Light-absorbing anisotropic film, laminate, compound lens, and virtual reality display device

A light-absorbing anisotropic film with a curved surface and dichroic substance array structure addresses ghosting in virtual reality display devices by controlling transmittance, improving display quality.

WO2024202820A1PCT designated stage expired Publication Date: 2024-10-03FUJIFILM CORP

Patent Information

Application Number
PCT/JP2024/007019
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-02-27
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Ghosting occurs when a laminated optical film is applied to a pancake lens type virtual reality display device, necessitating a solution to suppress this issue.

Method used

A light-absorbing anisotropic film with a curved surface, specific transmittance characteristics, and a dichroic substance array structure is developed, which satisfies certain transmittance and structural requirements to prevent ghosting when applied to a pancake lens type virtual reality display device.

Benefits of technology

The light-absorbing anisotropic film effectively suppresses ghosting in virtual reality display devices by ensuring the absolute difference in transmittance at specific locations is within a specified range, enhancing the display quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024007019_03102024_PF_FP_ABST
    Figure JP2024007019_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention addresses the problem of providing a light-absorbing anisotropic film that, when applied to a pancake lens-type virtual reality display device, suppresses the occurrence of ghosting. This light-absorbing anisotropic film includes a curved surface section, wherein transmittance, as measured by a prescribed procedure, satisfies formula (1). Formula (1): ΔT 1 =|T 11 -T 12 |≦ 2.5%.
Need to check novelty before this filing date? Find Prior Art

Description

Optically absorbing anisotropic film, laminate, composite lens and virtual reality display device

[0001] The present invention relates to an optically absorbing anisotropic film, a laminate, a composite lens, and a virtual reality display device.

[0002] A virtual reality display device is a display device that allows a user to feel as if they are immersed in a virtual world by wearing a dedicated headset on their head and viewing images displayed through lenses. A proposed configuration for virtual reality display devices is called a pancake lens, which includes an image display device, a reflective polarizer, a half mirror, and a retardation layer, and reduces the overall thickness of the headset by directing light emitted from the image display device back and forth between the reflective polarizer and the half mirror.

[0003] Patent Document 1 discloses a laminated optical film having, in this order, a reflective circular polarizer, a retardation layer that converts circularly polarized light into linearly polarized light, and a linear polarizer, and describes that this laminated optical film can be applied to a pancake lens-type virtual reality display device.

[0004] International Publication No. 2022 / 075475

[0005] As described in Patent Document 1, when a laminated optical film is applied to a virtual reality display device, the laminated optical film may be formed into a non-planar shape such as a curved shape to match the shape of a lens, etc. The present inventors have found that when a laminated optical film such as that described in Patent Document 1 is formed into a curved shape and applied to a pancake lens type virtual reality display device, the occurrence of ghosts is observed and it is necessary to suppress this.

[0006] In view of the above, an object of the present invention is to provide an optically absorbing anisotropic film that suppresses the occurrence of ghosts when applied to a pancake lens-type virtual reality display device. Another object of the present invention is to provide a laminate, a composite lens, and a virtual reality display device.

[0007] As a result of extensive research into achieving the above object, the inventors discovered that an optically absorbing anisotropic film in which the absolute value of the difference in transmittance between multiple specific locations is 2.5% or less can suppress the occurrence of ghosts when applied to a pancake lens type virtual reality display device, and thus completed the present invention. That is, the inventors discovered that the above object can be achieved by the following configuration.

[0008] [1] An optically absorptive anisotropic film having a curved surface, wherein the transmittance measured by the following procedure satisfies the formula (1) described below. Step 1: The optically absorptive anisotropic film is orthogonally projected to identify the maximum projected image with the largest area. 2: A circle X having the smallest area and including all of the maximum projected images of the optically absorptive anisotropic film is drawn with its center at the center of gravity of the maximum projected images of the optically absorptive anisotropic film. 3: A circle Y having a radius half the radius of the circle X is drawn with its center at the center of gravity of the maximum projected images of the optically absorptive anisotropic film. 4: The transmittance T at the intersection G of the optically absorptive anisotropic film and a line passing through the center of gravity of the maximum projected images of the optically absorptive anisotropic film and extending in the normal direction of the maximum projected images is determined. 11 5: The transmittance is measured at each intersection of the optically absorptive anisotropic film and each line passing through any four points on the circle Y and extending in the normal direction of the maximum projected image. 11 The transmittance T where the absolute value of the difference between 12 Here, the transmittance T 12 The point where the transmittance is measured is designated as intersection A. [2] Regarding the transmittance at intersection G, the transmittance before heating at 120°C for 10 minutes is designated as T 21 and the transmittance after heating is T 22 [3] The light absorption anisotropy film according to [1], wherein when the lightness at the intersection G is L 11 * and the chromaticity is a 11 * and b 11 * The lightness at the intersection point A is L 12 * and the chromaticity is a 12 * and b 12 *The optically absorptive anisotropic film according to [1] or [2], which satisfies formula (3) below when the content of the dichroic substance is 230 mg / cm. [4] The optically absorptive anisotropic film according to any one of [1] to [3], further comprising a dichroic substance. [5] The optically absorptive anisotropic film according to [4], in which at least a part of the dichroic substance forms an ordered structure. [6] The optically absorptive anisotropic film according to [5], in which, when 100 ordered structures present in a cross section of the optically absorptive anisotropic film observed with a scanning transmission electron microscope are selected, the number of ordered structures having a major axis length of less than 50 nm is 30 or less. [7] The content of the dichroic substance is 230 mg / cm. 3 The optically absorptive anisotropic film according to any one of [4] to [6], wherein the optically absorptive anisotropic film is a film obtained by fixing the alignment state of a liquid crystal composition containing a liquid crystal compound, and wherein the Log P value of the liquid crystal compound is 6 or less. Here, when the liquid crystal composition contains multiple types of liquid crystal compounds, the Log P value of the liquid crystal compound refers to the largest Log P value among the Log P values ​​of the various liquid crystal compounds. [9] A laminate comprising the optically absorptive anisotropic film according to any one of [1] to [8].

[10] The laminate according to [9], which has an optically absorptive anisotropic film, a retardation layer, and a reflective polarizer layer.

[11] A composite lens having the laminate according to [9], a lens, and a half mirror, in this order.

[12] A virtual reality display device comprising the laminate according to [9].

[0009] According to the present invention, it is possible to provide an optically absorbing anisotropic film that suppresses the occurrence of ghosts when applied to a pancake lens type virtual reality display device. According to the present invention, it is possible to provide a laminate, a composite lens, and a virtual reality display device.

[0010] FIG. 1 is a top view showing an example of an optically absorptive anisotropic film of the present invention. FIG. 2 is a cross-sectional view taken along line A-A in FIG. 1. FIG. 3 is a diagram illustrating a procedure for measuring transmittance. FIG. 4 is a diagram illustrating a procedure for molding a film using a mold having a concave molding surface. FIG. 5 is a diagram illustrating a procedure for molding a film using a mold having a concave molding surface. FIG. 6 is a top view of a film used for molding. FIG. 7 is a diagram illustrating a procedure for molding a film using a mold having a convex molding surface. FIG. 8 is a diagram illustrating a procedure for molding a film using a mold having a convex molding surface. FIG. 9 is a cross-sectional view showing an example of a laminate of the present invention. FIG. 10 is a cross-sectional view showing another example of a laminate of the present invention. FIG. 11 is a cross-sectional view showing an example of a composite lens of the present invention. FIG. 12 is a diagram illustrating an example of a virtual reality display device of the present invention, showing an example of light rays of a main image.

[0011] The present invention will be described in detail below. The following description of the constituent elements may be based on representative embodiments and specific examples, but the present invention is not limited to such embodiments. In this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the upper and lower limits. In this specification, the upper or lower limit of a numerical range described in stages may be replaced with the upper or lower limit of another numerical range described in stages. In this specification, the upper or lower limit of a numerical range described in stages may be replaced with a value shown in the Examples. In this specification, each component may be a single substance corresponding to the component, or two or more substances may be used in combination. When two or more substances are used in combination for each component, the content of that component refers to the total content of the substances used in combination, unless otherwise specified. In this specification, "(meth)acrylic" refers to "acrylic" or "methacrylic."

[0012] In this specification, the term "transmittance" refers to the average transmittance in the wavelength range of 380 to 780 nm.

[0013] In this specification, "absorption axis" refers to the polarization direction in which absorbance is maximized in a plane when linearly polarized light is incident. "Reflection axis" refers to the polarization direction in which reflectance is maximized in a plane when linearly polarized light is incident. "Transmission axis" refers to the direction perpendicular to the absorption axis or reflection axis in a plane. "Slow axis" refers to the direction in which refractive index is maximized in a plane.

[0014] In this specification, Re(λ) and Rth(λ) represent the in-plane retardation and the thickness retardation, respectively, at a wavelength λ. Unless otherwise specified, the wavelength λ is 550 nm. In the present invention, Re(λ) and Rth(λ) are values ​​measured at a wavelength λ using an AxoScan (manufactured by Axometrics). By inputting the average refractive index ((nx + ny + nz) / 3) and film thickness (d (μm)) into AxoScan, the following slow axis direction (°) is calculated: Re(λ) = R0(λ) Rth(λ) = ((nx + ny) / 2 - nz) × d. Note that R0(λ) is displayed as a numerical value calculated by AxoScan, but it means Re(λ).

[0015] In this specification, the refractive indices nx, ny, and nz are measured using an Abbe refractometer (NAR-4T, manufactured by Atago Co., Ltd.) with a sodium lamp (λ = 589 nm) as a light source. When measuring wavelength dependency, measurements can be made using a multi-wavelength Abbe refractometer DR-M2 (manufactured by Atago Co., Ltd.) in combination with an interference filter. Values ​​from the Polymer Handbook (John Wiley & Sons, Inc.) and catalogs of various optical films can also be used. Examples of average refractive index values ​​for major optical films are listed below: cellulose acylate (1.48), cycloolefin polymer (1.52), polycarbonate (1.59), polymethyl methacrylate (1.49), and polystyrene (1.59).

[0016] In this specification, A plates and C plates are defined as follows. There are two types of A plates: positive A plates (positive A plates) and negative A plates (negative A plates). When the refractive index in the in-plane slow axis direction (the direction in which the in-plane refractive index is maximum) of the film is nx, the refractive index in the in-plane direction perpendicular to the in-plane slow axis is ny, and the refractive index in the thickness direction is nz, the positive A plates satisfy the relationship of formula (A1), and the negative A plates satisfy the relationship of formula (A2). Note that the positive A plates have a positive Rth value, and the negative A plates have a negative Rth value. Formula (A1) nx>ny≒nz Formula (A2) ny<nx≒nz Note that the above "≒" includes not only the case where the two are completely identical, but also the case where the two are substantially identical. "Substantially the same" means, for example, that "ny ≒ nz" also includes cases where (ny - nz) x d (where d is the film thickness) is -10 to 10 nm, preferably -5 to 5 nm, and "nx ≒ nz" also includes cases where (nx - nz) x d is -10 to 10 nm, preferably -5 to 5 nm. There are two types of C plates: positive C plates (positive C plates) and negative C plates (negative C plates). Positive C plates satisfy the relationship of formula (C1), while negative C plates satisfy the relationship of formula (C2). Note that positive C plates have a negative Rth value, and negative C plates have a positive Rth value. Formula (C1) nz > nx ≒ ny Formula (C2) nz < nx ≒ ny Note that the above "≒" includes not only cases where the two are completely identical, but also cases where the two are substantially identical. The term "substantially the same" includes, for example, the case where (nx-ny) x d (where d is the thickness of the film) is 0 to 10 nm, preferably 0 to 5 nm, in "nx≈ny".

[0017] [Light-absorption anisotropic film] The light-absorption anisotropic film of the present invention has a curved surface portion, and the transmittance measured by the procedure described below satisfies the formula (1) described below. Furthermore, the light-absorption anisotropic film of the present invention is a film having absorption anisotropy, and it is preferable that the absorption anisotropy is in the in-plane direction of the light-absorption anisotropic film. In particular, it is preferable that the light-absorption anisotropic film functions as an absorptive linear polarizer.

[0018] [Curved Surface Portion] The optically absorptive anisotropic film of the present invention has a curved surface portion. Here, the term "curved surface portion" refers to a portion having a curved shape. The term "curved surface shape" refers to a shape having a curvature greater than zero, and includes a developable curved surface shape and a three-dimensional curved surface shape. The radius of curvature of a shape having a curvature is preferably 10 mm to 120 mm, more preferably 15 to 90 mm. A developable surface refers to a surface that can be developed into a plane without expanding or contracting each part of the surface. Examples of developable curved surfaces include surfaces corresponding to the circumferential surfaces of a cylinder, an elliptical cylinder, a cone, and an elliptical cone, and may be either a convex or concave curved surface. A three-dimensional curved surface refers to a curved surface that cannot be formed by deformation of a plane, i.e., a curved surface that is not developable. Examples of three-dimensional curved surfaces include surfaces corresponding to a sphere or a spheroid, and surfaces corresponding to a curved surface whose cross section is a parabola or hyperbola (e.g., a paraboloid of revolution), and may be either a convex or concave curved surface.

[0019] The curved surface shape of the curved surface portion is preferably a lens shape. Examples of the lens shape include a spherical shape and a spheroidal shape, and the shape may be a convex lens shape or a concave lens shape.

[0020] FIG. 1 shows an example of an optically absorptive anisotropic film of the present invention. FIG. 1 is a top view of the optically absorptive anisotropic film, and FIG. 2 is a cross-sectional view taken along line A-A in FIG. 1. As shown in FIGS. 1 and 2, the optically absorptive anisotropic film 10 has a curved shape. More specifically, as shown in FIG. 2, the optically absorptive anisotropic film 10 has a shape (convex shape) that is convexly curved toward the upper side of the paper. In other words, the optically absorptive anisotropic film 10 has a convex shape that protrudes toward one surface. It can also be said that the optically absorptive anisotropic film 10 has a concave shape that is concave toward the other surface. While FIG. 1 shows an embodiment in which the shape of the optically absorptive anisotropic film when viewed in plan is pentagonal, the present invention is not limited to this embodiment, and the shape of the optically absorptive anisotropic film when viewed in plan may be rectangular, circular, or another shape.

[0021] [Transmittance] The optically absorptive anisotropic film of the present invention has a transmittance measured by the following procedure that satisfies the following formula (1): Step 1: The optically absorptive anisotropic film is orthogonally projected, and the maximum projected image with the largest area is identified. Step 2: A circle X having the smallest area and including all of the maximum projected images of the optically absorptive anisotropic film is drawn with its center at the center of gravity of the maximum projected images of the optically absorptive anisotropic film. Step 3: A circle Y having a radius half the radius of circle X is drawn with its center at the center of gravity of the maximum projected images of the optically absorptive anisotropic film. Step 4: The transmittance T at the intersection G of the optically absorptive anisotropic film and a line passing through the center of gravity of the maximum projected images of the optically absorptive anisotropic film and extending in the normal direction of the maximum projected images is calculated. 11 5: The transmittance is measured at each intersection of the optically absorptive anisotropic film and each line passing through any four points on the circle Y and extending in the normal direction of the maximum projected image. 11 The transmittance T where the absolute value of the difference between 12 Here, the transmittance T 12 The point where ΔT is measured is defined as intersection point A. 1 = |T 11 -T 12 | ≦ 2.5%

[0022] The procedure for measuring transmittance will be described using Figure 3. The maximum projection image in Procedure 1 is the largest projected image among the orthogonal projection images of the optically absorptive anisotropic film 10 shown in Figure 1, as shown in maximum projection image 1 in Figure 3. Furthermore, circle X in Procedure 2 is the smallest circle that contains the entire maximum projection image 1, among the circles centered on the center of gravity 4 of the maximum projection image 1, as shown in circle X2 in Figure 3. Furthermore, circle Y in Procedure 3 is a circle with a radius half the radius of circle X2, as shown in circle Y3 in Figure 3. Furthermore, intersection point G in Procedure 4 refers to the point on the optically absorptive anisotropic film corresponding to the position of the center of gravity 4 of the maximum projection image 1, i.e., the intersection point between the optically absorptive anisotropic film and a line that passes through the center of gravity 4 of the maximum projection image 1 and extends toward the normal direction of the maximum projection image 1. The intersections in step 5 refer to the intersections of the optically absorptive anisotropic film with the lines that pass through any four points Z on the circle Y2 and extend in the normal direction of the maximum projected image 1.

[0023] The transmittance can be calculated in the wavelength range of 380 to 780 nm using a spectrophotometer (VAP-7070 manufactured by JASCO Corporation).

[0024] In the present invention, the transmittance T 11 and transmittance T 12 The absolute value of the difference between 1 ) is preferably 0.1% or more, more preferably 0.2% or more, and even more preferably 0.3% or more. 11 and transmittance T 12 The absolute value of the difference between 1 ) is preferably 2.0% or less, more preferably 1.8% or less.

[0025] In the present invention, when applied to a pancake lens type virtual reality display device, the occurrence of ghosts can be further suppressed. Therefore, the transmittance at the intersection G described above is set to T before heating at 120° C. for 10 minutes. 21 The transmittance after heating is T 22 When the above formula is satisfied, it is preferable that the following formula (2) is satisfied. 2 = |T 21 -T 22| ≦ 3.0%

[0026] In addition, the transmittance T 21 and transmittance T 22 The absolute value of the difference between 2 ) is preferably 0.1% or more, more preferably 0.2% or more, and even more preferably 0.3% or more. 21 and transmittance T 22 The absolute value of the difference between 2 ) is preferably 3.0% or less, more preferably 2.8% or less, and even more preferably 2.5% or less.

[0027] In the present invention, when applied to a pancake lens type virtual reality display device, the brightness at the intersection G is set to L 11 * and the chromaticity is a 11 * and b 11 * The lightness at the intersection point A is set to L 12 * and the chromaticity is a 12 * and b 12 * When this is the case, it is preferable that the following formula (3) is satisfied.

[0028] In addition, ΔE 1 is preferably 0.5% or more, more preferably 0.6% or more, and even more preferably 0.7% or more. Similarly, ΔE 1 is preferably 3.0% or less, more preferably 2.5% or less, and even more preferably 2.0% or less.

[0029] The average thickness of the optically absorptive anisotropic film is not particularly limited, but is preferably 0.3 to 5.0 μm, more preferably 0.5 to 3.0 μm.

[0030] [Dichroic Substance] The optically absorptive anisotropic film of the present invention preferably contains a dichroic substance. Here, the dichroic substance refers to a dye whose absorbance varies depending on the direction. The dichroic substance may or may not exhibit liquid crystallinity.

[0031] The dichroic substance is not particularly limited, and examples thereof include visible light absorbing substances (dichroic dyes), luminescent substances (fluorescent substances, phosphorescent substances), ultraviolet absorbing substances, infrared absorbing substances, nonlinear optical substances, carbon nanotubes, and inorganic substances (e.g., quantum rods), and any conventionally known dichroic substance (dichroic dye) can be used. Specifically, for example, paragraphs

[0067] to

[0071] of JP 2013-228706 A, paragraphs

[0008] to

[0026] of JP 2013-227532 A, paragraphs

[0008] to

[0015] of JP 2013-209367 A, paragraphs

[0045] to

[0058] of JP 2013-14883 A, paragraphs

[0012] to

[0029] of JP 2013-109090 A, paragraphs

[0009] to

[0017] of JP 2013-101328 A, Paragraphs

[0051] to

[0065] of JP 2013-37353 A, paragraphs

[0049] to

[0073] of JP 2012-63387 A, paragraphs

[0016] to

[0018] of JP 11-305036 A, paragraphs

[0009] to

[0011] of JP 2001-133630 A, paragraphs

[0030] to

[0169] of JP 2011-215337 A, paragraphs

[0021] to

[0075] of JP 2010-106242 A, paragraphs

[0016] to

[0018] of JP 2010-215846 A

[0011] to

[0025] paragraphs,

[0017] to

[0069] paragraphs of JP 2011-048311 A,

[0013] to

[0133] paragraphs of JP 2011-213610 A,

[0074] to

[0246] paragraphs of JP 2011-237513 A,

[0005] to

[0051] paragraphs of JP 2016-006502 A,

[0014] to

[0032] paragraphs of JP 2018-053167 A, and

[0014] to

[0033] paragraphs of JP 2020-11716 A paragraphs

[0005] to

[0041] of International Publication No. 2016 / 060173, paragraphs

[0008] to

[0062] of International Publication No. 2016 / 136561, paragraphs

[0014] to

[0033] of International Publication No. 2017 / 154835, paragraphs

[0014] to

[0033] of International Publication No. 2017 / 154695, paragraphs

[0013] to

[0037] of International Publication No. 2017 / 195833, paragraphs

[0014] to

[0034] of International Publication No. 2018 / 164252,Examples include those described in paragraphs

[0021] to

[0030] of International Publication No. 2018 / 186503, paragraphs

[0043] to

[0063] of International Publication No. 2019 / 189345, paragraphs

[0043] to

[0085] of International Publication No. 2019 / 225468, paragraphs

[0050] to

[0074] of International Publication No. 2020 / 004106, and paragraphs

[0015] to

[0038] of International Publication No. 2021 / 044843.

[0032] As the dichroic substance, a dichroic azo dye compound is preferred. A dichroic azo dye compound refers to an azo dye compound whose absorbance varies depending on the direction. A dichroic azo dye compound may or may not exhibit liquid crystallinity. When a dichroic azo dye compound exhibits liquid crystallinity, it may exhibit either nematic or smectic properties. The temperature range in which the liquid crystal phase is exhibited is preferably room temperature (approximately 20 to 28°C) to 300°C, and more preferably 50 to 200°C from the viewpoints of handleability and manufacturing suitability.

[0033] In the present invention, from the viewpoint of adjusting color hue, it is preferable to use at least one dye compound (first dichroic azo dye compound) having a maximum absorption wavelength in the wavelength range of 560 to 700 nm, and at least one dye compound (second dichroic azo dye compound) having a maximum absorption wavelength in the wavelength range of 455 nm or more and less than 560 nm.

[0034] In the present invention, three or more kinds of dichroic azo dye compounds may be used in combination. For example, from the viewpoint of making the light absorption anisotropic film closer to black, it is preferable to use a first dichroic azo dye compound, a second dichroic azo dye compound, and at least one dye compound (third dichroic azo dye compound) having a maximum absorption wavelength in the wavelength range of 380 nm or more and less than 455 nm in combination.

[0035] In the present invention, the dichroic azo dye compound preferably has a crosslinkable group, such as a (meth)acryloyl group, an epoxy group, an oxetanyl group, or a styryl group, with a (meth)acryloyl group being preferred.

[0036] In the present invention, it is preferable that at least a portion of the dichroic material forms an array structure, because this can further suppress the occurrence of ghosts when applied to a pancake lens-type virtual reality display device. Here, the array structure refers to a state in which the dichroic material gathers to form aggregates in the optically absorptive anisotropic film, and the molecules of the dichroic material are periodically arranged in the aggregates. The array structure may be formed solely of the dichroic material, or may be formed of a liquid crystal compound and a dichroic material. The array structure may be formed of one type of dichroic material or multiple types of dichroic materials. The optically absorptive anisotropic film may contain a mixture of array structures formed from one type of dichroic material and another type of dichroic material. When the optically absorptive anisotropic film contains multiple types of dichroic materials, all of the multiple types of dichroic materials contained in the optically absorptive anisotropic film may form an array structure, or only some of the dichroic materials may form an array structure.

[0037] Furthermore, in the present invention, the transmittance measured by the above-described procedure can be adjusted to easily satisfy the above formula (1), and when applied to a pancake lens type virtual reality display device, the occurrence of ghosts can be further suppressed. For these reasons, when 100 arrangement structures of a dichroic substance present in a cross section of an optically absorptive anisotropic film observed with a scanning transmission electron microscope are selected, the number of arrangement structures having a major axis length of less than 50 nm is preferably 30 or less, more preferably 0 to 25, even more preferably 0 to 15, and particularly preferably 0 to 10.

[0038] Specifically, cross-sectional observation using a scanning transmission electron microscope (hereinafter also abbreviated as "STEM") is performed as follows. First, an ultrathin section with a thickness of 100 nm in the film thickness direction is prepared from the optically absorbing anisotropic film using an ultramicrotome. Next, the ultrathin section is placed on a grid with a carbon support film for STEM observation. After that, the grid is placed in the scanning transmission electron microscope, and the cross section is observed at an electron beam acceleration voltage of 30 kV.

[0039] The length of the major axis of the array structure is specifically measured as follows. First, as described above, the cross section of the optically absorbing anisotropic film is observed using an STEM, and the captured image is analyzed to create a frequency histogram, determining the maximum frequency and the standard deviation of the frequency distribution. Next, the frequency 1.3 times the standard deviation on the dark side of the maximum frequency is set as the threshold. Next, an image is created using this threshold value to binarize the brightness, and portions of the binarized dark regions with a major axis of 20 nm or more are extracted as array structures. Furthermore, each extracted array structure is approximated as an ellipse, and the length of the major axis of the approximated ellipse is defined as the length of the major axis of the array structure. Furthermore, the angle formed by the axis perpendicular to the film surface (the normal direction of the optically absorbing anisotropic film) and the major axis of the approximated ellipse is defined as the angle formed by the major axis of the array structure and the normal direction of the optically absorbing anisotropic film. The length of the major axis of such an array structure can be measured using known image processing software. An example of the image processing software is the image processing software "ImageJ."

[0040] In the present invention, the transmittance measured by the above-described procedure can be adjusted to easily satisfy the above formula (1), and the content of the dichroic material is set to 230 mg / cm because the occurrence of ghosts can be further suppressed when the present invention is applied to a pancake lens type virtual reality display device. 3 It is preferable that the concentration is 230 to 300 mg / cm or more. 3 It is more preferable that the content of the dichroic material (mg / cm 3The dichroic substance content can be obtained by measuring a solution in which an optically absorptive anisotropic film is dissolved, or an extract obtained by immersing an optically absorptive film in a solvent, using high-performance liquid chromatography (HPLC), but is not limited to the above method. Quantification can be performed using the dichroic substance contained in the optically absorptive anisotropic film as a standard sample. One example of a method for calculating the content of the dichroic substance is to calculate the volume by multiplying the thickness of the optically absorptive anisotropic film obtained from a microscopic image of the cross section of the optically absorptive film by the area of ​​the optically absorptive film used to measure the amount of dye, and then dividing the volume by the amount of dye measured by HPLC to calculate the dye content.

[0041] [Liquid Crystal Compound] The optically absorptive anisotropic film of the present invention preferably contains a liquid crystal compound. This allows the dichroic material to be aligned with a higher degree of orientation while suppressing precipitation of the dichroic material. As the liquid crystal compound, either a polymer liquid crystal compound or a low molecular weight liquid crystal compound can be used, with the polymer liquid crystal compound being preferred because it allows for a higher degree of orientation. Furthermore, the liquid crystal compound may be a combination of a polymer liquid crystal compound and a low molecular weight liquid crystal compound. Here, "polymer liquid crystal compound" refers to a liquid crystal compound having a repeating unit in its chemical structure. Furthermore, "low molecular weight liquid crystal compound" refers to a liquid crystal compound having no repeating unit in its chemical structure. Examples of polymer liquid crystal compounds include the thermotropic liquid crystal polymers described in JP 2011-237513 A and the polymer liquid crystal compounds described in paragraphs

[0012] to

[0042] of WO 2018 / 199096 A. Examples of low molecular weight liquid crystal compounds include those described in paragraphs

[0072] to

[0088] of JP 2013-228706 A, and among them, liquid crystal compounds exhibiting smectic properties are preferred. Examples of such liquid crystal compounds include those described in paragraphs

[0019] to

[0140] of WO 2022 / 014340 A, the disclosures of which are incorporated herein by reference.

[0042] The content of the liquid crystal compound in the optically absorptive anisotropic film is preferably 25 to 2,000 parts by mass, more preferably 100 to 1,300 parts by mass, and even more preferably 200 to 900 parts by mass, per 100 parts by mass of the dichroic substance. When the content of the liquid crystal compound is within the above range, the degree of orientation of the dichroic substance is further improved. The liquid crystal compound may be contained alone, or two or more types may be contained. When two or more types of liquid crystal compounds are contained, the content of the liquid crystal compounds refers to the total content of the liquid crystal compounds.

[0043] The optically absorptive anisotropic film of the present invention can easily adjust the transmittance measured by the above-described procedure to satisfy the above formula (1). Furthermore, when applied to a pancake lens-type virtual reality display device, the film is formed by fixing the alignment state of a liquid crystal composition containing a liquid crystal compound, and the Log P value of the liquid crystal compound is preferably 6 or less. Furthermore, the Log P value of the liquid crystal compound is more preferably 2 or more, and even more preferably 3 or more. Furthermore, the upper limit is more preferably 6 or less, and even more preferably 5 or less. Here, the log P value is an index that expresses the hydrophilic and hydrophobic properties of a chemical structure and is sometimes referred to as the hydrophilicity / hydrophobicity parameter. The log P value can be calculated using software such as ChemBioDraw Ultra or HSPiP (Ver. 4.1.07). Alternatively, the log P value can be experimentally determined by the method of OECD Guidelines for the Testing of Chemicals, Section 1, Test No. 117. In the present invention, unless otherwise specified, the log P value is calculated by inputting the structural formula of the compound into HSPiP (Ver. 4.1.07). When a liquid crystal composition contains multiple liquid crystal compounds, the log P value of the liquid crystal compound refers to the largest Log P value among the Log P values ​​of the various liquid crystal compounds.

[0044] In the optically absorptive anisotropic film of the present invention, the liquid crystal compound is preferably homogeneously oriented. Also, in the optically absorptive anisotropic film of the present invention, the dichroic substance is preferably oriented in a specific direction. In particular, in the optically absorptive anisotropic film, it is more preferable that the dichroic substance is oriented in one in-plane direction. In particular, it is even more preferable that the dichroic substance is also oriented in the homogeneously oriented liquid crystal compound. As will be described later, the optically absorptive anisotropic film of the present invention is preferably a film formed using an optically absorptive anisotropic film-forming composition containing a liquid crystal compound and a dichroic substance.

[0045] [Surfactant] The optically absorptive anisotropic film of the present invention preferably contains a surfactant. It is preferable to use a compound having a so-called leveling function that flattens the coated film. For example, a silicon atom-containing compound, a polyacrylate compound, or a fluorine atom-containing compound can be used. In particular, from the viewpoint of reducing environmental pollution, the surfactant is preferably a silicon atom-containing compound or a polyacrylate compound, and a compound having a branched siloxane structure is preferred. The copolymer described in WO 2023 / 054164 is particularly preferred. The content of the surfactant in the optically absorptive anisotropic film is preferably 0.01% to 10%, more preferably 0.01% to 6.0%, and even more preferably 0.05% to 3.0%, relative to the total mass of the solids in the optically absorptive anisotropic film-forming composition (i.e., the mass of the optically absorptive anisotropic film).

[0046] [Other Components] In addition to the above-mentioned components, the optically absorptive anisotropic film may contain an adhesion improver, a plasticizer, a polymer, etc. Here, examples of the adhesion improver include the reactive additives listed in paragraphs

[0123] to

[0129] of JP 2019-91088 A and the boronic acid monomers listed in paragraphs

[0015] to

[0028] of WO 2015 / 053359 A.

[0047] [Method for Producing Optically Absorbent Anisotropic Film] The method for producing the optically absorbing anisotropic film of the present invention is not particularly limited as long as it can produce an optically absorbing anisotropic film having the above-mentioned properties. For example, a method can be used in which a planar optically absorbing anisotropic film is produced and then molded to produce an optically absorbing anisotropic film having a non-planar portion. Methods for molding a planar optically absorbing anisotropic film include, for example, a method using a mold having a convex molding surface and a mold having a concave molding surface (Method 1), and a method for molding a planar optically absorbing anisotropic film by heating the film with a heating temperature distribution in the in-plane direction during molding (Method 2). Below, we will first describe the method for producing a planar optically absorbing anisotropic film, and then describe Methods 1 and 2 in detail. In the following explanation of Methods 1 and 2, the procedure for obtaining the optically absorbing anisotropic film 10 shown in Figures 1 and 2 will be described in detail as an example.

[0048] <Method for manufacturing a planar optically absorptive anisotropic film> The method for manufacturing a planar optically absorptive anisotropic film is not particularly limited, and known methods can be used. Among these, a method for manufacturing a planar optically absorptive anisotropic film using a composition for forming an optically absorptive anisotropic film containing a dichroic substance and a liquid crystal compound is preferred. More specifically, for example, a method including, in this order, a step of applying a composition for forming an optically absorptive anisotropic film to a planar substrate to form a coating film (hereinafter also referred to as a "coating film forming step") and a step of orienting the liquid crystal component and dichroic substance contained in the coating film (hereinafter also referred to as an "orientation step"). The liquid crystal component includes not only the liquid crystal compound described above, but also the dichroic substance having liquid crystallinity if the dichroic substance described above has liquid crystallinity.

[0049] -Coating Film Forming Process- The coating film forming process is a process of forming a coating film by applying a composition for forming an optically absorptive anisotropic film onto a planar substrate. The composition for forming an optically absorptive anisotropic film contains the dichroic substance and liquid crystal compound described above. The dichroic substance and liquid crystal compound contained in the composition for forming an optically absorptive anisotropic film may have a polymerizable group. The polymerizable group is preferably an acryloyl group, a methacryloyl group, an epoxy group, an oxetanyl group, or a styryl group, and more preferably an acryloyl group or a methacryloyl group. When the dichroic substance and the liquid crystal compound have a polymerizable group, these compounds can be fixed in the optically absorptive anisotropic film in the curing process described below. The substrate used in this process is not particularly limited, and any known planar substrate can be used. Furthermore, an alignment film may be provided on the substrate, if necessary. By providing an alignment film, the liquid crystal component can be aligned. Examples of the alignment film include a photo-alignment film.

[0050] In this step, the composition for forming an optically absorbing anisotropic film can be easily applied by using a composition for forming an optically absorbing anisotropic film that contains a solvent, or by using a composition for forming an optically absorbing anisotropic film that has been converted into a liquid such as a melt by heating, etc. Examples of methods for applying the composition for forming an optically absorbing anisotropic film include known methods such as roll coating, gravure printing, spin coating, wire bar coating, extrusion coating, direct gravure coating, reverse gravure coating, die coating, spraying, and inkjet printing.

[0051] Orientation Process—The orientation process is a process for orienting the liquid crystalline component contained in the coating film. This results in a planar optically absorptive anisotropic film. The orientation process may include a drying process. Components such as the solvent can be removed from the coating film by the drying process. The drying process may be performed by leaving the coating film at room temperature for a predetermined time (e.g., natural drying), or by heating and / or blowing air. Here, the liquid crystalline component contained in the composition for forming an optically absorptive anisotropic film may be aligned by the above-described coating film formation process or drying process. For example, in an embodiment in which the composition for forming an optically absorptive anisotropic film is prepared as a coating liquid containing a solvent, the coating film is dried to remove the solvent from the coating film, thereby obtaining a coating film with optical absorptive anisotropy. When the drying process is performed at a temperature equal to or higher than the temperature at which the liquid crystalline component contained in the coating film transitions from a liquid crystal phase to an isotropic phase, the heat treatment described below may not be performed.

[0052] The transition temperature from the liquid crystal phase to the isotropic phase of the liquid crystalline component contained in the coating film is preferably 10 to 250°C, more preferably 25 to 190°C, from the viewpoint of manufacturability and the like. A transition temperature of 10°C or higher is preferable because it does not require a cooling process or the like to lower the temperature to a temperature range in which the liquid crystal phase is exhibited. Furthermore, a transition temperature of 250°C or lower is preferable because it does not require a high temperature even when heating until the isotropic phase is achieved in order to suppress alignment defects, thereby reducing waste of thermal energy and deformation and deterioration of the substrate.

[0053] The orientation step preferably includes a heat treatment. This allows the liquid crystalline component contained in the coating film to be oriented, and the heat-treated coating film can be suitably used as an optically absorptive anisotropic film. From the viewpoint of manufacturability and the like, the heat treatment is preferably performed at a temperature of 10 to 250°C, more preferably 25 to 190°C. The heating time is preferably 1 to 300 seconds, more preferably 1 to 60 seconds. In the present invention, it is preferable to perform the heat treatment multiple times, because this makes it easier to adjust the transmittance measured by the above-described procedure to satisfy the above formula (1), and also because this can further suppress the occurrence of ghosts when applied to a pancake lens-type virtual reality display device.

[0054] The alignment step may include a cooling treatment carried out after the heating treatment. The cooling treatment is a treatment in which the coated film after heating is cooled to about room temperature (20 to 25°C). This makes it possible to fix the alignment of the liquid crystalline component contained in the coated film. The cooling method is not particularly limited and can be carried out by a known method.

[0055] Other Steps The method for forming a planar optically absorptive anisotropic film may include a step of curing the optically absorptive anisotropic film (hereinafter also referred to as a "curing step") after the above-described alignment step. For example, when the compound contained in the optically absorptive anisotropic film has a polymerizable group, the curing step is performed by heating and / or light irradiation (exposure). Among these, the curing step is preferably performed by light irradiation from the viewpoint of productivity. Various light sources, such as infrared, visible light, and ultraviolet light, can be used as the light source for curing, but ultraviolet light is preferred. Furthermore, ultraviolet light may be irradiated while heating during curing, or ultraviolet light may be irradiated through a filter that transmits only specific wavelengths. When exposure is performed while heating, the heating temperature during exposure is preferably 25 to 140°C, although this depends on the transition temperature of the liquid crystal component contained in the liquid crystal film. Furthermore, exposure may be performed under a nitrogen atmosphere. When the curing of the liquid crystal film proceeds by radical polymerization, exposure under a nitrogen atmosphere is preferred because inhibition of polymerization by oxygen is reduced.

[0056] <Method 1> Method 1 uses a mold having a convex molding surface and a mold having a concave molding surface. First, the phenomenon that occurs when a film is molded using a mold having a concave molding surface will be explained using Figures 4 to 6. Figures 4 and 5 show the procedure for molding a film using a mold having a concave molding surface, and Figure 6 shows the film used for molding. As shown in Figure 4, a circular film 22 is placed on a mold 20 having a concave molding surface, and as shown in Figure 5, the film 22 is deformed so as to fit the molding surface of the mold 20, thereby obtaining a film 24 with the concave shape transferred thereto.

[0057] Next, the phenomenon that occurs when a film is molded using a mold having a convex molding surface will be explained using Figures 6 to 8. Figures 7 and 8 show the procedure for molding a film using a mold having a convex molding surface, and Figure 6 shows the film used for molding. As shown in Figure 7, a circular film 22 is placed on a mold 26 having a convex molding surface, and as shown in Figure 8, film 22 is deformed so as to fit the molding surface of mold 26, thereby obtaining a film 28 with the convex shape transferred thereto.

[0058] <Method 2> Method 2 is a method of molding a planar optically absorbing anisotropic film by heating it with a heating temperature distribution in the in-plane direction during molding. A first embodiment of Method 2 includes a manufacturing method comprising the steps of heating a planar optically absorbing anisotropic film so that the heating temperature of the peripheral portion surrounding the central portion of the planar optically absorbing anisotropic film is higher than the heating temperature of the central portion of the planar optically absorbing anisotropic film, and then deforming the heated planar optically absorbing anisotropic film along the molding surface using a mold having a concave molding surface. A second embodiment of Method 2 includes a manufacturing method comprising the steps of heating a planar optically absorbing anisotropic film so that the heating temperature of the peripheral portion surrounding the central portion is lower than the heating temperature of the central portion of the planar optically absorbing anisotropic film, and then deforming the heated planar optically absorbing anisotropic film along the molding surface using a mold having a convex molding surface.

[0059] The first embodiment of Method 2 will be representatively described below with reference to the drawings.

[0060] The heating conditions for the optically absorbing anisotropic film in Method 2 are appropriately selected optimally depending on the type of material of the optically absorbing anisotropic film used and the shape of the non-planar portion. In particular, the heating temperature is preferably equal to or higher than the glass transition temperature of the optically absorbing anisotropic film. There is no particular upper limit to the heating temperature, but it is preferably within (the glass transition temperature of the optically absorbing anisotropic film + 100°C). While the above description has been given of heating the optically absorbing anisotropic film itself, the laminate described below may also be applied to Method 2. In this case, if the laminate includes a support, it is preferable to heat the laminate to a temperature equal to or higher than the glass transition temperature of the support during the heat treatment.

[0061] The heating method in Method 2 is not particularly limited, and examples thereof include heating by contact with a heated solid, heating by contact with a heated liquid, heating by contact with a heated gas, heating by infrared radiation, heating by microwave radiation, etc. Among these, heating by infrared radiation, which allows heating remotely just before molding, is preferred.

[0062] The wavelength of the infrared radiation used for heating is preferably 1.0 to 30.0 μm, more preferably 1.5 to 5 μm. Examples of IR (infrared) light sources include near-infrared lamp heaters with a tungsten filament sealed in a quartz tube, and wavelength-controlled heaters with multiple quartz tubes and a mechanism for cooling a portion of the space between the quartz tubes with air. Methods for creating an intensity distribution of infrared radiation include varying the density of IR light sources and placing a filter with a patterned infrared transmittance between the IR light source and the planar optically absorptive anisotropic film. Examples of filters with patterned transmittance include glass with metal vapor deposition, a cholesteric liquid crystal layer with an infrared reflection band, a dielectric multilayer film with an infrared reflection band, and infrared-absorbing ink. The temperature of the planar optically absorptive anisotropic film is controlled by the intensity of the infrared radiation, and by the infrared radiation duration and irradiance. The temperature of the planar optically absorptive anisotropic film can be monitored using a non-contact radiation thermometer and a thermocouple, and molding can be performed at a target temperature.

[0063] [Laminate] The laminate of the present invention includes the above-mentioned optically absorptive anisotropic film. The laminate of the present invention includes other components in addition to the above-mentioned optically absorptive anisotropic film. The other components are not particularly limited, but include, for example, a retardation layer, a reflective polarizer layer (e.g., a cholesteric liquid crystal layer, a linear polarization type reflective polarizer, etc.), a surface antireflection layer, a pressure-sensitive adhesive layer, a support, and an alignment film. Among these, the other components preferably include a retardation layer and a reflective polarizer layer. That is, the laminate of the present invention is preferably a laminate having a optically absorptive anisotropic film, a retardation layer, and a reflective polarizer layer.

[0064] FIG. 9 shows an example of a laminate of the present invention. The laminate 50A shown in FIG. 9 includes, in this order, an optically absorptive anisotropic film 52, a retardation layer 54 having the function of converting linearly polarized light into circularly polarized light, a positive C plate 56, and a cholesteric liquid crystal layer 58. FIG. 10 shows another example of a laminate of the present invention. The laminate 50B shown in FIG. 10 includes, in this order, an optically absorptive anisotropic film 52, a linearly polarized reflective polarizer 60, a retardation layer 54 having the function of converting linearly polarized light into circularly polarized light, and a positive C plate 56. As shown in FIGS. 9 and 10, all components included in the laminates 50A and 50B have the same curved surface shape as the optically absorptive anisotropic film 52. When the retardation layer 54 in the laminates 50A and 50B is a λ / 4 plate, the angle between the slow axis of the retardation layer 54 and the transmission axis of the optically absorptive anisotropic film 52 is preferably within the range of 45°±10°. The laminates 50A and 50B each include two retardation layers: a retardation layer 54 and a positive C plate 56. A retardation layer having the function of converting linearly polarized light into circularly polarized light may be disposed on the side of the optically absorptive anisotropic film 52 of the laminate 50A opposite the retardation layer 54. A retardation layer having the function of converting linearly polarized light into circularly polarized light may be disposed on the side of the optically absorptive anisotropic film 52 of the laminate 50B opposite the linear polarization type reflective polarizer 60. The laminates 50A and 50B are suitable for use in the virtual reality display device described below. The optically absorptive anisotropic film 52 is the optically absorptive anisotropic film described above. The optically absorptive anisotropic film 52 corresponds to the optically absorptive anisotropic film 10 shown in FIGS. 1 and 2. Components other than the optically absorptive anisotropic film included in the laminate will be described in detail below.

[0065] [Retardation Layer Having the Function of Converting Linearly Polarized Light into Circularly Polarized Light] A retardation layer having the function of converting linearly polarized light into circularly polarized light (hereinafter also simply referred to as a "specific retardation layer") is a type of retardation layer. The specific retardation layer is not particularly limited as long as it has the function of converting linearly polarized light into circularly polarized light, and examples thereof include a λ / 4 plate. A λ / 4 plate is a plate having a λ / 4 function, specifically, a plate having the function of converting linearly polarized light of a certain wavelength (preferably visible light) into circularly polarized light (or circularly polarized light into linearly polarized light). The in-plane retardation of the λ / 4 plate at a wavelength of 550 nm is not particularly limited, but is preferably 120 to 150 nm, more preferably 125 to 145 nm, and even more preferably 135 to 140 nm. In addition to the λ / 4 plate, a retardation layer whose in-plane retardation at a wavelength of 550 nm is 3 / 4 or 5 / 4 of the wavelength of any light in visible light is also preferred.

[0066] The specific retardation layer may have reverse wavelength dispersion.The term "reverse wavelength dispersion" means that the retardation value at the wavelength increases as the wavelength increases.The specific retardation layer may also have a multi-layer structure, and a specific embodiment of this case may be a broadband λ / 4 plate formed by laminating a λ / 4 plate and a λ / 2 plate.The angle between the slow axis of the specific retardation layer and the absorption axis of the light absorption anisotropic film is not particularly limited, but is preferably within 45°±10°.

[0067] The specific retardation layer may be the layer that is made by fixing the liquid crystal compound that is twisted and aligned with the thickness direction as the helical axis.For example, as disclosed in Japanese Patent No. 05753922 and Japanese Patent No. 05960743, the retardation layer that has the layer that is made by fixing the rod-shaped liquid crystal compound or discotic liquid crystal compound that is twisted and aligned with the thickness direction as the helical axis can be enumerated.

[0068] The thickness of the specific retardation layer is not particularly limited, but is preferably 0.1 to 8 μm, more preferably 0.3 to 5 μm.

[0069] [Positive C Plate] A positive C plate is a type of retardation layer. A positive C plate is a retardation layer having an in-plane retardation of substantially zero and a negative retardation in the thickness direction. The positive C plate functions as an optical compensation layer for increasing the degree of polarization of transmitted light with respect to obliquely incident light. The in-plane retardation of the positive C plate at a wavelength of 550 nm is preferably 10 nm or less. The retardation of the positive C plate in the thickness direction at a wavelength of 550 nm is preferably −600 to −40 nm.

[0070] The material for forming the positive C plate is not particularly limited, but it is preferably formed from a composition containing a liquid crystal compound. Such a positive C plate can typically be obtained by vertically aligning a rod-shaped polymerizable liquid crystal compound contained in a polymerizable liquid crystal composition and fixing the alignment state by polymerization. Alternatively, the positive C plate can be formed from a composition containing a side-chain polymer liquid crystal compound as the liquid crystal compound.

[0071] The thickness of the positive C plate is not particularly limited, but from the viewpoint of thinning, it is preferably 0.5 to 10 μm, and more preferably 0.5 to 5 μm.

[0072] [Cholesteric Liquid Crystal Layer] A cholesteric liquid crystal layer is an optical component that separates incident light into right-handed circularly polarized light and left-handed circularly polarized light, specularly reflecting one circularly polarized light and transmitting the other circularly polarized light. Examples of cholesteric liquid crystal layers include cholesteric liquid crystal layers formed by fixing a cholesteric liquid crystal phase. Cholesteric liquid crystal layers are preferred as optical films used for curved surface molding because they suppress a decrease in the degree of polarization and distortion of the polarization axis when stretched or molded into a three-dimensional shape. Furthermore, they are less likely to experience a decrease in the degree of polarization due to distortion of the polarization axis.

[0073] The cholesteric liquid crystal layer preferably includes a blue light-reflecting layer having a reflectance of 40% or more at a wavelength of 460 nm, a green light-reflecting layer having a reflectance of 40% or more at a wavelength of 550 nm, a yellow light-reflecting layer having a reflectance of 40% or more at a wavelength of 600 nm, and a red light-reflecting layer having a reflectance of 40% or more at a wavelength of 650 nm. This configuration is preferable because it can exhibit high reflection characteristics over a wide wavelength range in the visible range. The reflectances mentioned above are those when unpolarized light is incident on the cholesteric liquid crystal layer at each wavelength. The cholesteric liquid crystal layer may also have a pitch gradient structure in which the helical pitch of the cholesteric liquid crystal phase is continuously varied in the thickness direction.

[0074] It is also preferable to use, as the cholesteric liquid crystal layer, a cholesteric liquid crystal layer formed by fixing a cholesteric liquid crystal phase containing a rod-shaped liquid crystal compound and a cholesteric liquid crystal layer formed by fixing a cholesteric liquid crystal phase containing a discotic liquid crystal compound in combination. In such a configuration, the cholesteric liquid crystal phase containing the rod-shaped liquid crystal compound has a positive Rth, while the cholesteric liquid crystal phase containing the discotic liquid crystal compound has a negative Rth, so that the Rths of the two phases are offset, thereby suppressing the occurrence of ghosts even when light is incident from an oblique direction, which is preferable.

[0075] The thickness of the cholesteric liquid crystal layer is not particularly limited, but is preferably 30 μm or less, more preferably 15 μm or less, from the viewpoint of thinning. There is no particular lower limit, and it is often 1 μm or more.

[0076] [Linearly Polarized Reflective Polarizer] A linearly polarized reflective polarizer is a polarizer that reflects one of mutually orthogonal linearly polarized light beams and transmits the other linearly polarized light beam. Examples of linearly polarized reflective polarizers include a film obtained by stretching a dielectric multilayer film and a wire grid polarizer. Commercially available products include a reflective polarizer (product name APF) manufactured by 3M and a wire grid polarizer (product name WGF) manufactured by Asahi Kasei Corporation.

[0077] [Surface Antireflection Layer] The laminate of the present invention may have a surface antireflection layer. In the laminate of the present invention, the surface antireflection layer is preferably disposed on the surface-most side. The surface antireflection layer may be disposed on only one surface side of the laminate, or on both surfaces. The type of surface antireflection layer is not particularly limited, but from the viewpoint of further reducing the reflectance, moth-eye films and AR (Anti-Reflection) films are preferred. Furthermore, moth-eye films are preferred because they can maintain high antireflection performance even when the film thickness varies due to stretching and molding. The angle between the transmission axis of the linear polarization type reflective polarizer and the transmission axis of the light absorption anisotropic film is preferably within the range of 0 to 10°.

[0078] [Adhesive Layer] The laminate of the present invention may or may not have an adhesive layer. When the laminate has an adhesive layer, the number of adhesive layers is preferably one or two. Examples of adhesives constituting the adhesive layer include pressure-sensitive adhesives and adhesives. Examples of adhesives include rubber-based adhesives, acrylic-based adhesives, silicone-based adhesives, urethane-based adhesives, vinyl alkyl ether-based adhesives, polyvinyl alcohol-based adhesives, polyvinylpyrrolidone-based adhesives, polyacrylamide-based adhesives, and cellulose-based adhesives, with acrylic-based adhesives (pressure-sensitive adhesives) being preferred. Examples of adhesives include aqueous adhesives, solvent-based adhesives, emulsion-based adhesives, solventless adhesives, active energy ray-curable adhesives, and heat-curable adhesives. Examples of active energy ray-curable adhesives include electron beam-curable adhesives, ultraviolet-curable adhesives, and visible light-curable adhesives, with ultraviolet-curable adhesives being preferred.

[0079] The thickness of the pressure-sensitive adhesive layer is not particularly limited, but from the viewpoint of thinning, it is preferably 25 μm or less, more preferably 15 μm or less, and even more preferably 5 μm or less. The lower limit is not particularly limited, and it is often 0.1 μm or more.

[0080] [Support] The laminate of the present invention may have a support. The support can be placed in any location. For example, when the cholesteric liquid crystal layer and the retardation layer are films to be transferred from a temporary support, the support can be used as the transfer destination. The type of support is not particularly limited, but a transparent support is preferred. Examples include films such as cellulose acylate, polycarbonate, polysulfone, polyethersulfone, polyacrylate, polymethacrylate, cyclic polyolefin, polyolefin, polyamide, polystyrene, and polyester. Among these, cellulose acylate film, cyclic polyolefin film, polyacrylate film, or polymethacrylate film is preferred as the support. Commercially available cellulose acetate films (e.g., "TD80U" and "Z-TAC" manufactured by Fujifilm Corporation) can also be used. Furthermore, it is preferable that the support have a small retardation. Specifically, the in-plane retardation at a wavelength of 550 nm is preferably 10 nm or less, and the absolute value of the retardation in the thickness direction at a wavelength of 550 nm is preferably 50 nm or less.

[0081] From the viewpoint of stretching and forming treatments, the support preferably has a tan δ peak temperature of 170° C. or less. From the viewpoint of enabling forming at low temperatures, the tan δ peak temperature is preferably 150° C. or less, more preferably 130° C. or less.

[0082] Here, the method for measuring tan δ will be described. Using a dynamic viscoelasticity measuring device (DVA-200 manufactured by IT Measurement Control Co., Ltd.), E" (loss modulus) and E' (storage modulus) are measured under the following conditions for a film sample that has been conditioned in advance in an atmosphere at a temperature of 25°C and a humidity of 60% Rh for at least 2 hours, and the value obtained from this is tan δ (= E" / E'). Device: DVA-200 manufactured by IT Measurement Control Co., Ltd. Sample: 5 mm, length 50 mm (gap 20 mm) Measurement conditions: tension mode Measurement temperature: -150 to 220°C Heating condition: 5°C / min Frequency: 1 Hz

[0083] The thickness of the support is not particularly limited, but is preferably from 5 to 300 μm, more preferably from 5 to 100 μm, and even more preferably from 5 to 30 μm.

[0084] The thickness of the laminate is not particularly limited, but when the laminate does not include a pressure-sensitive adhesive layer or a support, the thickness of the laminate is preferably 30 μm or less, more preferably 25 μm or less. The lower limit is not particularly limited, but is often 10 μm or more. When the laminate includes one of a pressure-sensitive adhesive layer and a support, but does not include the other, the value obtained by subtracting the thickness of one of the layers from the thickness of the laminate is preferably 30 μm or less, more preferably 25 μm or less. The lower limit is not particularly limited, but is often 10 μm or more. When the laminate includes both a pressure-sensitive adhesive layer and a support, the value obtained by subtracting the thickness of the pressure-sensitive adhesive layer and the thickness of the support from the thickness of the laminate is preferably 30 μm or less, more preferably 25 μm or less. The lower limit is not particularly limited, but is often 10 μm or more.

[0085] [Method for producing laminate] The method for producing the laminate of the present invention is not particularly limited, and known methods can be used. For example, a laminate may be produced by laminating another member onto the surface of an optically absorptive anisotropic film having a non-planar shaped portion via a pressure-sensitive adhesive layer, or a moldable laminate may be produced by laminating another member onto the surface of a planar optically absorptive anisotropic film via a pressure-sensitive adhesive layer, and then the moldable laminate may be used to carry out the optically absorptive anisotropic film molding method described in Methods 1 and 2 above, thereby molding the moldable laminate into a predetermined shape, thereby producing a laminate including an optically absorptive anisotropic film having a non-planar shaped portion.

[0086] [Composite Lens] The composite lens of the present invention comprises the above-described laminate of the present invention, a lens, and a half mirror, in this order. FIG. 11 shows an example of the composite lens of the present invention. A composite lens 70 comprises a laminate 72, a lens 74, and a half mirror 76, in this order. As shown in FIG. 11, all of the components included in the composite lens 70 have the same curved surface shape as the light-absorption anisotropic film. The configuration of the laminate 72 is as described above. The components other than the laminate included in the composite lens will be described in detail below.

[0087] [Lens] A compound lens has a lens. Examples of lenses include convex lenses and concave lenses. Examples of convex lenses include biconvex lenses, plano-convex lenses, and convex meniscus lenses. Examples of concave lenses include biconcave lenses, plano-concave lenses, and concave meniscus lenses. As lenses used in virtual reality display devices, convex meniscus lenses or concave meniscus lenses are preferred in terms of expanding the viewing angle, and concave meniscus lenses are more preferred in terms of minimizing chromatic aberration. Lens materials that are transparent to visible light, such as glass, crystal, and plastic, can be used. Since birefringence in lenses can cause rainbow unevenness and light leakage, the smaller the birefringence, the more preferable, and materials with zero birefringence are more preferred.

[0088] [Half Mirror] The composite lens of the present invention has a half mirror. The half mirror is a conventionally known half mirror that transmits approximately half of incident light and reflects the remaining approximately half. The transmittance of the half mirror is preferably 50±30%, more preferably 50±10%. The type of half mirror is not particularly limited, but examples include a reflective layer made of a metal. Examples of metals include silver and aluminum. The thickness of the reflective layer is preferably 1 to 20 nm, more preferably 2 to 10 nm, and even more preferably 3 to 6 nm.

[0089] [Virtual reality display device] The virtual reality display device of the present invention includes the optically absorptive anisotropic film, laminate, or composite lens of the present invention described above. FIG. 12 is a schematic diagram showing an example of the configuration of a virtual reality display device. The virtual reality display device 80 shown in FIG. 12 includes, from the right side of the figure, an image display panel 82, a circular polarizer 84, a half mirror 86, a lens 88, and a laminate 90 of the present invention. Note that the laminate 90 used in FIG. 12 has a configuration similar to the laminate 50A described above, with the optically absorptive anisotropic film 52 positioned on the eye side. The laminate 90, lens 88, and half mirror 86 shown in FIG. 12 constitute the composite lens described above. In the virtual reality display device 80 shown in FIG. 12, light ray 92 emitted from the image display panel 82 passes through the circular polarizer 84 to become circularly polarized light, and then passes through the half mirror 86. The light ray 92 then passes through the lens 88, enters the reflective polarizer layer (e.g., a cholesteric liquid crystal layer) included in the laminate 90 of the present invention, is reflected, passes through the lens 88 again, is reflected again by the half mirror 86, passes through the lens 88 again, and enters the laminate 90. At this time, the circular polarization state of the light ray 92 does not change when reflected by the laminate 90, but when reflected by the half mirror 86, it changes to circular polarization with a direction of rotation opposite to that of the circular polarization when it entered the laminate 90. Therefore, the light ray 92 passes through the laminate 90 and is visually recognized by the user. Furthermore, when the light ray 92 is reflected by the half mirror 86, the image is magnified because the half mirror is shaped like a concave mirror, allowing the user to view the magnified virtual image. The above-mentioned mechanism is called a round-trip optical system or a folded optical system. The optically absorptive anisotropic film of the present invention included in the laminate 90 functions as a so-called linear polarizer, blocking light that has unnecessarily passed through the cholesteric liquid crystal layer and preventing it from becoming leaky light (ghost light) and being observed by a user of the virtual reality display device. In the optically absorptive anisotropic film of the present invention, the transmittance measured by the above-mentioned procedure satisfies the above formula (1), and therefore the occurrence of the above-mentioned leaky light (ghost light) can be suppressed.

[0090] The image display panel 82 is a known image display panel (display panel) such as an organic electroluminescence display panel. In the illustrated example, the image display panel 82 emits an unpolarized image (image light). The unpolarized image emitted by the image display panel 82 passes through the circular polarizer 84 and is converted into circularly polarized light.

[0091] The present invention will be described in more detail below with reference to examples. The materials, amounts used, ratios, treatment contents, treatment procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be construed as being limited by the examples shown below.

[0092] [Example 1] [Preparation of Absorptive Polarizing Film 1 Having an Optically Absorbent Anisotropic Film] <Preparation of Support> The following composition was charged into a mixing tank, stirred, and further heated at 90°C for 10 minutes. The resulting composition was then filtered through filter paper with an average pore size of 34 μm and a sintered metal filter with an average pore size of 10 μm to prepare a dope. The solids concentration of the dope was 23.5 mass%, the amount of plasticizer added was the ratio relative to the cellulose acylate, and the solvent for the dope was methylene chloride / methanol / butanol = 81 / 18 / 1 (mass ratio).

[0093] ------------------------------------------------ Cellulose acylate dope -------------------------------------------------- Cellulose acylate (acetyl substitution degree 2.86, viscosity average degree of polymerization 310) 100 parts by mass Sugar ester compound 1 (formula (S4) below) 6.0 parts by mass Sugar ester compound 2 (formula (S5) below) 2.0 parts by mass Silica particle dispersion (AEROSIL R972, manufactured by Nippon Aerosil Co., Ltd.) 0.1 part by mass Solvent (methylene chloride / methanol / butanol) 351.9 parts by mass --------------------------------------------------

[0094]

[0095]

[0096] The dope prepared above was cast using a drum film-forming machine. The dope was cast from a die onto a metal support cooled to 0°C, and the resulting web (film) was then peeled off from the drum. The drum was made of SUS (stainless steel).

[0097] The web (film) obtained by casting was peeled from the drum and then dried for 20 minutes in a tenter apparatus, in which both ends of the web were clipped with clips while the film was being transported at 30 to 40°C. Subsequently, the web was post-dried by zone heating while being transported with a roll. The obtained web was knurled and then wound up to give cellulose acylate film A1. The obtained cellulose acylate film A1 had a thickness of 60 μm, an in-plane retardation Re(550) of 1 nm at a wavelength of 550 nm, and a thickness direction retardation Rth(550) of 35 nm at a wavelength of 550 nm.

[0098] <Formation of Photo-Alignment Film B1> A composition B1 for forming a photo-alignment film, which will be described later, was continuously applied onto the cellulose acylate film A1 using a wire bar. The cellulose acylate film A1 on which the coating film was formed was dried with hot air at 140°C for 120 seconds, and then the coating film was irradiated with polarized ultraviolet light (10 mJ / cm 2A photo-alignment film B1 was formed by irradiating the substrate with a TAC (triacetyl cellulose) film having a photo-alignment film B1. The photo-alignment film B1 had a thickness of 1.5 μm. ------------------------------------------------ Composition of composition B1 for forming a photo-alignment film------------------------------------------------ Photo-alignment compound PA-1 below: 100.00 parts by mass EPICLON N-695 (manufactured by DIC Corporation) 55.74 parts by mass jER YX7400 (manufactured by Mitsubishi Chemical Corporation) 18.75 parts by mass Polymerizable polymer PA-2 below: 8.01 parts by mass Thermal cationic polymerization initiator PAG-1 below: 16.75 parts by mass Stabilizer DIPEA below: 1.06 parts by mass Butyl acetate 1230.49 parts by mass

[0099] Photoalignment compound PA-1 (wherein the numerical value for each repeating unit represents the content (mass%) of each repeating unit relative to all repeating units; weight average molecular weight: 32,000)

[0100]

[0101] Polymerizable polymer PA-2 (wherein the numerical values ​​a, b, and c represent the content (mass%) of each repeating unit relative to the total repeating units; weight average molecular weight: 18,000)

[0102]

[0103] Thermal cationic polymerization initiator PAG-1

[0104]

[0105] Stabilizer DIPEA

[0106]

[0107] <Formation of Optically Absorbent Anisotropic Film C1> A composition for forming an optically absorbent anisotropic film C1 having the following composition was applied to the obtained photo-alignment film B1 using a wire bar to form a coating film. Next, the coating film was heated at 140°C for 15 seconds (first heating step), subsequently heat-treated at 80°C for 5 seconds, and then cooled to room temperature (25°C). Next, the coating film was heated at 100°C for 15 seconds (second heating step), and again cooled to room temperature. Thereafter, an LED (light emitting diode) lamp (center wavelength 365 nm) was used to heat the coating film at an illuminance of 200 mW / cm. 2 The optically absorptive anisotropic film C1 (polarizer) having a thickness of 1.6 μm was produced on the photo-alignment film B1 by irradiating the film with light for 2 seconds under the irradiation conditions of

[0049] . The transmittance of the optically absorptive anisotropic film C1 in the wavelength range of 380 to 780 nm was measured using a spectrophotometer, and the average visible light transmittance was found to be 43%. The absorption axis of the optically absorptive anisotropic film C1 was in the plane of the optically absorptive anisotropic film C1 and perpendicular to the width direction of the cellulose acylate film A1.

[0108] 0.08 parts by mass of the dichroic substance Dye-C1 below; 0.25 parts by mass of the dichroic substance Dye-C2 below; 1.43 parts by mass of the liquid crystal compound L-1 below; 0.61 parts by mass of the liquid crystal compound L-2 below; 0.04 parts by mass of the adhesion improver A-1 below; 0.08 parts by mass of polymerization initiator IRGACUREOXE-02 (manufactured by BASF); 0.08 parts by mass of surfactant F-1 below; 94.96 parts by mass of cyclopentanone; Benzyl alcohol 2.43 parts by mass ――――――――――――――――――――――――――――――

[0109] Dichroic substance Dye-Y1

[0110] Dichroic substance Dye-M1

[0111] Dichroic substance Dye-C1

[0112] Dichroic substance Dye-C2

[0113] Liquid crystal compound L-1 (In the formula below, the numerical values ​​("59", "15", "26") shown for each repeating unit represent the content (% by mass) of each repeating unit relative to all repeating units. Weight average molecular weight: 18,000)

[0114] Liquid crystal compound L-2 (a mixture of the following liquid crystal compounds (RA), (RB), and (RC) in a mass ratio of 84:14:2)

[0115] Adhesion improver A-1

[0116] Surfactant F-1 (wherein the numerical value for each repeating unit represents the content (% by mass) of each repeating unit relative to all repeating units; weight average molecular weight: 14,000)

[0117] <Formation of Protective Layer D1> A protective layer-forming coating solution D1 having the following composition was continuously applied onto the optically absorptive anisotropic film C1 using a wire bar. Thereafter, the coating was dried with hot air at 80°C for 5 minutes, and then irradiated with light from an LED (light emitting diode) lamp (center wavelength 365 nm) at 300 mJ to obtain a laminate having a 0.6 μm-thick protective layer D1 made of polyvinyl alcohol (PVA), i.e., an absorptive polarizing film 1 having a cellulose acylate film A1 (support), a photo-alignment film B1, an optically absorptive anisotropic film C1, and a protective layer D1 adjacent to each other in this order. -------------------------------------------------- Composition of coating liquid D1 for forming protective layer -------------------------------------------------- 3.31 parts by mass of modified polyvinyl alcohol shown below 0.17 parts by mass of initiator IRGACURE 2959 (manufactured by BASF) 0.07 parts by mass of glutaraldehyde 0.07 parts by mass of pyridinium paratoluenesulfonate 0.05 parts by mass of surfactant F-9 shown below 74.0 parts by mass of water 22.4 parts by mass of ethanol --------------------------------------------------

[0118] Modified polyvinyl alcohol (In the formula below, the numerical value for each repeating unit represents the content (mass%) of each repeating unit relative to all repeating units. Weight average molecular weight: 14,000)

[0119] Surfactant F-9

[0120] [Example 2] Absorptive polarizing film 2 was produced in the same manner as in Example 1, except that the following composition C2 for forming an optically absorptive anisotropic film was used instead of composition C1 for forming an optically absorptive anisotropic film, and the second heating step was carried out at 75°C. 0.04 part by mass of the adhesion improver A-1; 0.07 part by mass of polymerization initiator IRGACUREOXE-02 (manufactured by BASF); 0.006 part by mass of the surfactant F-1; 94.96 parts by mass of cyclopentanone; 0.34 part by mass of the dichroic substance Dye-C2; 1.33 parts by mass of the liquid crystal compound L-1; 0.57 parts by mass of the liquid crystal compound L-2; 0.04 part by mass of the adhesion improver A-1; 0.07 part by mass of polymerization initiator IRGACUREOXE-02 (manufactured by BASF); 0.006 part by mass of the surfactant F-1; 94.96 parts by mass of cyclopentanone; 2.43 parts by mass ――――――――――――――――――――――――――――――

[0121] [Example 3] Absorptive polarizing film 3 was produced in the same manner as in Example 1, except that the following composition C3 for forming an optically absorptive anisotropic film was used instead of composition C1 for forming an optically absorptive anisotropic film, and the second heating step was carried out at 75°C. 0.04 part by mass of the adhesion improver A-1; 0.07 part by mass of polymerization initiator IRGACUREOXE-02 (manufactured by BASF); 0.006 part by mass of the surfactant F-1; 94.96 parts by mass of cyclopentanone; 0.37 part by mass of the dichroic substance Dye-C2; 1.29 parts by mass of the liquid crystal compound L-1; 0.55 parts by mass of the liquid crystal compound L-2; 0.04 part by mass of the adhesion improver A-1; 0.07 part by mass of polymerization initiator IRGACUREOXE-02 (manufactured by BASF); 0.006 part by mass of the surfactant F-1; 94.96 parts by mass of cyclopentanone; 2.43 parts by mass ――――――――――――――――――――――――――――――

[0122] [Example 4] Absorptive polarizing film 4 was produced in the same manner as in Example 1, except that the following composition C4 for forming an optically absorptive anisotropic film was used instead of composition C1 for forming an optically absorptive anisotropic film, and the second heating step was carried out at 75°C. 0.08 parts by mass of the dichroic substance Dye-C1; 0.25 parts by mass of the dichroic substance Dye-C2; 1.43 parts by mass of the liquid crystal compound L-1; 0.61 parts by mass of the following liquid crystal compound L-3; 0.04 parts by mass of the above adhesion improver A-1; 0.08 parts by mass of polymerization initiator IRGACUREOXE-02 (manufactured by BASF); 0.08 parts by mass of the following surfactant F-2; 94.96 parts by mass of cyclopentanone; 2.43 parts by mass ――――――――――――――――――――――――――――――

[0123] Liquid crystal compound L-3

[0124] Surfactant F-2 (wherein the numerical value for each repeating unit represents the content (mass%) of each repeating unit relative to the total repeating units. Ac represents —C(O)CH 3 Weight average molecular weight: 15,000

[0125] [Example 5] Absorptive polarizing film 5 was produced in the same manner as in Example 1, except that the following composition C5 for forming an optically absorptive anisotropic film was used instead of composition C1 for forming an optically absorptive anisotropic film, and the second heating step was carried out at 75°C. 0.04 part by mass of the adhesion improver A-1; 0.07 part by mass of polymerization initiator IRGACUREOXE-02 (manufactured by BASF); 0.006 part by mass of the surfactant F-2; 94.96 parts by mass of cyclopentanone; 0.34 part by mass of the dichroic substance Dye-C2; 1.33 parts by mass of the liquid crystal compound L-1; 0.57 parts by mass of the liquid crystal compound L-3; 0.04 part by mass of the adhesion improver A-1; 0.07 part by mass of polymerization initiator IRGACUREOXE-02 (manufactured by BASF); 0.006 part by mass of the surfactant F-2; 94.96 parts by mass of cyclopentanone; 2.43 parts by mass ――――――――――――――――――――――――――――――

[0126] [Example 6] Absorptive polarizing film 6 was produced in the same manner as in Example 1, except that the following composition C6 for forming an optically absorptive anisotropic film was used instead of composition C1 for forming an optically absorptive anisotropic film, and the second heating step was carried out at 75°C. 0.04 part by mass of the adhesion improver A-1; 0.07 part by mass of polymerization initiator IRGACUREOXE-02 (manufactured by BASF); 0.006 part by mass of the surfactant F-2; 94.96 parts by mass of cyclopentanone; 0.37 parts by mass of the dichroic substance Dye-C2; 1.29 parts by mass of the liquid crystal compound L-1; 0.55 parts by mass of the liquid crystal compound L-3; 0.04 part by mass of the adhesion improver A-1; 0.07 part by mass of polymerization initiator IRGACUREOXE-02 (manufactured by BASF); 0.006 part by mass of the surfactant F-2; 94.96 parts by mass of cyclopentanone; 2.43 parts by mass ――――――――――――――――――――――――――――――

[0127] [Example 7] Absorptive polarizing film 7 was produced in the same manner as in Example 1, except that the following composition C7 for forming an optically absorptive anisotropic film was used instead of composition C1 for forming an optically absorptive anisotropic film, and the second heating step was carried out at 75°C. 0.08 parts by mass of the dichroic substance Dye-C1; 0.25 parts by mass of the dichroic substance Dye-C2; 1.43 parts by mass of the liquid crystal compound L-1; 0.61 parts by mass of the following liquid crystal compound L-4; 0.04 parts by mass of the adhesion improver A-1; 0.08 parts by mass of polymerization initiator IRGACUREOXE-02 (manufactured by BASF); 0.08 parts by mass of the surfactant F-2; 94.96 parts by mass of cyclopentanone; 2.43 parts by mass ――――――――――――――――――――――――――――――

[0128] Liquid crystal compound L-4

[0129] [Example 8] Absorptive polarizing film 8 was produced in the same manner as in Example 1, except that the following composition C8 for forming an optically absorptive anisotropic film was used instead of composition C1 for forming an optically absorptive anisotropic film, and the second heating step was carried out at 75°C. 0.04 part by mass of the adhesion improver A-1; 0.07 part by mass of polymerization initiator IRGACUREOXE-02 (manufactured by BASF); 0.006 part by mass of the surfactant F-2; 94.96 parts by mass of cyclopentanone; 0.34 part by mass of the dichroic substance Dye-C2; 1.33 parts by mass of the liquid crystal compound L-1; 0.57 parts by mass of the liquid crystal compound L-4; 0.04 part by mass of the adhesion improver A-1; 0.07 part by mass of polymerization initiator IRGACUREOXE-02 (manufactured by BASF); 0.006 part by mass of the surfactant F-2; 94.96 parts by mass of cyclopentanone; 2.43 parts by mass ――――――――――――――――――――――――――――――

[0130] [Example 9] Absorptive polarizing film 9 was produced in the same manner as in Example 1, except that the following composition C9 for forming an optically absorptive anisotropic film was used instead of composition C1 for forming an optically absorptive anisotropic film, and the second heating step was carried out at 75°C. 0.04 part by mass of the adhesion improver A-1; 0.07 part by mass of polymerization initiator IRGACUREOXE-02 (manufactured by BASF); 0.006 part by mass of the surfactant F-2; 94.96 parts by mass of cyclopentanone; 0.37 parts by mass of the dichroic substance Dye-C2; 1.29 parts by mass of the liquid crystal compound L-1; 0.55 parts by mass of the liquid crystal compound L-4; 0.04 part by mass of the adhesion improver A-1; 0.07 part by mass of polymerization initiator IRGACUREOXE-02 (manufactured by BASF); 0.006 part by mass of the surfactant F-2; 94.96 parts by mass of cyclopentanone; 2.43 parts by mass ――――――――――――――――――――――――――――――

[0131] Example 10 An absorptive polarizing film 10 was produced in the same manner as in Example 9, except that the second heating step was not carried out.

[0132] Example 11 An absorptive polarizing film 11 was produced in the same manner as in Example 1, except that the following composition C11 for forming an optically absorptive anisotropic film was used instead of the composition C1 for forming an optically absorptive anisotropic film. ------------------------------------------------ Optically absorptive anisotropic film-forming composition C11---------------------------------------------------------------- Upper dichroic substance Dye-Y1 0.013 parts by mass Dichroic substance Dye-M1 0.08 parts by mass Dichroic substance Dye-C1 0.33 parts by mass Liquid crystal compound L-1 1.43 parts by mass Liquid crystal compound L-2 0.61 parts by mass Adhesion improver A-1 0.04 parts by mass Polymerization initiator IRGACUREOXE-02 (manufactured by BASF) 0.08 parts by mass Surfactant F-1 0.007 parts by mass Cyclopentanone 94.96 parts by mass Benzyl alcohol 2.43 parts by mass ----------------------------------------------------------------------------------

[0133] Comparative Example 1 An absorptive polarizing film H1 was produced in the same manner as in Example 1, except that the temperature in the second heating step was 75°C.

[0134] Comparative Example 2 An absorptive polarizing film H2 was produced in the same manner as in Example 5, except that LED irradiation was not performed.

[0135] For the optically absorptive anisotropic films used in the preparation of the absorptive polarizing films of Examples 1 to 11 and Comparative Examples 1 and 2, 100 alignment structures of the dichroic material present in the cross section of the optically absorptive anisotropic film were observed with a scanning transmission electron microscope, and the number of alignment structures with a major axis length of less than 50 nm was calculated using the method described above. The results are shown in Table 1 below. Note that for the optically absorptive anisotropic film used in Example 10, no aggregates were formed, and therefore this is indicated by "-" in Table 1 below.

[0136] [Preparation of Virtual Reality Display Device] <Preparation of Retardation Layer Film 1 Having Positive A Plate> A coating solution E1 for forming a photo-alignment film having the following composition was continuously applied onto the above-mentioned cellulose acylate film A1 using a wire bar. The cellulose acylate film A1 on which the coating film was formed was dried with hot air at 140°C for 120 seconds, and then the coating film was irradiated with polarized ultraviolet light (10 mJ / cm 2 , using an ultra-high pressure mercury lamp) to form a photo-alignment film E1 with a thickness of 0.2 μm, thereby obtaining a TAC film with a photo-alignment film.

[0137] -------------------------------------------------- Coating liquid E1 for forming photoalignment film -------------------------------------------------- - 100.00 parts by mass of polymer PA-2 described below - 5.00 parts by mass of thermal cationic polymerization initiator PAG-1 described above - 0.005 parts by mass of acid generator CPI-110TF described below - 16.50 parts by mass of isopropyl alcohol - 1072.00 parts by mass of butyl acetate - 268.00 parts by mass of methyl ethyl ketone --------------------------------------------------

[0138] Polymer PA-2 (In the formula below, the numerical value for each repeating unit represents the content (% by mass) of each repeating unit relative to all repeating units; weight average molecular weight: 45,000)

[0139] Acid generator CPI-110TF

[0140] Composition F1 having the following composition was applied onto the photo-alignment film E1 using a bar coater. The coating film formed on the photo-alignment film E1 was heated to 120°C with hot air, then cooled to 60°C, and then irradiated with 100 mJ / cm2 at a wavelength of 365 nm using a high-pressure mercury lamp under a nitrogen atmosphere. 2 The coating film was irradiated with ultraviolet light of 500 mJ / cm 2 while being heated to 120°C. 2The coating film was irradiated with ultraviolet light of 1000 nm, thereby fixing the alignment of the liquid crystal compound, and a retardation layer film 1 having a positive A plate F1 was produced. The thickness of the positive A plate F1 was 2.5 μm, and Re(550) was 144 nm. The positive A plate also satisfied the relationship Re(450)≦Re(550)≦Re(650). Re(450) / Re(550) was 0.82. The positive A plate corresponds to a so-called λ / 4 plate.

[0141] ------------------------------------------------- Composition F1 ------------------------------------------------- 43.50 parts by mass of polymerizable liquid crystal compound LA-1 described below 43.50 parts by mass of polymerizable liquid crystal compound LA-2 described below 8.00 parts by mass of polymerizable liquid crystal compound LA-3 described below 5.00 parts by mass of polymerizable liquid crystal compound LA-4 described below 0.55 parts by mass of polymerization initiator PI-1 described below 0.20 parts by mass of leveling agent T-1 described below 235.00 parts by mass of cyclopentanone ------------------------------------------------

[0142] Polymerizable liquid crystal compound LA-1 (tBu represents a tertiary butyl group)

[0143] Polymerizable liquid crystal compound LA-2

[0144] Polymerizable liquid crystal compound LA-3

[0145] Polymerizable liquid crystal compound LA-4 (Me represents a methyl group)

[0146] Polymerization initiator PI-1

[0147] Leveling agent T-1 (in the formula below, the numerical value for each repeating unit represents the content (mass %) of each repeating unit relative to all repeating units; weight average molecular weight: 25,000)

[0148] <Preparation of Retardation Layer Film 2 Having Positive C Plate> The above-described cellulose acylate film A1 was used as a temporary support. The cellulose acylate film A1 was passed through a dielectric heating roll at a temperature of 60°C to raise the surface temperature of the film to 40°C, and then an alkaline solution having the composition shown below was applied to one side of the film using a bar coater in an amount of 14 ml / m. 2 The film was heated to 110°C and transported for 10 seconds under a steam-type far-infrared heater manufactured by Noritake Co., Ltd. Next, pure water was applied to the film at a rate of 3 ml / m using the same bar coater. 2 Next, after repeating washing with water using a fountain coater and draining with an air knife three times, the film was transported to a drying zone at 70° C. for 10 seconds and dried to prepare an alkali-saponified cellulose acylate film A1.

[0149] ---------------------------------------------------------------- (Alkaline solution) ---------------------------------------------------------------- Potassium hydroxide 4.7 parts by mass Water 15.8 parts by mass Isopropanol 63.7 parts by mass Fluorine-containing surfactant SF-1 (C 14 H 29 O (CH 2 CH 2 O) 20 H) 1.0 part by mass Propylene glycol 14.8 parts by mass

[0150] An alignment film-forming coating solution G1 having the following composition was continuously applied onto the above-mentioned alkali-saponified cellulose acylate film A1 using a #8 wire bar, and the resulting film was dried with hot air at 60°C for 60 seconds and then with hot air at 100°C for 120 seconds to form an alignment film G1.

[0151] ------------------------------------------------------------------ Coating liquid G1 for forming alignment film -------------------------------------------------- Polyvinyl alcohol (PVA103, manufactured by Kuraray) 2.4 parts by mass Isopropyl alcohol 1.6 parts by mass Methanol 36 parts by mass Water 60 parts by mass ------------------------------------------------------------------

[0152] A coating solution H1 for forming a positive C plate having the following composition was applied onto the alignment film G1, and the resulting coating film was aged at 60° C. for 60 seconds, and then irradiated with 70 mW / cm 2 2 An air-cooled metal halide lamp (manufactured by Eye Graphics Co., Ltd.) was used, and the light output was 1000 mJ / cm 2 The liquid crystal compound was vertically aligned by irradiating the film with ultraviolet light of 1000 W at 1000 W to fix the alignment state, thereby producing a retardation layer film 2 having a positive C plate H1 with a thickness of 0.5 μm. The Rth(550) of the obtained positive C plate was −60 nm.

[0153] -------------------------------- Coating liquid H1 for forming positive C-plate -------------------------------- 80 parts by mass of the following liquid crystal compound LC-1 20 parts by mass of the following liquid crystal compound LC-2 1 part by mass of the following vertical alignment liquid crystal compound promoter S01 8 parts by mass of ethylene oxide-modified trimethylolpropane triacrylate (V#360, manufactured by Osaka Organic Chemical Co., Ltd.) 3 parts by mass of Irgacure 907 (manufactured by BASF) 1 part by mass of Kayacure DETX (manufactured by Nippon Kayaku Co., Ltd.) 0.4 parts by mass of the following compound B03 170 parts by mass of methyl ethyl ketone 30 parts by mass of cyclohexanone --------------------------------

[0154] Liquid crystal compound LC-1

[0155] Liquid crystal compound LC-2

[0156] Vertical alignment liquid crystal compound promoter S01

[0157] Compound B03 (In the formula below, the numerical value for each repeating unit represents the content (% by mass) of each repeating unit relative to all repeating units; weight average molecular weight: 15,000)

[0158] <Preparation of Optical Laminate B0> The optical laminate B0 was prepared by the following procedure. A broadband dielectric multilayer film (trademark APF, 3M) was used as a linear polarization type reflective polarizer. The positive A plate side of the obtained retardation layer film 1 was attached to one surface of the APF, and the alignment layer and support were peeled off. Furthermore, the alignment film was peeled off, and the positive C plate side of the obtained retardation layer film 2 was attached to the exposed liquid crystal surface with an adhesive, and the support and alignment layer were peeled off. In this way, an optical laminate B0 consisting of a linear polarization type reflective polarizer / adhesive layer / positive A plate / positive C plate was prepared.

[0159] <Formation of Half Mirror Lens> Aluminum was vapor-deposited on the convex side of a lens (a convex meniscus lens LE1076-A (diameter 2 inches) manufactured by Thorlab) so that the reflectance was 40%, thereby forming a half mirror lens.

[0160] <Preparation of Absorptive Polarizer Film 1MK5> The protective layer side of the absorptive polarizer film 1 prepared in Example 1 was bonded to a PMMA film via an adhesive sheet, and only the support was peeled off to form an absorptive polarizer film 1M, which was then set in a molding device. At this time, the PMMA film side was positioned downward. The molding space within the molding device consisted of box 1 and box 2, separated by absorptive polarizer film 2. Mold 1 (a convex lens with a diameter of 2 inches and a curvature radius of 84 mm) was placed in box 1 below the absorptive polarizer film 1M, with the convex surface (molding surface) facing up. Furthermore, a transparent window was installed on the top of box 2 above the absorptive polarizer film 1M, and an IR light source for heating the absorptive polarizer film 1M was installed outside this window. Next, a vacuum was drawn using a vacuum pump to evacuate box 1 and box 2 to a pressure of 0.1 atmospheres or less. Next, in the step of heating the absorptive polarizer film 1M, infrared rays were irradiated and the absorptive polarizer film 1M was heated until its temperature reached 108 ° C. The glass transition temperature Tg of the PMMA film used as the support was 105 ° C., so the film was made to be easily stretched during molding. Next, in the step of pressing the absorptive polarizer film 1M against the mold 1 and deforming it to conform to the shape of the mold 1, gas was flowed into the box 2 from a gas cylinder to pressurize it to 300 kPa, and the absorptive polarizer film 1M was pressure-bonded to the mold 1. Finally, the absorptive polarizer film 1M was removed from the lens, which was the mold 1. This resulted in an absorptive polarizer film 1M molded into a non-planar shape. Next, the absorptive polarizer film 1M molded into a non-planar shape was set in a molding device, upside down from the initial molding, with the PMMA film side facing up. At this time, the non-planar region of the absorptive polarizer film 1M formed by the initial molding protruded downward. A meniscus lens (diameter 2 inches, radius of curvature of the concave surface 70 mm) with aluminum vapor-deposited on the convex surface was placed with the concave surface facing up just below the region molded into a non-planar shape in the absorptive polarizer film 1M, as the mold 2. Next, the insides of boxes 1 and 2 were each evacuated to a vacuum of 0.1 atmospheres or less using a vacuum pump.Next, in a step of heating the absorptive polarizer film 1M, the absorptive polarizer film 1M was irradiated with infrared rays and heated until its temperature reached 108° C. Next, in a step of pressing the absorptive polarizer film 1M against the mold 2 and deforming it to conform to the shape of the mold 2, gas was flowed into the box 2 from a gas cylinder to pressurize it to 300 kPa, and the absorptive polarizer film 1M was pressure-bonded to the mold 2. Finally, the absorptive polarizer film 1M was removed from the lens, which was the mold 2. In this way, an absorptive polarizer film 1MK5 molded onto a curved surface by molding method 1 was obtained.

[0161] <Preparation of Optical Laminate B0K5> The optical laminate B0 was set in a molding device. At this time, it was arranged so that the positive C plate side was on the bottom. Thereafter, an optical laminate B0K5 molded into a non-planar shape was obtained in the same manner as in the preparation method of the absorptive polarizer film 1MK5.

[0162] <Preparation of Optical Laminate B1K5> The APF (linear polarization type reflective polarizer) side of the optical laminate B0K5 obtained above was bonded to the photo-alignment film side of the absorptive polarizer film 1MK5 with an adhesive. The lamination was performed so that the transmission axis of the APF and the transmission axis of the optically absorptive anisotropic film coincided. In this way, an optical laminate B1K5 consisting of a positive C plate / positive A plate / adhesive layer / APF / adhesive layer / absorptive polarizer was prepared.

[0163] <Preparation of a composite lens> The half-mirror lens prepared above was adjusted to the lens diameter and curvature radius of mold 2 and molded into a non-planar shape in the same manner as in the preparation of absorptive polarizer film 1MK5. Next, the prepared optical laminate B1K5 was attached to the concave side of the non-planar molded half-mirror lens with an adhesive to obtain a composite lens. A composite lens was obtained in the same manner as above, except that the absorptive polarizer films prepared in Examples 2 to 11 and Comparative Examples 1 and 2 were used instead of absorptive polarizer film 1.

[0164] <Preparation of Virtual Reality Display Device> A virtual reality display device "Huawei VR Glass" manufactured by Huawei, which is a virtual reality display device employing a reciprocating optical system, was disassembled, and all of the compound lenses were removed. The compound lenses prepared above were incorporated into the main body in place of the removed compound lenses, and the compound lenses were positioned so that the light-absorbing anisotropic film side was facing the eye, thereby preparing a virtual reality display device. A black and white checkered pattern was displayed on the image display panel of the prepared virtual reality display device, and the ghost visibility was evaluated visually according to the following criteria. The results are shown in Table 1 below. (Ghost Evaluation) AA: Almost invisible. A: Very slightly visible, but not noticeable. B: Slightly visible, but not noticeable. C: A weak ghost was visible. D: A somewhat strong ghost was visible.

[0165]

[0166] As shown in Table 1, the transmittance T 11 and transmittance T 12 The absolute value of the difference between 1 ) is greater than 2.5%, ghosting occurs when the device is applied to a pancake lens type virtual reality display device (Comparative Examples 1 and 2). 11 and transmittance T 12 The absolute value of the difference between 1 ) is 2.5% or less, the occurrence of ghosts is suppressed when applied to a pancake lens type virtual reality display device (Examples 1 to 11). Furthermore, a comparison between Example 5 and Example 6, and a comparison between Examples 8 to 10, revealed that when 100 array structures of dichroic material present in a cross section of an optically absorbing anisotropic film observed with a scanning transmission electron microscope are selected, if the number of array structures having a major axis length of less than 50 nm is 30 or less, the occurrence of ghosts can be further suppressed when applied to a pancake lens type virtual reality display device. Furthermore, a comparison between Example 4 and Example 5, and a comparison between Example 7 and Example 8 revealed that when the content of the dichroic material is 230 mg / cm 3It was found that the occurrence of ghosts can be further suppressed when applied to a pancake lens type virtual reality display device by the above. Furthermore, from a comparison between Example 2 and Example 5, and a comparison between Example 3 and Example 6, it was found that if the optically absorptive anisotropic film is a film formed by fixing the alignment state of a liquid crystal composition containing a liquid crystal compound, and the Log P value of the liquid crystal compound is 6 or less, the occurrence of ghosts can be further suppressed when applied to a pancake lens type virtual reality display device.

[0167] 1 Maximum projected image 2 Circle X 3 Circle Y 4 Center of gravity 10 Light-absorbing anisotropic film Z Any four points on the circle Y 20 Mold having a concave molding surface 22 Film 24 Film to which a concave shape has been transferred 26 Mold having a convex molding surface 28 Film to which a convex shape has been transferred 50A, 50B Laminate 54 Retardation layer having the function of converting linearly polarized light into circularly polarized light 56 ​​Positive C plate 58 Cholesteric liquid crystal layer 60 Linearly polarized reflective polarizer 70 Compound lens 72, 90 Laminate 74, 88 Lens 76, 86 Half mirror 80 Virtual reality display device 82 Image display device 84 Circular polarizer 92 Light ray

Claims

1. An optically absorptive anisotropic film having a curved surface, the transmittance measured by the following procedure satisfies the following formula (1): Step 1: The optically absorptive anisotropic film is orthogonally projected to identify the maximum projected image with the largest area. 2: A circle X with the smallest area that includes all of the maximum projected images of the optically absorptive anisotropic film is drawn with the center of gravity of the maximum projected images of the optically absorptive anisotropic film as its center. 3: A circle Y with a radius that is 1 / 2 the radius of the circle X is drawn with the center of gravity of the maximum projected images of the optically absorptive anisotropic film as its center. 4: A transmittance T at an intersection G between the optically absorptive anisotropic film and a line that passes through the center of gravity of the maximum projected images of the optically absorptive anisotropic film and extends toward the normal direction of the maximum projected images. 11 5: Measure the transmittance at each intersection of the optically absorptive anisotropic film and each line passing through any four points on the circle Y and extending toward the normal direction of the maximum projected image. 11 The transmittance T where the absolute value of the difference between 12 Here, the transmittance T 12 The point where is measured is defined as intersection point A. 1 = |T 11 -T 12 | ≦ 2.5% 2. Regarding the transmittance at the intersection G, the transmittance before heating at 120°C for 10 minutes is T 21 The transmittance after heating is T 22 The optically absorptive anisotropic film according to claim 1, which satisfies the following formula (2) when 2 = |T 21 -T 22 | ≦ 3.0% 3. The lightness at the intersection point G is L 11 * and the chromaticity is a 11 * and b 11 * The lightness at the intersection point A is L 12 * and the chromaticity is a 12 * and b 12 * 3. The optically absorptive anisotropic film according to claim 1, which satisfies the following formula (3) when 4. The optically absorptive anisotropic film according to claim 1 or 2, further comprising a dichroic substance.

5. The optically absorptive anisotropic film according to claim 4, wherein at least a portion of said dichroic material forms an ordered structure.

6. The optically absorptive anisotropic film described in claim 5, wherein, when 100 of the array structures present in a cross-section of the optically absorptive anisotropic film observed with a scanning transmission electron microscope are selected, the number of array structures having a major axis length of less than 50 nm is 30 or less.

7. The content of the dichroic material is 230 mg / cm 3 The optically absorptive anisotropic film according to claim 4 .

8. The optically absorptive anisotropic film according to claim 1 or 2, wherein the optically absorptive anisotropic film is a film obtained by fixing the alignment state of a liquid crystal composition containing a liquid crystal compound, and the Log P value of the liquid crystal compound is 6 or less. Here, when the liquid crystal composition contains a plurality of liquid crystal compounds, the Log P value of the liquid crystal compound refers to the largest Log P value among the Log P values ​​of the various liquid crystal compounds.

9. A laminate comprising the optically absorptive anisotropic film according to claim 1 or 2.

10. The laminate according to claim 9, comprising the light absorbing anisotropic film, a retardation layer, and a reflective polarizer layer.

11. A compound lens comprising, in this order, the laminate according to claim 9, a lens, and a half mirror.

12. A virtual reality display device comprising the laminate of claim 9.

Citation Information

Patent Citations

  • Polarizing plate for curve surface and optical laminate

    JP2016200731A

  • Layered body, optical device, and display device

    WO2021111861A1

  • Optical element, image display device, virtual reality display device, electronic finder, and method for manufacturing polarizer

    WO2021246286A1

  • Laminated optical film and image display device

    WO2022075475A1

  • Polarizing plate subjected to curved surface machining and method for manufacturing same

    WO2022097631A1

Cited By

  • Light absorbing anisotropic film, light absorbing anisotropic film manufacturing method, layered body, compound lens, and virtual reality display device

    WO2026204498A1