Ferritic stainless steel sheet
A ferritic stainless steel sheet with a tailored chemical composition and crystal structure addresses the challenges of in-plane anisotropy and ridging, enhancing deep drawability and formability while maintaining low yield strength.
Patent Information
- Application Number
- PCT/JP2024/009697
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-13
- Publication Date
- 2024-10-03
AI Technical Summary
Ferritic stainless steel sheets exhibit surface unevenness and ridging due to in-plane anisotropy, which complicates deep drawing and increases yield strength, making it difficult to achieve both high formability and ridging resistance.
A ferritic stainless steel sheet with a specific chemical composition (C: 0.001-0.030%, Si: 0.01-1.00%, Mn: 0.01-1.00%, Cr: 10.5-30.0%, N: 0.001-0.030%, P: 0.005-0.050%, Ti: 0.01-0.50%, and Nb: 0.01-0.50%) and controlled crystal grain size and orientation, reducing in-plane anisotropy and yield strength while maintaining ridging resistance.
The solution results in a ferritic stainless steel sheet with improved deep drawability, reduced in-plane anisotropy, and low yield strength, effectively addressing the issues of surface defects and formability.
Smart Images

Figure JP2024009697_03102024_PF_FP_ABST
Abstract
Description
Ferritic stainless steel plate
[0001] The present invention relates to a ferritic stainless steel sheet.
[0002] When a ferritic stainless steel sheet is deep-drawn, unevenness may occur on the surface of the formed product due to the in-plane anisotropy of the material structure. Furthermore, ridge-like undulations may occur on the surface of the formed product along the rolling direction of the ferritic stainless steel sheet, and such surface defects are generally called ridging.
[0003] Conventionally, techniques for improving the formability of ferritic stainless steel sheets have been investigated (see, for example, Patent Documents 1 to 5).
[0004] Japanese Patent No. 5505555 Japanese Patent No. 4083669 Japanese Patent No. 2772237 Japanese Patent Publication No. 8-311542 Japanese Patent Publication No. 1983-35369
[0005] When ferritic stainless steels have high yield strength, the forming load during forming increases and the shape and dimensional accuracy after forming can deteriorate (springback). Coarsening the grains is an effective way to reduce yield strength, but if a texture with a specific orientation develops during grain growth, in-plane anisotropy increases. Furthermore, reducing in-plane anisotropy tends to decrease the r-value and worsen ridging.
[0006] An object of one aspect of the present invention is to provide a ferritic stainless steel sheet having a high r-value, reduced in-plane anisotropy, and low yield strength and ridging resistance.
[0007] In order to solve the above-mentioned problems, a ferritic stainless steel sheet according to one embodiment of the present invention contains, by mass%, C: 0.001 to 0.030%, Si: 0.01 to 1.00%, Mn: 0.01 to 1.00%, Cr: 10.5 to 30.0%, N: 0.001 to 0.030%, and P: 0.005 to 0.050%, and also contains at least one of Ti: 0.01 to 0.50% and Nb: 0.01 to 0.50%, and the S content is 0.0100% or less. The ferritic stainless steel plate has a chemical composition of 15 μm to 40 μm in a cross section parallel to the rolling direction and perpendicular to the rolling surface, the grain size calculated by a cutting method is 15 μm to 40 μm in a cross section parallel to the rolling surface at the center of the plate thickness of the ferritic stainless steel plate, the {111}<110> crystal orientation intensity is Ia, the {111}<112> crystal orientation intensity is Ib, and the larger of Ia and Ib is I. 111 It is called I 111 ≧10.0 and 0.2≦(Ia / Ib)≦4.0.
[0008] According to one aspect of the present invention, it is possible to provide a ferritic stainless steel sheet having a high r-value, reduced in-plane anisotropy, and low yield strength and ridging resistance.
[0009] 1 is a schematic diagram showing a cross section of a stainless steel sheet according to an embodiment of the present invention; 2 is a schematic diagram showing a cross section of a stainless steel sheet according to an embodiment of the present invention; 3 is a flowchart showing an example of a method for producing a ferritic stainless steel sheet according to an embodiment of the present invention;
[0010] The following describes embodiments of the present invention. Note that the following description is intended to provide a better understanding of the gist of the invention, and does not limit the present invention unless otherwise specified. Furthermore, in this application, "A to B" indicates A or more and B or less.
[0011] In this specification, the term "ferritic stainless steel" is not limited to the specific form of steel strip, steel plate, etc., and is used to describe the properties of the material itself. Also, since a "steel plate" can be considered to be a part of a "steel strip," "ferritic stainless steel plate" includes a "ferritic stainless steel strip."
[0012] The ferritic stainless steel sheet according to one embodiment of the present invention has a chemical composition that allows it to remain in a ferrite single phase up to its melting point, and contains reduced carbon and nitrogen contents as well as carbide-stabilizing elements (Ti, Nb, etc.). Ferritic stainless steels having such a chemical composition are sometimes called high-purity ferritic stainless steels.
[0013] <Overview of the present invention> Generally, the formability (deep drawability) of a ferritic stainless steel sheet can be evaluated by the r-value (Lankford value, plastic working strain ratio). Typically, deep drawability can be evaluated by the average r-value obtained by averaging multiple r-values measured in multiple different in-plane directions based on the rolling direction. Furthermore, in-plane anisotropy can be evaluated by the in-plane anisotropy index Δr calculated from the multiple r-values.
[0014] Ferritic stainless steel sheets (high-purity ferritic stainless steel sheets) with a chemical composition that does not undergo austenite transformation upon heating have a texture in their metal structure and are prone to the presence of colony structures (hereinafter referred to as colonies). These colonies are formed by the aggregation of crystal grains with similar crystal orientations. The crystal orientation of a colony differs from the crystal orientation of the texture around the colony.
[0015] A process in which hot-rolled sheet annealing is omitted to reduce the in-plane anisotropy Δr is known, but in this case, colony separation is insufficient, resulting in worsening ridging. On the other hand, when hot-rolled sheet annealing is performed, ridging is improved by colony separation, but in-plane anisotropy increases because only certain orientations are preferentially developed. Therefore, it is not easy to improve ridging resistance while maintaining a small Δr.
[0016] The present inventors have conducted extensive research into techniques for reducing in-plane anisotropy while maintaining a high r-value, and for achieving low yield strength and anti-ridging properties, and have arrived at the present invention. A ferritic stainless steel sheet according to one aspect of the present invention is realized by a manufacturing process approach that differs from conventional approaches. The various properties and manufacturing method of the ferritic stainless steel sheet according to one aspect of the present invention will be described in detail below.
[0017] (Regarding Prior Art) In order to facilitate understanding of the method for producing a ferritic stainless steel sheet according to one embodiment of the present invention, the techniques described in Patent Documents 1 to 5 will be briefly described below.
[0018] Generally, the manufacturing process of stainless steel sheets includes, in this order, a steelmaking process, a hot rolling process, a hot-rolled sheet annealing process, intermediate processes such as cold rolling, and a final annealing process.
[0019] The technology described in Patent Document 1 improves formability by refining crystal grains, but does not consider the reduction in yield strength. The technologies described in Patent Documents 2 and 4 perform texture control in the hot rolling process and omit the hot-rolled sheet annealing process. Patent Document 2 describes increasing the concentration of both the {111}<112> orientation and the {111}<011> orientation to reduce in-plane anisotropy while maintaining a high r-value, but does not aim to achieve both low yield strength and ridging resistance. Patent Document 4 describes effectively controlling texture in the hot rolling process by significantly reducing the carbon content to 0.005% or less and the nitrogen content to 0.012% or less, thereby achieving ridging resistance and a high r-value while reducing in-plane anisotropy. However, the technologies described in Patent Documents 2 and 4 omit the hot-rolled sheet annealing process, which may worsen ridging. In the technology described in Patent Document 4, consideration is given to ridging resistance, but the improvement in ridging resistance may be limited, and further, reducing the carbon and nitrogen contents to a high degree leads to problems with production costs.
[0020] Patent Document 3 describes reducing in-plane anisotropy while maintaining ridging resistance and a high r-value by controlling the conditions of the hot rolling process. However, it does not aim to achieve both low yield strength and a low Δr value. Lowering the annealing temperature of a cold-rolled sheet results in finer grains, thereby increasing yield strength. On the other hand, increasing the annealing temperature of a cold-rolled sheet reduces yield strength while increasing Δr. Furthermore, the technology described in Patent Document 5 reduces the carbon and nitrogen content and further fixes carbon and nitrogen by adding Ti, improving the workability of ferritic stainless steel. However, the ridging resistance is unclear, and recrystallization may be suppressed by Ti-based precipitates. Therefore, there is a limit to increasing the r-value.
[0021] <Composition of Steel Sheet> First, the composition (chemical composition) of the ferritic stainless steel sheet according to one embodiment of the present invention will be described below. In the following description, the ferritic stainless steel sheet according to one embodiment of the present invention may be abbreviated as "the present stainless steel sheet."
[0022] The stainless steel plate may have a chemical composition containing, in mass%, C: 0.001 to 0.030%, Si: 0.01 to 1.00%, Mn: 0.01 to 1.00%, Cr: 10.5 to 30.0%, N: 0.001 to 0.030%, and P: 0.005 to 0.050%, as well as at least one of Ti: 0.01 to 0.50% and Nb: 0.01 to 0.50%, with an S content of 0.0100% or less.
[0023] The stainless steel sheet may have a chemical composition with the balance being iron (Fe) and unavoidable impurities. Each of the elements mentioned above will be explained below.
[0024] (C: Carbon) Carbon is an element that forms carbides with Cr and other elements, thereby generating interfaces that become sources of dislocations when ferritic stainless steel is deformed. However, excessive addition of carbon reduces intergranular corrosion resistance and workability, and increases the cost of refining. Therefore, the carbon content may be 0.001 to 0.030 mass%, 0.001 to 0.020 mass%, or 0.002 to 0.010 mass%.
[0025] (Si: Silicon) Si acts as a deoxidizer during the melting stage. However, if excessive Si is added, the ferritic stainless steel becomes hard and its ductility decreases. Therefore, the Si content may be 0.01 to 1.00 mass%, 0.02 to 0.70 mass%, or 0.03 to 0.30 mass%.
[0026] (Mn: Manganese) Mn has the effect of acting as a deoxidizer. However, if excessive Mn is added, the amount of MnS produced increases, reducing the corrosion resistance of the ferritic stainless steel. Therefore, the Mn content may be 0.01 to 1.00 mass%, 0.02 to 0.70 mass%, or 0.03 to 0.30 mass%.
[0027] (Cr: Chromium) Cr is necessary to form a passive film on the surface of the cold-rolled steel sheet and improve corrosion resistance. However, if excessive Cr is added, the ductility of the ferritic stainless steel decreases. Therefore, the Cr content may be 10.5 to 30.0 mass%, or 12.0 to 25.0 mass%.
[0028] (N: Nitrogen) N forms nitrides with Cr and other elements, thereby generating interfaces that serve as sources of dislocations when ferritic stainless steel is deformed. However, excessive addition of N reduces ductility due to solid solution strengthening. Therefore, the N content may be 0.001 to 0.030 mass%, or 0.005 to 0.025 mass%. Furthermore, in this stainless steel sheet, the C+N content, which is the sum of the C content and the N content, may be 0.050 mass% or less, or 0.045 mass% or less. If the C+N content is too high, the amount of carbonitride precipitation may be excessive. On the other hand, because excessive reduction of the C+N content increases refining costs, the C+N content may be 0.010 mass% or more, or 0.015 mass% or more. The C+N content, in mass %, may be in the range of 0.010≦C+N≦0.050, or may be in the range of 0.015≦C+N≦0.050.
[0029] (P: Phosphorus) Excessive P content can deteriorate weldability, weld toughness, and workability. Furthermore, P is related to precipitates in the material structure (described later). Therefore, the P content may be 0.005 to 0.050 mass%, 0.005 to 0.040 mass%, or 0.010 to 0.030 mass%.
[0030] (Ti and Nb: Titanium and Niobium) Ti and Nb bond with C or N and fix them as precipitates such as TiC, TiN, NbC, or NbN, so that purifying ferritic stainless steel can improve the average r-value and product elongation. On the other hand, excessive Ti and Nb content increases raw material costs and can reduce manufacturability due to an increase in recrystallization temperature.
[0031] Therefore, in one embodiment of the present invention, the Ti content may be 0.01 to 0.50 mass%, 0.02 to 0.40 mass%, or 0.10 to 0.30 mass%. The Nb content may be 0.01 to 0.50 mass%, 0.02 to 0.40 mass%, or 0.10 to 0.30 mass%. The ferritic stainless steel may contain only either Ti or Nb, or may contain both Ti and Nb.
[0032] (S: Sulfur) S is an impurity atom that adversely affects hot workability, corrosion resistance, and oxidation resistance. Therefore, the S content may be 0.0100 mass% or less. Ferritic stainless steels do not need to contain S, and there is no particular lower limit for the S content. The S content may be 0 (including no addition) to 0.0100 mass%. An S content of "0 (including no addition)" means that S is allowed to be contained as an unavoidable impurity.
[0033] (Other Components) The present stainless steel sheet may have a chemical composition further containing, in mass %, one or more elements selected from the group consisting of Mo, Ni, Co, Cu, Al, Ca, Mg, B, V, W, Sn, Sb, Zr, Y, Hf, and rare earth elements.
[0034] (Mo: Molybdenum) Mo is an element effective in improving corrosion resistance. However, if excessive Mo is added, the raw material cost of stainless steel increases. Therefore, when Mo is included in the chemical composition, the Mo content may be 0.05 to 2.00 mass%.
[0035] (Ni: Nickel) Ni is an element effective in improving corrosion resistance. On the other hand, excessive Ni content destabilizes the ferrite phase and increases the raw material cost of ferritic stainless steel. Therefore, when Ni is included in the chemical composition, the Ni content may be 0.01 to 1.00 mass%. The Ni content may be 0.01 to 0.10 mass%. In this stainless steel, the Ni content may be 0.40 mass% or less, 0.10 mass% or less, or 0 (including no addition) to 0.10 mass%. "No addition" means that Ni is not artificially added during steelmaking. A Ni content of "0 (including no addition)" allows the inclusion of Ni as an unavoidable impurity.
[0036] (Co: Cobalt) Cobalt is an element that is effective in improving corrosion resistance and heat resistance. However, if excessive Co is added, the raw material cost of ferritic stainless steel increases. Therefore, when Co is included in the chemical composition, the Co content may be 0.005 to 0.500 mass%.
[0037] (Cu: Copper) Cu is an element effective in improving corrosion resistance. Therefore, when Cu is included in the chemical composition, the Cu content may be 0.05 to 1.00% by mass.
[0038] (Al: Aluminum) Al is an element effective for deoxidation, but also has a negative effect on press workability. 2 It is possible to reduce system inclusions. However, if excessive Al is added, surface defects increase. Therefore, when Al is included in the chemical composition, the Al content may be 0.01 to 1.00 mass%.
[0039] (Ca: Calcium) Ca is an element effective for degassing. Therefore, when Ca is included in the chemical composition, the Ca content may be 0.0001 to 0.0050 mass %.
[0040] (Mg: Magnesium) Mg forms Mg oxide together with Al in molten steel and acts as a deoxidizer. On the other hand, excessive Mg content reduces the toughness of the ferritic stainless steel, resulting in poor manufacturability. Therefore, when Mg is included in the chemical composition, the Mg content may be 0.0001 to 0.0050 mass%.
[0041] (B: Boron) B is an element effective in improving toughness. However, if an excessive amount of B is contained, the effect is saturated. Therefore, when B is contained in the chemical composition, the content of B may be 0.0001 to 0.0025 mass%.
[0042] (V: Vanadium) V is an element effective in improving hardness and strength. However, if excessive V is added, the raw material cost of ferritic stainless steel increases. Therefore, when V is included in the chemical composition, the V content may be 0.05 to 0.50 mass%.
[0043] (W: Tungsten) W is an element effective in improving high-temperature strength. However, if excessive W is added, the raw material cost of ferritic stainless steel increases. Therefore, when W is included in the chemical composition, the W content may be 0.05 to 1.00 mass%.
[0044] (Sn: Tin) Sn is an element effective in improving corrosion resistance. However, if excessive Sn is added, hot workability and toughness decrease. Therefore, when Sn is included in the chemical composition, the Sn content may be 0.005 to 0.500 mass%.
[0045] (Sb: Antimony) Sb is effective in improving workability by promoting the formation of deformation bands during rolling. However, if an excessive amount of Sb is contained, the effect saturates and workability further deteriorates. Therefore, when Sb is contained in the chemical composition, the Sb content may be 0.005 to 0.500 mass%.
[0046] (Zr: Zirconium) Zr is an element effective for denitrification, deoxidation, and desulfurization. However, if Zr is added in excess, the raw material cost of stainless steel increases. Therefore, when Zr is included in the chemical composition, the Zr content may be 0.050 to 0.500 mass%.
[0047] (Y: Yttrium) Yttrium is an element effective in improving hot workability and oxidation resistance. However, these effects are saturated when the content exceeds 0.20%. When Y is included in the chemical composition, the Y content may be 0.001 to 0.100 mass%.
[0048] (Hf: Hafnium) Hf is an element that improves oxidation resistance. However, excessive Hf content reduces the toughness of the steel plate and increases the raw material cost of the stainless steel. Therefore, when Hf is included in the chemical composition, the Hf content may be 0.001 to 0.100 mass%.
[0049] (REM: Rare Earth Metals) Rare earth elements refer to lanthanoid elements (elements with atomic numbers 57 to 71, such as La, Ce, Pr, Nd, and Sm). REM is effective in improving hot workability and oxidation resistance. However, these effects saturate when the REM content exceeds 0.100%. Therefore, when REM is included in the chemical composition, the REM content may be 0.001 to 0.100 mass%.
[0050] <Steel Sheet Properties> The present stainless steel sheet has the chemical composition described above, and by controlling the manufacturing conditions, a material structure (internal structure) having the following properties is formed. Briefly, in the hot-rolled sheet annealing process, the colonies are broken up, the metal structure is recrystallized, and low-temperature precipitates are solid-dissolved. These low-temperature precipitates have the effect of suppressing grain growth (so-called "pinning" effect). Then, in the final annealing process, by raising the temperature to a temperature range where precipitates do not form, recrystallization nuclei of crystal grains with various crystal orientations are formed, which causes grain growth, thereby promoting randomization of crystal orientation. More details will be described later in conjunction with an explanation of the manufacturing method of the present stainless steel sheet.
[0051] (Grain size of steel sheet) Figure 1 is a schematic diagram showing a cross section 12 of a stainless steel sheet 1 according to one embodiment of the present invention. As shown in Figure 1, the cross section 12 is parallel to the rolling direction of the stainless steel sheet 1 and perpendicular to the rolled surface 11. The thickness and width of the stainless steel sheet 1 are denoted by t and w, respectively.
[0052] The stainless steel plate 1 has a crystal grain size (average grain size d described below) calculated by a cutting method in a cross section 12 of 15 μm or more and 40 μm or less, preferably 18 μm or more and 35 μm or less.
[0053] The grain size calculated by the intercept method can be measured by the method specified in the JIS standard (JIS G 0551:2020). Specifically, first, a line segment with a total length L parallel to the rolling direction is drawn on the cross section 12, and the number n of grains crossed by this line segment is measured. Note that grains with the end of the line segment inside are counted as 1 / 2 grain. The average grain size d can be calculated by the formula d = L / n.
[0054] (Crystal orientation) Figure 2 is a schematic diagram showing a cross section 13 of a stainless steel sheet 1 according to one embodiment of the present invention. As shown in Figure 2, the cross section 13 is a cross section of the center of the sheet thickness parallel to the rolled surface 11 of the steel sheet 1. The rolling direction is abbreviated as RD (Rolling Direction), the normal direction to the rolled surface is abbreviated as ND (Normal Direction), and the direction perpendicular to the rolling is abbreviated as TD (Transverse Direction). The cross section 13 is a so-called ND plane.
[0055] Pole figure data can be obtained by performing XRD measurement on the cross section 13. From the obtained pole figure data, the grain orientation distribution function (ODF) can be analyzed to measure the intensity (crystal orientation intensity) for each crystal orientation. For example, pole figure data can be obtained by performing pole measurements using SmartLab manufactured by Rigaku. SmartLab Studio II can be used as ODF analysis software. Since known analysis methods can be used in this way, detailed explanations will be omitted, but a brief explanation is as follows.
[0056] Regarding the crystal orientation of a certain crystal grain, if the (hkl) plane is located parallel to the ND plane and the [uvw] direction is the rolling direction, the crystal orientation of the crystal grain is expressed as (hkl)[uvw]. The equivalent orientation group is expressed as {hkl}<uvw>.
[0057] ODF is a function of three variables (φ1, Φ, φ2) that uniquely specify the crystal orientation of a grain relative to the material coordinate axis system. φ1, Φ, and φ2 are Euler angles defined by Bunge's method. The material coordinate axis system defines the x, y, and z axes as RD, TD, and ND, respectively. φ1 is the counterclockwise rotation angle around the z axis, Φ is the counterclockwise rotation angle around the x' axis after the rotation of φ1, and φ2 is the counterclockwise rotation angle around the z' axis after the rotation of Φ.
[0058] In the cross section of Euler space at φ2=45°, the position at φ=55°, φ1=30° was set to the {111}<112> orientation, and the position at φ=55°, φ1=0° was set to the {111}<110> orientation.
[0059] XRD measurement was performed on the stainless steel plate 1 to obtain (200), (110), and (211) pole figures. ODF analysis was performed using the obtained pole figures. The {111}<110> crystal orientation intensity obtained by ODF analysis was designated as Ia, and the {111}<112> crystal orientation intensity obtained by ODF analysis was designated as Ib. The values of Ia and Ib can be obtained, for example, by outputting the contour data (ODF diagram) obtained using SmartLab Studio II as numerical values. The calculation method for ODF analysis can be the WIMV method by Matthies and Vinel, which does not use continuous functions in the analysis. The larger of Ia and Ib is designated as I. 111 For example, a SmartLab can be used as the X-ray diffraction instrument, and a Mo source can be used as the X-ray source. In this case, the pole figure data used in the ODF analysis is intensity normalized by correction processes such as background correction and randomization in the processing in SmartLab. This normalization process is performed under fixed conditions without individually setting the conditions by selecting a normalization checkbox displayed on the display of the user interface of the X-ray diffraction instrument. The above crystal orientation intensity can also be expressed as an orientation density or an X-ray random intensity ratio.
[0060] The stainless steel plate 1 is 111 is 10.0 or more, and the relationship 0.2≦(Ia / Ib)≦4.0 is satisfied.111 When Ia / Ib satisfies the above relational expression, the in-plane anisotropy can be reduced.
[0061] The stainless steel plate 1 is 111 may be 10.0 or more and 30.0 or less, or 15.0 or more and 30.0 or less, and may satisfy the relationship 1.0≦(Ia / Ib)≦3.8. 111 If Ia / Ib exceeds 30.0, it becomes difficult to satisfy the relationship 0.2≦(Ia / Ib)≦4.0. When a steel sheet is manufactured through the steps of hot rolling, hot-rolled sheet annealing, cold rolling, and final annealing (i.e., when intermediate annealing and additional cold rolling are not performed), Ia≧Ib often holds. Therefore, (Ia / Ib) may be 1 or more. (Ia / Ib) may be 3.8 or less, which can further reduce the in-plane anisotropy.
[0062] (Average r-value and Δr) The present stainless steel sheet can have an average r-value (average Lankford value) of 1.4 or more. The average r-value can be calculated by the following formula (1) using the r-value measured at a plastic strain of 14.4% according to the method specified in the JIS standard (JIS Z 2254:2021): Average r-value = (r L +2r D +r C ) / 4... (1).
[0063] In formula (1), r L , r D and r C are the r-values measured for JIS No. 13B test pieces taken from directions at 0° (parallel), 45°, and 90° to the rolling direction, respectively. The stainless steel sheet may have an average r-value of 1.4 or more and 2.1 or less, or 1.9 or more and 2.1 or less.
[0064] Furthermore, the stainless steel sheet of the present invention can have a Δr of -0.50 or more and 0.50 or less. The range of Δr is preferably 0 or more and 0.50 or less, and more preferably 0 or more and 0.48 or less. Δr can be calculated using the above r value according to the following formula (2): Δr=(r L -2rD +r C ) / 2... (2).
[0065] (Rigging Height) The present stainless steel sheet can have a ridging height of 15 μm or less. The ridging height is a value obtained by measuring the waviness height in the width direction (the direction perpendicular to the rolling direction of the stainless steel sheet) at the center of the rating interval for a test piece obtained by taking a JIS No. 5 tensile test piece perpendicular to the rolling direction and then subjecting the test piece to a 16% strain using the tensile test method specified in the JIS standard (JIS Z 2241:2011). The waviness height is the average height of the waviness curve elements measured by the surface texture measurement specified in JIS B 0601:2001, etc. The average height of the waviness curve elements measured in this manner is the waviness height (i.e., ridging height) of the present stainless steel sheet.
[0066] (Yield strength) The present stainless steel sheet can have a yield strength of 320 MPa or less. The yield strength is a value obtained by measuring the 0.2% yield strength of a JIS No. 13B test piece using the tensile test method specified in the JIS standard (JIS Z 2241:2011). The present stainless steel sheet may have a yield strength of 310 MPa or less, or 300 MPa or less.
[0067] <Method for manufacturing steel sheet> Figure 3 is a flowchart showing an example of a method for manufacturing a ferritic stainless steel sheet according to one embodiment of the present invention. As shown in Figure 3, this method for manufacturing a stainless steel sheet (hereinafter sometimes abbreviated as this manufacturing method) includes a hot rolling step, a hot-rolled sheet annealing step, an intermediate step, and a final annealing step, in this order.
[0068] The method for producing the slab to be subjected to the hot rolling process is not particularly limited, but may include, for example, a steelmaking process prior to the hot rolling process. In the steelmaking process, molten steel having a desired composition is poured into a mold and cooled to produce a slab of ferritic stainless steel. The slab is cut to a desired length and used in the hot rolling process. In addition, this production method may include a post-process after the final annealing process, as appropriate.
[0069] (Hot Rolling Process) The hot rolling process is a process of producing a hot-rolled sheet of a predetermined thickness by rolling (hot rolling) a slab at a high temperature. The hot rolling process can be performed using known equipment and methods. In this production method, typical production conditions for hot rolling processes can be adopted. For example, the heating temperature (rolling temperature) can be 1150 to 1250°C, and the total reduction can be 95 to 99%. The coiling temperature after hot rolling can be 200 to 500°C.
[0070] (Hot-rolled sheet annealing process) In the hot-rolled sheet annealing process, the hot-rolled sheet is heated to a temperature range of 900 to 1000°C and soaked. The soaking temperature in the hot-rolled sheet annealing process is preferably 910 to 980°C. The soaking time in the hot-rolled sheet annealing process is 20 to 120 seconds (seconds).
[0071] In the present manufacturing method, by carrying out the hot-rolled sheet annealing step as described above, it is possible to form precipitates into a solid solution in the ferritic stainless steel. In this specification, precipitates are distinguished into low-temperature precipitates and high-temperature precipitates.
[0072] Low-temperature precipitates are precipitates that precipitate in ferritic stainless steels in the temperature range of 600°C or higher and lower than 900°C. Examples of low-temperature precipitates include compounds containing Fe and at least one of Nb, Ti, and P. More specifically, examples of low-temperature precipitates include (i) phosphides, such as FeTiP, FeNbP, and Fe(Ti,Nb)P, and (ii) intermetallic compounds that form a phase known as a Laves phase, such as Fe 2 Examples include Nb.
[0073] Furthermore, precipitates of compounds having a melting point of 900° C. or higher are referred to as high-temperature precipitates. Examples of high-temperature precipitates include metal carbides (e.g., TiC and NbC) and metal nitrides (e.g., TiN and NbN).
[0074] In the hot-rolled sheet annealing process, low-temperature precipitates and high-temperature precipitates are dissolved in the ferritic stainless steel, and the hot-rolled structure that causes ridging is disrupted by recrystallization. Therefore, the lower limit of the heating temperature is set to 900°C, and the lower limit of the soaking time is set to 20 seconds. On the other hand, if the recrystallized structure of the hot-rolled sheet becomes coarse, ridging will worsen. Therefore, the upper limit of the heating temperature is set to 1000°C, and the upper limit of the soaking time is set to 120 seconds. This disrupts colonies in the metal structure.
[0075] The cooling rate after soaking in the hot-rolled sheet annealing process can be 5°C / s or more in the temperature range from the soaking temperature to 500°C. This makes it possible to suppress the precipitation of low-temperature precipitates during cooling. The cooling rate in the temperature range below 500°C is not particularly limited. The cooled semi-finished product is called a hot-rolled annealed sheet.
[0076] The annealing equipment used in the hot-rolled sheet annealing step is not particularly limited, and known equipment such as a continuous annealing furnace or a batch furnace can be used.
[0077] (Intermediate Step) After the hot-rolled sheet annealing step, at least one cold-rolling step is typically performed before the final annealing step. The hot-rolled annealed sheet may be subjected to a pickling step. The pickling step is a step of removing scale adhering to the surface of the hot-rolled annealed sheet using a pickling solution such as sulfuric acid, hydrochloric acid, or a mixture of nitric acid and hydrofluoric acid.
[0078] The cold rolling step is a step of cold rolling the hot-rolled annealed sheet (for example, at room temperature to 200°C) to obtain a cold-rolled sheet of a predetermined thickness. The rolling ratio in the cold rolling step is preferably 75% or more, since a higher rolling ratio is more effective in improving the average r-value and formability. The rolling ratio in the cold rolling step may be 90% or less.
[0079] The rolling equipment used in the cold rolling step is not particularly limited, and known equipment can be used.
[0080] In the intermediate step, cold rolling may be performed only once or may be performed two or more times. When cold rolling is performed two or more times, an intermediate annealing step may be performed between the cold rolling steps. The heating temperature in the intermediate annealing step may be, for example, 900 to 1000°C.
[0081] <Final annealing step> The final annealing step is a step in which the cold-rolled sheet is heated to a temperature range of 900 to 1000°C and then soaked for 0 to 120 seconds. The temperature rise rate in the final annealing step is 100°C / s or more. The temperature rise rate may be 100 to 2000°C / s, and preferably 100 to 1500°C / s.
[0082] In the final annealing step, the cold-rolled sheet is heated under the above conditions to prevent low-temperature precipitates from precipitating during the temperature rise, and to promote the growth rate of crystal grains while causing recrystallization in a random orientation. By setting the temperature rise rate to 100°C / s or more, the amount of low-temperature precipitates precipitated during the temperature rise process can be effectively reduced. Furthermore, if the temperature rise time is too short, the amount of heat required for recrystallization may be insufficient, so the temperature rise rate may be set to 2000°C / s or less, or may be set to 1500°C / s or less.
[0083] The temperature increase under the above conditions in the final annealing step suppresses the precipitation of low-temperature precipitates and promotes the growth of crystal grains in the metal structure. By dissolving the low-temperature precipitates in the hot-rolled sheet annealing step and then increasing the temperature under the above conditions in the final annealing step, it is possible to promote the growth of crystal grains with various crystal orientations.
[0084] The lower limit of the heating temperature (soaking temperature) in the final annealing step is 900°C, at which point no low-temperature precipitates are formed and recrystallization is completed. On the other hand, if grain growth becomes too large, in-plane anisotropy increases. Therefore, the upper limit of the heating temperature is set to 1000°C, and the upper limit of the soaking time is set to 120 seconds. The soaking temperature in the final annealing step is preferably 910 to 980°C, and the soaking time is preferably 5 to 100 seconds.
[0085] The final annealing step in this manufacturing method will be described in more detail below. First, for comparison, a case where annealing is performed at a typical heating rate will be described. When the temperature is increased at a typical heating rate, recrystallization occurs in the following order: {111} grains, {211} grains, {311} grains, and {100} grains. That is, during heating, recrystallization nuclei of {111} grains are formed at a temperature of, for example, about 800°C. Subsequently, recrystallization nuclei of grains in other orientations are formed with subsequent heating. As recrystallization by annealing progresses, crystal grains having a specific orientation (e.g., {111}<112> orientation) among the initially nucleated {111} grains grow preferentially. Therefore, when annealing at a typical heating rate, the anisotropy of the ferritic stainless steel sheet increases. In contrast, in the final annealing step in this manufacturing method, heating under the above conditions results in recrystallization nuclei of not only {111} grains but also other orientations at approximately the same timing. Therefore, it is possible to prevent preferential growth in only a specific direction.
[0086] The annealing equipment used in the final annealing step is not particularly limited, and known equipment such as a continuous annealing furnace or a batch furnace can be used.
[0087] After the final annealing step, a pickling step may be performed as needed. Also, if necessary, post-processing may be performed as needed, such as temper rolling and cutting into a desired shape.
[0088] [Summary] The ferritic stainless steel sheet according to aspect 1 of the present invention contains, by mass%, C: 0.001 to 0.030%, Si: 0.01 to 1.00%, Mn: 0.01 to 1.00%, Cr: 10.5 to 30.0%, N: 0.001 to 0.030%, and P: 0.005 to 0.050%, and also contains at least one of Ti: 0.01 to 0.50% and Nb: 0.01 to 0.50%, with an S content of 0.0100% or less, and the balance being Fe and unavoidable impurities. A ferritic stainless steel sheet having a pure chemical composition, wherein in a cross section of the ferritic stainless steel sheet parallel to the rolling direction and perpendicular to the rolling surface, the grain size calculated by a cutting method is 15 μm or more and 40 μm or less, and in a cross section parallel to the rolling surface at the center of the sheet thickness of the ferritic stainless steel sheet, the {111}<110> crystal orientation intensity is defined as Ia, the {111}<112> crystal orientation intensity is defined as Ib, and the larger of Ia and Ib is defined as I. 111 It is called I 111 ≧10.0 and 0.2≦(Ia / Ib)≦4.0.
[0089] The ferritic stainless steel sheet according to aspect 2 of the present invention is the same as that according to aspect 1, except that it has a yield strength of 320 MPa or less, an average r-value of 1.4 or more, and an in-plane anisotropy index Δr of the r-value of -0.50 or more and 0.50 or less. L +2r D +r C ) / 4, Δr=(r L -2r D +r C ) / 2, r L : Lankford value in the 0° direction relative to the rolling direction, r D : Lankford value in the direction of 45° to the rolling direction, r C : Lankford value in the direction at 90° to the rolling direction.
[0090] In Aspect 3 of the present invention, the ferritic stainless steel sheet of Aspect 1 or 2 is such that a ridging height, obtained by taking a JIS No. 5 tensile test piece from the ferritic stainless steel sheet perpendicular to the rolling direction, subjecting the JIS No. 5 tensile test piece to a 16% strain and measuring the waviness height in the width direction at the center of the rating line, is 15 μm or less.
[0091] A ferritic stainless steel sheet according to Aspect 4 of the present invention is the same as any one of Aspects 1 to 3, and contains, by mass%, Mo: 0.05 to 2.00%, Ni: 0.01 to 1.00%, Co: 0.005 to 0.500%, Cu: 0.05 to 1.00%, Al: 0.01 to 1.00%, Ca: 0.0001 to 0.0050%, Mg: 0.0001 to 0.0050%, B: 0.00 and further contains one or more elements selected from the group consisting of: 0.01 to 0.0025%, V: 0.05 to 0.50%, W: 0.05 to 1.00%, Sn: 0.005 to 0.500%, Sb: 0.005 to 0.500%, Zr: 0.050 to 0.500%, Y: 0.001 to 0.100%, Hf: 0.001 to 0.100%, and rare earth elements: 0.001 to 0.100%.
[0092] In a fifth aspect of the present invention, a method for producing a ferritic stainless steel sheet contains, by mass%, C: 0.001 to 0.030%, Si: 0.01 to 1.00%, Mn: 0.01 to 1.00%, Cr: 10.5 to 30.0%, N: 0.001 to 0.030%, and P: 0.005 to 0.050%, and also contains at least one of Ti: 0.01 to 0.50% and Nb: 0.01 to 0.50%, and the S content is 0.0 The method includes a hot-rolled sheet annealing step in which a hot-rolled sheet having a chemical composition in which the content of Cu is 1% or less, with the balance being Fe and unavoidable impurities, is heated to a temperature range of 900 to 1000°C and soaked for 20 to 120 seconds, and a final annealing step in which the hot-rolled annealed sheet obtained by cold-rolling the hot-rolled annealed sheet obtained by the hot-rolled sheet annealing step is heated to a temperature range of 900 to 1000°C at a heating rate of 100°C / s or more, and then cooled with or without soaking for 120 seconds or less.
[0093] [Additional Notes] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention.
[0094] An embodiment of the present invention will be described below. The method for manufacturing a ferritic stainless steel sheet described in this embodiment is merely an example.
[0095] (Production of Slabs) Steels having the chemical compositions shown in Table 1 below were vacuum melted to produce 30 kg slabs. In Table 1, steel types A to N have chemical compositions within the range of the present invention. Also in Table 1, steel types P, R, and S have chemical compositions outside the range of the present invention. Table 1 shows the composition of the elements contained in each steel type in mass %. The remainder other than the elements shown in Table 1 is Fe or unavoidable impurities. Also, the underlined parts in Table 1 indicate that the composition of the elements contained in each steel type according to the comparative example is outside the range of the present invention.
[0096]
[0097] The slab was heated at 1200° C. for 2 hours and then hot rolled to produce a hot rolled sheet having a thickness of 3 mm.
[0098] Next, a hot-rolled sheet annealing step and a final annealing step were carried out under the manufacturing conditions shown in Table 2, and steel sheets Nos. 1 to 38 with a sheet thickness of 0.6 mm were manufactured. In this example, cold rolling was carried out only once as an intermediate step. The cold rolling reduction ratio was 80%. Table 2 also shows the results of evaluating various physical properties for each steel sheet. Note that the underlines in Table 2 indicate that the manufacturing conditions and various physical properties of the steel sheet are outside the ranges of the present invention or outside the preferred ranges of the present invention. Grain size, crystal orientation strength (I 111 , Ia, Ib), yield strength, average r value, Δr, and ridging height were measured or calculated using the same methods as in the above-described embodiment. The diagonal lines in the description of the conditions for the hot-rolled sheet annealing process for Steel Sheet No. 3 indicate that the hot-rolled sheet annealing process was not performed (omitted).
[0099]
[0100] As shown in Table 2, all of the steel sheets of the examples of the present invention, which were manufactured by the manufacturing method of a ferritic stainless steel sheet according to one embodiment of the present invention, had the properties of grain size, crystal orientation strength, yield strength, average r-value, Δr, and ridging height.
[0101] In contrast, the steel sheets of the comparative examples did not satisfy the criteria for at least one of the above properties. Comparative steel sheet No. 3 had yield strength, average r-value, and Δr within the ranges of the present invention, but omission of the hot-rolled sheet annealing step resulted in insufficient colony separation, and therefore insufficient ridging resistance. Comparative steel sheet No. 6 also showed insufficient colony separation. Comparative steel sheet No. 8 had insufficient heating in the hot-rolled sheet annealing step, resulting in small grain size, increased yield strength, and insufficient ridging resistance. Comparative steel sheets Nos. 10 and 24 had coarse recrystallized structures, resulting in poor ridging resistance.
[0102] In comparative steel sheet No. 13, the heating rate in the final annealing step was outside the range of the present invention, and the in-plane anisotropy increased due to the precipitation of low-temperature precipitates and preferential grain growth in a specific direction (e.g., the {111}<112> orientation). In comparative steel sheets No. 16 and 28, the heating in the final annealing step was insufficient, resulting in small grain size and increased yield strength. On the other hand, in comparative steel sheets No. 19, 21, 30, and 33, the grain growth due to heating in the final annealing step was excessive, resulting in increased in-plane anisotropy.
[0103] 1 Stainless steel plate 11 Rolled surface 12 Cross section 13 Cross section
Claims
1. A ferritic stainless steel sheet containing, by mass%, C: 0.001-0.030%, Si: 0.01-1.00%, Mn: 0.01-1.00%, Cr: 10.5-30.0%, N: 0.001-0.030%, and P: 0.005-0.050%, as well as at least one of Ti: 0.01-0.50% and Nb: 0.01-0.50%, with an S content of 0.0100% or less and the balance being Fe and unavoidable impurities, wherein the crystal grain size calculated by a cutting method in a cross section parallel to the rolling direction and perpendicular to the rolling surface of the ferritic stainless steel sheet is 15 μm or more and 40 μm or less, In a cross section parallel to the rolling surface at the center of the thickness of the ferritic stainless steel plate, the {111}<110> crystal orientation intensity is defined as Ia, the {111}<112> crystal orientation intensity is defined as Ib, and the larger of Ia and Ib is defined as I 111 It is called I 111 ≧10.0 and 0.2≦(Ia / Ib)≦4.
0.
2. A ferritic stainless steel sheet according to claim 1, having a yield strength of 320 MPa or less, an average r-value of 1.4 or more, and an in-plane anisotropy index Δr of the r-value of -0.50 or more and 0.50 or less. (wherein, average r-value=(r L +2r D +r C ) / 4 Δr=(r L -2r D +r C ) / 2r L r: Lankford value in the direction of 0° to the rolling direction D r: Lankford value at 45° to the rolling direction C : Lankford value in the direction 90° to the rolling direction) 3. A ferritic stainless steel sheet according to claim 1 or 2, in which a JIS No. 5 tensile test piece is taken from the ferritic stainless steel sheet perpendicular to the rolling direction, and the JIS No. 5 tensile test piece is subjected to a 16% strain to measure the waviness height in the width direction at the center of the grade interval, and the ridging height obtained is 15 μm or less.
4. In mass%, Mo: 0.05 to 2.00%, Ni: 0.01 to 1.00%, Co: 0.005 to 0.500%, Cu: 0.05 to 1.00%, Al: 0.01 to 1.00%, C a: 0.0001 to 0.0050%, Mg: 0.0001 to 0.0050%, B: 0.0001 to 0.0025%, V: 0.05 to 0.50%, W: 0.05 to 1.00%, S The ferritic stainless steel sheet according to any one of claims 1 to 3, further comprising one or more selected from the group consisting of n: 0.005 to 0.500%, Sb: 0.005 to 0.500%, Zr: 0.050 to 0.500%, Y: 0.001 to 0.100%, Hf: 0.001 to 0.100% and rare earth elements: 0.001 to 0.100%.
Citation Information
Patent Citations
Ferritic stainless steel plate and method for producing the same
JP2018184660A
Ferritic stainless steel sheet, manufacturing method therefor, and ferritic stainless member
JP2019173149A
Ferritic stainless steel sheet and method for manufacturing the same
JP2022079072A
Ferritic stainless steel sheet and method of manufacturing the same
JP2023147504A
Ferrite-based stainless steel plate, steel pipe, and production method therefor
WO2016068139A1
Cited By
High-strength hoop and preparation method thereof
CN119506721A