Method for producing carbon nanotube dispersion paste and method for producing mixture paste for lithium-ion secondary battery

The method for producing a carbon nanotube dispersion paste with controlled polar functional groups and solvent recycling addresses the challenges of pigment dispersibility and storage stability, enhancing battery performance and recyclability.

WO2024204177A1PCT designated stage expired Publication Date: 2024-10-03KANSAI PAINT CO LTD

Patent Information

Application Number
PCT/JP2024/011914
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2024-03-26
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing methods for producing carbon nanotube dispersion pastes and composite materials for lithium ion secondary batteries face challenges with pigment dispersibility, storage stability, and solvent recyclability, particularly at high pigment concentrations or viscosities, leading to issues like gelation and inefficient energy use.

Method used

A method involving a carbon nanotube dispersion paste made with a pigment dispersion resin containing specific polar functional groups, N-methyl-2-pyrrolidone, and an amine compound, where the water content is controlled to prevent gelation, and the solvent is recycled, ensuring excellent dispersibility and stability.

Benefits of technology

The method achieves stable and uniform dispersion of carbon nanotubes, reduces viscosity, and allows for efficient recycling of solvents, resulting in improved battery performance and reduced waste, while maintaining excellent finishing properties of the electrode layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

The present invention addresses the problem of providing: methods for producing a carbon nanotube dispersion paste and a mixture paste which have excellent solvent recycling properties, pigment dispersibility, and storage stability; and an electrode layer for a lithium-ion secondary battery, the electrode layer having excellent performance in various aspects (finishing properties, battery performance, and the like). To solve the problem, provided is a method for producing a carbon nanotube dispersion paste obtained by mixing and dispersing components including a pigment dispersion resin (A), a carbon nanotube (B), an N-methyl-2-pyrrolidone (C), and an amine compound (D), wherein: the pigment dispersion resin (A) has at least one polar functional group selected from the group consisting of an amide group, an imide group, a hydroxyl group, a carboxyl group, a sulfonic acid group, a phosphoric acid group, a silanol group, a cyano group, a pyrrolidone group, and an amino group; the concentration of the polar functional group in the pigment dispersion resin (A) is 0.3-23 mmol / g; and when the boiling point of the N-methyl-2-pyrrolidone (C) is (Xc)ºC and the boiling point of the amine compound (D) is (Xd)ºC, (Xc)-10>(Xd) is satisfied.
Need to check novelty before this filing date? Find Prior Art

Description

Method for producing carbon nanotube dispersion paste and method for producing composite paste for lithium ion secondary batteries

[0001] The present invention relates to a method for producing a carbon nanotube-dispersed paste (also referred to as a conductive pigment paste in the present invention) that is excellent in solvent recyclability, pigment dispersibility, and storage stability, a method for producing a composite paste (for lithium ion secondary batteries), and a method for producing a battery electrode layer that has excellent battery performance.

[0002] Paste-like pigment dispersions in which a pigment is dispersed in a mixture of a pigment dispersing resin, a solvent, and the like have conventionally been widely used in fields such as paints, battery electrodes, coating materials, coating materials, electromagnetic wave shields, display panels, touch screen panels, colored films, colored sheets, decorative materials, protective materials, magnet modifiers, printing inks, device members, electronic device members, printed wiring boards, solar cells, functional rubber members, and resin molded films. Furthermore, conductive pigments, conductive polymers, and the like are incorporated into these materials to impart functions such as electrostatic coating properties, conductivity, electromagnetic wave shielding properties, and antistatic properties.

[0003] In these fields, there is an increasing demand for improvements in performance such as pigment dispersibility, storage stability, conductivity, coatability, and finish. To this end, pigment dispersing resins and pigment pastes are being developed that have excellent pigment dispersing ability and excellent pigment dispersion stability that prevents reagglomeration of pigment particles in the formed pigment dispersion.

[0004] When designing a pigment paste, it is important to prepare a highly concentrated and uniformly dispersed pigment paste using as little solvent and pigment dispersing resin as possible, in order to prevent the pigment dispersing resin from adversely affecting the conductive properties of the final product itself, such as the coating film, and from the perspective of reducing the amount of solvent and pigment dispersing resin used and reducing the energy used during drying.In addition, to reduce waste, be environmentally friendly, and cut costs, there is a demand for the recyclability of waste generated during the manufacturing process.

[0005] For example, Patent Document 1 discloses a method for producing an electrode slurry for a lithium secondary battery, which comprises dispersing a solvent containing fibrous carbon using a media (hereinafter sometimes referred to as "media") disperser to obtain a slurry, kneading the slurry with an electrode active material, and applying the resulting mixture to a current collector to obtain a slurry. However, in the case of a paste with a high pigment concentration and / or high viscosity, uniform dispersion is not possible, and storage stability is poor. In particular, if the slurry contains a large amount of water, high viscosity and gelation may occur. Furthermore, there is no specific disclosure regarding waste recycling.

[0006] JP 2014-182892 A

[0007] The object of the present invention is to provide a method for producing a carbon nanotube-dispersed paste and a method for producing a composite paste that are excellent in pigment dispersibility, storage stability, and solvent recyclability even in pastes with high pigment concentrations and / or high viscosity, and further to provide a method for producing a coating film (battery electrode layer) that is excellent in finish, etc.

[0008] As a result of intensive research into solving the above problems, the present inventors have found that the above-mentioned problems can be solved by a method for producing a carbon nanotube-dispersed paste obtained by mixing and dispersing components containing a pigment dispersion resin (A), carbon nanotubes (B), N-methyl-2-pyrrolidone (C), and an amine compound (D), wherein the pigment dispersion resin (A) has at least one polar functional group selected from the group consisting of an amide group, an imide group, a hydroxyl group, a carboxyl group, a sulfonic acid group, a phosphate group, a silanol group, a cyano group, a pyrrolidone group, and an amino group, and the polar functional group concentration of the pigment dispersion resin (A) is 0.3 mmol / g or more and 23 mmol / g or less, and when the boiling point of N-methyl-2-pyrrolidone (C) is (Xc) ° C. and the boiling point of the amine compound (D) is (Xd) ° C., (Xc) -10 > (Xd). This method for producing a carbon nanotube-dispersed paste has led to the completion of the present invention.

[0009] That is, the present invention provides the following methods for producing a carbon nanotube-dispersed paste, a composite paste, and an electrode layer for a lithium ion secondary battery: Item 1. A method for producing a carbon nanotube-dispersed paste obtained by mixing and dispersing components including a pigment dispersion resin (A), carbon nanotubes (B), N-methyl-2-pyrrolidone (C), and an amine compound (D), in which the pigment dispersion resin (A) has at least one polar functional group selected from the group consisting of an amide group, an imide group, a hydroxyl group, a carboxyl group, a sulfonic acid group, a phosphate group, a silanol group, a cyano group, a pyrrolidone group, and an amino group, and the concentration of the polar functional group in the pigment dispersion resin (A) is 0.3 mmol / g or more and 23 mmol / g or less, and where the boiling point of N-methyl-2-pyrrolidone (C) is (Xc)°C and the boiling point of the amine compound (D) is (Xd)°C, the relationship (Xc) - 10 > (Xd) is satisfied. Item 2. Item 3. A method for producing a carbon nanotube dispersion paste according to Item 1, wherein the N-methyl-2-pyrrolidone (C) is a recycled product, and the water content in the N-methyl-2-pyrrolidone (C) is controlled to 10,000 ppm or less, and the content of an amine compound in the N-methyl-2-pyrrolidone (C) is controlled to 10,000 ppm or less. Item 4. A method for producing a carbon nanotube dispersion paste according to any one of Items 1 to 3, wherein the content of carbon nanotubes (B) is 0.1 mass % or more and less than 15 mass %, based on 100 mass % of the total amount of the carbon nanotube dispersion paste. Item 5. A method for producing a carbon nanotube dispersion paste according to any one of Items 1 to 4, wherein the carbon nanotube dispersion paste further contains polyvinylidene fluoride (E). Item 6. Item 6. A method for producing a composite paste for a lithium ion secondary battery, comprising: mixing an electrode active material (G) with the carbon nanotube dispersion paste obtained by the method for producing a carbon nanotube dispersion paste according to any one of Items 1 to 5.Item 7. A method for producing an electrode layer for a lithium ion secondary battery, comprising coating on a current collector a composite paste for a lithium ion secondary battery obtained by the method for producing a composite paste for a lithium ion secondary battery according to Item 6. Item 8. A method for producing an electrode layer for a lithium ion secondary battery and a recycled product of N-methyl-2-pyrrolidone (C), the method comprising the steps of: coating on a current collector a composite paste for a lithium ion secondary battery obtained by the method for producing a composite paste for a lithium ion secondary battery according to Item 6 and drying by heating; recovering vapor containing N-methyl-2-pyrrolidone (C) and an amine compound (D) to produce a mixed solution; and separating the amine compound (D) from the mixed solution to produce a recycled product of N-methyl-2-pyrrolidone (C).

[0010] The method for producing a carbon nanotube-dispersed paste of the present invention is excellent in recyclability, pigment dispersibility, and storage stability (suppression of thickening), even at high pigment concentrations and / or high viscosities, and can sufficiently reduce the viscosity of the paste with a relatively small amount of dispersion resin.In addition, the coating film (battery electrode layer) produced thereby is excellent in finish and battery performance, etc.

[0011] Hereinafter, embodiments of the present invention will be described in detail.

[0012] The present invention is not limited to the following embodiments and should be understood to include various modifications implemented within the scope of the present invention. In the present invention, a paste containing carbon nanotubes is referred to as a "carbon nanotube dispersion paste," which can also be referred to as a "conductive pigment paste." The carbon nanotubes can also be abbreviated as "CNT." A paste prepared by further blending at least one electrode active material and, optionally, various other components, for coating the carbon nanotube dispersion paste is referred to as a "composite paste." The composite paste applied to a substrate and dried is referred to as a "coating film" or "composite layer." The carbon nanotube dispersion paste can be said to be a paste that does not substantially contain an electrode active material. When the coating film is used for a battery electrode, it can also be referred to as an "electrode layer."

[0013] In the present invention, the carbon nanotube-dispersed paste contains a specific pigment-dispersing resin (A) and an amine compound (D), which provides good pigment dispersibility and prevents the increase in viscosity and gelation during storage. Furthermore, by controlling the water content of the carbon nanotube-dispersed paste to 10,000 ppm or less (and the water content of N-methyl-2-pyrrolidone (C) to 10,000 ppm or less), the increase in viscosity and gelation during storage can be prevented.

[0014] The mechanism by which the carbon nanotube dispersion paste and the composite paste become viscous and gel is not clear, but the following mechanism is presumed.

[0015] For example, in carbon nanotube dispersion pastes and composite pastes containing polyvinylidene fluoride, the acidity of the protons adjacent to the fluorine groups in polyvinylidene fluoride is very high due to the electron-withdrawing properties of the fluorine groups. Therefore, proton desorption easily occurs, especially under basic conditions. It is believed that this proton desorption is particularly likely when moisture is present in the carbon nanotube dispersion paste and composite paste. After proton desorption, anions are generated on the carbon, which promotes the desorption of fluorine groups and creates double bonds in the main chain of the polyvinylidene fluoride molecules. It is believed that multiple polyvinylidene fluoride molecules with double bonds then polymerize, further polymerizing, leading to increased viscosity and gelation. In particular, because the electrode active material in the composite paste may contain lithium hydroxide, a relatively strong base, high viscosity and gelation are particularly pronounced in the composite paste.

[0016] In the present invention, by using raw materials with a specified moisture content and specifying the moisture content of the carbon nanotube dispersion paste and composite paste, it is believed that polymerization of the polymer component (polyvinylidene fluoride) can be suppressed, and the viscosity increase and gelation of the carbon nanotube dispersion paste or composite paste can be suppressed. Furthermore, the moisture content is virtually impossible to reduce to zero due to contamination from various raw materials (particularly solvents) and water vapor contained in the atmosphere during the manufacturing process. Therefore, the moisture content (lower limit) of the carbon nanotube dispersion paste that can be used in the present invention is preferably 100 ppm or more, more preferably 200 ppm or more, and even more preferably 500 ppm or more. Furthermore, the moisture content (lower limit) of N-methyl-2-pyrrolidone (C) is preferably 100 ppm or more, more preferably 200 ppm or more, and even more preferably 500 ppm or more. Within the above lower limit, production is possible without excessive moisture content control of the raw materials (reducing the moisture content) or the manufacturing process (reducing moisture contamination).

[0017] Furthermore, in the present invention, the recyclability of the solvent (mainly N-methyl-2-pyrrolidone) discharged during the production of an electrode layer for a lithium ion secondary battery is particularly important from the viewpoint of waste reduction, environmental aspects, and the like. When the boiling point of N-methyl-2-pyrrolidone (C) is (Xc)°C and the boiling point of the amine compound (D) is (Xd)°C, (Xc)-10>(Xd).

[0018] [Method for producing carbon nanotube-dispersed paste] The present invention provides a method for producing a carbon nanotube-dispersed paste obtained by mixing and dispersing components including a pigment-dispersed resin (A), carbon nanotubes (B), N-methyl-2-pyrrolidone (C), and an amine compound (D), wherein the pigment-dispersed resin (A) has at least one polar functional group selected from the group consisting of an amide group, an imide group, a hydroxyl group, a carboxyl group, a sulfonic acid group, a phosphate group, a silanol group, a cyano group, a pyrrolidone group, and an amino group, the concentration of the polar functional group in the pigment-dispersed resin (A) is 0.3 mmol / g or more and 23 mmol / g or less, and when the boiling point of N-methyl-2-pyrrolidone (C) is (Xc) °C and the boiling point of the amine compound (D) is (Xd) °C, the relationship (Xc) - 10 > (Xd) holds.

[0019] The water content (upper limit) of the carbon nanotube dispersion paste is usually 10,000 ppm or less, preferably 7,500 ppm or less, more preferably 5,000 ppm or less, even more preferably 2,500 ppm or less, and particularly preferably 1,000 ppm or less. The carbon nanotube dispersion paste used in the present invention can be said to be a substantially non-aqueous paste.

[0020] In the present invention, the water content can be measured by Karl Fischer coulometric titration. Specifically, the water content can be measured using a Karl Fischer moisture meter (manufactured by Kyoto Electronics Manufacturing Co., Ltd., product name "MKC-610") with the temperature of the moisture vaporizer (manufactured by Kyoto Electronics Manufacturing Co., Ltd., product name "ADP-611") attached to the meter set to 130°C.

[0021] Pigment Dispersion Resin (A) The pigment dispersion resin (A) has at least one polar functional group selected from the group consisting of amide, imide, hydroxyl, carboxyl, sulfonic acid, phosphate, silanol, cyano, pyrrolidone, and amino groups, and the polar functional group concentration of the pigment dispersion resin (A) is 0.3 mmol / g or more and 23 mmol / g or less. The acid groups may be in the form of salts. Among these, the polar functional groups preferably include at least amide, hydroxyl, carboxyl, sulfonic acid, phosphate, and amino groups, and more preferably include at least hydroxyl, carboxyl, and amino groups. The pigment dispersion resin (A) also preferably includes an alkyl group having 12 or more carbon atoms. The alkyl group having 12 or more carbon atoms can be any known alkyl group (hydrocarbon group) without any particular limitation. A linear or branched alkyl group is preferred, and a linear alkyl group is more preferred. The alkyl group having 12 or more carbon atoms is preferably an alkyl group having 12 to 30 carbon atoms, more preferably an alkyl group having 15 to 26 carbon atoms, and even more preferably an alkyl group having 19 to 24 carbon atoms. The alkyl group having 12 or more carbon atoms can be introduced into the resin by (co)polymerizing a polymerizable monomer containing an alkyl group having 12 or more carbon atoms. Examples of polymerizable monomers containing an alkyl group having 12 or more carbon atoms include lauryl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, behenyl (meth)acrylate, lauryl (meth)acrylamide, stearyl (meth)acrylamide, and behenyl (meth)acrylamide. These can be used alone or in combination of two or more. It is believed that when the pigment dispersing resin (A) has a relatively bulky side chain of an alkyl group having 12 or more carbon atoms, steric repulsion improves pigment dispersibility and storage stability.

[0022] The type of resin is not particularly limited as long as it is a resin other than polyvinylidene fluoride (E), which will be described later. Examples include acrylic resins, polyester resins, epoxy resins, polyether resins, alkyd resins, urethane resins, polyvinyl alcohol, polyvinyl acetal, polyvinylpyrrolidone, polyvinyl acetate, silicone resins, polycarbonate resins, chlorine-based resins, and composite resins thereof. These resins can be used alone or in combination of two or more. Among them, from the viewpoints of pigment dispersibility, storage stability, and finished quality, the pigment dispersing resin (A) preferably contains a vinyl (co)polymer (A1) obtained by polymerizing or copolymerizing a monomer containing a polymerizable unsaturated group-containing monomer of the following formula (1), and particularly preferably an acrylic resin (co)polymerized with at least one polymerizable unsaturated group-containing monomer containing a (meth)acryloyl group. Note that the "(co)polymer" in the present invention includes both a polymer obtained by polymerizing one type of monomer and a copolymer obtained by copolymerizing two or more types of monomers.

[0023] C(-R) 2 = C(-R) 2 ... Formula (1) [In the above formula, R may be the same or different and is a hydrogen atom or an organic group.] Examples of the vinyl (co)polymer (A1) include hydroxyl group-containing vinyl (co)polymers, carboxyl group-containing vinyl (co)polymers, amide group-containing vinyl (co)polymers, sulfonic acid group-containing vinyl (co)polymers, phosphate group-containing vinyl (co)polymers, pyrrolidone group-containing vinyl (co)polymers, and amino group-containing (co)polymers. These (co)polymers may be used alone or in combination of two or more.

[0024] Examples of hydroxyl group-containing vinyl (co)polymers include polyhydroxyethyl (meth)acrylate, polyvinyl alcohol, vinyl alcohol-fatty acid vinyl copolymer, vinyl alcohol-ethylene copolymer, vinyl alcohol-(N-vinylformamide) copolymer, copolymers of hydroxyethyl (meth)acrylate with other polymerizable unsaturated monomers, etc. The vinyl alcohol units in the (co)polymer may be those obtained by (co)polymerizing fatty acid vinyl units and then hydrolyzing them.

[0025] Examples of the carboxyl group-containing vinyl (co)polymer include a polymer of (meth)acrylic acid, and a copolymer of poly(meth)acrylic acid and other polymerizable unsaturated monomers.

[0026] Examples of the amide group-containing vinyl (co)polymer include a polymer of (meth)acrylamide, and a copolymer of (meth)acrylamide and other polymerizable unsaturated monomers.

[0027] Examples of sulfonic acid group-containing vinyl (co)polymers include polymers of allylsulfonic acid or styrenesulfonic acid, and copolymers of allylsulfonic acid and / or styrenesulfonic acid with other polymerizable unsaturated monomers.

[0028] Examples of the phosphoric acid group-containing vinyl (co)polymer include a polymer of (meth)acryloyloxyalkyl acid phosphate, and a copolymer of (meth)acryloyloxyalkyl acid phosphate with other polymerizable unsaturated monomers.

[0029] Examples of amino group-containing vinyl (co)polymers include copolymers of N,N-dimethylaminoethyl (meth)acrylate, N,N-diethylaminoethyl (meth)acrylate and other polymerizable unsaturated monomers.

[0030] Examples of other copolymerizable unsaturated monomers include vinyl carboxylate ester monomers such as vinyl formate, vinyl acetate, vinyl propionate, isopropenyl acetate, vinyl valerate, vinyl caprylate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl benzoate, vinyl versatate, and vinyl pivalate; olefins such as ethylene, propylene, and butylene; aromatic vinyls such as styrene and α-methylstyrene; methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate; Examples of the monomer include ethylenically unsaturated carboxylic acid alkyl ester monomers such as dimethyl fumarate, dimethyl maleate, diethyl maleate, and diisopropyl itaconate; vinyl ether monomers such as methyl vinyl ether, n-propyl vinyl ether, isobutyl vinyl ether, and dodecyl vinyl ether; halogenated vinyl monomers or vinylidene monomers such as vinyl chloride, vinylidene chloride, vinyl fluoride, and vinylidene fluoride; allyl compounds such as allyl acetate and allyl chloride; and quaternary ammonium group-containing monomers such as 3-(meth)acrylamidopropyltrimethylammonium chloride. These monomers can be used singly or in combination of two or more.

[0031] From the viewpoints of pigment dispersibility, storage stability, and compatibility with the solvent, the polar functional group concentration of the pigment dispersing resin (A) is preferably 0.3 mmol / g to 23 mmol / g, more preferably 0.3 mmol / g to 15.0 mmol / g, even more preferably 0.3 mmol / g to 8.5 mmol / g, and particularly preferably 0.3 mmol / g to 5.0 mmol / g. The acid groups and amino groups may be in the form of salts.

[0032] The vinyl (co)polymer (A1) can be produced by a polymerization method known per se, and for example, solution polymerization is preferably used, but is not limited thereto, and bulk polymerization, emulsion polymerization, suspension polymerization, etc. When solution polymerization is carried out, it may be continuous polymerization or batch polymerization, and the monomers may be charged all at once or in portions, or may be added continuously or intermittently.

[0033] The polymerization initiator used in the solution polymerization is not particularly limited, but specific examples thereof include azo compounds such as azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), azobis-2,4-dimethylpaleronitrile, and azobis(4-methoxy-2,4-dimethylpaleronitrile); acetyl peroxide, benzoyl peroxide, lauroyl peroxide, acetylcyclohexylsulfonyl peroxide, and 2,4,4-trimethylpentyl- ... peroxides such as diisopropyl peroxydicarbonate, di-2-ethylhexyl peroxydicarbonate, and diethoxyethyl peroxydicarbonate; perester compounds such as t-butyl peroxyneodecanate, α-cumyl peroxyneodecanate, and t-butyl peroxyneodecanate; and known radical polymerization initiators such as azobisdimethylvaleronitrile and azobismethoxyvaleronitrile can be used.

[0034] The polymerization reaction temperature is not particularly limited, but can usually be set in the range of about 30°C or higher and 200°C or lower.

[0035] The vinyl (co)polymer (A1) obtainable as described above has a degree of polymerization of, for example, 100 or more, preferably 150 or more, and for example, 4,000 or less, preferably 3,000 or less, more preferably 700 or less.

[0036] The weight average molecular weight is, for example, 1,000 or more, preferably 2,000 or more, more preferably 7,000 or more, and for example, 2,000,000 or less, preferably 1,000,000 or less, more preferably 500,000 or less.

[0037] Unless otherwise specified, the weight average molecular weight in this specification is a value obtained by converting the retention time (retention volume) measured using a gel permeation chromatograph (GPC) into the molecular weight of polystyrene using the retention time (retention volume) of a standard polystyrene of known molecular weight measured under the same conditions. Specifically, the gel permeation chromatograph is "HLC8120GPC" (manufactured by Tosoh Corporation, trade name) and four columns, "TSKgel G-4000HXL", "TSKgel G-3000HXL", "TSKgel G-2500HXL" and "TSKgel G-2000HXL" (all manufactured by Tosoh Corporation, trade name), can be measured under the conditions of a mobile phase of tetrahydrofuran, a measurement temperature of 40 ° C, a flow rate of 1 mL / min, and a detector RI.

[0038] After completion of the synthesis, the vinyl (co)polymer (A1) can be converted into a solid or a resin solution in which any solvent has been substituted by removing the solvent and / or replacing the solvent.

[0039] The solvent may be removed by heating at normal pressure or under reduced pressure. The solvent replacement method may involve adding a replacement solvent at any stage before, during, or after the solvent removal.

[0040] In the case of the vinyl (co)polymer (A1), the content of the alkyl group having 12 or more carbon atoms in the dispersion resin (A) is preferably 1 to 100% by mass, more preferably 10 to 90% by mass, even more preferably 20 to 80% by mass, and particularly preferably 30 to 60% by mass, when the total mass of all monomers is taken as 100% by mass. When a compound having a reactive alkyl group having 12 or more carbon atoms is subsequently added to the resin, the content of the alkyl group having 12 or more carbon atoms is calculated based on the mass proportion of the compound.

[0041] When the pigment dispersion resin (A) is converted from a solid state into a resin solution, it is preferable, from the viewpoint of solubility in the solvent, to first mix and dissolve it in a solvent at a liquid temperature of 60°C or higher (preferably 80°C or higher) (the upper limit is 200°C or lower, preferably 100°C or lower) to form a resin solution, and then mix it with other components [components (B), (C), (D), etc.]. The "liquid temperature" refers to the temperature of the solvent or resin solution at the time of dissolution. The solid pigment dispersion resin (A) may be mixed and dissolved in a solvent at 60°C or higher in advance, or the solid pigment dispersion resin (A) and solvent may be mixed and then heated to a temperature of 60°C or higher. The pigment dispersion resin (A) may also contain components other than the pigment dispersion resin (A) and the solvent. The solvents used may be used alone or in combination of two or more, and the types listed below as solvents can be suitably used.

[0042] The solid content of the pigment dispersion resin (A), based on 100% by mass of the total solid content of the carbon nanotube dispersion paste, is, for example, 0.1% by mass or more, preferably 1% by mass or more, more preferably 3% by mass or more, and for example, 40% by mass or less, preferably 30% by mass or less, more preferably 20% by mass or less. Also, the solid content of the pigment dispersion resin (A), based on 100% by mass of the total solid content of the carbon nanotube dispersion paste, is, for example, 0.1% by mass or more, preferably 0.4% by mass or more, more preferably 0.7% by mass or more, and for example, 10% by mass or less, preferably 5% by mass or less, more preferably 2% by mass or less.

[0043] The solid content of the pigment dispersion resin (A) is, based on 100% by mass of the carbon nanotube (B) content, for example, 0.1% by mass or more, preferably 1% by mass or more, more preferably 5% by mass or more, and for example, 150% by mass or less, preferably 120% by mass or less, more preferably 80% by mass or less.

[0044] Carbon nanotubes (B) As the carbon nanotubes (B), single-walled carbon nanotubes or multi-walled carbon nanotubes can be used alone or in combination. In particular, from the viewpoints of viscosity, conductivity, and cost, it is preferable to use multi-walled carbon nanotubes.

[0045] The content of carbon nanotubes (B) is, based on 100% by mass of the total amount of the carbon nanotube dispersion paste, 0.1% by mass or more, for example, 0.2% by mass or more, preferably 0.3% by mass or more, more preferably 0.5% by mass or more, even more preferably 1% by mass or more, and even more preferably 2% by mass or more, and less than 15% by mass, for example, less than 13% by mass, preferably 10% by mass or less, more preferably 7% by mass or less, and even more preferably 6% by mass or less. For example, it can be 0.1% by mass or more and less than 15% by mass, 0.2% by mass or more and less than 13% by mass, 0.3% by mass or more and less than 10% by mass, or 0.5% by mass or more and less than 7% by mass. Furthermore, based on 100% by mass of the total solid content of the carbon nanotube dispersion paste, it is, for example, 5% by mass or more, preferably 10% by mass or more, more preferably 20% by mass or more, and for example, 90% by mass or less, preferably 70% by mass or less, more preferably 50% by mass or less.

[0046] The average outer diameter of the carbon nanotubes (B) is, for example, 1 nm or more, preferably 3 nm or more, more preferably 5 nm or more, and for example, 30 nm or less, preferably 28 nm or less, more preferably 25 nm or less.

[0047] The average length of the carbon nanotubes (B) is, for example, 0.1 μm or more, preferably 1 μm or more, more preferably 5 μm or more, and for example, 100 μm or less, preferably 80 μm or less, more preferably 60 μm or less.

[0048] The BET specific surface area of ​​the carbon nanotubes (B) is usually 100 m 2 / g or more, preferably 130m 2 / g or more, more preferably 160m 2 / g or more, and is usually 800m 2 / g or less, preferably 600m 2 / g or less, more preferably 400m 2 / g or less.

[0049] The BET specific surface area of ​​the present invention can be calculated by the BET method using nitrogen adsorption measurement. Specifically, for example, the BET specific surface area (m 2 / g) can be measured.

[0050] The amount of acidic groups in the carbon nanotubes (B) is, from the viewpoint of dispersibility and storage stability, usually 0.01 mmol / g or more, preferably 0.01 mmol / g or more, and usually 1.0 mmol / g or less, preferably 0.5 mmol / g or less, more preferably 0.2 mmol / g or less, and even more preferably 0.1 mmol / g or less. If the amount of acidic groups is 0.01 mmol / g or more, dispersibility will be good, and if it is 1.0 mmol / g or less, storage stability will be good.

[0051] The acidic groups can be imparted to the carbon nanotubes by the acid treatment described below.

[0052] (Acid Treatment Method) The acid treatment method is not particularly limited as long as it can bring the carbon nanotubes into contact with an acid, but a method in which the carbon nanotubes are immersed in an acid treatment solution (aqueous acid solution) is preferred. The acid contained in the acid treatment solution is not particularly limited, but examples include nitric acid, sulfuric acid, and hydrochloric acid. These can be used alone or in combination of two or more. Among these, nitric acid and sulfuric acid are preferred. The amount of acidic groups in the carbon nanotubes can be adjusted by the concentration, temperature, treatment time, etc. of the acid treatment solution.

[0053] After the acid treatment, excess acid components adhering to the surface can be removed by a washing method described below, thereby obtaining acid-treated carbon nanotubes. The method for washing the acid-treated carbon nanotubes is not particularly limited, but washing with water is preferred. For example, carbon nanotubes are recovered from the acid-treated carbon nanotubes by a known method such as filtration, and then the carbon nanotubes are washed with water. After the washing, if necessary, water adhering to the surface can be removed by drying, thereby obtaining acid-treated carbon nanotubes.

[0054] Furthermore, the volume-equivalent median diameter (D50) of the carbon nanotubes (B), as measured by the method described in the Examples below, is typically 10 μm or more, preferably 15 μm or more, more preferably 20 μm or more, and typically 250 μm or less, preferably 200 μm or less, more preferably 150 μm or less. Here, the median diameter (D50) can be determined by irradiating carbon nanotube particles with laser light and converting the diameter of the carbon nanotubes from the scattered light into a spherical equivalent. A larger median diameter (D50) indicates more carbon nanotube agglomerates and poor dispersibility. If the median diameter (D50) is greater than 250 μm, the likelihood of carbon nanotube agglomerates being present in the electrode increases, resulting in non-uniform conductivity throughout the electrode. On the other hand, if the median diameter (D50) is less than 10 μm, the fiber length is short, resulting in insufficient conductive paths and reduced conductivity. When the median diameter (D50) is within the range of 10 μm or more and 250 μm or less, the carbon nanotubes can be uniformly dispersed in the electrode while maintaining their electrical conductivity.

[0055] In addition, in the Raman spectrum of the carbon nanotube (B), -1 More than 1600cm -1 The maximum peak intensity within the following range is G, 1310 cm -1 More than 1350cm -1 When the maximum peak intensity within the following range is defined as D, the G / D ratio is usually 0.1 or more, preferably 0.4 or more, more preferably 0.6 or more, and is usually 5.0 or less, preferably 3.0 or less, more preferably 1.0 or less.

[0056] Here, it is preferable that the G / D ratio is in the range of 0.1 to 5.0, since there are fewer defects and crystal interfaces on the carbon surface and the conductivity is likely to be high.

[0057] Unlike acetylene black, carbon nanotubes (B) have a fibrous shape and have a high viscosity, so if the content is 15% by mass or more, the viscosity becomes high and handling becomes difficult.

[0058] (Dry Dispersion of Carbon Nanotubes) The carbon nanotubes (B) can be dry-dispersed in advance using a media-type pulverizer before producing a carbon nanotube-dispersed paste. The "dry dispersion" of the present invention refers to pulverization (including disintegration) using a pulverizer at a solids concentration of 80% by mass or more (preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 98% by mass or more). While the carbon nanotubes (B) can be pulverized together with components other than the carbon nanotubes (B), it is preferable that the carbon nanotube (B) content in the solids of the pulverized component is typically 80% by mass or more, preferably 90% by mass or more, more preferably 95% by mass or more, even more preferably 98% by mass or more, and particularly preferably carbon nanotubes (B) alone. As components other than the carbon nanotubes (B) in the pulverized component, solvents, resins, and pigments other than the carbon nanotubes (B) can be suitably used, but it is preferable that the pulverized component essentially contains only the carbon nanotubes (B). The "solid content concentration" mentioned above is the proportion of solid content (mass %) when 1 g of the sample is dried by heating at 130°C for 3 hours.

[0059] The dry dispersion method involves grinding a pigment without adding any liquid components. This allows for direct application of energy to the pigment, enabling highly efficient and powerful grinding (disintegration). Furthermore, the grinding surface is activated and interacts with surrounding materials, resulting in good dispersibility and storage stability in the paste dispersion process described below, and the resulting coating film has excellent conductivity and finish. In the dry dispersion method, grinding is performed using a grinder equipped with grinding media such as glass beads, zirconia beads, or steel balls. Grinding is achieved by utilizing the crushing and destructive forces generated by collisions between grinding media and / or between the grinder and the grinding media. Known grinding devices, such as high-speed impact mills, jet mills, roll mills, attritors, ball mills, vibration mills, and bead mills, can be used.

[0060] During pulverization, various vapors or gases can be blown into the pulverizer to further activate the surface of the carbon nanotubes (B) or adjust the activity. Suitable vapors include acidic or basic compounds, and suitable gases include oxygen, nitrogen, and the like.

[0061] The outer diameter of the grinding media is preferably 0.1 mm to 5 mm, more preferably 0.5 mm to 3 mm. Within this range, a desired grinding force can be obtained, and the pigment can be efficiently ground and disintegrated without excessively destroying the fiber shape of the carbon nanotubes.

[0062] Other conductive pigments (B1) The carbon nanotube dispersion paste used in the present invention can also contain other conductive pigments (B1) other than the carbon nanotubes (B). Examples of other conductive pigments (B1) include at least one conductive carbon selected from the group consisting of acetylene black, ketjen black, furnace black, thermal black, graphene, and graphite. Preferably, the other conductive pigments (B1) are at least one selected from the group consisting of acetylene black, ketjen black, furnace black, and thermal black, more preferably at least one selected from the group consisting of acetylene black and ketjen black, and even more preferably acetylene black.

[0063] The average primary particle diameter of the other conductive pigment (B1) is, for example, 10 nm or more, preferably 20 nm or more, and more preferably, for example, 80 nm or less, preferably 70 nm or less. Here, the average primary particle diameter refers to the average particle diameter of primary particles obtained by observing the conductive pigment (B1) with an electron microscope, determining the projected area of ​​each of 100 particles, determining the diameter of a circle equivalent to that area, and then simply averaging the diameters of the 100 particles. Note that if the pigment is in an aggregated state, the calculation is based on the primary particles that make up the aggregated particles.

[0064] The BET specific surface area of ​​the other conductive pigment (B1) is not particularly limited. 2 / g or more, preferably 10m 2 / g or more, more preferably 20m2 / g or more, for example, 500m 2 / g or less, preferably 250m 2 / g or less, more preferably 200m 2 / g or less.

[0065] The dibutyl phthalate (DBP) oil absorption of the other conductive pigment (B1) is not particularly limited and is, in view of the relationship between pigment dispersibility and conductivity, for example, 60 ml / 100 g or more, preferably 150 ml / 100 g or more, and for example, 1,000 ml / 100 g or less, preferably 800 ml / 100 g or less.

[0066] N-methyl-2-pyrrolidone (C) preferably has a water content of 10,000 ppm or less, and is preferably controlled and adjusted before use so that the water content is below a certain level. Furthermore, from the viewpoints of waste reduction, environmental friendliness, and cost reduction, it is preferable to use a recycled product.

[0067] The water content (upper limit) of N-methyl-2-pyrrolidone (C) is preferably 10,000 ppm or less, more preferably 7,500 ppm or less, even more preferably 5,000 ppm or less, particularly preferably 2,500 ppm or less, and even particularly preferably 1,000 ppm or less. The water content (lower limit) is preferably 100 ppm or more, more preferably 200 ppm or more, and even more preferably 500 ppm or more.

[0068] N-methyl-2-pyrrolidone may contain amine components as impurities generated during production or as unreacted raw materials, and in the carbon nanotube dispersion paste of the present invention, the viscosity or tendency to thicken may vary from lot to lot depending on the amine components as impurities. Furthermore, there is also the problem of odor (work environment), so it is necessary to control the amount of N-methyl-2-pyrrolidone contained in the raw material to a certain level or less.

[0069] Furthermore, when the carbon nanotube dispersion paste of the present invention is applied to an electrode layer by the method described below, the solvent and other components volatilize and do not remain. However, it is preferable to recover and reuse the volatilized solvent to reduce waste, be environmentally friendly, and / or reduce raw material costs. That is, it is preferable to use a recycled product as N-methyl-2-pyrrolidone (C). This recycled solvent (recycled product) will also contain the amine compounds originally contained therein, which will also result in differences in the viscosity or thickening tendency of the paste from lot to lot. Furthermore, amine compounds often have a strong odor.

[0070] Therefore, in this case, it is preferable to control and adjust the amine compound content in the recycled N-methyl-2-pyrrolidone (C) so that it is below a certain level. The amine compound content is preferably 10,000 ppm or less, more preferably 7,500 ppm or less, even more preferably 5,000 ppm or less, particularly preferably 2,500 ppm or less, and even more particularly preferably 1,000 ppm or less. Since the recycled product contains a minimum amount of amine compounds, the lower limit is 1 ppm or more, 5 ppm or more, or 10 ppm or more. The amine compound content can be quantified by general analysis such as ion chromatography-mass spectrometry (IC-MS). The content can be quantified by creating a calibration curve in advance for the peaks of amine species that are expected to be contaminated.

[0071] The above-mentioned "use of recycled products" means that the N-methyl-2-pyrrolidone (C) used in the present invention contains recycled products in an amount of 5% by mass or more (preferably 10% by mass or more, more preferably 30% by mass or more, and even more preferably 50% by mass or more).

[0072] As the recycled product, it is preferable to use a recycled solvent recovered in the process of producing an electrode layer by heating and drying a composite paste, which will be described later.

[0073] Furthermore, from the viewpoint of recyclability, when the boiling point of N-methyl-2-pyrrolidone (C) is (Xc)°C and the boiling point of the amine compound (D) is (Xd)°C, it is preferable that (Xc)-10>(Xd) from the viewpoint of distillation (separation of the amine compound (D)), and it is more preferable that (Xc)-15>(Xd).

[0074] The content of N-methyl-2-pyrrolidone (C) in the carbon nanotube dispersion paste is, for example, 40% by mass or more, preferably 60% by mass or more, more preferably 80% by mass or more, and for example, 99% by mass or less, preferably 98% by mass or less, more preferably 97% by mass or less, based on 100% by mass of the total amount of the carbon nanotube dispersion paste. The solid content of the carbon nanotube dispersion paste is usually 0.1% by mass or more, for example, 1% by mass or more, preferably 2% by mass or more, more preferably 3% by mass or more, and usually less than 80% by mass, for example, 60% by mass or less, preferably 40% by mass or less, more preferably 20% by mass or less, based on 100% by mass of the total amount of the carbon nanotube dispersion paste.

[0075] The carbon nanotube dispersion paste may also contain a solvent other than N-methyl-2-pyrrolidone (C). Specifically, for example, hydrocarbon solvents such as n-butane, n-hexane, n-heptane, n-octane, cyclopentane, cyclohexane, and cyclobutane; aromatic solvents such as toluene and xylene; ketone solvents such as methyl isobutyl ketone; ether solvents such as n-butyl ether, dioxane, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, and diethylene glycol; ethyl acetate, n-butyl acetate, isobutyl acetate, ethylene glycol monomethyl ether, diethylene glycol monoethyl ... Examples of such solvents include ester-based solvents such as glycol monomethyl ether acetate and butyl carbitol acetate; ketone-based solvents such as methyl ethyl ketone, methyl isobutyl ketone and diisobutyl ketone; alcohol-based solvents such as ethanol, isopropanol, n-butanol, sec-butanol and isobutanol; and amide-based solvents such as Equamide (an amide-based solvent, trade name, manufactured by Idemitsu Kosan Co., Ltd.), N,N-dimethylformamide, N,N-dimethylacetamide, N-methylformamide, N-methylacetamide and N-methylpropioamide. These solvents may be used alone or in combination of two or more.

[0076] Amine Compound (D) Examples of the amine compound (D) include ammonia, primary amines, secondary amines, and tertiary amines. The amine compound (D) of the present invention also includes amine compounds present as impurities in the above-mentioned N-methyl-2-pyrrolidone (C) and amine compounds contained in recycled products of N-methyl-2-pyrrolidone (C). Examples of common amine compounds include the following amine compounds:

[0077] Examples of primary amines include ethylamine, n-propylamine, sec-propylamine, n-butylamine, sec-butylamine, i-butylamine, tert-butylamine, pentylamine, hexylamine, heptylamine, octylamine, decylamine, laurylamine, myristyrylamine, 1,2-dimethylhexylamine, 3-pentylamine, 2-ethylhexylamine, allylamine, aminoethanol, 1-aminopropanol, 2-aminopropanol, aminobutanol, aminopentanol, aminohexanol, 3-ethoxypropylamine, 3-propoxypropylamine, 3-isopropoxypropylamine, 3-butoxypropylamine, 3-isobutoxypropylamine, 3-(2-ethylhexyloxy)propylamine, aminocyclopentane, aminocyclohexane, aminonorbornene, aminomethylcyclohexane, aminobenzene, benzylamine, phenethylamine, α-phenylethylamine, naphthylamine, Primary monoamines such as furfurylamine; ethylenediamine, 1,2-diaminopropane, 1,3-diaminopropane, 1,2-diaminobutane, 1,3-diaminobutane, 1,4-diaminobutane, 1,5-diaminopentane, 1,6-diaminohexane, 1,7-diaminoheptane, 1,8-diaminooctane, dimethylaminopropylamine, diethylaminopropylamine, bis-(3-aminopropyl)ether, 1,2-bis-(3-aminopropoxy)ethane, 1,3-bis -(3-aminopropoxy)-2,2'-dimethylpropane, aminoethylethanolamine, 1,2-bisaminocyclohexane, 1,3-bisaminocyclohexane, 1,4-bisaminocyclohexane, 1,3-bisaminomethylcyclohexane, 1,4-bisaminomethylcyclohexane, 1,3-bisaminoethylcyclohexane, 1,4-bisaminoethylcyclohexane, 1,3-bisaminopropylcyclohexane, 1,4-bisaminopropylcyclohexane, hydrogenated 4,4'-Diaminodiphenylmethane, 2-aminopiperidine, 4-aminopiperidine, 2-aminomethylpiperidine, 4-aminomethylpiperidine, 2-aminoethylpiperidine, 4-aminoethylpiperidine, N-aminoethylpiperidine, N-aminopropylpiperidine, N-aminoethylmorpholine, N-aminopropylmorpholine, isophoronediamine, menthanediamine, 1,4-bisaminopropylpiperazine, o-phenylenediamine, m-phenylenediamine, p-phenylenediamine, 2,4-tolylenediamine, 2,6-tolylenediamine, 2,4-toluenediamine, m-aminobenzylamine, 4-chloro-o-phenylenediamine, tetrachloro-p-xylylenediamine, 4-methoxy-6-methyl-m-phenylenediamine, m-xylylenediamine, p-xylylenediamine, 1,5-naphthalenediamine, 2,6-naphthalenediamine, benzidine, 4,4'-bis( o-toluidine), dianisidine, 4,4'-diaminodiphenylmethane, 2,2-(4,4'-diaminodiphenyl)propane, 4,4'-diaminodiphenyl ether, 4,4'-thiodianiline, 4,4'-diaminodiphenyl sulfone, 4,4'-diaminoditolyl sulfone, methylenebis(o-chloroaniline), 3,9-bis(3-aminopropyl)2,4,8,10-tetraoxaspiro[5,5]undecane, diethylenetriamine, Examples of the primary polyamines include iminobispropylamine, methyliminobispropylamine, bis(hexamethylene)triamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, N-aminoethylpiperazine, N-aminopropylpiperazine, 1,4-bis(aminoethylpiperazine), 1,4-bis(aminopropylpiperazine), 2,6-diaminopyridine, and bis(3,4-diaminophenyl)sulfone.

[0078] Examples of secondary amines include diethylamine, dipropylamine, di-n-butylamine, di-sec-butylamine, diisobutylamine, di-n-pentylamine, di-3-pentylamine, dihexylamine, dioctylamine, di(2-ethylhexyl)amine, methylhexylamine, diallylamine, pyrrolidine, piperidine, 2,4-lupethidine, 2,6-lupethidine, 3,5-lupethidine, diphenylamine, Secondary monoamines such as N-methylaniline, N-ethylaniline, dibenzylamine, methylbenzylamine, dinaphthylamine, pyrrole, indoline, indole, and morpholine; N,N'-dimethylethylenediamine, N,N'-dimethyl-1,2-diaminopropane, N,N'-dimethyl-1,3-diaminopropane, N,N'-dimethyl-1,2-diaminobutane, N,N'-dimethyl-1,3-diaminobutane, N,N' -dimethyl-1,4-diaminobutane, N,N'-dimethyl-1,5-diaminopentane, N,N'-dimethyl-1,6-diaminohexane, N,N'-dimethyl-1,7-diaminoheptane, N,N'-diethylethylenediamine, N,N'-diethyl-1,2-diaminopropane, N,N'-diethyl-1,3-diaminopropane, N,N'-diethyl-1,2-diaminobutane, N,N'-diethyl-1,3-diaminobutane and secondary polyamines such as hexane, N,N'-diethyl-1,4-diaminobutane, N,N'-diethyl-1,6-diaminohexane, piperazine, 2-methylpiperazine, 2,5-dimethylpiperazine, 2,6-dimethylpiperazine, homopiperazine, 1,1-di-(4-piperidyl)methane, 1,2-di-(4-piperidyl)ethane, 1,3-di-(4-piperidyl)propane, and 1,4-di-(4-piperidyl)butane.

[0079] Examples of tertiary amines include trimethylamine, triethylamine, tri-n-propylamine, tri-iso-propylamine, tri-1,2-dimethylpropylamine, tri-3-methoxypropylamine, tri-n-butylamine, tri-iso-butylamine, tri-sec-butylamine, tri-pentylamine, tri-3-pentylamine, tri-n-hexylamine, tri-n-octylamine, tri-2-ethylhexylamine, tri-dodecylamine, tri-laurylamine, dicyclohexylethylamine, cyclohexyldiethylamine, tri-cyclohexylamine, N,N-dimethylhexylamine, N-methyldihexylamine, N,N-dimethylcyclohexylamine, N-methyldicyclohexylamine, N,N-diethylethanolamine, N,N-dimethylethanolamine, N-ethyldiethanolamine, triethanolamine, tribenzylamine, N,N-dimethylbenzylamine, diethylbenzylamine, tertiary monoamines such as diphenylamine, triphenylamine, N,N-dimethylamino-p-cresol, N,N-dimethylaminomethylphenol, 2-(N,N-dimethylaminomethyl)phenol, N,N-dimethylaniline, N,N-diethylaniline, pyridine, quinoline, N-methylmorpholine, N-methylpiperidine, 2-(2-dimethylaminoethoxy)-4-methyl-1,3,2-dioxabornane, and 2-, 3-, and 4-picoline; tetramethylethylenediamine , pyrazine, N,N'-dimethylpiperazine, N,N'-bis((2-hydroxy)propyl)piperazine, hexamethylenetetramine, N,N,N',N'-tetramethyl-1,3-butanamine, 2-dimethylamino-2-hydroxypropane, diethylaminoethanol, N,N,N-tris(3-dimethylaminopropyl)amine, 2,4,6-tris(N,N-dimethylaminomethyl)phenol, heptamethylisobiguanide, and other tertiary polyamines.

[0080] These can be used alone or in combination of two or more. Here, the amine compound (D) that can be used in the present invention is an amine compound that is within the range of (Xc)-10>(Xd), where the boiling point of N-methyl-2-pyrrolidone (C) is (Xc)°C and the boiling point of amine compound (D) is (Xd)°C. However, an amine compound outside this range can also be used together with amine compound (D).

[0081] Of these, primary amine compounds are preferred, and monoamine compounds (monoamines) are more preferred.

[0082] Examples of the amine compound (D) include alkanolamines, aliphatic amines, alicyclic amines, and aromatic amines, and any of these can be suitably used, with aromatic amines being preferred.

[0083] Since it is preferable that no amine compound (D) remains in the electrode layer after drying, the weight-average molecular weight of the amine compound (D) is preferably less than 1,000, more preferably 800 or less, even more preferably 500 or less, particularly preferably 350 or less, and even more particularly preferably 250 or less. Furthermore, if the boiling point is low, there is a possibility that the compound will volatilize during production or storage, and furthermore, from the viewpoint of odor, the lower limit of the boiling point is preferably 50°C or higher, more preferably 100°C or higher.

[0084] The amine value of the amine compound (D) is usually 5 mgKOH / g or more, preferably 50 mgKOH / g or more, more preferably 105 mgKOH / g or more, and is usually within the range of 1,000 mgKOH / g or less.

[0085] The inclusion of an amine compound (D) improves pigment dispersibility and storage stability, but many of them have a strong odor, which can worsen the working environment during blending or the drying process. Furthermore, since they are generally expensive, this can increase costs. Furthermore, for the sake of recyclability, which will be described later, the content must be kept to the minimum necessary.

[0086] The content of the amine compound (D) is, for example, 0.01% by mass or more, preferably 0.05% by mass or more, and more preferably 0.1% by mass or more, based on 100% by mass of the total amount of the carbon nanotube dispersion paste, and is, for example, 10% by mass or less, preferably 5% by mass or less, and more preferably 1% by mass or less.

[0087] Furthermore, based on 100% by mass of the solid content of the carbon nanotubes (B), the lower limit is, for example, 1% by mass or more, preferably 2% by mass or more, and more preferably 5% by mass or more. The upper limit is, for example, 500% by mass or less, preferably 50% by mass or less, and more preferably 15% by mass or less. Based on 100% by mass of the solid content of the carbon nanotube dispersion paste, the content is, for example, 1% by mass or more, preferably 1.5% by mass or more, and more preferably 2% by mass or more, and for example, 600% by mass or less, preferably 300% by mass or less, and more preferably 50% by mass or less.

[0088] Polyvinylidene fluoride (E) The carbon nanotube dispersion paste that can be used in the present invention preferably contains polyvinylidene fluoride (E), which is an essential component of the composite paste described below.

[0089] The polyvinylidene fluoride (E) is a resin intended for forming a film of the electrode layer, and may be variously modified. From the viewpoint of adhesion to the substrate, it preferably has a polar functional group.

[0090] The weight average molecular weight of the polyvinylidene fluoride (E) is, from the viewpoints of adhesion to the substrate, reinforcement of the film properties, and solvent resistance, for example, 100,000 or more, preferably 500,000 or more, more preferably 650,000 or more, and for example, 3,000,000 or less, preferably 2,000,000 or less.

[0091] The content of polyvinylidene fluoride (E) is, for example, 10.0% by mass or more, preferably 30.0% by mass or more, more preferably 40.0% by mass or more, and for example, 99.0% by mass or less, preferably 80.0% by mass or less, more preferably 60.0% by mass or less, based on 100% by mass of the solid content of the carbon nanotube dispersion paste. Also, for example, 0.1% by mass or more, preferably 0.5% by mass or more, more preferably 1% by mass or more, and for example, 10% by mass or less, preferably 7% by mass or less, more preferably 5% by mass or less, based on 100% by mass of the total amount of the carbon nanotube dispersion paste.

[0092] When the polyvinylidene fluoride (E) is converted from a solid state into a resin solution, it is preferably mixed and dissolved in a solvent having a liquid temperature of 40°C or higher (preferably 60°C or higher, more preferably 80°C or higher) (the upper limit is 200°C or lower, preferably 100°C or lower) in advance to form a resin solution, from the viewpoint of solubility in the solvent. After the resin solution is formed, it is preferably mixed with other components [components (A), (B), (C), etc.]. Note that the "liquid temperature" refers to the temperature of the solvent or resin solution at the time of dissolution. Solid polyvinylidene fluoride (E) may be mixed and dissolved in a solvent having a temperature of 40°C or higher in advance, or solid polyvinylidene fluoride (E) may be mixed with a solvent and then heated to a temperature of 40°C or higher. In addition, components other than polyvinylidene fluoride (E) and the solvent may be contained. The solvent used may be one type alone or two or more types in combination, and any solvent that dissolves polyvinylidene fluoride (E) may be suitably used, with N-methyl-2-pyrrolidone (C) being preferred. Furthermore, it is preferable to cool the resin solution obtained by heat dissolution as described above to a predetermined temperature of 10°C or higher and lower than 40°C, and in this cooling step, it is preferable that the cooling rate, defined by the following formula: cooling rate = (solution temperature at the start of cooling - solution temperature at the end of cooling) / cooling time, is 0.5°C / min or higher (preferably 1°C / min or higher) from the viewpoint of preventing precipitation.

[0093] Mixing and Dispersion In the manufacturing method of the present invention, the mixing and dispersing step is a step of mixing and further dispersing components containing at least the pigment dispersion resin (A), the carbon nanotubes (B), N-methyl-2-pyrrolidone (C), and the amine compound (D), and a liquid carbon nanotube dispersion paste can be obtained.

[0094] The upper limit of the solid content of the carbon nanotube dispersion paste is usually less than 80% by mass, preferably less than 50% by mass, more preferably less than 20% by mass, and even more preferably less than 10% by mass. The lower limit is usually 0.1% by mass or more, preferably 0.5% by mass or more, more preferably 1% by mass or more, and even more preferably 2% by mass or more.

[0095] In the mixing and dispersing step, the components can be uniformly mixed and dispersed using a conventional dispersing machine, such as a paint shaker, sand mill, ball mill, pebble mill, LMZ mill, DCP pearl mill, planetary ball mill, homogenizer, twin-screw kneader, or thin-film rotary high-speed mixer (manufactured by Filmix, trade name "Clearmix," etc.). The order in which the components are mixed is not particularly limited. The mixing and dispersing step preferably includes the following steps, sequentially: Step 1: Adding a component containing carbon nanotubes (B) in an amount of 70% by mass or less (preferably 50% by mass or less), based on 100% by mass of the total amount of carbon nanotubes (B) contained in the carbon nanotube-dispersed paste obtained after dispersion, to the dispersing machine, and performing a dispersion treatment; and Step 2: Adding carbon nanotubes (B) to the dispersing machine until the desired concentration is reached, and performing a dispersion treatment. The dispersion treatment time in Step 1 is preferably at least 30 seconds or more (preferably 1 minute or more). By carrying out the above-mentioned mixing and dispersion, aggregation of the carbon nanotubes (B) is alleviated, and a homogeneous paste with good dispersibility is obtained even in a highly concentrated paste, and the resulting battery electrode layer (coating film) has excellent finish, conductivity, battery performance, etc.

[0096] Other Components The carbon nanotube dispersion paste may further contain other components in addition to the above-mentioned components (A), (B), (C), and (D) and the component (E) which may be contained as needed.

[0097] Examples of other components include resins other than the pigment-dispersing resin (A) and polyvinylidene fluoride (E), neutralizing agents, antifoaming agents, preservatives, rust inhibitors, plasticizers, pigments other than the carbon nanotubes (B), and dehydrating agents (F).

[0098] Examples of pigments other than carbon nanotubes (B) include the aforementioned other conductive pigments (B1); white pigments such as titanium white and zinc oxide; blue pigments such as cyanine blue and indanthrene blue; green pigments such as cyanine green and verdigris; organic red pigments such as azo-based and quinacridone-based pigments, red pigments such as red iron oxide; organic yellow pigments such as benzimidazolone-based, isoindolinone-based, isoindoline-based, and quinophthalone-based pigments; and yellow pigments such as titanium yellow and yellow lead. These pigments can be used alone or in combination of two or more. These pigments other than carbon nanotubes (B) can be used for purposes such as color adjustment and film property reinforcement, as long as they do not significantly impair conductivity. They may be dispersed simultaneously with the pigment dispersion resin (A) and the carbon nanotubes (B), or they may be dispersed in the pigment dispersion resin (A) and the carbon nanotubes (B) to form a paste and then mixed as a pigment or pigment paste.

[0099] The content of pigments other than the carbon nanotubes (B) is preferably 10 mass % or less, more preferably 5 mass % or less, and even more preferably 1 mass % or less, based on 100 mass % of all pigments in the carbon nanotube dispersion paste, and it is particularly preferable that they are substantially not contained.

[0100] The viscosity of the carbon nanotube dispersion paste is determined from the viewpoint of pigment dispersibility and storage stability, and is set to a value of 2 s -1The viscosity at 1000 kJ / min is, for example, less than 5,000 mPa s, preferably less than 2,500 mPa s, and more preferably less than 1,000 mPa s, and is, for example, 10 mPa s or more, preferably 50 mPa s or more, and more preferably 100 mPa s or more. The viscosity can be measured using, for example, a cone and plate viscometer (manufactured by HAAKE, trade name "Mars2", diameter 35 mm, 2° inclined cone and plate).

[0101] The dehydrating agent (F) may be any known agent having a dehydrating effect, without any particular limitation. It may be a solid dehydrating agent that is insoluble in the solvent of the paste, or a dehydrating agent that dissolves in the solvent. Specific examples include solid dehydrating agents such as zeolite, silica gel, calcium oxide, molecular sieve, activated alumina, barium oxide, calcium hydride, and sodium sulfate; phosphate esters such as trimethyl phosphate, tri-2-propyl phosphate, tributyl phosphate, and tetraisopropylethylene phosphonate; phosphine oxides such as tributylphosphine oxide, trioctylphosphine oxide, and triphenylphosphine oxide; orthoformic acid methyl ester, orthoformic acid ethyl ester. orthoesters such as oxalic anhydride, methyl orthoacetate, ethyl orthoacetate, and ethyl orthobenzoate; and acid anhydrides such as oxalic anhydride, acetic anhydride, propionic anhydride, butyric anhydride, benzoic anhydride, trifluoroacetic anhydride, disulfuric acid, dinitrogen pentoxide, diphosphoric acid, diphosphorus pentoxide, diphosphorus trioxide, diarsenic pentoxide, diarsenic trioxide, methanesulfonic anhydride, trifluoromethanesulfonic anhydride, and sulfobenzoic anhydride, and these may be used alone or in combination of two or more.

[0102] [Method for Producing a Composite Paste (for Lithium-ion Secondary Batteries)] In the production method of the present invention, first, a carbon nanotube-dispersed paste containing carbon nanotubes (B) is prepared by the method described above. The carbon nanotube-dispersed paste and at least one electrode active material (G) are further mixed to produce a composite paste (for lithium-ion secondary batteries).

[0103] The solid content of the electrode active material (G) is usually 10% by mass or more, preferably 20% by mass or more, and usually 99% by mass or less, preferably 95% by mass or less, based on 100% by mass of the total amount of the composite paste. This is suitable from the standpoint of battery performance. Polyvinylidene fluoride (E), which was an optional component in the carbon nanotube dispersion paste, is an essential component in the composite paste and is always contained. The solid content of polyvinylidene fluoride (E), based on 100% by mass of the total amount of the composite paste, is usually 0.05% by mass or more, preferably 0.1% by mass or more, and usually 10% by mass or less, preferably 2% by mass or less. This is suitable from the standpoint of battery performance, paste viscosity, etc.

[0104] In the above-mentioned step of mixing the electrode active material (G), the composite paste can be mixed uniformly using a conventionally known mixer and disperser.

[0105] The solid content of the pigment dispersion resin (A) in the solid content of the composite paste is usually 0.01% by mass or more, preferably 0.05% by mass or more, based on 100% by mass of the total amount of the composite paste, and is usually 10% by mass or less, preferably 1% by mass or less, which is suitable from the viewpoints of battery performance, paste viscosity, etc.

[0106] In the composite paste of the present invention, from the viewpoint of storage stability (suppression of thickening) of the composite paste, it is preferable to include a sequence of first mixing the carbon nanotubes (B) with the amine compound (D), by bringing the amine compound (D) into contact with (wetting) the carbon nanotubes (B), and then mixing the electrode active material (G), thereby alleviating aggregation between the carbon nanotubes (B) and the electrode active material (G).

[0107] The solid content of carbon nanotubes (B) in the solid content of the composite paste of the present invention is, based on 100% by mass of the total amount of the composite paste, usually 0.01% by mass or more, preferably 0.05% by mass or more, more preferably 0.1% by mass or more, and usually 30% by mass or less, preferably 10% by mass or less, more preferably 5% by mass or less. This is suitable from the viewpoint of battery performance. Further, the content of N-methyl-2-pyrrolidone (C) in the composite paste of the present invention is, based on 100% by mass of the total amount of the composite paste, usually 1% by mass or more, preferably 4% by mass or more, more preferably 7% by mass or more, and usually 90% by mass or less, preferably 70% by mass or less, more preferably 50% by mass or less. This is suitable from the viewpoint of electrode drying efficiency and paste viscosity.

[0108] The composite paste is suitable for use as a positive or negative electrode for a lithium ion secondary battery, and is preferably used as a positive electrode.

[0109] In addition, the moisture content of the composite paste is usually 10,000 ppm or less, preferably 7,500 ppm or less, more preferably 5,000 ppm or less, even more preferably 2,500 ppm or less, and particularly preferably 1,000 ppm or less, from the viewpoint of suppressing the increase in viscosity or gelation of the composite paste. The composite paste used in the present invention can be said to be substantially a non-aqueous composite paste. Furthermore, for the reasons described above (moisture carried over from raw materials or moisture contamination during the manufacturing process), the moisture content of the composite paste is preferably 100 ppm or more, more preferably 200 ppm or more, and even more preferably 500 ppm or more.

[0110] Electrode active material (G) Examples of the electrode active material (G) include lithium nickel oxide (LiNiO 2 ), lithium manganese oxide (LiMn 2 O 4 ), lithium cobalt oxide (LiCoO 2 ), LiNi 1/3 Co 1/3 Mn 1/3 O 2 lithium composite oxides such as lithium iron phosphate (LiFePO 4), sodium composite oxide, potassium composite oxide, etc. These electrode active materials (G) can be used singly or in combination of two or more. The electrode active material containing lithium iron phosphate is inexpensive and has relatively good cycle characteristics and energy density, and therefore can be suitably used.

[0111] The particle size of the electrode active material is usually 0.5 μm or more, preferably 10.5 μm or more, and usually 30 μm or less, preferably 20 μm or less.

[0112] The solid content of the electrode active material (G) in 100% by mass of the solid content of the composite paste for a lithium ion secondary battery electrode of the present invention is usually 50% by mass or more, preferably 60% by mass or more, and is preferably less than 100% by mass in terms of battery capacity, battery resistance, etc.

[0113] When the electrode active material (G) is contained in the composite paste, the paste may thicken during storage. The reason for this is that the electrode active material (G) has alkali metal hydroxides (e.g., LiOH, KOH, NaOH, etc.) derived from the raw materials on the particle surface, which is thought to cause aggregation (thickening) due to the conductive pigment having an acidic surface. Therefore, by containing a certain amount or more of the amine compound (D), the thickening of the composite paste during storage can be suppressed.

[0114] Furthermore, the water content contained in the electrode active material (G) is usually 10,000 ppm or less, preferably 7,500 ppm or less, more preferably 5,000 ppm or less, even more preferably 2,500 ppm or less, and particularly preferably 1,000 ppm or less, from the viewpoint of suppressing an increase in viscosity or gelation of the composite paste described above.

[0115] Furthermore, the electrode active material (G) of the present invention can be suitably used as an electrode active material composite (G-1) in which at least a portion of its surface is covered with carbon nanotubes. The composite (G-1) can be obtained by previously mixing the electrode active material (G), carbon nanotubes, and, if necessary, other components (e.g., a solvent or a dispersion resin). If necessary, a drying step can be performed after mixing, thereby enabling the carbon nanotubes to be more uniformly adsorbed and / or fixed to the electrode active material (G). Furthermore, the electrode active material composite (G-1) produced as described above can form a uniform conductive network around the electrode active material by adsorbing and / or fixing the carbon nanotubes to the surface of the electrode active material. As the carbon nanotubes that can be used in the electrode active material composite (G-1), any known carbon nanotubes can be used without particular limitation, but the carbon nanotubes listed for the carbon nanotubes (B) can be suitably used.

[0116] As described above, an electrode layer for a lithium ion secondary battery (also referred to as an electrode mixture layer or a mixture layer) can be produced by applying a mixture paste for a lithium ion secondary battery to the surface of a core material (current collector) of a positive electrode or a negative electrode and drying the applied paste, and is particularly preferably used for a positive electrode.

[0117] In addition, the carbon nanotube dispersion paste obtained by the manufacturing method of the present invention can be used not only as a paste for a composite layer (electrode layer), but also as a primer layer (also referred to as a functional layer or adhesive layer) between an electrode core material and a composite layer (electrode layer). The lithium ion secondary battery composite paste can be applied by a known method using a die coater or the like. The amount of application of the lithium ion secondary battery composite paste is not particularly limited, but can be set so that the thickness of the composite layer after drying is, for example, 0.04 mm or more, preferably 0.06 mm or more, and, for example, 0.30 mm or less, preferably 0.24 mm or less. The temperature of the drying step can be appropriately set, for example, 80°C or more, preferably 100°C or more, and, for example, 250°C or less, preferably 200°C or less. The drying step time can be appropriately set, for example, 5 seconds or more, and, for example, 120 minutes or less, preferably 60 minutes or less.

[0118] In the drying step, all or a part of N-methyl-2-pyrrolidone (C) and amine compound (D) volatilize. As described above, in order to reduce waste, be environmentally friendly, and / or reduce costs, it is preferable to recover and reuse the volatilized components (C) and (D).

[0119] Furthermore, in lithium-ion secondary batteries, the presence of impurities such as moisture in the electrode layer reduces the cycle life. That is, if the carbon nanotube dispersion paste or composite paste contains more moisture than specified, or if the electrode layer is not sufficiently dried during the manufacturing process, moisture remains in the electrode layer, causing deterioration of the battery's cycle characteristics. The moisture content in the electrode layer is usually less than 1000 ppm, preferably less than 750 ppm, more preferably less than 500 ppm, even more preferably less than 250 ppm, and particularly preferably less than 100 ppm.

[0120] As described above, when the composite paste is applied to a current collector and dried by heating, it is preferable to recover vapor containing N-methyl-2-pyrrolidone (C) and the amine compound (D), etc., to produce a mixed solution, and then distill it to remove and separate as many impurities as possible other than N-methyl-2-pyrrolidone (C), thereby producing a recycled N-methyl-2-pyrrolidone (C). The moisture content and amine compound amount of the recycled N-methyl-2-pyrrolidone (C) are as described above, and are preferably controlled and adjusted to a certain level or less. Furthermore, it is desirable that components other than moisture and the amine compound are contained as little as possible. In this sense, the purity is at least 99.0% or more, preferably 99.9% or more, and more preferably 99.95% or more.

[0121] The method for removing and separating impurities to produce the above-mentioned recycled product can be carried out by a method known per se, such as the method disclosed in JP-A-10-310795 (specifically, filtration, distillation, contact with an acidic substance, etc.). These methods can be carried out singly or in combination of two or more, and can be repeated multiple times.

[0122] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these specific embodiments. In each example, "parts" means parts by mass and "%" means % by mass.

[0123] [Preparation of Dispersion Resin] Preparation Example 1: A reaction vessel equipped with a thermometer, thermostat, stirrer, reflux condenser, and water separator was charged with 75 parts of N-methyl-2-pyrrolidone (Note 1) and heated to 120°C in a nitrogen stream. Once the temperature reached 120°C, a mixture of the monomer species shown in Table 1 below (100 parts in total) and 2 parts of 2,2'-azobis(2-methylbutyronitrile) was added dropwise over 3 hours. After the addition was completed, the mixture was aged at 120°C for 30 minutes, and then a mixture of 1 part of 2,2'-azobis(2-methylbutyronitrile) and 20 parts of N-methyl-2-pyrrolidone (Note 1) was added dropwise over 1 hour. After further aging at 120°C for 1 hour, the mixture was cooled, and N-methyl-2-pyrrolidone (Note 1) was added to obtain an acrylic resin (A1) with a solids content of 50%. The polar functional group concentration was 1.3 (mmol / g). (Note 1) N-methyl-2-pyrrolidone: A solvent made by mixing new material with the recycled material produced in Application Example 1C in a 1:1 ratio, with a water content of 500 ppm (Note 2) and an amine content of 500 ppm (Note 2). (Note 2) The water content and amine content were measured using a Karl Fischer moisture meter (Kyoto Electronics Manufacturing Co., Ltd., product name "MKC-610") and an ion chromatograph (Shimadzu Corporation, product name "Prominence HIC-NS").

[0124] Production Example 2 Acrylic resin (A2) with a solids content of 50% was obtained in the same manner as in Production Example 1, except that the monomer species shown in Table 1 below were used. The weight-average molecular weight of the obtained resin is shown in Table 1 below. In the table, "resin A1" means acrylic resin (A1), and "resin A2" means acrylic resin (A2).

[0125]

[0126] The abbreviations for the monomer species in Table 1 above are as follows: iBA: i-butyl acrylate (having a hydrocarbon group with 4 carbon atoms) BEMA: behenyl methacrylate (having a hydrocarbon group with 22 carbon atoms) St: styrene DMAEMA: N,N-dimethylaminoethyl methacrylate.

[0127] [Production of Carbon Nanotube Dispersion Paste and Composite Paste] Example 1A Using a continuous dry bead mill "Drystar SDA1" (manufactured by Ashizawa Finetech Co., Ltd.), carbon nanotubes (CNT1 (Table 2)) were pulverized at a feed rate of 0.5 kg / hr using zirconia beads (diameter 3.0 mm), a filling rate of 70%, and a mill peripheral speed of 5.0 m / s. Next, 5,000 parts of N-methyl-2-pyrrolidone (Note 1), 200 parts of the above-mentioned crushed carbon nanotubes, 80 parts of polyvinylpyrrolidone as a dispersion resin (40 parts solids) (Note 3), 1,800 parts of a resin solution of KF Polymer W#7300 (manufactured by Kureha Corporation, trade name, polyvinylidene fluoride, weight average molecular weight 1,000,000) (180 parts solids) (Note 4), and 25 parts of benzylamine as an amine were mixed while stirring, and finally adjusted to a total mass of 10,000 parts with N-methyl-2-pyrrolidone (Note 1). Subsequently, the mixture was dispersed in a ball mill for 4 hours to produce a carbon nanotube dispersion paste (A-1). The water content of the carbon nanotube dispersion paste (A-1) was 800 ppm (Note 2). (Note 3) Polyvinylpyrrolidone: heterocycle-containing resin, weight-average molecular weight (Mw) 12,000, functional group concentration 9 (mmol / g) (Note 4) To prepare the polyvinylidene fluoride resin solution, polyvinylidene fluoride and N-methyl-2-pyrrolidone (Note 1) were mixed and dissolved at a temperature of 80°C in advance, and then cooled to 30°C at a cooling rate of approximately 1°C / min.

[0128]

[0129] The carbon nanotubes are multi-walled carbon nanotubes. The median diameter (D50), G / D ratio, specific surface area (BET specific surface area), and amount of acidic groups in Table 2 were measured by the methods described below.

[0130] Examples 2A to 5A, Comparative Examples 1A to 4A Carbon nanotube dispersion pastes (A-2) to (A-9) were obtained in the same manner as in Example 1A, except that the dispersion resin, carbon nanotubes (CNT), amine, and N-methyl-2-pyrrolidone were used as shown in Table 3 below and in the formulations shown in Table 3. Example 3A (carbon nanotube dispersion paste (A-3)) uses carbon nanotubes (CNT1) that have not been crushed (dry dispersed). Comparative Example 3A (carbon nanotube dispersion paste (A-8)) uses only new, non-recycled N-methyl-2-pyrrolidone (water content of 100 ppm or less, amine content of 100 ppm or less). The water content (Note 2) of the carbon nanotube dispersion paste and the results of the evaluation test described below are also shown in Table 3 below.

[0131]

[0132] The blending amount of the dispersing resin in Table 3 above is the value of the solid content. The composition of the dispersing resin (polymethyl methacrylate) in Table 3 above is as follows: Polymethyl methacrylate: weight average molecular weight 20,000, homopolymer of methyl methacrylate, polar functional group concentration 0 (mmol / g) The boiling points and molecular weights of the solvents and amine compounds in Table 3 above are as follows: N-methyl-2-pyrrolidone: 202°C, molecular weight 99 Benzylamine: boiling point 185°C, molecular weight 107 Aminomethylpropanol: boiling point 166°C, molecular weight 89 Phenylethylamine: 195°C, molecular weight 121 Diethanolamine: 217°C, molecular weight 105.

[0133] Examples 6A to 9A Water was added to the carbon nanotube dispersion paste (A-2) (water content: 800 ppm) obtained in Example 2A so that the water content was as follows (Note 2), and the mixture was thoroughly stirred to obtain the following carbon nanotube dispersion pastes (A-10) to (A-13). The dispersibility evaluation results of the carbon nanotube dispersion pastes are shown in Table 5 below. Example 6A: Carbon nanotube dispersion paste (A-10), water content: 2,000 ppm Example 7A: Carbon nanotube dispersion paste (A-11), water content: 4,000 ppm Example 8A: Carbon nanotube dispersion paste (A-12), water content: 8,000 ppm Example 9A: Carbon nanotube dispersion paste (A-13), water content: 12,000 ppm

[0134] Example 1B 100 parts of the carbon nanotube dispersion paste (A-1) were mixed with electrode active material particles (composition formula LiNi 0.5 Mn 1.5 O 4 Lithium nickel manganese oxide particles with a spinel structure represented by the formula (I), an average particle diameter of 6 μm, and a BET specific surface area of ​​0.7 m 2 900 parts of the cellulose acylate stearate (100 ppm) was mixed with a disperser to prepare a composite paste (B-1). The composite paste (B-1) had a moisture content of 800 ppm (Note 2).

[0135] Examples 2B to 5B, Comparative Examples 1B to 4B Composite pastes (B-2) to (B-9) were obtained in the same manner as in Example 1B except for the formulations shown in Table 4 below. The results of the evaluation tests of the composite pastes described below are also shown in Table 3 above.

[0136]

[0137] Examples 6B to 9B Composite pastes (B-10) to (B-13) were obtained in the same manner as in Example 1B except for the formulations shown in Table 5 below. The results of evaluating the storage stability of the composite pastes are also shown in Table 5 below.

[0138]

[0139] <Median diameter (D50)> The median diameter (D50) was measured using a laser diffraction / scattering particle size distribution analyzer "LA-960" (trade name, manufactured by HORIBA) according to the following procedure.

[0140] (Preparation of aqueous dispersion medium) 0.10 g of F10MC (trade name, manufactured by Nippon Paper Industries Co., Ltd., carboxymethyl cellulose sodium (hereinafter also referred to as CMCNa)) was added to 100 mL of distilled water, and the mixture was stirred at room temperature for 24 hours or more to dissolve, thereby preparing an aqueous dispersion medium containing 0.1 mass % CMCNa.

[0141] (Preparation of CMCNa Aqueous Solution) 2.0 g of F10MC (trade name, carboxymethylcellulose sodium, manufactured by Nippon Paper Industries Co., Ltd.) was added to 100 mL of distilled water and dissolved by stirring at room temperature for 24 hours or more to prepare a 2.0 mass % aqueous solution of CMCNa.

[0142] (Pre-treatment for measurement) 6.0 mg of carbon nanotubes were weighed into a vial, and 6.0 g of the aqueous dispersion medium was added. An ultrasonic homogenizer (Microtec Nichion Corporation, "SmurtNR-50") was used for the pre-treatment for measurement. The tip was confirmed to be free of deterioration, and the tip was adjusted so that it was immersed 10 mm or more below the surface of the sample being treated. A carbon nanotube aqueous dispersion was prepared by homogenizing the solution through ultrasonic irradiation using auto-power operation with a constant output power, with a time set (irradiation time) of 40 seconds, a power set of 50%, and a start power of 50% (output 50%).

[0143] [Measurement] <Proportion of Dispersed Carbon Nanotube Particles of 1 μm or Less and Median Diameter (D50)> Using the carbon nanotube aqueous dispersion, the proportion of dispersed carbon nanotube particles of 1 μm or less and the median diameter (D50) were measured according to the following method. The optical model of the LS 13 320 Universal Liquid Module was set to a refractive index of 1.520 for carbon nanotubes and 1.333 for water. After module cleaning, the module was filled with approximately 1.0 mL of CMCNa aqueous solution. After performing offset measurement, optical axis adjustment, and background measurement at a pump speed of 50%, the prepared carbon nanotube aqueous dispersion was added to a particle size distribution analyzer so that the relative concentration (RIDS), which indicates the percentage of light scattered outside the beam by particles, was 8-12% or the PIDS was 40-55%. The dispersion was then subjected to ultrasonic irradiation at 78 W for 2 minutes (measurement pretreatment) using the particle size distribution analyzer accessory. After circulating for 30 seconds to remove air bubbles, the particle size distribution was measured. A graph of particle size (particle diameter) versus volume % was obtained, and the proportion of dispersed particles of 1 μm or less and the median diameter (D50) were determined. For each carbon nanotube sample, three measurement samples were collected from different locations, and particle size distribution measurements were performed. The proportion of dispersed particles of 1 μm or less and the median diameter (D50) were calculated as the average values.

[0144] <G / D ratio of carbon nanotubes> The Raman spectrum of the carbon nanotubes was measured by placing the carbon nanotubes in a Raman microscope (manufactured by Horiba, Ltd., product name "XploRA") and using a laser wavelength of 532 nm. -1 More than 1600cm -1 The maximum peak intensity within the following range is G, 1310 cm -1 More than 1350cm -1 The G / D ratio of the carbon nanotube was determined by setting the maximum peak intensity within the following range as D.

[0145] <Specific surface area (BET specific surface area)> The BET specific surface area of ​​the carbon nanotubes was measured in accordance with JIS Z8830:2013 using a specific surface area measuring device (BERSORP-MAX (Microtrac Bell Co., Ltd.)).2 / g) was measured.

[0146] <Amount of Acidic Groups in Carbon Nanotubes (CNT)> 2 g of CNT was precisely weighed out, immersed in 50 ml of a 0.01 M benzylamine / n-methylpyrrolidone solution, and dispersed for 1 hour using an ultrasonic irradiator. The solution was then centrifuged, and the supernatant was filtered. The benzylamine remaining in the resulting filtrate was quantitatively analyzed by potentiometric titration with 0.1 M hydrochloric acid, and the amount of acidic groups (mmol / g) per 1 g of the resulting CNT was determined.

[0147] Evaluation Tests Evaluation tests were carried out on the carbon nanotube dispersion pastes and composite pastes obtained in the above Examples and Comparative Examples. If even one evaluation result was unacceptable, the evaluation was deemed unacceptable.

[0148] <Dispersibility> The dispersibility of the obtained carbon nanotube dispersion paste was evaluated using a particle gauge according to the dispersibility test of JIS K-5600-2-5, based on the following criteria: E is unacceptable. A: The pigment is dispersed at less than 10 μm. Dispersibility is very good. B: The pigment is dispersed at 10 μm or more and less than 20 μm. Dispersibility is somewhat good. C: The pigment is dispersed at 20 μm or more, but no agglomerates are visible to the naked eye. Dispersibility is normal. D: Some agglomerates are visible to the naked eye. Dispersibility is somewhat poor. E: Many large agglomerates are visible to the naked eye. Dispersibility is very poor.

[0149] <Storage Stability> The obtained composite paste was stored at a temperature of 50°C for 2 weeks, and the initial viscosity and the viscosity after storage were compared. The viscosity was measured using a cone and plate viscometer (manufactured by HAAKE, product name "Mars2", diameter 35 mm, cone and plate tilted at 2°) at a shear rate of 2.0 s -1The viscosity increase rate was calculated using the following formula and storage stability was evaluated according to the following criteria. D is a failure. Viscosity increase rate (%) = viscosity after storage (mPa s) / initial viscosity (mPa s) × 100 - 100 A: The viscosity increase rate (%) after storage is less than 20%. B: The viscosity increase rate (%) after storage is 20% or more and less than 100%. C: The viscosity increase rate (%) after storage is 100% or more and less than 300%. D: The viscosity increase rate (%) after storage is 300% or more (or gelation makes it impossible to measure).

[0150] <Recyclability> A solution was prepared using the composite paste compositions of the Examples and Comparative Examples, excluding the resin components (dispersion resin and polyvinylidene fluoride) and pigment components (CNT and active material). Subsequently, 100 g of the solution was placed in an open container equipped with a thermometer, thermostat, and stirrer. The container was heated to 200±2°C while stirring, and distilled until the solution was 95 g, producing a recycled N-methyl-2-pyrrolidone product. The amine content (Note 2) was measured, and the recyclability of the solvent was evaluated according to the following criteria. B and C were unsuccessful. A: The amine content in the solution was 1000 ppm or less. B: The amine content in the solution was greater than 1000 ppm and less than 2500 ppm. C: The amine content in the solution was greater than 2500 ppm.

[0151] [Production of Battery Electrode Layer] Application Examples 1C to 5C The composite pastes obtained in Examples 1B to 5B were applied to both sides of a long aluminum foil (positive electrode current collector) having an average thickness of 15 μm, with a basis weight per side of 10 mg / cm 2 The positive electrode layer was formed by applying the mixture in a strip shape by a roller coating method so that the solid content was 100% (based on the solid content) and drying (drying temperature 200°C, 30 minutes). The positive electrode active material layer (positive electrode layer) supported on the positive electrode current collector was rolled using a roll press to adjust the properties. The resulting electrode layer had a residual solvent content of less than 1% and was an electrode layer with good finish.

[0152] In addition, the vapor evaporated during the heating and drying process in the above step was recovered to obtain a recovered solution (mixed solution). Next, the mixed solution was placed in a flask equipped with a condenser, and the flask was heated to 185°C or higher to distill off the amine. This was continued until the amine content reached 1,000 ppm (Note 2), producing a recycled N-methyl-2-pyrrolidone product. The water content of the recycled N-methyl-2-pyrrolidone product was 1,000 ppm (Note 2).

Claims

1. A method for producing a carbon nanotube dispersion paste obtained by mixing and dispersing components including a pigment dispersion resin (A), carbon nanotubes (B), N-methyl-2-pyrrolidone (C), and an amine compound (D), wherein the pigment dispersion resin (A) has at least one polar functional group selected from the group consisting of amide groups, imide groups, hydroxyl groups, carboxyl groups, sulfonic acid groups, phosphate groups, silanol groups, cyano groups, pyrrolidone groups, and amino groups, and the concentration of the polar functional groups in the pigment dispersion resin (A) is 0.3 mmol / g or more and 23 mmol / g or less, and when the boiling point of N-methyl-2-pyrrolidone (C) is (Xc)°C and the boiling point of the amine compound (D) is (Xd)°C, (Xc)-10>(Xd).

2. A method for producing a carbon nanotube dispersion paste as described in claim 1, wherein N-methyl-2-pyrrolidone (C) is a recycled product, the moisture content in N-methyl-2-pyrrolidone (C) is controlled to 10,000 ppm or less, and the amine compound content in N-methyl-2-pyrrolidone (C) is controlled to 10,000 ppm or less.

3. The method for producing a paste having dispersed carbon nanotubes according to claim 1, wherein the water content of the paste having dispersed carbon nanotubes is 10,000 ppm or less.

4. A method for producing a carbon nanotube-dispersed paste according to claim 1, wherein the content of carbon nanotubes (B) is 0.1 mass % or more and less than 15 mass % based on 100 mass % of the total amount of the carbon nanotube-dispersed paste.

5. A method for producing a paste with dispersed carbon nanotubes according to claim 1, wherein the paste with dispersed carbon nanotubes further contains polyvinylidene fluoride (E).

6. A method for producing a composite paste for lithium ion secondary batteries, comprising a step of mixing an electrode active material (G) with a carbon nanotube dispersion paste obtained by the method for producing a carbon nanotube dispersion paste according to any one of claims 1 to 5.

7. A method for producing an electrode layer for a lithium ion secondary battery, comprising coating a composite paste for a lithium ion secondary battery obtained by the method for producing a composite paste for a lithium ion secondary battery according to claim 6 on a current collector.

8. A method for producing an electrode layer for a lithium ion secondary battery and a recycled N-methyl-2-pyrrolidone (C), comprising the steps of: applying a composite paste for lithium ion secondary batteries obtained by the method for producing a composite paste for lithium ion secondary batteries according to claim 6 onto a current collector and drying by heating; recovering vapor containing N-methyl-2-pyrrolidone (C) and an amine compound (D) to produce a mixed solution; and separating the amine compound (D) from the mixed solution to produce a recycled N-methyl-2-pyrrolidone (C).

Citation Information

Patent Citations

  • Conductive paste for lithium ion battery positive electrode and manufacturing method of composite material paste for lithium ion battery positive electrode

    JP2019021517A

  • Method for producing conductive paste

    JP2021002520A

  • Conductive pigment paste, coating material, and conductive coating film

    JP2021084945A

  • Carbon nanotube dispersion and use for same

    WO2019208637A1

  • Conductive pigment paste, coating material and coating film

    WO2022172847A1

Cited By

  • Binder polymer, binder composition, electrode slurry, electrode, and nonaqueous secondary battery

    WO2026140184A1

  • Binder polymer, binder composition, electrode slurry, electrode, and nonaqueous secondary battery

    WO2026140185A1