Method for manufacturing semiconductor substrate and underlayer film-forming composition for metal-containing resist

The use of a metal-containing resist underlayer film forming composition with specific structural units addresses the challenge of achieving good rectangularity in semiconductor substrate patterns, improving the quality of semiconductor substrates by reducing adhesion and residue issues.

WO2024203400A1PCT designated stage expired Publication Date: 2024-10-03JSR CORPORATION
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010059
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-14
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

The challenge in semiconductor substrate manufacturing is achieving good rectangularity of resist patterns, especially with the trend towards shorter exposure wavelengths and the use of metal-containing resist films, where existing methods struggle to maintain pattern quality due to excessive adhesion and development residue issues.

Method used

A method involving a metal-containing resist underlayer film forming composition containing specific structural units, such as polysiloxane or polycarbosilane compounds with aliphatic hydrocarbon groups, which suppress excessive adhesion and facilitate organic solvent penetration, thereby improving pattern rectangularity.

Benefits of technology

The solution effectively forms a metal-containing resist underlayer film with excellent pattern rectangularity, enhancing the quality of semiconductor substrates by reducing development residue and maintaining pattern integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010059_03102024_PF_FP_ABST
    Figure JP2024010059_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided are: a composition capable of forming an underlayer film for a metal-containing resist, the composition making it possible to obtain good rectangularity of a resist pattern; and a method for manufacturing a semiconductor substrate. The method for manufacturing a semiconductor substrate includes: a step for directly or indirectly coating a substrate with an underlayer film-forming composition for a metal-containing resist; a step for coating, with a composition for forming a metal-containing resist film, the metal-containing resist underlayer film formed by the coating step for coating with an underlayer film-forming composition for a metal-containing resist; a step for exposing, to extreme ultraviolet radiation, the metal-containing resist film formed by the step for coating with a composition for forming a metal-containing resist film; and a step for developing at least the exposed metal-containing resist film. The underlayer film-forming composition for a metal-containing resist contains a compound having at least one structural unit selected from the group consisting of a structural unit (α-1) represented by formula (1-1) and a structural unit (α-2) represented by formula (1-2), and a solvent. The total content ratio of the structural unit (α-1) and the structural unit (α-2) to all structural units constituting the compound is 50 mol% to 100 mol%. In formula (1-1), X is a C1-20 monovalent aliphatic hydrocarbon group or a C1-20 monovalent aliphatic hydrocarbon group substituted with at least one halogen atom. a is an integer from 1 to 3. When a is 2 or more, the plurality of X's are the same or different from one another. Y is a C1-20 monovalent organic group, a hydroxy group, or a halogen atom. b is an integer from 0 to 2. When b is 2, the two Y's are the same or different from one another. a + b is less than or equal to 3. In formula (1-2), X represents a C1-20 monovalent aliphatic hydrocarbon group or a C1-20 monovalent aliphatic hydrocarbon group substituted with at least one halogen atom. c is an integer from 1 to 3. When c is 2 or more, the plurality of X's are the same or are different from one another. Y is a C1-20 monovalent organic group, a hydroxy group, or a halogen atom. d is an integer from 0 to 2. When d is 2, the two Y's are the same or different from one another. R0 is a substituted or unsubstituted C1-20 divalent hydrocarbon group that is bonded to two silicon atoms. p is an integer from 1 to 3. When p is 2 or more, the plurality of R0's are the same or are different from one another. c + d + p is less than or equal to 4.
Need to check novelty before this filing date? Find Prior Art

Description

Semiconductor substrate manufacturing method and underlayer film forming composition for metal-containing resist

[0001] The present invention relates to a method for producing a semiconductor substrate and a metal-containing resist underlayer film-forming composition.

[0002] For pattern formation in the manufacture of semiconductor substrates, for example, a multilayer resist process is used in which a patterned substrate is formed by exposing and developing a resist film laminated on a substrate via an organic underlayer film, a silicon-containing film, etc., and then etching the resulting resist pattern as a mask (see WO 2022 / 260154).

[0003] International Publication No. 2022 / 260154

[0004] In recent years, semiconductor devices have become increasingly highly integrated, and the wavelength of the exposure light used has tended to be shortened from KrF excimer lasers (248 nm) and ArF excimer lasers (193 nm) to extreme ultraviolet (13.5 nm, hereinafter also referred to as "EUV"), which has led to the use of metal-containing resist films instead of organic resist films.

[0005] As the line width of resist patterns formed by exposure to extreme ultraviolet light and development continues to become finer, metal-containing resist underlayer films are required to have pattern rectangularity that ensures the rectangularity of the resist pattern by suppressing pattern footing and development residues at the bottom of the resist film.

[0006] An object of the present invention is to provide a composition capable of forming a metal-containing resist underlayer film that can provide a resist pattern with good rectangularity, and a method for producing a semiconductor substrate.

[0007] As a result of extensive research into solving the above problems, the present inventors have found that the above object can be achieved by employing the following configuration, and have thus completed the present invention.

[0008] In one embodiment, the present invention comprises the steps of: applying a metal-containing resist underlayer film-forming composition (hereinafter also referred to as "composition") directly or indirectly to a substrate; applying a metal-containing resist film-forming composition to the metal-containing resist underlayer film formed in the metal-containing resist underlayer film-forming composition-applying step; exposing the metal-containing resist film formed in the metal-containing resist film-forming composition-applying step to extreme ultraviolet light; and developing at least the exposed metal-containing resist film, wherein the metal-containing resist underlayer film-forming composition contains: a compound (hereinafter also referred to as "compound [A]") having at least one structural unit (hereinafter also referred to as "structural unit (α)") selected from the group consisting of a structural unit (α-1) represented by the following formula (1-1) and a structural unit (α-2) represented by the following formula (1-2): the total content of the structural unit (α-1) and the structural unit (α-2) relative to all structural units constituting the compound is 50 mol % or more and 100 mol % or less. In formula (1-1), X represents a monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms or a monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms and substituted with at least one halogen atom. a represents an integer of 1 to 3. When a is 2 or greater, multiple Xs are the same or different. Y represents a monovalent organic group having 1 to 20 carbon atoms, a hydroxy group, or a halogen atom. b represents an integer of 0 to 2. When b is 2, two Ys are the same or different, provided that a+b is 3 or less. In formula (1-2), X is a monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms or a monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms substituted with at least one halogen atom. c is an integer from 1 to 3. When c is 2 or greater, multiple Xs are the same or different. Y is a monovalent organic group having 1 to 20 carbon atoms, a hydroxy group, or a halogen atom. d is an integer from 0 to 2. When d is 2, two Ys are the same or different. R 0 is a substituted or unsubstituted divalent hydrocarbon group having 1 to 20 carbon atoms bonded to two silicon atoms. p is an integer of 1 to 3. When p is 2 or more, multiple R 0are the same or different, provided that c + d + p is 4 or less.

[0009] In the method for producing a semiconductor substrate, the metal-containing resist underlayer film-forming composition contains compound [A], which is a polysiloxane compound or polycarbosilane compound containing a structural unit (α) having an aliphatic hydrocarbon group. This allows the formation of a metal-containing resist underlayer film capable of exhibiting excellent pattern rectangularity, thereby enabling the efficient production of high-quality semiconductor substrates. While the reason for this is unclear, it is presumed as follows. For example, during organic solvent development of an exposed metal-containing resist film, the hydrophobic aliphatic hydrocarbon group derived from the structural unit (α) of the metal-containing resist underlayer film suppresses excessive adhesion to the overlying metal-containing resist film in the unexposed areas, thereby suppressing footing of the resist pattern. Furthermore, since the metal-containing resist underlayer film formed from the metal-containing resist underlayer film-forming composition contains the structural unit (α) having a relatively hydrophobic aliphatic hydrocarbon group, the organic solvent used for development easily penetrates into the metal-containing resist underlayer film, facilitating removal by the organic solvent and suppressing the generation of development residues. It is presumed that these effects enable the formation of excellent pattern rectangularity.

[0010] In this specification, the term "organic group" means a group containing at least one carbon atom, and the term "number of carbon atoms" means the number of carbon atoms constituting the group.

[0011] In another embodiment, the present invention relates to a metal-containing resist underlayer film-forming composition comprising: a compound having at least one structural unit selected from the group consisting of a structural unit (α-1) represented by the following formula (1-1) and a structural unit (α-2) represented by the following formula (1-2); and a solvent, wherein the total content of the structural unit (α-1) and the structural unit (α-2) relative to all structural units constituting the compound is 50 mol % or more and 100 mol % or less. In formula (1-1), X represents a monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms or a monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms and substituted with at least one halogen atom. a represents an integer of 1 to 3. When a is 2 or greater, multiple Xs are the same or different. Y represents a monovalent organic group having 1 to 20 carbon atoms, a hydroxy group, or a halogen atom. b represents an integer of 0 to 2. When b is 2, two Ys are the same or different, provided that a+b is 3 or less. In formula (1-2), X is a monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms or a monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms substituted with at least one halogen atom. c is an integer from 1 to 3. When c is 2 or greater, multiple Xs are the same or different. Y is a monovalent organic group having 1 to 20 carbon atoms, a hydroxy group, or a halogen atom. d is an integer from 0 to 2. When d is 2, two Ys are the same or different. R 0 is a substituted or unsubstituted divalent hydrocarbon group having 1 to 20 carbon atoms bonded to two silicon atoms. p is an integer of 1 to 3. When p is 2 or more, multiple R 0 are the same or different, provided that c + d + p is 4 or less.

[0012] The metal-containing resist underlayer film-forming composition makes it possible to efficiently form a metal-containing resist underlayer film that is capable of exhibiting excellent pattern rectangularity.

[0013] Hereinafter, the method for producing a semiconductor substrate and the metal-containing resist underlayer film-forming composition according to the embodiments of the present invention will be described in detail. In the embodiments, preferred combinations of aspects are also preferred.

[0014] <<Method for Manufacturing Semiconductor Substrate>> The method for manufacturing a semiconductor substrate according to this embodiment includes a step of applying a metal-containing resist underlayer film-forming composition directly or indirectly to a substrate (hereinafter also referred to as a “coating step (I)”), a step of applying a metal-containing resist film-forming composition to the metal-containing resist underlayer film formed in the metal-containing resist underlayer film-forming composition applying step (hereinafter also referred to as a “coating step (II)”), a step of exposing the metal-containing resist film formed in the metal-containing resist film-forming composition applying step to extreme ultraviolet light (hereinafter also referred to as an “exposure step”), and a step of developing at least the exposed metal-containing resist film (hereinafter also referred to as a “development step”).

[0015] The method for producing a semiconductor substrate may further include, as necessary, a step of forming an organic underlayer film directly or indirectly on the substrate (hereinafter also referred to as an "organic underlayer film forming step") prior to the coating step (I).

[0016] Furthermore, after the developing step, the method may further include a step of etching the metal-containing resist underlayer film using the resist pattern as a mask to form a metal-containing resist underlayer film pattern (hereinafter also referred to as a "metal-containing resist underlayer film pattern forming step"), or a step of etching using the metal-containing resist underlayer film pattern as a mask (hereinafter referred to as an "etching step").

[0017] According to the method for producing a semiconductor substrate, by using the composition in the metal-containing resist underlayer film forming step, it is possible to form a metal-containing resist underlayer film with excellent pattern rectangularity.

[0018] Hereinafter, a description will be given of a metal-containing resist underlayer film-forming composition used in the method for producing a semiconductor substrate, as well as a case where the method includes an optional organic underlayer film-forming step prior to the metal-containing resist underlayer film-forming step, a metal-containing resist underlayer film pattern-forming step following the development step, and an etching step.

[0019] <Metal-containing resist underlayer film-forming composition> The composition contains the compound [A] and the solvent [B]. The composition may contain other optional components as long as the effects of the present invention are not impaired.

[0020] The composition is suitable for use in forming a metal-containing resist underlayer film as an underlayer film for a metal-containing resist film. Each component contained in the composition will be described below.

[0021] <Compound [A]> The compound [A] has at least a structural unit (α). Each structural unit contained in the compound [A] will be described below.

[0022] (Structural Unit (α)) The structural unit (α) is at least one selected from the group consisting of a structural unit (α-1) represented by the following formula (1-1) and a structural unit (α-2) represented by the following formula (1-2).

[0023]

[0024] In formula (1-1), X is a monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms or a monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms substituted with at least one halogen atom. a is an integer from 1 to 3. When a is 2 or more, multiple Xs are the same or different. Y is a monovalent organic group having 1 to 20 carbon atoms, a hydroxy group, or a halogen atom. b is an integer from 0 to 2. When b is 2, two Ys are the same or different, provided that a+b is 3 or less.

[0025] In formula (1-2), X is a monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms or a monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms substituted with at least one halogen atom. c is an integer from 1 to 3. When c is 2 or greater, multiple Xs are the same or different. Y is a monovalent organic group having 1 to 20 carbon atoms, a hydroxy group, or a halogen atom. d is an integer from 0 to 2. When d is 2, two Ys are the same or different. R 0 is a substituted or unsubstituted divalent hydrocarbon group having 1 to 20 carbon atoms bonded to two silicon atoms. p is an integer of 1 to 3. When p is 2 or more, multiple R 0 are the same or different, provided that c+d+p is 4 or less.

[0026] In the above formulas (1-1) and (1-2), examples of the monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms represented by X include a monovalent chain aliphatic hydrocarbon group having 1 to 20 carbon atoms, a monovalent alicyclic hydrocarbon group having 3 to 20 carbon atoms, or a combination thereof.

[0027] Examples of the monovalent chain aliphatic hydrocarbon group having 1 to 20 carbon atoms include a monovalent chain aliphatic saturated hydrocarbon group having 1 to 20 carbon atoms and a monovalent chain aliphatic unsaturated hydrocarbon group having 1 to 20 carbon atoms. Examples of the monovalent chain aliphatic saturated hydrocarbon group having 1 to 20 carbon atoms include alkyl groups such as a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, an isobutyl group, and a tert-butyl group. Examples of the monovalent chain aliphatic unsaturated hydrocarbon group having 1 to 20 carbon atoms include alkenyl groups such as an ethenyl group, a propenyl group, and a butenyl group; and alkynyl groups such as an ethynyl group, a propynyl group, and a butynyl group.

[0028] Examples of the monovalent alicyclic hydrocarbon group having 3 to 20 carbon atoms include monocyclic alicyclic saturated hydrocarbon groups such as a cyclopentyl group and a cyclohexyl group; polycyclic alicyclic saturated hydrocarbon groups such as a norbornyl group, an adamantyl group, a tricyclodecyl group and a tetracyclododecyl group; monocyclic alicyclic unsaturated hydrocarbon groups such as a cyclopentenyl group and a cyclohexenyl group; and polycyclic alicyclic unsaturated hydrocarbon groups such as a norbornenyl group, a tricyclodecenyl group and a tetracyclododecenyl group.

[0029] The aliphatic hydrocarbon group is preferably a monovalent chain aliphatic saturated hydrocarbon group having 1 to 5 carbon atoms or a monovalent alicyclic saturated hydrocarbon group having 3 to 6 carbon atoms.

[0030] Examples of the monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms and substituted with at least one halogen atom, represented by X (hereinafter also referred to as a "halogenated aliphatic hydrocarbon group"), include groups in which some or all of the hydrogen atoms of the monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms have been substituted with halogen atoms. Examples of halogen atoms include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom (unless otherwise specified, "halogen atom" in this specification refers to these atoms). Preferred halogen atoms are fluorine atoms and iodine atoms. The number of halogen atoms in the halogenated aliphatic hydrocarbon group is preferably 1 to 4, and more preferably 1 to 3.

[0031] In the above formula (1-1) and formula (1-2), examples of the monovalent organic group having 1 to 20 carbon atoms represented by Y include: a monovalent hydrocarbon group having 1 to 20 carbon atoms; a group containing a divalent heteroatom-containing linking group between carbon atoms of the hydrocarbon group or at the end of the hydrocarbon group (hereinafter also referred to as "group (α)"); a group in which some or all of the hydrogen atoms of the hydrocarbon group or the group (α) have been substituted with a monovalent heteroatom-containing substituent (hereinafter also referred to as "group (β)"); and a group comprising a combination of at least two of the above hydrocarbon group, the group (α) and the group (β) (hereinafter also referred to as "group (γ)").

[0032] Examples of the monovalent hydrocarbon group having 1 to 20 carbon atoms include a monovalent chain hydrocarbon group having 1 to 20 carbon atoms, a monovalent alicyclic hydrocarbon group having 3 to 20 carbon atoms, and a monovalent aromatic hydrocarbon group having 6 to 20 carbon atoms.

[0033] As the monovalent chain hydrocarbon group having 1 to 20 carbon atoms, the monovalent chain aliphatic hydrocarbon group having 1 to 20 carbon atoms for X above can be suitably used.

[0034] As the monovalent alicyclic hydrocarbon group having 3 to 20 carbon atoms, the monovalent alicyclic hydrocarbon group having 1 to 20 carbon atoms for X above can be suitably used.

[0035] Examples of the monovalent aromatic hydrocarbon group having 6 to 20 carbon atoms include aryl groups such as phenyl, tolyl, xylyl, naphthyl, and anthryl groups, and aralkyl groups such as benzyl, phenethyl, naphthylmethyl, and anthrylmethyl groups.

[0036] Examples of heteroatoms constituting the divalent heteroatom-containing linking group and the monovalent heteroatom-containing substituent include oxygen atoms, nitrogen atoms, sulfur atoms, phosphorus atoms, silicon atoms, halogen atoms, etc. Examples of halogen atoms include fluorine atoms, chlorine atoms, bromine atoms, and iodine atoms.

[0037] Examples of the divalent heteroatom-containing linking group include —O—, —C(═O)—, —S—, —C(═S)—, —NR′—, and —SO 2 -, a group formed by combining two or more of these, etc. R' is a hydrogen atom or a monovalent hydrocarbon group.

[0038] Examples of the monovalent hetero atom-containing substituent include a halogen atom, a hydroxy group, a carboxy group, a cyano group, an amino group, and a sulfanyl group.

[0039] Y is preferably an alkoxy group.

[0040] In the above formula (1-1), a is preferably 1 or 2, and more preferably 1. In the above formula (1-1), b is preferably 0 or 1, and more preferably 0.

[0041] In the above formula (1-2), c is preferably 1 or 2, and more preferably 1. In the above formula (1-2), d is preferably 0 or 1, and more preferably 0.

[0042] In the above (1-2), R 0 Examples of the substituted or unsubstituted divalent hydrocarbon group having 1 to 20 carbon atoms and bonded to two silicon atoms include a substituted or unsubstituted divalent chain hydrocarbon group having 1 to 20 carbon atoms, a substituted or unsubstituted divalent aliphatic cyclic hydrocarbon group having 3 to 20 carbon atoms, and a substituted or unsubstituted divalent aromatic hydrocarbon group having 6 to 20 carbon atoms.

[0043] Examples of unsubstituted divalent chain hydrocarbon groups having 1 to 20 carbon atoms include chain saturated hydrocarbon groups such as methanediyl group and ethanediyl group, and chain unsaturated hydrocarbon groups such as ethenediyl group and propenediyl group.

[0044] Examples of the unsubstituted divalent aliphatic cyclic hydrocarbon group having 3 to 20 carbon atoms include monocyclic saturated hydrocarbon groups such as a cyclobutanediyl group, monocyclic unsaturated hydrocarbon groups such as a cyclobutenediyl group, polycyclic saturated hydrocarbon groups such as a bicyclo[2.2.1]heptanediyl group, and polycyclic unsaturated hydrocarbon groups such as a bicyclo[2.2.1]heptenediyl group.

[0045] Examples of the unsubstituted divalent aromatic hydrocarbon group having 6 to 20 carbon atoms include a phenylene group, a biphenylene group, a phenyleneethylene group, and a naphthylene group.

[0046] R 0 Examples of the substituent in the substituted divalent hydrocarbon group having 1 to 20 carbon atoms represented by the formula (I) include a halogen atom, a hydroxy group, a cyano group, a nitro group, an alkoxy group, an acyl group, and an acyloxy group.

[0047] R 0 As the alkyl group, an unsubstituted chain saturated hydrocarbon group or an unsubstituted aromatic hydrocarbon group is preferred, and a methanediyl group, an ethanediyl group or a phenylene group is more preferred.

[0048] In the above formula (1-2), p is preferably 2 or 3.

[0049] Examples of X in the above formula (1-1) and formula (1-2) include structures represented by the following formulas.

[0050]

[0051]

[0052] In the above formula, * represents a bond to the silicon atom in the above formula (1-1) and formula (1-2).

[0053] The total content of the structural unit (α-1) and the structural unit (α-2) relative to all structural units constituting the compound [A] is 50 mol% or more and 100 mol% or less. The lower limit of the content (total when multiple types are included) is preferably 60 mol%, more preferably 70 mol%, and even more preferably 80 mol%. The upper limit of the content is preferably 95 mol%, more preferably 90 mol%. By setting the total content of the structural unit (α-1) and the structural unit (α-2) within the above range, pattern rectangularity can be further improved.

[0054] (Structural Unit (β)) The compound (A) may have a structural unit (β) represented by the following formula (2).

[0055]

[0056] In formula (2), R 1 is a monovalent organic group having 1 to 20 carbon atoms (however, this does not include monovalent aliphatic hydrocarbon groups and halogenated aliphatic hydrocarbon groups having 1 to 20 carbon atoms), a hydroxy group, a hydrogen atom, or a halogen atom. h is 1 or 2. When h is 2, two R 1 are the same or different. 2 is a substituted or unsubstituted divalent hydrocarbon group having 1 to 20 carbon atoms bonded to two silicon atoms. q is an integer of 1 to 3. When q is 2 or more, multiple R 2 are the same or different, provided that h+q is 4 or less.

[0057] In the above formula (2-1), R 1 Examples of the monovalent organic group having 1 to 20 carbon atoms represented by the formula (1-1) and the formula (1-2) include the same groups as those exemplified as the monovalent organic group having 1 to 20 carbon atoms represented by Y in the formula (1-1) and the formula (1-2), except that it does not include a monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms and a halogenated aliphatic hydrocarbon group.

[0058] R 1is preferably a hydrogen atom, a monovalent chain hydrocarbon group, a monovalent aromatic hydrocarbon group, or a monovalent group in which some or all of the hydrogen atoms of a monovalent hydrocarbon group have been substituted with a monovalent heteroatom-containing group, more preferably a hydrogen atom, an alkyl group, or an aryl group, and even more preferably a hydrogen atom, a methyl group, an ethyl group, or a phenyl group.

[0059] R 2 Examples of the substituted or unsubstituted divalent hydrocarbon group having 1 to 20 carbon atoms bonded to two silicon atoms and represented by the formula (1-2) include R 0 Examples of the substituted or unsubstituted divalent hydrocarbon group having 1 to 20 carbon atoms bonded to two silicon atoms include the same groups as those exemplified above as the substituted or unsubstituted divalent hydrocarbon group having 1 to 20 carbon atoms bonded to two silicon atoms.

[0060] R 2 As the alkyl group, an unsubstituted chain saturated hydrocarbon group or an unsubstituted aromatic hydrocarbon group is preferred, and a methanediyl group, an ethanediyl group or a phenylene group is more preferred.

[0061] h is preferably 1. q is preferably 2 or 3.

[0062] When the compound [A] has the structural unit (β), the lower limit of the content of the structural unit (β) (total content when multiple types are included) is preferably 4 mol%, more preferably 6 mol%, and even more preferably 8 mol%, based on all structural units constituting the compound [A]. The upper limit of the content is preferably 70 mol%, more preferably 60 mol%, and even more preferably 50 mol%.

[0063] (Structural Unit (γ)) The compound (A) may have a structural unit (γ) represented by the following formula (3).

[0064]

[0065] In the above formula (3), R 12 is a substituted or unsubstituted monovalent alkoxy group having 1 to 20 carbon atoms, a hydroxy group, or a halogen atom. e is an integer of 0 to 3. When e is 2 or more, multiple R 12 are the same or different.)

[0066] In the above formula (3), R 12Specific examples of the monovalent alkoxy group having 1 to 20 carbon atoms represented by the formula (I) include alkoxy groups such as a methoxy group, an ethoxy group, an n-propyloxy group, and an isopropyloxy group. Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom.

[0067] In the above formula (3), R 12 is preferably an alkoxy group, more preferably a methoxy group.

[0068] In the above formula (3), e is preferably an integer of 0 to 2, and more preferably 0 or 1.

[0069] When the compound [A] has the structural unit (γ), the lower limit of the content of the structural unit (γ) in all structural units constituting the compound [A] is preferably 2 mol%, more preferably 5 mol%, and even more preferably 8 mol%, and the upper limit of the content is preferably 70 mol%, more preferably 60 mol%, and even more preferably 55 mol%.

[0070] The lower limit of the content of the compound [A] is preferably 0.1 mass %, more preferably 0.5 mass %, and even more preferably 0.8 mass %, relative to the total mass of the compound [A] and the solvent [B], and the upper limit of the content is preferably 10 mass %, more preferably 5 mass %, and even more preferably 2 mass %.

[0071] The compound [A] is preferably in the form of a polymer. A "polymer" refers to a compound having two or more structural units, and when two or more identical structural units are consecutive in a polymer, this structural unit is also referred to as a "repeating unit." When the compound [A] is in the form of a polymer, the lower limit of the weight average molecular weight (Mw) of the compound [A] measured by gel permeation chromatography (GPC) in terms of polystyrene is preferably 800, more preferably 1,000, even more preferably 1,200, and particularly preferably 1,400. The upper limit of the Mw is preferably 15,000, more preferably 10,000, even more preferably 7,000, and particularly preferably 3,000. The method for measuring the Mw of the compound [A] is as described in the Examples.

[0072] <Synthesis of Compound [A]> Compound [A] can be obtained, for example, by hydrolysis and condensation of a polysiloxane having the structural unit (α-1), hydrolysis and condensation of a polycarbosilane having the structural unit (α-2), or hydrolysis and condensation of a polycarbosilane having the structural unit (α-2) with a silane compound that provides the structural unit (α-1). If necessary, other silane compounds may be added during the hydrolysis and condensation. The hydrolysis and condensation can be carried out in a solvent such as diisopropyl ether in the presence of a catalyst such as oxalic acid and water, and preferably by purifying the solution containing the resulting hydrolysis and condensation product through solvent substitution in the presence of a dehydrating agent such as an orthoester or molecular sieves. It is believed that each hydrolyzable silane monomer is incorporated into Compound [A] regardless of its type through the hydrolysis and condensation reaction, and the proportions of the structural units (α-1), (α-2), and other structural units in the synthesized Compound [A] are generally equivalent to the proportions of the amounts of the respective monomer compounds used in the synthesis reaction.

[0073] <Solvent [B]> Examples of the solvent [B] include alcohol solvents, ketone solvents, ether solvents, ester solvents, nitrogen-containing solvents, water, etc. The solvent [B] can be used alone or in combination of two or more.

[0074] Examples of alcohol solvents include monoalcohol solvents such as methanol, ethanol, n-propanol, isopropanol, n-butanol, and isobutanol, and polyalcohol solvents such as ethylene glycol, 1,2-propylene glycol, diethylene glycol, and dipropylene glycol.

[0075] Examples of ketone solvents include acetone, 2-butanone, 2-pentanone, 4-methyl-2-pentanone, 2-heptanone, and cyclohexanone.

[0076] Examples of ether solvents include ethyl ether, isopropyl ether, ethylene glycol dibutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol diethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, and tetrahydrofuran.

[0077] Examples of ester solvents include ethyl acetate, γ-butyrolactone, n-butyl acetate, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, dipropylene glycol monomethyl ether acetate, dipropylene glycol monoethyl ether acetate, ethyl propionate, n-butyl propionate, methyl lactate, and ethyl lactate.

[0078] Examples of nitrogen-containing solvents include N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone.

[0079] Among these, ether-based solvents or ester-based solvents are preferred, and ether-based solvents or ester-based solvents having a glycol structure are more preferred because of their excellent film-forming properties.

[0080] Examples of ether solvents and ester solvents having a glycol structure include propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether acetate, etc. Among these, propylene glycol monomethyl ether acetate or propylene glycol monoethyl ether is preferred.

[0081] The content of the ether-based solvent and ester-based solvent having a glycol structure in the solvent (B) is preferably 20% by mass or more, more preferably 60% by mass or more, even more preferably 90% by mass or more, and particularly preferably 100% by mass.

[0082] The lower limit of the content of the solvent (B) in the composition is preferably 50% by mass, more preferably 80% by mass, even more preferably 90% by mass, and particularly preferably 95% by mass, and the upper limit of the content is preferably 99.9% by mass, more preferably 99% by mass.

[0083] <Other Optional Components> Examples of the other optional components include acid generators, basic compounds (including base generators), orthoesters, radical generators, surfactants, colloidal silica, colloidal alumina, organic polymers, etc. The other optional components may be used either individually or in combination of two or more.

[0084] (Acid Generator) The acid generator is a component that generates an acid upon exposure to light or heating. When the composition contains an acid generator, the condensation reaction of the compound (A) can be promoted even at relatively low temperatures (including room temperature).

[0085] Examples of acid generators that generate acid upon exposure (hereinafter also referred to as "photoacid generators") include the acid generators described in paragraphs

[0077] to

[0081] of JP-A No. 2004-168748, triphenylsulfonium trifluoromethanesulfonate, and the like.

[0086] Examples of acid generators that generate acid upon heating (hereinafter also referred to as "thermal acid generators") include onium salt-based acid generators exemplified as photoacid generators in the above-mentioned patent documents, as well as 2,4,4,6-tetrabromocyclohexadienone, benzoin tosylate, 2-nitrobenzyl tosylate, and alkylsulfonates.

[0087] When the composition contains an acid generator, the lower limit of the content of the acid generator is preferably 0.001 parts by mass and more preferably 0.01 parts by mass relative to 100 parts by mass of the compound [A], and the upper limit of the content of the acid generator is preferably 5 parts by mass and more preferably 1 part by mass relative to 100 parts by mass of the compound [A].

[0088] (Basic Compound) The basic compound accelerates the curing reaction of the composition, thereby improving the strength of the formed film. The basic compound also improves the removability of the film with an acidic solution. Examples of basic compounds include compounds having a basic amino group, and base generators that generate a compound having a basic amino group under the action of acid or heat. Examples of compounds having a basic amino group include amine compounds. Examples of base generators include amide group-containing compounds, urea compounds, and nitrogen-containing heterocyclic compounds. Specific examples of amine compounds, amide group-containing compounds, urea compounds, and nitrogen-containing heterocyclic compounds include the compounds described in paragraphs

[0079] to

[0082] of JP 2016-27370 A.

[0089] When the composition contains a basic compound, the lower limit of the content of the basic compound is preferably 0.001 parts by mass, more preferably 0.01 parts by mass, relative to 100 parts by mass of the compound [A], and the upper limit of the content is preferably 5 parts by mass, more preferably 1 part by mass.

[0090] (Orthoester) An orthoester is an ester of an orthocarboxylic acid. An orthoester reacts with water to give a carboxylic acid ester or the like. Examples of the orthoester include orthoformic acid esters such as methyl orthoformate, ethyl orthoformate, and propyl orthoformate; orthoacetic acid esters such as methyl orthoacetate, ethyl orthoacetate, and propyl orthoacetate; and orthopropionic acid esters such as methyl orthopropionate, ethyl orthopropionate, and propyl orthopropionate. Of these, orthoformic acid esters are preferred, and trimethyl orthoformate is more preferred.

[0091] When the composition contains an orthoester, the lower limit of the content of the orthoester is preferably 0.1 parts by mass, more preferably 0.5 parts by mass, and even more preferably 1 part by mass, relative to 100 parts by mass of the compound [A]. The upper limit of the content is preferably 30 parts by mass, more preferably 20 parts by mass, and even more preferably 10 parts by mass.

[0092] <Method for preparing metal-containing resist underlayer film-forming composition> The method for preparing the composition is not particularly limited, but the composition can be prepared, for example, by mixing a solution of the compound (A), the solvent (B), and other optional components used as needed in a predetermined ratio, and preferably filtering the resulting mixed solution through a filter or the like having a pore size of 0.4 μm or less.

[0093] [Organic Underlayer Film Formation Step] In this step, an organic underlayer film is formed directly or indirectly on the substrate prior to the metal-containing resist underlayer film formation step. This step is an optional step. By this step, an organic underlayer film is formed directly or indirectly on the substrate.

[0094] The organic underlayer film can be formed by coating an organic underlayer film-forming composition, etc. Examples of methods for forming an organic underlayer film by coating an organic underlayer film-forming composition include a method in which the organic underlayer film-forming composition is directly or indirectly applied to a substrate, and the resulting coating film is heated or exposed to light to cure it. Examples of the organic underlayer film-forming composition that can be used include "HM8006" manufactured by JSR Corporation. The heating and exposure conditions can be appropriately determined depending on the type of organic underlayer film-forming composition used, etc.

[0095] An example of a case where an organic underlayer film is formed indirectly on a substrate is a case where an organic underlayer film is formed on a low dielectric insulating film formed on a substrate.

[0096] [Coating Step (I)] In this step, a metal-containing resist underlayer film-forming composition is applied directly or indirectly to a substrate, forming a coating film of the composition directly or indirectly on the substrate, and this coating film is usually heated and cured to form a metal-containing resist underlayer film as a resist underlayer film.

[0097] Examples of the substrate include insulating films such as silicon oxide, silicon nitride, silicon oxynitride, and polysiloxane, and resin substrates. The substrate may also be a substrate patterned with wiring grooves (trenches), plug grooves (vias), and the like.

[0098] The method for applying the metal-containing resist underlayer film-forming composition is not particularly limited, and examples thereof include a rotary coating method.

[0099] Examples of cases in which the metal-containing resist underlayer film-forming composition is indirectly applied to a substrate include cases in which the metal-containing resist underlayer film-forming composition is applied to another film formed on the substrate, etc. Examples of other films formed on the substrate include an organic underlayer film formed by the organic underlayer film-forming step described above, an antireflective film, a low-dielectric insulating film, etc.

[0100] When the coating film is heated, the atmosphere is not particularly limited, and examples thereof include air and nitrogen atmospheres. Typically, the coating film is heated in air. When the coating film is heated, the heating temperature, heating time, and other conditions can be appropriately determined. The lower limit of the heating temperature is preferably 90°C, more preferably 150°C, and even more preferably 200°C. The upper limit of the heating temperature is preferably 550°C, more preferably 450°C, and even more preferably 300°C. The lower limit of the heating time is preferably 15 seconds, and more preferably 30 seconds. The upper limit of the heating time is preferably 1,200 seconds, and more preferably 600 seconds.

[0101] When the metal-containing resist underlayer film-forming composition contains an acid generator, and this acid generator is a radiation-sensitive acid generator, the formation of the metal-containing resist underlayer film can be promoted by combining heating and exposure. Examples of radiation used for exposure include the same radiation as those exemplified in the exposure step described below.

[0102] The lower limit of the average thickness of the metal-containing resist underlayer film formed by this step is preferably 1 nm, more preferably 2 nm, and even more preferably 3 nm. The upper limit of the average thickness is preferably 30 nm, more preferably 10 nm, even more preferably 6 nm, and particularly preferably 5 nm. The method for measuring the average thickness of the metal-containing resist underlayer film is as described in the Examples.

[0103] [Coating Step (II)] In this step, a metal-containing resist film-forming composition is coated on the metal-containing resist underlayer film formed in the above-mentioned metal-containing resist underlayer film-forming composition coating step, thereby forming a metal-containing resist film on the metal-containing resist underlayer film.

[0104] The method for applying the composition for forming a metal-containing resist film is not particularly limited, and examples thereof include a rotary coating method.

[0105] To explain this step in more detail, for example, a composition for forming a metal-containing resist film is applied so that the metal-containing resist film to be formed has a predetermined thickness, and then the composition is pre-baked (hereinafter also referred to as "PB") to volatilize the solvent in the coated film, thereby forming a resist film.

[0106] The lower limit of the average thickness of the metal-containing resist film formed in this step is preferably 10 nm, more preferably 20 nm, and even more preferably 30 nm, and the upper limit of the average thickness is preferably 60 nm, more preferably 50 nm, and even more preferably 40 nm.

[0107] The PB temperature and PB time can be appropriately determined depending on the type of metal-containing resist film-forming composition used, etc. The lower limit of the PB temperature is preferably 30°C, more preferably 50°C. The upper limit of the PB temperature is preferably 200°C, more preferably 150°C. The lower limit of the PB time is preferably 10 seconds, more preferably 30 seconds. The upper limit of the PB time is preferably 600 seconds, more preferably 300 seconds.

[0108] The composition for forming a metal-containing resist film used in this step includes a composition for forming a metal-containing resist film that contains a compound containing a metal atom (hereinafter also referred to as “[P] metal-containing compound”).

[0109] <Composition for forming a metal-containing resist film> The composition for forming a metal-containing resist film contains 50 mass % or more of the metal-containing compound [P] in terms of solid content. The composition for forming a metal-containing resist film preferably further contains a solvent [Q], and may further contain other components.

[0110] ([P] Metal-Containing Compound) The [P] metal-containing compound is a compound containing a metal atom. The [P] metal-containing compound may be used alone or in combination of two or more. The metal atoms constituting the [P] metal-containing compound may be used alone or in combination of two or more. Here, the term "metal atom" refers to a concept including metalloids, i.e., boron, silicon, germanium, arsenic, antimony, and tellurium.

[0111] The metal atoms constituting the metal-containing compound [P] are not particularly limited, and examples thereof include metal atoms of Groups 3 to 16. Specific examples of the metal atoms include metal atoms of Group 4 such as titanium, zirconium, and hafnium, metal atoms of Group 5 such as tantalum, metal atoms of Group 6 such as chromium and tungsten, metal atoms of Group 8 such as iron and ruthenium, metal atoms of Group 9 such as cobalt, metal atoms of Group 10 such as nickel, metal atoms of Group 11 such as copper, metal atoms of Group 12 such as zinc, cadmium, and mercury, metal atoms of Group 13 such as boron, aluminum, gallium, indium, and thallium, metal atoms of Group 14 such as germanium, tin, and lead, metal atoms of Group 15 such as antimony and bismuth, and metal atoms of Group 16 such as tellurium.

[0112] The metal atoms constituting the [P] metal-containing compound preferably include a first metal atom belonging to Group 4, Group 12, or Group 14 in the periodic table and belonging to Period 4, Period 5, or Period 6. That is, the metal atom preferably includes at least one of titanium, zirconium, hafnium, zinc, cadmium, mercury, germanium, tin, and lead. Thus, the inclusion of the first metal atom in the [P] metal-containing compound further promotes the emission of secondary electrons in the exposed areas of the resist film and the change in the solubility of the [P] metal-containing compound in the developer due to these secondary electrons. As a result, the pattern rectangularity can be improved. The first metal atom is preferably tin or zirconium.

[0113] It is preferable that the metal-containing compound [P] further contains atoms other than metal atoms. Examples of the other atoms include carbon atoms, hydrogen atoms, oxygen atoms, nitrogen atoms, phosphorus atoms, sulfur atoms, and halogen atoms, and among these, carbon atoms, hydrogen atoms, and oxygen atoms are preferred. The other atoms in the metal-containing compound [P] can be used alone or in combination of two or more.

[0114] The lower limit of the content of the metal-containing compound [P] in the composition for forming a metal-containing resist film, calculated as solid content, is preferably 70 mass %, more preferably 90 mass %, and even more preferably 95 mass %. The content may be 100 mass %. Here, the solid content in the composition for forming a metal-containing resist film refers to components other than the solvent [Q], which will be described later.

[0115] (Method for synthesizing the metal-containing compound [P]) The metal-containing compound [P] can be obtained by, for example, a method of subjecting a metal compound having a metal atom and a hydrolyzable group, a hydrolysate of this metal compound, a hydrolysis condensation product of the metal compound, or a combination thereof to a hydrolysis condensation reaction, a ligand exchange reaction, or the like. The metal compounds can be used alone or in combination of two or more.

[0116] The metal-containing compound [P] is preferably derived from a metal compound having a metal atom and a hydrolyzable group represented by the following formula (4) (hereinafter also referred to as "metal compound (1)"). By using such metal compound (1), a stable metal-containing compound [P] can be obtained.

[0117] In the above formula (4), M is a metal atom. 1 is a ligand or a monovalent organic group having 1 to 20 carbon atoms. a1 is an integer of 0 to 6. When a1 is 2 or more, a plurality of L 1 may be the same or different. Y is a monovalent hydrolyzable group. b1 is an integer of 2 to 6. Multiple Ys may be the same or different. 1 is a ligand or organic group that does not fall under Y.

[0118] The metal atom represented by M is preferably a first metal atom, more preferably tin.

[0119] The hydrolyzable group represented by Y can be appropriately changed depending on the metal atom represented by M, and examples thereof include a substituted or unsubstituted ethynyl group, a halogen atom, an alkoxy group, an acyloxy group, and a substituted or unsubstituted amino group.

[0120] As the substituent in the substituted or unsubstituted ethynyl group and the substituted or unsubstituted amino group represented by Y, a monovalent hydrocarbon group having 1 to 20 carbon atoms is preferable, a chain hydrocarbon group is more preferable, and an alkyl group is even more preferable.

[0121] Examples of the halogen atom represented by Y include a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, etc. Among these, a chlorine atom is preferred.

[0122] Examples of the alkoxy group represented by Y include a methoxy group, an ethoxy group, an n-propoxy group, an i-propoxy group, an n-butoxy group, etc. Among these, an ethoxy group, an i-propoxy group, and an n-butoxy group are preferred.

[0123] Examples of the acyloxy group represented by Y include a formyl group, an acetoxy group, an ethyryloxy group, a propionyloxy group, an n-butyryloxy group, a t-butyryloxy group, a t-amylyloxy group, an n-hexanecarbonyloxy group, an n-octanecarbonyloxy group, etc. Among these, an acetoxy group is preferred.

[0124] Examples of the substituted or unsubstituted amino group represented by Y include an amino group, a methylamino group, a dimethylamino group, a diethylamino group, a dipropylamino group, etc. Among these, a dimethylamino group and a diethylamino group are preferred.

[0125] Hereinafter, a preferred combination of a metal atom represented by M and a hydrolyzable group represented by Y will be described. When the metal atom represented by M is tin, the hydrolyzable group represented by Y is preferably a substituted or unsubstituted ethynyl group, a halogen atom, an alkoxy group, an acyloxy group, and a substituted or unsubstituted amino group, and more preferably a halogen atom. When the metal atom represented by M is germanium, the hydrolyzable group represented by Y is preferably a halogen atom, an alkoxy group, an acyloxy group, and a substituted or unsubstituted amino group. When the metal atom represented by M is hafnium, zirconium, or titanium, the hydrolyzable group represented by Y is preferably a halogen atom, an alkoxy group, or an acyloxy group.

[0126] L 1 The ligand represented by the formula (I) includes a monodentate ligand and a polydentate ligand.

[0127] Examples of the monodentate ligand include a hydroxo ligand, a nitro ligand, and ammonia.

[0128] Examples of the polydentate ligand include hydroxy acid esters, β-diketones, β-ketoesters, malonic acid diesters in which the carbon atom at the α-position may be substituted, and hydrocarbons having a π bond, or ligands derived from these compounds, and diphosphines.

[0129] Examples of the diphosphines include 1,1-bis(diphenylphosphino)methane, 1,2-bis(diphenylphosphino)ethane, 1,3-bis(diphenylphosphino)propane, 2,2'-bis(diphenylphosphino)-1,1'-binaphthyl, and 1,1'-bis(diphenylphosphino)ferrocene.

[0130] L 1 Examples of the monovalent organic group represented by the formula (1-1) and the formula (1-2) include the same groups as those exemplified as the monovalent organic group having 1 to 20 carbon atoms represented by Y. 1 The lower limit of the number of carbon atoms of the monovalent organic group represented by the formula (I) is preferably 2, more preferably 3. On the other hand, the upper limit of the number of carbon atoms is preferably 10, more preferably 5. 1 The monovalent organic group represented by the formula (I) is preferably a substituted or unsubstituted hydrocarbon group, more preferably a substituted or unsubstituted chain hydrocarbon group or a substituted or unsubstituted aromatic hydrocarbon group, further preferably a substituted or unsubstituted alkyl group or a substituted or unsubstituted aralkyl group, and particularly preferably an isopropyl group or a benzyl group.

[0131] As a1, 1 and 2 are preferred, and 1 is more preferred.

[0132] b1 is preferably an integer of 2 to 4. By setting b1 to the above value, the content of metal atoms in the [P] metal-containing compound can be increased, and the generation of secondary electrons by the [P] metal-containing compound can be more effectively promoted. As a result, the pattern rectangularity can be improved.

[0133] The metal compound (1) is preferably a metal halide compound, more preferably isopropyltin trichloride or benzyltin trichloride.

[0134] Examples of methods for carrying out the hydrolysis condensation reaction of metal compound (1) include stirring metal compound (1) in water or a solvent containing water in the presence of a base such as tetramethylammonium hydroxide, which is used as needed. In this case, other compounds having hydrolyzable groups may be added as needed. The lower limit of the amount of water used in this hydrolysis condensation reaction is preferably 0.2 times by mole, more preferably 1 time by mole, and even more preferably 3 times by mole, relative to the hydrolyzable groups of metal compound (1) or the like. By setting the amount of water in the hydrolysis condensation reaction within the above range, the metal-containing compound [P] can be efficiently obtained.

[0135] [P] In the synthesis reaction of the metal-containing compound, in addition to the metal compound (1), L in the compound of the above formula (4) 1 Alternatively, a compound capable of becoming a multidentate ligand represented by the formula (I) or a compound capable of becoming a bridging ligand may be added. Examples of the compound capable of becoming a bridging ligand include compounds having two or more coordinating groups such as a hydroxy group, an isocyanate group, an amino group, an ester group, and an amide group.

[0136] The lower limit of the temperature for the synthesis reaction of the metal-containing compound (P) is preferably 0° C., more preferably 10° C. The upper limit of the temperature is preferably 150° C., more preferably 100° C., and even more preferably 50° C.

[0137] The lower limit of the synthesis reaction time of the metal-containing compound [P] is preferably 1 minute, more preferably 10 minutes, and even more preferably 1 hour.The upper limit of the synthesis reaction time is preferably 100 hours, more preferably 50 hours, even more preferably 24 hours, and particularly preferably 4 hours.

[0138] (Solvent [Q]) The solvent [Q] is preferably an organic solvent. Specific examples of this organic solvent include the same solvents as those exemplified as the solvent [B] in the above-mentioned metal-containing resist underlayer film-forming composition.

[0139] [Q] The solvent is preferably an ether solvent, and more preferably propylene glycol monoethyl ether.

[0140] (Other Optional Components) The composition for forming a metal-containing resist film may contain other optional components, such as a compound that can serve as a ligand, a surfactant, and the like, in addition to the metal-containing compound (P) and the solvent (Q).

[0141] (Compound that can serve as a ligand) Examples of the compound that can serve as a ligand include compounds that can serve as multidentate ligands or bridging ligands, and specific examples thereof include the same compounds that can serve as multidentate ligands or bridging ligands as exemplified in the synthesis method for the metal-containing compound [P].

[0142] (Surfactant) The surfactant is a component that acts to improve the coatability, striations, etc. Examples of the surfactant include nonionic surfactants such as polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene oleyl ether, polyoxyethylene n-octylphenyl ether, polyoxyethylene n-nonylphenyl ether, polyethylene glycol dilaurate, and polyethylene glycol distearate, as well as commercial surfactants such as KP341 (Shin-Etsu Chemical Co., Ltd.), Polyflow No. 75, and Polyflow No. 85 (Shin-Etsu Chemical Co., Ltd.). 95 (all manufactured by Kyoeisha Chemical Co., Ltd.), F-Top EF301, EF303, EF352 (all manufactured by Tochem Products Co., Ltd.), Megafac F171, F173 (all manufactured by Dainippon Ink and Chemicals, Inc.), Fluorad FC430, FC431 (all manufactured by Sumitomo 3M Limited), Asahiguard AG710, Surflon S-382, Surflon SC-101, SC-102, SC-103, SC-104, SC-105, SC-106 (all manufactured by Asahi Glass Co., Ltd.), and the like.

[0143] (Method for Preparing a Composition for Forming a Metal-Containing Resist Film) The composition for forming a metal-containing resist film can be prepared, for example, by mixing the metal-containing compound [P] and, if necessary, other optional components such as the solvent [Q] in a predetermined ratio, and preferably filtering the resulting mixture through a membrane filter with a pore size of 0.4 μm or less. When the composition for forming a metal-containing resist film contains the metal-containing compound [P] and the solvent [Q], the content of the metal-containing compound [P] in the components other than the solvent [Q] in the composition for forming a metal-containing resist film is preferably 50% by mass or more. The lower limit of the content of the metal-containing compound [P] is more preferably 60% by mass, and even more preferably 70% by mass. On the other hand, the upper limit of the content is preferably 100% by mass, but may be 98% by mass or even 95% by mass.

[0144] [Exposure Step] In this step, the metal-containing resist film formed in the above-mentioned metal-containing resist film-forming composition coating step is exposed to extreme ultraviolet light (wavelength 13.5 nm, etc., also referred to as "EUV"). This step generates a difference in solubility in a developer between the exposed and unexposed areas of the resist film. The exposure conditions can be appropriately determined depending on the type of resist film-forming composition used, etc.

[0145] Furthermore, in this process, after the exposure, post-exposure baking (hereinafter also referred to as "PEB") can be performed to improve the performance of the resist film, such as resolution, pattern profile, and developability. The PEB temperature and PEB time can be appropriately determined depending on the type of resist film-forming composition used, etc. The lower limit of the PEB temperature is preferably 50°C, more preferably 70°C. The upper limit of the PEB temperature is preferably 200°C, more preferably 150°C. The lower limit of the PEB time is preferably 10 seconds, more preferably 30 seconds. The upper limit of the PEB time is preferably 600 seconds, more preferably 300 seconds.

[0146] [Development Step] In this step, at least the exposed metal-containing resist film is developed. Examples of the developer used for this development include an alkaline aqueous solution (alkaline developer), an organic solvent-containing solution (organic solvent developer), and the like. For example, in the case of a positive resist pattern using an alkaline developer, the solubility of the exposed portion of the metal-containing resist film in an alkaline aqueous solution is increased, so that the exposed portion is removed by alkaline development to form a positive resist pattern. In addition, in the case of a negative resist pattern using an organic solvent developer, the solubility of the exposed portion of the metal-containing resist film in an organic solvent is decreased, so that the unexposed portion, which has a relatively high solubility in an organic solvent, is removed by organic solvent development to form a negative resist pattern.

[0147] The developer used in alkaline development is not particularly limited, and known developers can be used. Examples of developers for alkaline development include alkaline aqueous solutions in which at least one alkaline compound such as sodium hydroxide, potassium hydroxide, sodium carbonate, sodium silicate, sodium metasilicate, aqueous ammonia, ethylamine, n-propylamine, diethylamine, di-n-propylamine, triethylamine, methyldiethylamine, ethyldimethylamine, triethanolamine, tetramethylammonium hydroxide (TMAH), pyrrole, piperidine, choline, 1,8-diazabicyclo-[5.4.0]-7-undecene, and 1,5-diazabicyclo-[4.3.0]-5-nonene is dissolved. Among these, a TMAH aqueous solution is preferred, and a 2.38 mass % TMAH aqueous solution is more preferred.

[0148] In addition, when organic solvent development is performed, examples of the developer include the same solvents as those exemplified as the solvents in the above-mentioned metal-containing resist underlayer film-forming composition, etc. As the organic solvent, ketone-based solvents and ester-based solvents are preferred, and 2-heptanone and propylene glycol monomethyl ether acetate are more preferred.

[0149] The development of the exposed metal-containing resist film is preferably an organic solvent development.

[0150] In this step, washing and / or drying may be carried out after the development.

[0151] [Metal-Containing Resist Underlayer Film Pattern Forming Step] In this step, the metal-containing resist underlayer film is etched using the resist pattern as a mask to form a metal-containing resist underlayer film pattern.

[0152] The etching may be either dry etching or wet etching, but dry etching is preferred.

[0153] Dry etching can be carried out using, for example, a known dry etching apparatus. The etching gas used for dry etching can be appropriately selected depending on the elemental composition of the metal-containing resist underlayer film to be etched, and for example, CHF 3 , C.F. 4 , C 2 F 6 , C 3 F 8 , SF 6 Fluorine-based gases such as Cl 2 , BCl 3 Chlorine gases such as O 2 , O 3 , H 2 Oxygen-based gases such as O, H 2 , N.H. 3 , CO, CO 2 , C.H. 4 , C 2 H 2 , C 2 H 4 , C 2 H 6 , C 3 H 4 , C 3 H 6 , C 3 H 8 , reducing gases such as HF, HI, HBr, HCl, and NO, He, N 2 Inert gases such as Ar and the like are used. These gases can also be used in combination. For dry etching of metal-containing resist underlayer films, fluorine-based gases are usually used, and mixtures of these with oxygen-based gases and inert gases are preferably used.

[0154] [Etching Step] In this step, etching is performed using the above-mentioned metal-containing resist underlayer film pattern as a mask. More specifically, etching is performed one or more times using the pattern formed in the metal-containing resist underlayer film obtained in the above-mentioned metal-containing resist underlayer film pattern forming step as a mask to obtain a patterned substrate.

[0155] When an organic underlayer film is formed on a substrate, a pattern of the organic underlayer film is formed by etching the organic underlayer film using the metal-containing resist underlayer film pattern as a mask, and then a pattern is formed on the substrate by etching the substrate using this organic underlayer film pattern as a mask.

[0156] The etching may be either dry etching or wet etching, but dry etching is preferred.

[0157] Dry etching for forming a pattern in an organic underlayer film can be carried out using a known dry etching apparatus. The etching gas used in dry etching can be appropriately selected depending on the elemental composition of the metal-containing resist underlayer film and the organic underlayer film to be etched. The etching gas can be suitably selected from the above-mentioned gases used for etching the metal-containing resist underlayer film, and these gases can also be used in combination. An oxygen-based gas is usually used for dry etching of an organic underlayer film using a metal-containing resist underlayer film pattern as a mask.

[0158] Dry etching when forming a pattern on a substrate using an organic underlayer film pattern as a mask can be performed using a known dry etching device. The etching gas used for dry etching can be appropriately selected depending on the elemental composition of the organic underlayer film and the substrate to be etched, and examples include etching gases similar to those exemplified as etching gases used in dry etching of the metal-containing resist underlayer film. Etching can be performed multiple times using different etching gases. After the above etching, a semiconductor substrate having a predetermined pattern can be produced.

[0159] The metal-containing resist underlayer film-forming composition contains a compound [A] and a solvent [B]. As the composition, the metal-containing resist underlayer film-forming composition used in the above-mentioned method for producing a semiconductor substrate can be suitably used.

[0160] Examples will be described below. Note that the examples shown below are representative examples of the present invention, and should not be construed as narrowing the scope of the present invention.

[0161] In the present examples, the average molecular weights (Mw) of the compound (a) and the compound [A] as intermediates, the concentration of the solution of the compound [A], and the average thickness of the film were measured by the following methods.

[0162] [Weight-average molecular weight (Mw)] The weight-average molecular weight (Mw) of compounds (a-1) to (a-13) as compound (a) and compound [A] was measured by gel permeation chromatography (GPC) using GPC columns (two "G2000HXL", one "G3000HXL", and one "G4000HXL") manufactured by Tosoh Corporation under the following conditions: Eluent: tetrahydrofuran (Wako Pure Chemical Industries, Ltd.) Flow rate: 1.0 mL / min Sample concentration: 1.0 mass% Sample injection amount: 100 μL Column temperature: 40° C. Detector: differential refractometer Standard material: monodisperse polystyrene

[0163] [Concentration of the Solution of the Compound [A]] 0.5 g of the solution of the compound [A] was baked at 250°C for 30 minutes, and the mass of the residue obtained was measured. The mass of this residue was divided by the mass of the solution of the compound [A] to calculate the concentration (mass %) of the solution of the compound [A].

[0164] [Average Film Thickness] The average film thickness was measured using a spectroscopic ellipsometer (J.A. WOOLLAM "M2000D"). Specifically, the film thickness was measured at nine arbitrary positions at 5 cm intervals including the center of the film formed on the silicon wafer, and the average value of the film thicknesses was calculated to obtain the average thickness.

[0165] <Synthesis of Compounds (a-1) to (a-13)> The monomers used in the synthesis in Synthesis Examples 1-1 to 1-13 (hereinafter also referred to as "monomers (H-1), (S-1) to (S-9)") are shown below.

[0166]

[0167] Synthesis Example 1-1 (Synthesis of Compound (a-1)) 5.83 g of magnesium and 11.12 g of tetrahydrofuran were added to a nitrogen-purged reaction vessel and stirred at 20°C. Next, 17.38 g of monomer (H-1) and 14.94 g of monomer (S-1) (molar ratio: 50 / 50 (mol %)) were dissolved in 111.15 g of tetrahydrofuran to prepare a monomer solution. The temperature inside the reaction vessel was brought to 20°C, and the monomer solution was added dropwise over 1 hour with stirring. The completion of the dropwise addition was designated the start time of the reaction, and the mixture was stirred at 40°C for 1 hour and then at 60°C for 3 hours. Thereafter, 66.69 g of tetrahydrofuran was added, and the mixture was cooled to below 10°C, thereby obtaining a polymerization reaction liquid. Next, 30.36 g of triethylamine was added to this polymerization reaction liquid, and then 9.61 g of methanol was added dropwise over 10 minutes with stirring. The end of the dropwise addition was designated as the start time of the reaction. After stirring at 20°C for 1 hour, the reaction solution was poured into 220 g of diisopropyl ether, and the precipitated salt was filtered off. Next, tetrahydrofuran, diisopropyl ether, triethylamine, and methanol were removed from the filtrate using an evaporator. 50 g of diisopropyl ether was poured into the resulting residue, and the precipitated salt was filtered off. Diisopropyl ether was then added to the filtrate, yielding compound (a-1) with a concentration of 12% by mass. The Mw of compound (a-1) was 850.

[0168] Synthesis Examples 1-2 to 1-13 (Synthesis of Compounds (a-2) to (a-13)) Diisopropyl ether solutions of compounds (a-2) to (a-13) were obtained in the same manner as in Synthesis Example 1-1, except that the types and amounts of each monomer shown in Table 1 below were used. The Mw of the resulting compound (a) is also shown in Table 1. In Table 1, "-" indicates that the corresponding monomer was not used.

[0169]

[0170] <Synthesis of Compound [A]> The monomers used in the synthesis of Synthesis Examples 2-1 to 2-29 (hereinafter also referred to as "monomers (M-1) to (M-9)") are shown below. In the following Synthesis Examples 2-1 to 2-29, mol % refers to a value when the total number of moles of silicon atoms in the compounds (a-1) to (a-13) and monomers (M-1) to (M-9) used is taken as 100 mol %.

[0171]

[0172] Synthesis Example 2-1 (Synthesis of Compound (A-1)) To a reaction vessel were added 23.87 g of the diisopropyl ether solution of compound (a-1) obtained in Synthesis Example 1-1 above and 24.29 g of acetone. The temperature inside the reaction vessel was brought to 30°C, and 1.84 g of a 3.2% by mass aqueous oxalic acid solution was added dropwise over 20 minutes with stirring. The reaction started when the dropwise addition was completed, and the mixture was stirred at 40°C for 4 hours, after which the temperature inside the reaction vessel was cooled to 30°C or below. Next, 25.0 g of diisopropyl ether and 150 g of water were added to the reaction vessel, and extraction was performed. 75 g of propylene glycol monomethyl ether acetate was added to the resulting organic layer, and the water, acetone, diisopropyl ether, alcohols produced by the reaction, and excess propylene glycol monomethyl ether acetate were removed using an evaporator. Next, 5.0 g of trimethyl orthoformate as a dehydrating agent was added to the resulting solution, and the mixture was allowed to react at 40°C for 1 hour, after which the temperature inside the reaction vessel was cooled to 30°C or below. The alcohols, esters, trimethyl orthoformate, and excess propylene glycol monomethyl ether acetate produced by the reaction were removed using an evaporator, yielding a 5% by mass solution of compound (A-1) as compound [A]. The Mw of compound (A-1) was 1,800.

[0173] Synthesis Examples 2-2 to 2-29 (Synthesis of Compounds (A-2) to (A-26) and (AJ-1) to (AJ-3)) Solutions of propylene glycol monomethyl ether acetate or propylene glycol monoethyl ether of compounds (A-2) to (A-26) and (AJ-1) to (AJ-3) as compound [A] were obtained in the same manner as in Synthesis Example 2-1, except that the types and amounts of each compound and each monomer shown in Table 2 below were used. In Table 2 below, a "-" next to a monomer indicates that the corresponding monomer was not used. The concentrations (% by mass) of the obtained solutions of compound [A] and the Mw of compound [A] are also shown in Table 2.

[0174]

[0175] <Preparation of metal-containing resist underlayer film-forming composition> The components used in preparing the metal-containing resist underlayer film-forming composition are shown below. Note that in the following Examples 1-1 to 1-32 and Comparative Examples 1-1 to 1-3, unless otherwise specified, parts by mass indicate values ​​where the total mass of the components used is 100 parts by mass.

[0176] [[A] Compounds (including comparative compounds)] A-1 to A-26: Compounds (A-1) to (A-26) synthesized above AJ-1 to AJ-3: Compounds (AJ-1) to (AJ-3) synthesized above for comparison

[0177] [B] Solvents: B-1: Propylene glycol monomethyl ether acetate B-2: Propylene glycol monomethyl ether

[0178] [C] Other optional components C-1 (orthoester): trimethyl orthoformate C-2 (acid generator): compound represented by the following formula (C-2) (wherein "Bu" represents an n-butyl group) C-3 (basic compound): compound represented by the following formula (C-3)

[0179]

[0180] Example 1-1 Preparation of Composition (J-1) 0.50 parts by mass of (A-1) as the [A] compound (excluding the solvent) and 99.50 parts by mass of (B-1) as the [B] solvent (including the solvent (B-1) contained in the solution of the [A] compound) were mixed, and the resulting solution was filtered through a polytetrafluoroethylene (PTFE) membrane filter having a pore size of 0.2 μm to prepare a silicon-containing composition (J-1).

[0181] [Examples 1-2 to 1-32, Comparative Examples 1-1 to 1-3] (Preparation of compositions (J-2) to (J-32) and (j-1) to (j-3)) Compositions (J-2) to (J-32) of Examples 1-2 to 1-32 and compositions (j-1) to (j-3) of Comparative Examples 1-1 to 1-3 were prepared in the same manner as in Example 1-1, except that the types and amounts of each component shown in Table 3 below were used. In Table 3 below, "-" indicates that the corresponding component was not used.

[0182] <Evaluation> Using the metal-containing resist underlayer film-forming compositions prepared above, the rectangularity of resist patterns was evaluated by the following method. The evaluation results are shown in Table 3 below.

[0183] <Preparation of Resist Composition (R-1)>

[0184] [Synthesis of Metal-Containing Compound] Compound (S-1), which was used as a metal-containing compound in preparing resist composition (R-1), was synthesized by the following procedure. In a reaction vessel, 6.5 parts by mass of isopropyltin trichloride was added to 150 mL of 0.5 N aqueous sodium hydroxide solution while stirring, and the mixture was stirred for 2 hours. The precipitate was collected by filtration, washed twice with 50 parts by mass of water, and then dried to obtain compound (S-1). Compound (S-1) was a hydroxide oxide product (i-PrSnO) of the hydrolysis product of isopropyltin trichloride. (3/2-x/2) (OH) x (where 0<x<3 is the structural unit).

[0185] 2 parts by mass of the compound (S-1) synthesized above and 98 parts by mass of propylene glycol monoethyl ether were mixed, and the resulting mixture was passed through an activated 4 Å molecular sieve to remove residual water, followed by filtration through a polytetrafluoroethylene (PTFE) membrane filter with a pore size of 0.2 μm to prepare resist composition (R-1).

[0186] [Resist Pattern Rectangularity (EUV Exposure)] An organic underlayer film-forming material ("HM8006" manufactured by JSR Corporation) was applied onto a 12-inch silicon wafer by spin coating using a spin coater ("CLEAN TRACK ACT12" manufactured by Tokyo Electron Limited), and then heated at 250°C for 60 seconds to form an organic underlayer film with an average thickness of 100 nm. The metal-containing resist underlayer film-forming composition prepared above was applied onto this organic underlayer film, and then heated at 220°C for 60 seconds, and then cooled at 23°C for 30 seconds to form a metal-containing resist underlayer film with an average thickness of 5 nm. Resist Composition (R-1) was applied onto this metal-containing resist underlayer film by spin coating using the spin coater, and after a predetermined time had elapsed, the resulting film was heated at 90°C for 60 seconds, and then cooled at 23°C for 30 seconds to form a resist film with an average thickness of 35 nm. EUV scanner (ASML's "TWINSCAN" The resist film was exposed to light using a NXE:3300B (NA 0.3, sigma 0.9, quadrupole illumination, 1:1 line and space mask with a line width of 25 nm on the wafer). After exposure, the substrate was heated at 110°C for 60 seconds and then cooled at 23°C for 60 seconds. The resist was then developed by the puddle method using Dev-1: 2-heptanone (20-25°C) or Dev-2: propylene glycol monomethyl ether acetate (20-25°C) as the developer, and then dried to obtain an evaluation substrate on which a resist pattern was formed. A scanning electron microscope (Hitachi High-Tech Corporation's "SU8220") was used to measure and observe the resist pattern of the evaluation substrate. The pattern rectangularity was evaluated as "A" (good) if the cross-sectional shape of the pattern was rectangular, "B" (fairly good) if the cross-sectional shape of the pattern had a footing, and "C" (poor) if there were residues (defects) in the pattern.

[0187]

[0188] As is clear from the results in Table 3 above, the metal-containing resist underlayer films formed from the compositions of the Examples were able to exhibit superior pattern rectangularity compared to the metal-containing resist underlayer films formed from the compositions of the Comparative Examples.

[0189] The method for producing a semiconductor substrate and the metal-containing resist underlayer film-forming composition of the present invention enable the formation of a metal-containing resist underlayer film having excellent pattern rectangularity, and therefore can be suitably used in the production of semiconductor substrates, etc.

Claims

a step of applying a metal-containing resist underlayer film-forming composition directly or indirectly to a substrate; a step of applying a metal-containing resist film-forming composition to the metal-containing resist underlayer film formed by the step of applying the metal-containing resist underlayer film-forming composition; a step of exposing the metal-containing resist film formed by the step of applying the metal-containing resist film-forming composition to extreme ultraviolet light; and a step of developing at least the exposed metal-containing resist film, wherein the metal-containing resist underlayer film-forming composition contains: a compound having at least one structural unit selected from the group consisting of a structural unit (α-1) represented by the following formula (1-1) and a structural unit (α-2) represented by the following formula (1-2); and a solvent, and the total content of the structural unit (α-1) and the structural unit (α-2) relative to all structural units constituting the compound is 50 mol % or more and 100 mol % or less. (In formula (1-1), X is a monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms or a monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms substituted with at least one halogen atom. a is an integer from 1 to 3. When a is 2 or more, multiple Xs are the same or different. Y is a monovalent organic group having 1 to 20 carbon atoms, a hydroxyl group, or a halogen atom. b is an integer from 0 to 2. When b is 2, two Ys are the same or different. However, a+b is 3 or less. In formula (1-2), X is a monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms or a monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms substituted with at least one halogen atom. c is an integer from 1 to 3. When c is 2 or more, the multiple Xs are the same or different. Y is a monovalent organic group having 1 to 20 carbon atoms, a hydroxyl group, or a halogen atom. d is an integer from 0 to 2. When d is 2, the two Ys are the same or different. R 0 is a substituted or unsubstituted divalent hydrocarbon group having 1 to 20 carbon atoms bonded to two silicon atoms. p is an integer of 1 to 3. When p is 2 or more, multiple R 0 are the same or different, provided that c+d+p is 4 or less.

2. The method for producing a semiconductor substrate according to claim 1, wherein the metal-containing resist underlayer film has a thickness of 6 nm or less.

3. The method for producing a semiconductor substrate according to claim 1 or 2, wherein the total content of the structural unit (α-1) and the structural unit (α-2) relative to all structural units constituting the compound is 60 mol % or more and 100 mol % or less.

4. A method for producing a semiconductor substrate as described in claim 1 or claim 2, wherein the composition for forming a metal-containing resist film contains a metal-containing compound and a solvent, and the content of the metal compound in the composition for forming a metal-containing resist film in components other than the solvent is 50 mass % or more.

5. The method for producing a semiconductor substrate according to claim 1 or 2, wherein the exposed metal-containing resist film is developed using an organic solvent.

6. A composition for forming an underlayer film for a metal-containing resist, comprising: a compound having at least one structural unit selected from the group consisting of a structural unit (α-1) represented by the following formula (1-1) and a structural unit (α-2) represented by the following formula (1-2); and a solvent, wherein the total content of the structural unit (α-1) and the structural unit (α-2) relative to all structural units constituting the compound is 50 mol % or more and 100 mol % or less. (In formula (1-1), X is a monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms or a monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms substituted with at least one halogen atom. a is an integer from 1 to 3. When a is 2 or more, multiple Xs are the same or different. Y is a monovalent organic group having 1 to 20 carbon atoms, a hydroxyl group, or a halogen atom. b is an integer from 0 to 2. When b is 2, two Ys are the same or different. However, a+b is 3 or less. In formula (1-2), X is a monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms or a monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms substituted with at least one halogen atom. c is an integer from 1 to 3. When c is 2 or more, the multiple Xs are the same or different. Y is a monovalent organic group having 1 to 20 carbon atoms, a hydroxyl group, or a halogen atom. d is an integer from 0 to 2. When d is 2, the two Ys are the same or different. R 0is a substituted or unsubstituted divalent hydrocarbon group having 1 to 20 carbon atoms bonded to two silicon atoms. p is an integer of 1 to 3. When p is 2 or more, multiple R 0 are the same or different, provided that c+d+p is 4 or less.

7. The metal-containing resist underlayer film forming composition according to claim 6, which is used for forming a metal-containing resist underlayer film having a film thickness of 6 nm or less.

8. The metal-containing resist underlayer film forming composition according to claim 6 or 7, wherein the total content of the structural unit (α-1) and the structural unit (α-2) relative to all structural units constituting the compound is 60 mol % or more and 100 mol % or less.

9. The metal-containing resist underlayer film forming composition according to claim 6 or 7, wherein in the above formulas (1-1) and (1-2), X is a monovalent linear aliphatic saturated hydrocarbon group having 1 to 5 carbon atoms or a monovalent alicyclic saturated hydrocarbon group having 3 to 6 carbon atoms.

10. A metal-containing resist underlayer film forming composition according to claim 6 or claim 7, wherein the composition for forming a metal-containing resist film contains a metal compound and a solvent, and the content of the metal compound in the components other than the solvent in the composition for forming a metal-containing resist film is 50 mass% or more.

Citation Information

Patent Citations

  • Resist underlayer film forming composition and semiconductor substrate production method

    WO2021215240A1

  • Composition for forming resist underlying film

    WO2021221171A1

  • Composition for forming silicon-containing resist underlayer film

    WO2022260154A1