Ratio of partial pressures of gases (O 2Gas partial pressure / Ar gas partial pressure): 0 to 1 / 20, preferably 0 to 1 / 30 Film formation rate: 0.5 μm / hr to 4 μm / hr, preferably 0.5 μm / hr to 2 μm / hr Total thickness of KNN film: 0.5 μm to 5 μm, preferably 1 μm to 3 μm
[0061] In addition, "O 2 The "gas partial pressure / Ar gas partial pressure is 0 (zero)" means that 2 This refers to a state where the gas partial pressure is 0, i.e., an atmosphere of only Ar gas. The "total thickness of the KNN film" refers to the total thickness of the KNN film 3a deposited at the first temperature and the KNN film 3b deposited at the second temperature. The deposition times for the KNN films 3a and 3b are adjusted appropriately depending on the target thicknesses of the KNN films 3a and 3b. As described above, the thickness of the KNN film 3a is preferably set to the minimum necessary to reduce the film stress in the KNN film 3b during deposition at the second temperature and to keep the film stress of the entire KNN film 3 at 150 MPa or less. Therefore, the deposition time for the KNN film 3a (deposition time at the first temperature) is preferably adjusted so that the thickness of the KNN film 3a is 20% or less of the total thickness of the KNN film 3, for example.
[0062] As described above, first, the KNN film 3a is deposited at a first temperature at which the (001) orientation rate is 95% or more and the film stress is 100 MPa or less. Then, the KNN film 3b is deposited on the KNN film 3a at a second temperature at which the piezoelectric constant and DC stress resistance are increased. This allows the film stress of the entire KNN film 3 after the KNN film 3b is deposited to be significantly reduced, even if the second temperature is high enough to cause a large film stress in the KNN film 3b. As a result, a KNN film 3 with a high piezoelectric constant and DC stress resistance and low film stress can be obtained. That is, by depositing the KNN film 3 (KNN film 3a and KNN film 3b) in two stages by changing the temperature under the above-mentioned conditions, a KNN film 3 having all of the above-mentioned features 1 to 3 can be obtained. Furthermore, by forming the KNN film 3 in two stages by changing the temperature under the above conditions, i.e., by providing a KNN film 3a with a high (001) orientation rate and low film stress, a KNN film 3 having all of the above-mentioned features 1 to 4 can also be obtained.
[0063] (Deposition of Upper Adhesion Layer and Upper Electrode Film) After the deposition of the KNN film 3 is completed, the upper adhesion layer 7 (for example, RuO 2 layer) and the upper electrode film 4 (for example, a Pt film) are deposited in this order.
[0064] RuO as the upper adhesive layer 7 2 The conditions for forming the upper adhesive layer 7 are exemplified as follows. The deposition time for the upper adhesive layer 7 is adjusted appropriately depending on the target thickness of the upper adhesive layer 7. Target: Ru plate or the like Temperature (substrate temperature): Room temperature (25°C) or higher and 500°C or lower Discharge power density: 0.3 W / cm 2 More than 2W / cm 2 or less, preferably 0.5 W / cm 2 1W / cm or more 2 Atmosphere: Ar / O 2 Mixed gas atmosphere O 2 The ratio of the partial pressure of Ar gas to the partial pressure of O 2 Gas partial pressure): 3 / 5 to 1 / 1, preferably 3 / 4 to 1 / 1 Atmospheric pressure: 0.1 Pa or more and 1.0 Pa or less, preferably 0.2 Pa or more and 0.7 Pa or less Thickness: 1 nm or more and 200 nm or less, preferably 5 nm or more and 50 nm or less
[0065] The conditions for depositing a Pt film or the like as the upper electrode film 4 are exemplified below. The deposition time for the upper electrode film 4 is adjusted appropriately depending on the target thickness of the upper electrode film 4. Target: Pt plate or the like Temperature (substrate temperature): Room temperature (25°C) or higher and 500°C or lower Discharge power density: 1 W / cm 2 More than 5W / cm 2 Preferably 2 W / cm or less 2 More than 4W / cm 2 Atmosphere: Ar gas atmosphere Atmosphere pressure: 0.1 Pa or more and 0.5 Pa or less, preferably 0.2 Pa or more and 0.4 Pa or less Thickness: 50 nm or more and 5000 nm or less, preferably 50 nm or more and 300 nm or less
[0066] As described above, by sequentially depositing the lower adhesive layer 6, the lower electrode film 2, the KNN film 3 (KNN films 3a and 3b), the upper adhesive layer 7, and the upper electrode film 4, a piezoelectric laminate 10 as shown in FIG. 1 is obtained.
[0067] (Fabrication of Piezoelectric Element) After fabricating the piezoelectric laminate 10 as shown in FIG. 1, the piezoelectric laminate 10 is processed to form an element having a KNN film 3 (also referred to as a piezoelectric element 20).
[0068] Specifically, first, the upper electrode film 4 (including the upper adhesive layer 7) and the KNN film 3 are individually patterned by dry etching using, for example, Ar gas or a reactive gas. In the patterning, the upper electrode film 4 (including the upper adhesive layer 7) and the KNN film 3 are each formed into a predetermined shape, and a portion of the lower electrode film 2 is exposed. In the patterning, a photoresist can be used as an etching mask. FIG. 2 shows the piezoelectric stack 10 after patterning, i.e., the piezoelectric element 20. The piezoelectric element 20 shown in FIG. 2 is also referred to as a simple piezoelectric element.
[0069] 2, the lower electrode film 2 and the lower adhesive layer 6 are patterned by dry etching using, for example, Ar gas or a reactive gas, to form the lower electrode film 2 and the lower adhesive layer 6 into predetermined shapes. In this patterning, a photoresist can be used as an etching mask.
[0070] After completing the patterning of the lower electrode film 2 and the lower adhesive layer 6, the insulating film 8 and the metal wirings 9a and 9b are provided. Specifically, first, a layer made of an insulating material is provided from the upper electrode film 4 to the substrate 1 so as to cover the side surface of the KNN film 3, and then a layer of Ar gas or CF 4 The insulating layer is patterned by dry etching using a reactive gas such as silicon dioxide (SiO 2 ) or wet etching to form an insulating film 8. 2 ), aluminum oxide (Al 2 O 3 ), tantalum oxide (Ta 2 O 5 The insulating film 8 may be a single layer film or a laminated film having multiple layers stacked on top of each other. The insulating film 8 may be formed by a method such as a CVD method or a sputtering method.
[0071] After providing the insulating film 8, a layer (metal wiring layer) made of a material containing metal is provided. Then, the metal wiring layer is patterned by dry etching using Ar gas or a reactive gas, or wet etching, to form metal wirings 9a and 9b. The metal wiring 9a is formed (patterned) so as to be connected to (contact) the lower electrode film 2 but not to (contact) the upper electrode film 4, while the metal wiring 9b is formed so as to be connected to the upper electrode film 4 but not to (contact) the lower electrode film 2. The metal wirings 9a and 9b can be formed using various metals, such as Au, Al, Ti, and Cr, or alloys containing these metals as their main components. The metal wirings 9a and 9b can be single-layer films or laminates of multiple layers. The metal wirings 9a and 9b (metal wiring layer) can be provided by methods such as sputtering, vapor deposition, plating, and metal paste deposition.
[0072] Further, by Deep-RIE or wet etching, a part of the substrate 1 is removed from the back surface side of the substrate 1 (one of the two main surfaces of the substrate 1 opposite to the surface on which the lower electrode film 2 and the like are formed), thereby obtaining a piezoelectric element 20 having a membrane structure, a cantilever structure, or the like, for example, a membrane-type MEMS piezoelectric element 20 as shown in FIG.
[0073] The etching conditions for pattern processing when forming the insulating film 8 and the metal wiring 9a, 9b, and the etching conditions for the substrate 1 when processing the piezoelectric stack 10 into the piezoelectric element 20 can be general etching conditions used in semiconductor device manufacturing processes, as long as the conditions do not deteriorate the insulating properties of the KNN film 3.
[0074] (Fabrication of Piezoelectric Device Module) By connecting a voltage application means 11a to the obtained piezoelectric element 20, a device module 30 having a KNN film 3 (hereinafter also referred to as piezoelectric device module 30) is obtained. FIG. 4 shows a schematic configuration diagram of the piezoelectric device module 30 according to this embodiment. The piezoelectric device module 30 includes at least the piezoelectric element 20 and a voltage application means 11a connected to the piezoelectric element 20. The voltage application means 11a is a means for applying a voltage between the lower electrode film 2 and the upper electrode film 4 (between the electrodes). Various known means can be used as the voltage application means 11a.
[0075] By connecting the voltage application means 11a between the lower electrode film 2 and the upper electrode film 4 of the piezoelectric element 20, the piezoelectric device module 30 can function as an actuator. By applying a voltage between the lower electrode film 2 and the upper electrode film 4 by the voltage application means 11a, the KNN film 3 can be deformed. This deformation action can operate various members connected to the piezoelectric element 20. In this case, examples of uses for the piezoelectric element 20 include a head for an inkjet printer, a MEMS mirror for a scanner, and a vibrator for an ultrasonic generator.
[0076] (3) Effects According to this aspect, one or more of the following effects can be obtained.
[0077] (a) The KNN film 3 has a piezoelectric constant e 31 is 10 C / m 2 When HALT under predetermined conditions is performed at a temperature of 200° C., the leakage current density flowing through the KNN film 3 from the start of voltage application is 30 mA / cm or more (the above-mentioned feature 1). 2 The KNN film 3 simultaneously has both the feature that it takes 5 hours or more for the temperature to exceed 1000 K (the above-mentioned feature 2) and the feature that the film stress is 150 MPa or less (the above-mentioned feature 3). In other words, the KNN film 3 is a film with a high piezoelectric constant and DC stress resistance, and a small film stress.
[0078] Piezoelectric constant e of the KNN film 3 31 is 10 C / m 2The above makes it possible to improve the piezoelectric characteristics of the KNN film 3. Furthermore, since the KNN film 3 has high DC stress resistance, the KNN film 3 is less likely to undergo dielectric breakdown even when a high voltage is applied to the KNN film 3 via the upper electrode film 4 for a long period of time when the piezoelectric element 20 (piezoelectric device module 30) is driven. These factors make it possible to suitably apply the piezoelectric element 20 (piezoelectric device module 30) to actuator applications.
[0079] By setting the film stress of the KNN film 3 to 150 MPa or less, it is possible to suppress large structural deformation when processing the piezoelectric stack 10 to fabricate the piezoelectric element 20 (piezoelectric device module 30) having a membrane structure, a cantilever structure, or the like. This allows the piezoelectric element 20 (piezoelectric device module 30) obtained by processing the piezoelectric stack 10 to operate normally. For example, it becomes possible for the piezoelectric element 20 (piezoelectric device module 30) to function reliably as an actuator.
[0080] In this way, since the KNN film 3 has all of the above-mentioned features 1 to 3, the piezoelectric element 20 (piezoelectric device module 30) obtained by processing the piezoelectric laminate 10 can be suitably used for actuator applications.
[0081] (b) By interposing the KNN film 3a having a high (001) orientation rate and small film stress between the lower electrode film 2 and the KNN film 3b, the KNN film 3 can further have the above-mentioned feature of being able to withstand more than 10 million application cycles (the above-mentioned feature 4) in addition to the above-mentioned features 1 to 3. That is, the KNN film 3 can be a film having a high piezoelectric constant and DC stress resistance, small film stress, and excellent AC stress resistance.
[0082] Since the KNN film 3 has excellent AC stress resistance, i.e., the piezoelectric displacement amount is less likely to decrease even if the KNN film 3 is repeatedly deformed significantly, it is possible to improve the reliability of the piezoelectric element 20 (piezoelectric device module 30).
[0083] In this way, since the KNN film 3 has all of the above-mentioned features 1 to 4, the piezoelectric element 20 (piezoelectric device module 30) obtained by processing the piezoelectric laminate 10 can be more suitably applied to actuator applications.
[0084] (c) When depositing the KNN film 3, first, the KNN film 3a is deposited at a first temperature at which the (001) orientation rate is 95% or more and the film stress is 100 MPa or less, and then the KNN film 3b is deposited on the KNN film 3a at a second temperature at which the piezoelectric constant and DC stress resistance are increased, thereby obtaining a KNN film 3 having all of the above-mentioned features 1 to 3, and preferably all of the above-mentioned features 1 to 4.
[0085] (4) Modifications The present disclosure is not limited to the above-described aspects, and can be modified as follows, for example.
[0086] (Modification 1) After the KNN film 3 is formed, preferably after the KNN film 3 is formed and before the upper electrode film 4 (upper adhesive layer 7) is formed, the KNN film 3 may be annealed. In this modification, the same effects as those of the above-mentioned embodiment can be obtained. In addition, in this modification, the DC stress resistance can be further improved. That is, when HALT under predetermined conditions is performed at a temperature of 200°C, the leakage current density flowing through the KNN film 3 from the start of voltage application is 30 mA / cm. 2 In addition, the time until the piezoelectric constant e 31 can also be definitely increased.
[0087] The annealing conditions are exemplified as follows: Atmosphere: O-containing atmosphere such as air Temperature: 500° C. to 700° C., preferably 550° C. to 650° C. Time: 10 minutes to 5 hours, preferably 30 minutes to 3 hours
[0088] <Other Aspects> One aspect of the present invention has been specifically described above. However, the present invention is not limited to the above aspect and can be modified in various ways without departing from the spirit of the present invention. Furthermore, these aspects can be combined in any way.
[0089] In the above embodiment, the piezoelectric device module 30 functions as an actuator, but this is not limiting. That is, the piezoelectric device module 30 may also function as a sensor. In this case, the piezoelectric device module 30 includes at least a piezoelectric element 20 obtained by molding the piezoelectric stack 10 into a predetermined shape and a voltage detection unit 11b (see FIG. 4 ) connected to the piezoelectric element 20. The voltage detection unit 11b detects the voltage generated between the lower electrode film 2 and the upper electrode film 4 (between the electrodes). Various known means can be used as the voltage detection unit 11b. Connecting the voltage detection unit 11b between the lower electrode film 2 and the upper electrode film 4 of the piezoelectric element 20 allows the piezoelectric device module 30 to function as a sensor. When the KNN film 3 deforms due to a change in some physical quantity, a voltage is generated between the lower electrode film 2 and the upper electrode film 4. By detecting this voltage with the voltage detection unit 11b, the magnitude of the physical quantity applied to the KNN film 3 can be measured. In this case, the piezoelectric device module 30 can be used for, for example, an angular velocity sensor, an ultrasonic sensor, a pressure sensor, an acceleration sensor, and the like.
[0090] Furthermore, for example, when the above-mentioned piezoelectric laminate 10 is molded into the piezoelectric element 20, the substrate 1 of the piezoelectric laminate 10 may be replaced with another substrate, as long as the piezoelectric device module 30 made using the piezoelectric laminate 10 (piezoelectric element 20) can be applied to a desired purpose such as an actuator.
[0091] The following describes experimental results that support the effects of the above-described embodiment.
[0092] [Experiment 1] An experiment was conducted to confirm the temperatures that can be applied to the first temperature and the second temperature when depositing a KNN film.
[0093] (Fabrication of Samples A to J) A Si substrate with a surface oriented in the (100) plane, a thickness of 610 μm, and a diameter of 6 inches (also referred to as "φ6 inches"), on which a thermally oxidized film (thickness 200 nm) was formed, was prepared. Then, on the thermally oxidized film of this Si substrate, a ZnO layer (thickness 25 nm) was formed as a lower adhesive layer, a Pt film (preferentially oriented in the (111) plane with respect to the surface of the substrate, thickness 200 nm) was formed as a lower electrode film, a KNN film (thickness 2 μm) was formed as a piezoelectric film, and a RuO 2 A KNN layer (10 nm thick) as a lower adhesive layer, and a Pt film (100 nm thick) as an upper electrode film were deposited in this order to fabricate samples A to J, which were piezoelectric laminates. In samples A to J, the lower adhesive layer, lower electrode film, KNN film, upper adhesive layer, and upper electrode film were all deposited by RF magnetron sputtering.
[0094] The conditions for depositing the ZnO layer as the lower adhesive layer were as follows: Target: ZnO sintered body Substrate temperature: 500° C. Discharge power density: 4 W / cm 2 Atmosphere: Ar / O 2 Mixed gas atmosphere Ambient pressure: 0.3 Pa Ar gas partial pressure / O 2 Gas partial pressure: 10 / 1 Film formation time: 3 minutes (thickness 25 nm)
[0095] The conditions for depositing a Pt film as the lower electrode film were as follows: Target: Pt plate Substrate temperature: 500° C. Discharge power density: 2 W / cm 2 Atmosphere: Ar gas atmosphere Atmosphere pressure: 0.3 Pa Film formation time: 14 minutes (thickness 200 nm)
[0096] The conditions for forming the KNN film were as follows: Target: KNN sintered body Discharge power density: 3 W / cm 2 Atmosphere: Ar / O 2 Mixed gas atmosphere Ambient pressure: 0.1 Pa O 2 Gas partial pressure / Ar gas partial pressure: 1 / 20 Film formation temperature: a predetermined temperature in the range of 300°C to 800°C Film formation time: 60 minutes (thickness 2000 nm (2 μm))
[0097] RuO as an upper adhesion layer 2The conditions for depositing the layer were as follows: Target: Ru plate Substrate temperature: room temperature (25° C.) Discharge power density: 0.5 W / cm 2 Atmosphere: Ar / O 2 Mixed gas atmosphere Ambient pressure: 0.3 Pa Ar gas partial pressure / O 2 Gas partial pressure: 1 / 1 Film formation time: 6 minutes (thickness 10 nm)
[0098] The conditions for depositing a Pt film as the upper electrode film were as follows: Target: Pt plate Substrate temperature: room temperature (25° C.) Discharge power density: 2 W / cm 2 Atmosphere: Ar gas atmosphere Atmosphere pressure: 0.3 Pa Film formation time: 7 minutes (thickness 100 nm)
[0099] Samples A to J were fabricated under the same conditions as described above, except for the deposition temperature of the KNN film. The deposition temperatures of the KNN films of Samples A to J are shown in Table 1 below.
[0100] <Evaluation> For samples A to J, the (001) orientation rate, film stress, DC stress resistance, and piezoelectric constant e of the KNN film were evaluated. 31 was evaluated.
[0101] (Evaluation of (001) Orientation Ratio) The (001) orientation ratio of the KNN film was evaluated by calculating using the above formula (1) based on the peak intensity of the X-ray diffraction pattern (2θ / θ) obtained by performing XRD measurement on the KNN film. The XRD measurement was performed after the KNN film was formed and before the upper adhesive layer and the upper electrode film were formed. The calculation results of the (001) orientation ratio are shown in Table 1 below. In Table 1, "orientation ratio" means the (001) orientation ratio of the KNN film.
[0102] (Evaluation of Film Stress) The stress of the thin film on the substrate can be calculated by measuring the amount of warpage of the substrate caused by the thin film, specifically, the radius of curvature of the warpage of the substrate, as shown in the following formula (2). Therefore, in this evaluation, the radius of curvature R of the warpage of the substrate (Si substrate) of each sample was measured after the lower adhesive layer, the lower electrode film, and the KNN film were formed, and before the upper adhesive layer and the upper electrode film were formed. Then, the film stress of the KNN film of each sample was calculated using the following formula (2). In this evaluation, the radius of curvature R of the Si substrate was calculated from the warpage shape measured by a laser displacement meter of the Si substrate after the lower adhesive layer, the lower electrode film, and the KNN film were formed.
[0103]
[0104] In the above formula (2), σ is the stress of the thin film (KNN film), E s / (1-ν s ) is the biaxial elastic modulus of the substrate (Pa), h is the thickness of the substrate (m), R is the radius of curvature of the warp of the substrate (m), and t is the thickness of the KNN film (m). In samples A to J, a Si substrate was used as the substrate, so the biaxial elastic modulus value was set to 30.3. The film stress (σ) of the KNN film was calculated assuming that the Si substrate was sufficiently flat. In samples A to J, a lower adhesion layer (ZnO layer) and a lower electrode film (Pt film) were formed, but the thickness of the lower adhesion layer (25 nm) and the thickness of the lower electrode film (200 nm) were sufficiently smaller than the thickness of the KNN film (2 μm). Therefore, the influence of the lower adhesion layer and the lower electrode film was ignored when calculating the film stress of the KNN film.
[0105] The calculation results of the film stress of the KNN film of samples A to J are shown in the following Table 1. In Table 1, "compressive" means that the film stress is compressive stress, and "tensile" means that the film stress is tensile stress.
[0106] (piezoelectric constant e 31 Evaluation of the piezoelectric constant e of the KNN film 31was calculated using the following method. First, small strips measuring 20 mm in length and 2.5 mm in width were cut from each of Samples A to J. Then, as shown in Figure 5(a), one longitudinal end of each small piece obtained from Samples A to J was fixed with a clamp, and a voltage application means (not shown) was connected between the lower electrode film and the upper electrode film to fabricate a simple unimorph cantilever. Then, using the voltage application means, a sine wave negative voltage was applied to the KNN film via the upper electrode film while the lower electrode film was grounded, so as to generate an electric field of 100 kV / cm between the lower electrode film and the upper electrode film (i.e., the KNN film), thereby expanding and contracting (deforming) the KNN film. The deformation of the KNN film caused the entire cantilever to bend and stretch (vibrate), and the tip of the cantilever to reciprocate up and down. The displacement Δ (piezoelectric displacement) of the tip of the cantilever at this time was measured by irradiating the tip of the cantilever with laser light L from a laser Doppler displacement meter as shown in Figure 5(b). Then, using the displacement Δ of the tip of the cantilever, the length of the cantilever, and the applied voltage, the piezoelectric constant e when an applied electric field of 100 kV / cm was calculated. 31 The piezoelectric constant e 31 The measurement results are shown in Table 1.
[0107] In addition, in Figures 5(a) and 5(b), for ease of understanding, the lower adhesive layer and the upper adhesive layer are omitted, and when the KNN film is a laminate of a first KNN film and a second KNN film, this laminate is illustrated as a KNN film.
[0108] (Evaluation of DC Stress Resistance) The DC stress resistance was evaluated by measuring the DC stress life. Specifically, the DC stress life was measured when a negative voltage was applied to the upper electrode film (through the KNN film) at 200° C. under HALT conditions to generate an electric field of 300 kV / cm in the KNN film, and the leakage current density flowing through the KNN film from the start of voltage application was 30 mA / cm. 2 The evaluation was performed by measuring the time until the voltage exceeded 0. In HALT, the lower electrode film was grounded and a predetermined negative voltage was applied to the upper electrode film. The measurement results are shown in Table 1 below.
[0109]
[0110] In sample A, the crystal structure of the KNN film was not a perovskite structure. Therefore, in the X-ray diffraction pattern obtained by XRD measurement, no peak was observed at least within the range of 2θ of 20° to 23°, and as a result, the (001) orientation rate could not be calculated. In addition, since the crystal structure of the KNN film was not a perovskite structure, the KNN film had low pressure resistance and the piezoelectric constant e 31 When measuring the piezoelectric constant e, it was not possible to apply a predetermined voltage to the KNN film via the upper electrode film. 31 From these results, it can be confirmed that neither the first temperature nor the second temperature can be applied to the film formation temperature of Sample A.
[0111] In samples B to D, the film stress was greater than 100 MPa, and the piezoelectric constant e 31 is 10 C / m 2 The DC stress lifetime was less than 5 hours. This confirms that neither the first temperature nor the second temperature can be applied to the deposition temperatures of samples B to D.
[0112] In samples E and F, the (001) orientation rate is 95% or more, and the film stress is 100 MPa or less. This confirms that the film formation temperature of samples E and F, i.e., the temperature range of 550°C or more and 600°C or less, is applicable to the first temperature. On the other hand, in samples E and F, the piezoelectric constant e 31 is 10 C / m 2 The DC stress lifetime was less than 5 hours. This confirms that the deposition temperatures of samples E and F cannot be applied to the second temperature.
[0113] In samples G to J, the piezoelectric constant e 31 is 10 C / m 2 or higher, and the DC stress lifetime is 5 hours or more. This confirms that the deposition temperatures of samples G to J, i.e., the temperature range of 650°C or higher and 800°C or lower, are applicable to the second temperature. On the other hand, in samples G to J, the (001) orientation rate is less than 95% and the film stress is greater than 100 MPa. This confirms that the deposition temperatures of samples G to J are not applicable to the first temperature.
[0114] [Experiment 2] An experiment was conducted to confirm the effect of forming a KNN film in two stages by changing the temperature.
[0115] (Fabrication of Samples 1 to 14) A Si substrate with a surface oriented in the (100) plane, a thickness of 610 μm, a diameter of 6 inches, and a thermally oxidized film (200 nm thick) formed on the surface was prepared. Then, on the thermally oxidized film of this Si substrate, a ZnO layer (25 nm thick) was formed as a lower adhesive layer, a Pt film (preferentially oriented in the (111) plane with respect to the surface of the substrate, 200 nm thick) was formed as a lower electrode film, a KNN film (2 μm thick) was formed as a piezoelectric film, and a RuO 2 A KNN layer (10 nm thick) as a lower electrode film, and a Pt film (100 nm thick) as a lower electrode film were deposited in this order to fabricate piezoelectric laminates Samples 1 to 14. The lower adhesive layer, lower electrode film, KNN film, upper adhesive layer, and upper electrode film were all deposited by RF magnetron sputtering.
[0116] For Samples 1 to 11, the KNN films were deposited in two stages under different temperature conditions. Specifically, a first KNN film was first deposited at a first temperature, and then a second KNN film was deposited on the first KNN film at a second temperature different from the first temperature. The first and second temperatures used to deposit the KNN films for Samples 1 to 11 were as shown in Table 2 below. The deposition time at the first temperature was 6 minutes (thickness: 200 nm), and the deposition time at the second temperature was 54 minutes (thickness: 1800 nm). For Samples 12 to 14, the KNN films were deposited at a predetermined temperature without changing the temperature conditions. The temperature used to deposit the KNN films for Samples 12 to 14 was as shown in the "Second Temperature" column in Table 2 below, and the deposition time was 60 minutes (thickness: 2000 nm). The conditions other than the film-forming temperature and film-forming time when forming the KNN film, and the film-forming conditions for each film (each layer) other than the KNN film, were the same as those in the above-mentioned Experiment 1. Moreover, Samples 1 to 14 were each produced under the same conditions as those described above, except for the film-forming temperature (first temperature, second temperature) of the KNN film.
[0117] <Evaluation> For samples 1 to 14, the piezoelectric constant e of the KNN film was 31The DC stress resistance, film stress, (001) orientation rate, and AC stress resistance were evaluated.
[0118] (Evaluation of KNN Films for Piezoelectric Constant, DC Stress Resistance, Film Stress, and (001) Orientation Rate) Piezoelectric constant e of Samples 1 to 14 31 , DC stress resistance, film stress, and (001) orientation rate, respectively, are the piezoelectric constant e of the KNN film in Experiment 1 above. 31 The evaluation results are shown in Table 2 below.
[0119] In addition, in samples 1 to 14, a lower adhesive layer and a lower electrode film were also formed, but as in samples A to J, the thicknesses of the lower adhesive layer and the lower electrode film were sufficiently smaller than the thickness of the KNN film. Therefore, the influence of the lower adhesive layer and the lower electrode film was ignored when calculating the film stress of the KNN film. Also in Table 2, "compression" means that the film stress is compressive stress, and "tensile" means that the film stress is tensile stress.
[0120] (Evaluation of AC Stress Resistance) The AC stress resistance was evaluated by measuring the AC stress life. The AC stress life was evaluated as follows. First, small strips of 20 mm length x 2.5 mm width were cut out from each of Samples 1 to 14. Then, the piezoelectric constant e 31 A simple unimorph cantilever as shown in FIG. 5(a) was fabricated using a method similar to that described in the evaluation of . Then, a negative voltage was continuously applied to the upper electrode film (via the KNN film) so as to generate a unipolar AC electric field of 300 kV / cm across the KNN film. Specifically, with the lower electrode film grounded, a unipolar sine wave AC voltage with an amplitude ranging from 0 V to −60 V was continuously applied to the KNN film via the upper electrode film at a frequency of 300 Hz, thereby continuously deforming each small piece of KNN film (2 μm thick). The deformation of the KNN film caused the entire cantilever to bend and stretch (vibrate), and the tip of the cantilever continuously reciprocated up and down. The displacement Δ (piezoelectric displacement) of the tip of the cantilever at this time was calculated using the piezoelectric constant e in Experiment 1 above. 31The measurement was performed using the same method as described in the evaluation of 1. In this evaluation, the displacement Δ was measured every time the number of application cycles reached 1 million. The number of application cycles at which the displacement Δ became 80% or less of the initial value was taken as the AC stress life. Note that if the displacement Δ remained 80% or more of the initial value even after the number of application cycles reached 50 million, the measurement was stopped and the measurement result of the AC stress life was taken as more than 50 million cycles (>50 million cycles). The measurement results are shown in Table 2 below.
[0121]
[0122] In samples 3 to 5, 7, and 8, the piezoelectric constant e 31 is 10 C / m 2 From samples 3 to 5, 7, and 8, when depositing the KNN film, first, the first KNN film is deposited at a first temperature at which the (001) orientation rate is 95% or more and the film stress is 100 MPa or less, and then the second KNN film is deposited on the first KNN film at a second temperature at which the piezoelectric constant and DC stress resistance are increased, thereby achieving a piezoelectric constant e 31 is 10 C / m 2 It can be seen that a KNN film having all three characteristics, namely, a DC stress lifetime of 5 hours or more (characteristic 1 described above), a DC stress lifetime of 5 hours or more (characteristic 2 described above), and a film stress of 150 MPa or less (characteristic 3 described above), can be obtained.
[0123] In samples 1, 2, and 6, the piezoelectric constant e 31 is 10 C / m 2 The DC stress lifetime was less than 5 hours. This is thought to be because the second temperature was less than 650°C (400°C, 500°C) in Samples 1, 2, and 6. This shows that if the second temperature is not a temperature at which the piezoelectric constant and DC stress resistance of the second KNN film are high, a KNN film with a high piezoelectric constant and DC stress resistance, i.e., a KNN film having the above-mentioned features 1 and 2, cannot be obtained.
[0124] In Samples 9 to 11, the film stress exceeds 150 MPa. This is thought to be because Samples 9 and 10 had a first temperature less than 550°C (400°C, 500°C), while Sample 11 had a first temperature greater than 600°C (650°C). Samples 9 to 11 reveal that a KNN film with low film stress cannot be obtained unless the first temperature is set at a temperature at which the film stress of the first KNN film is 100 MPa or less. Furthermore, in Samples 9 to 11, the (001) orientation rate of the KNN film is less than 90%. Samples 9 to 11 reveal that a (001) orientation rate of the second KNN film cannot be increased to 90% or more unless the first temperature is set at a temperature at which the (001) orientation rate of the first KNN film is 95% or more.
[0125] Furthermore, in Samples 1 to 8, the number of application cycles until the displacement Δ became 80% or less of the initial value exceeded 50 million, and they had excellent AC stress resistance. This is thought to be due to the presence of a KNN film with a high (001) orientation rate and low film stress (for example, a KNN film with a (001) orientation rate of 95% or more and a film stress of 100 MPa or less) between the lower electrode film and the second KNN film.
[0126] In particular, in samples 3 to 5, 7, and 8, the piezoelectric constant e 31 is 10 C / m 2 or more, the DC stress life is 5 hours or more, the film stress is 150 MPa or less, and the number of application cycles described above exceeds 10 million (50 million or more). That is, it can be seen that Samples 3 to 5, 7, and 8 have, in addition to the above-mentioned Features 1 to 3, the further feature of excellent AC stress resistance (Feature 4 described above). Samples 3 to 5, 7, and 8 show that when depositing a KNN film, first deposit a first KNN film at a first temperature at which the (001) orientation rate is 95% or more and the film stress is 100 MPa or less, and then deposit a second KNN film on the first KNN film at a second temperature that is a predetermined temperature higher than the first temperature, thereby obtaining a KNN film having all of the above-mentioned Features 1 to 4.
[0127] In contrast, in Samples 9 to 14, the number of application cycles until the displacement Δ became 80% or less of the initial value was 10 million or less, indicating low AC stress resistance. This is thought to be because, in Samples 9 to 11, the first KNN film was not deposited at a temperature at which the (001) orientation rate was 95% or more and the film stress was 100 MPa or less. That is, the (001) orientation rate of the first KNN film was low and the film stress was large. Furthermore, in Samples 12 to 14, the KNN film was not formed as a laminate of the first KNN film and the second KNN film. Specifically, a KNN film with a high (001) orientation rate and low film stress was not interposed between the lower electrode film and the KNN film.
[0128] In the deposition of the KNN film, the deposition time at the first temperature was set to 6 minutes for Samples 1 to 11, but this is not limited to this. The inventors have confirmed that results similar to those described above can be obtained if the deposition time at the first temperature is in the range of 1 minute to 12 minutes. In the deposition of the KNN film, it has been confirmed that the deposition time at the first temperature, i.e., the optimal value for the thickness of the KNN film deposited at the first temperature, may have a certain degree of range.
[0129] (Regarding evaluation of film stress) In the above-mentioned Experiments 1 and 2, the film stress of the KNN film was calculated from the amount of warpage of the substrate (Si substrate), i.e., the radius of curvature of the warpage of the substrate, but this is not limiting. The film stress of the KNN film can also be determined in the state of a piezoelectric element (piezoelectric device module) in which a MEMS structure is fabricated by processing a piezoelectric laminate by comparing the MEMS simulation with the shape of the actual object.
[0130] <Preferred Aspects of the Present Disclosure> Preferred aspects of the present disclosure will be additionally described below.
[0131] (Supplementary Note 1) According to one aspect of the present disclosure, there is provided a piezoelectric element comprising: a substrate; a lower electrode film formed on the substrate; and a piezoelectric film formed on the lower electrode film and made of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen, wherein the piezoelectric film has a piezoelectric constant e 31 is 10 C / m 2or more, and when a negative voltage is applied to the upper electrode film so as to generate an electric field of 300 kV / cm between the lower electrode film and an upper electrode film provided on the piezoelectric film at a temperature of 200° C., the leakage current density flowing through the piezoelectric film from the start of application of the negative voltage is 30 mA / cm 2 the time until the temperature exceeds 100°C is 5 hours or more, and the film stress of the piezoelectric film is 150 MPa or less.
[0132] (Appendix 2) In the piezoelectric stack described in Appendix 1, preferably, when a negative voltage is continuously applied to the upper electrode film so as to generate a unipolar AC electric field of 300 kV / cm between the lower electrode film and the upper electrode film, the number of cycles of application of the voltage until the piezoelectric displacement of the piezoelectric film decreases to 80% or less of its initial value exceeds 10 million.
[0133] (Supplementary Note 3) In the piezoelectric stack according to Supplementary Note 1 or 2, preferably, a layer containing zinc and oxygen is provided between the substrate and the lower electrode film.
[0134] (Supplementary Note 4) In the piezoelectric stack according to any one of Supplementary Notes 1 to 3, preferably, the piezoelectric film contains, as a dopant, at least one element selected from copper and manganese at a concentration of 0.1 at % or more and 2.0 at % or less.
[0135] (Supplementary Note 5) According to another aspect of the present disclosure, a method for fabricating a piezoelectric film includes the steps of: forming a lower electrode film on a substrate; and forming a piezoelectric film made of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen on the lower electrode film, wherein the step of fabricating the piezoelectric film includes first forming a first piezoelectric film, which is a part of the piezoelectric film, at a first temperature at which a (001) orientation rate is 95% or more and a film stress is 100 MPa or less, and then forming a second piezoelectric film, which is another ... second temperature at which a (001) orientation rate is 95% or more and a film stress is 100 MPa or less. 31 is 10 C / m 2When a negative voltage is applied to the upper electrode film so as to generate an electric field of 300 kV / cm between the lower electrode film and the upper electrode film formed on the second piezoelectric film, the leakage current density flowing through the second piezoelectric film is 30 mA / cm 2 and forming a film on the first piezoelectric film at a second temperature at which the time until the temperature exceeds the predetermined value is 5 hours or more.
[0136] (Supplementary Note 6) In the method according to Supplementary Note 5, preferably, the thickness of the first piezoelectric film is 20% or less of the total thickness of the piezoelectric film.
[0137] (Appendix 7) In the method according to appendix 5 or 6, preferably, the first temperature is a temperature at which, when the first piezoelectric film is deposited to a thickness of 2 μm at the first temperature, the (001) orientation rate of the first piezoelectric film is 95% or more.
[0138] (Appendix 8) In the method according to any one of Appendices 5 to 7, preferably, the first temperature is a temperature at which, when the first piezoelectric film is deposited to a thickness of 2 μm at the first temperature, the film stress of the first piezoelectric film is 100 MPa or less.
[0139] (Appendix 9) The method according to any one of Appendices 5 to 8 preferably further comprises a step of providing a layer containing zinc and oxygen on the substrate before the step of depositing the piezoelectric film, and in the step of depositing the lower electrode film, the lower electrode film is deposited on the layer containing zinc and oxygen.
[0140] (Supplementary Note 10) According to yet another aspect of the present disclosure, there is provided a piezoelectric element comprising: a substrate; a lower electrode film formed on the substrate; a piezoelectric film formed on the lower electrode film and composed of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen; and an upper electrode film formed on the piezoelectric film, wherein the piezoelectric film has a piezoelectric constant e 31 is 10 C / m 2or more, and when a negative voltage is applied to the upper electrode film so as to generate an electric field of 300 kV / cm between the lower electrode film and the upper electrode film at a temperature of 200° C., the leakage current density flowing through the piezoelectric film from the start of application of the negative voltage is 30 mA / cm 2 The piezoelectric element or the piezoelectric device module is provided, wherein the time until the temperature exceeds the threshold is 5 hours or more.
[0141] (Supplementary Note 11) According to yet another aspect of the present disclosure, there is provided a piezoelectric film made of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen, the piezoelectric film having a piezoelectric constant e 31 is 10 C / m 2 or more, and when a negative voltage is applied to an upper electrode film provided on the piezoelectric film so as to generate an electric field of 300 kV / cm in the piezoelectric film at a temperature of 200°C, the leakage current density flowing in the piezoelectric film from the start of application of the negative voltage is 30 mA / cm 2 The piezoelectric film has a time until the temperature exceeds 1000 K for 5 hours or more, and a film stress of 150 MPa or less.
[0142] (Appendix 12) In the piezoelectric film, piezoelectric element, or piezoelectric device module described in Appendix 10 or 11, preferably, when a negative AC voltage is continuously applied to the upper electrode film (the upper electrode film provided on the piezoelectric film) so as to generate a unipolar AC electric field of 300 kV / cm between the lower electrode film and the upper electrode film (in the piezoelectric film), the number of application cycles of the voltage until the piezoelectric displacement of the piezoelectric film decreases to 80% or less of its initial value exceeds 10 million.
[0143] REFERENCE SIGNS LIST 1 substrate 2 lower electrode film 3 piezoelectric film 4 upper electrode film 6 (lower) adhesion layer 7 (upper) adhesion layer 10 piezoelectric laminate 20 piezoelectric element 30 piezoelectric device module
Claims
1. A piezoelectric film comprising: a substrate; a lower electrode film formed on the substrate; and a piezoelectric film formed on the lower electrode film and made of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen; 31 is 10 C / m 2 or more, and when a negative voltage is applied to the upper electrode film so as to generate an electric field of 300 kV / cm between the lower electrode film and an upper electrode film provided on the piezoelectric film at a temperature of 200° C., the leakage current density flowing through the piezoelectric film from the start of application of the negative voltage is 30 mA / cm 2 the time until the piezoelectric film exceeds the threshold value is 5 hours or more, and the film stress of the piezoelectric film is 150 MPa or less.
2. The piezoelectric stack described in claim 1, wherein when a negative AC voltage is continuously applied to the upper electrode film so as to generate a unipolar AC electric field of 300 kV / cm between the lower electrode film and the upper electrode film, the number of cycles of voltage application until the piezoelectric displacement of the piezoelectric film decreases to 80% or less of its initial value exceeds 10 million.
3. The piezoelectric stack according to claim 1 or 2, wherein the piezoelectric film contains at least one element selected from copper and manganese as a dopant at a concentration of 0.1 at % or more and 2.0 at % or less.
4. A method for manufacturing a piezoelectric film comprising the steps of: forming a lower electrode film on a substrate; and forming a piezoelectric film composed of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen on the lower electrode film. In the step of forming the piezoelectric film, first, a first piezoelectric film, which is a part of the piezoelectric film, is formed at a first temperature at which the (001) orientation rate is 95% or more and the film stress is 100 MPa or less, and then, a second piezoelectric film, which is the other part of the piezoelectric film, is formed at a first temperature at which the piezoelectric constant e of the second piezoelectric film is 100 MPa or less. 31 is 10 C / m 2 or more, and when a negative voltage is applied to the upper electrode film so as to generate an electric field of 300 kV / cm between the lower electrode film and the upper electrode film formed on the second piezoelectric film, the leakage current density flowing through the second piezoelectric film is 30 mA / cm 2 forming a film on the first piezoelectric film at a second temperature at which the time it takes for the film to exceed the second temperature is 5 hours or more.
5. A piezoelectric device comprising: a substrate; a lower electrode film formed on the substrate; a piezoelectric film formed on the lower electrode film and composed of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen; and an upper electrode film formed on the piezoelectric film; 31 is 10 C / m 2 or more, and when a negative voltage is applied to the upper electrode film so as to generate an electric field of 300 kV / cm between the lower electrode film and the upper electrode film at a temperature of 200° C., the leakage current density flowing through the piezoelectric film from the start of application of the negative voltage is 30 mA / cm 2 the time until the piezoelectric film exceeds the threshold value is 5 hours or more, and the film stress of the piezoelectric film is 150 MPa or less.
6. The piezoelectric element described in claim 5, wherein when a negative voltage is continuously applied to the upper electrode film so as to generate a unipolar AC electric field of 300 kV / cm between the lower electrode film and the upper electrode film, the number of cycles of voltage application until the piezoelectric displacement of the piezoelectric film decreases to 80% or less of its initial value exceeds 10 million.
Citation Information
Patent Citations
Piezoelectric thin film element
JP2009295786A
Laminate board with piezoelectric film, element with piezoelectric film, and method for manufacturing laminate board with piezoelectric film
JP2018207055A
Piezoelectric elements, piezoelectric actuators, hard disk drives, inkjet printers, and piezoelectric sensors
JP2015529963A
Piezoelectric thin film-attached laminate board, piezoelectric thin-film device and manufacturing method thereof
JP2017076730A
Piezoelectric laminate, piezoelectric element, and manufacturing method of piezoelectric laminate
JP2021012909A
Cited By
Stacked substrate having piezoelectric film, method for manufacturing stacked substrate, and piezoelectric element
EP4580381A1
Device including piezoelectric element and method for manufacturing the device
EP4580382A1