Method for confirming reinforcing state of reinforcing member with respect to structure

The method employs a glass fiber sheet with (meth)acrylic and epoxy resin parts to visually confirm reinforcement state through discoloration, addressing the challenge of assessing reinforcement status in structures by indicating stress distribution and peeling progress without separating the member.

WO2024203402A1PCT designated stage expired Publication Date: 2024-10-03DENKA CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010075
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-14
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing methods for confirming the reinforcement status of reinforcing members in structures, such as concrete, are not straightforward and may fail to accurately assess the stress distribution and peeling progress without separating the member from the structure.

Method used

A method using a glass fiber sheet with a first resin part containing a cured product of a (meth)acrylic compound and a second resin part containing a cured product of an epoxy compound, where discoloration indicates stress generation, allowing for visual confirmation of the reinforcement state without treating the member.

Benefits of technology

Enables simple and effective visualization of the reinforcement state, including stress distribution and peeling progress, without separating the reinforcing member from the structure, providing excellent visibility and reinforcing effectiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010075_03102024_PF_FP_ABST
    Figure JP2024010075_03102024_PF_FP_ABST
Patent Text Reader

Abstract

This method for confirming a reinforcing state of a reinforcing member 100 with respect to a structure comprises a step for confirming the reinforcing state on the basis of discoloration of the reinforcing member 100 when stress occurs in the reinforcing member 100, wherein the reinforcing member 100 includes: a glass fiber sheet 10; a first resin part 20 covering the glass fiber sheet 10; and a second resin part 30 covering the first resin part 20. The first resin part 20 contains a cured product of a (meth)acrylic compound, and the second resin part 30 contains a cured product of an epoxy compound.
Need to check novelty before this filing date? Find Prior Art

Description

Method for checking the reinforcement condition of a reinforcing member for a structure

[0001] The present invention relates to a method for checking the reinforcement state of a structure by a reinforcing member.

[0002] Conventionally, various measures have been taken to reinforce structures such as concrete structures. For example, Patent Document 1 below describes the formation of a high-strength coating film on the surface of concrete. Patent Document 2 below describes a reinforcement coating method for forming a coating layer containing a continuous glass fiber sheet.

[0003] JP 2005-15329 A JP 2010-1707 A

[0004] When a structure is reinforced using a reinforcing member, the state of the reinforcing member may change due to deformation of the reinforcing member, external pressure, etc., which may cause the reinforcing member to peel off from the structure, making it impossible to maintain a good reinforcement state. In such cases, when a structure is reinforced using a reinforcing member, it is necessary to check the reinforcing state of the reinforcing member using a simple method.

[0005] An object of one aspect of the present invention is to provide a method for checking a reinforcement state that enables checking the reinforcement state of a structure by a reinforcing member in a simple manner.

[0006] In some aspects, the present invention relates to the following [1] to [4], etc. [1] A method for confirming the reinforcement state of a reinforcing member for a structure, comprising a step of confirming the reinforcement state based on discoloration of the reinforcing member when stress is generated in the reinforcing member, the reinforcing member comprising a glass fiber sheet, a first resin part covering at least a portion of the glass fiber sheet, and a second resin part covering at least a portion of the first resin part, the first resin part containing a cured product of a (meth)acrylic compound, and the second resin part containing a cured product of an epoxy compound. [2] The glass fiber sheet has a basis weight of 100 to 1000 g / m 2[3] The method for checking a reinforcement state according to [1] or [2], wherein the tensile modulus of the reinforcing member is 50 to 150 GPa. [4] The method for checking a reinforcement state according to any one of [1] to [3], wherein the structure is a concrete structure.

[0007] According to one aspect of the present invention, it is possible to provide a method for checking a reinforcement state that enables checking the reinforcement state of a structure by a reinforcing member using a simple technique.

[0008] Fig. 1 is a cross-sectional view showing an example of a reinforcing member. Fig. 2 is a view showing a connecting body used in appearance evaluation. Fig. 3 is a view showing a photograph when the reinforcing member of the connecting body is observed. Fig. 4 is a view showing a photograph when the reinforcing member of the connecting body is observed. Fig. 5 is a view showing a photograph when the reinforcing member of the connecting body is observed.

[0009] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to the following embodiments.

[0010] In this specification, a numerical range "A or greater" means a range exceeding A and A. A numerical range "A or less" means a range exceeding A and A. In the numerical ranges described in this specification, the upper or lower limit of a certain numerical range can be arbitrarily combined with the upper or lower limit of another numerical range. In the numerical ranges described in this specification, the upper or lower limit of the numerical range may be replaced with a value shown in the examples. "A or B" may include either A or B, or both. Unless otherwise specified, the materials exemplified in this specification can be used alone or in combination of two or more. When multiple substances corresponding to each component are present in the composition, the content of each component in the composition refers to the total amount of the multiple substances present in the composition, unless otherwise specified. The term "process" does not only refer to an independent process, but also includes processes that cannot be clearly distinguished from other processes as long as the intended effect of the process is achieved. The term "(meth)acrylic compound" refers to at least one of an acrylic compound and the corresponding methacrylic compound. The same applies to other similar expressions such as "(meth)acryloyl group." The spectral transmittance in this specification can be measured using, for example, a "UV-VIS-NIR spectrophotometer SolidSpec-3700i" manufactured by Shimadzu Corporation.

[0011] The method for checking a reinforcement state according to this embodiment is a method for checking the reinforcement state of a reinforcing member relative to a structure. The "reinforcing state" in this embodiment refers to the state of stress distribution acting on the structure, the degree of progress of peeling, and the like. The method for checking a reinforcement state according to this embodiment includes a reinforcement state checking step for checking the reinforcement state based on discoloration of the reinforcing member when stress is generated in the reinforcing member, wherein the reinforcing member includes a glass fiber sheet, a first resin part covering at least a portion of the glass fiber sheet, and a second resin part covering at least a portion of the first resin part, wherein the first resin part contains a cured product of a (meth)acrylic compound, and the second resin part contains a cured product of an epoxy compound.

[0012] The present inventors have discovered that a reinforcing member comprising a glass fiber sheet, a first resin portion, and a second resin portion, in which the first resin portion contains a cured product of a (meth)acrylic compound and the second resin portion contains a cured product of an epoxy compound, is prone to discoloration (e.g., clouding) when stress is generated in the reinforcing member, and have found that the discoloration of the reinforcing member when stress is generated in the reinforcing member can be used as an indicator to visualize the reinforcing state of the reinforcing member (stress distribution, degree of peeling, etc.).

[0013] According to the method for checking the reinforcement state of the present embodiment, the reinforcement state of the reinforcing member (stress distribution, degree of progress of peeling, etc.) is visualized using discoloration (e.g., clouding) of the reinforcing member when stress is generated in the reinforcing member as an indicator, and the reinforcement state can be checked simply by checking the discoloration of the reinforcing member, so that the reinforcement state of the reinforcing member can be checked by a simple method. According to the method for checking the reinforcement state of the present embodiment, the reinforcement state of the reinforcing member can be checked without performing any treatment on the reinforcing member (e.g., treatment to separate the reinforcing member from the structure) in order to check the reinforcement state of the reinforcing member.

[0014] According to the method for checking the reinforcement state of this embodiment, by using a glass fiber sheet as the fiber sheet, it is easier to visually check the base placed under the reinforcing member than when using other fiber sheets such as a carbon fiber sheet, and excellent visibility of the base can be obtained.

[0015] In the reinforcement state confirmation step, the reinforcement state is confirmed based on discoloration of the reinforcement member when stress is generated in the reinforcement member. The stress generated in the reinforcement member is not particularly limited, and may be stress generated due to deformation of the reinforcement member or stress generated due to external pressure. The discoloration of the reinforcement member may be clouding (whitening) of the reinforcement member.

[0016] In the reinforcement state confirmation process, the reinforcement state of the reinforcing member placed on the surface of the structure can be confirmed. However, when the above-mentioned reinforcing member including a glass fiber sheet, a first resin part, and a second resin part is used, the discoloration phenomenon of the reinforcing member can be confirmed by generating stress in the reinforcing member without placing the reinforcing member on the surface of the structure. The material, shape, and dimensions of the structure are not particularly limited. The structure may be a concrete structure.

[0017] The reinforcing member includes a glass fiber sheet. The composition of the glass constituting the glass fiber sheet is not particularly limited, and examples thereof include E-glass, AR-glass, S-glass, C-glass, D-glass, and ECR-glass. The glass fiber sheet may be a woven fiber fabric. Examples of the weave of the woven fiber fabric include plain weave, twill weave, satin weave, and rib weave.

[0018] The fineness of the glass fiber sheet may be 50 tex or more, 100 tex or more, 500 tex or more, 1000 tex or more, 1500 tex or more, or 2000 tex or more, from the viewpoint that openings are likely to be formed between the fibers, which facilitates impregnation with the resin material and improves workability. The fineness of the glass fiber sheet may be 5000 tex or less, 4000 tex or less, 3000 tex or less, or 2500 tex or less, from the viewpoint that handleability is likely to improve due to an increased fiber density. From these viewpoints, the fineness of the glass fiber sheet may be 50 to 5,000 tex, 50 to 4,000 tex, 50 to 3,000 tex, 500 to 5,000 tex, 500 to 4,000 tex, 500 to 3,000 tex, 1,500 to 5,000 tex, 1,500 to 4,000 tex, or 1,500 to 3,000 tex. The fineness may be an average fineness, and the average fineness may be an average value of five measurement points.

[0019] The basis weight of the glass fiber sheet (the content of the glass fiber sheet in the reinforcing member) may be in the following range: From the viewpoint of the reinforcing member being easily discolored (e.g., becoming cloudy) when stress is applied to the reinforcing member, and from the viewpoint of easily obtaining excellent strength and elongation, the basis weight of the glass fiber sheet is 100 g / m 2 Above, 150g / m 2 Above, 200g / m 2Above, 250g / m 2 Above, 300g / m 2 Above, 350g / m 2 Above, 400g / m 2 Above, 450g / m 2 Above, 500g / m 2 Above, 550g / m 2 Above, 600g / m 2 or more, or 650 g / m 2 The weight of the glass fiber sheet may be 1000 g / m or more from the viewpoint that the reinforcing member is likely to discolor (for example, become cloudy) when stress is applied to the reinforcing member, and from the viewpoint that excellent visibility of the base can be easily obtained. 2 Below, 950g / m 2 Below, 900g / m 2 Below, 850g / m 2 Below, 800g / m 2 Below, 750g / m 2 Below, 700g / m 2 or less, or 650 g / m 2 From these viewpoints, the weight per unit area of ​​the glass fiber sheet may be 100 to 1000 g / m 2 , 100-900g / m 2 , 100-800g / m 2 , 300~1000g / m 2 , 300-900g / m 2 , 300-800g / m 2 , 500-1000g / m 2 , 500-900g / m 2 , or 500 to 800 g / m 2 It may be.

[0020] The thickness of the glass fiber sheet in the reinforcing member may be within the following ranges. From the viewpoint of easily obtaining a sufficient reinforcing effect of the reinforcing member, the thickness of the glass fiber sheet may be 50 μm or more, 100 μm or more, 120 μm or more, 150 μm or more, or 170 μm or more. From the viewpoint of easily obtaining excellent substrate visibility, the thickness of the glass fiber sheet may be 400 μm or less, 350 μm or less, 300 μm or less, 250 μm or less, or 200 μm or less. From these viewpoints, the thickness of the glass fiber sheet may be 50 to 400 μm, 50 to 300 μm, 50 to 200 μm, 100 to 400 μm, 100 to 300 μm, 100 to 200 μm, 150 to 400 μm, 150 to 300 μm, or 150 to 200 μm. The thickness of the glass fiber sheet may be an average thickness, and the average thickness may be an average value of six measurement points. When the glass fiber sheet is a fiber fabric of intersecting threads (for example, a plain woven fiber fabric having warp threads and weft threads), the average thickness may be an average value of six measurement points in total, including three points at the intersections of the threads and three points at the non-intersections of the threads.

[0021] The content of the glass fiber sheet in the reinforcing member may be within the following ranges based on the total amount of the reinforcing member. From the viewpoint of easily obtaining a sufficient reinforcing effect of the reinforcing member, the content of the glass fiber sheet may be 15% by mass or more, 20% by mass or more, 25% by mass or more, 30% by mass or more, 35% by mass or more, 40% by mass or more, or 45% by mass or more. From the viewpoint of easily obtaining excellent substrate visibility, the content of the glass fiber sheet may be 75% by mass or less, 70% by mass or less, 65% by mass or less, 60% by mass or less, 55% by mass or less, or 50% by mass or less. From these viewpoints, the content of the glass fiber sheet may be 15 to 75% by mass, 15 to 65% by mass, 15 to 55% by mass, 30 to 75% by mass, 30 to 65% by mass, 30 to 55% by mass, 40 to 75% by mass, 40 to 65% by mass, or 40 to 55% by mass.

[0022] The reinforcing member includes a first resin portion covering at least a portion of the glass fiber sheet. The first resin portion may cover a portion of the glass fiber sheet (a portion of the glass fiber sheet may be exposed from the first resin portion), or may cover the entire glass fiber sheet. The first resin portion may be layer-shaped.

[0023] The first resin portion contains a cured product of a (meth)acrylic compound. The (meth)acrylic compound is a compound having a (meth)acryloyl group. According to the findings of the present inventors, when the first resin portion contains a cured product of the (meth)acrylic compound, the reinforcing member (particularly the first resin portion) is likely to discolor (e.g., become cloudy) when stress is generated in the reinforcing member.

[0024] The content of the cured product of the (meth)acrylic compound in the first resin part may be 50% by mass or more, 60% by mass or more, 70% by mass or more, 80% by mass or more, or 90% by mass or more based on the entire first resin part, from the viewpoint that the reinforcing member is likely to discolor (e.g., become cloudy) when stress is applied to the reinforcing member. The first resin part may be substantially composed of the cured product of the (meth)acrylic compound (an embodiment in which substantially 100% by mass of the first resin part is the cured product of the (meth)acrylic compound).

[0025] The first resin part may contain components other than the cured product of the (meth)acrylic compound, such as fillers, curing accelerators, curing retarders, light stabilizers, light absorbers, antioxidants, anti-degradants, pigments, dyes, silane coupling agents, antifoaming agents, leveling agents, dispersants, rheology control agents, waxes, etc.

[0026] The spectral transmittance in the visible light region (e.g., wavelength 550 nm) per 0.5 mm thickness of the first resin part may be 30% or more, 40% or more, 50% or more, 60% or more, 70% or more, 75% or more, 80% or more, 85% or more, or 90% or more, from the viewpoint of easily obtaining excellent substrate visibility.

[0027] The thickness of the first resin portion in the reinforcing member (thickness in the direction perpendicular to the surface of the glass fiber sheet) may be within the following ranges. The thickness of the first resin portion may be 50 μm or more, 100 μm or more, 150 μm or more, or 200 μm or more, from the viewpoint of easily obtaining a sufficient reinforcing effect of the reinforcing member and easily improving the handleability of the reinforcing member. The thickness of the first resin portion may be 400 μm or less, 350 μm or less, 300 μm or less, 250 μm or less, or 200 μm or less, from the viewpoint of easily obtaining excellent substrate visibility and easily improving the handleability of the reinforcing member. From these viewpoints, the thickness of the first resin portion may be 50 to 400 μm, 50 to 300 μm, 50 to 250 μm, 100 to 400 μm, 100 to 300 μm, 100 to 250 μm, 150 to 400 μm, 150 to 300 μm, or 150 to 250 μm. The thickness of the first resin portion may be an average thickness, and the average thickness may be an average value of values ​​measured at three points.

[0028] The content of the first resin portion in the reinforcing member may be in the following range: From the viewpoint of easily obtaining a sufficient reinforcing effect of the reinforcing member and easily improving the handleability of the reinforcing member, the content of the first resin portion is set to 50 g / m 2 Above, 100g / m 2 Above, 150g / m 2 or more, or 200 g / m 2 The content of the first resin part may be 400 g / m or more from the viewpoint of easily obtaining excellent visibility of the base and easily improving the handleability of the reinforcing member. 2 Below, 350g / m 2 Below, 300g / m 2 Below, 250g / m 2 or less than 200 g / m 2 From these viewpoints, the content of the first resin portion is 50 to 400 g / m 2 , 50-300g / m 2 , 50-250g / m 2 , 100-400g / m 2 , 100-300g / m 2 , 100-250g / m 2 , 150-400g / m 2 , 150-300g / m 2, or 150 to 250 g / m 2 It may be.

[0029] The content of the first resin portion in the reinforcing member may be within the following ranges based on the total amount of the reinforcing member. From the viewpoint of easily obtaining a sufficient reinforcing effect of the reinforcing member and easily improving the handleability of the reinforcing member, the content of the first resin portion may be 1% by mass or more, 3% by mass or more, 5% by mass or more, 8% by mass or more, 10% by mass or more, 12% by mass or more, or 14% by mass or more. From the viewpoint of easily obtaining excellent substrate visibility and easily improving the handleability of the reinforcing member, the content of the first resin portion may be 30% by mass or less, 25% by mass or less, 22% by mass or less, 20% by mass or less, 18% by mass or less, or 15% by mass or less. From these viewpoints, the content of the first resin part may be 1 to 30 mass%, 1 to 25 mass%, 1 to 20 mass%, 5 to 30 mass%, 5 to 25 mass%, 5 to 20 mass%, 10 to 30 mass%, 10 to 25 mass%, or 10 to 20 mass%.

[0030] The content of the first resin part in the reinforcing member may be in the following ranges relative to 100 parts by mass of the glass fiber sheet. From the viewpoint of easily obtaining a sufficient reinforcing effect of the reinforcing member and easily improving the handleability of the reinforcing member, the content of the first resin part may be 1 part by mass or more, 5 parts by mass or more, 10 parts by mass or more, 15 parts by mass or more, 20 parts by mass or more, 25 parts by mass or more, or 30 parts by mass or more. From the viewpoint of easily obtaining excellent substrate visibility and easily improving the handleability of the reinforcing member, the content of the first resin part may be 60 parts by mass or less, 55 parts by mass or less, 50 parts by mass or less, 45 parts by mass or less, 40 parts by mass or less, or 35 parts by mass or less. From these viewpoints, the content of the first resin part may be 1 to 60 parts by mass, 1 to 50 parts by mass, 1 to 40 parts by mass, 5 to 60 parts by mass, 5 to 50 parts by mass, 5 to 40 parts by mass, 15 to 60 parts by mass, 15 to 50 parts by mass, or 15 to 40 parts by mass.

[0031] The reinforcing member includes a second resin portion covering at least a portion of the first resin portion. The second resin portion may cover a portion of the first resin portion (a portion of the first resin portion may be exposed from the second resin portion), or may cover the entire first resin portion. The second resin portion may be disposed on at least one surface selected from the group consisting of one surface and the other surface of the glass fiber sheet. The second resin portion may be layer-shaped.

[0032] The second resin part contains a cured product of an epoxy compound (a compound containing an epoxy group). The cured product of the epoxy compound may be obtained by a one-component adhesive containing the epoxy compound, or may be obtained by a multiple-component adhesive (e.g., a two-component adhesive) having a first component containing the epoxy compound and a second component containing a curing agent. The cured product of the epoxy compound may be obtained by a room-temperature curing adhesive containing the epoxy compound.

[0033] The epoxy compound may be an epoxy resin. Examples of the epoxy compound include bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol A bis(polypropylene glycol glycidyl ether) ether, bisphenol A bis(polyethylene glycol glycidyl ether) ether, hydrogenated bisphenol A epoxy resin, hydrogenated bisphenol F epoxy resin, biphenyl epoxy resin, urethane-modified epoxy resin, rubber-modified epoxy resin, alkyl glycidyl ether, cresyl glycidyl ether, phenyl glycidyl ether, alkyl diglycidyl ether, polyethylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, glycerin triglycidyl ether, trimethylolpropane triglycidyl ether, and diglycidyl ether of alkanediol. From the viewpoint of easily obtaining a sufficient reinforcing effect of the reinforcing member, the epoxy compound may include a compound having a bisphenol A skeleton, a bisphenol A epoxy resin, or an alkylene oxide-added bisphenol A epoxy resin (for example, a propylene oxide-added bisphenol A epoxy resin).

[0034] From the viewpoint of easily obtaining a sufficient reinforcing effect of the reinforcing member, the content of the cured epoxy compound in the second resin part may be 50% by mass or more, 60% by mass or more, 70% by mass or more, 80% by mass or more, or 90% by mass or more based on the entire second resin part. The second resin part may be substantially composed of the cured epoxy compound (an embodiment in which substantially 100% by mass of the second resin part is the cured epoxy compound).

[0035] The second resin part may contain components other than the cured product of the epoxy compound, such as fillers (e.g., silica), curing accelerators, curing retarders, light stabilizers, light absorbers, antioxidants, anti-degradants, pigments, dyes, silane coupling agents, antifoaming agents, leveling agents, dispersants, rheology control agents, waxes, etc.

[0036] The spectral transmittance in the visible light region (e.g., wavelength 550 nm) per 0.5 mm thickness of the second resin part may be 30% or more, 40% or more, 50% or more, 60% or more, 70% or more, 75% or more, 80% or more, 85% or more, or 90% or more, from the viewpoint of easily obtaining excellent substrate visibility.

[0037] The thickness of the second resin portion in the reinforcing member (thickness in the direction perpendicular to the surface of the glass fiber sheet) may be within the following ranges. From the viewpoint of easily obtaining a sufficient reinforcing effect of the reinforcing member, the thickness of the second resin portion may be 100 μm or more, 200 μm or more, 300 μm or more, 400 μm or more, 450 μm or more, or 500 μm or more. From the viewpoint of easily obtaining excellent substrate visibility, the thickness of the second resin portion may be 800 μm or less, 700 μm or less, 600 μm or less, 550 μm or less, or 500 μm or less. From these viewpoints, the thickness of the second resin portion may be 100 to 800 μm, 100 to 700 μm, 100 to 600 μm, 300 to 800 μm, 300 to 700 μm, 300 to 600 μm, 400 to 800 μm, 400 to 700 μm, or 400 to 600 μm. The thickness of the second resin portion may be an average thickness, and the average thickness may be an average value of six measurement points. When the second resin portion is present on both sides of the glass fiber sheet, the thickness of the second resin portion may be an average value of the thickness of the second resin portion on one side of the glass fiber sheet and the thickness of the second resin portion on the other side of the glass fiber sheet, and may be an average value of three measurement points on each of the one side and the other side.

[0038] The content of the second resin portion in the reinforcing member may be in the following range: 100 g / m 2 Above, 200g / m 2 Above, 300g / m 2 Above, 400g / m 2 Above, 450g / m 2 or more, or 500 g / m 2 The content of the second resin portion may be 800 g / m or more from the viewpoint of easily obtaining excellent base visibility. 2 Below, 700g / m 2 Below, 600g / m 2 Below, 550g / m 2 or less, or 500 g / m 2 From these viewpoints, the content of the second resin portion is 100 to 800 g / m 2 , 100-700g / m 2 , 100-600g / m 2, 300-800g / m 2 , 300-700g / m 2 , 300-600g / m 2 , 400-800g / m 2 , 400-700g / m 2 , or 400 to 600 g / m 2 It may be.

[0039] The content of the second resin portion in the reinforcing member may be within the following ranges based on the total amount of the reinforcing member. From the viewpoint of easily obtaining a sufficient reinforcing effect of the reinforcing member, the content of the second resin portion may be 1% by mass or more, 5% by mass or more, 10% by mass or more, 15% by mass or more, 20% by mass or more, 25% by mass or more, 30% by mass or more, or 35% by mass or more. From the viewpoint of easily obtaining excellent base visibility, the content of the second resin portion may be 70% by mass or less, 65% by mass or less, 60% by mass or less, 55% by mass or less, 50% by mass or less, 45% by mass or less, or 40% by mass or less. From these viewpoints, the content of the second resin portion may be 1 to 70% by mass, 1 to 60% by mass, 1 to 50% by mass, 10 to 70% by mass, 10 to 60% by mass, 10 to 50% by mass, 20 to 70% by mass, 20 to 60% by mass, or 20 to 50% by mass.

[0040] The content of the second resin portion in the reinforcing member may be in the following ranges relative to 100 parts by mass of the glass fiber sheet. From the viewpoint of easily obtaining a sufficient reinforcing effect of the reinforcing member, the content of the second resin portion may be 10 parts by mass or more, 20 parts by mass or more, 30 parts by mass or more, 40 parts by mass or more, 50 parts by mass or more, 60 parts by mass or more, 65 parts by mass or more, 70 parts by mass or more, or 75 parts by mass or more. From the viewpoint of easily obtaining excellent base visibility, the content of the second resin portion may be 250 parts by mass or less, 200 parts by mass or less, 150 parts by mass or less, 100 parts by mass or less, 90 parts by mass or less, or 80 parts by mass or less. From these viewpoints, the content of the second resin part may be 10 to 250 parts by mass, 10 to 150 parts by mass, 10 to 100 parts by mass, 30 to 250 parts by mass, 30 to 150 parts by mass, 30 to 100 parts by mass, 50 to 250 parts by mass, 50 to 150 parts by mass, or 50 to 100 parts by mass.

[0041] The content of the second resin part in the reinforcing member may be in the following ranges relative to 100 parts by mass of the first resin part. From the viewpoint of easily obtaining a sufficient reinforcing effect of the reinforcing member, the content of the second resin part may be 50 parts by mass or more, 80 parts by mass or more, 100 parts by mass or more, 120 parts by mass or more, 150 parts by mass or more, 180 parts by mass or more, 200 parts by mass or more, 220 parts by mass or more, or 250 parts by mass or more. From the viewpoint of easily obtaining excellent base visibility, the content of the second resin part may be 850 parts by mass or less, 800 parts by mass or less, 700 parts by mass or less, 600 parts by mass or less, 500 parts by mass or less, 450 parts by mass or less, 400 parts by mass or less, 350 parts by mass or less, 300 parts by mass or less, or 250 parts by mass or less. From these viewpoints, the content of the second resin part may be 50 to 850 parts by mass, 50 to 550 parts by mass, 50 to 350 parts by mass, 100 to 850 parts by mass, 100 to 550 parts by mass, 100 to 350 parts by mass, 150 to 850 parts by mass, 150 to 550 parts by mass, or 150 to 350 parts by mass.

[0042] The reinforcing member may further include a member other than the glass fiber sheet, the first resin part, and the second resin part. The reinforcing member may include a member (e.g., an undercoat layer formed by a primer) disposed between the second resin part and the structure, and a member (e.g., a protective coating, a top coat layer, etc.) disposed on the opposite side of the glass fiber sheet from the structure.

[0043] The spectral transmittance of the reinforcing member in the visible light region (e.g., wavelength 550 nm) per 0.8 mm thickness may be 10% or more, 15% or more, 20% or more, 25% or more, 30% or more, 35% or more, or 40% or more, from the viewpoint of easily obtaining excellent visibility of the substrate.

[0044] The thickness of the reinforcing member (thickness in the direction perpendicular to the surface of the glass fiber sheet) may be within the following ranges. From the viewpoint of easily obtaining a sufficient reinforcing effect of the reinforcing member, the thickness of the reinforcing member may be 200 μm or more, 300 μm or more, 400 μm or more, 500 μm or more, 600 μm or more, 700 μm or more, or 800 μm or more. From the viewpoint of easily obtaining excellent substrate visibility, the thickness of the reinforcing member may be 1500 μm or less, 1200 μm or less, 1000 μm or less, 900 μm or less, or 800 μm or less. From these viewpoints, the thickness of the reinforcing member may be 200 to 1500 μm, 200 to 1200 μm, 200 to 1000 μm, 400 to 1500 μm, 400 to 1200 μm, 400 to 1000 μm, 600 to 1500 μm, 600 to 1200 μm, or 600 to 1000 μm. The thickness of the reinforcing member may be an average thickness, and the average thickness may be an average value of values ​​measured at three points.

[0045] The tensile modulus of the reinforcing member may be 50 GPa or more, 60 GPa or more, 70 GPa or more, 80 GPa or more, or 90 GPa or more, from the viewpoint of easily obtaining a sufficient reinforcing effect of the reinforcing member. The tensile modulus of the reinforcing member may be 150 GPa or less, 130 GPa or less, 120 GPa or less, 100 GPa or less, or 90 GPa or less, from the viewpoint of easily obtaining a sufficient adhesive force of the reinforcing member. From these viewpoints, the tensile modulus of the reinforcing member may be 50 to 150 GPa, 50 to 120 GPa, 50 to 100 GPa, 60 to 150 GPa, 60 to 120 GPa, 60 to 100 GPa, 80 to 150 GPa, 80 to 120 GPa, or 80 to 100 GPa. The tensile modulus of the reinforcing member may be the tensile modulus at 25°C. The tensile modulus of elasticity of the reinforcing member can be measured in accordance with JIS A1191 (Method B).

[0046] FIG. 1 is a cross-sectional view showing an example of a reinforcing member. The reinforcing member 100 of FIG. 1 includes a glass fiber sheet 10, a layered first resin portion 20 that covers the glass fiber sheet 10, and a layered second resin portion 30 that covers the first resin portion 20. FIG. 1 illustrates a cross section of each fiber that constitutes the glass fiber sheet 10, and the entire glass fiber sheet 10 is covered with the first resin portion 20. The first resin portion 20 is in contact with the glass fiber sheet 10 and contains a cured product of a (meth)acrylic compound. The second resin portion 30 is in contact with the first resin portion 20 and contains a cured product of an epoxy compound. The second resin portion 30 is disposed on both sides of the glass fiber sheet 10, and the entire first resin portion 20 is covered with the second resin portion 30.

[0047] The method for manufacturing a reinforcing member includes, in this order: a first coating step of coating at least a portion of a glass fiber sheet with a first resin material containing a (meth)acrylic compound; a first curing step of obtaining a first resin part by curing the first resin material; a second coating step of coating at least a portion of the first resin part with a second resin material containing an epoxy compound; and a second curing step of obtaining a second resin part by curing the second resin material.

[0048] The method of supplying the first resin material to the glass fiber sheet in the first covering step and the method of supplying the second resin material to the first resin portion in the second covering step are not particularly limited.

[0049] In the first curing step or the second curing step, the resin material (the first resin material or the second resin material) may be cured by heat, light, etc., or the resin material (the first resin material or the second resin material) may be cured at room temperature (for example, by mixing multiple materials and then curing them at room temperature).

[0050] The method for checking the reinforced state according to the present embodiment may include a reinforcing step of reinforcing the structure with a reinforcing member before the reinforcement state checking step. In the reinforcing step, a member to be reinforced can be placed on the surface of the structure.

[0051] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0052] <Preparation of (meth)acrylic composition> 70 parts by mass of bisphenol A ethylene oxide-modified (4 mol addition) dimethacrylate ((meth)acrylic compound, manufactured by MIWON Corporation, trade name "Miramer M241"), 30 parts by mass of bisphenol A ethylene oxide-modified (10 mol addition) dimethacrylate ((meth)acrylic compound, manufactured by MIWON Corporation, trade name "Miramer M2101"), and 3 parts by mass of 1-hydroxycyclohexyl phenyl ketone (photopolymerization initiator, manufactured by IGM Resins, trade name "Omnirad 184") were mixed in a container to obtain a mixture, and this mixture was stirred to prepare a (meth)acrylic composition.

[0053] <Preparation of two-component room temperature curing epoxy composition> 70 parts by mass of bisphenol A type epoxy resin (epoxy compound, manufactured by ADEKA Corporation, trade name "ADEKA RESIN EP-4100"), 15 parts by mass of propylene oxide-added bisphenol A type epoxy resin (epoxy compound, manufactured by ADEKA Corporation, trade name "ADEKA RESIN EP-4005"), 15 parts by mass of diglycidyl ether of 1,6-hexanediol (manufactured by ADEKA Corporation, trade name "ADEKA GLYCIROL ED-503"), and 4 parts by mass of hydrophilic fumed silica (manufactured by Nippon Aerosil Co., Ltd., trade name "Aerosil 200") were mixed in a container to obtain a mixture, and then this mixture was stirred to prepare a base resin. Furthermore, a curing agent was prepared by mixing 42 parts by mass of a polyamine compound (manufactured by T&K TOKA Corporation, trade name "Fujicure 8106-A") and 2 parts by mass of an amide-based thickener (manufactured by BYK Japan KK, trade name "BYK R607") in a container to obtain a mixture, and then stirring this mixture.

[0054] <Preparation of reinforcing member> (Example 1) A two-way plain woven glass fiber sheet (average fineness: 2400 tex, basis weight: 650 g / m 2 ) to which 200 g / m of the above-mentioned (meth)acrylic composition was added. 2 The glass fiber sheet was impregnated with the (meth)acrylic composition by applying the composition to the glass fiber sheet. Next, a UV-LED irradiation device was used to apply the composition to the glass fiber sheet at an illuminance of 200 mW / cm.2 , irradiation amount 8000mJ / cm 2 The (meth)acrylic composition was cured by irradiating the glass fiber sheet with ultraviolet light (wavelength: 365 nm), thereby obtaining a resin-impregnated sheet including a glass fiber sheet and a first resin portion (a cured product of the (meth)acrylic composition containing a (meth)acrylic compound) covering the glass fiber sheet.

[0055] Next, an epoxy composition (base:curing agent=2:1 [mass ratio]) obtained by premixing the base and curing agent of the two-component room temperature curing epoxy composition described above was applied to both sides of the resin-impregnated sheet. The total amount of the epoxy composition applied to both sides of the resin-impregnated sheet was 500 g / m. 2 Next, the epoxy composition was cured in air at room temperature (25°C) for one week to obtain a reinforcing member including a glass fiber sheet, a first resin part (a cured product of the (meth)acrylic composition containing a (meth)acrylic compound) covering the glass fiber sheet, and a second resin part (a cured product of the epoxy composition containing an epoxy compound) covering the first resin part.

[0056] In the reinforcing member, the average thickness of the glass fiber sheet was 174 μm, the average thickness of the first resin portion (thickness in the direction perpendicular to the surface of the glass fiber sheet) was 200 μm, and the average thickness of the second resin portion (thickness in the direction perpendicular to the surface of the glass fiber sheet) was 500 μm. The average thickness of the reinforcing member was 800 μm (because the first resin portion and the glass fiber sheet were integrated with each other, the total thickness of the glass fiber sheet, the first resin portion, and the second resin portion was different from the thickness of the reinforcing member).

[0057] In the reinforcing member, the content of the glass fiber sheet is 650 g / m 2 The content of the first resin portion is 200 g / m 2 and the content of the second resin portion is 500 g / m 2 Based on the total amount of the reinforcing member, the content of the glass fiber sheet was 48.2 mass %, the content of the first resin part was 14.8 mass %, and the content of the second resin part was 37.0 mass %.

[0058] The first resin portion and the second resin portion had a spectral transmittance of 90% at a wavelength of 550 nm per 0.5 mm thickness, and the reinforcing member had a spectral transmittance of 43% at a wavelength of 550 nm per 0.8 mm thickness.

[0059] (Comparative Example 1) A two-way plain woven glass fiber sheet (similar to Example 1) was premixed with the base and curing agent of the above-mentioned two-component room temperature curing epoxy composition, and 500 g / m of the epoxy composition (base:curing agent=2:1 [mass ratio]) was applied. 2 Next, the epoxy composition was cured in air at room temperature (25°C) for one week to obtain a reinforcing member including a glass fiber sheet and a resin portion (a cured product of the epoxy composition containing an epoxy compound) covering the glass fiber sheet.

[0060] (Comparative Example 2) Unidirectional high-strength carbon fiber sheet (manufactured by Toray Industries, Inc., product name "Torayka Cloth UT70-20G", basis weight: 200 g / m 2 ) and the base and curing agent of the above-mentioned two-part room temperature curing epoxy composition were mixed in advance, and 500 g / m of the epoxy composition (base:curing agent=2:1 [mass ratio]) was obtained. 2 Next, the epoxy composition was cured in air at room temperature (25°C) for one week to obtain a reinforcing member including a carbon fiber sheet and a resin portion (a cured product of the epoxy composition containing an epoxy compound) covering the carbon fiber sheet.

[0061] <Appearance Evaluation Before and After Stress Generation> (Before Stress Generation) Figure 2 shows the connector used for appearance evaluation, with (a) in Figure 2 being a side view of the connector, and (b) in Figure 2 being a plan view of the connector viewed from the surface side (the direction of the arrow in the center of (a) in Figure 2). As shown in Figure 2, a pair of aluminum tabs 200a were used to hold both sides of one end of a reinforcing member 100 (a reinforcing member of Example 1, Comparative Example 1, or Comparative Example 2, length: 350 mm, width: 20 mm), and a pair of aluminum tabs 200b were used to hold both sides of the other end of the reinforcing member 100. A mark M was placed in the center of one side of the reinforcing member 100 to obtain a connector 200. Each of the aluminum tabs 200a and 200b had a length of 100 mm, a width of 20 mm, and a thickness of 2 mm.

[0062] The connector was placed on a base with its surface facing the base. Figure 3 shows photographs of the reinforcing member of the connector observed from the back side of the connector (the direction opposite to the arrow in the center of Figure 2 (a)) ((a) Example 1, (b) Comparative Example 1, (c) Comparative Example 2). In the connector of Figure 3, wiring is connected to a mark M located in the center of one side of the reinforcing member and fixed with tape. In Example 1 and Comparative Example 1, the reinforcing member is transparent, whereas in Comparative Example 2, the use of a black carbon fiber sheet confirms that the reinforcing member is not transparent.

[0063] (After Stress Generation) With the longitudinal direction of the above-mentioned connector oriented vertically, the aluminum tabs at one end and the other end of the connector were gripped using a 300 kN universal testing machine (Shimadzu Corporation, Autograph AG-300KG), and an FRP tensile strength test was performed on the reinforcing member of the connector with reference to JIS A1191 (Method B), thereby generating stress in the longitudinal direction of the reinforcing member in the reinforcing member. While monotonically applying stress by controlling the displacement of the crosshead (tensile speed: 3.0 mm / min), the tensile modulus of the reinforcing member (Example) was measured, and the reinforcing member (Example and Comparative Example) was observed from a direction perpendicular to the surface of the reinforcing member.

[0064] Based on the stress-strain curve in an FRP tensile strength test in accordance with JIS A1191 (Method B), the tensile modulus of the reinforcing member was calculated by dividing the difference in stress between two points at 20% and 50% of the maximum tensile stress by the difference in strain between two points at 20% and 50% of the maximum tensile load. The tensile modulus of the reinforcing member of Example 1 was 90 GPa.

[0065] 4 and 5 are photographs of the reinforcing member of the connector observed from the surface side of the connector (the direction of the central arrow in (a) of FIG. 2) (FIG. 4: Example 1, FIG. 5: Comparative Example 1). (a) of FIG. 4 and 5 show the observation results before stress generation, and (b) of FIG. 4 and 5 show the observation results when a load of 3 kN is applied. In Example 1, the reinforcing member (particularly the first resin portion) became cloudy with the generation of stress, and the behavior of the stress could be visually confirmed. On the other hand, in Comparative Example 1, no change in appearance was visually observed before and after the generation of stress until the reinforcing member reached the fracture strain and broke, and the behavior of the stress could not be visually confirmed. Similarly, in Comparative Example 2, no change in appearance was visually observed before and after the generation of stress until the reinforcing member reached the fracture strain and broke, and the behavior of the stress could not be visually confirmed.

[0066] 10...glass fiber sheet, 20...first resin part, 30...second resin part, 100...reinforcing member, 200...connecting body, 200a, 200b...aluminum tabs, M...mark.

Claims

1. A method for checking a reinforcement state of a reinforcing member for a structure, comprising a step of checking the reinforcement state based on discoloration of the reinforcing member when stress is generated in the reinforcing member, wherein the reinforcing member comprises a glass fiber sheet, a first resin part covering at least a portion of the glass fiber sheet, and a second resin part covering at least a portion of the first resin part, the first resin part containing a cured product of a (meth)acrylic compound, and the second resin part containing a cured product of an epoxy compound.

2. The weight of the glass fiber sheet is 100 to 1000 g / m 2 The method for checking a reinforcement state according to claim 1, 3. The method for checking the reinforcement state according to claim 1, wherein the reinforcing member has a tensile modulus of elasticity of 50 to 150 GPa.

4. The method for checking reinforcement condition according to any one of claims 1 to 3, wherein the structure is a concrete structure.

Citation Information

Patent Citations

  • Reinforcing fiber sheet and concrete structure

    JP1997003745A

  • Earthquake resistance reinforcing method

    JP2000265680A

  • Reinforced coating method of concrete structure surface

    JP2010001707A

  • Concrete piece exfoliation prevention structure, concrete exfoliation prevention method, and alicyclic polyamine used therefor

    JP2016030716A

  • Concrete-structure-reinforcing fiber sheet

    WO2021039858A1