Polishing composition, and polishing method using same
The polishing composition with specific silica particles and inorganic anti-caking agents addresses the challenges of redispersibility and abrasive residue, improving the polishing efficiency for resin and filler materials by maintaining fluidity and reducing surface residue.
Patent Information
- Application Number
- PCT/JP2024/011365
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-22
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional polishing compositions for resin and filler materials face challenges in maintaining redispersibility of sediment and reducing abrasive grain residue on the polished surface, leading to inefficient polishing processes.
A polishing composition comprising silica particles with a specific particle size and circularity as abrasive grains, combined with an inorganic anti-caking agent, where the zeta potential product is positive, enhances redispersibility and reduces abrasive grain residue by maintaining fluidity and improving polishing efficiency.
The composition achieves excellent redispersibility and significantly reduces abrasive grain residue on the polished surface, enhancing the polishing rate and process efficiency for resin and filler materials.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002
Abstract
Description
Polishing composition and polishing method using the same
[0001] The present invention relates to a polishing composition and a polishing method using the same.
[0002] Conventionally, various studies have been conducted on polishing compositions made of various materials containing resins.
[0003] WO 2022 / 185793 (corresponding to US Patent Application Publication No. 2024 / 002697) discloses a polishing composition for polishing an object containing a resin and a filler. More specifically, WO 2022 / 185793 (corresponding to US Patent Application Publication No. 2024 / 002697) discloses that a polishing composition containing silica particles having an average particle size and circularity of a predetermined value or more as abrasive grains and a dispersion medium can reduce the abrasive grain residue on the surface of the object to be polished after polishing. In addition, WO 2022 / 185793 (corresponding to US Patent Application Publication No. 2024 / 002697) discloses that by leaving the polishing composition to stand, the polishing composition undergoes solid-liquid separation, resulting in sediment. However, it is disclosed that the polishing composition contains a redispersant, which can redisperse the sediment into the liquid portion.
[0004] The present inventor has found that, during the study of the stability of polishing composition, when the polishing composition is left standing for a long time, the fluidity of sediment is lost, and the re-dispersion of sediment may be difficult, and there is a need for a polishing composition that realizes high level of re-dispersibility of sediment.In addition, the present inventor has found that there is a need for further improvement in the reduction of abrasive grain residue on the surface of the polished object (especially the polished object that contains resin and filler) after polishing.Therefore, there is a need to achieve both the re-dispersibility of sediment generated in the polishing composition and the reduction of abrasive grain residue on the surface of the polished object after polishing at a sufficient level.
[0005] Therefore, the present invention has been made in consideration of the above circumstances, and aims to provide a means that has good redispersibility of sediments that occur in a polishing composition and can reduce abrasive grain residue on the surface of an object to be polished (especially an object to be polished that contains a resin and a filler) after polishing.
[0006] The present inventors have conducted extensive research to solve the above-mentioned problems, and as a result, have found that the above-mentioned problems can be solved by a polishing composition that contains silica particles having a specific particle size and circularity as abrasive grains and inorganic particles as an anti-caking agent, and in which the product of the zeta potential of the abrasive grains, the zeta potential of the anti-caking agent, and the zeta potential is positive, thereby completing the present invention.
[0007] That is, the above-mentioned problems of the present invention can be solved by the following means.
[0008] One embodiment of the present invention that can solve the above-mentioned problems is a polishing composition comprising abrasive grains, an anti-caking agent, and a dispersion medium, wherein the abrasive grains are silica particles having an average particle diameter (D50) of more than 1.0 μm and a primary particle circularity of 0.90 or more, the anti-caking agent is inorganic particles different from the abrasive grains, and the product of the zeta potential of the abrasive grains and the zeta potential of the anti-caking agent is positive.
[0009] The following describes embodiments of the present invention. The embodiments shown here are provided as examples to embody the technical concept of the present invention and are not intended to limit the present invention. Therefore, all other possible embodiments, methods of use, and operational techniques that can be conceived by those skilled in the art without departing from the spirit of the present invention are included in the scope and spirit of the present invention, as well as in the scope of the inventions described in the claims and their equivalents. The embodiments described in this specification can be combined in any manner to create other embodiments.
[0010] In this specification, unless otherwise specified, the operations and measurements of physical properties are carried out at room temperature (20° C. to 25° C.) and at a relative humidity of 40% RH to 50% RH.
[0011] <Polishing Composition> One aspect of the present invention relates to a polishing composition comprising abrasive grains, an anti-caking agent, and a dispersion medium, wherein the abrasive grains are silica particles having an average particle diameter (D50) of more than 1.0 μm and a primary particle circularity of 0.90 or more, the anti-caking agent is inorganic particles different from the abrasive grains, and the product of the zeta potential of the abrasive grains and the zeta potential of the anti-caking agent is positive. This aspect of the polishing composition provides good redispersibility of sediment generated in the polishing composition, maintains the fluidity of the sediment, and reduces abrasive grain residue on the surface of the polished object (especially an object containing a resin and a filler) after polishing. The abrasive grains contain silica particles having the above-mentioned specific particle size and circularity, and the anti-caking agent contains inorganic particles (excluding the silica particles contained as abrasive grains), and the product of the zeta potential of the abrasive grains and the zeta potential of the anti-caking agent is positive (i.e., both zeta potentials have the same sign). This allows for good redispersibility of sediments produced in the polishing composition, and reduces the amount of abrasive residue on the surface of the polished object (particularly the polished object containing resin and filler) after polishing. That is, it is possible to achieve a good balance between good redispersibility of sediments produced in the polishing composition and a reduction in the amount of abrasive residue on the surface of the polished object (particularly the polished object containing resin and filler) after polishing. Furthermore, it is possible to achieve a good balance between good redispersibility of sediments produced in the polishing composition and a reduction in the amount of abrasive residue on the surface of the polished object (particularly the polished object containing resin and filler) after polishing. Therefore, according to this embodiment, the redispersibility of the sediment generated in the polishing composition is good, and the abrasive grain residue on the surface of the polishing object (especially the polishing object containing a resin and a filler) after polishing can be reduced. Hereinafter, the redispersibility of the sediment generated in the polishing composition is also referred to as "redispersibility of the polishing composition."
[0012] The polishing composition according to this embodiment is typically supplied to an object to be polished in the form of a polishing liquid containing the polishing composition and used to polish the object to be polished. The polishing composition according to this embodiment may be used as a polishing liquid after dilution (typically with water), or may be used as a polishing liquid as is. That is, the concept of the polishing composition in the technology according to this embodiment includes both a polishing composition (working slurry) supplied to an object to be polished and used to polish the object to be polished, and a concentrated liquid (raw solution of working slurry) that is diluted and used for polishing. The concentration ratio of the concentrated liquid can be, for example, about 2 to 100 times on a volume basis, and is usually about 5 to 50 times.
[0013] [Abrasive grains] <Silica particles> The abrasive grains contained in the polishing composition according to this embodiment have an average particle diameter (D 50 ) and a primary particle circularity of 0.90 or more. In this specification, unless otherwise specified, the abrasive grains are silica particles having an average particle diameter (D 50 ) and a primary particle circularity of 0.90 or more are also simply referred to as "silica particles according to this embodiment" or "silica particles."
[0014] In one embodiment of this aspect, both dry silica particles and wet silica particles are preferably used as the silica particles. The silica particles can be easily produced by appropriately referring to known production methods. In addition, the silica particles have an average particle diameter (D 50 ) and the circularity of the primary particles are satisfied, commercially available products may be used. Methods for producing dry silica particles include a flame hydrolysis method, a deflagration method, and a fusion method. Methods for producing wet silica particles (particularly colloidal silica particles) include a sodium silicate method, an alkoxide method, and a sol-gel method. Regardless of the method used, the silica particles produced by any of these methods can have the average particle diameter (D 50 As long as the silica particles satisfy the above requirements, the silica particles of the present invention can be suitably used. Among these silica particles, dry silica particles are particularly preferred. Furthermore, the deflagration method and the melting method are preferred as the manufacturing methods.
[0015] In one embodiment, the raw silica particles are silica particles obtained by a sodium silicate method, which is a method of growing particles from activated silicic acid, typically obtained by ion-exchanging an aqueous solution of an alkali silicate such as water glass, as a raw material.
[0016] In one embodiment, the raw silica particles are silica particles obtained by the alkoxide method, which typically uses alkoxysilane as a raw material and subjects it to a hydrolysis and condensation reaction.
[0017] In one embodiment, the raw silica particles are silica particles obtained by a vaporized metal combustion method (VMC method). The VMC method is a method of producing silica particles by burning a combustion improver (such as a hydrocarbon gas) with a burner in an oxygen-containing atmosphere to form a chemical flame, and then adding metallic silica into the chemical flame in an amount sufficient to form a dust cloud, causing deflagration.
[0018] In one embodiment, the raw silica particles are obtained by a fusion method, which involves introducing silica into a flame, melting it, and then cooling it to obtain silica particles.
[0019] The type of silica particles used is not particularly limited, but for example, surface-modified silica particles can be used. For example, the silica particles may have a cationic group. Preferred examples of silica particles having a cationic group include silica particles with amino groups fixed to their surfaces. Examples of methods for producing silica particles having such cationic groups include a method described in JP 2005-162533 A in which a silane coupling agent having an amino group, such as aminoethyltrimethoxysilane, aminopropyltrimethoxysilane, aminoethyltriethoxysilane, aminopropyltriethoxysilane, aminopropyldimethylethoxysilane, aminopropylmethyldiethoxysilane, or aminobutyltriethoxysilane, is fixed to the surface of the abrasive grain. This allows for the production of silica particles with amino groups fixed to their surfaces (amino-group-modified silica particles).
[0020] Silica particles may have anionic group.Preferably, as the silica particles having anionic group, the silica particles that have anionic group such as carboxylic acid group, sulfonic acid group, phosphonic acid group, aluminic acid group, etc. fixed on the surface.The method for producing the silica particles having such anionic group is not particularly limited, and for example, the method of reacting the silane coupling agent having anionic group at the end with silica particles can be mentioned.
[0021] As a specific example, sulfonic acid groups can be immobilized on silica particles by the method described in, for example, "Sulfonic acid-functionalized silica through quantitative oxidation of thiol groups," Chem. Commun. 246-247 (2003). Specifically, silica particles having sulfonic acid groups immobilized on their surfaces can be obtained by coupling a silane coupling agent having a thiol group, such as 3-mercaptopropyltrimethoxysilane, to silica particles and then oxidizing the thiol group with hydrogen peroxide.
[0022] Alternatively, when carboxylic acid groups are immobilized on silica particles, this can be done, for example, by the method described in "Novel Silane Coupling Agents Containing a Photolabile 2-Nitrobenzyl Ester for Introduction of a Carboxy Group on the Surface of Silica Gel", Chemistry Letters, 3, 228-229 (2000). Specifically, silica particles having carboxylic acid groups immobilized on their surfaces can be obtained by coupling a silane coupling agent containing a photoreactive 2-nitrobenzyl ester to silica particles and then irradiating the particles with light.
[0023] The average particle diameter (D 50 ) is greater than 1.0 μm. 50If the average particle diameter (D) of the silica particles is 1.0 μm or less, the polishing rate of the object to be polished is insufficient. 50 ) is preferably greater than 1.2 μm, more preferably 1.5 μm or more, particularly preferably 1.8 μm or more, and most preferably 2.0 μm or more. 50 ) is preferably 20.0 μm or less, more preferably 15.0 μm or less, particularly preferably 13.0 μm or less, and particularly preferably 12.0 μm or less. In particular, the average particle diameter (D 50 When the average particle diameter (D) of the silica particles is 3.0 μm or more and 10.0 μm or less (particularly 5.0 μm or more and 8.0 μm or less), abrasive grain residue can be more effectively reduced while maintaining a high polishing rate. 50 A preferred example of the particle diameter is preferably more than 1.2 μm and not more than 20 μm, more preferably 1.5 μm or more and 15.0 μm or less, particularly preferably 1.8 μm or more and 13.0 μm or less, and most preferably 2.0 μm or more and 12.0 μm or less. Within the above range, the polishing speed of the object to be polished can be improved, and abrasive grain residue on the surface of the object to be polished after polishing can be reduced, resulting in a better balance between improved polishing speed and reduced abrasive grain residue. Furthermore, within this range, a smaller particle diameter is more suitable for reducing abrasive grain residue, and a larger particle diameter is more suitable for improving the polishing speed. The average particle diameter (average secondary particle diameter) of silica particles is the particle diameter (D) at which the cumulative frequency from the small particle diameter side in the volume-based particle size distribution becomes 50%. 50 ) where the average particle diameter of the silica particles (D 50 ) can be determined by dynamic light scattering, laser diffraction, laser scattering, or pore electrical resistance, etc. Specifically, the value determined by the measurement method described in the Examples below is used.
[0024] The particle diameter D of the silica particles, which are abrasive grains contained in the polishing composition according to this embodiment 10 is preferably greater than 1.2 μm, more preferably 1.5 μm or more, particularly preferably 1.8 μm or more, and most preferably 2.0 μm or more. 10is preferably 10.0 μm or less, more preferably 8.0 μm or less, particularly preferably 5.0 μm or less, and particularly preferably 4.0 μm or less. 10 When the particle diameter D of the silica particles is in the above range, a high polishing rate can be maintained while the abrasive grain residue can be more effectively reduced. 10 A preferred example of the particle diameter D of the silica particles is preferably more than 1.2 μm and not more than 10 μm, more preferably 1.5 μm or more and 8.0 μm or less, particularly preferably 1.8 μm or more and 5.0 μm or less, and most preferably 2.0 μm or more and 4.0 μm or less. 10 When the particle diameter D of the silica particles is within the above range, the polishing rate of the object to be polished can be improved and the amount of abrasive grain residue on the surface of the object to be polished after polishing can be reduced, thereby achieving a good balance between the improvement in the polishing rate and the reduction in the amount of abrasive grain residue. 10 is the particle diameter D at which the cumulative frequency from the small particle diameter side in the volume-based particle size distribution becomes 10%. 10 Here, the particle diameter D of the silica particles 10 is determined by dynamic light scattering, laser diffraction, laser scattering, or pore electrical resistance, etc. Specifically, the value determined by the measurement method described in the Examples below is used.
[0025] The circularity of the primary particles of the silica particles, which are abrasive grains contained in the polishing composition according to this embodiment (hereinafter also referred to simply as "circularity"), is 0.90 or more. If the circularity of the primary particles of the silica particles is less than 0.90, the abrasive grains will remain stuck on the surface of the object to be polished due to the unevenness of the surface, resulting in an excessive increase in abrasive grain residue on the surface after polishing. The circularity of the primary particles of the silica particles is preferably 0.92 or more, more preferably 0.95 or more, and particularly preferably greater than 0.95. A preferred example of the circularity of the primary particles of the silica particles is preferably 0.92 or more and 1.00 or less, more preferably 0.95 or more and 1.00 or less, and particularly preferably greater than 0.95 and 1.00 or less. Within the above range, the polishing rate of the object to be polished can be improved and the abrasive grain residue on the surface of the object to be polished after polishing can be reduced, thereby achieving a better balance between improved polishing rate and reduced abrasive grain residue. In this specification, the circularity of the primary particles of silica particles is determined to three decimal places by the method described in the Examples below, and the value obtained by rounding off the three decimal places is used. The closer the circularity is to 1 (1.00), the closer it is to a perfect sphere, and therefore, the closer the circularity is to 1 (1.00), the higher the proportion of particles that are close to perfect spheres contained in the silica particles. By using particles that are closer to perfect spheres as abrasive grains, the above-mentioned effects may be more easily obtained.
[0026] Here, the zeta potential of silica particles, which are abrasive grains contained in the polishing composition of this embodiment, is not particularly limited, as long as the product of the zeta potential of the anti-caking agent described below is positive, but for example, the absolute value of the zeta potential is 0.5 mV or more.The absolute value of the zeta potential of silica particles is preferably 10 mV or more, more preferably 20 mV or more, even more preferably 30 mV or more, particularly preferably 40 mV or more, and most preferably 45 mV or more.The absolute value of the zeta potential of silica particles is preferably 80 mV or less, more preferably 70 mV or less, even more preferably 65 mV or less, particularly preferably 60 mV or less, and most preferably 55 mV or less.When the absolute value of the zeta potential of silica particles is within the above range, the redispersibility of the precipitates generated in the polishing composition is further improved, and the abrasive grain residue on the surface of the object to be polished after polishing can be further reduced.
[0027] In one embodiment, the silica particles have a modified Mohs hardness of 5 or more and 9 or less. Such a hardness allows for a better balance between an improvement in the removal rate and a reduction in abrasive grain residue.
[0028] The silica particles may be used alone or in combination of two or more.
[0029] The concentration (content) of silica particles in the polishing composition according to this embodiment is not particularly limited.In the case of a polishing composition (typically a slurry-like polishing liquid, sometimes referred to as a working slurry or polishing slurry) that is used as a polishing liquid for polishing an object to be polished as is, the concentration (content) of silica particles is preferably 0.05% by mass or more, more preferably 0.1% by mass or more, even more preferably more than 0.1% by mass, and particularly preferably 0.2% by mass or more, based on the total mass of the polishing composition.As the concentration (content) of silica particles increases, the polishing rate is further improved.In addition, the concentration (content) of silica particles is preferably 20% by mass or less, more preferably 15% by mass or less, even more preferably 10% by mass or less, even more preferably less than 10% by mass, and particularly preferably 8% by mass or less, based on the total mass of the polishing composition.Within the above range, the occurrence of defects such as abrasive grain residue is further reduced. A preferred example of the concentration (content) of silica particles is preferably 0.05 mass% or more and 20 mass% or less, more preferably 0.1 mass% or more and 15 mass% or less, more preferably more than 0.1 mass% and 10 mass% or less, more preferably more than 0.1 mass% and less than 10 mass%, particularly preferably 0.2 mass% or more and 8 mass% or less, based on the total mass of the polishing composition.In the above range, the polishing speed of the object to be polished can be improved, and the redispersibility of the precipitates generated in the polishing composition can be further improved, so that the abrasive grain residue on the surface of the object to be polished after polishing can be further reduced.It should be noted that when using two or more kinds of silica particles, the concentration (content) of the silica particles refers to the total amount of all silica particles.
[0030] Furthermore, in the case of a polishing composition that is diluted and used for polishing (i.e., a concentrate, a raw solution of a working slurry), the concentration (content) of silica particles is usually appropriate to be 30% by mass or less, and more preferably 25% by mass or less, from the viewpoints of storage stability, filterability, etc. Furthermore, from the viewpoint of utilizing the advantages of forming a concentrate, the concentration (content) of silica particles is preferably 1% by mass or more, more preferably 4% by mass or more.
[0031] The abrasive grains have a substantially average particle diameter (D 50 ) is greater than 1.0 μm and the circularity of the primary particles is 0.90 or more. Here, "the abrasive grains are substantially composed of the silica particles according to this embodiment" means that the total content of the silica particles contained in the polishing composition is greater than 99% by mass (upper limit: 100% by mass) of the total content of the abrasive grains contained in the polishing composition. Preferably, the abrasive grains are composed only of the silica particles according to this embodiment (the total content of the silica particles according to this embodiment is 100% by mass of all the abrasive grains).
[0032] [Anti-caking agent] The anti-caking agent contained in the polishing composition according to this embodiment is an inorganic particle different from the silica particles contained as abrasive grains. That is, the anti-caking agent has an average particle diameter (D 50 ) is greater than 1.0 μm and the circularity of the primary particles is 0.90 or more. The anti-caking agent has the function of maintaining the fluidity of the sediment when the solid content (e.g., abrasive grains) contained in the polishing composition settles. Therefore, by using the anti-caking agent, the sediment formed in the polishing composition after storage can be easily redispersed in the liquid by shaking or stirring.
[0033] The anti-caking agent has an average particle size (D 50 ) and inorganic particles other than silica particles having a primary particle circularity of 0.90 or more, but 50 The anti-caking agent may be a synthetic product or a commercially available product.
[0034] Examples of inorganic particles used as anti-caking agents include silica (having an average particle diameter (D) of greater than 1.0 μm). 50(excluding silica particles having a primary particle circularity of 0.90 or more), and metal oxides such as alumina, zirconia, and titania. Alumina is preferred to efficiently achieve the desired effects of the present invention. Suitable examples of alumina include, but are not limited to, α-alumina, intermediate alumina (γ-alumina, δ-alumina, θ-alumina), colloidal alumina, and fumed alumina, all of which can be suitably used. Among these, colloidal alumina and fumed alumina are preferred, with colloidal alumina being more preferred. Therefore, in one embodiment of the present invention, the anti-caking agent is colloidal alumina. This embodiment maintains the fluidity of sediments in the workpiece and exhibits good redispersibility.
[0035] The average particle size of anti-caking agent is preferably 900nm or less, more preferably 800nm or less, even more preferably 700nm or less, particularly preferably 600nm or less, and most preferably 500nm or less.The average particle size of anti-caking agent is preferably 1nm or more, more preferably 5nm or more, even more preferably 10nm or more, particularly preferably 15nm or more, and most preferably 20nm or more.If the average particle size of anti-caking agent is within the above range, even when the solid content (abrasive grains) in the polishing composition settles, the sediment can maintain fluidity and exhibit better redispersibility. The average particle size of the anti-caking agent is determined by photographing the anti-caking agent with a scanning electron microscope (SEM) (manufactured by Hitachi High-Tech Corporation, product name: SU8000) or a scanning transmission electron microscope (STEM) (manufactured by Hitachi High-Tech Corporation, product name: HD-2700), and analyzing the resulting SEM image using image analysis software (manufactured by Mitani Shoji Co., Ltd., "WinROOF 2018"). Specifically, 30 particles are randomly selected as samples from the particles present in the SEM image, the particle size of each particle is measured, and the average is calculated, which is the average value that serves as the average particle size of the anti-caking agent.
[0036] In the polishing composition according to this embodiment, the average particle size of the anti-caking agent may be 450 nm or less, 400 nm or less, 350 nm or less, 300 nm or less, 250 nm or less, 200 nm or less, 150 nm or less, 100 nm or less, or 50 nm or less. In one embodiment, the anti-caking agent is alumina particles having an average particle size of 500 nm or less. In another embodiment, the anti-caking agent is alumina particles having an average particle size of 200 nm or less.
[0037] Here, the zeta potential of the anti-caking agent has a relationship such that the product of the zeta potential of the abrasive grains (silica particles) is positive. That is, in the polishing composition of this embodiment, the zeta potential of the abrasive grains and the zeta potential of the anti-caking agent have the same sign. For example, in the polishing composition of this embodiment, when the zeta potential of the abrasive grains is positive, the zeta potential of the anti-caking agent is also positive, and when the zeta potential of the abrasive grains is negative, the zeta potential of the anti-caking agent is also negative. When the zeta potential of the abrasive grains and the zeta potential of the anti-caking agent have such a relationship in the polishing composition, the fluidity of the sediment formed by leaving the polishing composition stationary can be maintained, and for example, it is thought that the sediment can be redispersed into the liquid portion simply by shaking or stirring the polishing composition in which the sediment has formed. The mechanism by which such an effect is achieved by the present invention is presumed as follows, but the following mechanism is merely speculation and does not limit the scope of the present invention.
[0038] When solid-liquid separation occurs in a polishing composition, the abrasive grains and the anti-caking agent are thought to form sediments. When the zeta potential of the abrasive grains and the zeta potential of the anti-caking agent are the same sign, repulsive forces act between the abrasive grains and the anti-caking agent, causing these particles to stack in a bulky state and form sediments. In this case, the particles forming the sediment have fluidity, and it is thought that simply shaking or stirring the polishing composition in which sediments have formed will redisperse the sediments into the liquid. On the other hand, when the zeta potential of the abrasive grains and the zeta potential of the anti-caking agent are opposite signs, attractive forces act between the abrasive grains and the anti-caking agent, causing these particles to stack in close proximity and form sediments. In this case, the particles forming the sediment lose fluidity, and it is thought that simply shaking or stirring the polishing composition in which sediments have formed will not loosen the sediments and make it impossible to redisperse them into the liquid. Furthermore, the present inventors have found that improving the redispersibility of a polishing composition tends to reduce abrasive grain residue. It is believed that this is because the aggregation state of the precipitates generated in the polishing composition affects the abrasive grain residue.When the redispersibility of the polishing composition is good, the fluidity of the precipitates is maintained, so it is assumed that the abrasive grains maintain a certain distance from each other even during polishing.On the other hand, when the redispersibility of the polishing composition is poor, the fluidity of the precipitates is not maintained, so the abrasive grains are in a state of being closely spaced from each other during polishing, and it is assumed that such abrasive grain aggregates are likely to penetrate the substrate as irregular particles.It has also been found that the polishing composition of the present invention has an unexpected effect, that is, by improving the redispersibility, good results are obtained in terms of abrasive grain residue.
[0039] The zeta potential of the anti-caking agent is not particularly limited as long as the product of the zeta potential of the anti-caking agent and the abrasive grains (silica particles) is positive, but for example, the absolute value is 0.5 mV or more. The absolute value of the zeta potential of the anti-caking agent is preferably 1 mV or more, more preferably 2 mV or more, even more preferably 3 mV or more, particularly preferably 4 mV or more, and most preferably 4.5 mV or more. The absolute value of the zeta potential of the silica particles is preferably 50 mV or less, more preferably 40 mV or less, even more preferably 30 mV or less, particularly preferably 20 mV or less, and most preferably 15 mV or less. When the absolute value of the zeta potential of the anti-caking agent is within the above range, the redispersibility of the precipitates generated in the polishing composition is further improved, and the abrasive grain residue on the surface of the object to be polished after polishing can be further reduced.
[0040] Whether the product of the zeta potentials of the abrasive grains and the anti-caking agent contained in the polishing composition is positive can be determined, for example, as follows. The abrasive grains and the anti-caking agent contained in the polishing composition differ in particle size or specific gravity (density), etc. Therefore, the abrasive grains and the anti-caking agent contained in the polishing composition are separated into two solutions, each containing a larger amount of one particle, by centrifugation or the like, and the zeta potential of each solution is measured. If the zeta potentials of these two solutions have charges of the same sign, it can be determined that the product of the zeta potentials of the abrasive grains and the anti-caking agent contained in the polishing composition is positive. The conditions for separating the abrasive grains and the anti-caking agent contained in the polishing composition into two solutions, each containing a larger amount of one particle, can be adjusted appropriately depending on the types of abrasive grains and the anti-caking agent, but examples include a method of centrifuging at RCF 85 (×g) for 1 hour. Alternatively, the polishing composition can be dried, and inorganic and organic particles can be identified from the dried product using a microscope or the like, and further classified by particle size or specific gravity, to obtain particles that may be abrasives or anti-caking agents. Each particle that may be abrasives or anti-caking agents can be dispersed in water (for example, an aqueous dispersion with a pH of 7.0 to 11.0), and the zeta potential of the aqueous dispersion of each particle can be measured. If the zeta potentials of the abrasives and anti-caking agents have charges of the same sign, it can be determined that the product of the zeta potentials of the abrasives and anti-caking agents contained in the polishing composition is positive. Furthermore, when inorganic particles are contained in addition to the abrasives and anti-caking agents, the abrasives and anti-caking agents can be identified by particle size, specific gravity (density), particle shape, constituent elements, etc.
[0041] Here, the product of the zeta potential of the anti-caking agent and the zeta potential of the abrasive grains (silica particles) is not particularly limited as long as it is positive, but is, for example, preferably 3 or more, more preferably 5 or more, even more preferably 50 or more, particularly preferably 100 or more, and most preferably 150 or more. The product of the zeta potential of the anti-caking agent and the zeta potential of the abrasive grains (silica particles) is preferably 1000 or less. When the product of the zeta potential of the abrasive grains and the zeta potential of the anti-caking agent is within the above range, the redispersibility of sediments generated in the polishing composition is further improved, and the abrasive grain residue on the surface of the object to be polished after polishing can be further reduced.
[0042] The specific gravity of the anti-caking agent is preferably 1.2 or more, more preferably 1.5 or more, even more preferably 1.8 or more, particularly preferably 2.0 or more, and most preferably 2.2 or more. The specific gravity of the anti-caking agent is preferably 4.5 or less. When the specific gravity of the anti-caking agent is within the above range, the redispersibility of sediment generated in the polishing composition is further improved, and abrasive grain residue on the surface of the object to be polished after polishing can be further reduced. In this specification, specific gravity is measured in accordance with JIS-R-9301-2-1 (1999).
[0043] The concentration (content) of the anti-caking agent in the polishing composition of this embodiment is not particularly limited, and can be appropriately selected according to the desired redispersibility of the polishing composition after storage.Whether the polishing composition is used as a polishing liquid for polishing an object as it is (typically a slurry-like polishing liquid, sometimes referred to as working slurry or polishing slurry), or the polishing composition is used after dilution for polishing (i.e., concentrated liquid, undiluted working slurry), the mass of the anti-caking agent can be selected relative to the mass of abrasive grains.For example, the content of the anti-caking agent is usually preferably 20% by mass or less, more preferably 15% by mass or less, even more preferably 10% by mass or less, particularly preferably 5% by mass or less, and most preferably 3% by mass or less, relative to the total mass (100% by mass) of the abrasive grains. Furthermore, the content of the anti-caking agent is preferably 0.1% by mass or more, more preferably 0.3% by mass or more, even more preferably 0.5% by mass or more, particularly preferably 0.8% by mass or more, and most preferably 1% by mass or more, relative to the total mass (100% by mass) of the abrasive grains. That is, the content of the anti-caking agent is preferably 0.1% by mass or more and 20% by mass or less, more preferably 0.3% by mass or more and 15% by mass or less, even more preferably 0.5% by mass or more and 10% by mass or less, particularly preferably 0.8% by mass or more and 5% by mass or less, and most preferably 1% by mass or more and 3% by mass or less, relative to the total mass (100% by mass) of the abrasive grains. Within the above range, the polishing composition can be easily redispersed after storage. Note that when two or more anti-caking agents are used, the content of the anti-caking agents refers to the total amount of all the anti-caking agents.
[0044] [Dispersion Medium] The polishing composition according to this embodiment contains a dispersion medium, which disperses or dissolves each component.
[0045] The dispersion medium preferably contains water.Furthermore, from the viewpoint of preventing the influence of impurities on other components of the polishing composition, it is preferable to use water with as high purity as possible.Specifically, it is preferable to use pure water or ultrapure water, which has been removed impurity ions by ion exchange resin and then filtered to remove foreign matter, or distilled water.Furthermore, the dispersion medium may further contain an organic solvent or the like for the purpose of controlling the dispersibility of other components of the polishing composition.
[0046] [pH Adjuster] The polishing composition according to one embodiment of the present invention preferably further contains a pH adjuster. The pH adjuster can contribute to adjusting the pH of the polishing composition by selecting the type and amount added.
[0047] The pH adjuster is not particularly limited as long as it is a compound having a pH adjusting function, and known compounds can be used. The pH adjuster is not particularly limited as long as it is a compound having a pH adjusting function, and examples thereof include acids and alkalis.
[0048] The acid may be either an inorganic acid or an organic acid. Examples of inorganic acids include, but are not limited to, sulfuric acid, nitric acid, boric acid, carbonic acid, hypophosphorous acid, phosphorous acid, and phosphoric acid. Examples of organic acids include, but are not limited to, 1-hydroxyethylidene-1,1-diphosphonic acid (HEDP), formic acid, acetic acid, propionic acid, butyric acid, valeric acid, 2-methylbutyric acid, n-hexanoic acid, 3,3-dimethylbutyric acid, 2-ethylbutyric acid, 4-methylpentanoic acid, n-heptanoic acid, 2-methylhexanoic acid, n-octanoic acid, 2-ethylhexanoic acid, benzoic acid, glycolic acid, salicylic acid, glyceric acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, maleic acid, phthalic acid, malic acid, tartaric acid, citric acid, and lactic acid, as well as methanesulfonic acid, ethanesulfonic acid, and isethionic acid. Among these, organic acids are preferred, and 1-hydroxyethylidene-1,1-diphosphonic acid (HEDP), malic acid, citric acid, and maleic acid are more preferred. When inorganic acids are used, nitric acid, sulfuric acid, and phosphoric acid are preferred.
[0049] The alkali is not particularly limited, but examples thereof include alkali metal hydroxides such as potassium hydroxide, ammonia, quaternary ammonium salts such as tetramethylammonium and tetraethylammonium, amines such as ethylenediamine and piperazine, etc. Among these, potassium hydroxide and ammonia are preferred.
[0050] The pH adjusters may be used alone or in combination of two or more.
[0051] The content of the pH adjuster is not particularly limited, and is preferably an amount that allows the pH value to fall within the preferred range described below.
[0052] [Other Components] The polishing composition according to the present embodiment may further contain known components such as abrasive grains, chelating agents, thickeners, oxidizing agents, dispersants, surface protective agents, wetting agents, surfactants, anticorrosives (rust inhibitors), preservatives, and antifungal agents, in addition to the above, within the range that does not impair the effects of the present invention. The contents of the other components may be appropriately set depending on the purpose of their addition.
[0053] [pH] In the case of a polishing composition that is used as a polishing liquid for polishing a polishing object as is, the pH of the polishing composition according to this embodiment is preferably 7.0 or higher. Furthermore, the pH of the polishing composition according to this embodiment is preferably 11.0 or lower, more preferably 10.5 or lower, and particularly preferably 10.0 or lower. That is, the pH of the polishing composition according to this embodiment is preferably 7.0 or higher and 11.0 or lower, more preferably 7.0 or higher and 10.5 or lower, and particularly preferably 7.0 or higher and 10.0 or lower. Within the above range, the product of the zeta potentials of the silica particles as abrasives and the anti-caking agent is easily made positive, contributing to improved redispersibility of the polishing composition. Furthermore, a better balance can be achieved between improved polishing rate and reduced abrasive residue. In this specification, the pH of the polishing composition is determined by the measurement method described in the Examples below.
[0054] In the case of a polishing composition that is used as a polishing liquid for polishing a polishing object as is, according to one embodiment, the pH of the polishing composition is preferably 4.0 or less, more preferably less than 4.0, and even more preferably 3.5 or less. Also, according to one embodiment, the pH of the polishing composition is preferably 1.0 or more, more preferably greater than 1.0, even more preferably 1.5 or more, and particularly preferably greater than 1.5. That is, according to one embodiment, the pH of the polishing composition is preferably 1.0 or more and 4.0 or less, more preferably greater than 1.0 and less than 4.0, even more preferably greater than 1.5 and 3.5 or less, and particularly preferably greater than 1.5 and 3.5 or less. Within the above range, an improvement in the polishing rate and a reduction in abrasive grain residue can be achieved in a more balanced manner. In this specification, the pH of the polishing composition is determined by the measurement method described in the Examples below.
[0055] In the case of a polishing composition that is diluted before use (i.e., a concentrated solution), the pH of the polishing composition is suitably 7.0 or higher, preferably greater than 7.0, more preferably 7.5 or higher. The pH of the polishing composition is suitably 11.0 or lower, preferably less than 11.0, more preferably 10.5 or lower.
[0056] In the case of a polishing composition (i.e., a concentrated liquid) that is diluted before use in polishing, according to one embodiment, the pH of the polishing composition is suitably 1.0 or higher, preferably greater than 1.0, more preferably 1.5 or higher. The pH of the polishing composition is suitably 7.5 or lower, preferably less than 5.5, more preferably less than 4.5.
[0057] <Method for producing polishing composition> The method for producing (preparing) the polishing composition is not particularly limited, and for example, a production method including preparing abrasive grains and an anti-caking agent, stirring and mixing a dispersion medium (preferably water) and, if necessary, other components, can be appropriately adopted. That is, another embodiment of the present invention is a method for producing a polishing composition having an average particle diameter (D 50The present invention relates to a method for producing a polishing composition, comprising: selecting silica particles as abrasive grains having a diameter (average diameter) of more than 1.0 μm and a primary particle circularity of 0.90 or more; selecting inorganic particles different from the abrasive grains as an anti-caking agent; and mixing the abrasive grains and the anti-caking agent with a dispersion medium. Note that the abrasive grains, the anti-caking agent, the dispersion medium, and other components are the same as those described above in the section entitled "Polishing Composition," and therefore further description thereof will be omitted here.
[0058] In one embodiment of the present invention, the average particle size (D 50 Silica particles having an average particle diameter (D) of more than 1.0 μm and a primary particle circularity of 0.90 or more can be obtained by selecting silica particles that satisfy the above-mentioned specific conditions from commercially available silica particles. 50 Silica particles having an average particle diameter (D) of more than 1.0 μm and a primary particle circularity of 0.90 or more can be obtained by producing silica particles under conditions that satisfy the above-mentioned specific conditions. 50 Silica particles having a particle diameter greater than 1.0 μm and a primary particle circularity of 0.90 or more can be obtained by controlling silica particles that do not satisfy the above-mentioned specific conditions so that they satisfy the above-mentioned specific conditions. In this case, known methods can be used as the control method, either in the same manner or with appropriate modifications. For example, in the case of the deflagration method, methods such as controlling the particle diameter, supply rate, and mixing ratio with oxygen of the metallic silicon can be applied.
[0059] The silica particles selected as abrasive grains and the inorganic particles selected as an anti-caking agent as described above are stirred and mixed with a dispersion medium (preferably water) and, if necessary, other components (for example, a pH adjuster) to produce a polishing composition.At this time, the mixing order of each component is not particularly limited.For example, in the case of a polishing composition containing abrasive grains, an anti-caking agent, and a dispersion medium, the abrasive grains, the anti-caking agent, and other components are all added together, and then, if necessary, a pH adjuster is added to obtain a desired pH; the abrasive grains and the anti-caking agent are added to the dispersion medium ... in this order, and then, if necessary, a pH adjuster is added to obtain a desired pH; the anti-caking agent and abrasive grains are added to the dispersion medium in this order, and then, if necessary, a pH adjuster is added to obtain a desired pH; and then, if necessary, a pH adjuster is added to obtain a desired pH; the anti-caking agent and abrasive grains are added to the dispersion medium in this order, and then, if necessary, a pH adjuster is added to obtain a desired pH.In addition, the temperature when stirring and mixing each component is not particularly limited, but is preferably 10°C or higher and 40°C or lower, and may be heated to increase the dissolution rate. The mixing time is not particularly limited.
[0060] <Object to be Polished> The object to be polished with the polishing composition of this embodiment is not particularly limited. Preferably, the object to be polished contains a resin and a filler. That is, in a preferred embodiment of the present invention, the polishing composition is used to polish an object to be polished containing a resin and a filler. When the polishing composition of this embodiment is used as an abrasive to polish an object to be polished containing a resin and a filler, polishing proceeds by simultaneously stripping off the filler and the surrounding resin, thereby achieving a specifically high polishing rate compared to other polishing abrasives. Furthermore, when simultaneously polishing a resin portion containing a filler and a metal portion such as copper, penetration of the abrasive into the metal surface can be suppressed or prevented (damage to the metal can be suppressed or prevented), i.e., abrasive residue on the surface of the object to be polished after polishing can be reduced. Therefore, when polishing an object to be polished containing a resin and a filler, both a high polishing rate and low abrasive residue on the surface of the object to be polished after polishing can be achieved. On the other hand, when alumina particles (crushed alumina particles), which are commonly used in polishing, are used as abrasives, polishing proceeds by sequentially scraping off the filler and resin from the surface. Furthermore, when a resin part containing a filler and a metal part such as copper are polished simultaneously, the abrasive grains are likely to pierce the metal part, which means that the amount of abrasive grain residue on the polished surface is likely to increase.
[0061] Hereinafter, an embodiment in which the object to be polished contains a resin and a filler will be described in detail, but the present invention is not limited to the following embodiment.
[0062] Here, the resin is not particularly limited, but examples thereof include acrylic resins such as polymethyl (meth)acrylate, methyl methacrylate-methyl acrylate copolymer, and urethane (meth)acrylate resin; epoxy resin; olefin resin such as ultra-high molecular weight polyethylene (UHPE); phenolic resin; polyamide resin (PA); polyimide resin (PI); polyester resin such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), and unsaturated polyester resin; polycarbonate resin (PC); polyphenylene sulfide resin (PPS); polystyrene resin such as syndiotactic polystyrene (SPS); polynorbornene resin; polybenzoxazole (PBO); polyacetal (POM); modified polyphenylene ether (m-PPE); amorphous polyarylate (PAR); polysulfone (PSF); polyethersulfone (PES); polyetheretherketone (PEEK); polyetherimide (PEI); fluororesin; and liquid crystal polymer (LCP). In this specification, "(meth)acrylic acid" refers to acrylic acid or methacrylic acid, as well as both acrylic acid and methacrylic acid. Similarly, in this specification, "(meth)acrylate" refers to acrylate or methacrylate, as well as both acrylate and methacrylate. Of these, from the viewpoint of processability, it is preferable that the resin has a cyclic molecular structure. That is, in a preferred embodiment of the present invention, the resin has a cyclic molecular structure. As resins having such cyclic molecular structures, epoxy resins, polycarbonate resins, and polyphenylene sulfide resins are preferably used. The above resins can be used alone or in combination of two or more. The above resins may also be cured with a curing agent.
[0063] The material constituting the filler is not particularly limited, but examples thereof include glass, carbon, calcium carbonate, magnesium carbonate, barium sulfate, magnesium sulfate, aluminum silicate, titanium oxide, alumina, zinc oxide, silica (silicon dioxide), kaolin, talc, glass beads, sericite activated clay, bentonite, aluminum nitride, polyester, polyurethane, rubber, etc. Among these, from the viewpoint of processability, glass and silica are preferred, and silica is particularly preferred.
[0064] Examples of the shape of the filler include powder, sphere, fibrous, and needle-like. Of these, from the viewpoint of processability, sphere and fibrous are preferred, and sphere is more preferred. The size of the filler is not particularly limited. For example, when the filler is spherical, the average particle diameter is, for example, 0.01 μm or more and 50 μm or less, preferably 1.0 μm or more and 6.5 μm or less. Here, the average particle diameter of the filler is determined by randomly selecting 200 fillers from an image of the polishing object taken with a scanning electron microscope (SEM) (manufactured by Hitachi High-Tech Corporation, product name: SU8000), measuring the particle diameter of each, and averaging these values. Furthermore, when the filler is fibrous, the average major axis is, for example, 100 μm or more and 300 μm or less, preferably 150 μm or more and 250 μm or less, and the average minor axis is, for example, 1 μm or more and 30 μm or less, preferably 10 μm or more and 20 μm or less. Here, the average major axis and the average minor axis of the filler are determined by randomly selecting 200 fillers from an image of the object to be polished taken with a scanning electron microscope (SEM) (manufactured by Hitachi High-Tech Corporation, product name: SU8000), measuring the major axis and the minor axis of each filler, and averaging these values to obtain the average major axis (μm) and the average minor axis (μm), respectively.
[0065] The silica particles as abrasive grains and the filler may be in any combination, but it is preferable that the size (average particle diameter) of the silica particles as abrasive grains is larger than the size (average particle diameter) of the filler. That is, in a preferred embodiment of the present invention, when the object to be polished contains a resin and a filler, the average particle diameter (D 50 ) is larger than the average particle diameter of the filler. 50) is larger than the average particle diameter of the filler, the polishing rate is improved. 50 When the average particle size of the filler and the silica particles have such a relationship, it is easier to improve the polishing rate and reduce the amount of abrasive residue. In the above embodiment, the relationship between the size of the silica particles and the size of the filler is not particularly limited, but the ratio of the average particle size of the abrasive particles (D 50 ) is preferably more than 1 and not more than 15, more preferably 1.5 or more and less than 10.0, and even more preferably more than 1.6 and less than 7.0. In the above, the average particle size of the filler means the average particle size when the filler is spherical, and means the average minor axis when the filler is fibrous.
[0066] However, when the average particle size of the abrasive grains (silica particles) is large, the individual particles of the sediment in the polishing composition tend to lose fluidity, and simply shaking or stirring the polishing composition containing the sediment does not loosen the sediment, making it difficult to redisperse the sediment in the liquid. Therefore, when polishing a polishing object containing resin and filler, if the average particle size of the abrasive grains is increased according to the average particle size of the filler, the sediment formed in the polishing composition cannot be redispersed and cannot be used for polishing. Therefore, it is difficult to achieve both an improvement in the polishing rate and a reduction in abrasive grain residue. On the other hand, with the polishing composition of this embodiment, even if the solid content (abrasive grains) in the polishing composition settles, the sediment can maintain fluidity and exhibit better redispersibility. In other words, when polishing a polishing object containing resin and filler, even if the average particle size of the abrasive grains is increased, the sediment can be redispersed, which is advantageous for achieving both an improvement in the polishing rate and a reduction in abrasive grain residue. For this reason, it can be suitably used for polishing sealing materials and insulating materials for electronic devices such as semiconductors.
[0067] The above fillers can be used alone or in combination of two or more.
[0068] Furthermore, the object to be polished may contain, as a polishing surface, materials other than the resin and filler, such as copper (Cu), aluminum (Al), tantalum (Ta), tantalum nitride (TaN), titanium (Ti), titanium nitride (TiN), nickel (Ni), ruthenium (Ru), cobalt (Co), tungsten (W), and tungsten nitride (WN).
[0069] The object to be polished may be prepared from a resin and a filler, or may be prepared using a commercially available product. Examples of commercially available products include the interlayer insulating material "Ajinomoto Build-Up Film (registered trademark)" (ABF) GX13, GX92, GX-T31, and GZ41 (all from Ajinomoto Fine-Techno Co., Ltd.), the glass fiber-reinforced grade of polycarbonate (PC) resin "Panlite (registered trademark)" (all from Teijin Limited), GF-reinforced DURAFIDE (registered trademark) PPS, and GF / inorganic filler-reinforced DURAFIDE (registered trademark) PPS (all from Polyplastics Co., Ltd.).
[0070] <Polishing method> Another aspect of the present invention relates to a polishing method, which comprises a step of polishing an object to be polished using the above-mentioned polishing composition. Preferred examples of the object to be polished in this aspect are the same as those described in the above-mentioned <Object to be polished>. For example, it is preferable to polish an object to be polished that contains a resin and a filler on the polishing surface. That is, a preferred aspect of the polishing method in this aspect comprises a step of polishing an object to be polished that contains a resin and a filler using the above-mentioned polishing composition.
[0071] Polishing an object to be polished using a polishing composition can be carried out using equipment and conditions commonly used for polishing. Common polishing equipment includes single-sided polishing equipment and double-sided polishing equipment. In single-sided polishing equipment, the object to be polished is generally held using a holder called a carrier, and while a polishing composition is supplied from above, a platen with a polishing pad attached is pressed against one side of the object to be polished and the platen is rotated to polish one side of the object to be polished. In double-sided polishing equipment, the object to be polished is generally held using a holder called a carrier, and while a polishing composition is supplied from above, a platen with a polishing pad attached is pressed against the opposite side of the object to be polished, and the plates are rotated in relative directions to polish both sides of the object to be polished. During this process, polishing is achieved by the physical action of friction between the polishing pad and polishing composition and the object to be polished, and the chemical action of the polishing composition on the object to be polished. Porous materials such as nonwoven fabrics, polyurethane, and suede can be used as the polishing pad without any particular restrictions. It is preferable that the polishing pad be treated to allow the polishing liquid to accumulate.
[0072] Examples of polishing conditions include polishing load, platen rotation speed, carrier rotation speed, flow rate of the polishing composition, and polishing time. There are no particular limitations on these polishing conditions. For example, the polishing load is preferably 0.1 psi (0.69 kPa) or more and 10 psi (69 kPa) or less per unit area of the object to be polished, more preferably 0.5 psi (3.5 kPa) or more and 8.0 psi (55 kPa) or less, and even more preferably 1.0 psi (6.9 kPa) or more and 6.0 psi (41 kPa) or less. Generally, the higher the load, the higher the frictional force caused by the abrasive grains, improving the mechanical processing force and increasing the polishing rate. Within this range, a sufficient polishing rate can be achieved, and damage to the object to be polished due to the load and the occurrence of defects such as scratches on the surface can be suppressed. The platen rotation speed and carrier rotation speed are preferably 10 rpm (0.17 s -1 ) or more 500rpm (8.3s -1) or less. The supply amount of the polishing composition is only required to be a supply amount (flow rate) that covers the entire object to be polished, and may be adjusted depending on conditions such as the size of the object to be polished. The method of supplying the polishing composition to the polishing pad is not particularly limited, and for example, a method of continuously supplying the polishing composition using a pump or the like is used. In addition, the processing time is not particularly limited as long as it is a time that can obtain the desired processing result, but it is preferable to use a shorter time due to the high polishing rate.
[0073] Furthermore, yet another aspect of the present invention relates to a method for producing a polished object, which comprises a step of polishing an object by the above-mentioned polishing method. Preferred examples of the object to be polished according to this aspect are the same as those described in the description of the <Object to be polished>. A preferred example is a method for producing an electronic circuit board, which includes polishing an object to be polished containing resin and metal by the above-mentioned polishing method.
[0074] Although the embodiments of the present invention have been described in detail, it is clear that this is for illustrative and exemplary purposes only and not for limitation, and that the scope of the present invention should be interpreted by the appended claims.
[0075] The present invention encompasses the following aspects and configurations.
[0076] [1] A polishing composition comprising abrasive grains, an anti-caking agent, and a dispersion medium, wherein the abrasive grains have an average particle diameter (D 50 ) is greater than 1.0 μm and the circularity of the primary particles is 0.90 or more, the anti-caking agent is inorganic particles different from the abrasive grains, and the product of the zeta potential of the abrasive grains and the zeta potential of the anti-caking agent is positive.
[0077] [2] The anti-caking agent has an average particle diameter (D 50 ) is an inorganic particle of 500 nm or less, the polishing composition according to the above [1].
[0078] [3] The anti-caking agent has an average particle diameter (D 50 ) is alumina particles of 200 nm or less.
[0079] [4] The polishing composition according to any one of the above [1] to [3], which is used for polishing an object to be polished containing a resin and a filler.
[0080] [5] The average particle diameter (D 50 ) is larger than the average particle size of the filler.
[0081] [6] The average particle diameter of the silica particles relative to the average particle diameter of the filler (D 50 6. The polishing composition according to claim 5, wherein the ratio of (a) to (b) is greater than 1 and less than 15.
[0082] [7] A method for producing a polishing composition containing abrasive grains, a dispersion medium, and an anti-caking agent, wherein the abrasive grains have an average particle diameter (D 50 a method for producing a polishing composition, comprising: selecting silica particles having a diameter greater than 1.0 μm and a primary particle circularity of 0.90 or more; selecting inorganic particles different from the abrasive grains as the anti-caking agent; and mixing the silica particles and the anti-caking agent with the dispersion medium.
[0083] [8] A polishing method comprising polishing an object to be polished containing a resin and a filler with the polishing composition according to any one of [1] to [6] above.
[0084] [9] The method according to [8] above, wherein the resin has a cyclic molecular structure.
[0085] The present invention will be described in more detail using the following examples and comparative examples. However, the technical scope of the present invention is not limited to the following examples. Unless otherwise specified, "%" and "parts" mean "% by mass" and "parts by mass", respectively.
[0086] <Method of measuring physical properties> [Average particle diameter of silica particles (D 50 ) and particle diameter D 10The silica particles were measured using a particle size distribution analyzer (Microtrac particle size distribution analyzer MT3300EX II, manufactured by Microtrac Bell Co., Ltd.) to determine the volumetric particle size distribution. In the obtained particle size distribution, the particle size at which the cumulative frequency from the small particle size side is 50% was defined as the average particle size (D 50 In the obtained particle size distribution, the particle diameter at which the cumulative frequency from the small particle diameter side becomes 10% is defined as the particle diameter D of the silica particles. 10 It was decided.
[0087] [Average particle size of colloidal alumina particles and crystalline cellulose particles] The average particle size of colloidal alumina particles and crystalline cellulose particles was measured using a scanning electron microscope (SEM) (Hitachi High-Tech Corporation, product name: SU8000) or a scanning transmission electron microscope (STEM) (Hitachi High-Tech Corporation, product name: HD-2700), and the obtained SEM images were analyzed using image analysis software (Mitani Shoji Co., Ltd., "WinROOF 2018"). Specifically, 500 particles were randomly selected as samples from the particles present in the SEM image, the particle size of each particle was measured, the average was calculated, and the average value was used as the average particle size.
[0088] [Circularity of Silica Particles] For silica particles, silica particle powder was dispersed in methanol and dropped onto an observation substrate, and the methanol was evaporated to obtain a dried sample. The sample was photographed using a scanning electron microscope (SEM) (manufactured by Hitachi High-Tech Corporation, product name: SU8000), and the obtained SEM image was analyzed using image analysis software (manufactured by Mitani Shoji Co., Ltd., "WinROOF 2018"). In detail, 30 silica particles were randomly selected as samples from the silica particles present in the SEM image, and the circularity (= 4πS / L 2 The circularity of the alumina particles was also measured in the same manner as above.
[0089] [Zeta Potential] The zeta potential of the abrasive grains and the anti-caking agent at each pH was confirmed using a Zetasizer (Zetasizer nano ZSP, manufactured by Malvern Panalytical).
[0090] [pH] The pH value of the polishing composition was confirmed using a pH meter (manufactured by Horiba, Ltd., model number: LAQUA (registered trademark)).
[0091] [Specific Gravity] The specific gravities of the abrasive grains and the anti-caking agent were measured according to the method of JIS-R-9301-2-1 (1999).
[0092] [Examples 1 to 4 and Comparative Examples 1 to 8] Dry silica particles and dry alumina particles (abrasive grains) listed in Table 1 below were prepared; colloidal alumina particles, sodium polyacrylate (listed as "Na polyacrylate" in Table 1), and crystalline cellulose (anti-caking agent); and potassium hydroxide and sulfuric acid (pH adjuster). While stirring, the silica particles or alumina particles (abrasive grains) listed in Table 1 were sequentially mixed with distilled water (dispersion medium) to a concentration of 4% by mass, and the colloidal alumina particles, sodium polyacrylate, and crystalline cellulose (anti-caking agent) listed in Table 1 to a concentration of 0.1% by mass. The pH was then adjusted to the pH listed in Table 1 using a pH adjuster (potassium hydroxide or sulfuric acid) to prepare a polishing composition (mixing temperature: about 25°C, mixing time: about 30 minutes). In Comparative Examples 6 to 8, crystalline cellulose (anti-caking agent) was not added.
[0093] [Examples 5 to 7] Dry silica particles (abrasive grains), colloidal alumina particles (anti-caking agent), and potassium hydroxide (pH adjuster) listed in Table 2 below were prepared. While stirring, the silica particles (abrasive grains) listed in Table 2 were mixed in an amount of 4 mass % and the colloidal alumina particles (anti-caking agent) listed in Table 2 in an amount of 0.1 mass % into distilled water (dispersion medium), and then the pH was adjusted to the pH listed in Table 1 using a pH adjuster (potassium hydroxide) to prepare a polishing composition (mixing temperature: about 25°C, mixing time: about 30 minutes). In Examples 5 to 7, the same polishing composition was used, but the polishing target (filler diameter contained in the substrate) was changed.
[0094] The redispersibility of the polishing composition obtained above was investigated according to the method described in the "Redispersibility" section below. Furthermore, for a polishing solution prepared by diluting the polishing composition 20 times by volume, the polishing rate and the number of abrasive grain residues on the surface of the object to be polished after polishing were evaluated according to the methods described in the "Removal Rate" and "Abrasive Grain Residue on Surface" sections. The results are shown in Tables 1 and 2 below. <Evaluation> [Redispersibility] 50 g of the polishing composition obtained above was placed in a cylindrical bottle (inner diameter 4 cm) and allowed to stand for 30 minutes. The bottle was then shaken at an amplitude of 2.5 cm and 200 spm for 72 hours to perform solid-liquid separation. From this state, the bottle was gently turned over, and the redispersibility was evaluated. Evaluation Criteria: ○: Sediment breaks down when the bottle is turned over; ×: Sediment does not break down when the bottle is turned over (hard cake formation).
[0095] [Polishing Rate] (Polishing Compositions of Examples 1 to 4 and Comparative Examples 1 to 8) As the object to be polished, a mixture of epoxy resin and filler (spherical silica, average particle diameter = 3.0 μm) so that the filler content was 70 mass % was prepared (object to be polished 1; density of object to be polished 1: 1.9 g / cm 3 ). A copper substrate was also prepared (object to be polished 2). Subsequently, using each polishing composition, objects to be polished 1 and 2 (substrates) were simultaneously polished using the polishing apparatus and polishing conditions described below. After polishing was completed, the polishing rates of the objects to be polished were evaluated according to the following (polishing rate evaluation method).
[0096] (Polishing Compositions of Examples 5 to 7) As the objects to be polished, epoxy resin and filler (spherical silica) having an average particle size shown in Table 1 were mixed so that the filler content was 70 mass % to prepare objects to be polished 3A to 3C. The density of objects to be polished 3A to 3C was 1.9 g / cm 3 The average particle diameters of the fillers contained in objects to be polished 3A to 3C were as follows: object to be polished 3A: average particle diameter of filler = 1.0 μm; object to be polished 3B: average particle diameter of filler = 2.0 μm; object to be polished 3C: average particle diameter of filler = 3.0 μm. A copper substrate was also prepared (object to be polished 2). Subsequently, using each polishing composition, one of objects to be polished 3A to 3C and 2 (substrate) were simultaneously polished using the polishing apparatus and polishing conditions described below. After polishing was completed, the polishing rate of the object to be polished was evaluated according to the following (polishing rate evaluation method).
[0097] (Polishing Apparatus and Polishing Conditions) Polishing apparatus: small tabletop polisher (EJ380IN manufactured by Engis Japan Co., Ltd.) Platen diameter: 380 mm Polishing pad: hard polyurethane pad (IC1010 manufactured by Nitta DuPont Co., Ltd.) Platen (platen) rotation speed: 45 rpm Head (carrier) rotation speed: 45 rpm Polishing pressure (polishing load): 4.5 psi (316 g / cm 2 Flow rate of polishing composition: 100 ml / min Polishing time: 1 min.
[0098] (Method for Evaluating Polishing Rate) 1. Using an analytical balance XS205 (manufactured by Mettler Toledo K.K.), the mass of the object to be polished before and after polishing was measured, and the mass change amount ΔM [kg] of the object to be polished before and after polishing was calculated from the difference between the mass and the mass; 2. The mass change amount ΔM [kg] of the object to be polished before and after polishing was divided by the density of the object to be polished (density of the material to be polished) to calculate the volume change amount ΔV [m 3 3. The volume change ΔV [m 3 ] is the area S [m 23. The thickness change Δd [m] of the object to be polished before and after polishing was calculated by dividing the thickness change Δd [m] of the object to be polished before and after polishing by the polishing time t [min], and the unit was further converted to [μm / min]. This value was taken as the polishing rate v [μm / min]. Note that, although a higher polishing rate is preferable, a rate of 4.0 μm / min or more is acceptable, and a rate of 5.0 μm / min or more is desirable.
[0099] [Abrasive grain residue on surface] The copper wire surface of the polishing object used for evaluating the polishing rate after polishing was photographed using a scanning electron microscope (SEM) (manufactured by Hitachi High-Tech Corporation, product name: SU8000), and the obtained SEM image was analyzed using image analysis software (manufactured by Mitani Shoji Co., Ltd., "WinROOF 2018"). Specifically, the number of abrasive grains (silica particles or alumina particles) present in an area of 110 μm × 110 μm in the SEM image was counted, and this number was divided into 1 mm 2 Number of abrasive grains per mm 2 ) and this was taken as the number of abrasive grains remaining on the surface of the object to be polished after polishing. In this evaluation, particles of 200 nm or more and 10 μm or less were counted as abrasive grains remaining on the surface of the object to be polished. Therefore, abrasive grains remaining are foreign matter of the above size present on the surface, and may also include residues other than abrasive grains.
[0100] Number of abrasive grains remaining on the surface of the object after polishing (pieces / mm 2 ) is preferably as low as possible, but 3 pieces / mm 2 If it is less than 600 x 10 3 pieces / mm 2 It is desirable that the value is less than 100×10 3 pieces / mm 2 It is particularly desirable that the number of abrasive grains remaining on the surface of the object to be polished after polishing is less than "<100" in Tables 1 and 2. 2 ) is the number of abrasive grains remaining on the surface (10 3 pieces / mm 2 ) shall be written.
[0101]
[0102]
[0103] As shown in Table 1, the use of the polishing composition according to this embodiment exhibits good redispersibility, enables polishing of the object to be polished at a high polishing rate, and reduces the number of abrasive grain residues on the surface of the object to be polished. On the other hand, when the polishing compositions of Comparative Example 1, in which the product of the zeta potential of the abrasive grains and the zeta potential of the anti-caking agent is negative, Comparative Examples 2 to 4, in which the anti-caking agent is a water-soluble polymer or organic particle, and Comparative Examples 6 to 8, which do not contain an anti-caking agent, were used, the results were inferior to those of the Examples in terms of redispersibility and the number of abrasive grain residues. Furthermore, when the polishing composition of Comparative Example 5, in which alumina particles were used as the abrasive grains, was used, the redispersibility was good, but the number of abrasive grain residues was significantly inferior.
[0104] In addition, in Examples 5 to 7, when the filler diameter contained in the object to be polished was changed using the same polishing composition, the polishing rate improved as the filler diameter became smaller. This is thought to be because it is correlated with the particle diameter of the abrasive grains, and polishing can be performed more efficiently when the filler diameter is smaller than the particle diameter of the abrasive grains. On the other hand, in Examples 5 to 7, all of the objects to be polished had good redispersibility, and it was shown that the number of abrasive grain residues on the object to be polished could be reduced.
[0105] These results show that the polishing composition of the present invention maintains fluidity, has good redispersibility, can polish the object to be polished at a high polishing rate, and can reduce the number of abrasive grain residues on the surface of the object to be polished, thereby achieving excellent effects.
[0106] This application is based on Japanese Patent Application No. 2023-055871, filed on March 30, 2023, the disclosure of which is incorporated herein by reference in its entirety.
Claims
1. A polishing composition comprising an abrasive grain, an anti-caking agent, and a dispersion medium, wherein the abrasive grain has an average particle diameter (D 50 ) is greater than 1.0 μm and has a circularity of 0.90 or more of primary particles; the anti-caking agent is an inorganic particle different from the abrasive grains; and the product of the zeta potential of the abrasive grains and the zeta potential of the anti-caking agent is positive.
2. The caking inhibitor has an average particle diameter (D 50 2. The polishing composition according to claim 1, wherein the abrasive particles are inorganic particles having a diameter of 500 nm or less.
3. The anti-caking agent has an average particle diameter (D 50 3. The polishing composition according to claim 1, wherein the alumina particles are 200 nm or less.
4. The polishing composition according to claim 1 or 2, which is used for polishing an object to be polished that contains a resin and a filler.
5. The average particle diameter of the silica particles (D 50 5. The polishing composition according to claim 4, wherein the average particle size of the filler is greater than the average particle size of the filler.
6. The average particle diameter of the silica particles relative to the average particle diameter of the filler (D 50 6. The polishing composition according to claim 5, wherein the ratio of 1 to 15 is greater than 1.
7. A method for producing a polishing composition comprising an abrasive grain, a dispersion medium, and a caking inhibitor, wherein the abrasive grain has an average particle diameter (D 50 ) is greater than 1.0 μm and has a primary particle circularity of 0.90 or more; selecting inorganic particles different from the abrasive grains as the caking inhibitor; and mixing the silica particles and the caking inhibitor with the dispersion medium.
8. A polishing method comprising polishing an object containing a resin and a filler with the polishing composition according to claim 1 or 2.
9. The method of claim 8, wherein the resin has a cyclic molecular structure.
Citation Information
Patent Citations
Abrasive and manufacturing method thereof
JP2012011525A
Polishing agent composition for aluminum nitride substrate and polishing method of aluminum nitride substrate
JP2018159033A
Silica slurry for polishing liquid composition
JP2019007000A
Polishing composition and polishing method using same
WO2022185793A1