Joined body manufacturing method and structure set
The method of using structures with conductive nanowires of specific length and distribution ensures strong bonding between electronic components, addressing the issue of insufficient bonding strength with short bonding times by ensuring sufficient entanglement and using heat to enhance the connection process.
Patent Information
- Application Number
- PCT/JP2024/008286
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-05
- Publication Date
- 2024-10-03
AI Technical Summary
Existing methods for electrically connecting electronic components, such as semiconductor devices and circuit boards, often result in insufficient bonding strength when the bonding time is shortened, limiting the efficiency of the connection process.
A method involving the use of first and second structures with conductive nanowires, where the arithmetic average length of the exposed nanowires is between 1 to 40 μm, and the standard deviation is 2 μm or less, ensuring sufficient entanglement and strong bonding even with short bonding times, along with a heating step at 150 to 300°C to enhance the bonding process.
This approach allows for the creation of a bonded body with excellent bonding strength, even when the bonding time is short, by ensuring the nanowires are sufficiently entangled, resulting in a robust electrical connection.
Smart Images

Figure JP2024008286_03102024_PF_FP_ABST
Abstract
Description
Method for manufacturing joined body and structure set
[0001] The present invention relates to a method for manufacturing a bonded body and a structure set.
[0002] Currently, various methods are used for electrically connecting electronic components such as semiconductor elements to each other and for electrically connecting electronic components to circuit boards. As a method for electrically connecting such electronic components to each other, Patent Document 1 discloses a method in which a number of nanowires provided on a first component, which is an electronic component, are brought into contact with a second component, which is also an electronic component, and then heated to bond the first component and the second component via the nanowires (claim 1, etc.).
[0003] Special Publication No. 2021-503185
[0004] The inventors used the method described in Patent Document 1 as a reference to bond a first structure to a second structure not provided with conductive nanowires via conductive nanowires provided on the first structure, and found that if the bonding time was short, sufficient bonding strength may not be obtained, indicating that there is room for improvement.
[0005] Therefore, an object of the present invention is to provide a method for manufacturing a bonded body that has excellent bonding strength even when the bonding time is short, and a structure set to be used for manufacturing the bonded body.
[0006] As a result of intensive research to solve the above-mentioned problems, the present inventors have discovered that when a first structure having a plurality of first conductive nanowires and a second structure having a plurality of second conductive nanowires are used to bond the first structure and the second structure by arranging the first conductive nanowires and the second conductive nanowires so that they are in contact with each other, a bonded structure with excellent bonding strength can be obtained even if the bonding time is short, so long as the arithmetic mean length of the exposed portions of the plurality of first conductive nanowires and the arithmetic mean length of the exposed portions of the plurality of second conductive nanowires are predetermined values, and have completed the present invention. That is, the present inventors have discovered that the above-mentioned problems can be solved by the following configuration.
[0007] [1] A method for manufacturing a bonded body obtained by bonding a first structure and a second structure, the method comprising the steps of: providing a plurality of first conductive nanowires in a first conductive region of a first member having a first conductive region on a surface thereof, to obtain the first structure having the first conductive nanowires; providing a plurality of second conductive nanowires in a second conductive region of a second member having a second conductive region on a surface thereof, to obtain the second structure having the second conductive nanowires; and a bonding step of arranging the first conductive nanowires and the second conductive nanowires so that they are in contact with each other, thereby bonding the first structure and the second structure, wherein the arithmetic mean length of exposed portions of the plurality of first conductive nanowires and the arithmetic mean length of exposed portions of the plurality of second conductive nanowires are both 1 to 40 μm. [2] A method for producing a bonded body according to [1], wherein at least one of the standard deviation of the lengths of the exposed portions of the first conductive nanowires is 2 μm or less and the standard deviation of the lengths of the exposed portions of the second conductive nanowires is 2 μm or less. [3] A method for producing a bonded body according to [1] or [2], wherein at least one of the average diameter of the first conductive nanowires is 45 to 75 nm and the average diameter of the second conductive nanowires is 45 to 75 nm. [4] A method for producing a bonded body according to any of [1] to [3], wherein at least one of the coverage area of the first conductive region with the first conductive nanowires is 20 to 50% of the surface area of the first conductive region and the coverage area of the second conductive nanowires is 20 to 50% of the surface area of the second conductive region. [5] The method for producing a junction according to any one of [1] to [4], wherein at least one of the first conductive nanowires is provided upright on the surface of the first conductive region and the second conductive nanowires is provided upright on the surface of the second conductive region.[6] The method for producing a bonded body according to any one of [1] to [5], further comprising a heating step of heating the contacted first conductive nanowire and the second conductive nanowire, wherein the heating step is carried out simultaneously with the bonding step and the heating step is carried out after the bonding step. [7] The method for producing a bonded body according to [6], wherein the heating temperature in the heating step is 150 to 300°C. [8] The method for producing a bonded body according to any one of [1] to [4], wherein the step of obtaining the first structure includes a process of adhering a composition containing the first conductive nanowire to the first conductive region, and the step of obtaining the second structure includes a process of adhering a composition containing the second conductive nanowire to the second conductive region. [9] The method for producing a bonded body according to any one of [1] to [8], wherein at least one of the first structure and the second structure includes a semiconductor element.
[10] A structure set for use in manufacturing a junction, comprising: a first structure having a first conductive region and a plurality of first conductive nanowires provided in the first conductive region; and a second structure having a second conductive region and a plurality of second conductive nanowires provided in the second conductive region, wherein the arithmetic mean length of exposed portions of the plurality of first conductive nanowires and the arithmetic mean length of exposed portions of the plurality of second conductive nanowires are both 1 to 40 μm.
[0008] According to the present invention, it is possible to provide a method for manufacturing a bonded body that has excellent bonding strength even when the bonding time is short, and a structure set used for manufacturing the bonded body.
[0009] 1 is a schematic cross-sectional view showing an example of a first structure in the structure set of the present invention. FIG. 1 is a schematic cross-sectional view showing an example of a first structure in the structure set of the present invention. FIG. 2 is a schematic cross-sectional view showing an example of a first structure in the structure set of the present invention. FIG. 3 is a schematic cross-sectional view showing an example of a second structure in the structure set of the present invention. FIG. 4 is a schematic cross-sectional view showing an example of a step of forming the first structure in the method for producing a bonded body of the present invention. FIG. 5 is a schematic cross-sectional view showing an example of a step of forming the first structure in the method for producing a bonded body of the present invention. FIG. 6 is a schematic cross-sectional view showing an example of a step of forming the first structure in the method for producing a bonded body of the present invention. FIG. 7 is a schematic cross-sectional view showing an example of a step of forming the first structure in the method for producing a bonded body of the present invention. FIG. 8 is a schematic cross-sectional view showing an example of a step of forming the first structure in the method for producing a bonded body of the present invention. FIG. 9 is a schematic cross-sectional view showing an example of a step of forming the first structure in the method for producing a bonded body of the present invention. FIG. 10 is a schematic cross-sectional view showing an example of a step of forming the first structure in the method for producing a bonded body of the present invention.
[0010] The method for manufacturing a bonded body and the structure set of the present invention will be described in detail below based on preferred embodiments shown in the accompanying drawings. The drawings described below are merely illustrative for explaining the present invention, and the present invention is not limited to these drawings. In the following, the "to" symbol indicating a numerical range includes the values written on both sides. For example, when ε is between α and β, the range of ε includes α and β, and expressed in mathematical symbols, α≦ε≦β. Unless otherwise specified, angles such as "perpendicular" include the error range generally accepted in the relevant technical field. Furthermore, unless otherwise specified, environmental factors such as temperature, humidity, or atmospheric pressure also include the error range generally accepted in the relevant technical field.
[0011] [Structure Set] The structure set of the present invention (hereinafter also referred to as "the present structure set") includes a first structure having a first conductive region and a plurality of first conductive nanowires provided in the first conductive region, and a second structure having a second conductive region and a plurality of second conductive nanowires provided in the second conductive region, wherein the arithmetic mean length of the exposed portions of the plurality of first conductive nanowires and the arithmetic mean length of the exposed portions of the plurality of second conductive nanowires are both 1 to 40 μm, and is used to manufacture a bonded body. By using the present structure set, a bonded body with excellent bonding strength can be obtained even with a short bonding time. Although the details of the reason for this are not clear, it is generally presumed as follows. That is, it is presumed that the arithmetic mean length of the exposed portions of the first conductive nanowires of the first structure and the arithmetic mean length of the exposed portions of the second conductive nanowires of the second structure are both predetermined values, thereby allowing the first conductive nanowires and the second conductive nanowires to be sufficiently entangled even with a short bonding process, thereby resulting in excellent bonding strength of the bonded body.
[0012] The structure set is used for manufacturing a bonded body. Specifically, the structure set is used for manufacturing a bonded body obtained by bonding a first structure and a second structure, and is preferably used in a bonding step in the method for manufacturing a bonded body of the present invention described below.
[0013] [First Structure] Fig. 1 is a schematic cross-sectional view showing an example of a first structure included in the structure set of the present invention. The first structure 10 shown in Fig. 1 has a first member 20 having a first conductive region 20a on its surface, and a plurality of first conductive nanowires 14 provided in a part of the first conductive region 20a.
[0014] The first member 20 is a member having a first conductive region 20a on at least a portion of its surface, and examples thereof include a semiconductor element and a substrate having an electrode (e.g., a wiring board and an interposer). For example, when the first structure 10 includes the first member 20 that is a semiconductor element, it can be said that the first structure 10 includes a semiconductor element.
[0015] The first conductive region 20a is a region formed from a conductive material and may be formed on at least a portion of the surface of the first member 20. The conductive material is not particularly limited, and examples thereof include metals. Specific examples of metals include gold (Au), silver (Ag), copper (Cu), aluminum (Al), magnesium (Mg), and nickel (Ni). From the viewpoint of electrical conductivity, copper, gold, aluminum, and nickel are preferred, copper and gold are more preferred, and copper is even more preferred. In addition to metals, oxide conductive materials may be used. Examples of oxide conductive materials include indium-doped tin oxide (ITO). However, metals have superior ductility and are more easily deformed than oxide conductors, even when compressed during bonding. Therefore, it is preferable to use metals. The conductor may also be made of a conductive resin containing nanoparticles of Cu or Ag, for example.
[0016] 1, the multiple first conductive nanowires 14 are erected on the surface of the first conductive region 20a. Specifically, the multiple first conductive nanowires 14 extend in a direction intersecting the surface of the first conductive region 20a (i.e., in a direction along the thickness direction Dt of the first structure 10). One end of each of the multiple first conductive nanowires 14 is in contact with the first conductive region 20a.
[0017] The first conductive nanowires 14 have electrical conductivity. The first conductive nanowires 14 are made of a conductive material, and specific examples and preferred aspects of the conductive material are the same as those of the conductive material that makes up the first conductive region 20a.
[0018] The arithmetic mean length ha of the exposed portions of the plurality of first conductive nanowires 14 is 1 to 40 μm. The arithmetic mean length ha of the exposed portions of the plurality of first conductive nanowires 14 is preferably 3 μm or more, more preferably 5 μm or more, in terms of achieving better effects of the present invention. The arithmetic mean length ha of the exposed portions of the plurality of first conductive nanowires 14 is preferably 20 μm or less, more preferably 10 μm or less. When the arithmetic mean length ha is 20 μm or less (particularly 10 μm or less), there is an advantage in that there are fewer regions (voids) where no conductive nanowires are present when a bonded body is formed, eliminating the need to fill the voids with resin or the like. Another advantage is that the time required to form the conductive nanowires can be shortened, and the time required to remove the anodic oxide film, which will be described later, can be shortened.
[0019] When the first conductive nanowires 14 are provided upright on the surface of the first conductive region 20a (see FIG. 1 ), the arithmetic mean length ha can be determined by, for example, cutting the first structure 10 in the thickness direction Dt, obtaining a cross-sectional image of the cut surface using a field emission scanning electron microscope (FE-SEM), measuring the lengths of the exposed portions of 100 first conductive nanowires based on the cross-sectional image, and calculating the arithmetic mean value of these lengths as the length of the exposed portions of the first conductive nanowires 14 (i.e., the arithmetic mean length). On the other hand, when the first conductive nanowires 14 are not provided upright on the first conductive region 20a (see FIG. 3 described below), the arithmetic mean length ha can be determined by, for example, obtaining a surface image of the first conductive region 20a using a field emission scanning electron microscope (FE-SEM), measuring the lengths of the exposed portions of 100 first conductive nanowires based on the surface image, and calculating the arithmetic mean value of these lengths as the length of the exposed portions of the first conductive nanowires 14 (i.e., the arithmetic mean length).
[0020] In order to obtain a superior effect of the present invention, the standard deviation of the lengths of the exposed portions of the first conductive nanowires 14 is preferably 2 μm or less, more preferably 1.5 μm or less, and even more preferably 1 μm or less. The lower limit of the standard deviation of the lengths of the exposed portions of the first conductive nanowires 14 is 0.01 μm. The standard deviation of the lengths of the exposed portions of the first conductive nanowires can be determined by a method such as calculating the arithmetic mean length ha of the exposed portions of the first conductive nanowires 14 from the lengths of the exposed portions of 100 first conductive nanowires that were used to measure the arithmetic mean length ha of the exposed portions of the first conductive nanowires 14.
[0021] The average diameter d of the first conductive nanowires 14 is preferably 45 to 75 nm, more preferably 45 to 60 nm, and even more preferably 50 to 60 nm. When the average diameter d is 45 nm or more, the strength of the conductive nanowires is superior. When the average diameter d is 75 nm or less, the nanowires are sufficiently entangled when bonded, resulting in superior bonding strength. When the first conductive nanowires 14 are erected on the surface of the first conductive region 20a, the average diameter of the first conductive nanowires 14 can be determined by, for example, obtaining a surface image of the first conductive region 20a using a field emission scanning electron microscope (FE-SEM), measuring the diameters (circle equivalent diameters) of 100 first conductive nanowires based on the surface image, and calculating the arithmetic mean of these diameters as the average diameter of the first conductive nanowires 14. When the first conductive nanowires 14 are not erected in the first conductive region 20a, the average diameter of the first conductive nanowires 14 can be determined by cutting the first structure 10 in the thickness direction Dt, obtaining a cross-sectional image of the cut surface using a field emission scanning electron microscope (FE-SEM), measuring the diameters (circle equivalent diameters) of 100 first conductive nanowires based on the cross-sectional image, and calculating the arithmetic mean value of these diameters as the average diameter of the first conductive nanowires 14.
[0022] The coverage area of the first conductive nanowires 14 with respect to the surface area of the first conductive region 20a is preferably 10 to 60%, and from the viewpoint of more excellent effects of the present invention, is more preferably 20 to 50%, even more preferably 30 to 50%, and particularly preferably 30 to 40%. The coverage area of the first conductive nanowires 14 can be determined by a method such as using a field emission scanning electron microscope (FE-SEM) to obtain surface images of 10 different locations in the first conductive region 20a, determining the coverage area (%) of the first conductive nanowires 14 with respect to the surface area of the first conductive region 20a for each surface image, and setting the arithmetic mean value of these values as the coverage area (%) of the first conductive nanowires 14 with respect to the surface area of the first conductive region 20a.
[0023] 1 shows an embodiment in which all of the side surfaces of the plurality of first conductive nanowires 14 are exposed, but this is not limiting. For example, as shown in FIG. 2, a portion of the side surfaces of the plurality of first conductive nanowires 14 may be covered with an insulating film or the like. Specifically, in the example of FIG. 2, the first structure 10 further includes an insulating film 12 having electrical insulation properties, and the plurality of first conductive nanowires 14 penetrate the insulating film 12 in the thickness direction. In this case, one end of each of the plurality of first conductive nanowires 14 is in contact with the first conductive region 20a. The other end of each of the plurality of first conductive nanowires 14 protrudes from the surface 12a of the insulating film 12, and a portion of each of the plurality of first conductive nanowires 14 is exposed from the insulating film 12.
[0024] 2, the insulating film 12 has a plurality of pores 13 penetrating in the thickness direction Dt. The plurality of pores 13 are provided with first conductive nanowires 14. The insulating film 12 is made of, for example, an inorganic material. 14Materials having an electrical resistivity of approximately Ω·cm can be used. The term "made of an inorganic material" is used to distinguish it from a polymeric material and does not limit the definition to an insulating substrate composed solely of inorganic materials, but rather refers to a substrate containing inorganic materials as the main component (50% by mass or more). The insulating film 12 is, for example, an anodized oxide film. The insulating film 12 can also be composed of, for example, ceramics such as metal oxides, metal nitrides, glass, silicon carbide, and silicon nitride, carbon substrates such as diamond-like carbon, polyimides, composites of these, and the like. Alternatively, the insulating film 12 may be formed, for example, on an organic material having through-holes, using an inorganic material containing 50% by mass or more of a ceramic material or a carbon material.
[0025] 1 shows an example in which the plurality of first conductive nanowires 14 are erected on the surface of the first conductive region 20a, but is not limited to such an example. For example, as shown in Fig. 3, the plurality of first conductive nanowires 14 may not be erected on the first conductive region 20a, but may be arranged along the in-plane direction of the first conductive region 20a (i.e., the direction intersecting with the thickness direction Dt of the first structure 10).
[0026] [Second Structure] Figure 4 is a schematic cross-sectional view showing an example of a second structure included in the structure set of the present invention. In Figure 4, components that are the same as those shown in Figure 1 are given the same reference numerals, and their description will be omitted. The second structure 100 shown in Figure 4 has a second member 20 having a second conductive region 20a on its surface, and a plurality of second conductive nanowires 14 provided in a part of the second conductive region 20a. In the example of Figure 4, an embodiment is shown in which the second structure 100 does not have an insulating film 12, but the second structure 100 may have an insulating film 12, as in the example of Figure 2.
[0027] The arithmetic mean length ha of the exposed portions of the plurality of second conductive nanowires 14 is 1 to 40 μm. The preferred embodiment and method for measuring the arithmetic mean length ha of the exposed portions of the plurality of second conductive nanowires 14 are similar to those for the arithmetic mean length ha of the exposed portions of the plurality of first conductive nanowires 14, and therefore a description thereof will be omitted.
[0028] The preferred embodiment and calculation method for the standard deviation of the length of the exposed portion of the second conductive nanowires 14 are similar to those for the standard deviation of the length of the exposed portion of the first conductive nanowires 14, and therefore a description thereof will be omitted.
[0029] The preferred embodiment and method of measuring the average diameter d of the second conductive nanowires 14 are the same as those for the average diameter d of the first conductive nanowires 14, and therefore the description thereof will be omitted.
[0030] The preferred embodiments and measurement methods for the coverage area of the second conductive nanowires 14 relative to the surface area of the second conductive region 20a are similar to those for the coverage area of the first conductive nanowires 14 relative to the surface area of the first conductive region 20a, and therefore will not be described here.
[0031] In the example of Figure 4, a configuration is shown in which multiple second conductive nanowires 14 are erected on the surface of the second conductive region 20a, but as in the configuration shown in Figure 3, the second conductive nanowires 14 may not be erected on the second conductive region 20a, but may be arranged along the in-plane direction of the second conductive region 20a.
[0032] [Preferred embodiment of structure set] In order to obtain better effects of the present invention, the structure set is preferably an embodiment in which both of the first structure and the second structure have the structure shown in FIG. 1 (FIG. 4), or one has the structure shown in FIG. 1 (FIG. 4) and the other has the structure shown in FIG. 3, and more preferably an embodiment in which both have the structure shown in FIG. 1 (FIG. 4).
[0033] [Method for manufacturing bonded structure] The method for manufacturing a bonded structure of the present invention (hereinafter also referred to as "the present manufacturing method") is a method for manufacturing a bonded structure obtained by bonding a first structure and a second structure, and includes the steps of: providing a plurality of first conductive nanowires in a first conductive region of a first member having a first conductive region on its surface, to obtain the first structure having the first conductive nanowires (hereinafter also referred to as "first structure forming step"); providing a plurality of second conductive nanowires in a second conductive region of a second member having a second conductive region on its surface, to obtain the second structure having the second conductive nanowires (hereinafter also referred to as "second structure forming step"); and a bonding step of arranging the first conductive nanowires and the second conductive nanowires so that they are in contact with each other, to bond the first structure and the second structure, wherein the arithmetic mean length of exposed portions of the plurality of first conductive nanowires and the arithmetic mean length of exposed portions of the plurality of second conductive nanowires are both 1 to 40 μm.
[0034] According to this manufacturing method, a bonded body having excellent bonding strength can be obtained even with a short bonding time. Although the details of the reason for this are not clear, it is generally assumed as follows. That is, since the arithmetic mean length of the exposed portions of the first conductive nanowires of the first structure and the arithmetic mean length of the exposed portions of the second conductive nanowires of the second structure are both predetermined values, the first conductive nanowires and the second conductive nanowires are sufficiently entangled even with a short bonding process, which is assumed to result in excellent bonding strength of the bonded body.
[0035] An example of this manufacturing method will be described below step by step with reference to the drawings.
[0036] [First structure formation step]
[0037] 5 to 12 are schematic cross-sectional views showing an example of the first structure formation step in the present manufacturing method in the order of steps. In this example of the first structure manufacturing method, a method of forming conductive nanowires using an anodized aluminum film will be described. An aluminum substrate is used to form the anodized aluminum film. Therefore, in this example of the first structure manufacturing method, an aluminum substrate 30 is first prepared, as shown in FIG. 5 . The size and thickness of the aluminum substrate 30 are determined appropriately depending on the arithmetic mean length ha of the exposed portions of the first conductive nanowires 14 in the final structure 10 (see FIG. 1 ), the processing equipment, and other factors. The aluminum substrate 30 is, for example, a rectangular plate. Note that the aluminum substrate is not limited to an aluminum substrate, and any metal substrate on which an electrically insulating insulating film 12 can be formed can be used.
[0038] The aluminum constituting the aluminum substrate 20 is not particularly limited, and specific examples include pure aluminum and aluminum alloys containing aluminum as the main component and trace amounts of other elements. The aluminum purity is preferably 99.5% by mass or more, more preferably 99.9% by mass or more, and even more preferably 99.99% by mass or more. When the aluminum purity is within the above range, the through-hole arrangement has sufficient regularity.
[0039] Furthermore, when forming an anodized film on the aluminum substrate 20, it is preferable that the surface to be anodized be subjected to heat treatment, degreasing treatment, and mirror finish treatment in advance. The heat treatment, degreasing treatment, and mirror finish treatment may be the same as those described in paragraphs
[0044] to
[0054] of JP 2008-270158 A.
[0040] Next, one surface 30a (see FIG. 5) of the aluminum substrate 30 is anodized. As a result, one surface 30a (see FIG. 5) of the aluminum substrate 30 is anodized, and an insulating film 12 having a plurality of pores 13 extending in the thickness direction Dt of the aluminum substrate 30, i.e., an anodic oxide film 15, is formed as shown in FIG. 6. A barrier layer 31 exists at the bottom of each pore 13. The above-mentioned anodization process is called an anodization process.
[0041] Although a conventionally known method can be used for the anodizing treatment step, it is preferable to use a self-ordering method or a constant voltage treatment from the viewpoint of increasing the regularity of the arrangement of the through holes or the arrangement of the recesses. Here, the self-ordering method and constant voltage treatment of the anodizing treatment can be the same as the treatments described in paragraphs
[0056] to
[0108] and FIG. 3 of JP 2008-270158 A.
[0042] As described above, the insulating film 12 having a plurality of pores 13 has a barrier layer 31 at the bottom of each pore 13. However, the barrier layer 31 shown in FIG. 6 is removed. This results in an insulating film 12 having a plurality of pores 13 without the barrier layer 31 (see FIG. 7). The process of removing the barrier layer 31 is referred to as a barrier layer removal process. In the barrier layer removal process, an alkaline aqueous solution containing ions of a metal M1, which has a higher hydrogen overvoltage than aluminum, is used to remove the barrier layer 31 from the insulating film 12. At the same time, a metal layer 35a (see FIG. 7) made of a metal (metal M1) is formed on the surface 32d (see FIG. 7) of the bottom 32c (see FIG. 7) of the pore 13. This allows the aluminum substrate 30 exposed in the pore 13 to be covered with the metal layer 35a. This facilitates the plating process when the pores 13 are filled with metal by plating, thereby preventing the pores from being insufficiently filled with metal and preventing the pores from being left unfilled with metal, thereby preventing poor formation of the first conductive nanowires 14. The alkaline aqueous solution containing ions of the metal M1 may further contain an aluminum ion-containing compound (sodium aluminate, aluminum hydroxide, aluminum oxide, etc.). The content of the aluminum ion-containing compound, converted into the amount of aluminum ions, is preferably 0.1 to 20 g / L, more preferably 0.3 to 12 g / L, and even more preferably 0.5 to 6 g / L.
[0043] In the barrier layer removal step, metal layer 35a made of a metal (metal M1) is formed on the bottom of pore 13, but the present invention is not limited to this. For example, only barrier layer 31 may be removed to expose aluminum substrate 30 at the bottom of pore 13, and aluminum substrate 30 may be used as an electrode for electrolytic plating in the exposed state.
[0044] The barrier layer removal step may be performed by, for example, using Cl 2 Alternatively, dry etching may be performed using a gas species such as a mixed gas of Ar and Ar.
[0045] Next, plating is performed on the surface 12a of the insulating film 12, which has a plurality of pores 13 extending in the thickness direction Dt. In this case, the metal layer 35a can be used as an electrode for electrolytic plating. Metal 35b is used for plating, and plating proceeds starting from the metal layer 35a formed on the surface 32d (see FIG. 7) of the bottom 32c (see FIG. 7) of the pore 13. As a result, as shown in FIG. 8, the pores 13 of the insulating film 12 are filled with the metal 35b constituting the first conductive nanowires 14. By filling the pores 13 with the metal 35b, first conductive nanowires 14 having electrical conductivity are formed. The metal layer 35a and the metal 35b are collectively referred to as the filled metal 35. The process of filling the pores 13 of the insulating film 12 with the metal 35b is referred to as the metal filling process. As described above, the first conductive nanowires 14 are not limited to being made of metal, and a conductive material can also be used. Electrolytic plating, for example, is used for the metal filling process. The surface 12 a of the insulating film 12 corresponds to one surface of the insulating film 12 .
[0046] The metal filling step is not limited to plating, and may be performed by ink jetting, transferring, spraying, screen printing, or the like to fill the inside of the pores 13 with a conductive material.
[0047] 9 , after the metal filling step, the surface 12a of the insulating film 12 on the side where the aluminum substrate 30 is not provided is partially removed in the thickness direction Dt, and the metal 35 filled in the metal filling step is made to protrude from the surface 12a of the insulating film 12. That is, the first conductive nanowires 14 are made to protrude from the surface 12a of the insulating film 12. The step of making the first conductive nanowires 14 protrude from the surface 12a of the insulating film 12 is called a surface metal protrusion step. The surface metal protrusion step allows the arithmetic mean length ha of the exposed portions of the plurality of first conductive nanowires 14 to fall within the above-mentioned range.
[0048] After the surface metal protruding step, the aluminum substrate 30 is removed as shown in Fig. 10. The step of removing the aluminum substrate 30 is called a substrate removing step. In this embodiment, an example in which the substrate removing step is performed after the surface metal protruding step is shown, but the present invention is not limited to this, and the substrate removing step may be performed before the surface metal protruding step.
[0049] After the substrate removal step, one surface 12a of the insulating film 12 and the surface of the first conductive region 20a of the first member 20 are arranged to face each other, and the ends of the first conductive nanowires 14 protruding from the surface 12a of the insulating film 12 are connected to the first conductive region 20a, as shown in Fig. 11. The step of connecting the first conductive nanowires 14 to the first conductive region 20a is called a member connecting step.
[0050] In the member connecting step, the connection between the first conductive nanowires 14 and the first conductive region 20a is preferably performed by applying pressure. The pressure conditions are not particularly limited, but are preferably 50 MPa or less, more preferably 30 MPa or less, and even more preferably 10 MPa or less. The lower limit of the pressure during pressing is preferably 1 MPa or more. The pressing time is not particularly limited, but is preferably 1 second to 60 minutes, and more preferably 5 seconds to 10 minutes.
[0051] Furthermore, in the member joining step, the connection between the first conductive nanowires 14 and the first conductive region 20a is preferably carried out under heating. The heating temperature is preferably 150 to 300°C, more preferably 170 to 300°C, and even more preferably 200 to 300°C. Heating may be carried out so that the heating temperature is increased in stages. The heating time is not particularly limited, but is preferably 1 second to 60 minutes, and more preferably 5 seconds to 10 minutes. The heating in the member joining step is preferably carried out together with the above-mentioned pressure application.
[0052] After the member connecting step, the insulating film 12 is removed (see FIG. 12 ). This results in a first structure 10. The step of removing the insulating film 12 is called an insulating film removing step. There is no particular limitation on the method for removing the insulating film 12, but for example, the insulating film 12 can be removed by dissolving it by etching. For the etching, a treatment liquid that dissolves the insulating film 12 but does not dissolve the first conductive nanowires 14 is used. When the insulating film 12 is made of aluminum oxide and the first conductive nanowires 14 are made of copper, for example, NaOH (sodium hydroxide) is used as the treatment liquid. The removal of the insulating film 12 is not limited to etching, and is not particularly limited as long as it can be removed without damaging the first conductive nanowires 14.
[0053] 5 to 12 show a method for obtaining a first structure 10 in which a plurality of first conductive nanowires 14 are erected on the surface of the first conductive region 20a, but the method for producing the first structure 10 is not limited to this. A first structure 10 in which a plurality of first conductive nanowires 14 are arranged along the in-plane direction of the first conductive region 20a as shown in Fig. 3 can be produced, for example, by a method of adhering a conductive composition containing the first conductive nanowires 14 to the surface of the first conductive region 20a in the first member 20.
[0054] (Conductive Composition) The conductive composition contains first conductive nanowires 14. The content of the first conductive nanowires 14 is preferably 50 to 95 mass %, more preferably 70 to 95 mass %, and even more preferably 80 to 95 mass %, relative to the total mass of the conductive composition.
[0055] The first conductive nanowires contained in the conductive composition can be obtained, for example, by removing the entire insulating film 12 during the surface metal protrusion step and then performing a substrate removal step.
[0056] The conductive composition may further contain a polymer material. The polymer material contained in the resin layer is not particularly limited, but is preferably a thermosetting resin because it can efficiently fill gaps between the structure and the object to be joined, such as a semiconductor chip or semiconductor wafer, and thereby improve adhesion between the structure and the semiconductor chip or semiconductor wafer. Specific examples of thermosetting resins include acrylonitrile resin, epoxy resin, phenolic resin, polyimide resin, polyester resin, polyurethane resin, bismaleimide resin, melamine resin, and isocyanate-based resin. Among these, it is preferable to use at least one of a polyimide resin and an epoxy resin because of improved insulation reliability and excellent chemical resistance.
[0057] When the conductive composition contains a polymer material, the content of the polymer material is preferably 5 to 50 mass %, more preferably 5 to 30 mass %, and even more preferably 5 to 20 mass %, relative to the total mass of the conductive composition.
[0058] The conductive composition may further contain an antioxidant. Specific examples of antioxidant materials include 1,2,3,4-tetrazole, 5-amino-1,2,3,4-tetrazole, 5-methyl-1,2,3,4-tetrazole, 1H-tetrazole-5-acetic acid, 1H-tetrazole-5-succinic acid, 1,2,3-triazole, 4-amino-1,2,3-triazole, 4,5-diamino-1,2,3-triazole, 4-carboxy-1H-1,2,3-triazole, 4,5-dicarboxy-1H-1,2,3-triazole, 1H-1,2,3-triazole-4-acetic acid, 4-carboxy-5-carboxymethyl-1H-1,2,3-triazole, and 1,2,4-triazole. Examples of suitable benzotriazoles include benzotriazole, 3-amino-1,2,4-triazole, 3,5-diamino-1,2,4-triazole, 3-carboxy-1,2,4-triazole, 3,5-dicarboxy-1,2,4-triazole, 1,2,4-triazole-3-acetic acid, 1H-benzotriazole, 1H-benzotriazole-5-carboxylic acid, benzofuroxan, 2,1,3-benzothiazole, o-phenylenediamine, m-phenylenediamine, catechol, o-aminophenol, 2-mercaptobenzothiazole, 2-mercaptobenzimidazole, 2-mercaptobenzoxazole, melamine, and derivatives thereof. Of these, benzotriazole and its derivatives are preferred. Benzotriazole derivatives include substituted benzotriazoles having a hydroxyl group, an alkoxy group (e.g., a methoxy group, an ethoxy group, etc.), an amino group, a nitro group, an alkyl group (e.g., a methyl group, an ethyl group, a butyl group, etc.), a halogen atom (e.g., a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, etc.) on the benzene ring of benzotriazole. Further examples include naphthalenetriazole, naphthalenebistriazole, and similarly substituted naphthalenetriazoles and substituted naphthalenebistriazoles.
[0059] Other examples of antioxidant materials contained in the resin layer include common antioxidants such as higher fatty acids, higher fatty acid copper salts, phenolic compounds, alkanolamines, hydroquinones, copper chelating agents, organic amines, and organic ammonium salts.
[0060] When the conductive composition contains an antioxidant, the content of the antioxidant is preferably 0.0001 mass % or more, more preferably 0.001 mass % or more, relative to the total mass of the conductive composition, and is preferably 5.0 mass % or less, more preferably 2.5 mass % or less, in order to obtain an appropriate electrical resistance in the present joining process.
[0061] The conductive composition may further contain a migration inhibitor, which can further improve insulation reliability by trapping metal ions, halogen ions, and metal ions derived from the semiconductor chip and semiconductor wafer.
[0062] Specific examples of the migration-preventing material include an ion exchanger, specifically a mixture of a cation exchanger and an anion exchanger, or a cation exchanger alone. Here, the cation exchanger and the anion exchanger can be appropriately selected from, for example, inorganic ion exchangers and organic ion exchangers, respectively, as described below.
[0063] Examples of inorganic ion exchangers include hydrous oxides of metals, such as hydrous zirconium oxide. Known metal types include zirconium, iron, aluminum, tin, titanium, antimony, magnesium, beryllium, indium, chromium, and bismuth. Among these, zirconium-based ion exchangers have a cation of Cu. 2+ , Al 3+ In addition, the iron-based materials have the ability to exchange Ag. + , Cu 2+ Similarly, tin-, titanium-, and antimony-based cation exchangers are cation exchangers. On the other hand, bismuth-based cation exchangers have the ability to exchange anions such as Cl. -They have the ability to exchange ions. Zirconium-based ion exchangers also exhibit anion exchange capacity depending on the manufacturing conditions. The same is true for aluminum-based and tin-based ion exchangers. Other inorganic ion exchangers known include acid salts of polyvalent metals such as zirconium phosphate, heteropolyacid salts such as ammonium molybdophosphate, and synthetic products such as insoluble ferrocyanides. Some of these inorganic ion exchangers are already commercially available, for example, various grades of the product name "IXE" from Toagosei Co., Ltd. are known. In addition to synthetic products, powders of inorganic ion exchangers such as natural zeolite or montmorillonite can also be used.
[0064] Examples of organic ion exchangers include crosslinked polystyrenes having sulfonic acid groups as cation exchangers, as well as those having carboxylic acid groups, phosphonic acid groups, or phosphinic acid groups, and crosslinked polystyrenes having quaternary ammonium groups, quaternary phosphonium groups, or tertiary sulfonium groups as anion exchangers.
[0065] These inorganic and organic ion exchangers may be appropriately selected taking into consideration the types of cations and anions to be captured and the exchange capacity for those ions. It goes without saying that inorganic and organic ion exchangers may be used in combination. Since the manufacturing process of electronic devices includes a heating process, inorganic ion exchangers are preferred.
[0066] When the conductive composition contains a migration inhibitor, the content of the migration inhibitor is preferably 0.0001 mass% or more, more preferably 0.001 mass% or more, and even more preferably 0.001 mass% or more, relative to the total mass of the conductive composition, and is preferably 3 mass% or less, more preferably 1 mass% or less, and even more preferably 0.5 mass% or less, relative to the total mass of the conductive composition.
[0067] The mixing ratio of the ion exchanger to the polymer material is, for example, preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 2.5% by mass or less, from the viewpoint of mechanical strength. Furthermore, from the viewpoint of suppressing migration when a semiconductor chip or semiconductor wafer is bonded to a structure, the mixing ratio of the ion exchanger is preferably 0.01% by mass or more.
[0068] The resin layer may further contain a curing agent. When a curing agent is contained, it is more preferable to use a curing agent that is liquid at room temperature rather than a curing agent that is solid at room temperature, from the viewpoint of suppressing poor bonding with the surface shape of the semiconductor chip or semiconductor wafer to be connected. Here, "solid at room temperature" means a substance that is solid at 25°C, for example, a substance whose melting point is higher than 25°C.
[0069] Specific examples of the curing agent include aromatic amines such as diaminodiphenylmethane and diaminodiphenylsulfone, aliphatic amines, imidazole derivatives such as 4-methylimidazole, dicyandiamide, tetramethylguanidine, thiourea adduct amine, carboxylic acid anhydrides such as methylhexahydrophthalic anhydride, carboxylic acid hydrazides, carboxylic acid amides, polyphenol compounds, novolac resins, and polymercaptans, and any curing agent that is liquid at 25° C. can be appropriately selected and used from these curing agents. The curing agents may be used alone or in combination of two or more.
[0070] When the conductive composition contains a curing agent, the content of the curing agent is preferably 0.0001% by mass or more, more preferably 0.001% by mass or more, relative to the total mass of the conductive composition, and is preferably 3% by mass or less, more preferably 1% by mass or less, and even more preferably 0.5% by mass or less, relative to the total mass of the conductive composition.
[0071] The conductive composition may contain various additives, such as dispersants, buffers, viscosity adjusters, inorganic fillers, monomer components (e.g., bisallylphenol, etc.), and polymerization initiators (e.g., maleimide compounds, etc.), which are commonly added to resin insulating films in semiconductor packages, within the range that does not impair its properties.
[0072] (Attachment Method) Examples of methods that can be used to attach the conductive composition to the surface of the first conductive region 20a of the first member 20 include inkjet printing, screen printing, jet printing, a dispenser, a jet dispenser, a comma coater, a slit coater, a die coater, a gravure coater, a slit coat, letterpress printing, intaglio printing, gravure printing, stencil printing, a bar coat, an applicator, a spray coater, and electro-deposition coating.
[0073] The amount of the conductive composition to be applied is not particularly limited, but for example, the conductive composition can be applied in an amount such that the thickness of the conductive composition becomes 1 to 100 μm.
[0074] After the conductive composition is applied to the surface of the first conductive region 20a, a step of drying the conductive composition may be included. The drying method may include drying at room temperature, drying by heating, or drying under reduced pressure. For drying by heating or drying under reduced pressure, a hot plate, a warm air dryer, a warm air heating furnace, a nitrogen dryer, an infrared dryer, an infrared heating furnace, a far-infrared heating furnace, a microwave heating device, a laser heating device, an electromagnetic heating device, a heater heating device, a steam heating furnace, a hot plate press, or the like may be used. The drying temperature and time are preferably adjusted appropriately depending on the type and amount of the dispersion medium used; for example, drying at 50 to 300°C for 1 to 180 minutes is preferred. Furthermore, from the viewpoint of suppressing oxidation of the metal, drying may be performed in a non-oxidizing or reducing atmosphere. Examples of suitable methods include substitution with a non-oxidizing gas such as argon, nitrogen, or water vapor, hydrogen, or formic acid, or spraying.
[0075] [Second Structure Forming Step] Specific examples of the method for manufacturing the second structure 100 (second structure forming step) include the same method as the first structure forming step described above, and therefore a description thereof will be omitted.
[0076] 13 to 15 are schematic cross-sectional views showing an example of the bonding step in the manufacturing method in the order of steps. In the bonding step, first, the surface of the first conductive region 20a on which the first conductive nanowires 14 are formed is arranged to face the surface of the second conductive region 20a on which the second conductive nanowires 14 are formed (see FIG. 13).
[0077] Next, the first structure 10 and the second structure 100 are brought close to each other and positioned so that the first conductive nanowires 14 and the second conductive nanowires 14 are in contact with each other, and bonding is initiated (see FIG. 14 ). In this case, it is preferable to apply pressure to the first structure 10 and the second structure 100 to bond them together. The pressure conditions are not particularly limited, but are preferably 50 MPa or less, more preferably 30 MPa or less, and particularly preferably 10 MPa or less. The lower limit of the pressure when applying pressure is preferably 1 MPa or more. The time for the bonding step is not particularly limited, but is preferably 1 second to 60 minutes, and more preferably 5 seconds to 10 minutes. When pressure is applied in the bonding step, the time for the bonding step corresponds to the pressure application time.
[0078] The atmosphere during bonding may be air, an inert gas such as nitrogen or argon, a reducing gas such as hydrogen or carboxylic acid, or a mixed gas of these inert gases and reducing gases. The atmosphere during bonding may also be a reduced-pressure atmosphere, including a vacuum atmosphere. Any of the above atmospheres can be achieved by a known method.
[0079] By carrying out the above steps, the first structure 10 and the second structure 100 are bonded together to obtain a bonded body 200 (see FIG. 15).
[0080] [Heating Step] The present manufacturing method preferably further includes a heating step of heating the contacted first conductive nanowires 14 and second conductive nanowires 14. The heating step preferably satisfies at least one of the following conditions: being performed simultaneously with the bonding step, or being performed after the bonding step.
[0081] The heating temperature is preferably 150 to 300°C, more preferably 170 to 300°C, and even more preferably 200 to 300°C. The heating step may be carried out so that the heating temperature is changed stepwise. The heating time is not particularly limited, but is preferably 1 second to 60 minutes, and more preferably 5 seconds to 10 minutes.
[0082] The bond strength of the bonded body 200 obtained by this manufacturing method is preferably 5 MPa or more, more preferably 20 MPa or more, and even more preferably 30 MPa or more. The bond strength can be measured according to the method described in the examples below.
[0083] The present invention is basically configured as described above. While the structure set of the present invention and the method for manufacturing the bonded body of the present invention have been described in detail above, the present invention is not limited to the above-described embodiments, and various improvements and modifications may be made without departing from the spirit and scope of the present invention.
[0084] The features of the present invention will be explained in more detail below with reference to examples. The materials, reagents, amounts and proportions of substances, and procedures shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention is not limited to the following examples.
[0085] [Example 1] The bonded structure of Example 1 was manufactured as follows. [Step of Forming First Structure A] <Preparation of Aluminum Substrate> A molten aluminum alloy containing 0.06% by mass of Si, 0.30% by mass of Fe, 0.005% by mass of Cu, 0.001% by mass of Mn, 0.001% by mass of Mg, 0.001% by mass of Zn, and 0.03% by mass of Ti, with the remainder being Al and unavoidable impurities, was prepared. The molten aluminum alloy was then treated and filtered, and an ingot measuring 500 mm thick and 1200 mm wide was produced by DC (Direct Chill) casting. The surface was then scraped off to an average thickness of 10 mm using a facing mill, and the ingot was then soaked at 550°C for approximately 5 hours. When the temperature dropped to 400°C, it was rolled into a 2.7 mm thick plate using a hot rolling mill. Further, the aluminum substrate was subjected to heat treatment at 500°C using a continuous annealing machine, and then cold-rolled to a thickness of 1.0 mm to obtain an aluminum substrate of JIS 1050. This aluminum substrate was cut to a width of 1030 mm and then subjected to the following treatments.
[0086] <Electrolytic Polishing Treatment> The above-mentioned aluminum substrate was subjected to electrolytic polishing treatment using an electrolytic polishing solution having the following composition under conditions of a voltage of 25 V, a solution temperature of 65°C, and a solution flow rate of 3.0 m / min. A carbon electrode was used as the cathode, and a GP0110-30R (manufactured by Takasago Machinery Co., Ltd.) was used as the power source. The flow rate of the electrolyte was measured using a vortex flow monitor FLM22-10PCW (manufactured by AS ONE Corporation).
[0087] (Electropolishing solution composition) 85 mass % phosphoric acid (reagent manufactured by Wako Pure Chemical Industries, Ltd.) 660 mL, purified water 160 mL, sulfuric acid 150 mL, ethylene glycol 30 mL
[0088] <Anodizing Treatment Step> Next, the aluminum substrate after electrolytic polishing treatment was subjected to anodizing treatment by a self-ordering method according to the procedure described in JP 2007-204802 A. The aluminum substrate after electrolytic polishing treatment was subjected to a pre-anodizing treatment for 5 hours in a 0.50 mol / L oxalic acid electrolytic solution under conditions of a voltage of 40 V, a solution temperature of 16 ° C, and a solution flow rate of 3.0 m / min. Thereafter, the aluminum substrate after pre-anodizing treatment was subjected to a film removal treatment by immersing it in a mixed aqueous solution (liquid temperature: 50 ° C) of 0.2 mol / L chromic anhydride and 0.6 mol / L phosphoric acid for 12 hours. Thereafter, a re-anodizing treatment was performed for 3 hours and 45 minutes in a 0.50 mol / L oxalic acid electrolytic solution under conditions of a voltage of 40 V, a solution temperature of 16 ° C, and a solution flow rate of 3.0 m / min, to obtain an anodized film with a film thickness of 30 μm. In both the pre-anodizing treatment and the re-anodizing treatment, a stainless steel electrode was used as the cathode, and a GP0110-30R power supply (manufactured by Takasago Machinery Co., Ltd.) was used. A NeoCool BD36 (manufactured by Yamato Scientific Co., Ltd.) was used as the cooling device, and a Pair Stirrer PS-100 (manufactured by EYELA Tokyo Rikakikai Co., Ltd.) was used as the stirring / heating device. Furthermore, the flow rate of the electrolyte was measured using a vortex flow monitor FLM22-10PCW (manufactured by AS ONE Corporation).
[0089] <Barrier Layer Removal Step> After the anodizing step, the aluminum substrate was subjected to an etching treatment by immersion in an alkaline aqueous solution prepared by dissolving zinc oxide in a sodium hydroxide aqueous solution (50 g / L) to a concentration of 2000 ppm at 30°C for 150 seconds, thereby removing the barrier layer at the bottom of the micropores of the anodized film and simultaneously depositing zinc on the exposed surface of the aluminum substrate. The average thickness of the anodized film after the barrier layer removal step was 10 µm.
[0090] <Metal Filling Step> Next, electrolytic plating was performed using the aluminum substrate as the cathode and platinum as the cathode. Specifically, a copper plating solution having the composition shown below was used, and constant-current electrolysis was performed to produce a metal-filled microstructure in which nickel was filled into the micropores. Constant-current electrolysis was performed using a plating device manufactured by Yamamoto Plating Tester Co., Ltd. and a power supply (HZ-3000) manufactured by Hokuto Denko Corporation. After confirming the deposition potential by performing cyclic voltammetry in the plating solution, the process was performed under the conditions shown below. (Copper Plating Solution Composition and Conditions) Copper sulfate 100 g / L Sulfuric acid 50 g / L Hydrochloric acid 15 g / L Temperature 25°C Current density 10 A / dm 2
[0091] The surface of the anodized film after filling the micropores with metal was observed using a field emission scanning electron microscope (FE-SEM), and the presence or absence of sealing with metal in 1,000 micropores was observed, and the sealing rate (number of sealed micropores / 1,000) was calculated to be 98%. Furthermore, the anodized film after filling the micropores with metal was cut in the thickness direction using a focused ion beam (FIB), and the surface of the cross section was photographed (magnification 50,000 times) using a field emission scanning electron microscope (FE-SEM) to confirm the interior of the micropores. It was found that the interior of the sealed micropores was completely filled with metal.
[0092] <Substrate Removal Step> Next, the aluminum substrate was dissolved and removed by immersion in a mixed solution of copper chloride / hydrochloric acid, to produce a metal-filled microstructure having an average thickness of 10 μm.
[0093] <Surface metal protrusion process> After the substrate removal process, the metal-filled microstructure was immersed in an aqueous sodium hydroxide solution (concentration: 5% by mass, liquid temperature: 20°C), and the immersion time was adjusted to selectively dissolve the surface of the anodized film.The structure was then washed with water and dried, causing one end of the conductive nanowire to protrude from the anodized film.
[0094] <Member Connection Step> The conductive nanowires of the metal-filled microstructure (i.e., the ends of the conductive nanowires protruding from the anodized film) were connected to the conductive region of the semiconductor element under pressure and heat to obtain a laminate (see FIG. 11 ). The heating and pressing were performed under conditions of a pressure of 30 MPa and a temperature of 250° C. for 10 minutes.
[0095] <Insulating Film Removal Step> The resulting laminate was immersed in a sodium hydroxide aqueous solution (concentration: 5% by mass, liquid temperature: 20°C) to remove the anodic oxide film from the laminate, thereby obtaining the first structure A in Example 1 (see Figures 1 and 12). The arithmetic mean length ha, the standard deviation of the lengths of the exposed portions, and the average diameter d of the multiple conductive nanowires were determined according to the methods described above. In addition, the coverage area of the conductive nanowires relative to the surface area of the first conductive region was determined according to the methods described above. These results are shown in Tables 1 and 2.
[0096] [Step of Forming Second Structure A] The second structure A in Example 1 was obtained in the same manner as the method for forming the first structure A in Example 1.
[0097] [Bonding Step] First, a laminate obtained by laminating the first structure A and the second structure A so that the conductive nanowires in the first structure A and the conductive nanowires in the second structure A contact each other was placed in the chamber of a wafer bonder (Bondtech WB-1000). -3 After the chamber was evacuated to 100 Pa, nitrogen gas containing 5% hydrogen was introduced into the chamber, and the pressure in the chamber was stabilized at 5 KPa. The chamber was then heated and pressurized at a temperature of 200°C and a pressure of 10 MPa, and this heated and pressurized state was maintained for 5 minutes. In this way, a bonded body 1 of Example 1 was obtained.
[0098] Example 2 A first structure B was obtained in the same manner as the formation process of the first structure A in Example 1, except that the nanopore diameter was changed by adjusting the conditions of the anodization process so that the coverage area and average diameter d were the values shown in the table. Also, a second structure B was obtained in the same manner as the formation process of the first structure B. A bonded body 2 of Example 2 was obtained in the same manner as the bonding process in Example 1, except that the obtained first structure B and second structure B were used.
[0099] Example 3 A bonded body 3 of Example 3 was obtained in the same manner as in Example 1, except that heating was not performed in the bonding step.
[0100] Example 4 A bonded body 4 of Example 4 was obtained in the same manner as in Example 1, except that the heating temperature in the bonding step was changed to 130°C.
[0101] [Example 5] A bonded body 5 of Example 5 was obtained in the same manner as in Example 1, except that a second structure X prepared as follows was used instead of the second structure A, and heating was not performed in the bonding process.
[0102] [Step of Forming Second Structure X] The steps up to the substrate removal step were performed with reference to the step of forming First Structure A in Example 1 to obtain a metal-filled microstructure with an average thickness of 20 μm. Next, the obtained metal-filled microstructure was immersed in a sodium hydroxide aqueous solution (concentration: 5% by mass, liquid temperature: 20°C) to remove the anodic oxide film. In this manner, conductive nanowires were obtained. The obtained conductive nanowires (90 parts by mass), methyl ethyl ketone (5 parts by mass), ethyl acrylate-acrylonitrile copolymer (1.6 parts by mass), maleimide compound (2.2 parts by mass), and bisallylphenol (1.2 parts by mass) were mixed to obtain a paste-like conductive composition 1. Next, the conductive composition 1 was applied to the conductive region of the semiconductor element to a thickness of 10 μm, and then heated at 250°C for 10 minutes to obtain Second Structure X (see FIG. 3 ).
[0103] Example 6 A first structure C was obtained in the same manner as in the formation process of the first structure A in Example 1, except that the film thickness of the anodic oxide film was adjusted so that the arithmetic mean length ha of the exposed portions of the multiple conductive nanowires was the value shown in the table. A second structure C was obtained in the same manner as in the formation process of the first structure C. A bonded body 6 of Example 6 was obtained in the same manner as in the bonding process in Example 1, except that the obtained first structure C and second structure C were used.
[0104] Example 7 A first structure D was obtained in the same manner as the forming process of the first structure A in Example 1, except that the nanopore diameter was changed by adjusting the conditions of the anodization treatment process so that the coverage area and average diameter d became the values shown in the table. A second structure D was obtained in the same manner as the forming process of the first structure D. A bonded body 7 of Example 7 was obtained in the same manner as the bonding process in Example 1, except that the obtained first structure D and second structure D were used.
[0105] Example 8 A first structure E was obtained in the same manner as the formation process of the first structure A in Example 1, except that the nanopore diameter was changed by adjusting the conditions of the anodization process so that the coverage area and average diameter d were the values shown in the table. A second structure E was obtained in the same manner as the formation process of the first structure E. A bonded body 8 of Example 8 was obtained in the same manner as the bonding process in Example 1, except that the obtained first structure E and second structure E were used.
[0106] Examples 9 to 11 Bonded bodies 9 to 11 of Examples 9 to 11 were obtained in the same manner as in Example 1, except that the heating temperature in the bonding step was changed as shown in the table.
[0107] Example 12 A bonded body 12 of Example 12 was obtained in the same manner as in Example 5, except that the heating temperature in the bonding step was changed as shown in the table.
[0108] Example 13 A first structure F was obtained in the same manner as in the formation step of the first structure A in Example 1, except that the copper plating current density was adjusted in the metal filling step so that the standard deviation of the lengths of the exposed portions of the conductive nanowires was the value shown in the table. A bonded body 13 of Example 13 was obtained in the same manner as in the bonding step in Example 1, except that the obtained first structure F and second structure A were used.
[0109] Example 14 A first structure G was obtained in the same manner as the formation step of the first structure A in Example 1, except that the copper plating current density was adjusted in the metal filling step so that the standard deviation of the lengths of the exposed portions of the conductive nanowires was the value shown in the table. A bonded body 14 of Example 14 was obtained in the same manner as the bonding step in Example 1, except that the obtained first structure G and second structure A were used.
[0110] Example 15 A first structure H was obtained in the same manner as in the formation step of the first structure A in Example 1, except that the copper plating current density was adjusted in the metal filling step so that the standard deviation of the lengths of the exposed portions of the conductive nanowires was the value shown in the table. A bonded body 15 of Example 15 was obtained in the same manner as in the bonding step in Example 1, except that the obtained first structure H and second structure A were used.
[0111] Example 16 A bonded body 16 of Example 16 was obtained in the same manner as in Example 1, except that the first structure A and the second structure C were used.
[0112] Example 17 A first structure I was obtained in the same manner as in the formation process of the first structure A in Example 1, except that the nanopore diameter was changed by adjusting the conditions of the anodization process so that the coverage area and average diameter d were the values shown in the table. Further, a second structure I was obtained in the same manner as in the formation process of the first structure I. A bonded body 17 of Example 17 was obtained in the same manner as in the bonding process in Example 1, except that the obtained first structure I and second structure I were used.
[0113] Comparative Example 1 A bonded body H1 of Comparative Example 1 was obtained in the same manner as in Example 1, except that a semiconductor element not provided with conductive nanowires was used instead of the second structural body A.
[0114] [Comparative Example 2] A first structure J was obtained in the same manner as the formation process of the first structure A in Example 1, except that the film thickness of the anodic oxide film was adjusted so that the arithmetic mean length ha of the exposed portions of the multiple conductive nanowires was the value shown in the table. A second structure J was obtained in the same manner as the formation process of the first structure J. A bonded body H2 of Comparative Example 2 was obtained in the same manner as the bonding process in Example 1, except that the obtained first structure J and second structure J were used.
[0115] Comparative Example 3 A bonded body H3 of Comparative Example 3 was obtained in the same manner as in Comparative Example 2, except that the second structure X was used instead of the second structure J.
[0116] [Evaluation Test] <Bonding Strength> The bonding strength of each bonded structure of the Examples and Comparative Examples was evaluated by measuring shear strength using a universal bond tester Dage-4000 (manufactured by Nordson Advanced Technologies Co., Ltd.). The bonding strength was calculated as the bonding strength value per area of the semiconductor element from the obtained breaking load. The results are shown in Tables 1 and 2.
[0117]
[0118]
[0119] As shown in Tables 1 and 2, when the first structure and the second structure were made of conductive nanowires whose arithmetic mean length ha of the exposed portions thereof satisfied a predetermined value, a bonded body having excellent bonding strength was obtained even when the bonding time was shortened (Examples). In contrast, when one of the first structure and the second structure did not have conductive nanowires, the bonding strength of the bonded body was insufficient when the bonding time was shortened (Comparative Example 1). Furthermore, when the first structure and the second structure were made of conductive nanowires whose arithmetic mean length ha of the exposed portions thereof did not satisfy a predetermined value, the bonding strength of the bonded body was insufficient when the bonding time was shortened (Comparative Examples 2 and 3).
[0120] REFERENCE SIGNS 10 First structure 12 Insulating film 12a Surface 13 Pore 14 First conductive nanowire (second conductive nanowire) 15 Anodic oxide film 20 First member (second member) 20a First conductive region (second conductive region) 30 Aluminum substrate 31 Barrier layer 30a Surface 32c Bottom 32d Face 35 Metal 35a Metal layer 35b Metal 100 Second structure 200 Bonded body Dt Thickness direction d Average diameter ha Arithmetic mean length
Claims
1. A method for manufacturing a bonded body obtained by bonding a first structure and a second structure, comprising the steps of: providing a plurality of first conductive nanowires in a first conductive region of a first member having a first conductive region on its surface, to obtain the first structure having the first conductive nanowires; providing a plurality of second conductive nanowires in the second conductive region of a second member having a second conductive region on its surface, to obtain the second structure having the second conductive nanowires; and a bonding step of arranging the first conductive nanowires and the second conductive nanowires so that they are in contact with each other, thereby bonding the first structure and the second structure, wherein the arithmetic mean length of exposed portions of the plurality of first conductive nanowires and the arithmetic mean length of exposed portions of the plurality of second conductive nanowires are both 1 to 40 μm.
2. A method for producing a junction as described in claim 1, which satisfies at least one of the following: the standard deviation of the length of the exposed portion of the first conductive nanowire is 2 μm or less; and the standard deviation of the length of the exposed portion of the second conductive nanowire is 2 μm or less.
3. A method for producing a junction described in claim 1 or 2, wherein at least one of the following is satisfied: the first conductive nanowires have an average diameter of 45 to 75 nm; and the second conductive nanowires have an average diameter of 45 to 75 nm.
4. A method for producing a junction described in claim 1 or 2, which satisfies at least one of the following: the coverage area of the first conductive nanowire is 20 to 50% of the surface area of the first conductive region, and the coverage area of the second conductive nanowire is 20 to 50% of the surface area of the second conductive region.
5. A method for producing a junction described in claim 1 or 2, which satisfies at least one of the following: the first conductive nanowire is erected on the surface of the first conductive region, and the second conductive nanowire is erected on the surface of the second conductive region.
6. A method for producing a bonded body as described in claim 1 or 2, further comprising a heating step of heating the contacted first conductive nanowire and second conductive nanowire, and satisfying at least one of the following: the heating step is performed together with the bonding step, and the heating step is performed after the bonding step.
7. The method for producing a bonded body according to claim 6, wherein the heating temperature in the heating step is 150 to 300°C.
8. A method for producing a junction described in claim 1 or 2, which satisfies at least one of the following: the step of obtaining the first structure includes a process of adhering a composition containing the first conductive nanowire to the first conductive region; and the step of obtaining the second structure includes a process of adhering a composition containing the second conductive nanowire to the second conductive region.
9. The method for producing a bonded structure according to claim 1 or 2, wherein at least one of the first structure and the second structure includes a semiconductor element.
10. A structure set for use in manufacturing a junction, comprising: a first structure having a first conductive region and a plurality of first conductive nanowires provided in the first conductive region; and a second structure having a second conductive region and a plurality of second conductive nanowires provided in the second conductive region, wherein the arithmetic mean length of exposed portions of the plurality of first conductive nanowires and the arithmetic mean length of exposed portions of the plurality of second conductive nanowires are both 1 to 40 μm.
Citation Information
Patent Citations
Field emission device, its manufacturing method, and device using it
JP2008305792A
Conductive Nanowires For Electrical Interconnect
US20100018747A1
Flexible artificial leaves for hydrogen production and methods for making
US20190358605A1
Nanowires plated on nanoparticles
US20200321302A1
Dielectric and metallic nanowire bond layers
US20200321304A1