Biological material, powder composition, bone prosthetic material, and method for using composition containing composite compound as biological material
Biomaterials with yttrium, oxygen, and silicon composite compounds address the biocompatibility issues of silicon nitride-based materials, offering improved biocompatibility and antibacterial properties for medical applications like bone grafting and implants.
Patent Information
- Application Number
- PCT/JP2024/012071
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-03
AI Technical Summary
Current biomaterials, particularly those based on silicon nitride, face insufficient biocompatibility, which limits their effectiveness in medical applications such as bone grafting and implants.
Development of biomaterials, powder compositions, and bone grafting materials containing composite compounds with yttrium, oxygen, and silicon, specifically Si3N4-SiO2-Y2O3-based compounds, which exhibit enhanced biocompatibility and antibacterial properties through optimized phase diagrams and surface characteristics.
These materials demonstrate improved biocompatibility, reduced cytotoxicity, and enhanced osteoconductivity, promoting cell differentiation and bone formation, making them suitable for implants and artificial joints.
Smart Images

Figure JP2024012071_03102024_PF_FP_ABST
Abstract
Description
Biomaterial, powder composition, bone filling material, and method for using a composition containing a complex compound as a biomaterial
[0001] The present disclosure relates to biomaterials, powder compositions, bone substitutes, and methods of using compositions containing complex compounds as biomaterials.
[0002] Silicon nitride is known to have antibacterial properties and biocompatibility. Patent Document 1 proposes changing the surface chemical properties of a bioimplant block containing silicon nitride ceramic material to improve its antibacterial properties. Patent Document 2 proposes filling a bioimplant such as polyether ether ketone (PEEK) with silicon nitride and providing a silicon nitride coating. Incidentally, silicon nitride forms composite oxides when fired with oxides. For example, it is known that when silicon nitride powder is mixed with an auxiliary agent containing yttrium oxide and sintered, composite oxides such as melilite, YAM, apatite, and wollastonite are formed at the grain boundaries of the silicon nitride particles (see, for example, Patent Document 3).
[0003] JP 2015-516239 A JP 2020-512072 A JP 2000-247748 A
[0004] Although attempts have been made to use ceramics such as silicon nitride as biomaterials, their biocompatibility is still insufficient. Therefore, the present disclosure provides a biomaterial, a powder composition, and a bone substitute material with excellent biocompatibility. It also provides a method for using a composition containing a complex compound as a biomaterial with excellent biocompatibility.
[0005] One aspect of the present disclosure provides the following biomaterial:
[0006] [1] A biomaterial containing, as a main component, a complex compound having yttrium, oxygen, silicon, and nitrogen as constituent elements.
[0007] The composite oxide has excellent biocompatibility.
[0008] The biomaterial of [1] above may be any one of the following [2] to [7]. These biomaterials have even better biocompatibility.
[0009] [2] The composite compound is Si 3 N 4 -SiO 2 -Y 2 O 3 Compounds and Si 3 N 4 -Y 2 O 3 [3] The biomaterial according to [1], comprising at least one selected from the group consisting of Si-based compounds. 3 N 4 , SiO 2 and Y 2 O 3 In the phase diagram of the three-component system, Y 5 Si 3 O 12 N.Y. 2 Si 3 O 3 N 4 and Y 4 Si 2 O 7 N 2 [4] The biomaterial according to [1] or [2], wherein the complex compound has a composition within a triangular region having three vertices: Y 5 Si 3 O 12 N, YSiO 2 N.Y. 4 Si 2 O 7 N 2 and Y 2 Si 3 O 3 N 4 [5] The biomaterial according to any one of [1] to [3], which contains at least one selected from the group consisting of: 2[6] The biomaterial according to any one of [1] to [5], wherein the content of ammonium ions in the liquid phase is 0.5 μg / mL or more after 10 minutes from the biomaterial being dispersed in water to a concentration of 6.0 w / v%. [7] The biomaterial according to [6], wherein the pH of the liquid phase is 10.0 or less.
[0010] One aspect of the present disclosure provides the following bone substitute: [8] A bone substitute comprising the biomaterial according to any one of [1] to [7] above.
[0011] The bone substitute contains a biomaterial with excellent biocompatibility, and is suitable for use as a component of implants and artificial joints.
[0012] One aspect of the present disclosure provides the following method.
[0013] [9] A method of using a composition containing, as a main component, a complex compound having yttrium, oxygen, silicon, and nitrogen as constituent elements, as a biomaterial.
[0014] A composite compound containing yttrium, oxygen, silicon, and nitrogen as constituent elements has excellent biocompatibility and can therefore be suitably used as a biomaterial.
[0015] The method [9] above may be any one of the following methods
[10] to
[15] . The biomaterials used in these methods have even better biocompatibility.
[0016]
[10] The composite compound is Si 3 N 4 -SiO 2 -Y 2 O 3 Compounds and Si 3 N 4 -Y 2 O 3
[11] The method according to [9], wherein the composite compound comprises at least one selected from the group consisting of Si-based compounds. 3 N 4 , SiO 2 and Y 2 O 3 In the phase diagram of the three-component system, Y5 Si 3 O 12 N.Y. 2 Si 3 O 3 N 4 and Y 4 Si 2 O 7 N 2
[12] The method according to [9] or
[10] , wherein the complex compound has a composition within a triangular region having three vertices: Y 5 Si 3 O 12 N, YSiO 2 N.Y. 4 Si 2 O 7 N 2 and Y 2 Si 3 O 3 N 4
[13] The method according to any one of [9] to
[11] , which comprises at least one selected from the group consisting of: 2
[14] The method according to any one of [9] to
[13] , wherein the ammonium ion content in the liquid phase is 0.5 μg / mL or more after 10 minutes from dispersion in water to a concentration of 6.0 w / v %.
[15] The method according to
[14] , wherein the pH of the liquid phase is 10.0 or less.
[0017] One aspect of the present disclosure provides the following powder composition:
[0018]
[16] A composite compound having yttrium, oxygen, silicon, and nitrogen as constituent elements as a main component, having a BET specific surface area of 0.3 m 2 / g or more.
[0019] The powder composition has excellent biocompatibility.
[0020] The powder composition of the above item
[16] may be any one of the following items
[17] to
[21] . These powder compositions have even better biocompatibility.
[0021]
[17] The composite compound is Si 3 N4 -SiO 2 -Y 2 O 3 Compounds and Si 3 N 4 -Y 2 O 3
[18] The powder composition according to
[16] , comprising at least one selected from the group consisting of Si-based compounds. 3 N 4 , SiO 2 and Y 2 O 3 In the phase diagram of the three-component system, Y 5 Si 3 O 12 N.Y. 2 Si 3 O 3 N 4 and Y 4 Si 2 O 7 N 2
[19] The powder composition according to
[16] or
[17] , wherein the complex compound has a composition within a triangular region having three vertices: Y 5 Si 3 O 12 N, YSiO 2 N.Y. 4 Si 2 O 7 N 2 and Y 2 Si 3 O 3 N 4
[20] The powder composition according to any one of
[16] to
[19] , which contains at least one selected from the group consisting of:
[19] ,
[20] The powder composition according to any one of
[16] to
[19] , wherein, when dispersed in water to a concentration of 6.0 w / v %, and 10 minutes have passed since dispersion, the content of ammonium ions contained in the liquid phase is 0.5 μg / mL or more.
[21] The powder composition according to
[20] , wherein the pH of the liquid phase is 10.0 or less.
[0022] According to the present disclosure, it is possible to provide a biomaterial, a powder composition, and a bone filler having excellent biocompatibility, and also to provide a method for using a composition containing a complex compound as a biomaterial having excellent biocompatibility.
[0023] Si 3 N 4 , SiO 2 and Y 2 O 3 1 is a phase diagram of a three-component system of the above. FIG. 2 is a front view of an example of a bone substitute material.
[0024] Hereinafter, embodiments of the present disclosure will be described. However, the following embodiments are merely examples for explaining the present disclosure and are not intended to limit the present disclosure to the following content. Note that each numerical range indicated with the symbol "to" includes both the lower and upper limits. That is, a numerical range indicated as "A to B" means A or more and B or less. The present disclosure also includes a case where the upper or lower limit of each numerical range is replaced with the numerical value of any of the examples. When multiple materials are exemplified, one of the materials may be used alone, or multiple materials may be used in combination.
[0025] In one embodiment, the biomaterial contains a complex compound having yttrium, oxygen, silicon, and nitrogen as constituent elements as a main component. 3 N 4 -SiO 2 -Y 2 O 3 based compounds, and Si 3 N 4 -Y 2 O 3 The compound may contain at least one selected from the group consisting of Si-based compounds. 3 N 4 -SiO 2 -Y 2 O 3 The Si-based compounds are shown in FIG. 3 N 4 , SiO 2 and Y 2 O 3 It is a complex compound included in the phase diagram of the three-component system.
[0026] The complex compound may have a composition within the shaded area (including the borders) in FIG. 5 Si 3 O 12 N (N-apatite), Y 2 Si 3 O 3 N 4(N-Melilite) and Y 4 Si 2 O 7 N 2 The complex compound is a triangular region with the three vertices of (N-YAM). This triangular region includes the composition on the boundary of the region. 5 Si 3 O 12 N (N-apatite), YSiO 2 N (N-wollastonite), Y 2 Si 3 O 3 N 4 (N-Melilite) and Y 4 Si 2 O 7 N 2 (N-YAM). This allows for sufficient enhancement of cell proliferation ability while sufficiently reducing cytotoxicity. In addition, due to its excellent osteoconductivity, it can promote the differentiation of undifferentiated mesenchymal cells into osteoblasts. Therefore, it is suitable as a biomaterial, for example, for bone replacement.
[0027] The biomaterial may be, for example, granular, a powder consisting of an aggregate of multiple particles, or a solid such as a membrane. In this disclosure, the term "major component" refers to the component that is most abundant when multiple components are included. Components other than the "major component" are referred to as "minor components." The biomaterial may consist only of a complex oxide, which is the major component, or may contain minor components different from the major component.
[0028] The content of the complex oxide in the biomaterial may be 90% by mass or more, 95% by mass or more, 98% by mass or more, 99% by mass or more, 99.5% by mass or more, or 99.7% by mass or more. The higher the content of the complex oxide in the biomaterial, the more likely it is to have improved biocompatibility. Examples of minor components that may be contained in the biomaterial include silicon nitride, silicon dioxide, and yttrium oxide. The biomaterial may also contain a complex oxide in which two of these three components are combined.
[0029] When a biomaterial is in powder form (powder composition), smaller primary particles and a larger specific surface area tend to improve both biocompatibility and antibacterial performance. The reason for the improved biocompatibility is thought to be that a larger specific surface area increases the amount of ammonium ions produced when the material comes into contact with water. The reason for the improved antibacterial performance is thought to be that a larger specific surface area increases the amount of ammonia produced when the material comes into contact with water. A larger specific surface area tends to improve antibacterial performance, particularly against Gram-positive bacteria.
[0030] The BET specific surface area of the biomaterial (powder composition) is 0.3 m 2 / g or more, 0.4m 2 / g or more, 0.5m 2 / g or more, 2.0m 2 / g or more, or 4.0m 2 / g or more. By increasing the BET specific surface area, osteoconductivity can be improved. If such a biomaterial is used as an implant or a component of an artificial joint, differentiation of undifferentiated mesenchymal cells into osteoblasts can be promoted, and bone can be smoothly formed. The BET specific surface area can be adjusted by changing the firing conditions (e.g., firing temperature and firing time) when synthesizing the complex oxide and the size of the raw material powder. The BET specific surface area of a biomaterial is 20 m 2 / g or less, 10m 2 / g or less, or 6.0m 2 / g or less. This can improve the handling of the biomaterial. An example of the range of the BET specific surface area is 0.3 to 20 m 2 The BET specific surface area can be measured by the method described in the Examples.
[0031] When the biomaterial is a powder (powder composition), the average particle size (D50, median diameter) may be 25 μm or less, 17 μm or less, 5 μm or less, or 2 μm or less. Smaller average particle sizes tend to improve biocompatibility and antibacterial performance. This is thought to be because smaller average particle sizes increase the amount of ammonium ions and ammonia produced by hydrolysis when the biomaterial comes into contact with water. From the viewpoints of ease of production and improved handleability, the average particle size may be 0.2 μm or more, 0.3 μm or more, or 0.5 μm or more. An example of the average particle size range is 0.2 to 25 μm. The particle size distribution is measured in accordance with the method described in JIS Z 8825:2013 "Particle size analysis - laser diffraction and scattering method." In a particle size distribution (cumulative distribution) shown with the horizontal axis representing particle size [μm] on a logarithmic scale and the vertical axis representing frequency [volume %], the particle size when the cumulative value from small particle sizes reaches 50% of the total is the above-mentioned average particle size (D50).
[0032] In the above particle size distribution, the particle size (D10) when the integrated value from small particle sizes reaches 10% of the total may be 0.1 to 6 μm, or 0.2 to 1 μm. In the above particle size distribution, the particle size (D90) when the integrated value from small particle sizes reaches 90% of the total may be 1.0 to 60 μm, or 1.0 to 3.0 μm. D10, D50, and D90 can be adjusted by changing the firing conditions (e.g., firing temperature and firing time) when synthesizing the composite oxide by firing or the pulverization conditions after firing.
[0033] The pH of the liquid phase (aqueous phase) after 10 minutes from the time when the biomaterial is dispersed in water to a concentration of 6.0 w / v % may be 10.0 or less, or 9.0 or less. This allows the concentration of ammonium ions (NH 4 +The biocompatibility can be further improved by increasing the concentration of ammonium hydroxide. The pH of the liquid phase may be 7.5 or higher or 8.0 or higher. This allows the ammonia concentration to be maintained and antibacterial performance to be enhanced. The pH of the liquid phase can be adjusted by changing the composition of the surface of the biomaterial. For example, treating the biomaterial with hydrofluoric acid or the like lowers the pH, and then washing with water or the like tends to raise the pH. The pH of the liquid phase may be, for example, 7.5 to 10.0. Even after 10 minutes have passed since the biomaterial was dispersed in water to a concentration of 3.6 w / v%, the pH of the liquid phase (aqueous phase) may be within the above-mentioned range.
[0034] When a biomaterial is dispersed in water to a concentration of 6.0 w / v% and 10 minutes have passed, the ammonium ion content in the liquid phase may be 0.5 μg / mL or more, 1.0 μg / mL or more, or 1.5 μg / mL or more. Increasing the ammonium ion content in the liquid phase can improve biocompatibility. The ammonium ion content may be 4.0 μg / mL or less, or 3.0 μg / mL or less. An example range of the ammonium ion content in the liquid phase may be 0.5 to 4.0 μg / mL. When a biomaterial is dispersed in water to a concentration of 3.6 w / v% and 10 minutes have passed, the ammonium ion content in the liquid phase may also be within the above-mentioned range.
[0035] When a biomaterial is dispersed in water to a concentration of 6.0 w / v% and 10 minutes have passed, the ammonia content in the liquid phase may be 0.1 μg / mL or more, or 0.2 μg / mL or more. Such a biomaterial may also have antibacterial properties. The ammonia content may be 1.0 μg / mL or less, or 0.8 μg / mL or less. An example range for the ammonia content in the liquid phase is 0.1 to 1.0 μg / mL. In the present disclosure, the unit "w / v%" is synonymous with "g / 100 mL." The ammonia and ammonium ion contents and pH in the liquid phase are measured under atmospheric pressure and a temperature of 20°C using the method described in the Examples. When a biomaterial is dispersed in water to a concentration of 3.6 w / v% and 10 minutes have passed, the ammonia content in the liquid phase may also be within the above-mentioned range.
[0036] The biomaterial can be manufactured, for example, by the following procedure. Silicon nitride powder, yttria powder, and silica powder are prepared as raw material powders. At least two of these are blended to obtain a mixed powder with the target crystal composition. The raw material powders may be mixed using, for example, a ball mill or the like. The raw material powders may also be mixed by wet mixing using a solvent. The mixed powder is sieved to remove coarse particles, and then fired in a nitrogen atmosphere at a temperature of 1500 to 1600°C. The firing time may be, for example, 2 to 20 hours. The resulting fired product is then subjected to a heating treatment using a ball mill or the like to be crushed, thereby obtaining a powdered biomaterial containing, as its main component, a complex compound having yttrium, oxygen, silicon, and nitrogen as constituent elements. The crystalline phase contained in the biomaterial can be analyzed by X-ray diffraction.
[0037] The biomaterial of this embodiment has excellent antibacterial properties against Gram-positive bacteria. The form of the biomaterial is not particularly limited, and may be, for example, a powder, bulk, thin film, or coating. The biomaterial may be, for example, coated onto a biological implant.
[0038] The powder composition according to one embodiment contains a composite compound having yttrium, oxygen, silicon, and nitrogen as constituent elements as a main component, and has a BET specific surface area of 0.3 m 2 / g or more. This powder composition may have the same composition, size, and properties as a powdered biomaterial. The description of the biomaterial embodiment also applies to the powder composition of this embodiment. The powder composition has excellent biocompatibility and can be suitably used as a biomaterial.
[0039] In one embodiment, a method of use uses a composition containing a complex compound having yttrium, oxygen, silicon, and nitrogen as its constituent elements as a main component as a biomaterial. The complex oxide contained as a main component in the composition is as described in the biomaterial embodiment. The contents of the main component and the subcomponents in the composition are as described in the biomaterial embodiment. The description of the complex oxide embodiment also applies to the method of use of this embodiment. That is, the composition may contain the same components as the biomaterial described above and may have the same shape and properties as the biomaterial described above. The form of the composition is not particularly limited and may be, for example, powder, bulk, thin film, or coating. The composition may be dispersed in a matrix such as a film or filter. The composition used in the method of use of this embodiment has excellent biocompatibility and is therefore suitable for use as a biomaterial.
[0040] A bone prosthesis according to one embodiment includes the biomaterial. The bone prosthesis may be, for example, an implant, a component 10 (stem) of an artificial joint as shown in FIG. 2, or a member to be inserted into a bone defect. The bone prosthesis may be in a paste form. The biomaterial may be coated on at least a portion of the surface of the base material of the bone prosthesis, or may be dispersed in the bone prosthesis.
[0041] Although the embodiments of the present disclosure have been described above, the present disclosure is not limited to the above-described embodiments.
[0042] The present disclosure will be described in more detail with reference to examples and comparative examples, but the present disclosure is not limited to the following examples.
[0043] Example 1 [Preparation of Biomaterial] A biomaterial was prepared according to the following procedure. 0.7 g of silicon nitride powder (manufactured by UBE Corporation, product name: E10), 11.5 g of yttria powder (manufactured by Shin-Etsu Chemical Co., Ltd., product name: UUHP), and 2.8 g of silica powder (manufactured by Kojundo Chemical Laboratory Co., Ltd.) were weighed out as raw material powders. The weighed raw material powders, 350 g of silicon nitride balls with a diameter of 16 mm, and 150 ml of ethanol were placed in a container (Nalgene plastic bottle, capacity: 500 ml). The container, sealed with a lid, was placed in a benchtop ball mill (manufactured by Eishin Co., Ltd., product name: BM-15), and the rotation speed was set to 82 rpm. Pre-mixing was carried out under these conditions for 1 hour to obtain a mixed slurry.
[0044] The powder was collected from the resulting mixed slurry using a membrane filter. The collected particles were dried at 120°C for 3 hours. The dried powder was sieved using a nylon sieve (#100). The powder that passed through the sieve was packed into a boron nitride molding container. This molding container was fired for 6 hours using an electric furnace (manufactured by Fuji Denpa Kogyo Co., Ltd., product name: Hi-Multi 500) under conditions of 1550°C, a nitrogen atmosphere, and 0.85 MPa (gauge pressure).
[0045] The powder obtained by firing was placed in a container (Nalgene plastic bottle, capacity: 500 ml). 375 g of silicon nitride balls with a diameter of 5 mm and 150 ml of ethanol were placed in this container, and the container was then sealed with a lid. The sealed container was placed on the above-mentioned bench ball mill, the rotation speed was set to 82 rpm, and a crushing treatment was carried out under these conditions for 6 hours. Powder was collected from the slurry after the crushing treatment using a membrane filter. The collected powder was dried at 110°C for 3 hours. The dried powder was sieved using a nylon sieve (#330). The powder that fell through the sieve was used as the Si powder of Example 1. 3 N 4 -SiO 2 -Y 2 O 3 The powder was analyzed using an X-ray diffractometer (Rigaku Corporation, model name: Ultima IV). 5 Si 3 O 12It was confirmed that the powder composition contained N-apatite as the main component. On the other hand, no components other than N-apatite were detected. This was designated as the biomaterial (powder composition) of Example 1.
[0046] [Evaluation of Biomaterials] <Particle Size Distribution> The particle size distribution of the biomaterials was measured by laser diffraction / scattering. The measurement was performed in accordance with the method described in JIS Z 8825:2013 "Particle Size Analysis - Laser Diffraction / Scattering Method." In the particle size distribution (cumulative distribution) shown with the horizontal axis representing particle size [μm] on a logarithmic scale and the vertical axis representing frequency [volume %], the particle sizes at which the cumulative value from the smallest particle size reached 10%, 50%, and 90% of the total were determined as D10, D50, and D90, respectively. The results are shown in Table 1.
[0047] <BET specific surface area> The BET specific surface area of the biomaterial was measured by the BET single-point method using nitrogen gas in accordance with JIS Z 8830:2013 "Method for measuring the specific surface area of powders (solids) by gas adsorption." The results are shown in the "SSA" column in Table 1.
[0048] <Evaluation of the liquid phase> 30 mL of distilled water was placed in a 50 mL vial. 1.8 g of biomaterial was placed in the vial and stirred for 30 seconds to obtain a dispersion. The vial was then closed with a lid, and the dispersion was left for 10 minutes. After 10 minutes had passed, the dispersion was filtered using a filter paper with a mesh size of 5.0 μm to obtain a filtrate (liquid phase). These operations were performed under atmospheric pressure and at 20°C.
[0049] Ammonia (NH 3 ) and ammonium ion (NH 4 + ) were quantified by ion chromatography (manufactured by Thermo Fisher Scientific, instrument name: ICS-2100). The pH of the filtrate was measured using a pH meter (manufactured by Mettler Toledo, instrument name: FP20-Std-Kit). The ammonia (NH 3 ) and ammonium ion (NH 4 + The contents of these compounds and the pH are shown in the "liquid phase" column of Table 1.
[0050] <Antibacterial activity> Bacteria (Staphylococcus aureus) were pre-cultured in BHI liquid medium to prepare a bacterial suspension (1 x 10 5 ~1 x 10 6 CFU / mL) was prepared. 0.15 g of biomaterial and 1 mL of distilled water were placed in a microtube to obtain a 15 w / v% dispersion. After sterilization with ultraviolet light, 1 mL of the above bacterial suspension was added to the microtube. After mixing for 5 minutes at room temperature (approximately 20°C) using a tube rotator, the supernatant was collected and the bacterial viability was measured by WST-8 assay and fluorescent imaging (Live & Dead staining: CFDA PI DAPI). The viability was also measured in the same manner when Staphylococcus epidermidis was used as the bacteria. The results are shown in Table 1. In Table 1, the viability results when no biomaterial was used are shown in the "ref." column.
[0051] <Biocompatibility> The biomaterial was crushed using a pestle and mortar, sieved, and granulated to a diameter of 75 μm or less. Suspensions of 1 mg / mL and 10 mg / mL biocompatible material were prepared using ultrapure water. The suspension was dispensed dropwise onto tissue culture microplates [Iwaki 3820-024 (24 wells) or MatTek P06G-0-20-F / H (6 wells)] to achieve concentrations of 0.1 mg / well and 1 mg / well. After dispensing, the microplates were dried in a dry heat sterilizer (TABAI LC-122) at 50°C for 24 hours and sterilized with ultraviolet light. In this way, cell culture beds were prepared. Growth medium and osteoblast differentiation medium were prepared on the prepared beds. The preparation methods for each medium were as follows.
[0052] The proliferation medium was prepared by adding 4.5 g / L glucose-containing DMEM (Nacalai tesque), 10% fetal bovine serum, and 1% PS. The osteoblast differentiation medium was prepared by adding 10 mM β-glycerophosphate, 50 μg / mL (L+) ascorbic acid, and 100 nM texamethasone to the proliferation medium prepared as described above.
[0053] The mouse bone marrow-derived KUSA-A1 cell line (JCRB) was selected as the first choice. The KUSA-A1 cell line was cultured in a proliferation medium and an osteoblast differentiation medium at a cell density of 5 × 10 cells. 4 / cm 2 After 3, 7 and 14 days, cell proliferation ability and cell viability (cytotoxicity) were evaluated.
[0054] WST-8 (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., trade name: Dojindo 341-07761) was used to evaluate cell proliferation ability. The measurement method for WST-8 followed the instructions attached to the product. After 14 days, the absorbance of the sample was measured (manufactured by Hitachi High-Tech Corporation, trade name: Spectrophotometer U-3900) to quantify the cell proliferation ability. The results are shown in Table 1. Higher absorbance indicates better cell proliferation ability.
[0055] Live or dead staining (Thermofisher Scientific, product name: Catsha-puL3224) was used to assess cell viability (cytotoxicity). The live or dead staining measurement method followed the instructions attached to the product. The surface of the culture medium after 14 days was observed with an optical microscope and evaluated according to the following criteria. Comparative Example 1 will be described later. The results are shown in Table 1. A: The proportion of yellow and red areas is lower than in Comparative Example 1. B: The proportion of yellow and red areas is equivalent to that in Comparative Example 1. C: The proportion of yellow and red areas is higher than that in Comparative Example 1.
[0056] The performance of osteoblast differentiation induction (calcification) was estimated and evaluated by Alizarin Red S staining. The Raman spectrum of the culture medium after staining was measured, and the degree of staining was evaluated according to the following criteria: A: The proportion of the stained area is greater than that of Comparative Example 1. B: The proportion of the stained area is equivalent to that of Comparative Example 1. C: The proportion of the stained area is less than that of Comparative Example 1.
[0057] (Example 2) 5 g of the biomaterial of Example 1 (powder containing N-apatite as the main component) was placed in a container (Nalgene plastic bottle, 500 ml capacity), followed by the addition of 375 g of 5 mm diameter silicon nitride balls and 150 ml of ethanol. The container was then capped and crushed using the same bench ball mill used in Example 1 (rotation speed: 82 rpm, treatment time: 24 hours). The crushed powder was used as the biomaterial of Example 2. The biomaterial was evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0058] (Example 3) A biomaterial was prepared by the following procedure. 3.2 g of silicon nitride powder (manufactured by UBE Corporation, product name: E10), 10.4 g of yttria powder (manufactured by Shin-Etsu Chemical Co., Ltd., product name: UUHP), and 1.4 g of silica powder (manufactured by Kojundo Chemical Laboratory Co., Ltd.) were weighed out. The same procedure as in Example 1 was carried out except for using this raw material powder, and the Si 3 N 4 -SiO 2 -Y 2 O 3 The powder was analyzed for its components in the same manner as in Example 1. As a result, it was found that the powder contained N-wollastonite (YSiO 2 It was confirmed that the biomaterial contained N-wollastonite as the main component. On the other hand, no components other than N-wollastonite were detected. This was designated as the biomaterial of Example 3. The biomaterial of Example 3 was evaluated using the same procedures as in Example 1. The evaluation results are shown in Table 1.
[0059] Example 4 5 g of the biomaterial of Example 3 (powder containing N-wollastonite as the main component) was placed in a container (Nalgene plastic bottle, 500 ml capacity), followed by the addition of 375 g of 5 mm diameter silicon nitride balls and 150 ml of ethanol. The container was then capped and crushed in the same bench ball mill used in Example 1 (rotation speed: 82 rpm, treatment time: 24 hours). The crushed powder was used as the biomaterial of Example 4. The biomaterial was evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0060] Example 5 A biomaterial was prepared by the following procedure. 1.9 g of silicon nitride powder (manufactured by UBE Corporation, product name: E10), 12.3 g of yttria powder (manufactured by Shin-Etsu Chemical Co., Ltd., product name: UUHP), and 0.8 g of silica powder (manufactured by Kojundo Chemical Laboratory Co., Ltd.) were weighed out. The same procedure as in Example 1 was carried out except for using this raw material powder, and the Si 3 N 4 -SiO 2 -Y 2 O 3 The powder was analyzed for its components in the same manner as in Example 1. As a result, it was found that the powder contained N-YAM(Y 4 Si 2 O 7 N2 ) as the main component. On the other hand, no components other than N-YAM were detected. This was used as the biomaterial of Example 5. The biomaterial of Example 5 was evaluated using the same procedures as in Example 1. The evaluation results are shown in Table 2.
[0061] Example 6 A biomaterial was prepared by the following procedure: 5.7 g of silicon nitride powder (manufactured by UBE Corporation, product name: E10) and 9.3 g of yttria powder (manufactured by Shin-Etsu Chemical Co., Ltd., product name: UUHP) were weighed out. The same procedure as in Example 1 was carried out except for using these raw material powders, and the Si 3 N 4 -Y 2 O 3 The powder was analyzed for its components in the same manner as in Example 1. As a result, it was found that the powder contained N-melilite (Y 2 Si 3 O 3 N 4 ) as the main component. Meanwhile, no components other than N-Melilite were detected. This was designated as the biomaterial of Example 6. The biomaterial of Example 6 was evaluated using the same procedures as in Example 1. The evaluation results are shown in Table 2.
[0062] Comparative Example 1 Cell proliferation ability, cytotoxicity, and calcification were evaluated using the same procedures as in Example 1, except that no biomaterial was used in the evaluation of biocompatibility. The results of each evaluation are shown in Table 1. In the evaluation of cytotoxicity and calcification, the results of Comparative Example 1 were used as the standard for evaluation of other Examples and Comparative Examples.
[0063] (Comparative Example 2) A commercially available silicon nitride powder (manufactured by Ube Industries, Ltd., product name: E10) was used as the biomaterial of Comparative Example 2. The biomaterial of Comparative Example 2 was evaluated using the same procedures as in Example 1. The evaluation results are shown in Table 2.
[0064]
[0065]
[0066] In Tables 1 and 2, "-" indicates that the measurement was not performed. As shown in Tables 1 and 2, it was confirmed that the biomaterials of Examples 1 to 6 all had excellent cell proliferation ability and sufficiently suppressed cytotoxicity. A comparison between Examples 1 and 2 and a comparison between Examples 3 and 4 confirmed that increasing the specific surface area promoted differentiation into osteoblasts and improved antibacterial properties against gram-positive bacteria (particularly Staphylococcus epidermidis).
[0067] According to the present disclosure, a biomaterial, a powder composition, and a bone filler having excellent biocompatibility can be provided. A method for using a composition containing a complex compound as a biomaterial having excellent biocompatibility can also be provided.
[0068] 10...Part (stem).
Claims
1. A biomaterial whose main component is a complex compound having the constituent elements yttrium, oxygen, silicon, and nitrogen.
2. The composite compound is Si 3 N 4 -SiO 2 -Y 2 O 3 Compounds and Si 3 N 4 -Y 2 O 3 The biomaterial according to claim 1 , comprising at least one selected from the group consisting of cyclic compounds.
3. The composite compound is Si 3 N 4 , SiO 2 and Y 2 O 3 In the phase diagram of the three-component system, Y 5 S 3 O 12 N.Y. 2 S 3 O 3 N 4 and Y 4 S 2 O 7 N 2 The biomaterial according to claim 1 , having a composition within a triangular area having three vertices:
4. The composite compound is Y 5 S 3 O 12 N,YSiO 2 N.Y. 4 S 2 O 7 N 2 and Y 2 S 3 O 3 N 4 The biomaterial according to claim 1 , comprising at least one selected from the group consisting of:
5. It is in powder form and has a BET specific surface area of 0.3 m 2 The biomaterial according to claim 1, wherein the molecular weight is 1 / g or more.
6. The biomaterial described in claim 1, which, when dispersed in water to a concentration of 6.0 w / v% for 10 minutes, has an ammonium ion content in the liquid phase of 0.5 μg / mL or more.
7. The biomaterial according to claim 6, wherein the pH of the liquid phase is 10.0 or less.
8. A bone substitute comprising the biomaterial according to any one of claims 1 to 7.
9. A method of using a composition containing as a main component a complex compound having yttrium, oxygen, silicon and nitrogen as constituent elements as a biomaterial.
10. A composite compound having yttrium, oxygen, silicon and nitrogen as its main component and having a BET specific surface area of 0.3 m 2 / g or more.
Citation Information
Patent Citations
Method for altering the surface chemical properties of biomedical implants and related devices.
JP2015516239A
High-toughness silicon nitride-based sintered compact
JP2000247748A
Composition, manufacture and use of silicon nitride as a biomaterial for medical purposes
JP2002506711A
Antimicrobial implants for living organisms, and related materials, devices and methods
JP2020512072A
Ceramic biomaterial, biological part, and method for manufacturing the same
JP2022191863A
Cited By
Antibacterial agent, silicon nitride powder, article containing same and methods for producing same