Heat insulating material for combustion chamber, water heater, and boiler

The use of a plate-shaped molded body with inorganic fibers and varying bulk densities addresses the limitations of existing insulation materials by enhancing heat insulation and stability while reducing weight and cost, effectively addressing the challenges of existing combustion chamber insulation materials.

WO2024203847A1PCT designated stage expired Publication Date: 2024-10-03IBIDEN CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011292
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing combustion chamber insulation materials, such as castable refractories, suffer from insufficient insulation, high weight, long drying times, and poor workability, while inorganic fiber-based materials lack stability, ease of installation, and durability, and are costly.

Method used

A plate-shaped molded body containing inorganic fibers with varying bulk densities is used, where the first main surface portion has a lower bulk density than the central portion, creating an air layer for enhanced insulation and arranged towards the inner wall of the combustion chamber, formed using a paper-making method to ensure stability and ease of installation.

Benefits of technology

The solution provides improved heat insulation, stability, ease of installation and maintenance, and durability while reducing weight and cost, effectively suppressing CO2 emissions and maintaining strength as a heat insulating material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011292_03102024_PF_FP_ABST
    Figure JP2024011292_03102024_PF_FP_ABST
Patent Text Reader

Abstract

This heat insulation material for a combustion chamber is a plate-like molding including inorganic fibers, the heat insulation material being characterized in that when the bulk densities of a first main surface part, a second main surface part, and a central part between the first main surface part and the second main surface part in the thickness direction are compared, at least the bulk density of the first main surface part is smaller than the bulk density of the central part, and the first main surface part is arranged toward the inner wall surface of the combustion chamber.
Need to check novelty before this filing date? Find Prior Art

Description

Combustion chamber insulation, water heaters and boilers

[0001] The present invention relates to a combustion chamber insulating material, a water heater, and a boiler.

[0002] 2. Description of the Related Art Boilers and water heaters are used as devices that supply steam or hot water using fuels such as petroleum.

[0003] Boilers and water heaters generate steam or hot water from water by burning fuel in a combustion chamber and transferring the combustion heat to water through water pipes placed inside the combustion chamber.

[0004] Because the combustion chamber reaches high temperatures, it is usually protected by refractories and heat insulating materials in order to protect surrounding equipment from heat damage and to reduce energy loss (see, for example, Patent Documents 1 and 2).

[0005] In particular, in combustion chambers where combustion gases can reach high temperatures, refractories and thermal insulation materials are typically made by pouring a fluid containing heat-resistant material onto the surface of the object to be installed and solidifying it. Such materials are also called castable materials. While castable materials can conform to surfaces of any shape and provide a certain degree of thermal insulation, they have problems such as insufficient thermal insulation, heavy weight, long drying times, and poor workability during installation.

[0006] Patent No. 4946594 Patent No. 4640705

[0007] The use of insulating materials containing inorganic fibers instead of castable materials is being considered, but insulating materials installed inside combustion chambers are required to have improved insulating properties, be stable and easy to install and maintain, be durable, and be available at low cost.

[0008] The present invention has been made to solve the above problems, and an object of the present invention is to provide a combustion chamber insulating material that has a greater insulating effect, can be stably and easily installed and maintained, is durable, and can be supplied at low cost.

[0009] That is, the combustion chamber insulating material of the present invention is a plate-shaped molded product containing inorganic fibers, and is characterized in that, when comparing the bulk densities of a first main surface portion, a second main surface portion, and a central portion located between the first main surface portion and the second main surface portion in the thickness direction, the bulk density of at least the first main surface portion is lower than the bulk density of the central portion, and the first main surface portion is arranged facing the inner wall surface of the combustion chamber. By reducing the bulk density of the first main surface portion and arranging the first main surface portion facing the inner wall surface of the combustion chamber, the combustion chamber insulating material of the present invention can create an air layer on the inner wall surface side of the combustion chamber, thereby enhancing the insulating effect.

[0010] It is preferable that the bulk density of the second main surface portion is (i) greater than the bulk density of the central portion, or (ii) less than the bulk density of the central portion.

[0011] The combustion chamber insulating material of the present invention is preferably formed by a papermaking method. By forming and drying by a papermaking method, the bulk density of the combustion chamber insulating material in the thickness direction can be easily adjusted.

[0012] The combustion chamber insulating material of the present invention preferably has a flat or curved shape. When the combustion chamber insulating material of the present invention has the above-mentioned shape, it can be placed at various locations inside the combustion chamber.

[0013] The combustion chamber insulating material of the present invention has an overall bulk density of 0.20 to 0.35 g / cm 3 When the bulk density of the whole is within the above range, the strength required for a heat insulating material can be ensured while the weight can be reduced compared to a fireproof material using an amorphous material.

[0014] The bulk density of the first main surface portion is preferably 3% or more lower than the larger of the bulk densities of the second main surface portion and the central portion. When the bulk density of the first main surface portion is in the above range, an air layer can be created on the inner wall surface side of the combustion chamber, thereby improving the insulating effect. Furthermore, by making the larger of the bulk density of the second main surface portion and the bulk density of the central portion 3% or more higher than the bulk density of the first main surface portion, the wind erosion resistance against contact with combustion gas can be improved, and the strength as an insulating material can be ensured, allowing the combustion chamber insulating material of the present invention to be used stably for a long period of time.

[0015] The water heater of the present invention comprises a combustion chamber, a heat exchanger installed in the combustion chamber, and the combustion chamber insulation material of the present invention, and is characterized in that the first main surface portion of the combustion chamber insulation material is arranged facing the inner wall surface of the combustion chamber.

[0016] The water heater of the present invention is equipped with the combustion chamber insulating material of the present invention, and since the bulk density of the first main surface portion is low, an air layer can be created on the inner wall surface side of the combustion chamber, thereby improving the insulating effect, and 2 It has excellent emission suppression effect.

[0017] The boiler of the present invention comprises a combustion chamber and the combustion chamber insulation material of the present invention, and is characterized in that the first main surface portion of the combustion chamber insulation material is arranged facing the inner wall surface of the combustion chamber.

[0018] The boiler of the present invention is equipped with the combustion chamber insulating material of the present invention, and since the bulk density of the first main surface portion is low, an air layer can be created on the inner wall surface side of the combustion chamber, thereby improving the insulating effect, and 2 It has excellent emission suppression effect.

[0019] FIG. 1 is a perspective view schematically showing an example of a combustion chamber insulating material of the present invention. FIG. 2 is a cross-sectional view taken along line A-A, schematically showing an example of the internal structure of the combustion chamber insulating material in FIG. 1. FIG. 3 is a cross-sectional view taken along line A-A, schematically showing another example of the internal structure of the combustion chamber insulating material in FIG. 1. FIG. 4 is a cross-sectional view schematically showing an example of a manufacturing process for a combustion chamber insulating material of the present invention. FIG. 5 is a cross-sectional view schematically showing another example of a manufacturing process for a combustion chamber insulating material of the present invention. FIG. 6 is a cross-sectional view schematically showing an example of a water heater of the present invention. FIG. 7 is a cross-sectional view schematically showing an example of a boiler of the present invention.

[0020] (Detailed Description of the Invention) [Insulating Material for Combustion Chamber] First, the insulating material for combustion chamber of the present invention will be described. The insulating material for combustion chamber of the present invention is a plate-shaped molded product containing inorganic fibers, characterized in that, when comparing the bulk densities of a first main surface portion, a second main surface portion, and a central portion located between the first main surface portion and the second main surface portion in the thickness direction, the bulk density of at least the first main surface portion is lower than the bulk density of the central portion, and the first main surface portion is arranged facing the inner wall surface of the combustion chamber.

[0021] In this specification, the term "plate-like" refers to a shape having two opposing main surfaces with relatively large areas and side surfaces connecting the two main surfaces. The direction in which the two main surfaces extend is also referred to as the surface direction, and the direction connecting the two main surfaces is also referred to as the thickness direction. At least one of the two opposing main surfaces may be curved.

[0022] Fig. 1 is a perspective view showing a schematic diagram of an example of a combustion chamber insulating material of the present invention. The combustion chamber insulating material 1 shown in Fig. 1 is composed of a plate-shaped molded body 10 containing inorganic fibers. The plate-shaped molded body 10 has a plate-like shape having a first main surface 10a and a second main surface 10b that are opposed to each other and have relatively large areas, and a side surface 10c that connects the first main surface 10a and the second main surface 10b.

[0023] The first main surface 10a and the second main surface 10b have a substantially circular shape when viewed from the thickness direction. Therefore, the outer shape of the plate-shaped molded body 10 and the combustion chamber insulating material 1 can be said to be a disk shape having a predetermined thickness.

[0024] The combustion chamber insulating material of the present invention preferably has a flat or curved shape. With the above-mentioned shape, the combustion chamber insulating material of the present invention can be arranged at various locations inside the combustion chamber. The shape of the combustion chamber insulating material is the shape of the plate-like molded body.

[0025] Since the combustion chamber insulating material 1 is composed only of the plate-shaped molded body 10, the plate-shaped molded body 10 can be said to be the combustion chamber insulating material 1. In other words, in the combustion chamber insulating material of the present invention, the plate-shaped molded body itself may be the combustion chamber insulating material.

[0026] The plate-shaped molded body contains inorganic fibers. The inorganic fibers preferably contain at least one selected from the group consisting of biosoluble fibers, alumina fibers, rock wool, and glass fibers. Examples of biosoluble fibers that can be used include alkaline earth silicate fibers (AES fibers). The plate-shaped molded body may also contain a shot component of non-fibrous particles. When the inorganic fibers contain the above-mentioned materials, a plate-shaped molded body with excellent heat resistance can be obtained.

[0027] The combustion chamber insulating material 1 is made of a plate-shaped molded body 10 containing inorganic fibers, and therefore has a smaller weight per volume and better workability than castable materials. The plate-shaped molded body 10 has the property of having little localized unevenness of the inorganic fibers and being resistant to deformation, making it suitable as an insulating material to be placed inside a combustion chamber.

[0028] The plate-shaped molded body may be a paper molded body or a needle-shaped body. A paper molded body is a molded body obtained by paper molding in which a slurry containing inorganic fibers is poured into a mold and suction-dehydrated, followed by drying (papermaking method). A plate-shaped molded body obtained by the papermaking method is also called a plate-shaped paper molded body. A needle-shaped body is a molded body obtained by subjecting an inorganic fiber aggregate to a needling treatment, and a plate-shaped molded body obtained by the needling treatment is also called a plate-shaped needle-shaped body.

[0029] The plate-shaped molded body is preferably one molded by a papermaking method. Papermaking bodies have the property of having little localized unevenness of the inorganic fibers and being resistant to deformation, and are therefore suitable as a heat insulating material to be placed inside a combustion chamber.

[0030] Although the average fiber diameter of the inorganic fibers is not particularly limited, when the plate-shaped molded product is a paper product, it is preferably 2.0 to 15.0 μm. When the average fiber diameter of the inorganic fibers is in the above range, a dense plate-shaped molded product with little local deviation in bulk density can be obtained.

[0031] The average fiber length of the inorganic fibers is not particularly limited, but when the plate-shaped molded product is a paper product, it is preferably 0.05 to 3.0 mm. When the average fiber length of the inorganic fibers is within the above range, a laminated plate-shaped molded product can be obtained with little localized unevenness of the inorganic fibers, and the bulk density and heat insulation properties can be stabilized.

[0032] The combustion chamber insulating material of the present invention has a different bulk density in the thickness direction of the plate-shaped molded body. Specifically, when comparing the bulk densities of the first main surface portion, the second main surface portion, and a central portion between the first and second main surface portions of the plate-shaped molded body in the thickness direction, the bulk density of at least the first main surface portion is lower than the bulk density of the central portion.

[0033] The internal structure of a combustion chamber insulating material 1A, which is a first embodiment of the combustion chamber insulating material 1, will be described below with reference to FIG. 2. FIG. 2 is a cross-sectional view taken along line A-A, schematically illustrating an example of the internal structure of the combustion chamber insulating material in FIG. 1. The combustion chamber insulating material 1A is composed of a plate-shaped molded body 10A. When comparing the bulk densities of the first main surface portion 11, the second main surface portion 12, and the central portion 13 located between the first main surface portion 11 and the second main surface portion 12 in the thickness direction of the plate-shaped molded body 10A, the first main surface portion 11 has the smallest bulk density, followed by the central portion 13 and the second main surface portion 12. The first main surface portion 11 includes a first main surface 10Aa, and the second main surface portion 12 includes a second main surface 10Ab.

[0034] Next, the internal structure of a combustion chamber insulating material 1B, which is a second embodiment of the combustion chamber insulating material 1, will be described below with reference to FIG. 3. Here, only the differences from the combustion chamber insulating material 1A, which is the first embodiment, will be described, and the common features will not be described. FIG. 3 is a cross-sectional view taken along line A-A, which schematically shows another example of the internal structure of the combustion chamber insulating material in FIG. 1. In the plate-shaped molded body 10B constituting the combustion chamber insulating material 1B, the first main surface portion 11 and the second main surface portion 12 have low bulk densities, and the central portion 13 has a high bulk density. The bulk density of the second main surface portion 12 may be intermediate between the bulk densities of the first main surface portion 11 and the central portion 13. The first main surface portion 11 includes a first main surface 10Ba, and the second main surface portion 12 includes a second main surface 10Bb.

[0035] In Figures 2 and 3, the first main surface portion 11, the second main surface portion 12, and the central portion 13 are divided into three equal parts in the thickness direction, but the thicknesses of the first main surface portion 11, the second main surface portion 12, and the central portion 13 do not have to be the same.

[0036] The bulk density of the second main surface portion is preferably (i) greater than the bulk density of the central portion, or (ii) less than the bulk density of the central portion. The bulk density of the second main surface portion may be approximately the same as the bulk density of the central portion.

[0037] In the combustion chamber insulating material of the present invention, the bulk density of the first main surface portion of the plate-shaped molded body is preferably at least 3% smaller than the larger of the bulk density of the second main surface portion and the bulk density of the central portion, and more preferably at least 5% smaller.

[0038] In the combustion chamber insulating material of the present invention, the first main surface portion is disposed facing the inner wall surface of the combustion chamber. By disposing the first main surface portion, which has a low bulk density, facing the inner wall surface of the combustion chamber, a large insulating effect can be obtained.

[0039] The combustion chamber insulating material of the present invention is an integrally formed plate-like molded body, and is not an assembly of a plurality of plate-like molded bodies having different bulk densities stacked in the thickness direction.

[0040] The bulk density of the combustion chamber insulation material is 0.20 to 0.35 g / cm 3 When the bulk density of the plate-like molded body is within the above range, the strength (bending strength) and heat insulating properties required for a combustion chamber insulation material can be maintained, while the weight of the combustion chamber can be prevented from increasing as compared with a fireproof material or heat insulating material made of an amorphous material.

[0041] The bulk density can be adjusted, for example, by adjusting the fiber length and aggregate floc size of the inorganic fibers, or by adjusting the compression conditions during dewatering of the slurry and the compression conditions during drying.

[0042] The bulk density of fireproof materials and heat insulating materials made of amorphous materials is usually 0.7 to 1.5 g / cm 3 This does not satisfy the above-mentioned preferable bulk density of the thermal insulating material for a combustion chamber.

[0043] The thickness of the plate-shaped molded body is preferably 1 to 10 cm. When the thickness of the plate-shaped molded body is in the above range, it can exhibit sufficient heat insulating properties as a heat insulating material.

[0044] The area of ​​the plate-shaped molded body as viewed in the thickness direction (planar area) is 350 to 15,000 cm 2 It is preferable that:

[0045] The volume of the plate-shaped molded body is 700 to 150,000 cm 3 When the volume of the plate-like molded body is within the above range, breakage due to thermal shrinkage is particularly unlikely to occur.

[0046] The plate-like molded body may be provided with holes penetrating in the thickness direction, which makes it easier to cover the inner wall surface of a combustion chamber in which piping such as water pipes and smoke pipes are arranged.

[0047] The plate-like molded body may contain components other than inorganic fibers, such as inorganic particles, inorganic binders, organic binders, and flocculants.

[0048] Examples of inorganic particles include silica particles, alumina particles, titania particles, zirconia particles, natural mineral particles, etc. Examples of inorganic binders include silica sol, alumina sol, titania sol, zirconia sol, fumed silica, etc. Examples of organic binders include polyvinyl alcohol, starch, acrylic resin, polyacrylamide, etc.

[0049] The weight ratio of the inorganic fibers in the plate-like molded product is preferably 30 to 97% by weight.

[0050] The method for producing the combustion chamber insulating material of the present invention is not particularly limited, but can be, for example, produced by the following procedure. Below, a method for producing a combustion chamber insulating material 1A will be described with reference to FIG. 4. FIG. 4 is a cross-sectional view schematically illustrating an example of a production process for a combustion chamber insulating material of the present invention. Step (1): A slurry containing water, inorganic fibers, an inorganic binder, an organic binder, and a flocculant is prepared, and a base sheet 50 of the insulating material is obtained by a papermaking method (FIG. 4A). Step (2): After papermaking, a SUS plate HP heated to 150°C is placed on the first main surface 50a of the moist base sheet, and dried for 30 minutes (FIG. 4B). Step (3): Next, the base sheet 50 of (2) is sandwiched between two SUS plates HP heated to 150°C from the first main surface 50a and the second main surface 50b, and dried for 1 hour while compressing the base sheet 50 to the desired thickness (FIG. 4C). In this way, a combustion chamber insulating material 1A can be obtained (D in FIG. 4).

[0051] In the above method, the organic binder solidifies on the first main surface 50a side of the original sheet 50 where drying has progressed, and even when compressed, the original sheet 50 does not collapse and the bulk density does not change. When the original sheet 50 is sandwiched between two SUS plates HP, the undried portion is compressed, and the bulk density of the inorganic fibers in the central portion 13 and second main surface portion 12 of the resulting plate-like molded body 10A increases. In the plate-like molded body 10A, the second main surface portion 12 has a higher bulk density than the central portion 13, which is thought to be because the central portion of the original sheet 50 dried slightly in the above step (2).

[0052] Next, a method for producing a combustion chamber insulating material 1B will be described with reference to FIG. 5. FIG. 5 is a cross-sectional view schematically illustrating another example of the manufacturing process for a combustion chamber insulating material of the present invention. (1) A slurry containing water, inorganic fibers, an inorganic binder, an organic binder, and a flocculant is prepared, and a base sheet 50 of the insulating material is obtained by a papermaking method (FIG. 5A). (2) After papermaking, a SUS plate HP heated to 150°C is placed on the second main surface 50b of the moist base sheet, and dried for 30 minutes (FIG. 5B). (3) Then, the base sheet 50 is turned upside down, and a SUS plate HP heated to 150°C is placed on the first main surface 50a, and dried for 30 minutes (FIG. 5C). (4) Next, the original sheet 50 from (3) is sandwiched between two SUS plates HP heated to 150°C from the first main surface 50a and the second main surface 50b, and dried for one hour while compressing the original sheet 50 to a desired thickness (Fig. 5D). In this way, a combustion chamber insulating material 1B can be obtained (Fig. 5E).

[0053] In the above method, the organic binder solidifies on the first main surface 50a and the second main surface 50b of the original sheet 50, where drying has progressed, and the original sheet 50 does not collapse even when compressed, and the bulk density does not change. When the original sheet 50 is sandwiched between two SUS plates HP, only the undried central portion is compressed, and the bulk density of the central portion 13 of the resulting plate-like molded body 10B increases.

[0054] The combustion chamber insulating material of the present invention has a surface with a lower bulk density facing the inner wall surface of the combustion chamber, thereby achieving a greater insulating effect. Because the combustion chamber insulating material of the present invention is a plate-shaped molded body containing inorganic fibers, it is lighter in weight than a castable molded body of the same volume and can be stably and easily attached to and maintained on the inner wall surface of the combustion chamber. Furthermore, because the combustion chamber insulating material of the present invention contains inorganic fibers, it is durable and can be supplied at low cost.

[0055] The combustion chamber insulating material of the present invention can be used, for example, in devices equipped with a combustion chamber, such as water heaters and boilers.

[0056] [Water heater] The water heater of the present invention comprises a combustion chamber, a heat exchanger installed in the combustion chamber, and the combustion chamber insulating material of the present invention, and is characterized in that the first main surface of the combustion chamber insulating material is arranged facing the inner wall surface of the combustion chamber. The water heater of the present invention comprises the combustion chamber insulating material of the present invention, and since the bulk density of the first main surface is low, an air layer can be created on the inner wall surface side of the combustion chamber to enhance the insulating effect, and CO 2 It has excellent emission suppression effect.

[0057] An example of a water heater of the present invention will be described below. FIG. 6 is a cross-sectional view schematically showing an example of a water heater of the present invention. The water heater 500 has a combustion chamber 540 and a heat exchanger 170 disposed within the combustion chamber 540. The combustion chamber 540 has a metal container 150 and two combustion chamber insulation materials 1 disposed on a top surface 150a and a bottom surface 150b of the metal container 150. The combustion chamber insulation material 1 is disposed such that a first main surface 10a faces the inner wall surface of the combustion chamber. Water flows within the heat exchanger 170, and the water within the heat exchanger 170 is heated in the combustion chamber 540 to become hot water (hot water), which is then supplied outside the water heater 500.

[0058] The temperature of the hot water supplied can be adjusted appropriately by adjusting the amount of fuel burned in the combustion chamber and the amount of water passing through the heat exchanger per unit time.

[0059] [Boiler] The boiler of the present invention comprises a combustion chamber and the combustion chamber insulating material of the present invention, and is characterized in that the first main surface of the combustion chamber insulating material is disposed facing the inner wall surface of the combustion chamber. The boiler of the present invention comprises the combustion chamber insulating material of the present invention, and since the bulk density of the first main surface is low, an air layer can be created on the inner wall surface side of the combustion chamber, thereby enhancing the insulating effect, and 2 It has excellent emission suppression effect.

[0060] An example of a boiler of the present invention will be described below. FIG. 7 is a cross-sectional view schematically illustrating an example of a boiler of the present invention. The boiler 600 includes a combustion chamber 550 and a water pipe 180 disposed within the combustion chamber 550. The combustion chamber 550 includes a metal container 160 and two combustion chamber insulation materials 1 disposed on the top surface 160a and bottom surface 160b of the metal container 160. The combustion chamber insulation material 1 is disposed with its first main surface 10a facing the inner wall surface of the combustion chamber. Water is supplied to the water pipe 180 from the lower part of the combustion chamber 550. The water passing through the water pipe 180 is heated within the combustion chamber 550 to become steam, which is then discharged from the upper part of the combustion chamber 550. The discharged steam is used for power generation, heating, cleaning, cooking, drying, disinfection, sterilization, and other purposes after separating the liquid water or superheating as necessary.

[0061] The method for disposing the combustion chamber insulating material on the inner wall surface of the combustion chamber is not particularly limited, and for example, it can be fixed with bolts and nuts. The first main surface portion of the combustion chamber insulating material may be disposed on the inner wall surface of the combustion chamber via an inorganic adhesive.

[0062] The present specification discloses the following:

[0063] The present disclosure (1) is a plate-shaped molded body containing inorganic fibers, characterized in that when comparing the bulk densities of a first main surface portion, a second main surface portion, and a central portion located between the first main surface portion and the second main surface portion in the thickness direction, the bulk density of at least the first main surface portion is smaller than the bulk density of the central portion, and the first main surface portion is arranged toward the inner wall surface of the combustion chamber.

[0064] The present disclosure (2) is a combustion chamber insulating material according to the present disclosure (1), wherein the bulk density of the second main surface portion is (i) greater than the bulk density of the central portion, or (ii) less than the bulk density of the central portion.

[0065] The present disclosure (3) is a combustion chamber insulating material according to the present disclosure (1) or (2), which is formed by a papermaking method.

[0066] The present disclosure (4) is a combustion chamber insulating material according to any one of the present disclosures (1) to (3), which has a flat or curved shape.

[0067] The present disclosure (5) provides a method for manufacturing a granular ... 3 The combustion chamber insulating material according to any one of the present disclosures (1) to (4),

[0068] The present disclosure (6) is a combustion chamber insulating material according to any one of the present disclosures (1) to (5), in which the bulk density of the first main surface portion is 3% or more smaller than the larger of the bulk density of the second main surface portion and the bulk density of the central portion.

[0069] The present disclosure (7) is a water heater comprising a combustion chamber, a heat exchanger installed in the combustion chamber, and a combustion chamber insulating material described in any one of the present disclosures (1) to (6), characterized in that a first main surface portion of the combustion chamber insulating material is arranged facing the inner wall surface of the combustion chamber.

[0070] The present disclosure (8) is a boiler comprising a combustion chamber and a combustion chamber insulating material described in any one of the present disclosures (1) to (6), wherein a first main surface portion of the combustion chamber insulating material is arranged facing the inner wall surface of the combustion chamber.

[0071] (Examples) Examples that more specifically disclose the present invention are shown below. Note that the present invention is not limited to these examples. In the following examples, the upper layer of the plate-shaped molded body corresponds to the first main surface portion, the middle layer corresponds to the central portion, and the lower layer corresponds to the second main surface portion.

[0072] Example 1: Water, AES fiber, inorganic binder (silica sol), organic binder (acrylate-based latex), and coagulant (aluminum sulfate) were added to a commercially available pulper and dispersed to prepare a slurry. The prepared slurry was poured into a mold, dehydrated, and a prototype sheet was obtained by a papermaking method. The thickness of the prototype sheet was 38 mm. A Teflon (registered trademark)-coated SUS metal plate was placed on the first main surface of the obtained prototype sheet and dried at 150°C for 30 minutes. Thereafter, the prototype sheet was sandwiched between two identical SUS metal plates from the first and second main surfaces, and the thickness of the prototype sheet was adjusted to 30 mm. The thickness was then adjusted to 30 mm and dried at 150°C for 1 hour to obtain a plate-shaped molded product. The bulk density of the upper layer of the obtained plate-shaped molded product was 0.294 g / cm 3 , the bulk density of the middle layer is 0.316 g / cm 3 , the bulk density of the lower layer is 0.338 g / cm 3 It was.

[0073] Example 2: Water, AES fiber, an inorganic binder (silica sol), an organic binder (acrylate-based latex), and a flocculant (aluminum sulfate) were added to a commercially available pulper and dispersed to prepare a slurry liquid according to Example 2. The prepared slurry liquid was poured into a mold, dehydrated, and a prototype sheet was obtained by a papermaking method. The thickness of the prototype sheet was 35 mm. A Teflon (registered trademark)-coated SUS metal plate was placed on the second main surface of the obtained prototype sheet and dried at 150°C for 30 minutes. Next, the prototype sheet was turned over, and the same SUS metal plate was placed on the first main surface and dried at 150°C for 30 minutes. Thereafter, the prototype sheet was sandwiched between two identical SUS metal plates from the first and second main surfaces, and the thickness of the prototype sheet was adjusted to 30 mm. The thickness was then adjusted to 30 mm and dried at 150°C for 1 hour to obtain a plate-shaped molded product. The bulk density of the upper layer of the obtained plate-like molded body was 0.221 g / cm 3 , the bulk density of the middle layer is 0.239 g / cm 3 , the bulk density of the lower layer is 0.226 g / cm 3 It was.

[0074] Example 3 Using the slurry prepared in Example 1, a base sheet was made and dried in the same manner as in Example 2 to obtain a plate-like molded product having a thickness of 30 mm. The bulk density of the upper layer of the obtained plate-like molded product was 0.291 g / cm 3, the bulk density of the middle layer is 0.320 g / cm 3 , the bulk density of the lower layer is 0.293 g / cm 3 It was.

[0075] Comparative Example 1 A 30 mm thick original sheet was obtained in the same manner as in Example 1. The obtained original sheet was placed on a plate-like shelf in a dryer and dried at 150°C for 3 hours to obtain a 30 mm thick plate-like molded product. The obtained plate-like molded product had a uniform bulk density of 0.300 g / cm. 3 It was.

[0076] Comparative Example 2 A 30 mm thick original sheet was obtained in the same manner as in Example 2. The obtained original sheet was placed on a plate-like shelf in a dryer and dried at 150°C for 3 hours to obtain a 30 mm thick plate-like molded product. The obtained plate-like molded product had a uniform bulk density of 0.220 g / cm. 3 It was.

[0077] Comparative Example 3 Water, AES fiber, an inorganic binder (silica sol), an organic binder (acrylate-based latex), and a flocculant (aluminum sulfate) were charged into a commercially available pulper and dispersed to prepare a slurry liquid according to Comparative Example 3. The prepared slurry liquid was poured into a mold, dehydrated, and a 15 mm thick original sheet was obtained by a papermaking method. The obtained original sheet was placed on a plate-like shelf in a dryer and dried at 150°C for 3 hours to obtain a plate-like molded product S. The obtained plate-like molded product had a uniform bulk density of 0.350 g / cm. 3 The same procedure as in Comparative Example 2 was used to obtain a 15 mm thick sheet with a bulk density of 0.220 g / cm. 3 The plate-shaped body T was placed on the plate-shaped body S to obtain a plate-shaped body having a thickness of 30 mm.

[0078] Comparative Example 4 A castable refractory material containing an appropriate amount of water was molded and dried to obtain a plate-shaped molded product having a diameter of 70 mm and a thickness of 30 mm. The bulk density was 0.760 g / cm. 3 It was.

[0079] (Measurement of bulk density) For the plate-like molded articles of Examples 1 to 3, the plate-like molded articles were punched into squares with sides of 50 mm and cut into three equal parts in the thickness direction. Next, the weight and thickness of each of the plate-like molded articles cut into three parts were measured. The thickness was measured with a vernier caliper. Then, as shown in the following formula, the bulk density of the first main surface portion, the bulk density of the second main surface portion, and the bulk density of the central portion were calculated from the areal specific gravity (weight / area) calculated from the weight and the thickness. (weight / area) / thickness = bulk density [g / cm 3 ]

[0080] The bulk density of the plate-like molded articles of Comparative Examples 1 and 2 and the castable molded article of Comparative Example 4 was calculated from the weight and thickness without cutting using the above formula.

[0081] The weight and thickness of each of the plate-shaped molded products S and T of Comparative Example 3 were measured, and the bulk density was calculated from the above formula.

[0082] (Insulation Evaluation) The insulation properties of the plate-shaped compacts of Examples 1 to 3 and Comparative Examples 1 to 3, and the castable compact of Comparative Example 4, were evaluated by the following method. A heating plate (Inconel: registered trademark) with an embedded heater to reproduce the temperature conditions in a combustion chamber and a stainless steel plate were prepared, and the plate-shaped compact or castable compact was sandwiched and fixed between these two plates. The plate-shaped compacts of Examples 1 to 3 and Comparative Example 3 were arranged so that the main surface of the upper layer side or the side with lower bulk density was in contact with the stainless steel plate. In Comparative Example 5, the main surface of the plate-shaped compact of Example 1 with higher bulk density was in contact with the stainless steel plate. The heating plate was heated to 1000°C and maintained for 10 minutes. Thereafter, the temperature of the stainless steel plate on the surface in contact with the plate-shaped compact or castable compact was measured. The results are shown in Table 1. A lower temperature indicates better insulation properties.

[0083] (Evaluation of bending strength) The bending strength of the plate-shaped molded product in the present invention was measured by preparing a sample of the plate-shaped molded product having a width of 40 mm, a length of 200 mm, and a thickness of 30 mm and using a universal testing machine (model number: 5567, manufactured by Instron). The measurement method was in accordance with JIS R2619 (Test method for bending strength of insulating firebricks), and the maximum load was determined using the above-mentioned sample dimensions, a pressure rate of 10 mm / min, and a distance between support rolls of 150 mm, and the bending strength was calculated. A bending strength of 0.28 MPa or more was evaluated as ◯, and a bending strength of less than 0.28 MPa was evaluated as △. The results are shown in Table 1.

[0084]

[0085] As shown in Table 1, the insulating materials of Examples 1 to 3, in which the upper layer (metal surface side) of the plate-shaped molded body has a lower bulk density than the middle layer, have superior insulating properties compared to the insulating material of Comparative Example 1, which uses a plate-shaped molded body with a uniform bulk density, and Comparative Example 4, which uses a castable molded body. Comparative Example 3 had a low bulk density of the plate-shaped molded body on the metal surface side, and the insulating properties were equivalent to those of Examples 1 to 3. However, because multiple plate-shaped molded bodies were stacked, the bending strength was lower than that of the insulating materials of Examples 1 to 3, which are integrated plate-shaped molded bodies, resulting in a high risk of breakage of the low-density portion during handling. Comparative Example 2 had the same insulating properties as Examples 1 to 3, but because the bulk density was too low, the bending strength was insufficient, resulting in a high risk of breakage during handling. Comparative Example 5 used the same plate-shaped molded body as Example 1, but the bulk density on the metal surface side was high, resulting in inferior insulating properties compared to Example 1.

[0086] DESCRIPTION OF SYMBOLS 1, 1A, 1B Heat insulating material for combustion chamber 10, 10A, 10B Plate-shaped molded body 10a, 10Aa, 10Ba First main surface of plate-shaped molded body 10b, 10Ab, 10Bb Second main surface of plate-shaped molded body 10c Side surface of plate-shaped molded body 11 First main surface portion 12 Second main surface portion 13 Central portion 50 Original sheet 50a First main surface of original sheet 50b Second main surface of original sheet HP SUS plate 150, 160 Metal container 150a, 160a Top surface of metal container 150b, 160b Bottom surface of metal container 170 Heat exchanger 180 Water pipe 540, 550 Combustion chamber 500 Water heater 600 Boiler

Claims

1. A combustion chamber insulation material comprising a plate-like molded body containing inorganic fibers, characterized in that, when comparing the bulk densities of a first main surface portion, a second main surface portion, and a central portion located between the first main surface portion and the second main surface portion in the thickness direction, the bulk density of at least the first main surface portion is smaller than the bulk density of the central portion, and the first main surface portion is disposed facing the inner wall surface of the combustion chamber.

2. A combustion chamber insulation material as described in claim 1, wherein the bulk density of the second main surface portion is (i) greater than the bulk density of the central portion, or (ii) less than the bulk density of the central portion.

3. The combustion chamber insulating material according to claim 1 or 2, which is formed by a papermaking method.

4. The combustion chamber insulating material according to any one of claims 1 to 3, which has a flat or curved shape.

5. Overall bulk density: 0.20-0.35 g / cm 3 The combustion chamber insulating material according to any one of claims 1 to 4.

6. A combustion chamber insulation material as described in any one of claims 1 to 5, wherein the bulk density of the first main surface portion is 3% or more smaller than the larger of the bulk density of the second main surface portion and the bulk density of the central portion.

7. A water heater comprising: a combustion chamber; a heat exchanger installed within the combustion chamber; and a combustion chamber insulation material according to any one of claims 1 to 6, wherein a first main surface portion of the combustion chamber insulation material is arranged facing the inner wall surface of the combustion chamber.

8. A boiler comprising: a combustion chamber; and a combustion chamber insulation material according to any one of claims 1 to 6, wherein a first main surface portion of the combustion chamber insulation material is arranged facing the inner wall surface of the combustion chamber.

Citation Information

Patent Citations

  • Hot-water boiler

    JP1984086853A

  • Heat-insulating method of high temperature furnace

    JP1989058987A

  • Molding insulated material

    JP1990227244A

  • Adiabatic acoustic material

    JP1993318639A

  • Inorganic fiber molded article having three-layer structure