Polarizing film equipped with adhesive sheet, optical laminate, and image display device
The use of a photocurable adhesive sheet with specific gel fraction and sol content, combined with a (meth)acrylic polymer and silane coupling agent, addresses peeling issues in image display devices by enhancing cohesive force and stress relaxation, ensuring reliable performance at high temperatures.
Patent Information
- Application Number
- PCT/JP2024/009904
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-13
- Publication Date
- 2024-10-03
AI Technical Summary
Photocurable adhesive sheets used in optical films for image display devices experience image quality deterioration due to peeling issues when exposed to high-temperature environments, as the adhesive sheets and adherends tend to peel off, leading to segregation of sol components at the interface.
A photocurable adhesive sheet with a gel fraction of 55% or more and less than 94% and a sol component A content of less than 6.6% by weight, combined with an optical film, which includes a (meth)acrylic polymer with structural units derived from carboxyl group-containing and nitrogen atom-containing monomers, and a silane coupling agent, to enhance stress relaxation properties and cohesive force, preventing peeling and sol component segregation.
The solution effectively suppresses peeling and sol component segregation at high temperatures, maintaining image quality by balancing stress relaxation and cohesive force, ensuring the adhesive sheet's reliability in high-temperature environments.
Smart Images

Figure JP2024009904_03102024_PF_FP_ABST
Abstract
Description
Polarizing film with adhesive sheet, optical laminate and image display device
[0001] The present invention relates to a polarizing film with a pressure-sensitive adhesive sheet, an optical laminate, and an image display device.
[0002] Various image display devices, such as liquid crystal display devices and electroluminescence (EL) display devices, generally include an optical laminate including an optical film such as a polarizing film and an adhesive sheet. An adhesive sheet is typically used to bond the optical films included in the optical laminate or to bond the optical laminate to an image display panel. A typical adhesive sheet is a sheet obtained by curing a group of monomers, such as acrylic monomers and silicone monomers, through polymerization and crosslinking. Patent Document 1 discloses a polarizing film with an adhesive sheet, which includes an adhesive sheet formed from a photocurable composition (hereinafter referred to as a photocurable adhesive sheet) and a polarizing film as an optical film. A type of adhesive sheet different from the photocurable type is a thermosetting adhesive sheet, which is formed by thermally curing a layer containing an adhesive composition and a solvent.
[0003] Japanese Patent Application Laid-Open No. 2021-56510
[0004] When a photocurable pressure-sensitive adhesive sheet is used in an optical film with a pressure-sensitive adhesive sheet, problems tend to occur in the quality of images in an image display device that may be exposed to a high-temperature environment.
[0005] An object of the present invention is to provide an optical film with a pressure-sensitive adhesive sheet that is suitable for use in an image display device that may be exposed to a high-temperature environment, while being provided with a photocurable pressure-sensitive adhesive sheet.
[0006] The present invention provides an optical film with a pressure-sensitive adhesive sheet, comprising: a photocurable pressure-sensitive adhesive sheet; and an optical film, wherein the gel fraction of the pressure-sensitive adhesive sheet is 55% or more and less than 94%, and the content of sol fraction A having a weight-average molecular weight of 100,000 or less in the pressure-sensitive adhesive sheet is less than 6.6% by weight.
[0007] The present invention further provides an optical laminate comprising the above-mentioned optical film with a pressure-sensitive adhesive sheet.
[0008] The present invention further provides an image display device comprising the above-mentioned optical film with a pressure-sensitive adhesive sheet.
[0009] According to the present invention, it is possible to provide an optical film with a pressure-sensitive adhesive sheet that is suitable for use in an image display device that may be exposed to a high-temperature environment, while being equipped with a photocurable pressure-sensitive adhesive sheet.
[0010] FIG. 1 is a cross-sectional view schematically showing an example of an optical film with a pressure-sensitive adhesive sheet of the present invention. FIG. 2 is a schematic view for explaining an example of a method for forming a pressure-sensitive adhesive sheet that can be provided on the optical film with a pressure-sensitive adhesive sheet of the present invention. FIG. 3 is a cross-sectional view schematically showing an example of an optical laminate of the present invention. FIG. 4 is a cross-sectional view schematically showing an example of an optical laminate of the present invention. FIG. 5 is a cross-sectional view schematically showing an example of an image display device of the present invention. FIG. 6 is a graph showing the relationship between the gel fraction and the content of sol fraction A having a weight-average molecular weight of 100,000 or less in each pressure-sensitive adhesive sheet of the Examples and Comparative Examples.
[0011] The optical film with adhesive sheet according to a first aspect of the present invention comprises a photocurable adhesive sheet and an optical film, wherein the gel fraction of the adhesive sheet is 55% or more and less than 94%, and the content of sol fraction A having a weight average molecular weight of 100,000 or less in the adhesive sheet is less than 6.6% by weight.
[0012] In a second aspect of the present invention, for example, in the pressure-sensitive adhesive sheet-attached optical film according to the first aspect, the content of the sol component A is 5.8% by weight or less.
[0013] In a third aspect of the present invention, for example, in the pressure-sensitive adhesive sheet-attached optical film according to the first aspect, the content of the sol component A is 4.9% by weight or less.
[0014] In a fourth aspect of the present invention, for example, in an optical film with an adhesive sheet according to any one of the first to third aspects, the weight average molecular weight of the polymer contained in the adhesive sheet is 700,000 or more but less than 800,000, and the weight average molecular weight of all sol components B contained in the adhesive sheet is 600,000 or more, or the weight average molecular weight of the polymer is 800,000 or more, and the weight average molecular weight of the sol components B is 450,000 or more.
[0015] In a fifth aspect of the present invention, for example, in the optical film with a pressure-sensitive adhesive sheet according to any one of the first to fourth aspects, the pressure-sensitive adhesive sheet contains a (meth)acrylic polymer.
[0016] In a sixth aspect of the present invention, for example, in the pressure-sensitive adhesive sheet-attached optical film according to the fifth aspect, the (meth)acrylic polymer has a constituent unit derived from a carboxyl group-containing monomer.
[0017] In a seventh aspect of the present invention, for example, in the pressure-sensitive adhesive sheet-attached optical film according to the fifth or sixth aspect, the (meth)acrylic polymer has a constituent unit derived from a nitrogen atom-containing monomer.
[0018] In an eighth aspect of the present invention, for example, in the optical film with a pressure-sensitive adhesive sheet according to any one of the first to seventh aspects, the pressure-sensitive adhesive sheet contains a silane coupling agent.
[0019] In a ninth aspect of the present invention, for example, in the optical film with a pressure-sensitive adhesive sheet according to any one of the first to eighth aspects, the pressure-sensitive adhesive sheet has a thickness of 50 μm or less.
[0020] In a tenth aspect of the present invention, for example, in the optical film with a pressure-sensitive adhesive sheet according to any one of the first to ninth aspects, the content of solvent in the pressure-sensitive adhesive sheet is 5 wt % or less.
[0021] In an eleventh aspect of the present invention, for example, in the optical film with a pressure-sensitive adhesive sheet according to any one of the first to tenth aspects, the pressure-sensitive adhesive sheet and the optical film are in contact with each other.
[0022] In a twelfth aspect of the present invention, for example, in the pressure-sensitive adhesive sheet-attached optical film according to any one of the first to eleventh aspects, the optical film is a polarizing film.
[0023] An optical laminate according to a thirteenth aspect of the present invention includes the optical film with a pressure-sensitive adhesive sheet according to any one of the first to twelfth aspects.
[0024] An image display device according to a fourteenth aspect of the present invention includes the optical film with a pressure-sensitive adhesive sheet according to any one of the first to twelfth aspects.
[0025] The present invention will be described in detail below, but the present invention is not limited to the following embodiments and can be implemented in any modified form without departing from the gist of the present invention.
[0026] [Optical film with adhesive sheet] An example of an optical film with adhesive sheet of this embodiment is shown in Figure 1. The optical film 11 with adhesive sheet of Figure 1 comprises an adhesive sheet 1 and an optical film 2. The adhesive sheet 1 and the optical film 2 are in contact. The adhesive sheet 1 is a photocurable adhesive sheet formed from a photocurable composition. The gel fraction of the adhesive sheet 1 is 55% or more and 94% or less. The content of sol fraction (sol fraction A) having a weight average molecular weight (hereinafter referred to as Mw) of 100,000 or less in the adhesive sheet 1 is less than 6.6% by weight. The gel fraction is based on weight.
[0027] Through research by the present inventors, it has been found that one of the factors behind the deterioration of image quality due to exposure to high-temperature environments is the tendency for the adhesive sheet in the optical laminate to peel off from the adherend (object to be adhered) in contact therewith at high temperatures. For the adhesive sheet 1, satisfying both the above-mentioned gel fraction and sol fraction A content ranges is presumed to contribute to achieving a balance between the stress relaxation properties and cohesive force of the adhesive sheet 1 that is suitable for suppressing the peeling at high temperatures, as well as to suppressing segregation of the sol fraction near the interface between the adhesive sheet 1 and the adherend. It is believed that regions where the sol fraction, particularly the sol fraction A having an Mw of 100,000 or less, segregates are relatively susceptible to destruction at high temperatures. An example of an adherend is a glass substrate.
[0028] The lower limit of the gel fraction of the PSA sheet 1 may be 56% or more, 57% or more, 58% or more, 59% or more, or even 60% or more. The upper limit of the gel fraction may be 93.5% or less, 93% or less, 92.5% or less, 92% or less, 91.5% or less, 91% or less, 90.5% or less, or even 90% or less.
[0029] The gel fraction of the pressure-sensitive adhesive sheet 1 can be evaluated as follows. A test piece of approximately 0.1 g is collected from the pressure-sensitive adhesive sheet 1, wrapped in a polytetrafluoroethylene porous sheet (average pore size 0.2 μm, product name "NTF1122", manufactured by Nitto Denko Corporation), and tied with kite string to obtain a measurement sample. Next, the weight of the obtained measurement sample (weight before immersion C) is measured. The weight before immersion C is the total weight of the test piece, the polytetrafluoroethylene porous sheet, and the kite string. Separately, the bag weight B, which is the total weight of the polytetrafluoroethylene porous sheet and the kite string, is measured. Next, the measurement sample is placed in a 50 mL container filled with ethyl acetate and allowed to stand at 23°C for 7 days. After standing, the measurement sample is removed from the container and transferred to an aluminum cup, and the ethyl acetate is removed by drying in a dryer at 130°C for 2 hours. The weight of the measurement sample after drying (weight after immersion A) is measured. The value calculated from the following formula is determined as the gel fraction of the pressure-sensitive adhesive sheet 1. Gel fraction (%)=(A−B) / (C−B)×100
[0030] The content of sol component A in the pressure-sensitive adhesive sheet 1 may be 6.5 wt% or less, 6.3 wt% or less, 6.0 wt% or less, 5.8 wt% or less, 5.5 wt% or less, 5.3 wt% or less, 5.0 wt% or less, 4.9 wt% or less, 4.5 wt% or less, 4.3 wt% or less, 4.1 wt% or less, 4.0 wt% or less, 3.8 wt% or less, 3.7 wt% or less, 3.6 wt% or less, 3.5 wt% or less, 3.3 wt% or less, 3.0 wt% or less, 2.8 wt% or less, 2.5 wt% or less, 2.4 wt% or less, 2.3 wt% or less, 2.2 wt% or less, 2.1 wt% or less, or even 2.0 wt% or less. The lower limit of the content is not particularly limited, and may be, for example, 0.0 wt% or more, 0.05 wt% or more, 0.1 wt% or more, or even 0.2 wt% or more.
[0031] In this specification, the sol content refers to components that can be extracted from the PSA sheet 1 with ethyl acetate. The sol content A refers to components with a Mw of 100,000 or less among all the sol contents (sol content B) contained in the PSA sheet 1. The content (wt %) of sol content B in the PSA sheet 1 can be specified as 100 - gel fraction (%).
[0032] The content of sol component A in the pressure-sensitive adhesive sheet 1 can be evaluated by gel permeation chromatography (GPC) as follows: A portion sampled from the pressure-sensitive adhesive sheet 1 is dissolved in a GPC eluent to prepare a solution with a sol component concentration of approximately 2.0 g / L. A GPC eluent is selected that does not substantially dissolve the gel component in the pressure-sensitive adhesive sheet 1 but dissolves the sol component. The prepared solution is left overnight and then filtered through a 0.45 μm membrane filter. GPC measurement is performed on the filtrate, and the proportion X of components with a Mw of 100,000 or less is calculated. The value calculated from the following formula can be specified as the content of sol component A in the pressure-sensitive adhesive sheet 1. Content of sol component A (wt%) = Content of sol component B (wt%) × X / 100
[0033] The gel fraction and the content of sol fraction A in the pressure-sensitive adhesive sheet 1 can vary depending on, for example, the composition of the photocurable composition used to form the pressure-sensitive adhesive sheet 1 and the curing conditions of the photocurable composition. Examples of the composition include the type and content of each monomer constituting the monomer group contained in the photocurable composition, the type and content of the photopolymerization initiator, and the type and content of the crosslinking agent. Examples of the curing conditions include the integrated light amount of the irradiated light, the type and wavelength distribution of the light source, and the thickness of the coating film of the photocurable composition irradiated with light.
[0034] <Adhesive Sheet> (Photocurable Composition) The adhesive sheet 1 is formed from a photocurable composition. The photocurable composition typically contains a group of monomers and / or a partial polymer of the monomers. Irradiating the photocurable composition with light generates a polymer from the group of monomers and / or the partial polymer, forming the adhesive sheet 1. The generated polymer is typically the main component of the adhesive sheet 1. The group of monomers may contain a (meth)acrylic monomer. The content of the (meth)acrylic component in the photocurable composition, i.e., the (meth)acrylic monomer and its partial polymer, may be 50% by weight or more, 60% by weight or more, 70% by weight or more, or even 80% by weight or more. In this case, an acrylic adhesive sheet containing a (meth)acrylic polymer can be formed. However, the photocurable composition is not limited to the above examples. In this specification, (meth)acrylic refers to acrylic and methacrylic. (Meth)acrylate refers to acrylate and methacrylate. In this specification, the term "main component" refers to the component with the largest content. The content of the main component is, for example, 50% by weight or more, and may be 60% by weight or more, 70% by weight or more, or even 80% by weight or more.
[0035] An example of the (meth)acrylic monomer is a (meth)acrylic acid alkyl ester having an alkyl group having 1 to 20 carbon atoms on the side chain. The number of carbon atoms in the alkyl group may be 7 or less, 6 or less, 5 or less, or even 4 or less. The alkyl group may be linear or branched. Examples of the (meth)acrylic acid alkyl ester include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, n-hexyl (meth)acrylate, isohexyl (meth)acrylate, isoheptyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate. acrylate, n-octyl(meth)acrylate, isooctyl(meth)acrylate, n-nonyl(meth)acrylate, isononyl(meth)acrylate, n-decyl(meth)acrylate, isodecyl(meth)acrylate, n-dodecyl(meth)acrylate (lauryl(meth)acrylate), n-tridecyl(meth)acrylate, n-tetradecyl(meth)acrylate, pentadecyl(meth)acrylate, hexadecyl(meth)acrylate, heptadecyl(meth)acrylate, and octadecyl(meth)acrylate. The (meth)acrylic acid alkyl ester may be n-butyl(meth)acrylate.
[0036] The content of the (meth)acrylic acid alkyl ester in the monomer group is, for example, 40% by weight or more, and may be 50% by weight or more, 60% by weight or more, 70% by weight or more, 80% by weight or more, 85% by weight or more, 90% by weight or more, or even 95% by weight or more. In calculating the content, the weight of the partially polymerized product is converted into the weight of each monomer before polymerization.
[0037] The monomer group may contain a carboxyl group-containing monomer. In this case, the (meth)acrylic polymer that the PSA sheet 1 may contain has a structural unit derived from the carboxyl group-containing monomer. The carboxyl group-containing monomer may be a (meth)acrylic monomer; in other words, the (meth)acrylic monomer may contain the carboxyl group-containing monomer. Examples of carboxyl group-containing monomers include (meth)acrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid. The content of the carboxyl group-containing monomer in the monomer group may be, for example, 10 wt% or less, 9 wt% or less, 8 wt% or less, 7 wt% or less, 6 wt% or less, 5.5 wt% or less, or even 5 wt% or less. The lower limit of the content is, for example, 0.1% by weight or more, and may be 0.5% by weight or more, 1% by weight or more, 1.5% by weight or more, 2% by weight or more, 2.5% by weight or more, 3% by weight or more, 3.5% by weight or more, 4% by weight or more, or even 4.5% by weight or more. The monomer group does not have to contain a carboxyl group-containing monomer.
[0038] The monomer group may include a hydroxy group-containing monomer. In this case, the (meth)acrylic polymer that may be included in the PSA sheet 1 has structural units derived from the hydroxy group-containing monomer. The hydroxy group-containing monomer may be a (meth)acrylic monomer; in other words, the (meth)acrylic monomer may include a hydroxy group-containing monomer. Examples of hydroxy group-containing monomers include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)-methyl acrylate. The hydroxy group-containing monomer is preferably 2-hydroxyethyl (meth)acrylate or 4-hydroxybutyl (meth)acrylate. The content of the hydroxy group-containing monomer in the monomer group is, for example, 10% by weight or less, and may be 5% by weight or less, 4% by weight or less, 3% by weight or less, 2% by weight or less, 1% by weight or less, 0.8% by weight or less, 0.5% by weight or less, 0.3% by weight or less, 0.2% by weight or less, or even 0.1% by weight or less. The lower limit of the content may be, for example, 0.01% by weight or more, 0.03% by weight or more, or even 0.05% by weight or more. The monomer group may not contain a hydroxy group-containing monomer.
[0039] The monomer group may include a nitrogen atom-containing monomer. In this case, the (meth)acrylic polymer that may be included in the pressure-sensitive adhesive sheet 1 has a structural unit derived from the nitrogen atom-containing monomer. A nitrogen atom-containing monomer refers to a monomer having at least one nitrogen atom in the molecule (per molecule). In this specification, a monomer having a hydroxy group and a nitrogen atom in the molecule is classified as a nitrogen atom-containing monomer. A monomer having a carboxyl group and a nitrogen atom in the molecule is classified as a carboxyl group-containing monomer.
[0040] Preferred nitrogen atom-containing monomers are N-vinyl cyclic amides, (meth)acrylamides, etc. The nitrogen atom-containing monomers may be used alone or in combination of two or more.
[0041] The N-vinyl cyclic amide is preferably one represented by the following formula (A):
[0042] In formula (A), R 1 is a divalent organic group, preferably a divalent saturated or unsaturated hydrocarbon group, and more preferably a divalent saturated hydrocarbon group (e.g., an alkylene group having 3 to 5 carbon atoms). 1 are directly bonded via a single bond to form a ring structure.
[0043] The N-vinyl cyclic amide represented by formula (A) is preferably N-vinyl-2-pyrrolidone (NVP), N-vinyl-2-piperidone, N-vinyl-2-caprolactam, N-vinyl-3-morpholinone, N-vinyl-1,3-oxazin-2-one, N-vinyl-3,5-morpholinedione, or the like, more preferably N-vinyl-2-pyrrolidone or N-vinyl-2-caprolactam, and even more preferably N-vinyl-2-pyrrolidone.
[0044] Examples of (meth)acrylamides include (meth)acrylamide, N-alkyl(meth)acrylamide, N,N-dialkyl(meth)acrylamide, etc. Examples of N-alkyl(meth)acrylamides include N-ethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N-n-butyl(meth)acrylamide, N-octylacrylamide, etc. N-alkyl(meth)acrylamides also include (meth)acrylamides having an amino group, such as dimethylaminoethyl(meth)acrylamide, diethylaminoethyl(meth)acrylamide, and dimethylaminopropyl(meth)acrylamide.
[0045] Examples of N,N-dialkyl(meth)acrylamides include N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-dipropyl(meth)acrylamide, N,N-diisopropyl(meth)acrylamide, N,N-di(n-butyl)(meth)acrylamide, and N,N-di(t-butyl)(meth)acrylamide.
[0046] (Meth)acrylamides also include, for example, various N-hydroxyalkyl(meth)acrylamides, such as N-methylol(meth)acrylamide, N-(2-hydroxyethyl)(meth)acrylamide, N-(2-hydroxypropyl)(meth)acrylamide, N-(1-hydroxypropyl)(meth)acrylamide, N-(3-hydroxypropyl)(meth)acrylamide, N-(2-hydroxybutyl)(meth)acrylamide, N-(3-hydroxybutyl)(meth)acrylamide, N-(4-hydroxybutyl)(meth)acrylamide, and N-methyl-N-2-hydroxyethyl(meth)acrylamide.
[0047] (Meth)acrylamides also include, for example, various N-alkoxyalkyl(meth)acrylamides, such as N-methoxymethyl(meth)acrylamide and N-butoxymethyl(meth)acrylamide.
[0048] Examples of nitrogen atom-containing monomers other than N-vinyl cyclic amides and (meth)acrylamides include amino group-containing monomers such as aminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, dimethylaminopropyl (meth)acrylate, and t-butylaminoethyl (meth)acrylate; cyano group-containing monomers such as acrylonitrile and methacrylonitrile; (meth)acryloylmorpholine, N-vinylpiperazine, N-vinylpyrrole, N-vinylimidazole, N-vinylpyrazine, N-vinylmorpholine, N-vinylpyrazole, vinylpyridine, vinylpyrimidine, vinyloxazole, vinylisoxazole, vinylthiazole, vinylisothiazole, vinylpyridazine, (meth)acryloylpyrrolidone, (meth)acryloylpyrrolidine, (meth)acryloylpiperidine, N-methyl Examples of the monomer include heterocycle-containing monomers such as vinylpyrrolidone; maleimide-based monomers such as N-cyclohexylmaleimide, N-isopropylmaleimide, N-laurylmaleimide, and N-phenylmaleimide; itaconimide-based monomers such as N-methylitaconimide, N-ethylitaconimide, N-butylitaconimide, N-octylitaconimide, N-2-ethylhexylitaconimide, N-laurylitaconimide, and N-cyclohexylitaconimide; and imide group-containing monomers such as succinimide-based monomers such as N-(meth)acryloyloxymethylenesuccinimide, N-(meth)acryloyl-6-oxyhexamethylenesuccinimide, and N-(meth)acryloyl-8-oxyoctamethylenesuccinimide; and isocyanate group-containing monomers such as 2-(meth)acryloyloxyethylisocyanate.
[0049] The content of the nitrogen atom-containing monomer in the monomer group is, for example, 40% by weight or less, 35% by weight or less, or even 30% by weight or less. The lower limit of the content is, for example, 5% by weight or more, 7% by weight or more, or even 10% by weight or more. The monomer group may not contain a nitrogen atom-containing monomer.
[0050] The monomer group preferably includes a carboxyl group-containing monomer and / or a nitrogen atom-containing monomer, and more preferably includes both a carboxyl group-containing monomer and a nitrogen atom-containing monomer. When a nitrogen atom-containing monomer, particularly both a nitrogen atom-containing monomer and a carboxyl group-containing monomer, is present in a photopolymerization system, the molecular weight of the polymer tends to increase. This tendency may be due to the fact that the increased viscosity of the polymerization system caused by the formation of hydrogen bonds suppresses termination reactions between the growing ends of the polymer, making it easier for the monomer to remain at the end of the growing chain. The increased molecular weight of the polymer may contribute to an excellent balance between stress relaxation properties and cohesive strength in the pressure-sensitive adhesive sheet 1. Note that in thermosetting pressure-sensitive adhesive compositions, the monomers are dispersed in the solvent, making it difficult for hydrogen bonds to form and causing frequent chain transfer of radicals to the solvent, so the above-mentioned effect of the nitrogen atom-containing monomer is not observed.
[0051] In the photocurable composition, each of the above-mentioned monomers may be contained as a partial polymer. The partial polymer may be either a homopolymer or a copolymer. The photocurable composition may not contain a partial polymer.
[0052] The photocurable composition typically contains a photopolymerization initiator. An example of a photopolymerization initiator is a photoradical generator that generates radicals upon irradiation with light. The photopolymerization initiator has an absorption coefficient for light with a wavelength of 340 nm of, for example, 0.1 L / (g cm) or more, and may be 0.5 L / (g cm) or more, 1.0 L / (g cm) or more, 3.0 L / (g cm) or more, or even 5.0 L / (g cm) or more. The upper limit of this absorption coefficient is not particularly limited, and is, for example, 50 L / (g cm) or less. The absorption coefficient of the photopolymerization initiator is a calculated value from the absorbance of a 0.01 mg / mL methanol solution measured with a visible-ultraviolet spectrophotometer using a quartz cell with a 1 cm optical path length.
[0053] Examples of the photopolymerization initiator include benzoin ethers such as benzoin methyl ether, benzoin isopropyl ether, and benzil dimethyl ketal; substituted benzoin ethers such as anisole methyl ether; substituted acetophenones such as 2,2-diethoxyacetophenone and 2,2-dimethoxy-2-phenylacetophenone; α-hydroxyalkylphenones such as 1-hydroxycyclohexyl-phenyl ketone, 2-hydroxy-2-methylpropiophenone, 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone, and 2,2'-dihydroxy-2,2'-dimethyl-1,1'-[methylenebis(4,1-phenylene)]bis(propan-1-one); and substituted alpha alkyl phenones such as 2-methyl-2-hydroxypropiophenone. aromatic sulfonyl chlorides such as 2-naphthalenesulfonyl chloride; photoactive oximes such as 1-phenyl-1,1-propanedione-2-(o-ethoxycarbonyl)-oxime; benzophenone-based compounds such as benzophenone, benzoylbenzoic acid, methyl benzoylbenzoate, 4-phenylbenzophenone, hydroxybenzophenone, acrylated benzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, and 3,3',4,4'-tetra(t-butylperoxycarbonyl)benzophenone; thioxanthone-based compounds such as thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, isopropylthioxanthone, 2,4-diisopropylthioxanthone, and 2,4-diethylthioxanthone;2,4,6-trichloro-s-triazine, 2-phenyl-4,6-bis(trichloromethyl)-s-triazine, 2-(p-methoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(p-tolyl)-4,6-bis(trichloromethyl)-s-triazine, 2-piperonyl-4,6-bis(trichloromethyl)-s-triazine, 2,4-bis(trichloromethyl)-6-styryl-s-triazine, 2-(naphth-1-yl)-4,6-bis(trichloromethyl)-s-triazine, 2-(4-methoxy-naphth-1-yl)-4,6-bis(trichloromethyl)-s-triazine, 2,4-trichloromethyl-(piperonyl)-6-triazine, 2,4-trichloromethyl- Examples of suitable photopolymerizable compounds include triazine-based compounds such as (4'-methoxystyryl)-6-triazine; oxime ester-based compounds such as 1,2-octanedione, 1-[4-(phenylthio)-, 2-(O-benzoyloxime)], and O-(acetyl)-N-(1-phenyl-2-oxo-2-(4'-methoxy-naphthyl)ethylidene)hydroxylamine; phosphine-based compounds such as bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide and 2,4,6-trimethylbenzoyldiphenylphosphine oxide; quinone-based compounds such as 9,10-phenanthrenequinone, camphorquinone, and ethylanthraquinone; borate-based compounds; carbazole-based compounds; imidazole-based compounds; and titanocene-based compounds. The photocurable composition may contain one or more photopolymerization initiators. α-Hydroxyalkylphenones tend to have high absorption of light with a wavelength of 340±10 nm.
[0054] Another example of the photopolymerization initiator is a compound having a chemical structure shown in the following formula (1) (hereinafter referred to as chemical structure X) in the molecule.
[0055] R in the formula (1) 1 and R 2 are each independently a C1 to C8 alkyl group; —OH, a C1 to C4 alkoxy group, —CN, —COOR 51 , -OOCR 52 , or -NR 53 R 54a C1-C4 alkyl group in which a hydrogen atom is substituted by -; a C3-C6 alkenyl group; or -CH2-C6H4-R 55 It is. 1 and R 2 may be bonded to each other to form a C2 to C9 alkylene group, a C3 to C6 oxyalkylene group, or an azaalkylene group. 51 is a C1 to C8 alkyl group. 52 is a C1 to C4 alkyl group. 53 and R 54 are each independently a hydrogen atom, a C1 to C12 alkyl group; —OH, a C1 to C4 alkoxy group, —CN, or —COOR 59 a C2-C4 alkyl group in which a hydrogen atom is substituted with at least one group selected from the group consisting of: a C3-C5 alkenyl group; or a cyclohexyl group. 53 and R 54 are bonded to each other to form —O— or —N(R 60 )-Optionally, it may be a C3 to C9 alkylene group. 55 is a C1 to C4 alkyl group. 59 is a C1 to C4 alkyl group. 60 represents a hydrogen atom, a C1-C4 alkyl group, an allyl group, a C1-C4 hydroxyalkyl group, -CH2CH2-COOR 61 Or -CH2CH2CN. 61 is a C1 to C4 alkyl group.
[0056] X is -OR 56 , or -NR 57 R 58 It is. 56 is a hydrogen atom, -SiR 62 3. A C1 to C8 alkyl group or a C3 to C6 alkenyl group. 57 and R 58 represents a C1 to C12 alkyl group; —OH, a C1 to C4 alkoxy group, —CN, and —COOR 63a C2-C4 alkyl group in which a hydrogen atom is substituted with at least one group selected from the group consisting of: a C3-C5 alkenyl group; or a cyclohexyl group. 57 and R 58 are bonded to each other to form —O— or —N(R 64 )-Optionally, it may be a C3 to C9 alkylene group. 62 is a C1 to C6 alkyl group. 63 is a C1 to C4 alkyl group. 64 represents a hydrogen atom, a C1-C4 alkyl group, an allyl group, a C1-C4 hydroxyalkyl group, -CH2CH2-COOR 65 Or -CH2CH2CN. 65 is a C1 to C4 alkyl group.
[0057] The chemical structure X can be bonded to a hydrogen atom or a structure substituted with a hydrogen atom through the carbon atom indicated by * in formula (1).
[0058] The alkyl group, alkoxy group, alkenyl group, alkylene group, oxyalkylene group, azaalkylene group, and hydroxyalkyl group described in the explanation of formula (1) may be unbranched or branched. Furthermore, the expression "Cn1 to Cn2" (n1 and n2 are natural numbers) in this specification, including the explanation of formula (1), means that the number of carbon atoms is in the range of n1 to n2.
[0059] R 1 and R 2 may be, independently of each other, a C1 to C8 alkyl group, a C3 to C6 alkenyl group, or a C1 to C8 alkyl group. 1 and R 2 may be, independently of each other, a C1 to C4 alkyl group, a C1 to C3 alkyl group, or a C1 to C2 alkyl group. 1 and R 2 may be a methyl group.
[0060] R 1 and R 2 may be the same.
[0061] X is -OR 56 It may be R 56 may be a hydrogen atom or a C1 to C8 alkyl group, or may be a hydrogen atom. In other words, X may be —OH.
[0062] R 1 , R 2 and X may take any combination of the above preferred examples.
[0063] The chemical structure X may be a structure shown in the following formula (2): In the chemical structure X of formula (2), when a substitution structure of a hydrogen atom is bonded to the carbon atom indicated by *, the substitution structure and —COCR in formula (2) 1 XR 2 The group is in a para-position relationship with respect to the benzene ring of the chemical structure X.
[0064] The photopolymerization initiator may be a compound having two or more chemical structures X in one molecule.
[0065] The photopolymerization initiator may be a compound represented by the following formula (3). The compound of formula (3) has two chemical structures X in one molecule. The two chemical structures X are located at both ends of the photopolymerization initiator molecule. More specifically, the two chemical structures X are bonded to each other via -A- at the carbon atom of the phenylene group represented by * above.
[0066] R in formula (3) 1 ' and R 2 ' are mutually exclusive and R 1 and R 2 Independently of 1 and R 2 R 1 ' and / or R 2 ' is R 1 and / or R 2 may be the same as R 1 , R 2 , R 1 ' and R 2 ' may all be the same.
[0067] X' in formula (3) is a group that can be taken as X, independently of X in formula (1). X' and X may be the same.
[0068] A is -O-, -CYR 3 - or -C(CH3)R 4 is.
[0069] Y is a hydrogen atom, —Cl, —Br, or —O—R 71 , -NR 72 R 73 , or -S-R 74 It is. 3 represents a hydrogen atom, a C1-C8 alkyl group, a C3-C6 alkenyl group, a benzyl group, -CH2-C6H4-R 75 or a phenyl group. 4 is a C1-C6 alkyl or alkylene group, and this alkylene group is bonded to a carbon atom of the phenylene group of the compound of formula (3).
[0070] R 71 is a hydrogen atom, -Si(R 76 ) 3, C1 to C12 alkyl group, C2 to C18 acyl group, —CO—NH—R 77 , a C2 to C20 hydroxyalkyl group, a C2 to C20 methoxyalkyl group, 3-R 78 -2-hydroxypropyl group, 3-[1,3,3,3-tetramethyl-1-[(trimethylsilyl)oxy]disiloxanyl]propyl group, 2,3-dihydroxypropyl group, or a C2 to C21 hydroxyalkyl group or a C3 to C25 alkyl group in which the carbon chain is interrupted by 1 to 9 oxygen atoms. 72 and R 73 are each independently a C1 to C12 alkyl group; —OH, a C1 to C4 alkoxy group, —CN, and —COOR 79 a C2-C4 alkyl group in which a hydrogen atom is substituted with at least one group selected from the group consisting of: a C3-C5 alkenyl group; a cyclohexyl group; or a C7-C9 phenylalkyl group. 72 and R 73 are bonded to each other to form —O— or —N(R 80)-Optionally, it may be a C3 to C9 alkylene group. 74 represents a C1 to C18 alkyl group, a hydroxyethyl group, a 2,3-dihydroxypropyl group, a cyclohexyl group, a benzyl group, a phenyl group, a C1 to C12 alkylphenyl group, -CH2-COOR 81 -CH2CH2-COOR 82 , or —CH(CH3)—COOR 83 It is. 75 is a C1 to C4 alkyl group. 76 is a C1 to C6 alkyl group. 77 is a C1 to C12 alkyl group. 78 is a C1 to C18 alkoxy group. 79 is a C1 to C4 alkyl group. 80 represents a hydrogen atom, a C1-C4 alkyl group, an allyl group, a benzyl group, a C1-C4 hydroxyalkyl group, -CH2CH2-COOR 84 , or —CH2CH2CN. 81 , R 82 and R 83 are each independently a C1 to C18 alkyl group. 84 is a C1 to C4 alkyl group.
[0071] The alkyl group, alkenyl group, acyl group, hydroxyalkyl group, methoxyalkyl group, alkoxy group, alkyl moiety in a phenylalkyl group, and alkylene group described in the explanation of formula (3) may all be unbranched or branched.
[0072] R in formula (3) 1 , R 2 , R 1 ' and R 2 Preferred examples of R ′ are those described above in the explanation of formula (1). 1 and R 2 The preferred examples of X′ in formula (3) are the same as the preferred examples of X described above in the explanation of formula (1). A is —CYR 3 -. Y may be a hydrogen atom. R 3may be a hydrogen atom. 3 - and Y and R 3 and may both be hydrogen atoms. In other words, A may be —CH—.
[0073] R in formula (3) 1 , R 2 , R 1 ', R 2 ', X, X', and A may take any combination of the preferred examples above.
[0074] The photopolymerization initiator may be a compound represented by the following formula (4): The compound of formula (4) is a type of compound of formula (3).
[0075] Specific examples of photopolymerization initiators are shown in the following formulas (5) to (9). The photopolymerization initiator may be a compound represented by at least one formula selected from the group consisting of formulas (5) to (9), a compound represented by at least one formula selected from the group consisting of formulas (5) to (8), a compound represented by at least one formula selected from the group consisting of formulas (5) to (7), or a compound represented by formula (5). The compound of formula (8) is derived from a vinyl compound having chemical structure X in its side chain. More specifically, it is an oligomer of the vinyl compound.
[0076]
[0077]
[0078]
[0079]
[0080]
[0081] The photopolymerization initiators represented by formulas (5) to (9) are commercially available as Omnirad 127, Esacure KIP 160, Esacure one, Esacure KIP 150, and Omnirad 1173 (all manufactured by IGM Resins). The photopolymerization initiator may be at least one selected from these groups.
[0082] Specific examples of the photopolymerization initiator include 1-hydroxycyclohexyl-phenyl ketone, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, and 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)2-methylpropan-1-one. Of these, 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)2-methylpropan-1-one is preferred. Each of the above photopolymerization initiators is commercially available as Omnirad 184, Omnirad 819, and Omnirad 127, respectively (all manufactured by IGM Resin).
[0083] The amount of the photopolymerization initiator in the photocurable composition is, for example, 20 parts by weight or less, and may be 10 parts by weight or less, 5.0 parts by weight or less, 3.0 parts by weight or less, 1.0 parts by weight or less, 0.5 parts by weight or less, 0.3 parts by weight or less, 0.25 parts by weight or less, 0.2 parts by weight or less, 0.15 parts by weight or less, 0.1 parts by weight or less, or even 0.05 parts by weight or less, relative to 100 parts by weight of the total of the monomer group and partial polymers thereof. The lower limit of the amount is, for example, 0.01 parts by weight or more, and may be 0.03 parts by weight or more, relative to 100 parts by weight of the total of the monomer group and partial polymers thereof.
[0084] The photocurable composition may contain a crosslinking agent. An example of the crosslinking agent is a polyfunctional monomer having two or more polymerizable functional groups in one molecule. The polyfunctional monomer may be a (meth)acrylic monomer. Examples of the polyfunctional monomer are a monomer having two or more C=C bonds in one molecule, and a monomer having one or more C=C bonds and one or more polymerizable functional groups such as epoxy groups, aziridine groups, oxazoline groups, hydrazine groups, methylol groups, etc. in one molecule. The polyfunctional monomer is preferably a monomer having two or more C=C bonds in one molecule.
[0085] Examples of the polyfunctional monomer include (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,2-ethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol diacrylate (N Polyfunctional acrylates (e.g., ester compounds of polyhydric alcohols and (meth)acrylic acid) such as 1,12-dodecanediol di(meth)acrylate, 1,12-dodecanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, and tetramethylolmethane tri(meth)acrylate; allyl (meth)acrylate, vinyl (meth)acrylate, divinylbenzene, epoxy acrylate, polyester acrylate, urethane acrylate, butyl di(meth)acrylate, and hexyl di(meth)acrylate. The polyfunctional monomer is preferably a polyfunctional acrylate, and more preferably 1,9-nonanediol diacrylate, trimethylolpropane tri(meth)acrylate, hexanediol di(meth)acrylate, or dipentaerythritol hexa(meth)acrylate.
[0086] The amount of crosslinking agent to be added varies depending on the molecular weight, the number of functional groups, etc., but may be, for example, 5 parts by weight or less, 3 parts by weight or less, 2 parts by weight or less, 1 part by weight or less, 0.5 parts by weight or less, 0.3 parts by weight or less, 0.2 parts by weight or less, 0.15 parts by weight or less, 0.1 parts by weight or less, or even 0.05 parts by weight or less, relative to 100 parts by weight of the total of the monomer group and its partial polymer. The lower limit of the amount to be added may be, for example, 0.01 parts by weight or more, 0.03 parts by weight or more, or even 0.05 parts by weight or more. The photocurable composition may not contain a crosslinking agent.
[0087] The photocurable composition may contain additives other than those described above. Examples of the additives include a chain transfer agent, a silane coupling agent, a viscosity modifier, a tackifier, a plasticizer, a softener, an antioxidant, a filler, a colorant, an antioxidant, a surfactant, an antistatic agent, and an ultraviolet absorber. The photocurable composition may not contain any additives.
[0088] Examples of the silane coupling agent include epoxy group-containing silane coupling agents such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; amino group-containing silane coupling agents such as 3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-triethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, and N-phenyl-γ-aminopropyltrimethoxysilane; (meth)acrylic group-containing silane coupling agents such as 3-acryloxypropyltrimethoxysilane and 3-methacryloxypropyltriethoxysilane; and isocyanate group-containing silane coupling agents such as 3-isocyanatepropyltriethoxysilane.
[0089] The silane coupling agent may be an oligomeric silane coupling agent. Oligomeric silane coupling agents typically have multiple alkoxysilyl groups in one molecule. Specific examples of oligomeric silane coupling agents are those manufactured by Shin-Etsu Silicones Co., Ltd. under the trade names "X-41-1053," "X-41-1056," "X-41-1059A," "X-41-1805," "X-41-1810," "X-41-1818," "X-40-2651," and "X-24-9591F." The oligomeric silane coupling agent may have a reactive functional group. Examples of the reactive functional group are an epoxy group, a mercapto group, an acid anhydride group, and an amino group. Of these, those having an epoxy group are preferred, and those having multiple epoxy groups in one molecule are more preferred. Examples of oligomeric silane coupling agents having an epoxy group are the above-mentioned "X-41-1053," "X-41-1056," and "X-41-1059A." Examples of oligomeric silane coupling agents having a mercapto group are the above-mentioned "X-41-1805," "X-41-1810," and "X-41-1818." An example of an oligomeric silane coupling agent having an acid anhydride group is the above-mentioned "X-24-9591F." An example of an oligomeric silane coupling agent having an amino group is the above-mentioned "X-40-2651."
[0090] The silane coupling agent may be an acetoacetyl group-containing silane coupling agent (for example, product name "A-100" manufactured by Soken Chemical & Engineering Co., Ltd.).
[0091] When the photocurable composition contains a silane coupling agent, the amount thereof is, for example, 5 parts by weight or less, and may be 3 parts by weight or less, 1 part by weight or less, 0.5 parts by weight or less, 0.2 parts by weight or less, 0.1 parts by weight or less, or even 0.05 parts by weight or less, relative to 100 parts by weight of the total of the monomer group and its partial polymer. The photocurable composition does not have to contain a silane coupling agent.
[0092] The viscosity of the photocurable composition is preferably 5 to 100 poise. A photocurable composition having a viscosity in the above range is particularly suitable for forming the pressure-sensitive adhesive sheet 1.
[0093] The solvent content in the photocurable composition may be, for example, 5 wt% or less, 4 wt% or less, 3 wt% or less, 2 wt% or less, 1 wt% or less, or even 0.5 wt% or less. The photocurable composition may be substantially free of solvent. "Substantially free of solvent" means that solvents derived from additives and the like are allowed at a content of, for example, 0.1 wt% or less, preferably 0.05 wt% or less, and more preferably 0.01 wt% or less. The solvent content in the pressure-sensitive adhesive sheet 1 may be within the above range. The pressure-sensitive adhesive sheet 1 may be substantially free of solvent.
[0094] (Method of manufacturing pressure-sensitive adhesive sheet) The pressure-sensitive adhesive sheet 1 can be formed, for example, by irradiating light 24 onto a first laminate 20 comprising, in this order, a base sheet 21, a coating layer 22 containing a photocurable composition, and a release liner 23 (see FIG. 2 ). The coating layer 22 is irradiated with light 24 and cured to form the pressure-sensitive adhesive sheet 1. Irradiation with light 24 is typically carried out from the side of the base sheet 21. In this case, the light 24 passes through the base sheet 21 and reaches the coating layer 22, curing the coating layer 22. However, irradiation with light 24 may also be carried out from the side of the release liner 23, or from both the side of the release liner 23 and the side of the base sheet 21.
[0095] The formed pressure-sensitive adhesive sheet 1 is sandwiched between the base sheet 21 and the release liner 23 until the release liner 23 is peeled off, and constitutes part of the second laminate 27. By peeling the release liner 23 from the second laminate 27, a third laminate 25 including the base sheet 21 and the pressure-sensitive adhesive sheet 1 is obtained. In the third laminate 25, the surface of the pressure-sensitive adhesive sheet 1 is exposed to the outside. An optical film can be laminated onto the exposed surface of the pressure-sensitive adhesive sheet 1 directly or via another layer.
[0096] The light 24 is, for example, visible light or ultraviolet light having a wavelength shorter than 450 nm. The light may include light having a wavelength in the same range as the absorption wavelength of the photopolymerization initiator contained in the photocurable composition. Light having a wavelength of 300 nm or less may be irradiated by filtering out short-wavelength light using a filter or the like. Filtering out short-wavelength light is suitable for suppressing deterioration of the base sheet 21 and / or the release liner 23 due to the light 24. The light source 28 of the light 24 is, for example, a light irradiation device equipped with an ultraviolet irradiation lamp. Examples of ultraviolet irradiation lamps include ultraviolet LEDs, low-pressure mercury lamps, medium-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, xenon lamps, microwave-excited mercury lamps, black light lamps, chemical lamps, germicidal lamps, low-pressure discharge mercury lamps, and excimer lasers. Two or more ultraviolet irradiation lamps may be combined. The ultraviolet LED allows the irradiated ultraviolet light band to be narrower than when other light sources are used.
[0097] The light source 28 may be an LED. Compared to black light sources, LEDs not only allow for easier adjustment of illuminance, but also tend to have a longer light source life. Compared to black light sources that use mercury, LEDs are also superior in terms of reducing environmental impact. When using an ultraviolet LED as the light source, an LED with a peak wavelength of 325 to 350 nm may be selected. According to the inventors' studies, the use of an LED with a peak wavelength of 325 to 350 nm may contribute to at least one of improving the polymerization rate of the monomer group in the pressure-sensitive adhesive sheet 1, improving the molecular weight of the polymer, and reducing the amount of residual photopolymerization initiator, compared to, for example, using a black light source. Furthermore, LEDs that emit light 14 with a peak wavelength of 325 to 350 nm tend to generate less heat and make it easier to control the temperature of the coating layer 22, compared to LEDs that emit light with a peak wavelength of approximately 365 nm. To the inventors' knowledge, no examples of pressure-sensitive adhesive sheets being produced using LEDs that emit light with a peak wavelength of 325 to 350 nm have been reported.
[0098] As the LED having a peak wavelength in the range of 325 to 350 nm, an LED having a peak wavelength of 340±10 nm (hereinafter referred to as LED 340) may be selected.
[0099] Focusing on the peak wavelength of the light 24, the peak wavelength of the light 24 irradiated onto the first laminate 20 (specifically, the coating layer 22) may be 325 nm to 350 nm. The peak wavelength of the light 24 is preferably 340±10 nm (330 nm to 350 nm), may be 340±5 nm (335 nm to 345 nm), may be 340±2 nm (338 nm to 342 nm), or may be 340 nm. The peak wavelength refers to the wavelength at which the intensity reaches a maximum value in the spectrum showing the relationship between the wavelength and intensity of the light 24. The light 24 may further have a peak wavelength in a wavelength range other than 325 nm to 350 nm, but preferably does not have such a peak wavelength.
[0100] The illuminance of the light 24 irradiated onto the first laminate 20 (specifically, the coating layer 22) is, for example, 2.0 to 30 mW / cm 2 The illuminance is 2.5 mW / cm 2 Above, 3.0mW / cm 2 Above, 3.5mW / cm 2 Above, 4.0mW / cm 2 Above, 5.0mW / cm 2 Above, 6.0mW / cm 2 Above, 7.0mW / cm 2 Above, 8.0mW / cm 2 Above, 9.0mW / cm 2 or more, and even 10 mW / cm 2 The upper limit of the illuminance may be, for example, 25 mW / cm 2 less than 20 mW / cm 2 Below 15mW / cm 2 It may be the following:
[0101] The time for irradiating the first laminate 20 (specifically, the coating layer 22) with the light 24 is, for example, 10 to 1,000 seconds, and may be 60 seconds or more, 100 seconds or more, 150 seconds or more, 200 seconds or more, 250 seconds or more, or even 300 seconds or more. The upper limit of the time is, for example, 800 seconds or less, and may be 600 seconds or less, 500 seconds or less, 400 seconds or less, 350 seconds or less, 300 seconds or less, or even 250 seconds or less. The irradiation with the light 24 may be continuous or intermittent.
[0102] The integrated light amount of the light 24 on the first laminate 20 (specifically, the coating layer 22) is, for example, 25 mJ / cm 2 or more, and 100 mJ / cm 2 Above, 250mJ / cm 2 Above, 500mJ / cm 2 Above, 750mJ / cm 2 Above, 850mJ / cm 2 Above, 1000mJ / cm 2 Above, 1250mJ / cm 2 or more, and even 1500 mJ / cm 2 The upper limit of the integrated light amount is not particularly limited, and may be, for example, 5000 mJ / cm 2 or less, and 2 Below, 3000mJ / cm 2 Below, 2500mJ / cm 2 Below, 2000mJ / cm 2 Below, 1750 mJ / cm 2 It may be the following:
[0103] An example of the substrate of the release liner 23 (hereinafter referred to as "liner substrate") is a resin film. Examples of resins that can be contained in the liner substrate include polyesters such as polyethylene terephthalate and polyethylene naphthalate, acetate resins, polyethersulfone, polycarbonate, polyamide, polyimide, polyolefin, (meth)acrylic resins, polyvinyl chloride, polyvinylidene chloride, polystyrene, polyvinyl alcohol, polyarylate, and polyphenylene sulfide. The resin is preferably a polyester such as polyethylene terephthalate.
[0104] The release liner 23 may include a layer other than the liner substrate. The release liner 23 may include a release layer. The release liner 23 includes, for example, a liner substrate and a release layer formed on one surface of the liner substrate. This release liner 23 can be used such that the release layer faces the coating layer 22. The release layer is typically a cured layer of a release agent composition containing a release agent. Various release agents can be used as the release agent, such as silicone-based release agents, fluorine-based release agents, long-chain alkyl-based release agents, fatty acid amide-based release agents, and silica powder.
[0105] The release liner 23 may be in the form of a sheet or a continuous piece.
[0106] An example of the base sheet 21 is a resin film. Examples of the resin contained in the base sheet 21 are the same as the examples of the resin that can be contained in the liner base material.
[0107] The thickness of the base sheet 21 is, for example, 10 to 200 μm, and may be 25 to 150 μm.
[0108] The base sheet 21 may have a release layer on the surface facing the coating layer 22. Examples of the release layer that may be provided on the base sheet 21 are the same as the examples of the release layer that may be provided on the release liner 23. Both the release liner 23 and the base sheet 21 may have a release layer.
[0109] For the base sheet 21 , a sheet having a greater peel strength from the pressure-sensitive adhesive sheet 1 than the release liner 23 can usually be selected.
[0110] The base sheet 21 may be in the form of a sheet or a continuous sheet.
[0111] The first laminate 20 can be formed, for example, by forming a coating layer 22 on a base sheet 21 (or a release liner 23) and then placing the release liner 23 (or base sheet 21) on the formed coating layer 22. Alternatively, the first laminate 20 may be formed by applying the photocurable composition in a poured manner into the space between the base sheet 21 and the release liner 23, which are held at a predetermined distance so that their main surfaces face each other.
[0112] The coating layer 22 can be formed by various coating methods such as roll coating, kiss roll coating, gravure coating, reverse coating, roll brush, spray coating, dip roll coating, bar coating, knife coating, air knife coating, curtain coating, lip coating, and die coating.
[0113] The thickness of the coating layer 22 can be adjusted depending on the desired thickness of the pressure-sensitive adhesive sheet 1, and may be, for example, 5 to 100 μm, 5 to 50 μm, 5 to 25 μm, or even 5 to 20 μm.
[0114] The first laminate 20 may include a long base sheet 21, a long coating layer 22, and a long release liner 23, in other words, may be long. The long first laminate 20 can be obtained, for example, by forming the coating layer 22 between the base sheet 21 and the release liner 23 while conveying them after they have been unwound from a roll.
[0115] The Mw of the polymer contained in the pressure-sensitive adhesive sheet 1 is, for example, 500,000 or more, 550,000 or more, 600,000 or more, 650,000 or more, 700,000 or more, more than 700,000, 750,000 or more, 800,000 or more, 850,000 or more, 900,000 or more, 950,000 or more, 1,000,000 or more, 1,100,000 or more, 1,200,000 or more, 1,300,000 or more, or even 1,400,000 or more. The upper limit of Mw is not particularly limited, and is, for example, 3,000,000 or less. The Mw of the polymer and the Mw of the sol component B are measured by GPC (gel permeation chromatography) and determined from values calculated in polystyrene equivalent.
[0116] The Mw of the sol component B contained in the pressure-sensitive adhesive sheet 1 is, for example, 300,000 or more, and may be 350,000 or more, 400,000 or more, 450,000 or more, 500,000 or more, 550,000 or more, 600,000 or more, 650,000 or more, 700,000 or more, 750,000 or more, 800,000 or more, 850,000 or more, 900,000 or more, 950,000 or more, or even 1,000,000 or more. The upper limit of Mw is not particularly limited, and is, for example, 3,000,000 or less.
[0117] In the pressure-sensitive adhesive sheet 1, (I) the Mw of the polymer may be 700,000 or more but less than 800,000, and the Mw of the sol component B may be 600,000 or more. In the pressure-sensitive adhesive sheet 1, (II) the Mw of the polymer may be 800,000 or more, and the Mw of the sol component B may be 450,000 or more. A pressure-sensitive adhesive sheet 1 that satisfies the condition (I) or (II) is particularly suitable for suppressing peeling of the pressure-sensitive adhesive sheet 1 from an adherend at high temperatures. The adherend is, for example, a glass substrate.
[0118] The thickness of the pressure-sensitive adhesive sheet 1 is, for example, 2 to 70 μm. The thickness may be 50 μm or less, 40 μm or less, 30 μm or less, 25 μm or less, or even 20 μm or less. The lower limit of the thickness may be 5 μm or more, 10 μm or more, or even 15 μm or more. Even when the thickness of the pressure-sensitive adhesive sheet 1 is, for example, 30 μm or less, it is suitable for suppressing foaming and peeling from the adherend in a high-temperature environment.
[0119] <Optical Film> Examples of the optical film 2 include a polarizing film, a retardation film, and a laminate film including a polarizing film and / or a retardation film. However, the optical film 2 is not limited to the above examples. The optical film 2 may also include a glass film.
[0120] The optical film 2 may be a polarizing film, and the pressure-sensitive adhesive sheet 1 may be in contact with the polarizing film. Among optical films, polarizing films tend to undergo large dimensional changes due to heat. Dimensional changes in the polarizing film can cause peeling from the pressure-sensitive adhesive film. For this reason, the present invention is particularly advantageous when the optical laminate further includes a polarizing film.
[0121] The polarizing film includes a polarizer. The polarizing film typically includes a polarizer and a protective film (transparent protective film). The protective film is disposed, for example, in contact with a main surface (the surface having the largest area) of the polarizer. The polarizer may be disposed between two protective films. The protective film may be disposed on at least one surface of the polarizer.
[0122] The polarizer is not particularly limited, and examples thereof include a hydrophilic polymer film such as a polyvinyl alcohol film, a partially formalized polyvinyl alcohol film, or an ethylene-vinyl acetate copolymer partially saponified film, which has been uniaxially stretched after adsorbing a dichroic substance such as iodine or a dichroic dye; a polyene-based oriented film such as a dehydrated polyvinyl alcohol or a dehydrochlorinated polyvinyl chloride; etc. A polarizer typically comprises a polyvinyl alcohol film (polyvinyl alcohol films include an ethylene-vinyl acetate copolymer partially saponified film) and a dichroic substance such as iodine.
[0123] The thickness of the polarizer is not particularly limited and may be, for example, 80 μm or less, 50 μm or less, 30 μm or less, 25 μm or less, or even 20 μm or less. The lower limit of the polarizer thickness is not particularly limited and may be, for example, 1 μm or more, 5 μm or more, 10 μm or more, or even 15 μm or more. A thin polarizer (for example, a thickness of 20 μm or less) is suppressed in dimensional change and can contribute to improving the durability of the optical laminate, particularly durability at high temperatures.
[0124] The material for the protective film may be, for example, a thermoplastic resin having excellent transparency, mechanical strength, thermal stability, moisture-blocking properties, isotropy, etc. Specific examples of such thermoplastic resins include cellulose resins such as triacetyl cellulose, polyester resins, polyethersulfone resins, polysulfone resins, polycarbonate resins, polyamide resins, polyimide resins, polyolefin resins, (meth)acrylic resins, cyclic polyolefin resins (norbornene-based resins), polyarylate resins, polystyrene resins, polyvinyl alcohol resins, and mixtures thereof. The material for the protective film may be a thermosetting resin or an ultraviolet-curable resin such as a (meth)acrylic, urethane, acrylic urethane, epoxy, or silicone-based resin. When the polarizing film has two protective films, the materials of the two protective films may be the same or different. For example, a protective film made of a thermoplastic resin may be bonded to one main surface of the polarizer via an adhesive, and a protective film made of a thermosetting resin or an ultraviolet-curable resin may be bonded to the other main surface of the polarizer. The protective film may contain one or more optional additives, such as ultraviolet absorbers, antioxidants, lubricants, plasticizers, release agents, color inhibitors, flame retardants, nucleating agents, antistatic agents, pigments, and colorants.
[0125] The thickness of the protective film can be determined as appropriate, but is generally about 5 to 200 μm in view of strength, workability such as handling, thinness, and the like.
[0126] The polarizer and the protective film are usually adhered to each other via an aqueous adhesive or the like. Examples of aqueous adhesives include isocyanate-based adhesives, polyvinyl alcohol-based adhesives, gelatin-based adhesives, vinyl latex, aqueous polyurethane, and aqueous polyester. Examples of adhesives other than the above-mentioned adhesives include ultraviolet-curable adhesives and electron beam-curable adhesives. Electron beam-curable polarizing film adhesives exhibit suitable adhesiveness to various protective films. The adhesive may contain a metal compound filler.
[0127] In the polarizing film, a retardation film or the like can be formed on the polarizer instead of the protective film. Another protective film or a retardation film or the like can be further provided on the protective film.
[0128] The protective film may have a hard coat layer on the surface opposite to the surface bonded to the polarizer, and may also be subjected to treatments for purposes such as anti-reflection, anti-sticking, diffusion, and anti-glare.
[0129] The polarizing film may be a circular polarizing film.
[0130] The thickness of the polarizing film is, for example, 500 μm or less, and may be 300 μm or less, 200 μm or less, 100 μm or less, or even 60 μm or less. The lower limit of the thickness may be, for example, 10 μm or more, 25 μm or more, or even 40 μm or more.
[0131] The retardation film is a film having birefringence in the in-plane direction and / or the thickness direction, and is, for example, a stretched resin film or a film in which a liquid crystal material is oriented and fixed.
[0132] The retardation film may be a λ / 4 plate, a λ / 2 plate, an anti-reflection retardation film (see, for example, paragraphs 0221, 0222, and 0228 of JP 2012-133303 A), a viewing angle compensation retardation film (see, for example, paragraphs 0225 and 0226 of JP 2012-133303 A), or an inclined orientation retardation film for viewing angle compensation (see, for example, paragraph 0227 of JP 2012-133303 A). The retardation film is not limited to the above examples as long as it has birefringence in the in-plane direction and / or the thickness direction. There are also no limitations on the retardation value, arrangement angle, three-dimensional birefringence, whether the retardation film is single-layer or multi-layer, etc. of the retardation film. Known films can be used as the retardation film.
[0133] The thickness of the optical film 2 is, for example, 1 to 200 μm.
[0134] The optical film 2 may be a single layer or a laminated film composed of two or more layers. When the optical film 2 is a laminated film, the pressure-sensitive adhesive sheet 1 may be used to bond the layers together.
[0135] The pressure-sensitive adhesive sheet-attached optical film 11 may include layers other than the pressure-sensitive adhesive sheet 1 and the optical film 2. Although other layers may be disposed between the pressure-sensitive adhesive sheet 1 and the optical film 2, it is preferable that the pressure-sensitive adhesive sheet 1 and the optical film 2 are in contact with each other.
[0136] The pressure-sensitive adhesive sheet-attached optical film 11 can be used in, for example, an optical laminate or an image display device, but the uses of the pressure-sensitive adhesive sheet-attached optical film 11 are not limited to the above examples.
[0137] [Optical laminate] An example of an optical laminate of this embodiment is shown in Figure 3. The optical laminate 30A in Figure 3 comprises the optical film 11 with a pressure-sensitive adhesive sheet of this embodiment. The optical laminate 30A has a layered structure in which a release liner 3, a pressure-sensitive adhesive sheet 1, and an optical film 2 are layered in this order. By peeling off the release liner 3, the optical laminate 30A can be used as the optical film 11 with a pressure-sensitive adhesive sheet.
[0138] The release liner 3 is typically a resin film. Examples of resins that make up the release liner 3 include polyesters such as polyethylene terephthalate (PET), polyolefins such as polyethylene and polypropylene, polycarbonate, acrylic, polystyrene, polyamide, and polyimide. The surface of the release liner 3 that comes into contact with the pressure-sensitive adhesive sheet 1 may be subjected to a release treatment. The release treatment is, for example, a treatment with a silicone compound. However, the release liner 3 is not limited to the above examples. The release liner 3 is peeled off when the optical laminate 30A is used, for example, when it is attached to the image forming layer.
[0139] Another example of the optical laminate of the present embodiment is shown in Figure 4. The optical laminate 30B in Figure 4 includes the pressure-sensitive adhesive sheet-attached optical film 11 of the present embodiment. The optical laminate 30B has a layered structure in which a release liner 3, a pressure-sensitive adhesive sheet 4, a retardation film 2B, a pressure-sensitive adhesive sheet 1, and a polarizing film 2A are layered in this order. After the release liner 3 is peeled off, the optical laminate 30B can be used by being attached to, for example, an image-forming layer.
[0140] A known adhesive sheet can be used as the adhesive sheet 4. The adhesive sheet 1 may also be used as the adhesive sheet 4.
[0141] Another example of the optical laminate of this embodiment is shown in Figure 5. Optical laminate 30C in Figure 5 includes an optical film 11 with a pressure-sensitive adhesive sheet of this embodiment. Optical laminate 30C has a layered structure in which a release liner 3, a pressure-sensitive adhesive sheet 4, a retardation film 2B, a pressure-sensitive adhesive sheet 1, a polarizing film 2A, and a protective film 5 are layered in this order. After peeling off the release liner 3, optical laminate 30C can be used by being attached to, for example, an image-forming layer.
[0142] The protective film 5 has the function of protecting the optical film 2 (polarizing film 2A), which is the outermost layer, during distribution and storage of the optical laminate 30C and when the optical laminate 30C is incorporated into an image display device. The protective film 5 may also function as a window to the external space when incorporated into an image display device. The protective film 5 is typically a resin film. Examples of resins constituting the protective film 5 include polyesters such as PET, polyolefins such as polyethylene and polypropylene, acrylics, cycloolefins, polyimides, and polyamides, with polyesters being preferred. However, the protective film 5 is not limited to the above examples. The protective film 5 may be a glass film or a laminate film including a glass film. The protective film 5 may be subjected to surface treatments such as anti-glare, anti-reflection, and anti-static.
[0143] The protective film 5 may be bonded to the optical film 2 by any adhesive. Bonding by an adhesive sheet 1 is also possible.
[0144] The optical laminate of this embodiment may include any layer other than the above-mentioned layers. The optical laminate of this embodiment may have any configuration as long as it includes the pressure-sensitive adhesive sheet-attached optical film 11.
[0145] The optical laminate of this embodiment can be distributed and stored, for example, as a rolled body obtained by rolling up a strip-shaped optical laminate, or as a sheet-shaped optical laminate.
[0146] The optical laminate of this embodiment is typically used in an image display device, such as a liquid crystal display, an organic EL display, or an inorganic EL display.
[0147] [Image display device] An example of an image display device of this embodiment is shown in Figure 6. The image display device 31 of Figure 6 has a layered structure in which a substrate 7, an image forming layer (e.g., an organic EL layer or a liquid crystal layer) 6, a pressure-sensitive adhesive sheet 4, a retardation film 2B, a pressure-sensitive adhesive sheet 1, a polarizing film 2A, and a protective film 5 are layered in this order. The image display device 31 includes the pressure-sensitive adhesive sheet-attached optical film 11 of Figure 1 and the optical laminates 30A, 30B, and 30C of Figures 3 to 5 (excluding the release liner 3). The substrate 7 and the image forming layer 6 may have the same configurations as the substrate and the image forming layer, respectively, of known image display devices.
[0148] The image display device 31 in Fig. 6 may be an organic EL display or a liquid crystal display. However, the image display device 31 is not limited to this example. The image display device 31 may be an electroluminescence (EL) display, a plasma display (PD), a field emission display (FED), or the like. The image display device 31 may be used for home appliances, in-vehicle applications, public information displays (PID), and the like.
[0149] The image display device 31 may have any configuration as long as it includes the pressure-sensitive adhesive sheet-attached optical film 11 and / or the optical laminate of this embodiment.
[0150] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the examples shown below.
[0151] [Preparation of Photocurable Composition] (Monomer Syrup A1) 95.1 parts by weight of n-butyl acrylate (BA), 0.1 parts by weight of 4-hydroxybutyl acrylate (HBA), 4.8 parts by weight of acrylic acid (AA), and 0.05 parts by weight of Omnirad 184 (manufactured by IGM Resin) as a photopolymerization initiator were placed in a four-neck flask. Next, the liquid in the flask was irradiated with ultraviolet light under a nitrogen atmosphere to partially photopolymerize the monomers, yielding Monomer Syrup A1. UV irradiation was continued until the viscosity of the liquid in the flask reached 20 Pa s (measurement conditions: BH viscometer No. 5 rotor, 10 rpm, measurement temperature 30°C).
[0152] (Monomer Syrups A2 to A6) Monomer syrups A2 to A6 were prepared in the same manner as for monomer syrup A1, except that the monomers and photopolymerization initiators were changed as shown in Table 1.
[0153]
[0154] The abbreviations in Table 1 are as follows: BA: n-butyl acrylate HBA: 4-hydroxybutyl acrylate AA: acrylic acid Omnirad 184: 1-hydroxycyclohexyl-phenyl ketone (Omnirad 184, manufactured by IGM Resins) Omnirad 819: bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (Omnirad 819, manufactured by IGM Resins) Omnirad 127: 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)2-methylpropan-1-one (Omnirad 127, manufactured by IGM Resins)
[0155] (Photocurable Compositions C1 to C29) Next, the monomer syrup, the monomer, the crosslinking agent, and the silane coupling agent were mixed so as to have the compositions shown in Table 2 below, to obtain photocurable compositions C1 to C29.
[0156]
[0157] The abbreviations in Table 2 are as follows: AA: Acrylic acid NVP: N-vinyl-2-pyrrolidone NDDA: 1,9-nonanediol diacrylate KBM403: 3-glycidoxypropyltrimethoxysilane (manufactured by Shin-Etsu Silicones Co., Ltd., trade name "KBM-403") X-41-1056: Epoxy group-containing oligomer type silane coupling agent (manufactured by Shin-Etsu Silicones Co., Ltd., trade name "X-41-1056")
[0158] The final composition of the monomers contained in each photocurable composition is shown in Table 3 below.
[0159]
[0160] [Preparation of Pressure-Sensitive Adhesive Sheet] Example 1 (Preparation of Release Liner) A silicone-based release agent composition was obtained by mixing 30 parts by weight of an addition reaction curable silicone (LTC761 containing a hexenyl group-containing polyorganosiloxane, a 30 wt % toluene solution, manufactured by Dow Corning Toray), 0.9 parts by weight of a release control agent (BY24-850 containing an unreactive silicone resin, manufactured by Dow Corning Toray), and 2 parts by weight of a curing catalyst (SRX212 containing a platinum catalyst, manufactured by Dow Corning Toray), and a toluene / hexane mixed solvent (volume ratio 1:1) as a dilution solvent. The concentration of silicone solids in the release agent composition was 1.0 wt %. Next, the release agent composition was applied with a wire bar to one side of a liner substrate (Lumirror XD500P, a polyester film, 75 μm thick), and heated at 130° C. for 1 minute to prepare a release liner having a release layer (thickness 60 nm) on one side.
[0161] (Preparation of Pressure-Sensitive Adhesive Sheet) Monomer syrup C1 was applied to one side of a substrate sheet (PET separator, manufactured by Mitsubishi Plastics, MRF38) using an applicator to form a coating layer (thickness: 20 μm). Next, a release liner was placed on the formed coating layer to obtain a first laminate. The release liner was placed so that the release layer was in contact with the coating layer. Next, an illuminance of 3.5 mW / cm was applied from the substrate sheet side of the first laminate. 2 and irradiation time 460 seconds (integrated light amount 1600 mJ / cm 2) was used as the light source, and the peak wavelength of the irradiated light was 340 nm. As a result, the coating layer was photocured, and the PSA sheet of Example 1 (thickness: 20 μm) sandwiched between the base sheet and the release liner was obtained. The illuminance of the light was measured using an illuminance meter (UD-T3040T2, manufactured by Topcon Technohouse Co., Ltd.) at a position near the ultraviolet light incident surface of the base sheet.
[0162] Examples 2 to 24, Comparative Examples 1 to 6 Pressure-sensitive adhesive sheets of Examples 2 to 24 and Comparative Examples 1 to 6 were obtained by the same method as Example 1, except that the photocurable composition used and the light irradiation conditions were changed as shown in Table 4. Regarding the light source, "LED" refers to the LED used in Example 1, and "BL+LED" refers to a combination of a black light source and the LED used in Example 1. The integrated light amount in the case of "BL+LED" is the sum of the integrated light amounts from both light sources. The irradiation conditions for each light source in the case of "BL+LED" were as follows: BL: Illuminance 6.2 mW / cm 2 and irradiation time 95 seconds (integrated light amount 589 mJ / cm 2 ) LED: Illuminance 3.1mW / cm 2 and irradiation time 90 seconds (cumulative light amount 279 mJ / cm 2 )
[0163] [Evaluation Method] <Mw of Polymer> Samples were prepared having the same composition as the photocurable compositions used in Examples 1 to 24 and Comparative Examples 1 to 6, except that they did not contain a crosslinking agent. The samples were irradiated with light under the conditions of the corresponding Examples and Comparative Examples. This caused the monomer groups contained in the samples to polymerize, forming a polymer. The Mw of this polymer was measured. The Mw was measured by GPC. The measuring device and measuring conditions were as follows. The measuring device and measuring conditions were different for the NVP-containing composition and the NVP-free composition.
[0164] (NVP-free composition) Analytical equipment: HLC-8320GPC, manufactured by Tosoh Corporation Column: TSKgel GMH-H(S) x 2, manufactured by Tosoh Corporation Column size: 7.8 mmφ x 30 cm each, 60 cm in total Column temperature: 40°C Flow rate: 0.5 mL / min Injection volume: 100 μL Eluent: tetrahydrofuran Detector: differential refractometer (RI) Standard sample: polystyrene
[0165] (NVP-containing composition) Analytical equipment: Agilent 1200, manufactured by Agilent Technologies Column: TSKgel SuperAWM-H + superAW4000 + superAW2500, manufactured by Tosoh Corporation Column size: 6.0 mmφ x 15 cm each, total 45 cm Column temperature: 40°C Flow rate: 0.4 mL / min Injection volume: 40 μL Eluent: N,N-dimethylformamide (DMF) Detector: differential refractometer (RI) Standard sample: polystyrene
[0166] <Content of Sol Fraction A> The content of sol fraction A in each PSA sheet of the Examples and Comparative Examples was measured by the above-mentioned method using GPC. The GPC measurement device and measurement conditions were as follows. The measurement device and measurement conditions were different for the NVP-containing composition and the NVP-free composition.
[0167] (NVP-free composition) Analytical equipment: HLC-8320GPC, manufactured by Tosoh Corporation Column: TSKgel GMH-H(S) x 2, manufactured by Tosoh Corporation Column size: 7.8 mmφ x 30 cm each, 60 cm in total Column temperature: 40°C Flow rate: 0.5 mL / min Injection volume: 100 μL Eluent: tetrahydrofuran Detector: differential refractometer (RI) Standard sample: polystyrene
[0168] (NVP-containing composition) Analytical equipment: Agilent 1200, manufactured by Agilent Technologies Column: TSKgel SuperAWM-H + superAW4000 + superAW2500, manufactured by Tosoh Corporation Column size: 6.0 mmφ x 15 cm each, total 45 cm Column temperature: 40°C Flow rate: 0.4 mL / min Injection volume: 40 μL Eluent: N,N-dimethylformamide (DMF) Detector: differential refractometer (RI) Standard sample: polystyrene
[0169] <Mw of Sol Fraction B> The Mw of sol fraction B in each of the pressure-sensitive adhesive sheets of the Examples and Comparative Examples was determined by the same GPC measurement used to evaluate the content of sol fraction A.
[0170] [Gel Fraction] The gel fraction of each of the pressure-sensitive adhesive sheets of the Examples and Comparative Examples was measured by the method described above.
[0171] (Reliability Test) <Preparation of Polarizing Film> An 80 μm thick polyvinyl alcohol film was stretched 3 times between rolls with different speed ratios while dyeing for 1 minute in a 0.3% iodine solution at 30°C. Next, the film was stretched to a total stretch ratio of 6 times while immersing for 0.5 minutes in an aqueous solution containing 4% boric acid and 10% potassium iodide at 60°C. The film was then immersed for 10 seconds in an aqueous solution containing 1.5% potassium iodide at 30°C for cleaning, followed by drying at 50°C for 4 minutes to obtain a 28 μm thick polarizer. A 30 μm thick transparent protective film made of a modified acrylic polymer having a lactone ring structure was attached to one side of the polarizer using a polyvinyl alcohol adhesive. Furthermore, a 47 μm-thick transparent protective film, which was a triacetyl cellulose film (manufactured by Konica Minolta, product name "KC4UY") with a hard coat layer (HC), was attached to the other surface of the polarizer using a polyvinyl alcohol adhesive. The polarizing film was prepared by heating and drying for 5 minutes in an oven set at 70°C. Furthermore, a discharge amount of 63 W / m was applied to the surface of the polarizing film on the transparent protective film side made of a modified acrylic polymer. 2 The corona treatment was carried out for 1 min.
[0172] <Preparation of polarizing film with adhesive sheet> The above-mentioned polarizing film was placed on the exposed surface of each adhesive sheet prepared in Examples and Comparative Examples to prepare a polarizing film with an adhesive sheet. The polarizing film was placed so that the surface of the transparent protective film made of a modified acrylic polymer was in contact with the adhesive sheet.
[0173] <Reliability Test (85°C)> The reliability (85°C reliability) of the prepared polarizing film with adhesive sheet was evaluated using the following method. First, the polarizing film with adhesive sheet was cut into a strip measuring 228 mm long x 128 mm wide to prepare a test specimen. Next, the test specimen was attached to the surface of 0.7 mm thick alkali-free glass (manufactured by Corning Incorporated, product name "EG-XG") using the adhesive sheet. The test specimen was attached to the alkali-free glass using a laminator. After attaching the test specimen, the specimen was placed in an autoclave at 50°C and 0.5 MPa for 15 minutes to homogenize the bond between the alkali-free glass and the adhesive sheet, thereby adhering the adhesive sheet to the alkali-free glass. Next, the test specimen was subjected to a heat treatment at 85°C under atmospheric pressure for 500 hours. The vicinity of the edge of the test specimen was observed using an optical microscope to check for peeling from the edge of the test specimen and the presence or absence of bubbles near the edge. A: No peeling or foaming that would affect the image display was observed. B: There was slight foaming at the edge, but not to the extent that it would affect the image display. C: There were multiple bubbles at the edge, but not to the extent that it would affect the image display. D: There was peeling and / or foaming that would affect the image display. E: There was peeling and / or foaming that would significantly affect the image display.
[0174] <Reliability Test (95°C)> The 95°C reliability was evaluated in the same manner as for the 85°C reliability, except that the heat treatment temperature was changed from 85°C to 95°C. The evaluation items A to E were the same as for the 85°C reliability.
[0175] The evaluation results are shown in the following Table 4. The relationship between the gel fraction and the content of sol fraction A in each of the pressure-sensitive adhesive sheets of the Examples and Comparative Examples is shown in FIG.
[0176]
[0177] As shown in Table 4, the pressure-sensitive adhesive sheets of the examples had improved reliability in high-temperature environments compared to the pressure-sensitive adhesive sheets of the comparative examples.
[0178] The optical film with a pressure-sensitive adhesive sheet of the present invention can be used in optical laminates and image display devices.
Claims
1. An optical film with an adhesive sheet, comprising a photocurable adhesive sheet and an optical film, wherein the gel fraction of the adhesive sheet is 55% or more and less than 94%, and the content of sol fraction A having a weight average molecular weight of 100,000 or less in the adhesive sheet is less than 6.6% by weight.
2. The optical film with adhesive sheet according to claim 1, wherein the content of the sol component A is 5.8% by weight or less.
3. The optical film with adhesive sheet according to claim 1, wherein the content of the sol component A is 4.9% by weight or less.
4. An optical film with an adhesive sheet as described in claim 1, wherein the weight average molecular weight of the polymer contained in the adhesive sheet is 700,000 or more and less than 800,000, and the weight average molecular weight of all sol components B contained in the adhesive sheet is 600,000 or more, or the weight average molecular weight of the polymer is 800,000 or more, and the weight average molecular weight of the sol components B is 450,000 or more.
5. The optical film with a pressure-sensitive adhesive sheet according to claim 1, wherein the pressure-sensitive adhesive sheet contains a (meth)acrylic polymer.
6. The optical film with adhesive sheet according to claim 5, wherein the (meth)acrylic polymer has a structural unit derived from a carboxyl group-containing monomer.
7. The optical film with adhesive sheet according to claim 5, wherein the (meth)acrylic polymer has a structural unit derived from a nitrogen atom-containing monomer.
8. The optical film with adhesive sheet according to claim 1, wherein the adhesive sheet contains a silane coupling agent.
9. The optical film with adhesive sheet according to claim 1, wherein the thickness of the adhesive sheet is 50 μm or less.
10. The optical film with adhesive sheet according to claim 1, wherein the solvent content in the adhesive sheet is 5% by weight or less.
11. The optical film with adhesive sheet according to claim 1, wherein the adhesive sheet and the optical film are in contact with each other.
12. The optical film with adhesive sheet according to claim 1, wherein the optical film is a polarizing film.
13. An optical laminate comprising an optical film with a pressure-sensitive adhesive sheet according to any one of claims 1 to 12.
14. An image display device comprising the optical film with a pressure-sensitive adhesive sheet according to any one of claims 1 to 12.
Citation Information
Patent Citations
Acrylic adhesive composition for polarizing plates containing a photoinitiator group
JP2010508386A
Optical layered film having adhesive layer and image display device
JP2020122141A
Adhesive sheet
JP2022064782A
Optically clear adhesive sheet
JP2023137397A
Transparent adhesive tape, film laminate with metal thin film, cover panel-touch panel module laminate, cover panel-display panel module laminate, touch panel module-display panel module laminate, and image display device
WO2012173247A1