Thermoelectric element

The thermoelectric element achieves high efficiency and miniaturization by using a first thermoelectric material with a higher Seebeck coefficient and resistivity in a parallel circuit configuration, addressing the limitations of conventional elements and enabling efficient energy harvesting.

WO2024203801A1PCT designated stage expired Publication Date: 2024-10-03MITSUBISHI MATERIALS CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011198
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-03-01
Filing Date
2024-03-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional thermoelectric elements face challenges in achieving high thermoelectric conversion efficiency, particularly in obtaining a high ZT value and being miniaturized for surface mounting, due to limitations in material performance and circuit configuration.

Method used

A thermoelectric element is designed with a first thermoelectric material having a higher Seebeck coefficient and electrical resistivity than the second material, forming a parallel circuit with electrodes connected to the first material, allowing for high thermoelectric conversion efficiency and miniaturization through a compact chip structure.

Benefits of technology

This configuration enables high thermoelectric conversion efficiency and ZT value, facilitating easy surface mounting and installation, while maintaining high electrical conductivity and Seebeck effect, thus enhancing energy harvesting capabilities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011198_03102024_PF_FP_ABST
    Figure JP2024011198_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a thermoelectric element which has high thermoelectric conversion efficiency and is capable of achieving a high ZT value, while being able to be surface mounted and miniaturized. A thermoelectric element according to the present invention is provided with: a first thermoelectric material unit 1 which has one end 1a and the other end 1b; a second thermoelectric material unit 2 which is joined to the first thermoelectric material unit directly or via a conductor 2a; and a pair of electrodes 3 which are connected to the first thermoelectric material unit. The first thermoelectric material unit has a higher absolute value of the Seebeck coefficient and a higher electrical resistivity than the second thermoelectric material unit, a joined body 4 of the first thermoelectric material unit and the second thermoelectric material unit has end surfaces on one end side and the other end side, and the pair of electrodes are in contact with the first thermoelectric material unit without being in contact with the second thermoelectric material unit, while being formed on the one end-side end surface and the other end-side end surface of the joined body.
Need to check novelty before this filing date? Find Prior Art

Description

thermoelectric element

[0001] The present invention relates to a thermoelectric element that can achieve high thermoelectric conversion efficiency.

[0002] Conventionally, so-called segmented thermoelectric elements in which a plurality of materials with different compositions are bonded together have been known. For example, Patent Document 1 describes a thermoelectric element in which a first electrode, a second electrode, a P-type semiconductor thin film made of a thermoelectric material, and an N-type semiconductor thin film made of a thermoelectric material are formed on a substrate, the P-type semiconductor thin film being connected to the first electrode, and the N-type semiconductor thin film being connected to the second electrode, in which the P-type semiconductor thin film and the N-type semiconductor thin film are overlapping and bonded together, and the bonded surface is present over substantially the entire surface of the substrate.

[0003] Patent Documents 2 and 3 also describe thermoelectric elements in which a first thermoelectric material and a second thermoelectric material made of different materials are joined together, one of a pair of electrodes is connected to the first thermoelectric material, and the other of the pair of electrodes is connected to the second thermoelectric material. That is, in these conventional thermoelectric elements, electrodes are provided on the joined first thermoelectric material and second thermoelectric material, and the first thermoelectric material and the second thermoelectric material are electrically connected in series.

[0004] Japanese Patent Laid-Open No. 10-303471 Japanese Patent Laid-Open No. 2009-32960 Japanese Patent Laid-Open No. 2018-152464

[0005] The above-mentioned conventional techniques have the following problems remaining. That is, as a performance of a thermoelectric element required for practical use of thermoelectric power generation, the ZT value (a dimensionless figure of merit ZT (= S 2 T / ρκ): where S, T, ρ, and κ are required to have a Seebeck coefficient (thermoelectric power; electromotive force generated per 1 K temperature difference), absolute temperature, electrical resistivity, and thermal conductivity κ of 1 or more. In order to increase both the voltage output and the amount of power generated (= voltage x current) obtained by thermoelectric conversion, the material must have P-type and N-type characteristics, the absolute value of the Seebeck coefficient must be 100 μV / K or more, and the power factor (Power factor PW=S 2 / ρ) is 1 × 10 -3 W / mK 2There is a demand for thermoelectric devices with high performance exceeding that of the conventional segmented thermoelectric element. Research and development has been conducted to date using a single material with the aim of increasing the ZT value using various material systems. However, the only commercially available material with a ZT value of approximately 1 at temperatures near room temperature is a Bi-Te-based material. However, Bi-Te-based materials have low heat resistance, are limited to use at temperatures below approximately 200°C, and have low thermoelectric conversion efficiency, making practical use of thermoelectrics difficult. On the other hand, when using the conventional segmented thermoelectric element, a thermoelectric material with a heat resistance of 200°C or higher can be placed on the high-temperature side. However, the ZT value of each thermoelectric material constituting the segmented thermoelectric element is low, and multiple thermoelectric elements form an electrical and thermal series circuit, resulting in a small ZT value for the entire element, making it difficult to increase the thermoelectric conversion efficiency. Furthermore, there is a demand for a thermoelectric element that can be surface-mounted and miniaturized.

[0006] The present invention has been made in view of the above-mentioned problems, and aims to provide a thermoelectric element that has high thermoelectric conversion efficiency, can obtain a high ZT value, and can be surface-mounted and miniaturized.

[0007] The present invention employs the following configuration to solve the above problems: That is, a thermoelectric element according to a first aspect of the invention comprises a first thermoelectric material part having one end and the other end, a second thermoelectric material part joined to the first thermoelectric material part directly or via an electric conductor, and a pair of electrodes connected to the first thermoelectric material part, wherein the first thermoelectric material part has a higher absolute value of the Seebeck coefficient and a higher electrical resistivity than the second thermoelectric material part, a joint between the first thermoelectric material part and the second thermoelectric material part has end faces on the one end side and the other end side, and the pair of electrodes are in contact with the first thermoelectric material part without contacting the second thermoelectric material part, and are formed on the end face on the one end side and the end face on the other end side of the joint part.

[0008] In this thermoelectric element, the junction of the first thermoelectric material part and the second thermoelectric material part has end faces on one end and the other end, and a pair of electrodes contacts the first thermoelectric material part without contacting the second thermoelectric material part, and is formed on the end face on one end of the junction and the other end of the junction. This allows for surface mounting and miniaturization, and enables the realization of an element with high thermoelectric conversion efficiency and ZT value. In other words, the thermoelectric element of the present invention is entirely chip-shaped, and has electrodes formed on both end faces, making it easy to surface mount using solder or the like. The compact shape allows for a high degree of freedom in installation location. For example, while existing pi-shaped thermoelectric modules have multiple thermoelectric elements with electrodes electrically connected in series on a substrate, the chip-shaped thermoelectric element of the present invention can be installed without changing the structure of the thermoelectric module.

[0009] In this thermoelectric element, the first thermoelectric material section has a higher absolute value of the Seebeck coefficient and a higher electrical resistivity than the second thermoelectric material section, and a pair of electrodes is connected to one end and the other end of the first thermoelectric material section at a distance from each other, so that the first thermoelectric material section and the second thermoelectric material section form an electrical and thermal parallel circuit, and when a temperature difference occurs between the one end and the other end (heat flow occurs), an electromotive force is generated with high thermoelectric conversion efficiency. That is, the first thermoelectric material section, which is connected to the pair of electrodes and has a high Seebeck coefficient (absolute value) and high electrical resistance, forms an electromotive voltage path that is mainly due to the Seebeck effect, and the second thermoelectric material section, which is joined to and in contact with the first thermoelectric material section and has a low electrical resistance, forms a current path. It is desirable that the value of the current flowing in the second thermoelectric material section obeys Ohm's law. In this way, by forming a parallel circuit of the electromotive voltage path and the current path, a current path that serves as a current path is formed separately from the electromotive voltage path, thereby increasing the electrical conductivity while maintaining the high Seebeck coefficient (absolute value) of the first thermoelectric material section, and achieving high thermoelectric conversion efficiency and ZT value. The second thermoelectric material section and the pair of electrodes are not directly joined, but are in electrical contact via the first thermoelectric material section. The present invention has a thermoelectric element structure in which multiple materials with different compositions are joined together, but is characterized in that a pair of electrodes (two electrodes) is connected to the first thermoelectric material section. (Segment-type thermoelectric elements also have a structure in which multiple materials with different compositions are joined together, but the pair of electrodes are connected to different thermoelectric materials, and use an electrode connection method different from that of the present invention.)

[0010] A thermoelectric element according to a second invention is the first invention, characterized in that it further comprises a pair of insulating material parts formed to cover at least the second thermoelectric material parts at the end faces on the one end side and the other end side of the junction body. That is, in this thermoelectric element, since the pair of insulating material parts are formed to cover at least the second thermoelectric material parts at the end faces on the one end side and the other end side of the junction body, the insulating material parts can prevent the pair of electrodes from contacting the second thermoelectric material parts at the end faces of the junction body.

[0011] A thermoelectric element according to a third invention is the thermoelectric element according to the first or second invention, characterized in that the first thermoelectric material part is joined to the upper and lower surfaces of the second thermoelectric material part, respectively, and the pair of electrodes is connected to the first thermoelectric material parts on the upper and lower surfaces, respectively. That is, in this thermoelectric element, the first thermoelectric material part is laminated on the upper and lower surfaces of the second thermoelectric material part, respectively, and the pair of electrodes is connected to the first thermoelectric material parts on the upper and lower surfaces, respectively, so that electromotive voltage paths are formed on the top and bottom, respectively, and higher thermoelectric conversion efficiency can be obtained.

[0012] A thermoelectric element according to a fourth invention is the third invention, characterized in that the first thermoelectric material section is also joined to both side surfaces of the second thermoelectric material section, and the pair of electrodes is also connected to each of the first thermoelectric material sections on both side surfaces. That is, in this thermoelectric element, the first thermoelectric material section is also joined to both side surfaces of the second thermoelectric material section, and a pair of electrodes is also connected to each of the first thermoelectric material sections on both side surfaces, so that electromotive voltage paths are formed not only on the top and bottom surfaces but also on both side surfaces, and even higher thermoelectric conversion efficiency can be obtained.

[0013] A thermoelectric element according to a fifth aspect of the present invention is the same as that of the first aspect, except that the first thermoelectric material portion is also bonded to both end surfaces of the second thermoelectric material portion, and the pair of electrodes is formed on the first thermoelectric material portion on both end surfaces. In other words, in this thermoelectric element, the first thermoelectric material portion is also bonded to both end surfaces of the second thermoelectric material portion, and a pair of electrodes is formed on the first thermoelectric material portion on both end surfaces. Therefore, an electromotive voltage path is formed from the pair of electrodes to at least the first thermoelectric material portion on the outer peripheral surface via the first thermoelectric material portion on both end surfaces, thereby achieving higher thermoelectric conversion efficiency. Furthermore, there is no need to form insulating material portions on both end surfaces of the second thermoelectric material portion, thereby reducing the manufacturing process.

[0014] A thermoelectric element according to a sixth aspect of the present invention is the thermoelectric element according to the first or second aspect of the present invention, characterized in that the first thermoelectric material section has a Seebeck coefficient that is 50 μV / K or more larger in absolute value than the second thermoelectric material section, and an electrical resistivity that is 10 times or more larger. That is, in this thermoelectric element, the first thermoelectric material section has a Seebeck coefficient that is 50 μV / K or more larger in absolute value than the second thermoelectric material section, and an electrical resistivity that is 10 times or more larger, and therefore an electromotive voltage path with a sufficiently high Seebeck effect and a current path with sufficiently high electrical conductivity are configured, thereby making it possible to obtain higher thermoelectric conversion efficiency and ZT value.

[0015] A thermoelectric element according to a seventh aspect of the present invention is the thermoelectric element according to the first or second aspect of the present invention, wherein the first thermoelectric material section and the second thermoelectric material section are both A 2+δ The first thermoelectric material portion A is characterized in that it is formed of M (wherein A is at least one of Ag and Cu, and M is at least one of S, Se and Te). 2+δ M is the second thermoelectric material portion A 2+δ By designing the composition of the material so that the absolute value of the Seebeck coefficient is 50 μV / K or more larger than M and the electrical resistivity is 10 times or more larger, it is possible to obtain a large ZT value.

[0016] A thermoelectric element according to an eighth aspect of the present invention is the thermoelectric element of the seventh aspect, characterized in that the first thermoelectric material portion is made of Ag—S, and the second thermoelectric material portion is made of Ag—Se or Ag—S—Se. 2 S, and the second thermoelectric material portion is made of Ag 2 By forming the film from Se, it is possible to obtain a ZT value of 1 or more at least at room temperature.

[0017] A thermoelectric element according to a ninth aspect of the present invention is the thermoelectric element according to the seventh aspect, characterized in that the first thermoelectric material portion is made of Cu—S and the second thermoelectric material portion is made of Cu—Se. 2 The second thermoelectric material portion is made of Cu. 2 By forming the film from Se, it is possible to obtain a ZT value of 1 or more at least at room temperature.

[0018] A thermoelectric element according to a tenth aspect of the present invention is the thermoelectric element according to any one of the first to sixth aspects of the present invention, characterized in that the first thermoelectric material portion is formed of a material containing at least Bi and Te. That is, in this thermoelectric element, the first thermoelectric material portion is a material containing at least Bi and Te, such as Bi-Te or Bi-Sb-Te, and for example, the first thermoelectric material portion is formed of Bi. 2 Te 3 and the second thermoelectric material portion is formed of Cu. 0.55 Ni 0.45 (Constantan), at least Bi 2 Te 3 It is possible to obtain a power factor that is about twice that of the single thermoelectric material section. Note that, if the first thermoelectric material section has a higher absolute value of the Seebeck coefficient and a higher electrical resistivity than the second thermoelectric material section, the thermoelectric properties will be improved compared to the first thermoelectric material section alone, regardless of the composition of the second thermoelectric material section.

[0019] The present invention has the following advantages. That is, in a thermoelectric element according to the present invention, the junction of the first thermoelectric material part and the second thermoelectric material part has end faces on one end and the other end, and a pair of electrodes are in contact with the first thermoelectric material part without contacting the second thermoelectric material part, and are formed on the end face on one end and the end face on the other end of the junction. This allows for surface mounting and miniaturization, and makes it possible to realize an element with high thermoelectric conversion efficiency and ZT value. Therefore, the thermoelectric element according to the present invention has a high degree of installation flexibility and can be easily mounted in a circuit or module, and because it achieves a high thermoelectric conversion efficiency and ZT value, it becomes possible to put into practical use environmental power generation that extracts electricity highly efficiently using a temperature difference.

[0020] FIG. 1 is a cross-sectional view showing a thermoelectric element in a first embodiment of the thermoelectric element according to the present invention. FIG. 2 is a conceptual diagram for explaining the principle of a thermoelectric element in the first embodiment. FIG. 3 is a cross-sectional view showing a thermoelectric element perpendicular to the axial direction (direction from one end to the other end) in a second embodiment of the thermoelectric element according to the present invention. FIG. 4 is a perspective view showing a thermoelectric element in the second embodiment. FIG. 5 is a cross-sectional view showing a thermoelectric element along the axial direction (direction from one end to the other end) in a third embodiment of the thermoelectric element according to the present invention. FIG. 6 is a cross-sectional view showing an example of a thermoelectric element of the present invention that was produced to demonstrate the principle of the thermoelectric element of the present invention. FIG. 7 is a graph showing the results of evaluating the power generation characteristics of a thermoelectric element in an example of a thermoelectric element according to the present invention.

[0021] A first embodiment of a thermoelectric element according to the present invention will be described below with reference to Figures 1 and 2. Note that in the drawings used in the following description, the scale is appropriately changed as necessary to make each part recognizable or easily recognizable.

[0022] As shown in FIGS. 1 and 2 , the thermoelectric element 10 of this embodiment includes a first thermoelectric material portion 1 having one end 1a and the other end 1b, a second thermoelectric material portion 2 joined to the first thermoelectric material portion 1 directly or via a conductor 2a, and a pair of electrodes 3 connected to the first thermoelectric material portion 1. When the first thermoelectric material portion 1 and the second thermoelectric material portion 2 are joined via the conductor 2a, the conductor 2a also functions as an intermediate layer. The conductor 2a is a conductive joining material such as solder or In. The first thermoelectric material portion 1 has a higher Seebeck coefficient and higher electrical resistivity than the second thermoelectric material portion 2. The joined body 4 between the first thermoelectric material portion 1 and the second thermoelectric material portion 2 is formed in a chip shape having end faces on one end and the other end. That is, the joined body 4 has a plate or rectangular parallelepiped shape, and the one end 1a and the other end 1b of the first thermoelectric material portion 1 are disposed on both end faces. The thickness of the first thermoelectric material part 1 (i.e., the thickness in the stacking direction of the first thermoelectric material part 1 and the second thermoelectric material part 2) is preferably 100 nm to 10 mm, and may be 1 μm to 3 mm. The thickness of the second thermoelectric material part 2 is preferably 0.1 mm to 10 mm, and may be 0.5 mm to 3 mm.

[0023] The pair of electrodes 3 contact the first thermoelectric material part 1 without contacting the second thermoelectric material part 2. That is, the thermoelectric element 10 of this embodiment includes a pair of insulating material parts 5 formed to cover at least the second thermoelectric material part 2 on the end face on one end 1a side and the end face on the other end 1b side of the junction 4. The pair of electrodes 3 are formed on the end face on one end 1a side and the end face on the other end 1b side of the junction 4. That is, the pair of electrodes 3 are connected to the one end 1a side and the other end 1b side of the first thermoelectric material part 1 while being spaced apart from each other. Furthermore, the pair of electrodes 3 do not contact the second thermoelectric material part 2 and are arranged apart from the second thermoelectric material part 2. The end face on one end 1a side and the end face on the other end 1b side of the junction 4 are arranged opposite each other.

[0024] The first thermoelectric material parts 1 are respectively joined to the upper and lower surfaces of the second thermoelectric material part 2. The pair of electrodes 3 are connected to the first thermoelectric material parts 1 on the upper and lower surfaces, respectively. That is, the pair of electrodes 3 are connected to the surfaces of the first thermoelectric material parts 1 and are formed on both end surfaces of the joined body 4, covering the pair of insulating material parts 5. The pair of electrodes 3 extend beyond the pair of insulating material parts 5 to the upper and lower surfaces (first thermoelectric material parts 1) of the joined body 4. In this way, the pair of electrodes 3 are connected in contact with only the first thermoelectric material part 1, and are not in contact with the second thermoelectric material part 2 due to the pair of insulating material parts 5.

[0025] The first thermoelectric material part 1 preferably has a Seebeck coefficient that is 50 μV / K or more in absolute value and 10 times or more in electrical resistivity than the second thermoelectric material part 2. The electrical resistivity of the first thermoelectric material part 1 at room temperature is 10 -5 For example, the first thermoelectric material part 1 and the second thermoelectric material part 2 each have a resistance of A 2+δ M (where A is at least one of Ag and Cu, and M is at least one of S, Se and Te). The range of δ is preferably −0.5≦δ≦+0.5. The range of δ is more preferably −0.05 to +0.02.

[0026] In the present invention, a material having an absolute value of a Seebeck coefficient of 0.1 μV / K or more is defined as a thermoelectric material. That is, the absolute value of the Seebeck coefficient of the second thermoelectric material portion 2 is 0.1 μV / K or more. Furthermore, the absolute value of the Seebeck coefficient of the first thermoelectric material portion 1 is preferably 10 mV / K or less. Furthermore, when the electrical resistivity of the first thermoelectric material portion 1 at room temperature is 10 mΩcm or less, the first thermoelectric material portion 1 is preferably thinner than the second thermoelectric material portion 2. Furthermore, when the electrical resistivity of the first thermoelectric material portion 1 at room temperature is 10 mΩcm or less and the electrical resistivity of the second thermoelectric material portion 2 at room temperature is 1 mΩcm or less and the thermal conductivity is 10 W / mK or more, the thickness of the first thermoelectric material portion 1 is preferably thicker than the thickness of the second thermoelectric material portion 2.

[0027] A 2+δ As for M, in the case of an N-type thermoelectric element, for example, a configuration in which the first thermoelectric material portion 1 is made of Ag—S and the second thermoelectric material portion 2 is made of Ag—Se or Ag—S—Se can be adopted. In the case of a P-type thermoelectric element, for example, a configuration in which the first thermoelectric material portion 1 is made of Cu—S and the second thermoelectric material portion 2 is made of Cu—Se can be adopted. For example, when the first thermoelectric material portion 1 is made of Ag 2 S, and the second thermoelectric material portion 2 is made of Ag 2 It can be formed of Se. 2 S is Ag 2 The absolute value of the Seebeck coefficient is 50 μV / K or more larger than that of Se, and the electrical resistivity is 10 times or more larger than that of Se. 2 The second thermoelectric material portion 2 is made of Cu. 2 It may be formed of Se. 2 S is Cu 2 The absolute value of the Seebeck coefficient is 50 μV / K or more higher than that of Se, and the electrical resistivity is 10 times or more higher. The first thermoelectric material portion 1 may be formed of a material containing at least Bi and Te, such as Bi—Te or Bi—Sb—Te. For example, the first thermoelectric material portion 1 may be formed of Bi 2 Te 3 or (Bi 0.7 Sb 0.3 ) Te 3 The second thermoelectric material portion 2 is formed of Cu0.55 Ni 0.45 (Constantan). 2 Te 3 and (Bi 0.7 Sb 0.3 ) Te 3 is Cu 0.55 Ni 0.45 The absolute value of the Seebeck coefficient is 50 μV / K or more higher and the electrical resistivity is 10 times or more higher than that of the first thermoelectric material portion 1. Note that it is also possible to use the first thermoelectric material portion 1 in which impurities such as Ru or Cu are added to the material containing Bi and Te.

[0028] As described above, the first thermoelectric material unit 1 is made of a semiconductor material or insulating material with high electrical resistance, such as a low thermal conductivity chalcogenide material, and the second thermoelectric material unit 2 is made of a conductive material with low electrical resistance, such as a semiconductor material or alloy. Furthermore, in order to increase the temperature difference applied to the thermoelectric element 10, it is preferable that both the first thermoelectric material unit 1 and the second thermoelectric material unit 2 have low thermal conductivities. In particular, the first thermoelectric material unit 1 preferably has a thermal conductivity of 10 W / mK or less in order to obtain a high thermoelectric power by the Seebeck effect. The thermal conductivity of the first thermoelectric material unit is preferably 0.02 W / mK or more.

[0029] The first thermoelectric material unit 1 may be a thin film, but the second thermoelectric material unit 2 is preferably a bulk conductor thicker than the first thermoelectric material unit 1. The thickness of the first thermoelectric material unit 1 (i.e., the thickness in the stacking direction of the first thermoelectric material unit 1 and the second thermoelectric material unit 2) is preferably 100 nm to 10 mm, and may be 1 μm to 3 mm. The thickness of the second thermoelectric material unit 2 is preferably 0.1 mm to 10 mm, and may be 0.5 mm to 3 mm. When the first thermoelectric material unit 1 and the second thermoelectric material unit 2 are joined via the conductor 2a, a conductive joining material such as solder or In can be used as the conductor 2a. The electrical resistivity of the conductor 2a used in this joining portion is preferably approximately the same as that of the second thermoelectric material unit 2. In many cases, alloy materials and solder materials have approximately the same electrical resistivity (10 -4 For example, Cu as an alloy material 0.55 Ni 0.45When constantan (Constantan) is used, the electrical resistivity of the second thermoelectric material portion 2 and the solder are approximately the same, so that from the viewpoint of electrical conductivity, the solder can be regarded as part of the second thermoelectric material portion 2 for the first thermoelectric material portion 1, thereby increasing the degree of freedom in designing the thermoelectric element. The pair of electrodes 3 can be made of, for example, Ag paste or Ag solder, and are formed on both end surfaces of the joined body 4 by dipping or the like. The material of the pair of electrodes 3 should have an electrical resistivity of 10 -4 The insulating material portion 5 is made of, for example, alumina or SiO 2 It is formed by the following:

[0030] The method for manufacturing the thermoelectric element 10 of this embodiment includes a bonding step of bonding the second thermoelectric material unit 2 and the first thermoelectric material unit 1 together, and an electrode formation step of forming a pair of electrodes 3 on the first thermoelectric material unit 1. For example, in the bonding step, the second thermoelectric material unit 2 and the first thermoelectric material unit 1 are bonded together using a conductive bonding material such as solder. Furthermore, in the bonding step, various thin film growth methods (vapor phase growth methods such as PVD, sputtering, and CVD) are employed. Note that, when a chalcogenide material is used for the first thermoelectric material unit 1, it is preferable to form the first thermoelectric material unit 1 on the second thermoelectric material unit 2 by MBD (molecular beam deposition).

[0031] In the joining step, the first thermoelectric material part 1 may be formed by a sol-gel method on the second thermoelectric material part 2. In the joining step, a hot press method may be used in which, in a state in which powder that will become the first thermoelectric material part 1 and powder that will become the second thermoelectric material part 2 are stacked, the first thermoelectric material part 1 and the second thermoelectric material part 2 are sintered, and the first thermoelectric material part 1 and the second thermoelectric material part 2 are joined together at the same time.

[0032] As described above, in the thermoelectric element 10 of this embodiment, the junction 4 of the first thermoelectric material part 1 and the second thermoelectric material part 2 has end faces on one end side and the other end side, and the pair of electrodes 3 are in contact with the first thermoelectric material part 1 without contacting the second thermoelectric material part 2, and are formed on the end face on one end 1a side and the end face on the other end 1b side of the junction 4, so that surface mounting and miniaturization are possible, and an element with high thermoelectric conversion efficiency and ZT value can be realized. That is, the thermoelectric element 10 of this embodiment is formed entirely as a chip, and the electrodes 3 are formed on both end faces, so that surface mounting by soldering or the like is easy, and the compact shape provides a high degree of freedom in the installation location.

[0033] In this thermoelectric element 10, the first thermoelectric material part 1 has a higher Seebeck coefficient and higher electrical resistivity than the second thermoelectric material part 2, and the pair of electrodes 3 are connected to one end 1a side and the other end 1b side of the first thermoelectric material part 1 at a distance from each other. Therefore, the first thermoelectric material part 1 and the second thermoelectric material part 2 form a parallel circuit, and when a temperature difference occurs between the one end 1a side and the other end 1b side (heat flow occurs), an electromotive force is generated with high thermoelectric conversion efficiency.

[0034] That is, as shown in FIG. 2 , the first thermoelectric material unit 1, which is connected to a pair of electrodes 3 and has a high Seebeck coefficient (absolute value) and high electrical resistance, forms an electromotive voltage path R1 that is mainly dependent on the Seebeck effect, while the second thermoelectric material unit 2, which is joined to and in contact with the first thermoelectric material unit 1 and has a low electrical resistance, forms a current path R2. It is desirable that the current value flowing through the second thermoelectric material unit 2 obeys Ohm's law. By forming a parallel circuit of the electromotive voltage path R1 and the current path R2 in this manner, the current path R2 is formed as a current path separate from the electromotive voltage path R1. This increases the electrical conductivity flowing between the pair of electrodes 3 while maintaining the high Seebeck coefficient (absolute value) of the first thermoelectric material unit 1, thereby achieving a high thermoelectric conversion efficiency and ZT value. Note that the arrow Y in FIG. 2 indicates the heat flow direction (the direction in which heat flux flows, the direction in which a temperature difference occurs).

[0035] Furthermore, since the joined body 4 is provided with a pair of insulating material parts 5 formed to cover at least the second thermoelectric material parts 2 on the end face on one end 1a side and the end face on the other end 1b side, the insulating material parts 5 can prevent the pair of electrodes 3 from contacting the second thermoelectric material parts 2 at the end faces of the joined body 4. Furthermore, since the first thermoelectric material parts 1 are laminated on the upper and lower faces of the second thermoelectric material parts 2, respectively, and the pair of electrodes 3 are connected to the first thermoelectric material parts 1 on the upper and lower faces, respectively, electromotive force paths R1 are formed on the upper and lower faces, and higher thermoelectric conversion efficiency can be obtained.

[0036] Furthermore, since the first thermoelectric material unit 1 has a Seebeck coefficient whose absolute value is 50 μV / K or more higher than that of the second thermoelectric material unit 2 and whose electrical resistivity is 10 times or more higher, a voltage path R1 with a sufficiently high Seebeck effect and a current path R2 with sufficiently high electrical conduction are configured, thereby achieving higher thermoelectric conversion efficiency and ZT value. The absolute value of the Seebeck coefficient of the first thermoelectric material unit 1 may be 100 μV / K or more higher than that of the second thermoelectric material unit 2. The larger the difference between the absolute value of the Seebeck coefficient of the first thermoelectric material unit 1 and the absolute value of the Seebeck coefficient of the second thermoelectric material unit 2, the more desirable it is, and there is no particular upper limit, but it may be 10,000 μV / K.

[0037] The first thermoelectric material portion 1 is made of Ag 2 S, and the second thermoelectric material portion 2 is made of Ag 2 By forming it with Se, Ag 2 S alone, Ag 2 The power factor (PW = S) of the composite thermoelectric element of the present invention is higher than that of Se alone. 2 / ρ) becomes large, and it becomes possible to obtain an N-type thermoelectric element with a ZT value of 1 or more at least at room temperature. 2 The second thermoelectric material portion 2 is made of Cu. 2 By forming it with Se, Cu 2 S element, Cu 2 The power factor (PW = S) of the composite thermoelectric element of the present invention is higher than that of Se alone. 2 / ρ) becomes large, and it becomes possible to obtain a P-type thermoelectric element with a ZT value of 1 or more at least at room temperature. 2 Te3 The second thermoelectric material portion 2 is formed of Cu. 0.55 Ni 0.45 (Constantan), at least Bi 2 Te 3 It is possible to obtain an N-type thermoelectric element having a power factor about twice that of a single body. 0.7 Sb 0.3 ) 2 Te 3 The second thermoelectric material portion 2 is formed of Cu. 0.55 Ni 0.45 (Constantan), at least (Bi 0.7 Sb 0.3 ) 2 Te 3 It is possible to obtain a P-type thermoelectric element having a power factor about twice that of a single element.

[0038] Next, second and third embodiments of the thermoelectric element according to the present invention will be described below with reference to Fig. 3 to Fig. 6. In the following description of each embodiment, the same components as those described in the above embodiments are denoted by the same reference numerals, and the description thereof will be omitted.

[0039] The second embodiment differs from the first embodiment in that, in the first embodiment, the first thermoelectric material portion 1 is bonded to the upper and lower surfaces of the second thermoelectric material portion 2, respectively, and a pair of electrodes 3 is connected to the first thermoelectric material portions 1 on the upper and lower surfaces, respectively, whereas in the thermoelectric element 20 of the second embodiment, the first thermoelectric material portion 1 is also bonded to both side surfaces of the second thermoelectric material portion 2, respectively, and a pair of electrodes 3 is also connected to the first thermoelectric material portions 1 on both side surfaces, respectively, as shown in Figures 3 and 4. The bonded body 4 is formed in the shape of a plate or rectangular parallelepiped chip, and the upper and lower surfaces of the second thermoelectric material portion 2 are perpendicular to both side surfaces of the second thermoelectric material portion 2.

[0040] That is, in the second embodiment, the first thermoelectric material part 1 covers the entire outer peripheral surface of the second thermoelectric material part 2, and the first thermoelectric material part 1 is joined to all four outer peripheral surfaces of the second thermoelectric material part 2. In this way, in the thermoelectric element 20 of the second embodiment, the first thermoelectric material part 1 is joined to both side surfaces of the second thermoelectric material part 2, and a pair of electrodes 3 is connected to each of the first thermoelectric material parts 1 on both side surfaces, so that electromotive voltage paths R1 are formed not only on the top and bottom surfaces but also on both side surfaces, and thus even higher thermoelectric conversion efficiency can be obtained.

[0041] Next, the third embodiment differs from the second embodiment in that, while in the second embodiment the first thermoelectric material part 1 is joined to the top, bottom and both side surfaces of the second thermoelectric material part 2, in the thermoelectric element 30 of the third embodiment, as shown in FIG. 5 , the first thermoelectric material part 1 is joined to both end surfaces of the second thermoelectric material part 2, and a pair of electrodes 3 is formed on the first thermoelectric material part 1 on each of the end surfaces.

[0042] That is, in the third embodiment, the entire surface of the chip-shaped second thermoelectric material portion 2 is covered with the first thermoelectric material portion 1. As described above, in the thermoelectric element 30 of the third embodiment, the first thermoelectric material portion 1 is joined to both end faces of the second thermoelectric material portion 2, and a pair of electrodes 3 is formed on the first thermoelectric material portions 1 on the end faces. Therefore, an electromotive voltage path R1 is formed from the pair of electrodes 3 to each first thermoelectric material portion 1 on the outer peripheral surface via the first thermoelectric material portions 1 on the end faces, thereby achieving higher thermoelectric conversion efficiency. Furthermore, there is no need to form insulating material portions on both end faces of the second thermoelectric material portion 2, which reduces the manufacturing process.

[0043] In order to demonstrate the principles of the thermoelectric properties of the present invention, a sample as shown in FIG. 6 was fabricated as an example, and the evaluation results are shown in Tables 1 and 2. In the examples of the present invention, the first thermoelectric material portion and the second thermoelectric material portion were fabricated using the materials and manufacturing methods described in the above embodiment, and their thermoelectric properties (conductivity type determination (P / N type determination), Seebeck coefficient, electrical resistivity, and power factor) at room temperature (300 K) were investigated. Furthermore, as a comparative example of the present invention, a thermoelectric element fabricated using only the thermoelectric material was evaluated in the same manner as in the examples of the present invention. Each example was fabricated as follows. Note that in the examples of the present invention, for evaluation purposes, the first thermoelectric material portion 1 was joined only to the top surface of the second thermoelectric material portion 2. Furthermore, a pair of electrodes 3 was formed on the top surface of the first thermoelectric material portion 1.

[0044] Examples 1 and 2 and Examples 9 to 12 (Solder Bonding) First, a Bi-Te bulk sintered body (or a Bi-Sb-Te bulk sintered body) for the first thermoelectric material part and a Cu-Ni alloy plate or Cu plate for the second thermoelectric material part were prepared and cut to a predetermined size, and the bonding surfaces were polished. Subsequently, solder foil was placed on the bonding surface between the Bi-Te bulk sintered body and the Cu-Ni alloy plate or Cu plate, and the Bi-Te bulk sintered body and the Cu-Ni alloy plate or Cu plate were bonded using a hot press machine by utilizing solder melting. That is, the second thermoelectric material part was bonded to the first thermoelectric material part via an intermediate layer of solder as a conductor. The bonding conditions were a pressure of 100 MPa, a bonding temperature of 250°C, and a holding time of approximately 5 minutes. After visually confirming that the solder had melted, a cooling process and a pressure reduction process were carried out. Thereafter, two pairs of electrodes were formed on the first thermoelectric material part side (Bi—Te side) using Ag paste or the like, to form Examples 1 and 2.

[0045] Example 3 (MBD Film Formation) First, an Ag film for the second thermoelectric material portion was formed in an MBD (molecular beam deposition) device. 2 On the Se bulk sintered body, Ag which will be the first thermoelectric material part is 2 A thin film of Ag was formed. 2The Se bulk sintered body was formed by the SHS (Self-Propagating High Temperature Synthesis) method. In the film formation by the MBD method, the substrate temperature was set to room temperature, and the cell containing the raw materials Ag and S was heated to an appropriate temperature by a heater to form a film. 2 A single-phase thin film of Ag was obtained by X-ray diffraction experiments. 2 S thin film, Ag 2 It has been confirmed that the sintered bulk Se is a crystalline material. 2 S 1-x Se x In the system, in the low-temperature phase near room temperature below the phase transition temperature, when x≦0.6, Ag 2 It has the same crystal structure as Ag(x) (monoclinic, space group P21 / c), and when x≧0.7, it is 2 It has the same crystal structure as Se (orthorhombic, space group P212121) (in the composition range of 0.6<x<0.7, it takes on a mixed phase or a different crystal structure depending on the film formation conditions). The electrode was fabricated in the same manner as in Examples 1 and 2.

[0046] <Examples 4 to 8> <Examples 13 to 17> (Hot Press) First, raw material powders (e.g., Ag, S, Cu, etc.) for the first thermoelectric material portion and the second thermoelectric material portion were weighed and mixed so as to have a predetermined stoichiometric ratio, and then molded using a press. After that, by heat treatment at a predetermined temperature, for example, Ag 2 A single-phase sintered body of S can be obtained. When using a chalcogenide containing S, Se, or Te, a single-phase sintered body can also be obtained using the self-heating reaction method. If an unreacted phase is confirmed by the X-ray diffraction experiment, the sintered body is crushed into powder and the above process is repeated. Since a single-phase sintered body is obtained by the X-ray diffraction experiment, this process is repeated.

[0047] After the single-phase sintered body is obtained, the sintered body is pulverized using a mortar or the like, and then, for example, Ag 2 S, Ag 2 Se, Cu 2-δ S, Cu 2-δUsing these powders, a hot press is used to heat and pressurize the powders to produce bulk bodies of the first thermoelectric material part and the second thermoelectric material part, and at the same time, a bonded body of the first thermoelectric material part and the second thermoelectric material part is produced. Note that, during the hot press, Ag is used in consideration of density. 2 S, Ag 2 Se, Cu 2-δ S, Cu 2-δ Se is weighed to a predetermined thickness, and the raw materials are added in order and molded.

[0048] The bonding conditions using a hot press were a pressure of 100 MPa, a predetermined holding temperature, and a holding time of 20 minutes to form a bonded body. The bonded body was then cut using a wire saw or the like to obtain a chip-shaped bonded body measuring, for example, 17 mm x 3 mm x 2 mm. The electrode was fabricated in the same manner as in Examples 1 and 2.

[0049] <Method for Evaluating Thermoelectric Elements> When a temperature difference ΔT is applied to a thermoelectric element, a voltage ΔV proportional to the temperature difference is generated. This phenomenon is called the Seebeck effect, and the generated voltage is called thermoelectromotive force. The proportionality coefficient S = ΔV / ΔT is defined as the Seebeck coefficient S. In other words, measuring the Seebeck coefficient requires both measuring the potential difference (thermoelectromotive force) between two terminals and the temperature difference. The Seebeck coefficient was measured using two commercially available Peltier elements, with one Peltier element cooled and the other heated, creating a temperature difference between the two Peltier elements. The thermocouple used for measurement was a T-type thermocouple (Cu-Constantan). An ultra-thin thermocouple (approximately 20 microns thick) was selected. Furthermore, a load was applied using a rubber material with high electrical insulation and thermal insulation properties, ensuring good thermal and electrical contact between the material and the thermocouple. Furthermore, a two-terminal method known as a thermoelectric probe was employed, using Cu wiring of two T-type thermocouples to measure the potential difference (thermoelectric power) between the two terminals. The relationship between the thermoelectric power ΔV and the temperature difference ΔT was plotted, and the Seebeck coefficient was evaluated from the linear relationship near zero temperature difference (near the origin of ΔV / ΔT). The P-type and N-type conductivity (conductivity type) were determined from the sign of the measured Seebeck coefficient. Furthermore, when joining the first thermoelectric material part and the second thermoelectric material part, it is desirable to align the P-type / N-type polarities, i.e., joining P-type to P-type or N-type to N-type, but it is also possible to join opposite polarities, i.e., joining P-type to N-type. Even in this case, the first thermoelectric material part has a higher absolute Seebeck coefficient and a higher electrical resistivity than the second thermoelectric material part to which it is joined.

[0050] The electrical resistivity (electrical conductivity) was measured by a four-terminal method. In this measurement, both a terminal for measuring current and a terminal for measuring voltage were connected to the electrode terminal. When calculating the electrical resistivity from the electrical resistance value, the sum of the thicknesses of multiple materials was used. For example, in Example 4, the thickness of the 0.1 mm Ag 2 S (first thermoelectric material part) and 2 mm of Ag 2When determining the electrical resistivity of the bonded body with Se (second thermoelectric material portion), the thickness was set to 2.1 mm, which is the sum of the thicknesses of the two materials. The power factor is expressed as the product of the square of the Seebeck coefficient and the reciprocal of the electrical resistivity (=electrical conductivity), and was calculated from the measured Seebeck coefficient and electrical resistivity.

[0051]

[0052] As can be seen from the above evaluation results, the examples of the present invention all have significantly improved power factors compared to the comparative examples in which the first or second thermoelectric material section is made of a single material. The absolute values ​​of the Seebeck coefficients of the Bi-Te-based materials in Comparative Examples 1 and 2 are 50 μV / K or more greater than the absolute value of the Seebeck coefficient of the Cu-Ni material in Comparative Example 3, and the electrical resistivity of the Bi-Te-based materials in Comparative Examples 1 and 2 is 10 times or more greater than the electrical resistivity of the Cu-Ni material in Comparative Example 3. Therefore, in Examples 1 and 2 in which the first thermoelectric material section is made of a Bi-Te-based material and the second thermoelectric material section is made of Cu-Ni, both an electromotive voltage path with a sufficiently high Seebeck effect and a current path with sufficiently high electrical conductivity are formed, thereby increasing both the electromotive voltage value and the current value output from between the pair of electrodes and significantly improving the power factor. N-type characteristics are obtained in Example 1, and P-type characteristics are obtained in Example 2.

[0053] Ag of Comparative Example 4 2 The absolute value of the Seebeck coefficient of S is 2 The absolute value of the Seebeck coefficient is 50 μV / K or more larger than that of Se, and Ag of Comparative Example 4 2 The electrical resistivity of S is 2 The electrical resistivity of the first thermoelectric material portion is 10 times or more larger than that of Se. 2 The second thermoelectric material is made of S-based material, and the second thermoelectric material is made of Ag 2In Examples 3 to 6, in which Se was used, both an electromotive voltage path with a sufficiently high Seebeck effect and a current path with a sufficiently high electrical conductivity were formed, thereby increasing both the electromotive voltage value and the current value output from between the pair of electrodes, and significantly improving the output factor. Note that Example 5 exhibits N-type characteristics, while Example 4 exhibits P-type characteristics. However, since this material normally exhibits N-type characteristics, it is believed that Example 4 exhibited P-type characteristics due to impurities, crystal defects, etc.

[0054] In addition, Cu in Comparative Example 6 2 The absolute value of the Seebeck coefficient of S is 2 The absolute value of the Seebeck coefficient is 50 μV / K or more larger than that of Se, and the Cu of Comparative Example 6 2 The electrical resistivity of S is 2 The electrical resistivity of the first thermoelectric material portion is 10 times or more larger than that of Se. 2-δ The second thermoelectric material is made of S-based material, and the second thermoelectric material is made of Cu. 2-δ In Examples 7, 8, and 13 to 17 in which Se was used, both an electromotive voltage path with a sufficiently high Seebeck effect and a current path with a sufficiently high electrical conductivity were configured, and as a result, both the electromotive voltage value and the current value output from between the pair of electrodes became large, and the output factor was significantly improved.

[0055] Furthermore, the absolute values ​​of the Seebeck coefficients of the Bi—Te based materials of Comparative Examples 1 and 2 are at least 50 μV / K greater than the absolute value of the Seebeck coefficient of Cu of Comparative Example 8, and the electrical resistivity of the Bi—Te based materials of Comparative Examples 1 and 2 is at least 10 times greater than the electrical resistivity of Cu of Comparative Example 8. Therefore, in Examples 9 to 12 in which the first thermoelectric material section is made of a Bi—Te based material and the second thermoelectric material section is made of Cu, both an electromotive voltage path with a sufficiently high Seebeck effect and a current path with sufficiently high electrical conductivity are configured, and as a result, the electromotive voltage value and current value output from between the pair of electrodes both become large, and the output factor is significantly improved.

[0056] The first thermoelectric material portion is Ag 2 S, the second thermoelectric material portion is Ag 2 In the example, Ag 2 S, Ag 2It has been confirmed that Se has a thermal conductivity of less than 1 W / mK at room temperature. For example, in Example 4, a high thermoelectric performance with a ZT value of approximately 3 at room temperature was obtained. Furthermore, a pi-shaped thermoelectric conversion module with four elements was fabricated using two Bi-Te / Cu-Ni elements exhibiting N-type characteristics as in Example 1 and two Bi-Sb-Te / Cu-Ni elements exhibiting P-type characteristics as in Example 2, and the power generation performance was compared with that of a pi-shaped thermoelectric conversion module with four elements consisting only of Bi-Te (Comparative Example 1) and Bi-Sb-Te (Comparative Example 2). As a result, it was confirmed that the thermoelectric conversion module using the elements of the example had a 38.4% improvement in power generation output when a temperature difference of 30 K was applied (the temperature on the low-temperature side was approximately 20°C near room temperature).

[0057] Examples 21 to 25 (Hot Pressing) Examples 21 to 25 of the present invention were fabricated by the same manufacturing method as the above-described Examples 4 to 6, and the temperature dependence of the thermoelectric properties was evaluated for Examples 21 to 25. Note that in Example 22, the second thermoelectric material part was joined by hot pressing to the first thermoelectric material part via an intermediate layer of Ag as a conductor, and in Example 23, via an intermediate layer of In as a conductor.

[0058] In the evaluation method of Examples 1 to 17, the thermoelectric properties were measured at room temperature (25°C), but in Examples 21 to 25 of the present invention, the thermoelectric properties were measured at high temperatures of 88 to 95°C. In Examples 21 to 25, the first thermoelectric material portion was made of Ag 2 S, the second thermoelectric material portion is Ag 2 The results are shown in Table 2. As can be seen from the evaluation results of Examples 21 to 25, a high Seebeck coefficient (absolute value) was maintained even at a measurement temperature of 88 to 95°C, and the power factor was significantly improved. 2 S alone and Ag 2 The power factor of Se alone is 2 x 10 -3 W / mK 2 The thermoelectric elements of Examples 21 to 25 have significantly higher thermoelectric conversion properties than single elements. The thermal conductivity of the thermoelectric elements of Examples 21 to 25 is 1.2 W / mK or less. In Examples 24 and 25, the ZT value (=S2 T / ρκ): where S, T, ρ, and κ are the Seebeck coefficient, absolute temperature, electrical resistivity, and thermal conductivity, respectively. In Example 21, a ZT value of 5 or more was measured, indicating that very high thermoelectric conversion properties were obtained.

[0059]

[0060] Evaluation of power generation characteristics Next, as Example 26, a first thermoelectric material portion was formed of Ag 2 S, the second thermoelectric material portion is Ag 2 S 0.5 Se 0.5 The power generation characteristics of the thermoelectric element were evaluated. 2 S and Ag 2 S 0.5 Se 0.5 Both show N-type characteristics. 2 S and Ag 2 S 0.5 Se 0.5 The bonding was performed by hot pressing at a temperature of 200° C. or less. In Example 26, no intermediate layer was used, and the element was directly bonded. 2 The thickness of S is 10 μm, and the thickness of the second thermoelectric material part is Ag 2 S 0.5 Se 0.5 The thickness of the element was 0.70 mm. The width of the element was 2.2 mm. The distance between the pair of electrodes was 2.91 mm. The electrodes were needle electrodes, which were brought into dotted line contact with the first thermoelectric material portion to evaluate the power generation characteristics.

[0061] FIG. 7 shows the Ag of Example 26 of the present invention. 2 S / Ag 2 S 0.5 Se 0.5The results of evaluating the power generation characteristics of a thermoelectric element are shown below. To evaluate the power generation characteristics, a closed circuit consisting of a thermoelectric element, a variable resistance element (external load resistance element), and an ammeter was constructed. A temperature difference was applied across the thermoelectric element, and the voltage, current, and power output from the thermoelectric element were measured. Figure 7 shows the output voltage (shown on the left axis) and power generation density (shown on the right axis) versus current. Because the thermoelectric element of Example 26 exhibits N-type characteristics, the voltage values ​​are negative. However, the voltage values ​​shown on the left axis of Figure 7 are absolute values. The amount of power generation is expressed as the product of the voltage and current values. The power generation density is calculated by dividing the amount of power generation by the cross-sectional area of ​​the element (the product of the element thickness and width). Figure 7 plots actual measured values, and the calculated value based on the actual measured values ​​is displayed as a line. The voltage value when the output current is zero is called the open-circuit voltage. The current value when the output voltage is 0 V is called the short-circuit current. FIG. 7 also shows the results of evaluating the open-circuit voltage when the low-temperature side temperature of the element is set to 50° C., 60° C., and 70° C., and the temperature difference is set to 3 K.

[0062] As a result of evaluating the power generation characteristics of the thermoelectric element of Example 26, when the low-temperature side temperature of the element was 60°C, the open-circuit voltage was 0.59 mV, the short-circuit current was 191 μA, and the power generation output density was 1.7 μW cm ―2 The absolute value of the Seebeck coefficient calculated from the open circuit voltage was 196 μV / K. 2 S 0.5 Se 0.5 Since the absolute value of the Seebeck coefficient of the Ag single material is 130 μV / K, it can be seen that the output voltage of Example 26 is increased. 2 The electrical resistivity of S alone is high, and the short-circuit current value of Example 26 is 2 It is more than 1000 times larger than S alone. 2 S alone, Ag 2 S 0.5 Se 0.5 The power generation output density of each unit is 0.1 μW cm ―2 Less than 1.0 μW cm ―2 In contrast, the Ag of Example 26 2 S / Ag 2 S 0.5 Se 0.5The power generation output density of the thermoelectric element (= 1.7 μW cm ―2 ) is large, and it is clear that extremely high thermoelectric conversion properties are obtained compared to a single element.

[0063] The technical scope of the present invention is not limited to the above-described embodiments and examples, and various modifications can be made without departing from the spirit of the present invention. For example, in the above-described embodiments, the thermoelectric element of the present invention is described as being used for power generation, but the thermoelectric element of the present invention may also be used for Peltier cooling, Peltier temperature control, etc. Furthermore, although the thermoelectric element shown in FIG. 3 has a rectangular prism shape, it may also have a cylindrical shape (a combination of a cylindrical first thermoelectric material portion and a cylindrical second thermoelectric material portion) or a polygonal prism shape.

[0064] REFERENCE SIGNS LIST 1...first thermoelectric material portion, 1a...one end portion, 1b...other end portion, 2...second thermoelectric material portion, 2a...conductor, 3...electrode, 4...junction body, 5...insulating material portion, 10, 20, 30...thermoelectric element

Claims

1. A thermoelectric element comprising: a first thermoelectric material part having one end and another end; a second thermoelectric material part joined to the first thermoelectric material part directly or via an electric conductor; and a pair of electrodes connected to the first thermoelectric material part, wherein the first thermoelectric material part has a higher absolute value of Seebeck coefficient and a higher electrical resistivity than the second thermoelectric material part, a joint between the first thermoelectric material part and the second thermoelectric material part has end faces on the one end side and the other end side, and the pair of electrodes are in contact with the first thermoelectric material part without contacting the second thermoelectric material part, and are formed on the end face on the one end side and the end face on the other end side of the joint.

2. A thermoelectric element as claimed in claim 1, characterized in that it comprises a pair of insulating material sections formed to cover at least the second thermoelectric material section at an end face on the one end side and an end face on the other end side of the junction.

3. A thermoelectric element as described in claim 1, characterized in that the first thermoelectric material part is joined to the upper and lower surfaces of the second thermoelectric material part, respectively, and the pair of electrodes is connected to each of the first thermoelectric material parts on the upper and lower surfaces.

4. A thermoelectric element as described in claim 3, characterized in that the first thermoelectric material part is also joined to both side surfaces of the second thermoelectric material part, and the pair of electrodes is also connected to each of the first thermoelectric material parts on both side surfaces.

5. A thermoelectric element as described in claim 3, characterized in that the first thermoelectric material part is also joined to both end faces of the second thermoelectric material part, and the pair of electrodes are formed on the first thermoelectric material part on both end faces.

6. A thermoelectric element as claimed in claim 1, characterized in that the first thermoelectric material section has a Seebeck coefficient whose absolute value is 50 μV / K or more greater than that of the second thermoelectric material section, and an electrical resistivity which is 10 times or more greater.

7. The thermoelectric element according to claim 1, wherein the first thermoelectric material section and the second thermoelectric material section are both A 2+δ A thermoelectric element comprising: a first metal, a second metal, and a third metal, each of which is selected from the group consisting of A, Ag, Cu, and M, and which is at least one of S, Se, and Te.

8. A thermoelectric element according to claim 7, characterized in that the first thermoelectric material portion is formed of Ag-S, and the second thermoelectric material portion is formed of Ag-Se or Ag-S-Se.

9. A thermoelectric element according to claim 7, characterized in that the first thermoelectric material portion is made of Cu--S, and the second thermoelectric material portion is made of Cu--Se.

10. A thermoelectric element according to claim 1, wherein the first thermoelectric material portion is formed of a material containing at least Bi and Te.

Citation Information

Patent Citations

  • Thermoelectric transducer and thermoelectric conversion power generator

    JP2013042113A

  • Nitride thermoelectric conversion material, manufacturing method therefor and thermoelectric conversion element

    JP2016184599A

  • Semiconductor material for thermoelectric conversion and thermoelectric conversion element using the same

    JP2022018710A

  • Split thermo-electric cycles for simultaneous cooling, heating, and temperature control