Method for manufacturing clad steel sheet

The described manufacturing method for clad steel plates, focusing on composition and thermal processing, addresses the challenge of achieving high tensile strength and low-temperature toughness in thick plates by refining the microstructure and enhancing HIC resistance, resulting in plates with superior mechanical properties.

WO2024203768A1PCT designated stage expired Publication Date: 2024-10-03JFE STEEL CORP

Patent Information

Application Number
PCT/JP2024/011140
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-03-21
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing methods struggle to produce thick clad steel plates with excellent low-temperature toughness and hydrogen-induced cracking (HIC) resistance while maintaining a tensile strength of 535 MPa or more, due to challenges in refining the microstructure and achieving uniform cooling in thicker plates.

Method used

A manufacturing method involving specific composition control and thermal processing, including reheating and quenching after rolling, to achieve a bainite-dominated microstructure with refined grain size and controlled cooling rates, ensuring a bonding interface strength of 300 MPa or more between the base and laminated steel plates.

Benefits of technology

The method enables the production of thick clad steel plates with tensile strength exceeding 535 MPa, excellent low-temperature toughness, and enhanced HIC resistance, as demonstrated by ductile fracture ratios and crack area ratios meeting or exceeding target values.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

Provided is a method for manufacturing a clad steel sheet in which a thick clad steel sheet exhibiting excellent low temperature toughness can be manufactured while ensuring a tensile strength of 535 MPa or greater. The method for manufacturing a clad steel sheet according to the present invention comprises: a step for obtaining a clad slab by laminating a first material sheet having a prescribed component composition and a second material sheet comprising a corrosion-resistant alloy; a step for heating the clad slab to a prescribed temperature; a step for subsequently subjecting the clad slab to hot rolling under a prescribed condition to obtain a clad rolled sheet in which the first material sheet and the second material sheet are joined to form a base material steel sheet and a laminated material sheet, respectively; a step for cooling the clad rolled sheet; a step for subsequently reheating the clad rolled sheet to 850-1050°C; a step for subsequently cooling the clad rolled sheet such that the average cooling rate of the base material steel sheet is 2-20°C / s; and a step for subsequently tempering the clad rolled sheet to 450-650°C.
Need to check novelty before this filing date? Find Prior Art

Description

Clad steel plate manufacturing method

[0001] The present invention relates to a method for manufacturing a clad steel plate, and more particularly to a method for manufacturing a clad steel plate suitable for use as a material for line pipes.

[0002] Clad steel plates are steel plates made by joining a base steel plate, such as carbon steel, with a clad plate made of a corrosion-resistant alloy. Clad steel plates have the advantage of being highly economical, since they can maintain the same corrosion resistance as solid steel while reducing the amount of expensive alloy elements used.

[0003] In recent years, oil and natural gas development has expanded to regions where line pipes are exposed to severely corrosive environments. Accordingly, demand for line pipes that enable economical transportation of oil and natural gas is expected to increase. Demand is expected for clad steel plates, particularly Ni-based alloy clad steel plates and austenitic stainless clad steel plates, due to their high corrosion resistance, for line pipe applications exposed to severely corrosive environments.

[0004] Furthermore, in recent years, against the backdrop of line pipe leak accidents in wet hydrogen sulfide environments, there has been a trend toward safer designs, and clad steel plates for line pipes are also required to have improved hydrogen-induced cracking resistance (hereinafter also referred to as "HIC resistance") of the base steel plate.

[0005] Here, clad steel plates for line pipes are required to have not only the corrosion resistance of clad steel plates but also predetermined mechanical properties, particularly excellent low-temperature toughness from the viewpoint of preventing brittle fracture of line pipes.

[0006] As an example of such a clad steel plate, Patent Document 1 describes a clad steel plate having a Ni alloy as a cladding material and a low alloy steel as a base material, in which the chemical components of the base material are, in mass %, C: 0.020 to 0.100%, Si: 0.10 to 0.50%, Mn: 0.75 to 1.80%, P: 0.015% or less, S: 0.0030% or less, Cu: 0.01 to 0.50%, Ni: 0.01 to 0.45%, Cr: 0.01 The document discloses a Ni alloy clad steel plate having excellent low temperature toughness and HAZ toughness of the base material and excellent corrosion resistance of the clad material, characterized in that it contains: Cr: 0.01 to 0.50%, Mo: 0.01 to 0.50%, Nb: 0.005 to 0.080%, Ti: 0.005 to 0.030%, N: 0.0010 to 0.0060%, Al: 0.070% or less, Ca: 0.0010 to 0.0040%, and the balance being Fe and unavoidable impurities.

[0007] Furthermore, Patent Document 2 describes a clad steel plate in which a Ni alloy is used as a cladding material and a low alloy steel is used as a base material, and the chemical components of the base material are, in mass %, C: 0.020 to 0.100%, Si: 0.10 to 0.50%, Mn: 0.75 to 1.80%, P: 0.015% or less, S: 0.0030% or less, Cu: 0.01 to 0.50%, Ni: 0.01 to 0.45%, Cr: 0.01 to 0.50%, M "A Ni alloy clad steel plate having excellent low temperature toughness and HAZ toughness of the base material and excellent corrosion resistance of the clad material, characterized by containing 0.01 to 0.50% of Co, 0.005 to 0.080%, 0.005 to 0.030%, 0.0010 to 0.0060%, 0.070% or less of Al, 0.0010 to 0.0040% of Ca, with the balance being Fe and unavoidable impurities."

[0008] Furthermore, Patent Document 3 describes a clad steel plate having an austenitic stainless steel clad material and a low alloy steel base material, in which the base material contains, in mass %, C: 0.020 to 0.100%, Si: 0.10 to 0.50%, Mn: 0.75 to 1.80%, P: 0.015% or less, S: 0.0030% or less, Cu: 0.01 to 0.50%, Ni: 0.01 to 0.45%, Cr: 0.01 to 0.50%, Mo: 0.01 to 0.50%, and "An austenitic stainless clad steel plate having excellent low-temperature toughness and HAZ toughness of the base material and excellent corrosion resistance of the clad material, characterized by containing: 0.01 to 0.50%, Nb: 0.005 to 0.080%, Ti: 0.005 to 0.030%, N: 0.0010 to 0.0060%, Al: 0.070% or less, Ca: 0.0010 to 0.0040%, with the balance being Fe and unavoidable impurities."

[0009] Furthermore, Patent Document 4 describes a clad steel plate in which a clad material made of a corrosion-resistant alloy is bonded to one side of a base steel plate, the base steel plate containing, in mass %, C: 0.020 to 0.100%, Si: 0.05 to 0.50%, Mn: 0.75 to 1.80%, P: 0.015% or less, S: 0.0030% or less, Al: 0.010 to 0.070%, Nb: 0.005 to 0.080%, Ti: 0.005 to 0.030%, and N: 0.0010 to 0.0 "A clad steel plate having a component composition consisting of 0.060% of Fe, with the balance consisting of Fe and unavoidable impurities, wherein the base steel plate has a steel structure in which, at a half-thickness position in the plate thickness direction of the base steel plate, it has 94% or more of bainite and 6% or less of island martensite in terms of area ratio, and the average crystal grain size of the bainite is 25 μm or less, and further, the shear strength of the joint interface between the base steel plate and the clad material is 300 MPa or more."

[0010] Furthermore, Patent Document 5 discloses, as a technology aimed at improving HIC resistance, "a clad steel plate which has excellent HIC resistance and further improved low-temperature toughness while maintaining a tensile strength of 535 MPa or more," and "a clad steel plate having a clad material made of a corrosion-resistant alloy bonded to one side of a base steel plate, wherein the base steel plate has a chemical composition in which the ACR and PHIC values ​​are appropriately controlled, and the base steel plate has a steel structure in which, at a half-thickness position in the plate thickness direction of the base steel plate, it has bainite in an area ratio of 94% or more and the average crystal grain size of the bainite is 25 μm or less, and further the shear strength of the joint interface between the base steel plate and the clad material is 300 MPa or more."

[0011] JP 2015-86422 A JP 2015-117408 A JP 2015-105399 A International Publication No. 2018 / 181381 International Publication No. 2020 / 004410

[0012] In the technologies of Patent Documents 1 to 3, by applying TMCP (Thermo-mechanical control process), it is possible to improve the corrosion resistance of cladding materials without impairing productivity, and to achieve a plate thickness of 30 mm or less, a tensile strength of 535 MPa or more, and a DWTTSA of 1000 MPa or more. -20℃ Furthermore, in Patent Document 4, the clad slab is directly quenched and tempered after rolling, thereby achieving mechanical properties of DWTTSA. -30℃ In Patent Document 5, similar to Patent Document 4, the clad slab is rolled and then directly quenched and tempered, thereby achieving mechanical properties of DWTTSA. -30℃ A clad steel plate is disclosed that realizes mechanical properties of ≥ 85% and also has HIC resistance.

[0013] Here, DWTTSA -20℃ and DWTTSA -30℃ These are the ductile fracture surface rates obtained in a DWTT (Drop Weight Tear Test) conforming to API-5L when the test temperatures are −20° C. and −30° C., respectively.

[0014] In order to improve the low-temperature toughness, which is emphasized in the present invention, it is important to refine the microstructure of the base steel plate in the clad steel plate. The techniques described in Patent Documents 1 to 5 achieve appropriate transformation strengthening by ensuring a predetermined reduction rate in a specific temperature range during rolling and performing accelerated cooling, thereby avoiding grain coarsening associated with high-temperature transformation. However, when the clad steel plate is thick, for example, 25 mm or thicker, it becomes difficult to impart rolling strain to the interior of the steel plate. Furthermore, with accelerated cooling, the cooling behavior of the steel plate is rate-limited by the thermal conductivity of the steel plate, making it difficult to achieve a desired cooling rate all the way to the center of the plate thickness. As a result, it is not possible to achieve grain refinement like in thin clad steel plates, and there is still room for improvement in low-temperature toughness. Therefore, a manufacturing technology that can achieve high strength and excellent low-temperature toughness in thick clad steel plates has been sought.

[0015] In view of the above problems, the first object of the present invention is to provide a method for manufacturing clad steel plate that can produce thick clad steel plate that has excellent low-temperature toughness while ensuring a tensile strength of 535 MPa or more.

[0016] A second object of the present invention is to provide a method for manufacturing clad steel plates that can produce thick clad steel plates that have excellent low-temperature toughness and HIC resistance while maintaining a tensile strength of 535 MPa or more.

[0017] The term "excellent low-temperature toughness" refers to the ductile fracture area ratio DWTTSA obtained by the DWTT test (test temperature: -30°C) in accordance with API-5L. -30℃ Furthermore, "excellent HIC resistance" means that the crack area ratio (CAR) obtained in an HIC test in accordance with NACE Standard TM0284-2003 is 5.0% or less.

[0018] The inventors conducted extensive research to develop a thick clad steel plate that has improved low-temperature toughness while maintaining predetermined tensile properties, and have discovered the following: (A) In order to obtain excellent low-temperature toughness, it is effective to simultaneously refine the structure of the base steel plate, which increases brittle crack propagation resistance, and reduce hard phases that can serve as brittle crack initiation sites. To achieve this, it is preferable that the steel structure of the base steel plate be a structure mainly composed of bainite. Specifically, it is effective to set the area fraction of bainite at the half-thickness position in the plate thickness direction of the base steel plate to 94% or more and the average grain size of bainite to 23 μm or less.

[0019] (B) To achieve the above-mentioned structural control, it is important to properly control the chemical composition and manufacturing conditions, and in particular, to apply reheating, quenching, and tempering after rolling the clad slab, and to properly control these conditions.

[0020] The gist and configuration of the present invention, which has been completed based on the above findings, is as follows. [1] In mass%, C: 0.020% or more and 0.100% or less, Si: 0.10% or more and 0.50% or less, Mn: 0.75% or more and 1.80% or less, P: 0.015% or less, S: 0.0030% or less, Al: 0.01% or more and 0.07% or less, Nb: 0.005% or more and 0.080% or less, Ti: 0.005% or more and 0.030% or less, N: 0.0010% or more and 0.0060% or less, and O (oxygen): 0.0030% or less, and further containing Cu: 0.50% or less, Ni: 0.50% or less, Cr: 0.50% or less, Mo: 0.50% or less, V: 0.100% or less, and and Ca: 0.0040% or less, and having a chemical composition in which Ceq defined by the following formula (1) is 0.40 or more and 0.50 or less, with the balance being Fe and unavoidable impurities; preparing a second material plate made of a corrosion-resistant alloy; stacking the first material plate and the second material plate to obtain a clad slab; heating the clad slab to 1050°C or more and 1200°C or less; thereafter, hot rolling the clad slab at a rolling finish temperature of 900°C or more to obtain a clad rolled plate in which the first material plate and the second material plate are joined together to form a base steel plate and a clad plate, respectively; cooling the clad rolled plate; and thereafter, reheating the clad rolled plate to 850°C or more and 1050°C or less. a step of cooling the clad rolled plate so that the average cooling rate of the base steel plate is 2°C / s or more and 20°C / s or less, and a step of tempering the clad rolled plate to 450°C or more and 650°C or less, thereby producing a clad steel plate having the cladding plate joined to one side of the base steel plate. Ceq=C+Mn / 6+(Cu+Ni) / 15+(Cr+Mo+V) / 5 (1) The element symbols in formula (1) represent the content (mass%) of each element, and zero is substituted if the element is not contained.

[0021] [2] In the composition of the first blank plate, the Ca content is, in mass%, 0.0005% or more and 0.0040% or less, the ACR defined by the following formula (2) is 1.00 or more and 6.00 or less, and the P defined by the following formula (3) is HIC ACR={Ca−(0.18+130Ca)×O} / (1.25S) (2) P HIC = 4.46C + 2.37Mn / 6 + (1.18Cr + 1.95Mo + 1.74V) / 5 + (1.74Cu + 1.7Ni) / 15 + 22.36P (3) The element symbols in formulas (2) and (3) represent the content (mass%) of each element, and zero is substituted when the element is not contained.

[0022] [3] The method for manufacturing a clad steel plate according to the above [1] or [2], wherein the corrosion-resistant alloy is a Ni-based alloy such as either Alloy 825 or Alloy 625, or an austenitic stainless steel.

[0023] [4] A method for manufacturing a clad steel plate according to any one of [1] to [3] above, wherein the clad slab is formed by stacking the first material plate, the second material plate, the second material plate, and the first material plate in that order, and a release material is applied between the two second material plates, thereby obtaining two clad rolled plates by hot rolling, and after the tempering, the two clad rolled plates are peeled off via the release material.

[0024] According to the first embodiment of the present invention, it is possible to manufacture a thick clad steel plate that has excellent low-temperature toughness while ensuring a tensile strength of 535 MPa or more.

[0025] Furthermore, according to the second embodiment of the present invention, it is possible to manufacture a thick clad steel plate that is excellent in both low-temperature toughness and HIC resistance while ensuring a tensile strength of 535 MPa or more.

[0026] One embodiment of the present invention relates to a method for manufacturing a clad steel plate formed by bonding a clad plate to one side of a base steel plate. The method for manufacturing a clad steel plate according to this embodiment includes the steps of: laminating a first blank sheet having a predetermined chemical composition with a second blank sheet made of a corrosion-resistant alloy to obtain a clad slab; heating the clad slab to a predetermined heating temperature; hot rolling the clad slab under predetermined conditions to obtain a clad rolled plate in which the first blank sheet and the second blank sheet are bonded together to form the base steel plate and the clad plate, respectively; allowing the clad rolled plate to cool; reheating and quenching the clad rolled plate to a predetermined reheating temperature and then cooling it; and tempering the clad rolled plate to a predetermined tempering temperature. The first blank sheet is the base steel plate material, and the second blank sheet is the clad plate material.

[0027] The thickness of the clad steel plate manufactured in this embodiment (total thickness of the base steel plate and cladding plate) is 25 mm or more, preferably 30 mm or more. There is no particular upper limit to the thickness of the clad steel plate manufactured in this embodiment, but the thickness of the clad steel plate is preferably, for example, 50 mm or less. Furthermore, the thicknesses of the base steel plate and cladding plate in the clad steel plate manufactured in this embodiment are preferably 8 mm or more and 46 mm or less and 3.0 mm or more and 4.0 mm or less, respectively.

[0028] 1. Chemical Composition of Base Steel Plate and First Material Plate The chemical compositions of the base steel plate and the first material plate will be described. Note that the unit of the content of elements in the chemical composition is always "mass%", but hereinafter, unless otherwise specified, it will be simply expressed as "%".

[0029] (1-1) First embodiment In the first embodiment, the elemental composition of the base steel plate and the first material plate is, in mass%, C: 0.020% or more and 0.100% or less, Si: 0.10% or more and 0.50% or less, Mn: 0.75% or more and 1.80% or less, P: 0.015% or less, S: 0.0030% or less, Al: 0.01% or more and 0.07% or less, Nb: 0.005% or more and 0.080% or less, Ti: 0.005% or more and 0.030% or less. %, N: 0.0010% or more and 0.0060% or less, and O (oxygen): 0.0030% or less, and further containing one or more elements selected from the group consisting of Cu: 0.50% or less, Ni: 0.50% or less, Cr: 0.50% or less, Mo: 0.50% or less, V: 0.100% or less, and Ca: 0.0040% or less, with the balance consisting of Fe and unavoidable impurities. This first embodiment has a component composition necessary to achieve a tensile strength of 535 MPa or more and excellent low-temperature toughness.

[0030] C: 0.020% or more and 0.100% or less C is an element that contributes to precipitation strengthening as a carbide. If the C content is less than 0.020%, sufficient strength cannot be ensured in the base steel plate. Therefore, the C content is set to 0.020% or more, preferably 0.030% or more. On the other hand, if the C content exceeds 0.100%, the low-temperature toughness and weld heat-affected zone toughness of the base steel plate deteriorate, and the HIC resistance also deteriorates. Therefore, the C content is set to 0.100% or less, preferably 0.080% or less.

[0031] Si: 0.10% or more and 0.50% or less Si is an element added to ensure the strength of steel sheets through deoxidation and solid solution strengthening. From the viewpoint of obtaining this effect, the Si content is set to 0.10% or more, preferably 0.15% or more, and more preferably 0.20% or more. On the other hand, if the Si content exceeds 0.50%, toughness and weldability deteriorate. Therefore, the Si content is set to 0.50% or less, preferably 0.40% or less.

[0032] Mn: 0.75% or more and 1.80% or less Mn is an element added to ensure strength and toughness. From the viewpoint of obtaining this effect, the Mn content is set to 0.75% or more, preferably 1.00% or more. On the other hand, if the Mn content exceeds 1.80%, weldability deteriorates. Therefore, the Mn content is set to 1.80% or less, preferably 1.70% or less.

[0033] P: 0.015% or less P is an inevitable impurity that deteriorates weldability. Therefore, the P content is set to 0.015% or less, preferably 0.010% or less. The lower limit of the P content is not particularly limited, and the P content can be 0.000% or more.

[0034] S: 0.0030% or less S generally exists as sulfide-based inclusions in steel and deteriorates ductility and toughness. Therefore, it is preferable to reduce S as much as possible, and the S content is set to 0.0030% or less, preferably 0.0010% or less. There is no particular lower limit for the S content, and the S content can be 0.0000% or more.

[0035] Al: 0.01% or more and 0.07% or less Al is an element added for deoxidation. From the viewpoint of obtaining this effect, the Al content is set to 0.01% or more, preferably 0.02% or more. On the other hand, if the Al content exceeds 0.07%, alumina clusters are formed, deteriorating ductility. Therefore, the Al content is set to 0.07% or less, preferably 0.04% or less.

[0036] Nb: 0.005% or more and 0.080% or less Nb is effective in increasing the strength of steel sheets by precipitation strengthening and increasing hardenability. It also has the effect of expanding the austenite non-recrystallization temperature range and contributes to improving toughness by refining the structure. From the viewpoint of obtaining these effects, the Nb content is set to 0.005% or more, preferably 0.010% or more. On the other hand, if the Nb content exceeds 0.080%, the toughness and HIC resistance of the weld heat-affected zone deteriorate. Therefore, the Nb content is set to 0.080% or less, preferably 0.060% or less.

[0037] Ti: 0.005% or more and 0.030% or less Ti suppresses coarsening of austenite through the pinning effect of nitride formation, contributing to ensuring the toughness of the base material and the weld heat-affected zone. Ti is also an element effective in increasing the strength of steel plates through precipitation strengthening. From the viewpoint of obtaining these effects, the Ti content is set to 0.005% or more, preferably 0.010% or more. On the other hand, if the Ti content exceeds 0.030%, nitrides become coarse and become the starting point for brittle fracture or ductile fracture. Therefore, the Ti content is set to 0.030% or less, preferably 0.020% or less.

[0038] N: 0.0010% or more and 0.0060% or less N suppresses coarsening of austenite through the pinning effect of nitride formation, contributing to ensuring the toughness of the base material and the weld heat affected zone. Therefore, the N content is set to 0.0010% or more, preferably 0.0020% or more. On the other hand, if the N content exceeds 0.0060%, the toughness of the weld heat affected zone deteriorates. Therefore, the N content is set to 0.0060% or less, preferably 0.0050% or less.

[0039] In order to fully exert the pinning effect due to nitride formation, it is preferable to regulate the ratio of Ti content to N content. Specifically, when the Ti content / N content ratio is less than 2.0 or more than 3.5 by mass%, the pinning effect due to nitride formation is not fully exerted, and austenite becomes coarse, which may result in a deterioration in toughness. Therefore, it is preferable to set the Ti content / N content ratio to 2.0 or more and 3.5 or less.

[0040] O (oxygen): 0.0030% or less O generally exists in steel as oxides of Al and Ca. If excessive O is contained, the amount of oxides in the steel increases, deteriorating toughness and HIC resistance. Therefore, the O content is set to 0.0030% or less, and preferably 0.0020% or less. The lower limit of the O content is not particularly limited, and the O content can be 0.0000% or more.

[0041] The elemental composition of the base steel plate and the first material plate contains, in addition to the above-mentioned basic components, one or more elements selected from the group consisting of Cu: 0.50% or less, Ni: 0.50% or less, Cr: 0.50% or less, Mo: 0.50% or less, V: 0.100% or less, and Ca: 0.0040% or less.

[0042] Cu: 0.50% or less, Cr: 0.50% or less, Mo: 0.50% or less Cu, Cr, and Mo are all elements that improve hardenability and contribute to increasing the strength of the base material and the weld heat affected zone. To achieve this effect, when Cu, Cr, and Mo are contained, the content of each element is 0.01% or more, preferably 0.05% or more. On the other hand, if the Cu, Cr, and Mo contents each exceed 0.50%, the toughness of the weld heat affected zone may deteriorate. Therefore, when Cu, Cr, and Mo are contained, the content of each element is 0.50% or less, preferably 0.40% or less.

[0043] Ni: 0.50% or less Ni is an element that improves hardenability and contributes to increasing the strength of the base material and the weld heat affected zone. From the viewpoint of obtaining this effect, when Ni is contained, the Ni content is set to 0.01% or more, preferably 0.05% or more. On the other hand, since Ni is an expensive element, adding a large amount of Ni increases costs. Therefore, when Ni is contained, the Ni content is set to 0.50% or less, preferably 0.40% or less.

[0044] V: 0.100% or less V contributes to increasing the strength of steel sheets through precipitation strengthening. From the viewpoint of obtaining this effect, when V is contained, the V content is set to 0.010% or more. On the other hand, when the V content exceeds 0.100%, the toughness of the weld heat affected zone deteriorates. Therefore, when V is contained, the V content is set to 0.100% or less.

[0045] Ca: 0.0040% or less Ca fixes S in steel and improves the toughness of the steel plate. From the viewpoint of obtaining this effect, when Ca is contained, the Ca content is set to 0.0010% or more. On the other hand, if the Ca content exceeds 0.0040%, the amount of inclusions in the steel increases, which may deteriorate the toughness. Therefore, when Ca is contained, the Ca content is set to 0.0040% or less, preferably 0.0030% or less.

[0046] Carbon equivalent Ceq defined by the following formula (1): 0.40 or more and 0.50 or less The carbon equivalent Ceq defined by the following formula (1) correlates with the strength of the steel plate. In the case of the reheating, quenching, and tempering process, which is the manufacturing method of this embodiment, in order to obtain a high strength of 535 MPa or more in tensile strength, the carbon equivalent Ceq is set to 0.40 or more, preferably 0.42 or more. On the other hand, an excessively large carbon equivalent Ceq may result in a deterioration in toughness. Therefore, the carbon equivalent Ceq is set to 0.50 or less, preferably 0.48 or less. Ceq = C + Mn / 6 + (Cu + Ni) / 15 + (Cr + Mo + V) / 5 (1) Note that the element symbols in formula (1) refer to the content (mass%) of each element in the base steel plate or the first material plate, and zero is substituted if the element is not contained.

[0047] (1-2) Second embodiment Next, the chemical composition of the base steel plate and the first blank sheet according to the second embodiment, which is necessary for the base steel plate to exhibit excellent HIC resistance in addition to a tensile strength of 535 MPa or more and excellent low-temperature toughness, will be described. Below, items that are different from the first embodiment and items that are added will be described. Items not described below conform to the first embodiment.

[0048] P: 0.010% or less P is an inevitable impurity that increases the hardness of the center segregation region, thereby deteriorating HIC resistance. Therefore, when HIC resistance is required, the P content is preferably 0.010% or less, and more preferably 0.006% or less. There is no particular lower limit for the P content, and the P content can be 0.000% or more.

[0049] S: 0.0010% or less S generally exists as sulfide-based inclusions in steel and deteriorates toughness and HIC resistance. Therefore, when HIC resistance is required, the S content is preferably 0.0010% or less, and more preferably 0.0008% or less. The lower limit of the S content is not particularly limited and can be 0.0000% or more.

[0050] Ca: 0.0005% or more and 0.0040% or less Ca fixes S in the steel to improve the toughness and HIC resistance of the steel plate. From the viewpoint of obtaining these effects, the Ca content is preferably 0.0005% or more, more preferably 0.0010% or more, and even more preferably 0.0020% or more. On the other hand, if the Ca content exceeds 0.0040%, the amount of inclusions in the steel increases, which may deteriorate the toughness and HIC resistance. Therefore, the Ca content is preferably 0.0040% or less, and more preferably 0.0030% or less.

[0051] When HIC resistance is required, the ACR and P defined by the following formulas (2) and (3), respectively, are HIC It is preferable to properly control the value of ACR={Ca−(0.18+130Ca)×O} / (1.25S) (2) HIC = 4.46C + 2.37Mn / 6 + (1.18Cr + 1.95Mo + 1.74V) / 5 + (1.74Cu + 1.7Ni) / 15 + 22.36P (3) The element symbols in formulas (2) and (3) represent the content (mass%) of each element in the base steel plate or the first material plate, and zero is substituted if the element is not contained.

[0052] ACR: 1.00 or more and 6.00 or less The ACR is a numerical value that serves as an index of the effect of Ca in suppressing MnS formation. MnS in steel affects hydrogen-induced cracking, and in order to improve HIC resistance, it is effective to fix S in the steel with Ca and suppress MnS formation. When the ACR is 1.00 or more, the effect of suppressing MnS formation is fully exerted. Therefore, the ACR is preferably 1.00 or more, and more preferably 1.40 or more. On the other hand, when the ACR value exceeds 6.00, although MnS formation is suppressed, a large amount of Ca-based oxides is formed, which actually deteriorates HIC resistance. Therefore, the ACR is preferably 6.00 or less, and more preferably 3.30 or less.

[0053] P HIC : Less than 1.250 P HIC is a numerical value that serves as an index of the hardness of the central segregation portion, and the larger this numerical value, the higher the hardness of the central segregation portion. Since the hardness of the central segregation portion affects hydrogen-induced cracking, it is effective to suppress the increase in hardness of the central segregation portion in order to improve HIC resistance. For this reason, P HIC is preferably less than 1.250, and more preferably 1.000 or less. HIC Although there is no particular limitation on the lower limit of P, from the viewpoint of ensuring sufficient strength in the base steel sheet, HIC is preferably 0.750 or more.

[0054] 2. Microstructure of Base Steel Plate (Preferred Conditions) In the clad steel plate manufactured according to this embodiment, the base steel plate preferably has the following microstructure.

[0055] Area fraction of bainite at half thickness position in the thickness direction of the base steel plate: 94% or more Bainite is an important structure for achieving both strength and low-temperature toughness. Bainite is also a transformation strengthening structure and effectively contributes to improving the strength of the steel plate. For this reason, it is preferable that the steel structure of the base steel plate is a structure mainly composed of bainite. Specifically, it is preferable that the area fraction of bainite at half thickness position in the thickness direction of the base steel plate (hereinafter simply referred to as "half thickness position") is 94% or more. The area fraction of bainite is more preferably 97% or more, and may be 100%.

[0056] The steel structure of the base steel plate must basically be composed of bainite, but may contain trace amounts of island martensite (MA: martensite-austenite constituent), ferrite, cementite, etc. as remaining structures other than bainite. The total area ratio of the remaining structures at the half-thickness position is acceptable if it is 6% or less. The area ratio of the remaining structures may be 0%. If the area ratio of the remaining structures exceeds 6%, the area ratio of bainite becomes small, which is not preferable because it may not be possible to achieve both strength and low-temperature toughness.

[0057] Here, the area ratio of each phase at the half-thickness position can be determined as follows: After mirror polishing an L cross section (a cross section parallel to the rolling direction and parallel to the normal direction of the rolling surface) of a base steel sheet, the L cross section is corroded with nital or electrolytic etching (electrolyte: 100 ml distilled water + 25 g sodium hydroxide + 5 g picric acid), and a scanning electron microscope (SEM) is used to measure the area ratio of a randomly selected 1.2 × 10 -2 mm 2 This can be determined by observing the area and analyzing the image.

[0058] Average grain size of bainite at half thickness position: 23 μm or less Because bainite grain boundaries act as resistance to brittle crack propagation, refinement of grains increases the number of grain boundaries, contributing to improved low-temperature toughness. Therefore, the average grain size of bainite at half thickness position is preferably 23 μm or less, and more preferably 20 μm or less. There is no particular lower limit for the average grain size, but the average grain size can be 5 μm or more.

[0059] Here, the average grain size of bainite can be determined as follows: After mirror polishing the L cross section (a cross section parallel to the rolling direction and parallel to the normal direction of the rolling surface) of the base steel sheet, 1.2 × 10 randomly selected grains at a position halfway through the sheet thickness in the L cross section are measured by electron backscatter diffraction (EBSP). -2 mm 2 The crystal orientation of the region is measured, and the region where the angle difference between adjacent pixels is 15° or more is determined as the grain boundary by image analysis. area is the area occupied by each grain a i and the circle equivalent diameter d of each crystal grain i It can be calculated using the following formula: area =Σ(a i ・d i ) / Σa i

[0060] 3. Cladding Plate and Second Blank Plate In this embodiment, the cladding plate and the second blank plate are made of a corrosion-resistant alloy. The corrosion-resistant alloy is preferably a Ni-based alloy or austenitic stainless steel. In particular, a Ni-based alloy is preferred because it exhibits high stress corrosion cracking resistance in a high hydrogen sulfide partial pressure environment (sour environment). The Ni-based alloy is, for example, Alloy 625 or Alloy 825, and Alloy 625 is particularly preferred from the viewpoint of stress corrosion cracking resistance.

[0061] The following describes the preferred composition of the clad sheet and the second blank sheet. The unit of the content of elements in the composition is "mass %", but hereinafter, unless otherwise specified, it will be simply expressed as "%".

[0062] (3-1) Preferred Component Composition of Alloy625 Alloy625 is a Ni-based alloy equivalent to NCF625 in JIS G 4902:2019. Among them, a Ni-based alloy having a component composition containing, in mass%, C: 0.030% or less, Si: 0.02 to 0.50%, Mn: 0.02 to 0.50%, P: 0.010% or less, S: 0.0010% or less, Cr: 20.0 to 23.0%, Mo: 8.00 to 10.00%, Fe: 5.0% or less, Al: 0.02 to 0.40%, Ti: 0.10 to 0.40%, and a total amount of Nb and Ta: 3.15 to 4.15%, with the balance being Ni and unavoidable impurities, is preferred.

[0063] C: 0.030% or less C precipitates as carbides at grain boundaries during the thermal history during the production of clad steel plate, degrading corrosion resistance. If the C content exceeds 0.030%, carbide precipitation is promoted, degrading corrosion resistance. Therefore, the C content is preferably 0.030% or less, and more preferably 0.020% or less. There is no particular lower limit for the C content, and the C content can be 0.000% or more.

[0064] Si: 0.02 to 0.50% Si is added for deoxidation. From the viewpoint of obtaining this effect, the Si content is preferably 0.02% or more. On the other hand, if the Si content exceeds 0.50%, corrosion resistance deteriorates. Therefore, the Si content is preferably 0.50% or less, and more preferably 0.20% or less.

[0065] Mn: 0.02 to 0.50% Mn is added for deoxidation. From the viewpoint of obtaining this effect, the Mn content is preferably 0.02% or more. On the other hand, if the Mn content exceeds 0.50%, corrosion resistance deteriorates. Therefore, the Mn content is preferably 0.50% or less, and more preferably 0.15% or less.

[0066] P: 0.010% or less P is an impurity element that segregates at grain boundaries and deteriorates corrosion resistance. Therefore, the P content is preferably 0.010% or less, and more preferably 0.005% or less. The lower limit of the P content is not particularly limited, and the P content can be 0.000% or more.

[0067] S: 0.0010% or less Like P, S is an impurity element that segregates at grain boundaries and deteriorates corrosion resistance. Therefore, the S content is preferably 0.0010% or less, and more preferably 0.0005% or less. There is no particular limitation on the lower limit of the S content, and the S content can be 0.0000% or more.

[0068] Cr: 20.0 to 23.0% Cr forms a highly protective oxide film on the surface of the metal, improving pitting corrosion resistance and intergranular corrosion resistance. Furthermore, when added in combination with Ni, Cr improves stress corrosion cracking resistance in sour environments. From the viewpoint of achieving these effects, the Cr content is preferably 20.0% or more, and more preferably 21.5% or more. However, from the viewpoint of the balance with Ni and other alloys, the Cr content is preferably 23.0% or less.

[0069] Mo: 8.00 to 10.00% Mo improves pitting corrosion resistance and crevice corrosion resistance. Furthermore, Mo, when added in combination with Ni, improves stress corrosion cracking resistance in sour environments. From the viewpoint of obtaining these effects, the Mo content is preferably 8.00% or more. However, from the viewpoint of the balance with Ni and other alloys, the Mo content is preferably 10.00% or less.

[0070] Fe: 5.0% or less Fe is an impurity that is inevitably mixed in when ferrochromium, ferromolybdenum, or the like is used as a raw material, and if the Fe content exceeds 5.0%, corrosion resistance deteriorates. Therefore, the Fe content is preferably 5.0% or less, and more preferably 3.5% or less. There is no particular lower limit for the Fe content, and the Fe content can be 0.0% or more.

[0071] Al: 0.02 to 0.40% Al is an effective deoxidizing element. From the viewpoint of obtaining this effect, the Al content is preferably 0.02% or more. On the other hand, if the Al content exceeds 0.40%, stress corrosion cracking resistance deteriorates. Therefore, the Al content is preferably 0.40% or less, and more preferably 0.25% or less.

[0072] Ti: 0.10 to 0.40% Ti fixes C, which deteriorates corrosion resistance, by precipitating it as carbide. From the viewpoint of obtaining this effect, the Ti content is preferably 0.10% or more. On the other hand, if the Ti content exceeds 0.40%, Ti precipitates as an intermetallic compound, which reduces the bondability with the base steel sheet. Therefore, the Ti content is preferably 0.40% or less, and more preferably 0.30% or less.

[0073] Total amount of Nb and Ta: 3.15 to 4.15% Both Nb and Ta are effective in fixing C. From the viewpoint of obtaining this effect, the total amount of Nb and Ta is preferably 3.15% or more. On the other hand, if the total amount of Nb and Ta exceeds 4.15%, Nb and Ta form an intermetallic compound with a low melting point, which reduces hot workability. Therefore, the total amount of Nb and Ta is preferably 4.15% or less.

[0074] Components other than those mentioned above are Ni and unavoidable impurities. Ni is an element that improves corrosion resistance, and particularly significantly improves stress corrosion cracking resistance in sour environments. For this reason, the Ni content is preferably 58% or more.

[0075] (3-2) Preferred Component Composition of Alloy825 Alloy825 is a Ni-based alloy equivalent to NCF825 in JIS G 4902:2019, and among these, a Ni-based alloy having a component composition containing, in mass%, C: 0.020% or less, Si: 0.50% or less, Mn: 1.00% or less, P: 0.030% or less, S: 0.0050% or less, Ni: 38.0 to 46.0%, Cr: 19.5 to 23.5%, Mo: 2.50 to 3.50%, Cu: 1.50 to 3.00%, Al: 0.01 to 0.20%, and Ti: 0.60 to 1.20%, with the balance being Fe and unavoidable impurities, is preferred.

[0076] C: 0.020% or less C precipitates as carbides at grain boundaries during the thermal history during the production of clad steel plate, degrading corrosion resistance. If the C content exceeds 0.020%, carbide precipitation is promoted, degrading corrosion resistance. Therefore, the C content is preferably 0.020% or less, and more preferably 0.015% or less. There is no particular lower limit for the C content, and the C content can be 0.000% or more.

[0077] Si: 0.50% or less Si is added for deoxidation. However, if the Si content exceeds 0.50%, Si remains as non-metallic inclusions, deteriorating corrosion resistance. Therefore, the Si content is preferably 0.50% or less, and more preferably 0.20% or less. There is no particular lower limit for the Si content, but from the viewpoint of obtaining a sufficient deoxidation effect, the Si content is preferably 0.02% or more.

[0078] Mn: 1.00% or less Mn is added for deoxidation. However, if the Mn content exceeds 1.00%, corrosion resistance deteriorates. Therefore, the Mn content is preferably 1.00% or less, and more preferably 0.50% or less. There is no particular lower limit for the Mn content, but from the viewpoint of obtaining a sufficient deoxidation effect, the Mn content is preferably 0.02% or more.

[0079] P: 0.030% or less P is an impurity element that segregates at grain boundaries and deteriorates corrosion resistance. Therefore, the P content is preferably 0.030% or less, and more preferably 0.020% or less. The lower limit of the P content is not particularly limited, and the P content can be 0.000% or more.

[0080] S: 0.0050% or less S, like P, is an impurity element that segregates at grain boundaries and deteriorates corrosion resistance. Therefore, the S content is preferably 0.0050% or less, and more preferably 0.0010% or less. The lower limit of the S content is not particularly limited, and the S content can be 0.0000% or more.

[0081] Ni: 38.0 to 46.0% Ni is an element that improves corrosion resistance, and significantly improves stress corrosion cracking resistance, particularly in sour environments. From the viewpoint of achieving this effect, the Ni content is preferably 38.0% or more. However, because Ni is a very expensive element, adding a large amount of Ni increases costs. Therefore, from the viewpoint of balancing the effect of improving corrosion resistance with costs, the Ni content is preferably 46.0% or less.

[0082] Cr: 19.5 to 23.5% Cr forms a highly protective oxide film on the surface of the metal, improving pitting corrosion resistance and intergranular corrosion resistance. Furthermore, when added in combination with Ni, Cr improves stress corrosion cracking resistance in sour environments. From the viewpoint of achieving these effects, the Cr content is preferably 19.5% or more, and more preferably 21.5% or more. However, from the viewpoint of the balance with Ni and other alloys, the Cr content is preferably 23.5% or less.

[0083] Mo: 2.50 to 3.50% Mo improves pitting corrosion resistance and crevice corrosion resistance. Furthermore, Mo, when added in combination with Ni, improves stress corrosion cracking resistance in sour environments. From the viewpoint of obtaining these effects, the Mo content is preferably 2.50% or more, and more preferably 3.00% or more. However, from the viewpoint of the balance with Ni and other alloys, the Mo content is preferably 3.50% or less.

[0084] Cu: 1.50 to 3.00% Cu improves general corrosion resistance. From the viewpoint of obtaining this effect, the Cu content is preferably 1.50% or more, and more preferably 1.80% or more. On the other hand, if the Cu content exceeds 3.00%, the effect saturates, so the Cu content is preferably 3.00% or less.

[0085] Al: 0.01 to 0.20% Al is an effective deoxidizing element. From the viewpoint of obtaining this effect, the Al content is preferably 0.01% or more, and more preferably 0.10% or more. On the other hand, if the Al content exceeds 0.20%, stress corrosion cracking resistance deteriorates. Therefore, the Al content is preferably 0.20% or less, and more preferably 0.15% or less.

[0086] Ti: 0.60 to 1.20% Ti fixes C, which deteriorates corrosion resistance, by precipitating it as carbide. From the viewpoint of obtaining this effect, the Ti content is preferably 0.60% or more, and more preferably 0.70% or more. On the other hand, if the Ti content exceeds 1.20%, Ti precipitates as an intermetallic compound, which reduces the bondability with the base steel sheet, so the Ti content is preferably 1.20% or less.

[0087] The components other than those mentioned above are Fe and unavoidable impurities.

[0088] (3-3) Austenitic Stainless Steel A suitable chemical composition of the austenitic stainless steel contains, in mass%, C: 0.030% or less, Si: 1.00% or less, Mn: 2.00% or less, P: 0.045% or less, S: 0.030% or less, Ni: 12.0 to 15.0%, Cr: 16.0 to 18.0%, and Mo: 2.00 to 3.00%, with the balance being Fe and unavoidable impurities.

[0089] C: 0.030% or less C precipitates as carbides at grain boundaries during the thermal history during the production of clad steel plate, degrading corrosion resistance. If the C content exceeds 0.030%, carbide precipitation is promoted, degrading corrosion resistance. Therefore, the C content is preferably 0.030% or less, more preferably 0.020% or less, and even more preferably 0.015% or less. The lower limit of the C content is not particularly limited, and the C content can be 0.000% or more.

[0090] Si: 1.00% or less If the Si content exceeds 1.00%, Si remains as non-metallic inclusions, deteriorating corrosion resistance. Therefore, the Si content is preferably 1.00% or less, and more preferably 0.75% or less. There is no particular lower limit for the Si content, and the Si content can be 0.00% or more.

[0091] Mn: 2.00% or less If the Mn content exceeds 2.00%, corrosion resistance deteriorates. Therefore, the Mn content is preferably set to 2.00% or less, more preferably set to 1.40% or less, and even more preferably set to 1.00% or less. The lower limit of the Mn content is not particularly limited, and the Mn content may be 0.00% or more.

[0092] P: 0.045% or less P is an impurity element that segregates at grain boundaries and deteriorates corrosion resistance. Therefore, the P content is preferably 0.045% or less, and more preferably 0.030% or less. The lower limit of the P content is not particularly limited, and the P content can be 0.000% or more.

[0093] S: 0.030% or less S, like P, is an impurity element that segregates at grain boundaries and deteriorates corrosion resistance. Therefore, the S content is preferably 0.030% or less, and more preferably 0.010% or less. The lower limit of the S content is not particularly limited, and the S content can be 0.000% or more.

[0094] Ni: 12.0 to 15.0% Ni is an element that improves corrosion resistance, significantly improving stress corrosion cracking resistance, particularly in sour environments. From the viewpoint of achieving this effect, the Ni content is preferably 12.0% or more, and more preferably 12.5% ​​or more. However, because Ni is a very expensive element, adding a large amount of Ni increases costs. Therefore, from the viewpoint of balancing the effect of improving corrosion resistance and costs, the Ni content is preferably 15.0% or less, and more preferably 14.5% or less.

[0095] Cr: 16.0 to 18.0% Cr forms a highly protective oxide film on the surface of the metal, improving pitting corrosion resistance and intergranular corrosion resistance. Furthermore, when added in combination with Ni, Cr improves stress corrosion cracking resistance in sour environments. From the viewpoint of achieving these effects, the Cr content is preferably 16.0% or more, and more preferably 16.5% or more. However, from the viewpoint of the balance with Ni and other alloys, the Cr content is preferably 18.0% or less, and more preferably 17.5% or less.

[0096] Mo: 2.00 to 3.00% Mo improves pitting corrosion resistance and crevice corrosion resistance. Furthermore, Mo, when added in combination with Ni, improves stress corrosion cracking resistance in sour environments. From the viewpoint of achieving these effects, the Mo content is preferably 2.00% or more, and more preferably 2.20% or more. However, from the viewpoint of the balance with Ni and other alloys, the Mo content is preferably 3.00% or less, and more preferably 2.80% or less.

[0097] The components other than those mentioned above are Fe and unavoidable impurities.

[0098] 4. Manufacturing conditions for clad steel plate A manufacturing method for a clad steel plate according to one embodiment of the present invention includes the steps of stacking a first material plate having the above-described chemical composition and a second material plate made of a corrosion-resistant alloy to obtain a clad slab, heating the clad slab to 1050°C or more and 1200°C or less, then subjecting the clad slab to hot rolling at a rolling finish temperature of 900°C or more to obtain a clad rolled plate in which the first material plate and the second material plate are joined together to form a base steel plate and a clad plate, respectively, a step of cooling the clad rolled plate, a step of reheating the clad rolled plate to 850°C or more and 1050°C or less, a step of cooling the clad rolled plate so that the average cooling rate of the base steel plate is 2°C / s or more and 20°C / s or less, and a step of tempering the clad rolled plate to 450°C or more and 650°C or less.

[0099] In this embodiment, the temperature conditions specified as manufacturing conditions all relate to the surface temperature of the steel sheet, which can be measured using, for example, a radiation thermometer.

[0100] (4-1) Step of Obtaining a Clad Slab First, a first material plate that will become a base steel plate and a second material plate that will become a clad plate are laminated to obtain a clad slab. -4 A clad slab can be obtained by temporarily joining the first material plate and the second material plate together by, for example, electron beam welding or laser welding in an environment of a pressure of 1000 psi or less.

[0101] Furthermore, it is preferable to form a clad slab by stacking a first blank sheet, a second blank sheet, a second blank sheet, and a first blank sheet in this order, with a release material applied between the two second blank sheets. That is, a clad slab is formed by overlapping two sets of stacks, each stacking a first blank sheet and a second blank sheet, with the second blank sheets facing each other. Two clad rolled sheets are obtained by hot rolling this clad slab. After tempering, the two clad rolled sheets are peeled off via the release material to obtain a clad steel sheet that will serve as the product sheet. In this case, symmetry in the sheet thickness direction is maintained during rolling, so that warpage in the vertical direction during rolling can be suppressed.

[0102] (4-2) Clad Rolling Process Clad Slab Heating Temperature: 1050°C or More and 1200°C or Less If the clad slab heating temperature is less than 1050°C, the reduction ratio cannot be sufficiently ensured during rolling from the start of rolling after heating to the rolling end temperature described below, resulting in poor bonding between the base steel plate and the clad plate in the finally obtained clad steel plate. Furthermore, if the slab heating temperature is less than 1050°C, Nb and other elements contained in the first material plate that becomes the base steel plate are not sufficiently dissolved, making it difficult to ensure the strength of the base steel plate in the finally obtained clad steel plate. Therefore, the clad slab heating temperature is set to 1050°C or more. On the other hand, if the clad slab heating temperature exceeds 1200°C, austenite coarsens in the first material plate that becomes the base steel plate, and the structure of the base steel plate cannot be sufficiently refined in the finally obtained clad steel plate, resulting in poor toughness. Therefore, the clad slab heating temperature is set to 1200°C or less, preferably 1100°C or less.

[0103] Rolling end temperature: 900°C or higher The bondability between the base steel plate and the clad plate in a clad steel plate is ensured by rolling in a high temperature range. That is, rolling in a high temperature range reduces the deformation resistance of the base steel plate and the clad plate, forming a good bonded interface, which facilitates interdiffusion of elements at the bonded interface, thereby ensuring the bondability between the base steel plate and the clad plate. For this reason, the rolling end temperature is 900°C or higher, and preferably 950°C or higher. There is no particular upper limit to the rolling end temperature, but the rolling end temperature can be 1000°C or lower.

[0104] (4-3) Natural cooling process After the hot rolling is completed, the obtained clad rolled sheet is allowed to cool naturally. Here, natural cooling refers to a process in which the clad rolled sheet is not forcibly cooled after rolling, but is placed in a predetermined storage area such as a yard within a factory and left there to wait for the temperature of the clad rolled sheet to drop. Therefore, the cooling rate is not particularly limited. The cooling stop temperature in natural cooling may be any temperature as long as it is a temperature at which the ferrite transformation is completely completed. In practice, it is often necessary to wait for the temperature to drop to around room temperature (e.g., 25°C), but it is not necessarily required that the temperature drop to around room temperature. The cooling stop temperature in natural cooling may be, for example, 100°C or less.

[0105] (4-4) Reheating and Quenching (Reheating and Cooling) Next, reheating and quenching is carried out in which the clad rolled plate is reheated and then cooled.

[0106] Reheating temperature: 850°C or higher and 1050°C or lower First, in the reheating treatment, the naturally cooled clad rolled sheet is heated to a reheating temperature of 850°C or higher and 1050°C or lower. If the reheating temperature is lower than 850°C, ferrite is generated in the base steel sheet prior to bainite transformation, making it impossible to obtain the target strength and reducing the Charpy absorbed energy. Therefore, the reheating temperature is set to 850°C or higher, preferably 900°C or higher. On the other hand, if the reheating temperature exceeds 1050°C, coarsening of austenite grains occurs, significantly reducing low-temperature toughness. Therefore, the reheating temperature is set to 1050°C or lower, preferably 1000°C or lower.

[0107] Average cooling rate in base steel plate: 2°C / s or more and 20°C / s or less Next, the reheated clad rolled plate is subjected to a cooling treatment in which the average cooling rate in the base steel plate is 2°C / s or more and 20°C / s or less. If the average cooling rate is less than 2°C / s, ferrite transformation occurs in the base steel plate, the target strength cannot be obtained, and low-temperature toughness is significantly reduced. Therefore, the average cooling rate is 2°C / s or more, preferably 5°C / s or more. From the viewpoint of microstructural refinement and reducing hard phases that may serve as initiation points for brittle cracks, the average cooling rate is more preferably 7°C / s or more. Although there is no particular upper limit for the average cooling rate, if the average cooling rate is too high, the strength of the transformed structure may increase excessively, which may result in a decrease in Charpy absorbed energy. Therefore, from the viewpoint of preventing a decrease in Charpy absorbed energy, the average cooling rate is preferably 20°C / s or less. The average cooling rate is the temperature difference from the cooling start temperature (i.e., reheating temperature) to the cooling end temperature divided by the time required from the start of cooling to the end of cooling.

[0108] The cooling stop temperature in the reheating and quenching is preferably 200°C or less to prevent a decrease in the toughness of the base steel plate. The lower limit of the cooling stop temperature is not particularly limited, and the cooling stop temperature may be, for example, 25°C or more.

[0109] (4-5) Tempering process Tempering temperature: 450°C or higher and 650°C or lower The cooled clad rolled plate is heated for tempering. If the tempering temperature is lower than 450°C, the decomposition of island martensite and the recovery of dislocations are insufficient, resulting in a deterioration in the toughness of the base steel plate. Therefore, the tempering temperature is set to 450°C or higher. On the other hand, if the tempering temperature exceeds 650°C, precipitates such as cementite become coarse, resulting in a deterioration in the toughness of the base steel plate. Furthermore, the formation of precipitates may also deteriorate the corrosion resistance of the clad plate. Therefore, the tempering temperature is set to 650°C or lower, preferably 500°C or lower.

[0110] A clad slab was formed by stacking a first material plate (base steel plate material) having the chemical composition shown in Table 1 (the balance being Fe and unavoidable impurities) and a second material plate (clad plate material) of a corrosion-resistant alloy having the chemical composition shown in Table 2 (the balance being Fe and unavoidable impurities) in the order of the first material plate, the second material plate, the second material plate, and the first material plate in this order. The clad rolled plate was then subjected to clad rolling under the conditions shown in Table 3 to produce a clad steel plate having a thickness of 35 mm (base steel plate thickness: 32 mm, clad plate thickness: 3 mm). The cooling stop temperature for natural cooling was 30°C, and the cooling stop temperature for reheating and quenching was 30°C.

[0111] Test pieces for tensile tests and DWTT tests were taken from the clad steel plates thus obtained. The tensile tests were carried out in accordance with API-5L to determine the tensile strength TS and yield strength YS. The DWTT tests were carried out in accordance with API-5L at a test temperature of -30°C, and the ductile fracture surface area ratio DWTTSA was measured. -30℃ The results are shown in Table 4. Tensile strength and ductile fracture surface area ratio DWTTSA -30℃ The target values ​​are as follows: Tensile strength: 535 MPa or more Ductile fracture surface ratio: DWTTSA -30℃ : 85% or more

[0112] Furthermore, an HIC test was conducted in accordance with NACE Standard TM0284-2003, and the HIC resistance of the base steel plate was evaluated by the crack area ratio (CAR). The target value for the crack area ratio (CAR) is as follows: Crack area ratio (CAR): 5.0% or less (1.0% or less is particularly excellent). The crack area ratio (CAR) is measured using a hydrogen sulfide saturated solution of 5 mass% NaCl + 0.5 mass% CH 3 Three test pieces taken from the same steel plate were immersed in a COOH aqueous solution for 96 hours, and then the test pieces were subjected to ultrasonic testing to detect defects. The evaluation was based on the maximum crack area ratio (CAR) measured for the three test pieces. The results are shown in Table 4.

[0113] Furthermore, the area ratio and average grain size of bainite were measured at the half-thickness position in the thickness direction of the base steel plate by the above-mentioned method. These results are shown in Table 4.

[0114] From Table 4, all of the invention examples that satisfy claim 1 have a tensile strength of 535 MPa or more and a ductile fracture surface area ratio DWTTSA -30℃ In addition, all of the invention examples satisfying claim 2 have a tensile strength of 535 MPa or more and a ductile fracture surface area ratio DWTTSA of 85% or more. -30℃ On the other hand, none of the comparative examples shown in Table 4 achieved the desired properties.

[0115]

[0116]

[0117]

[0118]

[0119] The clad steel plate produced by the present invention is extremely useful industrially because it exhibits excellent low-temperature toughness when applied to line pipes for transporting oil or natural gas, which are exposed to severe corrosive environments.

Claims

1. Containing, by mass%, the following: C: 0.020% or more and 0.100% or less, Si: 0.10% or more and 0.50% or less, Mn: 0.75% or more and 1.80% or less, P: 0.015% or less, S: 0.0030% or less, Al: 0.01% or more and 0.07% or less, Nb: 0.005% or more and 0.080% or less, Ti: 0.005% or more and 0.030% or less, N: 0.0010% or more and 0.0060% or less, and O (oxygen): 0.0030% or less, and further containing: Cu: 0.50% or less, Ni: 0.50% or less, Cr: 0.50% or less, Mo: 0.50% or less, V: 0.100% or less, and Ca: 0.0040% or less, and having a component composition in which Ceq defined by the following formula (1) is 0.40 to 0.50, with the balance being Fe and unavoidable impurities; preparing a second material plate made of a corrosion-resistant alloy; stacking the first material plate and the second material plate to obtain a clad slab; heating the clad slab to 1050°C to 1200°C; thereafter, hot rolling the clad slab at a rolling end temperature of 900°C or more to obtain a clad rolled plate in which the first material plate and the second material plate are joined together to become a base steel plate and a clad material plate, respectively; cooling the clad rolled plate; and thereafter, reheating the clad rolled plate to 850°C to 1050°C. Thereafter, the method for producing a clad steel plate includes a step of cooling the clad rolled plate so that the average cooling rate of the base steel plate is 2°C / s or more and 20°C / s or less, and a step of tempering the clad rolled plate to 450°C or more and 650°C or less, thereby producing a clad steel plate in which the clad plate is bonded to one side of the base steel plate. Ceq=C+Mn / 6+(Cu+Ni) / 15+(Cr+Mo+V) / 5 ... (1) The element symbols in formula (1) represent the content (mass%) of each element, and zero is substituted if the element is not contained.

2. In the composition of the first material plate, the Ca content is, in mass%, 0.0005% or more and 0.0040% or less, the ACR defined by the following formula (2) is 1.00 or more and 6.00 or less, and the P defined by the following formula (3) is HIC The method for producing a clad steel plate according to claim 1, wherein ACR={Ca-(0.18+130Ca)×O} / (1.25S) (2) is less than 1.

250. HIC = 4.46C + 2.37Mn / 6 + (1.18Cr + 1.95Mo + 1.74V) / 5 + (1.74Cu + 1.7Ni) / 15 + 22.36P (3) The element symbols in formulas (2) and (3) indicate the content (mass%) of each element, and zero is substituted when the element is not contained.

3. The method for producing a clad steel plate according to claim 1 or 2, wherein the corrosion-resistant alloy is a Ni-based alloy selected from the group consisting of Alloy 825 and Alloy 625, or an austenitic stainless steel.

4. A method for manufacturing a clad steel plate as described in any one of claims 1 to 3, wherein the clad slab is formed by stacking the first material plate, the second material plate, the second material plate, and the first material plate in that order, with a release material being applied between the two second material plates, thereby obtaining two clad rolled plates by hot rolling, and after the tempering, the two clad rolled plates are peeled off via the release material.

Citation Information

Patent Citations

  • Ni ALLOY CLAD STEEL SHEET EXCELLENT IN LOW TEMPERATURE TOUGHNESS AND HAZ TOUGHNESS OF BASE MATERIAL AND CORROSION RESISTANCE OF CLADDING MATERIAL, AND METHOD OF PRODUCING THE SAME

    JP2015086422A

  • Austenitic stainless clad steel plate excellent in low temperature toughness of base material and HAZ toughness, and corrosion resistance of cladding metal and production method of the same

    JP2015105399A

  • Ni ALLOY CLAD STEEL SHEET EXCELLENT IN LOW TEMPERATURE TOUGHNESS AND HAZ TOUGHNESS OF BASE MATERIAL AND CORROSION RESISTANCE OF CLADDING METAL AND MANUFACTURING METHOD THEREFOR

    JP2015117408A

  • Clad steel sheet and method for producing same

    WO2018181381A1

  • Clad steel sheet and production method thereof

    WO2020004410A1

Cited By

  • Production method of nickel-based composite pipeline steel plate

    CN119307699A