Solid electrolyte and method for producing same

By integrating nitrogen into the sulfide solid electrolyte with specific molar ratios and using ammonium halides, the generation of hydrogen sulfide is suppressed, addressing the stability and safety issues in sulfide solid electrolytes, thus enhancing the performance of all-solid-state batteries.

WO2024203814A1PCT designated stage expired Publication Date: 2024-10-03MITSUI MINING & SMELTING CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011219
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-03-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Sulfide solid electrolytes used in all-solid-state batteries can react with moisture to generate hydrogen sulfide, compromising their stability and safety.

Method used

Incorporating nitrogen (N) into the sulfide solid electrolyte composition, specifically with a molar ratio of lithium (Li) to sulfur (S) to phosphorus (P) between 1.5 and 2.2, and lithium (Li) plus halogen (X) to phosphorus (P) between 7.1 and 10.0, while using ammonium halides in the manufacturing process, to suppress hydrogen sulfide generation.

Benefits of technology

The modified electrolyte effectively reduces hydrogen sulfide production, enhancing safety and maintaining the electrolyte's characteristics, thereby improving the performance and durability of solid-state batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011219_03102024_PF_FP_ABST
    Figure JP2024011219_03102024_PF_FP_ABST
Patent Text Reader

Abstract

This solid electrolyte contains elemental lithium, elemental phosphorus, elemental sulfur, elemental halogen, and elemental nitrogen. The molar ratio of the difference between the amounts of elemental lithium and elemental sulfur to the amount of elemental phosphorus is 1.5-2.2. The molar ratio of the sum of the amounts of elemental lithium and elemental halogen to the amount of elemental phosphorus is preferably 7.1-10.0. The X-ray diffraction pattern measured by an X-ray diffractometer preferably has peaks at positions of 2θ=25.5°±1.0°, 29.8°±0.5°, and 31.2°±1.0°.
Need to check novelty before this filing date? Find Prior Art

Description

Solid electrolyte and method for producing the same

[0001] The present invention relates to a solid electrolyte and a method for producing the same.

[0002] In recent years, CO 2 Secondary batteries have been attracting attention as an effort to prevent global warming by reducing CO2 emissions. Among these, all-solid-state batteries using sulfide solid electrolytes synthesized using starting materials such as lithium sulfide have attracted attention. All-solid-state batteries using sulfide solid electrolytes do not use flammable organic solvents, which allows for simplified safety devices and offers advantages such as low manufacturing costs and productivity. Furthermore, this type of solid electrolyte is advantageous from the perspective of improving safety and durability, since ionic species other than lithium ions do not migrate within the electrolyte, preventing side reactions due to the migration of anions.

[0003] As the solid electrolyte, for example, a sulfide solid electrolyte containing lithium (Li), phosphorus (P), sulfur (S), and a halogen element has been proposed (see Patent Documents 1 and 2).

[0004] US2020 / 091552A1US2020 / 127325A1

[0005] Since sulfide solid electrolytes are substances containing sulfur, there is a possibility that sulfur may react with moisture to generate hydrogen sulfide depending on the environment. Therefore, an object of the present invention is to provide a solid electrolyte in which the generation of hydrogen sulfide is suppressed.

[0006] As a result of intensive research conducted by the present inventors to solve the above-mentioned problems, it was discovered that by reducing the sulfur (S) element in a sulfide solid electrolyte while incorporating nitrogen (N), it is possible to suppress the amount of hydrogen sulfide generated while maintaining the properties of the solid electrolyte. The present invention was made based on this discovery, and solves the above-mentioned problems by providing a solid electrolyte comprising lithium (Li), phosphorus (P), sulfur (S), a halogen (X), and nitrogen (N), wherein the molar ratio of the difference between the lithium (Li) element and the sulfur (S) element to the phosphorus (P) element is 1.5 or more and 2.2 or less, and the molar ratio of the sum of the lithium (Li) element and the halogen (X) element to the phosphorus (P) element is 7.1 or more and 10.0 or less.

[0007] The present invention also provides a method for producing a solid electrolyte containing lithium (Li), phosphorus (P), sulfur (S), a halogen (X), and nitrogen (N), the method comprising a step of firing a raw material composition for the solid electrolyte, the raw material composition including one or more compounds containing at least one of lithium (Li), phosphorus (P), sulfur (S), and a halogen (X), and including an ammonium halide.

[0008] Fig. 1 shows X-ray diffraction patterns of the solid electrolytes obtained in Examples 1, 2, 3, and 4 and Comparative Examples 1 and 3. Fig. 2 shows X-ray diffraction patterns of the solid electrolytes obtained in Example 5 and Comparative Example 2. Fig. 3 shows an enlarged view of a main portion of the X-ray diffraction pattern of the solid electrolyte obtained in Example 1, and an enlarged view of a main portion of the X-ray diffraction pattern of the solid electrolyte obtained in Comparative Example 1. Fig. 4 is a graph showing the initial charge-discharge characteristics of solid batteries containing the solid electrolytes obtained in Examples 1 and 2.

[0009] The present invention will be described below based on preferred embodiments. The solid electrolyte of the present invention contains lithium (Li), phosphorus (P), sulfur (S), halogen (X), and nitrogen (N). That is, the solid electrolyte of the present invention is a sulfide solid electrolyte.

[0010] Examples of the X element include at least one of fluorine (F), chlorine (Cl), bromine (Br), and iodine (I). In particular, from the viewpoint of increasing lithium ion conductivity, the solid electrolyte may contain at least Cl or Br as the X element, or may contain Cl and Br.

[0011] The solid electrolyte of the present invention can suppress the generation of hydrogen sulfide by containing elemental nitrogen. The reason for this is not clear, but it is presumed to be as follows. That is, when the solid electrolyte contains elemental nitrogen, some of the P-S bonds in the solid electrolyte are replaced with P-N bonds, resulting in a decrease in the content of elemental sulfur and suppression of the generation of hydrogen sulfide. In addition, when the solid electrolyte comes into contact with water, the reaction between the P-N bonds and water occurs preferentially over the reaction between the P-S bonds and water, which is thought to result in the suppression of the generation of hydrogen sulfide.

[0012] The N element may be substituted for some of the constituent elements in a compound containing the Li element, the P element, the S element, and the X element. Alternatively, the N element may exist independently, separate from the compound containing the Li element, the P element, the S element, and the X element. In the present invention, from the viewpoint of the above-mentioned mechanism of action, it is preferable that the N element be substituted for some of the constituent elements in a compound containing the Li element, the P element, the S element, and the X element.

[0013] When the N element exists independently from the solid electrolyte containing the Li, P, S, and X elements, the N element can exist as a compound containing the N element (hereinafter also referred to as an "N-element-containing compound"). The N-element-containing compound is not particularly limited, but examples thereof include ammonium halides. Examples of ammonium halides include ammonium chloride, ammonium bromide, and ammonium iodide. Only one type of N-element-containing compound may be present in the solid electrolyte, or two or more types may be present. From the viewpoint of more effectively exhibiting the performance of a battery using the solid electrolyte of the present invention, the N-containing compound is preferably ammonium chloride.

[0014] The solid electrolyte containing Li, S, P, and X elements is not particularly limited as long as it is a material that functions as a solid electrolyte, and examples thereof include conventionally known sulfide solid electrolytes. 2 S-P 2 S 5 , Li 2 S-P 2 S 5 -LiX, Li 2 S-P 2 S 5 -P 2 O 5 , Li 2 S-Li 3 P.O. 4 -P 2 S 5 , Li 3 P.S. 4 , Li 4 P 2 S 6 , Li 10 GeP 2 S 12 , Li 3.25 Ge 0.25 P 0.75 S 4 , Li 7 P 3 S 11 , Li 3.25 P 0.95 S 4 , Li a P.S. b X c (wherein a is a number of 3.0 or more and 6.0 or less, b is a number of 3.5 or more and 4.8 or less, and c is a number of 0.1 or more and 3.0 or less).

[0015] In the solid electrolyte of the present invention, when the molar ratio of the difference between Li and S elements to P element is expressed as (Li-S) / P, the value of (Li-S) / P is preferably 1.5 or more, more preferably 1.6 or more, and even more preferably 1.7 or more. Furthermore, the value of (Li-S) / P is, for example, preferably 2.2 or less, more preferably 2.0 or less, and even more preferably 1.8 or less. By having the value of (Li-S) / P within the above range, the generation of hydrogen sulfide can be more effectively suppressed. Note that "the molar ratio of the difference between Li and S elements to P element" refers to the ratio of the difference between Li and S elements to P element when the solid electrolyte has, for example, a composition formula Li 7-x P.S. 6-x X x In the case where x is the number of digits, {(7-x)-(6-x)} / 1=1.

[0016] From the viewpoint of more effectively suppressing hydrogen sulfide from the solid electrolyte, in the solid electrolyte of the present invention, when the molar ratio of the sum of Li element and X element to P element is expressed as (Li + X) / P, the value of (Li + X) / P is, for example, preferably 7.1 or more, more preferably 7.2 or more, and even more preferably 7.25 or more. From the same viewpoint, the value of (Li + X) / P is, for example, preferably 10.0 or less, more preferably 8.5 or less, and even more preferably 7.6 or less. Note that the "molar ratio of the sum of Li element and X element to P element" refers to the ratio of the sum of Li element and X element to P element when the solid electrolyte has, for example, a composition formula Li 7-x P.S. 6-x X x In the case where x is expressed as {(7-x)+x} / 1=7.

[0017] From the viewpoint of more effectively suppressing the generation of hydrogen sulfide from the solid electrolyte, in the solid electrolyte of the present invention, when the molar ratio of S element to P element is defined as S / P, the value of S / P is, for example, preferably 2.0 or more, more preferably 2.5 or more, even more preferably 2.9 or more, and even more preferably 3.1 or more. By appropriately increasing the amount of S element relative to P element, it is possible to obtain S (for example, P) crosslinked with P, which has a chemical structure that is highly reactive with water and easily generates hydrogen sulfide gas. 2 S 74- etc.), and generates less hydrogen sulfide gas. 4 3― On the other hand, the value of S / P is preferably, for example, 4.5 or less, more preferably 4.0 or less, and even more preferably 3.5 or less. By appropriately reducing the amount of S element relative to P element, it is possible to obtain S which does not bond with P and has high reactivity. 2- PS, which suppresses the generation of hydrogen sulfide gas and produces less hydrogen sulfide gas 4 3- It can accelerate the creation of units.

[0018] From the viewpoint of more effectively suppressing hydrogen sulfide from the solid electrolyte, in the solid electrolyte of the present invention, when the molar ratio of X element to P element is defined as X / P, the value of X / P is, for example, preferably 1.5 or more, more preferably 1.9 or more, and even more preferably 2.2 or more. On the other hand, from the viewpoint of sufficiently increasing the ionic lithium conductivity of the solid electrolyte, the value of X / P is, for example, preferably 4.5 or less, more preferably 3.5 or less, even more preferably 2.8 or less, and even more preferably 2.5 or less.

[0019] As described above, the solid electrolyte of the present invention contains N element. The inclusion of N element in the solid electrolyte suppresses the generation of hydrogen sulfide from the solid electrolyte. To effectively achieve this advantage, the amount of N element contained in the solid electrolyte, expressed as N / P (the molar ratio of N element to P element), is preferably 0.01 or more, more preferably 0.05 or more, even more preferably 0.06 or more, and even more preferably 0.1 or more. From the viewpoint of sufficiently increasing the lithium ion conductivity of the solid electrolyte, the amount of N element contained in the solid electrolyte is preferably 0.5 or less, even more preferably 0.4 or less, even more preferably 0.25 or less, and even more preferably 0.2 or less. Taking the above into consideration, in the solid electrolyte of the present invention, the N / P value is preferably 0.01 or more and 0.5 or less, even more preferably 0.05 or more and 0.4 or less, even more preferably 0.06 or more and 0.25 or less, and even more preferably 0.1 or more and 0.2 or less.

[0020] The amounts of each element constituting the solid electrolyte, including Li (but excluding N and S), can be measured by, for example, ICP atomic emission spectrometry. The amount of N can be measured using an oxygen, nitrogen, and hydrogen analyzer. The amount of S can be measured by barium sulfate gravimetry. The above-mentioned molar ratios (Li-S) / P and (Li+X) / P can be calculated based on the measured amounts of each element.

[0021] The solid electrolyte of the present invention may contain elements other than Li, P, S, X, and N. For example, part of the Li element may be replaced with another alkali metal element, part of the P element may be replaced with another pnictogen element, or part of the S element may be replaced with another chalcogen element such as oxygen (O). In addition to the above-mentioned elements, the solid electrolyte of the present invention may contain impurities to the extent that the effects of the present invention are not impaired. The content of the impurities may be, for example, less than 5 mol%, preferably less than 3 mol%, and particularly less than 1 mol%.

[0022] The solid electrolyte of the present invention may be a crystalline material or an amorphous material such as glass ceramics or glass. When the solid electrolyte of the present invention is a crystalline material, it is preferable that the solid electrolyte contains a crystalline phase having, for example, an argyrodite-type crystalline structure, from the viewpoint of effectively improving ionic conductivity. The argyrodite-type crystalline structure is represented by the chemical formula: Ag 8 GeS 6 This is the crystal structure of a group of compounds derived from minerals represented by the formula:

[0023] Among sulfide solid electrolytes, conventional solid electrolytes containing a crystalline phase having an argyrodite-type crystal structure are prone to generating hydrogen sulfide, whereas the solid electrolyte of the present invention has a low content of element S and a high content of element X, and therefore suppresses the generation of hydrogen sulfide compared to conventional solid electrolytes. Thus, even when the solid electrolyte of the present invention contains a crystalline phase having an argyrodite-type crystal structure, the effect of suppressing the generation of hydrogen sulfide can be made more pronounced.

[0024] In the solid electrolyte of the present invention, it is preferable that characteristic diffraction peaks resulting from a crystalline phase are observed at 2θ=25.5°±1.0°, 29.8°±0.5°, and 31.2°±1.0° in a diffraction pattern measured by XRD using CuKα1 radiation, from the viewpoint of further suppressing the generation of hydrogen sulfide from the solid electrolyte.

[0025] In addition to the diffraction peaks, it is preferable that characteristic diffraction peaks are also observed at 2θ=44.7°±1.0°, 47.8°±1.0°, and 52.5°±1.0°, from the viewpoint of further suppressing the generation of hydrogen sulfide from the solid electrolyte.

[0026] Furthermore, it is particularly preferable that the solid electrolyte of the present invention has at least two peaks at 2θ = 25.5° ± 1.0° in an X-ray diffraction pattern measured by XRD using CuKα1 radiation, since this further suppresses the generation of hydrogen sulfide from the solid electrolyte. In this case, it is particularly preferable that the ratio of the peak intensity of the next most intense peak to the peak intensity of the most intense peak among the multiple peaks at 2θ = 25.5° ± 1.0° (hereinafter also referred to as the "peak intensity ratio") is 0.2 or more, since this further suppresses the generation of hydrogen sulfide from the solid electrolyte. Furthermore, when there are three peaks at 2θ = 25.5° ± 1.0° with a peak intensity ratio of 0.2 or more, when these peaks are designated as Peak A, Peak B, and Peak C from the low-angle side, Peak B / Peak A, which is the ratio of the intensity of Peak B to the intensity of Peak A, is preferably 2.0 or less, more preferably 1.6 or less, even more preferably 1.0 or less, and even more preferably 0.5 or less.

[0027] The particle size of the solid electrolyte of the present invention is a volume cumulative particle size D at 50% by volume of cumulative volume measured by a laser diffraction scattering particle size distribution measurement method. 50 The particle diameter is preferably 10 μm or less, more preferably 5 μm or less, even more preferably 3 μm or less, even more preferably 1.5 μm or less, and even more preferably 1.0 μm or less. By having such a particle diameter, the contact points and contact area between the solid electrolyte and the active material particles become large, and the input / output characteristics of the battery can be effectively improved. In addition, the particle diameter D of the solid electrolyte 50 For example, the particle size is preferably 0.1 μm or more, more preferably 0.3 μm or more, and particularly preferably 0.5 μm or more. By having such a particle size, an excessive increase in the surface area of ​​the solid electrolyte can be suppressed, and an increase in resistance can be suppressed. In addition, mixing with the active material can be facilitated.

[0028] The solid electrolyte of the present invention has lithium ion conductivity in a solid state. The lithium ion conductivity of the solid electrolyte of the present invention is, for example, preferably 0.1 mS / cm or more, more preferably 0.5 mS / cm or more, and even more preferably 1.0 mS / cm or more at room temperature, i.e., 25°C. The lithium ion conductivity is measured, for example, by the following method. The solid electrolyte is placed in a glove box purged with sufficiently dried argon gas (dew point -60°C or less) and heated to a temperature of about 6 t / cm. 2 The mixture is subjected to uniaxial pressure molding under a load of 1000 kJ / cm2, and pellets of 10 mm diameter and approximately 1 to 8 mm thickness are prepared as samples for measuring lithium ion conductivity. The lithium ion conductivity is measured using a Solartron 1255B impedance measuring instrument manufactured by Toyo Corporation. The measurement conditions are an AC impedance method at a temperature of 25°C, a frequency of 100 Hz to 1 MHz, and an amplitude of 100 mV.

[0029] Next, a preferred method for producing the solid electrolyte of the present invention, i.e., a solid electrolyte containing the elements Li, P, S, X, and N, will be described. The solid electrolyte can be preferably synthesized by a solid-phase reaction in which a raw material composition is heated and sintered. The raw material composition is a mixture of raw materials containing the above-mentioned elements that constitute the solid electrolyte. The raw material composition contains one or more compounds containing at least one of the elements Li, P, S, and X, and also contains an ammonium halide.

[0030] The compound may be, for example, a compound containing an Li element, a compound containing an S element, a compound containing a P element, a compound containing an X element, or a compound containing an N element.

[0031] Furthermore, the compound may contain at least two or more elements selected from Li, P, S, X, and N in one compound. For example, the compound may be a compound containing Li and X, a compound containing P and S, a compound containing Li and S, a compound containing P and X, a compound containing S and X, or a compound containing N and X. As the compound containing Li and X, for example, lithium halide may be used. As the compound containing P and S, for example, diphosphorus trisulfide (P 2 S 3 ) and diphosphorus pentasulfide (P 2 S 5 As a compound containing Li and S, for example, lithium sulfide (Li 2 As a compound containing P element and X element, for example, PX 3 and P 2 X 5 Examples of compounds containing S and X elements include SX 2 , SX 4 , SX 6 , S 2 X 10 As the compound containing N and X elements, an ammonium halide is used. As the ammonium halide, for example, ammonium chloride, ammonium bromide, or ammonium iodide is preferably used from the viewpoint of successfully obtaining the target solid electrolyte. In particular, it is preferable to use ammonium chloride.

[0032] In particular, it is preferable that the raw material composition contains lithium sulfide, phosphorus sulfide, lithium halide, and ammonium halide as the compounds, from the viewpoint of successfully synthesizing a solid electrolyte containing N element.

[0033] When preparing the raw material composition, when expressed by a composition formula of elements excluding N element, Li a P.S. b X cFrom the viewpoint of being able to suppress the generation of hydrogen sulfide from the solid electrolyte, it is preferable to mix each compound in an amount represented by the formula: From this viewpoint, in the composition formula, a is preferably 3.0 or more and 6.0 or less, more preferably 4.0 or more and 5.5 or less, and even more preferably 4.5 or more and 5.2 or less. In the composition formula, b is preferably 2.0 or more and 4.8 or less, more preferably 2.5 or more and 4.0 or less, and even more preferably 3.0 or more and 3.4 or less. In the composition formula, c is preferably 1.5 or more and 4.5 or less, more preferably 1.9 or more and 3.5 or less, and even more preferably 2.2 or more and 2.5 or less.

[0034] When preparing the raw material composition, when expressed by a composition formula of elements excluding N element, Li 7-x P.S. 6-x X x From the viewpoint of being able to suppress the generation of hydrogen sulfide from the solid electrolyte, it is also preferable to mix the compounds in an amount expressed as follows: From this viewpoint, x is preferably greater than 1.0 and not greater than 3.0, more preferably 1.4 or greater and not greater than 2.6, and even more preferably 1.8 or greater and not greater than 2.2.

[0035] The raw material composition is prepared by mixing the above-mentioned compounds. For mixing, for example, an attritor, paint shaker, planetary ball mill, ball mill, bead mill, homogenizer, etc. can be used. The amounts of each raw material added when mixing are appropriately adjusted so as to satisfy the composition of the desired solid electrolyte.

[0036] The resulting raw material composition is subjected to a firing process to cause a solid-state reaction, thereby obtaining a crystalline fired product. The firing atmosphere can be, for example, an inert gas atmosphere such as an argon atmosphere or a nitrogen atmosphere, or a hydrogen sulfide atmosphere. From the viewpoint of reducing the proportion of sulfur element contained in the solid electrolyte, it is preferable to use an inert gas atmosphere.

[0037] From the viewpoint of ensuring that a solid-phase reaction of the raw material composition occurs, the firing temperature is, for example, preferably 200° C. or higher, more preferably 300° C. or higher, even more preferably 350° C. or higher, and even more preferably 400° C. or higher. On the other hand, in consideration of industrial producibility and economic efficiency, the firing temperature is, for example, preferably 700° C. or lower, more preferably 600° C. or lower, and even more preferably 550° C. or lower.

[0038] The firing time is not critical, and may be any time that allows a fired product of the desired composition to be obtained. Specifically, the firing time is preferably long enough for the solid-phase reaction of the raw material composition to occur sufficiently. The firing time may be, for example, 30 minutes or more, 2 hours or more, or 3 hours or more. On the other hand, the firing time may be, for example, 10 hours or less, or 5 hours or less.

[0039] During the calcination, sulfur in the sulfide contained in the raw material composition reacts with hydrogen in the ammonium halide to generate hydrogen sulfide, and therefore the composition of each element contained in the calcined product may differ from the theoretical composition of the raw material composition.

[0040] After firing, the fired product may be crushed and pulverized as necessary, and may further be classified as necessary. For example, it is preferable to crush or crush the fired product using a crusher such as a planetary ball mill, a vibration mill, or a tumbling mill, or a kneader.

[0041] The solid electrolyte thus obtained can be used alone or in combination with other solid electrolytes.

[0042] The solid electrolyte of the present invention can be used as a material constituting a solid electrolyte layer, a positive electrode layer, or a negative electrode layer. Specifically, the solid electrolyte of the present invention can be used in a battery having a positive electrode layer, a negative electrode layer, and a solid electrolyte layer located between the positive electrode layer and the negative electrode layer. That is, the solid electrolyte can be used in so-called solid-state batteries. More specifically, it can be used in lithium solid-state batteries. The lithium solid-state battery may be a primary battery or a secondary battery. There is no particular limitation on the shape of the battery, and shapes such as a laminate type, a cylindrical type, and a prismatic type can be adopted. The term "solid-state battery" includes not only solid-state batteries that do not contain any liquid or gel-like substance as an electrolyte, but also batteries that contain, for example, 50% by mass or less, 30% by mass or less, or 10% by mass or less of a liquid or gel-like substance as an electrolyte.

[0043] When the solid electrolyte layer contains the solid electrolyte of the present invention, the solid electrolyte layer can be produced, for example, by dropping a slurry consisting of the solid electrolyte, a binder, and a solvent onto a substrate and scraping it off with a doctor blade or the like, by contacting the substrate with the slurry and then cutting it with an air knife, or by forming a coating film by screen printing or the like and then heating and drying to remove the solvent. Alternatively, the solid electrolyte can be produced by compacting a powdered solid electrolyte by pressing or the like and then appropriately processing it. The thickness of the solid electrolyte layer is typically preferably 5 μm to 300 μm, and more preferably 10 μm to 100 μm, in order to balance short-circuit prevention and volumetric capacity density.

[0044] The solid electrolyte of the present invention is used together with an active material to form an electrode mixture. The proportion of the solid electrolyte in the electrode mixture is typically 10% by mass or more and 50% by mass or less. The electrode mixture may contain other materials such as a conductive material as needed. An electrode mixture, a binder, and a solvent are mixed to prepare a paste, which is then applied to a current collector such as aluminum foil and dried to produce electrodes such as positive and negative electrodes.

[0045] The cathode material constituting the cathode layer can be any cathode material used as a cathode active material in lithium-ion batteries. For example, lithium-containing cathode active materials, specifically spinel-type lithium transition metal oxides and lithium metal oxides with layered structures, can be used. The use of a high-voltage cathode material as the cathode material can improve energy density. In addition to the cathode active material, the cathode material may contain a conductive material or other materials.

[0046] As the negative electrode material constituting the negative electrode layer, a negative electrode material used as a negative electrode active material in a lithium ion battery can be appropriately used. Since the solid electrolyte of the present invention is electrochemically stable, it can be used at a potential of lithium metal or a lower potential comparable to that of lithium metal (about 0.1 V vs. Li + Carbonaceous materials such as graphite, artificial graphite, natural graphite, and non-graphitizable carbon (hard carbon), which are materials that are charged and discharged using a lithium-ion battery (Li / Li), can be used as the negative electrode material. This can significantly improve the energy density of solid-state batteries. Silicon or tin, which are promising high-capacity materials, can also be used as the active material. The negative electrode material may also contain a conductive material or other materials in addition to the negative electrode active material.

[0047] In relation to the above-described embodiments, the present invention further discloses the following solid electrolyte, electrode mixture, electrode, battery, and method for manufacturing a solid electrolyte. <1> A solid electrolyte containing lithium (Li), phosphorus (P), sulfur (S), a halogen (X), and nitrogen (N), wherein the molar ratio of the difference between the lithium (Li) and the sulfur (S) to the phosphorus (P) is 1.5 or more and 2.2 or less, and the molar ratio of the sum of the lithium (Li) and the halogen (X) to the phosphorus (P) is 7.1 or more and 10.0 or less. <2> The solid electrolyte according to <1>, wherein an X-ray diffraction pattern measured by an X-ray diffractometer has peaks at 2θ = 25.5° ± 1.0°, 29.8° ± 0.5°, and 31.2° ± 1.0°. <3> The solid electrolyte according to <1> or <2>, having peaks at 2θ = 44.7° ± 1.0°, 47.8° ± 1.0°, and 52.5° ± 1.0° in an X-ray diffraction pattern measured with an X-ray diffractometer. <4> The solid electrolyte according to any one of <1> to <3>, having at least two peaks at 2θ = 25.5° ± 1.0° in an X-ray diffraction pattern. <5> The solid electrolyte according to any one of <1> to <4>, having a molar ratio of the nitrogen (N) element to the phosphorus (P) element of 0.01 or more and 0.5 or less. <6> An electrode mixture comprising the active material according to any one of <1> to <5>, a solid electrolyte, and a conductive material. <7> An electrode comprising the electrode mixture according to <6> and a binder. <8> A battery having a positive electrode layer, a negative electrode layer, and a solid electrolyte layer located between the positive electrode layer and the negative electrode layer, the battery containing the solid electrolyte according to any one of <1> to <5>. <9> A method for producing a solid electrolyte containing lithium (Li), phosphorus (P), sulfur (S), a halogen (X), and nitrogen (N), the method comprising a step of firing a raw material composition for the solid electrolyte, the raw material composition containing one or more compounds containing at least one of lithium (Li), phosphorus (P), sulfur (S), and a halogen (X), and containing an ammonium halide.<10> The method according to <9>, wherein the raw material composition contains lithium sulfide, phosphorus sulfide, and a lithium halide as the compound. <11> The method according to <9> or <10>, wherein the raw material composition contains ammonium chloride as the ammonium halide.

[0048] The present invention will be described in more detail below with reference to examples. However, the scope of the present invention is not limited to such examples. Unless otherwise specified, "%" means "% by mass."

[0049] Comparative Example 1 (1) Preparation of Raw Material Composition Lithium sulfide (Li 2 S) powder and diphosphorus pentasulfide (P 2 S 5 Lithium chloride (LiCl) powder, lithium bromide (LiBr) powder, and lithium fluoride (LiBr) powder were weighed out. Heptane was added to these powders to prepare a slurry. This slurry was placed in a zirconia container and set in a planetary ball mill. Zirconia balls with a diameter of 5 mm were used as the grinding media. The ball mill was operated at 100 rpm, and wet mixing was carried out for 10 hours. The mixed slurry was vacuum dried at room temperature to remove the heptane. In this way, a raw material composition was obtained.

[0050] (2) Calcination The raw material composition was calcined to obtain a calcined product. Calcination was carried out using a tubular electric furnace. Nitrogen gas with 100% purity was circulated through the electric furnace during calcination. Calcination was carried out by increasing the temperature to 300°C at 200°C / h and maintaining it at 300°C for 4 hours, then increasing the temperature to 500°C at 200°C / h and maintaining it at 500°C for 4 hours, for a total of 10.5 hours.

[0051] (3) Pulverization The fired material was crushed in a mortar and passed through a 250 μm sieve to obtain a pulverized powder. This pulverized powder was coarsely pulverized using a planetary ball mill. Zirconia balls with a diameter of 5 mm were used as the pulverization media. Heptane was used as the solvent. The ball mill was operated at 100 rpm, and the coarse pulverization was carried out for 3 hours. The resulting slurry was vacuum dried at room temperature to remove the solvent. In this way, the desired solid electrolyte powder was obtained.

[0052] [Examples 1, 2 and 3] Lithium sulfide (Li 2 S) powder and diphosphorus pentasulfide (P 2 S 5 ) powder, lithium chloride (LiCl) powder, lithium bromide (LiBr) powder, and ammonium chloride (NH 4 The powder of the solid electrolyte was obtained in the same manner as in Comparative Example 1 except for the above.

[0053] [Example 4] Lithium sulfide (Li 2 S) powder and diphosphorus pentasulfide (P 2 S 5 ) powder, lithium chloride (LiCl) powder, lithium bromide (LiBr) powder, lithium iodide (LiI) powder, and ammonium chloride (NH 4 The powder of the solid electrolyte was obtained in the same manner as in Comparative Example 1 except for the above.

[0054] Comparative Example 2 Lithium sulfide (Li 2 S) powder and diphosphorus pentasulfide (P 2 S 5 A raw material composition was obtained by weighing out lithium chloride (LiCl) powder, lithium bromide (LiBr) powder, and lithium fluoride (LiBr) powder. A solid electrolyte powder was obtained in the same manner as in Comparative Example 1 except for this.

[0055] [Example 5] Lithium sulfide (Li 2 S) powder and diphosphorus pentasulfide (P 2 S 5 ) powder, lithium chloride (LiCl) powder, lithium bromide (LiBr) powder, and ammonium chloride (NH 4 The powder of the solid electrolyte was obtained in the same manner as in Comparative Example 1 except for the above.

[0056] [Comparative Example 3] This comparative example is an example in which the molar ratio of S / P in a solid electrolyte containing Li, P, S, and X elements but not N is reduced to reduce the generation of hydrogen sulfide. Lithium sulfide (Li 2 S) powder and diphosphorus pentasulfide (P 2 S 5 A raw material composition was obtained by weighing out lithium chloride (LiCl) powder, lithium bromide (LiBr) powder, and lithium fluoride (LiBr) powder. A solid electrolyte powder was obtained in the same manner as in Comparative Example 1 except for this.

[0057] [Evaluation] The elements of the solid electrolytes obtained in the examples and comparative examples were quantified by the methods described below, and the molar ratios shown in Table 1 were calculated. The solid electrolyte powder was melted by the alkali fusion method, and the elements Li, P, Br, Cl, and I were quantified using an ICP optical emission spectrometer ("SPS3520DDUV" manufactured by Hitachi High-Tech Co., Ltd.). The S element was oxidized to sulfate ions and then quantified by the barium sulfate gravimetric method. The N element was quantified using an oxygen, nitrogen, and hydrogen analyzer (EMGA930 manufactured by Horiba, Ltd.) by melting the solid electrolyte powder in a graphite crucible and removing the generated gas. 2 Agents and de-H 2 Using O agent, CO 2 and H 2 After removing O, N was measured using a thermal conductivity detector. 2 The amount of hydrogen sulfide generated and the particle size D were determined by the following method. 50The characteristics of solid-state batteries containing the solid electrolyte were evaluated using the method described below. The results are shown in Table 1. Furthermore, XRD measurements were performed on the solid electrolytes obtained in Examples 1 to 5 and Comparative Examples 1 to 3 to obtain diffraction patterns. The XRD measurements were performed using an X-ray diffractometer "Smart Lab SE" manufactured by Rigaku Corporation. The measurement conditions were: no exposure to air; scanning axis: 2θ / θ; scanning range: 10° to 120°; step width: 0.02°; and scanning speed: 1° / min. The X-ray source was CuKα1 radiation. The tube voltage was 40 kV and the tube current was 80 mA. The measurement results are shown in Figures 1 and 2. For the solid electrolytes of the Examples and Comparative Examples, Table 1 shows the number of peaks with a peak intensity ratio of 0.2 or greater, which is the ratio of the peak intensity of the second-highest peak to the peak intensity of the highest peak, among the multiple peaks located at 2θ = 25.5° ± 1.0°. When there are three peaks located at 2θ = 25.5° ± 1.0°, the value of Peak B / Peak A is shown in Table 1. The above-mentioned peak intensities were calculated using the average intensity between 2θ = 75.5° and 76.0° as the background. In Figure 3, peaks counted under the above conditions in Example 1 and Comparative Example 1 are indicated by a "▼" mark. In the XRD chart of the solid electrolyte of Example 5, diffraction peaks were observed at 2θ = 25.5° ± 1.0°, 29.8° ± 0.5°, 31.2° ± 1.0°, 44.7° ± 1.0°, 47.8° ± 1.0°, and 52.5° ± 1.0°, but two or more diffraction peaks were not observed at 2θ = 25.5° ± 1.0°.

[0058] [Amount of Hydrogen Sulfide Generated] The amount of hydrogen sulfide generated from the solid electrolyte was measured using a detector tube. 2 mg of solid electrolyte was weighed into a metal container in a glove box purged with thoroughly dried Ar gas (dew point -60°C or less), and then placed in a sealed laminated film bag. A 1000 ml glass separable flask was placed in a thermo-hygrostat chamber maintained at room temperature (25°C) and a dew point of -30°C adjusted by mixing dry air and atmospheric air. The flask was then maintained until the interior of the flask was identical to the environment inside the thermo-hygrostat chamber. Next, the sealed bag containing the solid electrolyte was opened in the thermo-hygrostat chamber, and the solid electrolyte was quickly placed in the separable flask. The separable flask was then sealed. The amount of hydrogen sulfide generated from immediately after sealing until 30 minutes had elapsed was measured using a gas detector (Gastec No. 4LL) 30 minutes later.

[0059] [Particle size D 50 Using an automatic sample feeder for a laser diffraction particle size distribution measurement device ("Microtorac SDC" manufactured by Nikkiso Co., Ltd.), the flow rate of the measurement sample containing the solid electrolyte was set to 50%, and the measurement sample containing the solid electrolyte was irradiated with 30 W ultrasonic waves for 60 seconds. Thereafter, the particle size distribution was measured using a laser diffraction particle size distribution measurement device "MT3000II" manufactured by Nikkiso Co., Ltd., and the particle size at which the cumulative volume was 50% by volume was determined from the obtained volume-based particle size distribution chart, and this value was designated as D 50 It was decided.

[0060] [Battery Characteristics] The positive electrode active material is a ternary layered compound LiNi whose surface is coated with lithium niobate. 0.6 Co 0.2 Mn 0.2 O 2(NCM) powder was used. Graphite (Gr) powder was used as the negative electrode active material. The solid electrolyte powder obtained in Examples 1 and 2 was finely pulverized using a planetary ball mill (D50 = 0.7 μm) and used. The positive electrode mixture was prepared by mixing the positive electrode active material powder, solid electrolyte powder, and conductive additive in a mortar at a mass ratio of 60:37:3. This positive electrode mixture was uniaxially press-molded at 20 MPa to prepare positive electrode mixture pellets. The negative electrode mixture powder was prepared by mixing the graphite powder and solid electrolyte powder in a mortar at a mass ratio of 64:36.

[0061] The lower opening of a polypropylene cylinder (opening diameter 10.5 mm, height 18 mm) with open top and bottom was blocked with a positive electrode (made of SUS), and a positive electrode mixture pellet was placed on the positive electrode. A solid electrolyte powder was placed on top of the positive electrode and uniaxially pressed at 180 MPa to form a positive electrode mixture and a solid electrolyte layer. A negative electrode mixture powder was then placed on top of the positive electrode mixture. This resulted in an all-solid-state battery cell consisting of a three-layer structure: a positive electrode mixture, a solid electrolyte layer approximately 300 μm thick, and a negative electrode mixture approximately 20 μm thick. Using the all-solid-state battery cell prepared as described above, battery characteristics (initial charge / discharge characteristics) were evaluated using the following method. The all-solid-state battery cell was placed in an environmental test chamber maintained at 25°C and connected to a charge / discharge device to evaluate the battery characteristics. The battery was charged / discharged at 1 mA at 1 C. The battery was charged at 0.1 C to 4.5 V using the CC-CV method, and the initial charge capacity was obtained. Discharge was performed at 0.1 C to 2.5 V by CC method to obtain the initial discharge capacity. The initial charge-discharge curves of Examples 1 and 2 are shown in FIG.

[0062]

[0063] As is clear from the results shown in Table 1, the solid electrolytes obtained in each example were found to produce less hydrogen sulfide.

[0064] 4, the initial charge capacity was 217.4 mAh / g and the initial discharge capacity was 182.2 mAh / g in Example 1. The initial charge capacity was 211.4 mAh / g and the initial discharge capacity was 176.8 mAh / g in Example 2. These results demonstrate that the solid electrolytes obtained in each Example functioned satisfactorily as solid electrolytes.

[0065] As described above in detail, the present invention provides a solid electrolyte in which generation of hydrogen sulfide is suppressed and a method for producing the same.

Claims

1. A solid electrolyte comprising lithium (Li), phosphorus (P), sulfur (S), halogen (X) and nitrogen (N), wherein the molar ratio of the difference between the lithium (Li) and sulfur (S) elements to the phosphorus (P) element is 1.5 or more and 2.2 or less, and the molar ratio of the sum of the lithium (Li) and halogen (X) elements to the phosphorus (P) element is 7.1 or more and 10.0 or less.

2. The solid electrolyte according to claim 1, which has peaks at 2θ=25.5°±1.0°, 29.8°±0.5°, and 31.2°±1.0° in an X-ray diffraction pattern measured by an X-ray diffractometer.

3. The solid electrolyte according to claim 2, which has peaks at 2θ=44.7°±1.0°, 47.8°±1.0°, and 52.5°±1.0° in an X-ray diffraction pattern measured by an X-ray diffractometer.

4. The solid electrolyte according to claim 2, having at least two peaks at 25.5°±1.0° in an X-ray diffraction pattern.

5. An electrode mixture comprising the active material according to any one of claims 1 to 4, a solid electrolyte, and a conductive material.

6. An electrode comprising the electrode mixture according to claim 5 and a binder.

7. A battery having a positive electrode layer, a negative electrode layer, and a solid electrolyte layer located between the positive electrode layer and the negative electrode layer, the battery containing the solid electrolyte according to any one of claims 1 to 4.

8. A method for producing a solid electrolyte containing lithium (Li), phosphorus (P), sulfur (S), halogen (X) and nitrogen (N), the method comprising a step of firing a raw material composition for the solid electrolyte, the raw material composition containing one or more compounds containing at least one of lithium (Li), phosphorus (P), sulfur (S) and halogen (X), and containing ammonium halide.

9. The method according to claim 8, wherein the raw material composition contains lithium sulfide, phosphorus sulfide and lithium halide as the compounds.

10. The manufacturing method according to claim 8 or 9, wherein the raw material composition contains ammonium chloride as the ammonium halide.

Citation Information

Patent Citations

  • Sulfide solid electrolyte

    US20200091552A1

  • Solid Electrolyte of Lithium Secondary Battery and Sulfide Compound for Said Solid Electrolyte

    US20200127325A1

  • Production method of solid electrolyte, solid electrolyte, active material layer, formation method of active material layer, separator layer, formation method of separator layer, and all-solid-state battery

    JP2019145489A

  • Method for manufacturing sulfide solid electrolyte, sulfide solid electrolyte, all-solid battery, and method for selecting raw material compound used to manufacture sulfide solid electrolyte

    WO2020045634A1

  • Method for producing sulfide solid electrolyte

    WO2023132167A1