Pressure-sensitive adhesive sheet and display

The pressure-sensitive adhesive sheet with an active energy ray-curable adhesive layer addresses the issues of light reflection and crack formation in display modules by shifting the peak temperature of the loss tangent and maintaining high gel fraction and molecular weight, ensuring improved image quality and weather resistance.

WO2024202755A1PCT designated stage expired Publication Date: 2024-10-03LINTEC CORP

Patent Information

Application Number
PCT/JP2024/006473
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-02-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

The existing adhesive layers used in display modules, especially those with air gaps between protective panels and display modules, suffer from significant light reflection losses due to refractive index differences, leading to deteriorated image quality, and are prone to needle-like cracks when exposed to high-intensity ultraviolet rays, particularly during accelerated weather resistance tests.

Method used

A pressure-sensitive adhesive sheet with an active energy ray-curable adhesive layer that has specific properties, including a peak temperature shift of the loss tangent after ultraviolet irradiation, a high gel fraction, and controlled molecular weight, which suppresses the formation of needle-like cracks and enhances weather resistance.

Benefits of technology

The adhesive sheet effectively prevents needle-like cracks and maintains excellent adhesion and weather resistance even after prolonged exposure to high-intensity ultraviolet rays, thereby improving the image quality and durability of display modules.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024006473_03102024_PF_FP_ABST
    Figure JP2024006473_03102024_PF_FP_ABST
Patent Text Reader

Abstract

A pressure-sensitive adhesive sheet 1 having a pressure-sensitive adhesive layer 11 for bonding two display-body-constituting members to each other, wherein the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer 11 is an active energy ray-curable pressure-sensitive adhesive, and, when the peak temperature of the loss tangent tan δ of the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer 11' after active energy ray curing is taken as Tb (°C) and the peak temperature of the loss tangent tan δ of the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer 11' after applying 100 mW / cm2 UV rays for 120 hours to the pressure-sensitive adhesive layer 11' after active energy ray curing is taken as Ta (°C), the value obtained by subtracting Tb from Ta exceeds 3. The pressure-sensitive sheet 1 can suppress the occurrence of needle-like cracks and has excellent weather resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Adhesive sheets and displays

[0001] The present invention relates to an adhesive sheet for bonding two display component members together, and to an indicator obtained by using an adhesive layer of the adhesive sheet.

[0002] BACKGROUND ART In recent years, various mobile electronic devices such as mobile phones, smartphones, and tablet terminals are equipped with displays that use display modules having liquid crystal elements, light-emitting diodes (LED elements), organic electroluminescence (organic EL) elements, etc.

[0003] In such displays, a protective panel is usually provided on the front side of the display module. As electronic devices become thinner and lighter, the protective panel is increasingly being replaced by a plastic plate such as an acrylic plate or a polycarbonate plate, rather than the conventional glass plate.

[0004] Here, a gap is provided between the protective panel and the display module so that even when the protective panel is deformed by an external force, the deformed protective panel will not collide with the display module.

[0005] However, when such a gap, i.e., an air layer, is present, there is a problem that the difference in refractive index between the protective panel and the air layer, and the difference in refractive index between the air layer and the display module, results in a large light reflection loss, which reduces the image quality of the display.

[0006] Therefore, it has been proposed to improve the image quality of a display by filling the gap between the protective panel and the display module with an adhesive layer. For example, Patent Document 1 discloses an adhesive layer having a shear storage modulus (G') of 1.0 x 10 at 25°C and 1 Hz, which is used to fill the gap between the protective panel and the display module. 5 The document discloses a pressure-sensitive adhesive layer having a viscosity of 100 Pa or less and a gel fraction of 40% or more.

[0007] JP 2010-97070 A

[0008] However, when a display obtained using the above-described pressure-sensitive adhesive layer is irradiated with high-intensity ultraviolet light for a long period of time, needle-like cracks may occur in the pressure-sensitive adhesive layer. In particular, such a problem is likely to occur when an accelerated weather resistance test is performed in which high-intensity ultraviolet light is irradiated for a long period of time.

[0009] The present invention has been made in view of the above circumstances, and has an object to provide a pressure-sensitive adhesive sheet and a display that can suppress the occurrence of needle-like cracks and have excellent weather resistance.

[0010] In order to achieve the above object, first, the present invention provides a pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer for bonding two display component members to each other, wherein the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer is an active energy ray-curable pressure-sensitive adhesive, and the peak temperature of the loss tangent tanδ of the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer after active energy ray curing is defined as Tb (°C), and the pressure-sensitive adhesive layer after active energy ray curing has an illuminance of 100 mW / cm 2 The present invention provides a pressure-sensitive adhesive sheet characterized in that, when Ta (°C) is the peak temperature of the loss tangent tanδ of the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer after 120 hours of irradiation with ultraviolet light of 1000 nm or less, the value obtained by subtracting Tb from Ta exceeds 3 (Invention 1).

[0011] In the pressure-sensitive adhesive layer of the pressure-sensitive adhesive sheet according to the above invention (Invention 1), even when exposed to high-intensity ultraviolet light for a long period of time (e.g., 20 hours, 40 hours, etc.), destruction of crosslinking points that serve as starting points for needle-like cracks is suppressed, and good adhesion to display component members is exhibited. As a result, the pressure-sensitive adhesive sheet can suppress the occurrence of needle-like cracks and has excellent weather resistance.

[0012] In the above invention (Invention 1), the gel fraction of the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer is preferably 20% or more and 85% or less (Invention 2).

[0013] In the above inventions (Inventions 1 and 2), the gel fraction of the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer after curing with active energy rays is preferably 30% or more and 95% or less (Invention 3).

[0014] In the above inventions (Inventions 1 to 3), the illuminance of the pressure-sensitive adhesive layer after curing with active energy rays is 100 mW / cm 2 It is preferable that the gel fraction of the adhesive constituting the adhesive layer after 120 hours of irradiation with ultraviolet light of 40% or more and 99% or less (Invention 4).

[0015] In the above inventions (Inventions 1 to 4), it is preferable that the average peak molecular weight of the sol component of the adhesive constituting the adhesive layer after curing with active energy rays is 10,000 or more and 250,000 or less (Invention 5).

[0016] In the above inventions (Inventions 1 to 5), the pressure-sensitive adhesive layer after curing with active energy rays has an illuminance of 100 mW / cm 2 It is preferable that the average peak molecular weight of the sol component of the adhesive constituting the adhesive layer after 120 hours of irradiation with ultraviolet light of 10,000 or more and 200,000 or less (Invention 6).

[0017] In the above inventions (Inventions 1 to 6), it is preferable that the storage modulus G' at 23°C of the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer after curing with active energy rays is 0.01 MPa or more and 2 MPa or less (Invention 7).

[0018] In the above inventions (Inventions 1 to 7), the pressure-sensitive adhesive layer after curing with active energy rays has an illuminance of 100 mW / cm 2 It is preferable that the storage modulus G' of the adhesive constituting the adhesive layer at 23°C after irradiation with ultraviolet light of 1000 kJ / cm2 for 120 hours is 0.01 MPa or more and 2 MPa or less (Invention 8).

[0019] In the above inventions (Inventions 1 to 8), it is preferable that the storage modulus G' of the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer at -15°C after curing with active energy rays is 0.01 MPa or more and 100 MPa or less (Invention 9).

[0020] In the above inventions (Inventions 1 to 9), the illuminance of the pressure-sensitive adhesive layer after curing with active energy rays is 100 mW / cm 2 It is preferable that the storage modulus G' of the adhesive constituting the adhesive layer at -15°C after irradiation with ultraviolet light of 1000 MPa for 120 hours is 0.1 MPa or more and 1000 MPa or less (Invention 10).

[0021] In the above inventions (Inventions 1 to 10), it is preferable that the storage modulus G' at 100°C of the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer after curing with active energy rays is 0.0001 MPa or more and 1 MPa or less (Invention 11).

[0022] In the above inventions (Inventions 1 to 11), the pressure-sensitive adhesive layer after curing with active energy rays has an illuminance of 100 mW / cm 2 It is preferable that the storage modulus G' of the adhesive constituting the adhesive layer at 100°C after irradiation with ultraviolet light of 100°C for 120 hours is 0.0001 MPa or more and 1 MPa or less (Invention 12).

[0023] In the above inventions (Inventions 1 to 12), the pressure-sensitive adhesive is preferably an acrylic pressure-sensitive adhesive (Invention 13).

[0024] In the above inventions (Inventions 1 to 13), it is preferable that the pressure-sensitive adhesive sheet comprises two release sheets, and the pressure-sensitive adhesive layer is sandwiched between the release sheets so as to contact the release surfaces of the two release sheets (Invention 14).

[0025] Secondly, the present invention provides a display comprising one display component, another display component, and an adhesive layer for bonding the one display component and the other display component to each other, wherein the adhesive layer is formed from the adhesive layer of the adhesive sheet (Inventions 1 to 14) (Invention 15).

[0026] In the above invention (Invention 15), both the one display member and the other display member may be hard plates (Invention 16).

[0027] The pressure-sensitive adhesive sheet and indicator according to the present invention can suppress the occurrence of needle-like cracks and have excellent weather resistance.

[0028] 1 is a cross-sectional view of a pressure-sensitive adhesive sheet according to one embodiment of the present invention;

[0029] Hereinafter, an embodiment of the present invention will be described. [Adhesive Sheet] The adhesive sheet according to this embodiment has an adhesive layer for bonding two display member components to each other. The specific configuration of the adhesive sheet and the display member components will be described later.

[0030] The pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer in the pressure-sensitive adhesive sheet according to this embodiment is an active energy ray-curable pressure-sensitive adhesive. In the pressure-sensitive adhesive sheet according to this embodiment, the peak temperature of the loss tangent tanδ of the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer after being cured with the active energy ray is defined as Tb (°C), and the illuminance of the pressure-sensitive adhesive layer after being cured with the active energy ray is 100 mW / cm. 2 When the peak temperature of the loss tangent tanδ of the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer after 120 hours of irradiation with ultraviolet light (hereinafter sometimes referred to as "S-UV irradiation") is Ta (°C), it is preferable that the value obtained by subtracting Tb from Ta exceeds 3 (Ta - Tb > 3). The method for measuring the loss tangent tanδ is as shown in the test examples described later.

[0031] Here, the term "pressure-sensitive adhesive layer after active energy ray curing" as used herein refers to a pressure-sensitive adhesive layer that has been completely cured by irradiation with active energy rays. Specifically, this refers to a pressure-sensitive adhesive layer in which, when the pressure-sensitive adhesive layer after active energy ray curing is further irradiated with active energy rays at the same dose (light amount) as when the pressure-sensitive adhesive layer was cured with the active energy rays, the increase in gel fraction of the pressure-sensitive adhesive layer is 10% or less, and particularly refers to a pressure-sensitive adhesive layer in which the increase is 5% or less. Furthermore, in this specification, "relative humidity α%" may also be expressed as "α% RH" (RH; Relative humidity).

[0032] Generally, prolonged exposure to high-intensity UV light, as described above, is thought to cause changes in the crosslinking structure of the adhesive, resulting in needle-like cracks. In contrast, the adhesive of the present invention satisfies the above-described relationship, shifting the peak temperature of the loss tangent tanδ to a higher temperature after S-UV irradiation, thereby shifting the point at which the adhesive's viscoelastic viscosity increases from a lower temperature to a room temperature. As a result, even after prolonged exposure to high-intensity UV light (e.g., 20 hours, 40 hours, etc.), destruction of crosslinking points that could be the starting point for needle-like cracks is suppressed, resulting in excellent adhesion to display component members. Thus, the adhesive sheet according to the present embodiment can suppress the occurrence of needle-like cracks and has excellent weather resistance.

[0033] From the viewpoint of suppressing the occurrence of needle-like cracks, the value of Ta - Tb is more preferably 4 or more, even more preferably 5 or more, particularly preferably 6 or more, even more preferably 7 or more, and of these, preferably 8 or more. On the other hand, from the viewpoint of appropriately shifting the point at which the viscoelastic viscosity of the pressure-sensitive adhesive increases toward room temperature, the upper limit of Ta - Tb is preferably 30 or less, more preferably 24 or less, particularly preferably 18 or less, even more preferably 15 or less, and of these, preferably 12 or less.

[0034] The peak temperature Ta of the loss tangent tanδ of the pressure-sensitive adhesive after S-UV irradiation of the pressure-sensitive adhesive layer after active energy ray curing (hereinafter simply referred to as "pressure-sensitive adhesive after S-UV irradiation") is preferably −30 to 30° C., more preferably −20 to 20° C., particularly preferably −10 to 10° C., further preferably −5 to 5° C., and of these, preferably −4 to 2° C. This makes it easier for the value of Ta−Tb to fall within the preferred range.

[0035] The pressure-sensitive adhesive has a peak temperature Tb of loss tangent tanδ after curing with the active energy rays (before S-UV irradiation) of preferably −30 to 30° C., more preferably −25 to 20° C., particularly preferably −20 to 10° C., further preferably −15 to 5° C., and most preferably −10 to 0° C. This makes it easier for the value of Ta−Tb to fall within a preferred range, and also makes it easier to obtain good adhesiveness after curing with the active energy rays.

[0036] The gel fraction of the adhesive constituting the adhesive layer in the adhesive sheet according to this embodiment is preferably 20 to 85%, more preferably 30 to 80%, particularly preferably 40 to 75%, even more preferably 46 to 70%, and most preferably 52 to 67%. This makes it easier for the sheet to exhibit good adhesive properties when attached to an adherend. The method for measuring the gel fraction in this specification is as shown in the test examples described below.

[0037] The gel fraction of the adhesive constituting the adhesive layer in the adhesive sheet according to this embodiment after curing with active energy rays is preferably 30 to 95%, more preferably 40 to 92%, particularly preferably 50 to 90%, even more preferably 60 to 88%, and of these, preferably 70 to 86%. This makes it easier to achieve good adhesive strength after laminating the display component.

[0038] The gel fraction of the pressure-sensitive adhesive after S-UV irradiation is preferably 40 to 99%, more preferably 55 to 98%, particularly preferably 70 to 97%, even more preferably 78 to 96%, and most preferably 84 to 95%, which makes it easier for the Ta-Tb value to fall within the preferred range.

[0039] The average peak molecular weight of the sol component of the adhesive constituting the adhesive layer of the adhesive sheet according to this embodiment after curing with active energy rays is preferably 10,000 to 250,000, more preferably 30,000 to 200,000, particularly preferably 50,000 to 150,000, even more preferably 60,000 to 100,000, and most preferably 62,000 to 75,000. This facilitates good adhesive strength after lamination of the display component. The average peak molecular weight of the sol component in this specification is a value measured by gel permeation chromatography (GPC) in terms of standard polystyrene. Specific measurement methods are as shown in the test examples described below.

[0040] The average peak molecular weight of the sol component of the pressure-sensitive adhesive after S-UV irradiation is preferably 10,000 to 200,000, more preferably 30,000 to 160,000, particularly preferably 40,000 to 120,000, further preferably 50,000 to 80,000, and most preferably 55,000 to 70,000. This makes it easier for the Ta-Tb value to fall within the preferred range.

[0041] The storage modulus G' at 23°C of the adhesive constituting the adhesive layer in the adhesive sheet according to this embodiment after curing with active energy rays is preferably 0.01 to 2 MPa, more preferably 0.04 to 1 MPa, more preferably 0.08 to 0.8 MPa, particularly preferably 0.12 to 0.6 MPa, even more preferably 0.15 to 0.5 MPa, and most preferably 0.18 to 0.4 MPa. This tends to ensure good adhesive strength after bonding to the display component. The method for measuring the storage modulus G' in this specification is as shown in the test examples described below.

[0042] The storage modulus G' of the pressure-sensitive adhesive at 23°C after S-UV irradiation is preferably 0.01 to 2 MPa, more preferably 0.05 to 1.5 MPa, more preferably 0.1 to 1 MPa, particularly preferably 0.15 to 0.8 MPa, and even more preferably 0.18 to 0.6 MPa. This makes it easier for the Ta - Tb value to fall within the preferred range.

[0043] The storage modulus G' at -15°C of the adhesive constituting the adhesive layer in the adhesive sheet according to this embodiment after curing with active energy rays is preferably 0.01 to 100 MPa, more preferably 0.1 to 80 MPa, more preferably 1 to 60 MPa, particularly preferably 1 to 40 MPa, even more preferably 5 to 30 MPa, and of these, preferably 10 to 30 MPa. This makes it easier to achieve good adhesive strength at low temperatures after lamination of the display component.

[0044] The storage modulus G' of the pressure-sensitive adhesive after S-UV irradiation at -15°C is preferably 0.1 to 1000 MPa, more preferably 1 to 500 MPa, more preferably 5 to 200 MPa, particularly preferably 10 to 100 MPa, and even more preferably 18 to 50 MPa. This makes it easier for the Ta - Tb value to fall within the preferred range.

[0045] The storage modulus G' at 100°C of the adhesive constituting the adhesive layer in the adhesive sheet according to this embodiment after curing with active energy rays is preferably 0.0001 to 1 MPa, more preferably 0.001 to 0.7 MPa, more preferably 0.005 to 0.4 MPa, particularly preferably 0.01 to 0.2 MPa, even more preferably 0.02 to 0.1 MPa, and of these, preferably 0.03 to 0.07 MPa. This tends to ensure good adhesive strength at high temperatures after lamination of the display component.

[0046] The storage modulus G' of the pressure-sensitive adhesive at 100°C after S-UV irradiation is preferably 0.0001 to 1 MPa, more preferably 0.0005 to 0.7 MPa, more preferably 0.001 to 0.4 MPa, particularly preferably 0.005 to 0.2 MPa, even more preferably 0.01 to 0.1 MPa, and of these, preferably 0.02 to 0.09 MPa. This makes it easier for the Ta-Tb value to fall within the preferred range.

[0047] The adhesive strength of the adhesive layer of the pressure-sensitive adhesive sheet according to this embodiment after curing with active energy rays (before S-UV irradiation) to soda-lime glass is preferably 1 to 100 N / 25 mm, more preferably 5 to 75 N / 25 mm, particularly preferably 10 to 50 N / 25 mm, and even more preferably 15 to 35 N / 25 mm. This tends to result in excellent weather resistance and blister resistance. The above adhesive strength basically refers to the adhesive strength measured by the 180-degree peel method in accordance with JIS Z0237:2009, and the specific test method is as shown in the test examples described below.

[0048] In the pressure-sensitive adhesive sheet according to this embodiment, the total light transmittance of the pressure-sensitive adhesive layer after active energy ray curing (before S-UV irradiation) is preferably 80% or more, more preferably 90% or more, particularly preferably 95% or more, and even more preferably 99% or more. This results in extremely high transparency and makes the sheet suitable for optical applications (for displays). The upper limit of the total light transmittance is not particularly limited, and may be 100%, or may be a value slightly exceeding 100% due to measurement constraints. It is preferable that the total light transmittances of the pressure-sensitive adhesive layer before active energy ray curing and the pressure-sensitive adhesive layer after S-UV irradiation are in the same numerical range as the pressure-sensitive adhesive layer before S-UV irradiation. The total light transmittance in this specification is a value measured in accordance with JIS K7361-1:1997, and specific test methods are as shown in the test examples described below.

[0049] The haze value of the pressure-sensitive adhesive layer in the pressure-sensitive adhesive sheet according to this embodiment after active energy ray curing (before S-UV irradiation) is preferably 2% or less, and particularly preferably 1% or less. This provides very high transparency and makes the sheet suitable for optical applications (for displays). The lower limit of the haze value is not particularly restricted and may be 0%. The haze values ​​of the pressure-sensitive adhesive layer before active energy ray curing and the pressure-sensitive adhesive layer after S-UV irradiation are preferably in the same numerical range as the pressure-sensitive adhesive layer before S-UV irradiation. The haze value in this specification is a value measured in accordance with JIS K7136:2000, and specific test methods are as shown in the test examples described below.

[0050] The chromaticity b* (chromaticity b*1) defined by the CIE 1976 L*a*b* color system of the pressure-sensitive adhesive layer in the pressure-sensitive adhesive sheet according to this embodiment after curing with active energy rays is preferably −20 to 20, more preferably −10 to 10, particularly preferably −5 to 5, even more preferably −1 to 1, and most preferably −0.5 to 0.5. This makes the pressure-sensitive adhesive layer nearly colorless and transparent, making it suitable for optical applications.

[0051] The chromaticity b* (chromaticity b*2) of the pressure-sensitive adhesive layer, which has been cured with active energy rays and then irradiated with S-UV, as defined by the CIE 1976 L*a*b* color system is preferably −20 to 20, more preferably −10 to 10, particularly preferably −6 to 6, even more preferably −2 to 2, and most preferably −1 to 1. This means that the pressure-sensitive adhesive layer has a small degree of yellowness even after S-UV irradiation, and is excellent in weather resistance from the standpoint of chromaticity.

[0052] The absolute value of the ratio (b*2 / b*1) of the chromaticity b*2 to the chromaticity b*1 is preferably 20 or less, more preferably 15 or less, particularly preferably 10 or less, even more preferably 5 or less, and most preferably 2 or less. This reduces the degree of yellowing of the pressure-sensitive adhesive layer even after S-UV irradiation, and can be said to have excellent weather resistance from the perspective of chromaticity. The lower limit of the absolute value of the ratio (b*2 / b*1) is not particularly limited, but is most preferably 1.

[0053] The adhesive constituting the adhesive layer in this embodiment is an active energy ray-curable adhesive, and its type may be any of an acrylic adhesive, a polyester adhesive, a polyurethane adhesive, a rubber adhesive, a silicone adhesive, etc. Furthermore, the adhesive may be any of an emulsion type, a solvent type, or a solventless type, and may be any of a crosslinked type or a non-crosslinked type. Among them, an acrylic adhesive is preferred because of its excellent adhesive properties, optical properties, etc.

[0054] The adhesive constituting the adhesive layer in this embodiment preferably contains a (meth)acrylic acid ester polymer as the adhesive main component, and particularly preferably contains a crosslinked (meth)acrylic acid ester polymer. Furthermore, the adhesive constituting the adhesive layer in this embodiment preferably contains a main adhesive component and an active energy ray-curable component. That is, the adhesive constituting the adhesive layer in this embodiment preferably contains a crosslinked (meth)acrylic acid ester polymer and an active energy ray-curable component. The crosslinked (meth)acrylic acid ester polymer is preferably a crosslinked (meth)acrylic acid ester polymer and a crosslinking agent.

[0055] Specifically, the adhesive constituting the adhesive layer in this embodiment is preferably obtained by crosslinking (preferably thermally crosslinking) an adhesive composition (hereinafter sometimes referred to as "adhesive composition P") containing a (meth)acrylic acid ester polymer (A), a crosslinking agent (B), and an active energy ray-curable component (C). In this specification, (meth)acrylic acid means both acrylic acid and methacrylic acid. The same applies to other similar terms. Furthermore, the term "polymer" also includes the concept of "copolymer."

[0056] (1) Components (1-1) (Meth)acrylic acid ester polymer (A) The (meth)acrylic acid ester polymer (A) preferably contains a structural unit derived from a (meth)acrylic acid alkyl ester. This allows the polymer to exhibit good adhesiveness. Note that the (meth)acrylic acid alkyl ester does not include the hard monomer described below.

[0057] From the viewpoint of adhesiveness, the (meth)acrylic acid alkyl ester is preferably a (meth)acrylic acid alkyl ester having an alkyl group containing 1 to 20 carbon atoms. Examples of (meth)acrylic acid alkyl esters having an alkyl group containing 1 to 20 carbon atoms include methyl acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, n-decyl (meth)acrylate, n-dodecyl (meth)acrylate, myristyl (meth)acrylate, palmityl (meth)acrylate, and stearyl (meth)acrylate. These may be used alone or in combination of two or more. Among the above, from the viewpoint of further improving adhesiveness, (meth)acrylic acid esters having an alkyl group with 1 to 14 carbon atoms are preferred, (meth)acrylic acid esters having an alkyl group with 2 to 10 carbon atoms are more preferred, and (meth)acrylic acid esters having an alkyl group with 3 to 8 carbon atoms are particularly preferred. Specifically, for example, methyl acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, or isooctyl (meth)acrylate are preferred, and n-butyl acrylate or 2-ethylhexyl acrylate are particularly preferred.

[0058] From the viewpoint of imparting adhesiveness, the (meth)acrylic acid ester polymer (A) preferably contains 99% by mass or less of structural units derived from (meth)acrylic acid alkyl esters, more preferably 96% by mass or less, and particularly preferably 92% by mass or less. When an acid-free adhesive is preferred due to compatibility with the target adherend, the resulting adhesive preferably contains 85% by mass or less of structural units derived from (meth)acrylic acid alkyl esters, more preferably 80% by mass or less, particularly preferably 75% by mass or less, and even more preferably 70% by mass or less. Meanwhile, the lower limit is preferably 40% by mass or more, more preferably 48% by mass or more, particularly preferably 54% by mass or more, and even more preferably 60% by mass or more. In addition, if it is preferred that the resulting pressure-sensitive adhesive contain an acid component due to compatibility with the target adherend, etc., it is preferable that the pressure-sensitive adhesive contain the above-mentioned structural unit in an amount of 70% by mass or more, more preferably 75% by mass or more, particularly preferably 80% by mass or more, and even more preferably 85% by mass or more.

[0059] The (meth)acrylic acid ester polymer (A) preferably contains a structural unit derived from a reactive functional group-containing monomer, whereby the reactive functional group derived from the reactive functional group-containing monomer reacts with the crosslinking agent (B) to form a crosslinked structure (three-dimensional network structure), thereby obtaining a pressure-sensitive adhesive having the desired cohesive strength.

[0060] Preferred examples of the reactive group-containing monomer include a monomer having a hydroxyl group in the molecule (hydroxyl group-containing monomer), a monomer having a carboxyl group in the molecule (carboxyl group-containing monomer), a monomer having an amino group in the molecule (amino group-containing monomer), etc. Among these, a hydroxyl group-containing monomer or a carboxyl group-containing monomer, which has excellent reactivity with the crosslinking agent (B), is preferred.

[0061] Examples of hydroxyl group-containing monomers include (meth)acrylic acid hydroxyalkyl esters such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. Among these, 2-hydroxyethyl (meth)acrylate or 4-hydroxybutyl (meth)acrylate is preferred from the viewpoints of reactivity with the crosslinking agent (B) and copolymerizability with other monomers. These may be used alone or in combination of two or more.

[0062] Examples of carboxyl group-containing monomers include ethylenically unsaturated carboxylic acids such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, itaconic acid, and citraconic acid. Among them, acrylic acid or methacrylic acid is preferred in terms of reactivity with the crosslinking agent (B) and copolymerizability with other monomers, and acrylic acid is particularly preferred. These may be used alone or in combination of two or more.

[0063] From the viewpoint of cohesive strength, the content of the structural unit derived from the reactive functional group-containing monomer in the (meth)acrylic acid ester polymer (A) is preferably 1 to 40 mass%, more preferably 3 to 32 mass%, particularly preferably 6 to 26 mass%, and even more preferably 8 to 22 mass%. In particular, when an acid-free PSA is preferred as the resulting PSA, the content is preferably 12 to 21 mass%, particularly preferably 16 to 20 mass%, and when an PSA containing an acid component is preferred, the content is preferably 9 to 14 mass%.

[0064] The (meth)acrylic acid ester polymer (A) also preferably contains a structural unit derived from a hard monomer having a glass transition temperature (Tg) of 70°C or higher as a homopolymer. The aforementioned reactive functional group-containing monomer is excluded from the hard monomer. This improves the cohesive strength of the resulting PSA, making it easier to achieve excellent blister resistance. In particular, when a structural unit derived from a (meth)acrylic acid ester having an alkyl group with 5 to 8 carbon atoms is contained, the cohesive strength tends to be low, so it is preferable to contain the structural unit derived from the hard monomer. The glass transition temperature (Tg) of the hard monomer as a homopolymer is preferably 75 to 200°C, particularly preferably 80 to 180°C, and even more preferably 90 to 150°C.

[0065] Examples of the hard monomer include methyl methacrylate (Tg 105° C.), isobornyl acrylate (Tg 94° C.), isobornyl methacrylate (Tg 180° C.), adamantyl acrylate (Tg 115° C.), adamantyl methacrylate (Tg 141° C.), etc. These may be used alone or in combination of two or more.

[0066] Among the above hard monomers, methyl methacrylate or isobornyl acrylate is more preferred from the viewpoint of better demonstrating the performance of the hard monomer while preventing adverse effects on other properties such as adhesion, transparency, etc. In particular, methyl methacrylate is preferred from the viewpoint of weather resistance, and isobornyl acrylate, which is a monomer having an alicyclic structure in the molecule (alicyclic structure-containing monomer), is particularly preferred from the viewpoint of adhesion.

[0067] When the (meth)acrylic acid ester polymer (A) contains the structural unit derived from the hard monomer, the content thereof is preferably 1 to 35% by mass, more preferably 4 to 28% by mass, particularly preferably 8 to 22% by mass, and even more preferably 12 to 17% by mass, from the viewpoint of easily exhibiting the desired cohesive strength and viscoelasticity and from the viewpoint of blister resistance.

[0068] The (meth)acrylic acid ester polymer (A) preferably contains a structural unit derived from a monomer having a nitrogen atom in the molecule (nitrogen atom-containing monomer). In particular, when an alicyclic structure-containing monomer, particularly isobornyl acrylate, is used as the hard monomer, it is preferable to contain a structural unit derived from a nitrogen atom-containing monomer. The presence of a structural unit derived from a nitrogen atom-containing monomer can impart a predetermined polarity to the adhesive and improve the adhesiveness.

[0069] As the nitrogen atom-containing monomer, a monomer having a nitrogen-containing heterocycle is preferred from the viewpoint of providing the (meth)acrylic acid ester polymer (A) with appropriate rigidity. Also, from the viewpoint of increasing the degree of freedom of the nitrogen atom-containing monomer-derived portion in the higher-order structure of the pressure-sensitive adhesive constituted, it is preferred that the nitrogen atom-containing monomer does not contain a reactive unsaturated double bond group other than one polymerizable group used in polymerization to form the (meth)acrylic acid ester polymer (A).

[0070] Examples of monomers having a nitrogen-containing heterocycle include N-(meth)acryloylmorpholine, N-vinyl-2-pyrrolidone, N-(meth)acryloylpyrrolidone, N-(meth)acryloylpiperidine, N-(meth)acryloylpyrrolidine, N-(meth)acryloylaziridine, aziridinylethyl (meth)acrylate, 2-vinylpyridine, 4-vinylpyridine, 2-vinylpyrazine, 1-vinylimidazole, N-vinylcarbazole, and N-vinylphthalimide. Among these, N-(meth)acryloylmorpholine, which exhibits superior adhesive strength, is preferred, and N-acryloylmorpholine is particularly preferred. These may be used alone or in combination of two or more.

[0071] When the (meth)acrylic acid ester polymer (A) contains a constituent unit derived from a nitrogen atom-containing monomer, the content thereof is preferably 1 to 20 mass%, more preferably 2 to 16 mass%, particularly preferably 3 to 12 mass%, and even more preferably 4 to 8 mass%, from the viewpoint of making it easier to exhibit the desired viscoelasticity and from the viewpoint of better adhesiveness.

[0072] The (meth)acrylic acid ester polymer (A) may contain structural units derived from other monomers, if desired. The other monomers are preferably monomers that do not contain reactive functional groups, so as not to interfere with the action of the reactive group-containing monomer. Examples of such other monomers include (meth)acrylic acid alkoxyalkyl esters such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate, vinyl acetate, and styrene. These may be used alone or in combination of two or more.

[0073] The (meth)acrylic acid ester polymer (A) may be a polymer obtained by solution polymerization, a polymer obtained without a solvent, or an emulsion polymerization. Among these, a solution polymer obtained by solution polymerization is preferred. By using a solution polymer, a high molecular weight polymer can be easily obtained, and the above-mentioned Ta-Tb value is more likely to fall within the preferred range.

[0074] The polymerization mode of the (meth)acrylic acid ester polymer (A) may be a random copolymer or a block copolymer.

[0075] The weight-average molecular weight of the (meth)acrylic acid ester polymer (A) is preferably 100,000 to 3,000,000, more preferably 200,000 to 2,000,000, particularly preferably 300,000 to 1,200,000, and even more preferably 400,000 to 800,000. This makes it easier for the aforementioned Ta-Tb value to fall within the preferred range. Furthermore, it also makes it easier for the polymer to exhibit desired cohesive strength and viscoelasticity, as well as suitable adhesiveness. The weight-average molecular weight in this specification is a value measured by gel permeation chromatography (GPC) in terms of standard polystyrene.

[0076] In the pressure-sensitive adhesive composition P, the (meth)acrylic acid ester polymer (A) may be used alone or in combination of two or more.

[0077] The content of the (meth)acrylic acid ester polymer (A) in the pressure-sensitive adhesive composition P according to this embodiment is preferably 60 to 99.9% by mass, more preferably 70 to 99% by mass, particularly preferably 80 to 98% by mass, and even more preferably 85 to 97% by mass. When an acid-free pressure-sensitive adhesive is preferred, the content is preferably 90 to 96% by mass. When an acid-containing pressure-sensitive adhesive is preferred, the content is preferably 86 to 91% by mass. This makes it easier for the Ta-Tb value described above to fall within the preferred range.

[0078] (1-2) Crosslinking Agent (B) The crosslinking agent (B) crosslinks the (meth)acrylic acid ester polymer (A) by heating the pressure-sensitive adhesive composition P, enabling the formation of a favorable three-dimensional network crosslinked structure. This allows for the production of a pressure-sensitive adhesive having a predetermined cohesive strength and viscoelasticity, making it easier for the above-mentioned Ta - Tb value to fall within a preferred range. This in turn makes it easier to obtain excellent blister resistance.

[0079] The crosslinking agent (B) may be any agent that reacts with the reactive functional group (hydroxyl group or carboxyl group) of the (meth)acrylic acid ester polymer (A). Examples include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, amine-based crosslinking agents, melamine-based crosslinking agents, aziridine-based crosslinking agents, hydrazine-based crosslinking agents, aldehyde-based crosslinking agents, oxazoline-based crosslinking agents, metal alkoxide-based crosslinking agents, metal chelate-based crosslinking agents, metal salt-based crosslinking agents, and ammonium salt-based crosslinking agents. When the (meth)acrylic acid ester polymer (A) contains a structural unit derived from a hydroxyl group-containing monomer, it is preferable to use an isocyanate-based crosslinking agent that has excellent reactivity with hydroxyl groups as the crosslinking agent (B). When the (meth)acrylic acid ester polymer (A) contains a structural unit derived from a carboxyl group-containing monomer, it is preferable to use an epoxy-based crosslinking agent that has excellent reactivity with carboxyl groups as the crosslinking agent (B). The crosslinking agent (B) may be used alone or in combination of two or more.

[0080] The isocyanate-based crosslinking agent contains at least a polyisocyanate compound. Examples of polyisocyanate compounds include aromatic polyisocyanates such as tolylene diisocyanate, diphenylmethane diisocyanate, and xylylene diisocyanate; aliphatic polyisocyanates such as hexamethylene diisocyanate; alicyclic polyisocyanates such as isophorone diisocyanate and hydrogenated diphenylmethane diisocyanate; and biuret and isocyanurate forms thereof, as well as adducts thereof that are reaction products with low-molecular-weight active hydrogen-containing compounds such as ethylene glycol, propylene glycol, neopentyl glycol, trimethylolpropane, and castor oil. Among these, trimethylolpropane-modified aromatic polyisocyanates, particularly trimethylolpropane-modified tolylene diisocyanate or trimethylolpropane-modified xylylene diisocyanate, are preferred from the viewpoint of reactivity with hydroxyl groups.

[0081] Examples of epoxy crosslinking agents include 1,3-bis(N,N'-diglycidylaminomethyl)cyclohexane, N,N,N',N'-tetraglycidyl-m-xylylenediamine, ethylene glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane diglycidyl ether, diglycidylaniline, diglycidylamine, etc. Among these, 1,3-bis(N,N'-diglycidylaminomethyl)cyclohexane or N,N,N',N'-tetraglycidyl-m-xylylenediamine is preferred from the viewpoint of reactivity with carboxy groups.

[0082] The content of the crosslinking agent (B) in the pressure-sensitive adhesive composition P is preferably 0.001 to 10 parts by mass, more preferably 0.005 to 5 parts by mass, and particularly preferably 0.01 to 1 part by mass, relative to 100 parts by mass of the (meth)acrylic acid ester polymer (A). When an acid-free pressure-sensitive adhesive is preferred, the content is preferably 0.05 to 0.8 parts by mass, more preferably 0.1 to 0.6 parts by mass. From the viewpoint of weather resistance, the content is preferably 0.2 to 0.4 parts by mass. When an acid-containing pressure-sensitive adhesive is preferred, the content is preferably 0.015 to 0.5 parts by mass, more preferably 0.02 to 0.1 parts by mass. This makes it easier for the Ta-Tb value described above to fall within the preferred range.

[0083] (1-3) Active Energy Ray-Curable Component (C) When the pressure-sensitive adhesive composition P contains the active energy ray-curable component (C), the resulting pressure-sensitive adhesive becomes active energy ray-curable.

[0084] The active energy ray-curable component (C) is not particularly limited as long as it is a component that is cured by irradiation with active energy rays and that can provide the above-mentioned physical properties, and may be any of a monomer, oligomer, or polymer, or a mixture thereof. Among them, preferred is a polyfunctional acrylate-based monomer that makes it easier for the above-mentioned Ta-Tb value to fall within the preferred range.

[0085] Examples of polyfunctional acrylate monomers include bifunctional monomers such as 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, neopentyl glycol adipate di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, dicyclopentanyl di(meth)acrylate, caprolactone-modified dicyclopentenyl di(meth)acrylate, ethylene oxide-modified phosphate di(meth)acrylate, di(acryloxyethyl)isocyanurate, allylated cyclohexyl di(meth)acrylate, ethoxylated bisphenol A diacrylate, and 9,9-bis[4-(2-acryloyloxyethoxy)phenyl]fluorene; trifunctional types such as diglycerol tetra(meth)acrylate and pentaerythritol tetra(meth)acrylate; pentafunctional types such as propionic acid-modified dipentaerythritol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, propylene oxide-modified trimethylolpropane tri(meth)acrylate, tris(acryloxyethyl)isocyanurate, and ε-caprolactone-modified tris-(2-(meth)acryloxyethyl)isocyanurate; tetrafunctional types such as diglycerol tetra(meth)acrylate and pentaerythritol tetra(meth)acrylate; pentafunctional types such as propionic acid-modified dipentaerythritol penta(meth)acrylate; and hexafunctional types such as dipentaerythritol hexa(meth)acrylate and caprolactone-modified dipentaerythritol hexa(meth)acrylate. Among the above, from the viewpoint of the blister resistance of the resulting PSA, preferred are polyfunctional acrylate monomers containing an isocyanurate structure in the molecule, such as di(acryloxyethyl)isocyanurate, tris(acryloxyethyl)isocyanurate, and ε-caprolactone-modified tris-(2-(meth)acryloxyethyl)isocyanurate, more preferred are polyfunctional acrylate monomers which are tri- or higher functional and contain an isocyanurate structure in the molecule, and particularly preferred is ε-caprolactone-modified tris-(2-(meth)acryloxyethyl)isocyanurate.These may be used alone or in combination of two or more. Furthermore, from the viewpoint of making it easier for the resulting pressure-sensitive adhesive to exhibit the desired viscoelasticity, the polyfunctional acrylate monomer preferably has a molecular weight of less than 20,000, more preferably less than 10,000, and particularly preferably less than 5,000. Furthermore, from the viewpoint of compatibility with the (meth)acrylic acid ester polymer (A), a polyfunctional acrylate monomer preferably has a molecular weight of less than 1,000.

[0086] The content of the active energy ray-curable component (C) in the pressure-sensitive adhesive composition P is preferably 1 to 50 parts by mass, more preferably 2 to 40 parts by mass, particularly preferably 3 to 30 parts by mass, and even more preferably 4 to 20 parts by mass, per 100 parts by mass of the (meth)acrylic acid ester polymer (A). When an acid-free pressure-sensitive adhesive is preferred as the resulting pressure-sensitive adhesive, the content is preferably 4.5 to 10 parts by mass, even more preferably 5 to 8 parts by mass. Furthermore, when an acid-containing pressure-sensitive adhesive is preferred as the resulting pressure-sensitive adhesive, the content is preferably 5 to 16 parts by mass, even more preferably 8 to 14 parts by mass. This makes it easier for the Ta-Tb value described above to fall within the preferred range.

[0087] (1-4) Photopolymerization initiator (D) When ultraviolet rays are used as active energy rays to cure the pressure-sensitive adhesive layer, the pressure-sensitive adhesive composition P preferably contains a photopolymerization initiator (D), which allows the active energy ray-curable component (C) to be cured efficiently and also reduces the polymerization curing time and the ultraviolet irradiation dose.

[0088] Examples of the photopolymerization initiator (D) include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin-n-butyl ether, benzoin isobutyl ether, acetophenone, dimethylaminoacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propan-1-one, 4-(2-hydroxyethoxy)phenyl-2-(hydroxy-2-propyl)ketone, benzophenone, p-phenylbenzophenone, 4,4 Examples of suitable benzoxanthraquinones include 2-methyl-2-hydroxybenzoyl-1-methyl-1-methyl-2-methyl-1 ...

[0089] Among the above, from the viewpoint of suppressing the occurrence of needle-like cracks, phosphine-based photopolymerization initiators such as 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, or a mixture of benzophenone and 1-hydroxycyclohexyl phenyl ketone are particularly preferred, and from the viewpoints of weather resistance and blister resistance, 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide or a mixture of benzophenone and 1-hydroxycyclohexyl phenyl ketone are particularly preferred.

[0090] The content of the photopolymerization initiator (D) in the pressure-sensitive adhesive composition P is preferably 1 to 40 parts by mass, more preferably 3 to 30 parts by mass, particularly preferably 6 to 22 parts by mass, and even more preferably 8 to 14 parts by mass, relative to 100 parts by mass of the active energy ray-curable component (C). This makes it easier for the resulting pressure-sensitive adhesive to satisfy the above-mentioned physical properties.

[0091] (1-5) Silane Coupling Agent (E) The pressure-sensitive adhesive composition P preferably further contains a silane coupling agent (E). This improves the adhesion of the resulting pressure-sensitive adhesive to a glass member when the adherend is a glass member. Furthermore, even when the adherend is a plastic plate, the resulting pressure-sensitive adhesive improves the adhesion of the resulting pressure-sensitive adhesive to the plastic plate. This makes it easier to satisfy the above-mentioned physical properties, and makes it easier to obtain excellent blister resistance in the pressure-sensitive adhesive.

[0092] The silane coupling agent (E) is preferably an organosilicon compound having at least one alkoxysilyl group in the molecule, which has good compatibility with the (meth)acrylic acid ester polymer (A) and has optical transparency.

[0093] Examples of such silane coupling agents (E) include polymerizable unsaturated group-containing silicon compounds such as vinyltrimethoxysilane, vinyltriethoxysilane, and methacryloxypropyltrimethoxysilane; silicon compounds having an epoxy structure such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, and 3-mercaptopropyldimethoxymethylsilane; Examples of suitable silicon compounds include hydroxyl group-containing silicon compounds, amino group-containing silicon compounds such as 3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, and N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-chloropropyltrimethoxysilane, and 3-isocyanatepropyltriethoxysilane, as well as condensates of at least one of these with alkyl group-containing silicon compounds such as methyltriethoxysilane, ethyltriethoxysilane, methyltrimethoxysilane, and ethyltrimethoxysilane. These may be used alone or in combination of two or more.

[0094] The content of the silane coupling agent (E) in the pressure-sensitive adhesive composition P is preferably 0.01 to 10 parts by mass, more preferably 0.04 to 5 parts by mass, particularly preferably 0.08 to 1 part by mass, even more preferably 0.12 to 0.5 parts by mass, and especially preferably 0.15 to 0.35 parts by mass, relative to 100 parts by mass of the (meth)acrylic acid ester polymer (A). This allows the composition to exhibit excellent adhesion, and provides excellent weather resistance and blister resistance.

[0095] (1-6) Various Additives The pressure-sensitive adhesive composition P may contain, if desired, various additives commonly used in acrylic pressure-sensitive adhesives, such as a light stabilizer, an ultraviolet absorber, an oxygen absorber, an antioxidant, a tackifier, a softener, a colorant, an infrared absorber, a rust inhibitor, an antistatic agent, a filler, a refractive index adjuster, etc.

[0096] Examples of the light stabilizer include hindered amine light stabilizers and hindered phenol light stabilizers, and from the viewpoint of suppressing needle cracks, hindered amine light stabilizers are preferred. Examples of the hindered amine light stabilizer include tetrakis(1,2,2,6,6-pentamethyl-4-piperidyl)-1,2,3,4-butanetetracarboxylate, tetrakis(2,2,6,6-tetramethyl-4-piperidyl)1,2,3,4-butanetetracarboxylate, bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate, bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate, bis(1-undecanoxy-2,2,6,6-tetramethylpiperidin-4-yl)carbonate, 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate, and 2,2,6,6-tetramethyl-4-piperidyl methacrylate. Among these, from the viewpoint of weather resistance and blister resistance, bis(1-undecanoxy-2,2,6,6-tetramethylpiperidin-4-yl)carbonate is preferred. These may be used alone or in combination of two or more.

[0097] The content of the light stabilizer in the pressure-sensitive adhesive composition P is preferably 0.01 to 20 parts by mass, more preferably 0.05 to 10 parts by mass, particularly preferably 0.1 to 5 parts by mass, even more preferably 0.2 to 2 parts by mass, and especially preferably 0.3 to 1 part by mass, relative to 100 parts by mass of the (meth)acrylic acid ester polymer (A). This makes it easier to suppress needle-like cracks and also tends to provide excellent blister resistance.

[0098] (2) Production of adhesive composition The adhesive composition P can be produced by producing a (meth)acrylic acid ester polymer (A), mixing the obtained (meth)acrylic acid ester polymer (A) with a crosslinking agent (B) and an active energy ray-curable component (C), and adding a photopolymerization initiator (D), a silane coupling agent (E), an additive, etc., as desired.

[0099] The (meth)acrylic acid ester polymer (A) can be produced by polymerizing a mixture of monomers constituting the polymer by a conventional radical polymerization method. The polymerization of the (meth)acrylic acid ester polymer (A) is preferably carried out by a solution polymerization method using a polymerization initiator as desired. However, the present invention is not limited thereto, and the polymerization may be carried out in the absence of a solvent.

[0100] Examples of polymerization solvents include ethyl acetate, n-butyl acetate, isobutyl acetate, toluene, acetone, hexane, and methyl ethyl ketone, and two or more of these may be used in combination. Examples of polymerization initiators include azo compounds and organic peroxides, and two or more of these may be used in combination. In the polymerization step, the weight-average molecular weight of the resulting polymer can be adjusted by adding a chain transfer agent such as 2-mercaptoethanol.

[0101] Once the (meth)acrylic acid ester polymer (A) is obtained, a crosslinking agent (B), an active energy ray-curable component (C), and optionally a photopolymerization initiator (D), a silane coupling agent (E), additives, a dilution solvent, etc. are added to a solution of the (meth)acrylic acid ester polymer (A), and the mixture is thoroughly mixed to obtain a solvent-diluted adhesive composition P (coating solution). Note that, when a solid component is used for any of the above components, or when precipitation occurs when the component is mixed with other components in an undiluted state, the component may be dissolved or diluted alone in a dilution solvent before being mixed with other components.

[0102] Examples of the dilution solvent include aliphatic hydrocarbons such as hexane, heptane, and cyclohexane; aromatic hydrocarbons such as toluene and xylene; halogenated hydrocarbons such as methylene chloride and ethylene chloride; alcohols such as methanol, ethanol, propanol, butanol, and 1-methoxy-2-propanol; ketones such as acetone, methyl ethyl ketone, 2-pentanone, isophorone, and cyclohexanone; esters such as ethyl acetate and butyl acetate; and cellosolve-based solvents such as ethyl cellosolve.

[0103] The concentration and viscosity of the coating solution prepared in this manner are not particularly limited as long as they are within a range that allows coating, and can be appropriately selected depending on the situation. For example, the pressure-sensitive adhesive composition P is diluted so that the concentration is 10 to 60 mass %. Note that the addition of a dilution solvent or the like is not a necessary condition for obtaining the coating solution, and as long as the pressure-sensitive adhesive composition P has a viscosity that allows coating, the addition of a dilution solvent is not necessary. In this case, the pressure-sensitive adhesive composition P becomes a coating solution in which the polymerization solvent for the (meth)acrylic acid ester polymer (A) is used as the dilution solvent.

[0104] (3) Production of Pressure-Sensitive Adhesive The pressure-sensitive adhesive composition P described above is applied to a desired object and then crosslinked to obtain a pressure-sensitive adhesive (pressure-sensitive adhesive layer).

[0105] Crosslinking of the pressure-sensitive adhesive composition P can be carried out by a heat treatment. This heat treatment can also serve as a drying treatment after application of the pressure-sensitive adhesive composition P. The heating temperature for the heat treatment is preferably 50 to 150°C, and more preferably 70 to 120°C. The heating time is preferably 10 seconds to 10 minutes, and more preferably 50 seconds to 2 minutes.

[0106] After the heat treatment, a curing period of about 1 to 2 weeks may be provided at room temperature (e.g., 23°C, 50% RH), if necessary. If this curing period is required, the pressure-sensitive adhesive is formed after the curing period has elapsed. If no curing period is required, the pressure-sensitive adhesive is formed after the heat treatment has been completed.

[0107] By the above heat treatment (and curing), a crosslinked product of the (meth)acrylic acid ester polymer (A) crosslinked by the crosslinking agent (B) is formed.

[0108] (4) Thickness of Pressure-Sensitive Adhesive Layer The thickness of the pressure-sensitive adhesive layer of the pressure-sensitive adhesive sheet according to this embodiment (measured in accordance with JIS K7130) is preferably 1 to 1000 μm, more preferably 10 to 800 μm, and particularly preferably 30 to 600 μm, from the viewpoint of adhesive strength and blister resistance, and is preferably 50 to 400 μm, further preferably 80 to 300 μm, and especially preferably 120 to 260 μm, from the viewpoint of weather resistance.

[0109] (5) Specific Configuration of the Pressure-Sensitive Adhesive Sheet A specific configuration as an example of the pressure-sensitive adhesive sheet according to the present embodiment is shown in Figure 1. As shown in Figure 1, the pressure-sensitive adhesive sheet 1 according to one embodiment is composed of two release sheets 12a, 12b and a pressure-sensitive adhesive layer 11 sandwiched between the two release sheets 12a, 12b so as to be in contact with the release surfaces of the two release sheets 12a, 12b. Note that the release surface of the release sheet in this specification refers to the surface of the release sheet that has releasability, and includes both a surface that has been subjected to a release treatment and a surface that exhibits releasability even without being subjected to a release treatment.

[0110] The pressure-sensitive adhesive layer 11 is the pressure-sensitive adhesive layer in the pressure-sensitive adhesive sheet according to the above-described embodiment.

[0111] The release sheets 12a and 12b protect the adhesive layer until the adhesive sheet is used, and are peeled off when the adhesive sheet (adhesive layer) is to be used. In the adhesive sheet 1 according to this embodiment, one or both of the release sheets 12a and 12b are not necessarily required.

[0112] Examples of materials that can be used as the release sheets 12a and 12b include polyethylene films, polypropylene films, polybutene films, polybutadiene films, polymethylpentene films, polyvinyl chloride films, vinyl chloride copolymer films, polyethylene terephthalate films, polyethylene naphthalate films, polybutylene terephthalate films, polyurethane films, ethylene vinyl acetate films, ionomer resin films, ethylene-(meth)acrylic acid copolymer films, ethylene-(meth)acrylic acid ester polymer films, polystyrene films, polycarbonate films, polyimide films, and fluororesin films. Crosslinked films of these materials can also be used. Furthermore, laminated films of these materials may also be used. From the perspective of the SDGs, the material constituting the release sheets may be a material with a high biomass content, a recyclable or reusable material, or a recycled or reused material.

[0113] It is preferable that a release treatment be performed on the release surfaces of the release sheets 12 a and 12 b (particularly the surfaces that come into contact with the pressure-sensitive adhesive layer 11). Examples of release agents used for the release treatment include alkyd-based, silicone-based, fluorine-based, unsaturated polyester-based, polyolefin-based, and wax-based release agents.

[0114] There is no particular limitation on the thickness of the release sheets 12a and 12b, but it is usually about 20 to 150 μm.

[0115] From the viewpoint of handling, it is preferable that one of the two release sheets 12a, 12b be a heavy release type release sheet with a large release force and the other be a light release type release sheet with a small release force.

[0116] (6) Production of Pressure-Sensitive Adhesive Sheet In one example of producing the pressure-sensitive adhesive sheet 1, a coating solution of the pressure-sensitive adhesive composition P is applied to the release surface of one release sheet 12a (or 12b), and a heat treatment is carried out to thermally crosslink the pressure-sensitive adhesive composition P to form a coating layer, after which the release surface of the other release sheet 12b (or 12a) is superimposed on the coating layer. If a curing period is required, a curing period is allowed, but if no curing period is required, the coating layer becomes the pressure-sensitive adhesive layer 11 as is. The pressure-sensitive adhesive sheet 1 is obtained by the above steps. The conditions for the heat treatment and curing are as described above.

[0117] The coating solution of the pressure-sensitive adhesive composition P can be applied by, for example, bar coating, knife coating, roll coating, blade coating, die coating, gravure coating, or the like.

[0118] [Display Body] A display body according to one embodiment of the present invention includes one display body component, another display body component, and an adhesive layer that bonds the one display body component and the other display body component to each other. The adhesive layer is formed from the adhesive layer of the adhesive sheet according to the embodiment described above.

[0119] At least one of the one display member constituting member and the other display member constituting member may have a step at least on the surface on the side to be bonded by the pressure-sensitive adhesive layer.

[0120] Both the first display member and the second display member may be hard plates. When two hard plates are to be bonded together, since the hard plates are hard and inflexible, the adhesive layer is attached to one of the hard plates, and the two hard plates are pressed vertically to bring the adhesive layer into close contact with each other, thereby bonding the two hard plates together.

[0121] A display according to one embodiment of the present invention will be described with reference to the drawings. As shown in Fig. 2, the display 2 according to this embodiment is configured to include a first display component 21 (one display component), a second display component 22 (another display component), and a cured adhesive layer 11' located therebetween and bonding the first display component 21 and the second display component 22 to each other.

[0122] At least one of the first display body component 21 and the second display body component 22 may have a step on the surface that is bonded by the cured adhesive layer 11'. In the present embodiment shown in Figure 2, the first display body component 21 has a step due to the printing layer 3 or the like on the surface that faces the cured adhesive layer 11'.

[0123] The cured adhesive layer 11' in the display member 2 is obtained by curing the adhesive layer 11 of the adhesive sheet 1 described above by irradiating it with active energy rays.

[0124] Examples of the display 2 include a liquid crystal (LCD) display, a light-emitting diode (LED) display, an organic electroluminescence (OLED) display, and electronic paper, and may also be a touch panel. Note that LED displays also include those using mini LEDs and micro LEDs.

[0125] The first display member 21 is preferably a protective panel made of a glass plate, a plastic plate, or a laminate containing these. In this case, the printing layer 3 is generally formed in a frame shape on the side of the first display member 21 facing the cured adhesive layer 11′.

[0126] The glass plate is not particularly limited, and examples thereof include chemically strengthened glass, alkali-free glass, quartz glass, soda-lime glass, barium-strontium-containing glass, aluminosilicate glass, lead glass, borosilicate glass, barium borosilicate glass, etc. The thickness of the glass plate is not particularly limited, but is usually 0.1 to 5 mm, and preferably 0.2 to 2 mm.

[0127] The plastic plate is not particularly limited, and examples thereof include an acrylic plate, a polycarbonate plate, etc. The thickness of the plastic plate is not particularly limited, but is usually 0.2 to 5 mm, and preferably 0.4 to 3 mm.

[0128] On one or both sides of the glass plate or plastic plate, various functional layers (transparent conductive film, metal layer, silica layer, hard coat layer, anti-glare layer, etc.) may be provided, or optical members may be laminated. Furthermore, the transparent conductive film and metal layer may be patterned.

[0129] The second display component 22 is preferably an optical element to be attached to the first display component 21, a display module (e.g., a liquid crystal (LCD) module, a light-emitting diode (LED) module, an organic electroluminescence (organic EL) module, etc.), an optical element as part of a display module, or a laminate including a display module.

[0130] Examples of the optical member include a shatterproof film, a polarizing plate (polarizing film), a polarizer, a retardation plate (retardation film), a viewing angle compensation film, a brightness improvement film, a contrast improvement film, a liquid crystal polymer film, a diffusion film, a semi-transmitting reflective film, a transparent conductive film, etc. A preferred example of the transparent conductive film is an ITO-PET film in which a tin-doped indium oxide (ITO) layer is formed on one surface of a polyethylene terephthalate film.

[0131] The material constituting the printing layer 3 is not particularly limited, and known materials for printing can be used. The thickness of the printing layer 3, i.e., the height of the step, is preferably 0.5 to 50 μm, more preferably 1 to 30 μm, and particularly preferably 3 to 20 μm. When the thickness of the printing layer 3 is within the above range, the step-following ability of the cured pressure-sensitive adhesive layer 11′ is effectively exhibited, and the concealing property that is the purpose of the printing layer 3 can be sufficiently ensured. Note that the printing layer 3 is generally formed in a frame shape on the side of the cured pressure-sensitive adhesive layer 11′ of the display component.

[0132] To manufacture the display body 2, as an example, one of the release sheets 12a of the adhesive sheet 1 is peeled off, and the exposed adhesive layer 11 of the adhesive sheet 1 is attached to the surface of the first display body component 21 on which the printing layer 3 is present.

[0133] Next, the other release sheet 12b is peeled off from the adhesive layer 11 of the adhesive sheet 1, and the exposed adhesive layer 11 of the adhesive sheet 1 is bonded to the second display body component 22 to obtain a display body. As another example, the bonding order of the first display body component 21 and the second display body component 22 may be reversed.

[0134] After laminating the laminate of the first display body component 21 and the adhesive layer 11 to the second display body component 22, active energy rays are irradiated onto the adhesive layer 11 through the first display body component 21 and / or the second display body component 22 to harden the adhesive layer 11 to form a hardened adhesive layer 11'.

[0135] The active energy ray refers to an electromagnetic wave or a charged particle beam that has an energy quantum, and specific examples thereof include ultraviolet rays, electron beams, etc. Among active energy rays, ultraviolet rays are particularly preferred because they are easy to handle.

[0136] The ultraviolet irradiation can be performed using a high-pressure mercury lamp, a Heraeus H lamp, a xenon lamp, or the like, and the amount of ultraviolet irradiation is set to an illuminance of 50 to 1000 mW / cm. 2 The light intensity is preferably about 50 to 10,000 mJ / cm. 2 is preferably 80 to 5000 mJ / cm2 More preferably, it is 300 to 2000 mJ / cm 2 On the other hand, the electron beam irradiation can be carried out by an electron beam accelerator or the like, and the irradiation dose of the electron beam is preferably about 10 to 1000 krad.

[0137] In the above-mentioned display body 2, since the adhesive constituting the cured adhesive layer 11' has the physical properties described above, even when high-intensity ultraviolet light is irradiated for a long period of time (e.g., 20 hours, 40 hours, etc.), the occurrence of needle-shaped cracks in the cured adhesive layer 11' is suppressed, and the weather resistance is excellent.

[0138] The above-described embodiments have been described to facilitate understanding of the present invention, and are not intended to limit the present invention. Therefore, each element disclosed in the above embodiments is intended to include all design modifications and equivalents that fall within the technical scope of the present invention.

[0139] For example, one or both of the release sheets 12a and 12b in the pressure-sensitive adhesive sheet 1 may be omitted, or a desired optical member may be laminated in place of the release sheets 12a and / or 12b. The first display member 21 may have no steps. Furthermore, not only the first display member 21 but also the second display member 22 may have steps on the side of the pressure-sensitive adhesive layer 11' after curing.

[0140] In this specification, when it is stated that "X to Y" (X and Y are any numbers), it means "X or more and Y or less" unless otherwise specified, and also means "preferably greater than X" or "preferably smaller than Y". Furthermore, when it is stated that "X or more" (X is any number), it means "preferably greater than X" unless otherwise specified, and when it is stated that "Y or less" (Y is any number), it also means "preferably smaller than Y" unless otherwise specified.

[0141] The present invention will be explained in more detail below with reference to examples, but the scope of the present invention is not limited to these examples.

[0142] Example 1 1. Preparation of (meth)acrylic acid ester polymer 65 parts by mass of 2-ethylhexyl acrylate, 15 parts by mass of isobornyl acrylate, 5 parts by mass of N-acryloylmorpholine, and 15 parts by mass of 2-hydroxyethyl acrylate were copolymerized by solution polymerization to prepare a (meth)acrylic acid ester polymer (A). The molecular weight of this (meth)acrylic acid ester polymer (A) was measured by the method described below, and the weight average molecular weight (Mw) was found to be 500,000.

[0143] 2. Preparation of adhesive composition 100 parts by mass (solids equivalent value; the same applies hereinafter) of the (meth)acrylic acid ester polymer (A) obtained in step 1 above, 0.15 parts by mass of an isocyanate-based crosslinking agent (B1; manufactured by Mitsui Chemicals, Inc., product name "Takenate D-101E"), 5.2 parts by mass of ε-caprolactone-modified tris-(2-acryloxyethyl)isocyanurate (manufactured by Shin-Nakamura Chemical Co., Ltd., product name "NK Ester A-9300-1CL") as the active energy ray-curable component (C), 0.9 parts by mass of 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide (D1) as the photopolymerization initiator (D), and 0.27 parts by mass of 3-glycidoxypropyltrimethoxysilane as the silane coupling agent (E) were mixed, thoroughly stirred, and diluted with methyl ethyl ketone to obtain a coating solution of an adhesive composition.

[0144] Here, the formulations (solid content equivalent) of the pressure-sensitive adhesive compositions when the (meth)acrylic acid ester polymer (A) is taken as 100 parts by mass (solid content equivalent) are shown in Table 1. Details of the abbreviations and the like shown in Table 1 are as follows. [(Meth)acrylic acid ester polymer (A)] 2EHA: 2-ethylhexyl acrylate BA: n-butyl acrylate MMA: methyl methacrylate IBXA: isobornyl acrylate ACMO: N-acryloylmorpholine HEA: 2-hydroxyethyl acrylate AA: acrylic acid [Crosslinking agent (B)] B1: isocyanate-based crosslinking agent (manufactured by Mitsui Chemicals, Inc., product name "Takenate D-101E") B2: 1,3-bis(N,N'-diglycidylaminomethyl)cyclohexane (epoxy-based crosslinking agent) [Photopolymerization initiator (D)] D1: 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide D2: bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide D3: mixture of benzophenone and 1-hydroxycyclohexyl phenyl ketone (mass ratio 50:50) D4: 1-Hydroxycyclohexyl phenyl ketone D5: Mixture of 2-oxy-2-phenylacetic acid 2-(2-oxo-2-phenylacetoxyethoxy)ethyl ester and 2-oxy-2-phenylacetic acid 2-(2-hydroxyethoxy)ethyl ester (manufactured by IGM Resins, product name "OMNIRAD 754") [Light stabilizer] F1: Tetrakis(1,2,2,6,6-pentamethyl-4-piperidyl)-1,2,3,4-butanetetracarboxylate F2: Bis(1-undecanoxy-2,2,6,6-tetramethylpiperidin-4-yl)carbonate

[0145] 3. Production of Pressure-Sensitive Adhesive Sheet The coating solution of the pressure-sensitive adhesive composition obtained in step 2 above was applied using a coater to the release-treated surface of a heavy-release type release sheet R1, which had been prepared by treating one side of a polyethylene terephthalate film with a silicone-based release agent. A coating layer was then formed by heating at 90°C for 1 minute. The coating layer on the release sheet R1 obtained above was then attached to a light-release type release sheet R2, which had been prepared by treating one side of a polyethylene terephthalate film with a silicone-based release agent, so that the release-treated surface of the release sheet R2 was in contact with the coating layer. This was then cured for 7 days under conditions of 23°C and 50% RH to produce a pressure-sensitive adhesive sheet having a thickness of 50 μm, i.e., a pressure-sensitive adhesive sheet having a configuration of release sheet R1 / adhesive layer (thickness: 50 μm) / release sheet R2.

[0146] The thickness of the pressure-sensitive adhesive layer was measured using a constant pressure thickness measuring device (manufactured by Teclock Corporation, product name "PG-02") in accordance with JIS K 7130. It was also confirmed that the release strength of release sheet R1 was greater than that of release sheet R2 in the resulting pressure-sensitive adhesive sheet.

[0147] Examples 2 to 7, Comparative Examples 1 to 3 Pressure-sensitive adhesive sheets were produced in the same manner as in Example 1, except that the type and weight-average molecular weight (Mw) of each monomer constituting the (meth)acrylic acid ester polymer (A), the type and amount of crosslinking agent (B), the amount of active energy ray-curable component (C), and the type and amount of photopolymerization initiator (D) were changed as shown in Table 1. In Examples 3 and 4, light stabilizers (F1 / F2) were further added in the amounts shown in Table 1.

[0148] The weight average molecular weight (Mw) is a polystyrene-equivalent weight average molecular weight measured by gel permeation chromatography (GPC) under the following conditions (GPC measurement). <Measurement conditions> Measurement device: HLC-8320, manufactured by Tosoh Corporation GPC columns (passed in the following order): TSK gel super H-H, TSK gel super HM-H, TSK gel super H2000, manufactured by Tosoh Corporation Measurement solvent: tetrahydrofuran Measurement temperature: 40°C

[0149] [Test Example 1] (Measurement of gel fraction) A pressure-sensitive adhesive layer having a thickness of 250 μm was prepared by laminating multiple layers of the pressure-sensitive adhesive sheets produced in the Examples and Comparative Examples. The pressure-sensitive adhesive layer (thickness: 250 μm) was cut into a size of 70 mm × 150 mm, and the pressure-sensitive adhesive layer was wrapped in a polyester mesh (mesh size 200). The mass was measured using a precision balance, and the mass of the mesh alone was subtracted to calculate the mass of the pressure-sensitive adhesive alone. This mass was designated M1.

[0150] Next, the adhesive wrapped in the polyester mesh was immersed in ethyl acetate at room temperature (23°C) for 24 hours. The adhesive was then removed and air-dried for 24 hours in an environment of 23°C and 50% RH, and then further dried in an oven at 80°C for 12 hours. After drying, the mass was weighed using a precision balance, and the mass of the mesh alone was subtracted to calculate the mass of the adhesive alone. This mass was designated M2. The gel fraction (%; before UV) was expressed as (M2 / M1) x 100. The results are shown in Table 2.

[0151] Furthermore, a 250 μm thick adhesive layer was prepared by laminating multiple adhesive layers of the adhesive sheets produced in the Examples and Comparative Examples. The adhesive layer (thickness: 250 μm) was irradiated with active energy rays (ultraviolet rays; UV) to cure the adhesive layer. The gel fraction (%; after UV) of the adhesive in the adhesive layer after curing with the active energy rays was measured in the same manner as above. The results are shown in Table 2. The irradiation conditions for the active energy rays were as follows:

[0152] <Activated energy ray irradiation conditions> - High pressure mercury lamp used - Illuminance: 200 mW / cm 2 , Light amount: 1000mJ / cm 2 ・UV illuminance and light intensity meter used is "UVPF-A1" manufactured by Eye Graphics

[0153] Furthermore, a 250 μm thick adhesive layer was prepared by laminating multiple adhesive layers from the adhesive sheets produced in the Examples and Comparative Examples. This adhesive layer (thickness: 250 μm) was used to bond two soda-lime glass plates (manufactured by Nippon Sheet Glass Co., Ltd., thickness: 1.1 mm, length: 70 mm × width: 150 mm) to prepare a laminate (soda-lime glass plate / adhesive layer (250 μm) / soda-lime glass plate). The laminate was irradiated with active energy rays (ultraviolet rays; UV) under the active energy ray irradiation conditions described above to cure the adhesive layer. Next, the laminate including the active energy ray-cured adhesive layer was irradiated with ultraviolet rays under the following conditions (S-UV irradiation). The adhesive layer was then separated from the two soda-lime glass plates in the laminate after S-UV irradiation. The gel fraction (%; after S-UV) of the adhesive in the separated adhesive layer was measured in the same manner as described above. The results are shown in Table 2.

[0154] <Ultraviolet light irradiation conditions> Device: Eye Super UV Tester SUV-W151 (manufactured by Iwasaki Electric Co., Ltd.) UV lamp: ME06-L31WX / SUV (manufactured by Iwasaki Electric Co., Ltd.) Water-cooled jacket: WJ50-SUV-4 (manufactured by Iwasaki Electric Co., Ltd.) Illuminance: 100 mW / cm 2 Irradiation time: 120 hours Light intensity: 43.2 kJ / cm 2 Temperature: 63°C Humidity: 70% RH Temperature and humidity control: Closed circulation method

[0155] Test Example 2 (Measurement of the Average Peak Molecular Weight of the Sol Fraction) A 250 μm thick adhesive layer was prepared by laminating multiple adhesive layers from the adhesive sheets produced in the Examples and Comparative Examples. The adhesive layer was irradiated with active energy rays (ultraviolet rays; UV) under the same active energy ray irradiation conditions as in Test Example 1, thereby curing the adhesive layer. Ethyl acetate (after immersion in the adhesive and removal), obtained in the same manner as in Test Example 1, was concentrated in an evaporator to obtain a sol fraction. The sol fraction was then diluted with tetrahydrofuran to a 0.3% by mass solution, filtered through a 0.45 μm filter, and the average peak molecular weight (Mp; before S-UV) of the sol fraction was measured by GPC measurement. The GPC measurement conditions were as described above. The results are shown in Table 2.

[0156] Furthermore, the same laminate as in Test Example 1 was produced using the pressure-sensitive adhesive sheets produced in the Examples and Comparative Examples. The laminate was irradiated with active energy rays (ultraviolet rays; UV) under the same active energy ray irradiation conditions as in Test Example 1, thereby curing the pressure-sensitive adhesive layer. Next, the laminate including the active energy ray-cured pressure-sensitive adhesive layer was irradiated with ultraviolet rays under the same ultraviolet irradiation conditions as in Test Example 1 (S-UV irradiation). The pressure-sensitive adhesive layer was then separated from the two soda-lime glass plates in the laminate after S-UV irradiation. The average peak molecular weight (Mp; after S-UV) of the sol content of the pressure-sensitive adhesive in the separated pressure-sensitive adhesive layer was measured in the same manner as above. The results are shown in Table 2.

[0157] [Test Example 3] (Measurement of dynamic viscoelasticity) A 250 μm thick adhesive layer was produced by laminating multiple adhesive layers of the adhesive sheets produced in the Examples and Comparative Examples. The adhesive layer was irradiated with active energy rays (ultraviolet rays; UV) under the same active energy ray irradiation conditions as in Test Example 1, and the adhesive layer was cured. A cylindrical body with a diameter of 8 mm (height 0.25 mm) was punched out from the adhesive layer after curing with active energy rays, and this was used as a sample.

[0158] The dynamic viscoelasticity of the above sample was measured in accordance with JIS K7244-1 using a viscoelasticity measuring device (manufactured by Anton Paar, product name "MCR302") by the torsional shear method under the following conditions, and the storage modulus G'(-15) (MPa; before S-UV) at -15°C, the storage modulus G'(23) (MPa; before S-UV) at 23°C, and the storage modulus G'(100) (MPa; before S-UV) at 100°C were calculated. In addition, the peak temperature (°C) of the loss tangent tanδ (before S-UV: Tb) was calculated. The results are shown in Table 2. Measurement frequency: 1 Hz Measurement temperature range: -20°C to 140°C Heating rate: 4°C / min

[0159] Furthermore, a laminate similar to that in Test Example 1 was produced using the pressure-sensitive adhesive sheets produced in the Examples and Comparative Examples. The laminate was irradiated with active energy rays (ultraviolet rays; UV) under the same active energy ray irradiation conditions as in Test Example 1, thereby curing the pressure-sensitive adhesive layer. Next, the laminate including the active energy ray-cured pressure-sensitive adhesive layer was irradiated with ultraviolet rays under the same ultraviolet irradiation conditions as in Test Example 1 (S-UV irradiation). The pressure-sensitive adhesive layer was then separated from the two soda-lime glass plates in the laminate after S-UV irradiation. The dynamic viscoelasticity of the separated pressure-sensitive adhesive layer was measured in the same manner as above, and the storage modulus G'(-15) at -15°C (MPa; after S-UV), the storage modulus G'(23) at 23°C (MPa; after S-UV), and the storage modulus G'(100) at 100°C (MPa; after S-UV) were calculated. The peak temperature (°C) of the loss tangent tanδ (after S-UV: Ta) was also calculated. The results are shown in Table 2.

[0160] Furthermore, the value (Ta - Tb) was calculated by subtracting Tb from Ta obtained above. The results are shown in Table 2.

[0161] [Test Example 4] (Measurement of adhesive strength) The release sheet R2 was peeled off from the pressure-sensitive adhesive sheets produced in the Examples and Comparative Examples, and the exposed pressure-sensitive adhesive layer was attached to one side of a polyethylene terephthalate (PET) film (manufactured by Toyobo Co., Ltd., product name "Cosmoshine A4360", thickness: 100 μm) having easy-adhesion layers on both sides, to obtain a release sheet R1 / adhesive layer / PET film laminate. The laminate was cut into a 25 mm wide, 100 mm long sample.

[0162] The release sheet R1 was peeled off from the sample in an environment of 23°C and 50% RH, and the exposed pressure-sensitive adhesive layer was attached to soda lime glass (manufactured by Nippon Sheet Glass Co., Ltd.), and then pressurized for 20 minutes at 0.5 MPa and 50°C in an autoclave manufactured by Kurihara Manufacturing Co., Ltd. Then, active energy rays (ultraviolet rays; UV) were irradiated through the soda lime glass under the same active energy ray irradiation conditions as in Test Example 1, to cure the pressure-sensitive adhesive layer.

[0163] After that, the adhesive strength (N / 25 mm) was measured using a tensile tester (Tensilon, manufactured by Orientec Co., Ltd.) at a peel speed of 300 mm / min and a peel angle of 180 degrees. The measurement was conducted under conditions other than those described here in accordance with JIS Z0237:2009. The results are shown in Table 2.

[0164] [Test Example 5] (Measurement of Total Light Transmittance) A 250 μm thick pressure-sensitive adhesive layer was prepared by laminating multiple pressure-sensitive adhesive layers from the pressure-sensitive adhesive sheets produced in the Examples and Comparative Examples. A laminate was prepared using this pressure-sensitive adhesive layer (thickness: 250 μm) in the same manner as in Test Example 1. The laminate was irradiated with active energy rays (ultraviolet rays; UV) under the same active energy ray irradiation conditions as in Test Example 1 to cure the pressure-sensitive adhesive layer, which was used as a measurement sample. After background measurement using soda-lime glass, the measurement sample was measured for total light transmittance (%; before S-UV) using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., product name "NDH-5000") in accordance with JIS K7361-1:1997. The results are shown in Table 2. The total light transmittance of the pressure-sensitive adhesive layer before curing with active energy rays was also measured, yielding similar results.

[0165] Test Example 6 (Haze Value Measurement) A measurement sample was prepared in the same manner as in Test Example 5. After background measurement was performed on the measurement sample using glass, the haze value (%; before S-UV) was measured using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., product name "NDH-5000") in accordance with JIS K7136:2000. The results are shown in Table 2. The haze value of the pressure-sensitive adhesive layer before curing with active energy rays was also measured, and the same measurement result was obtained.

[0166] [Test Example 7] (Measurement of L*a*b*) The same laminate as in Test Example 1 was produced using the pressure-sensitive adhesive sheets produced in the Examples and Comparative Examples. The laminate was irradiated with active energy rays (ultraviolet rays; UV) under the same active energy ray irradiation conditions as in Test Example 1 to cure the pressure-sensitive adhesive layer. The pressure-sensitive adhesive layer after the active energy ray irradiation was measured for chromaticity b* (chromaticity b*1) defined by the CIE 1976 L*a*b* color system using a simultaneous photometric spectrophotometer colorimeter (manufactured by Nippon Denshoku Industries Co., Ltd., product name "SQ2000"). The results are shown in Table 2.

[0167] Furthermore, the same laminate as in Test Example 1 was produced using the pressure-sensitive adhesive sheets produced in the Examples and Comparative Examples. The laminate was irradiated with active energy rays (ultraviolet rays; UV) under the same active energy ray irradiation conditions as in Test Example 1, thereby curing the pressure-sensitive adhesive layer. Next, the laminate including the active energy ray-cured pressure-sensitive adhesive layer was irradiated with ultraviolet rays under the same ultraviolet irradiation conditions as in Test Example 1 (S-UV irradiation). Then, the chromaticity b* (chromaticity b*2) of the pressure-sensitive adhesive layer in the laminate after S-UV irradiation was measured in the same manner as above. The results are shown in Table 2.

[0168] Furthermore, the absolute value of the ratio (b*2 / b*1) of the chromaticity b*2 to the chromaticity b*1 obtained above was calculated. The results are shown in Table 2.

[0169] [Test Example 8] (Evaluation of Weather Resistance) The same laminate as in Test Example 1 was produced using the pressure-sensitive adhesive layers of the pressure-sensitive adhesive sheets produced in the Examples and Comparative Examples. The laminate was irradiated with active energy rays (ultraviolet rays; UV) under the same active energy ray irradiation conditions as in Test Example 1 to cure the pressure-sensitive adhesive layer. Next, the active energy ray-cured pressure-sensitive adhesive layer was irradiated with ultraviolet rays for 20 hours (light amount: 7.2 kJ / cm 2 ) and 40 hours (light intensity: 14.4 kJ / cm 2 The adhesive layer was then visually inspected and its weather resistance was evaluated based on the following criteria. The results are shown in Table 2. ⊚: No needle-like cracks occurred, and no bubbles, lifting, or peeling occurred. ◯: No needle-like cracks occurred, but some bubbles occurred. ×: Needle-like cracks occurred.

[0170] Test Example 9 (Evaluation of Blister Resistance) The release sheet R2 was peeled off from the pressure-sensitive adhesive sheets produced in the Examples and Comparative Examples, and the exposed pressure-sensitive adhesive layer was bonded to the PC plate side of a plastic plate (manufactured by Mitsubishi Gas Chemical Company, Inc., product name "Iupilon Sheet MR58U", thickness: 0.7 mm) consisting of a polycarbonate (PC) plate and a polymethyl methacrylate (PMMA) layer laminated thereon. The release sheet R1 was then peeled off from the pressure-sensitive adhesive layer to expose the pressure-sensitive adhesive layer, and a transparent conductive film (manufactured by Oike Kogyo Co., Ltd., laminate of a PET film and an ITO layer (ITO-PET film), total thickness 125 μm) was bonded to the pressure-sensitive adhesive layer so that the ITO layer side was in contact with the pressure-sensitive adhesive layer. The sheet was then autoclaved for 20 minutes at 50°C and 0.5 MPa.

[0171] The pressure-sensitive adhesive layer of the obtained laminate was cured by irradiating it with active energy rays (ultraviolet rays; UV) through the transparent conductive film under the same conditions as in Test Example 1. Thereafter, the laminate was left to stand at normal pressure, 23°C, and 50% RH for 24 hours, and this was used as a sample.

[0172] The obtained sample was stored under high temperature and high humidity conditions of 85°C and 85% RH for 72 hours. Thereafter, the condition of the interface between the pressure-sensitive adhesive layer and the adherend (plastic plate) was visually inspected, and blister resistance was evaluated according to the following criteria. The results are shown in Table 2. ○: No bubbles, lifting, or peeling occurred. △: Bubbles less than 1 mm in diameter occurred, but no lifting or peeling occurred. ×: Bubbles, lifting, or peeling occurred throughout the sample.

[0173]

[0174]

[0175] As can be seen from Table 2, the adhesive sheets produced in the examples were able to suppress the occurrence of needle-shaped cracks even when exposed to high-intensity ultraviolet light for long periods of time (20 hours / 40 hours), and had excellent weather resistance.

[0176] The pressure-sensitive adhesive sheet of the present invention can be suitably used, for example, in the production of a display, for bonding a display component such as a protective panel to a desired display component.

[0177] DESCRIPTION OF SYMBOLS 1... Adhesive sheet 11... Adhesive layer 12a, 12b... Release sheets 2... Display body 11'... Post-cured adhesive layer 21... First display body constituent member 22... Second display body constituent member 3... Printed layer

Claims

1. An adhesive sheet having an adhesive layer for bonding two display component members to each other, wherein the adhesive constituting the adhesive layer is an active energy ray curable adhesive, the peak temperature of the loss tangent tan δ of the adhesive constituting the adhesive layer after active energy ray curing is Tb (°C), and the illuminance of the adhesive layer after active energy ray curing is 100 mW / cm 2 a peak temperature of a loss tangent tanδ of the adhesive constituting the adhesive layer after irradiation with ultraviolet light of 100 nm for 120 hours, where Ta (°C) is a value obtained by subtracting Tb from Ta, and the value is greater than 3.

2. The adhesive sheet according to claim 1, characterized in that the gel fraction of the adhesive constituting the adhesive layer is 20% or more and 85% or less.

3. The adhesive sheet according to claim 1, characterized in that the gel fraction of the adhesive constituting the adhesive layer after curing with active energy rays is 30% or more and 95% or less.

4. Illuminance of the adhesive layer after curing with active energy rays is 100 mW / cm 2 2. The pressure-sensitive adhesive sheet according to claim 1, wherein the gel fraction of the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer after irradiation with ultraviolet light of 100 nm for 120 hours is 40% or more and 99% or less.

5. The adhesive sheet according to claim 1, characterized in that the average peak molecular weight of the sol component of the adhesive constituting the adhesive layer after curing with active energy rays is 10,000 or more and 250,000 or less.

6. Illuminance of the adhesive layer after curing with active energy rays is 100 mW / cm 2 2. The pressure-sensitive adhesive sheet according to claim 1, characterized in that after being irradiated with ultraviolet light of 10,000 for 120 hours, the average peak molecular weight of the sol component of the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer is 10,000 or more and 200,000 or less.

7. The adhesive sheet according to claim 1, characterized in that the storage modulus G' of the adhesive constituting the adhesive layer at 23°C after curing with active energy rays is 0.01 MPa or more and 2 MPa or less.

8. Illuminance of the adhesive layer after curing with active energy rays is 100 mW / cm 2 2. The pressure-sensitive adhesive sheet according to claim 1, wherein the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer has a storage modulus G' at 23°C of 0.01 MPa or more and 2 MPa or less after being irradiated with ultraviolet light of 1000 nm for 120 hours.

9. The pressure-sensitive adhesive sheet according to claim 1, wherein the storage modulus G' of the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer at -15°C after curing with active energy rays is 0.01 MPa or more and 100 MPa or less.

10. Illuminance of the adhesive layer after curing with active energy rays is 100 mW / cm 2 2. The pressure-sensitive adhesive sheet according to claim 1, wherein the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer has a storage modulus G' at -15°C of 0.1 MPa or more and 1000 MPa or less after being irradiated with ultraviolet light of 1000 nm for 120 hours.

11. The adhesive sheet according to claim 1, characterized in that the storage modulus G' of the adhesive constituting the adhesive layer at 100°C after curing with active energy rays is 0.0001 MPa or more and 1 MPa or less.

12. Illuminance of the adhesive layer after curing with active energy rays is 100 mW / cm 2 2. The pressure-sensitive adhesive sheet according to claim 1, wherein the pressure-sensitive adhesive layer has a storage modulus G' at 100°C of 0.0001 MPa or more and 1 MPa or less after being irradiated with ultraviolet light of 100°C for 120 hours.

13. The adhesive sheet according to claim 1, wherein the adhesive is an acrylic adhesive.

14. The adhesive sheet according to claim 1, characterized in that the adhesive sheet comprises two release sheets, and the adhesive layer is sandwiched between the release sheets so as to be in contact with the release surfaces of the two release sheets.

15. A display comprising: one display component; another display component; and an adhesive layer for bonding said one display component and said other display component to each other, wherein said adhesive layer is formed from an adhesive layer of an adhesive sheet according to any one of claims 1 to 14.

16. The display according to claim 15, wherein both the one display member and the other display member are hard plates.

Citation Information

Patent Citations

  • Adhesive sheet and laminate

    JP2015010197A

  • Adhesive sheet, display body and manufacturing method therefor

    JP2017149807A

  • Adhesive sheet and display body

    JP2019035061A

  • Constituent and method for manufacturing the same, display body, and adhesive sheet for optical use

    JP2019042965A

  • Adhesive sheet, display body and method for manufacturing display body

    JP2019044023A

Cited By

  • Adhesive, adhesive sheet, optical structure, and display body

    JPWO2025203862A1