Repellent
A water-dispersed repellent with a modified polyol, characterized by a high endothermic peak temperature and specific hydrocarbon groups, addresses the challenge of imparting oil resistance to base materials, achieving effective liquid repellency and enhancing their performance in various applications.
Patent Information
- Application Number
- PCT/JP2024/010275
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2024-03-15
- Publication Date
- 2024-10-03
AI Technical Summary
Current repellents fail to effectively impart oil resistance to base materials such as fibers and paper, which is essential for applications requiring protection against oils and other liquids.
A water-dispersed repellent comprising a modified polyol with specific characteristics, including a maximum endothermic peak temperature of 55°C or higher and four or more monovalent hydrocarbon groups with 20 to 40 carbon atoms, is used to treat base materials, providing oil resistance and liquid repellency.
The repellent effectively imparts oil resistance and liquid repellency to base materials, enhancing their durability and performance in applications like food packaging and textile products.
Smart Images

Figure JPOXMLDOC01-APPB-I000001 
Figure JPOXMLDOC01-APPB-I000002 
Figure JPOXMLDOC01-APPB-I000003
Abstract
Description
repellent
[0001] FIELD OF THE DISCLOSURE The present disclosure relates to repellents and products treated with repellents.
[0002] In recent years, development of non-fluorine-based repellents capable of imparting liquid repellency (water repellency, oil repellency, oil resistance, and / or water resistance) to various substrates has progressed.
[0003] Japanese Patent Application Laid-Open No. 2021-155492
[0004] Patent Document 1 does not describe oil resistance.
[0005] An object of the present disclosure is to provide a novel repellent that can impart oil resistance to a substrate (for example, textiles, paper).
[0006] The present disclosure includes the following aspects: [Item 1] A water-dispersible repellent comprising a polyol modified product and a dispersant, the repellent satisfying one or more of (1) and (2). (1) In differential scanning calorimetry of the polyol modified product, or in differential scanning calorimetry of a solid component obtained by removing the liquid medium from the repellent, the temperature of the maximum endothermic peak in the temperature range of 25°C to 180°C is 55°C or higher. (2) The polyol modified product has four or more monovalent hydrocarbon groups having from 20 to 40 carbon atoms, which may have a substituent. [Item 2] The repellent according to Item 1, in which differential scanning calorimetry of the polyol modified product, in the temperature range of 25°C to 180°C, the temperature of the maximum endothermic peak is 55°C or higher. [Item 3] The repellent according to Item 1 or 2, in which differential scanning calorimetry of a solid component obtained by removing the liquid medium from the repellent, the temperature of the maximum endothermic peak is 55°C or higher in the temperature range of 25°C to 180°C. [Item 4] The peak intensity A of the maximum peak at a measurement temperature of 25°C in the range of 2θ of 15° to 30° measured by variable temperature X-ray diffraction method of the solid component obtained by removing the liquid medium from the repellent agent. 25℃ and the peak intensity A of the maximum peak at the measurement temperature of 55 ° C. 55℃ Diffraction intensity ratio [A 55℃ / A 25℃Item 5: The repellent according to any one of Items 1 to 3, wherein the polyol-modified product has four or more optionally substituted monovalent hydrocarbon groups having from 20 to 40 carbon atoms. Item 6: The repellent according to Item 5, wherein the optionally substituted monovalent hydrocarbon groups having from 20 to 40 carbon atoms are alkyl groups. Item 7: The polyol-modified product has four or more hydroxy groups of the polyol substituted with the following formula: -Y-Z n [Wherein, Y is Y 1 and Y 2 Y is a 1+n valent group consisting of one or more groups selected from the group consisting of 1 represents a direct bond, —O—, —C(═O)—, —C(═NR′)—, —S—, —S(═O) 2 -, -NR'-, -C(OR')R'-, and -C(OR')(-) 2 , -N(-) 2 (wherein R′ is independently in each occurrence a hydrogen atom or an organic group having 1 to 30 carbon atoms), and Y 2 is a group consisting of one or more members selected from the group consisting of optionally substituted di- to tetravalent aliphatic hydrocarbon groups having 1 to 40 carbon atoms, optionally substituted di- to tetravalent hydrocarbon aromatic rings, and optionally substituted di- to tetravalent heterocycles, Z is an optionally substituted monovalent hydrocarbon group having from 20 to 40 carbon atoms, and n is an integer of from 1 to 3. [Item 8] The repellent according to any one of Items 1 to 6, wherein Y is -O-Y 11 - or -O-Y 11 -Y 21 -Y 12 wherein each symbol represents independently at each occurrence: Y 11 is a direct bond, —C(═O)—, —C(═O)—NR′—, or —C(═S)—NR′—; Y 21 is a hydrocarbon group having 1 to 40 carbon atoms which may have a substituent, and Y 12is -O-, -O-C(=O)-, -O-C(=O)-O-, -C(=O)-NR'-, -O-C(=O)-NR'-, -NR'-, -NR'-C(=O)-, -NR'-C(=O)-O-, -NR'-C(=O)-NR'-, -C(=O)-, -C(=O)-O-, -C(=O)-NR'-, -SO 2 -, -SO 2 NR'-, -C(OR')R'-, or -C(OR')(-) 2[Item 9] The repellent according to any one of Items 1 to 8, wherein the polyol is at least one selected from the group consisting of monosaccharides, oligosaccharides, polysaccharides, sugar alcohols, hydroxy acids, amino acids, vitamins, flavonols, hydroxy hydrocarbons, and hydroxy group-containing compound polymers. [Item 10] The polyol is selected from the group consisting of glucose, fructose, galactose, xylose; sucrose, cycloamylose, cyclodextrin, maltose, trehalose, lactose, sucralose; sorbitol, maltitol, erythritol, isomalt, lactitol, mannitol, xylitol, sorbitan, and lactitol; starch, cellulose, curdlan, pullulan, alginic acid, carrageenan, guar gum, chitin, chitosan, locust bean gum, kappa carrageenan, iota carrageenan, isomaltodextrin, gellan gum, and tamarind seed gum; ascorbic acid, kojic acid, quinic acid, chlorogenic acid, and gluconic acid; glucosamine; inositol; catechin, quercetin, and anthocyanin; The repellent according to any one of Items 1 to 9, wherein the repellent is at least one selected from the group consisting of ethylene glycol, propylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, neopentyl glycol, trimethylene glycol, glycerol, trimethylolpropane, and trimethylolethane; polyglycerin, polyvinyl alcohol, hydroxyethyl (meth)acrylate polymers, hydroxypropyl (meth)acrylate polymers, and hydroxybutyl (meth)acrylate polymers. [Item 11] The repellent according to any one of Items 1 to 10, wherein the volume abundance ratio of particles of 100 μm or more measured by a laser diffraction scattering method is 25% or less. [Item 12] The repellent according to any one of Items 1 to 11, wherein the biobased ratio of the polyol modified product is 20% or more. [Item 13] The polyol modified product is a repellent according to any one of Items 1 to 11, wherein the hydroxy group of the polyol is converted to a group represented by the following formula: -Y-Z n [Wherein, Y is —O—Y 11 - or -O-Y 11 -Y 21 -Y 12wherein each symbol represents independently at each occurrence: Y 11 is a direct bond, —C(═O)—, —C(═O)—NR′—, or —C(═S)—NR′—; Y 21 is a hydrocarbon group having 1 to 40 carbon atoms which may have a substituent, and Y 12 is -O-, -O-C(=O)-, -O-C(=O)-O-, -C(=O)-NR'-, -O-C(=O)-NR'-, -NR'-, -NR'-C(= O)-, -NR'-C(=O)-O-, -NR'-C(=O)-NR'-, -C(=O)-, -C(=O)-O-, -C(=O)-NR'-, -SO 2 -, -SO 2 NR'-, -C(OR')R'-, or -C(OR')(-) 2Z is a hydrocarbon group having 6 to 40 carbon atoms, and n is an integer of 1 to 3. and the polyol is selected from the group consisting of glucose, fructose, galactose, xylose; sucrose, cycloamylose, cyclodextrin, maltose, trehalose, lactose, sucralose; sorbitol, maltitol, erythritol, isomalt, lactitol, mannitol, xylitol, sorbitan, and lactitol; starch, cellulose, curdlan, pullulan, alginic acid, carrageenan, guar gum, chitin, chitosan, locust bean gum, kappa carrageenan, iota carrageenan, isomaltodextrin, gellan gum, and tamarind seed gum; ascorbic acid, kojic acid, quinic acid, chlorogenic acid, and gluconic acid; glucosamine; inositol; catechin, quercetin, and anthocyanin; Item 14. The repellent according to any one of Items 1 to 13, wherein the polyol-modified product is at least one selected from the group consisting of ethylene glycol, propylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, neopentyl glycol, trimethylene glycol, glycerol, trimethylolpropane, and trimethylolethane; polyglycerin, polyvinyl alcohol, a hydroxyethyl (meth)acrylate polymer, a hydroxypropyl (meth)acrylate polymer, and a hydroxybutyl (meth)acrylate polymer, and the hydroxy group substitution rate in the polyol-modified product is 30% or more. [Item 15] The repellent according to any one of Items 1 to 13, wherein the polyol-modified product is a compound in which hydroxy groups in a polyglycerin having a degree of polymerization of 5 to 15 or a sugar alcohol are substituted with a group represented by the following formula: -O-C(=O)-Z, or -O-C(=O)NH-Z, wherein Z is an alkyl group having 20 to 24 carbon atoms, and the hydroxy group substitution rate in the polyol-modified product is 50% or more. [Item 15] The repellent according to any one of Items 1 to 14, which is for use in textile products or paper products. [Item 16] A product treated with the repellent according to any one of Items 1 to 15. [Item 17] The product according to Item 16, which is a textile product or a paper product.[Item 18] The product according to Item 16 or 17, which is greaseproof paper or water-resistant paper. [Item 19] The product according to any one of Items 16 to 18, which is food packaging material or a food container. [Item 20] A method for producing a treated product, comprising a step of treating a substrate with the repellent according to any one of Items 1 to 15. [Item 21] The production method according to Item 20, wherein the treatment is an internal addition treatment.
[0007] The repellent agent of the present disclosure can impart good liquid repellency (especially oil resistance) to paper products.
[0008] 1 shows the results of a variable temperature X-ray diffraction measurement of the solid component obtained by removing the liquid medium from the repellent agent in the examples or comparative examples.
[0009] <Definition of Terms> As used herein, an "n-valent group" refers to a group having n bonds, i.e., a group that forms n bonds. Furthermore, an "n-valent organic group" refers to an n-valent group containing carbon. Such an organic group is not particularly limited, but may be a hydrocarbon group or a derivative thereof. A hydrocarbon group derivative refers to a group having one or more of N, O, S, Si, amide, sulfonyl, siloxane, carbonyl, carbonyloxy, halogen, etc. at the end or molecular chain of the hydrocarbon group.
[0010] As used herein, the term "hydrocarbon group" refers to a group containing carbon and hydrogen, which is a group obtained by removing a hydrogen atom from a hydrocarbon. Such hydrocarbon groups include, but are not limited to, C 1-20 Examples of hydrocarbon groups include aliphatic hydrocarbon groups and aromatic hydrocarbon groups. The "aliphatic hydrocarbon group" may be linear, branched, or cyclic, and may be saturated or unsaturated. The hydrocarbon group may contain one or more ring structures. The hydrocarbon group may be substituted with one or more substituents, if explicitly stated.
[0011] In this specification, when a term (symbol) that may appear multiple times in a chemical structure is defined, that definition applies independently at each occurrence, unless otherwise stated, regardless of whether "independently at each occurrence," "independently of each other," "independently of each other," or similar expressions are explicitly stated.
[0012] The chemical structures described herein should be understood not to encompass chemical structures that would be recognized by those skilled in the art as chemically impossible or extremely unstable.
[0013] <Repellent>
[0014] The repellent agent in the present disclosure imparts liquid repellency (water repellency, oil repellency, oil resistance, and / or water resistance) to a substrate (e.g., a fiber substrate, a paper substrate), and can function as at least one selected from the group consisting of a water repellent, an oil repellent, an oil-resistant agent, and a water-resistant agent. The repellent agent in the present disclosure can effectively impart oil resistance (oil repellency) and / or water resistance (water repellency) to the substrate, and can, for example, effectively impart both oil resistance and water resistance.
[0015] The repellent according to the present disclosure may be a water-dispersible repellent containing a polyol modifier and a dispersant. The repellent according to the present disclosure may be a repellent that satisfies one or more of the following (1) and (2): (1) In differential scanning calorimetry of the polyol modifier or in differential scanning calorimetry of a solid component obtained by removing the liquid medium from the repellent, the temperature of the maximum endothermic peak in the temperature range of 25°C to 180°C is 55°C or higher. (2) The polyol modifier has four or more monovalent hydrocarbon groups having from 20 to 40 carbon atoms, which may have a substituent.
[0016] The repellent agent in the present disclosure may not contain any compound selected from the group consisting of a compound having a fluoroalkyl group having 8 or more carbon atoms, a compound having a perfluoroalkyl group having 8 or more carbon atoms, a compound having a fluoroalkyl group having 4 or more carbon atoms, a compound having a perfluoroalkyl group having 4 or more carbon atoms, a compound having a perfluoroalkyl group, a compound having a fluoroalkyl group, and a compound having a fluorine atom. The repellent agent in the present disclosure can impart liquid repellency to a substrate even if it does not contain these fluorine compounds.
[0017] [Volumetric abundance ratio of particles] The volumetric abundance ratio of particles of 100 μm or larger in the repellent of the present disclosure, as measured by laser diffraction scattering, may be 25% or less, 20% or less, 15% or less, 10% or less, 5% or less, 3% or less, or 1.5% or less, and is preferably 15% or less or 5% or less. From the viewpoint of coating properties, it is preferable that the volumetric abundance ratio of particles of 100 μm or larger be within the above range. There are no particular limitations on the method for adjusting the volumetric abundance ratio of particles of 100 μm or larger, as measured by laser diffraction scattering, to 25% or less. For example, the particles in the raw material and / or dispersion may be micronized using a grinder, homogenizer, or the like.
[0018] [Volume Median Diameter] The volume median diameter of the repellent agent of the present disclosure, as measured by a laser diffraction scattering method, may be 10 nm or more, 30 nm or more, 50 nm or more, or 100 nm or more, preferably 150 nm or more or 200 nm or more, and may be 100 μm or less, 90 μm or less, 80 μm or less, 70 μm or less, 60 μm or less, 50 μm or less, 40 μm or less, 30 μm or less, 20 μm or less, or 10 μm or less, preferably 30 μm or less or 25 μm or less. In the present disclosure, the volume median diameter refers to the median diameter (D50) in a volume-based particle size distribution measured by a laser diffraction scattering method.
[0019] [Differential Scanning Calorimetry] In differential scanning calorimetry of the solid component obtained by removing the liquid medium from the repellent of the present disclosure, the maximum endothermic peak temperature in the temperature range of 25°C to 180°C is preferably 55°C or higher. This allows the effects of the present disclosure to be more effectively achieved. The maximum endothermic peak temperature may be 55°C or higher, 60°C or higher, or 65°C or higher. The maximum endothermic peak temperature may be 100°C or lower, 90°C or lower, 80°C or lower, or 70°C or lower.
[0020] [Variable Temperature X-ray Diffraction Measurement] In a variable temperature X-ray diffractometry measurement of the solid component obtained by removing the liquid medium from the repellent agent of the present disclosure, the peak intensity A of the maximum peak at a measurement temperature of 25°C in the 2θ range of 15° to 30° was 25℃ and the peak intensity A of the maximum peak at the measurement temperature of 55 ° C. 55℃ The diffraction intensity ratio [A55℃ / A 25℃ ] is preferably 0.5 or more. 55℃ / A 25℃ ] may be 0.6 or more, 0.7 or more, 0.8 or more, 0.9 or more, 1.0 or more, or 1.1 or more, preferably 0.8 or more or 0.9 or more, and may be 3 or less, 2.75 or less, 2.5 or less, 2.35 or less, or 2.0 or less. By being in the above range, for example, equal to or greater than the above lower limit, the arrangement structure of the alkyl chains can be maintained even in a high temperature range, and the effects of the present disclosure can be more favorably achieved.
[0021] [Modified Polyol] The modified polyol in the present disclosure is capable of adhering to a substrate and imparting liquid repellency to the substrate.
[0022] [Properties of Polyol Modified Body] The HD (n-hexadecane) contact angle of the polyol modified body may be 10° or more, 15° or more, 25° or more, 35° or more, 40° or more, 45° or more, 50° or more, 55° or more, or 65° or more, preferably 30° or more, and may be 100° or less, 90° or less, or 75° or less. When the polyol modified body has an HD contact angle equal to or greater than the above lower limit, it can impart good liquid repellency (particularly oil repellency) to the substrate. The HD contact angle is the static contact angle of the polyol modified body with respect to a spin-coated film, as shown in the examples, and is obtained by dropping 2 μL of HD onto the spin-coated film and measuring the contact angle 1 second after the drop has landed.
[0023] The water contact angle of the polyol-modified body may be 35° or more, 40° or more, 45° or more, 50° or more, 55° or more, 65° or more, 75° or more, 85° or more, 90° or more, or 100° or more, and may be 160° or less, 140° or less, 130° or less, 120° or less, 110° or less, 100° or less, or 90° or less. When the polyol-modified body has a water contact angle equal to or greater than the above lower limit, it can impart good liquid repellency (particularly water repellency) to the substrate. As shown in the examples, the water contact angle is the static contact angle of the polyol-modified body with respect to a spin-coated film, and is obtained by dropping 2 μL of water onto the spin-coated film and measuring the contact angle 1 second after the drop has landed.
[0024] The polyol modified product is preferably a compound containing carbon of biobased origin. The biobased content is measured in accordance with ASTM D6866. The biobased content may be 20% or more, preferably 30% or more, more preferably 50% or more, even more preferably 60% or more, even more preferably 70% or more, and most preferably 80% or more or 90% or more, for example, 100%. A high biobased content means that the amount of fossil resource-based materials, such as petroleum, used is reduced. From this perspective, the higher the biobased content of the polyol modified product, the more preferable it is.
[0025] The polyol-modified product preferably has a biodegradability of 5% or more. Higher biodegradability is preferable because it reduces the environmental impact. The biodegradability of the polyol-modified product may be, for example, 10% or more, 20% or more, 30% or more, 50% or more, 60% or more, 70% or more, 80% or more, or 90% or more, preferably 60% or more, more preferably 70% or more, even more preferably 80% or more, and most preferably 90% or more. Such biodegradability may be the biodegradability at 180 days as specified in JIS K 6953-1 or ASTM D6400.
[0026] The polyol modifier may not have any group selected from the group consisting of a fluoroalkyl group having 8 or more carbon atoms, a perfluoroalkyl group having 8 or more carbon atoms, a fluoroalkyl group having 4 or more carbon atoms, a perfluoroalkyl group having 4 or more carbon atoms, a perfluoroalkyl group, a fluoroalkyl group, and a fluorine atom. Even if the polyol modifier does not contain these fluorine-containing groups, it can still impart liquid repellency to a substrate.
[0027] In differential scanning calorimetry of the modified polyol, the maximum endothermic peak temperature in the temperature range of 25°C to 180°C is preferably 55°C or higher. This allows the effects of the present disclosure to be more effectively achieved. The maximum endothermic peak temperature may be 55°C or higher, 60°C or higher, or 65°C or higher. The maximum endothermic peak temperature may be 100°C or lower, 90°C or lower, 80°C or lower, or 70°C or lower.
[0028] The polyol-modified product is a polymer having a degree of polymerization of at least 1. From the viewpoint of improving liquid repellency, the degree of polymerization of the polyol-modified product may be 2 or more, 3 or more, 5 or more, 6 or more, preferably 7 or more, more preferably 8 or more, and even more preferably 9 or more; and from the viewpoint of improving the handleability of the repellent, it may be 100 or less, preferably 50 or less, more preferably 30 or less, even more preferably 15 or less, and particularly preferably 12 or less. The degree of polymerization refers to the number of repeating monomer units constituting the polymer.
[0029] The degree of polymerization in the present disclosure refers to the average degree of polymerization. The average degree of polymerization in the present disclosure refers to the polymerization obtained by measurement under the following conditions. When the polyol-modified product in the present disclosure is a polyglycerol-modified product obtained by modifying polyglycerol, the degree of polymerization of the polyol-modified product refers to the average degree of polymerization of the polyglycerol. The average degree of polymerization of polyglycerol is the average degree of polymerization (n) calculated from the hydroxyl value by end group analysis. Specifically, the average degree of polymerization and the average molecular weight are calculated from the following formulas (Formula 1) and (Formula 2). (Formula 1) Average molecular weight = 74n + 18 (Formula 2) Hydroxyl value = 56110(n + 2) / average molecular weight The hydroxyl value in the above (Formula 2) is a numerical value that serves as an index of the number of hydroxyl groups contained in the polyglycerol. The hydroxyl value is calculated from the amount of potassium hydroxide required to neutralize the acetic acid required to acetylate the free hydroxyl groups contained in 1 g of polyglycerol, and is calculated in accordance with "Standard Test Methods for the Analysis of Fats, Oils and Related Compounds (I), 2003 Edition," compiled by the Japan Oil Chemists' Society. The hydroxyl value of the raw material polyglycerol is measured according to the above-mentioned Standard Test Methods for the Analysis of Fats, Oils and Related Compounds, and the average degree of polymerization and average molecular weight of the polyglycerol can be calculated from the above-mentioned relational equation.
[0030] When the polyol-modified product in the present disclosure is a polyvinyl alcohol-modified product obtained by modifying polyvinyl alcohol, the degree of polymerization of the polyol-modified product refers to the average degree of polymerization of the polyvinyl alcohol, which can be measured in accordance with JIS K 6726, Testing Method for Polyvinyl Alcohol.
[0031] When the polyol-modified product in the present disclosure is a polysaccharide-modified product obtained by modifying a polysaccharide, the degree of polymerization of the polyol-modified product refers to the average degree of polymerization of the polysaccharide. Analysis of the average degree of polymerization of a polysaccharide can be performed as follows. The degree of polymerization refers to the number of monosaccharide units (fructose and glucose units) in the polysaccharide, and the average degree of polymerization is determined, for example, by taking the top of the peak in each analysis result obtained by a conventional analytical method such as HPLC, GC, or HPAEC as the average degree of polymerization. Measurements can be performed using, for example, an ULTRON PS-80N (8 x 300 mm) column manufactured by Shinwa Chemical Industry Co., Ltd. (solvent: water, flow rate: 0.5 ml / min, temperature: 50°C) or a TSK-GEL G30000 PWXL (7.8 x 300 mm) column manufactured by TOSOH Corporation (solvent: water, flow rate: 0.5 ml / min, temperature: 50°C) and a differential refractometer as a detector.
[0032] The polyol-modified product may be low molecular weight (e.g., weight average molecular weight less than 1500, less than 1000, or 500 or less) and / or high molecular weight. The weight average molecular weight of the polyol-modified product may be 100 or more, 300 or more, 500 or more, 1000 or more, 3000 or more, 5000 or more, 10,000 or more, 30,000 or more, 100,000 or more, 300,000 or more, or 500,000 or more; or 1,000,000 or less, 750,000 or less, 500,000 or less, 300,000 or less, 100,000 or less, 75,000 or less, 50,000 or less, 30,000 or less, 10,000 or less, 5000 or less, 300,000 or less, 2,000 or less, 1,000 or less, or 500 or less.
[0033] The substitution rate of hydroxy groups in the modified polyol may be 1% or more, 3% or more, 5% or more, 10% or more, 20% or more, 30% or more, 40% or more, 50% or more, 60% or more, 70% or more, 80% or more, 90% or more, or 100%, and is preferably 10% or more, for example, 30% or more, 40% or more, 50% or more, 60% or more, 70% or more, particularly 80% or more, and may be 100% or less, 95% or less, 85% or less, 75% or less, 65% or less, 55% or less, 45% or less, 35% or less, 25% or less, 15% or less, for example, 95% or less. Here, the "substitution rate" refers to the proportion (mol%) of hydroxy groups derived from the polyol that are modified, and may refer to the proportion (mol%) that are modified with monovalent hydrocarbon groups having from 1 to 40 carbon atoms (e.g., from 20 to 40 carbon atoms) that may have a substituent.
[0034] The residual rate of hydroxyl groups in the polyol-modified product may be 1% or more, 3% or more, 5% or more, 10% or more, 20% or more, 30% or more, 40% or more, 50% or more, 60% or more, 70% or more, 80% or more, or 90% or more, for example, 5% or more, and may be 100% or less, 95% or less, 85% or less, 75% or less, 65% or less, 55% or less, 45% or less, 35% or less, 25% or less, 15% or less, or 5% or less, for example, 50% or less, 30% or less, or 10% or less. Here, the "residual rate" refers to the proportion (mol %) of hydroxyl groups derived from the polyol that are not modified.
[0035] The number of modifying groups (monovalent hydrocarbon groups having from 1 to 40 carbon atoms (e.g., from 20 to 40 carbon atoms)) contained in the modified polyol may be 2 or more, 4 or more, 5 or more, 7 or more, 8 or more, 9 or more, 10 or more, 12 or more, 15 or more, 30 or more, or 50 or more, and may be 1,000 or less, 750 or less, 500 or less, 300 or less, 100 or less, 50 or less, 30 or less, or 20 or less.
[0036] The modifying group equivalent weight of the polyol modified product may be 150 or more, 250 or more, 350 or more, 450 or more, 550 or more, 650 or more, 750 or more, or 1000 or more, and may be 2500 or less, 2000 or less, 1500 or less, 1000 or less, 750 or less, 500 or less, or 400 or less. This is the value obtained by dividing the weight average molecular weight of the polyol modified product by the number of modifying groups.
[0037] [Modifying Group Structure] In the polyol modified product, one or more hydroxy groups of the polyol are substituted with a modifying group. From the viewpoint of improving liquid repellency, the modifying group may have a monovalent hydrocarbon group having 1 to 40 carbon atoms (e.g., 20 to 40 carbon atoms) which may have a substituent.
[0038] (Optionally Substituted Monovalent Hydrocarbon Group) The hydrocarbon group used to modify the polyol of the modified polyol is a monovalent hydrocarbon group which may have a substituent.
[0039] The hydrocarbon group may be a monovalent hydrocarbon group having from 1 to 40 carbon atoms (for example, from 20 to 40 carbon atoms). The hydrocarbon group may be an aromatic hydrocarbon group or an aliphatic hydrocarbon group, and is preferably an aliphatic hydrocarbon group, particularly a saturated aliphatic hydrocarbon group (alkyl group). The hydrocarbon group may be branched, cyclic, or linear, and is more preferably linear.
[0040] The number of carbon atoms in the hydrocarbon group may be 1 or more, 3 or more, 6 or more, 8 or more, 10 or more, 12 or more, 14 or more, 16 or more, 18 or more, 20 or more, 22 or more, 24 or more, 26 or more, or 28 or more, preferably 6 or more, 10 or more, 12 or more, or 16 or more, and may be 40 or less, 35 or less, 30 or less, or 25 or less, preferably 35 or less, or 30 or less.
[0041] The hydrocarbon group may have a substituent, but is preferably unsubstituted. Examples of the substituent include -OR' and -N(R'). 2, —COOR′, and halogen atoms (wherein R′, in each occurrence, is independently a hydrogen atom or an organic group (e.g., a hydrocarbon group, particularly an aliphatic hydrocarbon group) having 1 to 30, 1 to 20, 1 to 10, or 1 to 4 carbon atoms). The substituent may or may not have active hydrogen. The number of substituents may be 6 or less, 5 or less, 4 or less, 3 or less, 2 or less, 1 or less, or 0. In the substituted hydrocarbon group, the amount of carbon atoms relative to the amount of carbon atoms and heteroatoms may be 70 mol% or more, 80 mol% or more, 90 mol% or more, 95 mol% or more, or 99 mol% or more, preferably 75 mol% or more, and may be 95 mol% or less, 90 mol% or less, 85 mol% or less, or 80 mol% or less.
[0042] (-Y-Z n In the present disclosure, the modified polyol is a polyol in which one or more hydroxy groups of the polyol are represented by the following formula: n [Wherein, Y is Y 1 and Y 2 Y is a 1+n valent group consisting of one or more groups selected from the group consisting of 1 represents a direct bond, —O—, —C(═O)—, —C(═NR′)—, —S—, —S(═O) 2 -, -NR'-, -C(OR')R'-, and -C(OR')(-) 2 , -N(-) 2 (wherein R′ is independently in each occurrence a hydrogen atom or an organic group (e.g., a hydrocarbon group, particularly an aliphatic hydrocarbon group) having 1 to 30 carbon atoms (e.g., 1 to 20, 1 to 10, or 1 to 4 carbon atoms), and Y 2 is a group consisting of one or more members selected from the group consisting of optionally substituted di- to tetravalent aliphatic hydrocarbon groups having 1 to 40 carbon atoms, optionally substituted di- to tetravalent aromatic hydrocarbon rings, and optionally substituted di- to tetravalent heterocycles, Z is an optionally substituted monovalent hydrocarbon group having 1 to 40 carbon atoms (for example, 20 to 40 carbon atoms), and n is an integer of 1 to 3.
[0043] (Y) Y is Y1 and Y 2 Y is a 1+n valent group consisting of one or more groups selected from the group consisting of 1 represents a direct bond, —O—, —C(═O)—, —C(═NR′)—, —S—, —S(═O) 2 -, -NR'-, -C(OR')R'-, and -C(OR')(-) 2 , -N(-) 2 (wherein R′ is independently in each occurrence a hydrogen atom or an organic group (e.g., a hydrocarbon group, particularly an aliphatic hydrocarbon group) having 1 to 30 carbon atoms (e.g., 1 to 20, 1 to 10, or 1 to 4 carbon atoms), and Y 2 is a group composed of one or more members selected from the group consisting of optionally substituted di- to tetravalent aliphatic hydrocarbon groups having 1 to 40 carbon atoms, optionally substituted di- to tetravalent hydrocarbon aromatic rings, and optionally substituted di- to tetravalent heterocycles.
[0044] n is the number of Z's bonded to Y, and may be an integer of 1 to 3. n may be 1 or more, 2 or more, or 3 or more, and may be 3 or less, 2 or less, or 1 or less, for example, 2 or less.
[0045] The molecular weight of Y may be 10 or more, 50 or more, 100 or more, 200 or more, 300 or more, 500 or more, or 750 or more, and may be 3000 or less, 2500 or less, 2000 or less, 1500 or less, 1000 or less, 750 or less, 500 or less, 300 or less, 200 or less, 100 or less, or 50 or less.
[0046] ○ Y 1 Y 1 is a non-hydrocarbon linker.
[0047] Y 1 is a direct bond or a divalent or higher valent group. 1 The valence of Y may be 2 to 4, 2 to 3, or 2. 1 is preferably not only a direct bond.
[0048] Y 1The molecular weight of may be 10 or more, 50 or more, 100 or more, 200 or more, 300 or more, or 500 or more, and may be 2000 or less, 1500 or less, 1000 or less, 750 or less, or 500 or less.
[0049] Y 1 represents a direct bond, —O—, —C(═O)—, —S(═O) 2 -, -NR'-, -C(OR')R'-, and -C(OR')(-) 2 (wherein, R' in each occurrence is independently a hydrogen atom or an organic group (e.g., a hydrocarbon group, particularly an aliphatic hydrocarbon group) having 1 to 30 carbon atoms (e.g., 1 to 20, 1 to 10, or 1 to 4 carbon atoms). Y 1 Examples of include a direct bond, —O—, —O—C(═O)—, —O—C(═O)—O—, —O—C(═O)—NR′—, —NR′—, —NR′-C(═O)—O—, —NR′-C(═O)—NR′—, —C(═O)—, —C(═O)—O—, —C(═O)—NR′—, —SO 2 -, -SO 2 NR'-, -C(OR')R'-, -C(OR')(-) 2 and the like (wherein R' in each occurrence is independently a hydrogen atom or an organic group (e.g., a hydrocarbon group, particularly an aliphatic hydrocarbon group) having 1 to 30 carbon atoms (e.g., 1 to 20, 1 to 10, or 1 to 4 carbon atoms).
[0050] ○ Y 2 Y 2 is a linker of a hydrocarbon ring which may have a substituent, a hydrocarbon aromatic ring which may have a substituent, or a heterocyclic ring which may have a substituent.
[0051] Y 2 Y may be a hydrocarbon group or a non-hydrocarbon group (including heteroatoms). 2 Y may be aliphatic or aromatic. 2 may be linear, branched or cyclic.
[0052] Y 2 is a divalent or higher valent group. 2The valency of may be, for example, 2-4, 2-3, or 2.
[0053] Y 2 may have 1 or more, 2 or more, 3 or more, 4 or more, 6 or more, 8 or more, 10 or more, 12 or more, 14 or more, 16 or more, or 18 or more carbon atoms, and may be 40 or less, 35 or less, 30 or less, 25 or less, 20 or less, 15 or less, 10 or less, or 5 or less.
[0054] Y 2 is composed of one or more selected from the group consisting of optionally substituted di- to tetravalent aliphatic hydrocarbon groups having 1 to 40 carbon atoms, optionally substituted di- to tetravalent aromatic hydrocarbon rings, and optionally substituted di- to tetravalent heterocycles.
[0055] The di- to tetravalent aliphatic hydrocarbon group having 1 to 40 carbon atoms may be a cyclic, branched, or straight-chain hydrocarbon group. The di- to tetravalent aliphatic hydrocarbon group having 1 to 40 carbon atoms may be a saturated or unsaturated (e.g., saturated) aliphatic hydrocarbon group. The number of carbon atoms in the aliphatic hydrocarbon group having 1 to 40 carbon atoms may be 1 or more, 2 or more, 3 or more, 4 or more, 6 or more, 8 or more, or 10 or more, and may be 35 or less, 30 or less, 25 or less, 20 or less, 15 or less, 10 or less, or 5 or less. The valence of the aliphatic hydrocarbon group may be 2 or more, 3 or more, or 4 or less, 3 or less, or 2.
[0056] The aliphatic hydrocarbon group may have a substituent. Examples of the substituent include —OR′ and —N(R′). 2, —COOR′, and halogen atoms (wherein R′, in each occurrence, is independently a hydrogen atom or an organic group (e.g., a hydrocarbon group, particularly an aliphatic hydrocarbon group) having 1 to 30, 1 to 20, 1 to 10, or 1 to 4 carbon atoms). The substituent may or may not have active hydrogen. The number of substituents may be 6 or less, 5 or less, 4 or less, 3 or less, 2 or less, 1 or less, or 0. In the substituted aliphatic hydrocarbon group, the amount of carbon atoms relative to the amount of carbon atoms and heteroatoms may be 70 mol% or more, 80 mol% or more, 90 mol% or more, 95 mol% or more, or 99 mol% or more, preferably 75 mol% or more, and may be 95 mol% or less, 90 mol% or less, 85 mol% or less, or 80 mol% or less.
[0057] Examples of divalent to tetravalent hydrocarbon aromatic rings include groups obtained by removing 2 to 4 hydrogen atoms from hydrocarbon aromatic rings such as benzene, naphthalene, anthracene, phenanthrene, tetracene (naphthacene), pentacene, pyrene, and coronene. The number of ring-constituting atoms of the hydrocarbon aromatic ring is 3 to 20, 4 to 16, or 5 to 12, and preferably 5 to 12. The valence of the hydrocarbon aromatic ring may be 2 or more, 3 or more, or 4, or 4 or less, 3 or less, or 2.
[0058] The hydrocarbon aromatic ring may have a substituent. Examples of the substituent include -R', -OR', and -N(R'). 2 , —COOR′, and halogen atoms (wherein R′, in each occurrence, is independently a hydrogen atom or an organic group (e.g., a hydrocarbon group, particularly an aliphatic hydrocarbon group) having 1 to 30, 1 to 20, 1 to 10, or 1 to 4 carbon atoms). The substituent may or may not have active hydrogen. The number of substituents may be 6 or less, 5 or less, 4 or less, 3 or less, 2 or less, 1 or less, or 0. In the substituted hydrocarbon aromatic ring, the amount of carbon atoms relative to the amount of carbon atoms and heteroatoms may be 70 mol% or more, 80 mol% or more, 90 mol% or more, 95 mol% or more, or 99 mol% or more, preferably 75 mol% or more, and may be 95 mol% or less, 90 mol% or less, 85 mol% or less, or 80 mol% or less.
[0059] The divalent to tetravalent heterocycle may be an aliphatic group or an aromatic group. Examples of divalent to tetravalent heterocycles include groups obtained by removing 2 to 4 hydrogen atoms from pyridine, pyrazine, pyrimidine, pyridazine, triazine, quinoline, isoquinoline, quinazoline, cinnoline, phthalazine, quinoxaline, pyrrole, indole, furan, benzofuran, thiophene, benzothiophene, pyrazole, imidazole, benzimidazole, triazole, oxazole, benzoxazole, thiazole, benzothiazole, isothiazole, benzisothiazole, pyrrolidine, piperidine, piperazine, imidazolidine, thiazoline, etc. The number of ring-constituting atoms of the heterocycle is 3 to 20, 4 to 16, or 5 to 12, preferably 5 to 12. The valence of the heterocycle may be 2 or more, 3 or more, or 4, or 4 or less, 3 or less, or 2.
[0060] The heterocycle may have a substituent. Examples of the substituent include -R', -OR', and -N(R'). 2 , —COOR′, and halogen atoms (wherein R′, in each occurrence, is independently a hydrogen atom or an organic group (e.g., a hydrocarbon group, particularly an aliphatic hydrocarbon group) having 1 to 30, 1 to 20, 1 to 10, or 1 to 4 carbon atoms). The substituent may or may not have active hydrogen. The number of substituents may be 6 or less, 5 or less, 4 or less, 3 or less, 2 or less, 1 or less, or 0. In the substituted heterocycle, the amount of carbon atoms relative to the amount of carbon atoms and heteroatoms may be 60 mol% or more, 70 mol% or more, 80 mol% or more, 90 mol% or more, 95 mol% or more, or 99 mol% or more, for example, 65 mol% or more, and may be 95 mol% or less, 90 mol% or less, 85 mol% or less, 80 mol% or less, or 70 mol% or less.
[0061] Y 2 Examples of -Ali- -Cy- -Ali(-) 2 -Cy(-) 2 (-) 2 Ali- (-) 2 Cy- (-) 2 Ali (-)2 (-) 2 Cy(-) 2 -Ali-Cy- -Cy-Ali- -Cy-Ali-Cy- -Ali-Cy-Ali- (wherein Ali is an aliphatic hydrocarbon group having 1 to 20 carbon atoms, and Cy is a hydrocarbon aromatic ring or heterocycle.)
[0062] Y 2 Specific examples of -(CH 2 ) p -(p is 1 to 40, 1 to 20, or 1 to 10), a linear hydrocarbon group having an unsaturated bond and having 1 to 40, 1 to 20, or 1 to 10 carbon atoms, a hydrocarbon group having a branched structure and having 1 to 40, 1 to 20, or 1 to 10 carbon atoms, -(CH 2 ) q -Cy-(CH 2 ) r -(q and r each independently represent a number from 0 to 20, for example, from 1 to 10, and Cy represents a hydrocarbon aromatic ring or a heterocycle), and the like.
[0063] (Examples of Y) Examples of Y are described below. In the following, R' is independently in each occurrence a hydrogen atom or an organic group (e.g., a hydrocarbon group, particularly an aliphatic hydrocarbon group) having 1 to 30 carbon atoms (e.g., 1 to 20, 1 to 10, or 1 to 4 carbon atoms).
[0064] Examples of Y include, when Y is divalent, -Y 1 -, -Y 1 -Y 2 -, -Y 1 -Y 2 -Y 1 -, -Y 1 -Y 2 -Y 1 -Y 2 -, -Y 2 -, -Y 2 -Y 1 -, -Y 2 -Y 1 -Y 2 -, -Y 2 -Y 1 -Y 2 -Y 1 - etc.
[0065] As an example of Y, when Y is trivalent, -Y 1 (-) 2 , -Y 1 -Y 2 (-) 2 , -Y 1 -(Y 2 -) 2 , -Y 1 -Y 2 -Y 1 (-) 2 , -Y 1 -Y 2 (-Y 1 -) 2 / / , -Y 1 -(Y 2 1 -Y 2 -) / / , -Y 1 2 -Y 1 -Y 2 -Y 2 1 (-) 2 , -Y 1 -Y 2 -Y 2、 -(Y 1 -) 2 -Y 1 -Y 2 -(Y 2、 -Y 1 -) 2 -Y 1 -(Y 2 -Y 2 -Y 2 -) 2 ; -Y 2 (-) 1 , -Y 2 -Y 2 (-) 1 , -Y 2 -(Y 2 -) 1 , -Y 2 -Y 2 -Y 2 (-) 1 , -Y 2 -Y 2 (-Y 2 -) 1 , -Y 2 -(Y 2 -Y 2 -) 1 , -Y 2 -Y 1 -Y 2 -Y1 (-) 2 ,-Y 2 -Y 1 -Y 2 -(Y 1 -) 2、 -Y 2 -Y 1 -(Y 2 -Y[[ID=,20]] 1 -) 2、 -Y 2 -(Y 1 -Y 2 -Y 1 -) 2 ; etc.
[0066] As an example of Y, when Y is tetravalent, -Y 1 (-) 3 ,-Y 1 -Y 2 (-) 3 ,-Y 1 -(Y 2 -) 3 ,-Y 1 -Y 2 -Y 1 (-) 3 ,-Y 1 -Y 2 (-Y 1 -) 3 ,-Y 1 -(Y 2 -Y 1 -) 3 ,-Y 1 -Y 2 -Y 1 -Y 2 (-) 3 ,-Y 1 -Y 2 -Y 1 -(Y 2 -) 3、 -Y 1 -Y 2 -(Y 1 -Y 2 -) 3、 -Y 1 -(Y 2 1 -Y 2 -) 3 ;-Y 2 (-) 3 ,-Y 2 -Y 1 (-)3 , -Y 2 -(Y 1 -) 3 , -Y 2 -Y 1 -Y 2 (-) 3 , -Y 2 -Y 1 (-Y 2 -) 3 , -Y 2 -(Y 1 -Y 2 -) 3 , -Y 2 -Y 1 -Y 2 -Y 1 (-) 3 , -Y 2 -Y 1 -Y 2 -(Y 1 -) 3、 -Y 2 -Y 1 -(Y 2 -Y 1 -) 3、 -Y 2 -(Y 1 -Y 2 -Y 1 -) 3 ; etc.
[0067] Preferred examples of Y include -Y 1 -, -Y 1 -Y 2 -, -Y 1 -Y 2 -Y 1 -, -Y 1 -Y 2 (-) 2 , -Y 2 -, -Y 2 -Y 1 -, -Y 2 -Y 1 -Y 2 -, -Y 2 -Y 1 (-) 2 , etc.
[0068] (Preferred Examples of Y) Preferably, Y is —O—Y 11 - or -O-Y 11 -Y 21 -Y12 wherein each symbol represents independently at each occurrence: Y 11 is a direct bond, —C(═O)—, —C(═O)—NR′—, or —C(═S)—NR′—; Y 21 is a hydrocarbon group having 1 to 40 carbon atoms which may have a substituent, and Y 12 is -O-, -OC(=O)-, -OC(=O)-O-, -OC(=O)-NR'-, -NR'-, -NR'-C(=O)-, -N R'-C(=O)-O-, -NR'-C(=O)-NR'-, -C(=O)-, -C(=O)-O-, -C(=O)-NR'-, -SO 2 -, -SO 2 NR'-, -C(OR')R'-, or -C(OR')(-) 2 ], or
[0069] Y 11 is a non-hydrocarbon linker, which is a direct bond or a divalent or higher valent group.
[0070] Y 11 The molecular weight of may be 10 or more, 50 or more, 100 or more, 200 or more, 300 or more, or 500 or more, and may be 2000 or less, 1500 or less, 1000 or less, 750 or less, or 500 or less.
[0071] Y 11 may be a direct bond, —C(═O)—, —C(═O)—NR′—, or —C(═S)—NR′—.
[0072] Y 21 is a divalent hydrocarbon linker, which may be a hydrocarbon group having 1 to 40 carbon atoms.
[0073] Y 21 may have 1 or more, 2 or more, 3 or more, 4 or more, 6 or more, 8 or more, 10 or more, 12 or more, 14 or more, 16 or more, or 18 or more carbon atoms, and may be 40 or less, 35 or less, 30 or less, 25 or less, 20 or less, 15 or less, 10 or less, or 5 or less.
[0074] Here, the hydrocarbon group having 1 to 40 carbon atoms may be a cyclic, branched, or straight-chain hydrocarbon group, and may be a saturated or unsaturated (e.g., saturated) aliphatic hydrocarbon group. The hydrocarbon group may have a substituent. Examples of the substituent include -OR', -N(R')2, -COOR', and a halogen atom (wherein R' is, independently in each occurrence, a hydrogen atom or an organic group (e.g., a hydrocarbon group, particularly an aliphatic hydrocarbon group) having 1 to 30, 1 to 20, 1 to 10, or 1 to 4 carbon atoms). The substituent may or may not have an active hydrogen. The number of substituents may be 6 or less, 5 or less, 4 or less, 3 or less, 2 or less, 1 or less, or 0. In the substituted hydrocarbon group, the amount of carbon atoms relative to the amount of carbon atoms and heteroatoms may be 70 mol% or more, 80 mol% or more, 90 mol% or more, 95 mol% or more, or 99 mol% or more, and preferably 75 mol% or more, and may be 95 mol% or less, 90 mol% or less, 85 mol% or less, or 80 mol% or less.
[0075] Y 21 Specific examples of -(CH 2 ) p -(p is 1 to 40, 1 to 20, or 1 to 10), a linear hydrocarbon group having an unsaturated bond and having 1 to 40, 1 to 20, or 1 to 10 carbon atoms, a hydrocarbon group having a branched structure and having 1 to 40, 1 to 20, or 1 to 10 carbon atoms, -(CH 2 ) q -Cy-(CH 2 ) r -(q and r each independently represent a number from 0 to 20, for example, from 1 to 10, and Cy represents a hydrocarbon aromatic ring or a heterocycle), and the like.
[0076] Y 12 -O-, -OC(=O)-, -OC(=O)-O-, -C(=O)-NR'-, -OC(=O)-NR'-, -NR'-, -NR'-C( =O)-, -NR'-C(=O)-O-, -NR'-C(=O)-NR'-, -C(=O)-, -C(=O)-O-, -C(=O)-NR'-, -SO 2 -, -SO 2 NR'-, -C(OR')R'-, or -C(OR')(-)2 It may be.
[0077] [Z] Z is a monovalent hydrocarbon group having 1 to 40 carbon atoms (for example, 20 to 40 carbon atoms) which may have a substituent, and the explanation in the above section (Monovalent hydrocarbon group which may have a substituent) is incorporated herein. The number of carbon atoms in the hydrocarbon group is preferably 6 or more, 8 or more, 10 or more, 12 or more, 14 or more, 16 or more, or 18 or more, and preferably 30 or less, 25 or less, 20 or less, 15 or less, or 10 or less. The hydrocarbon group may also contain unsaturated bonds, and the number of unsaturated bonds is preferably 4 or less, 2 or less, or 1, preferably 1. The substituent is preferably OH (hydroxy group).
[0078] [Other modifying groups] The hydroxy group of the polyol is -Y-Z n Examples of modifying groups are anionic and / or cationic groups.
[0079] Examples of the anionic group include a monomer having a carboxyl group, a sulfonic acid group, or a phosphoric acid group.
[0080] Examples of salts of anionic groups include alkali metal salts, alkaline earth metal salts, and ammonium salts, such as methylammonium salts, ethanolammonium salts, and triethanolammonium salts.
[0081] The cationic group is an amino group, preferably a tertiary amino group or a quaternary amino group. In the tertiary amino group, two groups bonded to the nitrogen atom may be the same or different and may be an aliphatic group having 1 to 5 carbon atoms (particularly an alkyl group), an aromatic group having 6 to 20 carbon atoms (aryl group), or an araliphatic group having 7 to 25 carbon atoms (particularly an aralkyl group, for example a benzyl group (C 6 H 5 -CH 2 In the quaternary amino group, the three groups bonded to the nitrogen atom are the same or different and are an aliphatic group having 1 to 5 carbon atoms (particularly an alkyl group), an aromatic group having 6 to 20 carbon atoms (aryl group), or an araliphatic group having 7 to 25 carbon atoms (particularly an aralkyl group, for example a benzyl group (C 6 H 5 -CH 2In the tertiary amino group and the quaternary amino group, the remaining group bonded to the nitrogen atom may have a carbon-carbon double bond. The cationic group may be in the form of a salt.
[0082] The cationic group in the form of a salt is a salt with an acid (organic acid or inorganic acid). Organic acids, such as carboxylic acids having 1 to 20 carbon atoms (particularly monocarboxylic acids such as acetic acid, propionic acid, butyric acid, and stearic acid) are preferred.
[0083] [Production Method] The modified polyol may be produced by reacting a modifying agent having a modifying group (or a precursor structure of the modifying group) with a hydroxy group of a polyol.
[0084] (Polyol) A polyol is a compound having two or more hydroxy groups and is a compound that serves as a raw material for a modified polyol. A polyol is a compound having two or more hydroxy groups in the molecule. The polyol may be aliphatic or aromatic, but is preferably aliphatic.
[0085] The polyol may have an ether bond. Preferably, the polyol may have two or more ether bonds. Specifically, the polyol is preferably a compound having two or more hydroxy groups and two or more ether bonds. In other words, the polyol is preferably a polyether having two or more hydroxy groups.
[0086] When the polyol is a polymer, the repeating structure of the monomer unit may contain a hydroxy group and an ether bond.
[0087] The polyol may be low molecular weight (e.g., weight average molecular weight less than 1,000, 500 or less) and / or high molecular weight. The weight average molecular weight of the polyol may be 50 or more, 100 or more, 300 or more, 500 or more, 1,000 or more, 3,000 or more, 5,000 or more, 10,000 or more, 30,000 or more, 100,000 or more, 300,000 or more, or 500,000 or more; or 1,000,000 or less, 750,000 or less, 500,000 or less, 300,000 or less, 100,000 or less, 75,000 or less, 50,000 or less, 30,000 or less, 10,000 or less, 5,000 or less, 3,000 or less, 2,000 or less, 1,000 or less, or 500 or less.
[0088] The number of hydroxy groups in the polyol may be 2 or more, 5 or more, 7 or more, 10 or more, 15 or more, 30 or more, 50 or more, or 100 or more, and may be 3000 or less, 1000 or less, 750 or less, 500 or less, 300 or less, 100 or less, 50 or less, 30 or less, or 20 or less.
[0089] The hydroxy group equivalent weight of the polyol may be 20 or more, 40 or more, 60 or more, 80 or more, 100 or more, 120 or more, or 150 or more, and may be 1000 or less, 800 or less, 600 or less, 400 or less, 200 or less, 100 or less, or 75 or less. The hydroxy group equivalent weight of the polyol is the value obtained by dividing the weight average molecular weight of the polyol by the number of hydroxyl groups.
[0090] The polyol may be a natural product. The natural product may be a high molecular weight natural product, a low molecular weight natural product, or a derivative thereof. The above natural products also include compounds converted from microorganisms. Examples of polyols include monosaccharides, oligosaccharides, polysaccharides, sugar alcohols (reducing sugars), hydroxy acids, amino acids, vitamins, flavonols, hydroxy hydrocarbons, hydroxy group-containing compound polymers, polyether polyols, polymer polyols, polyester polyols, and other polyols.
[0091] Examples of monosaccharides include glucose, fructose, galactose, and xylose.
[0092] Examples of oligosaccharides include sucrose, cycloamylose, cyclodextrin, maltose, trehalose, lactose, and sucralose.
[0093] Examples of sugar alcohols (reducing sugars) include sorbitol, maltitol, erythritol, glycerin, isomalt, lactitol, mannitol, xylitol, sorbitan, and lactitol.
[0094] Examples of polysaccharides include starch, cellulose, curdlan, pullulan, alginic acid, carrageenan, guar gum, chitin, chitosan, locust bean gum, kappa carrageenan, iota carrageenan, isomaltodextrin, gellan gum, and tamarind seed gum.
[0095] Examples of hydroxy acids include ascorbic acid, kojic acid, quinic acid, chlorogenic acid, and gluconic acid.
[0096] Examples of amino acids include glucosamine.
[0097] Examples of vitamins include ascorbic acid and inositol.
[0098] Examples of flavonols include catechin, quercetin, and anthocyanin.
[0099] Examples of hydroxy hydrocarbons include ethylene glycol, propylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, neopentyl glycol, trimethylene glycol, glycerin, trimethylolpropane, trimethylolethane, etc. Hydroxy hydrocarbons are hydrocarbons having a hydroxy group and may be aromatic or aliphatic, but are preferably aliphatic. The term "hydroxy hydrocarbon" may also refer to hydroxy hydrocarbons other than compounds included in other groups such as polysaccharides (other hydroxy hydrocarbons).
[0100] Examples of the hydroxy group-containing compound polymer include polyglycerin, polyvinyl alcohol, hydroxyethyl (meth)acrylate polymer, hydroxypropyl (meth)acrylate polymer, and hydroxybutyl (meth)acrylate polymer.
[0101] An example of a polyether polyol may be a compound obtained by addition polymerization of an alkylene oxide with an initiator. Examples of initiators include compounds having two or more functional hydroxyl groups. Examples of initiators include propylene glycol, polypropylene glycol, ethylene glycol, polyethylene glycol, glycerin, polyglycerin, trimethylolpropane, triethanolamine, pentaerythritol, ethylenediamine, aromatic diamines, diethylenetriamine, sorbitol, and sucrose. Examples of alkylene oxides include ethylene oxide and propylene oxide. Polyether polyols obtained by addition polymerization of alkylene oxide with the above initiators are also referred to as polyoxyalkylene polyols or oxyalkylene derivatives of polyols. Representative examples of polyether polyols include polyoxypropylene triols obtained by addition polymerization of propylene oxide with glycerin, and polyoxypropylene polyglyceryl ethers obtained by addition polymerization of propylene oxide with polyglycerin.
[0102] An example of a polymer polyol is a compound obtained by polymerizing at least a portion of a polyether polyol with an ethylenically unsaturated monomer, such as acrylonitrile or styrene.
[0103] Examples of polyester polyols include compounds obtained by dehydration condensation of a compound having a bifunctional or higher carboxyl group and a compound having a bifunctional or higher hydroxyl group. Examples of compounds having a bifunctional or higher carboxyl group include terephthalic acid, isophthalic acid, phthalic acid, methylphthalic acid, trimellitic acid, pyromellitic acid, adipic acid, sebacic acid, succinic acid, maleic acid, fumaric acid, tetrahydrophthalic acid, methyltetrahydrophthalic acid, hexahydrophthalic acid, and acid anhydrides thereof. Examples of compounds having a bifunctional or higher hydroxyl group include ethylene glycol, propylene glycol, propanediol, neopentyl glycol, glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, and polymers thereof.
[0104] (Modifying Agent) The modifying agent is a compound reactive with polyol, and is preferably a compound having the above-mentioned monovalent hydrocarbon group having 1 to 40 carbon atoms (for example, 20 to 40 carbon atoms) which may have a substituent.
[0105] Examples of modifying agents are: Acid halide G(O=)C-Z Acid anhydride O(C(=O)-Z) 2 Carboxylic acid HO(O=)C-Z Isocyanate O=C=N-Z Thioisocyanate S=C=N-Z Epoxy (CH 2 OCH)CH 2 O-Z Halide G-Z Amine H 2 N-Z hydroxy HO-Z, wherein Z is as defined above and G is a halogen atom (e.g., F, Cl, Br, or I).
[0106] Z in the structure of the modifying agent described above may be replaced with any group constituting a modifying group. For example, Z may be a monovalent hydrocarbon group having 1 to 40 carbon atoms (e.g., 20 to 40 carbon atoms) which may have a substituent, or Z may be -Y-Z n It may also be possible to use the following.
[0107] The modified polyol may be synthesized by reacting a polyol with a modifying agent. For example, a modified polyol can be synthesized by reacting a modifying agent such as an acid halide compound, an acid anhydride, or a carboxylic acid with a hydroxy group of a polyol to form an ester bond. Alternatively, a modified polyol can be produced by reacting a modifying agent such as a halide or an epoxy compound with a hydroxy group of a polyol to form an ether bond. Those skilled in the art can appropriately design the reaction conditions between the polyol and the modifying agent, such as by using a catalyst (e.g., an acid catalyst or a base catalyst) or a condensing agent, depending on the desired product.
[0108] [Dispersant] The repellent of the present disclosure preferably contains a dispersant.
[0109] The dispersant may be selected from organic dispersants and inorganic dispersants. At least one type may be used. The dispersant may be at least one type selected from anionic dispersants, nonionic dispersants, cationic dispersants, amphoteric dispersants, and inorganic dispersants. The repellent may not contain an anionic dispersant. The dispersant may contain a dispersant other than a fatty acid ester having an HLB value of 7 or more. For example, the dispersant may contain a fatty acid ester-based dispersant having an HLB value of less than 7, or may contain a dispersant other than a fatty acid ester.
[0110] As the dispersant, an organic dispersant and an inorganic dispersant may be used individually, or a combination of an organic dispersant and an inorganic dispersant may be used.
[0111] An organic dispersant may be used as the dispersant. The organic dispersant can be classified into a nonionic dispersant, an anionic dispersant, a cationic dispersant, and an amphoteric dispersant, and the organic dispersant may refer to a surfactant.
[0112] The dispersant may be fluorine-free.
[0113] [Nonionic Dispersant] The dispersant may contain a nonionic dispersant, which may be a nonionic surfactant.
[0114] The nonionic dispersant may be a low molecular weight or a high molecular weight dispersant, and may have a molecular weight of 100 or more, 500 or more, 1000 or more, 2000 or more, 4000 or more, or 6000 or more, and may be 100,000 or less, 10,000 or less, 7,500 or less, 5,000 or less, 25,000 or less, 750 or less, or 250 or less.
[0115] Examples of nonionic dispersants include ethers, esters, ester ethers, alkanolamides, polyols and amine oxides.
[0116] An example of an ether is a compound having an oxyalkylene group (preferably a polyoxyethylene group).
[0117] An example of the ester is an ester of an alcohol and a fatty acid. An example of the alcohol is a mono- to trio-hydric (particularly di- to deca-hydric) alcohol (e.g., aliphatic alcohol) having 1 to 50 carbon atoms (particularly 10 to 30 carbon atoms). An example of the fatty acid is a saturated or unsaturated fatty acid having 2 to 50 carbon atoms, particularly 5 to 30 carbon atoms.
[0118] An example of an ester ether is a compound in which an alkylene oxide (particularly ethylene oxide) is added to an ester of an alcohol and a fatty acid. An example of an alcohol is a mono- to trio-hydric (particularly di- to deca-hydric) alcohol (e.g., aliphatic alcohol) having 1 to 50 carbon atoms (particularly 3 to 30 carbon atoms). An example of a fatty acid is a saturated or unsaturated fatty acid having 2 to 50 carbon atoms, particularly 5 to 30 carbon atoms.
[0119] Examples of alkanolamides are those formed from fatty acids and alkanolamines. The alkanolamides may be monoalkanolamides or dialkanolamines. Examples of fatty acids include saturated or unsaturated fatty acids having 2 to 50 carbon atoms, particularly 5 to 30 carbon atoms. The alkanolamines may be alkanols having 2 to 50 carbon atoms, particularly 5 to 30 carbon atoms, and having 1 to 3 amino groups and 1 to 5 hydroxyl groups.
[0120] The polyol may be a di- to penta-hydric alcohol having 10 to 30 carbon atoms. The amine oxide may be an oxide (for example, having 5 to 50 carbon atoms) of an amine (secondary amine or preferably tertiary amine).
[0121] The nonionic dispersant is preferably a nonionic dispersant having an oxyalkylene group (preferably a polyoxyethylene group). The number of carbon atoms in the alkylene group in the oxyalkylene group is preferably 2 to 10. The number of oxyalkylene groups in the molecule of the nonionic dispersant is generally preferably 2 to 100.
[0122] The nonionic dispersant is selected from the group consisting of ethers, esters, ester ethers, alkanolamides, polyols and amine oxides, and is preferably a nonionic dispersant having an oxyalkylene group.
[0123] The nonionic dispersant may be an alkylene oxide adduct of a linear and / or branched aliphatic (saturated and / or unsaturated) group, a polyalkylene glycol ester of a linear and / or branched fatty acid (saturated and / or unsaturated), a sorbitan ester of a linear and / or branched fatty acid (saturated and / or unsaturated), a glycerin ester of a linear and / or branched fatty acid (saturated and / or unsaturated), a polyglycerin ester of a linear and / or branched fatty acid (saturated and / or unsaturated), a sucrose ester of a linear and / or branched fatty acid (saturated and / or unsaturated), a polyoxyethylene (POE) / polyoxypropylene (POP) copolymer (random copolymer or block copolymer), an alkylene oxide adduct of acetylene glycol, or the like. Among these, those in which the alkylene oxide adduct moiety and the polyalkylene glycol moiety have a structure of polyoxyethylene (POE), polyoxypropylene (POP), or a POE / POP copolymer (which may be a random copolymer or a block copolymer) are preferred. Furthermore, the nonionic dispersant does not have to contain an aromatic group.
[0124] The nonionic dispersant has the formula: 1 O-(CH 2 CH 2 O) p - (R 2 O) q -R 3 [In the formula, R 1is an alkyl group having 1 to 22 carbon atoms, or an alkenyl group or acyl group having 2 to 22 carbon atoms, 2 are independently the same or different and are alkylene groups having 3 or more carbon atoms (e.g., 3 to 10), 3 is a hydrogen atom, an alkyl group having 1 to 22 carbon atoms, or an alkenyl group having 2 to 22 carbon atoms, p is a number of 2 or more, and q is a number of 0 or 1 or more.
[0125] R 1 R preferably has 8 to 20 carbon atoms, particularly 10 to 18 carbon atoms. 1 Preferred specific examples of R include an octyl group, a nonyl group, a trimethylnonyl group, a lauryl group, a tridecyl group, an oleyl group, and a stearyl group. 2 Examples of the nonionic dispersant are a propylene group and a butylene group. In the nonionic dispersant, p may be a number of 3 or more (for example, 5 to 200). q may be a number of 2 or more (for example, 5 to 200). That is, -(R 2 O) q - may form a polyoxyalkylene chain. The nonionic dispersant may be a polyoxyethylene alkylene alkyl ether containing a hydrophilic polyoxyethylene chain and a hydrophobic oxyalkylene chain (particularly a polyoxyalkylene chain) at the center. Examples of the hydrophobic oxyalkylene chain include an oxypropylene chain, an oxybutylene chain, and a styrene chain, with the oxypropylene chain being preferred.
[0126] Specific examples of nonionic dispersants include ethylene oxide and hexylphenol, isooctatylphenol, hexadecanol, oleic acid, alkanes (C 12 -C 16 ) thiol, sorbitan mono fatty acid (C 7 -C 19 ) or alkyl (C 12 -C 18) condensation products with amines, etc., sorbitan fatty acid esters, glycerin fatty acid esters, polyglycerin fatty acid esters, sucrose fatty acid esters, propylene glycol fatty acid esters, polyoxyethylene alkyl ethers, polyoxyethylene polyoxypropylene alkyl ethers, polyoxyethylene glycerin fatty acid esters, polyoxyethylene sorbitan fatty acid esters, lecithin derivatives, etc.
[0127] The proportion of polyoxyethylene blocks can be 5 to 80% by weight, for example 30 to 75% by weight, and particularly 40 to 70% by weight, based on the molecular weight of the nonionic dispersant (copolymer). The average molecular weight of the nonionic dispersant is generally 300 to 5,000, for example 500 to 3,000. The nonionic dispersant may be a single type or a mixture of two or more types. The nonionic dispersant may be a mixture of a compound having an HLB (hydrophilic-hydrophobic balance) of less than 15 (particularly 5 or less) and a compound having an HLB of 15 or more. Specifically, it is preferable to select from polyoxyethylene alkyl ethers, polyoxyethylene polyoxypropylene alkyl ethers, polyoxyethylene, and polyoxypropylenes having an HLB value of 1 to 18, and sorbitan fatty acid esters, glycerin fatty acid esters, polyglycerin fatty acid esters, sucrose fatty acid esters, propylene glycol fatty acid esters, polyoxyethylene glycerin fatty acid esters, and polyoxyethylene sorbitan fatty acid esters having an HLB value of less than 7.
[0128] [Cationic Dispersant] The dispersant may contain a cationic dispersant. The cationic dispersant may be a cationic surfactant. The cationic dispersant may be a low molecular weight type (e.g., molecular weight of 2000 or less, particularly 10000 or less) or a high molecular weight type (e.g., molecular weight of 2000 or more). The cationic dispersant may be a compound having no amide group.
[0129] The cationic dispersant may be a low molecular weight or a high molecular weight dispersant, and may have a molecular weight of 100 or more, 500 or more, 1000 or more, 2000 or more, 4000 or more, or 6000 or more, and may have a molecular weight of 100,000 or less, 10,000 or less, 7,500 or less, 5,000 or less, 25,000 or less, 750 or less, or 250 or less.
[0130] The cationic dispersant may be an amine salt, a quaternary ammonium salt, or an oxyethylene adduct ammonium salt.Specific examples of the cationic dispersant include, but are not limited to, amine salt-type dispersants such as alkylamine salts, amino alcohol fatty acid derivatives, polyamine fatty acid derivatives, and imidazoline, and quaternary ammonium salt-type dispersants such as alkyltrimethylammonium salts, dialkyldimethylammonium salts, alkyldimethylbenzylammonium salts, pyridinium salts, alkylisoquinolinium salts, benzethonium chloride, and benzalkonium chloride.
[0131] Preferred examples of cationic dispersants are: 21 -N + (-R 22 ) (-R 23 ) (-R 24 ) X - [In the formula, R 21 , R 22 , R 23 and R 24 is a hydrocarbon group having 1 to 40 carbon atoms, and X is an anionic group. 21 , R 22 , R 23 and -R 24 Specific examples of X are alkyl groups (e.g., methyl, butyl, stearyl, and palmityl). Specific examples of X are halogens (e.g., chlorine) and acids (e.g., hydrochloric acid and acetic acid). The cationic dispersant is particularly preferably a monoalkyltrimethylammonium salt (wherein the alkyl has 4 to 40 carbon atoms).
[0132] The cationic dispersant is preferably an ammonium salt. The cationic dispersant has the formula: 1 p -N + R 2q X - [In the formula, R 1 is C12 or more (e.g. C 12 ~C 50 ) linear and / or branched aliphatic (saturated and / or unsaturated) groups, R 2 is H or a C1-4 alkyl group, a benzyl group, a polyoxyethylene group (the number of oxyethylene groups is, for example, 1 (particularly 2, particularly 3) to 50) (CH 3 , C 2 H 5 is particularly preferred), X is a halogen atom (for example), C 1 ~C 4 where p is 1 or 2, q is 2 or 3, and p+q=4. 1 may have 12 to 50 carbon atoms, for example, 12 to 30 carbon atoms.
[0133] Specific examples of cationic dispersants include dodecyltrimethylammonium acetate, trimethyltetradecylammonium chloride, hexadecyltrimethylammonium bromide, trimethyloctadecylammonium chloride, (dodecylmethylbenzyl)trimethylammonium chloride, benzyldodecyldimethylammonium chloride, methyldodecyldi(hydropolyoxyethylene)ammonium chloride, benzyldodecyldi(hydropolyoxyethylene)ammonium chloride, and N-[2-(diethylamino)ethyl]oleamide hydrochloride.
[0134] [Anionic Dispersant] The dispersant may contain an anionic dispersant. The anionic dispersant may be an anionic surfactant. The dispersant may not contain an anionic dispersant.
[0135] The anionic dispersant may be a low molecular weight or a high molecular weight dispersant, and may have a molecular weight of 100 or more, 500 or more, 1000 or more, 2000 or more, 4000 or more, or 6000 or more, and may have a molecular weight of 100,000 or less, 10,000 or less, 7,500 or less, 5,000 or less, 25,000 or less, 750 or less, or 250 or less.
[0136] Examples of anionic dispersants include alkyl ether sulfates, alkyl sulfates, alkenyl ether sulfates, alkenyl sulfates, olefin sulfonates, alkanesulfonates, saturated or unsaturated fatty acid salts, alkyl or alkenyl ether carboxylates, α-sulfonic acid salts, N-acylamino acid type dispersants, phosphate mono- or diester type dispersants, and sulfosuccinate esters.
[0137] [Amphoteric Dispersant] The dispersant may contain an amphoteric dispersant, which may be an amphoteric surfactant.
[0138] The amphoteric dispersant may be a low molecular weight or a high molecular weight dispersant, and may have a molecular weight of 100 or more, 500 or more, 1000 or more, 2000 or more, 4000 or more, or 6000 or more, and may have a molecular weight of 100,000 or less, 10,000 or less, 7,500 or less, 5,000 or less, 25,000 or less, 750 or less, or 250 or less.
[0139] Examples of amphoteric dispersants include alanines, imidazolinium betaines, amido betaines, and acetic acid betaine, and specific examples include lauryl betaine, stearyl betaine, lauryl carboxymethyl hydroxyethyl imidazolinium betaine, lauryl dimethylamino acetic acid betaine, and fatty acid amidopropyl dimethylamino acetic acid betaine.
[0140] [Inorganic Dispersant] The dispersant may contain an inorganic dispersant.
[0141] The average primary particle size of the inorganic dispersant may be 5 nm or more, 30 nm or more, 100 nm or more, 1 μm or more, 10 μm or more, or 25 μm or more, and may be 100 μm or less, 50 μm or less, 10 μm or less, 1 μm or less, 500 nm or less, or 300 nm or less. The average primary particle size can be measured, for example, by observation with a microscope (scanning electron microscope or transmission electron microscope). The inorganic dispersant may be hydrophilic particles.
[0142] Examples of inorganic dispersants include polyvalent metal phosphates such as tricalcium phosphate, magnesium phosphate, aluminum phosphate, zinc phosphate, and hydroxyapatite; carbonates such as calcium carbonate and magnesium carbonate; silicates such as calcium metasilicate; sulfates such as calcium sulfate and barium sulfate; and hydroxides such as calcium hydroxide, magnesium hydroxide, and aluminum hydroxide.
[0143] [Amount of Dispersant] The amount of dispersant may be 0.01 parts by weight or more, 0.1 parts by weight or more, 1 part by weight or more, 3 parts by weight or more, 5 parts by weight or more, 10 parts by weight or more, 15 parts by weight or more, 20 parts by weight or more, 50 parts by weight or more, 75 parts by weight or more, or 100 parts by weight or more, relative to 100 parts by weight of the modified polyol. Alternatively, the amount of dispersant may be 500 parts by weight or less, 300 parts by weight or less, 200 parts by weight or less, 100 parts by weight or less, 30 parts by weight or less, 20 parts by weight or less, 10 parts by weight or less, 5 parts by weight or less, 3 parts by weight or less, or 1 part by weight or less.
[0144] [Liquid Medium] The repellent agent of the present disclosure may contain a liquid medium. The liquid medium may be water, an organic solvent, or a mixture of water and an organic solvent. The repellent agent may be a dispersion or a solution. The repellent agent of the present disclosure may be a water-dispersed type and may contain at least water.
[0145] Examples of organic solvents include esters (e.g., esters having 2 to 40 carbon atoms, specifically, ethyl acetate and butyl acetate), ketones (e.g., ketones having 2 to 40 carbon atoms, specifically, methyl ethyl ketone and diisobutyl ketone), alcohols (e.g., alcohols having 1 to 40 carbon atoms, specifically, isopropyl alcohol), aromatic solvents (e.g., toluene and xylene), and petroleum solvents (e.g., alkanes having 5 to 10 carbon atoms, specifically, naphtha and kerosene). The organic solvent is preferably a water-soluble organic solvent. The water-soluble organic solvent may contain a compound having at least one hydroxy group (e.g., alcohol, polyols such as glycol-based solvents, ethers of polyols (e.g., monoethers), etc.). These may be used alone or in combination.
[0146] [Amount of Liquid Medium] The amount of the liquid medium may be 1 part by weight or more, 3 parts by weight or more, 5 parts by weight or more, 10 parts by weight or more, 20 parts by weight or more, 30 parts by weight or more, 40 parts by weight or more, 50 parts by weight or more, 100 parts by weight or more, 200 parts by weight or more, 300 parts by weight or more, 500 parts by weight or more, or 1000 parts by weight or more, relative to 1 part by weight of the polyol modified product, and may be 3000 parts by weight or less, 2000 parts by weight or less, 1000 parts by weight or less, 500 parts by weight or less, 200 parts by weight or less, 175 parts by weight or less, 150 parts by weight or less, 125 parts by weight or less, 100 parts by weight or less, 80 parts by weight or less, 60 parts by weight or less, 40 parts by weight or less, 20 parts by weight or less, or 10 parts by weight or less.
[0147] The amount of water may be 1 part by weight or more, 3 parts by weight or more, 5 parts by weight or more, 10 parts by weight or more, 20 parts by weight or more, 30 parts by weight or more, 40 parts by weight or more, 50 parts by weight or more, 100 parts by weight or more, 200 parts by weight or more, 300 parts by weight or more, 500 parts by weight or more, or 1000 parts by weight or more, and may be 3000 parts by weight or less, 2000 parts by weight or less, 1000 parts by weight or less, 500 parts by weight or less, 200 parts by weight or less, 175 parts by weight or less, 150 parts by weight or less, 125 parts by weight or less, 100 parts by weight or less, 80 parts by weight or less, 60 parts by weight or less, 40 parts by weight or less, 20 parts by weight or less, or 10 parts by weight or less, per part by weight of the polyol modified product.
[0148] The amount of organic solvent may be 1 part by weight or more, 3 parts by weight or more, 5 parts by weight or more, 10 parts by weight or more, 20 parts by weight or more, 30 parts by weight or more, 40 parts by weight or more, 50 parts by weight or more, 100 parts by weight or more, 200 parts by weight or more, 300 parts by weight or more, 500 parts by weight or more, or 1000 parts by weight or more, and may be 3000 parts by weight or less, 2000 parts by weight or less, 1000 parts by weight or less, 500 parts by weight or less, 200 parts by weight or less, 175 parts by weight or less, 150 parts by weight or less, 125 parts by weight or less, 100 parts by weight or less, 80 parts by weight or less, 60 parts by weight or less, 40 parts by weight or less, 20 parts by weight or less, or 10 parts by weight or less, per part by weight of the polyol modified product.
[0149] [Silicone] The repellent agent according to the present disclosure may contain silicone (polyorganosiloxane). By containing silicone, it is possible to obtain good texture and durability in addition to good liquid repellency.
[0150] As the silicone, known silicones can be used, and examples of silicones include polydimethylsiloxane and modified silicones (amino-modified, epoxy-modified silicone, carboxy-modified silicone, methylhydrogen silicone, etc.). The silicone may be a silicone wax having wax-like properties. These may be used alone or in combination of two or more.
[0151] The weight average molecular weight of the silicone may be 1,000 or more, 10,000 or more, or 50,000 or more. The weight average molecular weight of the silicone may be 500,000 or less, 2,500,000 or less, 100,000 or less, or 50,000 or less.
[0152] [Amount of Silicone] The amount of silicone may be 0.1 parts by weight or more, 1 part by weight or more, 3 parts by weight or more, 5 parts by weight or more, 10 parts by weight or more, 15 parts by weight or more, 20 parts by weight or more, 50 parts by weight or more, 75 parts by weight or more, or 100 parts by weight or more, relative to 100 parts by weight of the polyol modified product, and may be 500 parts by weight or less, 300 parts by weight or less, 200 parts by weight or less, 100 parts by weight or less, 50 parts by weight or less, 40 parts by weight or less, 30 parts by weight or less, 20 parts by weight or less, 10 parts by weight or less, or 5 parts by weight or less.
[0153] [Wax] The repellent agent according to the present disclosure may contain wax. By including wax, it is possible to impart good liquid repellency to the substrate.
[0154] Examples of waxes include paraffin wax, microcrystalline wax, Fischer-Tropsch wax, polyolefin wax (polyethylene wax, polypropylene wax, etc.), oxidized polyolefin wax, silicone wax, animal and vegetable wax, mineral wax, etc. Paraffin wax is preferred. Specific examples of compounds constituting the wax include normal alkanes (e.g., tricosane, tetracosane, pentacosane, hexacosane, heptacosane, octacosane, nonacosane, triacontane, hentriacontane, dotriacontane, tritriacontane, tetratriacontane, pentatriacontane, and hexatriacontane), and normal alkenes (e.g., 1-eicosane, 1-docosene, 1-tricosene, 1-tetracosene, 1-pentacosene, 1-hexacosene, 1-heptacosene, 1-octacosene, nonacosane, triacontane, hentriacontane, dotriacontane, tritriacontane, tetratriacontane, pentatriacontane, and hexatriacontane). The number of carbon atoms in the compounds constituting the wax is preferably 20 to 60, for example, 25 to 45. The molecular weight of the wax may be from 200 to 2000, for example, from 250 to 1500, or from 300 to 1000. These may be used alone or in combination of two or more.
[0155] The melting point of the wax may be 50° C. or higher, 55° C. or higher, 60° C. or higher, 65° C. or higher, or 70° C. or higher, preferably 55° C. or higher, more preferably 60° C. or higher. The melting point of the wax is measured in accordance with JIS K 2235-1991.
[0156] [Amount of Wax] The amount of wax may be 0.1 parts by weight or more, 1 part by weight or more, 3 parts by weight or more, 5 parts by weight or more, 10 parts by weight or more, 15 parts by weight or more, 20 parts by weight or more, 50 parts by weight or more, 75 parts by weight or more, or 100 parts by weight or more, relative to 100 parts by weight of the polyol modified product, and may be 500 parts by weight or less, 300 parts by weight or less, 200 parts by weight or less, 100 parts by weight or less, 50 parts by weight or less, 40 parts by weight or less, 30 parts by weight or less, 20 parts by weight or less, 10 parts by weight or less, or 5 parts by weight or less.
[0157] [Organic Acid] The repellent of the present disclosure may contain an organic acid. Known organic acids can be used. Preferred organic acids include carboxylic acids, sulfonic acids, sulfinic acids, etc., with carboxylic acids being particularly preferred. Examples of the carboxylic acid include formic acid, acetic acid, propionic acid, butyric acid, oxalic acid, succinic acid, glutaric acid, adipic acid, malic acid, citric acid, etc., with formic acid or acetic acid being particularly preferred. In the present disclosure, one type of organic acid may be used, or two or more types may be used in combination. For example, formic acid and acetic acid may be used in combination.
[0158] [Amount of Organic Acid] The amount of organic acid may be 0.1 parts by weight or more, 1 part by weight or more, 3 parts by weight or more, 5 parts by weight or more, 10 parts by weight or more, 15 parts by weight or more, 20 parts by weight or more, 50 parts by weight or more, 75 parts by weight or more, or 100 parts by weight or more, relative to 100 parts by weight of the polyol-modified product, and may be 500 parts by weight or less, 300 parts by weight or less, 200 parts by weight or less, 100 parts by weight or less, 50 parts by weight or less, 40 parts by weight or less, 30 parts by weight or less, 20 parts by weight or less, 10 parts by weight or less, or 5 parts by weight or less. The amount of organic acid may be adjusted so that the pH of the repellent is 3 to 10, for example, 5 to 9, particularly 6 to 8. The repellent may be acidic (pH 7 or less, for example, 6 or less).
[0159] [Hardening Agent] The repellent of the present disclosure may contain a hardening agent (active hydrogen-reactive compound or active hydrogen-containing compound).
[0160] The curing agent (crosslinking agent) in the repellent agent can effectively cure the modified polyol. The curing agent may be an active hydrogen-reactive compound or an active hydrogen-containing compound that reacts with the active hydrogen or active hydrogen-reactive groups of the modified polyol. Examples of active hydrogen-reactive compounds include isocyanate compounds, epoxy compounds, chloromethyl group-containing compounds, carboxyl group-containing compounds, and hydrazide compounds. Examples of active hydrogen-containing compounds include hydroxyl group-containing compounds, amino group-containing compounds, carboxyl group-containing compounds, ketone group-containing compounds, hydrazide compounds, and melamine compounds.
[0161] The curing agent may contain an isocyanate compound. The isocyanate compound may be a polyisocyanate compound. The polyisocyanate compound is a compound having two or more isocyanate groups in one molecule. The polyisocyanate compound functions as a crosslinking agent. Examples of polyisocyanate compounds include aliphatic polyisocyanates, alicyclic polyisocyanates, araliphatic polyisocyanates, aromatic polyisocyanates, and derivatives of these polyisocyanates. The isocyanate compound may be a blocked isocyanate compound (for example, a blocked polyisocyanate compound). The blocked isocyanate compound is a compound in which the isocyanate group of an isocyanate compound is masked with a blocking agent to inhibit reaction.
[0162] Examples of aliphatic polyisocyanates include trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, pentamethylene diisocyanate, 1,2-propylene diisocyanate, 1,2-butylene diisocyanate, 2,3-butylene diisocyanate, 1,3-butylene diisocyanate, 2,4,4- or 2,2,4-trimethylhexamethylene diisocyanate, 2,6-diisocyanate, Aliphatic diisocyanates such as cyanatomethyl caproate, and aliphatic triisocyanates such as lysine ester triisocyanate, 1,4,8-triisocyanatooctane, 1,6,11-triisocyanatoundecane, 1,8-diisocyanato-4-isocyanatomethyloctane, 1,3,6-triisocyanatohexane, and 2,5,7-trimethyl-1,8-diisocyanato-5-isocyanatomethyloctane. These may be used alone or in combination of two or more.
[0163] Examples of alicyclic polyisocyanates include alicyclic diisocyanates and alicyclic triisocyanates. Specific examples of alicyclic polyisocyanates include 1,3-cyclopentene diisocyanate, 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate (isophorone diisocyanate), and 1,3,5-triisocyanatocyclohexane. These may be used alone or in combination of two or more.
[0164] Examples of araliphatic polyisocyanates include araliphatic diisocyanates and araliphatic triisocyanates. Specific examples of araliphatic polyisocyanates include 1,3- or 1,4-xylylene diisocyanate or a mixture thereof, 1,3- or 1,4-bis(1-isocyanato-1-methylethyl)benzene (tetramethylxylylene diisocyanate) or a mixture thereof, and 1,3,5-triisocyanatomethylbenzene. These may be used alone or in combination of two or more.
[0165] Examples of aromatic polyisocyanates include aromatic diisocyanates, aromatic triisocyanates, and aromatic tetraisocyanates. Specific examples of aromatic polyisocyanates include m-phenylene diisocyanate, p-phenylene diisocyanate, 4,4'-diphenyl diisocyanate, 1,5-naphthalene diisocyanate, 2,4'- or 4,4'-diphenylmethane diisocyanate or a mixture thereof, 2,4- or 2,6-tolylene diisocyanate or a mixture thereof, triphenylmethane-4,4',4''-triisocyanate, and 4,4'-diphenylmethane-2,2',5,5'-tetraisocyanate. These may be used alone or in combination of two or more.
[0166] Examples of the polyisocyanate derivatives include various derivatives of the above-mentioned polyisocyanate compounds, such as dimers, trimers, biurets, allophanates, carbodiimides, uretdiones, uretimines, isocyanurates, and iminooxadiazinediones. These may be used alone or in combination of two or more.
[0167] These polyisocyanates can be used alone or in combination of two or more. As the polyisocyanate compound, it is preferable to use a blocked polyisocyanate compound (blocked isocyanate), which is a compound in which the isocyanate group of a polyisocyanate compound is blocked with a blocking agent. It is preferable to use a blocked polyisocyanate compound because it is relatively stable in solution and can be used in the same solution as the repellent.
[0168] The blocking agent blocks free isocyanate groups. When the blocked polyisocyanate compound is heated to, for example, 100°C or higher, e.g., 130°C or higher, the isocyanate groups are regenerated and can easily react with hydroxyl groups. Examples of blocking agents include phenolic compounds, lactam compounds, aliphatic alcohol compounds, and oxime compounds. The polyisocyanate compounds can be used alone or in combination of two or more.
[0169] An epoxy compound is a compound having an epoxy group. Examples of epoxy compounds include epoxy compounds having a polyoxyalkylene group, such as polyglycerol polyglycidyl ether and polypropylene glycol diglycidyl ether; and sorbitol polyglycidyl ether. A chloromethyl group-containing compound is a compound having a chloromethyl group. An example of a chloromethyl group-containing compound is chloromethyl polystyrene. A carboxyl group-containing compound is a compound having a carboxyl group. Examples of a carboxyl group-containing compound are (poly)acrylic acid, (poly)methacrylic acid, etc.
[0170] Specific examples of ketone group-containing compounds include (poly)diacetone acrylamide and diacetone alcohol. Specific examples of hydrazide compounds include hydrazine, carbohydrazide, and adipic acid hydrazide. Specific examples of melamine compounds include melamine resins and methyl etherified melamine resins.
[0171] [Amount of Curing Agent] The amount of curing agent may be 0.1 parts by weight or more, 1 part by weight or more, 3 parts by weight or more, 5 parts by weight or more, 10 parts by weight or more, 15 parts by weight or more, 20 parts by weight or more, 50 parts by weight or more, 75 parts by weight or more, or 100 parts by weight or more, relative to 100 parts by weight of the modified polyol. Alternatively, the amount may be 500 parts by weight or less, 300 parts by weight or less, 200 parts by weight or less, 100 parts by weight or less, 50 parts by weight or less, 40 parts by weight or less, 30 parts by weight or less, 20 parts by weight or less, 10 parts by weight or less, or 5 parts by weight or less.
[0172] [Other Components] The repellent may contain other components in addition to the above components. Examples of other components include polysaccharides, paper strength agents, flocculants, retention aids, coagulants, binder resins, anti-slip agents, sizing agents, paper strength agents, fillers, antistatic agents, preservatives, UV absorbers, antibacterial agents, deodorizers, fragrances, etc. These may be used alone or in combination of two or more. In addition to the above components, other components include other water and / or oil repellents, dispersants, texture adjusters, softeners, flame retardants, paint fixatives, wrinkle inhibitors, drying speed adjusters, crosslinking agents, film-forming aids, compatibilizers, antifreeze agents, viscosity adjusters, UV absorbers, antioxidants, pH adjusters, insect repellents, antifoaming agents, shrinkage inhibitors, anti-wrinkle agents after washing, shape retention agents, drape retention agents, ironing improvers, whitening agents, whitening agents, fabric softening clay, dye transfer inhibitors such as polyvinylpyrrolidone, polymer dispersants, stain release agents, scum dispersants, fluorescent whitening agents such as 4,4-bis(2-sulfostyryl)biphenyl disodium (Tinopal CBS-X manufactured by Ciba Specialty Chemicals), dye fixatives, and anti-fading agents such as 1,4-bis(3-aminopropyl)piperazine. The following may be blended: stain removers, enzymes such as cellulase, amylase, protease, lipase, keratinase, etc. as fiber surface modifiers; foam inhibitors; silk protein powder, surface-modified products thereof, or emulsified dispersions thereof (e.g., K-50, K-30, K-10, A-705, S-702, L-710, FP series (Idemitsu Petrochemical), hydrolyzed silk liquid (Jomo), Silkgen G Soluble S (Ichimaru Falcos)); stain inhibitors (e.g., nonionic polymer compounds composed of alkylene terephthalate and / or alkylene isophthalate units and polyoxyalkylene units (e.g., FR627 manufactured by GOO Chemical Industry Co., Ltd.), SRC-1 manufactured by Clariant Japan, etc.) that can impart silk texture and functionality such as moisture absorption and release. These may be used alone or in combination of two or more.
[0173] [Polysaccharides] Examples of polysaccharides include starch, xanthan gum, karaya gum, welan gum, guar gum, pectin, tamarind gum, carrageenan, chitosan, gum arabic, locust bean gum, cellulose, alginic acid, agar, dextran, cellulose, carboxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, chitin nanofiber, cellulose nanofiber, pullulan, etc. The polysaccharide may be a substituted modified polysaccharide (excluding the above-mentioned polyol-modified polysaccharides), and in particular, a modified polysaccharide into which a hydroxyl group or a cationic group has been introduced.
[0174] [Paper Strength Agents, Flocculants, Retention Aids, or Coagulants] Examples of paper strength agents, flocculants, retention aids, or coagulants include styrene polymers (styrene / maleic acid polymers, styrene / acrylic acid polymers), urea-formaldehyde polymers, polyethyleneimine, melamine-formaldehyde polymers, polyamidoamine-epichlorohydrin polymers, polyacrylamide polymers, polyamine polymers, polydiallyldimethylammonium chloride, alkylamine-epichlorohydrin condensates, condensates of alkylene dichlorides and polyalkylenepolyamines, dicyandiamide-formalin condensates, dimethyldiallylammonium chloride polymers, and olefin / maleic anhydride polymers.
[0175] Sizing Agents Examples of sizing agents include cellulose-reactive sizing agents, e.g., rosin-based sizing agents such as rosin-based soaps, rosin-based emulsions / dispersions, cellulose-reactive sizing agents, e.g., emulsions / dispersions of acid anhydrides such as alkyl and alkenyl succinic anhydrides (ASA), alkenyl and alkyl ketene dimers (AKD) and polymers, and anionic, cationic and amphoteric polymers of ethylenically unsaturated monomers, e.g., copolymers of styrene and acrylate.
[0176] [Antistatic Agent] Examples of antistatic agents include cationic antistatic agents having cationic functional groups such as quaternary ammonium salts, pyridinium salts, and primary, secondary, and tertiary amino groups; anionic antistatic agents having anionic functional groups such as sulfonates, sulfate ester salts, phosphonates, and phosphate ester salts; amphoteric antistatic agents such as alkylbetaine and its derivatives, imidazoline and its derivatives, alanine and its derivatives, and nonionic antistatic agents such as aminoalcohols and its derivatives, glycerin and its derivatives, and polyethylene glycol and its derivatives. Ion-conductive polymers obtained by polymerizing or copolymerizing monomers having these cationic, anionic, or amphoteric ionic conductive groups may also be used. These may be used alone or in combination of two or more.
[0177] [Preservatives] Preservatives can be used mainly to enhance antiseptic and bactericidal properties and maintain antiseptic properties during long-term storage. Examples of preservatives include isothiazolone organic sulfur compounds, benzisothiazolone organic sulfur compounds, benzoic acids, and 2-bromo-2-nitro-1,3-propanediol.
[0178] [Ultraviolet Absorber] An ultraviolet absorber is a chemical agent that has the effect of protecting against ultraviolet rays, and is a component that absorbs ultraviolet rays and converts them into infrared rays, visible light, etc. Examples of ultraviolet absorbers include aminobenzoic acid derivatives, salicylic acid derivatives, cinnamic acid derivatives, benzophenone derivatives, azole compounds, and 4-t-butyl-4'-methoxybenzoylmethane.
[0179] [Antibacterial Agent] An antibacterial agent is a component that has the effect of suppressing the growth of bacteria on fibers and further suppressing the generation of unpleasant odors resulting from microbial decomposition products. Examples of the antibacterial agent include cationic disinfectants such as quaternary ammonium salts, bis-(2-pyridylthio-1-oxide)zinc, polyhexamethylenebiguanidine hydrochloride, 8-oxyquinoline, and polylysine.
[0180] [Deodorant] Examples of deodorants include cluster dextrin, methyl-β-cyclodextrin, 2-hydroxypropyl-β-cyclodextrin, monoacetyl-β-cyclodextrin, acylamidopropyldimethylamine oxide, and aminocarboxylic acid metal complexes (e.g., zinc complex of trisodium methylglycine diacetate described in WO 2012 / 090580).
[0181] [Amount of Other Components] The amount of each or the total amount of the other components may be 0.1 parts by weight or more, 1 part by weight or more, 3 parts by weight or more, 5 parts by weight or more, 10 parts by weight or more, 15 parts by weight or more, 20 parts by weight or more, 50 parts by weight or more, 75 parts by weight or more, or 100 parts by weight or more, relative to 100 parts by weight of the polyol modified product, and may be 500 parts by weight or less, 300 parts by weight or less, 200 parts by weight or less, 100 parts by weight or less, 50 parts by weight or less, 40 parts by weight or less, 30 parts by weight or less, 20 parts by weight or less, 10 parts by weight or less, or 5 parts by weight or less.
[0182] <Method for Producing Treated Textile or Paper Products> The method for producing a repellent-treated product according to the present disclosure includes treating a substrate with the repellent described above.
[0183] The term "treatment" refers to applying the repellent to a substrate by immersion, spraying, coating, or the like. The treatment causes the polyol-modified compound, which is the active ingredient of the repellent, to adhere to the interior and / or surface of the substrate. Here, "adhesion" may be physical or chemical; for example, the polyol-modified compound may be physically or chemically modified (by reaction) with hydroxyl groups of the substrate (fiber, paper, glass, etc.).
[0184] [Substrate] The substrate to be treated with the repellent agent of the present disclosure is not limited, but is preferably a textile product or a paper product, particularly a paper product.
[0185] The repellent agent in the present disclosure imparts liquid repellency to a substrate (e.g., a fiber substrate or a paper substrate) and can function as at least one selected from the group consisting of a water repellent agent, an oil repellent agent, an oil-resistant agent, and a water-resistant agent. The substrate treated with the repellent agent in the present disclosure is, for example, greaseproof paper or water-resistant paper.
[0186] Examples of substrates for textile products include natural fibers of animal or plant origin such as cotton, hemp, wool, and silk, synthetic fibers such as polyamide, polyester, polyvinyl alcohol, polyacrylonitrile, polyvinyl chloride, and polypropylene, semi-synthetic fibers such as rayon and acetate, inorganic fibers such as glass fiber, carbon fiber, and asbestos fiber, or mixtures of these fibers. Textile products include woven fabrics, knitted fabrics, and nonwoven fabrics, as well as cloth in the form of clothing (for example, water-repellent clothing such as raincoats) and carpets, but the treatment may also be applied to fibers, yarns, and intermediate textile products (for example, slivers or rovings) in a state prior to being made into cloth.
[0187] Examples of substrates for paper products include paper made from bleached or unbleached chemical pulp such as kraft pulp or sulfite pulp, bleached or unbleached high-yield pulp such as groundwood pulp, mechanical pulp or thermomechanical pulp, recycled paper pulp such as recycled newspaper, recycled magazine paper, recycled corrugated cardboard or deinked recycled paper, paper containers, paper molded articles, etc. Specific examples of paper products include food packaging materials, food containers, gypsum board base paper, coated base paper, medium-quality paper, general liners and corrugating media, neutral white roll paper, neutral liner, rust-proof liner and metal interleaving paper, kraft paper, neutral printing and writing paper, neutral coated base paper, neutral PPC paper, neutral thermal paper, neutral pressure-sensitive base paper, neutral inkjet paper and neutral information paper, molded paper (molded containers), etc., and suitable examples include food packaging materials and food containers.
[0188] Substrates that can be treated with the repellent of the present disclosure are not limited to textiles or paper products, but also include stone, filters (e.g., electrostatic filters), dust masks, fuel cell components (e.g., gas diffusion electrodes and gas diffusion supports), glass, wood, leather, fur, asbestos, brick, cement, metals and oxides, ceramic products, plastics, painted surfaces, and plaster.
[0189] When the substrate is glass, the produced glass product may be an optical component. A layer (or film), such as a hard coat layer or an anti-reflection layer, may be formed on the surface (outermost layer) of the glass substrate. The anti-reflection layer may be either a single-layer anti-reflection layer or a multi-layer anti-reflection layer. Examples of inorganic substances that can be used for the anti-reflection layer include SiO 2 , SiO, ZrO 2 , TiO 2 , TiO, Ti 2 O 3 , Ti 2 O 5 , Al 2 O 3 , Ta 2 O 5 , CeO 2 , MgO, Y 2 O 3 , SnO 2 , MgF 2 , W.O. 3 These inorganic substances may be used alone or in combination of two or more (for example, as a mixture). When a multi-layer antireflection layer is formed, the outermost layer may contain SiO 2 and / or SiO is preferably used. When the article to be manufactured is an optical glass component for a touch panel, a transparent electrode, for example, a thin film using indium tin oxide (ITO) or indium zinc oxide, may be provided on a portion of the surface of the substrate (glass). Furthermore, the substrate may have an insulating layer, an adhesive layer, a protective layer, a decorative frame layer (I-CON), an atomization film layer, a hard coating film layer, a polarizing film, a phase difference film, a liquid crystal display module, or the like, depending on its specific specifications.
[0190] [Treatment Method] The repellent agent of the present disclosure can be applied to a substrate as a treatment agent (particularly a surface treatment agent) by a conventionally known method. The treatment method may involve dispersing and diluting the repellent agent of the present disclosure in an organic solvent or water, as needed, and applying it to the interior and / or surface of the substrate by a known method such as dip coating, spray coating, foam coating, or the like, followed by drying. After drying, a product is obtained with the solid components of the repellent adhered thereto. If necessary, the repellent agent may be applied together with an appropriate crosslinking agent and cured. If necessary, the repellent agent of the present disclosure may also be used in combination with various additives, such as water and / or oil repellents, antislip agents, antistatic agents, texture modifiers, softeners, antibacterial agents, flame retardants, paint fixatives, wrinkle inhibitors, drying speed modifiers, crosslinking agents, film-forming aids, compatibilizers, antifreeze agents, viscosity modifiers, UV absorbers, antioxidants, pH adjusters, insect repellents, and antifoaming agents. Examples of the various additives may be the same as those described above under "Other Components." The concentration of the repellent in the treatment agent to be brought into contact with the substrate may be varied as appropriate depending on the application, but may be 0.01 to 10% by weight, for example 0.05 to 5% by weight.
[0191] The repellent agent can be applied to the substrate by any of the known methods for treating a substrate with a liquid. The substrate may be immersed in the repellent agent, or a solution may be applied or sprayed onto the substrate. The treated substrate is preferably dried and cured by heating to develop liquid repellency. The heating temperature may be, for example, 100°C to 200°C, 100°C to 170°C, or 100°C to 120°C. In the present disclosure, good performance can be obtained even with low-temperature heating (e.g., 100°C to 140°C). In the present disclosure, the heating time may be 5 seconds to 60 minutes, for example, 30 seconds to 3 minutes. When the textile product is paper, the repellent agent may be coated on the paper, or the solution may be applied or sprayed onto the paper, or the repellent agent may be mixed with the pulp slurry before papermaking. The treatment may be an external or internal addition treatment. Alternatively, the repellent agent may be applied to the textile product by a cleaning method, such as a laundry application or a dry cleaning method.
[0192] [Treatment of Paper Products] Paper substrates include paper, paper containers, paper molded articles (e.g., pulp molds), etc. The modified polyols of the present disclosure can adhere well to paper substrates.
[0193] The paper can be produced by a conventional papermaking method, such as an internal treatment method in which the repellent is added to the pulp slurry before papermaking, or an external treatment method in which the repellent is applied to the paper after papermaking.
[0194] Size presses using external additive treatment methods can also be divided into the following categories based on the application method. One application method is the so-called pond-type two-roll size press, in which a coating liquid (size liquid) is supplied to the nip formed by passing paper between two rubber rolls, creating a pool of coating liquid called a pond, and the paper is passed through this pool of coating liquid to apply the size liquid to both sides of the paper. Other application methods include the gate roll type, in which the size liquid is applied using a surface transfer method, and the rod metering size press. In the pond-type two-roll size press, the size liquid easily penetrates into the paper, while in the surface transfer type, the size liquid components tend to remain on the paper surface. In the surface transfer type, the coating layer tends to remain on the paper surface compared to the pond-type two-roll size press, and a larger coating layer is formed on the surface than in the pond-type two-roll size press. In the present disclosure, performance can be imparted to paper even when the former pond-type two-roll size press is used. Papers treated in this way may exhibit excellent oil and water resistance etc., after simple drying at room temperature or at elevated temperatures, optionally followed by a heat treatment which may range in temperature up to 300°C, e.g. up to 200°C, especially 80°C to 180°C, depending on the properties of the paper.
[0195] The internal treatment method may refer to a treatment method in which a repellent is added to a pulp slurry before papermaking. The internal treatment method may include, but is not limited to, one or more of the following steps: adding a repellent to a pulp slurry and stirring and mixing it; suction-dewatering the pulp composition prepared in the above step through a mesh of a predetermined shape to deposit the pulp composition and form a pulp molded intermediate; and molding and drying the pulp molded intermediate in a heated mold to obtain paper, a paper container, or a molded paper product. The treated paper may be subjected to a heat treatment after simple drying at room temperature or at an elevated temperature, depending on the paper's properties. The heat treatment temperature may be 150°C or higher, 180°C or higher, or 210°C or higher, and may be 300°C or lower, 250°C or lower, or 200°C or lower, and particularly 80°C to 180°C. Heat treatment within this temperature range can exhibit excellent oil resistance, water resistance, etc.
[0196] The present disclosure can be used in gypsum board base paper, coated base paper, medium paper, general liners and mediums, neutral pure white roll paper, neutral liners, anti-rust liners and metal interleaving paper, kraft paper, etc. It can also be used in neutral printing and writing paper, neutral coated base paper, neutral PPC paper, neutral thermal paper, neutral pressure-sensitive base paper, neutral inkjet paper, and neutral information paper.
[0197] Pulp raw materials that can be used include bleached or unbleached chemical pulps such as kraft pulp or sulfite pulp, bleached or unbleached high-yield pulps such as groundwood pulp, mechanical pulp or thermomechanical pulp, and recycled paper pulp such as recycled newspapers, recycled magazines, recycled corrugated cardboard, and deinked recycled paper. Mixtures of the above pulp raw materials with synthetic fibers such as asbestos, polyamide, polyimide, polyester, polyolefin, and polyvinyl alcohol can also be used.
[0198] A sizing agent can be added to improve the water resistance of paper. Examples of sizing agents include cationic sizing agents, anionic sizing agents, and rosin-based sizing agents (e.g., acidic rosin-based sizing agents and neutral rosin-based sizing agents). The amount of sizing agent may be 0.01 to 5% by weight of the pulp.
[0199] If necessary, the paper can contain additives used in paper production, such as paper strength agents such as starch, modified starch, carboxymethyl cellulose, and polyamide polyamine-epichlorohydrin resin, flocculants, fixing agents, retention aids, dyes, fluorescent dyes, slime control agents, and antifoaming agents, to the extent that they are commonly used. Starch and modified starch are preferably used. If necessary, repellents can be applied to the paper using starch, polyvinyl alcohol, dyes, coating colors, anti-slip agents, etc., using a size press, gate roll coater, bill blade coater, calendar, etc.
[0200] In the case of external addition, the amount of the polyol modified substance contained in the coating layer is 0.01 to 2.0 g / m 2 , particularly 0.1 to 1.0 g / m 2 The coating layer is preferably formed from a repellent and starch and / or modified starch. The solid content of the paper repellent in the coating layer is preferably 2 g / m. 2 In the internal addition, the repellent is preferably mixed with the pulp so that the amount of the repellent is 0.01 to 50 parts by weight or 0.01 to 30 parts by weight, for example 0.01 to 10 parts by weight, particularly 0.2 to 5.0 parts by weight, per 100 parts by weight of the pulp forming the paper.
[0201] In the external addition, oil resistance can also be imparted to paper by using a so-called pond-type two-roll size press treatment, in which a treatment solution is accumulated between rolls and the base paper is passed through the treatment solution between the rolls at any roll speed and nip pressure.
[0202] In the external additive treatment, the paper substrate may contain additives such as sizing agents, strength agents, flocculants, retention agents, or coagulants. The additives may be nonionic, cationic, anionic, or amphoteric. The ionic charge density of the additives may be -10,000 to 10,000 μeq / g, preferably -4,000 to 8,000 μeq / g, and more preferably -1,000 to 7,000 μeq / g. Additives such as sizing agents, strength agents, flocculants, retention agents, or coagulants (solids or active ingredients) are generally used in amounts of 0.1 to 10% by weight (e.g., 0.2 to 5.0% by weight) based on the pulp. In the case of paper substrates containing cationic additives (e.g., sizing agents, strength agents, flocculants, retention agents, or coagulants), the repellent is preferably anionic.
[0203] In the internal addition treatment, it is preferable to make paper from a pulp slurry having a pulp concentration of 0.5 to 5.0% by weight (e.g., 2.5 to 4.0% by weight).Additives (e.g., sizing agents, paper strength agents, flocculants, retention agents, coagulants, etc.) and polyol modifiers can be added to the pulp slurry. Examples of additives (for example, sizing agents, paper strength agents, flocculants, retention agents, or coagulants) include alkylketene dimers, alkenyl succinic anhydrides, styrene polymers (styrene / maleic acid polymers, styrene / acrylic acid polymers), urea-formaldehyde polymers, polyethyleneimine, melamine-formaldehyde polymers, polyamidoamine-epichlorohydrin polymers, polyacrylamide polymers, polyamine polymers, polydiallyldimethylammonium chloride, alkylamine-epichlorohydrin condensates, condensates of alkylene dichlorides and polyalkylenepolyamines, dicyandiamide-formalin condensates, dimethyldiallylammonium chloride polymers, and olefin / maleic anhydride polymers.
[0204] [Pretreatment of Textile Products] The textile product may be pretreated before being treated with the repellent of the present disclosure. Pretreatment of the textile product can impart excellent durability to the textile product after treatment with the repellent.
[0205] Examples of pretreatments for textile products include cationization treatment by reaction with a reactive quaternary ammonium salt, anionization treatment such as sulfonation, carboxylation, and phosphate, acetylation treatment after anionization treatment, benzoylation treatment, carboxymethylation treatment, grafting treatment, tannic acid treatment, and polymer coating treatment.
[0206] The method for pretreating a textile product is not limited, and the textile product can be pretreated by a conventionally known method. The pretreatment liquid may be dispersed and diluted in an organic solvent or water as necessary, and applied to the interior and / or surface of the textile product by a known method such as dip coating, spray coating, foam coating, etc., followed by drying. The pH and temperature of the pretreatment liquid may be adjusted depending on the desired degree of treatment. As an example of a method for pretreating a textile product, a method for pretreating a textile product with the above-mentioned treatment agent will be described in detail.
[0207] The pretreatment method for textile products is to add -SO 3 M 1 (In the formula, M 1 represents a monovalent cation), 2 (In the formula, M 2 represents a monovalent cation), and —O—P(O)(OX 1 ) (OX 2 ) (wherein, X 1 and X 2 and each independently represent a hydrogen atom or an alkyl group having 1 to 22 carbon atoms) (hereinafter, also referred to as "specific functional groups").
[0208] M 1 Examples of M include H, K, Na, and ammonium ions which may have a substituent. 2 Examples of X include H, K, Na, and ammonium ions which may have a substituent. 1 or X 2 When is an alkyl group, it is preferably an alkyl group having 1 to 22 carbon atoms, and more preferably an alkyl group having 4 to 12 carbon atoms.
[0209] Fibers containing the specific functional groups (hereinafter sometimes referred to as "functional group-containing fibers") can be prepared, for example, by the following methods: (i) A compound having the specific functional groups is attached to a fiber material. The attachment of the compound may be in a state where a portion of the compound is chemically bonded to a portion of the fiber, to the extent that a sufficient amount of the specific functional groups remains. (ii) Fibers are prepared in which the specific functional groups are directly introduced into the material that constitutes the fiber.
[0210] In the case of (i), for example, functional group-containing fibers can be obtained by a functional group introduction step in which a fiber material is treated with a pretreatment liquid containing one or more compounds having the above-mentioned specific functional groups.
[0211] The material of the fiber material is not particularly limited, and examples thereof include natural fibers such as cotton, linen, silk, and wool, semi-synthetic fibers such as rayon and acetate, synthetic fibers such as polyamide (nylon, etc.), polyester, polyurethane, and polypropylene, and composite fibers and blended fibers thereof. The form of the fiber material may be any form such as fiber (tow, sliver, etc.), yarn, knitted fabric (including interwoven fabric), woven fabric (including interwoven fabric), nonwoven fabric, etc.
[0212] In this embodiment, from the viewpoint of improving the water repellency of the resulting textile product, it is preferable to use a textile material containing polyamide and polyester as raw materials, and it is particularly preferable to use nylons such as nylon 6 and nylon 6,6, polyesters such as polyethylene terephthalate (PET), polytrimethyl terephthalate and polylactic acid, and mixed fibers containing these.
[0213] Above -SO 3 M 1 A phenolic polymer can be used as the compound having the formula:
[0033] Such a phenolic polymer can be, for example, one containing at least one compound represented by the following general formula:
[0214] [In the formula, X 2 Ha-SO 3 M 3 (In the formula, M 3represents a monovalent cation) or a group represented by the following general formula, and n is an integer of 20 to 3000.
[0215] [In the formula, M 4 represents a monovalent cation.
[0216] The above M 3 Examples of the cation include H, K, Na, and an ammonium ion which may have a substituent.
[0217] The above M 4 Examples of the cation include H, K, Na, and an ammonium ion which may have a substituent.
[0218] The compound represented by the above general formula may be, for example, a formalin condensate of phenolsulfonic acid or a formalin condensate of sulfonated bisphenol S.
[0219] Above - COOM 2 Examples of compounds having the formula include polycarboxylic acid polymers.
[0220] As the polycarboxylic acid polymer, for example, a polymer synthesized by a conventionally known radical polymerization method using acrylic acid, methacrylic acid, maleic acid, or the like as a monomer, or a commercially available product can be used.
[0221] Examples of methods for producing polycarboxylic acid polymers include adding a radical polymerization initiator to an aqueous solution of the above-mentioned monomer and / or its salt and heating the mixture at 30 to 150°C for 2 to 5 hours. At this time, an alcohol such as methanol, ethanol, or isopropyl alcohol, or an aqueous solvent such as acetone, may be added to the aqueous solution of the above-mentioned monomer and / or its salt. Examples of radical polymerization initiators include persulfates such as potassium persulfate, sodium persulfate, and ammonium persulfate; redox-based polymerization initiators such as combinations of persulfates and sodium bisulfite; hydrogen peroxide; and water-soluble azo-based polymerization initiators. These radical polymerization initiators may be used alone or in combination. Furthermore, during radical polymerization, a chain transfer agent (e.g., octyl thioglycolate) may be added to adjust the degree of polymerization.
[0222] In addition to the above-mentioned monomers, copolymerizable monomers can be used for radical polymerization. Examples of copolymerizable monomers include vinyl monomers such as ethylene, vinyl chloride, and vinyl acetate, acrylamide, acrylates, and methacrylates. Preferred acrylates and methacrylates have a hydrocarbon group having 1 to 3 carbon atoms which may have a substituent such as a hydroxyl group. Examples of such acrylates or methacrylates include methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, propyl acrylate, and propyl methacrylate. These copolymerizable monomers may be used alone or in combination of two or more.
[0223] The carboxyl group in the polycarboxylic acid polymer may be free or may be neutralized with an alkali metal, an amine compound, etc. Examples of the alkali metal include sodium, potassium, and lithium, and examples of the amine compound include ammonia, monoethanolamine, diethanolamine, and triethanolamine.
[0224] The weight average molecular weight of the polycarboxylic acid polymer is preferably from 1,000 to 20,000, more preferably from 3,000 to 15,000, from the viewpoint of improving the water repellency of the resulting textile product.
[0225] As the polycarboxylic acid polymer, commercially available products such as "Neocrystal 770" (trade name, manufactured by Nicca Chemical Co., Ltd.) and "Ceropol PC-300" (trade name, manufactured by Sanyo Chemical Industries, Ltd.) can be used.
[0226] The above -O-P(O)(OX 1 ) (OX 2 ) may be exemplified by phosphate ester compounds represented by the following general formula: [In the formula, X 1 or X 2 is as defined above, and X 3 represents an alkyl group having 1 to 22 carbon atoms.
[0227] As the phosphate ester compound, phosphate monoesters, diesters and triesters, in which the alkyl ester moiety is an alkyl group having 1 to 22 carbon atoms, and mixtures thereof can be used.
[0228] From the viewpoint of improving the water repellency of the resulting textile product, it is preferable to use lauryl phosphate and decyl phosphate.
[0229] As the phosphate ester compound, for example, commercially available products such as "Phosphanol ML-200" (trade name, manufactured by Toho Chemical Industry Co., Ltd.) can be used.
[0230] The pretreatment liquid containing one or more compounds having the specific functional group may be, for example, an aqueous solution of the compounds described above. The pretreatment liquid may also contain an acid, an alkali, a surfactant, a chelating agent, etc.
[0231] Methods for treating textile materials with the pretreatment liquid include, for example, padding, immersion, spraying, and coating. Examples of padding include methods using padding devices described on pages 396-397 of "Textile Dyeing and Processing Dictionary" (published by Nikkan Kogyo Shimbun, 1963) and pages 256-260 of "Color Dyeing Chemistry III" (published by Jikkyo Publishing Co., Ltd., 1975). Examples of coating include methods using coating machines described on pages 473-477 of "Dyeing and Finishing Equipment Directory" (published by Sen-sha, 1981). Examples of immersion include methods using batch dyeing machines described on pages 196-247 of "Dyeing and Finishing Equipment Directory" (published by Sen-sha, 1981). These machines include jet dyeing machines, air jet dyeing machines, drum dyeing machines, winch dyeing machines, washer dyeing machines, and cheese dyeing machines. Examples of spray treatment include air spraying, in which the treatment liquid is atomized using compressed air, and methods using a hydraulic atomization air spray. The treatment conditions, such as the concentration of the treatment liquid and the heat treatment after application, can be adjusted appropriately, taking into account various conditions, such as the purpose and performance. Furthermore, when the pretreatment liquid contains water, it is preferable to dry the pretreatment liquid after application to remove the water. The drying method is not particularly limited, and may be either a dry heat method or a wet heat method. The drying temperature is also not particularly limited, and may be, for example, drying at room temperature to 200°C for 10 seconds to several days. If necessary, heat treatment at a temperature of 100 to 180°C for 10 seconds to 5 minutes may be performed after drying.
[0232] When the textile material is to be dyed, the treatment with the pretreatment liquid may be carried out before dyeing or in the same bath as the dyeing. However, when reduction soaping is carried out, there is a risk that the compound having the specific functional group (e.g., a phenolic polymer compound) adsorbed during the treatment may fall off, so it is preferable to carry out the treatment after reduction soaping after dyeing.
[0233] The treatment temperature in the immersion treatment can be 60 to 130° C. The treatment time can be 5 to 60 minutes.
[0234] In the functional group introduction step using a pretreatment liquid, the amount of the compound having the specific functional group attached is preferably 1.0 to 7.0 parts by weight per 100 parts by weight of the textile material. Within this range, durable water repellency and texture can both be achieved at high levels.
[0235] The pH of the pretreatment liquid is preferably adjusted to 3 to 5. The pH can be adjusted using a pH adjuster such as acetic acid or malic acid.
[0236] The pretreatment solution may contain a salt to effectively adsorb the compound having the specific functional group onto the fiber material through a salting-out effect. Examples of salts that can be used include sodium chloride, sodium carbonate, ammonium sulfate, and sodium sulfate.
[0237] In the functional group introduction step using a pretreatment liquid, it is preferable to remove the compound having the specific functional group that has been treated in excess. An example of a removal method is washing with water. By performing sufficient removal, it is possible to prevent the development of water repellency in the subsequent water-repellent treatment from being hindered, and in addition, the feel of the resulting textile product is improved. Furthermore, it is preferable to thoroughly dry the resulting functional group-containing fiber before contacting it with the above-mentioned treatment agent.
[0238] (ii) An example of a fiber in which the specific functional group is directly introduced into the material that constitutes the fiber is cationic dyeable polyester (CD-PET).
[0239] From the viewpoint of improving the water repellency of the resulting textile product, the functional group-containing fiber preferably has a surface zeta potential of −100 to −0.1 mV, more preferably −50 to −1 mV. The zeta potential of the fiber surface can be measured, for example, using a zeta potential / particle size measurement system ELSZ-1000ZS (manufactured by Otsuka Electronics Co., Ltd.).
[0240] Although the embodiments have been described above, it will be understood that various changes in form and details can be made without departing from the spirit and scope of the claims.
[0241] The present disclosure will be described in detail below with reference to examples, but the present disclosure is not limited to these examples.
[0242] <Test Method> The test procedure is as follows.
[0243] [Volume ratio of particles of 100 μm or more] The volume ratio of particles of 100 μm or more was calculated from the frequency distribution obtained by measuring the water-dispersible repellent with a laser diffraction / scattering device, by dividing the volume ratio of particles of 100 μm or more by the volume ratio of all particles. Specifically, the calculation was performed using the following formula:
[0244] Volumetric abundance ratio of particles 100 μm or larger = [abundance of particles 100 μm or larger / abundance of all particles] * 100
[0245] [Median diameter D50] The median diameter D50 was determined by measuring the water-dispersible repellent agent using a laser diffraction / scattering device.
[0246] [Differential Scanning Calorimetry of Polyol-Modified Products] The maximum endothermic peak temperature, melting point, crystallization temperature, and glass transition temperature of the polyol-modified products were calculated by differential scanning calorimetry (DSC). DSC measurements were performed under a nitrogen atmosphere, with the product cooled to -20°C, followed by measuring the endothermic peak observed during the subsequent heating process to 180°C at a rate of 10°C / min. When multiple melting peaks appeared, the peak with the largest endothermic heat was taken as the maximum endothermic peak, and the top of this peak was taken as the maximum endothermic peak temperature. The endothermic heat was calculated by calculating the heat within a range of ±10°C from the endothermic peak temperature.
[0247] [Differential Scanning Calorimetry of the Solid Component Obtained by Removing the Liquid Medium from the Repellent] The maximum endothermic peak temperature, melting point, crystallization temperature, and glass transition temperature of the solid component obtained by removing the liquid medium from the repellent were calculated by differential scanning calorimetry (DSC). The liquid medium was removed from the repellent by drying the repellent at 150°C for 1 hour. DSC measurements were performed under a nitrogen atmosphere, cooling to -20°C, and then measuring the endothermic peaks observed during the subsequent temperature increase to 180°C at a rate of 10°C / min. When multiple endothermic peaks appeared, the endothermic peak with the highest temperature was designated as the maximum endothermic peak, and the top of this peak was designated as the maximum endothermic peak temperature. The endothermic heat was calculated by calculating the heat quantity within a range of ±10°C from the endothermic peak temperature.
[0248] [Variable temperature X-ray diffraction measurement of solid component obtained by removing liquid medium from repellent agent] The crystalline state of the solid component obtained by removing the liquid medium from the repellent agent was measured by X-ray diffraction (XRD) using RIGAKU's SmartLab. Cu Kα radiation was used as the light source. Variable temperature XRD (XRD-DSC) measurement was performed in a nitrogen atmosphere by cooling to -20°C, then raising the temperature to 25°C or 55°C at a rate of 5°C / min, and holding for 5 minutes before measurement. The half-width of the peak was defined as the 2θ width between the baseline and the peak at half the intensity of the peak top. The diffraction intensity ratio [A 55℃ / A 25℃ The intensity of the maximum point of the diffraction intensity in the region of 2θ from 15° to 30° at a measurement temperature of 25°C was calculated as [peak intensity A 25℃ The intensity of the maximum point of the diffraction intensity in the region of 2θ from 15° to 30° at a measurement temperature of 55°C was defined as [Peak Intensity A 55℃ ] was calculated as follows: 55℃ ] to [Peak Intensity A 25℃ ] to obtain the diffraction intensity ratio [A 55℃ / A 25℃ The diffraction intensity ratio [A 55℃ / A 25℃ ] = [Peak intensity A 55℃ ] / [Peak intensity A 25℃ The liquid medium was removed from the repellent agent by drying at 150° C. for 1 hour.
[0249] [HD Contact Angle] A solution (or dispersion) of the polyol-modified compound with a solids concentration of 1.0% was spin-coated onto a silicon wafer at 2500 rpm for 25 seconds to obtain a spin-coated film. This was then heated at 140°C for 1 minute to produce a silicon wafer treated with the polyol-modified compound. Chloroform was used as the solvent or dispersion medium. 2 μL of HD (hexadecane) was dropped onto the polyol-modified silicon wafer, and the contact angle measured 1 second after the drop landed was taken as the HD contact angle of the polyol-modified compound.
[0250] [Water Contact Angle] A solution (or dispersion) of the polyol-modified compound with a solids concentration of 1.0% was spin-coated onto a silicon wafer at 2500 rpm for 25 seconds to obtain a spin-coated film. This was then heated at 140°C for 1 minute to produce a silicon wafer treated with the polyol-modified compound. Chloroform was used as the solvent or dispersion medium. 2 μL of water was dropped onto the polyol-modified silicon wafer, and the contact angle measured 1 second after the drop landed was taken as the water contact angle of the polyol-modified compound.
[0251] [Preparation of Pulp Mold] Pulp mold was molded using an automatic molding machine. A mesh-like body was placed on a metal pulp mold mold with multiple suction holes at the bottom, and a metal tank was placed on top. A mixture of pulp slurry and water-dispersible repellent was placed in the upper metal tank. A vacuum pump was used to suck and dehydrate the pulp-containing aqueous composition through the pulp mold mold and mesh-like body from the side opposite the side where the mesh-like body was placed in the pulp mold mold, and the solids (pulp, etc.) contained in the pulp-containing aqueous composition were deposited on the mesh-like body to obtain a pulp mold intermediate. Next, the obtained pulp mold intermediate was dried from above and below in a metal male-female mold heated to 60 to 250°C under a pressure of 0.05 to 5 MPa. This produced a pulp molded product molded into the shape of a container.
[0252] [65°C oil resistance test] 100 ml of corn oil at 65°C was poured into a pulp mold, and after leaving it at room temperature for 45 minutes, the corn oil was removed from the pulp mold and the degree of staining of the pulp mold was evaluated. The following evaluation values were set depending on the degree of staining: 5: No staining on the inside 4: Stained on the inside. No staining on the back side 3: Stained on the inside. Slight staining on the back side 2: Stained on the inside. Staining on the back side was less than 50% of the area 1: Stained on the inside. Staining on the back side was 50% or more but less than 100% of the area 0: Stained on the entire back side
[0253] [Oil resistance test at room temperature] 100 ml of corn oil at 25°C was poured into a pulp mold, and after leaving it at room temperature for 45 minutes, the corn oil was removed from the pulp mold and the degree of staining of the pulp mold was evaluated. The following evaluation values were set depending on the degree of staining: 5: No staining on the inside 4: Stained on the inside. No staining on the back side 3: Stained on the inside. Slight staining on the back side 2: Stained on the inside. Staining on the back side was less than 50% of the area 1: Stained on the inside. Staining on the back side was 50% or more but less than 100% of the area 0: Stained on the entire back side
[0254] [65°C Water Resistance Test] 100 ml of water at 65°C was poured into a pulp mold, and after leaving it at room temperature for 45 minutes, the water was removed from the pulp mold and the degree of staining of the pulp mold was evaluated. The following evaluation values were set depending on the degree of staining: 5: No staining on the inside 4: Stained on the inside. No staining on the backside 3: Stained on the inside. Slight staining on the backside 2: Stained on the inside. Staining on the backside was less than 50% of the area 1: Stained on the inside. Staining on the backside was 50% or more but less than 100% of the area 0: Stained on the entire backside
[0255] [Water resistance test at room temperature] 100 ml of water at 25°C was poured into the pulp mold, and after leaving it at room temperature for 45 minutes, the water was removed from the pulp mold and the degree of staining of the pulp mold was evaluated. The following evaluation values were set depending on the degree of staining: 5: No staining on the inside 4: Stained on the inside. No staining on the backside 3: Stained on the inside. Slight staining on the backside 2: Stained on the inside. Staining on the backside was less than 50% of the area 1: Stained on the inside. Staining on the backside was 50% or more but less than 100% of the area 0: Stained on the entire backside
[0256] [Preparation of Treated Paper] A pulp slurry was prepared using wood pulp in a weight ratio of 60% by weight of LBKP (hardwood bleached kraft pulp) and 40% by weight of NBKP (softwood bleached kraft pulp) and the pulp had a freeness of 400 ml (Canadian Standard Freeness). A wet strength agent and a sizing agent were added to the pulp slurry, and the treated paper was processed on a Fourdrinier paper machine to a paper density of 0.58 g / cm.3 Basis weight 45 g / m 2 The paper was used as the base paper for external treatment (size press treatment). The oil resistance (KIT value) of this base paper was 0, and the water resistance (Cobb value) was 52 g / m 2 A treatment solution prepared by dissolving the compound in chloroform at a ratio of 14.9 mg / mL was applied to this base paper using a Baker applicator with a gap set to 0 mil, followed by drying. This procedure was repeated three times, and the paper was then dried at 140°C for one minute to produce treated paper.
[0257] [KIT test (oil resistance)] Measurements were made using the 3M kit test (TAPPI T-559cm-02). The 3M kit test method involves placing a test oil containing a blend of castor oil, toluene, and heptane on the surface of treated paper, wiping the test oil off after 15 seconds, and evaluating the oil resistance based on whether or not the treated paper stains with oil. Tests were conducted using test oils numbered 1 to 6, and the highest kit number that produced no stains was used to evaluate the oil resistance.
[0258] Corn oil resistance test (oil resistance) Corn oil was placed on the surface of treated paper, and after 15 seconds, the test oil was wiped off. The test paper was evaluated based on whether or not there was oil staining. If there was no staining, it was marked as ◯, and if there was staining, it was marked as ×.
[0259] [HD Contact Angle Measurement Results and Differential Scanning Calorimetry of Polyol-Modified Products] Table 1 shows the results of HD contact angle measurement and differential scanning calorimetry (DSC) of the following modified polyols: decaglycerol dodecabehenyl ester (degree of polymerization 10, hydroxy group substitution rate: 12 / 12*100, biobased ratio: 100%), decaglycerol heptabehenyl ester (degree of polymerization 10, hydroxy group substitution rate: 7 / 12*100), decaglycerol decastearyl ester (degree of polymerization 10, hydroxy group substitution rate: 10 / 12*100), hexaglycerol pentastearyl ester (degree of polymerization 6, hydroxy group substitution rate: 5 / 8*100), and tetraglycerol tristearyl ester (degree of polymerization 4, hydroxy group substitution rate: 3 / 6*100).
[0260] Precursor A of a water-dispersible repellent was obtained by mixing 2 g of decaglycerol dodecabehenyl ester (degree of polymerization: 10, hydroxy group substitution rate: 12 / 12*100, biobased ratio: 100%) as a modified polyol, 0.2 g of polyethylene oxide alkyl ether (alkyl carbon number: 6 to 16, HLB: 7), and 17.8 g of water. Precursor A of the water-dispersible repellent was heated to 80°C and then allowed to cool while stirring with a magnetic stirrer, thereby obtaining precursor B of the water-dispersible repellent. Precursor B of the water-dispersible repellent was treated twice in a high-pressure wet microparticulation device at 100 MPa to obtain a water-dispersible repellent. The volume fraction of particles 100 μm or larger in the obtained water-dispersible repellent was 0%, and the median diameter D50 was 6.1 μm. The solid component obtained by removing the liquid medium from the water-dispersible repellent was subjected to differential scanning calorimetry and variable-temperature X-ray diffraction analysis, and the results are shown in Table 1. A pulp composition was prepared by adding the aqueous dispersion composition to a pulp slurry having a concentration of 0.5 wt % so that the ratio of the aqueous dispersion composition to the pulp was 3.5 wt % in terms of solid content. The pulp composition was placed in an automatic molding machine to produce a pulp mold. The pulp mold was subjected to an oil resistance test at 65°C and a water resistance test at 65°C, and the oil resistance was rated 4 points and the water resistance was rated 4 points. The results are shown in Table 1. Room temperature oil resistance and room temperature water resistance tests were also conducted, and the results are shown in Table 1.
[0261] Precursor A of a water-dispersible repellent was obtained by mixing 2 g of decaglycerol dodecabehenyl ester (degree of polymerization: 10, hydroxy group substitution rate: 12 / 12*100, biobased ratio: 100%) as a modified polyol, 0.2 g of polyethylene oxide trimethylnonyl ether (HLB: 13), and 17.8 g of water. This water-dispersible repellent precursor A was heated to 80°C and then stirred at 7000 rpm for 20 minutes using a homogenizer to obtain a water-dispersible repellent. The volume fraction and median diameter D50 of particles of 100 μm or larger in the obtained water-dispersible repellent, as well as differential scanning calorimetry and variable temperature X-ray diffraction analysis of the solid component obtained by removing the liquid medium from the water-dispersible repellent, were measured. The results are shown in Table 1. As in Example 1, the oil resistance test and water resistance test were conducted at 65°C, resulting in an oil resistance of 4 and a water resistance of 4. The results are shown in Table 1. In addition, oil resistance and water resistance tests at room temperature were also carried out, and the results are shown in Table 1.
[0262] Precursor A of a water-dispersible repellent was prepared by mixing 2 g of decaglycerol heptabehenyl ester (degree of polymerization: 10, hydroxy group substitution rate: 7 / 12*100, biobased ratio: 100%) as a modified polyol, 0.2 g of polyethylene oxide trimethylnonyl ether, and 17.8 g of water. This water-dispersible repellent precursor A was heated to 80°C and then stirred at 7000 rpm for 20 minutes using a homogenizer to obtain a water-dispersible repellent. The volume fraction and median diameter D50 of particles 100 μm or larger in the obtained water-dispersible repellent, as well as differential scanning calorimetry and variable-temperature X-ray diffraction measurements of the solid component obtained by removing the liquid medium from the water-dispersible repellent, were measured. The results are shown in Table 1. The water-dispersible composition was added to a 0.5 wt% pulp slurry to obtain a pulp composition at a ratio of 5 wt% of the pulp in terms of solids content. The pulp composition was placed in an automatic molding machine to prepare a pulp mold. The pulp mold was subjected to an oil resistance test at 65°C and a water resistance test at 65°C, and the oil resistance was 4 points and the water resistance was 4 points. In addition, room temperature oil resistance and room temperature water resistance tests were also conducted, and the results are shown in Table 1.
[0263] A water-dispersible repellent was obtained in the same manner as in Example 2, except that polyethylene oxide alkyl ether was changed to benzalkonium chloride. The volume abundance ratio of particles of 100 μm or more and the median diameter D50 of the obtained water-dispersible repellent were 1% and 7.7 μm, respectively. When subjected to an oil resistance test at 65°C and a water resistance test at 65°C as in Example 1, the oil resistance was 4 points and the water resistance was 4 points.
[0264] A water-dispersible repellent was obtained in the same manner as in Example 1. A pulp slurry was prepared using wood pulp in a weight ratio of 60% by weight of LBKP (broadleaf bleached kraft pulp) and 40% by weight of NBKP (softleaf bleached kraft pulp) and the pulp had a freeness of 400 ml (Canadian Standard Freeness). A wet strength agent and a sizing agent were added to the pulp slurry, and the slurry was spun on a Fourdrinier paper machine to a paper density of 0.58 g / cm. 3 Basis weight 45 g / m 2 The paper was used as the base paper for external treatment (size press treatment). The oil resistance (KIT value) of this base paper was 0, and the water resistance (Cobb value) was 52 g / m 2 A treatment solution prepared by dissolving the compound in chloroform at a ratio of 14.9 mg / mL was applied to this base paper using a Baker applicator with a gap set to 7 mil, followed by drying. This process was repeated three times, and the paper was then dried at 140°C for 5 minutes to produce treated paper. The corn oil resistance of the treated paper was rated "Good" and the KIT score was 4 points.
[0265] A water-dispersed repellent was obtained in the same manner as in Example 1. 2.5 g of cationic starch was mixed with 47.5 g of water and stirred at 60°C for 1 hour to prepare a cationic starch aqueous solution. The water-dispersed repellent was added to a pulp slurry with a concentration of 0.5 wt% so that the ratio of the cationic starch to the pulp was 3.5 wt% in terms of solid content, and then a cationic starch aqueous solution was added so that the ratio of the cationic starch to the pulp was 10 wt% in terms of solid content, to prepare a pulp composition. The pulp composition was placed in an automatic molding machine to produce a pulp mold. The pulp mold was subjected to a room temperature oil resistance test and scored 4 points. Comparative Example 1
[0266] 2 g of decaglycerol decastearyl ester (degree of polymerization: 10, hydroxy group substitution rate: 10 / 12*100) as a modified polyol, 0.2 g of polyethylene oxide trimethylnonyl ether, and 17.8 g of water were mixed to obtain a water-dispersible repellent precursor A. This water-dispersible repellent precursor A was heated to 80°C and then stirred at 7000 rpm for 20 minutes using a homogenizer to obtain a water-dispersible repellent. The volume fraction and median diameter D50 of particles of 100 μm or larger in the obtained water-dispersible repellent, as well as differential scanning calorimetry and variable temperature X-ray diffraction measurements of the solid component obtained by removing the liquid medium from the water-dispersible repellent, are shown in Table 1. As in Example 3, when subjected to an oil resistance test at 65°C and a water resistance test at 65°C, the oil resistance and water resistance were scored as 0 points. Comparative Example 2
[0267] A water-dispersible repellent was obtained in the same manner as in Comparative Example 1, except that the polyol modifier was changed to hexaglycerol pentastearyl ester (degree of polymerization 6, hydroxy group substitution rate: 5 / 8*100). The volumetric abundance ratio and median diameter D50 of particles of 100 μm or more of the obtained water-dispersible repellent, as well as the results of differential scanning calorimetry and variable temperature X-ray diffraction measurement of the solid component obtained by removing the liquid medium from the water-dispersible repellent, are shown in Table 1. When subjected to an oil resistance test at 65°C and a water resistance test at 65°C as in Example 3, the oil resistance and water resistance were scored as 0 points. Comparative Example 3
[0268] A water-dispersible repellent was obtained in the same manner as in Comparative Example 1, except that the polyol modifier was changed to tetraglycerol tristearyl ester (degree of polymerization 4, hydroxy group substitution rate: 3 / 6*100). The volume abundance ratio and median diameter D50 of particles of 100 μm or more of the obtained water-dispersible repellent, as well as the results of differential scanning calorimetry and variable temperature X-ray diffraction measurement of the solid component obtained by removing the liquid medium from the water-dispersible repellent, are shown in Table 1. When subjected to an oil resistance test at 65°C and a water resistance test at 65°C as in Example 3, the oil resistance and water resistance were scored as 0 points. Comparative Example 4
[0269] A water-dispersible repellent was obtained in the same manner as in Comparative Example 1, except that the solvent was changed to glycerin tristearyl ester (degree of polymerization 1, hydroxy group substitution rate: 3 / 3*100). The volumetric abundance ratio and median diameter D50 of particles of 100 μm or more of the obtained water-dispersible repellent, as well as the results of differential scanning calorimetry and variable temperature X-ray diffraction measurement of the solid component obtained by removing the liquid medium from the water-dispersible repellent, are shown in Table 1. When subjected to an oil resistance test at 65°C and a water resistance test at 65°C as in Example 3, the oil resistance and water resistance were scored as 0 points.
[0270]
Claims
1. A water-dispersible repellent comprising a modified polyol and a dispersant, which satisfies one or more of (1) and (2): (1) In differential scanning calorimetry of the modified polyol, or in differential scanning calorimetry of a solid component obtained by removing the liquid medium from the repellent, the temperature of the maximum endothermic peak in the temperature range of 25°C to 180°C is 55°C or higher; (2) The modified polyol has four or more monovalent hydrocarbon groups having 20 to 40 carbon atoms, which may have a substituent.
2. The repellent according to claim 1, wherein the polyol modified product has a maximum endothermic peak temperature of 55°C or higher in the temperature range of 25°C to 180°C in differential scanning calorimetry.
3. The repellent according to claim 1 or 2, wherein in differential scanning calorimetry of the solid component obtained by removing the liquid medium from the repellent, the temperature of the maximum endothermic peak in the temperature range of 25°C to 180°C is 55°C or higher.
4. The peak intensity A of the maximum peak at a measurement temperature of 25° C. in the 2θ range of 15° to 30° measured by variable temperature X-ray diffraction method of the solid component obtained by removing the liquid medium from the repellent agent 25℃ and the peak intensity A of the maximum peak at the measurement temperature of 55 °C 55℃ Diffraction intensity ratio [A 55℃ / A 25℃ 4. The repellent according to claim 1, wherein the value of is 0.5 or more.
5. A repellent according to any one of claims 1 to 4, wherein the modified polyol has four or more monovalent hydrocarbon groups having 20 to 40 carbon atoms, which may have a substituent.
6. The repellent according to claim 5, wherein the monovalent hydrocarbon group having 20 to 40 carbon atoms which may have a substituent is an alkyl group.
7. The polyol modification is such that four or more hydroxy groups of the polyol are substituted with a compound of the following formula: n [Wherein, Y is Y 1 and Y 2 Y is a 1+n valent group consisting of one or more selected from the group consisting of 1 is a direct bond, -O-, -C(=O)-, -C(=NR')-, -S-, -S(=O) 2 -, -NR'-, -C(OR')R'-, and -C(OR')(-) 2 , -N(-) 2 (wherein, R′ is independently at each occurrence a hydrogen atom or an organic group having 1 to 30 carbon atoms); 2 is a group consisting of one or more selected from the group consisting of optionally substituted di- to tetravalent aliphatic hydrocarbon groups having 1 to 40 carbon atoms, optionally substituted di- to tetravalent aromatic hydrocarbon rings, and optionally substituted di- to tetravalent heterocycles, Z is an optionally substituted monovalent hydrocarbon group having 20 to 40 carbon atoms, and n is an integer of 1 or more and 3 or less.
8. Y is -O-Y 11 - or -O-Y 11 -Y 21 -Y 12 wherein each symbol represents independently at each occurrence: Y 11 is a direct bond, —C(═O)—, —C(═O)—NR′—, or —C(═S)—NR′—; Y 21 is a hydrocarbon group having 1 to 40 carbon atoms which may have a substituent; Y 12 is -O-, -O-C(=O)-, -O-C(=O)-O-, -C(=O)-NR'-, -O-C(=O)-NR'-, -NR'-, -NR'-C(= O)-, -NR'-C(=O)-O-, -NR'-C(=O)-NR'-, -C(=O)-, -C(=O)-O-, -C(=O)-NR'-, -SO 2 -, -SO 2 NR'-, -C(OR')R'-, or -C(OR')(-) 2 The repellent according to claim 7, wherein 9. The repellent according to any one of claims 1 to 8, wherein the polyol is at least one selected from the group consisting of monosaccharides, oligosaccharides, polysaccharides, sugar alcohols, hydroxy acids, amino acids, vitamins, flavonols, hydroxy hydrocarbons, and hydroxy group-containing compound polymers.
10. Polyols are selected from the group consisting of glucose, fructose, galactose, xylose; sucrose, cycloamylose, cyclodextrin, maltose, trehalose, lactose, sucralose; sorbitol, maltitol, erythritol, isomalt, lactitol, mannitol, xylitol, sorbitan, lactitol; starch, cellulose, curdlan, pullulan, alginic acid, carrageenan, guar gum, chitin, chitosan, locust bean gum, kappa carrageenan, iota carrageenan, isomaltodextrin, gellan gum, tamarind seed gum; ascorbic acid, kojic acid, quinic acid, chlorogenic acid, gluconic acid; glucosamine; inositol; catechin, quercetin, anthocyanin; The repellent according to any one of claims 1 to 9, which is at least one selected from the group consisting of ethylene glycol, propylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, neopentyl glycol, trimethylene glycol, glycerol, trimethylolpropane, trimethylolethane; polyglycerin, polyvinyl alcohol, hydroxyethyl (meth)acrylate polymers, hydroxypropyl (meth)acrylate polymers, and hydroxybutyl (meth)acrylate polymers.
11. The repellent according to any one of claims 1 to 10, wherein the volumetric ratio of particles having a size of 100 μm or more is 25% or less as measured by a laser diffraction scattering method.
12. The repellent according to any one of claims 1 to 11, wherein the bio-based ratio of the modified polyol is 20% or more.
13. The polyol modification product is a compound in which the hydroxy group of the polyol is replaced with a compound represented by the following formula: n [Wherein, Y is -O-Y 11 - or -O-Y 11 -Y 21 -Y 12 wherein each symbol represents independently at each occurrence: Y 11 is a direct bond, —C(═O)—, —C(═O)—NR′—, or —C(═S)—NR′—; Y 21 is a hydrocarbon group having 1 to 40 carbon atoms which may have a substituent; Y 12 is -O-, -O-C(=O)-, -O-C(=O)-O-, -C(=O)-NR'-, -O-C(=O)-NR'-, -NR'-, -NR'-C(= O)-, -NR'-C(=O)-O-, -NR'-C(=O)-NR'-, -C(=O)-, -C(=O)-O-, -C(=O)-NR'-, -SO 2 -, -SO 2 NR'-, -C(OR')R'-, or -C(OR')(-) 2 Z is a hydrocarbon group having 6 to 40 carbon atoms, and n is an integer of 1 to 3. and the polyol is selected from the group consisting of glucose, fructose, galactose, xylose; sucrose, cycloamylose, cyclodextrin, maltose, trehalose, lactose, sucralose; sorbitol, maltitol, erythritol, isomalt, lactitol, mannitol, xylitol, sorbitan, lactitol; starch, cellulose, curdlan, pullulan, alginic acid, carrageenan, guar gum, chitin, chitosan, locust bean gum, kappa carrageenan, iota carrageenan, isomaltodextrin, gellan gum, tamarind seed gum; ascorbic acid, kojic acid, quinic acid, chlorogenic acid, gluconic acid; glucosamine; inositol; catechin, quercetin, anthocyanin; The repellent according to any one of claims 1 to 12, which is at least one selected from the group consisting of ethylene glycol, propylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, neopentyl glycol, trimethylene glycol, glycerol, trimethylolpropane, and trimethylolethane; polyglycerin, polyvinyl alcohol, a hydroxyethyl (meth)acrylate polymer, a hydroxypropyl (meth)acrylate polymer, and a hydroxybutyl (meth)acrylate polymer, and wherein the hydroxyl group substitution rate in the polyol modified product is 30% or more.
14. The repellent according to any one of claims 1 to 13, wherein the polyol modified product is a compound in which hydroxy groups of polyglycerin or sugar alcohol having a degree of polymerization of 5 to 15 are substituted with groups represented by the following formula: -O-C(=O)-Z, or -O-C(=O)NH-Z, wherein Z is an alkyl group having 20 to 24 carbon atoms, and the hydroxy group substitution rate in the polyol modified product is 50% or more.
15. The repellent according to any one of claims 1 to 14, which is for textile products or paper products.
16. A product treated with a repellent according to any one of claims 1 to 15.
17. The product of claim 16 which is a textile product or a paper product.
18. The product of claim 16 or 17, which is a greaseproof or waterproof paper.
19. The product according to any one of claims 16 to 18, which is a food packaging material or food container.
20. A method for producing a treated product, comprising the step of treating a substrate with a repellent according to any one of claims 1 to 15.
21. The method of claim 20, wherein the treatment is an internal addition treatment.
Citation Information
Patent Citations
ignition device for internal combustion engines
FR627E
Water repellent agent
JP2021155492A
Liquid deodorant composition for textile products
WO2012090580A1
Antifogging agent for polyolefin-based resin and use thereof
JP2019090009A
Modified natural material and use thereof
WO2022065382A1
Cited By
Oil-resistant composition
JP2026148551A
Oil-resistant agent composition
WO2026186884A1