Electron-accepting compound, composition for organic electroluminescent element, method for producing organic electroluminescent element, organic electroluminescent element, display device, and illumination device
The electron-accepting compound with a crosslinking temperature of 200°C or less addresses the short operating life issue in organic electroluminescent devices by reducing thermal decomposition and enhancing heat resistance, resulting in improved device longevity and efficiency.
Patent Information
- Application Number
- PCT/JP2024/011659
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-03
AI Technical Summary
Existing organic electroluminescent devices face a short operating life due to high crosslinking temperatures required for electron-accepting compounds, leading to thermal decomposition and reduced productivity in the wet film formation method.
Development of an electron-accepting compound with a crosslinking temperature of 200°C or less, represented by specific formulas, which reduces side reactions and hole traps, allowing for lower calcination temperatures and improved heat resistance during the manufacturing process.
The solution extends the driving life of organic electroluminescent devices by lowering the crosslinking temperature, reducing thermal decomposition, and enhancing heat resistance, thereby improving the operational efficiency and longevity of the devices.
Smart Images

Figure JP2024011659_03102024_PF_FP_ABST
Abstract
Description
Electron-accepting compound, composition for organic electroluminescent element, method for manufacturing organic electroluminescent element, organic electroluminescent element, display device and lighting device
[0001] The present invention relates to an electron-accepting compound useful as a hole injection layer and a hole transport layer of an organic electroluminescent element, a composition for an organic electroluminescent element containing the compound, a method for producing an organic electroluminescent element including a step of using the composition, an organic electroluminescent element, and a display device and a lighting device including the organic electroluminescent element.
[0002] In recent years, electroluminescence (EL) elements using organic materials (organic electroluminescence elements) have been developed instead of inorganic materials such as ZnS. High luminous efficiency is one of the important factors for organic electroluminescence elements, and the luminous efficiency has been significantly improved by organic electroluminescence elements provided with a hole transport layer containing an aromatic amine compound and a luminescent layer made of an aluminum complex of 8-hydroxyquinoline.
[0003] However, although the luminous efficiency has been improved, a major problem in expanding the demand for organic electroluminescent devices is their short operating life.
[0004] Methods for forming organic layers in organic electroluminescent devices include vacuum deposition and wet film formation. Vacuum deposition has the advantage of facilitating lamination, improving charge injection from the anode and / or cathode, and facilitating exciton confinement in the light-emitting layer. On the other hand, wet film formation has the advantages of not requiring a vacuum process, facilitating large-area fabrication, and easily forming layers containing multiple materials with various functions by using a coating liquid containing a mixture of multiple materials with various functions.
[0005] For example, Patent Document 1 describes an electron-accepting compound having a crosslinking group that is insolubilized after coating in order to perform lamination by a wet film-forming method, and has studied an organic electroluminescent device that can be driven with high efficiency, using an electron-accepting compound having 1,2-dihydrocyclobuta[a]naphthalene as the crosslinking group in combination with a charge-transporting compound.
[0006] International Publication No. 2017 / 164268
[0007] However, in the method described in Patent Document 1, the crosslinking temperature of the crosslinking group is high, and the baking temperature for insolubilizing the electron-accepting compound cannot be sufficiently low, resulting in insufficient productivity. Furthermore, in this method, the high crosslinking temperature causes thermal decomposition of the compound along with the crosslinking, which reduces the operating life of the organic electroluminescent device. The present invention aims to solve these problems.
[0008] The present invention has the following aspects.
[0009] A first aspect of the present invention is an electron-accepting compound having a crosslinking group with a crosslinking temperature of 200° C. or less and represented by the following formula (1):
[0010]
[0011] (In formula (1), Ar 1 each independently represents an aromatic hydrocarbon group which may have a substituent or an aromatic heterocyclic group which may have a substituent; X + represents a counter cation.)
[0012] A second aspect of the present invention is the electron-accepting compound of the first aspect, wherein the crosslinking group is represented by the following formula (6) or (7):
[0013]
[0014]
[0015] (In formula (6) and formula (7), Ar 6 ~Ar 9 each independently represents an aromatic hydrocarbon group which may have a substituent or an aromatic heterocyclic group which may have a substituent, R 1 represents a hydrogen atom or a substituent, 1 represents an oxygen atom or a sulfur atom, n1 represents an integer of 0 to 5, n2 represents an integer of 0 to 5, n3 represents an integer of 0 to 5, and "-*" represents a site that bonds to the electron-accepting skeleton.
[0016] Aspect 3 of the present invention is an electron-accepting compound according to aspect 2, wherein HA in the formula (6) or the formula (7) is 1is an electron-accepting compound in which the oxygen atom is
[0017] A fourth aspect of the present invention is the electron-accepting compound of the second or third aspect, wherein the formula (6) is selected from the following structures:
[0018]
[0019] A fifth aspect of the present invention is the electron-accepting compound according to any one of the second to fourth aspects, wherein the formula (7) is selected from the following structures:
[0020]
[0021]
[0022] A sixth aspect of the present invention is the electron-accepting compound according to any one of the first to fifth aspects, which is an electron-accepting compound represented by the following formula (2), which has at least two crosslinking groups having a crosslinking temperature of 200° C. or less:
[0023]
[0024] (In formula (2), R 81 ~R 84 are each independently a hydrogen atom, a deuterium atom, a halogen atom, an aromatic hydrocarbon group which may have a substituent, an aromatic heterocyclic group which may have a substituent, a fluorine-substituted alkyl group, or a bridging group. 1 , Ph 2 , Ph 3 , Ph 4 is a symbol indicating each benzene ring. + is a counter cation represented by the following formula (3).
[0025]
[0026] In formula (3), Ar 2 , Ar 3 are each independently an aromatic hydrocarbon group which may have a substituent.
[0027] A seventh aspect of the present invention is a composition for organic electroluminescent devices, comprising the electron-accepting compound of any one of aspects 1 to 6, a hole-transporting compound, and a solvent.
[0028] An eighth aspect of the present invention is the composition for organic electroluminescent elements according to the seventh aspect, wherein the hole transporting compound is an aromatic tertiary amine compound.
[0029] A ninth aspect of the present invention is a method for producing an organic electroluminescent device, comprising the step of forming an organic layer using the organic electroluminescent device composition according to the seventh or eighth aspect by a wet film-forming method.
[0030] A tenth aspect of the present invention is an organic electroluminescent device having an anode and a cathode on a substrate, and at least one organic layer between the anode and the cathode, wherein at least one of the organic layers contains a crosslinking reaction product of an electron-accepting compound, and the electron-accepting compound has a crosslinking group having a crosslinking temperature of 200° C. or less and is an electron-accepting compound represented by the following formula (1):
[0031]
[0032] (In formula (1), Ar 1 each independently represents an aromatic hydrocarbon group which may have a substituent or an aromatic heterocyclic group which may have a substituent; X + represents a counter cation.)
[0033] An eleventh aspect of the present invention is a display device comprising the organic electroluminescent device according to the tenth aspect.
[0034] A twelfth aspect of the present invention is a lighting device comprising the organic electroluminescent device according to the tenth aspect.
[0035] By using the composition for organic electroluminescent elements containing the electron-accepting compound of the present invention, an organic electroluminescent element having excellent driving life can be obtained.
[0036] Fig. 1 is a schematic diagram of a DSC chart. Fig. 2 is a schematic cross-sectional view showing an example of the structure of the organic electroluminescent device of this embodiment.
[0037] In this specification, "mass" and "weight" have the same meaning. The electron-accepting compound of this embodiment has a crosslinking group having a crosslinking temperature of 200°C or less, and is represented by formula (1) described below. In this embodiment, since the crosslinking temperature of the crosslinking group is 200°C or less, when a composition containing the electron-accepting compound is applied by a wet film-forming method to produce an organic electroluminescent device, the baking temperature for insolubilizing the electron-accepting compound does not become too high, and the energy of the activated state in which the crosslinks are ring-opened is reduced, thereby reducing side reactions in moieties involved in charge transport, decreasing hole trapping, and presumably lowering the driving voltage of the organic electroluminescent device.
[0038] In this specification, the terms "crosslinking temperature" and "crosslinking initiation temperature" have the same meaning. The crosslinking initiation temperature refers to the temperature at which crosslinking groups begin to bond with each other as the temperature rises. The preferred range of the crosslinking initiation temperature is usually 100°C or higher and 400°C or lower, and from the viewpoint of compound stability, it is more preferably 130°C or higher and 350°C or lower, particularly preferably 140°C or higher and 300°C or lower, and most preferably 150°C or higher and 280°C or lower. The crosslinking initiation temperature is measured by a differential scanning calorimetry (DSC) method. In the DSC method, a chart is obtained in which the horizontal axis represents temperature and the vertical axis represents heat generation, and the heat generation rate when the sample is heated at a constant rate is plotted. A schematic diagram of the chart is shown in Figure 1. In this chart, the region before heat generation is regarded as the baseline, and the region where the heat generation rate increases at a constant rate is regarded as the line during the crosslinking reaction. The temperature at the point where these two lines intersect by extrapolation is determined as the crosslinking initiation temperature.
[0039] In this embodiment, the crosslinking initiation temperature of a crosslinking group is determined by measuring the crosslinking initiation temperature using a compound in which the crosslinking group is provided. In this embodiment, the crosslinking group refers to a group that reacts with another crosslinking group located in the vicinity of the crosslinking group by heat, irradiation with active energy rays, or the like to form a new chemical bond. In this case, the reactive group may be the same as or different from the crosslinking group.
[0040] In view of improving heat resistance, the decomposition initiation temperature of the crosslinking group in this embodiment is preferably 230° C. or higher, more preferably 240° C. or higher. Furthermore, in view of improving heat resistance, the decomposition peak temperature of the crosslinking group in this embodiment is preferably 235° C. or higher, more preferably 245° C. or higher.
[0041] The decomposition onset temperature and decomposition peak temperature are measured by the DSC method. In the DSC method, the horizontal axis represents temperature and the vertical axis represents heat generation, and a chart is obtained in which the heat generation rate is plotted when the sample is heated at a constant rate. In this chart, at the heat generation peak accompanied by weight loss from the DSC chart, the region before heat generation in the DSC chart is taken as the baseline, and the region where the heat generation rate increases at a constant rate is considered to be the line during thermal decomposition. The temperature at the intersection of these two lines by extrapolation is determined as the decomposition onset temperature. The temperature at which the heat generation rate peaks in the temperature range where weight loss occurs in the DSC chart is taken as the decomposition peak temperature. Weight loss is observed by simultaneous differential thermal and thermogravimetric measurements.
[0042] The crosslinking group is not limited as long as the crosslinking temperature is 200° C. or less, but a crosslinking group represented by the following formula (6) or (7) is preferred.
[0043]
[0044]
[0045] In the formula (6) and the formula (7), Ar 6 ~Ar 9 each independently represents an aromatic hydrocarbon group which may have a substituent or an aromatic heterocyclic group which may have a substituent, R 1 represents a hydrogen atom or a substituent, HA 1 represents an oxygen atom or a sulfur atom, n1 represents an integer of 0 to 5, n2 represents an integer of 0 to 5, n3 represents an integer of 0 to 5, and "-*" represents a site that bonds to the electron-accepting skeleton.
[0046] In addition, Ar 6 ~Ar 9It is preferable that the aromatic hydrocarbon group does not have a substituent. Examples of the aromatic hydrocarbon group include aromatic hydrocarbon rings having one or two free valences, and the aromatic hydrocarbon rings are preferably aromatic hydrocarbon rings having 6 to 30 carbon atoms. Specifically, benzene rings, naphthalene rings, anthracene rings, triphenylyl rings, acenaphthene rings, fluoranthene rings, fluorene rings, etc. are preferred.
[0047] Examples of the aromatic heterocyclic group include aromatic heterocycles having one or two free valences. The aromatic heterocycle is preferably an aromatic heterocycle having 3 to 30 carbon atoms and containing a nitrogen atom, an oxygen atom, or a sulfur atom as a heteroatom. Specific examples include a pyridine ring, a pyrimidine ring, a pyrazine ring, a triazine ring, an imidazole ring, an oxazole ring, a thiazole ring, a benzothiazole ring, a benzoxazole ring, a benzimidazole ring, a quinoline ring, an isoquinoline ring, a quinoxaline ring, a quinazoline ring, a naphthyridine ring, and a phenanthridine ring, preferably a pyridine ring, a pyrazine ring, a pyrimidine ring, an imidazole ring, a benzothiazole ring, a benzoxazole ring, a quinoline ring, an isoquinoline ring, a quinoxaline ring, and a quinazoline ring, more preferably a pyridine ring, an imidazole ring, a benzothiazole ring, a quinoline ring, an isoquinoline ring, a quinoxaline ring, and a quinazoline ring, and most preferably a pyridine ring, an imidazole ring, a benzothiazole ring, a quinoline ring, a quinoxaline ring, and a quinazoline ring, and even more preferably a furan ring, a benzofuran ring, a thiophene ring, and a benzothiophene ring.
[0048] Ar 6 ~Ar 9 is preferably a benzene ring, a naphthalene ring, or a fluorene ring having one or two free valences, particularly preferably a benzene ring or a fluorene ring, and most preferably a benzene ring. 6 is a benzene ring, Ar in formula (7) 8 is preferably a phenyl group. 1Examples of the substituent in R include an alkyl group, an alkenyl group, an alkynyl group, an alkoxy group, an aromatic hydrocarbon group, and an aromatic heterocyclic group. These may further have a substituent. 1 is preferably a hydrogen atom.
[0049] The HA 1 represents an oxygen atom or a sulfur atom. 1 is preferably an oxygen atom. From the viewpoint of durability, n1 is preferably an integer of 4 or less, more preferably an integer of 3 or less, even more preferably an integer of 2 or less, and most preferably an integer of 1 or less.
[0050] From the viewpoint of solubility, n2 is preferably an integer of 1 or more, and more preferably an integer of 2 or more. From the viewpoint of durability, n2 is preferably an integer of 4 or less, and more preferably an integer of 3 or less. From the viewpoint of reactivity of the crosslinking group, n3 is preferably an integer of 3 or less, more preferably an integer of 2 or less, even more preferably an integer of 1 or less, and most preferably 0.
[0051] (Ar 6 ) n1, (Ar 7 ) n2 preferably has at least one partial structure selected from the following formulas (72-1) to (72-6) from the viewpoint of the solubility and durability of the compound. 6 ) n1, (Ar 7 ) n2 preferably has a partial structure represented by formula (72-1) or a partial structure represented by formula (72-2).
[0052]
[0053] In each of the formulas (72-1) to (72-6), * represents a bond to an adjacent structure or a hydrogen atom, and at least one of two * represents a bonding position to an adjacent structure. In the following description, * has the same definition unless otherwise specified.
[0054] Formula (72-2) is preferably the following formula (72-2-2).
[0055]
[0056] More preferably, formula (72-2) is the following formula (72-2-3).
[0057]
[0058] Specific examples of the group represented by formula (6) are listed below.
[0059]
[0060] Specific examples of the group represented by the formula (7) are listed below.
[0061]
[0062]
[0063] The formulas (6) and (7) have a structure in which an aryloxy group such as a phenoxy group, a heteroaryloxy group, an arylthio group, or a heteroarylthio group is bonded to a cyclobutene ring, and therefore have strong electron donating properties to the cyclobutene ring. Therefore, the activation energy required for the ring-opening reaction of the structures represented by the formulas (6) and (7) is thought to be low enough to allow the crosslinking reaction to proceed at a low temperature. Furthermore, lowering the crosslinking temperature reduces the energy required for the ring-opened activated state. As a result, it is thought that side reactions in the moieties involved in charge transport can be reduced, and hole trapping can be reduced.
[0064] An electron-accepting compound is a compound that extracts electrons from another compound, oxidizing the compound and reducing itself; examples of such compounds include the structures described in International Publication No. 2017 / 164268. The electron-accepting compound of this embodiment has a crosslinking group with a crosslinking temperature of 200°C or less, and is an ionic compound comprising a counter anion, which is a non-coordinating anion, and a counter cation, and is an ionic compound comprising a tetraarylborate ion represented by the following formula (1) and a counter cation. The electron-accepting compound of this embodiment may also be referred to as an electron-accepting ionic compound. The counter anion of the electron-accepting compound represented by the following formula (1) is electrochemically stable, and therefore the electron-accepting compound has excellent electrochemical durability. Furthermore, the counter anion of the electron-accepting compound represented by the following formula (1) has a delocalized negative charge, and therefore exhibits little interaction with cations and is less likely to interfere with charge transport.
[0065]
[0066] In the formula (1), Ar 1 each independently represents an aromatic hydrocarbon group which may have a substituent or an aromatic heterocyclic group which may have a substituent; X + represents a counter cation.
[0067] The counter cation is preferably an iodonium cation, a sulfonium cation, a carbocation, an oxonium cation, an ammonium cation, a phosphonium cation, a cycloheptyltrienyl cation, or a ferrocenium cation having a transition metal, more preferably an iodonium cation, a sulfonium cation, a carbocation, or an ammonium cation, and particularly preferably an iodonium cation.
[0068] Furthermore, the electron-accepting compound is more preferably an electron-accepting compound represented by the following formula (2) which has at least two crosslinking groups having a crosslinking temperature of 200° C. or less.
[0069]
[0070] In formula (2), R 81 ~R 84are each independently a hydrogen atom, a deuterium atom, a halogen atom, an aromatic hydrocarbon group which may have a substituent, an aromatic heterocyclic group which may have a substituent, a fluorine-substituted alkyl group, or a bridging group. 1 , Ph 2 , Ph 3 , Ph 4 are symbols indicating the respective benzene rings. 81 ~R 84 From the viewpoint of stability, X is preferably a fluorine atom, a fluorine-substituted alkyl group, or a crosslinking group. + is a counter cation represented by the following formula (3).
[0071]
[0072] In formula (3), Ar 2 , Ar 3 are each independently an aromatic hydrocarbon group which may have a substituent.
[0073] The aromatic hydrocarbon group is preferably an aromatic hydrocarbon group having 6 to 18 carbon atoms, more preferably an aromatic hydrocarbon group having 6 to 12 carbon atoms, and most preferably a phenyl group.
[0074] The Ar 1 ~Ar 3 , R 81 ~R 84 A preferred example of the substituent that the aromatic hydrocarbon group in the Ar group may have is an alkyl group. 1 , R 81 ~R 84 Examples of the substituent that the aromatic heterocyclic group in the formula (I) may have include an alkyl group, an alkoxy group, and an aromatic hydrocarbon group, and an alkyl group is preferred.
[0075] The formula (3) is more preferably an iodonium cation having the structure of the following formula (5).
[0076]
[0077] In formula (5), Ar 4 , Ar 5 The definition of Ar 2 , Ar 3The molecular weight of the electron-accepting compound of this embodiment is usually 900 or more, preferably 1000 or more, and more preferably 1200 or more, and usually 10000 or less, preferably 5000 or less, and more preferably 3000 or less. If the molecular weight is too small, the delocalization of positive and negative charges will be insufficient, which may result in a decrease in electron-accepting ability, whereas if the molecular weight is too large, charge transport may be hindered.
[0078] The method for producing the electron-accepting compound of this embodiment is not particularly limited, and the compound can be produced using a known method. For example, the methods described in Chem. Rev., Vol. 66, p. 243, 1966 and J. Org. Chem., Vol. 53, p. 5571, 1988 can be mentioned. Specific examples of the electron-accepting compound of this embodiment are listed below.
[0079]
[0080]
[0081]
[0082] The electron-accepting compound of this embodiment can be used as a composition for an organic electroluminescent device. The composition for an organic electroluminescent device includes a hole-transporting compound and a solvent. As the hole-transporting compound, for example, a known hole-transporting compound described in WO 2017 / 164268 can be used.
[0083] As the hole transport compound, a compound having an ionization potential of 4.5 eV to 5.5 eV is preferred in terms of hole transport ability. Examples include aromatic amine compounds, phthalocyanine derivatives or porphyrin derivatives, and oligothiophene derivatives. Among these, aromatic amine compounds are preferred from the viewpoints of amorphousness, solubility in solvents, and visible light transmittance. Among aromatic amine compounds, aromatic tertiary amine compounds are preferred. Note that the aromatic tertiary amine compound referred to in this embodiment is a compound having an aromatic tertiary amine structure, and also includes compounds having a group derived from an aromatic tertiary amine.
[0084] The type of aromatic tertiary amine compound is not particularly limited, but from the viewpoint of surface smoothing effect, an aromatic tertiary amine polymer compound that is a polymer compound having a weight-average molecular weight of 1,000 or more and 1,000,000 or less is more preferable. As the solvent contained in the composition for organic electroluminescent elements, any known solvent that dissolves the electron-accepting compound can be used. Preferred solvents include, for example, aromatic hydrocarbon solvents, ether solvents, and ester solvents. These may be used alone or in any combination and ratio of two or more.
[0085] When the composition of this embodiment is used in an organic electroluminescent device, the organic electroluminescent device is formed by laminating layers made of a large number of organic compounds, and therefore each layer is required to be a uniform layer. When forming a layer by a wet film-forming method, if moisture is present in the solution (composition) for forming a thin film, the moisture will be mixed into the coating film and the uniformity of the film will be impaired, so it is preferable that the moisture content in the solution is as low as possible. Furthermore, since organic electroluminescent devices generally use many materials that are significantly deteriorated by moisture, such as the cathode, the presence of moisture is also undesirable from the viewpoint of deterioration of the device.
[0086] Specifically, the amount of water contained in the composition of this embodiment is preferably kept to 1% by mass or less, more preferably 0.1% by mass or less, and even more preferably 0.05% by mass or less. Methods for reducing the amount of water in the composition include, for example, nitrogen gas sealing, use of a desiccant, pre-dehydration of the solvent, and use of a solvent with low water solubility. Among these, from the viewpoint of preventing the phenomenon in which the solution coating film absorbs moisture from the atmosphere during the coating process and turns white, it is preferable to use a solvent with low water solubility.
[0087] When used in applications involving film formation by a wet film-forming method, the composition of this embodiment preferably contains a solvent with low water solubility, specifically a solvent with a water solubility of 1% by mass or less, preferably 0.1% by mass or less, at a concentration of preferably 10% by mass or more, more preferably 30% by mass or more, and particularly preferably 50% by mass or more, relative to the total composition. The composition for a charge transport film of this embodiment is formed into a thin film by a wet film-forming method, dried, and then subjected to a heat treatment, as described below. When the composition for a charge transport film of this embodiment contains an electron-accepting compound having a crosslinking group, a crosslinking reaction occurs during the heat treatment.
[0088] <Organic Electroluminescent Device> The organic electroluminescent device of this embodiment is formed using the electron-accepting compound, preferably the composition for organic electroluminescent devices, and preferably by a wet film-forming method. The organic electroluminescent device preferably has at least an anode, a cathode, and at least one organic layer between the anode and the cathode on a substrate, and at least one of the organic layers is a layer formed using the electron-accepting compound of this embodiment. This layer preferably contains a crosslinking reaction product of the electron-accepting compound, and more preferably is a layer formed using the composition for organic electroluminescent devices. Furthermore, this layer is more preferably formed by a wet film-forming method. Furthermore, the organic layer includes a hole-injection layer, and more preferably this hole-injection layer is a layer formed using the composition for organic electroluminescent devices of this embodiment.
[0089] The wet film formation method is a film formation method, i.e., a coating method, which employs a wet film formation method such as spin coating, dip coating, die coating, bar coating, blade coating, roll coating, spray coating, capillary coating, inkjet printing, nozzle printing, screen printing, gravure printing, or flexographic printing, and then dries the film formed by such a method to form a film.
[0090] 2 is a schematic cross-sectional view showing a suitable structural example of the organic electroluminescent element 8 of this embodiment. In FIG. 2, reference numeral 1 represents a substrate, reference numeral 2 represents an anode, reference numeral 3 represents a hole injection layer, reference numeral 4 represents a hole transport layer, reference numeral 5 represents a light-emitting layer, reference numeral 6 represents an electron transport layer, reference numeral 7 represents a cathode, and reference numeral 8 represents an organic electroluminescent element. Known materials can be used as materials for these structures, and there are no particular restrictions. However, specific examples of typical materials and manufacturing methods for each layer include the organic electroluminescent elements disclosed in International Publication No. WO 2022 / 255403.
[0091] The organic electroluminescent element of this embodiment can have a structure opposite to that described above, i.e., for example, a cathode, an electron injection layer, an electron transport layer, a hole blocking layer, a light-emitting layer, a hole transport layer, a hole injection layer, and an anode stacked on a substrate in this order. When the organic electroluminescent element of this embodiment is applied to an organic electroluminescent device, it may be used as a single organic electroluminescent element, or may be used in a configuration in which a plurality of organic electroluminescent elements are arranged in an array, or may be used in a configuration in which an anode and a cathode are arranged in an X-Y matrix.
[0092] <Method for manufacturing organic electroluminescent element> The organic electroluminescent element of this embodiment can be manufactured by a manufacturing method including a step of forming an organic layer by a wet film-forming method using the composition of this embodiment. Preferably, in a method for manufacturing an organic electroluminescent element having an anode and a cathode on a substrate and an organic layer between the anode and the cathode, the method includes a step of forming the organic layer by a wet film-forming method using the composition of this embodiment. It is more preferable that the organic layer is an organic layer located between the anode and the light-emitting layer.
[0093] <Display Device> The display device (organic electroluminescent device display device) of this embodiment includes the organic electroluminescent device of this embodiment. There are no particular limitations on the type or structure of the display device of this embodiment, and it can be assembled using the organic electroluminescent device of this embodiment in accordance with a conventional method. For example, the organic EL display device of this embodiment can be formed by a method such as that described in "Organic EL Display" (Ohmsha, published August 20, 2004, by Shizuo Tokito, Chinaya Adachi, and Hideyuki Murata).
[0094] <Lighting Device> The lighting device (organic electroluminescent element lighting device) of this embodiment includes the organic electroluminescent element of this embodiment. The type and structure of the lighting device of this embodiment are not particularly limited, and it can be assembled using the organic electroluminescent element of this embodiment according to a conventional method.
[0095] The present invention will be described in more detail below with reference to examples. The present invention is not limited to the following examples, and can be practiced with any modifications within the scope of the invention. In addition, Ac means an acetyl group, Ph means a phenyl group, dppf means 1,1'-bis(diphenylphosphino)ferrocene, DMSO means dimethyl sulfoxide, Bu means a butyl group, and DMF means N,N-dimethylformamide.
[0096] In the following examples and comparative examples, evaluation was carried out on the following compound 1 and comparative compounds 1 to 3. Comparative compounds 1 to 3 were synthesized according to the method described in WO 2017 / 164268. Compound 1 was synthesized by the method described below.
[0097]
[0098]
[0099]
[0100]
[0101] <Crosslinking Temperature, Decomposition Onset Temperature, and Decomposition Peak Temperature> Differential scanning calorimetry (DSC, under nitrogen, at a heating rate of 10°C / min) of the electron-accepting compound was performed using a NEXTA DSC600 manufactured by Hitachi High-Technologies Corporation. Simultaneous differential thermal and thermogravimetric measurement (TG-DTA, under nitrogen, at a heating rate of 10°C / min) of the electron-accepting compound was performed using a NEXTA STA300 manufactured by Hitachi High-Technologies Corporation.
[0102] In the DSC chart, the region before heat generation was taken as the baseline, and the region where the amount of heat generation increased at a constant rate was considered to be the line during the crosslinking reaction. The temperature at the point where these two lines intersected by extrapolation was determined as the crosslinking initiation temperature. In addition, in the exothermic peak accompanied by weight loss in the DSC chart, the region before heat generation in the DSC chart was taken as the baseline, and the region where the amount of heat generation increased at a constant rate was considered to be the line during thermal decomposition. The temperature at the point where these two lines intersected by extrapolation was determined as the decomposition initiation temperature. In addition, the temperature at which the amount of heat generation peaked in the temperature range where weight loss occurred in the DSC chart was determined as the decomposition peak temperature. Weight loss was observed by simultaneous differential thermal and thermogravimetric measurements.
[0103] Example 1 Synthesis of Compound 1-c
[0104]
[0105] Under a nitrogen atmosphere, DMF (50 mL) was added to compound 1-a (5.19 g, 27.5 mmol) and potassium carbonate (15.2 g, 110 mmol). A solution of compound 1-b (12.6 g, 68.6 mmol) in DMF (50 mL) was added dropwise, and the mixture was stirred at 70°C for 7 hours. After cooling to room temperature, distilled water was added, and extraction was carried out using ethyl acetate. The organic layer was washed with a saturated aqueous sodium chloride solution and dried over magnesium sulfate, and the solvent was then distilled off under reduced pressure. The residue was subjected to silica gel column chromatography to obtain compound 1-c (yield 9.2 g, 85%).
[0106] <Synthesis of Compound 1-e>
[0107]
[0108] Under a nitrogen atmosphere, anhydrous DMSO (100 mL) was added to compound 1-c (9.17 g, 23.3 mmol), compound 1-d (8.88 g, 34.9 mmol), and potassium acetate (6.86 g, 69.9 mmol), and the mixture was heated to 50°C. PdCl2(dppf)CHCl2 (0.95 g, 1.17 mmol) was added, and the mixture was stirred at 85°C for 4 hours. After cooling to room temperature, distilled water was added, and the mixture was subjected to suction filtration. The collected residue was dissolved in dichloromethane, washed with a saturated aqueous sodium chloride solution, dried over magnesium sulfate, and the solvent was distilled off under reduced pressure. The residue was subjected to silica gel column chromatography to obtain compound 1-e (yield 9.5 g, 93%).
[0109] <Synthesis of Compound 1-g>
[0110]
[0111] Under a nitrogen atmosphere, compound 1-e (6.76 g, 15.4 mmol) and compound 1-f (10.5 g, 23.0 mmol) were sequentially added with nitrogen-bubbled toluene (100 mL), ethanol (30 mL), and an aqueous solution of tripotassium phosphate (2.0 mol / L, 30 mL) and heated to 40°C. Subsequently, Pd(PPh3)4 (0.18 g, 0.15 mmol) was added, and the mixture was stirred at 80°C for 7 hours. After cooling to room temperature, saturated aqueous sodium chloride solution was added, and extraction was performed using toluene. The organic layer was washed with saturated aqueous sodium chloride solution and dried over magnesium sulfate, and the solvent was then distilled off under reduced pressure. The residue was subjected to silica gel column chromatography to obtain compound 1-g (yield 6.1 g, 58%).
[0112] <Synthesis of Compound 1-i>
[0113]
[0114] Under an argon atmosphere, ultra-dehydrated diethyl ether (14 mL) was added to compound 1-h (1.44 g) and the mixture was cooled to an internal temperature of -74°C. n-BuLi (1.6 M hexane solution, 3.3 mL) was added dropwise at an internal temperature of -74 to -65°C, and the mixture was further stirred at the same temperature for 1 hour. Then, BCl3 (1 M heptane solution, 1.9 mL) was added at an internal temperature of -74 to -65°C. After raising the internal temperature to -20°C, the mixture was stirred for 1 hour at an internal temperature of -20 to -12°C. The mixture was again cooled to an internal temperature of -74°C (Solution 1A).
[0115] In a separate reaction vessel, under an argon atmosphere, ultra-dehydrated diethyl ether (40 mL) was added to compound 1-g (2.00 g) and cooled to an internal temperature of -68°C. n-BuLi (1.6 M hexane solution, 2.0 mL) was added dropwise at an internal temperature of -68°C. The internal temperature was once raised to -40°C, then cooled to -75°C and stirred for 1 hour (Solution 1B). Under an argon atmosphere, Solution 1B was added dropwise to Solution 1A at an internal temperature of -74°C to -62°C. After raising the internal temperature to 35°C, the mixture was stirred at the same temperature for 2.5 hours and then at room temperature overnight. After cooling to an internal temperature of 0°C, purified water (25 mL) was added, and extraction was performed using ethyl acetate. The organic layer was washed with saturated aqueous sodium chloride solution, dried over magnesium sulfate, and the solvent was distilled off under reduced pressure. The residue was subjected to silica gel column chromatography to obtain Compound 1-i (yield 1.2 g, yield <23%, c <48.8 wt % ethyl acetate adduct).
[0116] <Synthesis of Compound 1>
[0117]
[0118] Under an argon atmosphere, dichloromethane (2.3 mL) and methanol (8.9 mL) were added to compound 1-i (1.17 g, c<48.8 wt%). Compound 1-j (0.167 mg) was added at a bath temperature of 10°C. After raising the bath temperature to 25°C, the mixture was stirred for 2 hours. The solvent was distilled off under reduced pressure, and azeotropic distillation was performed with dichloromethane (12 mL x 2). Dichloromethane (12 mL) was added, and the insoluble matter was suction filtered and rinsed with dichloromethane (30 mL). The filtrate was concentrated, and the residue was subjected to silica gel column chromatography to obtain compound 1 (yield 0.28 g, 40%).
[0119]
[0120] These results confirmed that the specific bridging group contained in Compound 1 undergoes a crosslinking reaction at a temperature 45°C lower than that of 1,2-dihydrocyclobuta[a]naphthalene contained in Comparative Compound 1. Therefore, it is believed that the electron-accepting compound of the present invention having the above formula (6) or (7) as a bridging group becomes insoluble in a solvent at a lower temperature than conventional electron-accepting compounds having 1,2-dihydrocyclobuta[a]naphthalene as a bridging group. Therefore, the electron-accepting compound of the present invention can achieve insolubilization at low temperatures. It was also confirmed that the specific bridging group contained in Compound 1 has a higher decomposition onset temperature and a higher decomposition peak temperature than 1,2-dihydrocyclobuta[a]naphthalene contained in Comparative Compound 1. Therefore, it is believed that the electron-accepting compound of the present invention having the above formula (6) or (7) as a bridging group exhibits higher heat resistance than conventional electron-accepting compounds having 1,2-dihydrocyclobuta[a]naphthalene as a bridging group.
[0121] [Fabrication and Performance Evaluation of Organic Electroluminescent Devices] [Example I-1] An organic electroluminescent device was fabricated by the following method. A 50 nm thick indium tin oxide (ITO) transparent conductive film (manufactured by Geomatec Co., Ltd., sputter-deposited film) was deposited on a glass substrate and patterned into 2 mm wide stripes using standard photolithography techniques and hydrochloric acid etching to form an anode. The substrate with the ITO pattern thus formed was cleaned in this order: ultrasonic cleaning with a surfactant aqueous solution, washing with ultrapure water, ultrasonic cleaning with ultrapure water, and washing with ultrapure water, then dried with compressed air, and finally subjected to ultraviolet ozone cleaning.
[0122] As a composition for forming a hole injection layer, a composition was prepared by dissolving a hole transporting polymer compound having a repeating structure of the following formula (P-1) in ethyl benzoate so as to give a concentration of 3.0 mass % and an electron accepting compound of the following compound 1 in ethyl benzoate so as to give a concentration of 0.6 mass %.
[0123]
[0124]
[0125] This composition for forming a hole injection layer was spin-coated onto the substrate in the atmosphere and dried on a hot plate in the atmosphere at 210° C. for 30 minutes to form a uniform thin film with a thickness of 40 nm, which was used as a hole injection layer.
[0126] Next, a charge-transporting polymer compound having a repeating structure of the following formula (HT-1) was dissolved in 1,3,5-trimethylbenzene to prepare a 2.0% by mass solution. This solution was spin-coated onto the substrate on which the hole-injection layer had been formed in a nitrogen glove box, and dried on a hot plate in the nitrogen glove box at 230°C for 30 minutes to form a uniform thin film with a thickness of 40 nm, which served as a hole-transporting layer.
[0127]
[0128] Subsequently, as materials for the light-emitting layer, a composition for forming a light-emitting layer was prepared by dissolving in cyclohexylbenzene 1.5 mass % of a compound represented by the following formula (H-1), 1.5 mass % of a compound represented by the following formula (H-2), 3.0 mass % of a compound represented by the following formula (H-3), and 1.8 mass % of a compound represented by the following formula (D-1).
[0129]
[0130]
[0131]
[0132]
[0133] The composition for forming the light-emitting layer was spin-coated on the substrate on which the hole transport layer had been formed in a nitrogen glove box, and dried on a hot plate in the nitrogen glove box at 120°C for 20 minutes to form a uniform thin film with a thickness of 60 nm, which was used as the light-emitting layer.
[0134] The substrate on which the light-emitting layer had been formed was placed in a vacuum deposition apparatus, and the inside of the apparatus was heated to 2 × 10 -4 The chamber was evacuated to a pressure of 100 Pa or less. Next, a compound (ET-1) represented by the following formula and 8-hydroxyquinolinolatolithium were co-deposited on the light-emitting layer by vacuum deposition in a thickness ratio of 2:3 to form an electron-transporting layer having a thickness of 30 nm.
[0135]
[0136] Next, a 2 mm wide striped shadow mask was attached to the substrate as a mask for cathode deposition so as to be perpendicular to the ITO stripes of the anode, and aluminum was heated in a molybdenum boat to form an aluminum layer with a thickness of 80 nm, thereby forming a cathode.
[0137] In this manner, an organic electroluminescent device having a light-emitting area measuring 2 mm x 2 mm was obtained.
[0138] Comparative Example I-1 An organic electroluminescent device was fabricated in the same manner as in Example I-1, except that the above-mentioned comparative compound 1 was used instead of compound 1 as the material for the hole injection layer.
[0139] An organic electroluminescent device was fabricated in the same manner as in Example I-1, except that the material for the hole injection layer was the comparative compound 2 instead of the compound 1. The crosslinking temperature of the comparative compound 2 was higher than 200°C.
[0140] An organic electroluminescent device was fabricated in the same manner as in Example I-1, except that the material for the hole injection layer was the comparative compound 3 instead of the compound 1. The crosslinking temperature of the comparative compound 2 was higher than 200°C.
[0141] [Evaluation of Devices] The organic electroluminescent devices obtained in Example I-1 and Comparative Examples I-1 to I-3 were used, and a current of 15 mA / cm 2 The time (LT95) until the luminance decreased to 95% of the initial luminance when a current was continuously passed through the element at a current density of 1000 kJ / s was measured. The results of these measurements are shown in Table 2. In Table 2, the values for Example I-1 and Comparative Examples I-1 to I-2 are relative values, with the value for Comparative Example I-3 being set to 1. The results in Table 2 demonstrate that organic electroluminescent devices using compositions according to embodiments of the present invention have long operating lives.
[0142]
[0143] The polymer of the present invention has excellent electrochemical stability, and therefore, for example, an element including a layer formed using the polymer can be applied to flat panel displays (for example, those for office automation computers and wall-mounted televisions), in-vehicle display elements, mobile phone displays, light sources taking advantage of the characteristics of surface light emitters (for example, light sources for copiers, backlight light sources for liquid crystal displays and meters), display boards, and marker lights.
[0144] While the present invention has been described in detail and with reference to specific embodiments, it should be understood that the present invention is not limited to such examples. It is clear to those skilled in the art that various modifications and alterations can be made within the scope of the claims, and it is understood that such modifications and alterations are within the scope of the present invention. Furthermore, the components of the above-described embodiments may be combined in any manner without departing from the spirit of the invention.
[0145] This application is based on a Japanese patent application (Patent Application No. 2023-051960) filed on March 28, 2023, the contents of which are incorporated herein by reference.
[0146] REFERENCE SIGNS LIST 1 substrate 2 anode 3 hole injection layer 4 hole transport layer 5 light emitting layer 6 electron transport layer 7 cathode 8 organic electroluminescent device
Claims
1. An electron-accepting compound having a crosslinking group with a crosslinking temperature of 200° C. or less and represented by the following formula (1): (In formula (1), Ar 1 each independently represents an aromatic hydrocarbon group which may have a substituent or an aromatic heterocyclic group which may have a substituent; X + represents a counter cation.) 2. The electron-accepting compound according to claim 1, wherein the bridging group is represented by the following formula (6) or (7). (In formula (6) and formula (7), Ar 6 ~Ar 9 each independently represents an aromatic hydrocarbon group which may have a substituent or an aromatic heterocyclic group which may have a substituent; R 1 represents a hydrogen atom or a substituent, 1 represents an oxygen atom or a sulfur atom, n1 represents an integer of 0 to 5, n2 represents an integer of 0 to 5, n3 represents an integer of 0 to 5, and "-*" represents a site that bonds to the electron-accepting skeleton.
3. HA in the formula (6) and the formula (7) 1 The electron accepting compound according to claim 2, wherein is an oxygen atom.
4. The electron accepting compound according to claim 2, wherein the formula (6) is selected from the following structures:
5. The electron accepting compound according to claim 2, wherein the formula (7) is selected from the following structures:
6. An electron-accepting compound according to claim 1 or 2, which has at least two crosslinking groups having a crosslinking temperature of 200° C. or less and is represented by the following formula (2): (In formula (2), R 81 ~R 84 are each independently a hydrogen atom, a deuterium atom, a halogen atom, an aromatic hydrocarbon group which may have a substituent, an aromatic heterocyclic group which may have a substituent, a fluorine-substituted alkyl group, or a bridging group. 1 , Ph 2 , Ph 3 , Ph 4 are symbols that indicate the respective benzene rings. + is a counter cation represented by the following formula (3). In formula (3), Ar 2 , Ar 3 each independently represents an aromatic hydrocarbon group which may have a substituent.
7. A composition for organic electroluminescent devices comprising the electron accepting compound according to claim 1 or 2, a hole transporting compound and a solvent.
8. The composition for organic electroluminescent devices according to claim 7, wherein the hole transporting compound is an aromatic tertiary amine compound.
9. A method for producing an organic electroluminescent device, comprising the step of forming an organic layer by a wet film-forming method using the organic electroluminescent device composition according to claim 7.
10. An organic electroluminescence device having an anode and a cathode on a substrate, and at least one organic layer between the anode and the cathode, wherein at least one of the organic layers contains a crosslinking reaction product of an electron-accepting compound, and the electron-accepting compound has a crosslinking group having a crosslinking temperature of 200° C. or less and is an electron-accepting compound represented by the following formula (1): (In formula (1), Ar 1 each independently represents an aromatic hydrocarbon group which may have a substituent or an aromatic heterocyclic group which may have a substituent; X + represents a counter cation.) 11. A display device comprising the organic electroluminescent device according to claim 10.
12. A lighting device comprising the organic electroluminescent element according to claim 10.
Citation Information
Patent Citations
Composition for organic electroluminescent element, polymer film, organic electroluminescent element, organic el-display, and organic el lighting
JP2009295974A
Polymer Charge Transfer Layer and Organic Electronic Device Containing the Same
JP2018504484A
Quantum dot light-emitting element, quantum dot display device, quantum dot lighting, and manufacturing method for quantum dot light-emitting element
JP2022164474A
Nail service providing method based on application using platform and apparatus therefore
KR1020230162520A
Curved battery cell thickness measurement apparatus comprising a lower static pressure callipers and a curved cell thickness measurement method using the same
KR1020240053436A