Rail and method for manufacturing same
The rail steel composition and manufacturing method address the issue of poor fatigue resistance in high axle-heavy railways by minimizing pro-eutectoid cementite formation, resulting in improved crack propagation resistance and extended rail life.
Patent Information
- Application Number
- PCT/JP2024/001016
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2024-01-16
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional rail steels with pearlite structures, used in high axle-heavy railways, suffer from poor fatigue crack propagation resistance due to the formation of hard and brittle pro-eutectoid cementite structures, leading to increased breakage and frequent rail replacement.
A rail steel composition with specific ranges of C, Si, Mn, and Cr, controlled to minimize pro-eutectoid cementite formation through optimized austenite grain size and pearlite block size, using a component parameter (HC) to suppress brittle crack propagation, and a manufacturing method involving hot rolling and controlled cooling rates to enhance fatigue resistance.
The solution effectively reduces fatigue crack propagation rates, extending rail life and preventing railway accidents by stabilizing fatigue crack propagation resistance, even with high axle loads and increased wheel traffic.
Smart Images

Figure JP2024001016_03102024_PF_FP_ABST
Abstract
Description
Rail and manufacturing method thereof
[0001] The present invention relates to a rail and a method for manufacturing the same.
[0002] In high-axle-load railways, which are primarily used for transporting ore, the load on the axles of freight cars is much higher than that of passenger cars, and the rails are used in a harsh environment. For this reason, steel with a pearlite structure has traditionally been used for the rails, with an emphasis on wear resistance.
[0003] In recent years, efforts have been made to further increase the load weight of freight cars in order to improve the efficiency of rail transport. In addition, the number of wheels passing over the rails has also increased due to the expansion of transport capacity.
[0004] The passage of wheels applies repeated tensile and compressive stress to rails. As load weights and the number of wheels passing over rails increase, rail breakage occurs at the sole of the rail, and the frequency of rail replacement tends to increase year by year. For this reason, there is a growing demand for rail steel with improved fatigue crack propagation resistance at the sole of the rail.
[0005] Under the above-mentioned circumstances, various studies have been conducted with the aim of further improving the breakage resistance of the rail base. For example, Patent Document 1 describes a steel rail having a pearlite structure containing 0.65 to 1.40% C, in which pearlite blocks with grain sizes of 1 to 15 μm are present in an area of 0.2 mm at least in a region extending from the bottom surface to a depth of 10 mm. 2 More than 200 rails per square meter have been proposed.
[0006] Patent Document 2 proposes a rail containing, by mass%, 0.65 to 1.20% C, 0.05 to 2.00% Si, and 0.05 to 2.00% Mn, with the remainder being Fe and unavoidable impurities, in which 97% or more of the head and bottom surfaces are pearlite structures, the surface hardness of the pearlite structure is in the range of Hv 320 to 500, the maximum surface roughness is 180 μm or less, and the ratio of the surface hardness to the maximum surface roughness is 3.5 or more.
[0007] Patent Document 3 discloses a rail in which, after rolling, the rail head is accelerated from the austenite region while the rail bottom is accelerated between 800 and 450°C at a cooling rate of 1 to 5°C / sec, resulting in an average pearlite hardness of HB320 or more at the rail bottom.
[0008] JP 2006-57127 A International Publication No. 2011 / 021582 JP 1-139724 A
[0009] However, the above-mentioned conventional technologies still have the following problems to be solved. When the C content is set to 0.65 to 1.40%, as in the technologies described in Patent Documents 1 and 2, depending on the heat treatment conditions, a hard and brittle pro-eutectoid cementite structure is formed at the prior austenite grain boundaries, so improvement in fatigue damage resistance cannot be expected. Furthermore, with the technology described in Patent Document 3, depending on the combination of ingredients and manufacturing conditions, a pro-eutectoid cementite structure may also be formed, resulting in an increase in the fatigue crack propagation rate, so it is difficult to say that material control is sufficient.
[0010] The present invention has been made to advantageously solve the above-mentioned problems, and has as its object to provide a rail having excellent fatigue crack propagation resistance at the sole of the rail, together with a method for manufacturing the same.
[0011] To solve the above problems, the inventors fabricated rails with varying contents of C, Si, Mn, and Cr and conducted extensive research into the microstructure and fatigue crack propagation resistance of the rail base sole. As a result, they discovered a compositional parameter (the HC parameter, expressed by equation (1) below) defined by the C, Si, Mn, and Cr contents, and found that the value of this parameter is related to the amount of pro-eutectoid cementite. Furthermore, they discovered that by controlling the value of the HC parameter to a value equal to or smaller than the value of the parameter composed of the prior austenite grain size and pearlite block size in the rail base sole, excellent fatigue crack propagation resistance can be obtained in the rail base sole, even if a large amount of pro-eutectoid cementite is present. More details are as follows.
[0012] The present inventors have discovered that the increase in fatigue crack propagation rate due to the presence of pro-eutectoid cementite is due to the brittle fracture of the {100} plane of ferrite in pearlite adjacent to the pro-eutectoid cementite in the plastic zone at the tip of the fatigue crack, as shown in the schematic diagram of Figure 1. Furthermore, the present inventors have discovered that by controlling the ratio of the prior austenite grain size, which serves as the pro-eutectoid cementite formation site, to the pearlite block size, which corresponds to the structural unit of the brittle fracture, depending on the amount of pro-eutectoid cementite formed, the frequency of encounter between the plastic zone formed at the tip of the fatigue crack and the {100} plane of ferrite in pearlite can be reduced, thereby suppressing brittle crack propagation. In other words, even when a large amount of pro-eutectoid cementite is present, the aforementioned effect of suppressing fatigue crack propagation rate can be stably obtained by coarsening the prior austenite grain size or reducing the pearlite block size.
[0013] The present invention is based on the above findings and has the following gist: [1] A rail having a chemical composition containing 0.70 to 1.20 mass% C, 0.10 to 1.20 mass% Si, 0.10 to 1.50 mass% Mn, 0.035 mass% or less P, 0.020 mass% or less S, and 0.05 to 2.00 mass% Cr, with the balance being Fe and unavoidable impurities, in which the area fraction of pearlite structures at a depth of 1 mm from the surface of the central part of the rail foot sole is 95% or more, and the value of HC, expressed by the following formula (1), satisfies the following formula (2): HC={(12 × [% C])+([% Si] / 10)+([% Mn] / 20)+([% Cr] / 18)} 2... (1) HC ≦ (120 × GS) / (1.1 × BS) ... (2) where, [%C], [%Si], [%Mn] and [%Cr] are the contents (mass%) of C, Si, Mn and Cr, respectively, GS is the prior austenite grain size (μm) in the center of the sole of the rail, and BS is the pearlite block size (μm) in the center of the sole of the rail. [2] The rail of [1], wherein the chemical composition further contains at least one selected from the group consisting of V: 0.30% by mass or less, Cu: 1.0% by mass or less, Ni: 1.0% by mass or less, Nb: 0.05% by mass or less, Mo: 2.0% by mass or less, Al: 0.07% by mass or less, W: 1.0% by mass or less, Co: 1.0% by mass or less, B: 0.005% by mass or less, Ti: 0.05% by mass or less, Sb: 0.05% by mass or less, Mg: 0.01% by mass or less, Ca: 0.02% by mass or less, and Sn: 0.05% by mass or less. [3] A manufacturing method of a rail according to [1] or [2], comprising heating a steel material having the chemical composition according to [1] or [2] at a heating temperature of 1350°C or less, hot rolling the steel material under conditions that the finishing temperature at the center of the rail foot sole is 850°C or more, cooling the steel material at the center of the rail foot sole from 850°C at an average cooling rate CR1 (°C / sec) until the temperature at the center of the rail foot sole reaches 750°C, and then cooling the steel material at an average cooling rate CR2 (°C / sec) from 750°C until the temperature at the center of the rail foot sole reaches a cooling stop temperature T, wherein the cooling stop temperature T is in the range of 400 to 650°C, and the average cooling rates CR1 (°C / sec) and CR2 (°C / sec) satisfy the following formulas (3) and (4), respectively: HC / 300≦CR1≦3.0 ... (3) HC / 120≦CR2≦6.0 ... (4)
[0014] According to the present invention, it is possible to provide a rail with excellent fatigue crack propagation resistance in the rail base portion, together with a manufacturing method thereof. The rail of the present invention contributes to extending the service life of rails for high axle load railways and preventing railway accidents, and is industrially useful. Furthermore, the rail manufacturing method of the present invention is industrially useful because it can stably improve the fatigue crack propagation resistance in the rail base portion by optimizing the heat treatment conditions after hot rolling.
[0015] 5 is a schematic diagram showing the influence of pro-eutectoid cementite, prior austenite grain size, and pearlite block size on fatigue crack propagation rate. Fig. 5 is a cross-sectional view of a rail showing each portion of the rail and the position where test specimens for observing the prior austenite grain size and pearlite block size were taken. Fig. 5 is a diagram showing the cross-sectional area and thickness of the rail base. Fig. 5 is a diagram showing the position where test specimens for fatigue crack propagation tests are taken. Fig. 5 explains the shape of test specimens for fatigue crack propagation tests. Fig. 5(a) is a front view, Fig. 5(b) is a side view, and Fig. 5(c) is an enlarged front view of the notch.
[0016] <Rail Parts> First, the designations of each part of a rail in the present invention will be explained with reference to the rail cross-sectional view of Figure 2. In the rail 1 shown in Figure 2, 11 denotes the rail head, 12 denotes the rail web, and 13 denotes the rail foot, with the underside of the rail foot 13 referred to as the rail sole 14. The rail sole center is the portion located near the center of the rail sole in the width direction. For example, if the width dimension of the rail sole 14 is W, the rail sole center is the area within a width range of ±0.075 × W from the center of the width of the rail sole 14. Hereinafter, the rail head, rail web, rail foot, rail sole, and rail sole center will also be referred to as the head, web, foot, sole, and sole center, respectively.
[0017] <Composition of Rail> Next, the composition of the steel of the rail of the present invention will be described. In the following description, "%" represents "mass %" unless otherwise specified.
[0018] C: 0.70-1.20% C is an essential element for ensuring the strength of the pearlite structure, i.e., fatigue damage resistance. If the C content is less than 0.70%, it is difficult to achieve excellent fatigue crack propagation resistance in the sole. Furthermore, if the C content exceeds 1.20%, a large amount of proeutectoid cementite forms at the austenite grain boundaries during cooling after hot rolling, resulting in an increase in the fatigue crack propagation rate. While proeutectoid cementite may be present even when the C content is 1.20% or less, its effects can be avoided by controlling the prior austenite grain size and block size in the central sole so that they satisfy the above formula (2). For these reasons, the C content is set to a range of 0.70-1.20%, preferably 0.70-0.89%, and more preferably 0.70-0.85%.
[0019] Si: 0.10 to 1.20% In addition to its effect as a deoxidizer, Si contributes to reducing the fatigue crack propagation rate by raising the pearlite equilibrium transformation temperature and reducing lamellar spacing. For this reason, the Si content must be 0.10% or more. However, if it exceeds 1.20%, weldability deteriorates due to the high bonding strength of Si with oxygen. Furthermore, because Si has the effect of shifting the eutectoid point toward the low-C side, excessive addition promotes the formation of pro-eutectoid cementite, leading to an increase in the fatigue crack propagation rate. For these reasons, the Si content is limited to a range of 0.10 to 1.20%, preferably 0.15 to 1.10%, and more preferably 0.20 to 1.00%.
[0020] Mn: 0.10 to 1.50% Mn is an element that contributes to reducing the fatigue crack propagation rate by lowering the pearlite transformation temperature and reducing lamellar spacing. A Mn content of less than 0.10% does not provide sufficient effects. On the other hand, a Mn content of more than 1.50% is likely to produce a martensite structure, which can lead to hardening and embrittlement during heat treatment and welding of rails, resulting in material deterioration. Furthermore, because Mn has the effect of shifting the eutectoid point toward the low-C side, excessive addition promotes the formation of pro-eutectoid cementite, leading to an increase in the fatigue crack propagation rate. For these reasons, the Mn content is limited to a range of 0.10 to 1.50%, preferably 0.20 to 1.40%, and more preferably 0.30 to 1.30%.
[0021] P: 0.035% or less If P is contained in an amount exceeding 0.035%, ductility will be deteriorated. Therefore, the P content is set to 0.035% or less, preferably 0.020% or less. The lower limit of the P content is not particularly limited and may be 0%, but industrially it is usually set to more than 0%, and excessively reducing the P content will increase refining costs. From an economical standpoint, it is preferable that the P content be 0.001% or more.
[0022] S: 0.020% or less S is an element that exists in steel mainly in the form of A-type inclusions. However, if the S content exceeds 0.020%, the amount of these inclusions increases significantly and coarse inclusions form, resulting in a deterioration in the cleanliness of the steel. Therefore, the S content is set to 0.020% or less, preferably 0.015% or less, and more preferably 0.010% or less. The lower limit of the S content is not particularly limited and may be 0%, but industrially it is usually set to more than 0%, and excessively reducing the S content increases refining costs. From an economic standpoint, it is preferable that the S content be 0.0005% or more.
[0023] Cr: 0.05 to 2.00% Cr is an element that contributes to reducing the fatigue crack propagation rate by increasing the pearlite equilibrium transformation temperature and reducing lamellar spacing. A Cr content of less than 0.05% does not adequately suppress fatigue crack propagation. On the other hand, a Cr content of more than 2.00% increases the hardenability of the steel and makes martensite more likely to form. Furthermore, when manufactured under conditions that prevent martensite formation, proeutectoid cementite forms at prior austenite grain boundaries, increasing the fatigue crack propagation rate. For these reasons, the Cr content is set to a range of 0.05 to 2.00%, preferably 0.10 to 1.60%, and more preferably 0.15 to 1.40%.
[0024] Furthermore, in the composition of the present invention, it is not sufficient for each element to satisfy the above-mentioned range; it is also important to control the value of the component parameter HC, which corresponds to the amount of pro-eutectoid cementite, to a value equal to or smaller than the value of a predetermined parameter composed of the prior austenite grain size GS and the pearlite block size BS in the center of the sole of the rail.
[0025] The value of the component parameter HC corresponding to the amount of pro-eutectoid cementite is calculated by the following formula (1): HC = {(12 × [%C]) + ([%Si] / 10) + ([%Mn] / 20) + ([%Cr] / 18)} 2 ... (1) Here, [%C], [%Si], [%Mn], and [%Cr] are the respective contents (mass%) of C, Si, Mn, and Cr. The HC value is preferably 75 to 200, more preferably 90 to 150, from the viewpoint of achieving both high strength of pearlite structure and suppression of pro-eutectoid cementite, i.e., ensuring fatigue damage resistance.
[0026] In the present invention, a predetermined parameter consisting of the prior austenite grain size GS and the pearlite block size BS is expressed as (120×GS) / (1.1×BS). The value of this parameter and the value of HC satisfy the relationship of the following formula (2): HC≦(120×GS) / (1.1×BS) (2) where, GS is the prior austenite grain size (μm) in the center of the sole of the rail, and BS is the pearlite block size (μm) in the center of the sole of the rail.
[0027] The chemical composition of the rail used in the present invention may optionally contain, in addition to the above-mentioned essential elements, at least one element selected from the following: V: 0.30 mass% or less, Cu: 1.0 mass% or less, Ni: 1.0 mass% or less, Nb: 0.05 mass% or less, Mo: 2.0 mass% or less, Al: 0.07 mass% or less, W: 1.0 mass% or less, Co: 1.0 mass% or less, B: 0.005 mass% or less, Ti: 0.05 mass% or less, Sb: 0.05 mass% or less, Mg: 0.01 mass% or less, Ca: 0.02 mass% or less, and Sn: 0.05 mass% or less. The above-mentioned optional elements will be explained below.
[0028] V: 0.30% or less V is an element that forms carbonitrides in steel and disperses and precipitates in the matrix, improving the wear resistance of the steel. If the V content exceeds 0.30%, workability deteriorates and alloy costs, i.e., rail manufacturing costs, increase. For these reasons, when the composition contains V, it is preferable to set the V content upper limit to 0.30%. To achieve the effect of improving wear resistance, the V content is preferably 0.001% or more. A more preferable range for the V content is 0.001 to 0.15%.
[0029] Cu: 1.0% or less Like Cr, Cu is an element that can further increase the strength of steel through solid solution strengthening. If the Cu content exceeds 1.0%, Cu cracking is more likely to occur, so if the composition contains Cu, the Cu content is preferably 1.0% or less. From the perspective of increasing strength, the Cu content is preferably 0.001% or more. A more preferred range for the Cu content is 0.001 to 0.5%.
[0030] Ni: 1.0% or less Ni is an element that can increase the strength of steel without degrading ductility. Furthermore, adding Ni in combination with Cu can suppress Cu cracking, so it is desirable to also add Ni when the composition contains Cu. However, if the Ni content exceeds 1.0%, the hardenability of the steel increases, the amount of martensite and bainite formed increases, and the wear resistance and fatigue damage resistance of the railhead tend to decrease. For these reasons, if the composition contains Ni, the Ni content is preferably 1.0% or less. From the viewpoint of increasing strength, the Ni content is preferably 0.001% or more. A more preferred range of Ni content is 0.001 to 0.5%.
[0031] Nb: 0.05% or less Nb combines with C in the steel during and after hot rolling to form a rail, precipitating as carbides. This effectively refines the pearlite colony size, significantly improving wear resistance, fatigue damage resistance, and ductility, and significantly contributing to extending the service life of the rail. However, even if the Nb content exceeds 0.05%, the improvement in wear resistance and fatigue damage resistance saturates, and no effect commensurate with the increase in content is obtained. For these reasons, if the composition contains Nb, the upper limit of the Nb content is preferably 0.05%. To obtain a sufficient effect on extending the service life of the rail, the Nb content is preferably 0.001% or more. A more preferred range of Nb content is 0.001 to 0.03%.
[0032] Mo: 2.0% or less Mo is an element that can further increase the strength of steel through solid solution strengthening. Mo also has the effect of shifting the eutectoid point toward the high-C side, thereby suppressing the formation of pro-eutectoid cementite. However, if the Mo content exceeds 2.0%, the amount of bainite formed in the steel increases, reducing the wear resistance of the rail head. For these reasons, if the composition contains Mo, the Mo content is preferably 2.0% or less. From the viewpoint of increasing strength, the Mo content is preferably 0.001% or more. A more preferred range of Mo content is 0.001 to 1.0%.
[0033] Al: 0.07% or less Al is an element that can be added as a deoxidizer. If the Al content exceeds 0.07%, the high bonding strength of Al with oxygen causes the formation of large amounts of oxide-based inclusions in the steel, resulting in a decrease in the ductility of the steel. Therefore, if the composition contains Al, the Al content is preferably 0.07% or less. There is no particular lower limit for the Al content, but for deoxidation purposes, it is preferably 0.001% or more. A more preferred range for the Al content is 0.001 to 0.03%.
[0034] W: 1.0% or less W is an element that precipitates as carbides during and after hot rolling to form the rail shape, improving the strength and ductility of the rail through precipitation strengthening. If the W content exceeds 1.0%, martensite forms in the steel, resulting in reduced ductility. For these reasons, if the composition contains W, the W content is preferably 1.0% or less. There is no particular lower limit for the W content, but to achieve the aforementioned effect of improving strength and ductility, a W content of 0.001% or more is preferred. A more preferred range for the W content is 0.001 to 0.5%.
[0035] Co: 1.0% or less Co is an element that can further increase the strength of steel by increasing the pearlite equilibrium transformation temperature and reducing lamellar spacing. Co also has the effect of suppressing the precipitation of proeutectoid cementite. If the Co content exceeds 1.0%, martensite forms in the steel, resulting in a decrease in ductility. For these reasons, if the composition contains Co, the Co content is preferably 1.0% or less. There is no particular lower limit for the Co content, but for high strength, it is preferably 0.001% or more. A more preferred range of Co content is 0.001 to 0.5%.
[0036] B: 0.005% or less B is an element that precipitates as a nitride in steel during and after hot rolling to form a rail shape, improving the strength and ductility of the steel through precipitation strengthening. If the B content exceeds 0.005%, martensite is formed, resulting in a decrease in the ductility of the steel. For these reasons, if the composition contains B, the B content is preferably 0.005% or less. There is no particular lower limit for the B content, but to achieve the aforementioned effect of improving strength and ductility, it is preferably 0.001% or more. A more preferred range for the B content is 0.001 to 0.003%.
[0037] Ti: 0.05% or less. Ti precipitates in steel as carbides, nitrides, or carbonitrides during and after hot rolling to form a rail shape, improving the strength and ductility of the steel through precipitation strengthening. If the Ti content exceeds 0.05%, coarse carbides, nitrides, or carbonitrides are formed, resulting in a decrease in the ductility of the steel. For these reasons, if the composition contains Ti, the Ti content is preferably 0.05% or less. While there is no particular lower limit for the Ti content, a Ti content of 0.001% or more is preferred to achieve the aforementioned effects of improving strength and ductility. A more preferred range of Ti content is 0.001 to 0.03%.
[0038] Sb: 0.05% or less Sb is an element that has a significant effect of preventing decarburization of steel during reheating of rail steel material in a heating furnace before hot rolling. If the Sb content exceeds 0.05%, it adversely affects the ductility and toughness of the steel. Therefore, if the composition contains Sb, the Sb content is preferably 0.05% or less. While there is no particular lower limit for the Sb content, a content of 0.001% or more is preferred to achieve the effect of reducing the decarburized layer. A more preferred range of Sb content is 0.001 to 0.03%.
[0039] Mg: 0.01% or less Mg is an element that combines with oxygen to precipitate MgO, further increasing strength. If the Mg content exceeds 0.01%, the increase in MgO has a negative effect on the ductility and toughness of the steel. Therefore, if the composition contains Mg, the Mg content is preferably 0.01% or less. There is no particular lower limit for the Mg content, but in order to achieve the above-mentioned strength-improving effect, it is preferably 0.001% or more. A more preferred range for the Mg content is 0.001 to 0.005%.
[0040] Ca: 0.02% or less Ca is an element that combines with oxygen to precipitate CaO, further increasing strength. If the Ca content exceeds 0.02%, the increase in CaO has a negative effect on the ductility and toughness of the steel. Therefore, if the composition contains Ca, the Ca content is preferably 0.02% or less. There is no particular lower limit for the Ca content, but in order to achieve the above-mentioned strength-improving effect, it is preferably 0.001% or more. A more preferred range of Ca content is 0.001 to 0.01%.
[0041] Sn: 0.05% or less Sn is an element that has a significant effect of preventing decarburization of steel during reheating of rail steel material in a heating furnace before hot rolling. Sn content exceeding 0.05% adversely affects the ductility and toughness of steel, so if the composition contains Sn, the Sn content is preferably 0.05% or less. While there is no particular lower limit for the Sn content, a value of 0.001% or more is preferred to achieve the effect of reducing the decarburized layer. A more preferred range of Sn content is 0.001 to 0.01%.
[0042] The chemical composition of the steel for rails of the present invention, other than the above-mentioned essential and optional elements, consists of Fe and unavoidable impurities. Examples of unavoidable impurities include N and O, with N content up to 0.008% and O content up to 0.004%. Depending on the raw materials, resources, and manufacturing equipment, impurities other than N and O may be unavoidably mixed into the steel. Examples of raw materials include iron ore, reduced iron, and scrap. The above impurities are also acceptable as long as they do not impair the objectives of the present invention. Examples of impurities other than N and O include Pb, Zr, Bi, Zn, Se, As, Te, Tl, Cd, Hf, Ag, Hg, Ga, Ge, and REM.
[0043] <Rail Microstructure> The rail of the present invention is a pearlitic rail. From the viewpoint of fatigue crack propagation resistance, the microstructure at a depth of 1 mm from the surface of the central sole of the rail has an area fraction of pearlite of 95.0% or more. The area fraction of pearlite may be 100%. The remaining structure other than pearlite at a depth of 1 mm from the surface of the central sole is acceptable if its area fraction is 5.0% or less, and may even be 0%. In particular, pro-eutectoid cementite is acceptable if its area fraction is 3.0% or less, as it does not significantly affect fatigue crack propagation resistance. Examples of remaining structures other than pro-eutectoid cementite include ferrite, bainite, and martensite. The microstructure and area fraction of the central sole can be measured using the measurement methods described in the Examples below.
[0044] (Prior austenite grain size GS in the center of the sole) In the rail of the present invention, the prior austenite grain size GS in the center of the sole is preferably 30 to 140 μm, and more preferably 30 to 80 μm from the viewpoint of preventing excessive deterioration in ductility and toughness. The prior austenite grain size GS in the center of the sole can be measured by the measurement method described in the Examples below.
[0045] (Pearlite Block Size BS) The rail of the present invention preferably has a pearlite block size BS in the center of the sole of 15 to 45 μm, more preferably 15 to 30 μm, because by reducing the pearlite block size, which corresponds to the structural unit of brittle fracture, it is possible to further shorten the length of brittle crack propagation. The pearlite block size BS in the center of the sole can be measured by the measurement method described in the Examples below.
[0046] <Rail Shape> The shape of the rail in the present invention is not particularly limited, and may be any of the rail shapes described in JIS E 1101:2001, BS EN13674-1:2011, American Railway Engineering and Maintenance-of-Way Association (AREMA), etc.
[0047] <Rail Manufacturing Method> A method for manufacturing a rail of the present invention will now be described. The rail of the present invention can be manufactured by sequentially subjecting a steel material having the above-described chemical composition to the following treatments (1) to (3): (1) hot rolling, (2) primary cooling, and (3) secondary cooling.
[0048] The steel material used as the rail material has the above-mentioned rail composition and can be produced by any method. In general, it is preferable to produce the steel material by casting, particularly continuous casting.
[0049] (1) Hot rolling Heating temperature: 1350°C or less Prior to hot rolling, the steel material is heated to a heating temperature of 1350°C or less. If the heating temperature exceeds 1350°C, the steel material may partially melt due to excessive temperature rise, which may cause defects inside the rail. There is no particular lower limit for the heating temperature, but it is preferably 1150°C or higher in order to reduce deformation resistance during rolling.
[0050] Finishing rolling temperature: 850°C or higher. The heated steel material is hot-rolled to form a rail shape. Here, finishing rolling refers to one pass of final rolling using the final rolling groove of a single final rolling mill. The finishing rolling temperature in hot rolling is 850°C or higher. If the finishing rolling temperature is lower than 850°C, rolling is performed in the low-austenite temperature range, which not only introduces processing strain into the austenite grains but also significantly elongates the austenite grains. The increased austenite grain boundary area increases the number of nucleation sites for pro-eutectoid cementite, resulting in a decrease in fatigue crack propagation resistance. Therefore, the finishing rolling temperature is 850°C or higher, preferably 900°C or higher. While there is no particular upper limit for the finishing rolling temperature, excessive coarsening of the prior austenite grain size reduces ductility and toughness, so it is preferable to set it to 1050°C or lower. Here, the rolling finish temperature is the surface temperature of the center of the rail sole at the entry side of the rolling mill in the final rolling pass, and can be measured with a radiation thermometer.
[0051] The thickness reduction (thickness reduction) of the rail base in the final rolling pass, the finish rolling, is preferably set to a value greater than the area reduction of the previous pass. For example, the area reduction may be set to 11%, while the thickness reduction at the center of the rail base is set to 15% or more. This allows for the introduction of large strain into the center of the rail base, further promoting the refinement of the microstructure after pearlite transformation and effectively increasing the fatigue strength of the base. Furthermore, by designing the groove shape so that the width of the base is increased during the finish rolling, rolling with a relatively large thickness reduction compared to the area reduction can be performed stably. The area reduction of the rail base is calculated based on the area of the shaded area marked with S in the rail cross-section diagram in Figure 3, where S0 is the cross-sectional area of the base before finish rolling and S1 is the cross-sectional area of the base after finish rolling, as follows: Area Reduction (%) = {(S0 - S1) / S0} × 100. The thickness reduction rate of the rail base is calculated based on the height indicated by H in the figure, where H0 is the thickness of the base before finish rolling and H1 is the cross-sectional area of the base after finish rolling, as follows: Thickness reduction rate (%) = {(H0 - H1) / H0} × 100. Other hot rolling conditions are not particularly limited.
[0052] (2) Primary Cooling: Average Cooling Rate (CR1 [°C / sec]) from 850°C to 750°C: HC / 300≦CR1≦3.0 Next, accelerated cooling is performed. The cooling from 850°C to 750°C is referred to as primary cooling. The temperature range from 850°C to 750°C corresponds to the temperature range in which pro-eutectoid cementite forms. If the average cooling rate CR1 in this temperature range is less than HC / 300 [°C / sec], the amount of pro-eutectoid cementite increases. This increases the likelihood of cracks occurring at the interface of the pro-eutectoid cementite structure, potentially reducing the fatigue damage resistance of the rail. Therefore, the average cooling rate CR1 in primary cooling is set to at least HC / 300 [°C / sec], and preferably at least HC / 200 [°C / sec].
[0053] On the other hand, if the average cooling rate CR1 of the primary cooling exceeds 3.0°C / sec, a martensite structure may be formed, which may result in a decrease in ductility and fatigue damage resistance. Therefore, the average cooling rate CR1 of the primary cooling is set to 3.0°C / sec or less, and preferably 2.0°C / sec or less.
[0054] (3) Secondary Cooling: Average cooling rate (CR2 [°C / sec]) from 750°C to the cooling stop temperature T: HC / 120 ≤ CR2 ≤ 6.0. Secondary cooling follows the primary cooling described above. Secondary cooling is performed from 750°C to the cooling stop temperature T, which is in the range of 400–650°C. If the average cooling rate from the secondary cooling start temperature of 750°C to the cooling stop temperature T of the secondary cooling in the range of 400–650°C is less than HC / 120 [°C / sec], the pearlite block size becomes coarse and the lamellar spacing also becomes coarse. In other words, the increase in pearlite block size, which corresponds to the structural unit of brittle fracture, causes brittle crack propagation to take longer, potentially reducing the fatigue damage resistance of the rail. In addition, the increased cooling time at low temperatures reduces productivity and increases the manufacturing costs of the rail. Therefore, the average cooling rate CR2 of the secondary cooling is set to HC / 120 [°C / sec] or more, and preferably HC / 100 [°C / sec] or more.
[0055] On the other hand, if the average cooling rate CR2 of the secondary cooling exceeds 6.0°C / sec, a martensite structure may be formed, which may result in a decrease in ductility and fatigue damage resistance. Therefore, the average cooling rate CR2 of the secondary cooling is set to 6.0°C / sec or less, and preferably 4.0°C / sec or less.
[0056] The value of HC in relation to the average cooling rates CR1 and CR2 can be calculated by the above formula (1), and is preferably 75-200, more preferably 90-150.
[0057] In both primary and secondary cooling, the temperature used to determine the average cooling rate is the surface temperature at the center of the rail's sole, which can be measured with a radiation thermometer. The cooling stop temperature T during secondary cooling is the surface temperature at the center of the rail's sole after accelerated cooling has stopped (before reheating), measured with a radiation thermometer.
[0058] The accelerated cooling method is not particularly limited, and can be carried out, for example, by cooling using online heat treatment equipment. The cooling medium is not particularly limited, and one or more selected from air, spray water, mist, etc. can be used, but air is preferred. For example, the average cooling rate of the rail sole can be controlled by installing multiple air injection devices on the sole and adjusting the injection time and pressure of the air ejected from each device.
[0059] In the manufacturing method of the present invention, it is important to cool the surface temperature of the center of the base sole of the rail after hot rolling so as to satisfy a predetermined average cooling rate, and as long as this condition is satisfied, the cooling method for other parts of the rail (e.g., the rail head, etc.) is not particularly limited. For example, accelerated cooling may be applied to the base part of the rail, and other parts of the rail (e.g., the rail head, etc.) may be allowed to cool naturally, or may be subjected to accelerated cooling in the same manner as the base part.
[0060] (4) Others After cooling, the rail material may be subjected to known treatments, for example, cold roller straightening.
[0061] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the examples, and appropriate modifications can be made within the scope of the spirit of the present invention, and all of these modifications are included in the technical scope of the present invention.
[0062] Steel stock with the chemical composition shown in Table 1 was heated and hot-rolled under the conditions shown in Table 2. After hot rolling, accelerated cooling was performed to produce 60 kg rails conforming to JIS E1101. The rails were allowed to cool naturally after cooling was stopped. The rolling finish temperature in Table 2 refers to the surface temperature at the center of the rail foot sole at the entry side of the final rolling mill, measured with a radiation thermometer. The cooling stop temperature T in Table 2 refers to the surface temperature at the center of the rail foot sole at the time of cooling stop during secondary cooling, measured with a radiation thermometer. The average cooling rate (°C / sec) was calculated by converting the temperature change from the start of cooling to the end of cooling for primary cooling (from 850°C to 750°C) and secondary cooling (from 750°C to cooling stop temperature T) per unit time (seconds). Finish rolling in the hot rolling process was performed with a thickness reduction rate of 15% at the center of the base. Under these conditions, the thickness reduction rate was greater than the 11% reduction rate during finish rolling. The accelerated cooling was performed by air injection using an air injection device.
[0063]
[0064]
[0065] The rails obtained were pearlitic rails. Each rail was evaluated for prior austenite grain size (GS), pearlite block size (BS), and fatigue crack propagation resistance. The test results are shown in Table 2. Each evaluation item is explained in detail below.
[0066] <Rail Microstructure> The microstructure and area ratio of the central sole were measured as follows. Test specimens for microstructure observation were taken from the central part of the rail sole, shown in Figure 2, at a depth of 1 mm from the surface. They were embedded in resin and mirror-polished. After that, a plane perpendicular to the rolling direction at a depth of 1 mm from the surface was observed at 200x magnification using an optical microscope in 10 fields (each field being 300 μm × 400 μm). The area ratio of the constituent phases was determined for each field, and the average value was taken as the area ratio of the microstructure.
[0067] <Prior Austenite Grain Size GS> The prior austenite grain size GS in the center of the sole was measured as follows. A test piece for microstructural observation was taken from the center of the rail sole, 1 mm deep from the surface, as shown in Figure 2. It was embedded in resin, mirror-polished, and then niter-etched to reveal the pro-eutectoid cementite precipitated at the prior austenite grain boundaries. A surface perpendicular to the rolling direction at a depth of 1 mm from the surface was observed at 200x magnification using a scanning electron microscope. The grain size in the region surrounded by pro-eutectoid cementite was measured by tracing using image analysis software. More than 400 regions were measured, and the average value was taken as the prior austenite grain size GS.
[0068] <Pearlite Block Size BS> The pearlite block size BS at the center of the sole was measured as follows. A test specimen for microstructure observation was taken from a depth of 1 mm from the surface of the center of the rail sole, as shown in Figure 2. After embedding the specimen in resin and mirror polishing, orientation analysis was performed using electron backscatter diffraction (EBSD). The grain boundaries where the misorientation between adjacent crystal orientations was 15° or more were defined as pearlite block boundaries. The average value of the grain diameters measured on a circle was used to determine the pearlite block size BS. The measurement area was 300 μm square, with measurement intervals of 0.3 μm. Measurement points with a Confidex index of 0.1 or less, which indicates the reliability of the measurement orientation, were excluded from the measurement. Furthermore, crystal grains that overlapped the edges of the measurement area were also excluded from the measurement.
[0069] <Fatigue crack propagation resistance> Fatigue crack propagation test specimens were taken from a position 1 mm deep from the surface of the center of the rail sole as shown in Figure 4, and fatigue crack propagation tests were conducted. Figure 5 is a schematic diagram showing an example of a test specimen, with Figure 5(a) showing a front view, Figure 5(b) showing a side view, and Figure 5(c) showing an enlarged front view of the notch. The test specimen was a plate-like specimen with a width W = 20 mm, height H = 100 mm, and thickness B = 5 mm as shown in Figure 5. A notch was formed at one width end of the central H / 2 portion of the height H. The notch was formed on the center side of the rail sole. The notch had a length L = 2 mm, a width C = 0.2 mm, and a curvature R = 0.1 mm at the end of the notch. The stress ratio (R ratio = minimum stress / maximum stress) was set to 0.2, and the stress intensity factor range ΔK = 20 MPa m 1/2 The fatigue crack propagation rate da / dN (m / cycle) was measured and the fatigue crack propagation resistance was evaluated. -8 If the test piece had a fatigue crack propagation inhibiting effect, it was determined that the test piece had a fatigue crack propagation inhibiting effect.
[0070] As shown in Table 2, the fatigue crack propagation rates of the test results (Test Nos. 1 to 40 in Table 2) for the rail materials of the invention were all 7.0 × 10 -8 On the other hand, in the comparative examples (Test Nos. 41 to 48 and 50 to 54 in Table 2) in which the component composition of the rail material did not satisfy the conditions of the present invention, the pearlite area ratio did not satisfy the conditions of the present invention, or the condition of formula (2) was not satisfied, the fatigue crack propagation rate da / dN (m / cycle) was 7.0 × 10 -8 In Test No. 49, the heating temperature was too high, causing part of the steel material to melt during heating. As a result, it was not possible to roll the material due to concerns about breakage during rolling, and the material was not even evaluated for properties.
[0071] According to the present invention, it is possible to provide a rail with excellent fatigue crack propagation resistance in the rail base portion, together with a manufacturing method thereof. The rail of the present invention contributes to extending the service life of rails for high axle load railways and preventing railway accidents, and is industrially useful. Furthermore, the rail manufacturing method of the present invention is industrially useful because it can stably improve the fatigue crack propagation resistance in the rail base portion by optimizing the heat treatment conditions after hot rolling.
[0072] 1 Rail 11 Rail head (head) 12 Rail body (body) 13 Rail foot (foot) 14 Rail sole (sole)
Claims
1. A rail containing 0.70-1.20% by mass of C, 0.10-1.20% by mass of Si, 0.10-1.50% by mass of Mn, 0.035% by mass or less of P, 0.020% by mass or less of S, and 0.05-2.00% by mass of Cr, with the balance being Fe and unavoidable impurities, the area ratio of pearlite structures at a depth of 1 mm from the surface of the central part of the rail sole is 95.0% or more, and the value of HC expressed by the following formula (1) satisfies the following formula (2): HC={(12×[%C])+([%Si] / 10)+([%Mn] / 20)+([%Cr] / 18)} 2 ... (1) HC≦(120×GS) / (1.1×BS) ... (2) Where, [%C], [%Si], [%Mn] and [%Cr] are the contents (mass%) of C, Si, Mn and Cr, respectively, GS is the prior austenite grain size (μm) at the center of the sole of the rail, and BS is the pearlite block size (μm) at the center of the sole of the rail.
2. A rail according to claim 1, wherein the chemical composition further contains at least one selected from the group consisting of V: 0.30 mass% or less, Cu: 1.0 mass% or less, Ni: 1.0 mass% or less, Nb: 0.05 mass% or less, Mo: 2.0 mass% or less, Al: 0.07 mass% or less, W: 1.0 mass% or less, Co: 1.0 mass% or less, B: 0.005 mass% or less, Ti: 0.05 mass% or less, Sb: 0.05 mass% or less, Mg: 0.01 mass% or less, Ca: 0.02 mass% or less, and Sn: 0.05 mass% or less.
3. A method for manufacturing a rail as claimed in claim 1 or 2, comprising the steps of heating a steel material having the chemical composition as claimed in claim 1 or 2 at a heating temperature of 1350°C or less, hot rolling the steel material under conditions in which the finishing temperature at the center of the base sole of the rail is 850°C or more, cooling the steel material at the center of the base sole of the rail from 850°C at an average cooling rate CR1 (°C / sec) until the temperature at the center of the base sole of the rail reaches 750°C, and then cooling the steel material at an average cooling rate CR2 (°C / sec) from 750°C until the temperature at the center of the base sole of the rail reaches a cooling stop temperature T, wherein the cooling stop temperature T is in the range of 400 to 650°C, and the average cooling rates CR1 (°C / sec) and CR2 (°C / sec) satisfy the following formulas (3) and (4), respectively: HC / 300≦CR1≦3.0 ... (3) HC / 120≦CR2≦6.0 ... (4)
Citation Information
Patent Citations
Heat treatment for steel rail excellent in falling load-resisting characteristic
JP1989139724A
Pearlitic rail having excellent drop fracture resistance
JP2006057127A
Pearlite rail
WO2011021582A1
Rail
WO2013187470A1
rail
WO2016117692A1