Regenerated resin production method
The use of a vibrating transport bed to disentangle molding waste products addresses the entanglement issue, thereby improving recycling efficiency and producing high-quality recycled resin.
Patent Information
- Application Number
- PCT/JP2024/011548
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-09-20
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-03
AI Technical Summary
The recycling efficiency of molding waste products is hindered by entanglement issues due to their structure, which complicates the recycling process and reduces the effectiveness of waste composition handling.
A method involving the use of a vibrating transport bed to disentangle molding waste products by vibrating the waste product composition, which includes steps of supplying the waste composition to the bed and processing it to produce recycled resin, optimizing parameters such as frequency, feed rate, and supply amount to effectively eliminate entanglement.
This approach significantly enhances the recycling efficiency of molding waste products by reducing entanglement, allowing for smoother processing and improved production of high-quality recycled resin.
Smart Images

Figure JP2024011548_03102024_PF_FP_ABST
Abstract
Description
Recycled resin manufacturing method
[0001] The present invention relates to a method for producing recycled resin.
[0002] In recent years, concerns have grown over the deterioration of the natural environment and the increase in waste emissions, and efforts to recycle plastic products have become increasingly popular in an effort to realize a recycling-oriented society.
[0003] Injection molding is a typical method for manufacturing plastic products. Specifically, a plastic product (molded body) can be produced by injecting heated and molten resin into a mold and cooling it to form a desired shape. Depending on the injection molding method, molding waste may also be generated along with the plastic product, resulting from the passage of the molten resin through the mold. Such molding waste can be very large in volume when plastic products are manufactured industrially, and recycling of molding waste has been considered.
[0004] For example, Patent Document 1 describes an invention relating to a manufacturing method for recycled thermoplastic resin molded products, in which sprue runners (molding waste) and / or defective molded products generated during the molding process of thermoplastic resin molded products are crushed and mixed with a new thermoplastic resin, and then a thermoplastic resin molded product is injection-molded again using the resulting mixture. This invention is characterized by the fact that molding is performed using a gas-assisted molding method under the same molding conditions as those used for molding with a new thermoplastic resin, even under conditions in which the melt flow characteristics of the mixture change. Patent Document 1 also describes the ability to obtain recycled resin molded products with stable dimensions and high commercial value, free of defects such as sink marks, distortion, and warpage.
[0005] Japanese Patent Application Laid-Open No. 2006-256339
[0006] When recycling molding waste, the generated molding waste is collected and the resulting waste composition is subjected to a recycling process. However, the molding waste originates from the passage of molten resin in a mold, and due to its structure, molding waste is likely to be entangled with each other in the waste composition. As a result, if the waste composition is recycled as it is, the recycling efficiency may be low.
[0007] Therefore, the present invention provides a method for producing recycled resin that is excellent in recycling efficiency of molding waste products.
[0008] The present invention is, for example, as follows.
[0009] [1] A method for producing recycled resin, comprising: a step (1) of supplying a waste composition containing molded waste products having runners to a vibrating conveying bed and vibratingly conveying the waste composition; and a step (2) of obtaining recycled resin from the vibratingly conveyed waste composition. [2] The method according to [1] above, wherein the vibration frequency of the vibrating conveying bed is 1 to 1,000 Hz. [3] The method according to [1] or [2] above, wherein the feed rate of the waste composition to the vibrating conveying bed is 5 to 100 g / sec. [4] The method according to any one of [1] to [3] above, wherein the feed rate of the waste composition is 100 to 5,000 g / m relative to the width of the vibrating conveying bed. [5] The method according to any one of [1] to [4] above, wherein the specific gravity of the molded waste products is 0.9 to 1.5. [6] The resin constituting the molded waste products is represented by the following general formulas (1) to (5): [In the formula, X a , X b , X c , X d , X e , and X f each independently represents an alkylene group having 1 to 4 carbon atoms; a , R b , R c , R cc , R d , R dd , R e , R ee , R f、 and R ff each independently represents a halogen atom, an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, a cycloalkyl group having 5 to 20 carbon atoms, a cycloalkoxy group having 5 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, a heteroaryl group having 3 to 20 carbon atoms containing one or more hetero ring atoms selected from O, N, and S, an aryloxy group having 6 to 20 carbon atoms, and —C≡C—R i is selected from R irepresents an aryl group having 6 to 20 carbon atoms or a heteroaryl group having 3 to 20 carbon atoms and containing one or more hetero ring atoms selected from O, N, and S; a, b, c, d, e, and f each independently represent an integer of 0 to 10; h, i, j, j', k, k', m, m', n, and n' each independently represent an integer of 0 to 4; R g and R h [7] The manufacturing method according to any one of the above [1] to [5], wherein the resin constituting the molding waste contains at least one structural unit selected from the group consisting of the following general formulas (6) to (8): [In the formula, X g each independently represents an alkylene group having 1 to 10 carbon atoms; j , R k , and R l each independently represents a halogen atom, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkoxy group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 5 to 20 carbon atoms, a substituted or unsubstituted cycloalkoxy group having 5 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, a substituted or unsubstituted heteroaryl group having 3 to 20 carbon atoms containing one or more hetero ring atoms selected from O, N, and S, a substituted or unsubstituted aryloxy group having 6 to 20 carbon atoms, and —C≡C—R i is selected from R i represents a substituted or unsubstituted aryl group having 6 to 20 carbon atoms or a heteroaryl group having 3 to 20 carbon atoms and containing one or more hetero ring atoms selected from O, N, and S; each p independently represents an integer of 0 or 1; each q, r, and s independently represents an integer of 0 to 10; and t represents an integer of 1 to 3, where q is 2 or more and two R j When two R j may be joined together to form a ring structure, r is 2 or more, and two R k When two R k may be joined together to form a ring structure, s is 2 or more, and two Rl When two R l may be joined together to form a ring structure, R m represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms.]. [8] The manufacturing method according to any one of the above [1] to [6], wherein the resin constituting the molding waste contains an impurity resin having at least one structural unit selected from the group consisting of the following general formulas (9) to (11): [In the formula, X h each independently represents an alkylene group having 1 to 8 carbon atoms; m , R n , R o , R p , R q , and R r are each independently selected from a halogen atom, a cyano group, and a substituted or unsubstituted alkyl group having 1 to 6 carbon atoms, and u, v, w, x, y, and z each independently represent an integer of 0 to 2.
[0010] According to the present invention, recycled resin can be produced from molding waste with excellent recycling efficiency.
[0011] 1A and 1B are diagrams showing an embodiment of a mold, a diagram showing an embodiment after injection molding, and a diagram showing a united product of a plastic product and molding waste obtained after injection molding.
[0012] According to the present invention, there is provided a method for producing recycled resin, which includes a step (1) of supplying a waste composition containing molded waste products having runner portions to a vibrating conveying bed and vibratingly conveying the waste composition, and a step (2) of obtaining recycled resin from the vibratingly conveyed waste composition.
[0013] The present invention will be described below with reference to the drawings. Note that the drawings may be exaggerated for the purpose of explanation and may differ from the actual dimensions.
[0014] 1 is a diagram showing a schematic diagram of one embodiment of a mold. The mold 1 has a sprue 2, a runner 3, a gate 4, a cavity core 5, and cold slug wells 6 and 6'.
[0015] Molten resin is injected and poured into the mold 1 through the sprue 2. The inner diameter of the sprue 2 is circular and increases toward the inside of the mold 1. Therefore, the sprue 2 has a roughly truncated cone shape. The length of the sprue 2 usually depends on the distance to the runner 3, i.e., the thickness of the mold.
[0016] The molten resin injected from the sprue 2 passes through the runner 3, which branches into two. The length and inner diameter of the runner 3 are set taking into consideration the shape of the molded product, the properties of the molten resin, and the like. The runner 3 usually has a substantially cylindrical shape. Although the runner 3 in FIG. 1 branches into two, it may have only one runner without branching, or it may branch into three or more runners. When the molded product is small, from the viewpoint of manufacturing efficiency, the runner 3 preferably branches into three or more runners, more preferably 3 to 30 runners, even more preferably 3 to 25 runners, particularly preferably 3 to 20 runners, extremely preferably 3 to 10 runners, and most preferably 4 to 8 runners.
[0017] The molten resin that has passed through the runner 3 passes through the gate 4. The gate 4 has the function of controlling the injection speed of the molten resin into the cavity core 5. The inner diameter of the gate 4 is usually set smaller than the inner diameter of the runner 3, which allows the injection speed of the molten resin to be increased. In FIG. 1, the gate 4 is formed perpendicular to the runner 3, but it may also be formed parallel to the runner 3.
[0018] The molten resin that passes through the gate 4 is injected into the cavity core 5. Here, the cavity core 5 consists of a cavity, which is a recessed portion, and a core, which is a protruding portion. The molten resin is injected into the cavity (recessed portion) of the cavity core 5, and the cavity (recessed portion) and the core (protruding portion) join together to create a hollow portion that can be molded into the shape of the desired plastic product (molded body). Note that the cavity core 5 can have a so-called "nested structure" in which a pocket is machined in the mold 1 and a separately manufactured cavity and core are attached to the machined pocket.
[0019] Mold 1 has cold slug well 6 formed at the end of sprue 2 and cold slug well 6' formed at the end of the runner. Cold slug wells 6 and 6' function to prevent molding defects in plastic products by sealing in impurities, decomposition gases, etc. that may be contained in the tip of the molten resin.
[0020] After the molten resin is injected, the mold is cooled, solidifying the molten resin present in the sprue 2, runner 3, gate 4, cavity core 5, and cold slug wells 6 and 6' (cold runner method). Figure 2 is a schematic diagram showing one embodiment after injection molding. In Figure 2, the plastic product 11 has been separated from the molding waste and removed. Alternatively, the plastic product 11 and the molding waste may be removed together, and then the plastic product 11 may be separated.
[0021] The molding waste shown in FIG. 2 includes a sprue portion 7 derived from the sprue, a runner portion 8 derived from the runner, a gate portion 9 derived from the gate, and cold slug well portions 10 and 10′ derived from the cold slug well. The molding waste, for example, tends to become entangled with each other due to the presence of the runner portion 8. Therefore, for example, when attempting to feed a waste composition containing molding waste into a crusher, the entangled molding waste may hinder feeding into the crusher. Thus, if an attempt is made to use the waste composition as is, the recycling efficiency may be low.
[0022] In contrast, according to the present invention, the entanglement of the molding waste can be eliminated or reduced by a vibration transport step before recycling the waste composition, and as a result, recycled resin can be produced from the molding waste with excellent recycling efficiency.
[0023] Each step will be described in detail below.
[0024] 1. Step (1) Step (1) is a step of supplying a waste composition containing molded waste products having a runner portion to a vibrating conveying bed and vibratingly conveying the waste composition.
[0025] <Waste composition> The waste composition includes molding waste having a runner portion. The waste composition may further include molded products recovered after being used in the market as part of a product, defective products generated in the molding process, defective products generated in the commercialization process, unused molded products that are no longer needed, etc.
[0026] The waste composition may be made by collecting molding waste from the same lot, or by collecting molding waste from different lots and combining these.
[0027] (Molding Scrap) The molding scrap comprises a runner portion. The molding scrap may further comprise at least one selected from the group consisting of a sprue portion, a gate portion, and a cold slug well portion. At least one of the runner portion, sprue portion, gate portion, and cold slug well portion may fall off from the molding scrap due to breakage caused by mechanical impact during collection, transportation, and mixing of the molding scrap. In one embodiment, the molding scrap comprises a sprue portion and a runner portion. In one embodiment, the molding scrap comprises a sprue portion, a runner portion, and a gate portion. In one embodiment, the molding scrap comprises a sprue portion, a runner portion, and a cold slug well portion. In one embodiment, the molding scrap comprises a sprue portion, a runner portion, a gate portion, and a cold slug well portion. The molding scrap composition may contain molding scrap of different shapes. In this specification, the term "comprises" is intended to include other configurations, and is synonymous with "includes," for example.
[0028] In this specification, the term "runner portion" refers to a portion having a shape derived from a runner (a flow path for molten resin) in a mold. When molding waste has a runner portion, the molding waste becomes more likely to become entangled with each other. The shape of the runner portion is preferably cylindrical. Furthermore, the runner portion may have a shape that branches in two or more directions, preferably two or three directions, along the way. The runner portion is preferably formed perpendicular to the length of the sprue portion. This can prevent molding defects. However, forming a runner portion perpendicular to the length of the sprue portion can be a factor that makes molding waste more likely to become entangled with each other. Furthermore, as described above, the mold may have a structure in which the molten resin injected from the sprue flows in two or more directions due to the branched runners. Therefore, molding waste may have two or more runner portions. In one embodiment, the molding waste preferably has three or more runners, more preferably 3 to 30 runners, even more preferably 3 to 25 runners, particularly preferably 3 to 20 runners, extremely preferably 3 to 10 runners, and most preferably 4 to 8 runners. The inner diameter of the runners varies depending on the physical properties of the molten resin used, the shape of the desired plastic product (molded article), and the like, but is preferably 0.1 to 5 mm, more preferably 0.1 to 4 mm, and even more preferably 1 to 4 mm. The length of the runners (equivalent to the height of the cylinder if it is cylindrical) is preferably 0.1 to 200 mm, more preferably 1 to 100 mm, and even more preferably 1 to 50 mm.
[0029] As used herein, the term "sprue portion" refers to a portion having a shape derived from the sprue (flow path for molten resin) within a mold. The shape of the sprue portion is not particularly limited, but is preferably a truncated cone. The inner diameter of the sprue portion varies depending on the physical properties of the molten resin used, the shape of the desired plastic product (molded article), and the like, but is preferably 0.1 to 10 mm, more preferably 1 to 8 mm, and even more preferably 1 to 6 mm. In this specification, the term "inner diameter" refers to the maximum distance between two points on the outline of a cross section perpendicular to the longitudinal direction of an object. For example, if the sprue portion has a truncated cone shape, the maximum inner diameter corresponds to the "inner diameter." The length of the sprue portion (which corresponds to the height of the truncated cone in the case of a truncated cone shape) is preferably 0.1 to 200 mm, more preferably 1 to 100 mm, and even more preferably 1 to 50 mm.
[0030] In this specification, the term "gate portion" refers to a portion having a shape derived from a gate (a flow path for molten resin) in a mold. The shape of the gate portion is not particularly limited and can be set appropriately depending on the physical properties of the molten resin used, the shape of the desired plastic product (molded article), and the like. The inner diameter of the gate portion varies depending on the physical properties of the molten resin used, the shape of the desired plastic product (molded article), and the like, but is preferably 0.1 to 5 mm, more preferably 0.1 to 3 mm, and even more preferably 0.1 to 2 mm. The inner diameter of the gate portion is preferably smaller than the inner diameter of the runner portion. The length of the gate portion is also not particularly limited and can be set appropriately depending on the physical properties of the molten resin used, the shape of the desired plastic product (molded article), and the like.
[0031] As used herein, the term "cold slug well" refers to a portion having a shape derived from the cold slug well (a portion containing molten resin containing impurities, decomposition gases, etc.) within a mold. The shape of the cold slug well is not particularly limited, but is preferably a test tube, a truncated cone, or a cylindrical shape. The inner diameter of the cold slug well varies depending on the physical properties of the molten resin used and the shape of the desired plastic product (molded article), but is preferably 0.1 to 10 mm, more preferably 1 to 8 mm, when the gate is formed at the end of the sprue. Furthermore, the inner diameter of the cold slug well is preferably 0.1 to 5 mm, more preferably 1 to 4 mm, when the gate is formed at the end of the runner. The length of the cold slug well is not particularly limited, but is preferably 0.1 to 20 mm, more preferably 0.1 to 10 mm.
[0032] The specific gravity of the molding waste is preferably 0.9 to 1.5, more preferably 0.9 to 1.4, more preferably 1.0 to 1.4, even more preferably 1.0 to 1.3, and particularly preferably 1.0 to 1.1 or 1.1 to 1.3. Having the specific gravity of the molding waste within the above range is preferable because it facilitates elimination or reduction of entanglement between molding waste by vibration transport. In one embodiment, when the resin constituting the molding waste contains a resin having at least one structural unit selected from the group consisting of general formulas (1) to (5) described below, the specific gravity of the molding waste is preferably 1.0 to 1.5, more preferably 1.0 to 1.4, and even more preferably 1.1 to 1.3. In addition, in one embodiment, when the resin constituting the molding waste contains an impurity resin having at least one structural unit selected from the group consisting of general formulas (6) to (8) described below, the specific gravity of the molding waste is preferably 0.9 to 1.1, more preferably 1.0 to 1.1. Furthermore, in one embodiment, when the resin constituting the molding waste contains a resin having at least one structural unit selected from the group consisting of general formulas (9) to (11) described later, the specific gravity of the molding waste is preferably 1.0 to 1.5, more preferably 1.0 to 1.4, and even more preferably 1.1 to 1.3.
[0033] Molding waste includes resins, additives, decomposition products thereof, etc. In this specification, "resin" means a material having a weight average molecular weight of 1,000 or more.
[0034] The resin constituting the molding waste is not particularly limited, but is usually a thermoplastic resin. The type and combination of resins can be determined depending on the physical properties of the desired plastic product (molded body).
[0035] In one embodiment, the resin constituting the molding waste preferably contains a resin having at least one structural unit selected from the group consisting of the following general formulas (1) to (5), and more preferably contains a resin having at least one structural unit selected from the group consisting of general formulas (1) to (4).
[0036] In the above formula, X a , X b , X c , X d , X e , and X f each independently represents an alkylene group having 1 to 4 carbon atoms. Examples of the alkylene group having 1 to 4 carbon atoms include methylene, ethylene, propylene, isopropylene, butylene, isobutylene, sec-butylene, and tert-butylene. Of these, methylene and ethylene are preferred, and ethylene is more preferred.
[0037] R a , R b , R c , R cc , R d , R dd , R e , R ee , R f、 and R ff each independently represents a halogen atom, an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, a cycloalkyl group having 5 to 20 carbon atoms, a cycloalkoxy group having 5 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, a heteroaryl group having 3 to 20 carbon atoms containing one or more hetero ring atoms selected from O, N, and S, an aryloxy group having 6 to 20 carbon atoms, and —C≡C—R i is selected from.
[0038] Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom.
[0039] Examples of the alkyl group having 1 to 20 carbon atoms include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, an undecyl group, a dodecyl group, and an icosyl group.
[0040] Examples of the alkoxy group having 1 to 20 carbon atoms include a methoxy group, an ethoxy group, a propyloxy group, an isopropyloxy group, a butoxy group, an isobutoxy group, a sec-butoxy group, a tert-butoxy group, a pentyloxy group, a hexyloxy group, a heptyloxy group, an octyloxy group, a nonyloxy group, a decyloxy group, an undecyloxy group, a dodecyloxy group, and an icosyloxy group.
[0041] Examples of the cycloalkyl group having 5 to 20 carbon atoms include a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, a cyclooctyl group, a cyclododecyl group, a cyclotridecyl group, a cyclotetradecyl group, a cyclopentadecyl group, a cyclooctadecyl group, a bicyclo[2.2.1]heptyl group, and a bicyclo[2.2.2]octyl group.
[0042] Examples of the cycloalkoxy group having 5 to 20 carbon atoms include a cyclopentyloxy group, a cyclohexyloxy group, a cycloheptyloxy group, a cyclooctyloxy group, a cyclododecyloxy group, a cyclotridecyloxy group, a cyclotetradecyloxy group, a cyclopentadecyloxy group, a cyclooctadecyloxy group, a bicyclo[2.2.1]heptyloxy group, and a bicyclo[2.2.2]octyloxy group.
[0043] Examples of the aryl group having 6 to 20 carbon atoms include a phenyl group, a tolyl group, a xylyl group, a trimethylphenyl group, a tetramethylphenyl group, an ethylphenyl group, an ethylmethylphenyl group, a diethylphenyl group, a propylphenyl group, an isopropylphenyl group, an isopropylmethylphenyl group, a benzyl group, a phenethyl group, a phenylpropyl group, a naphthyl group, an anthracenyl group, a phenanthrenyl group, a naphthacenyl group, a chryserinyl group, a pyrenyl group, a biphenyl group, a terphenyl group, and a quaterphenyl group.
[0044] Examples of the heteroaryl group having 3 to 20 carbon atoms and containing one or more heterocyclic atoms selected from O, N, and S include a furanyl group, a benzofuranyl group, an isobenzofuranyl group, a pyrrolyl group, an imidazolyl group, a pyrazolyl group, a triazolyl group, a pyridyl group, a pyrazyl group, a pyrimidyl group, a pyridazyl group, a pyrrolidyl group, an indolyl group, an isoindolyl group, an indazolyl group, a quinolyl group, an isoquinolyl group, a naphthyridyl group, a quinoxalyl group, a quinazolyl group, a propanol ... Examples thereof include a teridyl group, a phenanthridyl group, an acridinyl group, a pyrimidinyl group, a phenanthrolinyl group, a phenazinyl group, a thiophenyl group, a thiopyranyl group, a benzothiophenyl group, a benzothiopyranyl group, an oxazolyl group, an isoxazolyl group, a thiazolyl group, an isothiazolyl group, a furazanyl group, an oxadiazolyl group, a dithiazolyl group, a benzoxazolyl group, a benzisoxazolyl group, a benzothiazolyl group, and a benzisothiazolyl group.
[0045] Examples of the aryloxy group having 6 to 20 carbon atoms include a phenyloxy group, a tolyloxy group, a xylyloxy group, a trimethylphenyloxy group, a tetramethylphenyloxy group, an ethylphenyloxy group, an ethylmethylphenyloxy group, a diethylphenyloxy group, a propylphenyloxy group, an isopropylphenyloxy group, an isopropylmethylphenyloxy group, a naphthyloxy group, an anthracenyloxy group, a phenanthrenyloxy group, a naphthacenyloxy group, a chryserinyloxy group, a pyrenyloxy group, a biphenyloxy group, a terphenyloxy group, and a quaterphenyloxy group.
[0046] Of these, R a , R b , R c , R cc , R d , R dd , R e , R ee , R f、 and R ff is preferably a phenyl group or a naphthyl group, more preferably a phenyl group, a 1-naphthyl group or a 2-naphthyl group.
[0047] R irepresents an aryl group having 6 to 20 carbon atoms or a heteroaryl group having 3 to 20 carbon atoms and containing one or more heterocyclic atoms selected from O, N, and S. Examples of the aryl group having 6 to 20 carbon atoms and the heteroaryl group having 3 to 20 carbon atoms and containing one or more heterocyclic atoms selected from O, N, and S include those mentioned above. Among these, R i is preferably a phenyl group or a naphthyl group, more preferably a phenyl group, a 1-naphthyl group or a 2-naphthyl group.
[0048] a, b, c, d, e, and f each independently represent an integer of 0 to 10. In one embodiment, a, b, c, d, e, and f each independently represent preferably an integer of 0 to 5, more preferably an integer of 0 to 3, and even more preferably an integer of 0 or 1. In another embodiment, a, b, c, d, e, and f each independently represent preferably an integer of 1 to 5, more preferably an integer of 1 to 3, and even more preferably an integer of 1 or 2.
[0049] h, i, j, j', k, k', m, m', n, and n'n each independently represent an integer of 0 to 4, preferably 0 to 3, more preferably 0 to 2, even more preferably 0 or 1, and particularly preferably 0.
[0050] R g Each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. Examples of the alkyl group having 1 to 3 carbon atoms include a methyl group, an ethyl group, a propyl group, and an isopropyl group. g are each preferably independently a hydrogen atom.
[0051] Specific examples of the structural unit represented by formula (1) include structural units derived from 2,2'-bis(1-hydroxymethoxy)-1,1'-binaphthalene, 2,2'-bis(2-hydroxyethoxy)-1,1'-binaphthalene (also referred to as "BNE"), 2,2'-bis(2-hydroxyethoxy)-6,6'-diphenyl-1,1'-binaphthalene (also referred to as "DP"), 2,2'-bis(3-hydroxypropyloxy)-1,1'-binaphthalene, 2,2'-bis(4-hydroxybutoxy)-1,1'-binaphthalene, and the like. In one embodiment, the constitutional unit represented by formula (1) includes at least one constitutional unit derived from 2,2'-bis(2-hydroxyethoxy)-1,1'-binaphthalene (BNE) or 2,2'-bis(2-hydroxyethoxy)-6,6'-diphenyl-1,1'-binaphthalene (DP).
[0052] Specific examples of the structural unit represented by formula (2) include 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene (also referred to as "BPEF"), 9,9-bis(4-hydroxyphenyl)fluorene, 9,9-bis[4-(2-hydroxyethoxy)-3-methylphenyl]fluorene, 9,9-bis[4-(2-hydroxyethoxy)-3-tert-butylphenyl]fluorene, 9,9-bis[4-(2-hydroxyethoxy)-3-isopropylphenyl]fluorene, 9,9-bis[4-(2-hydroxyethoxy)-3-cyclohexylphenyl]fluorene, and 9,9-bis[4-(2-hydroxyethoxy)-3-phenylphenyl]fluorene (also referred to as "BPPEF") and the like. In one embodiment, the constitutional unit represented by formula (2) includes at least one constitutional unit derived from a compound selected from 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene (BPEF) and 9,9-bis[4-(2-hydroxyethoxy)-3-phenylphenyl]fluorene (BPPEF).
[0053] Specific examples of the structural unit represented by formula (3) include structural units derived from 9,9-bis(hydroxy(poly)alkoxynaphthyl)fluorenes. For example, structural units derived from a compound selected from 9,9-bis[6-(1-hydroxymethoxy)naphthalen-2-yl]fluorene (also referred to as "BNEF"), 9,9-bis[6-(2-hydroxyethoxy)naphthalen-2-yl]fluorene, 9,9-bis[6-(3-hydroxypropoxy)naphthalen-2-yl]fluorene, and 9,9-bis[6-(4-hydroxybutoxy)naphthalen-2-yl]fluorene are included. In one embodiment, the structural unit represented by formula (3) includes a structural unit derived from 9,9-bis[6-(2-hydroxyethoxy)naphthalen-2-yl]fluorene (BNEF).
[0054] Specific examples of the structural unit represented by formula (4) include structural units derived from decahydro-1,4:5,8-dimethanonaphthalene diols (also referred to as "D-NDM"). For example, structural units derived from compounds selected from (decahydro-1,4:5,8-dimethanonaphthalene-2,6-diyl)dimethanol, (decahydro-1,4:5,8-dimethanonaphthalene-2,7-diyl)dimethanol, (2-methyldecahydro-1,4:5,8-dimethanonaphthalene-2,6-diyl)dimethanol, (2-methyldecahydro-1,4:5,8-dimethanonaphthalene-2,7-diyl)dimethanol, (2-ethyldecahydro-1,4:5,8-dimethanonaphthalene-2,6-diyl)dimethanol, and (2-ethyldecahydro-1,4:5,8-dimethanonaphthalene-2,7-diyl)dimethanol.
[0055] Specific examples of the structural unit represented by formula (5) include structural units derived from decahydro-1,4:5,8-dimethanonaphthalene-2-methoxycarbonyl-6(7)-methanols. For example, decahydro-1,4:5,8-dimethanonaphthalene-2-methoxycarbonyl-6-methanol, decahydro-1,4:5,8-dimethanonaphthalene-2-methoxycarbonyl-7-methanol, 2-methyl-decahydro-1,4:5,8-dimethanonaphthalene-2-methoxycarbonyl-6-methanol, 2-methyl-decahydro-1,4:5,8-dimethanonaphthalene-2-methoxycarbonyl-7-methanol, 2-ethyl-decahydro-1,4:5,8-dimethanonaphthalene-2-methoxycarbonyl-6-methanol, 2-ethyl-decahydro-1,4:5,8-dimethanonaphthalene-2-methoxycarbonyl-7-methanol.
[0056] The structural units of the general formulas (1) to (5) may be contained alone in the resin, or two or more types may be contained in combination. In addition to the structural units described above, the resin may further contain structural units of other polycarbonate resins, or may further contain structural units of other resins (polyester resins, polyester carbonate resins, polyolefin resins), etc.
[0057] For example, other structural units of polycarbonate resins include structural units derived from diols such as 2,2'-[1,4-phenylenebis(methyleneoxy[1,1'-binaphthalene]-2',2-diyloxy)]di(ethan-1-ol) (DBHBNABHP) represented by the following formula, spiroglycol (3,9-bis(1,1-dimethyl-2-hydroxyethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane, SPG), bisphenol TMC, and bisphenol A.
[0058] Further, examples of the structural units of polyester resins or polyester carbonate resins include structural units derived from dicarboxylic acids or ester derivatives thereof, such as terephthalic acid, naphthalenedicarboxylic acid, 9H-fluorene 9,9-dipropionic acid or its monoalkyl (methyl, ethyl, propyl, isopropyl, butyl) ester derivatives or dialkyl ester derivatives (for example, 9,9-di(2-methoxycarbonylethyl)fluorene, 9,9-di(2-carboxyethyl)fluorene), 2,2′-bis(carboxymethoxy)-1,1′-binaphthyl, 2,2′-bis(carboxyethoxy)-1,1′-binaphthyl, 2,2′-bis(carboxyphenoxy)-1,1′-binaphthyl, and compounds represented by the following formula:
[0059] Resins having at least one structural unit selected from the group consisting of general formulas (1) to (5) can be produced, for example, by reacting a compound (diol) that derives the structural units represented by general formulas (1) to (5) with a carbonate diester in the presence of a basic compound catalyst and / or a transesterification catalyst, or in the absence of a catalyst, by solution condensation. In this case, as described above, compounds that derive structural units of other polycarbonate resins, compounds that derive structural units of other resins (polyester resins, polyestercarbonate resins, polyolefin resins), etc., can be used in combination with the compound (diol) that derives the structural units represented by general formulas (1) to (5) and the carbonate diester.
[0060] When the resin constituting the molding waste contains a resin having at least one structural unit selected from the group consisting of general formulas (1) to (5), the specific gravity of the molding waste falls within a suitable range (for example, preferably 1.0 to 1.5, more preferably 1.0 to 1.4, and even more preferably 1.1 to 1.3), and the entanglement between the molding waste can be suitably eliminated or reduced by the vibration transport described below, and since the resin is expensive, it is economically advantageous.
[0061] The weight-average molecular weight (Mw) of the resin having at least one structural unit selected from the group consisting of the general formulas (1) to (5) is not particularly limited, but is preferably 10,000 to 70,000, and more preferably 15,000 to 50,000. A weight-average molecular weight (Mw) of 10,000 or more is preferable because it can maintain appropriate strength as a molded product, such as a resin for optical lenses. On the other hand, a weight-average molecular weight (Mw) of 70,000 or less is preferable because it can maintain appropriate fluidity during resin molding and improve moldability. In this specification, "weight-average molecular weight (Mw)" refers to the weight-average molecular weight in terms of polystyrene measured by gel permeation chromatography (GPC).
[0062] In one embodiment, the resin constituting the molding waste preferably contains an impurity resin having at least one structural unit selected from the group consisting of the following general formulas (6) to (8). The impurity resin having the structural unit is usually a cyclic polyolefin.
[0063]
[0064] In the above formula, X g each independently represents an alkylene group having 1 to 10 carbon atoms. Examples of the alkylene group having 1 to 10 carbon atoms include methylene, ethylene, propylene, isopropylene, butylene, isobutylene, sec-butylene, tert-butylene, and pentylene. Of these, methylene, ethylene, propylene, butylene, isobutylene, and sec-butylene are preferred, and methylene, ethylene, and propylene are more preferred.
[0065] R j , R k , and R leach independently represents a halogen atom, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkoxy group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 5 to 20 carbon atoms, a substituted or unsubstituted cycloalkoxy group having 5 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, a substituted or unsubstituted heteroaryl group having 3 to 20 carbon atoms containing one or more hetero ring atoms selected from O, N, and S, a substituted or unsubstituted aryloxy group having 6 to 20 carbon atoms, and —C≡C—R i The R j , R k , and R l As the above, X a , X b , X c , X d , X e , and X f The same can be mentioned.
[0066] However, R j , R k , and R l may have a substituent. The substituent is not particularly limited, but examples thereof include a halogen atom, an alkyl group having 1 to 10 carbon atoms, a cycloalkyl group having 5 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, a cycloalkyloxy group having 5 to 10 carbon atoms, an alkyloxycarbonyl group having 2 to 10 carbon atoms, a cycloalkyloxycarbonyl group having 5 to 10 carbon atoms, an aryloxycarbonyl group having 7 to 15 carbon atoms, an alkylcarbonyloxy group having 2 to 10 carbon atoms, a cycloalkylcarbonyloxy group having 5 to 10 carbon atoms, an arylcarbonyloxy group having 7 to 15 carbon atoms, a hydroxyalkylcarbonyl group having 2 to 10 carbon atoms, a glycidyloxycarbonyl group, a hydroxy group, a carboxy group, a cyano group, and an amide group having 1 to 10 carbon atoms.
[0067] Examples of the alkyl group having 1 to 10 carbon atoms include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, and a pentyl group.
[0068] Examples of the cycloalkyl group having 5 to 10 carbon atoms include a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, a bicyclo[2.2.1]heptyl group, and a bicyclo[2.2.2]octyl group.
[0069] Examples of the alkoxy group having 1 to 10 carbon atoms include a methoxy group, an ethoxy group, a propyloxy group, an isopropyloxy group, a butoxy group, an isobutoxy group, a sec-butoxy group, a tert-butoxy group, and a pentyloxy group.
[0070] Examples of the cycloalkyloxy group having 5 to 10 carbon atoms include a cyclopentyloxy group, a cyclohexyloxy group, a bicyclo[2.2.1]heptyloxy group, and a bicyclo[2.2.2]octyloxy group.
[0071] Examples of the alkyloxycarbonyl group having 2 to 10 carbon atoms include a methyloxycarbonyl group, an ethyloxycarbonyl group, a propyloxycarbonyl group, an isopropyloxycarbonyl group, a butyloxycarbonyl group, an isobutyloxycarbonyl group, a sec-butyloxycarbonyl group, and a tert-butyloxycarbonyl group.
[0072] Examples of the cycloalkyloxycarbonyl group having 5 to 10 carbon atoms include a cyclopentyloxycarbonyl group, a cyclohexyloxycarbonyl group, a bicyclo[2.2.1]heptyloxycarbonyl group, and a bicyclo[2.2.2]octyloxycarbonyl group.
[0073] Examples of the aryloxycarbonyl group having 7 to 15 carbon atoms include a phenyloxycarbonyl group, a tolyloxycarbonyl group, a xylyloxycarbonyl group, a trimethylphenyloxycarbonyl group, a tetramethylphenyloxycarbonyl group, an ethylphenyloxycarbonyl group, an ethylmethylphenyloxycarbonyl group, a diethylphenyloxycarbonyl group, and a naphthyloxycarbonyl group.
[0074] Examples of the alkylcarbonyloxy group having 2 to 10 carbon atoms include a methylcarbonyloxy group, an ethylcarbonyloxy group, a propylcarbonyloxy group, an isopropylcarbonyloxy group, and a butylcarbonyloxy group.
[0075] Examples of the cycloalkylcarbonyloxy group having 5 to 10 carbon atoms include a cyclopentylcarbonyloxy group, a cyclohexylcarbonyloxy group, a bicyclo[2.2.1]heptylcarbonyloxy group, and a bicyclo[2.2.2]octylcarbonyloxy group.
[0076] Examples of the arylcarbonyloxy group having 7 to 15 carbon atoms include a phenylcarbonyloxy group, a tolylcarbonyloxy group, a xylylcarbonyloxy group, a trimethylphenylcarbonyloxy group, a tetramethylphenylcarbonyloxy group, an ethylphenylcarbonyloxy group, an ethylmethylphenylcarbonyloxy group, a diethylphenylcarbonyloxy group, and a naphthylcarbonyloxy group.
[0077] Examples of the hydroxyalkylcarbonyl group having 2 to 10 carbon atoms include a hydroxymethylcarbonyl group, a hydroxyethylcarbonyl group, and a hydroxypropylcarbonyl group.
[0078] Examples of the amide group having 1 to 10 carbon atoms include a methylaminocarbonyl group, an ethylaminocarbonyl group, a dimethylaminocarbonyl group, and an acetylamino group.
[0079] The above-mentioned substituents may be present alone or in combination of two or more kinds.
[0080] R i represents an aryl group having 6 to 20 carbon atoms or a heteroaryl group having 3 to 20 carbon atoms and containing one or more hetero ring atoms selected from O, N, and S. i is the same as above.
[0081] Each p independently represents an integer of 0 or 1.
[0082] q, r, and s each independently represent an integer of 0 to 10, preferably 0 to 5, and more preferably 0 to 3.
[0083] t represents an integer of 1 to 3, preferably 1 or 2.
[0084] where q is 2 or more and two R j When two R j may be joined together to form a ring structure. For example, when q is 2 and two R j are both substituted or unsubstituted alkyl groups, the general formula (6) becomes the following formula (6-1), where q is 2 and two R j When is a substituted or unsubstituted alkyl and a substituted or unsubstituted cycloalkyl, general formula (6) can be the following formula (6-2), (6-3), or (6-4).
[0085]
[0086] In the above formula, X g and p is as defined above.
[0087] R n is the above-mentioned substituent, and specific examples thereof include a halogen atom, an alkyl group having 1 to 10 carbon atoms, a cycloalkyl group having 5 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, a cycloalkyloxy group having 5 to 10 carbon atoms, an alkyloxycarbonyl group having 2 to 10 carbon atoms, a cycloalkyloxycarbonyl group having 5 to 10 carbon atoms, an aryloxycarbonyl group having 7 to 15 carbon atoms, an alkylcarbonyloxy group having 2 to 10 carbon atoms, a cycloalkylcarbonyloxy group having 5 to 10 carbon atoms, an arylcarbonyloxy group having 7 to 15 carbon atoms, a hydroxyalkylcarbonyl group having 2 to 10 carbon atoms, a glycidyloxycarbonyl group, a hydroxy group, a carboxy group, a cyano group, and an amide group having 1 to 10 carbon atoms.
[0088] Although z is not particularly limited, it is preferably 0 to 6, more preferably 0 to 3, and even more preferably 0 or 1.
[0089] u represents an integer of 1 to 3, preferably 1 or 2.
[0090] In addition, r is 2 or more, and two R k When two R k may be joined together to form a ring structure. For example, when r is 2 and two R k are both substituted or unsubstituted alkyl groups, the general formula (7) becomes the following formula (7-1) or (7-2), where r is 2 and the two R k When is a substituted or unsubstituted alkyl and a substituted or unsubstituted cycloalkyl, general formula (7) can be the following formula (7-3).
[0091]
[0092] In the above formula, X g , p, R n , z, and u are as defined above.
[0093] Furthermore, s is 2 or more, and two R l When two R l may be joined together to form a ring structure. For example, when s is 2 and two R l are both substituted or unsubstituted alkyl groups, the general formula (8) becomes the following formula (8-1) or (8-2), where s is 2 and the two R l When is a substituted or unsubstituted alkyl and a substituted or unsubstituted cycloalkyl, general formula (8) can be the following formula (8-3) or (8-4).
[0094]
[0095] In the above formula, X g , p, R n , z, and u are as defined above.
[0096] R m represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. The alkyl group having 1 to 3 carbon atoms is not particularly limited, but examples thereof include a methyl group, an ethyl group, a propyl group, and an isopropyl group.
[0097] Specific examples of impurity resins include those containing at least one selected from the group consisting of structural units represented by the following formulas 1 to 8.
[0098]
[0099] The above-mentioned structural units may be contained alone or in combination of two or more in the impurity resin. In addition, the above-mentioned structural units may be combined with structural units of other cyclic polyolefins, or with structural units of other resins (polyolefin resins, polyester resins), etc.
[0100] An impurity resin having at least one structural unit selected from the group consisting of general formulas (6) to (8) can be produced, for example, by polymerizing a compound (cyclic olefin) that derives the structural units represented by general formulas (6) to (8). In this case, as described above, in addition to the compound that derives the structural units represented by general formulas (6) to (8), a compound that derives the structural units of other cyclic polyolefins, a compound that derives the structural units of other resins (polyolefin resins, polyester resins), etc. can be used in combination.
[0101] In a preferred embodiment, an impurity resin having at least one structural unit selected from the group consisting of the general formulas (6) to (8) is used in combination with a resin having at least one structural unit selected from the group consisting of the general formulas (1) to (5). A relatively expensive resin having at least one structural unit selected from the group consisting of the general formulas (1) to (5) is recycled to produce a recycled resin, and a relatively inexpensive resin having at least one structural unit selected from the group consisting of the general formulas (6) to (8) is used as an impurity resin. Separating the two has the effect of providing excellent economic efficiency. In another preferred embodiment, an impurity resin having at least one structural unit selected from the group consisting of the general formulas (6) to (8) is used in combination with a resin having at least one structural unit selected from the group consisting of the general formulas (9) to (11), which will be described later. The relatively expensive resin having at least one structural unit selected from the group consisting of general formulas (9) to (11) is recycled to produce a recycled resin, and the relatively inexpensive resin having at least one structural unit selected from the group consisting of general formulas (6) to (8) is separated as an impurity resin, thereby achieving effects such as excellent economy.
[0102] The weight average molecular weight (Mw) of the impurity resin is not particularly limited, but is preferably 1,000 to 3,000,000, more preferably 10,000 to 3,000,000, even more preferably 20,000 to 1,000,000, and particularly preferably 30,000 to 500,000. A weight average molecular weight (Mw) of the impurity resin of 1,000 or more is preferable because separation is easier. On the other hand, a weight average molecular weight (Mw) of the impurity resin of 3,000,000 or less is preferable because it is less likely to become a source of gel impurities when trace amounts of impurity resin contaminate the recycled resin.
[0103] In one embodiment, the resin constituting the molding waste preferably contains a resin having at least one structural unit selected from the group consisting of the following general formulas (9) to (11): General formula (9) is a 9,9-bis(carboxyalkyl)fluorene, general formula (10) is a 9,9-bis(carboxyalkyl)-diarylfluorene, and general formula (11) is a 9,9-bis(carboxyalkyl)-dinaphthylfluorene.
[0104] In the above formula, X h Each of X independently represents an alkylene group having 1 to 8 carbon atoms. Examples of the alkylene group having 1 to 8 carbon atoms include methylene, ethylene, propylene, isopropylene, butylene, isobutylene, sec-butylene, tert-butylene, and pentylene. h is preferably methylene, ethylene, propylene, butylene, isobutylene, or sec-butylene, more preferably methylene, ethylene, or propylene, even more preferably methylene or ethylene, and particularly preferably ethylene.
[0105] R m , R n , R o , R p , R q , and R r are each independently selected from a halogen atom, a cyano group, and a substituted or unsubstituted alkyl group having 1 to 6 carbon atoms.
[0106] Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom.
[0107] Examples of the alkyl group having 1 to 6 carbon atoms include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, and a hexyl group. In this case, the alkyl group having 1 to 6 carbon atoms may have a substituent. Examples of the substituent include, but are not particularly limited to, a halogen atom, a hydroxy group, a carboxy group, and a cyano group. These substituents may be present alone or in combination of two or more.
[0108] Each of u, v, w, x, y, and z independently represents an integer of 0 to 2, preferably 0 to 1.
[0109] Specific examples of the structural unit represented by formula (9) include structural units derived from 9,9-bis(carboxy C2-6 alkyl)fluorenes, preferably 9,9-bis(carboxy C2-4 alkyl)fluorenes, and more preferably 9,9-bis(carboxy C2-3 alkyl)fluorenes. In this case, the compound from which the structural unit is derived may be an alkyl ester, acid halide, or acid anhydride. Examples include structural units derived from 9,9-bis(2-carboxyethyl)fluorene, 9,9-bis(2-carboxypropyl)fluorene, and alkyl esters, acid halides, and acid anhydrides thereof, preferably 9,9-bis(2-carboxyethyl)fluorene, and structural units derived from compounds selected from the group consisting of alkyl esters, acid halides, and acid anhydrides thereof.
[0110] Specific examples of the structural unit represented by formula (10) include 9,9-bis(carboxyC2-6 alkyl)-diphenylfluorenes. In this case, the compound from which the structural unit is derived may be an alkyl ester, an acid halide, or an acid anhydride. Examples include structural units derived from compounds selected from 9,9-bis(2-carboxyethyl)-1,8-diphenylfluorene, 9,9-bis(2-carboxyethyl)-2,7-diphenylfluorene, 9,9-bis(2-carboxyethyl)-3,6-diphenylfluorene, 9,9-bis(2-carboxyethyl)-4,5-diphenylfluorene, and 9,9-bis(2-carboxypropyl)-2,7-diphenylfluorene, as well as alkyl esters, acid halides, and acid anhydrides thereof.
[0111] Specific examples of the structural unit represented by formula (11) include structural units derived from 9,9-bis(carboxyC2-6 alkyl)-dinaphthylfluorenes. In this case, the compound from which the structural unit is derived may be an alkyl ester, an acid halide, or an acid anhydride. Examples of such structural units include those derived from compounds selected from 9,9-bis(2-carboxyethyl)-1,8-di(2-naphthyl)fluorene, 9,9-bis(2-carboxyethyl)-2,7-di(2-naphthyl)fluorene, 9,9-bis(2-carboxyethyl)-3,6-di(2-naphthyl)fluorene, 9,9-bis(2-carboxyethyl)-4,5-di(2-naphthyl)fluorene, 9,9-bis(2-carboxypropyl)-2,7-di(2-naphthyl)fluorene, 9,9-bis(2-carboxyethyl)-2,7-di(1-naphthyl)fluorene, alkyl esters thereof, acid halides, and acid anhydrides thereof.
[0112] Resins having at least one structural unit selected from the group consisting of general formulas (9) to (11) typically contain a structural unit derived from a diol, in addition to the structural units of general formulas (9) to (11).
[0113] Examples of the diol include compounds that derive the structural units represented by the above general formulas (1) to (5), compounds that derive structural units of other polycarbonate resins, and alkylene glycols.
[0114] Examples of compounds that derive the structural unit represented by general formula (1) include 2,2'-bis(1-hydroxymethoxy)-1,1'-binaphthalene, 2,2'-bis(2-hydroxyethoxy)-1,1'-binaphthalene (BNE), 2,2'-bis(2-hydroxyethoxy)-6,6'-diphenyl-1,1'-binaphthalene (DP), 2,2'-bis(3-hydroxypropyloxy)-1,1'-binaphthalene, and 2,2'-bis(4-hydroxybutoxy)-1,1'-binaphthalene. Examples of compounds that derive the structural unit represented by general formula (2) include 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene (BPEF), 9,9-bis(4-hydroxyphenyl)fluorene, 9,9-bis[4-(2-hydroxyethoxy)-3-methylphenyl]fluorene, 9,9-bis[4-(2-hydroxyethoxy)-3-tert-butylphenyl]fluorene, 9,9-bis[4-(2-hydroxyethoxy)-3-isopropylphenyl]fluorene, 9,9-bis[4-(2-hydroxyethoxy)-3-cyclohexylphenyl]fluorene, and 9,9-bis[4-(2-hydroxyethoxy)-3-phenylphenyl]fluorene (BPPEF). Examples of compounds that derive the structural unit represented by general formula (3) include 9,9-bis[6-(1-hydroxymethoxy)naphthalen-2-yl]fluorene (BNEF), 9,9-bis[6-(2-hydroxyethoxy)naphthalen-2-yl]fluorene, 9,9-bis[6-(3-hydroxypropoxy)naphthalen-2-yl]fluorene, and 9,9-bis[6-(4-hydroxybutoxy)naphthalen-2-yl]fluorene.Examples of compounds that derive the structural unit represented by general formula (4) include (decahydro-1,4:5,8-dimethanonaphthalene-2,6-diyl)dimethanol, (decahydro-1,4:5,8-dimethanonaphthalene-2,7-diyl)dimethanol, (2-methyldecahydro-1,4:5,8-dimethanonaphthalene-2,6-diyl)dimethanol, (2-methyldecahydro-1,4:5,8-dimethanonaphthalene-2,7-diyl)dimethanol, (2-ethyldecahydro-1,4:5,8-dimethanonaphthalene-2,6-diyl)dimethanol, and (2-ethyldecahydro-1,4:5,8-dimethanonaphthalene-2,7-diyl)dimethanol. Examples of compounds that derive the structural unit represented by general formula (5) include decahydro-1,4:5,8-dimethanonaphthalene-2-methoxycarbonyl-6-methanol, decahydro-1,4:5,8-dimethanonaphthalene-2-methoxycarbonyl-7-methanol, 2-methyl-decahydro-1,4:5,8-dimethanonaphthalene-2-methoxycarbonyl-6-methanol, 2-methyl-decahydro-1,4:5,8-dimethanonaphthalene-2-methoxycarbonyl-7-methanol, 2-ethyl-decahydro-1,4:5,8-dimethanonaphthalene-2-methoxycarbonyl-6-methanol, and 2-ethyl-decahydro-1,4:5,8-dimethanonaphthalene-2-methoxycarbonyl-7-methanol.
[0115] Examples of compounds that derive structural units of other polycarbonate resins include 2,2'-[1,4-phenylenebis(methyleneoxy[1,1'-binaphthalene]-2',2-diyloxy)]di(ethan-1-ol) (DBHBNABHP), spiroglycol (3,9-bis(1,1-dimethyl-2-hydroxyethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane, SPG), bisphenol TMC, and bisphenol A.
[0116] Examples of the alkylene glycol include ethylene glycol, propylene glycol, butylene glycol, pentylene glycol, neopentyl glycol, and octylene glycol.
[0117] Furthermore, the resin having at least one structural unit selected from the group consisting of general formulas (9) to (11) may further contain, in addition to the above-mentioned structural unit, a structural unit of another resin (polyester resin, polyester carbonate resin, polyolefin resin) or the like.
[0118] Resins having at least one structural unit selected from the group consisting of general formulas (9) to (11) can be produced, for example, by reacting a compound (carboxylic acid, alkyl ester, acid halide, acid anhydride) that derives the structural unit represented by general formulas (9) to (11) with a diol. In this case, as described above, compounds that derive the structural units of other resins (polyester resins, polyester carbonate resins, polyolefin resins), etc., can be used in combination with the compounds (carboxylic acid, alkyl ester, acid halide, acid anhydride) and diol that derive the structural units represented by general formulas (9) to (11).
[0119] When the resin constituting the molding waste contains a resin having at least one structural unit selected from the group consisting of general formulas (9) to (11), the specific gravity of the molding waste falls within a suitable range (for example, preferably 1.0 to 1.5, more preferably 1.0 to 1.4, and even more preferably 1.1 to 1.3), and the entanglement between the molding waste can be suitably eliminated or reduced by the vibration transport described below. In addition, since the resin is expensive, there are other effects such as excellent economy.
[0120] The weight-average molecular weight (Mw) of the resin having at least one structural unit selected from the group consisting of the general formulas (9) to (11) is not particularly limited, but is preferably 10,000 to 70,000, and more preferably 15,000 to 50,000. A weight-average molecular weight (Mw) of 10,000 or more is preferable because it can maintain appropriate strength as a molded product, such as a resin for an optical lens. On the other hand, a weight-average molecular weight (Mw) of 70,000 or less is preferable because it can maintain appropriate fluidity during resin molding and improve moldability.
[0121] The content of the molding waste is preferably 30% by mass or more, more preferably 40% by mass or more, even more preferably 50% by mass or more, and particularly preferably 50 to 100% by mass, based on the total mass of the waste composition.
[0122] In one embodiment, the content of the resin having at least one structural unit selected from the group consisting of general formulas (1) to (5) is preferably 80% by mass or more, more preferably 80 to 99% by mass, based on the total mass of the waste resin composition. A content of the resin of 80% by mass or more is preferred because it increases recycling efficiency.
[0123] In one embodiment, the content of the impurity resin having at least one structural unit selected from the group consisting of general formulas (6) to (8) is preferably 50% by mass or less, more preferably 0.001 to 50% by mass, even more preferably 0.01 to 0% by mass, and particularly preferably 0.1 to 20% by mass, based on the total mass of the waste resin composition. A content of the impurity resin of 50% by mass or less is preferred because it increases recycling efficiency.
[0124] In one embodiment, the content of the resin having at least one structural unit selected from the group consisting of general formulas (9) to (11) is preferably 80% by mass or more, more preferably 80 to 99% by mass, based on the total mass of the waste resin composition. A content of the resin of 80% by mass or more is preferred because it increases recycling efficiency.
[0125] The additives constituting the molding waste are not particularly limited, and known additives can be used. Examples of decomposition products of resins constituting the molding waste include monomers, dimers, copolymers, and oligomers of resins or impurity resins having at least one structural unit selected from the group consisting of general formulas (1) to (11), aryl alcohols such as phenol, carbonate diesters such as diphenyl carbonate, modified monomers such as those represented by the following formulas (A-1) and (A-2), and modified resins having partial structures represented by the following formulas (B-1) and (B-2).
[0126] <Vibrating conveying bed> The vibrating conveying bed is not particularly limited as long as it can eliminate or reduce the entanglement between the formed waste products having runner portions contained in the waste composition by vibrating and conveying the waste composition. Specifically, the vibrating conveying bed may be a plate-like member, a conveyor, a turntable, or any other shape, but is preferably a plate-like member or a conveyor, and more preferably a conveyor. In this case, the size of the vibrating conveying bed can be appropriately set. In addition, the vibrating conveying bed may be installed parallel to a horizontal plane or at an incline.
[0127] When the vibrating conveying bed is a plate-like member or a conveyor, the width of the vibrating conveying bed is preferably 5 cm to 5 m, more preferably 10 cm to 3 m, and even more preferably 20 cm to 1 m. The length of the vibrating conveying bed is preferably 50 cm to 30 m, more preferably 1 to 10 m, and even more preferably 1 to 5 m.
[0128] The vibrating transport floor is usually provided with a vibration mechanism (for example, an induction motor, a resonator, a vibration motor, etc.).
[0129] In addition, the vibrating conveying bed may further be provided with a feeder for supplying the waste composition to the vibrating conveying bed, a vibration control mechanism (constant drive, intermittent drive, variable speed drive, etc.) for controlling the vibration mechanism, a discharge mechanism for removing the waste composition after the vibrating conveying bed, etc.
[0130] <Vibration Conveyance> By vibrating and transporting the waste composition on a vibrating transport bed, it is possible to eliminate or reduce entanglement between the molded waste products having runner portions contained in the waste composition.
[0131] The vibration frequency of the vibrating conveying bed is preferably 1 to 1000 Hz, more preferably 5 to 500 Hz, even more preferably 10 to 100 Hz, and even more preferably 30 to 80 Hz. When the vibration frequency of the vibrating conveying bed is within the above range, entanglement is easily eliminated, energy consumption is reduced, and operating efficiency is good, which is preferable.
[0132] The supply amount of the waste composition relative to the width of the vibrating conveying bed is preferably 100 to 5000 g / m, more preferably 100 to 2000 g / m, and from the viewpoint of effectively eliminating or reducing entanglement, is further preferably 100 to 1500 g / m, particularly preferably 100 to 1000 g / m, and from the viewpoint of high production efficiency, is most preferably 500 to 1000 g / m.
[0133] The feed rate of the waste composition to the vibrating conveying bed is preferably 5 to 100 g / sec, more preferably 5 to 60 g / sec, more preferably 5 to 40 g / sec from the viewpoint of effectively eliminating or reducing entanglement, and even more preferably 15 to 40 g / sec from the viewpoint of production efficiency.
[0134] In one embodiment, the supply amount of the waste composition relative to the width of the vibrating conveying bed is preferably 100 to 2000 g / m, and the supply rate of the waste composition to the vibrating conveying bed is preferably 5 to 40 g / sec, more preferably 100 to 1500 g / m, and the supply rate is preferably 5 to 40 g / sec, and even more preferably 500 to 1000 g / m, and the supply rate is preferably 15 to 40 g / sec.
[0135] 2. Step (2) Step (2) is a step of obtaining a recycled resin from the waste composition that has been vibrationally transported. Since the waste composition is obtained from step (1), the entanglement of the molding waste with runners contained in the waste composition is eliminated or reduced. Therefore, in step (2), a recycled resin can be produced from the waste composition with high recycling efficiency.
[0136] The process (2) is not particularly limited as long as it can produce a recycled resin from the waste composition that has been vibrationally transported, and any known method can be used. In a preferred embodiment, the process (2) includes a process (2-1) of pulverizing the waste composition, a process (2-2) of removing impurities contained in the waste composition, and a process (2-3) of producing a recycled resin.
[0137] <Step (2-1)> Step (2-1) is a step of pulverizing the waste composition.
[0138] The waste composition can be pulverized to provide a form suitable for recycling.
[0139] The pulverization method is not particularly limited, and any of compression, impact, shear, and friction methods may be used.
[0140] Examples of crushers that can be used include coarse crushers such as jaw crushers, gyratory crushers, impact crushers, uniaxial crushers, and biaxial crushers; medium crushers such as roll crushers, edge runners, disintegrators, SAG (Semi-Autogenous Grinding) mills, crushing rolls, hammer mills, and roller mills; and fine crushers such as bead mills, ball mills, vibration ball mills, rod mills, jet mills, and planetary mills. Of these, coarse crushers are preferred, and uniaxial crushers and biaxial crushers are more preferred. Specific examples of crushers include high-power crushers 35-560, 35-720, 55-770, and 55-1050 (manufactured by Tanaka Corporation), and low-speed crushers KGA-250 and KGA-350 (manufactured by Kawata Corporation). The above-mentioned crushers may be used alone or in combination of two or more.
[0141] In step (1), the entanglement between the formed waste products having runner portions contained in the waste composition is eliminated or reduced, so that the waste composition can be efficiently fed into the crusher.
[0142] <Step (2-2)> Step (2-2) is a step of removing impurities contained in the waste composition. The molded waste contained in the waste composition may contain two or more resins. In addition, the waste composition may also contain additives, decomposition products of resins, decomposition products of additives, etc. From the viewpoint of producing a recycled resin with excellent physical properties, it is preferable to remove impurities from the waste composition.
[0143] The method for removing impurities contained in the waste composition is not particularly limited, and examples thereof include a method that utilizes the difference in physical properties between the target resin and the impurities, and a method that utilizes the difference in chemical properties between the target resin and the impurities.
[0144] Methods that utilize the difference in physical properties between the target resin and impurities include a method that uses magnetic force, a method that uses wind force, a method that uses a sieve, a method that uses specific gravity, and a method that uses buoyancy.
[0145] For example, if the impurities are metals, they can be removed by a method using magnetic force. Specifically, metals that may be contained in the waste composition can be removed by using a magnet or a metal detector. Other methods that can be applied include a method of removing impurities using salt water to utilize differences in buoyancy, a method of removing impurities using activated carbon to utilize differences in adsorption force, and a method of removing impurities using hydrocyclone treatment to utilize differences in specific gravity.
[0146] As a method utilizing the difference in chemical properties between the target resin and impurities, there is a method of depolymerizing the target resin.
[0147] For example, a resin having at least one structural unit selected from the group consisting of the above general formulas (1) to (4) can be depolymerized by treating it with an alkaline aqueous solution to obtain at least one dihydroxy compound (depolymerized monomer) selected from the group consisting of the following general formulas (1') to (4'):
[0148] Furthermore, for example, a resin having at least one structural unit selected from the group consisting of the above general formulas (9) to (11) can be depolymerized by treating it with an alkaline aqueous solution to obtain at least one dicarboxylic acid compound (depolymerized monomer) selected from the group consisting of the following general formulas (9') to (11'):
[0149] On the other hand, impurity resins having at least one structural unit selected from the group consisting of general formulae (6) to (8) are not depolymerized even when treated with an aqueous alkaline solution.
[0150] Therefore, when a waste composition contains a resin having at least one structural unit selected from the group consisting of general formulas (1) to (4) and an impurity resin having at least one structural unit selected from the group consisting of general formulas (6) to (8), treatment with an alkaline aqueous solution will depolymerize only the resin having at least one structural unit selected from the group consisting of general formulas (1) to (4). Also, when a waste composition contains a resin having at least one structural unit selected from the group consisting of general formulas (9) to (11) and an impurity resin having at least one structural unit selected from the group consisting of general formulas (6) to (8), treatment with an alkaline aqueous solution will depolymerize only the resin having at least one structural unit selected from the group consisting of general formulas (9) to (11).
[0151] The resulting dihydroxy compound (depolymerized monomer) has properties significantly different from those of an impurity resin having at least one structural unit selected from the group consisting of general formulas (6) to (8), and therefore the impurity resin can be removed.
[0152] The alkali treatment can be carried out by any known method without any particular limitation. For example, the alkali treatment can be carried out by adding the waste composition and an alkaline aqueous solution to a reaction solvent and allowing them to react with each other.
[0153] The reaction solvent is not particularly limited, but examples thereof include aliphatic hydrocarbon solvents and aromatic hydrocarbon solvents.
[0154] The aliphatic hydrocarbon solvent is not particularly limited, but examples thereof include pentane, hexane, heptane, octane, nonane, decane, cyclohexane, and cyclodecane.
[0155] The aromatic hydrocarbon solvent is not particularly limited, but examples thereof include toluene, xylene, and mesityle.
[0156] Among these, the reaction solvent is preferably an aromatic hydrocarbon solvent, more preferably toluene or xylene. The above-mentioned reaction solvents may be used alone or in combination of two or more.
[0157] The amount of reaction solvent used is not particularly limited, but is preferably 30 to 2000 parts by mass, more preferably 40 to 1500 parts by mass, and even more preferably 100 to 1000 parts by mass, relative to 100 parts by mass of the waste composition. When the amount of reaction solvent used is 30 parts by mass or more, the organic components of the waste composition are sufficiently dissolved in the reaction solvent, which is preferable, thereby increasing the reaction efficiency. On the other hand, when the amount of reaction solvent used is 2000 parts by mass or less, the reaction time is shortened, which is preferable.
[0158] The alkaline aqueous solution contains a metal oxide and water.
[0159] The metal oxide is not particularly limited, but examples thereof include alkali metals such as sodium hydroxide, potassium hydroxide, and rubidium hydroxide; and alkaline earth metals such as calcium hydroxide and barium hydroxide. Among these, the metal oxide is preferably an alkali metal, more preferably sodium hydroxide or potassium hydroxide, and even more preferably potassium hydroxide. These metal oxides may be used alone or in combination of two or more.
[0160] The amount of the metal oxide used is not particularly limited, but is preferably 1.5 to 10 mol, more preferably 2 to 8 mol, and even more preferably 2 to 4 mol, per mol of carbonate bond in the polycarbonate resin. A metal oxide used in an amount of 1.5 mol or more is preferred because depolymerization is sufficiently carried out. On the other hand, a metal oxide used in an amount of 10 mol or less is preferred because production costs are reduced.
[0161] The concentration of the metal oxide in the alkaline aqueous solution is preferably 10 to 60% by mass, more preferably 15 to 55% by mass, and even more preferably 20 to 50% by mass, based on the total mass of the alkaline aqueous solution. A metal oxide concentration of 10% by mass or more is preferred because it increases the depolymerization reaction rate. On the other hand, a metal oxide concentration of 60% by mass or less is preferred because it prevents the alkaline aqueous solution from becoming a slurry and facilitates the reaction.
[0162] The treatment temperature (depolymerization reaction temperature) is not particularly limited, but is preferably 120° C. or lower, more preferably 100° C. or lower, and even more preferably 30 to 90° C. A treatment temperature of 120° C. or lower is preferred because side reactions can be prevented.
[0163] <Step (2-3)> Step (2-3) is a step of producing a recycled resin.
[0164] In the step (2-2), when the impurities are removed by a method that utilizes the difference in physical properties between the target resin and the impurities, the composition of the target resin remains unchanged, and the resin obtained by removing the impurities is a recycled resin.
[0165] On the other hand, when the impurities are removed by a method utilizing the difference in chemical properties between the target resin and the impurities, the depolymerized monomer of the target resin can be polymerized to produce a recycled resin. In this case, the recycled resin produced may be the same as or different from the target resin contained in the waste composition.
[0166] The method for producing a recycled resin by polymerizing a target depolymerized monomer of a resin is not particularly limited, and the recycled resin can be produced by a known method. For example, when the depolymerized monomer is at least one dihydroxy compound selected from the group consisting of the above general formulas (1') to (4'), the recycled resin can be produced by subjecting the dihydroxy compound and a carbonate diester to a solution condensation method in the presence of a basic compound catalyst and / or a transesterification catalyst, or in the absence of a catalyst.
[0167] The carbonic acid diester is not particularly limited, but examples thereof include diphenyl carbonate, ditolyl carbonate, bis(chlorophenyl) carbonate, m-cresyl carbonate, dimethyl carbonate, diethyl carbonate, dibutyl carbonate, dicyclohexyl carbonate, etc. Among these, diphenyl carbonate is preferred.
[0168] The amount of the diester carbonate compound used is preferably 0.97 to 1.20 mol, more preferably 0.98 to 1.10 mol, and even more preferably 1.00 to 1.10 mol, per mol of the dihydroxy compound.
[0169] The basic compound catalyst is not particularly limited, but examples thereof include alkali metal compounds, alkaline earth metal compounds, and nitrogen-containing compounds.
[0170] The alkali metal compound is not particularly limited, and examples thereof include organic acid salts, inorganic salts, oxides, hydroxides, hydrides, and alkoxides of alkali metals.Specific examples thereof include sodium hydroxide, potassium hydroxide, cesium hydroxide, lithium hydroxide, sodium bicarbonate, sodium carbonate, potassium carbonate, cesium carbonate, lithium carbonate, sodium acetate, potassium acetate, cesium acetate, lithium acetate, sodium stearate, potassium stearate, cesium stearate, lithium stearate, sodium borohydride, sodium phenylborohydride, sodium benzoate, potassium benzoate, cesium benzoate, lithium benzoate, disodium hydrogen phosphate, dipotassium hydrogen phosphate, dilithium hydrogen phosphate, disodium phenylphosphate, disodium salt, dipotassium salt, dicesium salt, or dilithium salt of bisphenol A, and sodium salt, potassium salt, cesium salt, or lithium salt of phenol.
[0171] The alkaline earth metal compound is not particularly limited, and examples thereof include organic acid salts, inorganic salts, oxides, hydroxides, hydrides, and alkoxides of alkaline earth metal compounds. Specific examples include magnesium hydroxide, calcium hydroxide, strontium hydroxide, barium hydroxide, magnesium hydrogen carbonate, calcium hydrogen carbonate, strontium hydrogen carbonate, barium hydrogen carbonate, magnesium carbonate, calcium carbonate, strontium carbonate, barium carbonate, magnesium acetate, calcium acetate, strontium acetate, barium acetate, magnesium stearate, calcium stearate, calcium benzoate, and magnesium phenylphosphate.
[0172] The nitrogen-containing compound is not particularly limited, but examples thereof include quaternary ammonium hydroxides, salts thereof, amines, etc. Specific examples include quaternary ammonium hydroxides having an alkyl group, an aryl group, etc., such as tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, and trimethylbenzylammonium hydroxide; tertiary amines such as triethylamine, dimethylbenzylamine, and triphenylamine; secondary amines such as diethylamine and dibutylamine; primary amines such as propylamine and butylamine; imidazoles such as 2-methylimidazole, 2-phenylimidazole, and benzimidazole; ammonia, tetramethylammonium borohydride, tetrabutylammonium borohydride, tetrabutylammonium tetraphenylborate, and tetraphenylammonium tetraphenylborate.
[0173] Examples of the transesterification catalyst include salts of zinc, tin, zirconium, lead, etc. Specific examples include zinc acetate, zinc benzoate, zinc 2-ethylhexanoate, tin(II) chloride, tin(IV) chloride, tin(II) acetate, tin(IV) acetate, dibutyltin dilaurate, dibutyltin oxide, dibutyltin dimethoxide, zirconium acetylacetonate, zirconium oxyacetate, zirconium tetrabutoxide, lead(II) acetate, and lead(IV) acetate.
[0174] The above-mentioned basic compound catalysts and transesterification catalysts may be used alone or in combination of two or more kinds.
[0175] The amount of the basic compound catalyst and the transesterification catalyst (total amount when used in combination) used is 1 × 10 per mole of the dihydroxy compound. -9 ~1 x 10 -3 mol, preferably 1×10 -7 ~1 x 10 -4 More preferably, it is moles.
[0176] In the melt polycondensation method, it is desirable to melt a dihydroxy compound and a carbonate diester in a reaction vessel and then carry out the reaction in a state in which the produced monohydroxy compound remains. In order to retain the monohydroxy compound, the pressure can be controlled by, for example, closing the reaction vessel or reducing or increasing the pressure.
[0177] Furthermore, for example, when the depolymerized monomer is at least one dicarboxylic acid compound selected from the group consisting of the above general formulae (9') to (11'), the dicarboxylic acid compound can be converted into an alkyl ester, an acid halide, or an acid anhydride, and then reacted with a diol compound to produce a recycled resin.
[0178] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these. Unless otherwise specified, "%" is based on mass.
[0179] Example 1 Molding waste (a mixture of a resin having structural units of BPEF (9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene) and a resin having structural units of BNE (2,2'-bis(2-hydroxyethoxy)-1,1'-binaphthalene)) was collected from an optical material manufacturing factory, and a waste composition (molding waste content: 100 mass%, specific gravity: 1.25) was obtained. FIG. 3 is a schematic diagram of an integrated product of a plastic product and molding waste obtained after injection molding. The molding waste product is a plastic product 11 cut off from the one-piece product, and has a sprue portion 7 (inner diameter: 4.3 mm, length: 48.1 mm), eight runner portions 8 with a branching structure (inner diameter: 2.5 mm, length to branching structure: 12 mm, length of each branching structure portion: 9.6 mm), a gate portion 9 (inner diameter: 1.0 mm), and a cold slug well portion 10 at the end of the sprue portion (inner diameter: 4.3 mm, length: 6.3 mm).
[0180] The waste composition was charged onto one end of a conveyor (vibrating conveying floor, width: 30 cm, length: 1.5 m) vibrated at 50 Hz, with 500 g of the waste composition being charged over 10 seconds.
[0181] After the waste composition reached the other end of the vibrating transport bed, the waste composition was collected.
[0182] The waste compositions recovered after the vibration transport were evaluated for entanglement according to the following criteria. The results are shown in Table 1 below: A: No entanglement B: Almost no entanglement C: Slight entanglement D: Entanglement
[0183] Example 2 The waste composition was collected in the same manner as in Example 1, except that 500 g of the waste composition was added over 20 seconds.
[0184] Example 3 The waste composition was collected in the same manner as in Example 1, except that 250 g of the waste composition was added over 10 seconds.
[0185] Example 4 The waste composition was collected in the same manner as in Example 1, except that 100 g of the waste composition was added over 10 seconds.
[0186] Example 5 The waste composition was recovered in the same manner as in Example 1, except that the vibration frequency of the vibrating transport bed was changed to 40 Hz and 250 g of the waste composition was added over 10 seconds.
[0187] Example 6 The waste composition was recovered in the same manner as in Example 1, except that the vibration frequency of the vibrating transport bed was changed to 60 Hz and 250 g of the waste composition was added over 10 seconds.
[0188] Comparative Example 1 The waste composition was recovered in the same manner as in Example 1, except that the vibration frequency of the vibrating transport bed was changed to 0 Hz and 100 g of the waste composition was added over 10 seconds.
[0189]
[0190] The results in Table 1 show that the entanglement of the waste composition was eliminated or reduced, and therefore it is possible to suitably produce recycled resin from the waste composition.
[0191] REFERENCE SIGNS LIST 1 mold 2 sprue 3 runner 4 gate 5 cavity core 6, 6' cold slug well 7 sprue section 8 runner section 9 gate section 10, 10' cold slug well section
Claims
1. A method for producing recycled resin, comprising: a step (1) of supplying a waste composition including molded waste products having at least a runner portion to a vibrating transport bed and vibratingly transporting the waste composition; and a step (2) of obtaining a recycled resin from the vibratingly transported waste composition.
2. The method according to claim 1, wherein the vibration frequency of the vibrating transport bed is 1 to 1000 Hz.
3. The method according to claim 1, wherein the waste composition is fed to the vibrating transport bed at a rate of 5 to 100 g / sec.
4. The method according to claim 1, wherein the amount of the waste composition fed is 100 to 5000 g / m2 relative to the width of the vibrating transport bed.
5. The manufacturing method according to claim 1, wherein the specific gravity of the molding waste is 0.9 to 1.
5.
6. The resin constituting the molding waste is represented by the following general formulas (1) to (5): [In the formula, X a , X b , X c , X d , X e , and X f each independently represents an alkylene group having 1 to 4 carbon atoms; R a , R b , R c , R cc , R d , R dd , R e , R ee , R f、 and R ff each independently represents a halogen atom, an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, a cycloalkyl group having 5 to 20 carbon atoms, a cycloalkoxy group having 5 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, a heteroaryl group having 3 to 20 carbon atoms containing one or more hetero ring atoms selected from O, N, and S, an aryloxy group having 6 to 20 carbon atoms, and -C≡C-R i is selected from i represents an aryl group having 6 to 20 carbon atoms or a heteroaryl group having 3 to 20 carbon atoms containing one or more hetero ring atoms selected from O, N, and S; a, b, c, d, e, and f each independently represent an integer of 0 to 10; h, i, j, j', k, k', m, m', n, and n' each independently represent an integer of 0 to 4; R g and R h each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms.
7. The resin constituting the molding waste is represented by the following general formulas (6) to (8): [In the formula, X g each independently represents an alkylene group having 1 to 10 carbon atoms; R j , R k , and R l each independently represents a halogen atom, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkoxy group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 5 to 20 carbon atoms, a substituted or unsubstituted cycloalkoxy group having 5 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, a substituted or unsubstituted heteroaryl group having 3 to 20 carbon atoms containing one or more hetero ring atoms selected from O, N, and S, a substituted or unsubstituted aryloxy group having 6 to 20 carbon atoms, and -C≡C-R i is selected from i represents a substituted or unsubstituted aryl group having 6 to 20 carbon atoms or a heteroaryl group having 3 to 20 carbon atoms containing one or more hetero ring atoms selected from O, N, and S; each p independently represents an integer of 0 or 1; each q, r, and s independently represents an integer of 0 to 10; and t represents an integer of 1 to 3, where q is 2 or more and two R j When R are on adjacent carbon atoms, two R j may be joined together to form a ring structure, r is 2 or more, and two R k When R are on adjacent carbon atoms, two R k may be joined together to form a ring structure, s is 2 or more, and two R l When R are on adjacent carbon atoms, two R l may be taken together to form a ring structure, R m represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms.]. The method according to any one of claims 1 to 5, further comprising the step of:
8. The resin constituting the molding waste is represented by the following general formulas (9) to (11): [In the formula, X h each independently represents an alkylene group having 1 to 8 carbon atoms; R m , R n , R o , R p , R q , and R r are each independently selected from a halogen atom, a cyano group, and a substituted or unsubstituted alkyl group having 1 to 6 carbon atoms, and u, v, w, x, y, and z each independently represent an integer of 0 to 2.
Citation Information
Patent Citations
Manufacturing method for producing molded article of reclaimed thermoplastic resin
JP2006256339A
JP1982156909U
Recycled resin composition
JP2002265798A
Polycarbonate resin composition and molded article
JP2022131815A