Cover protector, method for manufacturing cover protector, and battery module

The integration of a cover protector with an adhesive layer and inorganic fiber sheet within a battery module enhances heat insulation and flame protection, addressing the inadequacies of existing materials in managing thermal runaway and fire risks in lithium-ion batteries.

WO2024203354A1PCT designated stage expired Publication Date: 2024-10-03IBIDEN CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/009870
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-02-09
Filing Date
2024-03-13
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Current heat insulating materials for lithium-ion secondary batteries, such as those described in Patent Document 1, fail to provide sufficient heat insulation and protection against thermal runaway, leading to potential damage and fire risks due to their inadequate heat insulation performance.

Method used

A cover protector comprising a heat insulating material with inorganic particles and an inorganic fiber sheet bonded by an adhesive layer containing organic material, where the adhesive layer has a unique island-like and mesh-like structure to enhance heat insulation and prevent damage from flying objects, is integrated into a battery module.

Benefits of technology

The cover protector significantly improves heat insulation and flame retardant performance, preventing damage from thermal runaway and flame spread, while maintaining adhesive strength and being cost-effective to manufacture.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024009870_03102024_PF_FP_ABST
    Figure JP2024009870_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided are a cover protector that can protect a heat insulating material from scattered objects and can further improve heat insulation performance, a method for manufacturing the cover protector, and a battery module. A cover protector (1) comprises: a heat insulating material (2) containing inorganic particles; an inorganic fiber sheet (3); and an adhesive layer (4) that joins the heat insulating material (2) and the inorganic fiber sheet (3), and contains an organic material. When viewed in the lamination direction of the heat insulating material (2) and the inorganic fiber sheet (3), the adhesive layer (4) has a plurality of island-shaped parts (5) and a mesh-shaped part (6) that connects the island-shaped parts (5) to each other.
Need to check novelty before this filing date? Find Prior Art

Description

Cover protector, manufacturing method thereof, and battery module

[0001] The present invention relates to a cover protector, a manufacturing method thereof, and a battery module including the cover protector.

[0002] In recent years, in order to protect the environment, lithium-ion secondary batteries have been used in electric vehicles, etc. However, because lithium-ion secondary batteries use an organic electrolyte, there is a risk of fire if they ignite during thermal runaway, causing damage to the battery pack.

[0003] As a countermeasure, for example, Patent Document 1 proposes a multilayer material for use as a thermal barrier in an electrical energy storage system, which includes at least one inorganic fabric layer bonded to a nonwoven fabric layer containing inorganic particles and inorganic fibers by an inorganic adhesive, the inorganic adhesive including at least 99% by weight of an inorganic component and 0.01% by weight or more but less than 1% by weight of an organic additive.

[0004] International Publication No. 2021 / 022130

[0005] However, with the recent increase in battery capacity, the number of stacks has also increased, and the amount of organic electrolyte has also increased, so there is a strong demand for safety measures in the event of thermal runaway in the battery. However, the multilayer material described in Patent Document 1 above does not provide sufficient heat insulation performance.

[0006] The present invention has been made in consideration of the above-mentioned problems, and aims to provide a cover protector and a manufacturing method thereof, as well as a battery module, that can protect insulation material from flying debris and further improve insulation performance.

[0007] The above object of the present invention is achieved by the following configuration [1] relating to the cover protector.

[0008] [1] A cover protector comprising: an insulating material containing inorganic particles; an inorganic fiber sheet; and an adhesive layer that bonds the insulating material and the inorganic fiber sheet and contains an organic material, wherein, when viewed in the stacking direction of the insulating material and the inorganic fiber sheet, the adhesive layer has a plurality of island-shaped portions and a mesh-shaped portion that connects the plurality of island-shaped portions to each other.

[0009] Further, preferred embodiments of the present invention relating to the cover protector relate to the following [2] to [8].

[0010] [2] The cover protector according to [1], characterized in that the organic material contained in the adhesive layer is at least one selected from synthetic rubber, polyolefin-based organic materials, polyamide-based organic materials, and polyurethane-based organic materials. [3] The cover protector according to [1] or [2], characterized in that the content of the organic material is 80 mass% or more with respect to the total mass of the adhesive layer. [4] The cover protector according to any one of [1] to [3], characterized in that the mesh portion has a plurality of linear elements, and the plurality of linear elements extend in multiple directions while partially intersecting with each other to form the mesh portion. [5] The cover protector according to any one of [1] to [4], characterized in that a void portion is formed between the inorganic fiber sheet and the insulating material. [6] The cover protector according to any one of [1] to [5], characterized in that the organic material constituting the adhesive layer penetrates into the inorganic fiber sheet in a region extending from the surface in contact with the adhesive layer to the interior. [7] The cover protector according to any one of [1] to [6], characterized in that the adhesive layer contains a portion of the inorganic particles contained in the heat insulating material. [8] The cover protector according to any one of [1] to [7], characterized in that the inorganic fiber sheet is made of at least one type of fiber selected from silica fiber, alumina fiber, glass fiber, and metal fiber processed into a sheet shape.

[0011] The above object of the present invention is also achieved by the following configuration [9] relating to a method for manufacturing a cover protector.

[0012] [9] A method for manufacturing a cover protector according to any one of [1] to [8], comprising: a placement step of placing an adhesive material constituting the adhesive layer between the heat insulating material and the inorganic fiber sheet; and a joining step of heating and pressurizing the area where the heat insulating material, the adhesive material, and the inorganic fiber sheet are stacked; wherein the placement step includes a step of placing a plurality of fibrous adhesive materials extending in a plurality of directions between the heat insulating material and the inorganic fiber sheet, and the adhesive material is placed so that the amount of the adhesive material placed in a plurality of first areas is greater than the amount of the adhesive material placed in other second areas; and wherein the joining step forms the island-shaped portion in the first area and the mesh-shaped portion in the second area.

[0013] Furthermore, preferred embodiments of the present invention relating to a method for manufacturing a cover protector relate to the following

[10] to

[12] .

[0014]

[10] The method for manufacturing a cover protector according to [9], characterized in that the first region is a region where the plurality of fibrous adhesive materials overlap each other.

[11] The method for manufacturing a cover protector according to [9], characterized in that the adhesive material is made of an organic material and a plurality of fibers extending in a plurality of directions processed into a sheet shape, and the fibers are arranged so that the density of the fibers in the first region is higher than the density of the fibers in the second region.

[12] The method for manufacturing a cover protector according to

[11] , characterized in that the first region is a region where the plurality of fibers overlap each other.

[0015] The above object of the present invention is also achieved by the following configuration

[13] relating to a battery module.

[0016]

[13] A battery module comprising: the cover protector according to any one of [1] to [8]; a storage battery; and a battery case that houses the cover protector and the storage battery.

[0017] A preferred embodiment of the present invention relating to a battery module relates to the following

[14] .

[0018]

[14] The battery module according to

[13] , characterized in that the battery case has a ceiling surface, side wall surfaces, and bottom wall surfaces therein, the heat insulating material is arranged to face at least one selected from the ceiling surface, the side wall surfaces, and the bottom wall surfaces, and the cover protector is attached inside the battery case.

[0019] The cover protector of the present invention is formed by bonding an inorganic fiber sheet and a thermal insulating material with an adhesive layer. Since the thermal insulating material contains at least one of inorganic fibers and infusible fibers, the cover protector has excellent thermal insulating and flame retardant properties. Furthermore, the inorganic fiber sheet can prevent flying debris from directly impacting the thermal insulating material. Furthermore, since the adhesive layer has a unique structure, the thermal insulating properties can be improved while maintaining adhesive properties.

[0020] Furthermore, the cover protector of the present invention can be manufactured simply by sandwiching an adhesive material containing an organic material between an inorganic fiber sheet and an insulating material, and then applying heat and pressure, and therefore can be easily manufactured at low manufacturing costs.

[0021] Furthermore, since the battery module of the present invention has the cover protector of the present invention installed in the battery case that houses the storage battery, it can suppress damage caused by flying debris during thermal runaway, and can more reliably prevent the spread of fire to the outside even if a flame occurs.

[0022] Fig. 1 is a schematic cross-sectional view showing a cover protector according to the present embodiment. Fig. 2 is a photograph showing an adhesive layer in the cover protector shown in Fig. 1 as viewed in the stacking direction. Fig. 3 is a photograph showing a cross-section of a portion of the cover protector shown in Fig. 1. Fig. 4 is a schematic view showing an example of a method for manufacturing a cover protector according to an embodiment of the present invention. Fig. 5 is a schematic cross-sectional view showing a battery module according to an embodiment of the present invention.

[0023] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. Note that the present invention is not limited to the embodiments described below, and can be implemented with any modifications within the scope of the gist of the present invention.

[0024] [Cover protector] Fig. 1 is a schematic cross-sectional view showing a cover protector according to this embodiment. Fig. 2 is a photograph showing an adhesive layer in the cover protector shown in Fig. 1 as viewed in the stacking direction, and Fig. 3 is a photograph showing a cross-section of a portion of the cover protector shown in Fig. 1. As shown in Fig. 1, the cover protector 1 has a heat insulating material 2 containing inorganic particles, an inorganic fiber sheet 3, and an adhesive layer 4 that bonds the heat insulating material 2 and the inorganic fiber sheet 3. The adhesive layer 4 contains an organic material.

[0025] As shown in Figure 2, when viewed in the lamination direction parallel to the lamination direction of the thermal insulating material 2 and the inorganic fiber sheet 3, the adhesive layer 4 has a plurality of island-shaped portions 5 and a mesh-shaped portion 6 that connects these island-shaped portions 5 to each other. More specifically, the mesh-shaped portion 6 has a plurality of linear bodies that extend in a plurality of different directions while partially intersecting with each other to form the mesh-shaped portion 6. The mesh-shaped portion 6 connects the plurality of island-shaped portions 5 to each other.

[0026] The linear elements constituting the mesh portion 6 are not limited to straight linear elements, but may be curved linear elements. Furthermore, the linear elements extend in multiple directions from the intersections where the linear elements intersect with each other, but the number of directions is not limited to four, and may be three, five, or more. The width of the linear elements does not need to be uniform, and the mesh portion 6 may include narrow linear elements 9a with a width of 100 μm or less, and wide linear elements 9b with a width at least twice that of the narrow linear elements 9a.

[0027] The island-shaped portions 5 have a shape that is wider than the width (length in the direction perpendicular to the longitudinal direction) of the linear body and spreads out in a plane. The width of the island-shaped portions 5 in the short direction is, for example, three times or more the width of the wide linear body. The island-shaped portions 5 are formed in a dispersed manner in the adhesive layer 4, but the spacing between adjacent island-shaped portions 5 does not need to be uniform, and some island-shaped portions 5 are close to each other, and some island-shaped portions 5 are far apart.

[0028] As described above, the multiple linear bodies extend in various directions, thereby forming voids 7 of various sizes in regions around the island-shaped portions 5 where no linear bodies are present. The shape of the voids 7 when viewed in the stacking direction is a flattened circle or a polygon. Many small-area voids 7 are formed in regions between close island-shaped portions 5, while large-area voids 7 are formed in regions between distant island-shaped portions 5. In this embodiment, the inorganic fiber sheet 3 is formed by alternately weaving weft threads 3a and warp threads 3b made of inorganic fibers.

[0029] 3, the adhesive layer 4 has a mesh portion 6, and therefore voids 7 are formed between the thermal insulation material 2 and the inorganic fiber sheet 3 in regions where the island portions 5 and mesh portion 6 are not present. In addition, inorganic particles 8 contained in the thermal insulation material 2 are shown as dots in the figure, and the adhesive layer 4 contains some of these inorganic particles 8. Furthermore, the organic material contained in the adhesive layer 4 penetrates into the inorganic fiber sheet 3 in a region extending from the surface in contact with the adhesive layer 4 to the interior.

[0030] The cover protector 1 according to this embodiment configured as described above has the insulating material 2 with heat insulating properties, and therefore can obtain excellent heat insulating and fire retardant effects. Furthermore, since the inorganic fiber sheet 3 is bonded to the insulating material 2, if an item is damaged around the cover protector 1 and scattered, the inorganic fiber sheet 3 can protect the insulating material 2. Therefore, damage to the insulating material 2 can be suppressed, and excellent heat insulating and fire retardant effects can be maintained.

[0031] Furthermore, in this embodiment, the adhesive layer 4 bonding the thermal insulating material 2 and the inorganic fiber sheet 3 has island-shaped portions 5, which have a planar shape, thereby enabling good bonding between the thermal insulating material 2 and the inorganic fiber sheet 3. Furthermore, because voids 7 are formed between the thermal insulating material 2 and the inorganic fiber sheet 3, the thermal insulating performance can be further improved compared to bonding the two with an adhesive applied in a flat manner to the entire surface of the thermal insulating material 2 or the inorganic fiber sheet 3. Furthermore, because the adhesive layer 4 has voids 7 of various sizes, when the cover protector 1 is not pressed in its thickness direction, the larger voids 7 contribute to improved thermal insulating properties. When the cover protector 1 is pressed in its thickness direction, the smaller voids 7 are supported by the surrounding linear bodies, suppressing volume reduction and maintaining thermal insulating performance.

[0032] Furthermore, in this embodiment, because the mesh portion 6 has the characteristic shape as described above, even when the cover protector 1 is pressed or bent, the mesh portion 6 flexes flexibly, thereby preventing the inorganic fiber sheet 3 from separating from the thermal insulation material 2. Furthermore, if the linear bodies have a wide width at the bases close to the island portions 5, the linear bodies can be prevented from breaking away from the island portions 5 when the cover protector 1 is pressed or bent. As a result, the adhesive layer 4 can follow changes in the shape of the cover protector 1, further preventing the inorganic fiber sheet 3 from separating from the thermal insulation material 2.

[0033] Furthermore, since the inorganic particles 8 contained in the insulating material 2 are contained in the adhesive layer 4 and the organic material contained in the adhesive layer 4 penetrates into the inorganic fiber sheet 3, the bonding strength between the insulating material 2 and the inorganic fiber sheet 3 can be further increased.

[0034] The materials of the heat insulating material 2, the inorganic fiber sheet 3, and the adhesive layer 4 that constitute the cover protector 1 according to this embodiment will be described in detail below.

[0035] [Insulating Material] The insulating material 2 used in the cover protector according to this embodiment is not particularly limited as long as it has an insulating effect. Thermal conductivity can be used as an index of insulating effect. In this embodiment, the thermal conductivity of the insulating material 2 is preferably less than 1 (W / m·K), more preferably less than 0.5 (W / m·K), and even more preferably less than 0.2 (W / m·K). Furthermore, the thermal conductivity of the insulating material 2 is more preferably less than 0.1 (W / m·K), more preferably less than 0.05 (W / m·K), and particularly preferably less than 0.02 (W / m·K). The thermal conductivity of the insulating material 2 can be measured in accordance with JIS R 2251, "Test Method for Thermal Conductivity of Refractories."

[0036] The heat insulating material 2 contains inorganic particles and, as other components, may contain at least one selected from inorganic fibers, organic fibers, and organic particles. Specific examples of each are shown below.

[0037] <Inorganic particles> As the inorganic particles, a single inorganic particle may be used, or two or more types of inorganic particles may be used in combination.As the type of inorganic particles, from the viewpoint of heat insulating effect, it is preferable to use particles made of at least one inorganic material selected from oxide particles, carbide particles, nitride particles and inorganic hydrate particles, and it is more preferable to use oxide particles.In addition, the shape is not particularly limited, but it is preferable to include at least one selected from nanoparticles, hollow particles and porous particles.Specifically, it is also possible to use inorganic balloons such as silica nanoparticles, metal oxide particles, microporous particles and hollow silica particles, particles made of thermally expandable inorganic materials, particles made of hydrous porous bodies, etc.

[0038] When the average secondary particle diameter of the inorganic particles is 0.01 μm or more, they are easily available and the increase in production costs can be suppressed. When the average secondary particle diameter is 200 μm or less, the desired heat insulating effect can be obtained. Therefore, the average secondary particle diameter of the inorganic particles is preferably 0.01 μm or more and 200 μm or less, and more preferably 0.05 μm or more and 100 μm or less.

[0039] In addition, when two or more inorganic particles with different heat insulating effects are used in combination, the heat generating body can be cooled in multiple stages, and the heat absorption effect can be exerted over a wider temperature range. Specifically, it is preferable to use a mixture of large-diameter particles and small-diameter particles. For example, when nanoparticles are used as one of the inorganic particles, it is preferable to include inorganic particles made of a metal oxide as the other inorganic particle. Hereinafter, the inorganic particles will be described in more detail, with the small-diameter inorganic particles being referred to as the first inorganic particles and the large-diameter inorganic particles being referred to as the second inorganic particles.

[0040] <First Inorganic Particles> (Oxide Particles) When oxide particles are used as the first inorganic particles, radiant heat transfer can be suppressed, particularly in high-temperature regions such as abnormal heat generation. As the oxide particles, at least one type of particle selected from silica, titania, zirconia, zircon, barium titanate, zinc oxide, and alumina can be used. That is, among the above oxide particles that can be used as inorganic particles, only one type may be used, or two or more types of oxide particles may be used. In particular, silica is a component with high heat insulating properties, and titania is a component with a higher refractive index than other metal oxides, and is highly effective in scattering light and blocking radiant heat in high-temperature regions of 500°C or higher. Therefore, it is most preferable to use silica and titania as the oxide particles.

[0041] Since oxide particles have a high refractive index and a strong effect of diffusely reflecting light, the particle size of the oxide particles may affect the effect of reflecting radiant heat. Therefore, by limiting the average primary particle size of the oxide particles to a predetermined range, even higher thermal insulation properties can be obtained.

[0042] (Average primary particle diameter of oxide particles: 0.001 μm or more and 50 μm or less) When the average primary particle diameter of the oxide particles is 0.001 μm or more, the oxide particles are sufficiently larger than the wavelength of light that contributes to heating and efficiently diffusely reflect light, thereby suppressing radiative heat transfer within the cover protector in high-temperature ranges of 500° C. or more and further improving heat insulation. On the other hand, when the average primary particle diameter of the oxide particles is 50 μm or less, the number and contact points between particles do not increase even when compressed, making it difficult to form paths for conductive heat transfer, thereby reducing the impact on heat insulation, particularly in normal temperature ranges where conductive heat transfer is dominant.

[0043] In the present invention, the average primary particle size can be determined by observing particles under a microscope, comparing with a standard scale, and taking the average of any 10 particles.

[0044] (Nanoparticles) In the present invention, nanoparticles refer to particles on the nanometer order that are spherical or nearly spherical and have an average primary particle diameter of less than 1 μm. Nanoparticles have a low density, which suppresses conductive heat transfer. When nanoparticles are used as the first inorganic particles, the fine voids are dispersed, resulting in excellent thermal insulation that suppresses convective heat transfer. Therefore, nanoparticles are preferred because they can suppress heat conduction between adjacent nanoparticles during normal battery operation at room temperature. Furthermore, when nanoparticles with a small average primary particle diameter are used as oxide particles, an increase in conductive heat transfer through the insulating material can be suppressed even when the insulating material is compressed due to expansion caused by thermal runaway in the battery cell, increasing its internal density. This is thought to be because nanoparticles are prone to forming fine voids between particles due to electrostatic repulsion, and their low bulk density allows the particles to be packed together to provide cushioning.

[0045] When nanoparticles are used as the first inorganic particles, there are no particular limitations on the material as long as they comply with the definition of nanoparticles. For example, silica nanoparticles are a material with high heat insulating properties, and the contact points between particles are small, so the amount of heat conducted by silica nanoparticles is smaller than when silica particles with a large particle diameter are used. Furthermore, commonly available silica nanoparticles have a bulk density of 0.1 (g / cm3 ), for example, even if a large compressive stress is applied to the heat insulating material, the size (area) and number of contact points between silica nanoparticles do not increase significantly, and heat insulating properties can be maintained. Therefore, it is preferable to use silica nanoparticles as the nanoparticles. Examples of silica nanoparticles include wet silica, dry silica, and aerogel, but silica nanoparticles that are particularly suitable for this embodiment will be described below.

[0046] (Average primary particle diameter of nanoparticles: 1 nm or more and 100 nm or less) Limiting the average primary particle diameter of nanoparticles to a predetermined range can achieve even higher thermal insulation. That is, when the average primary particle diameter of nanoparticles is 1 nm or more and 100 nm or less, convective heat transfer and conductive heat transfer within the thermal insulation material can be suppressed, particularly in the temperature range below 500°C, thereby further improving the thermal insulation. Furthermore, even when compressive stress is applied, the voids remaining between the nanoparticles and the contact points between many particles suppress conductive heat transfer, thereby maintaining the thermal insulation properties of the thermal insulation material. The average primary particle diameter of nanoparticles is more preferably 2 nm or more, and even more preferably 3 nm or more. On the other hand, the average primary particle diameter of nanoparticles is more preferably 50 nm or less, and even more preferably 10 nm or less.

[0047] (Inorganic hydrate particles) When inorganic hydrate particles receive heat from a heating element and reach a temperature above the thermal decomposition initiation temperature, they undergo thermal decomposition, releasing their own water of crystallization to lower the temperature of the heating element and its surroundings, thereby exhibiting the so-called "endothermic effect." After releasing the water of crystallization, they become porous, and exhibit heat insulating properties due to the countless air holes. Specific examples of inorganic hydrates include aluminum hydroxide (Al(OH) 3 ), magnesium hydroxide (Mg(OH) 2 ), calcium hydroxide (Ca(OH) 2 ), zinc hydroxide (Zn(OH) 2 ), iron hydroxide (Fe(OH) 2 ), manganese hydroxide (Mn(OH) 2 ), zirconium hydroxide (Zr(OH) 2 ), gallium hydroxide (Ga(OH)3 ) etc.

[0048] For example, aluminum hydroxide contains about 35% water of crystallization, and as shown in the following formula, it thermally decomposes, releasing the water of crystallization and exhibiting an endothermic effect. After releasing the water of crystallization, it becomes a porous alumina (Al 2 O 3 ) and functions as a heat insulating material. 2Al(OH) 3 →Al 2 O 3 +3H 2 O

[0049] In a battery cell that has experienced thermal runaway, the temperature rises sharply to over 200° C. and continues to rise to around 700° C. Therefore, the inorganic particles contained in the thermal insulating material 2 are preferably made of inorganic hydrates whose thermal decomposition temperature begins at 200° C. or higher.

[0050] The thermal decomposition starting temperatures of the inorganic hydrates listed above are approximately 200°C for aluminum hydroxide, approximately 330°C for magnesium hydroxide, approximately 580°C for calcium hydroxide, approximately 200°C for zinc hydroxide, approximately 350°C for iron hydroxide, approximately 300°C for manganese hydroxide, approximately 300°C for zirconium hydroxide, and approximately 300°C for gallium hydroxide. All of these temperatures roughly overlap with the temperature range in which a battery cell experiencing thermal runaway experiences a sudden rise in temperature, and can efficiently suppress the temperature rise, making these inorganic hydrates preferable.

[0051] (Average secondary particle diameter of inorganic hydrate particles: 0.01 μm or more and 200 μm or less) Furthermore, when inorganic hydrate particles are used as the first inorganic particles, if the average particle diameter is too large, it takes a certain amount of time for the first inorganic particles (inorganic hydrate) near the center of the thermal insulation material 2 to reach their thermal decomposition temperature, and therefore the first inorganic particles near the center of the thermal insulation material 2 may not be completely thermally decomposed. For this reason, the average secondary particle diameter of the inorganic hydrate particles is preferably 0.01 μm or more and 200 μm or less, and more preferably 0.05 μm or more and 100 μm or less.

[0052] (Particles Made of Thermally Expandable Inorganic Material) Examples of thermally expandable inorganic materials include vermiculite, bentonite, mica, and perlite.

[0053] (Particles Made of Hydrous Porous Material) Specific examples of hydrous porous materials include zeolite, kaolinite, montmorillonite, acid clay, diatomaceous earth, wet silica, dry silica, aerogel, mica, and vermiculite.

[0054] (Inorganic Balloons) The thermal insulating material 2 used in the present invention may contain inorganic balloons as the first inorganic particles. When inorganic balloons are contained, convective heat transfer or conductive heat transfer within the thermal insulating material 2 can be suppressed in a temperature range of less than 500°C, thereby further improving the thermal insulation properties of the thermal insulating material 2. As the inorganic balloons, at least one type selected from shirasu balloons, silica balloons, fly ash balloons, barite balloons, and glass balloons can be used.

[0055] (Content of inorganic balloons: 60 mass % or less based on the total mass of the heat insulating material) The content of inorganic balloons is preferably 60 mass % or less based on the total mass of the heat insulating material.

[0056] (Average Particle Diameter of Inorganic Balloons: 1 μm or More and 100 μm or Less) The average particle diameter of the inorganic balloons is preferably 1 μm or more and 100 μm or less.

[0057] <Second inorganic particles> When two types of inorganic particles are contained in the thermal insulating material 2, the second inorganic particles are not particularly limited as long as they are different from the first inorganic particles in terms of material, particle size, etc. Examples of the second inorganic particles that can be used include oxide particles, carbide particles, nitride particles, inorganic hydrate particles, silica nanoparticles, metal oxide particles, inorganic balloons such as microporous particles and hollow silica particles, particles made of a thermally expandable inorganic material, and particles made of a hydrous porous body, the details of which are as described above.

[0058] Nanoparticles have extremely low conductive heat transfer and can maintain excellent heat insulation even when compressive stress is applied to the heat insulating material. Metal oxide particles such as titania have a high effect of blocking radiant heat. Furthermore, when large-diameter inorganic particles and small-diameter inorganic particles are used, the small-diameter inorganic particles penetrate into the gaps between the large-diameter inorganic particles, resulting in a denser structure and improved heat insulating properties. Therefore, when nanoparticles are used as the first inorganic particles, it is preferable to further include metal oxide particles larger in diameter than the first inorganic particles as the second inorganic particles in the heat insulating material.

[0059] Examples of metal oxides include silicon oxide, titanium oxide, aluminum oxide, barium titanate, zinc oxide, zircon, zirconium oxide, etc. In particular, titanium oxide (titania) is a component with a higher refractive index than other metal oxides, and is highly effective in scattering light and blocking radiant heat in a high temperature range of 500°C or higher, so titania is most preferably used.

[0060] When at least one type of particle selected from silica nanoparticles and silica aerogel is used as the first inorganic particles, and at least one type of particle selected from titania, zircon, zirconia, silicon carbide, zinc oxide, and alumina is used as the second inorganic particles, in order to obtain excellent heat insulating performance within a temperature range of 90 ° C. or less, the first inorganic particles are preferably 50 mass % or more, more preferably 60 mass % or more, and even more preferably 70 mass % or more, based on the total mass of the inorganic particles. Furthermore, the first inorganic particles are preferably 95 mass % or less, more preferably 90 mass % or less, and even more preferably 80 mass % or less, based on the total mass of the inorganic particles.

[0061] On the other hand, in order to obtain excellent heat insulating performance within a temperature range exceeding 90° C., the content of the second inorganic particles is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 20% by mass or more, based on the total mass of the inorganic particles. Furthermore, the content of the second inorganic particles is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less, based on the total mass of the inorganic particles.

[0062] (Average primary particle diameter of second inorganic particles) When second inorganic particles made of a metal oxide are contained in a thermal insulating material, if the average primary particle diameter of the second inorganic particles is 1 μm or more and 50 μm or less, radiation heat transfer can be efficiently suppressed in a high temperature range of 500° C. or more. The average primary particle diameter of the second inorganic particles is more preferably 5 μm or more and 30 μm or less, and most preferably 10 μm or less.

[0063] (Inorganic Particle Content) In this embodiment, if the total content of inorganic particles in the thermal insulation material 2 is appropriately controlled, the thermal insulation properties of the thermal insulation material 2 can be sufficiently ensured. The total content of inorganic particles is preferably 60% by mass or more, and more preferably 70% by mass or more, relative to the total mass of the thermal insulation material. Furthermore, if the total content of inorganic particles becomes too high, the content of organic fibers will relatively decrease. Therefore, in order to sufficiently obtain the skeleton reinforcing effect and the inorganic particle retention effect, the total content of inorganic particles is preferably 95% by mass or less, and more preferably 90% by mass or less, relative to the total mass of the thermal insulation material.

[0064] The content of inorganic particles in the heat insulating material can be calculated, for example, by heating the heat insulating material at 800° C., decomposing the organic components, and then measuring the mass of the remaining portion.

[0065] <Inorganic Fibers> As the inorganic fibers, a single inorganic fiber may be used, or two or more inorganic fibers may be used in combination. Examples of inorganic fibers include ceramic fibers such as silica fiber, alumina fiber, alumina silicate fiber, zirconia fiber, carbon fiber, soluble fiber, refractory ceramic fiber, aerogel composite, magnesium silicate fiber, alkaline earth silicate fiber, potassium titanate fiber, silicon carbide fiber, and potassium titanate whisker fiber; glass fibers such as glass fiber, glass wool, and slag wool; and natural mineral fibers such as rock wool, basalt fiber, wollastonite, and mullite fiber. These inorganic fibers are preferred in terms of heat resistance, strength, and availability. Among the inorganic fibers, from the viewpoint of handleability, it is particularly preferred to use at least one selected from silica fiber, alumina fiber, alumina silicate fiber, zirconia fiber, glass fiber, and natural mineral fibers other than these fibers.

[0066] The cross-sectional shape of the inorganic fiber is not particularly limited, and examples thereof include a circular cross section, a flat cross section, a hollow cross section, a polygonal cross section, a core cross section, etc. Among these, modified cross section fibers having a hollow cross section, a flat cross section, or a polygonal cross section are preferably used because they have slightly improved heat insulation properties.

[0067] (Average fiber length of inorganic fibers) The preferred lower limit of the average fiber length of inorganic fibers is 0.1 mm, more preferably 0.5 mm. On the other hand, the preferred upper limit of the average fiber length of inorganic fibers is 50 mm, more preferably 10 mm. If the average fiber length of inorganic fibers is less than 0.1 mm, the inorganic fibers are less likely to be entangled with each other, which may reduce the mechanical strength of the insulating material. On the other hand, if the average fiber length exceeds 50 mm, although a reinforcing effect can be obtained, the inorganic fibers may not be able to be tightly entangled with each other, or may be curled up by a single inorganic fiber, which may result in a reduction in insulating properties.

[0068] The preferred lower limit of the average fiber diameter of the inorganic fibers is 1 μm, more preferably 2 μm, and even more preferably 3 μm. On the other hand, the preferred upper limit of the average fiber diameter of the inorganic fibers is 15 μm, and more preferably 10 μm. If the average fiber diameter of the inorganic fibers is less than 1 μm, the mechanical strength of the inorganic fibers themselves may be reduced. Furthermore, from the viewpoint of the effects on human health, the average fiber diameter of the inorganic fibers is preferably 3 μm or more. On the other hand, if the average fiber diameter of the inorganic fibers is greater than 15 μm, solid heat transfer through the inorganic fibers may increase, leading to a decrease in thermal insulation properties, and the moldability and strength of the thermal insulation material may be deteriorated.

[0069] (Inorganic Fiber Content) In the present embodiment, when the thermal insulating material 2 contains inorganic fibers, the content of the inorganic fibers is preferably 3 mass % or more and 15 mass % or less with respect to the total mass of the thermal insulating material.

[0070] Furthermore, the content of inorganic fibers is more preferably 5% by mass or more and 10% by mass or less of the total mass of the thermal insulation material. By setting the content in this range, the shape retention, pressing force resistance, wind pressure resistance, and inorganic particle retention ability of the inorganic fibers are exhibited in a balanced manner. Furthermore, by appropriately controlling the content of inorganic fibers, the organic fibers and inorganic fibers are entangled with each other to form a three-dimensional network, which further improves the effect of retaining inorganic particles and other compounding materials described below.

[0071] <Organic Fibers> Organic fibers have the effect of imparting flexibility to the insulating material, and by forming a skeleton, they have the effect of increasing the strength of the insulating material. Furthermore, if inorganic particles and other organic fibers are fused to the surface of the organic fibers, the effect of improving the strength of the insulating material and the effect of maintaining its shape can be further improved. Furthermore, if the insulating material contains organic fibers in an appropriate content, multiple voids are formed inside the insulating material, and when the insulating material is heated, air and moisture can be released to the outside through the voids.

[0072] As the organic fiber material for the insulation material 2, in addition to single-component organic fibers such as cellulose fiber, polyvinyl alcohol (PVA) fiber, polyethylene fiber, nylon fiber, polyurethane fiber, ethylene-vinyl alcohol copolymer fiber, etc. can be used.

[0073] When the heat insulating material is manufactured by a papermaking method, it is difficult to raise the heating temperature above 250°C. Therefore, the glass transition point of the organic fiber is preferably 250°C or lower, and more preferably 200°C or lower.

[0074] Although the lower limit of the glass transition point of the organic fiber is not particularly limited, when a resin binder is used, if the difference between the glass transition point of the organic fiber and the glass transition point of the resin binder is 10°C or more, the resin binder will solidify after the organic fiber, which was in a semi-molten state, has completely solidified in the cooling step during production, and therefore the skeleton reinforcing effect of the resin binder can be sufficiently obtained. Therefore, the difference between the glass transition point of the resin binder and the glass transition point of the organic fiber is preferably 10°C or more, and more preferably 30°C or more.

[0075] On the other hand, if the difference in glass transition point between the two is 130°C or less, the time from when the organic fibers completely solidify until the resin binder starts to solidify can be appropriately adjusted, and the resin binder solidifies while remaining in a well-dispersed state, thereby achieving an even greater reinforcement effect for the skeleton. Therefore, the difference between the glass transition point of the resin binder and the glass transition point of the organic fibers is preferably 130°C or less, more preferably 120°C or less, even more preferably 100°C or less, even more preferably 80°C or less, and particularly preferably 70°C or less.

[0076] The organic fibers may also be binder fibers with a sheath-core structure. The binder fibers have a core extending in the longitudinal direction of the fiber and a sheath formed to cover the outer surface of the core. In this case, the core is made of a first organic material, and the sheath is made of a second organic material, and the melting point of the first organic material is higher than that of the second organic material.

[0077] (First Organic Material) In the present embodiment, when a binder fiber having a core-sheath structure is used, the first organic material constituting the core is not particularly limited as long as it has a melting point higher than that of the sheath present on the outer surface of the core, i.e., the second organic material. Examples of the first organic material include at least one selected from polyethylene terephthalate, polypropylene, and nylon.

[0078] (Second Organic Material) The second organic material is not particularly limited as long as it has a melting point lower than that of the first organic material constituting the organic fiber. Examples of the second organic material include at least one selected from polyethylene terephthalate, polyethylene, polypropylene, and nylon. The melting point of the second organic material is preferably 90°C or higher, more preferably 100°C or higher. The melting point of the second organic material is preferably 150°C or lower, more preferably 130°C or lower.

[0079] (Organic fiber content) When the organic fiber content in the thermal insulation material 2 is appropriately controlled, a sufficient skeleton reinforcing effect can be obtained. The organic fiber content is preferably 5 mass% or more, and more preferably 10 mass% or more, relative to the total mass of the thermal insulation material. Furthermore, if the organic fiber content is too high, the inorganic particle content will relatively decrease. Therefore, in order to obtain the desired thermal insulation performance, the organic fiber content is preferably 25 mass% or less, and more preferably 20 mass% or less, relative to the total mass of the thermal insulation material.

[0080] (Fiber length of organic fibers) The fiber length of the organic fibers is not particularly limited, but from the viewpoint of ensuring moldability and processability, the average fiber length of the organic fibers is preferably 10 mm or less. On the other hand, from the viewpoint of making the organic fibers function as a skeleton and ensuring the compressive strength of the thermal insulating material, the average fiber length of the organic fibers is preferably 0.5 mm or more.

[0081] (Infusible Fiber) The heat insulating material 2 may contain infusible fiber as the fiber. Examples of the infusible fiber include fibers obtained by infusibility treatment of thermoplastic resins such as polyacrylonitrile, cellulose, and pitch. The infusible fiber is, for example, a fiber that has been infusible treated, and examples of the infusible treatment include a method of crosslinking by irradiation with radiation or an electron beam, and a method of exposing the fiber to high temperatures in oxygen or water vapor to make it infusible by the action of oxygen.

[0082] (Carbon Content) The infusible fiber preferably has a carbon content of 55 to 95% by mass. When the carbon content is 55% by mass or more, weight loss due to thermal decomposition has already progressed, so shrinkage due to thermal decomposition is small, and even if directly exposed to flames during thermal runaway, the fiber retains its original shape and maintains its thermal insulation properties. When the carbon content is 95% by mass or less, components other than carbon are eliminated and the fiber changes to a structure consisting only of carbon, causing an endothermic reaction, which can delay the time it takes for heat to reach the back surface of the flame-retardant structure.

[0083] The lower limit of the carbon content is preferably 60% by mass or more, and the upper limit of the carbon content is preferably 90% by mass or less, and more preferably 85% by mass or less.

[0084] The carbon content can be adjusted by heat treatment. For example, heat treatment in air or oxygen at a temperature in the range of 150 to 300°C can further promote infusibility and remove components other than carbon, thereby increasing the carbon content. For example, heat treatment at a temperature in the range of 300 to 1000°C can promote the formation of condensed polycyclic aromatic structures and generate decomposition gases, thereby increasing the carbon content.

[0085] The infusible fibers are not limited to fibers that have been infusible from thermoplastic fibers, and may be inorganic fibers as long as they have a carbon content within the above range.

[0086] (Fiber Shape) The infusible fibers are preferably short fibers. Short fibers mean that they are not continuous fibers. Continuous fibers, like cloth or filament winding, form fiber bundles with the fibers oriented in the same direction, whereas short fibers form aggregates (mats, blankets, and paper products) with the fibers oriented in random directions. Furthermore, insulation materials using short fibers have short conductive paths, so they can have low conductivity even when carbonization of fibers progresses or when carbonization progresses due to thermal runaway. Furthermore, the random orientation of the fibers makes them more likely to form point contacts with each other, thereby reducing thermal conductivity.

[0087] When manufacturing a thermal insulation material containing infusible fibers, it is preferable to use milled or chopped infusible fibers (fiber length of about 0.01 to 10 mm). The infusible fibers preferably have a fiber diameter of 1 to 30 μm. When the fiber diameter of the infusible fibers is 1 μm or more, the rate of air oxidation and sublimation can be suppressed even when exposed to high temperatures, and the flame-retardant effect can be maintained for a long period of time. On the other hand, when the fiber diameter of the infusible fibers is 30 μm or less, a certain degree of flexibility can be maintained even when exposed to high temperatures and carbonized, making them less susceptible to breakage even when deformed or impacted.

[0088] <Organic Particles> As the organic particles, hollow polystyrene particles or the like can be used.

[0089] <Other Compounding Materials> (Resin Binder) The material of the heat insulating material 2 in this embodiment can also be bound by a resin binder. There are no particular limitations on the resin binder as long as it has a glass transition point lower than the glass transition point of the single-component organic fiber. For example, a resin binder containing at least one selected from styrene-butadiene resin, acrylic resin, silicone-acrylic resin, and styrene resin can be used.

[0090] The glass transition point of the resin binder is not particularly specified, but is preferably -10°C or higher. If the glass transition point of the resin binder is room temperature or higher, the strength of the insulating material can be further improved when the insulating material containing the resin binder is used at room temperature. Therefore, the glass transition point of the resin binder is, for example, more preferably 20°C or higher, even more preferably 30°C or higher, even more preferably 50°C or higher, and particularly preferably 60°C or higher.

[0091] The content of the resin binder is preferably 0.5% by mass or more, more preferably 1% by mass or more, based on the total mass of the heat insulating material, and is preferably 20% by mass or less, more preferably 10% by mass or less.

[0092] (Hot Melt Powder) In addition to the inorganic particles, inorganic fibers, organic fibers, and organic particles, the mixture used to manufacture the insulating material 2 may contain hot melt powder. When using the core-sheath binder fiber, the hot melt powder contains, for example, a third organic material different from the first and second organic materials, and is a powder that melts when heated. When the hot melt powder is added to the material mixture of the insulating material 2 and heated, the hot melt powder melts, and when cooled, it hardens in a state that includes the surrounding inorganic particles. This further prevents the inorganic particles from falling off the insulating material.

[0093] Hot melt powders with various melting points can be used, but a hot melt powder with an appropriate melting point can be selected taking into account the melting points of the core and sheath of the binder fiber used. When a core-sheath binder fiber is used as the organic fiber, if the third organic material constituting the hot melt powder has a melting point lower than that of the first organic material constituting the organic fiber, the heating temperature can be set to melt the sheath and hot melt powder while leaving the core. For example, if the melting point of the hot melt powder is lower than that of the sheath, the heating temperature during production can be set between the melting points of the core and the sheath, making it even easier to set the heating temperature.

[0094] Alternatively, the type of hot melt powder used can be selected so that its melting point lies between the melting points of the core and the sheath. When a hot melt powder with such a melting point is used, the sheath and hot melt powder melt together, and then when they cool and harden, the organic fibers (core), the molten sheath around them, and the hot melt powder present in the gaps between the inorganic particles harden first. As a result, the position of the organic fibers can be fixed, and then the molten sheath is fused to the organic fibers, facilitating the formation of a three-dimensional skeleton. This further improves the strength of the entire insulation.

[0095] If the melting point of the third organic material constituting the hot melt powder is sufficiently lower than that of the first organic material constituting the core, the heating temperature setting margin in the heating step can be expanded, making it easier to set the temperature to obtain the desired structure. For example, the melting point of the first organic material is preferably 60°C or more higher than that of the third organic material, more preferably 70°C or more higher, and even more preferably 80°C or more higher.

[0096] The melting point of the hot melt powder (third organic material) is preferably 80° C. or higher, and more preferably 90° C. or higher. The melting point of the hot melt powder (third organic material) is preferably 180° C. or lower, and more preferably 150° C. or lower. Examples of components constituting the hot melt powder include polyethylene, polyester, polyamide, and ethylene vinyl acetate.

[0097] (Hot melt powder content) When hot melt powder is contained in the material of the insulating material to suppress the shedding of inorganic particles, even a small amount of hot melt powder can be used to suppress powder shedding. Therefore, the content of the hot melt powder is preferably 0.5% by mass or more, more preferably 1% by mass or more, based on the total mass of the materials constituting the insulating material. On the other hand, since the content of inorganic particles and the like decreases relatively when the content of the hot melt powder is increased, in order to obtain the desired insulating performance, the content of the hot melt powder is preferably 5% by mass or less, more preferably 4% by mass or less, based on the total mass of the materials constituting the insulating material.

[0098] When the insulating material contains a hot melt powder, the heating temperature in the heating step is preferably set to be at least 10°C higher, more preferably 20°C higher, than the higher of the melting point of the second organic material constituting the sheath and the melting point of the third organic material constituting the hot melt powder. On the other hand, the heating temperature is preferably set to be at least 10°C lower, more preferably 20°C lower, than the melting point of the first organic material constituting the core. Setting the heating temperature at such a temperature allows a strong skeleton to be formed, further improving the strength of the insulating material and preventing the inorganic particles from falling off.

[0099] The heat insulating material 2 may further contain other binders, colorants, etc. as needed. These are all useful for the purpose of reinforcing the heat insulating material or improving its formability, and the total amount of these additives is preferably 10 mass % or less based on the total mass of the heat insulating material.

[0100] In the present invention, the method for producing the heat insulating material 2 is not particularly limited, and commonly used wet and dry methods can be used to produce the heat insulating material 2. As for the materials used in production, a material suitable for the production method may be selected from the materials listed above depending on the required properties.

[0101] [Inorganic Fiber Sheet] The inorganic fiber sheet 3 in this embodiment is formed by processing inorganic fibers into a sheet, and the inorganic fibers used are not particularly limited. For example, the inorganic fibers described in the above-mentioned thermal insulating material 2 can also be used. Among them, it is preferable to use silica fiber, alumina fiber, glass fiber, metal fiber, etc., because they are inexpensive, easy to handle, and have high heat resistance.

[0102] There are no restrictions on the shape of the inorganic fibers, such as the fiber diameter, etc. However, in consideration of preventing collisions with flying particles during thermal runaway, it is preferable that the mesh size is small.

[0103] [Adhesive Layer] The adhesive layer 4 in this embodiment contains an organic material. The adhesive layer 4 in this embodiment is formed, for example, by placing an adhesive material made of an organic material between the thermal insulation 2 and the inorganic fiber sheet 3, and then heating and pressurizing the adhesive layer 4. At this time, the inorganic particles 8 in the thermal insulation 2 penetrate into the adhesive layer 4, so the adhesive layer 4 also contains the inorganic particles 8. However, the content of the organic material is preferably 80 mass% or more of the total mass of the adhesive layer.

[0104] The organic material is not particularly limited, but examples thereof include synthetic rubber, polyolefin-based organic materials, polyamide-based organic materials, and polyurethane-based organic materials. Among these, it is preferable to use at least one of polyolefin-based organic materials and polyamide-based organic materials. In particular, the use of polyolefin-based organic materials allows for the formation of an adhesive layer at low cost, while the use of polyamide-based organic materials can improve bonding strength. Therefore, the material for the adhesive layer can be selected according to the required characteristics. Specific examples of polyolefin-based organic materials include polyethylene and polypropylene. These materials have properties such as flexibility, shock absorption, softness, low rigidity, easy deformation, and the ability to be stretched into a film. Therefore, polyethylene and polypropylene can be suitably used as the material for the adhesive layer in this embodiment.

[0105] [Method of Manufacturing Cover Protector] Fig. 4 is a schematic view showing an example of a method of manufacturing a cover protector according to an embodiment of the present invention. The method of manufacturing the cover protector will be described in order of steps with reference to Fig. 4 .

[0106] <Placement Process> The placement process is a process of placing an adhesive material that forms an adhesive layer between the thermal insulation material and the inorganic fiber sheet. Specifically, an inorganic fiber sheet material 12 is pulled out from a wound sheet roll 11, and while moving it horizontally, fibrous adhesive material 14 is ejected from multiple nozzles 13 arranged above the inorganic fiber sheet material 12. Then, a thermal insulation sheet material 15 is placed on the inorganic fiber sheet material 12 on which the adhesive material 14 has been placed.

[0107] In the process of placing adhesive material 14 on the upper surface of the inorganic fiber sheet material 12, a plurality of fibrous adhesive materials 14 extending in multiple directions are placed on the inorganic fiber sheet material 12 in a state where they overlap each other at least in part.

[0108] <Bonding process> The bonding process is a process of heating and pressurizing the area where the heat insulating material, adhesive material, and inorganic fiber sheet are laminated. Specifically, the inorganic fiber sheet material 12, adhesive material 14, and heat insulating sheet material 15 are further moved and passed between a pair of hot rolls 16 arranged above and below them, thereby heating and pressurizing the area where they are laminated. Thereafter, they are cooled, thereby bonding the inorganic fiber sheet material 12 and the heat insulating sheet material 15 together.

[0109] In the joining step, the adhesive material 14 spreads and fuses in the overlapping regions, forming the island-shaped portions 5 shown in Fig. 2. In the regions where the island-shaped portions 5 are not formed, the adhesive material 14 spreads out slightly due to pressure, but the fibrous shape remains intact, forming the mesh-shaped portions 6.

[0110] <Molding process> Thereafter, the region where the inorganic fiber sheet material 12 and the heat insulating sheet material 15 are bonded together is cut using a cutting machine 17 or the like to form the desired shape and size. In this way, the cover protector 1 can be manufactured in which the heat insulating material 2 and the inorganic fiber sheet 3 are bonded together by the adhesive layer 4. Note that the unnecessary portion after cutting is taken up by a take-up roll 18.

[0111] According to the above manufacturing method, it is possible to easily form the adhesive layer 4 having the island-shaped portions 5 and the mesh-shaped portions 6, and the island-shaped portions 5 can firmly bond the heat insulating material 2 and the inorganic fiber sheet 3. Furthermore, since the mesh-shaped portions 6 form the voids 7 shown in Fig. 3, it is possible to further improve the heat insulating performance compared to when the heat insulating material 2 and the inorganic fiber sheet 3 are bonded with a normal bonding material.

[0112] The shape of the fibrous adhesive material 14 is not particularly limited, and the fibrous adhesive material 14 may be arranged irregularly, for example, like a nonwoven fabric. Alternatively, multiple fibrous adhesive materials 14 extending in a first direction, a second direction different from the first direction, and a third direction different from the first and second directions may be arranged so as to overlap each other. Alternatively, multiple fibrous adhesive materials 14 may be arranged in a spiral or wave shape.

[0113] Furthermore, in order to form island-shaped portions 5, it is preferable to arrange the adhesive material 14 so that the amount of fibrous adhesive material arranged in the plurality of first regions is greater than the amount of adhesive material arranged in the other second regions. For example, the first regions may be regions where the plurality of fibrous adhesive materials 14 overlap each other. Furthermore, the amount of adhesive material 14 arranged in a desired region (first region) may be intentionally adjusted to be greater so as to form island-shaped portions 5.

[0114] The method for manufacturing the cover protector 1 is not limited to the above method. For example, a method can be adopted in which an adhesive sheet is prepared in advance as the adhesive material, and the adhesive sheet is placed between a heat insulating material formed into a desired shape and an inorganic fiber sheet, followed by heating and pressure. The adhesive sheet can be made by processing a plurality of fibers made of an organic material and extending in multiple directions into a sheet. In this case, the fibers made of the organic material can be arranged so that the fiber density in the plurality of first regions is higher than the fiber density in the second regions. For example, by forming a region in which a plurality of fibers overlap each other, this region can be designated as the first region.

[0115] [Battery Module] Fig. 5 is a schematic cross-sectional view showing a battery module according to an embodiment of the present invention. As shown in Fig. 5, the battery module 100 includes a plurality of storage batteries 110 housed in a battery case 120. The electrode terminals 111 of the storage batteries 110 are connected in series by a bus bar 130.

[0116] The battery case 120 has a ceiling surface 120a, side wall surfaces 120b, and a bottom wall surface 120c inside. The cover protector 1 according to the present embodiment is attached with tape or the like to the entire surface of the ceiling surface 120a of the battery case 120. Although not shown in the drawings, the cover protector 1 is disposed so that the inorganic fiber sheet of the cover protector 1 faces the electrode terminal 111 and so that the heat insulating material of the cover protector 1 faces the ceiling surface of the battery case 120.

[0117] In the battery module 100 configured in this manner, the cover protector 1 has excellent heat insulating properties, so even if the storage battery 110 experiences thermal runaway, becomes hot, or catches fire, it is possible to delay the transfer of heat to the outside of the battery case 120. Furthermore, in this embodiment, the inorganic fiber sheet and the heat insulating material are joined with high bonding strength, so that if the storage battery 110 explodes due to thermal runaway, the inorganic fiber sheet will not fall, protecting the heat insulating material and preventing damage to the heat insulating material.

[0118] Although the battery module 100 shown in FIG. 5 has the cover protector 1 attached only to the ceiling surface 120a of the battery case 120, the present invention is not limited to this configuration. For example, attaching the cover protector 1 to at least one of the ceiling surface 120a, side wall surface 120b, and bottom wall surface 120c of the battery case 120 can slow the transfer of heat to the outside of the battery case 120. Attaching the cover protector 1 to all of the ceiling surface 120a, side wall surface 120b, and bottom wall surface 120c of the battery case 120 can further improve thermal insulation and flame resistance. Furthermore, the cover protector 1 may be attached between multiple storage batteries 110.

[0119] Although various embodiments have been described above, it goes without saying that the present invention is not limited to such examples. It is clear that a person skilled in the art can conceive of various modifications or alterations within the scope of the claims, and it is understood that these also naturally fall within the technical scope of the present invention. Furthermore, the components of the above embodiments may be combined in any manner as long as they do not deviate from the spirit of the invention.

[0120] This application is based on a Japanese patent application filed on March 29, 2023 (Patent Application No. 2023-053777) and a Japanese patent application filed on February 9, 2024 (Patent Application No. 2024-018668), the contents of which are incorporated by reference into this application.

[0121] REFERENCE SIGNS LIST 1 Cover protector 2 Heat insulating material 3 Inorganic fiber sheet 4 Adhesive layer 5 Island-shaped portion 6 Mesh-shaped portion 7 Void portion 8 Inorganic particles 14 Adhesive material 100 Battery module 110 Storage battery 120 Battery case

Claims

1. A cover protector comprising: an insulating material containing inorganic particles; an inorganic fiber sheet; and an adhesive layer containing an organic material that bonds the insulating material and the inorganic fiber sheet, wherein when viewed in the stacking direction of the insulating material and the inorganic fiber sheet, the adhesive layer has a plurality of island-shaped portions and a mesh-shaped portion that connects the plurality of island-shaped portions to each other.

2. The cover protector according to claim 1, characterized in that the organic material contained in the adhesive layer is at least one selected from the group consisting of synthetic rubber, polyolefin-based organic material, polyamide-based organic material, and polyurethane-based organic material.

3. The cover protector according to claim 1, characterized in that the content of the organic material is 80 mass % or more with respect to the total mass of the adhesive layer.

4. The cover protector as described in claim 1, characterized in that the mesh portion has a plurality of linear elements, the plurality of linear elements extending in a plurality of directions while partially intersecting with each other to form the mesh portion.

5. The cover protector according to claim 1, characterized in that a gap is provided between the inorganic fiber sheet and the heat insulating material.

6. A cover protector as described in claim 1, characterized in that the organic material constituting the adhesive layer penetrates into the inorganic fiber sheet in a region extending from the surface in contact with the adhesive layer to the inside.

7. The cover protector according to claim 1, characterized in that the adhesive layer contains a portion of inorganic particles contained in the insulating material.

8. The cover protector according to claim 1, characterized in that the inorganic fiber sheet is made by processing at least one type of fiber selected from the group consisting of silica fiber, alumina fiber, glass fiber and metal fiber into a sheet shape.

9. A method for manufacturing a cover protector as described in any one of claims 1 to 8, comprising: an arrangement step of arranging an adhesive material constituting the adhesive layer between the insulating material and the inorganic fiber sheet; and a joining step of heating and pressurizing the area where the insulating material, the adhesive material, and the inorganic fiber sheet are laminated, wherein the arrangement step comprises a step of arranging a plurality of fibrous adhesive materials extending in a plurality of directions between the insulating material and the inorganic fiber sheet, and the adhesive material is arranged so that the amount of the adhesive material arranged in a plurality of first areas is greater than the amount of the adhesive material arranged in other second areas, and wherein in the joining step, the island-shaped portion is formed in the first area, and the mesh-shaped portion is formed in the second area.

10. The method for manufacturing a cover protector according to claim 9, wherein the first region is a region in which the plurality of fibrous adhesive materials overlap each other.

11. A method for manufacturing a cover protector as described in claim 9, characterized in that the adhesive material is made of an organic material and is formed into a sheet of multiple fibers extending in multiple directions, and the fibers are arranged so that the density of the fibers in the first region is greater than the density of the fibers in the second region.

12. The method for manufacturing a cover protector according to claim 11, wherein the first region is a region where the plurality of fibers overlap each other.

13. A battery module comprising: a cover protector according to any one of claims 1 to 8; a storage battery; and a battery case that houses the cover protector and the storage battery.

14. The battery module described in claim 13, characterized in that the battery case has a ceiling surface, side wall surfaces and bottom wall surfaces therein, the heat insulating material is arranged to face at least one selected from the ceiling surface, side wall surfaces and bottom wall surfaces, and the cover protector is attached inside the battery case.

Citation Information

Patent Citations

  • Manufacturing method for manufacturing joined body

    JP2023053777A

  • Game machine

    JP2024018668A

  • Thermal barrier material for a rechargeable electrical energy storage system

    WO2021022130A1

  • Insulating material