Diffusion film, light diffusion device, and method for manufacturing diffusion film

The multi-layer diffusion film with varying haze levels and alternately laminated supporting base materials addresses the non-uniformity and durability issues in PDLC-based light diffusion devices, achieving enhanced in-plane brightness and stability.

WO2024203123A1PCT designated stage expired Publication Date: 2024-10-03NITTO DENKO CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/008811
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-07
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing diffusion films used in light diffusion devices, particularly those with PDLC layers, often result in non-uniform in-plane luminance and are prone to issues like scratches, pattern changes, or bubble formation when laminated, which affect their scattering properties and durability.

Method used

A diffusion film with multiple layers of a polymer matrix and dispersed liquid crystal particles, where each layer can have varying haze levels and be alternately laminated with supporting base materials, allowing for increased thickness and improved uniformity of light scattering, and optionally including a thickening layer for enhanced distance from the light source.

Benefits of technology

The multi-layer structure enhances the uniformity of in-plane brightness and prevents issues like scratches and pattern changes, ensuring consistent light emission and improved durability by increasing the total thickness of the diffusion layers while maintaining handleability and mechanical strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024008811_03102024_PF_FP_ABST
    Figure JP2024008811_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a diffusion film capable of achieving more uniform surface light emission when used as a light diffusion device in combination with a light source unit. A diffusion film according to an embodiment of the present invention has two or more diffusion layers including: a polymer matrix; and dispersion particles that are dispersed in the polymer matrix and contain at least one selected from among a liquid crystal compound and a liquid crystal polymer.
Need to check novelty before this filing date? Find Prior Art

Description

Diffusion film, light diffusion device, and method for manufacturing the diffusion film

[0001] The present invention relates to a diffusion film, a light diffusion device, and a method for manufacturing a diffusion film.

[0002] A PDLC film having a polymer dispersed liquid crystal (hereinafter sometimes referred to as "PDLC") layer between a pair of transparent electrode layers is a type of light control film that can be switched between a light scattering state (scattering state) and a light transmitting state (non-scattering state or transparent state) by switching between a voltage applied state and a voltage not applied state. Specifically, the PDLC layer includes a polymer matrix and droplets of a liquid crystal compound (hereinafter sometimes referred to as "liquid crystal droplets") dispersed in the polymer matrix, and the liquid crystal droplets act as scattering particles, causing light scattering due to the difference in refractive index between the liquid crystal compound in the liquid crystal droplets and the polymer matrix, etc.

[0003] In recent years, display devices and lighting devices that use light-emitting diodes (hereinafter referred to as LEDs) as light sources have become widespread due to their low power consumption and the ability to be made smaller and thinner, and a diffusion film is placed over the light source to obtain uniform surface light emission.

[0004] The above-mentioned diffusion film includes a surface-type diffusion film in which a diffusion pattern is formed on the surface by textured processing, dot printing, etc. When a surface-type diffusion film is laminated to an adjacent member without an adhesive layer, scratches may be caused on the adjacent member due to rubbing, or the diffusion pattern may change over time, etc. Furthermore, when the surface-type diffusion film is laminated to an adjacent member via an adhesive layer, the diffusion pattern may change or disappear due to the adhesive, or air bubbles may be generated in the textured portions, etc.

[0005] Another type of diffusion film is an internal diffusion film containing scattering particles inside. A PDLC film having the above-mentioned PDLC layer can be used as an internal diffusion film by utilizing the scattering effect of the liquid crystal droplets (for example, Patent Document 1).

[0006] Japanese Patent Application Laid-Open No. 2021-077534

[0007] When a PDLC film is combined with a light source and used as a light diffusion device, the in-plane luminance may not be uniform enough. Therefore, a main object of the present invention is to provide a diffusion film that can achieve more uniform surface emission when combined with a light source and used as a light diffusion device.

[0008] [1] According to one aspect of the present invention, there is provided a diffusion film having two or more diffusion layers each including a polymer matrix and dispersed particles containing at least one selected from a liquid crystal compound and a liquid crystal polymer, the particles being dispersed in the polymer matrix. [2] In the diffusion film of [1] above, the diffusion layers may have a total thickness of 50 μm or more. [3] The diffusion film of [1] or [2] above may have two or more structural units each including a pair of supporting substrates and the diffusion layer disposed therebetween. [4] The diffusion film of [1] or [2] above may have a laminated structure in which the supporting substrates and the diffusion layers are alternately arranged. [5] The diffusion film of any of [1] to [4] above may further include a thickening layer. [6] In the diffusion film of any of [1] to [5] above, at least one of the diffusion layers may have regions with different hazes in plan view. [7] In the diffusion film of [6] above, the regions with different hazes may be arranged in a predetermined pattern. [8] In the diffusion film according to [6] or [7] above, the difference between the maximum and minimum haze values ​​may be 10% or more. [9] According to another aspect of the present invention, there is provided a light diffusion device comprising the diffusion film according to any one of [1] to [8] above and a light source unit.

[10] In the light diffusion device according to [9] above, the light source unit may include a plurality of point light sources.

[11] According to another aspect of the present invention, there is provided a method for producing a diffusion film, comprising: Step I of applying a coating liquid containing a polymer matrix-forming resin, a liquid crystal compound, and a solvent to a supporting substrate to obtain a coating layer; Step II of drying the coating layer to obtain a polymer-dispersed liquid crystal layer containing a polymer matrix and dispersed particles containing the liquid crystal compound dispersed in the polymer matrix; and Step III of laminating another supporting substrate on the polymer-dispersed liquid crystal layer, wherein Steps I to III are repeated two or more times to produce a laminate in which two or more supporting substrates and two or more polymer-dispersed liquid crystal layers are alternately arranged.

[12] In the manufacturing method described in

[11] above, the liquid crystal compound may include a polymerizable liquid crystal compound and a non-polymerizable liquid crystal compound, and the manufacturing method may include applying an active energy ray to a predetermined region while applying a voltage to the polymer dispersed liquid crystal layer included in the laminate, thereby polymerizing the polymerizable liquid crystal compound.

[0009] While it is difficult to increase the thickness of a PDLC layer due to film-forming properties, the diffusion film according to the present invention has two or more diffusion layers, ensuring a sufficient total thickness of the diffusion layers, thereby improving scattering properties and more effectively achieving uniform in-plane luminance.

[0010] 1A to 1C are schematic cross-sectional views each illustrating a configuration of a diffusion film according to one embodiment of the present invention. 1A to 1C are schematic cross-sectional views each illustrating an example of a configuration of a diffusion layer. 1B are schematic views each illustrating an example of a manufacturing method of a diffusion layer. 1C are schematic cross-sectional views each illustrating an example of a manufacturing method of a diffusion layer. 1D are schematic cross-sectional views each illustrating a configuration of a light diffusion device according to one embodiment of the present invention.

[0011] Preferred embodiments of the present invention will be described below, but the present invention is not limited to these embodiments. Furthermore, the embodiments can be combined as appropriate. In this specification, the expression "to" indicating a range of values ​​includes the upper and lower limits.

[0012] A. Diffusion Film The diffusion film according to an embodiment of the present invention has two or more diffusion layers, each containing a polymer matrix and dispersed particles, the particles including at least one selected from a liquid crystal compound and a liquid crystal polymer, dispersed in the polymer matrix. This configuration allows the diffusion film according to an embodiment of the present invention to achieve more uniform surface emission when used in combination with a light source as a light diffusion device. Furthermore, because the two or more diffusion layers are integrated, problems such as deterioration due to friction between films, film waviness, and watermarks, which may occur when diffusion films are stacked without being integrated, can be avoided.

[0013] The haze of the diffusion film can be set appropriately depending on the application, etc. The haze of the diffusion film can be, for example, 50% to 80%, or for example, 70% to 100%. When the diffusion film includes a diffusion layer having regions with different hazes as described below, the maximum haze of the diffusion film can be, for example, 30% to 100%, and the minimum haze can be, for example, 0% to 70%. The difference between the maximum and minimum haze values ​​typically exceeds 0%, and can be, for example, 5% or more, preferably 10% or more, more preferably 20% to 100%, and even more preferably 30% to 100%.

[0014] 1(a) to 1(c) are schematic cross-sectional views illustrating the configuration of a diffusion film according to one embodiment of the present invention. The diffusion film shown in FIG. 1(a) has two structural units, each including a pair of support substrates and a diffusion layer disposed therebetween. Specifically, the diffusion film 100A has a first structural unit 30a, which includes a pair of support substrates 20a, 20a' and a diffusion layer 10a disposed therebetween, and a second structural unit 30b, which includes a pair of support substrates 20b, 20b' and a diffusion layer 10b disposed therebetween. The first structural unit 30a and the second structural unit 30b are typically laminated via an adhesive layer (not shown). The diffusion layer and the support substrate may be laminated via an adhesive layer, or may be laminated in close contact without an adhesive layer. In one embodiment, the diffusion layer and the support substrate are laminated in close contact without an adhesive layer. Preferred examples of the adhesive layer include an adhesive layer or a pressure-sensitive adhesive layer. The thickness of the adhesive layer is, for example, 0.1 μm to 50 μm, preferably 0.3 μm to 30 μm.

[0015] The diffusion film shown in Fig. 1(b) has a laminated structure in which support substrates and diffusion layers are alternately arranged. Specifically, diffusion film 100B has, in this order, a first support substrate 20a, a first diffusion layer 10a, a second support substrate 20b, a second diffusion layer 10b, and a third support substrate 20c. These diffusion layers and support substrates are typically laminated without an adhesive layer. In a diffusion film having a laminated structure in which support substrates and diffusion layers are alternately arranged, support substrates are preferably arranged on both sides of the diffusion layer from the standpoints of handleability, durability, etc.

[0016] The diffusion film shown in FIG. 1( c) further includes a thickening layer in addition to the support substrate and the diffusion layer. Specifically, the diffusion film 100C includes a thickening layer 40 disposed on the first support substrate 20a side of the diffusion film 100B. The thickening layer is typically laminated to the first support substrate 20a via an adhesive layer. When a diffusion film having a thickening layer is disposed above a light source, the distance from the light source to the diffusion layer can be sufficiently secured, resulting in more uniform in-plane brightness. The thickening layer may be disposed on one side (the light source side) of two or more diffusion layers, as in the illustrated example, or may be disposed between two or more diffusion layers, as in the illustrated example.

[0017] The number of diffusion layers in the diffusion film is not limited to the illustrated example. The number of diffusion layers in the diffusion film may be, for example, 2 to 4, and preferably 2 to 3. Therefore, for example, embodiments of the present invention also include a configuration in which one or more of the above structural units are laminated to second structural unit 30b of diffusion film 100A via an adhesive layer, and a configuration in which one or more of the above structural units are laminated to third support substrate 20c of diffusion film 100B via an adhesive layer.

[0018] The total thickness of the diffusion layers included in the diffusion film is, for example, 50 μm or more, preferably 60 μm or more, more preferably 70 μm or more, and even more preferably 80 μm or more. Due to their structure, it is difficult to increase the thickness of each diffusion layer used in embodiments of the present invention. However, by stacking two or more diffusion layers, the total thickness of the diffusion layers can be increased, resulting in a diffusion film with excellent diffusion properties. The upper limit of the total thickness of the diffusion layers is, for example, 300 μm or less, or, for example, 200 μm or less, from the viewpoint of reducing the complexity of the manufacturing process and thinning the diffusion film.

[0019] In the above-mentioned diffusion film, at least one of the thicknesses from one surface to the diffusion layer disposed furthest from the surface (thickness indicated by T1 or T2 in FIG. 1(c)) is, for example, 100 μm or more, preferably 100 μm to 400 μm, and more preferably 100 μm to 300 μm. If the distance from one surface to the diffusion layer is within the above range, when the film is disposed above a light source unit, the distance from the light source unit to the diffusion layer can be ensured, and as a result, the in-plane luminance can be more suitably uniformed.

[0020] The total thickness of the diffusion film is, for example, 100 μm to 450 μm, preferably 125 μm to 425 μm, and more preferably 150 μm to 400 μm.

[0021] A-1. Diffusion Layer The diffusion layer comprises a polymer matrix and dispersed particles, dispersed in the polymer matrix, containing at least one selected from a liquid crystal compound and a liquid crystal polymer. Two or more diffusion layers included in the diffusion film may have the same configuration (type or composition of the polymer matrix, liquid crystal compound, and liquid crystal polymer, dispersed particle size, thickness, etc.) or different configurations.

[0022] The diffusion layer may have a substantially uniform haze in plan view, or may have regions with different hazes. The regions with different hazes may be formed in any suitable pattern depending on the purpose. For example, for a light source unit having point light sources arranged in a predetermined pattern, a diffusion film having a diffusion layer with high haze regions in a pattern corresponding to the arrangement of the point light sources and other regions with low haze regions can be used to suitably achieve uniform in-plane brightness. Note that the diffusion film may include both a diffusion layer with a substantially uniform haze in plan view and a diffusion layer with regions with different hazes. Furthermore, when the diffusion film includes two or more diffusion layers with regions with different hazes, the formation patterns of the regions with different hazes in these diffusion layers may be the same or different.

[0023] The haze of the diffusion layer can be set appropriately depending on the application of the diffusion film, the number of diffusion layers in the diffusion film, etc. The haze of a diffusion layer having a substantially uniform haze can be, for example, 50% to 80%, or, for example, 70% to 100%. The maximum haze of a diffusion layer having regions with different hazes can be, for example, 30% to 100%, and the minimum haze can be, for example, 0% to 70%. The difference between the maximum and minimum haze values ​​typically exceeds 0%, and can be, for example, 5% or more, preferably 10% or more, more preferably 20% to 100%, and even more preferably 30% to 100%.

[0024] 2(a) to 2(d) are schematic cross-sectional views illustrating an example of the configuration of a diffusion layer. The diffusion layer 10 shown in FIG. 2(a) includes a polymer matrix 12 and dispersed particles 16a containing a liquid crystal compound 13 dispersed in the polymer matrix 12. The liquid crystal compound 13 is in a non-oriented state in the dispersed particles 16a, and diffusibility is exhibited due to the difference in refractive index between the polymer matrix 12 and the dispersed particles 16a. The liquid crystal compound 13 used in this embodiment may be a polymerizable liquid crystal compound or a non-polymerizable liquid crystal compound.

[0025] The diffusion layer 10 shown in FIG. 2( b) includes a polymer matrix 12 and dispersed particles 16 b containing a liquid crystal polymer 14 dispersed in the polymer matrix 12. The liquid crystal polymer 14 is fixed in a non-oriented state within the dispersed particles 16 b, and diffusivity is exhibited due to the difference in refractive index between the polymer matrix 12 and the dispersed particles 16 b. The liquid crystal polymer is a polymer of a polymerizable liquid crystal compound and is non-liquid crystal. That is, the liquid crystal polymer does not undergo, for example, the transition to a liquid crystal phase, glass phase, or crystalline phase due to temperature changes that is typical of liquid crystal compounds. In this embodiment, dispersed particles containing a liquid crystal polymer and a liquid crystal compound may be used instead of the dispersed particles 16 b. In this case, a non-polymerizable liquid crystal compound is preferably used as the liquid crystal compound.

[0026] The diffusion layer 10 shown in FIG. 2( c) includes a polymer matrix 12 and dispersion particles 16 c dispersed in the polymer matrix 12 and containing a non-polymerizable liquid crystal compound 13 a and a liquid crystal polymer 14. In region A, the liquid crystal polymer 14 in the dispersion particles 16 c is fixed in a non-oriented state, and the non-polymerizable liquid crystal compound 13 a is also non-oriented along with the liquid crystal polymer 14. On the other hand, in region B, the liquid crystal polymer 14 in the dispersion particles 16 c is fixed in a state oriented in the thickness direction (substantially perpendicular to the main surface), and the non-polymerizable liquid crystal compound 13 a is also oriented along with the liquid crystal polymer 14. With a diffusion layer configured in this manner, region A exhibits a higher haze than region B in a planar view. In this embodiment, dispersion particles containing a liquid crystal polymer but not a non-polymerizable liquid crystal compound may be used instead of the dispersion particles 16 c, as long as they can form the above-described orientation state of the liquid crystal polymer.

[0027] The diffusion layer 10 shown in FIG. 2( d ) includes a polymer matrix 12, dispersion particles 16 c containing a non-polymerizable liquid crystal compound 13 a and a liquid crystal polymer 14, and dispersion particles 16 d containing a non-polymerizable liquid crystal compound 13 a and a polymerizable liquid crystal compound 13 b. In region A, the non-polymerizable liquid crystal compound 13 a and the polymerizable liquid crystal compound 13 b in the dispersion particles 16 d are both non-oriented. Meanwhile, in region B, the liquid crystal polymer 14 in the dispersion particles 16 c is fixed in an oriented state in the thickness direction (substantially perpendicular to the main surface), and the non-polymerizable liquid crystal compound 13 a is also oriented along with the liquid crystal polymer 14. With a diffusion layer having such a configuration, region A exhibits a higher haze than region B in a planar view. In this embodiment, dispersion particles containing a liquid crystal polymer but not a non-polymerizable liquid crystal compound and dispersion particles containing a polymerizable liquid crystal compound but not a non-polymerizable liquid crystal compound may be used instead of the dispersion particles 16 c and the dispersion particles 16 d, as long as they can form the above-described orientation state of the liquid crystal polymer.

[0028] The polymer matrix may be composed of any appropriate resin. The resin for forming the polymer matrix may be appropriately selected depending on the light transmittance, the refractive index of the liquid crystal polymer or liquid crystal compound, the adhesion to the support substrate, etc. For example, water-soluble or water-dispersible resins such as urethane-based resins, polyvinyl alcohol-based resins, polyethylene-based resins, polypropylene-based resins, and acrylic-based resins may be preferably used. The resin for forming the polymer matrix may be used alone or in combination.

[0029] The content of the polymer matrix in the diffusion layer is, for example, 30 to 70% by weight, preferably 35 to 65% by weight, and more preferably 40 to 60% by weight. If the content of the polymer matrix is ​​within this range, good mechanical strength can be obtained, and effects such as prevention of liquid crystal leakage from the edges can be obtained.

[0030] As the non-polymerizable liquid crystal compound, any suitable non-polymerizable liquid crystal compound can be used alone or in combination of two or more. The dielectric anisotropy of the non-polymerizable liquid crystal compound may be positive or negative. The non-polymerizable liquid crystal compound may be, for example, a nematic, smectic, or cholesteric liquid crystal compound. It is preferable to use a nematic liquid crystal compound because it can achieve high transparency in the aligned state.

[0031] Examples of nematic liquid crystal compounds include biphenyl-based compounds, phenylbenzoate-based compounds, cyclohexylbenzene-based compounds, azoxybenzene-based compounds, azobenzene-based compounds, azomethine-based compounds, terphenyl-based compounds, biphenylbenzoate-based compounds, cyclohexylbiphenyl-based compounds, phenylpyridine-based compounds, cyclohexylpyrimidine-based compounds, cholesterol-based compounds, fluorine-based compounds, etc. These low-molecular-weight liquid crystal compounds may be used alone or in combination.

[0032] The birefringence Δn (=ne−no; ne is the refractive index of the liquid crystal compound molecules in the major axis direction, and no is the refractive index of the liquid crystal compound molecules in the minor axis direction) of the non-polymerizable liquid crystal compound at a wavelength of 589 nm is preferably 0.05 to 0.50, more preferably 0.10 to 0.45.

[0033] As the polymerizable liquid crystal compound, a polymerizable liquid crystal compound appropriately selected depending on the light transmittance, compatibility with the non-polymerizable liquid crystal compound, etc., can be used alone or in combination of two or more. The polymerizable liquid crystal compound may be a bifunctional or higher crosslinked type. Examples of the polymerizable liquid crystal compound include polymerizable mesogenic compounds described in JP-A-2002-533742 (WO 00 / 37585), EP 358208 (US 5,211,877), EP 66137 (US 4,388,453), WO 93 / 22397, EP 0,261,712, DE 19504224, DE 4408171, and GB 2,280,445. Nematic liquid crystal monomers are preferred as the polymerizable liquid crystal compound. The birefringence Δn of the polymerizable liquid crystal compound at a wavelength of 589 nm is preferably 0.05 to 0.50, more preferably 0.10 to 0.45.

[0034] The liquid crystal polymer is a polymer of the above polymerizable liquid crystal compound, and is non-liquid crystal, as described above.

[0035] The total content of the liquid crystal polymer and the liquid crystal compound (non-polymerizable liquid crystal compound and polymerizable liquid crystal compound) in the diffusion layer is, for example, 30% to 70% by weight, preferably 35% to 65% by weight, and more preferably 40% to 60% by weight. When the dispersed particles contain a liquid crystal polymer, the content of the liquid crystal polymer relative to the total content of the liquid crystal polymer and the liquid crystal compound in the diffusion layer may be, for example, 5% by weight or more, preferably 7% by weight or more, and more preferably 10% by weight or more, and may be, for example, 100% by weight or less, preferably 80% by weight or less, and more preferably 50% by weight or less. The total content of the polymer matrix, liquid crystal polymer, and liquid crystal compound in the diffusion layer may be, for example, 90% by weight to 99.9% by weight, and preferably 95% by weight to 99.9% by weight.

[0036] The diffusion layer may further contain any appropriate component, as necessary. Such optional components include a polymerization initiator, a surfactant, a leveling agent, a crosslinking agent, a dispersion stabilizer, etc. The total content of the optional components in the diffusion layer may be, for example, 0.1 to 10% by weight, preferably 0.1 to 5% by weight.

[0037] The average particle diameter of the dispersed particles can be, for example, 0.2 μm to 9 μm, preferably 0.3 μm to 8 μm. If the average particle diameter of the dispersed particles is too small, the dispersed particle size is smaller than the wavelength of light, so light passes through the dispersed particles without being scattered, which can result in a problem of insufficient haze being obtained. If the average particle diameter is too large, the dispersed particle size is larger than the wavelength of light, so can a problem of insufficient haze being obtained. Note that the average particle diameter of the dispersed particles in the diffusion layer is the volume average particle diameter of the dispersed particles when viewed from a direction perpendicular to the main surface of the diffusion layer.

[0038] The thickness of the diffusion layer is, for example, 10 μm to 60 μm, preferably 15 μm to 55 μm, and more preferably 20 μm to 50 μm.

[0039] A-2. Supporting Substrate The supporting substrate includes a substrate body. The supporting substrate may have a hard coat (HC) layer on one or both sides of the substrate body, as needed.

[0040] The substrate body may be formed using any suitable material. Specific examples include glass films and polymer films. Polymer films are preferred because they have excellent smoothness and can be continuously produced using rolls, greatly improving productivity.

[0041] The substrate body is typically a polymer film primarily composed of a thermoplastic resin. Examples of thermoplastic resins include polyester resins; cycloolefin resins such as polynorbornene; acrylic resins; polycarbonate resins; and cellulose resins. Among these, polyester resins, cycloolefin resins, and acrylic resins are preferred. These resins are excellent in transparency, mechanical strength, thermal stability, moisture barrier properties, and the like. The thermoplastic resins may be used alone or in combination of two or more. Optical films used in polarizing plates, such as low-retardation substrates, high-retardation substrates, retardation plates, absorptive polarizing films, and polarized selective reflection films, can also be used as the substrate body.

[0042] The haze of the supporting substrate is preferably 20% or less, more preferably 10% or less, and even more preferably 0.1% to 10%.

[0043] The total light transmittance of the supporting substrate is preferably 30% or more, more preferably 60% or more, and even more preferably 80% or more. The total light transmittance can be measured in accordance with JIS K 7361.

[0044] The thickness of the support substrate is, for example, 200 μm or less, preferably 3 μm to 150 μm, and more preferably 5 μm to 100 μm. When the diffusion layer is formed while applying a voltage as described in Section B, the thickness of the support substrate is preferably 50 μm or less, more preferably 3 μm to 40 μm, and even more preferably 5 μm to 30 μm.

[0045] A-3. Thickened Layer The thickened layer may be made of any suitable material as long as the effects of the present invention can be obtained. The thickened layer is, for example, a glass film or a polymer film, and is preferably a polymer film. Examples of polymer films constituting the thickened layer include films similar to the polymer film constituting the main body of the supporting substrate.

[0046] The haze of the thickened layer is preferably 20% or less, more preferably 10% or less, and even more preferably 0.1% to 10%.

[0047] The total light transmittance of the thickened layer is preferably 30% or more, more preferably 60% or more, and even more preferably 80% or more.

[0048] The thickness of the thickened layer may be, for example, 30 μm or more, preferably 40 μm or more, more preferably 50 μm or more, and may be, for example, 300 μm or less, preferably 250 μm or less.

[0049] B. Method for Producing Diffusion Film The diffusion film described in Section A can be produced by any suitable method. In one embodiment, the method for producing a diffusion film includes: applying a coating liquid containing a polymer matrix-forming resin, a liquid crystal compound, and a solvent to one support substrate to obtain a coating layer; drying the coating layer to obtain a PDLC layer containing a polymer matrix and dispersed particles containing the liquid crystal compound dispersed in the polymer matrix; and laminating the other support substrate on the PDLC layer to form a structural unit containing a pair of support substrates and a PDLC layer disposed therebetween; and laminating two or more of the structural units via an adhesive layer. According to this production method (also referred to as "production method A"), a diffusion film having two or more structural units containing a pair of support substrates and a diffusion layer (PDLC layer) disposed therebetween can be obtained.

[0050] In another embodiment, a method for producing a diffusion film includes: Step I: applying a coating liquid containing a polymer matrix-forming resin, a liquid crystal compound, and a solvent to a supporting substrate to obtain a coating layer; Step II: drying the coating layer to obtain a PDLC layer containing a polymer matrix and dispersed particles containing the liquid crystal compound dispersed in the polymer matrix; and Step III: laminating another supporting substrate on the PDLC layer, and repeating Steps I to III two or more times to produce a laminate in which two or more supporting substrates and two or more PDLC layers are alternately arranged. According to this production method (also referred to as "Production Method B"), a diffusion film having a laminate structure in which supporting substrates and diffusion layers (PDLC layers) are alternately arranged can be obtained.

[0051] In the above diffusion film manufacturing methods A and B, the coating liquid is preferably an emulsion coating liquid in which liquid crystal particles containing a liquid crystal compound are dispersed in a solvent. The solvent is preferably water or a mixed solvent of water and a water-miscible organic solvent. Examples of water-miscible organic solvents include C1-3 alcohol, acetone, and DMSO. The coating liquid may further contain optional components such as a polymerization initiator, a surfactant, a leveling agent, a crosslinking agent, and a dispersion stabilizer, depending on the purpose.

[0052] In the above-mentioned diffusion film manufacturing methods A and B, the diffusion layer is a PDLC layer (for example, the diffusion layer shown in FIG. 2( a)) containing a polymer matrix and dispersed particles containing a liquid crystal compound dispersed in the polymer matrix. However, by preparing a PDLC layer using a coating liquid containing a polymerizable liquid crystal compound as the liquid crystal compound and then polymerizing the polymerizable liquid crystal compound, a diffusion layer (for example, the diffusion layer shown in FIG. 2( b)) containing a polymer matrix and dispersed particles containing a liquid crystal polymer dispersed in the polymer matrix can be formed. In manufacturing method A, polymerization may be performed for each structural unit and then laminated, or polymerization may be performed collectively after laminating the structural units. In manufacturing method B, polymerization may be performed for each cycle of steps I to III, or polymerization may be performed on a laminate in which two or more support substrates and two or more PDLC layers are alternately arranged.

[0053] Furthermore, in the above-mentioned diffusion film manufacturing methods A and B, a PDLC layer is produced using a coating liquid containing a polymerizable liquid crystal compound as the liquid crystal compound, and then the polymerizable liquid crystal compound is polymerized while applying a voltage from the first principal surface side and the second principal surface side of the PDLC layer so as to generate regions with different electric field strengths, thereby forming a diffusion layer (for example, the diffusion layer shown in FIG. 2(c)) that contains a polymer matrix and dispersed particles containing a liquid crystal polymer dispersed in the polymer matrix and has regions with different hazes in plan view.

[0054] Explaining this in detail with reference to FIG. 3( a), a structural unit includes a pair of support substrates 20, 20′ and a PDLC layer 10 disposed therebetween. A first electrode 310 having a recessed surface is disposed on the outer side of one support substrate 20, and a flat-surfaced second electrode (e.g., an ITO-coated glass substrate) 320 is disposed on the outer side of the other support substrate 20′. By applying a voltage to these electrodes, regions of different electric field strengths can be generated in the PDLC layer 10. More specifically, the electric field strength is high in region B, where the distance between the electrodes is small, and the non-polymerizable liquid crystal compound 13a and the polymerizable liquid crystal compound 13b in this region can be aligned in the direction of the electric field. On the other hand, the electric field strength is low in region A, where the distance between the electrodes is large, and the non-polymerizable liquid crystal compound 13a and the polymerizable liquid crystal compound 13b in this region are in a non-aligned state. By irradiating the polymerizable liquid crystal compound 13b under such conditions with light, a liquid crystal polymer with a fixed non-aligned state is produced in region A, and a liquid crystal polymer 14 with a fixed substantially vertical alignment is produced in region B ( FIG. 3(b) ). Region A can exhibit a higher haze than region B. In the illustrated example, the polymerization treatment is performed on a single structural unit 30. However, the polymerization treatment may also be performed on a laminate of two or more structural units or a laminate in which a support substrate and a PDLC layer are alternately arranged. Furthermore, as shown in the illustrated example, the dispersed particles 16d contain not only the polymerizable liquid crystal compound 13b but also the non-polymerizable liquid crystal compound 13a, thereby expanding the temperature range of the liquid crystal phase (e.g., the nematic phase) and enabling more suitable alignment control. However, depending on the purpose, the dispersed particles may not contain the non-polymerizable liquid crystal compound.

[0055] In the above manufacturing method, a desired inter-electrode distance can be achieved in a desired pattern by providing the electrode surface with irregularities, steps, inclinations, or the like in any desired pattern. For example, the inter-electrode distance can be continuously changed by providing tapered convex portions on the electrode surface. Specifically, by changing the height and inclination angle of the tapered convex portions, the amount and rate of change of the inter-electrode distance can be controlled as desired, and as a result, the resulting diffusion layer can have a haze change with any desired gradient.

[0056] Furthermore, in the above-mentioned diffusion film manufacturing methods A and B, a PDLC layer is produced using a coating liquid containing a polymerizable liquid crystal compound and a non-polymerizable liquid crystal compound as liquid crystal compounds, and then, while a voltage is applied to the PDLC layer, active energy rays are irradiated to a predetermined region to polymerize the polymerizable liquid crystal compound, thereby forming a diffusion layer (for example, the diffusion layer shown in FIG. 2(d)) that contains a polymer matrix, dispersed particles that are dispersed in the polymer matrix and contain a non-polymerizable liquid crystal compound and a liquid crystal polymer, and dispersed particles that contain a non-polymerizable liquid crystal compound and a polymerizable liquid crystal compound, and has regions with different hazes in plan view.

[0057] Referring to FIG. 4( a), a first electrode 310 is disposed on the outer side of the first support substrate 20a, and a second electrode (e.g., an ITO-coated glass substrate) 320 is disposed on the outer side of the third support substrate 20c. Applying a voltage to these electrodes aligns the non-polymerizable liquid crystal compound 13a and the polymerizable liquid crystal compound 13b in the PDLC layer 10 in the direction of the electric field. By irradiating the polymerizable liquid crystal compound 13b with light through a photomask 330 in this state, a liquid crystal polymer 14 with a fixed, approximately vertical alignment is formed in region B (irradiated region), while the non-polymerizable liquid crystal compound 13a and the polymerizable liquid crystal compound 13b remain in a non-aligned state in region A (non-irradiated region) (FIG. 4( b)). Region A can exhibit a higher haze than region B. In the illustrated example, the polymerization treatment is performed on a laminate in which a support substrate and a PDLC layer are alternately arranged, but the polymerization treatment may also be performed on a laminate of two or more structural units, or the polymerization treatment may be performed on one structural unit and then laminated with another structural unit. Furthermore, as in the illustrated example, the dispersed particles 16 d contain the non-polymerizable liquid crystal compound 13 a in addition to the polymerizable liquid crystal compound 13 b, thereby widening the temperature range of the liquid crystal phase (e.g., nematic phase) and enabling more suitable alignment control. However, depending on the purpose, the dispersed particles may not contain the non-polymerizable liquid crystal compound.

[0058] In the above-mentioned diffusion film manufacturing methods A and B, a diffusion film further having a thickened layer can be obtained by laminating a thickened layer at a desired location.

[0059] C. Light Diffusion Device A light diffusion device according to an embodiment of the present invention includes the diffusion film described in Section A and a light source unit. FIG. 5 is a schematic cross-sectional view showing the configuration of a light diffusion device according to one embodiment of the present invention. The light diffusion device 200 includes a light source layer 110 and a diffusion film 100C disposed thereon. The diffusion film 100C is disposed so that the thickened layer 40 faces the light source layer 110, thereby increasing the distance between the diffusion layers 10a and 10b and the light source unit. The diffusion film 100C may be laminated to the light source layer 110 via an adhesive layer, or may be placed without an adhesive layer.

[0060] The light source layer 110 includes a light source section 112 and a sealing resin layer 114 that seals the light source section 112 .

[0061] The light source unit 112 is typically composed of a plurality of point light sources 112a. The plurality of point light sources are, for example, arranged two-dimensionally in a predetermined pattern. As the point light source, a light source that emits light with high directionality is preferable, and for example, an LED element can be used.

[0062] Examples of resins that can form the encapsulating resin layer 114 include thermosetting resins such as silicone resin, epoxy resin, polyester resin, urethane resin, and ethylene vinyl acetate; ultraviolet-curable resins such as acrylic resin, urethane resin, vinyl ester resin, and alkyd resin; and thermoplastic resins such as polyolefin, polystyrene, polyisobutylene, and isobutylene-based elastomers. Among these, silicone resin and epoxy resin are preferred, and silicone resin is more preferred, because they have high adhesion to resin films in general and can favorably achieve the effects of the present invention. The encapsulating resin layer may be formed using a single resin or a combination of two or more resins.

[0063] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring each property are as follows. Unless otherwise specified, "parts" and "%" in the examples and comparative examples are by weight.

[0064] (1) Thickness: Measured using a digital micrometer (manufactured by Anritsu Corporation, product name "KC-351C"). (2) Volume average particle diameter of liquid crystal particles in liquid crystal emulsion: The volume average particle diameter was calculated using a particle size distribution measuring device (manufactured by Microtrac, product name "MT3300EXII"). (3) Average particle diameter of resin particles: A measurement sample was prepared by adding a few drops of resin dispersion to 100 mL of water. Using a dynamic light scattering particle size distribution measuring device (manufactured by Microtrac, product name "Nanotrac150"), the measurement sample was placed in the measurement holder of the device, and measurements were performed after confirming on the device monitor that the concentration was measurable. (4) Haze: Measured using a product name "NDH4000" manufactured by Nippon Denshoku Co., Ltd., in accordance with JIS K 7136.

[0065] [Example 1] 1. Preparation of emulsion coating liquid 34.1 parts of a non-polymerizable liquid crystal compound (manufactured by JNC Corporation, product name "JC-5240XX", birefringence Δn = 0.252 (ne = 1.766, no = 1.514), viscosity = 75 mPa s), 3.8 parts of a polymerizable liquid crystal compound (manufactured by BASF Corporation, product name "PALIOCOLOR LC-242"), 0.1 parts of a photopolymerization initiator (manufactured by IGM, product name "OMNIRAD651"), 60.0 parts of pure water, and 2.0 parts of a dispersant (manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd., "Noigen ET159") were mixed and irradiated with ultrasonic waves at a frequency of 24 kHz for 1 minute using an ultrasonic homogenizer (manufactured by Hielscher Ultrasonics, UP-200S) to prepare a liquid crystal emulsion. The average particle size of the liquid crystal particles in the obtained liquid crystal emulsion was 0.8 μm. An emulsion coating solution was obtained by mixing 19.03 parts of the liquid crystal emulsion, 9.16 parts of a polyether-based polyurethane resin aqueous dispersion (manufactured by DSM, product name "NeoRez R967", polymer average particle size: 80 nm, solid content: 40 wt%), 8.12 parts of a polyester-based polyurethane resin aqueous dispersion (manufactured by Sanyo Chemical Industries, Ltd., product name "Eucoat C-102", polymer average particle size: 168 nm, solid content: 45 wt%), 0.38 parts of a leveling agent (manufactured by DIC Corporation, product name "F-444"), 1.23 parts of a crosslinking agent (tris[3-(2-methylaziridin-1-yl)propionic acid]=propylidinetrimethyl), and 62.0 parts of pure water.

[0066] 2. Formation of First PDLC Layer The emulsion coating liquid was applied to one side of a PET film (25 μm thick) serving as a first supporting substrate, forming a 150 μm thick coating layer using a wire bar. The coating layer was then dried at 25° C. for 90 minutes to form a 45 μm thick first PDLC layer. The resulting first PDLC layer exhibited a uniform haze (haze: 99%) across the entire main surface.

[0067] 3. Lamination of Second Supporting Substrate A PET film (thickness: 25 μm) was laminated as a second supporting substrate on the first PDLC layer while applying a lamination pressure of 0.4 MPa / m using a laminator.

[0068] 4. Formation of Second PDLC Layer The same emulsion coating liquid as in 1 above was applied to the surface of the second supporting substrate to form a coating layer with a thickness of 150 μm using a wire bar. The coating layer was then dried at 25° C. for 90 minutes to form a second PDLC layer with a thickness of 45 μm. The resulting second PDLC layer exhibited a uniform haze across the entire main surface.

[0069] 5. Lamination of Third Support Substrate A PET film (thickness: 25 μm) was laminated as a third support substrate on the second PDLC layer using a laminator at a lamination pressure of 0.4 MPa / m, thereby obtaining a laminate having a structure of [first support substrate / first PDLC layer / second support substrate / second PDLC layer / third support substrate].

[0070] 6. UV Irradiation A flat metal electrode was placed on the first support substrate side of the laminate, and an ITO-coated glass electrode was placed on the third support substrate side. While applying a voltage of 7 kV to 8 kV to these electrodes, UV irradiation was performed from the third support substrate side through a photomask (φ1.5) having a predetermined pattern. Specifically, UV irradiation was performed using a UV-LED lamp (manufactured by Hamamatsu Photonics, product name "C11924-101", peak wavelength 365 nm) at 20 mW / cm. 2The film was then exposed to light at 25°C for 3 minutes. This polymerized the polymerizable liquid crystal compound in the irradiated region, resulting in a diffusion film 1 having a structure of [first supporting substrate / first patterned diffusion layer / second supporting substrate / second patterned diffusion layer / third supporting substrate]. In the resulting diffusion film 1, the non-irradiated region exhibited a higher haze than the irradiated region. Furthermore, the non-irradiated region (high haze region) was arranged in a pattern corresponding to the arrangement pattern of point light sources in light source layer A, which will be described later.

[0071] Example 2: A laminate having a configuration of [first supporting substrate / first PDLC layer / second supporting substrate / second PDLC layer / third supporting substrate] was obtained in the same manner as in steps 1 to 5 of Example 1. The same emulsion coating liquid as in step 1 of Example 1 was applied to the surface of the third supporting substrate to form a 150 μm-thick coating layer using a wire bar. The coating layer was then dried at 25°C for 90 minutes to form a 45 μm-thick third PDLC layer. The resulting third PDLC layer exhibited uniform haze across the entire main surface. A PET film (25 μm thick) was laminated onto the third PDLC layer as a fourth supporting substrate using a laminator while applying a lamination pressure of 0.4 MPa / m. This resulted in a laminate having a structure of [first supporting substrate / first PDLC layer / second supporting substrate / second PDLC layer / third supporting substrate / third PDLC layer / fourth supporting substrate]. The laminate was then irradiated with UV light through a photomask in the same manner as in Example 1, step 6. This polymerized the polymerizable liquid crystal compound in the irradiated region, resulting in a diffusion film 2 having a structure of [first supporting substrate / first patterned diffusion layer / second supporting substrate / second patterned diffusion layer / third supporting substrate / third patterned diffusion layer / fourth supporting substrate]. In the resulting diffusion film 2, the non-irradiated region exhibited a higher haze than the irradiated region.

[0072] [Example 3] A PET film (thickness 100 μm) was attached as a thickened layer to the first support substrate side of the diffusion film 1 produced in Example 1 via a transparent adhesive layer (thickness 25 μm), thereby obtaining a diffusion film 3 having a structure of [thickened layer / first support substrate / first patterned diffusion layer / second support substrate / second patterned diffusion layer / third support substrate].

[0073] Example 4 Two laminates (structural units) having a structure of [first supporting substrate / first PDLC layer / second supporting substrate] were prepared in the same manner as in Examples 1-3. The two laminates were separately irradiated with UV light through a photomask in the same manner as in Example 1-6, thereby polymerizing the polymerizable liquid crystal compound in the irradiated regions. The laminates were bonded to both sides of a PET film (thickness 50 μm) as a thickened layer via a transparent adhesive layer (thickness 25 μm) with the patterns aligned so that the irradiated regions and non-irradiated regions overlapped, thereby obtaining a diffusion film 4 having a structure of [first supporting substrate / first patterned diffusion layer / second supporting substrate / thickened layer / third supporting substrate / second patterned diffusion layer / fourth supporting substrate].

[0074] [Comparative Example 1] A laminate having a structure of [first supporting substrate / first PDLC layer / second supporting substrate] was prepared in the same manner as in steps 1 to 3 of Example 1. The laminate was then irradiated with UV light through a photomask in the same manner as in step 6 of Example 1. This polymerized the polymerizable liquid crystal compound in the irradiated area, resulting in a diffusion film 1c having a structure of [first supporting substrate / first patterned diffusion layer / second supporting substrate].

[0075] A light source layer including a light source unit and a silicone resin layer (thickness 150 μm) sealing the light source unit was removed from a liquid crystal display device (Apple iPad Pro (registered trademark) 12.9 inches (5th generation)) and used as light source layer A. The light source unit was composed of mini-LEDs arranged two-dimensionally in 119 rows and 88 columns. The diffusion films obtained in the Examples and Comparative Examples were laminated on light source layer A without an adhesive layer, thereby obtaining a light diffusion device. In the obtained light diffusion device, the non-irradiated areas (high haze areas) of the diffusion film corresponded to the positions of the LEDs in a planar view. The light diffusion device was turned on, and the in-plane luminance uniformity was evaluated as follows. The results are shown in Table 1, along with the configuration of the light diffusion device. Note that the "total thickness" in the table refers to the total thickness of the diffusion film. <In-plane luminance uniformity> The luminance of the diffusion film side surface of the light diffusion device was measured with a 2D spectroradiometer (SR-5000HS, manufactured by Topcon Technohouse) at a resolution of 0.2 mm x 0.2 mm, and the in-plane luminance uniformity was calculated by substituting the maximum luminance (Lmax) and minimum luminance (Lmin) into the following formula. The in-plane luminance uniformity for the light source layer alone was 30.6%. In-plane luminance uniformity (%) = [1 - (Lmax - Lmin) / (Lmax + Lmin)] x 100

[0076]

[0077] The diffusion film of the example having two or more diffusion layers was able to significantly improve the in-plane luminance uniformity compared to the diffusion film of the comparative example having only one diffusion layer, and this effect was further enhanced when there were a large number of diffusion layers and when a thickened layer was provided.

[0078] The light diffusing device of the present invention is suitably used in display devices such as liquid crystal display devices.

[0079] REFERENCE SIGNS LIST 10 Diffusion layer (PDLC layer) 12 Polymer matrix 16 Dispersed particles 20 Support substrate 30 Structural unit 40 Thickened layer 100 Diffusion film 110 Light source layer 112 Light source section 200 Light diffusion device

Claims

1. A diffusion film having two or more diffusion layers each including a polymer matrix and dispersed particles, dispersed in the polymer matrix, the dispersed particles including at least one type selected from a liquid crystal compound and a liquid crystal polymer.

2. The diffusion film according to claim 1, wherein the total thickness of the diffusion layer is 50 μm or more.

3. The diffusion film according to claim 1, which has two or more structural units each including a pair of supporting substrates and the diffusion layer disposed therebetween.

4. The diffusion film according to claim 1, which has a laminated structure in which supporting substrates and the diffusion layers are alternately arranged.

5. The diffusion film of claim 1, further comprising a thickening layer.

6. The diffusion film according to claim 1, wherein at least one of the diffusion layers has regions with different hazes when viewed in a plan view.

7. The diffusion film according to claim 6, wherein the regions of different haze are arranged in a predetermined pattern.

8. The diffusion film according to claim 6, wherein the difference between the maximum and minimum haze values ​​is 10% or more.

9. A light diffusion device comprising the diffusion film according to any one of claims 1 to 8 and a light source unit.

10. The light diffusing device according to claim 9, wherein the light source section includes a plurality of point light sources.

11. A method for producing a diffusion film, comprising: step I of applying a coating liquid containing a polymer matrix-forming resin, a liquid crystal compound, and a solvent to a supporting substrate to obtain a coating layer; step II of drying the coating layer to obtain a polymer-dispersed liquid crystal layer containing a polymer matrix and dispersed particles containing the liquid crystal compound dispersed in the polymer matrix; and step III of laminating another supporting substrate on the polymer-dispersed liquid crystal layer, wherein steps I to III are repeated two or more times to produce a laminate in which two or more of the supporting substrates and two or more of the polymer-dispersed liquid crystal layers are alternately arranged.

12. The method for producing a diffusion film according to claim 11, wherein the liquid crystal compound comprises a polymerizable liquid crystal compound and a non-polymerizable liquid crystal compound, and the method comprises applying a voltage to the polymer dispersed liquid crystal layer contained in the laminate and irradiating a predetermined region with active energy rays to polymerize the polymerizable liquid crystal compound.

Citation Information

Patent Citations

  • Backlight

    JP1994095107A

  • Liquid crystal display device

    JP1996106105A

  • Light scattering film and liquid crystal display device using the same

    JP2002267812A

  • Liquid crystal display apparatus

    JP2007279224A

  • Light diffusion plate and backlight device using the same

    JP2011008005A