Method of manufacturing electrode active substance for lithium–sulfur battery
The production of a lithium-sulfur battery electrode active material using a porous carbon-sulfur-metal sulfide composite addresses the outflow of lithium polysulfide, enhancing cycle capacity and energy density by uniformly depositing metal sulfides on the surface, thus improving battery stability and performance.
Patent Information
- Application Number
- PCT/JP2024/008512
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-06
- Publication Date
- 2024-10-03
AI Technical Summary
Lithium-sulfur batteries face challenges in maintaining cycle capacity and charge/discharge performance due to the outflow of lithium polysulfide, which affects their energy density and stability, particularly in large-scale applications like electric vehicles and drones.
A method for producing an electrode active material involving a composite of porous carbon, sulfur, and a specific metal sulfide, where the metal source includes Ti, V, Mn, Fe, Co, Ni, Cu, Zn, Ge, Zr, In, Sn, Nb, Mo, Ta, and W, is used. This composite is formed by mixing porous carbon with sulfur and a metal source in a liquid medium, followed by heat treatment to precipitate and deposit metal compounds on the surface, enhancing the attachment of metal sulfides, thereby suppressing lithium polysulfide outflow.
The method improves the cycle characteristics and energy density of lithium-sulfur batteries by uniformly depositing metal sulfides on the surface, preventing lithium polysulfide leakage and maintaining battery performance over multiple cycles.
Smart Images

Figure JP2024008512_03102024_PF_FP_ABST
Abstract
Description
Method for producing electrode active material for lithium-sulfur batteries
[0001] The present disclosure relates to a method for producing an electrode active material for a lithium-sulfur battery.
[0002] Lithium-sulfur batteries are secondary batteries with high energy density per unit mass, and for example, mesoporous carbon-sulfur composites, in which sulfur is arranged within mesopores, are used. Lithium-sulfur batteries are lighter than conventional lithium-ion batteries, and are expected to be used in applications such as large power equipment like electric vehicles and aviation applications like drones. These applications require improvements in cycle capacity retention and charge / discharge capacity.
[0003] In relation to the above, for example, JP-A No. 2021-531228 proposes a positive electrode material containing iron sulfide that adsorbs lithium polysulfides.
[0004] An object of one aspect of the present disclosure is to provide a method for producing an electrode active material for a lithium-sulfur battery that can be used to construct a battery with improved cycle characteristics.
[0005] A first aspect is a method for producing an electrode active material for a lithium-sulfur battery, the method comprising: mixing a composite material containing a porous carbon material and sulfur supported on the porous carbon material, a metal source, and a liquid medium to obtain a first modified composite material having a metal compound derived from the metal source attached thereto; and heat-treating the first modified composite material to obtain a second modified composite material having a metal sulfide attached thereto. The metal source includes at least one specific metal selected from the group consisting of Ti, V, Mn, Fe, Co, Ni, Cu, Zn, Ge, Zr, In, Sn, Nb, Mo, Ta, and W.
[0006] In one aspect, a method for producing an electrode active material for a lithium-sulfur battery may include heat-treating a mixture containing a composite material including a porous carbon material and sulfur supported on the porous carbon material, a metal source, and a liquid medium under pressure to precipitate a metal compound derived from the metal source on the surface of the composite material, thereby obtaining a first modified composite material having the metal compound attached thereto; and heat-treating the first modified composite material to obtain a second modified composite material having a metal sulfide derived from the metal source attached thereto.
[0007] In one aspect, a method for producing an electrode active material for a lithium-sulfur battery may include adjusting the pH of a mixture containing a composite material including a porous carbon material and sulfur supported on the porous carbon material, a metal source, and a liquid medium to precipitate a metal compound derived from the metal source on a surface of the composite material, thereby obtaining a first modified composite material having the metal compound attached thereto; and heat-treating the first modified composite material to obtain a second modified composite material having a metal sulfide derived from the metal source attached thereto.
[0008] In one aspect, a method for producing an electrode active material for a lithium-sulfur battery may include: adding a sulfur source to a mixture containing a composite material including a porous carbon material and sulfur supported on the porous carbon material, a metal source, and a liquid medium, thereby precipitating a metal compound derived from the metal source on a surface of the composite material, thereby obtaining a first modified composite material having the metal compound attached thereto; and heat-treating the first modified composite material to obtain a second modified composite material having a metal sulfide derived from the metal source attached thereto.
[0009] A second aspect of the present invention provides a cathode active material for a lithium-sulfur battery, comprising a composite material including a porous carbon material and sulfur supported on the porous carbon material, and a metal sulfide including a specific metal. The cathode active material for a lithium-sulfur battery has a mass ratio of the specific metal to the total amount of carbon, sulfur, oxygen, nitrogen, and the specific metal near the surface of the cathode active material for a lithium-sulfur battery, as measured by energy dispersive spectroscopy, relative to the mass content of the specific metal in the cathode active material for a lithium-sulfur battery, as measured by inductively coupled plasma atomic emission spectroscopy, of 0.3 or more. The specific metal includes at least one selected from the group consisting of Ti, V, Mn, Fe, Co, Ni, Cu, Zn, Ge, Zr, In, Sn, Nb, Mo, Ta, and W.
[0010] According to one aspect of the present disclosure, it is possible to provide a method for producing an electrode active material for a lithium-sulfur battery that can form a battery with improved cycle characteristics.
[0011] FIG. 1 is a diagram showing an example of an X-ray diffraction spectrum of an electrode active material according to Example 1. FIG. 2 is a diagram showing an example of an X-ray diffraction spectrum of an electrode active material according to Example 2. FIG. 3 is a diagram showing an example of an X-ray diffraction spectrum of an electrode active material according to Example 3. FIG. 4 is a diagram showing an example of an X-ray diffraction spectrum of an electrode active material according to Example 4. FIG. 5 is a diagram showing an example of an X-ray diffraction spectrum of an electrode active material according to Comparative Example 1. FIG. 6 is a diagram showing an example of an X-ray diffraction spectrum of an electrode active material according to Comparative Example 2. FIG. 7 is a diagram showing an example of a scanning electron microscope image of the electrode active material according to Example 1.
[0012] In this specification, the term "process" refers not only to an independent process, but also to processes that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved. Furthermore, the "content of each component in a composition" refers to the total amount of each component in the composition, unless otherwise specified, when multiple substances corresponding to each component are present in the composition. Furthermore, the upper and lower limits of the numerical ranges described in this specification can be arbitrarily selected and combined from the numerical values exemplified as numerical ranges. Hereinafter, embodiments of the present invention will be described in detail. However, the embodiments described below exemplify electrode active materials for lithium-sulfur batteries and methods for producing the same, in order to embody the technical concept of the present invention. The present invention is not limited to the electrode active materials for lithium-sulfur batteries and methods for producing the same shown below.
[0013] 1. Method for Producing Electrode Active Material for Lithium-Sulfur Batteries The method for producing an electrode active material for lithium-sulfur batteries (hereinafter also simply referred to as the "production method") includes a first modification step of mixing a porous carbon material, a composite material containing sulfur supported on the porous carbon material, a metal source, and a liquid medium to obtain a first modified composite material having a metal compound derived from the metal source attached thereto, and a second modification step of heat-treating the first modified composite material to obtain a second modified composite material having a metal sulfide derived from the metal source attached thereto. In addition to the first modification step and the second modification step, the production method may further include other steps as necessary.
[0014] In the presence of a liquid medium, a metal compound containing a metal derived from a metal source is precipitated on the surface of a composite material including a sulfur-supported porous carbon material, thereby obtaining a first modified composite material, which is a composite material having the metal compound uniformly adhered to the surface. Heat-treating the obtained first modified composite material obtains a second modified composite material having a metal sulfide derived from the metal source uniformly adhered to the surface of the composite material. The metal sulfide disposed on the surface can suppress the outflow of lithium polysulfide, which is generated during discharge of a lithium-sulfur battery, from the porous carbon material. This improves the cycle characteristics of the lithium-sulfur battery. This can be attributed, for example, to the fact that the metal sulfide present on the surface of the composite material allows lithium ions to pass through while suppressing the passage of the electrolyte.
[0015] In the first modification step, a composite material, a metal source, and a liquid medium are mixed to obtain a mixture, and a first modified composite material is obtained in which a metal compound derived from the metal source is precipitated on the surface of the composite material. The composite material used to prepare the mixture may be obtained by receiving a composite material or by preparing a desired composite material by a conventional method. The composite material can be prepared, for example, by heat-treating a mixture of a porous carbon material and sulfur.
[0016] The porous carbon material used to prepare the composite material may have a substantially spherical shape. Alternatively, the porous carbon material may be formed by agglomerating fibrous carbon such as carbon nanotubes. The porous carbon material may have a volume average particle size of, for example, 0.5 μm to 50 μm, such as 1 μm to 1.5 μm, or 2 μm, or 40 μm to 30 μm, 15 μm to 10 μm, or 5 μm to 5 μm. When the volume average particle size of the porous carbon material is within the above range, an electrode with less coating unevenness tends to be produced. The volume average particle size (D50) of the porous carbon material is measured as the particle size corresponding to 50% of the cumulative volume from the smallest diameter side in the volume-based particle size distribution. The volume-based particle size distribution is measured using a laser diffraction particle size distribution analyzer.
[0017] The porous carbon material may have an aspect ratio (major axis / minor axis) of, for example, 1 or more and 3 or less. The aspect ratio may preferably be 1.05 or more, and may preferably be 2 or less, 1.5 or less, or 1.2 or less. The major axis and minor axis of the porous carbon material are measured by a method of calculating the lengths of the major axis and minor axis from an image obtained from an optical microscope, an electron microscope, or the like, or by using an image-based particle size distribution analyzer. Specifically, for example, the volume average particle size D50 is measured using a laser diffraction particle size distribution analyzer, and 30 to 50 porous carbon material particles having a particle size, which is the arithmetic mean value of the major axis and minor axis measured from a scanning electron microscope (SEM) image, are arbitrarily selected, and the aspect ratio of each particle is calculated. The aspect ratio of the porous carbon material is calculated as the arithmetic mean value of these particles. The aspect ratio is determined in accordance with the Japanese Industrial Standards (JIS Z8900-1:2008) by measuring the maximum major axis of a particle and the minor axis, which is the width perpendicular to the maximum major axis, calculating the ratio of the major axis to the minor axis, and taking the arithmetic mean value as the aspect ratio. For example, this can be automatically analyzed using software such as Image J.
[0018] The porous carbon material may have a peak pore diameter of, for example, 0.5 nm or more and 10 nm or less, 1.5 nm or more, 2.0 nm or more, or 2.5 nm or more, or 8 nm or less, 6 nm or less, 4 nm or less, or 3 nm or less. When the peak pore diameter of the porous carbon material is within the above range, the reaction between the metal source and sulfur tends to be appropriately suppressed, and a decrease in the charge / discharge capacity of the lithium-sulfur battery tends to be more effectively suppressed. Here, the peak pore diameter refers to the pore diameter showing the largest peak in a pore distribution curve obtained by quenched solid density functional theory (QSDFT) from a nitrogen adsorption isotherm obtained by nitrogen gas adsorption / desorption measurement.
[0019] The porous carbon material has a specific surface area of, for example, 1000 m 2 / g or more, preferably 1500m 2 / g or more, 2000m 2 / g or more, or 2500m 2 The specific surface area may be, for example, 3500 m 2 / g or less, 3300m2 / g or less, or 3000m 2 The specific surface area of the porous carbon material may be measured by a BET (Brunauer Emmett Teller) method based on the BET theory. Specifically, for example, it is measured by a multipoint method using nitrogen gas.
[0020] The pore volume of the porous carbon material may be, for example, 0.8 ml / g or more and 4 ml / g or less, 0.9 ml / g or more, 1.0 ml / g or more, or 1.2 ml / g or more, and 3 ml / g or less, 2.5 ml / g or less, 2.3 ml / g or less, 2 ml / g or less, or 1.5 ml / g or less. It is particularly preferable that the pore volume of pores having a diameter of 0.5 nm or more and 4.0 nm or less is within the above range. When the pore volume of the porous carbon material is within the above range, more sulfur can be packed into the pores of the porous carbon material, which tends to increase the energy density of lithium-sulfur batteries. The pore volume of the porous carbon material is measured, for example, by nitrogen gas adsorption / desorption measurement.
[0021] The carbon content in the porous carbon material may be, for example, 80% by mass or more, preferably 90% by mass or more, or 95% by mass or more, and may consist essentially of carbon. Here, the term "substantially" is intended to not exclude other elements that are inevitably mixed in.
[0022] Specific examples of porous carbon materials include carbon nanotubes, graphene, and carbon materials obtained by carbonizing and activating resins, petroleum pitch, or plant-derived compounds. The porous carbon material may contain at least activated carbon. One type of porous carbon material may be used alone, or two or more types may be used in combination.
[0023] The composite material includes sulfur supported on a porous carbon material. At least a portion of the sulfur may be disposed in the pores of the porous carbon material or on the surface of the porous carbon material. The purity of the sulfur supported on the porous carbon material may be, for example, 50% by mass or more, 90% by mass or more, or 100% by mass or less.
[0024] By using a porous carbon material having sulfur disposed on the surface as the composite material, metal sulfides are more uniformly disposed on the surface of the composite material, and the outflow of lithium polysulfides generated during discharge from the porous carbon material can be more effectively suppressed.
[0025] The sulfur content in the composite material may be, for example, 100% by mass or more and 500% by mass or less, preferably 120% by mass or more, 140% by mass or more, 150% by mass or more, or 200% by mass or more, relative to the porous carbon material, and preferably 300% by mass or less, or 200% by mass or less.
[0026] The composite material can be prepared by heat-treating a mixture containing a porous carbon material and sulfur. In addition to the porous carbon material and sulfur, the mixture may further contain compounds containing phosphorus, boron, nitrogen, etc., transition metals, polymer compounds, etc., as needed. The heat treatment of the mixture can be carried out, for example, in a sealed container at a heat treatment temperature of 100°C or higher and 450°C or lower. The heat treatment temperature may be 120°C or higher or 400°C or lower. The pressure during the heat treatment may be atmospheric pressure or higher and 15 MPa or lower in gauge pressure. The heat treatment time may be, for example, 1 hour or higher and 72 hours or lower, or 1.5 hours or higher, or 36 hours or lower.
[0027] The content of the composite material in the mixture containing the composite material, the metal source, and the liquid medium in the first modification step may be, for example, 1% by mass or more and 70% by mass or less, 5% by mass or more, 7% by mass or more, 10% by mass or more, 20% by mass or more, or 30% by mass or more, and 50% by mass or less, or 40% by mass or less, relative to the total mass of the mixture. If the content of the composite material is within the above range, the wet dispersion treatment can be carried out more efficiently.
[0028] The metal contained in the metal source constituting the mixture may include at least one specific metal selected from the group consisting of titanium (Ti), vanadium (V), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zinc (Zn), germanium (Ge), zirconium (Zr), indium (In), tin (Sn), niobium (Nb), molybdenum (Mo), tantalum (Ta), and tungsten (W), and may include at least Zn. It is believed that the specific metal reacts with sulfur to form a metal sulfide that is permeable to lithium ions but impermeable to the electrolyte. The metal source may include a simple substance of the specific metal, an alloy, a compound containing the specific metal, or the like. Examples of compounds containing the specific metal include metal salts such as sulfates, nitrates, oxalates, phosphates, and borates, as well as oxides, nitrides, carbides, borides, sulfides, phosphides, composite oxides, and composite oxynitrides. The purity of the compound containing the specific metal used as the metal source may be, for example, 30% by mass or more, 60% by mass or more, or 90% by mass or more, or less than 100% by mass.
[0029] The metal source may be a substance soluble in the liquid medium described below. By using a metal source soluble in the liquid medium, a modified composite material can be obtained more efficiently. Here, "soluble in the liquid medium" means that the solubility in 100 g of the liquid medium is 0.01 g or more at room temperature (e.g., 25°C) or at the temperature of the heat treatment. The solubility may be 0.02 g or more.
[0030] The content of the metal source in the mixture containing the composite material, the metal source, and the liquid medium may be, for example, 0.1 mass % or more and 50 mass % or less, 1 mass % or more, 1.5 mass % or more, 2 mass % or more, or 3 mass % or more, and may be 30 mass % or less, 20 mass % or less, 10 mass % or less, 5 mass % or less, or 4 mass % or less, relative to the total mass of the mixture. When the content of the metal source is within the above range, the metal source can be added homogeneously to the composite material.
[0031] In the mixture, the mass ratio of the content of the metal source to the content of the composite material may be, for example, 0.1 mass% or more and 20 mass% or less, preferably 0.5 mass% or more, 1 mass% or more, 2 mass% or more, or 5 mass% or more, and preferably 18 mass% or less, 15 mass% or less, 12 mass% or less, or 10 mass% or less. When the mass ratio of the metal source to the composite material is within the above range, it tends to be possible to produce a positive electrode material for a lithium-sulfur battery while suppressing a decrease in the energy density of the lithium-sulfur battery.
[0032] The liquid medium constituting the mixture containing the composite material, the metal source, and the liquid medium may be any substance capable of dissolving at least a portion of the metal source, and may contain at least water. When the liquid medium contains water, the water content in the liquid medium may be 20% by mass or more, 40% by mass or more, or 60% by mass or more, relative to the total mass of the liquid medium. Furthermore, the water content in the liquid medium may be 100% by mass or less, or less than 100% by mass. The liquid medium may contain a liquid medium other than water. Examples of liquid media other than water include water-soluble organic solvents such as ethanol.
[0033] The content of the liquid medium in the mixture containing the composite material, the metal source, and the liquid medium may be, for example, 10% by mass or more and 99% by mass or less, 20% by mass or more, 30% by mass or more, 50% by mass or more, or 60% by mass or more, and may be 95% by mass or less, 90% by mass or less, 80% by mass or less, or 70% by mass or less, relative to the total mass of the mixture. If the content of the liquid medium is within the above range, the wet dispersion treatment can be carried out more efficiently.
[0034] The pH of the mixture containing the composite material, the metal source, and the liquid medium may be, for example, 1 or more and 14 or less, preferably 1.5 or more or 2 or more, and preferably 13.5 or less, 7 or less, or 5 or less. The pH of the mixture may be set depending on the type of the metal source.
[0035] The mixture is obtained by mixing the composite material, the metal source, and the liquid medium. The mixing method for obtaining the mixture may be appropriately selected from commonly used wet dispersion treatment methods. Specific examples include a method using a propeller-type agitator, a method using beads, and a method using a homogenizer. The temperature during mixing may be, for example, 0°C or higher and 100°C or lower. The mixing time may be, for example, 1 minute or higher and 72 hours or lower.
[0036] In the first modification step, a first modified composite material is obtained in which a metal compound derived from a metal source is precipitated on the surface. Examples of the precipitated metal compound include metal oxides, metal hydroxides, metal sulfides, metal phosphates, and metal borates. Methods for precipitating the metal compound include heat treatment of the mixture, adjusting the pH of the liquid medium constituting the mixture, removing the liquid medium from the mixture, and adjusting the ion concentration of the ions constituting the precipitated metal compound.
[0037] In one embodiment, the production method may be a first production method in which the first modification step includes a first heat treatment step of heat-treating the mixture. In the first heat treatment step, the resulting mixture may be heat-treated in a sealed, pressurized state. This allows a first modified composite material to be obtained. By reacting the sulfur contained in the composite material with the metal source in the presence of a liquid medium, a deposit containing, for example, a metal sulfide is precipitated on the surface of the composite material, thereby forming the first modified composite material. Furthermore, by precipitating the metal sulfide in the liquid medium, the metal sulfide can be uniformly precipitated on the surface of the composite material.
[0038] The first heat treatment step may be carried out in a sealed state. Specifically, it can be carried out by heating the mixture in a pressure-resistant sealed container. The pressurization condition in the first heat treatment step may be the vapor pressure of the liquid medium in the first heat treatment step. For example, when the liquid medium is water and the temperature in the first heat treatment step is 230°C, the absolute pressure is 2.8 MPa. Other pressurization conditions may be, for example, 2.0 MPa or more and 15 MPa or less, 4.7 MPa or more, or 7.4 MPa or less.
[0039] The temperature of the first heat treatment step may be, for example, a temperature equal to or higher than the boiling point of the liquid medium. The first heat treatment step may include a temperature-raising step in which the mixture is heated to a predetermined temperature, and a maintenance step in which the predetermined temperature is maintained for a predetermined period of time. The temperature-raising rate in the temperature-raising step may be adjusted so that the maximum temperature during the temperature rise does not exceed the target temperature, and may be, for example, 1°C / min or more and 20°C / min or less. The predetermined heat treatment temperature in the first heat treatment step may be, for example, 120°C or more and 300°C or less, 150°C or more, or 200°C or more, and may be 270°C or less, or 250°C or less. The predetermined time in the maintenance step may be, for example, 30 minutes or more, 1 hour or more, or 3 hours or more. The predetermined time in the maintenance step may be, for example, 72 hours or less, 48 hours or less, or 24 hours or less. The predetermined heat treatment time in the maintenance step begins when the temperature set within the above-mentioned temperature range is reached, and ends when the temperature-lowering operation is performed.
[0040] The atmosphere in the first heat treatment step may be, for example, any of air, nitrogen, and argon atmospheres.
[0041] The first heat treatment step may include a cooling step, following the maintaining step, of lowering the temperature of the resulting dispersion containing the first modified composite material. The cooling step begins when the temperature lowering operation is performed and ends when the temperature has been lowered to 50° C. or less. The temperature lowering rate may be, for example, 1° C. / min or more and 10° C. / min or less.
[0042] The first production method may further include a separation step of separating the obtained first modified composite material from the mixture, and may further include a purification step as necessary. In the separation step, for example, the first modified composite material may be isolated by subjecting the mixture containing the first modified composite material to solid-liquid separation. In the purification step, the first modified composite material may be washed with pure water or the like. The isolated first modified composite material may be dried, for example, by heat drying, vacuum degassing, natural drying, or a combination thereof.
[0043] The first production method includes a second modification step in which a first modified composite material is heat-treated to obtain a second modified composite material having a metal sulfide derived from a metal source attached thereto. In the second modification step, the first modified composite material, which is a composite material having a metal sulfide attached thereto, is re-heat-treated to obtain a second modified composite material having a more stable sulfur state, with the metal sulfide attached to its surface. The metal sulfide contained in the second modified composite material may be a metal sulfide containing a specific metal and may include at least zinc sulfide. The heat treatment in the second modification step of the first production method may include removing at least a portion of the liquid medium attached to the first modified composite material to obtain a dried product.
[0044] The heat treatment in the second modification step of the first manufacturing method may include a temperature increase step in which the first modified composite material is heated to a predetermined temperature and a maintenance step in which the predetermined temperature is maintained for a predetermined time. The temperature increase rate in the temperature increase step may be, for example, 1°C / min or more and 20°C / min or less. The predetermined heat treatment temperature in the heat treatment may be, for example, 100°C or more and 450°C or less, 120°C or more, or 150°C or more, and 430°C or less, or 400°C or less. The predetermined time in the maintenance step may be, for example, 30 minutes or more, 1 hour or more, or 3 hours or more. The predetermined time in the maintenance step may be, for example, 72 hours or less, 48 hours or less, or 24 hours or less. The predetermined heat treatment time in the maintenance step begins when the temperature set in the above-mentioned temperature range is reached and ends when the temperature decrease operation is performed. The heat treatment atmosphere may be, for example, air, nitrogen, argon, or the like.
[0045] The heat treatment in the second modification step may include a cooling step of lowering the temperature of the first modified composite material following the above-mentioned maintaining step. The cooling step begins when the temperature lowering operation is performed and ends when the temperature has been lowered to 50°C or less. The temperature lowering rate may be, for example, 1°C / min or more and 10°C / min or less.
[0046] In one embodiment, the production method may be a second production method in which the first modification step includes a pH adjustment step of adjusting the pH of the liquid medium constituting the mixture. By adjusting the pH of the liquid medium, the metal compound with reduced solubility is precipitated on the surface of the composite material, resulting in a first modified composite material, which is a composite material with the metal compound attached to the surface. By precipitating the metal compound in the liquid medium, the metal compound can be uniformly precipitated on the surface of the composite material. Examples of metal compounds precipitated in the pH adjustment step include metal hydroxides, metal oxides, metal sulfides, metal phosphates, and metal borates, and the mixture may include at least one selected from the group consisting of these.
[0047] The pH adjustment step may be carried out by adjusting the pH of the liquid medium to precipitate a metal compound containing a metal derived from the metal source. Specifically, for example, the pH of the liquid medium may be adjusted by adding a basic compound or an acidic compound to the mixture. Examples of basic compounds used for pH adjustment include hydroxide salts such as alkali metal hydroxides and alkaline earth hydroxides, and aqueous ammonia solutions. Examples of acidic compounds include nitric acid, sulfuric acid, phosphoric acid, and boric acid. The pH adjustment range in the pH adjustment step may be, for example, 2 to 14, and preferably 2.5 or more or 13.5 or less. The pH adjustment step may, for example, increase the pH of the liquid medium, preferably by 1 or more, or by 2 or more. The increase in pH may be 12 or less. The pH adjustment step may, for example, decrease the pH of the liquid medium, preferably by 1 or more, or by 2 or more. The decrease in pH may be 14 or less.
[0048] After adjusting the pH of the liquid medium, a precipitation step of precipitating the metal compound may be included. In the precipitation step, the metal compound may be precipitated while stirring the mixture, or may be precipitated in a stationary state. The temperature in the precipitation step may be, for example, 0°C or higher and 100°C or lower, and preferably 10°C or higher or 90°C or lower. The precipitation time in the precipitation step may be, for example, 1 minute or higher and 72 hours or lower, and preferably 5 minutes or higher or 48 hours or lower.
[0049] The second production method may further include a separation step of separating the obtained first modified composite material from the mixture, and may further include a purification step as necessary. In the separation step, for example, the first modified composite material may be isolated by subjecting the mixture containing the first modified composite material to solid-liquid separation. In the purification step, the first modified composite material may be washed with pure water or the like. The isolated first modified composite material may be dried, for example, by heat drying, vacuum degassing, natural drying, or a combination thereof.
[0050] The second production method includes a second modification step of heat-treating a first modified composite material to obtain a second modified composite material having a metal sulfide derived from a metal source attached thereto. In the second modification step, the first modified composite material, which is a composite material having a metal compound attached thereto, is heat-treated, for example, to cause the metal compound to react with sulfur contained in the composite material to produce a metal sulfide, thereby obtaining a second modified composite material, which is a composite material having a metal sulfide attached thereto. The metal sulfide contained in the second modified composite material may be a metal sulfide containing a specific metal and may include at least zinc sulfide. The heat treatment in the second modification step of the second production method may include removing at least a portion of the liquid medium attached to the first modified composite material to obtain a dried product.
[0051] The heat treatment in the second modification step of the second manufacturing method may include a temperature increase step in which the first modified composite material is heated to a predetermined temperature and a maintenance step in which the predetermined temperature is maintained for a predetermined time. The temperature increase rate in the temperature increase step may be, for example, 1°C / min or more and 20°C / min or less. The predetermined heat treatment temperature in the heat treatment may be, for example, 50°C or more and 450°C or less, 100°C or more, or 150°C or more, and 400°C or less, or 350°C or less. The predetermined time in the maintenance step may be, for example, 30 minutes or more, 1 hour or more, or 3 hours or more. The predetermined time in the maintenance step may be, for example, 72 hours or less, 48 hours or less, or 24 hours or less. The predetermined heat treatment time in the maintenance step begins when the temperature set in the above-mentioned temperature range is reached and ends when the temperature decrease operation is performed. The heat treatment atmosphere may be, for example, air, nitrogen, argon, or the like.
[0052] The heat treatment in the second modification step may include a cooling step of lowering the temperature of the first modified composite material following the above-mentioned maintaining step. The cooling step begins when the temperature lowering operation is performed and ends when the temperature has been lowered to 50°C or less. The temperature lowering rate may be, for example, 1°C / min or more and 10°C / min or less.
[0053] In one embodiment, the production method may be a third production method in which the first modification step includes a sulfur source addition step of adding a sulfur source to the mixture. By adding the sulfur source to the mixture, the metal compound, whose solubility has been reduced, precipitates on the surface of the composite material, thereby obtaining a first modified composite material, which is a composite material having the metal compound attached to the surface. Precipitating the metal compound in a liquid medium allows the metal compound to be uniformly precipitated on the surface of the composite material. Examples of metal compounds precipitated in the sulfur source addition step include metal sulfides, metal hydroxides, and metal oxides, and the metal compound may include at least one selected from the group consisting of these.
[0054] The sulfur source added to the mixture may be, for example, a compound capable of generating sulfide ions. Specific examples of sulfur sources include hydrogen sulfide, carbon disulfide, silicon disulfide, nitrogen sulfide, phosphorus sulfide, and arsenic sulfide. The amount of sulfur source added, in terms of sulfide ions, relative to the content of metal ions contained in the metal sources constituting the mixture, may be, for example, 0.5 times or more by mol, and preferably 0.8 times or more by mol. The amount of sulfur source added, in terms of sulfide ions, may be, for example, 3.0 times or less by mol, and preferably 2.5 times or less by mol, or 2.0 times or less by mol.
[0055] The sulfur source addition step may further include adjusting the pH of the mixture. The pH adjustment may be performed prior to the start of sulfur source addition or during the addition of the sulfur source. Furthermore, the pH adjustment may be performed to suppress pH fluctuations in the mixture due to the addition of the sulfur source. Specifically, the pH adjustment of the mixture may be performed, for example, by adding a basic compound or an acidic compound to the mixture. Examples of basic compounds used for pH adjustment include hydroxide salts such as alkali metal hydroxides and alkaline earth hydroxides, and aqueous ammonia solutions. Examples of acidic compounds include nitric acid, sulfuric acid, phosphoric acid, and boric acid. The pH adjustment range may be, for example, 2 or more and 14 or less, and preferably 2.5 or more. The pH adjustment may be, for example, by increasing the pH of the mixture, preferably by increasing it by 1 or more or by 2 or more. The pH adjustment may be, for example, by decreasing the pH of the mixture, preferably by decreasing it by 1 or more or by 2 or more. Furthermore, the pH may be adjusted, for example, to suppress pH fluctuations of the mixture, and pH fluctuations accompanying the addition of the sulfur source may be suppressed to, for example, 13.5 or less, preferably 12 or less.
[0056] After the addition of the sulfur source, a precipitation step of precipitating a metal compound may be included. In the precipitation step, the metal compound may be precipitated while stirring the mixture, or may be precipitated in a stationary state. The temperature in the precipitation step may be, for example, 0°C or higher and 100°C or lower, and preferably 10°C or higher or 90°C or lower. The precipitation time in the precipitation step may be, for example, 1 minute or higher and 72 hours or lower, and preferably 5 minutes or higher or 48 hours or lower.
[0057] The third production method may further include a separation step of separating the obtained first modified composite material from the mixture, and may further include a purification step as necessary. In the separation step, for example, the first modified composite material may be isolated by subjecting the mixture containing the first modified composite material to solid-liquid separation. In the purification step, the first modified composite material may be washed with pure water or the like. The isolated first modified composite material may be dried, for example, by heat drying, vacuum degassing, natural drying, or a combination thereof.
[0058] The third production method includes a second modification step of heat-treating the first modified composite material to obtain a second modified composite material having a metal sulfide derived from a metal source attached thereto. The details of the second modification step in the third production method are the same as those of the second modification step in the first production method.
[0059] Electrode Active Material for Lithium-Sulfur Batteries The electrode active material for lithium-sulfur batteries includes a composite material containing a porous carbon material and sulfur supported on the porous carbon material, and a metal sulfide containing a specific metal disposed on the surface of the composite material. The positive electrode active material for lithium-sulfur batteries has a ratio (Cx / Ci) of 0.3 or more of the mass ratio (Cx) of the specific metal to the total amount of carbon, sulfur, oxygen, nitrogen, and the specific metal in the lithium-sulfur battery positive electrode active material measured by energy dispersive X-ray spectroscopy, relative to the mass content (Ci) of the specific metal in the lithium-sulfur battery positive electrode active material measured by inductively coupled plasma atomic emission spectroscopy. The specific metal may include at least one selected from the group consisting of Ti, V, Mn, Fe, Co, Ni, Cu, Zn, Ge, Zr, In, Sn, Nb, Mo, Ta, and W. Preferably, the specific metal may include at least Zn. That is, the metal sulfide may include at least zinc sulfide.
[0060] The electrode active material for a lithium-sulfur battery may include a coated composite material in which at least a portion of the surface of the composite material is coated with a metal sulfide. The coated composite material may be, for example, the second modified composite material in the above-described manufacturing method. By disposing the metal sulfide on the surface of the composite material, it is possible to more effectively suppress the outflow of lithium polysulfide, which is generated during charging and discharging of the lithium-sulfur battery, from the porous carbon material. The presence of the metal sulfide can be detected, for example, by X-ray diffraction (XRD) spectroscopy or transmission electron microscopy (TEM). For example, when the specific metal is zinc, the presence of ZnS can be confirmed by the presence of a peak derived from the (111) plane of ZnS around 28.5° in XRD measurement. Furthermore, the (111) plane of ZnS can also be assigned from the diffraction point in the electron beam diffraction image by TEM observation.
[0061] In the electrode active material for lithium-sulfur batteries, metal sulfides are disposed on the surface of the composite material. The state of arrangement of the metal sulfides on the surface of the composite material can be evaluated, for example, by the ratio of the content of the specific metal present in a partial region of the surface of the electrode active material for lithium-sulfur batteries to the total content of the specific metal contained in the electrode active material for lithium-sulfur batteries (hereinafter also referred to as the dispersion index of the specific metal). The larger the dispersion index value, the more uniformly the specific metal is dispersed throughout the entire surface of the composite material.
[0062] The total content of the specific metals contained in the electrode active material for a lithium-sulfur battery can be evaluated as the mass-based content (Ci) of the specific metals in the positive electrode active material for a lithium-sulfur battery measured by inductively coupled plasma (ICP) atomic emission spectrometry.
[0063] Furthermore, the respective contents of carbon, sulfur, oxygen, nitrogen, and specific metal near the surface of a lithium-sulfur battery electrode active material comprising carbon, sulfur, and the specific metal can be evaluated by energy dispersive spectroscopy (EDX). That is, the content of the specific metal present on the surface of a lithium-sulfur battery electrode active material can be evaluated by the mass ratio (Cx) of the specific metal relative to the total mass of carbon, oxygen, nitrogen, sulfur, and specific metal near the surface of the lithium-sulfur battery positive electrode active material measured by energy dispersive X-ray (EDX) spectroscopy. The appropriate measurement conditions for SEM-EDX vary depending on the particle size, but the magnification may be such that at least 100 particles, preferably 500 particles, and more preferably 1000 particles are present in the observation area. For example, when D50 is about 2 μm, a magnification of 1500x can be selected.
[0064] Here, the surface vicinity measured by EDX spectroscopy is a depth that varies depending on the element being measured, even under the same measurement conditions. For example, for carbon, sulfur, etc., the depth is several μm (10 -6 Even under measurement conditions that allow detection to depths of several hundred nm (10 m order), metal compounds -7It is thought that the metal compound is only detected to a depth of about 1000 m (order of magnitude of 1000 m). Therefore, when a metal compound is localized to a certain thickness near the surface of an electrode active material for a lithium-sulfur battery, the content of the metal atoms contained in the metal compound is detected as being lower than that of carbon, sulfur, etc. Therefore, when the dispersion index (Cx / Ci) of a specific metal is evaluated for an electrode active material for a lithium-sulfur battery, if the specific metal is uniformly distributed near the surface of the electrode active material for a lithium-sulfur battery, the value is close to 1. On the other hand, if the specific metal is localized near the surface of the electrode active material for a lithium-sulfur battery, the value is smaller than when the specific metal is uniformly distributed.
[0065] In the electrode active material for a lithium-sulfur battery, the dispersion index of the specific metal may be 0.3 or more, preferably 0.5 or more, or 0.7 or more. The dispersion index of the specific metal may be 1.2 or less. When the dispersion index of the specific metal is within the above range, it tends to be possible to more effectively suppress the outflow of lithium polysulfide, which is generated during discharge of a lithium-sulfur battery, from the porous carbon material. The dispersion index of the specific metal is evaluated as the arithmetic average value of measurements taken in any three regions.
[0066] When the electrode active material for a lithium-sulfur battery contains zinc sulfide as the metal sulfide, the intensity ratio of the peak intensity derived from the (220) plane to the peak intensity derived from the (111) plane of zinc sulfide in an X-ray diffraction (XRD) pattern may be 0.42 or more, preferably 0.421 or more, or 0.422 or more. Furthermore, the peak intensity ratio may be 0.5 or less. When the peak intensity ratio in the XRD pattern is within the above range, the cycle retention rate tends to be further improved. Here, the peak derived from the (111) plane of zinc sulfide is observed at around 28.5°, and the peak derived from the (220) plane is observed at around 47.5°.
[0067] The content of the specific metal contained in the electrode active material for lithium-sulfur batteries may be, for example, 0.1% by mass or more and 30% by mass or less, or 0.5% by mass or more, or 20% by mass or less. Furthermore, in the electrode active material for lithium-sulfur batteries, the mass ratio of the metal sulfide content to the composite material content may be, for example, 0.15% by mass or more and 30% by mass or less, or 0.75% by mass or more, or 40% by mass or less. Furthermore, in the electrode active material for lithium-ion batteries, the mass ratio of the metal sulfide content to the total sulfur content may be, for example, 0.2% by mass or more and 60% by mass or less, or 1% by mass or more, or 30% by mass or less. When the content of the specific metal is within the above range, there is a tendency that the outflow of lithium polysulfide generated during discharge of the lithium-sulfur battery from the porous carbon material can be more effectively suppressed.
[0068] Positive electrode for lithium-sulfur battery A positive electrode for a lithium-sulfur battery (hereinafter also simply referred to as "positive electrode") includes a current collector and a positive electrode active material layer disposed on the current collector. The positive electrode active material layer may contain the above-described electrode active material for lithium-sulfur batteries. The positive electrode is manufactured, for example, by applying an electrode composition containing the above-described electrode active material for lithium-sulfur batteries, a liquid medium, a binder, a conductive additive, etc., onto a current collector, followed by drying and pressure molding to form a positive electrode active material layer on the current collector.
[0069] The liquid medium may be an organic solvent, water, or the like, depending on the application. Examples of organic solvents include amide-based solvents such as N-methyl-2-pyrrolidone (NMP), ketone-based solvents such as diisopropyl ketone, diisobutyl ketone, and methyl ethyl ketone, hydrocarbon-based solvents such as heptane, ether-based solvents such as tetrahydrofuran, dimethoxyethane, and dioxolane, amine-based solvents such as diethylenetriamine, and ester-based solvents. The organic solvents may be used alone or in combination of two or more. The content of the liquid medium may be, for example, 10% by mass or more and 90% by mass or less with respect to the total mass of the electrode composition.
[0070] The binder is a material that aids in adhesion between the electrode active material and the conductive additive, and in adhesion of the electrode composition to the current collector. Examples of binders include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene rubber (EPDM), sulfonated EPDM, styrene-butylene rubber, fluororubber, and various copolymers. The binder content may be, for example, 0.05% by mass or more and 50% by mass or less relative to the total mass of the electrode composition.
[0071] The conductive additive is, for example, a material that improves the electrical conductivity of the positive electrode composition layer. Examples of the conductive additive include graphite such as modified graphene, natural graphite, and artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; and carbon materials such as graphene and carbon nanotubes. The content of the conductive additive may be, for example, 0.5% by mass or more and 30% by mass or less with respect to the total mass of the electrode composition.
[0072] Examples of current collectors include metals such as copper, stainless steel, aluminum, nickel, and titanium; composite materials in which the surface of copper or stainless steel is surface-treated with carbon, nickel, titanium, silver, or the like; and carbon foil. When manufacturing a lightweight lithium-sulfur battery, for example, aluminum and carbon foil are preferred as lightweight current collectors. The current collector can also have fine irregularities on its surface to increase the adhesive strength of the positive electrode composition layer, etc. Various forms are possible, such as films, sheets, foils, nets, porous bodies, foams, and nonwoven fabrics. The thickness of the current collector may be, for example, 3 μm or more and 500 μm or less.
[0073] A positive electrode active material layer formed containing the above-described electrode active material for a lithium-sulfur battery may be formed as a dense layer with few voids. The porosity of the positive electrode active material layer in the positive electrode may be, for example, 75% or less, preferably 60% or less, 55% or less, or 50% or less. The lower limit of the porosity of the positive electrode active material layer may be, for example, 1% or more. The porosity of the positive electrode active material layer may be calculated from the ratio of the theoretical density of the positive electrode composition layer calculated from the materials constituting the positive electrode composition layer to the pressed density calculated from the thickness measured when the positive electrode composition layer is pressed. Alternatively, the porosity may be calculated by specifying a predetermined area in a cross-sectional SEM image of the positive electrode active material layer and measuring the area ratio of the void portion using image analysis software.
[0074] Lithium-sulfur secondary battery The lithium-sulfur battery includes the above-mentioned positive electrode for a lithium-sulfur battery. The lithium-sulfur battery includes a positive electrode for a lithium-sulfur battery, a negative electrode, an electrolyte disposed between the positive electrode and the negative electrode, and the like. The lithium-sulfur battery may also include a separator as necessary. The electrolyte may be contained in the positive electrode, negative electrode, and separator for the lithium-sulfur battery.
[0075] Anode: Any known material may be used as the anode of the lithium-sulfur battery. Examples of anode materials include Li metal, Li-Si alloy, Li-Al alloy, Li-In alloy, and lithium titanate (e.g., Li 4 Ti 5 O 12 and LiTi 2 O 4 ), lithium titanium composite oxide (e.g., Li 4 Ti 5-x Mn x O 12 ;0<x≦0.3), Li x C (x≦6), etc. In these negative electrode materials, a part of the lithium may be substituted with other alkali metals. Examples of negative electrode materials include Li metal, Li-Si alloy, Li-Al alloy, Li-In alloy, Li x C (x≦6) is preferred. These materials allow a high voltage to be extracted from the lithium-sulfur battery.
[0076] Separator The separator may be made of a known material, such as porous polyethylene, polypropylene, etc. Also, a known separator may be used after being coated.
[0077] The electrolyte may contain a lithium salt and may be appropriately selected from lithium salts used in conventional lithium ion batteries. The lithium salt may contain, for example, an anion having a fluorine element. Specific examples of lithium salts containing an anion having a fluorine element include LiPF 6 , LiBF 4 , LiSbF 6 , LiAsF 6 , LiSO 3 CF 3 , LiN(SO 2 CF 3 ) 2 (LiTFSI), LiN(SO 2 F) 2 (LiFSI), etc. The electrolyte may be lithium nitrate, LiClO 4 The electrolyte may contain a lithium salt not containing fluorine element, such as: One of these may be used alone, or two or more may be used in combination.
[0078] The electrolyte may contain an organic solvent. Examples of the organic solvent include carbonate solvents, ether solvents, ester solvents, amide solvents, nitrile solvents, and sulfur-containing solvents. Alternatively, organic solvents in which some of the elements of the above organic solvents have been substituted with fluorine may also be used. Examples of the organic solvent include carbonate solvents such as propionate carbonate, ethylene carbonate, dimethyl carbonate, ethyl methyl carbonate, and fluoroethylene carbonate; ether solvents such as 1,3-dioxolane, 1,2-dimethoxyethane, 1,3-dimethoxypropane, 2,2,3,3-tetrafluoropropyl difluoromethyl ether and tetrahydrofuran; ester solvents such as methyl formate, methyl acetate, and γ-butyl lactone; amide solvents such as N,N-dimethylacetamide and N,N-dimethylformamide; and sulfur-containing solvents such as sulfolane, dimethyl sulfoxide, and 1,3-propane sultone.
[0079] Another aspect of the present invention relates to the use of the electrode active material for a lithium-sulfur battery in the manufacture of a positive electrode for a lithium-sulfur battery or a lithium-sulfur battery, and an electrode active material for a lithium-sulfur battery used in the manufacture of a positive electrode for a lithium-sulfur battery or a lithium-sulfur battery.
[0080] The invention according to the present disclosure may include, for example, the following aspects: [1] A method for producing an electrode active material for a lithium-sulfur battery, the method comprising: mixing a composite material containing a porous carbon material and sulfur supported on the porous carbon material, a metal source, and a liquid medium to obtain a first modified composite material having a metal compound derived from the metal source attached thereto; and heat-treating the first modified composite material to obtain a second modified composite material having a metal sulfide attached thereto, wherein the metal source contains at least one specific metal selected from the group consisting of Ti, V, Mn, Fe, Co, Ni, Cu, Zn, Ge, Zr, In, Sn, Nb, Mo, Ta, and W.
[0081] [2] The method for producing an electrode active material for a lithium-sulfur battery according to [1], wherein obtaining the first modified composite material includes heat-treating a mixture containing the composite material, the metal source, and the liquid medium under pressure to precipitate the metal compound on a surface of the composite material.
[0082] [3] The method for producing an electrode active material for a lithium-sulfur battery according to [2], wherein the heat treatment under pressure is carried out at a temperature equal to or higher than the boiling point of the liquid medium.
[0083] [4] The method for producing an electrode active material for a lithium-sulfur battery according to [2] or [3], wherein the heat treatment under pressure is carried out in a closed system.
[0084] [5] The method for producing an electrode active material for a lithium-sulfur battery according to [1], wherein obtaining the first modified composite material includes adjusting a pH of a mixture containing the composite material, a metal source, and a liquid medium to precipitate the metal compound on a surface of the composite material.
[0085] [6] The method for producing an electrode active material for a lithium-sulfur battery according to [1], wherein obtaining the first modified composite material includes adding a sulfur source to a mixture containing the composite material, a metal source, and a liquid medium, and precipitating the metal compound on a surface of the composite material.
[0086] [7] The method for producing an electrode active material for a lithium-sulfur battery according to [6], wherein obtaining the first modified composite material further comprises adjusting a pH of the mixture.
[0087] [8] The method for producing an electrode active material for a lithium-sulfur battery according to any one of [1] to [7], wherein the porous carbon material has a peak pore size of 0.5 nm or more and 10 nm or less.
[0088] [9] The method for producing an electrode active material for a lithium-sulfur battery according to any one of [1] to [8], wherein the porous carbon material has a volume average particle size of 0.5 μm or more and 20 μm or less.
[0089]
[10] The method for producing an electrode active material for a lithium-sulfur battery according to any one of [1] to [9], wherein the porous carbon material has an aspect ratio of 1 or more and 3 or less.
[0090]
[11] The method for producing an electrode active material for a lithium-sulfur battery according to any one of [1] to
[10] , wherein the heat treatment of the first modified composite material includes removing at least a part of the liquid medium to obtain a dried product.
[0091]
[12] The method for producing an electrode active material for a lithium-sulfur battery according to
[11] , wherein the heat treatment of the first modified composite material further includes heat treating the dried material at 50°C or higher and 400°C or lower.
[0092]
[13] A positive electrode active material for a lithium-sulfur battery, comprising a porous carbon material, sulfur supported on the porous carbon material, and a metal sulfide containing a specific metal, wherein the ratio of the mass ratio of the specific metal to the total amount of carbon, sulfur, oxygen, nitrogen, and the specific metal in the vicinity of the surface of the positive electrode active material for a lithium-sulfur battery measured by X-ray photoelectron spectroscopy to the mass content of the specific metal in the positive electrode active material for a lithium-sulfur battery measured by inductively coupled plasma atomic emission spectroscopy is 0.3 or more, and the specific metal comprises at least one selected from the group consisting of Ti, V, Mn, Fe, Co, Ni, Cu, Zn, Ge, Zr, In, Sn, Nb, Mo, Ta, and W.
[0093]
[14] The electrode active material for a lithium-sulfur battery according to
[13] , wherein the porous carbon material has a peak pore diameter of 0.5 nm or more and 10 nm or less.
[0094]
[15] The electrode active material for a lithium-sulfur battery according to
[13] or
[14] , wherein the porous carbon material has a volume average particle size of 0.5 μm or more and 20 μm or less.
[0095]
[16] The electrode active material for a lithium-sulfur battery according to any one of
[13] to
[15] , wherein the porous carbon material has an aspect ratio of 1 or more and 3 or less.
[0096]
[17] The positive electrode active material for a lithium-sulfur battery according to any one of
[13] to
[16] , wherein the metal sulfide includes zinc sulfide.
[0097]
[18] The electrode active material for a lithium-sulfur battery according to
[17] , wherein the intensity ratio of a peak derived from a (220) plane of zinc sulfide to a peak derived from a (111) plane of zinc sulfide in an X-ray diffraction pattern is 0.42 or more.
[0098]
[19] The positive electrode active material for a lithium-sulfur battery according to any one of
[13] to
[18] , wherein the content of the specific metal in the positive electrode active material for a lithium-sulfur battery is 0.1 mass % or more and 20 mass % or less.
[0099]
[20] The cathode active material for a lithium-sulfur battery according to any one of
[13] to
[19] , wherein the ratio of the mass ratio of the specific metal to the total amount of carbon, sulfur, oxygen, nitrogen, and the specific metal in the vicinity of the surface of the cathode active material for a lithium-sulfur battery measured by X-ray photoelectron spectroscopy to the mass content of the specific metal in the cathode active material for a lithium-sulfur battery measured by inductively coupled plasma atomic emission spectroscopy is 0.5 or more.
[0100]
[21] The cathode active material for a lithium-sulfur battery according to any one of
[13] to
[20] , wherein the ratio of the mass ratio of the specific metal to the total amount of carbon, sulfur, oxygen, nitrogen, and the specific metal in the vicinity of the surface of the cathode active material for a lithium-sulfur battery measured by X-ray photoelectron spectroscopy to the mass content of the specific metal in the cathode active material for a lithium-sulfur battery measured by inductively coupled plasma atomic emission spectroscopy is 0.7 or more.
[0101] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples.
[0102] Example 1: Preparation of ZnS-containing sulfur-carbon positive electrode active material. 12 g of a porous carbon material (manufactured by AT Electrode Co., Ltd., AP20-0001HC) and 18 g of sulfur powder (weight ratio: 40:60) were mixed to obtain a mixture. The resulting mixture was placed in a pressure-resistant container and heat-treated at 150°C for 3 hours to obtain a composite material as a sulfur-carbon composite. The physical properties of the porous carbon material used are shown in Table 1. The nitrogen adsorption isotherm, BET specific surface area, and pore size distribution were analyzed using the quenched solid density functional theory (QSDFT) method using a "Novatouch" manufactured by Quantachrome. The aspect ratio was calculated as follows.
[0103] Calculation of aspect ratio The porous carbon material before impregnation with sulfur was mounted on a carbon tape, and the shape of the porous carbon material was observed using an electron microscope (Hitachi High-Technologies Corporation, FLEXSEM1000II). The observation was performed under conditions of an acceleration voltage of 5 kV and a magnification of 10,000 times. Any particle whose particle shape can be confirmed (visually observed under SEM, the arithmetic mean of the major and minor diameters is D50 The aspect ratios of the 47 particles (47 particles with a particle size of 0.1 to 1.5 times the particle size) were determined using Image J, and the average value was calculated, resulting in an aspect ratio of 1.15.
[0104] Measurement of particle size distribution The volumetric particle size distribution was measured using a laser diffraction particle size distribution analyzer (MASTERSIZER 2000 manufactured by Malvern). For the measurement sample, an appropriate amount of carbon material was dispersed in 170 mL of ethanol solvent so that the laser intensity of the measurement device was within the appropriate range. The stirring process was carried out at 2500 rpm for 60 seconds. The volumetric average particle size was calculated as the 50% particle size D where the volume cumulative value from the small particle size side in the volumetric particle size distribution is 50%. 50 The 10% particle size D was calculated as the value at which the volume integrated value from the small particle size side becomes 10% and 90%. 10 and 90% particle size D 90 The results are shown in Table 1.
[0105]
[0106] 4 g of the composite material was mixed with 0.3 g of zinc oxide. 8 g of pure water was added to the mixture of zinc oxide and the composite material and mixed to obtain a slurry as a dispersion of zinc oxide and the composite material. The obtained slurry was placed in a pressure-resistant container and heat-treated at 230°C for 3 hours in a sealed system. The heat-treated slurry was subjected to suction filtration, and the filtered material was dried at 50°C for 30 minutes to obtain a dried product. The dried product was placed in a sealed container and heat-treated at 300°C for 3 hours to obtain the ZnS-containing sulfur-carbon positive electrode active material of Example 1 as a coated composite material.
[0107] Example 2 A ZnS-containing sulfur-carbon positive electrode active material of Example 2 was prepared in the same manner as in Example 1, except that the amount of zinc oxide added to the mixture was changed to 0.15 g.
[0108] Example 3 A ZnS-containing sulfur-carbon positive electrode active material of Example 3 was prepared in the same manner as in Example 1, except that the amount of zinc oxide added to the mixture was changed to 0.6 g.
[0109] Example 4: 1.05 g of zinc sulfate heptahydrate (Fujifilm Wako Pure Chemical Industries, Ltd.) was added to 36 g of pure water to obtain a zinc sulfate aqueous solution. 4.0 g of the composite material was mixed with the resulting solution to obtain a dispersion slurry. 0.58 g of sodium hydroxide (Fujifilm Wako Pure Chemical Industries, Ltd.) was added to 40 g of pure water and dissolved to obtain a sodium hydroxide aqueous solution. The sodium hydroxide aqueous solution was added to the dispersion slurry obtained above and stirred for 10 minutes. The pH of the slurry was 12.8 to 12.9. After stirring, the slurry was suction filtered, and the filtered product was heated at 50°C for 30 minutes to obtain a dried product. The steam-dried product was placed in a sealed oven and heat-treated at 300°C for 3 hours to obtain the ZnS-containing sulfur-carbon positive electrode material of Example 4 as a coated composite material.
[0110] Comparative Example 1: Preparation of Sulfur-Carbon Positive Electrode Active Material 12 g of a porous carbon material (manufactured by AT Electrode Co., Ltd., AP20-0001HC) and 18 g of sulfur powder (weight ratio: 40:60) were mixed. The mixture of the porous carbon material and sulfur powder was placed in a pressure-resistant container and heat-treated at 150°C for 3 hours. The mixture was then returned to room temperature and heat-treated at 350°C for 3 hours to obtain the sulfur-carbon positive electrode active material of Comparative Example 1.
[0111] Comparative Example 2 A composite material was obtained as a sulfur-carbon composite in the same manner as in Example 1. 4.0 g of the obtained composite material and 0.36 g of zinc sulfide (Kishida Chemical Co., Ltd.) were mixed, placed in a sealed container, and heat-treated at 300°C for 3 hours to obtain a ZnS-containing sulfur-carbon positive electrode active material of Comparative Example 2.
[0112] X-ray Diffraction (XRD) Analysis XRD analysis (Miniflex, manufactured by Rigaku Corporation) was performed on the ZnS-containing sulfur-carbon positive electrode active materials prepared in Examples 1, 2, 3, 4, and Comparative Examples 1 and 2. Figures 1 to 4 show the XRD analysis results for the ZnS-containing sulfur-carbon positive electrode active materials prepared in Examples 1 to 4. Figure 5 shows the XRD analysis results for the sulfur-carbon positive electrode active material of Comparative Example 1, and Figure 6 shows the XRD analysis results for the positive electrode active material of Comparative Example 2.
[0113] 1, a peak originating from the (111) plane of ZnS was observed around 28.5°, confirming that crystalline ZnS was formed in the sulfur-carbon positive electrode active material containing ZnS produced in Example 1. A peak originating from the (220) plane of ZnS was also observed around 47.5°. Furthermore, a peak originating from the (311) plane of ZnS was also observed around 56.5°.
[0114] ICP Analysis The positive electrode active material obtained above was subjected to inductively coupled plasma (ICP) atomic emission spectroscopy to determine the mass-based content (Ci) of Zn, a specific metal contained in the positive electrode active material. Specifically, a sample was prepared using nitric acid and heated and dissolved by microwaves, and the Zn content was determined using an inductively coupled plasma (ICP) atomic emission spectroscopy analyzer (ICP-AES; Optima 8300: manufactured by Perkin Elmer). The results are shown in Table 2.
[0115] Surface composition analysis: Using a scanning electron microscope (SEM) / energy dispersive X-ray analyzer (EDX) (Hitachi High-Technologies Corporation; accelerating voltage 5 kV, magnification 1500x, spectral area counts > 2,500,000), the ratio (Cx) of zinc to the total amount of carbon, sulfur, oxygen, nitrogen, and zinc near the surface of the positive electrode active material was determined at three locations, and the arithmetic average was calculated. Furthermore, the dispersion index Cx / Ci of the specific metal was calculated. The results are shown in Table 2. The SEM image used for EDX analysis of Example 1 is shown in FIG. 7.
[0116] Preparation of Positive Electrode for Lithium-Sulfur Secondary Battery A positive electrode slurry composition was prepared by mixing 85 parts by weight of the sulfur-carbon positive electrode active material prepared in Example 1 and Comparative Example 1, 10 parts by weight of carbon black, and 5 parts by weight of styrene butadiene rubber (SBR) / carboxymethyl cellulose (CMC) / polyvinylpyrrolidone (PVP) (SBR / CMC / PVP=2.0 / 2.5 / 0.5).
[0117] The obtained positive electrode slurry composition was applied to a current collector and dried at 50° C. for 30 minutes. The current collector was an aluminum foil coated with carbon. The dried product was pressed with a roll press to a density of the active material layer of 1.0 g / cm. 3After that, the positive electrode for a lithium-sulfur secondary battery of Example 1 was obtained by cutting it into a predetermined size.
[0118] Preparation of non-aqueous electrolyte solution Fluoroethylene carbonate (FEC) and dimethyl carbonate (DMC) were mixed in a volume ratio of 71:100 to obtain a mixed solution. Lithium hexafluorophosphate (LiPF 6 ) was dissolved in the solution to a concentration of 1.0 mol / L to prepare a non-aqueous electrolyte solution.
[0119] Assembly of Lithium-Sulfur Secondary Battery A lead electrode was attached to the positive electrode obtained above, and a separator made of porous polypropylene (Celgard 2400) was placed inside a bag-shaped laminate pack. After storage, the pack was vacuum dried at 50°C to remove moisture adsorbed by each component. After vacuum drying, the metallic lithium of the negative electrode placed on SUS foil was placed inside the laminate pack facing the positive electrode via the porous polypropylene, and the nonaqueous electrolyte prepared above was poured into the laminate pack and sealed to obtain a laminate-type lithium-sulfur secondary battery as an evaluation battery. The following battery characteristics were evaluated using the obtained evaluation battery.
[0120] Evaluation of Charge-Discharge Cycle Capacity Retention Rate The test battery obtained as described above was placed in a thermostatic chamber at 25°C, and a test to evaluate the cycle capacity retention rate was conducted. The charge-discharge voltage was in the range of 1.0 V to 3.0 V. The discharge current was the current value when 0.1 C capacity was extracted. The discharge capacity per mass of sulfur, Qcyc(2), at the second cycle immediately after the start of discharge was measured. Next, charge and discharge were repeated, and the discharge capacity, Qcyc(30), at the 30th cycle was measured. The capacity retention rate, Pcyc, after 30 cycles was calculated by dividing Qcyc(30) by the obtained Qcyc(2) (= 100 × Qcyc(30) / Qcyc(2)) (%). The results are shown in Table 2.
[0121]
[0122] The evaluation batteries containing the ZnS-containing sulfur-carbon positive electrode active material in Examples 1 to 4 had improved cycle characteristics compared to Comparative Example 1. The cycle characteristics in Comparative Example 2 were worse. This is thought to be because the dispersion index was low, causing ZnS to segregate, which prevented the coating from sufficiently suppressing side reactions between sulfur and the electrolyte. Furthermore, the peak intensity ratio (220 / 111) of ZnS in Examples 1 to 4 was higher than in the comparative example. A low ratio (220 / 111) is thought to indicate a low occupancy rate of S sites in ZnS, resulting in S defects in the structure. Therefore, the crystal structure of ZnS became unstable during repeated charge and discharge, resulting in poor cycle characteristics.
[0123] The disclosure of Japanese Patent Application No. 2023-050319 (filing date: March 27, 2023) is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards mentioned herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard was specifically and individually indicated to be incorporated by reference.
Claims
1. A method for producing an electrode active material for a lithium-sulfur battery, comprising: mixing a composite material comprising a porous carbon material and sulfur supported on the porous carbon material, a metal source, and a liquid medium to obtain a first modified composite material having a metal compound derived from the metal source attached thereto; and heat-treating the first modified composite material to obtain a second modified composite material having a metal sulfide derived from the metal source attached thereto, wherein the metal source comprises at least one specific metal selected from the group consisting of Ti, V, Mn, Fe, Co, Ni, Cu, Zn, Ge, Zr, In, Sn, Nb, Mo, Ta and W.
2. A method for producing an electrode active material for a lithium-sulfur battery as described in claim 1, wherein obtaining the first modified composite material includes heat-treating a mixture containing the composite material, the metal source and the liquid medium under pressure to precipitate the metal compound on the surface of the composite material.
3. The method for producing an electrode active material for a lithium-sulfur battery according to claim 2, wherein the heat treatment under pressure is carried out at a temperature equal to or higher than the boiling point of the liquid medium.
4. The method for producing an electrode active material for a lithium-sulfur battery according to claim 2 or 3, wherein the heat treatment under pressure is carried out in a closed system.
5. A method for producing an electrode active material for a lithium-sulfur battery as described in claim 1, wherein obtaining the first modified composite material includes adjusting the pH of a mixture containing the composite material, the metal source and the liquid medium to precipitate the metal compound on the surface of the composite material.
6. A method for producing an electrode active material for lithium-sulfur batteries as described in claim 1, wherein obtaining the first modified composite material includes adding a sulfur source to a mixture containing the composite material, the metal source and the liquid medium, and precipitating the metal compound on the surface of the composite material.
7. The method for producing an electrode active material for a lithium-sulfur battery according to claim 6, wherein obtaining the first modified composite material further comprises adjusting a pH of the mixture.
8. A method for producing an electrode active material for a lithium-sulfur battery according to any one of claims 1 to 7, wherein the porous carbon material has a peak pore diameter of 0.5 nm or more and 10 nm or less.
9. A method for producing an electrode active material for a lithium-sulfur battery according to any one of claims 1 to 8, wherein the porous carbon material has a volume average particle size of 0.5 μm or more and 20 μm or less.
10. A method for producing an electrode active material for a lithium-sulfur battery described in any one of claims 1 to 9, wherein the porous carbon material has an aspect ratio of 1 or more and 3 or less.
11. A method for producing an electrode active material for a lithium-sulfur battery as described in claim 1, wherein the heat treatment of the first modified composite material includes removing at least a portion of the liquid medium to obtain a dried product.
12. The method for producing an electrode active material for a lithium-sulfur battery according to claim 11, wherein the heat treatment of the first modified composite material further comprises heat treating the dried material at 50°C or more and 400°C or less.
13. A positive electrode active material for a lithium-sulfur battery comprising a porous carbon material, sulfur supported on the porous carbon material, and a metal sulfide containing a specific metal, wherein a ratio of a mass ratio of the specific metal to a total amount of carbon, sulfur, oxygen, nitrogen, and the specific metal in the vicinity of a surface of the positive electrode active material for a lithium-sulfur battery measured by X-ray photoelectron spectroscopy relative to a mass content of the specific metal in the positive electrode active material for a lithium-sulfur battery measured by inductively coupled plasma atomic emission spectroscopy is 0.3 or more, and the specific metal comprises at least one selected from the group consisting of Ti, V, Mn, Fe, Co, Ni, Cu, Zn, Ge, Zr, In, Sn, Nb, Mo, Ta, and W.
14. The electrode active material for a lithium-sulfur battery according to claim 13, wherein the porous carbon material has a peak pore size of 0.5 nm or more and 10 nm or less.
15. The electrode active material for a lithium-sulfur battery according to claim 13 or 14, wherein the porous carbon material has a volume average particle size of 0.5 μm or more and 20 μm or less.
16. The electrode active material for a lithium-sulfur battery according to any one of claims 13 to 15, wherein the porous carbon material has an aspect ratio of 1 or more and 3 or less.
17. A positive electrode active material for a lithium-sulfur battery according to any one of claims 13 to 16, wherein the ratio of the mass ratio of the specific metal to the total amount of carbon, sulfur, oxygen, nitrogen and the specific metal in the vicinity of the surface of the positive electrode active material for a lithium-sulfur battery measured by X-ray photoelectron spectroscopy to the mass-based content of the specific metal in the positive electrode active material for a lithium-sulfur battery measured by inductively coupled plasma atomic emission spectroscopy is 0.5 or more.
18. A positive electrode active material for a lithium-sulfur battery as described in claim 17, wherein the ratio of the mass ratio of the specific metal to the total amount of carbon, sulfur, oxygen, nitrogen and the specific metal in the vicinity of the surface of the positive electrode active material for a lithium-sulfur battery as measured by X-ray photoelectron spectroscopy to the mass-based content of the specific metal in the positive electrode active material for a lithium-sulfur battery as measured by inductively coupled plasma atomic emission spectroscopy is 0.7 or more.
19. The positive electrode active material for a lithium-sulfur battery according to any one of claims 13 to 18, wherein the metal sulfide includes zinc sulfide.
20. The positive electrode active material for a lithium-sulfur battery according to claim 19, wherein in an X-ray diffraction pattern, the intensity ratio of the peak originating from the (220) plane of zinc sulfide to the peak originating from the (111) plane is 0.42 or more.
21. A positive electrode active material for a lithium-sulfur battery according to any one of claims 13 to 20, wherein the content of the specific metal in the positive electrode active material for a lithium-sulfur battery is 0.1 mass % or more and 20 mass % or less.
Citation Information
Patent Citations
Composite material, positive electrode for lithium sulfur battery, lithium sulfur battery, and method for manufacturing composite material
JP2021136126A
Positive electrode material for lithium ion batteries, and lithium ion battery
WO2012086196A1