Boron nitride powder and method for producing boron nitride powder

The boron nitride powder with agglomerated particles, formed by mixing hexagonal boron nitride and an alkoxysilyl compound, addresses the anisotropy in thermal conductivity, enhancing heat dissipation in the thickness direction of resin sheets by reducing particle orientation and improving thermal conductivity.

WO2024203302A1PCT designated stage expired Publication Date: 2024-10-03DENKA CO LTD

Patent Information

Application Number
PCT/JP2024/009642
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-12
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Boron nitride powders used as fillers in heat dissipation materials exhibit anisotropy in thermal conductivity, limiting their effectiveness in the thickness direction of resin sheets, as primary particles tend to orient in specific directions, reducing the utilization of high in-plane thermal conductivity.

Method used

A boron nitride powder with agglomerated particles formed by mixing primary hexagonal boron nitride particles with a compound containing an alkoxysilyl group and heat-treating the mixture, resulting in particles with a larger average diameter and improved crushing strength, which reduces orientation and enhances thermal conductivity in the thickness direction.

Benefits of technology

The method produces a boron nitride powder that improves heat dissipation properties in the thickness direction of resin sheets by suppressing particle orientation and maintaining high thermal conductivity, leading to enhanced performance as a heat dissipation filler.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure 00000020_0000
    Figure 00000020_0000
  • Figure 00000021_0000
    Figure 00000021_0000
Patent Text Reader

Abstract

One aspect of the present disclosure provides a boron nitride powder which contains aggregated particles each containing a plurality of primary particles of hexagonal boron nitride, the boron nitride powder having an average particle diameter of 20 μm or more. With respect to this boron nitride powder, the atomic ratio of silicon atoms to boron atoms is 0.10 × 10-2 or more, and the atomic ratio of carbon atoms to boron atoms is 3.00 × 10-2 or more.
Need to check novelty before this filing date? Find Prior Art

Description

Boron nitride powder and method for producing the same

[0001] The present disclosure relates to boron nitride powder and methods for making the same.

[0002] Boron nitride powder has lubricity, high thermal conductivity, and insulating properties, and studies are being conducted to adjust the properties of boron nitride to suit various applications so that it can be used in a wide range of applications, such as as a solid lubricant, thermally conductive filler, insulating filler, etc. The use of boron nitride powder as a filler in heat dissipation components that require thermal conductivity is also being studied.

[0003] For example, primary particles of hexagonal boron nitride, which has excellent crystallinity, have a relatively thin, scale-like shape. Therefore, when filled into a resin or the like and molded, the primary particles tend to be oriented in a certain direction in the resin due to factors such as molding pressure. For example, in a resin sheet formed by filling hexagonal boron nitride powder into a resin and molding it into a sheet by extrusion molding or the like, the major surfaces of the resin sheet and the major axes of the boron nitride primary particles generally tend to be oriented parallel to each other. Furthermore, the anisotropy of the shape of the primary particles of hexagonal boron nitride can also lead to anisotropy in various physical properties. While the thermal conductivity of the primary particles of hexagonal boron nitride in the in-plane direction (a-axis direction) is high at approximately 400 W / (m·K), the thermal conductivity in the thickness direction (c-axis direction) is only approximately 2 W / (m·K), demonstrating significant anisotropy of the physical properties depending on the direction.

[0004] For the reasons mentioned above, methods have been investigated in which hexagonal boron nitride powder is used as a filler for resin, and when preparing a heat-dissipating sheet, the orientation direction is adjusted so that the a-axis direction of the primary particles is parallel to the thickness direction of the heat-dissipating sheet, thereby making use of the high thermal conductivity in the a-axis direction of the primary particles. For example, a technique is known in which the a-axis direction of the primary particles of hexagonal boron nitride is aligned parallel to the thickness direction of the heat-dissipating sheet (see, for example, Patent Document 1).

[0005] Furthermore, from the viewpoint of reducing the anisotropy due to the shape as described above, a method of forming an aggregate by aggregating and fusing a plurality of primary particles without orienting them has been studied. Patent Document 2 discloses spherical boron nitride aggregate particles formed by aggregating boron nitride primary particles, and describes that by increasing the strength of the aggregate particles to a level that can prevent the agglomerated particles from collapsing even when a predetermined molding pressure is applied, the boron nitride primary particles are prevented from being oriented in the same direction.

[0006] JP 2000-154265 A JP 2016-135731 A

[0007] The spherical boron nitride agglomerated particles described above are secondary particles formed by aggregating a plurality of the primary particles so that the a-axes of the primary particles are oriented in random directions, and therefore, while anisotropy can be reduced, the heat dissipation direction also becomes isotropic, meaning that the high thermal conductivity of the hexagonal boron nitride primary particles in the in-plane direction (the a-axis direction) cannot be fully utilized. When agglomerated particles formed by aggregating hexagonal boron nitride primary particles are used as a heat dissipation filler, there is still room for improvement in terms of improving the heat dissipation properties along the thickness direction of a resin sheet.

[0008] An object of the present disclosure is to provide a boron nitride powder that can be used to prepare a resin sheet that has excellent heat dissipation properties in the thickness direction, and a method for producing the same.

[0009] The present disclosure provides the following [1] to [8].

[0010] [1] A boron nitride powder containing agglomerated particles containing a plurality of primary particles of hexagonal boron nitride, wherein the average particle size is 20 μm or more, and the atomic ratio of silicon atoms to boron atoms is 0.10 × 10 -2 or more, and the atomic ratio of carbon atoms to boron atoms is 3.00 × 10 -2or more. [2] The powder according to [1], wherein the atomic ratio of nitrogen atoms to boron atoms is 1.00 or more. [3] The powder according to [1] or [2], wherein the atomic ratio of carbon atoms to silicon atoms is 20.0 or less. [4] The powder according to any one of [1] to [3], wherein the average particle size of the primary particles is 8 μm or more. [5] The powder according to any one of [1] to [4], wherein the crushing strength of the agglomerated particles is 0.1 to 2.0 MPa. [6] The powder according to any one of [1] to [5], wherein the average particle size of the boron nitride powder is 30 to 80 μm. [7] A method for producing a boron nitride powder, comprising mixing a raw material powder composed of primary particles of hexagonal boron nitride with a compound having an alkoxysilyl group, and heat-treating the mixture to form agglomerated particles containing a plurality of the primary particles. [8] The compound having an alkoxysilyl group is a compound represented by the general formula (1): (RO) 3 Si(CH 2 ) nM [in the general formula (1), R represents an alkyl group having 1 or more carbon atoms, M represents a functional group selected from an epoxy group, an amino group, and a hydroxysilyl group, and n is 10 or less].

[0011] One aspect of the present disclosure is a boron nitride powder comprising aggregated particles containing a plurality of primary particles of hexagonal boron nitride, the aggregated particles having an average particle size of 20 μm or more and an atomic ratio of silicon atoms to boron atoms of 1×10 -3 or more, and the atomic ratio of carbon atoms to boron atoms is 3×10 -3 As described above, a boron nitride powder is provided.

[0012] The boron nitride powder contains agglomerated particles containing multiple primary particles of hexagonal boron nitride. The inventors presume that the boron nitride powder contains silicon atoms and carbon atoms, and that the primary particles maintain their agglomerated particle form due to components containing these elements. Furthermore, the powder containing the agglomerated particles has a relatively large average particle size of 20 μm or more, which can suppress orientation within a resin when blended with the powder compared to powders composed primarily of primary particles. Such boron nitride powder can be used as a filler in a resin to produce a heat-dissipating sheet with superior thermal conductivity in the thickness direction.

[0013] One aspect of the present disclosure provides a method for producing boron nitride powder, comprising: mixing a raw material powder composed of primary particles of hexagonal boron nitride with a compound having an alkoxysilyl group, and heat-treating the mixture to form aggregated particles containing a plurality of the primary particles.

[0014] In the method for producing the boron nitride powder, primary particles of hexagonal boron nitride in a raw material powder are mixed with a compound having an alkoxysilyl group, followed by a heat treatment, which causes a reaction between the compound and agglomerates the primary particles to form aggregated particles, thereby providing the boron nitride powder described above.

[0015] According to the present disclosure, it is possible to provide a boron nitride powder that can be used to prepare a resin sheet that has excellent heat dissipation properties in the thickness direction, and a method for producing the same.

[0016] Fig. 1 is a scanning electron micrograph showing the powder prepared in Example 1. Fig. 2 is a scanning electron micrograph showing the powder prepared in Comparative Example 1.

[0017] Hereinafter, embodiments of the present disclosure will be described. However, the following embodiments are merely examples for explaining the present disclosure, and are not intended to limit the present disclosure to the following content. In this specification, a numerical range indicated by the symbol "to" includes a lower limit and an upper limit. In other words, a numerical range indicated by "x to y" means a range equal to or greater than x and equal to or less than y.

[0018] Unless otherwise specified, the materials exemplified in this specification can be used singly or in combination of two or more. When a plurality of substances corresponding to each component are present in the composition, the content of each component in the composition means the total amount of the plurality of substances present in the composition, unless otherwise specified.

[0019] One embodiment of the boron nitride powder comprises agglomerated particles containing a plurality of primary particles of hexagonal boron nitride. The boron nitride powder has an average particle size of 20 μm or more and an atomic ratio of silicon atoms to boron atoms of 0.10×10 -2 or more, and the atomic ratio of carbon atoms to boron atoms is 3.00 × 10 -2 That's all.

[0020] The boron nitride powder may be mainly composed of agglomerated particles, with a small proportion of primary particles present. The agglomerated particles may have a flat shape overall.

[0021] The primary particles of hexagonal boron nitride have a scale shape. The agglomerated particles are aggregates containing multiple primary particles and correspond to secondary particles. Aggregated particles according to the present disclosure do not include those in which only two or three primary particles are combined. The agglomerated particles may include five or more primary particles. At least some of the multiple primary particles are chemically or physically bonded to each other by components containing silicon and carbon as constituent atoms to form the agglomerated particles. The agglomerated particles may include primary particles bonded to each other with their main surfaces facing each other, and a large proportion of primary particles in this state may be present. In such cases, a large proportion of the primary particles constituting the agglomerated particles may have their major axis direction (a-axis direction) oriented along the major axis direction of the entire agglomerated particle.

[0022] The atomic ratio of silicon atoms to boron atoms (Si atom number / B atom number: Si / B value) corresponds to the proportion of silicon atoms present between primary particles of hexagonal boron nitride in the agglomerated particles. The lower limit of the Si / B value is, for example, 0.10 × 10 -2 That's it, 0.50 x 10 -2 That's it, 0.60 x 10-2 That's it, 0.70 x 10 -2 That's it, 0.80 x 10 -2 That's it, 0.90 x 10 -2 That's it, 1.00 x 10 -2 That's it, 1.10 x 10 -2 That's it, 1.20 x 10 -2 That's it, 1.30 x 10 -2 or more, or 1.50 x 10 -2 The lower limit of the Si / B value within the above range can appropriately improve the crushing strength of the agglomerated particles. The upper limit of the Si / B value can be, for example, 20.00 × 10 -2 Below, 15.00 x 10 -2 Below, 10.00 x 10 -2 Below, 8.00 x 10 -2 Below, 6.00 x 10 -2 Below, 5.00 x 10 -2 Below, 3.00 x 10 -2 or less, or 2.00 x 10 -2 When the upper limit of the Si / B value is within the above range, the proportion of hexagonal boron nitride constituting the agglomerated particles becomes larger, and the heat dissipation properties can be further improved when the boron nitride powder is used as a heat dissipation filler.

[0023] The lower limit of the atomic ratio of carbon atoms to boron atoms (number of C atoms / number of B atoms: C / B value) is, for example, 3.00 × 10 -2 That's it, 5.00 x 10 -2 That's it, 7.00 x 10 -2 That's it, 8.00 x 10 -2 That's it, 9.00 x 10 -2 That's it, 10.00 x 10 -2 That's it, 11.00 x 10 -2 That's it, 12.00 x 10 -2 That's it, 13.00 x 10 -2 That's it, 14.00 x 10 -2 or more, or 15.0 x 10 -2 When the lower limit of the C / B value is within the above range, the crushing strength of the agglomerated particles can be further improved. The upper limit of the C / B value is, for example, 40.00 × 10 -2 Below, 35.00 x 10 -2 Below, 30.00 x 10-2 Below, 20.00 x 10 -2 or less, or 15.00 x 10 -2 When the upper limit of the C / B value is within the above range, the affinity between the resin and the boron nitride powder can be further improved.

[0024] The lower limit of the atomic ratio of nitrogen atoms to boron atoms (number of N atoms / number of B atoms: N / B value) may be, for example, 1.00 or more, or 1.01 or more. When the lower limit of N / B is within the above range, the boron nitride powder has an appropriate number of amino-based reaction sites, thereby further improving its affinity with resins. The upper limit of the N / B value may be, for example, 1.10 or less, or 1.05 or less. When the upper limit of N / B is within the above range, coarsening of aggregated particles can be prevented, and the insulating properties can be further improved when the boron nitride powder is used as an insulating filler.

[0025] The upper limit of the atomic ratio of carbon atoms to silicon atoms (number of C atoms / number of Si atoms: C / Si value) may be, for example, 20.0 or less, 15.0 or less, or 12.0 or less. When the upper limit of the C / Si value is within the above range, coarsening of the agglomerated particles can be prevented, and the insulating properties can be further improved when the boron nitride powder is used as an insulating filler. The lower limit of the C / Si value may be, for example, 1.0 or more, 5.0 or more, 8.0 or more, or 10.0 or more. When the lower limit of the C / Si value is within the above range, the crushing strength of the agglomerated particles can be further improved.

[0026] In this specification, the number of atoms of elements excluding carbon refers to a value measured using an X-ray fluorescence (XRF) analyzer. As the X-ray fluorescence analyzer, for example, "Primus II" (product name) manufactured by Rigaku Corporation can be used.

[0027] The number of carbon atoms in this specification refers to a value measured using a carbon / sulfur simultaneous analyzer. As the carbon / sulfur simultaneous analyzer, for example, the "IR-412" (product name) manufactured by LECO Corporation can be used.

[0028] The agglomerated particles contained in the boron nitride powder are formed by agglomerating primary particles via a silicon-containing component, and are more likely to collapse when force is applied than agglomerated particles in which primary particles are agglomerated in a manner such that they are sintered together, and their crushing strength is relatively small.

[0029] The upper limit of the crushing strength of the agglomerated particles may be, for example, 2.0 MPa or less, or 1.5 MPa or less. When the upper limit of the crushing strength is within the above range, the agglomeration force of the agglomerated particles is not too strong, and when the boron nitride powder is used as a heat-dissipating filler, the agglomerated state can be appropriately deformed or disintegrated in the resin, thereby approaching close packing and further improving the heat dissipation properties of the resulting resin sheet. The lower limit of the crushing strength of the agglomerated particles may be, for example, 0.1 MPa or more, 0.3 MPa or more, or 0.5 MPa or more. When the lower limit of the crushing strength is within the above range, the agglomerated particles can be more sufficiently prevented from completely collapsing when added to a resin. The crushing strength of the agglomerated particles may be adjusted within the above range, for example, 0.1 to 2.0 MPa.

[0030] The crushing strength of an agglomerate in this specification refers to a value measured in accordance with the description in JIS R 1639-5:2007 "Fine ceramics - Determination of granule characteristics - Part 5: Single granule crushing strength." The crushing strength σ (unit: MPa) of a single agglomerate particle is calculated as follows: σ = α × P / (π × d) where α (α = 2.48), which varies depending on the position within the agglomerate, the crushing test force P (unit: N), and the particle diameter d (unit: μm). 2 ) is calculated using the formula. Measurements were performed on 20 or more agglomerated particles, and the value at the time when the cumulative destruction rate reached 63.2% was calculated. A micro-compression tester can be used for the measurement. For example, the "MCT-W500" (product name) manufactured by Shimadzu Corporation can be used as the micro-compression tester.

[0031] The boron nitride powder has an average particle size of 20 μm or more, but this may be adjusted depending on the thickness of the resin sheet, etc. The lower limit of the average particle size of the boron nitride powder may be, for example, 30 μm or more, 35 μm or more, 38 μm or more, 40 μm or more, 45 μm or more, 48 μm or more, or 50 μm or more. When the lower limit of the average particle size is within the above range, the heat dissipation properties can be further improved when the boron nitride powder is used as a heat dissipation filler. The upper limit of the average particle size of the boron nitride powder may be, for example, 100 μm or less, 90 μm or less, 80 μm or less, 70 μm or less, or 60 μm or less. When the upper limit of the average particle size is within the above range, the unevenness of the resin sheet surface can be further reduced when the resin sheet is prepared. The average particle size of the boron nitride powder may be adjusted within the above range, and may be, for example, 20 to 100 μm, 30 to 100 μm, 30 to 80 μm, or 30 to 60 μm.

[0032] In this specification, the average particle size of boron nitride powder refers to the 50% cumulative diameter (median diameter) in the volume-based cumulative particle size distribution. More specifically, it refers to the particle size (D50) when the cumulative value reaches 50% in the volume-based cumulative particle size distribution obtained by laser diffraction scattering for the powder. The laser diffraction scattering method is measured in accordance with the method described in JIS Z 8825:2013 "Particle Size Analysis - Laser Diffraction and Scattering Method." For the measurement, a laser diffraction scattering particle size distribution analyzer or the like can be used. For example, the "LS-13 320" (product name) manufactured by Beckman Coulter, Inc. can be used as the laser diffraction scattering particle size distribution analyzer. Note that when measuring the average particle size of boron nitride powder, the measurement is performed without treating the powder to be measured with a homogenizer or the like.

[0033] In the boron nitride powder, the average particle size of the primary particles of hexagonal boron nitride may be relatively large. The lower limit of the average particle size of the primary particles may be 8 μm or more, 10 μm or more, 12 μm or more, or 15 μm or more. By setting the lower limit of the average particle size within the above range, the interfacial resistance between the primary particles can be reduced, and the heat dissipation performance can be further improved when the boron nitride powder is used as a heat dissipation filler. The upper limit of the average particle size of the primary particles may be 30 μm or less, 28 μm or less, or 25 μm or less. By setting the upper limit of the average particle size within the above range, the surface roughness of the resin composition can be reduced when added to a resin. The average particle size of the primary particles of hexagonal boron nitride may be adjusted within the above range, for example, 8 to 30 μm or 12 to 25 μm.

[0034] In this specification, the average particle size of the primary particles of hexagonal boron nitride is measured by the same method as that for measuring the average particle size of boron nitride powder. However, the powder to be measured is treated with a homogenizer before measurement. Here, the homogenizer device that can be used is a "VC-505" (product name) manufactured by Ieda Trading Co., Ltd. The treatment with the homogenizer is performed, for example, at a frequency of 20 kHz for 2 minutes.

[0035] One embodiment of a method for producing boron nitride powder includes mixing a raw material powder composed of primary particles of hexagonal boron nitride with a compound having an alkoxysilyl group, and heat-treating the mixture to form aggregated particles containing a plurality of the primary particles.

[0036] The raw material powder is composed of primary particles of hexagonal boron nitride, and may be purchased or prepared by hand if available. The raw material powder may not contain a sintering aid for hexagonal boron nitride.

[0037] The raw material powder can be prepared, for example, by applying a method of firing a mixture of a boron compound such as boric acid and a nitrogen-containing compound such as melamine (particularly when boric acid and melamine are used, this method is also called, for example, a borate-melamine method).

[0038] An example of a method for preparing a raw material powder using the melamine borate method includes the steps of: calcining a raw material composition containing a boron-containing compound including boric acid and a nitrogen-containing compound including melamine in an atmosphere containing at least one of an inert gas and ammonia gas at 600 to 1300°C to obtain a calcined product containing at least one selected from the group consisting of low-crystalline boron nitride and amorphous boron nitride (calcination step); calcining a mixed powder containing the calcined product, boric acid, and an auxiliary agent in an atmosphere containing at least one of an inert gas and ammonia gas at a temperature of 1600°C or higher but lower than 2100°C to obtain a calcined product (calcination step); and pulverizing the calcined product to obtain a powder with adjusted particle size (pulverization step). The calcination step may be repeated multiple times (hereinafter referred to as the first calcination step, the second calcination step, etc.). When the calcination step is repeated multiple times, the calcined product obtained in each calcination step may be pulverized. By pulverizing the fired product, it is possible to sufficiently consume melamine and the like in the raw material composition in the second firing step and subsequent firing steps. The pulverization step may also include washing and drying the powder obtained by pulverization to obtain a dry powder.

[0039] The boron-containing compound is a compound having a boron atom as a constituent element. The boron-containing compound may further contain, in addition to boric acid, for example, boron oxide, borax, etc. The nitrogen-containing compound is a compound having a nitrogen atom as a constituent element and may be an organic compound. The nitrogen-containing compound may further contain, in addition to melamine, for example, dicyandiamide, urea, etc. The raw material composition may contain components other than the above compounds. For example, it may contain carbonates such as lithium carbonate, sodium carbonate, and calcium carbonate as a calcination aid. It may also contain a reducing substance such as carbon.

[0040] In the calcination step, the raw material composition is calcined, for example, using an electric furnace, to obtain a calcined product. The calcination step is performed in an atmosphere containing at least one of an inert gas and ammonia gas. Examples of the inert gas include nitrogen gas and a rare gas. Examples of the rare gas include helium gas and argon gas. The calcination step may be performed in a mixed gas atmosphere containing an inert gas and ammonia gas. The calcination temperature may be, for example, 600 to 1300°C, 800 to 1200°C, or 900 to 1100°C. The calcination time may be, for example, 0.5 to 5 hours, or 1 to 4 hours.

[0041] The calcined product obtained by calcination contains at least one selected from the group consisting of low-crystalline boron nitride and amorphous boron nitride, and may further contain hexagonal boron nitride. The calcination step allows the reaction of boron nitride to proceed at a lower temperature than the firing step described below. By lowering the calcination temperature, grain growth can be suppressed, and the average particle size of the raw material powder can be reduced. Furthermore, by lowering the calcination temperature, grain growth can be suppressed, and the specific surface area of ​​the raw material powder can be increased.

[0042] Next, in the firing step, the calcined product obtained as described above is blended with boric acid and an auxiliary agent and mixed to prepare a mixed powder, which is then fired. In the firing step, in the presence of boric acid and the auxiliary agent, the raw material composition is sufficiently consumed while the production and crystallization of boron nitride proceeds. This increases the crystallinity of the boron nitride contained in the calcined product, allowing hexagonal boron nitride to form. By adding additional boric acid in the firing step, melamine in the raw material composition, amorphous carbon and graphite produced by the reaction of the raw material composition, and the like are sufficiently reacted, reducing their content, thereby obtaining a high-purity raw material powder.

[0043] The content of boric acid in the mixed powder may be, for example, 1 to 30 parts by mass, 10 to 30 parts by mass, 10 to 20 parts by mass, or 1 to 15 parts by mass per 100 parts by mass of the calcined product. By setting the lower limit of the boric acid content within the above range, it is possible to more sufficiently reduce residual melamine and the like, and obtain a raw material powder with high purity. By setting the upper limit of the boric acid content within the above range, it is possible to obtain a raw material powder with a low amount of residual boric acid.

[0044] Examples of the auxiliary include borates such as sodium borate, and carbonates such as sodium carbonate, calcium carbonate, and lithium carbonate. The amount of the auxiliary blended relative to 100 parts by mass of the calcined product containing boron nitride may be 2 to 20 parts by mass, or may be 2 to 8 parts by mass.

[0045] In the firing step, the mixed powder is fired, for example, using an electric furnace or the like to obtain a fired product. The firing step is carried out in an atmosphere containing at least one of an inert gas and ammonia gas. Examples of the inert gas include nitrogen gas and rare gas. Examples of the rare gas include helium gas and argon gas. The firing step may be carried out in a mixed gas atmosphere containing an inert gas and ammonia gas.

[0046] The firing temperature is equal to or higher than 1600° C. and lower than 2100° C. The firing temperature may be 1800 to 2050° C., or may be 1900 to 2000° C. The firing time may be, for example, 0.5 to 5 hours, or may be 1 to 4 hours.

[0047] In this specification, the terms "firing time," "heating time," etc. refer to the time (retention time) during which the temperature of the environment surrounding the object is maintained at a predetermined temperature after the temperature reaches that temperature.

[0048] By maintaining a relatively high firing temperature, the consumption of the raw material composition, the consumption of amorphous carbon and graphite produced by the reaction of the raw material composition, and the production and crystallization of hexagonal boron nitride can be sufficiently promoted. By reducing the amount of carbon-containing raw materials such as melamine in the raw material composition, the quality of the obtained raw material powder can be further improved. A similar tendency is also observed by extending the firing time. On the other hand, if the firing temperature is too high, the crystal growth of hexagonal boron nitride tends to proceed too quickly, making fine pulverization difficult. A similar tendency is also observed when the firing time is too long.

[0049] The fired product obtained in the firing step may be pulverized using, for example, a pulverizer. Examples of pulverizers that may be used include impact pulverizers (pulverizers). Impact pulverizers that can adjust the particle size of the pulverized product using a screen, such as an impact screen-type fine pulverizer, can be suitably used. The openings of the screen may be, for example, 0.1 to 1 mm, or 1 to 3 mm.

[0050] In the pulverization step, the sintered product is pulverized to adjust the particle size. The pulverized powder obtained by pulverizing the sintered product may contain impurities other than hexagonal boron nitride. Therefore, a process (purification process) to reduce the impurities may be carried out. Examples of impurities include remaining raw materials and auxiliary agents, as well as water-soluble boron compounds. The purification process reduces the amount of such impurities, for example, by washing. After washing, the product is subjected to solid-liquid separation and drying to obtain a dry powder.

[0051] The average particle size of the primary particles of hexagonal boron nitride in the raw material powder may be relatively large. Note that, in the above-mentioned production method, the dissolution, recrystallization, and sintering of the primary particles of hexagonal boron nitride are suppressed, and therefore the average particle size of the primary particles in the raw material powder will be approximately the same as the average particle size of the primary particles in the boron nitride powder obtained by the above-mentioned production method.

[0052] The lower limit of the average particle size of the primary particles in the raw material powder may be 8 μm or more, 10 μm or more, 11 μm or more, 12 μm or more, or 15 μm or more. By setting the lower limit of the average particle size within the above range, the interfacial resistance between the primary particles can be reduced, and the heat dissipation properties can be further improved when the boron nitride powder is used as a heat dissipation filler. The upper limit of the average particle size of the primary particles may be 30 μm or less, 28 μm or less, 26 μm or less, or 25 μm or less. By setting the upper limit of the average particle size within the above range, the surface roughness of the resin composition can be reduced when added to a resin. The average particle size of the primary particles of hexagonal boron nitride may be adjusted within the above range, and may be, for example, 8 to 30 μm or 12 to 25 μm.

[0053] The compound having an alkoxysilyl group has a silicon atom and a carbon atom as constituent atoms. The compound having an alkoxysilyl group may include, for example, a compound represented by the following general formula (1): General formula (1): (RO) 3 Si(CH 2 ) nM [In the above general formula (1), R represents an alkyl group having 1 or more carbon atoms, M represents a functional group selected from an epoxy group, an amino group, and a hydroxysilyl group, and n is 10 or less]

[0054] In the general formula (1), R is an alkyl group having 1 or more carbon atoms, but may be, for example, an alkyl group having 1 to 3 carbon atoms, specifically at least one selected from the group consisting of a methyl group, an ethyl group, and a propyl group, and may be a methyl group or an ethyl group, or may be a methyl group. In the general formula (1), multiple R may be the same or different from each other, but may be the same from the viewpoint of ease of availability.

[0055] In the above general formula (1), M is a functional group selected from an epoxy group, an amino group, and a hydroxysilyl group, and the functional group can be selected from the viewpoint of improving affinity with the target resin when, for example, the boron nitride powder containing the agglomerated particles according to the present disclosure is filled into a resin for use. For example, when used by filling into an epoxy resin, M in the above general formula (1) preferably includes an epoxy group.

[0056] In the above general formula (1), n ​​may be 1 to 10, 2 to 8, or 3 to 7, and is preferably an integer in the range of 2 to 8 from the viewpoint of achieving superior agglomerated particle size and crushing strength in the boron nitride powder.

[0057] Specific examples of the compound having an alkoxysilyl group include 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, and 8-glycidoxyoctyltrimethoxysilane. The compound having an alkoxysilyl group preferably includes 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, and 8-glycidoxyoctyltrimethoxysilane.

[0058] In the above-described production method, the compound having an alkoxysilyl group to be mixed with the raw material powder does not necessarily have to be one type, and a plurality of compounds may be used in combination.

[0059] The lower limit of the heating temperature in the heat treatment in the above-described production method may be, for example, 130°C or higher, 150°C or higher, or 200°C or higher. By setting the lower limit of the heating temperature within the above range, the reaction of the compound having an alkoxysilyl group can be more sufficient, and the crushing strength of the aggregated particles can be further improved. The upper limit of the heating temperature in the heat treatment may be, for example, 300°C or lower, or 250°C or lower. By setting the upper limit of the heating temperature within the above range, decomposition of the compound having an alkoxysilyl group can be more sufficiently suppressed.

[0060] The lower limit of the heating time for the heat treatment in the above-described production method may be, for example, 0.5 hours or more, or 1 hour or more. By setting the lower limit of the heating time within the above range, the reaction of the compound having an alkoxysilyl group can be more sufficient, and the crushing strength of the aggregated particles can be further improved. The upper limit of the heating time for the heat treatment may be, for example, 10 hours or less, 8 hours or less, 6 hours or less, or 5 hours or less. By setting the upper limit of the heating time within the above range, the heat treatment can be completed in a shorter time, and further improvement in productivity can be expected.

[0061] Although several embodiments have been described above, the present disclosure is not limited to the above embodiments. Furthermore, the descriptions of the above embodiments can be applied to each other.

[0062] The present disclosure will be described in more detail below using examples and comparative examples, but the present disclosure is not limited to the following examples.

[0063] Example 1 Boron nitride powder (manufactured by Denka Co., Ltd., grade: SGP) having an average primary particle size of 15 μm was used as the raw material powder.

[0064] [Production of boron nitride powder] 10 parts by mass of the raw material powder prepared as described above and 0.5 parts by mass of 3-glycidoxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.) as a compound having an alkoxysilyl group were weighed into a container, mixed for 5 minutes using a mixer, heated at 130°C for 2 hours, crushed in a mortar, and sieved through a 150 μm mesh sieve to obtain boron nitride powder. An image of the obtained boron nitride powder observed with a scanning electron microscope is shown in Figure 1.

[0065] <Evaluation of properties of boron nitride powder> The boron nitride powder obtained as described above was evaluated for the average particle size of the powder, the atomic ratio of each component constituting the powder, and the crushing strength of the agglomerated particles according to the methods described below. The results are shown in Table 1.

[0066] [Measurement of average particle size of powder] The average particle size of the boron nitride powder was measured in accordance with the method described in JIS Z 8825:2013 "Particle size analysis - laser diffraction and scattering method." For the measurement, a laser diffraction and scattering particle size distribution analyzer (manufactured by Microtrac, product name "MT3300EXII") was used. Note that when measuring the average particle size of the boron nitride powder, the powder to be measured was not subjected to any treatment using a homogenizer or the like.

[0067] [Measurement of Composition of Constituent Elements in Powder] The composition of the constituent elements in the boron nitride powder was measured. The number of atoms of elements other than carbon in the boron nitride powder was measured using an X-ray fluorescence (XRF) analyzer (manufactured by Rigaku Corporation, product name "Primus II"). The number of carbon atoms in the boron nitride powder was measured using a carbon / sulfur simultaneous analyzer (manufactured by LECO Corporation, product name "IR-412 type").

[0068] [Measurement of Crushing Strength of Agglomerated Particles] The crushing strength of the agglomerated particles was measured in accordance with the description in JIS R 1639-5:2007 "Fine ceramics - Determination of granule characteristics - Part 5: Single granule crushing strength." For the measurement, a microcompression tester (manufactured by Shimadzu Corporation, product name "MCT-W500") was used. The measurement was performed on 20 or more agglomerated particles, and the value at the cumulative fracture rate of 63.2% was calculated.

[0069] <Evaluation of Boron Nitride Powder as Filler> The obtained boron nitride powder was used as a filler in a resin and its heat dissipation properties were evaluated.

[0070] [Preparation of Evaluation Sheet] A resin composition was obtained by mixing 6.75 parts by mass of a naphthalene-type epoxy resin (manufactured by Mitsubishi Chemical Corporation, product name: 806) and 0.52 parts by mass of an imidazole compound (manufactured by Mitsubishi Chemical Corporation, product name: 113) as a curing agent, with 10 parts by mass of boron nitride powder. The proportion of the boron nitride powder in the resin composition was 65% by volume. A Thinky Mixer (Thinky Corporation) was used to knead the resin. The kneading conditions were a reduced pressure of 100 Pa, 2000 rpm, and 5 minutes. The obtained resin composition was applied to a PET film to a thickness of 0.3 mm. It was then kneaded at a temperature of 150°C and 50 kgf / cm. 2 The resin sheet (evaluation sheet) was prepared by heating and pressing the resin sheet under relatively mild conditions for 30 minutes under the above conditions.

[0071] [Measurement of Thermal Conductivity] Thermal conductivity was measured by a steady-state method in accordance with ASTM D5470. A resin material thermal resistance measuring device (manufactured by Hitachi Technology and Services Co., Ltd., product name: TRM-046RHHT) was used for the measurement. The resin composition was processed to a width of 10 mm x 10 mm, and the thermal resistance value in the thickness direction was measured while applying a load of 2 N. The results are shown in Table 1.

[0072] (Examples 2 and 3) Boron nitride powders were prepared in the same manner as in Example 1, except that the components and blending amounts were adjusted as shown in Table 1. The obtained boron nitride powders were evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0073] Comparative Example 1 A boron nitride powder was prepared in the same manner as in Example 1, except that no compound having an alkoxysilyl group was used. The obtained boron nitride powder was evaluated in the same manner as in Example 1. The results are shown in Table 1. An image of the obtained boron nitride powder observed with a scanning electron microscope is shown in Figure 2.

[0074]

[0075] According to the present disclosure, it is possible to provide a boron nitride powder that can be used to prepare a resin sheet that has excellent heat dissipation properties in the thickness direction, and a method for producing the same.

Claims

1. A boron nitride powder containing agglomerated particles containing a plurality of primary particles of hexagonal boron nitride, having an average particle size of 20 μm or more, and an atomic ratio of silicon atoms to boron atoms of 0.10 × 10 -2 or more, and the atomic ratio of carbon atoms to boron atoms is 3.00 × 10 -2 That's all, boron nitride powder.

2. The powder according to claim 1, wherein the atomic ratio of nitrogen atoms to boron atoms is 1.00 or more.

3. The powder according to claim 1 or 2, wherein the atomic ratio of carbon atoms to silicon atoms is 20.0 or less.

4. The powder according to claim 1 or 2, wherein the average particle size of the primary particles is 15 μm or more.

5. The powder according to claim 1 or 2, wherein the crushing strength of the agglomerated particles is 0.1 to 2.0 MPa.

6. The powder according to claim 1 or 2, wherein the average particle size of the boron nitride powder is 30 to 80 μm.

7. A method for producing boron nitride powder, comprising mixing a raw material powder composed of primary particles of hexagonal boron nitride with a compound having an alkoxysilyl group, and heat-treating the mixture to form aggregated particles containing a plurality of the primary particles.

8. The compound having an alkoxysilyl group is represented by the general formula (1): (RO) 3 Si(CH 2 8. The method according to claim 7, wherein the general formula (1) is represented by: nM (wherein R represents an alkyl group having 1 or more carbon atoms, M represents a functional group selected from an epoxy group, an amino group, and a hydroxysilyl group, and n is 10 or less).

Citation Information

Patent Citations

  • Hexagonal boron nitride primary particle aggregate and application of the same

    JP2018104253A

  • Method for producing surface-coated hexagonal boron nitride particle and surface-coated hexagonal boron particle

    JP2022183821A

  • Boron nitride aggregated grain, method for producing same, and thermally conductive resin composition using same

    WO2018066277A1

  • Powder composed of organic-inorganic composite particles

    WO2019188444A1

  • Surface-modified boron nitride particles, method of producing surface-modified boron nitride particles, thermally conductive material-forming composition, thermally conductive material, thermally conductive sheet, and device having thermally conductive layer

    WO2022070718A1

Cited By

  • Hexagonal boron nitride filler, production method for hexagonal boron nitride filler, resin composition, and production method for resin composition

    WO2026141151A1