High-beta crystalline phase polyvinylidene fluoride fiber piezoelectric film and preparation method thereof
Through emulsion polymerization and electrospinning technology, polyvinylidene fluoride nanofiber membrane with high β crystal phase content was prepared, which solved the problems of low piezoelectric efficiency and poor mechanical properties of nanofibers during electrospinning, and achieved more efficient Piezoelectric properties.
Patent Information
- Application Number
- CN202411056199.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-02
AI Technical Summary
In the prior art, the nanofibers obtained by polyvinylidene fluoride during electrospinning are not piezoelectric, have poor mechanical properties, and insufficient β crystal form content, resulting in the failure of the performance of piezoelectric materials to fully exert their performance.
The polyvinylidene fluoride resin with a certain long branched chain content was prepared by emulsion polymerization. By adjusting the viscosity and concentration of the electrospinning solution, a nanofiber film with high β crystal phase content was formed under the action of an electric field. Specific steps include emulsion polymerization, electrospinning and heat treatment, controlling the long branched chain content and solution concentration to increase the proportion of β crystal form.
It has achieved the preparation of finer and higher β-crystalline polyvinylidene fluoride nanofiber membranes, which has improved the efficiency and mechanical properties of piezoelectric materials and has good application prospects.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of piezoelectric materials, and specifically relates to PVDF fiber piezoelectric film technology. Background Art
[0002] Piezoelectric materials can realize the conversion between mechanical energy and electrical energy, which is beneficial to energy conservation. When mechanical force is applied to piezoelectric polymers, charges will be generated on the polymer surface. These charges can be exported through electrodes and used by external electrical devices, thus realizing the conversion between mechanical energy and electrical energy. Piezoelectric ceramics, which have obvious piezoelectric effect among piezoelectric materials, have been widely used in sensors, transducers and other fields.
[0003] Polyvinylidene fluoride (PVDF) has outstanding piezoelectric properties - good flexibility, impact resistance, and friction resistance. These properties of PVDF will help greatly expand the application areas of piezoelectric materials.
[0004] At present, polyvinylidene fluoride has been found to have five crystal forms: α, β, γ, δ and ε. Among them, the α crystal form has the highest stability, while the β crystal form is an important factor in the piezoelectricity of PVDF. The existing piezoelectric products using polyvinylidene fluoride as raw material are mainly piezoelectric films prepared by the casting method, and the high β crystal content and β crystal orientation are achieved by stretching and polarizing the film. However, the above preparation method has relatively harsh conditions, complicated steps, and high requirements for equipment.
[0005] The electrospinning method is currently considered to be a relatively simple method for preparing ultrafine fibers or nanofibers. By adjusting the process parameters of electrospinning (such as solution concentration, solvent ratio, solution conductivity, voltage, flow rate, receiving distance, etc.), the morphological structure or aggregated structure of the fiber can be easily changed or controlled. During the electrospinning process, the polymer jet is stretched and thinned by the electric field force in the high-voltage electrostatic field, while the solvent evaporates and solidifies, and finally forms fibers deposited on the receiving plate. During the fiber forming process, the stretching of the electric field force helps the α crystal form of the PVDF fiber to transform into the β crystal form, which provides better conditions for preparing fibers with a higher β crystal content. At present, many studies have shown that electrospinning is a simple method for preparing PVDF submicron or nanofibers with a higher β crystal content. However, the β crystal form in the PVDF nanofibers obtained by electrospinning is almost less than 85%, which leads to the low efficiency of piezoelectric materials. There are also nano-doping, blending and other means to increase the proportion of β crystal form, which also leads to the excellent performance of PVDF not being fully exerted. Summary of the invention
[0006] In view of the defects of the prior art, the present invention provides a high-β crystalline polyvinylidene fluoride fiber piezoelectric film and a preparation method thereof, which solves the problem that the piezoelectric efficiency of the nanofibers obtained in the electrospinning process of the existing polyvinylidene fluoride is low and the mechanical properties are poor.
[0007] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0008] First, a method for preparing a high-β crystalline polyvinylidene fluoride fiber piezoelectric film is provided, comprising the following steps:
[0009] Step 1: using vinylidene fluoride monomer and difluoromonochloroethane for emulsion polymerization to prepare a polyvinylidene fluoride resin having a weight average molecular weight of 500,000 to 800,000, a long branched chain content of 1.2‰ to 5‰, and a rotational viscosity of 5000 to 8000 mPa.s in a 7% mass fraction NMP solution at 25°C;
[0010] Step 2: Prepare the polyvinylidene fluoride resin obtained in step 1 into an electrospinning precursor solution, and use an electrospinning method to spin the electrospinning precursor solution into a film, wherein the concentration of the electrospinning precursor solution is ≤10%.
[0011] Preferably, the concentration of the electrospinning precursor solution is ≤8%, the purity of the vinylidene fluoride monomer is 99.5% to 99.9%, and the content of difluorochloroethane is 500ppm to 1000ppm.
[0012] Preferably, when the polyvinylidene fluoride resin is prepared by emulsion polymerization, a redox initiator is used for initiation, and the polymerization is carried out in the presence of a dispersant, a chain transfer agent, and a dispersant. The polymerization temperature is 25-70° C. and the reaction pressure is 2.5-5 MPa.
[0013] Preferably, the oxidant is one of ammonium persulfate, potassium persulfate, sodium persulfate, hydrogen peroxide, succinic acid peroxide, methyl ethyl ketone peroxide, cyclohexane peroxide, tert-butyl hydroperoxide, and potassium permanganate; and / or, the reducing agent is one of sodium metabisulfite, sodium hypochlorite, sodium sulfite, ferrous sulfate, ascorbic acid, sodium citrate, bleaching agent, oxalic acid, and N,N-dimethylaniline.
[0014] Preferably, the molar ratio of the oxidant to the reductant is 1:0.8 to 1:3.5.
[0015] Preferably, the dispersing agent is one or two or more of polyethylene imine, polyvinyl pyrrolidone, polyethylene glycol-maleimide, stearic acid-polyethylene glycol-maleimide; and / or, the amount of the dispersing agent relative to the mass fraction of the vinylidene fluoride monomer participating in the reaction is 0.5‰ to 5‰.
[0016] Preferably, the steps of spinning and film making by electrospinning are as follows:
[0017] S1: dissolving polyvinylidene fluoride in a mixed solution of N-methyl-2-pyrrolidone and acetone, heating in a water bath at 60-80°C and magnetically stirring for 4-8h, and stirring evenly to obtain a precursor solution for electrospinning;
[0018] S2: placing the electrospinning precursor solution in an electrospinning device for electrospinning;
[0019] S3: heat-treating the vinylidene fluoride nanofiber membrane to further remove the solvent, wherein the heat-treating temperature is 80-130°C.
[0020] Preferably, the polyvinylidene fluoride is dissolved in powder form; and / or the mass concentration of the polyvinylidene fluoride in the precursor solution is 4% to 20%.
[0021] Preferably, in step S1, the mass ratio of N-methyl-2-pyrrolidone to acetone in the mixed solution of N-methyl-2-pyrrolidone and acetone is 85:10 to 75:10; and / or, in step S1, the mass ratio of polyvinylidene fluoride, N-methyl-2-pyrrolidone, and acetone is 5 to 15:75 to 85:10; and / or, the electrospinning process parameters are: the inner diameter of the metal needle is 0.4 mm to 0.8 mm; the spinning voltage is 12 kV to 20 kV; the receiving distance is 15 cm to 35 cm; the spinning solution propulsion speed is 0.5 mL / h to 4 mL / h, and the polyvinylidene fluoride film is collected with aluminum foil.
[0022] In addition, a high-β-crystalline polyvinylidene fluoride piezoelectric film is provided, which is prepared by the above-mentioned preparation method and has a 50-100nm nanoscale fiber structure and a β-crystalline structure greater than 85%.
[0023] The present invention adopts the above technical solution and has the following beneficial effects:
[0024] By adopting emulsion polymerization, a polyvinylidene fluoride resin with a certain long chain branch content is obtained. By adjusting the content of the long chain branches and the viscosity of the electrospinning solution, a finer polyvinylidene fluoride nanofiber membrane with a higher β-crystal content can be prepared.
[0025] Wherein, the long chain branch content of the polyvinylidene fluoride is 1.2‰ to 5‰. When the long chain branch content of polyvinylidene fluoride is low, there are fewer entanglement points in the low-concentration electrospinning solution, which is not conducive to the preparation of a nanofiber membrane with a complete morphology at a low concentration. When the long chain branch content is too much, the interaction between the polyvinylidene fluoride molecular chains is more obvious. Therefore, controlling the content of the long chain branch is more conducive to more entanglement points at low concentrations, and in electrospinning, it can be fully stretched in the electric field. Better preparation of finer nanofiber membranes with higher β-crystalline content.
[0026] The applicant has found through research that if the side chain is quite long, that is, the molecular weight of the side chain reaches or exceeds three times the critical molecular weight (Mb>3Mc), the side chain itself becomes entangled. At this time, the PVDF molecular chains are intertwined to form a "self-crosslinking" system, which is characterized by a high or ultra-high solution viscosity of the polymer. This system can obtain high viscosity at low concentrations, so that finer nanofibers and a higher proportion of β crystals can be obtained in electrospinning. Generally speaking, the concentration of electrospinning solution is generally above 8%, but in order to reduce the diameter of the nanofibers, it is preferred to reduce the concentration of the spinning solution to below 8%. Therefore, for the viscosity of polyvinylidene fluoride resin, it is designed to be 5000 to 8000 mpa.s for the rotational viscosity of 7% mass fraction NMP solution at 25°C, so that the above-mentioned low-concentration solution can obtain high viscosity, which is convenient for spinning processing and obtains nanofibers with finer diameters.
[0027] Moreover, the nanofiber membrane has good application prospects in the field of piezoelectric materials.
[0028] The specific technical solutions and beneficial effects of the present invention will be described in detail in the following specific embodiments. DETAILED DESCRIPTION
[0029] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] Those skilled in the art will appreciate that, in the absence of conflict, the features in the following embodiments and implementations may be combined with each other.
[0031] The applicant starts from the polymer system. The factors that affect the viscosity of polymer solutions are mainly concentration, solvent and polymer side chains. Many existing patents have studied the first two aspects. This application starts from the influence of long polymer side chains on the viscosity of polymer solutions. If the side chains are quite long, that is, the molecular weight of the side chains reaches or exceeds three times the critical molecular weight (Mb>3Mc), the side chains themselves become entangled. At this time, the PVDF molecular chains are intertwined to form a "self-crosslinking" system, and its obvious feature is that the polymer has a high or ultra-high solution viscosity. This system allows the spinning solution to still have a higher viscosity at a lower concentration than the polyvinylidene fluoride resin in the prior art, so that finer nanofibers and a higher proportion of β crystals can be obtained in electrospinning.
[0032] In order to overcome the problem that the nanofibers obtained in the electrospinning process of existing polyvinylidene fluoride have low piezoelectric efficiency and poor mechanical properties, based on the above research on the influence of long polymer branch chains on the viscosity of polymer solutions, the present invention provides a method for preparing a high-β crystalline polyvinylidene fluoride fiber piezoelectric film, comprising the following steps:
[0033] Step 1: using vinylidene fluoride monomer and difluoromonochloroethane for emulsion polymerization to prepare a polyvinylidene fluoride resin having a weight average molecular weight of 500,000 to 800,000, a long branched chain content of 1.2‰ to 5‰, and a rotational viscosity of 5000 to 8000 mPa.s in a 7% mass fraction NMP solution at 25°C;
[0034] Step 2: Prepare the polyvinylidene fluoride resin obtained in step 1 into a polyvinylidene fluoride solution, and use an electrostatic spinning method to spin the polyvinylidene fluoride solution into a film.
[0035] For the above technical scheme, the present invention obtains polyvinylidene fluoride resin with long chain branches through emulsion polymerization method, uses this resin as raw material to prepare low concentration electrospinning solution, and obtains polyvinylidene fluoride nanofibers with high β crystal phase ratio and small fiber size through electrospinning.
[0036] Among them, the content of long chain branches is 1.2‰ to 5‰. The long chain branch content described in the present invention refers to the proportion of carbon atoms containing long chain branches on the main chain of the polymer. When there are N carbon atoms with long chain branches on 1000 carbon atoms, the long chain branch content is N‰. In vinylidene fluoride polymers, long chain branches refer to branches containing side chains of -CH2CF2-CH(CH2CF2-)CF2-; the specific degree of branching can be calculated by the fluorine spectrum of NMR.
[0037] When the content of long chain branches of polyvinylidene fluoride is low, there are fewer entanglement points in the low-concentration electrospinning solution, which is not conducive to the preparation of a nanofiber membrane with a complete morphology at a low concentration. When the content of long chain branches is high, the interaction between the molecular chains of polyvinylidene fluoride is more obvious. Therefore, controlling the content of long chain branches is more conducive to more entanglement points at low concentrations, and in electrospinning, it can be fully stretched in the electric field. Better preparation of finer, higher β-crystalline nanofiber membranes. However, the content of long chain branches should not be too much, which can easily lead to gelation of the electrospinning solution and cannot be processed. Preferably, the long chain branch content of the polyvinylidene fluoride is 2‰ to 5‰, for example, 3‰ to 4‰.
[0038] Based on the principle of electrospinning, the lower the solution concentration, the finer the nanofibers, and the more β-crystals will account for. However, the solution concentration cannot be infinitely low, and there is a minimum concentration. If the concentration is too low, the nanofibers will be uneven and the utilization value will be low. Usually, the concentration of electrospinning solution is generally 8%-15%. The present invention controls the concentration of spinning solution to ≤10%, preferably 3%-8%, such as 3%, 5%, and 8%. In order to prepare nanofibers with finer fiber diameters, if the concentration of the spinning solution is too low, the spinning process will be unstable and easy to break. If the concentration is too high, the diameter of the obtained nanofibers will be large and the expected performance target will not be achieved.
[0039] The rotational viscosity of the electrospinning solution is mainly affected by the degree of branching and the average molecular weight. When the degree of branching is high or the molecular weight is large, the molecular chains are easily entangled, the electrospinning solution has a high viscosity, and gel appears after a long time of standing; when the degree of branching is small or the molecular weight is small, there are fewer entanglements between the polyvinylidene fluoride molecular chains, and the rotational viscosity of the spinning solution is low, making it difficult to stabilize the size of the nanofibers during the spinning process. Therefore, when the above-mentioned long chain branch content is determined, the molecular weight is controlled within the range of 500,000 to 800,000 to obtain a more stable nanofiber membrane. Preferably, the weight average molecular weight of the polyvinylidene fluoride is 600,000 to 750,000, for example, 650,000, 700,000, or 750,000.
[0040] The polyvinylidene fluoride resin prepared by the present invention has a rotational viscosity of 5000-8000 mPa.s in a 7% mass fraction NMP solution at 25° C. and is used for electrospinning, so that it still has a high solution viscosity under the above low concentration conditions, and finer nanofibers can be obtained in electrospinning, and the fibers have a higher proportion of β crystals.
[0041] The present invention adopts emulsion polymerization method to prepare the polyvinylidene fluoride resin, which is initiated by redox initiator, in the presence of dispersant, chain transfer agent and auxiliary dispersant, with polymerization temperature of 25-70°C and reaction pressure of 2.5-5MPa.
[0042] Generally speaking, the molecular weight of polyvinylidene fluoride resin can be easily adjusted by conventional means. However, increasing the content of long-chain branches is relatively complicated. The existing technology generally achieves this by increasing the reaction temperature, using graft polymerization, using cross-linking methods, etc., but it is difficult to achieve precise control and the process is cumbersome.
[0043] The polyvinylidene fluoride resin with a higher β-crystalline content can be prepared by a redox-initiated emulsion polymerization method, so the present application has made further research on this basis.
[0044] The applicant discovered through experiments that the use of low-purity vinylidene fluoride monomers for polymerization reactions will produce more long chain branches than the use of high-purity vinylidene fluoride monomers, especially after the content of difluoromonochloroethane increases, the phenomenon is more obvious. The applicant speculates that it may be that multiple chain transfer and re-initiation processes have occurred for difluoromonochloroethane in the reaction, resulting in the formation of a multi-arm structure. However, in order to increase the content of PVDF long chain branches, the applicant increased the content of difluoromonochloroethane, and the reaction efficiency was too low and the product molecular weight was low. Afterwards, the applicant was pleasantly surprised to find that the use of some polyamine surfactants has a promoting effect on the above-mentioned process of producing long chain branches, so that in the presence of a certain content of difluoromonochloroethane, adding such substances can achieve the purpose of increasing the content of PVDF long chain branches.
[0045] According to the above findings, preferably, the low-purity vinylidene fluoride monomer has a purity of 99.5% to 99.9%, for example, 99.8% to 99.9%. The content of difluoromonochloroethane is 500ppm to 1000ppm, for example, 600ppm, 800ppm. The polyamine surfactant is one or two or more of polyethyleneimine, polyvinylpyrrolidone, polyethylene glycol-maleimide, and stearic acid-polyethylene glycol-maleimide. The applicant uses one or a combination of two or more of them as a dispersant in the preparation process of polyvinylidene fluoride. The amount of dispersant used is 0.5‰ to 5‰ relative to the mass fraction of vinylidene fluoride monomer. The amount is adjusted according to the need for long chain branching content.
[0046] Preferably, the redox initiator, the oxidant is one of ammonium persulfate, potassium persulfate, sodium persulfate, hydrogen peroxide, succinic acid peroxide, methyl ethyl ketone peroxide, cyclohexane peroxide, tert-butyl hydroperoxide, potassium permanganate, and the reducing agent is one of sodium metabisulfite, sodium hypochlorite, sodium sulfite, ferrous sulfate, ascorbic acid, sodium citrate, chlorinated oxalic acid, oxalic acid, and N,N-dimethylaniline. The molar ratio of the oxidant to the reducing agent is 1:0.8 to 1:3.5, for example, 1:0.8, 1:2, 1:3. Different oxidants and reducing agents are selected for combination according to the reaction temperature.
[0047] Preferably, the redox initiator is composed of potassium persulfate and ascorbic acid, and the molar ratio thereof is 1:1 to 1:3, such as 1:1, 1:2, 1:3. Preferably, the dispersant is a dispersant used in conventional polyvinylidene fluoride emulsion polymerization, and a common fluorinated surfactant or a non-fluorinated surfactant can be used.
[0048] Preferably, the chain transfer agent is a chain transfer agent used in conventional polyvinylidene fluoride emulsion polymerization, such as alkanes, alcohols, ketones and other substances with chain transfer ability.
[0049] The steps of preparing nanofibers and polyvinylidene fluoride membranes with high β-crystalline content by electrospinning are as follows:
[0050] S1: Dissolve polyvinylidene fluoride with long chain branches in a mixed solution of N-methyl-2-pyrrolidone and acetone, heat in a water bath at 60-80°C and stir magnetically for 4-8 hours, and stir evenly to obtain a precursor solution for electrospinning.
[0051] S2: Place the electrospinning precursor solution in the electrospinning equipment. The electrospinning process parameters are: the inner diameter of the metal needle is 0.4mm-0.8mm; the spinning voltage is 12kV-20kV; the receiving distance is 15cm-35cm; the spinning solution propulsion speed is 0.5mL / h-4mL / h. The polyvinylidene fluoride film is collected with aluminum foil.
[0052] S3: heat-treating the vinylidene fluoride nanofiber membrane to further remove the solvent, wherein the heat-treating temperature is 80-130°C.
[0053] Preferably, in step S1, PVDF is in powder form, which is easier to dissolve in the organic solvent used. PVDF is first dissolved in a mixed solution of N-methyl-2-pyrrolidone and acetone. The heating temperature in step S1 is preferably 60-70°C.
[0054] Preferably, the heating time in step S1 is 4 to 6 hours.
[0055] The mass concentration of PVDF in the solution is 4% to 20%, preferably, the mass concentration of PVDF in the solution is 5% to 15%. Since polyvinylidene fluoride has long branched chains, it has a higher viscosity at low concentrations. Too high a concentration can easily cause needle blockage and discontinuous fibers; too low a concentration can also easily cause the fibers to be too thin and broken.
[0056] In step S1, the ratio of the mixed solution of N-methyl-2-pyrrolidone and acetone is preferably (85:10 to 75:10). The addition of acetone makes the solvent more volatilized during the electrospinning process and has the effect of inducing the formation of β-crystalline phase. However, the acetone content cannot be too high. Acetone is a poor solvent, and adding too much will have a certain impact on the dissolution of PVDF.
[0057] Preferably, in step S2, the spinning voltage of electrospinning is preferably 14-18 kV. If the spinning voltage is too high, unstable flow may occur when the solution is sprayed. If the spinning voltage is too low, the fiber received by the receiving device may contain nodes or particles. The propulsion rate affects the speed and spinning process of the spinning fiber. If the propulsion rate is too low, the continuity of the spinning fiber will be affected because the continuous supply of the spinning solution cannot be formed. If the propulsion rate is too high, the amount of spinning solution at the moment is too much, which may easily cause clogging of the needle and cause the spinning to be unable to proceed. Preferably, the propulsion rate of spinning is 0.5 ml / h to 1.0 ml / h.
[0058] Preferably, in step S3, the temperature of the heat treatment is 80-130° C. More preferably, the temperature of the heat treatment is 100-125° C.
[0059] The relative content of the β-crystalline phase F(β) refers to the ratio of the β-crystalline phase to the total crystalline components of PVDF, which can be calculated from the peak area of the absorption peak corresponding to the crystal form in the FTIR data.
[0060] Compared with the prior art, the advantages of the present invention are:
[0061] By adopting a specific emulsion polymerization method, a polyvinylidene fluoride resin with a certain long chain branch content is obtained. By adjusting the content of the long chain branch and the viscosity of the electrospinning solution, a finer polyvinylidene fluoride nanofiber membrane with a higher β-crystalline content is prepared. The nanofiber membrane has good application prospects in the field of piezoelectric materials.
[0062] The technical solution of the present invention is described below in conjunction with specific embodiments.
[0063] The weight average molecular weight in the present invention is obtained by gel permeation chromatography (GPC) testing, and the mobile phase is N,N-dimethylformamide (DMF).
[0064] The degree of branching was tested by nuclear magnetic resonance (NMR) and 19F spectrum.
[0065] The long chain branching test method is:
[0066] Long chain branching refers to a branch containing a side chain of -CH2CF2-CH(CH2CF2-)CF2-, which is at -99.5ppm in the 19F spectrum; long chain branch content C = I(-99.5ppm) / I(-92ppm~118ppm), I(-99.5ppm) refers to the peak integrated intensity at -99.5ppm in the 19F spectrum, and I(-92ppm~118ppm) refers to the sum of the peak integrated intensities from -92ppm to 118ppm.
[0067] The β-crystal form was measured by infrared spectroscopy.
[0068] Infrared spectrum measurement method:
[0069] There are three common crystal forms in PVDF: α-crystal, β-crystal and γ-crystal. In the infrared spectrum, the peak position of α-crystal is at 408cm -1 、532cm -1 、612cm -1 、766cm -1 、795cm -1 、855cm -1 、976cm -1 、1182cm -1 、1400cm -1 The peak position of β-crystal is 445cm -1 、470cm -1 、511cm -1 、600cm -1 、840cm -1 、1279cm -1 The peak position of γ-crystal is 431cm -1 、512cm -1 、776cm -1 、812cm -1 、833cm -1 、1234cm -1 The relative content of β crystal was calculated according to the intensity and area integration of each absorption peak.
[0070] The diameter of PVDF nanofiber membranes was measured by scanning electron microscopy.
[0071] Scanning electron microscope measurement method:
[0072] The polyvinylidene fluoride nanofiber membrane obtained by electrospinning was sliced, glued to the test platform of the scanning electron microscope with conductive glue, and then gold was sprayed. After the gold spraying was completed, an electron microscope test was performed, and then the diameter and diameter distribution of the nanofiber were measured.
[0073] Example 1
[0074] In a 15L autoclave, add 10kg of deionized water, 30g of dispersant ammonium perfluoropolyether carboxylate, 3g of co-dispersant polyethyleneimine, and 3g of chain transfer agent ethyl acetate, and replace with nitrogen until the oxygen content in the reactor is less than 30ppm. Heat the reactor to 40°C, fill the reactor with vinylidene fluoride until the pressure is 3.5MPa, add 12g of oxidant potassium persulfate and 8g of reducing agent ascorbic acid, start the reaction, and continuously add vinylidene fluoride during the reaction to keep the pressure of the reactor constant, wherein the content of difluoromonochloroethane in the vinylidene fluoride monomer is 500ppm. When the reaction amount reaches 3kg, stop the reaction, then release the pressure of the reactor to obtain polyvinylidene fluoride emulsion, and the emulsion is filtered, washed, and dried to obtain polyvinylidene fluoride.
[0075] The test results are as follows: solution viscosity 6000 mPa.s (25°C, 7 wt% PVDF / NMP solution), weight average molecular weight 700,000, and long chain branch content 1.3%.
[0076] 5g of the prepared PVDF powder was dissolved in a mixed solvent of 85g NMP and 10g acetone, stirred magnetically at 70°C for 4 hours, cooled to room temperature, and a 5wt% PVDF solution was prepared. The solution was used for electrostatic spinning, the capacity of the syringe used was 10ml, the model of the needle was 27G (inner diameter 0.21mm, outer diameter 0.41mm), the spinning temperature was 25°C, the humidity was 25%, the spinning voltage was 16kV, the spinning capacity was 4ml, the propulsion rate was 0.8ml / h, the receiving distance was 15cm, the roller rotation rate was 2000rpm, and the spinning time was 5h. The prepared nanofibers were heat treated at 110°C for 6h.
[0077] The test results are as follows: the diameter of the polyvinylidene fluoride nanofiber is 110 nm, and the relative content of β crystal is 90%.
[0078] Example 2
[0079] Compared with Example 1, the experimental pressure was changed to 5 MPa, and the content of dichloroethylene in the monomer vinylidene fluoride was 800 ppm. Other conditions remained unchanged.
[0080] The test results are as follows: solution viscosity 6800mPa.s (25°C, 7wt% PVDF / NMP solution), weight average molecular weight 750,000, and long chain branch content 2.28%.
[0081] The test results are as follows: the diameter of the polyvinylidene fluoride nanofiber is 100 nm, and the relative content of β crystal is 90%.
[0082] Example 3
[0083] Compared with Example 1, the experimental temperature was changed by 60° C., and the content of dichloroethylene in the monomer vinylidene fluoride was 800 ppm. Other conditions remained unchanged.
[0084] The test results are as follows: solution viscosity 6500mPa.s (25°C, 7wt% PVDF / NMP solution), weight average molecular weight 680,000, and long chain branch content 3.35%.
[0085] The test results are as follows: the diameter of the polyvinylidene fluoride nanofiber is 85 nm, and the relative content of β crystal is 93%.
[0086] Example 4
[0087] Compared with Example 1, the amount of polyethyleneimine was increased to 9 g, and other conditions remained unchanged.
[0088] The test results are as follows: solution viscosity 6900 mPa.s (25°C, 7 wt% PVDF / NMP solution), weight average molecular weight 640,000, and long chain branch content 2.75%.
[0089] The test results are as follows: the diameter of the polyvinylidene fluoride nanofiber is 90 nm, and the relative content of β crystal is 90%.
[0090] Comparative Example 1
[0091] Compared with Example 1, no reducing agent was added, 40% of the oxidizing agent was initially added, and the remaining 60% was continuously added during the reaction. The reaction temperature was 90°C.
[0092] The test results are as follows: solution viscosity 4000 mPa.s (25°C, 7 wt% PVDF / NMP solution), weight average molecular weight 470,000, and long chain branch content 2.12%.
[0093] The spinning solution concentration in Example 1 could not be spun normally, so the PVDF solution concentration was increased to 8%.
[0094] The test results are as follows: the diameter of the polyvinylidene fluoride nanofiber is 190 nm, and the relative content of β crystal is 74%.
[0095] Comparative Example 2
[0096] Compared with Example 1, the concentration of monomer vinylidene fluoride is 99.95%, and the content of difluorochloroethane is 10 ppm.
[0097] The test results are as follows: solution viscosity 3000 mPa.s (25°C, 7 wt% PVDF / NMP solution), weight average molecular weight 810,000, long chain branch content 0.3%.
[0098] The spinning solution concentration in Example 1 could not be spun normally, so the PVDF solution concentration was increased to 12%.
[0099] The test results are as follows: the diameter of the polyvinylidene fluoride nanofiber is 410 nm, and the relative content of β crystal is 88%.
[0100] Comparative Example 3
[0101] Compared to Example 1, no polyethyleneimine was added.
[0102] The test results are as follows: solution viscosity 3300 mPa.s (25°C, 7 wt% PVDF / NMP solution), weight average molecular weight 710,000, and long chain branch content 0.9%.
[0103] The spinning solution concentration in Example 1 could not be spun normally, so the PVDF solution concentration was increased to 12%.
[0104] The test results are as follows: the diameter of the polyvinylidene fluoride nanofiber is 370 nm, and the relative content of β crystal is 87%.
[0105] It can be seen from Experimental Example 1 and Comparative Examples 2 and 3 that difluoromonochloroethane is conducive to the generation of long chain branches of polyvinylidene fluoride resin, while polyethyleneimine has a significant promoting effect. Polyvinylidene fluoride with long chain branches can be used to prepare finer polyvinylidene fluoride nanofiber membranes by electrospinning at lower concentrations. Mainly due to the presence of long chain branches, polyvinylidene fluoride can be better entangled at low concentrations. The low concentration spinning solution is stretched more thoroughly under the action of the electric field in electrospinning, and the prepared nanofibers are finer.
[0106] It can be seen from Examples 1, 2, 3 and Comparative Example 1 that the use of a redox system at a relatively low reaction temperature can effectively increase the content of the β-crystalline phase.
[0107] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that the present invention includes but is not limited to the contents described in the above specific embodiments. Any modification that does not deviate from the functional and structural principles of the present invention will be included in the scope of the claims.
Claims
1. A method for preparing a high-β crystalline polyvinylidene fluoride fiber piezoelectric film, characterized in that: The steps include: Step 1: using vinylidene fluoride monomer and difluoromonochloroethane for emulsion polymerization to prepare a polyvinylidene fluoride resin having a weight average molecular weight of 500,000 to 800,000, a long branched chain content of 1.2‰ to 5‰, and a rotational viscosity of 5000 to 8000 mPa.s in a 7% mass fraction NMP solution at 25°C; Step 2: Prepare the polyvinylidene fluoride resin obtained in step 1 into an electrospinning precursor solution, and use an electrospinning method to spin the electrospinning precursor solution into a film, wherein the concentration of the electrospinning precursor solution is ≤10%.
2. The method for preparing a high-β crystalline polyvinylidene fluoride fiber piezoelectric film according to claim 1, characterized in that: The concentration of the electrospinning precursor solution is ≤8%, the purity of the vinylidene fluoride monomer is 99.5% to 99.9%, and the content of difluorochloroethane is 500ppm to 1000ppm.
3. The method for preparing a high-β crystalline polyvinylidene fluoride fiber piezoelectric film according to claim 1, characterized in that: When the polyvinylidene fluoride resin is prepared by emulsion polymerization, a redox initiator is used for initiation, and the polymerization is carried out in the presence of a dispersant, a chain transfer agent, and an auxiliary dispersant, and the polymerization temperature is 25-70° C. and the reaction pressure is 2.5-5 MPa.
4. The method for preparing a high-β crystalline polyvinylidene fluoride fiber piezoelectric film according to claim 3, characterized in that: The oxidant is one of ammonium persulfate, potassium persulfate, sodium persulfate, hydrogen peroxide, succinic acid peroxide, methyl ethyl ketone peroxide, cyclohexane peroxide, tert-butyl hydroperoxide, and potassium permanganate; and / or the reducing agent is one of sodium metabisulfite, sodium hypochlorite, sodium sulfite, ferrous sulfate, ascorbic acid, sodium citrate, bleaching agent, oxalic acid, and N,N-dimethylaniline.
5. The method for preparing a high-β crystalline polyvinylidene fluoride fiber piezoelectric film according to claim 3 or 4, characterized in that: The molar ratio of the oxidant to the reductant is 1:0.8 to 1:3.
5.
6. The method for preparing a high-β crystalline polyvinylidene fluoride fiber piezoelectric film according to claim 3, characterized in that: The dispersing aid is one or two or more of polyethylene imine, polyvinyl pyrrolidone, polyethylene glycol-maleimide, stearic acid-polyethylene glycol-maleimide; and / or, the amount of the dispersing aid is 0.5‰ to 5‰ relative to the mass fraction of the vinylidene fluoride monomer participating in the reaction.
7. The method for preparing a high-β crystalline polyvinylidene fluoride fiber piezoelectric film according to claim 1, characterized in that: The steps of spinning and film making by electrospinning are as follows: S1: dissolving polyvinylidene fluoride in a mixed solution of N-methyl-2-pyrrolidone and acetone, heating in a water bath at 60-80°C and magnetically stirring for 4-8h, and stirring evenly to obtain a precursor solution for electrospinning; S2: placing the electrospinning precursor solution in an electrospinning device for electrospinning; S3: heat-treating the vinylidene fluoride nanofiber membrane to further remove the solvent, wherein the heat-treating temperature is 80-130°C.
8. The method for preparing a high-β crystalline polyvinylidene fluoride fiber piezoelectric film according to claim 7, characterized in that: The polyvinylidene fluoride is dissolved in powder form; and / or the mass concentration of the polyvinylidene fluoride in the precursor solution is 4% to 20%.
9. The method for preparing a high-β crystalline polyvinylidene fluoride fiber piezoelectric film according to claim 7, characterized in that: In step S1, the mass ratio of N-methyl-2-pyrrolidone to acetone in the mixed solution of N-methyl-2-pyrrolidone and acetone is 85:10-75:10; and / or, in step S1, the mass ratio of polyvinylidene fluoride, N-methyl-2-pyrrolidone and acetone is 5-15:75-85:10; and / or, the electrospinning process parameters are: the inner diameter of the metal needle is 0.4mm-0.8mm; the spinning voltage is 12kV-20kV; the receiving distance is 15cm-35cm; the spinning solution propulsion speed is 0.5mL / h-4mL / h, and the polyvinylidene fluoride film is collected with aluminum foil.
10. A high-β crystalline polyvinylidene fluoride piezoelectric film, characterized in that: The fiber is prepared by the preparation method described in any one of claims 1 to 9, has a 50-100nm nanoscale fiber structure, and has a β crystal content of more than 85%.
Citation Information
Patent Citations
Anti-static high-beta-crystal-content polyvinylidene fluoride nanometer composite fiber film and preparation method thereof
CN103556234A
Polyvinylidene fluoride directionally arranged piezoelectric fiber membrane and preparation method thereof
CN104695129A
Preparation method of polyvinylidene fluoride hollow fiber ultrafiltration membrane
CN113441018A
Preparation method of polyvinylidene fluoride piezoelectric nanofiber membrane with branch piezoelectric enhanced nanostructure
CN114960027A
Low temperature production of fluoropolymers
CN118159572A
Cited By
High-purity beta-phase PVDF (Polyvinylidene Fluoride) nanofiber membrane as well as preparation method and application thereof
CN121087698A