Sheet for wafer processing and method for processing wafer
A multilayer wafer processing sheet with controlled storage modulus and melting points addresses the issue of followability and residue in conventional sheets, providing improved protection and adhesion during wafer processing, enhancing processing precision and yield.
Patent Information
- Application Number
- PCT/JP2024/006410
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-02-22
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional wafer processing sheets fail to adequately follow the uneven surface of wafers, leading to insufficient adhesion, residue issues, and damage during processes like backgrinding, due to insufficient followability and lack of direct protection for protrusions.
A multilayer wafer processing sheet with a first layer for releasability, an intermediate layer for followability, and a second layer for mechanical strength, where the storage modulus ratio and melting points are controlled within specific ranges to ensure excellent followability and peelability, preventing residue formation.
The multilayer structure effectively follows and protects the wafer surface during processing, reducing residue and damage, while maintaining mechanical strength and precision, thereby enhancing the yield and quality of processed chips.
Smart Images

Figure JP2024006410_03102024_PF_FP_ABST
Abstract
Description
Wafer processing sheet and wafer processing method
[0001] The present invention relates to a wafer processing sheet and a wafer processing method.
[0002] When processing a wafer, a sheet is attached to protect the wafer from damage caused by the processing. For example, in the back-grinding process, which is performed to thin a wafer with bumps or the like formed on its surface, a sheet is attached to the surface on which the bumps or the like are formed to protect the surface. Also, in the dicing process, which cuts semiconductor chips from the wafer, dicing is performed with the sheet attached to the wafer.
[0003] Such sheets are required to be able to conform to the irregularities of the wafer surface. Conventionally, the conformability of sheets has been improved by increasing the thickness of the adhesive or by providing a soft, cushioning resin layer between the base film and the adhesive. However, when the wafer surface is significantly uneven, there are problems such as insufficient conformability, or the adhesive layer penetrating deep into the recesses on the wafer surface, resulting in adhesive residue, reduced yield, and malfunction of the processed chips.
[0004] As a method for solving such problems, Patent Document 1 discloses a technology in which a sheet is configured so that one side of a base sheet has a non-adhesive portion with a diameter smaller than the outer diameter of the semiconductor wafer to be attached and an adhesive portion surrounding the non-adhesive portion, and the adhesive strength of the adhesive portion at 23°C is set to 500 mN or more, thereby preventing adhesive residue and a decrease in protective performance.
[0005] JP 2013-211438 A
[0006] However, the technology described in Patent Document 1 simply provides an adhesive portion that adheres to the edge of the semiconductor wafer, and is not configured to directly protect bumps, etc. in the non-adhesive portion. Therefore, for example, in a backgrinding process, if protruding electrodes are provided on the semiconductor wafer, the backside of the semiconductor wafer is ground with only the tips of the protruding electrodes in contact with the base sheet, and therefore, excessive load is applied to the protruding electrodes during backgrinding, which may cause the protruding electrodes to be damaged.
[0007] Furthermore, the technology described in Patent Document 1 simply provides an adhesive portion that adheres to the edge of a semiconductor wafer, and does not disclose anything about, for example, how the adhesive portion that comes into contact with the unevenness of the wafer surface can be easily peeled off without leaving any adhesive residue.
[0008] The present invention has been made in consideration of the above-mentioned problems, and aims to provide a wafer processing sheet that has excellent conformability and releasability to the wafer surface and leaves little residue when peeled from the wafer surface, and a wafer processing method using the wafer processing sheet.
[0009] The present inventors have conducted extensive research to solve the above-mentioned problems, and as a result have found that the above-mentioned problems can be solved by using a multilayer structure as a layer that conforms to and protects irregularities formed on the wafer main surface, and by setting the storage modulus of the multilayer structure within a predetermined range, thereby completing the present invention.
[0010] That is, the present invention is as follows. [1] A wafer processing sheet comprising a first layer having a surface in contact with the wafer main surface, a second layer having a back surface opposite to the first surface, and an intermediate layer located between the first and second layers, wherein the ratio G'(140°C) / G'(110°C) of the storage modulus G'(140°C) at 140°C to the storage modulus G'(110°C) at 110°C is 0.001 to 0.100, the melting point Tm1 of the first layer is 120 to 140°C, and the melting point Tm2 of the second layer is 133 to 155°C. [2] The wafer processing sheet according to [1], wherein the intermediate layer is laminated on the surface of the first layer opposite to the first surface. [3] The wafer processing sheet according to [1] or [2], wherein the melting point Tm1 is lower than the melting point Tm2. [4] The wafer processing sheet according to any one of [1] to [3], wherein the thickness T1 of the first layer is 1 to 20 μm. [5] The wafer processing sheet according to any one of [1] to [4], wherein the thickness T3 of the intermediate layer is 30 to 300 μm. [6] The wafer processing sheet according to any one of [1] to [5], wherein the thickness T2 of the second layer is 10 to 100 μm. [7] The wafer processing sheet according to any one of [1] to [6], wherein the first layer contains a polyolefin. [8] The wafer processing sheet according to any one of [1] to [7], wherein the intermediate layer contains a polyolefin. [9] The wafer processing sheet according to any one of [1] to [8], wherein the second layer contains a polyolefin.
[10] The wafer processing sheet according to any one of [1] to [9], wherein the ratio G'(110°C) / G'(50°C) of the storage modulus G'(110°C) at 110°C to the storage modulus G'(50°C) at 50°C is 0.001 to 0.700.
[11] A wafer processing method comprising: a laminating step of laminating a surface of a first layer of the heated wafer processing sheet according to any one of [1] to
[10] to a main surface of a wafer; and a processing step of processing the wafer with the wafer processing sheet and the wafer laminated together.
[12] The wafer processing method according to
[11] , wherein in the processing step, a main surface of the wafer to which the wafer processing sheet is not attached is ground to obtain a thinned wafer.
[13] The wafer processing method according to
[11] or
[12] , wherein in the processing step, a semiconductor chip is obtained.
[0011] According to the present invention, it is possible to provide a wafer processing sheet that has excellent conformability and releasability to the wafer surface and leaves little residue when peeled off from the wafer surface, and a wafer processing method using the wafer processing sheet.
[0012] 1 is a cross-sectional view showing an example of back-grinding of a wafer using the wafer processing sheet of the present embodiment. 2 is a graph showing the results of dynamic viscoelasticity measurement in Example 2.
[0013] An embodiment of the present invention (hereinafter referred to as "the present embodiment") will be described in detail below, but the present invention is not limited to this embodiment and various modifications are possible without departing from the spirit of the present invention. In the drawings, the same elements are given the same reference numerals and redundant explanations will be omitted. Furthermore, positional relationships such as up, down, left, and right are based on the positional relationships shown in the drawings unless otherwise specified. Furthermore, the dimensional ratios of the drawings are not limited to those shown in the drawings.
[0014] 1. Wafer Processing Sheet The wafer processing sheet of this embodiment has a first layer having a surface that contacts the main surface of the wafer, a second layer having a back surface opposite to the first surface, and an intermediate layer located between the first and second layers, and the ratio G'(140°C) / G'(110°C) of the storage modulus G'(140°C) at 140°C to the storage modulus G'(110°C) at 110°C is 0.001 to 0.100, the melting point Tm1 of the first layer is 120 to 140°C, and the melting point Tm2 of the second layer is 133 to 155°C.
[0015] First, a brief description of how the wafer processing sheet of this embodiment is used will be given. Fig. 1 shows a cross-sectional view illustrating an example of wafer backgrinding using the wafer processing sheet of this embodiment. In Fig. 1, the wafer processing sheet 10 includes a first layer 11 having a surface 10a that contacts the wafer's main surface 20a, an intermediate layer 12, and a second layer 13 having a back surface 10b opposite the surface 10a. Here, the first layer 11 may ensure peelability, the intermediate layer 12 may provide conformability as a buffer layer, and the second layer 13 may provide mechanical strength as a base layer.
[0016] The wafer 20 has a convex portion 20b on the wafer main surface 20a. The convex portion 20b may be a structure derived from a circuit or the like in a semiconductor wafer. The wafer processing sheet 10 of this embodiment is used by attaching the surface 10a of the first layer 11 to the wafer main surface 20a in a processing process of the wafer 20, such as a back-grinding process or a dicing process.
[0017] More specifically, before the processing process, the wafer processing sheet 10 is heated with the wafer main surface 20a and the surface 10a of the first layer 11 in contact with each other (Step A). When heated, the elastic modulus of the wafer processing sheet 10 decreases, and the wafer processing sheet 10 is bonded to the wafer main surface 20a so as to conform to the convex portions 20b formed on the wafer main surface 20a (Step B).
[0018] The wafer processing sheet 10 is then cooled, and back-grinding of the back surface 20c of the wafer 20 is performed (step C). Finally, the wafer processing sheet 10 is peeled off from the wafer main surface 20a (step D). The specific method of back-grinding is not particularly limited, and known methods can be used. For example, a method of grinding the back surface 20c of the wafer 20 while supplying a slurry containing abrasive grains to the wafer 20 to thin the wafer 20 is exemplified. When the wafer processing sheet 10 is cooled before back-grinding, the elastic modulus recovers while conforming to the wafer main surface 20a, preventing misalignment between the wafer main surface 20a and the surface 10a of the first layer 11, protecting the wafer main surface 20a.
[0019] In this case, when a wafer having a complex shape, such as deep recesses and protrusions, is used, the wafer processing sheet 10 may not be able to sufficiently follow the gaps formed by the recesses and protrusions (Step B). If the wafer processing step (Step C) is performed with such insufficient following, the liquid used in wafer grinding will seep into the gaps due to the insufficient following, contaminating the wafer.
[0020] On the other hand, if the wafer processing sheet 10 is made to be more easily softened by heating in order to improve conformability, it will be easier for the wafer processing sheet 10 to penetrate into the complex shapes of the wafer, such as deep irregularities. However, the wafer processing sheet 10 will break when peeled off from the wafer after the wafer processing step (step D), and the broken wafer processing sheet 10 will remain as residue on the wafer, contaminating the wafer.
[0021] In contrast, in this embodiment, the wafer processing sheet has, in this order, a first layer that is less likely to produce residue and has excellent peelability, an intermediate layer that has excellent conformability, and a second layer that has excellent mechanical strength as a film. That is, the wafer processing sheet of this embodiment has a multilayer structure having a layer that is less likely to produce residue and has excellent peelability, and a layer that has excellent conformability. This provides excellent conformability and peelability to the wafer surface, and also reduces residue when peeled from the wafer surface. Below, each component of the wafer processing sheet of this embodiment will be described in detail.
[0022] 1.1. First Layer The first layer has a surface that contacts the wafer's main surface and constitutes the outermost surface of the wafer processing sheet of this embodiment that contacts the wafer's main surface. The melting point Tm1 of the first layer is 120 to 140°C, preferably 122.5 to 137.5°C, 125 to 135°C, or 127.5 to 132.5°C. Having a melting point Tm1 of the first layer of 120°C or higher tends to improve peelability and reduce the likelihood of residue. Furthermore, having a melting point Tm1 of the first layer of 140°C or lower tends to improve conformability.
[0023] The melting point Tm1 is preferably lower than the melting point Tm2, which will be described later. This improves the conformability of the first layer and prevents the second layer from deforming when the wafer processing sheet 10 is heated and bonded together, which tends to improve the accuracy of wafer processing.
[0024] The melting point T1 can be controlled by adjusting the type of resin used in the first layer and the type and ratio of comonomers in the copolymer. In this embodiment, the melting point of each layer can be measured in accordance with JIS K7121.
[0025] The thickness T1 of the first layer is preferably 1 to 20 μm, 2 to 20 μm, 3 to 20 μm, 4 to 15 μm, 4 to 10 μm, or 5 to 7.5 μm. When the thickness T1 of the first layer is 1 μm or more, even when the first layer is stretched to conform to the surface that contacts the wafer main surface, the peelability is improved and residue tends to be less likely to be generated. When the thickness T1 of the first layer is 20 μm or less, the conformability tends to be improved.
[0026] The material constituting the first layer is not particularly limited, but examples thereof include polyolefin, ethylene-vinyl acetate copolymer, polyacrylic resin, and polyester resin. Among these, it is preferable that the first layer contains polyolefin. By containing polyolefin, conformability and peelability are further improved, and residue tends to be further suppressed. The resin may be used alone or in combination of two or more types.
[0027] The polyolefin is not particularly limited, but examples thereof include a homopolymer of ethylene or propylene, or a copolymer formed from at least two monomers selected from the group consisting of ethylene, propylene, 1-butene, 4-methyl-1-pentene, 1-hexene, and 1-octene.
[0028] Among these, polypropylene-based resins are preferred. The polypropylene-based resins are not particularly limited as long as they are polymers composed mainly of propylene, and examples thereof include polypropylene homopolymers and copolymers of propylene with monomers having unsaturated double bonds, such as ethylene, 1-butene, 4-methyl-1-pentene, 1-hexene, and 1-octene.
[0029] Here, "composed mainly of propylene" means that the molar ratio of propylene is 50 mol% or more relative to all structural units of the polypropylene-based resin. In the first layer, the molar ratio of propylene in the polypropylene-based resin is preferably 60 mol% or more, 70 mol% or more, 80 mol% or more, or 90 mol% or more relative to the total amount of polypropylene-based resin. Furthermore, the molar ratio of propylene is preferably 99 mol% or less, 98 mol% or less, or 97 mol% or less relative to the total amount of polypropylene-based resin.
[0030] The polyolefin resin may also contain a flexible polypropylene resin. The flexible polypropylene resin is not particularly limited, but examples thereof include a polypropylene resin blended with a rubber component. The rubber component used here is not particularly limited, but examples thereof include styrene-butadiene copolymer rubber, styrene-butadiene-styrene block copolymer rubber, styrene-isoprene-styrene block copolymer rubber, and ethylene-propylene copolymer rubber.
[0031] The weight average molecular weight (Mw) of the resin contained in the first layer is preferably 5.0×10 4 ~3.5 x 10 5 is 1.0 × 10 5 ~3.0 x 10 5 is 1.5 × 10 5 ~2.5 x 10 5 In this embodiment, the weight average molecular weight (Mw) can be measured by gel permeation gel chromatography according to a known method.
[0032] The first layer may contain additives as needed, including, but not limited to, known plasticizers, heat stabilizers, colorants, organic lubricants, inorganic lubricants, surfactants, and processing aids.
[0033] 1.2. Second Layer The second layer has a back surface opposite the front surface and constitutes the outermost surface of the wafer processing sheet of this embodiment, which does not contact the wafer's main surface. The melting point Tm2 of the second layer is 133 to 155°C, preferably 135 to 152.5°C, 137.5 to 150°C, 137.5 to 147.5°C, or 137.5 to 145°C. Having a melting point Tm2 of the second layer of 133°C or higher tends to improve mechanical strength and tear resistance. Furthermore, deformation of the second layer can be suppressed when the wafer processing sheet 10 is heated and bonded, which tends to improve wafer processing accuracy. Furthermore, having a melting point Tm2 of the first layer of 155°C or lower tends to improve conformability.
[0034] The melting point T2 of the second layer can be controlled by adjusting the type of resin used in the second layer and the type and ratio of comonomers in the copolymer.
[0035] The thickness T2 of the second layer is preferably 10 to 100 μm, 12.5 to 90 μm, 15 to 80 μm, 17.5 to 70 μm, 20 to 60 μm, 22.5 to 50 μm, or 25 to 40 μm. Having a thickness T2 of 10 μm or more for the second layer tends to improve mechanical strength and tear resistance. Furthermore, deformation of the second layer can be suppressed when the wafer processing sheet 10 is heated and bonded, which tends to improve wafer processing accuracy. Furthermore, having a thickness T2 of 100 μm or less for the second layer tends to improve conformability.
[0036] The material constituting the second layer is not particularly limited, but examples thereof include polyolefin, ethylene-vinyl acetate copolymer, polyacrylic resin, and polyester resin. Among these, the second layer preferably contains polyolefin, and more preferably polypropylene resin. By containing polyolefin, the conformability and peelability are further improved, and residue tends to be further suppressed. Examples of polyolefin include the same polyolefins as those exemplified for the first layer. The resin may be used alone or in combination of two or more types.
[0037] Examples of the monomer constituting the polyolefin or polypropylene-based resin include the same monomers as those exemplified for the first layer.
[0038] In the second layer, the molar ratio of propylene in the polypropylene-based resin, relative to the total amount of the polypropylene-based resin, is preferably 60 mol% or more, 70 mol% or more, 80 mol% or more, or 90 mol% or more, and is preferably 99 mol% or less, 98 mol% or less, or 97 mol% or less.
[0039] When both the first layer and the second layer use polypropylene-based resins, the molar ratio of propylene in the polypropylene-based resin of the first layer may be greater than the molar ratio of propylene in the polypropylene-based resin of the second layer.
[0040] 1.3 Intermediate Layer The intermediate layer is located between the first layer and the second layer. The intermediate layer may be directly laminated on the surface opposite to the surface of the first layer, or may be indirectly laminated via another layer. Among these, it is preferable that the intermediate layer be directly laminated on the surface opposite to the surface of the first layer.
[0041] The thickness T3 of the intermediate layer is preferably 30 to 300 μm, 40 to 290 μm, 50 to 280 μm, 60 to 270 μm, 70 to 260 μm, 80 to 250 μm, 90 to 260 μm, 100 to 250 μm, 110 to 240 μm, 120 to 230 μm, or 130 to 220 μm. When the thickness T3 of the intermediate layer is 30 μm or more, the followability tends to be further improved. When the thickness T3 of the intermediate layer is 300 μm or less, the releasability tends to be further improved.
[0042] The total thickness of the wafer processing sheet is preferably 50 to 500 μm, 70 to 400 μm, or 100 to 300 μm. When the total thickness of the wafer processing sheet is within the above range, sufficient conformability to the irregularities on the wafer surface is exhibited, and the strength of the sheet is maintained, so that the sheet is less likely to break when peeled off, and peelability also tends to be improved.
[0043] The material constituting the intermediate layer is not particularly limited, but examples thereof include polyolefin, ethylene-vinyl acetate copolymer, polyacrylic resin, and polyester resin. Among these, it is preferable that the intermediate layer contains polyolefin. By containing polyolefin, the conformability and peelability are further improved, and residue tends to be further suppressed and improved. Examples of polyolefin include the same polyolefins as those exemplified for the first layer.
[0044] The polyolefin is not particularly limited, but examples thereof include a homopolymer of ethylene or propylene, or a copolymer formed from at least two monomers selected from the group consisting of ethylene, propylene, 1-butene, 4-methyl-1-pentene, 1-hexene, and 1-octene.
[0045] Among these, polypropylene-based resins are preferred. The polypropylene-based resins are not particularly limited as long as they are polymers composed mainly of propylene, and examples thereof include polypropylene homopolymers and copolymers of propylene with monomers having unsaturated double bonds, such as ethylene, 1-butene, 4-methyl-1-pentene, 1-hexene, and 1-octene.
[0046] In the intermediate layer, the molar ratio of propylene in the polypropylene resin is preferably 60 mol% or more, 70 mol% or more, or 80 mol% or more, relative to the total amount of the polypropylene resin, and is preferably 99 mol% or less, 98 mol% or less, or 97 mol% or less, relative to the total amount of the polypropylene resin.
[0047] The intermediate layer is mainly composed of a resin, and may contain additives as necessary. The resin may be used alone or in combination of two or more kinds.
[0048] 1.4 Storage Elastic Modulus G' In order to properly protect the wafer main surface 20a during the above-described processing of the wafer 20, the wafer processing sheet 10 is required to conform to the wafer main surface 20a. Therefore, in this embodiment, the decrease in the storage elastic modulus G' (elastic component) during heating and bonding is specified.
[0049] The storage modulus G'(110°C) at 110°C is preferably 2.50 x 10 5 ~2.00 x 10 7 is 5.00 × 10 5 ~1.50 x 10 7 is 7.50 × 10 5 ~1.00 x 10 7 is 1.00 × 10 6 ~7.50 x 10 6 is 2.50 × 10 6 ~5.00 x 10 6 When the storage modulus G' (110°C) is within the above range, the conformability tends to be further improved.
[0050] The storage modulus G'(140°C) at 140°C is preferably 2.50 x 10 3 ~7.50 x 10 5 is 5.00 × 10 3 ~5.00 x 10 5 is 7.50 × 10 3 ~2.50 x 10 5 is 2.00 × 10 4 ~1.00 x 10 5 is 3.50 × 10 4 ~7.50 x 10 4 When the storage modulus G' (140°C) is within the above range, the conformability tends to be further improved.
[0051] The storage modulus G'(50°C) at 50°C is preferably 7.50 x 10 6 ~2.50 x 10 9 is 1.00 × 10 7 ~1.00 x 10 9 is 2.50 × 10 7 ~7.50 x 10 8 is 5.00 × 10 7 ~5.00 x 10 8 is 7.50 × 10 7 ~2.50 x 10 8 When the storage modulus G' (50°C) is within the above range, the conformability tends to be further improved.
[0052] The ratio G'(140°C) / G'(110°C) of the storage modulus G'(140°C) to the storage modulus G'(110°C) is preferably 0.001 to 0.100, 0.003 to 0.075, 0.005 to 0.050, or 0.007 to 0.025. When the ratio G'(140°C) / G'(110°C) is 0.001 or more, conformability tends to be further improved. When the ratio G'(140°C) / G'(110°C) is 0.100 or less, releasability is further improved and residue is further suppressed.
[0053] The ratio G'(110°C) / G'(50°C) of the storage modulus G'(110°C) to the storage modulus G'(50°C) is preferably 0.001 to 0.700, 0.003 to 0.650, 0.005 to 0.550, 0.010 to 0.500, 0.015 to 0.450, or 0.020 to 0.400. When the ratio G'(110°C) / G'(50°C) is 0.001 or more, conformability tends to be further improved. When the ratio G'(110°C) / G'(50°C) is 0.700 or less, releasability is further improved and residue is further suppressed.
[0054] The dynamic viscoelasticity of the wafer processing sheet of this embodiment can be measured according to a conventional method. For example, a sample can be stored in a thermo-hygrostat at a temperature of 23°C (±2°C) and a relative humidity of 50% (±5%). For example, a known device such as the "Rheomeric Series RSA III" (manufactured by TA Instruments) can be used. Other conditions are not particularly limited, but measurements can be performed under the conditions described in the examples.
[0055] 1.5. Other Layers The wafer processing sheet 10 of this embodiment may have other layers, as needed, between the first layer and the intermediate layer, between the intermediate layer and the second layer, on the surface side of the second layer, etc. Examples of other layers include, but are not limited to, an adhesive layer between the first layer and the intermediate layer, an adhesive layer between the intermediate layer and the second layer, and an adhesive layer on the surface of the second layer. The adhesive layer is provided to improve adhesion between layers. The adhesive layer is also used to secure the wafer processing sheet 10 to the stage of a wafer processing device.
[0056] Like the adhesive layer, the wafer processing sheet 10 of this embodiment may optionally include other layers depending on the type of processing. For example, an interference layer may be included in addition to the adhesive layer. The other layer may be a single layer or a laminate of layers having the same or different functions.
[0057] In addition, from the viewpoint of improving the peelability of the wafer processing sheet 10 to the wafer main surface 20a and suppressing residues, it is preferable that the wafer processing sheet 10 of this embodiment does not have an adhesive layer or the like on the surface 10a (surface of the first layer 11) that comes into contact with the surface on which the convex portion 20b of the wafer main surface 20a is formed.
[0058] 2. Wafer Processing Method The wafer processing method of this embodiment includes a lamination step of laminating the heated surface of the first layer of the wafer processing sheet to the main surface of the wafer, and a processing step of processing the wafer in a state where the wafer processing sheet and the wafer are laminated together. Each step will be described below with reference to FIG.
[0059] In the lamination step, the heated surface 10 a of the first layer 11 of the wafer processing sheet 10 is bonded to the wafer main surface 20 a. In the lamination step, the wafer processing sheet 10 may be bonded to the wafer main surface 20 a in a preheated state, or the wafer processing sheet 10 may be bonded to the wafer main surface 20 a and then heated.
[0060] By bonding the surface 10 a of the first layer 11 to the main surface 20 a of the wafer in a heated state, the surface 10 a can be bonded in a state where it conforms to the main surface 20 a of the wafer (see B in FIG. 1). In this way, the convex portions 20 b are sunk into the wafer processing sheet 10, so that the main surface 20 a of the wafer having the convex portions 20 b can be protected.
[0061] The heating temperature is preferably 60 to 150°C, more preferably 70 to 140°C, and even more preferably 80 to 130°C. The heating time of the wafer processing sheet 10 is preferably 3 to 120 seconds, more preferably 5 to 90 seconds. By keeping the heating conditions within the above range, the conformability of the wafer processing sheet 10 tends to be further improved.
[0062] 2.2 Processing Process The processing process for processing the wafer 20 in a state in which the wafer processing sheet 10 and the wafer 20 are bonded together is not particularly limited, and any wafer processing process can be applied as appropriate. For example, processing processes include back-grinding, in which the back surface 20c of the wafer to which the wafer processing sheet 10 is not bonded is ground to obtain a thinned wafer 21, and dicing, in which the wafer 20 is diced to obtain semiconductor chips. Among these, the wafer processing method of this embodiment is suitable for back-grinding.
[0063] The specific method of back-grinding is not particularly limited, and any known method can be used. For example, a method of grinding while supplying a slurry containing abrasive grains to the back surface 20c of the wafer can be used. The thickness of the thinned wafer 21 obtained by this method is not particularly limited as long as it is a thickness suitable for the processing purpose, but as an example, it is preferably 300 μm or less, more preferably 150 μm or less, and even more preferably 50 μm or less.
[0064] In back-grinding, a load is applied in the thickness direction of the wafer, which can easily damage the protrusions 20b and reduce yield. In contrast, by using the wafer processing sheet of this embodiment, processing can be performed with at least a portion of the protrusions 20b embedded in the wafer processing sheet 10, thereby preventing damage to the protrusions 20b and the like.
[0065] In the wafer processing method of this embodiment, when a back-grinding process is performed on a wafer having grooves formed on its front surface for thinning the wafer from its rear surface, the wafer may be thinned to approximately the same depth as the grooves, thereby allowing thinning by back-grinding and singulation to be performed simultaneously.
[0066] 2.3 Peeling Step The wafer processing method of this embodiment may include a peeling step of peeling the thinned wafer 21 from the wafer processing sheet 10. The method for peeling the wafer processing sheet 10 is not particularly limited, but for example, as shown in FIG. 1 , the wafer processing sheet 10 may be bent in direction F so that one end of the wafer processing sheet 10 moves away from the thinned wafer 21.
[0067] Alternatively, when the individual semiconductor chips are simultaneously separated by back-grinding as described above, the individual semiconductor chips may be picked up from the wafer processing sheet 10 .
[0068] The peeling step may be carried out at room temperature or under heating. The temperature at which the peeling step is carried out is preferably 10 to 70°C, more preferably 20 to 60°C.
[0069] When using a conventional wafer processing sheet with an adhesive layer, there is a problem of adhesive residue remaining on the main surface 20a of the wafer 20. However, the wafer processing sheet of this embodiment has predetermined viscoelastic properties, making it possible to peel it off without leaving any adhesive residue.
[0070] As mentioned above, the present invention is not limited to the above-described embodiment, and various modifications are possible within the scope of the gist of the present invention. In other words, the above-described embodiment is merely an example in all respects and should not be interpreted as being restrictive.
[0071] For example, the lamination process may be performed under reduced pressure in addition to atmospheric pressure. Furthermore, a curable resin may be used instead of or in addition to other layers. When using a curable resin, for example, the curable resin is supplied onto the film, and pressure is applied to the surface opposite the surface 10a of the wafer processing sheet 10 opposite the wafer main surface 20a, so as to spread the curable resin. Then, by curing the curable resin, the wafer processing sheet 10 can be fixed onto the film.
[0072] Furthermore, although FIG. 1 mainly shows an example of back grinding, the wafer processing sheet of this embodiment can also be used in dicing and other wafer processing processes.
[0073] The present invention will be described in more detail below using examples and comparative examples, but the present invention is not limited to the following examples.
[0074] 1. Method for Producing Wafer Processing Sheet 1.1. Example 1 A wafer processing sheet was produced by coextrusion using a propylene-ethylene copolymer (molar ratio: propylene / ethylene = 95 / 5 mol%) for the first layer, a propylene-ethylene copolymer (molar ratio: propylene / ethylene = 94 / 6 mol%) for the second layer, and a propylene-butene copolymer for the intermediate layer, with the first layer being 5 μm thick, the intermediate layer being 500 μm thick, and the second layer being 25 μm thick.
[0075] 1.2. Example 2 A wafer processing sheet was produced by coextrusion in the same manner as in Example 1, except that a propylene-butene-ethylene terpolymer was used for the first and second layers, and a propylene-butene copolymer was used for the intermediate layer.
[0076] 1.3. Examples 3 to 7 and Comparative Examples 1 to 6 Wafer processing sheets were produced in the same manner as in Examples 1 and 2, except that the copolymerization ratios were changed and resins having the melting points and storage moduli listed in Table 1 were used for the first layer, second layer, and intermediate layer.
[0077] 2. Measurement and Evaluation 2.1. Dynamic Viscoelasticity Measurement Dynamic viscoelasticity measurements were performed on the wafer processing sheet under the following conditions. First, the wafer processing sheet was held in a thermo-hygrostat chamber at a temperature of 23°C (±2°C) and a relative humidity of 50% (±5%) for 40 hours. Using the obtained wafer processing sheet as a sample, dynamic viscoelasticity measurements were performed under normal atmospheric conditions (dry conditions). A "Rheomeric Series RSA III" (manufactured by TA Instruments) was used as the dynamic viscoelasticity measuring device. The storage modulus G' of Example 2 and that of single-component polypropylene obtained by the measurement are compared in Figure 2. (Measurement conditions) Measuring device: Rheomeric Series III (manufactured by TA Instruments) Sample: 7 cm length x 0.5 cm width x 0.018 cm thickness Test length: 1 cm Pretreatment: Hold in an atmosphere at a temperature of 23°C and a relative humidity of 50% for 40 hours Test mode: Tension in a direction parallel to the surface of the wafer processing sheet Frequency: 1 Hz Temperature range: 30°C to 150°C Heating rate: 2°C / min Strain range: 0.10% Measurement interval: 1 Point / °C
[0078] 2.2. Melting Point The melting point of each layer of the wafer processing sheet was measured under the following conditions. First, the wafer processing sheet was kept in a thermo-hygrostat at a temperature of 23°C (±2°C) and a relative humidity of 50% (±5%) for 40 hours. A sample was obtained from the obtained wafer processing sheet using a surface and interface physical property analyzer (SAICAS), and differential scanning calorimetry (DSC) measurement was performed. The DSC measurement device used was a "Heat Flux DSC3400" (manufactured by Netsch). (Sample collection) Equipment: SAICAS NN-04-01 (manufactured by Daipla Wintes) Measurement mode: Low speed mode Horizontal speed: 100 nm / sec Vertical speed: 5 μm / sec Cutting edge: Diamond cutting edge, width 0.3 mm, 20° squeezing, 10° recession (Melting point measurement) Heating conditions: From room temperature to 250°C, heating rate 10°C / min Carrier gas: Nitrogen (40 ml / min) Container: Aluminum pan (with sheet lid) Reference: Empty pan Sample weight: 1 mg
[0079] 2.3. Conformability A wafer having a groove of 50 μm width and 400 μm depth on its surface was prepared. A wafer processing sheet was pressed against the surface of the wafer on which the groove was formed at 133°C for 1 minute to adhere it. The temperature was then lowered to room temperature (25°C). Conformability was evaluated based on the depth to which the wafer processing sheet conformed to the wafer groove. (Evaluation criteria) ◯: Conformability depth is 230 μm or more △: Conformability depth is 200 μm or more but less than 230 μm ×: Conformability depth is less than 200 μm
[0080] 2.4. Residue A wafer was prepared having multiple recesses formed in sections measuring 800 μm in length, 400 μm in width, and 140 μm in depth. A wafer processing sheet was pressed against the surface of the wafer with the recesses at 133°C for 1 minute and attached. The temperature was then lowered to room temperature (25°C), and the wafer processing sheet was peeled off. The sections were then observed to determine whether any residue from the wafer processing sheet remained. The residue occurrence rate was calculated using the following formula, and the residue was evaluated based on the residue occurrence rate. Residue occurrence rate = (number of sections where residue was found) / (total number of sections present on the wafer surface) (Evaluation criteria) ◯: Residue occurrence rate less than 1% △: Residue occurrence rate 1% or more but less than 5% ×: Residue occurrence rate 5% or more
[0081] 2.5. Peelability A wafer was prepared having multiple recesses formed in sections measuring 800 μm in length, 400 μm in width, and 140 μm in depth. A wafer processing sheet was pressed against the surface of the wafer with the recesses at 133°C for 1 minute and attached. The temperature was then lowered to room temperature (25°C), and the wafer processing sheet was peeled off. The wafer processing sheet was then observed to determine whether or not tears had occurred within the sections, and the tear rate was calculated using the following formula. Peelability was evaluated based on the tear rate. Break rate = (number of sections with tears) / (total number of sections on the wafer surface) (Evaluation criteria) ◯: Break rate was 0% △: Break rate was greater than 0% but not greater than 1% ×: Break rate was greater than 1%
[0082]
[0083] The wafer processing sheet of the present invention has industrial applicability as a protective sheet used in back-grinding, dicing, and other wafer processing processes.
[0084] 10... wafer processing sheet, 10a... front surface, 10b... back surface, 11... first layer, 12... intermediate layer, 13... second layer, 20... wafer, 20a... main surface, 20a... wafer main surface, 20b... convex portion, 20c... back surface, 21... thinned wafer
Claims
1. A wafer processing sheet comprising: a first layer having a surface in contact with a wafer main surface; a second layer having a back surface opposite to the first surface; and an intermediate layer located between the first layer and the second layer, wherein a ratio G'(140°C) / G'(110°C) of a storage modulus G'(140°C) at 140°C to a storage modulus G'(110°C) at 110°C is 0.001 to 0.100, a melting point Tm1 of the first layer is 120 to 140°C, and a melting point Tm2 of the second layer is 133 to 155°C.
2. The wafer processing sheet according to claim 1, wherein the intermediate layer is laminated on the surface opposite to the surface of the first layer.
3. The wafer processing sheet according to claim 1, wherein the melting point Tm1 is lower than the melting point Tm2.
4. The wafer processing sheet according to claim 1, wherein the thickness T1 of the first layer is 1 to 20 μm.
5. The wafer processing sheet according to claim 1, wherein the thickness T3 of the intermediate layer is 30 to 300 μm.
6. The wafer processing sheet according to claim 1, wherein the thickness T2 of the second layer is 10 to 100 μm.
7. The wafer processing sheet according to claim 1, wherein the first layer comprises a polyolefin.
8. The wafer processing sheet according to claim 1, wherein the intermediate layer comprises a polyolefin.
9. The wafer processing sheet according to claim 1, wherein the second layer comprises a polyolefin.
10. The wafer processing sheet according to claim 1, wherein the ratio G'(110°C) / G'(50°C) of the storage modulus G'(110°C) at 110°C to the storage modulus G'(50°C) at 50°C is 0.001 to 0.
700.
11. A method for processing a wafer, comprising: a lamination step of laminating a surface of a first layer of a heated wafer processing sheet according to any one of claims 1 to 10 to a main surface of a wafer; and a processing step of processing the wafer in a state in which the wafer processing sheet and the wafer are laminated together.
12. The wafer processing method according to claim 11, wherein in the processing step, the main surface of the wafer to which the wafer processing sheet is not attached is ground to obtain a thinned wafer.
13. The wafer processing method according to claim 11, wherein a semiconductor chip is obtained in the processing step.
Citation Information
Patent Citations
Methods of processing wafers and protective sheets for use in such methods
JP2018526826A
Back grinding adhesive tape
JP2022121480A
Adhesive sheet for rear surface grinding, semiconductor wafer manufacturing method, and base material sheet
WO2022249888A1