Adhesive sheet for flexible devices, flexible laminate and flexible device

The pressure-sensitive adhesive sheet addresses color unevenness and adhesive issues in flexible displays by using an adhesive layer with specific properties and composition, ensuring strong adhesion and maintaining display quality even when bent repeatedly.

WO2024203781A1PCT designated stage expired Publication Date: 2024-10-03LINTEC CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011167
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-21
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Flexible displays experience color unevenness and adhesive issues when bent repeatedly due to changes in the optical properties of the adhesive layer, leading to a decline in display quality and potential lifting or peeling of the adhesive layer.

Method used

A pressure-sensitive adhesive sheet with an adhesive layer having a storage modulus of 0.12 MPa or less, a CIE1976 L* a* b* Lightness of 95 or less, and a recovery rate of 80% or more, which includes a colorant such as a black pigment, and is composed of an acrylic adhesive with specific monomer units and a crosslinking agent, to maintain adhesion and suppress color unevenness.

Benefits of technology

The solution effectively suppresses color unevenness and adhesive lifting at bent portions, maintaining the design integrity and display quality of flexible displays while ensuring strong adhesion and flexibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011167_03102024_PF_FP_ABST
    Figure JP2024011167_03102024_PF_FP_ABST
Patent Text Reader

Abstract

[Problem] To provide an adhesive sheet in which lifting and separation of an adhesive layer in a bent part are suppressed and color unevenness in the bent part is suppressed without impairing the designability of a flexible display in cases where the adhesive sheet is used for bonding of a flexible member, or the like. [Solution] An adhesive sheet for flexible devices, the adhesive sheet having an adhesive layer for bonding a first flexible member and a second flexible member to each other, wherein: the adhesive layer has a storage elastic modulus of 0.12 MPa or less at 23°C; the lightness L* of the adhesive layer as defined by the CIE 1976 L*a*b* color system is 95 or less; the restoration rate of the adhesive layer is 80% or more; and the adhesive force of the adhesive layer is 4 N / 25 mm or more, or the gel fraction of the adhesive layer is 84% or less.
Need to check novelty before this filing date? Find Prior Art

Description

Adhesive sheet for flexible devices, flexible laminate and flexible device

[0001] The present invention relates to a pressure-sensitive adhesive sheet for flexible devices, a flexible laminate, and a flexible device.

[0002] A display member having a liquid crystal element, a light-emitting diode (LED) element, an organic electroluminescence (organic EL) element, or the like is laminated with another member (for example, a protective panel for protecting the display member, or the like) to form a display (display) of a device such as an electronic device. Such a laminate of a display member and another member is generally formed by bonding the display member and the other member together using an adhesive layer of an adhesive sheet.

[0003] In recent years, bendable displays, so-called flexible displays, have been proposed as displays for electronic devices. Flexible displays are expected to have a wide range of applications, for example, as stationary displays that are curved and installed on a cylindrical pillar, or as mobile displays that can be folded or rolled up for portability.

[0004] Examples of types of flexible displays include organic electroluminescence (organic EL) displays, electrophoretic displays (electronic paper), and liquid crystal displays that use a plastic film as a substrate.

[0005] Examples of such flexible displays include displays that are bent during molding and maintained in a bent state, and displays that are repeatedly bent during use.

[0006] Patent Document 1 discloses an adhesive sheet having an adhesive layer for bonding one flexible member to another flexible member that constitutes a flexible display.

[0007] JP 2018-45213 A

[0008] Such flexible displays are required to have improved design as a display in order to increase their commercial value. One method to satisfy such a requirement is to make the boundaries between the components constituting the flexible display less visible when the display is turned off, in order to give a sense of unity between the display and its peripheral components, such as a frame material, i.e., to make the display seamless.

[0009] One possible solution to satisfy this seamlessness requirement is to color the adhesive used to bond the components that make up the flexible display, which would improve the seamlessness of the flexible display made up of multiple components and thereby enhance its design.

[0010] On the other hand, as described above, flexible displays are intended to be bent. The present inventors have found that, particularly at bent portions of flexible displays that are repeatedly bent during use, the optical properties of the adhesive change due to bending, causing unintended coloring of image-forming light as it passes through the bent portions, resulting in color unevenness in the displayed image.

[0011] Such color unevenness can lead to problems such as a decrease in display quality.

[0012] The present invention has been made in consideration of the above-described circumstances, and aims to provide an adhesive sheet that, even when used for bonding flexible materials, does not impair the design of a flexible display, suppresses lifting or peeling of the adhesive layer at bent portions, and suppresses color unevenness at bent portions.

[0013] The aspects of the present invention are as follows.

[0014] [1] A pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer for bonding a first flexible member and a second flexible member, wherein the pressure-sensitive adhesive layer has a storage modulus of 0.12 MPa or less at 23°C, and the pressure-sensitive adhesive layer has a CIE1976L * a * b * Lightness L defined by the color system *The adhesive sheet for flexible devices has a viscosity of 95 or less, an adhesive strength of the adhesive layer of 4 N / 25 mm or more, and a recovery rate of the adhesive layer of 80% or more.

[0015] [2] A pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer for bonding a first flexible member and a second flexible member, wherein the pressure-sensitive adhesive layer has a storage modulus of 0.12 MPa or less at 23°C, and the pressure-sensitive adhesive layer has a CIE1976L * a * b * Lightness L defined by the color system * the gel fraction of the pressure-sensitive adhesive layer is 84% ​​or less; and the recovery rate of the pressure-sensitive adhesive layer is 80% or more.

[0016] [3] The pressure-sensitive adhesive sheet for flexible devices according to [1] or [2], wherein the pressure-sensitive adhesive layer contains a colorant.

[0017] [4] The pressure-sensitive adhesive sheet for flexible devices according to [3], wherein the colorant is a black pigment or dye.

[0018] [5] The pressure-sensitive adhesive sheet for flexible devices according to any one of [1] to [4], wherein the pressure-sensitive adhesive layer has a haze value of 80% or less.

[0019] [6] The pressure-sensitive adhesive sheet for flexible devices according to any one of [1] to [5], wherein the pressure-sensitive adhesive layer has a total light transmittance of 3% or more.

[0020] [7] The pressure-sensitive adhesive sheet for flexible devices according to any one of [1] to [6], wherein the pressure-sensitive adhesive layer has a gel fraction of 30% or more.

[0021] [8] The pressure-sensitive adhesive sheet for flexible devices according to any one of [1] to [7], wherein the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer is an acrylic pressure-sensitive adhesive.

[0022] [9] The pressure-sensitive adhesive sheet for flexible devices according to [8], wherein the acrylic pressure-sensitive adhesive contains a (meth)acrylic acid ester polymer and a crosslinking agent.

[0023]

[10] The pressure-sensitive adhesive sheet for flexible devices according to [9], wherein the (meth)acrylic acid ester polymer contains an aromatic ring-containing monomer as a monomer unit constituting the (meth)acrylic acid ester polymer.

[0024]

[11] The pressure-sensitive adhesive sheet for flexible devices according to [9] or

[10] , wherein the (meth)acrylic acid ester polymer contains a reactive functional group-containing monomer as a monomer unit constituting the (meth)acrylic acid ester polymer.

[0025]

[12] A flexible material laminate comprising a first flexible material, a second flexible material, and an adhesive layer that bonds the first flexible material and the second flexible material to each other, wherein the adhesive layer is an adhesive layer that is included in the adhesive sheet for flexible devices according to any one of [1] to

[11] .

[0026]

[13] A flexible device comprising the flexible material laminate according to

[12] .

[0027] According to the present invention, an adhesive sheet can be provided that, even when used for bonding flexible materials, does not impair the design of a flexible display, suppresses lifting or peeling of the adhesive layer at bent portions, and suppresses color unevenness at bent portions.

[0028] Fig. 1 is a cross-sectional view of a pressure-sensitive adhesive sheet according to one embodiment of the present invention. Fig. 2 is a cross-sectional view of a flexible material laminate according to one embodiment of the present invention. Fig. 3 is a cross-sectional view of a flexible device according to one embodiment of the present invention. Fig. 4 is a schematic view for explaining a static bending test in the examples. Fig. 5 is a schematic view for explaining the amount of deformation of a test piece in a static bending test in the examples. Fig. 6 is a schematic view for explaining the amount of deformation of a test piece in a dynamic bending test in the examples.

[0029] The present invention will be described in detail below based on specific embodiments.

[0030] (1. Adhesive Sheet for Flexible Devices) As shown in FIG. 1 , the adhesive sheet 1 for flexible devices according to this embodiment has an adhesive layer 10 having a predetermined brightness, a first release sheet 11, and a second release sheet 12. That is, in this embodiment, the adhesive layer 10 is colored. The adhesive constituting the adhesive layer 10 will be described later. Two release sheets (first release sheet 11 and second release sheet 12) support the adhesive layer 10, and are arranged so that their release surfaces contact both main surfaces 10a, 10b of the adhesive layer, making them releasable from the adhesive layer. In other words, the adhesive layer 10 is releasably sandwiched between the two release sheets (first release sheet 11 and second release sheet 12). In this specification, the release surface of the release sheet refers to the surface of the release sheet that has releasability, and includes both a surface that has been subjected to a release treatment and a surface that exhibits releasability even without being subjected to a release treatment. Release sheets will be described later.

[0031] The pressure-sensitive adhesive sheet according to this embodiment is used to bond a first member and a second member, and is particularly suitable for use in bonding bendable members (flexible members).

[0032] A flexible member is a member that maintains its function even when bent, such as folded. Examples of flexible members include a member that is molded to bend during the manufacture of a device that includes the flexible member and that maintains its bent state, and a member that is repeatedly bent during the use of a device that includes the flexible member.

[0033] Here, the design is enhanced by providing a sense of unity between the display frame and the display when the display is turned off. One known method for enhancing the design is to color the adhesive used to bond the components that make up the display.

[0034] When this method is applied to a flexible display made of a flexible member, the adhesive will bend along with the flexible member when the flexible display is bent. In particular, flexible displays that are repeatedly bent during use will be bent many times.

[0035] The inventors have discovered that the optical properties of the adhesive at the bent portion of such a flexible display may change due to bending. When the optical properties of the adhesive change, when an image generated on the flexible display passes through the adhesive and is observed by a user, the light forming the image may be unintentionally colored a different color from its original color. When this coloring occurs, even if the same color is displayed, the color at the bent portion is observed as a color unevenness that differs from the color in other portions. This results in a deterioration of the display quality.

[0036] Such changes in the optical properties of the adhesive are thought to be the result of some change in the physical properties of the adhesive caused by repeated bending.

[0037] Therefore, in order to suppress color unevenness at the bent portion of a flexible display, it is necessary to suppress the changes in the physical properties of the adhesive caused by repeated bending.

[0038] To address the above-mentioned problems, in the pressure-sensitive adhesive sheet according to this embodiment, the physical properties of the pressure-sensitive adhesive layer having a predetermined brightness are controlled. The components of the pressure-sensitive adhesive sheet according to this embodiment will be described in detail below.

[0039] (1.1. Adhesive Layer) The adhesive layer having a predetermined brightness bonds the first member and the second member. In this embodiment, the adhesive layer preferably bonds the first flexible member and the second flexible member.

[0040] The pressure-sensitive adhesive layer may be composed of one layer (single layer) or two or more layers. When the pressure-sensitive adhesive layer has multiple layers, these multiple layers may be the same or different from each other, and the combination of layers constituting these multiple layers is not particularly limited.

[0041] In this embodiment, the adhesive layer has the following physical properties, so that the design of the flexible device in which the first flexible member and the second flexible member are bonded together is not impaired, lifting or peeling of the adhesive layer at the bent portion is suppressed, and color unevenness at the bent portion is effectively suppressed.

[0042] The thickness of the pressure-sensitive adhesive layer 10 is preferably 5 to 1000 μm, more preferably 10 to 500 μm, even more preferably 20 to 250 μm, particularly preferably 30 to 100 μm, and most preferably 40 to 70 μm. This provides adhesiveness that allows the first flexible member and the second flexible member to be bonded well, and thus excellent flexibility. In particular, lifting and peeling of the pressure-sensitive adhesive layer at bent portions is suppressed, and color unevenness at bent portions is easily and effectively suppressed.

[0043] (1.2. Physical Properties of Pressure-Sensitive Adhesive Layer) In this embodiment, the pressure-sensitive adhesive layer 10 has the following physical properties.

[0044] (1.2.1. Storage modulus of pressure-sensitive adhesive layer) In this embodiment, the storage modulus (G') of the pressure-sensitive adhesive layer at 23°C and a frequency of 1 Hz is preferably 0.12 MPa or less. The storage modulus is one index of the ease of deformation (hardness) of the pressure-sensitive adhesive layer. This allows the pressure-sensitive adhesive layer to sufficiently conform to bending even when repeatedly bent, and prevents lifting or peeling from the member to which it is attached.

[0045] From the above viewpoints, the storage modulus of the pressure-sensitive adhesive layer is preferably 0.001 to 0.12 MPa, more preferably 0.003 to 0.1 MPa, even more preferably 0.005 to 0.09 MPa, particularly preferably 0.01 to 0.08 MPa, and of these, preferably 0.02 to 0.07 MPa, most preferably 0.03 to 0.05 MPa. The storage modulus of the pressure-sensitive adhesive layer can be adjusted, for example, by changing the composition of the pressure-sensitive adhesive (the type and amount of reactive functional groups, the molecular structure and glass transition temperature of the monomer composition used, etc.), the molecular weight of the materials constituting the pressure-sensitive adhesive, etc.

[0046] The storage modulus (G') may be measured by a known method. For example, the pressure-sensitive adhesive layer is prepared into a sample of a predetermined size, and the sample is strained at a predetermined frequency within a predetermined temperature range using a dynamic viscoelasticity measuring device to measure the modulus. From the measured modulus, the storage modulus under the above conditions can be calculated.

[0047] (1.2.2. Adhesion strength of adhesive layer) In this embodiment, the adhesive strength of the adhesive layer to soda lime glass is preferably 4 N / 25 mm or more. This ensures sufficient adhesion to the adherend to which it is attached, provides excellent repeated bending resistance, and suppresses peeling of the adhesive layer from the attached member. From the above perspectives, the adhesive strength is more preferably 4 to 100 N / 25 mm, even more preferably 6 to 50 N / 25 mm, particularly preferably 8 to 30 N / 25 mm, and of these, 10 to 20 N / 25 mm is preferred. A method for measuring the adhesive strength of the adhesive layer will be described in detail in the Examples below.

[0048] (1.2.3. Restoration rate of pressure-sensitive adhesive layer) The restoration rate of the pressure-sensitive adhesive layer according to this embodiment is preferably 80% or more. The restoration rate indicates the percentage of recovery of the state of the pressure-sensitive adhesive layer 60 seconds after the pressure-sensitive adhesive layer is released in a bent state compared to the state of the pressure-sensitive adhesive layer when it is not bent. In other words, when the state of the pressure-sensitive adhesive layer 60 seconds after the pressure-sensitive adhesive layer is released in a bent state is the same as the state of the pressure-sensitive adhesive layer when it is not bent, the restoration rate is 100%.

[0049] By having the recovery rate within the above range, the bent state of the adhesive layer is close to the unbent state, changes in the properties of the adhesive layer due to bending are suppressed, and color unevenness in the bent portion can be suppressed.

[0050] The lower limit of the restoration rate of the pressure-sensitive adhesive layer is preferably 84% or more, more preferably 88% or more, even more preferably 92% or more, and particularly preferably 95% or more, while the upper limit of the restoration rate of the pressure-sensitive adhesive layer is usually preferably 100%.

[0051] The recovery rate of the pressure-sensitive adhesive layer can be adjusted, for example, by changing the composition of the pressure-sensitive adhesive (the type and amount of reactive functional groups, the molecular structure and glass transition temperature of the monomer composition used, etc.), the molecular weight of the material constituting the pressure-sensitive adhesive, etc. Specific measurement methods will be described in detail in the Examples below.

[0052] (1.2.4. Lightness and chromaticity of pressure-sensitive adhesive layer) The CIE1976L * a * b * Lightness L defined by the color system * is preferably 95 or less. This makes it possible to color the pressure-sensitive adhesive layer, making the boundary between the display portion and the peripheral member (for example, a frame material) less visible, and to easily impart a sense of unity between the display portion and the peripheral member (seamlessness).

[0053] From the above viewpoint, the lightness L * is preferably 1 to 92, more preferably 10 to 88, further preferably 30 to 84, particularly preferably 50 to 80, and among these, 50 to 74 is preferred.

[0054] CIE1976L * a * b * Chromaticity a defined by the color system * is preferably −30 to 30, more preferably −15 to 15, particularly preferably −5 to 5, further preferably −2 to 2, and most preferably −1 to 1. * a * b * Chromaticity b defined by the color system * , preferably -30 to 30, more preferably -18 to 18, particularly preferably -10 to 10, further preferably -3 to 3, and most preferably -1.5 to 1.5. * and chromaticity b * When the thickness is within the above range, the visibility of the image displayed on the flexible device is good.

[0055] (1.2.5. Total Light Transmittance of Pressure-Sensitive Adhesive Layer) The total light transmittance of the pressure-sensitive adhesive layer according to this embodiment is preferably 3% or more, more preferably 10% or more, particularly preferably 30% or more, and even more preferably 40% or more. This improves the visibility of the display unit. The upper limit of the total light transmittance is usually 100% or less, but the upper limit of the lightness L * From the viewpoint of easily satisfying the above, it is preferably 97% or less, more preferably 90% or less, particularly preferably 80% or less, even more preferably 70% or less, and among these, it is preferably 60% or less, and most preferably 52% or less.

[0056] (1.2.6. Haze Value of Pressure-Sensitive Adhesive Layer) The haze value of the pressure-sensitive adhesive layer according to this embodiment is preferably 80% or less, more preferably 60% or less, particularly preferably 40% or less, even more preferably 25% or less, and particularly preferably 15% or less, most preferably 10% or less. This makes it easier to control the total light transmittance of the pressure-sensitive adhesive layer within the above range, and also makes it easier to impart a sense of unity between the display unit and peripheral components (e.g., frame material) in a flexible display. The lower limit of the haze value is typically 0%. The haze value in this specification is a value measured in accordance with JIS K7136:2000.

[0057] The optical properties (brightness, chromaticity, total light transmittance, haze value, etc.) of the pressure-sensitive adhesive can be adjusted, for example, by changing the type and content of the colorant described below, the composition of the pressure-sensitive adhesive, etc. The method for measuring the optical properties of the pressure-sensitive adhesive will be described in detail in the examples described below.

[0058] (1.2.7. Gel fraction of pressure-sensitive adhesive layer) The gel fraction of the pressure-sensitive adhesive layer according to this embodiment is preferably 30% or more and 84% or less. This allows the pressure-sensitive adhesive to exhibit suitable cohesive strength that can withstand repeated bending. As a result, the repeated bending property described above is more excellent.

[0059] From the above viewpoints, the gel fraction of the pressure-sensitive adhesive layer is more preferably 34 to 80%, particularly preferably 38 to 75%, even more preferably 42 to 70%, and of these, preferably 45 to 66%. The method for measuring the gel fraction of the pressure-sensitive adhesive will be described in detail in the Examples below.

[0060] (1.3. Composition of Pressure-Sensitive Adhesive) As long as the pressure-sensitive adhesive layer has the above-described physical properties, the composition of the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer is not particularly limited. For example, it may be any of an acrylic pressure-sensitive adhesive, a polyester pressure-sensitive adhesive, a polyurethane pressure-sensitive adhesive, a rubber pressure-sensitive adhesive, a silicone pressure-sensitive adhesive, etc. Furthermore, the pressure-sensitive adhesive may be any of an emulsion type, a solvent type, or a solventless type. Furthermore, the pressure-sensitive adhesive may or may not have a cross-linked structure. Furthermore, the pressure-sensitive adhesive may be active energy ray-curable or non-active energy ray-curable.

[0061] In this embodiment, from the viewpoint of ease of realizing the above-mentioned physical properties, and from the viewpoint of adhesive properties, optical properties, etc., an acrylic adhesive is preferred as the adhesive, and an acrylic adhesive having a crosslinked structure is more preferred.

[0062] Specifically, the adhesive is preferably an adhesive obtained by crosslinking an adhesive composition (hereinafter sometimes referred to as "adhesive composition P") containing a (meth)acrylic acid ester polymer (A) and a crosslinking agent (B). Such an adhesive is likely to satisfy the above-mentioned physical properties and easily obtain good adhesive strength. Furthermore, from the perspective of the SDGs, the adhesive may be made of a material with a high biomass content, a material that can be recycled or reused, or a recycled or reused material. In this specification, (meth)acrylic acid means both acrylic acid and methacrylic acid. The same applies to other similar terms. Furthermore, the term "polymer" also includes the concept of "copolymer."

[0063] (1.3.1. (Meth)acrylic acid ester polymer (A)) The (meth)acrylic acid ester polymer (A) preferably contains, as monomer units constituting the polymer, a (meth)acrylic acid alkyl ester and a monomer having a reactive functional group in the molecule (reactive functional group-containing monomer). This makes it easier to obtain a pressure-sensitive adhesive having a crosslinked structure and good adhesiveness.

[0064] Furthermore, the (meth)acrylic acid ester polymer (A) preferably contains an aromatic ring-containing monomer as a monomer unit constituting the polymer, which makes it easier to obtain the above-mentioned physical properties.

[0065] Furthermore, the (meth)acrylic acid ester polymer (A) preferably contains a nitrogen atom-containing monomer as a monomer unit constituting the polymer, which makes it easier to obtain the above-mentioned physical properties.

[0066] Therefore, the (meth)acrylic acid ester polymer (A) preferably contains, as monomer units constituting the polymer, a (meth)acrylic acid alkyl ester, a reactive functional group-containing monomer, and an aromatic ring-containing monomer, and also preferably contains a (meth)acrylic acid alkyl ester, a reactive functional group-containing monomer, an aromatic ring-containing monomer, and a nitrogen atom-containing monomer.

[0067] By including a (meth)acrylic acid alkyl ester, the resulting pressure-sensitive adhesive can exhibit desirable adhesiveness. As the (meth)acrylic acid alkyl ester, a (meth)acrylic acid alkyl ester having an alkyl group having 1 to 20 carbon atoms is preferred. The alkyl group may be linear or branched, or may have a cyclic structure.

[0068] Examples of (meth)acrylic acid alkyl esters having an alkyl group containing 1 to 20 carbon atoms include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, n-decyl (meth)acrylate, n-dodecyl (meth)acrylate, myristyl (meth)acrylate, palmityl (meth)acrylate, and stearyl (meth)acrylate.

[0069] Among these, from the viewpoint of physical properties related to the storage modulus G' at 23°C, (meth)acrylic acid esters having an alkyl group with 1 to 8 carbon atoms are preferred, and (meth)acrylic acid esters having an alkyl group with 4 to 8 carbon atoms are particularly preferred. Specifically, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and n-octyl (meth)acrylate are preferred, and n-butyl acrylate, 2-ethylhexyl acrylate, and n-octyl acrylate are particularly preferred. These may be used alone or in combination of two or more.

[0070] The (meth)acrylic acid ester polymer (A) preferably contains 60 to 99.9 mass% of (meth)acrylic acid alkyl esters, the alkyl group of which has 1 to 20 carbon atoms, as monomer units constituting the polymer. This allows the (meth)acrylic acid ester polymer (A) to have suitable adhesive properties, and also makes it easy to adjust the storage modulus G' of the resulting pressure-sensitive adhesive to a lower value. Furthermore, it is possible to incorporate desired amounts of other monomer components into the (meth)acrylic acid ester polymer (A), making it easier to design pressure-sensitive adhesives that exhibit desired performance.

[0071] The (meth)acrylic acid ester polymer (A) contains a reactive functional group-containing monomer as a monomer unit constituting the polymer, and thus the (meth)acrylic acid ester polymer (A) reacts with the crosslinking agent (B) described below via the reactive functional group derived from the reactive functional group-containing monomer, forming a crosslinked structure (three-dimensional network structure) in the pressure-sensitive adhesive. As a result, a pressure-sensitive adhesive having the desired cohesive strength is obtained, and the pressure-sensitive adhesive is likely to satisfy the above-mentioned physical properties.

[0072] Preferred examples of reactive functional group-containing monomers include monomers having a hydroxyl group in the molecule (hydroxyl group-containing monomers), monomers having a carboxyl group in the molecule (carboxyl group-containing monomers), and monomers having an amino group in the molecule (amino group-containing monomers). These reactive functional group-containing monomers may be used alone or in combination of two or more. Among these, hydroxyl group-containing monomers or carboxyl group-containing monomers are preferred, and hydroxyl group-containing monomers are particularly preferred. By including a hydroxyl group-containing monomer, the physical properties related to the storage modulus G' described above are more likely to be satisfied, and fine adjustment of the storage modulus G' is also facilitated.

[0073] Examples of hydroxyl group-containing monomers include (meth)acrylic acid hydroxyalkyl esters such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. Among these, from the viewpoint of easily achieving the physical properties related to the storage modulus G' described above, (meth)acrylic acid hydroxyalkyl esters having a hydroxyalkyl group having 1 to 4 carbon atoms are preferred. Specific examples include 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate, and particularly 2-hydroxyethyl acrylate or 4-hydroxybutyl acrylate. These may be used alone or in combination of two or more.

[0074] Examples of the carboxyl group-containing monomer include ethylenically unsaturated carboxylic acids such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, itaconic acid, and citraconic acid. Among these, acrylic acid is preferred from the viewpoint of the adhesive strength of the resulting (meth)acrylic acid ester polymer (A). These may be used alone or in combination of two or more.

[0075] The (meth)acrylic acid ester polymer (A) preferably contains 0.1 to 30 mass %, more preferably 0.3 to 20 mass %, even more preferably 0.6 to 10 mass %, particularly preferably 0.8 to 5 mass %, and even more preferably 0.9 to 2 mass %, of the reactive functional group-containing monomer as a monomer unit constituting the polymer. This ensures that the cohesive strength of the pressure-sensitive adhesive obtained by the crosslinking reaction with the crosslinking agent (B) is appropriate, and the above-mentioned physical properties are likely to be satisfied.

[0076] It is also preferable that the (meth)acrylic acid ester polymer (A) does not contain a carboxy group-containing monomer as a monomer unit constituting the polymer. Since a carboxy group is an acid component, by not containing a carboxy group-containing monomer, even when the target to which the pressure-sensitive adhesive is applied includes a material that is susceptible to problems caused by acid, such as a transparent conductive film such as tin-doped indium oxide (ITO), a metal film, or a metal mesh, problems caused by acid (corrosion, resistance change, etc.) can be suppressed.

[0077] Here, "not containing a carboxy group-containing monomer" means that the carboxy group-containing monomer is substantially not contained, and includes not only the case where the carboxy group-containing monomer is not contained at all, but also the case where the carboxy group-containing monomer is contained to an extent that the carboxy group does not cause corrosion of the transparent conductive film, metal wiring, etc. Specifically, the (meth)acrylic acid ester polymer (A) may contain the carboxy group-containing monomer as a monomer unit in an amount of 0.1 mass % or less, preferably 0.01 mass % or less, and more preferably 0.001 mass % or less.

[0078] Examples of aromatic ring-containing monomers include phenyl (meth)acrylate, 2-phenylethyl (meth)acrylate, benzyl (meth)acrylate, naphthyl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, phenoxybutyl (meth)acrylate, ethoxylated-o-phenylphenol acrylate, phenoxydiethylene glycol (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate, biphenyl di(meth)acrylate, pentafluorobenzyl (meth)acrylate, etc. Among these, from the viewpoint of easily satisfying the above-mentioned physical properties, phenyl (meth)acrylate, 2-phenylethyl (meth)acrylate, benzyl (meth)acrylate, naphthyl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, and phenoxybutyl (meth)acrylate are preferred, and from the viewpoint of easily achieving favorable recovery, 2-phenoxyethyl (meth)acrylate is more preferred, and 2-phenoxyethyl acrylate is particularly preferred. These may be used alone or in combination of two or more.

[0079] The (meth)acrylic acid ester copolymer (A) preferably contains, as a monomer unit constituting the polymer, an aromatic ring-containing monomer in an amount of 0.1 to 30% by mass, more preferably 0.4 to 20% by mass, even more preferably 0.8 to 10% by mass, particularly preferably 1.2 to 6% by mass, and of these, 1.5 to 3% by mass is preferred. By setting the content of the aromatic ring-containing monomer within the above range, the above-mentioned physical properties are likely to be satisfied.

[0080] The nitrogen atom-containing monomer may be a monomer having an amino group, a monomer having an amide group, or a monomer having a nitrogen-containing heterocycle, among which a monomer having a nitrogen-containing heterocycle is preferred.In addition, from the viewpoint of increasing the degree of freedom of the nitrogen atom-containing monomer-derived portion in the higher-order structure of the pressure-sensitive adhesive, it is preferred that the nitrogen atom-containing monomer does not contain a reactive unsaturated double bond group other than one polymerizable group used in polymerization to form the (meth)acrylic acid ester polymer (A).The nitrogen atom-containing monomer may be used alone or in combination of two or more.

[0081] Examples of the monomer having an amino group include monomethylaminoethyl (meth)acrylate, monoethylaminoethyl (meth)acrylate, monomethylaminopropyl (meth)acrylate, monoethylaminopropyl (meth)acrylate, and dimethylaminoethyl (meth)acrylate.

[0082] Examples of monomers having an amide group include (meth)acrylamide, N-methyl(meth)acrylamide, N-methylol(meth)acrylamide, N-tert-butyl(meth)acrylamide, N,N-dimethyl(meth)acrylamide, N-ethyl(meth)acrylamide, N,N-dimethylaminopropyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N-phenyl(meth)acrylamide, N-(n-butoxymethyl)(meth)acrylamide, dimethylaminopropyl(meth)acrylamide, and N-vinylcaprolactam.

[0083] Examples of monomers having a nitrogen-containing heterocycle include N-(meth)acryloylmorpholine, N-vinyl-2-pyrrolidone, N-(meth)acryloylpyrrolidone, N-(meth)acryloylpiperidine, N-(meth)acryloylpyrrolidine, N-(meth)acryloylaziridine, aziridinylethyl (meth)acrylate, 2-vinylpyridine, 4-vinylpyridine, 2-vinylpyrazine, 1-vinylimidazole, N-vinylcarbazole, and N-vinylphthalimide. Among these, N-(meth)acryloylmorpholine is preferred, and N-acryloylmorpholine is particularly preferred.

[0084] The (meth)acrylic acid ester polymer (A) preferably contains, as a monomer unit constituting the polymer, a nitrogen atom-containing monomer in an amount of 0.1 to 20 mass %, more preferably 0.5 to 12 mass %, and even more preferably 1 to 6 mass %, which makes it easier to satisfy the above-mentioned physical properties.

[0085] It is also preferred that the (meth)acrylic acid ester polymer (A) contains a monomer having an alicyclic structure in the molecule (alicyclic structure-containing monomer) as a monomer unit constituting the polymer. Since the alicyclic structure-containing monomer is bulky, it is presumed that the presence of this in the polymer increases the spacing between the polymers, resulting in excellent flexibility of the resulting pressure-sensitive adhesive. This improves the above-mentioned physical properties.

[0086] The carbon ring of the alicyclic structure in the alicyclic structure-containing monomer may be a saturated structure or may partially contain an unsaturated bond. The alicyclic structure may be a monocyclic alicyclic structure or a polycyclic alicyclic structure (polycyclic structure) such as a bicyclic or tricyclic structure. From the viewpoint of optimizing the distance between the resulting (meth)acrylic acid ester polymer (A) and imparting high stress relaxation properties to the PSA, the alicyclic structure is preferably a polycyclic structure. Furthermore, in consideration of the compatibility of the (meth)acrylic acid ester polymer (A) with other components, the polycyclic structure is particularly preferably a bicyclic to tetracyclic structure. Similarly, from the viewpoint of imparting stress relaxation properties and compatibility, the number of carbon atoms in the alicyclic structure (meaning the total number of carbon atoms in the ring, or the total number of carbon atoms in the case where multiple rings are present independently) is preferably 5 to 15, more preferably 7 to 10.

[0087] Specific examples of alicyclic structure-containing monomers include cyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, adamantyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, and dicyclopentenyloxyethyl (meth)acrylate. Among these, dicyclopentanyl (meth)acrylate (alicyclic structure carbon number: 10), adamantyl (meth)acrylate (alicyclic structure carbon number: 10), or isobornyl (meth)acrylate (alicyclic structure carbon number: 7) are preferred, as they exhibit superior adhesiveness, with isobornyl (meth)acrylate being more preferred, and isobornyl acrylate being particularly preferred. These may be used alone or in combination of two or more.

[0088] The (meth)acrylic acid ester polymer (A) preferably contains an alicyclic structure-containing monomer as a monomer unit constituting the polymer in an amount of 1 to 30 mass %, more preferably 4 to 24 mass %, even more preferably 8 to 18 mass %, and particularly preferably 11 to 16 mass %, which makes it easier to satisfy the above-mentioned physical properties.

[0089] In this embodiment, the (meth)acrylic acid ester polymer (A) may contain other monomers as monomer units constituting the polymer, if desired. As the other monomers, monomers that do not contain reactive functional groups are preferred so as not to inhibit the above-mentioned action of the reactive functional group-containing monomer. Examples of such monomers include (meth)acrylic acid alkoxyalkyl esters such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate, vinyl acetate, and styrene. These may be used alone or in combination of two or more.

[0090] The polymerization mode of the (meth)acrylic acid ester polymer (A) may be a random copolymer or a block copolymer.

[0091] The weight average molecular weight of the (meth)acrylic acid ester polymer (A) is preferably 200,000 to 3,000,000, more preferably 400,000 to 2,400,000, even more preferably 650,000 to 2,000,000, particularly preferably 900,000 to 1,700,000, and most preferably 1,100,000 to 1,400,000. This makes it easier for the resulting PSA to satisfy the physical properties related to the storage modulus G' described above. Note that the weight average molecular weight in this specification is a value measured by gel permeation chromatography (GPC) in terms of standard polystyrene.

[0092] In the pressure-sensitive adhesive composition P, the (meth)acrylic acid ester polymer (A) may be used alone or in combination of two or more.

[0093] (1.3.2. Crosslinking agent (B)) The crosslinking agent (B) crosslinks the (meth)acrylic acid ester polymer (A) and forms a crosslinked structure (three-dimensional network structure) when the pressure-sensitive adhesive composition P containing the crosslinking agent (B) is heated, etc. As a result, the cohesive strength of the resulting pressure-sensitive adhesive is improved, and the above-mentioned physical properties are more likely to be satisfied.

[0094] The crosslinking agent (B) may be any agent that reacts with the reactive group of the (meth)acrylic acid ester polymer (A). Examples include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, amine-based crosslinking agents, melamine-based crosslinking agents, aziridine-based crosslinking agents, hydrazine-based crosslinking agents, aldehyde-based crosslinking agents, oxazoline-based crosslinking agents, metal alkoxide-based crosslinking agents, metal chelate-based crosslinking agents, metal salt-based crosslinking agents, and ammonium salt-based crosslinking agents. Among these, it is preferable to use an isocyanate-based crosslinking agent that has excellent reactivity with reactive functional group-containing monomers. The crosslinking agent (B) may be used alone or in combination of two or more.

[0095] The isocyanate crosslinking agent contains at least a polyisocyanate compound, such as aromatic polyisocyanates such as tolylene diisocyanate, diphenylmethane diisocyanate, and xylylene diisocyanate, aliphatic polyisocyanates such as hexamethylene diisocyanate, alicyclic polyisocyanates such as isophorone diisocyanate and hydrogenated diphenylmethane diisocyanate, and biuret and isocyanurate forms thereof, as well as adducts thereof that are reaction products with low-molecular-weight active hydrogen-containing compounds such as ethylene glycol, propylene glycol, neopentyl glycol, trimethylolpropane, and castor oil.

[0096] The content of the crosslinking agent (B) in the pressure-sensitive adhesive composition P is preferably 0.01 to 2 parts by mass, more preferably 0.05 to 1 part by mass or more, even more preferably 0.08 to 0.6 parts by mass, particularly preferably 0.10 to 0.3 parts by mass, and of these, preferably 0.12 to 0.21 parts by mass, relative to 100 parts by mass of the (meth)acrylic acid ester polymer (A). This makes it easier to satisfy the above-mentioned physical properties.

[0097] (1.3.3. Colorant (C)) The pressure-sensitive adhesive composition P according to the present embodiment preferably contains a colorant (C) for coloring the pressure-sensitive adhesive layer. This allows the pressure-sensitive adhesive layer to have a high total light transmittance, a high haze value, and a high CIE 1976L * a * b * Lightness L defined by the color system * , chromaticity a * and chromaticity b * can be adjusted to a desired range, and the design of the flexible device to which the pressure-sensitive adhesive layer is attached can be improved.

[0098] The colorant may be a pigment or a dye. The pigment may be an inorganic pigment or an organic pigment. From the viewpoint of the durability of the resulting pressure-sensitive adhesive, inorganic pigments are preferred. The color of the colorant can be appropriately selected to match the color of the flexible member from the viewpoints of seamlessness, screen color, etc., but generally, a dark or deep color such as black, brown, navy blue, purple, or blue is preferred, and black is particularly preferred.

[0099] Examples of inorganic pigments include carbon black, cobalt-based pigments, iron-based pigments, chromium-based pigments, titanium-based pigments, vanadium-based pigments, zirconium-based pigments, molybdenum-based pigments, ruthenium-based pigments, platinum-based pigments, ITO (indium tin oxide)-based pigments, and ATO (antimony tin oxide)-based pigments.

[0100] Examples of organic pigments and organic dyes include aminium-based dyes, cyanine-based dyes, merocyanine-based dyes, croconium-based dyes, squarium-based dyes, azulenium-based dyes, polymethine-based dyes, naphthoquinone-based dyes, pyrylium-based dyes, phthalocyanine-based dyes, naphthalocyanine-based dyes, naphtholactam-based dyes, azo-based dyes, condensed azo-based dyes, indigo-based dyes, perinone-based dyes, perylene-based dyes, dioxazine-based dyes, quinacridone-based dyes, isoindolinone-based dyes, quinophthalone-based dyes, pyrrole-based dyes, thioindigo-based dyes, metal complex-based dyes (metal complex dyes), dithiol metal complex-based dyes, indolephenol-based dyes, triallylmethane-based dyes, anthraquinone-based dyes, dioxazine-based dyes, naphthol-based dyes, azomethine-based dyes, benzimidazolone-based dyes, pyranthrone-based dyes, and threne-based dyes.

[0101] Examples of black pigments include carbon black, copper oxide, iron oxide, manganese dioxide, aniline black, activated carbon, etc. Examples of black dyes include high-concentration vegetable dyes and azo dyes.

[0102] The above pigments or dyes can be used in appropriate mixtures so as to obtain the desired physical properties in the pressure-sensitive adhesive layer.

[0103] Among the above colorants, carbon black, nigrosine-based black dyes, and chromate-based black dyes are preferred because they are likely to satisfy the above-mentioned physical properties and from the viewpoints of seamlessness, screen color, etc. The carbon black may or may not have been subjected to a predetermined surface treatment (for example, a solvent-philic treatment).

[0104] From the viewpoint of optical properties, the colorant (C) preferably satisfies the following properties.

[0105] The colorant (C) preferably has an average haze, which is the average of the haze value at a wavelength of 780 nm and the haze value at a wavelength of 380 nm, of 0.1 to 60%, more preferably 1 to 45%, particularly preferably 2 to 30%, even more preferably 3 to 20%, and of which 4 to 10% is preferred, when a solution of the colorant diluted 10,000 times with ethyl acetate is used. By using an appropriate amount of such a colorant, the optical properties of the pressure-sensitive adhesive layer described above are more likely to be satisfied.

[0106] The colorant (C) is preferably one in which the difference between the haze value at a wavelength of 780 nm and the haze value at a wavelength of 380 nm, when the colorant is diluted 10,000 times with ethyl acetate, is 0 to 30 points, more preferably 1 to 25 points, particularly preferably 3 to 20 points, and even more preferably 6 to 16 points. By using an appropriate amount of such a colorant, the optical properties of the pressure-sensitive adhesive layer described above are more likely to be satisfied.

[0107] The haze value at a wavelength of 780 nm of a solution obtained by diluting colorant (C) 10,000 times with ethyl acetate is preferably 0.1 to 50%, more preferably 0.5 to 24%, particularly preferably 1 to 12%, and even more preferably 2 to 5%. Furthermore, the haze value at a wavelength of 380 nm of a solution obtained by diluting the colorant 10,000 times with ethyl acetate is preferably 1 to 60%, more preferably 3 to 45%, particularly preferably 6 to 30%, and even more preferably 10 to 20%. This makes it easier for the optical properties of the pressure-sensitive adhesive layer to be satisfied.

[0108] Furthermore, the standard deviation of the haze value at each wavelength in 5 nm increments in the wavelength range of 380 nm to 780 nm (i.e., 380 nm, 385 nm, 390 nm, ..., 775 nm, 780 nm) of a solution obtained by diluting colorant (C) 10,000 times with ethyl acetate is preferably 0.01 to 10, more preferably 0.1 to 8, particularly preferably 0.5 to 6, and even more preferably 1 to 5. This makes it easier for the pressure-sensitive adhesive layer to satisfy the optical properties described above.

[0109] The content of the colorant (C) relative to 100 parts by mass of the (meth)acrylic acid ester polymer (A) is preferably 0.01 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, even more preferably 0.1 to 1 part by mass, particularly preferably 0.2 to 0.8 parts by mass, and of these, preferably 0.3 to 0.6 parts by mass. This makes it easier for the pressure-sensitive adhesive layer to satisfy the optical properties described above.

[0110] (1.3.4. Silane Coupling Agent (D)) The pressure-sensitive adhesive composition P according to the present embodiment preferably contains a silane coupling agent (D). This improves adhesion to the adherend and also makes it possible to suppress lifting and peeling even when the composition is repeatedly bent.

[0111] The silane coupling agent is preferably an organosilicon compound having at least one alkoxysilyl group in the molecule, which has good compatibility with the adhesive component, particularly the (meth)acrylic acid ester polymer (A), and has optical transparency.

[0112] Examples of such silane coupling agents include polymerizable unsaturated group-containing silicon compounds such as vinyltrimethoxysilane, vinyltriethoxysilane, and methacryloxypropyltrimethoxysilane; silicon compounds having an epoxy structure such as 3-glycidoxypropyltrimethoxysilane and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; and mercapto group-containing silicon compounds such as 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, and 3-mercaptopropyldimethoxymethylsilane. Examples of such silane compounds include amino group-containing silicon compounds such as 3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, and N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-chloropropyltrimethoxysilane, and 3-isocyanatepropyltriethoxysilane, as well as condensates of at least one of these with alkyl group-containing silicon compounds such as methyltriethoxysilane, ethyltriethoxysilane, methyltrimethoxysilane, and ethyltrimethoxysilane. These compounds may be used alone or in combination of two or more.

[0113] The content of the silane coupling agent (D) relative to 100 parts by mass of the (meth)acrylic acid ester polymer (A) is preferably 0.05 to 5 parts by mass, more preferably 0.1 to 1 part by mass, even more preferably 0.15 to 0.7 parts by mass, and particularly preferably 0.18 to 0.4 parts by mass. This makes it easier to achieve the above-mentioned properties.

[0114] (1.3.5. Antistatic agent (E)) The pressure-sensitive adhesive composition P according to this embodiment also preferably contains an antistatic agent (E), which allows the pressure-sensitive adhesive layer to exhibit excellent antistatic properties.

[0115] The antistatic agent may be any agent capable of imparting antistatic properties to the pressure-sensitive adhesive layer, and examples thereof include ionic compounds, nonionic compounds, etc., with ionic compounds being preferred. The ionic compound may be a liquid (ionic liquid) or a solid (ionic solid) at room temperature. Here, the ionic compound in this specification refers to a compound in which cations and anions are primarily bonded by electrostatic attraction. The antistatic agent may be used alone or in combination of two or more.

[0116] The ionic compound is preferably a nitrogen-containing onium salt, a sulfur-containing onium salt, a phosphorus-containing onium salt, an alkali metal salt, or an alkaline earth metal salt, and from the viewpoint of blister resistance, a nitrogen-containing onium salt or an alkali metal salt is particularly preferred. The nitrogen-containing onium salt is preferably an ionic compound composed of a nitrogen-containing heterocyclic cation and its counter anion.

[0117] The nitrogen-containing heterocyclic skeleton of the nitrogen-containing heterocyclic cation is preferably a pyridine ring, a pyrimidine ring, an imidazole ring, a triazole ring, an indole ring, etc., and more preferably a pyridine ring or an imidazole ring. The cation constituting the alkali metal salt is preferably a lithium ion, a potassium ion, or a sodium ion, and more preferably a lithium ion or a potassium ion.

[0118] On the other hand, preferred anions constituting the ionic compounds include halogenated phosphate anions or sulfonylimide anions. Preferred examples of halogenated phosphate anions include hexafluorophosphate. Preferred examples of sulfonylimide anions include bis(fluoroalkylsulfonyl)imides or bis(fluorosulfonyl)imides. The bis(fluoroalkylsulfonyl)imides may be bis(perfluoroalkylsulfonyl)imides, and preferred examples of such bis(trifluoromethanesulfonyl)imides are bis(trifluoromethanesulfonyl)imides.

[0119] Specific examples of nitrogen-containing onium salts having a pyridine ring and a halogenated phosphate anion include 1-butyl-4-methylpyridinium hexafluorophosphate, 1-hexyl-3-methylpyridinium hexafluorophosphate, 1-hexyl-4-methylpyridinium hexafluorophosphate, 1-octylpyridinium hexafluorophosphate, 1-octyl-4-methylpyridinium hexafluorophosphate, 1-dodecylpyridinium hexafluorophosphate, 1-tetradecylpyridinium hexafluorophosphate, 1-hexadecylpyridinium hexafluorophosphate, 1-dodecyl-4-methylpyridinium hexafluorophosphate, 1-tetradecyl-4-methylpyridinium hexafluorophosphate, 1-hexadecyl-4-methylpyridinium hexafluorophosphate, and the like.

[0120] Specific examples of nitrogen-containing onium salts having a pyridine ring and a sulfonylimide anion include 1-decylpyridinium bis(fluorosulfonyl)imide, 1-ethylpyridinium bis(fluorosulfonyl)imide, 1-butylpyridinium bis(fluorosulfonyl)imide, 1-hexylpyridinium bis(fluorosulfonyl)imide, 1-butyl-3-methylpyridinium bis(fluorosulfonyl)imide, 1-butyl-4-methylpyridinium bis(fluorosulfonyl)imide, 1-hexyl-3-methylpyridinium bis(fluorosulfonyl)imide, 1-butyl-3,4-dimethylpyridinium bis(fluorosulfonyl)imide, and 4-methyl-1-octylpyridinium bis(fluorosulfonyl)imide.

[0121] Specific examples of nitrogen-containing onium salts having an imidazole ring include 1-ethyl-3-methylimidazolium bis(fluorosulfonyl)imide, 1-propyl-3-methylimidazolium bis(fluorosulfonyl)imide, 1-butyl-3-methylimidazolium bis(fluorosulfonyl)imide, 1-hexyl-3-methylimidazolium bis(fluorosulfonyl)imide, 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, 1-propyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, and 1-hexyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide.

[0122] Specific examples of the alkali metal salt include potassium bis(fluorosulfonyl)imide, lithium bis(fluorosulfonyl)imide, potassium bis(fluoromethanesulfonyl)imide, lithium bis(fluoromethanesulfonyl)imide, potassium bis(trifluoromethanesulfonyl)imide, and lithium bis(trifluoromethanesulfonyl)imide.

[0123] The content of the antistatic agent in 100% by mass of the adhesive is preferably 0.1 to 10% by mass, more preferably 0.5 to 6% by mass, and even more preferably 1 to 3% by mass, which makes it easier to exhibit excellent antistatic properties.

[0124] (1.3.6. Other Additives) The adhesive composition P may contain additives that are commonly used in acrylic adhesives, if necessary. Examples of such additives include ultraviolet absorbers, infrared absorbers, tackifiers, antioxidants, light stabilizers, softeners, rust inhibitors, fillers, refractive index adjusters, etc. It should be noted that the polymerization solvents and dilution solvents described below are not included in the additives that constitute the adhesive composition P.

[0125] (1.4. Release Sheets) The release sheets 11 and 12 protect the pressure-sensitive adhesive layer 10 until the pressure-sensitive adhesive sheet 1 is to be used, and are peeled off when the pressure-sensitive adhesive sheet 1 (pressure-sensitive adhesive layer 10) is to be used. In the pressure-sensitive adhesive sheet 1 according to this embodiment, one or both of the release sheets 11 and 12 are not necessarily required.

[0126] Examples of materials that can be used as the release sheets 11 and 12 include polyethylene films, polypropylene films, polybutene films, polybutadiene films, polymethylpentene films, polyvinyl chloride films, vinyl chloride copolymer films, polyethylene terephthalate films, polyethylene naphthalate films, polybutylene terephthalate films, polyurethane films, ethylene vinyl acetate films, ionomer resin films, ethylene-(meth)acrylic acid copolymer films, ethylene-(meth)acrylic acid ester copolymer films, polystyrene films, polycarbonate films, polyimide films, and fluororesin films. Crosslinked films of these materials can also be used. Furthermore, laminated films of these materials may also be used. From the perspective of the SDGs, the material constituting the release sheets may be a material with a high biomass content, a recyclable or reusable material, or a recycled or reused material.

[0127] The release surfaces of the release sheets 11, 12 (particularly the surfaces that come into contact with the pressure-sensitive adhesive layer 10) are preferably subjected to a release treatment. Examples of release agents used for the release treatment include alkyd-based, silicone-based, fluorine-based, unsaturated polyester-based, polyolefin-based, and wax-based release agents. It is preferable that one of the release sheets 11, 12 is a heavy-release type release sheet with a high release strength, and the other is a light-release type release sheet with a low release strength.

[0128] There is no particular limitation on the thickness of the release sheets 11 and 12, but it is usually about 20 to 150 μm.

[0129] (1.5. Production of Pressure-Sensitive Adhesive Composition) The pressure-sensitive adhesive composition P can be produced, for example, by first producing a (meth)acrylic acid ester polymer (A) and then mixing the resulting (meth)acrylic acid ester polymer (A) with a crosslinking agent (B). If necessary, a colorant (C), a silane coupling agent (D), an antistatic agent (E), and additives may be added.

[0130] The (meth)acrylic acid ester polymer (A) can be produced, for example, by polymerizing a mixture of monomers constituting the polymer using a conventional radical polymerization method. The polymerization of the (meth)acrylic acid ester polymer (A) can be carried out by a solution polymerization method, using a polymerization initiator as needed. By polymerizing the (meth)acrylic acid ester polymer (A) using a solution polymerization method, it becomes easy to increase the molecular weight of the resulting polymer and adjust the molecular weight distribution, and it also becomes possible to reduce the production of low molecular weight substances. As a result, it is easy to obtain a pressure-sensitive adhesive that is excellent in resistance to repeated bending.

[0131] Examples of polymerization solvents used in solution polymerization include ethyl acetate, n-butyl acetate, isobutyl acetate, toluene, acetone, hexane, and methyl ethyl ketone. One type of polymerization solvent may be used, or two or more types may be used in combination. Examples of polymerization initiators include azo compounds and organic peroxides, and two or more types may be used in combination. In the polymerization step, the weight average molecular weight of the resulting polymer can be adjusted by adding a chain transfer agent such as 2-mercaptoethanol.

[0132] Subsequently, the crosslinking agent (B) is added to the obtained solution of the (meth)acrylic acid ester polymer (A) and mixed thoroughly to obtain a solvent-diluted pressure-sensitive adhesive composition P (coating solution). If necessary, a dilution solvent, a colorant (C), a silane coupling agent (D), an antistatic agent (E), and additives may be added.

[0133] In addition, if any of the above components is a solid component, or if it is a component that will precipitate when mixed with other components in an undiluted state, that component may be dissolved or diluted in advance alone in a dilution solvent and then mixed with the other components.

[0134] Examples of dilution solvents include aliphatic hydrocarbons such as hexane, heptane, and cyclohexane; aromatic hydrocarbons such as toluene and xylene; halogenated hydrocarbons such as methylene chloride and ethylene chloride; alcohols such as methanol, ethanol, propanol, butanol, and 1-methoxy-2-propanol; ketones such as acetone, methyl ethyl ketone, 2-pentanone, isophorone, and cyclohexanone; esters such as ethyl acetate and butyl acetate; and cellosolve-based solvents such as ethyl cellosolve.

[0135] The concentration and viscosity of the prepared coating solution may be within a range that allows coating, and can be appropriately selected depending on the situation. For example, the adhesive composition P is diluted so that the concentration is 10 to 60 mass %. Note that the addition of a dilution solvent or the like is not a necessary condition for obtaining the coating solution, and as long as the adhesive composition P has a viscosity that allows coating, the addition of a dilution solvent is not necessary. In this case, the adhesive composition P becomes a coating solution in which the polymerization solvent for the (meth)acrylic acid ester polymer (A) is used as the dilution solvent.

[0136] (1.6. Production of Pressure-Sensitive Adhesive) The pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer is preferably obtained by crosslinking the above-mentioned pressure-sensitive adhesive composition P. Crosslinking of the pressure-sensitive adhesive composition P can usually be carried out by a heat treatment. Note that this heat treatment can also serve as a drying treatment for volatilizing dilution solvents and the like from a coating film of the pressure-sensitive adhesive composition P applied to a desired object.

[0137] The heating temperature for the heat treatment is preferably 50 to 150° C., more preferably 70 to 120° C. The heating time is preferably 10 seconds to 10 minutes, more preferably 50 seconds to 2 minutes.

[0138] After the heat treatment, a curing period of about 1 to 2 weeks may be provided at room temperature (e.g., 23°C, relative humidity 50%), if necessary. When curing is required, a pressure-sensitive adhesive having a crosslinked structure is obtained after the curing period has elapsed. When curing is not required, a pressure-sensitive adhesive having a crosslinked structure is obtained after the heat treatment is completed.

[0139] (1.7. Production of Pressure-Sensitive Adhesive Sheet) The method for producing the pressure-sensitive adhesive sheet 1 is not particularly limited, and it may be produced by a known method. For example, a coating solution of the above-mentioned pressure-sensitive adhesive composition P is applied to the release surface of one of the first release sheets 11 (or the second release sheet 12), and a heat treatment is carried out to crosslink the pressure-sensitive adhesive composition P, thereby forming a coating layer having a predetermined thickness. The release surface of the other second release sheet 12 (or the first release sheet 11) is then superimposed on the formed coating layer. If curing is required, the coating layer will become the pressure-sensitive adhesive layer 10 after a predetermined curing period has elapsed. Alternatively, if curing is not required, the coating layer will become the pressure-sensitive adhesive layer 10 as is. In this way, the pressure-sensitive adhesive sheet 1 is obtained.

[0140] In another method for producing the pressure-sensitive adhesive sheet 1, the release surface of one of the first release sheets 11 is coated with a coating liquid of the above-mentioned pressure-sensitive adhesive composition P, and a heat treatment is performed to crosslink the pressure-sensitive adhesive composition P and form a coating layer, thereby obtaining a first release sheet 11 with a coating layer. The release surface of the other of the second release sheets 12 is coated with a coating liquid of the above-mentioned pressure-sensitive adhesive composition P, and a heat treatment is performed to crosslink the pressure-sensitive adhesive composition P and form a coating layer, thereby obtaining a second release sheet 12 with a coating layer. The first release sheet 11 with the coating layer and the second release sheet 12 with the coating layer are then bonded together so that the two coating layers are in contact with each other. If curing is required, the coating layer becomes the pressure-sensitive adhesive layer 10 after a predetermined curing period. If curing is not required, the coating layer becomes the pressure-sensitive adhesive layer 10 as is. This produces the pressure-sensitive adhesive sheet 1. This production method allows stable production even when the pressure-sensitive adhesive layer 10 is thick.

[0141] Examples of methods for applying the coating solution of the adhesive composition P include bar coating, knife coating, roll coating, blade coating, die coating, and gravure coating.

[0142] (2. Flexible Material Laminate) As shown in Figure 2, the flexible material laminate 2 of this embodiment is composed of a first flexible member 21 (one flexible member), a second flexible member 22 (another flexible member), and an adhesive layer 10 located between them and bonding the first flexible member 21 and the second flexible member 22 to each other.

[0143] The adhesive layer 10 in the flexible material laminate 2 is the adhesive layer 10 of the adhesive sheet 1 described above.

[0144] The flexible material laminate 2 is a flexible device itself or a component constituting part of a flexible device. The flexible device may be a device including a component that is bent once during manufacturing and maintains the bent state, or may be a device including a component that can be repeatedly bent (including folded). The flexible device is preferably a display, but is not limited to this. Examples of flexible devices include organic electroluminescence (organic EL) displays, electrophoretic displays (electronic paper), liquid crystal displays using a plastic substrate (film) as a substrate, light-emitting diode (LED) displays, foldable displays, stretchable displays, and rollable displays. These may also be touch panels.

[0145] The first flexible member 21 and the second flexible member 22 are, for example, members that can be repeatedly bent (including folded). Examples of flexible members include a cover film, a barrier film, a hard coat film, a polarizing film (polarizing plate), a polarizer, a retardation film (retardation plate), a viewing angle compensation film, a brightness enhancement film, a contrast enhancement film, a diffusion film, a semi-transmitting reflective film, an electrode film, a transparent conductive film, a metal mesh film, a film sensor (touch sensor film), a liquid crystal polymer film, a light-emitting polymer film, a film-like liquid crystal module, an organic EL module (organic EL film, organic EL element), an electronic paper module (film-like electronic paper), a TFT (Thin Film Transistor) substrate, and the like.

[0146] The Young's modulus of each of the first flexible member 21 and the second flexible member 22 is preferably 0.1 to 10 GPa, more preferably 0.5 to 7 GPa, and even more preferably 1 to 5 GPa. When the Young's modulus of the first flexible member 21 and the second flexible member 22 is within the above range, it becomes easy to repeatedly bend each flexible member.

[0147] The thickness of each of the first flexible member 21 and the second flexible member 22 is preferably 10 to 3000 μm, more preferably 25 to 1000 μm, and even more preferably 50 to 500 μm. When the thickness of the first flexible member 21 and the second flexible member 22 is within the above range, each flexible member can be easily bent repeatedly.

[0148] The interlayer adhesion (adhesive strength) between the first flexible member 21 and the second flexible member 22 preferably has a lower limit of 1 N / 25 mm or more, particularly preferably 2 N / 25 mm or more, and even more preferably 5 N / 25 mm or more. When the interlayer adhesion strength is 1 N / 25 mm or more, the flexible display has excellent flex resistance. Furthermore, the interlayer adhesion strength preferably has an upper limit of 30 N / 25 mm or less, more preferably 25 N / 25 mm or less, and particularly preferably 20 N / 25 mm or less. When the interlayer adhesion strength is 20 N / 25 mm or less, the reworkability can be said to be excellent. This allows the flexible members to be easily peeled off even if a bonding error occurs between them, making it possible to reuse the flexible members (especially expensive flexible members).

[0149] Here, the interlayer adhesion (adhesive strength) in this specification basically refers to the adhesive strength measured by the 180-degree peel method in accordance with JIS Z0237:2009. The measurement sample is 25 mm wide and 100 mm long, and a laminate consisting of a first flexible member / adhesive layer / second flexible member is prepared. After applying pressure of 0.5 MPa and 50°C for 20 minutes, the laminate is left to stand for 24 hours under conditions of normal pressure, 23°C, and a relative humidity of 50%, and then the adhesive strength is measured at a peel speed of 300 mm / min.

[0150] An example of manufacturing the flexible material laminate 2 will be shown below. First, one of the second release sheets 12 of the adhesive sheet 1 is peeled off, and the exposed adhesive layer 10 of the adhesive sheet 1 is attached to one surface of the first flexible material 21.

[0151] Thereafter, the other first release sheet 11 is peeled off from the pressure-sensitive adhesive layer 10 of the pressure-sensitive adhesive sheet 1, and the exposed pressure-sensitive adhesive layer 10 of the pressure-sensitive adhesive sheet 1 is bonded to the second flexible member 22 to obtain the flexible member laminate 2. As another example, the bonding order of the first flexible member 21 and the second flexible member 22 may be reversed.

[0152] (3. Flexible Device) The flexible device according to this embodiment includes the flexible material laminate 2 described above, and may consist of only the flexible material laminate 2, or may be configured with one or more flexible material laminates 2 and other flexible materials. When laminating one flexible material laminate 2 with another flexible material laminate 2, or when laminating a flexible material laminate 2 with another flexible material, it is preferable to laminate them via the adhesive layer 10 of the adhesive sheet 1 described above.

[0153] In the flexible device according to the present embodiment, since the components are bonded together by the above-described adhesive layer, even when the flexible device is repeatedly bent (for example, 100,000 times), peeling of the adhesive layer from the bonded components is suppressed, and color unevenness at the bent portion is suppressed. Furthermore, since the components are bonded together by the above-described adhesive layer, the flexible device according to the present embodiment has excellent design properties.

[0154] A flexible device as an example of this embodiment is shown in Fig. 3. However, the flexible device according to the present invention is not limited to this flexible device.

[0155] 3 , the flexible device 3 according to this embodiment is configured by laminating, from top to bottom, a cover film 31, a first adhesive layer 32, a polarizing film 33, a second adhesive layer 34, a touch sensor film 35, a third adhesive layer 36, an organic EL element 37, a fourth adhesive layer 38, and a TFT substrate 39. The cover film 31, the polarizing film 33, the touch sensor film 35, the organic EL element 37, and the TFT substrate 39 correspond to flexible members.

[0156] At least one of the first pressure-sensitive adhesive layer 32, the second pressure-sensitive adhesive layer 34, the third pressure-sensitive adhesive layer 36, and the fourth pressure-sensitive adhesive layer 38 is preferably the pressure-sensitive adhesive layer 10 of the pressure-sensitive adhesive sheet 1. It is preferable that two or more of the first pressure-sensitive adhesive layer 32, the second pressure-sensitive adhesive layer 34, the third pressure-sensitive adhesive layer 36, and the fourth pressure-sensitive adhesive layer 38 are the pressure-sensitive adhesive layer 10 of the pressure-sensitive adhesive sheet 1, and it is most preferable that all of the pressure-sensitive adhesive layers 32, 34, 36, and 38 are the pressure-sensitive adhesive layer 10 of the pressure-sensitive adhesive sheet 1.

[0157] In this specification, when it is stated that "X to Y" (X and Y are any numbers), it means "X or more and Y or less" unless otherwise specified, and also means "preferably greater than X" or "preferably smaller than Y". Furthermore, when it is stated that "X or more" (X is any number), it means "preferably greater than X" unless otherwise specified, and when it is stated that "Y or less" (Y is any number), it also means "preferably smaller than Y" unless otherwise specified.

[0158] Although the embodiments of the present invention have been described above, the present invention is not limited to the above-described embodiments and may be modified in various ways within the scope of the present invention.

[0159] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples.

[0160] Example 1 1. Preparation of (meth)acrylic acid ester polymer 48.6 parts by mass of n-butyl acrylate, 48.6 parts by mass of 2-ethylhexyl acrylate, 1.8 parts by mass of 2-phenoxyethyl acrylate, and 1 part by mass of 4-hydroxybutyl acrylate were copolymerized to prepare a (meth)acrylic acid ester polymer (A). The molecular weight of the resulting (meth)acrylic acid ester polymer (A) was measured by the method described below, and the weight average molecular weight (Mw) was found to be 1,200,000.

[0161] The weight average molecular weight (Mw) is a polystyrene-equivalent weight average molecular weight measured using gel permeation chromatography (GPC) under the following conditions (GPC measurement). (Measurement conditions) GPC measurement device: HLC-8020, manufactured by Tosoh Corporation GPC columns (passed in the following order): TSK guard column HXL-H, TSK gel GMHXL (x2), TSK gel G2000HXL, manufactured by Tosoh Corporation Measurement solvent: tetrahydrofuran Measurement temperature: 40°C

[0162] 2. Preparation of adhesive composition 100 parts by mass (solid content equivalent; the same applies hereinafter) of the (meth)acrylic acid ester polymer (A) obtained above, 0.14 parts by mass of an isocyanate-based crosslinking agent (manufactured by Mitsui Chemicals, Inc., product name "Takenate D-101E") (B1) as the crosslinking agent (B), 0.26 parts by mass of a colorant (C1) having the physical properties shown in Table 2 as the colorant (C), and 0.2 parts by mass of 3-glycidoxypropyltrimethoxysilane (D1) as the silane coupling agent (D) were mixed, thoroughly stirred, and diluted with methyl ethyl ketone to obtain a coating solution of an adhesive composition having a solid content concentration of 50% by mass.

[0163] 3. Production of Pressure-Sensitive Adhesive Sheet The obtained coating solution of the pressure-sensitive adhesive composition was applied using a knife coater to the release-treated surface of a heavy-release type release sheet R1, one side of which had been release-treated with a silicone-based release agent for polyethylene terephthalate film. The coating layer was then heat-treated at 90°C for 1 minute to promote a crosslinking reaction, thereby forming a coating layer made of a pressure-sensitive adhesive having a crosslinked structure composed of a (meth)acrylic acid ester polymer (A) and a crosslinking agent (B).

[0164] Next, the coating layer on the release sheet R1 obtained above was bonded to a light-release type release sheet R2, one side of which was a polyethylene terephthalate film treated with a silicone-based release agent, so that the release-treated surface contacted the coating layer, and the sheet was aged for 7 days under conditions of 23°C and 50% relative humidity to produce a pressure-sensitive adhesive sheet having a 50 μm thick adhesive layer. This pressure-sensitive adhesive sheet had a configuration of release sheet R1 / adhesive layer (thickness: 50 μm) / release sheet R2. The thickness of the adhesive layer was measured in accordance with JIS K7130 using a constant-pressure thickness gauge (PG-02, manufactured by Teclock Corporation). It was also confirmed that the release sheet R1 had a greater peel strength from the adhesive layer than release sheet R2.

[0165] (Examples 2 to 11, Comparative Examples 1 to 4) Pressure-sensitive adhesive sheets were produced in the same manner as in Example 1, except that the composition and molecular weight of the (meth)acrylic acid ester polymer (A), the type and amount of the crosslinking agent (B), the type and amount of the colorant (C), the amount of the silane coupling agent (D), the type and amount of the antistatic agent (E), and the thickness of the pressure-sensitive adhesive layer were changed as shown in Table 1. In Table 1, the amounts of the crosslinking agent (B), colorant (C), silane coupling agent (D), and antistatic agent (E) are expressed as amounts (in terms of solid content) relative to 100 parts by mass (in terms of solid content) of the (meth)acrylic acid ester polymer (A).

[0166]

[0167] Details of the abbreviations and the like in Table 1 are as follows. Regarding colorant (C), Table 2 shows the optical properties of solutions obtained by diluting colorants C1, C2, and C3 listed in Table 1 by a factor of 10,000 with ethyl acetate. The optical properties shown in Table 2 were calculated from the haze values ​​(%) obtained for the above-mentioned diluted solutions using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., product name "SH-7000") in accordance with JIS K7136:2000. The difference in haze value is the difference between the haze value at a wavelength of 780 nm and the haze value at a wavelength of 380 nm, the average haze is the average value of the haze value at a wavelength of 780 nm and the haze value at a wavelength of 380 nm, and the standard deviation of the haze values ​​is the standard deviation of the haze values ​​at each wavelength in 5-nm increments in the wavelength range from 380 nm to 780 nm. ((Meth)acrylic acid ester copolymer (A)) BA: n-butyl acrylate 2EHA: 2-ethylhexyl acrylate PhEA: 2-phenoxyethyl acrylate 4HBA: 4-hydroxybutyl acrylate ACMO: N-acryloylmorpholine IBXA: isobornyl acrylate HEA: 2-hydroxyethyl acrylate AA: acrylic acid (Crosslinking agent (B)) B1: isocyanate-based crosslinking agent (manufactured by Mitsui Chemicals, Inc., product name "Takenate D-101E") B2: isocyanate-based crosslinking agent (manufactured by Soken Chemical & Engineering Co., Ltd., product name "TD-75") (Silane coupling agent (D)) D1: 3-glycidoxypropyltrimethoxysilane (Antistatic agent (E)) E1: 4-methyl-1-octylpyridinium bis(fluorosulfonyl)imide

[0168]

[0169] [Production Example 1] A polyethylene terephthalate (PET) film (manufactured by Toyobo Co., Ltd., product name "Cosmoshine A4160", thickness: 50 μm) with one side treated for easy adhesion was used as a substrate, and a composition containing an ultraviolet (UV) curable resin and reactive silica (manufactured by Arakawa Chemical Industries, Ltd., product name "Opstar Z7530") was applied to one side of the substrate (the smooth side not treated for easy adhesion) using a Mayer bar to form a coating film, and the coating film was dried at 70°C for 1 minute. Then, using a conveyor-type UV light irradiation device (manufactured by Fusion Co., Ltd., product name "F600V"), the coating film was irradiated with UV under the following conditions to cure the coating film and form a 1 μm thick anchor coat layer. <UV irradiation conditions> UV lamp: high-pressure mercury lamp Line speed: 20 m / min Accumulated light intensity: 120 mJ / cm 2 ・Illuminance: 200mW / cm 2 ・Lamp height: 104mm

[0170] Next, a coating material containing perhydropolysilazane as a main component (manufactured by Merck Performance Materials, product name "AZ-110a-20") was applied to the surface of the anchor coat layer by spin coating. Then, the resulting material was heated at 120°C for 1 minute to form a polysilazane layer containing perhydropolysilazane. The thickness of the formed polysilazane layer was 200 nm.

[0171] Then, using a plasma ion implantation device, argon (Ar) was plasma ion implanted into the surface of the polysilazane layer to form a gas barrier layer made of modified polysilazane. In this way, a gas barrier film was obtained having a gas barrier layer made of modified polysilazane on one side of the substrate (PET film). Note that the modification of polysilazane proceeds from the surface of the polysilazane layer. Therefore, the degree of modification does not affect the surface condition of the gas barrier layer, and therefore does not affect flex resistance, etc.

[0172] (Storage Modulus G' of Pressure-Sensitive Adhesive Layer) A plurality of pressure-sensitive adhesive layers of the pressure-sensitive adhesive sheets prepared in the Examples and Comparative Examples were laminated to form a laminate having a thickness of 3 mm. A cylindrical body having a diameter of 8 mm (height of 3 mm) was punched out from the obtained pressure-sensitive adhesive layer laminate to provide a sample for measuring storage modulus. The storage modulus (G') (MPa) of the measurement sample was measured by a torsional shear method using a viscoelasticity measuring device (DYNAMICANALAYZER, manufactured by REOMETRIC) in accordance with JIS K7244-6, at a measurement temperature of 23°C and a measurement frequency of 1 Hz. The results are shown in Table 3.

[0173] (Lightness L of adhesive layer * , chromaticity a * and chromaticity b * The pressure-sensitive adhesive layers of the pressure-sensitive adhesive sheets obtained in the examples and comparative examples were measured using a simultaneous spectrophotometric colorimeter (manufactured by Nippon Denshoku Industries Co., Ltd., product name "SQ2000") according to CIE 1976L. * a * b * Lightness L defined by the color system * , chromaticity a * and chromaticity b * The results are shown in Table 3.

[0174] (Restoration rate of adhesive layer) The restoration rate of the adhesive layer was measured as follows. Under an environment of 23°C and 50% relative humidity, the release sheet R2 was peeled from the adhesive sheets prepared in the Examples and Comparative Examples, and the exposed adhesive layer was bonded to one side of a polyimide (PI) film (manufactured by DuPont-Toray Co., Ltd., product name "Kapton 100PI", thickness: 25 μm, Young's modulus: 3.4 GPa). Next, the release sheet R1 was peeled off, and the exposed adhesive layer was bonded to the gas barrier layer side of the gas barrier film (Young's modulus: 4.2 GPa) prepared in Production Example 1. Then, after pressurizing at 0.5 MPa and 50°C for 20 minutes in an autoclave manufactured by Kurihara Manufacturing Co., Ltd., the laminate was left at 23°C and 50% relative humidity for 24 hours. The laminate consisting of the PI film / adhesive layer / gas barrier film obtained in this way was cut into a width of 50 mm and a length of 200 mm, which was used as a test piece S.

[0175] The obtained test piece S was held in a bent state between two holding plates P (distance between them: 4 mm) made of upright glass plates in an environment of 23°C and a relative humidity of 50% for 24 hours, as shown in Fig. 4. At this time, the test was carried out while the test piece S was bent so that the gas barrier film sides faced each other.

[0176] After the static bending test, the test piece S was placed on a flat plate as shown in Figure 5, and the height h from the surface of the flat plate to the apex of the bent portion (deformed portion) was measured as the static bending deformation (mm) immediately after the test and one hour after the test. From the static bending deformation (mm) immediately after the test and one hour after the test, the recovery rate (%) was calculated according to the following formula, and the recovery was evaluated according to the following criteria. The results are shown in Table 3. Recovery rate (%) = (1 - static bending deformation after one hour of test / static bending deformation immediately after test) x 100

[0177] (Evaluation of Gel Fraction of Pressure-Sensitive Adhesive) The pressure-sensitive adhesive layers prepared in the Examples and Comparative Examples were cut to a size of 80 mm x 80 mm, and the pressure-sensitive adhesive layers were wrapped in a polyester mesh (product name: Tetron Mesh #200), and the mass thereof was weighed using a precision balance. The mass of the pressure-sensitive adhesive alone was calculated by subtracting the mass of the mesh alone from the weighed value. This mass was designated M1.

[0178] Next, the adhesive wrapped in the polyester mesh was immersed in ethyl acetate at room temperature (23°C) for 24 hours. The mesh was then removed and air-dried for 24 hours in an environment with a temperature of 23°C and a relative humidity of 50%, and then dried in an oven at 80°C for 12 hours. After drying, the mesh was weighed using a precision balance. The mass of the adhesive alone was calculated by subtracting the mass of the mesh alone from the weighed value. This mass was designated M2. The gel fraction was calculated using the obtained M1 and M2 according to the following formula. The results are shown in Table 3. Gel fraction (%) = (M2 / M1) x 100

[0179] (Measurement of adhesive strength of adhesive layer) The release sheet R2 was peeled off from the adhesive sheets obtained in the Examples and Comparative Examples, and the exposed adhesive layer was attached to an easy-adhesion layer of a polyethylene terephthalate (PET) film (manufactured by Toyobo Co., Ltd., product name "Cosmoshine A4160", thickness: 100 μm) having an easy-adhesion layer, to obtain a release sheet R1 / adhesive layer / PET film laminate. The obtained laminate was cut into a width of 25 mm and a length of 100 mm, and this was used as a sample.

[0180] The release sheet R1 was peeled from the sample under an environment of 23°C and 50% relative humidity, and the exposed adhesive layer was attached to soda lime glass (manufactured by Nippon Sheet Glass Co., Ltd.), and then pressurized in an autoclave manufactured by Kurihara Manufacturing Co., Ltd. at 0.5 MPa and 50°C for 20 minutes. After leaving the sample at 23°C and 50% relative humidity for 24 hours, the adhesive strength (N / 25 mm) was measured using a tensile tester (manufactured by Orientec Co., Ltd., product name "Tensilon") at a peel speed of 300 mm / min and a peel angle of 180°. Measurements were conducted under conditions other than those described here in accordance with JIS Z0237:2009. The results are shown in Table 3.

[0181] (Measurement of total light transmittance) The pressure-sensitive adhesive layer of the pressure-sensitive adhesive sheet obtained in the Examples and Comparative Examples was attached to glass to prepare a measurement sample. After background measurement was performed on the glass, the total light transmittance (%) of the measurement sample was measured in accordance with JIS K7361-1:1997 using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., product name "NDH-5000"). The results are shown in Table 3.

[0182] (Measurement of Haze Value) The haze values ​​(%) of the pressure-sensitive adhesive layers of the pressure-sensitive adhesive sheets obtained in the Examples and Comparative Examples were measured using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., product name "NDH-5000") in accordance with JIS K7136: 2000. The obtained total light haze values ​​(%) are shown in Table 3.

[0183] (Evaluation of Design) In an environment of 23 ° C. and 50% relative humidity, the release sheet R2 was peeled from the pressure-sensitive adhesive sheets obtained in the examples and comparative examples, and the exposed pressure-sensitive adhesive layer was attached to one side of a polyethylene terephthalate film (manufactured by Toyobo Co., Ltd., product name "Cosmoshine A4160", thickness: 50 μm). Next, the release sheet R1 was peeled off, and the exposed pressure-sensitive adhesive layer was attached to one side of another polyethylene terephthalate film (manufactured by Toyobo Co., Ltd., product name "Cosmoshine A4160", thickness: 50 μm). Then, after applying pressure of 0.5 MPa and 50 ° C. for 20 minutes in an autoclave manufactured by Kurihara Seisakusho Co., Ltd., the laminate was left for 24 hours under conditions of 23 ° C. and 50% relative humidity. The laminate thus obtained, consisting of a PET film / pressure-sensitive adhesive layer / PET film, was used as a sample.

[0184] The obtained sample was placed immediately in front of a display (manufactured by Fujitsu, product name "LIFEBOOKA574 / H", size 15.6 inches, resolution 1366 x 768) that was turned off. The sample was placed so that the periphery of the sample was adjacent to the frame material of the display. The color (blackness / whiteness) of the sample was then visually judged under a three-band fluorescent lamp (distance from the fluorescent lamp: 200 cm), and the design quality regarding the color of the screen was evaluated according to the following criteria. The results are shown in Table 3. A: Deep blackness is present even under fluorescent lamp reflection. B: Deep blackness is present without fluorescent lamp reflection. F: The entire screen appears whitish.

[0185] The visibility of the boundary between the sample portion and the frame material of the display was also visually judged, and the design quality regarding seamlessness was evaluated according to the following criteria. The results are shown in Table 3. A: The boundary is not visible. B: The boundary is slightly visible but not noticeable. F: The boundary is clearly visible.

[0186] Next, the properties of the pressure-sensitive adhesive sheet were evaluated as follows.

[0187] (Flexibility) In the same manner as in the evaluation of the design property, a laminate consisting of a PET film / adhesive layer / PET film was prepared and cut into a size of 150 mm x 50 mm to prepare sample S.

[0188] As shown in FIG. 6 , both ends of the obtained sample S were fixed to two holding plates P of a surface condition no-load U-shaped expansion / contraction tester (manufactured by Yuasa System Co., Ltd., product name "DLDMLH-FS"). Then, sample S was bent 100,000 times under conditions of 23°C, 50% relative humidity, a bending diameter of 6 mm, a stroke of 80 mm, and a bending speed of 30 rpm. After the test, the presence or absence of lifting or peeling at the interface between the pressure-sensitive adhesive layer and the adherend at the bent portion was visually confirmed according to the following criteria. The results are shown in Table 3. <Evaluation criteria for repeated bending resistance> A... No lifting or peeling occurred at the bent portion. B... Lifting or peeling of less than 1 mm occurred near the edge of the bent portion, but the lifting or peeling did not spread beyond the bent portion, and the sample was at a level sufficient for practical use. C... Lifting or peeling of 1 mm or more but less than 2 mm occurred near the edge of the bent portion, but the lifting or peeling did not spread beyond the bent portion, and the sample was at a level sufficient for practical use. F: Significant lifting or peeling occurred at the bent portion and other than the bent portion.

[0189] Furthermore, color unevenness of the pressure-sensitive adhesive layer at the bent portion was visually confirmed according to the following criteria. The results are shown in Table 3. <Evaluation criteria for color unevenness> A... No change in color of the pressure-sensitive adhesive layer was visible at the bent portion. B... A slight change in color of the pressure-sensitive adhesive layer was visible at the bent portion, but at a level that was barely noticeable. C... A change in color of the pressure-sensitive adhesive layer was visible at the bent portion, but at a level that was practically usable. F... A noticeable change in color of the pressure-sensitive adhesive layer was visible at the bent portion.

[0190]

[0191] From Table 3, it was confirmed that the adhesive sheets of Examples 1 to 11, even when used for bonding flexible materials, do not impair the design of the flexible display, suppress lifting or peeling of the adhesive layer at bent portions, and suppress color unevenness at bent portions.

[0192] The pressure-sensitive adhesive sheet of the present invention can be suitably used, for example, to attach a flexible member.

[0193] REFERENCE SIGNS LIST 1... Adhesive sheet 10... Adhesive layer 11... First release sheet 12... Second release sheet 2... Flexible member laminate 21... First flexible member 22... Second flexible member 3... Flexible device 31... Cover film 32... First adhesive layer 33... Polarizing film 34... Second adhesive layer 35... Touch sensor film 36... Third adhesive layer 37... Organic EL element 38... Fourth adhesive layer 39... TFT substrate

Claims

1. A pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer for bonding a first flexible member and a second flexible member, wherein the pressure-sensitive adhesive layer has a storage modulus of 0.12 MPa or less at 23° C., and the pressure-sensitive adhesive layer has a CIE1976L * a * b * Lightness L defined by the color system * a viscosity index of 95 or less, an adhesive strength of the adhesive layer being 4 N / 25 mm or more, and a recovery rate of the adhesive layer being 80% or more.

2. A pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer for bonding a first flexible member and a second flexible member, wherein the pressure-sensitive adhesive layer has a storage modulus of 0.12 MPa or less at 23° C., and the pressure-sensitive adhesive layer has a CIE1976L * a * b * Lightness L defined by the color system * a gel fraction of the pressure-sensitive adhesive layer is 84% ​​or less; and a recovery rate of the pressure-sensitive adhesive layer is 80% or more.

3. The adhesive sheet for flexible devices according to claim 1 or 2, wherein the adhesive layer contains a colorant.

4. The pressure-sensitive adhesive sheet for flexible devices according to claim 3, wherein the colorant is a black pigment or dye.

5. The pressure-sensitive adhesive sheet for flexible devices according to claim 1 or 2, wherein the haze value of the pressure-sensitive adhesive layer is 80% or less.

6. The pressure-sensitive adhesive sheet for flexible devices according to claim 1 or 2, wherein the pressure-sensitive adhesive layer has a total light transmittance of 3% or more.

7. The pressure-sensitive adhesive sheet for flexible devices according to claim 1 or 2, wherein the gel fraction of the pressure-sensitive adhesive layer is 30% or more.

8. The adhesive sheet for flexible devices according to claim 1 or 2, wherein the adhesive constituting the adhesive layer is an acrylic adhesive.

9. The pressure-sensitive adhesive sheet for flexible devices according to claim 8, wherein the acrylic pressure-sensitive adhesive comprises a (meth)acrylic acid ester polymer and a crosslinking agent.

10. An adhesive sheet for flexible devices according to claim 9, wherein the (meth)acrylic acid ester polymer contains an aromatic ring-containing monomer as a monomer unit constituting the (meth)acrylic acid ester polymer.

11. The adhesive sheet for flexible devices according to claim 10, wherein the (meth)acrylic acid ester polymer contains a reactive functional group-containing monomer as a monomer unit constituting the (meth)acrylic acid ester polymer.

12. A flexible material laminate comprising a first flexible material, a second flexible material, and an adhesive layer that bonds the first flexible material and the second flexible material to each other, wherein the adhesive layer is an adhesive layer possessed by the adhesive sheet for flexible devices described in claim 1 or 2.

13. A flexible device comprising the flexible member laminate according to claim 12.

Citation Information

Patent Citations

  • Adhesive sheet and display body

    JP2020007500A

  • Adhesive sheet, repeated bending laminate member and repeated bending device

    JP2022156356A