Insulated wire

The insulated wire's dual surface structure, with a rough area for flexibility and a smooth area for improved adhesion and wear resistance, addresses the issue of low surface smoothness in high-flexibility wires, enhancing performance and reliability.

WO2024204189A1PCT designated stage expired Publication Date: 2024-10-03AUTONETWORKS TECH LTD +2
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011932
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-26
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Insulated wires with high flexibility due to amorphous organic polymers in the insulation coating suffer from low surface smoothness, leading to poor adhesion and wear resistance, especially at contact points with other components, which can result in decreased waterproof performance and damage.

Method used

The insulated wire features a dual surface structure with a rough area for high flexibility and a smooth area for improved adhesion and wear resistance, achieved by forming a smooth region on a raw wire with a rough surface using a mold to enhance surface smoothness without compromising flexibility.

Benefits of technology

This dual surface design effectively suppresses the negative effects of low surface smoothness at contact points while maintaining high flexibility, enhancing adhesion, wear resistance, and waterproof performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011932_03102024_PF_FP_ABST
    Figure JP2024011932_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is an insulated wire that, while having an insulating coating with low surface smoothness, is capable of suppressing an influence caused by the low surface smoothness in a region such as a contact point with another member in which it is not preferable for surface smoothness to be low. The insulated wire 1 has a conductor 11 and an insulating coating 13 that coats the outer circumference of the conductor 11. The insulating coating 13 comprises a rough-surface region 2 and a smooth region 3 along the axial direction, and the surface smoothness of the insulating coating 13 is higher in the smooth region 3 than in the rough-surface region 2.
Need to check novelty before this filing date? Find Prior Art

Description

insulated wire

[0001] The present disclosure relates to insulated wire.

[0002] Flexibility is one of the important properties of insulated wires. For example, in the automotive field, the conductor cross-sectional area of ​​insulated wires is increasing due to the need to carry large currents as electric vehicles become more widespread. In such cases, it is important that the insulated wires have high flexibility in order to maintain sufficient routing ability. One method for increasing the flexibility of insulated wires is to use a highly flexible material, such as an amorphous organic polymer or an organic polymer with a large amorphous component, as the constituent material of the insulating coating that covers the outer periphery of the conductor.

[0003] JP 2014-234404 A JP 2022-072651 A

[0004] As described above, using an amorphous organic polymer or one with a high amorphous content as the organic polymer constituting the insulating coating of an insulated wire can improve the flexibility of the insulated wire. However, using such organic polymers tends to reduce the surface smoothness of the insulating coating. This is because, when forming the insulating coating by extrusion molding of the coating material, the slipperiness between the coating material and the die surface decreases, making melt fracture more likely to occur due to friction. The tendency for an increased content of amorphous components in an insulating coating to improve flexibility but reduce surface smoothness is also mentioned in, for example, Patent Document 1. In addition to using a coating material with a high amorphous content, an insulating coating with low surface smoothness can also be formed when forming the insulating coating at a high extrusion speed.

[0005] As such, there are situations in which it is advantageous to use an insulated wire with a low surface smoothness of the insulating coating, such as by using a material containing a large amount of amorphous components to improve the flexibility of the insulating coating or by increasing the extrusion speed of the insulating coating to improve productivity. However, poor surface smoothness can cause problems when the insulated wire is used in contact with other components. When the surface of the insulating coating is less smooth, fine irregularities are present on the surface, resulting in microscopic contact points being concentrated at the convex portions of the irregularities at the contact interface between the insulated wire and other components. This can result in poor adhesion to components, such as waterproof plugs, when attached to the outer periphery of the insulated wire. Poor adhesion to the waterproof plug can lead to reduced waterproofing. Furthermore, when friction occurs between the insulating coating and an external component, the frictional load is concentrated at the microscopic contact points, potentially reducing the abrasion resistance of the insulating coating or causing damage to the external component.

[0006] In view of the above, an object of the present invention is to provide an insulated wire that has an insulating coating with a low surface smoothness, but that can suppress the effects caused by the low surface smoothness in areas where a low surface smoothness is undesirable, such as areas in contact with other members.

[0007] The insulated wire of the present disclosure includes a conductor and an insulating coating that covers the outer periphery of the conductor. The insulating coating has a roughened region and a smooth region along the axial direction, and the smoothness of the surface of the insulating coating is higher in the smooth region than in the roughened region.

[0008] The insulated wire of the present disclosure has an insulating coating with low surface smoothness, but is capable of suppressing the effects caused by low surface smoothness in areas where low surface smoothness is undesirable, such as areas of contact with other members.

[0009] Fig. 1 is a perspective view schematically illustrating an insulated electric wire according to one embodiment of the present disclosure. Fig. 2A and Fig. 2B are photographs of a raw insulated electric wire before smoothing and an insulated electric wire with a smooth region formed in a region including an end portion, respectively. Fig. 3A and Fig. 3B are optical microscope images of the surfaces of the roughened region and the smooth region, respectively, of an insulated electric wire with a smooth region formed.

[0010] [Description of Embodiments of the Present Disclosure] First, embodiments of the present disclosure will be listed and described. An insulated wire of the present disclosure has the following configuration.

[0011] [1] An insulated wire according to the present disclosure includes a conductor and an insulating coating covering the outer periphery of the conductor. The insulating coating has a roughened region and a smooth region along an axial direction, and the smoothness of the surface of the insulating coating is higher in the smooth region than in the roughened region.

[0012] In the insulated wire, both roughened regions with low surface smoothness and smooth regions with high surface smoothness of the insulating coating coexist. In the roughened regions, the properties of the insulating coating with low surface smoothness, such as high flexibility, can be utilized. On the other hand, in the smooth regions, the high surface smoothness facilitates the formation of a microscopically uniform contact interface when the insulated wire comes into contact with another component, resulting in improved adhesion and abrasion resistance with the other component, and reduced damage to the other component. Thus, by providing smooth regions in regions where low surface smoothness is undesirable, such as contact points with other components, and leaving other regions as roughened regions, the properties of the insulating coating with low surface smoothness can be utilized in the roughened regions while reducing the effects of low surface smoothness in the smooth regions. An insulated wire having both roughened and smooth regions can be easily formed by placing a mold around the areas to be smooth regions of a raw insulated wire entirely composed of roughened regions and heating the insulating coating at those areas through the mold.

[0013] [2] In the above aspect [1], the surface roughness Ra of the insulating coating may be 50% or more smaller in the smooth region than in the rough region, thereby making it possible to particularly effectively suppress the effects of low surface smoothness in the smooth region.

[0014] [3] In the above aspect [1] or [2], the flexibility of the insulating coating may be higher in the roughened region than in the smooth region. The high flexibility of the insulating coating in the roughened region allows the insulated electric wire to be flexibly bent using the roughened region. This improves the convenience of the insulated electric wire during wiring and other operations. As described above, when a smooth region is formed by heating a raw insulated electric wire entirely composed of a roughened region using a molding die, the smoothness of the surface of the insulating coating is improved in the smooth region, but the flexibility of the insulating coating is likely to decrease.

[0015] [Details of Embodiments of the Present Disclosure] Insulated wires according to embodiments of the present disclosure will be described in detail below with reference to the drawings. In this specification, with respect to the structure of each part of an insulated wire, concepts indicating the shape or arrangement of components, such as circularity, include errors from the geometric concepts within the ranges permissible for this type of insulated wire, such as deviations of approximately ±15% in length and deviations of approximately ±15° in angle.

[0016] <Configuration of insulated wire> First, the configuration of a wire harness according to an embodiment of the present disclosure will be described. Fig. 1 is a perspective view showing an outline of an insulated wire 1 according to an embodiment of the present disclosure. The insulated wire 1 has a conductor 11 and an insulating coating 13 that covers the outer periphery of the conductor 11.

[0017] The insulated wire 1 has a roughened region 2 and a smooth region 3 along the axial direction (longitudinal direction). The surface smoothness of the insulating coating 13 is higher in the smooth region 3 than in the roughened region 2. In the illustrated embodiment, the smooth region 3 is formed in a partial region including the end of the insulated wire 1, and the remaining region is the roughened region 2. The roughened region 2 and the smooth region 3 are continuous with each other. In other words, the conductor 11 and the insulating coating 13 that constitute the insulated wire 1 are integrally continuous between the roughened region 2 and the smooth region 3, respectively. The differences in state and characteristics between the roughened region 2 and the smooth region 3 will be described in detail later.

[0018] In the insulated wire 1 according to this embodiment, the materials constituting the conductor 11 and the insulating coating 13 are not particularly limited. Various metal materials can be used as the material for the conductor 11, including copper and copper alloys, aluminum and aluminum alloys, etc. Copper or copper alloys are particularly preferred because of their high conductivity and flexibility. The conductor 11 may be configured as a single wire, but is preferably made up of multiple strands 12 from the viewpoint of increasing flexibility during bending. The multiple strands 12 may be bundled to form the conductor 11, or may be twisted together to form a stranded wire. The conductor 11 may be compression molded.

[0019] The insulating coating 13 is made of a material containing an organic polymer. The type of organic polymer is not particularly limited, and examples include olefin-based polymers such as polyolefins and olefin-based copolymers, halogen-based polymers such as polyvinyl chloride (PVC), fluorine-based polymers, various engineering plastics, elastomers, rubber, etc. The organic polymer may be crosslinked. The organic polymer may also be foamed.

[0020] To enhance the flexibility of the insulated wire 1, the material constituting the insulating coating 13 preferably contains an amorphous organic polymer or an organic polymer containing a large amount of amorphous components. Suitable amorphous organic polymers and organic polymers containing a large amount of amorphous components include olefin block copolymers, polyolefins such as low-density polyethylene (LDPE), halogen-based polymers such as PVC, and various elastomers. These amorphous organic polymers and organic polymers containing a large amount of amorphous components preferably account for 2% by mass or more of the polymer components constituting the insulating coating 13. Furthermore, the overall crystallinity of the polymer components constituting the insulating coating 13 should preferably be kept to 75% or less. As described below, when forming the smooth region 3 by heating a raw insulated wire entirely consisting of the roughened region 2, the organic polymer constituting the insulating coating 13 must have thermoplastic properties. All of the organic polymers listed here are thermoplastic polymers.

[0021] In addition to the organic polymer, the insulating coating 13 may contain appropriate additives, such as a flame retardant, an antioxidant, a lubricant, a metal deactivator, and a colorant.

[0022] The specific dimensions of the insulated wire 1 are not particularly limited. However, from the viewpoint of effectively utilizing the high flexibility of the insulating coating 13 exhibited by the rough surface region 2 to improve the convenience of wiring operations, etc., the conductor cross-sectional area is set to 16 mm. 2 The upper limit of the conductor cross-sectional area is not specified, but it is generally 200 mm 2 Furthermore, from the viewpoint of increasing the effect of providing the roughened region 2 and the smooth region 3 depending on the state of the insulating coating 13, the thickness of the insulating coating 13 in the roughened region 2 should be 0.8 mm or more. There is no particular upper limit to the thickness of the insulating coating 13, but it is generally recommended to set it to 2.0 mm or less.

[0023] <Method for Manufacturing Insulated Wire> Before describing the details of the rough surface region 2 and the smooth region 3, an example of a method for manufacturing the insulated wire 1 according to this embodiment will be described.

[0024] The insulated wire 1 having the roughened region 2 and the smooth region 3 can be easily produced using a raw insulated wire whose entire region is composed of the roughened region 2, that is, a raw insulated wire whose entire region along the axial direction has the same configuration as the roughened region 2 to be provided in the insulated wire 1, including the degree of surface smoothness of the insulating coating 13. The raw insulated wire is produced by forming the insulating coating 13 around the outer periphery of the conductor 11 by extrusion molding or the like. The degree of surface smoothness of the formed insulating coating 13 depends on the conditions under which the insulating coating 13 is formed, as well as the component composition of the coating material that becomes the insulating coating 13 by extrusion molding or the like. For example, performing extrusion molding at a high speed makes melt fracture more likely to occur, reducing the surface smoothness of the insulating coating 13.

[0025] By forming smooth regions 3 at desired locations on a raw insulated electric wire entirely composed of rough surface regions 2 and leaving the remaining regions as rough surface regions 2, it is possible to obtain an insulated electric wire 1 in which rough surface regions 2 and smooth regions 3 coexist. The smooth regions 3 can be formed by heating using a molding die (metal mold). That is, the molding die is placed in close contact with the surface of the insulating coating 13 of the raw insulated electric wire at the location where the smooth regions 3 are to be formed. The molding die is then heated, thereby heating the insulating coating 13 via the molding die. It is also preferable to preheat the raw insulated electric wire and / or the molding die before placing the molding die around the outer periphery of the raw insulated electric wire.

[0026] By heating the insulating coating 13 through the mold in this manner, the surface of the insulating coating 13 becomes smoother than its original state, thereby forming the smooth region 3. The smoothing of the surface of the insulating coating 13 occurs as the organic polymer constituting the insulating coating 13 softens with heating, eliminating the uneven structure that existed on the surface of the insulating coating 13 of the raw insulated electric wire, and reconstructing a smooth surface that conforms to the surface of the mold. To effectively smooth the surface of the insulating coating 13, it is preferable to set the heating temperature of the insulating coating 13 to a temperature at which the constituent material of the insulating coating 13 softens, at least on the surface. The insulating coating 13 may be heated to a temperature at which the surface melts. However, it is preferable not to heat the insulating coating 13 to a temperature high enough to melt the entire surface. It is preferable to use a mold whose cavity surface has a smoothness equal to or greater than that of the surface of the insulating coating 13 in the smooth region 3 to be produced. Furthermore, the smoothness of the insulating coating 13 can be effectively improved by applying a force from the outside to the inside of the insulating coating 13 while heating it using the mold.

[0027] The heating of the insulating coating 13 to form the smooth region 3 is a process in which the coating material containing an organic polymer comes into contact with the surface of a mold member at a high temperature, similar to the process of forming the insulating coating 13 by extrusion molding in the raw insulated wire manufacturing process. However, while extrusion molding can cause friction between the coating material and the surface of the mold member, heating to form the smooth region 3 heats the insulating coating 13 in a static state, so there is no friction between the insulating coating 13 and the mold member. Therefore, in this process, the smoothness of the surface of the insulating coating 13 is not substantially reduced due to friction.

[0028] <Differences in Conditions and Characteristics of Rough Surface Region and Smooth Surface Region> As described above, the insulated wire 1 according to this embodiment has a rough surface region 2 and a smooth region 3, and the surface smoothness of the insulating coating 13 is higher in the smooth region 3 than in the rough surface region 2. Generally, factors that cause the surface smoothness of an insulating coating of an insulated wire to be low are thought to be due to the component composition of the insulating coating, such as an organic polymer containing a high amount of amorphous components, or manufacturing conditions, such as high-speed extrusion molding. However, since the insulated wire 1 according to this embodiment has a rough surface region 2 with low surface smoothness, the properties brought about by these factors can be utilized in the rough surface region 2. For example, if the organic polymer constituting the insulating coating 13 contains a high amount of amorphous components, the insulating coating 13 tends to have high flexibility. This allows the insulated wire 1 to be flexibly bent in the rough surface region 2, making it more convenient to perform operations such as wiring. Furthermore, high productivity can be achieved when the insulating coating 13 is manufactured by high-speed extrusion molding.

[0029] On the other hand, the smooth region 3 can suppress the effects that occur when the surface has low smoothness, such as in the rough region 2. For example, in the rough region 2, the microscopic contact surface tends to concentrate at the contact surface of the convex portions when contacting another component due to the fine unevenness of the surface. In contrast, in the smooth region 3, the surface has fewer and / or smaller unevenness, allowing for a microscopically uniform contact surface to be formed with the other component. Therefore, the smooth region 3 can be suitably used for attaching other components. Furthermore, the smooth region 3 can be suitably disposed in locations where contact with other components may occur. As a specific example, when attaching a waterproof plug such as a rubber stopper to the periphery of the insulated electric wire 1, if the waterproof plug is attached to the periphery of the smooth region 3, the waterproof plug will adhere microscopically to the surface of the insulating coating 13, making it less likely that a small gap will form between the waterproof plug and the insulated electric wire 1, thereby achieving high waterproofing. Furthermore, even if friction occurs between the insulated wire 1 and another member in contact with it in the smooth region 3, the load due to the friction is less likely to be concentrated in a small area, so the insulating coating 13 is less likely to wear, resulting in high wear resistance. Similarly, the load is less likely to be concentrated in a small area on the other member in contact with the insulated wire 1, so the other member is less likely to be damaged, such as scratched.

[0030] In this way, by having both the rough surface region 2 and the smooth region 3 coexist in the insulated wire 1, it is possible to utilize the characteristics of each region. From the viewpoint of ensuring a large difference in the characteristics between the rough surface region 2 and the smooth region 3, and particularly from the viewpoint of enhancing the characteristics obtained by the high surface smoothness in the smooth region 3, it is preferable that the surface roughness Ra of the insulating coating 13 in the smooth region 3 is 50% or more smaller than that of the rough surface region 2. In other words, assuming that the surface roughness Ra of the rough surface region 2 is 100%, the reduction in the surface roughness Ra in the smooth region 3 should be 50% or more. More preferably, the reduction should be 60% or more, or even 65% or more. Since the surface smoothness of the smooth region 3 is preferably as high as possible, there is no particular upper limit to the difference in smoothness between the rough surface region 2 and the smooth region 3. However, considering the degree of smoothness that can be achieved when the smooth region 3 is formed by heating using a molding die, the reduction in the surface roughness Ra in the smooth region 3 should be approximately 90% or less. The specific surface roughness Ra values ​​of the rough region 2 and the smooth region 3 are not particularly limited, but examples include a value of 150 μm or more and 500 μm or less in the rough region 2 and a value of 50 μm or more and 150 μm or less in the smooth region 3. The surface smoothness of the insulating coating 13 in the rough region 2 and the smooth region 3 can be easily compared by visually comparing the gloss. Alternatively, the surface roughness Ra may be quantitatively evaluated based on JIS B 0601:2013.

[0031] In the insulated wire 1 according to this embodiment, as described above, the smooth region 3 has a higher surface smoothness of the insulating coating 13 than the rough region 2. However, it is preferable that the flexibility of the insulating coating 13 is higher in the smooth region 3 than in the rough region 2. If the rough region 2 has high flexibility, the smooth region 3 can be suitably used for applications in which the insulated wire 1 comes into contact with other components. Furthermore, by utilizing the rough region 2 to flexibly bend the insulated wire 1, the convenience of wiring and other operations can be improved. As described above, when the insulating coating 13 is formed using an amorphous organic polymer or an organic polymer containing a large amount of amorphous components, the surface smoothness of the insulating coating 13 tends to be low. However, amorphous organic polymers and organic polymers containing a large amount of amorphous components have high flexibility. Therefore, the rough region 2 can be easily formed as a region with low surface smoothness and high flexibility. Furthermore, as described above, when the smooth region 3 is formed by heating a raw insulated wire entirely composed of the rough region 2 using a molding die, the flexibility of many organic polymers that can form the insulating coating 13 tends to decrease.

[0032] The difference in flexibility of the insulating coating 13 between the roughened region 2 and the smooth region 3 can be evaluated, for example, by a three-point bending test of the insulated wire 1. The three-point bending test can be performed as a bending test in accordance with JIS K 7171:2016. That is, a sample electric wire is supported at two points spaced a predetermined distance apart along the length, and the maximum repulsive force when the wire is bent at the center is measured as the repulsive load. A smaller repulsive load indicates a higher flexibility of the insulated wire 1. A three-point bending test can be performed by setting the same fulcrum distance as a ratio of the outer diameter of the insulated wire 1 for each of the roughened region 2 and the smooth region 3 (for example, as in the examples below, the fulcrum distance is set to four times the outer diameter of the insulated wire 1 in each of the regions 2 and 3), and comparing the repulsive loads. For example, the repulsive load in the smooth region 3 should be at least 20% higher than that in the roughened region 2. In other words, assuming that the repulsive load of the rough surface region 2 is 100%, it is sufficient that the increase in the repulsive load of the smooth region 3 is 20% or more. This means that the bending flexibility of the rough surface region 2 can be considered to be sufficiently higher than that of the smooth region 3. More preferably, the increase in the repulsive load is 25% or more, or even 30% or more. While there is no particular upper limit to the increase in the repulsive load, it is preferable to keep it at, for example, 60% or less in order to ensure a certain degree of flexibility in the smooth region 3. The flexibility of the insulated wire 1 evaluated by the repulsive load obtained in a three-point bending test includes the contribution of the conductor 11. However, if the conductor cross-sectional area is within the preferred range described above, it can be considered that a sufficient difference in the flexibility of the insulating coating 13 exists between the rough surface region 2 and the smooth region 3, provided that the increase in the repulsive load falls within the above-mentioned range.

[0033] The specific positions and lengths of the roughened region 2 and the smooth region 3 in the insulated wire 1 are not particularly specified, and the smooth region 3 may be provided in regions where poor surface smoothness of the insulating coating 13 could have undesirable effects, such as positions where other components are attached or where unwanted contact with other components is expected. In this way, the effect of the smooth surface of the smooth region 3 suppressing the effects that could be caused by poor surface smoothness can be effectively utilized. For example, when a component such as a waterproof plug is attached to or near the end of the insulated wire 1, or when a connector is attached to the end of the insulated wire 1 and there is a concern that the insulating coating 13 will be worn due to contact with the connector housing, the smooth region 3 may be provided in a region including the end of the insulated wire 1. Furthermore, when a member such as a protective material is attached to the midpoint of the axial direction of the insulated wire 1, or when there is a possibility that the midpoint of the insulated wire 1 may come into undesired contact with a nearby external member, which may cause wear of the insulating coating 13 or damage to the external member, a smooth region 3 may be provided at a necessary location midpoint of the axial direction of the insulated wire 1. The roughened region 2 and / or the smooth region 3 may be provided in multiple locations. When smooth regions 3 are provided in two or more locations, the surface smoothness of the smooth regions 3 may be the same or different. The length ratio between the roughened region 2 and the smooth region 3 is not particularly specified, but from the viewpoint of effectively utilizing the properties of the roughened region 2, such as high flexibility, it is preferable to make the total length of the roughened region 2 longer than the total length of the smooth region 3.

[0034] The specific shapes of the roughened surface region 2 and the smooth region 3 are not particularly specified. In the illustrated embodiment, both the smooth region 2 and the roughened surface region 3 have circular cross sections, and their outer diameters are not significantly different. By minimizing the changes in the cross-sectional shapes and sizes of the roughened surface region 2 and the smooth region 3 in this manner, the difference in the overall outer shape of the insulated wire 1 from that of a conventional insulated wire, whose surface smoothness is constant throughout, can be minimized. As described above, when the raw insulated wire entirely composed of the roughened surface region 2 is heated using a molding die to form the smooth region 3, the outer diameter of the smooth region 3 may become smaller than that of the roughened surface region 2 due to the force applied to the raw insulated wire from the molding die. However, from the viewpoint of minimizing changes in the cross-sectional shape and cross-sectional size of the smooth region 3 and the rough surface region 2, it is advisable to limit the difference in outer diameter between the smooth region 3 and the rough surface region 2 to 20% or less, or even 10%, of the outer diameter of the rough surface region 2, by using a molding die having a cavity with a shape and size similar to that of the raw insulated electric wire.

[0035] On the other hand, it is also possible to actively change the cross-sectional shapes and / or cross-sectional sizes of the smooth region 3 and the rough region 2. For example, if the cross-sectional shape of the rough region 2 is not circular, the cross-sectional shape of the smooth region 3 can be made closer to a circle, or if the cross-sectional size of the rough region 2 is large, the cross-sectional size of the smooth region 3 can be made smaller, which may improve the convenience of attaching other components to the smooth region 3. Another possible change in cross-sectional shape is to make the cross-section of one of the rough region 2 and the smooth region 3 a flat shape, such as one that can approximate an oval or a rectangle, and make the cross-section of the other a shape with a lower degree of flatness, such as one that can approximate a circle or a square. To differentiate the cross-sectional shape and / or cross-sectional size between the smooth region 3 and the rough region 2, for example, when a raw insulated electric wire whose entire area is the rough region 2 is heated using a molding die to form the smooth region 3, a molding die having a cavity corresponding to the shape and cross-sectional size of the smooth region 3 to be formed is used, and a force is applied to deform the insulating coating 13 and the conductor 11, thereby smoothing the surface of the insulating coating 13 and simultaneously changing the cross-sectional shape and / or cross-sectional size.

[0036] Examples are shown below. The present invention is not limited to these examples. Insulated wires having a smooth region and a roughened region were prepared, and the surface smoothness and flexibility of the smooth and roughened regions were compared. Unless otherwise specified, sample preparation and evaluation were carried out at room temperature in the atmosphere.

[0037] <Preparation of Samples> As the raw insulated wire, an insulated wire was prepared by extruding an insulating coating of a uniform thickness around the outer periphery of a conductor. A stranded wire made by twisting together copper alloy wires was used as the conductor. The conductor cross-sectional area was 95 mm. 2 The insulating coating was made of cross-linked polyethylene and had a thickness of 2.0 mm.

[0038] The raw insulated wire was cut into a length of 300 mm, and a smooth region was formed in a region extending 150 mm from one end. The remaining region was left as a roughened region, thereby obtaining an insulated wire having a smooth region and a roughened region. The smooth region was formed by placing a molding die having a cylindrical cavity with an inner diameter slightly smaller than the outer diameter of the raw insulated wire around the outer periphery of the raw insulated wire and heating it. The temperature of the molding die was set to 150°C.

[0039] <Sample Evaluation> The obtained insulated wire was visually observed to confirm the formation of a smooth region in addition to a rough region. Furthermore, the surface of the insulating coating was observed with an optical microscope for each of the rough region and the smooth region, and the surface roughness Ra was evaluated using a surface roughness measuring device in accordance with JIS B 0601:2013.

[0040] Furthermore, a three-point bending test was conducted in accordance with JIS K 7171:2016 to measure the repulsion load of the insulated wire in the roughened and smooth regions. Test specimens were cut out from the insulated wire in lengths of 150 mm each in the roughened and smooth regions. Each test specimen was supported at two points separated by a predetermined support distance, and then bent at the center. The maximum repulsion force (unit: N) was measured and recorded as the repulsion load. The support distance was set to four times the outer diameter of each test specimen. Specifically, since the outer diameter of the insulated wire was 17.8 mm in the roughened region and 16.6 mm in the smooth region, the support distance was set to 71.2 mm for the test specimen in the roughened region and 66.4 mm for the test specimen in the smooth region.

[0041] <Evaluation Results> Figures 2A and 2B show photographs of the raw insulated electric wire before the formation of the smooth region and the insulated electric wire after the formation of the smooth region, respectively. Figures 3A and 3B show images of the insulated electric wire after the formation of the smooth region, observed with an optical microscope. Figure 3A shows the rough region, and Figure 3B shows the smooth region. Table 1 below shows the evaluation results of the surface roughness Ra and the rebound load in a three-point bending test for the rough region and the smooth region, respectively. Table 1 also shows the amount of change in the value of the smooth region relative to the value of the rough region.

[0042]

[0043] Comparing the photographs in Figures 2A and 2B, it can be seen that the entire surface in Figure 2A is matte, whereas in Figure 2B, only the leftmost region where the smooth region is formed is glossy. This confirms that heating using a molding die has resulted in the formation of a smooth region with improved surface smoothness in the insulating coating. Furthermore, comparing the microscopic images in Figures 3A and 3B, it can be seen that Figure 3A, which shows the roughened region, shows a microstructure with unevenly distributed light and dark areas indicating an uneven structure, whereas Figure 3B, which shows the smooth region, shows a highly uniform surface, confirming the increased surface smoothness.

[0044] Furthermore, looking at the evaluation results in Table 1, as seen by comparing Figures 3A and 3B, the surface roughness Ra is smaller in the smooth region than in the rough region, quantitatively confirming improved smoothness. The surface roughness Ra is 68% smaller in the smooth region than in the rough region. The rebound load in the three-point bending test is larger in the smooth region than in the rough region, indicating that the rough region has higher flexibility. The rebound load in the smooth region is 31% higher than in the rough region.

[0045] These results confirm that an insulated wire with both rough and smooth regions can be produced by heating the raw insulation coating using a molding die. It also confirms that the smoothness of the surface of the insulation coating is higher in the smooth region than in the rough region. Furthermore, it is clear that the flexibility of the insulation coating is higher in the rough region than in the smooth region.

[0046] Although the embodiments of the present disclosure have been described in detail above, the present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the gist of the present invention.

[0047] REFERENCE SIGNS LIST 1 insulated wire 11 conductor 12 wire 13 insulating coating 2 rough surface area 3 smooth surface area

Claims

1. An insulated wire comprising a conductor and an insulating coating covering the outer periphery of the conductor, the insulating coating having a roughened region and a smooth region along the axial direction, the smoothness of the surface of the insulating coating being higher in the smooth region than in the rough region.

2. The insulated wire according to claim 1, wherein the surface roughness Ra of the insulating coating is at least 50% smaller in the smooth region than in the rough region.

3. The insulated wire according to claim 1 or 2, wherein the flexibility of the insulating coating is higher in the rough area than in the smooth area.

Citation Information

Patent Citations

  • Production method and device of cable for signal transmission

    JP2019160484A

  • Communication wire, wire with terminal, and wire harness

    JP2022151330A