Electrode, method for producing electrode, and electrochemical device

The electrode configuration with a three-dimensional porous current collector and optimized active material distribution addresses the capacity retention challenges in electrochemical devices, enhancing performance by improving the interaction between the current collector and active material, thus reducing resistance and ensuring effective electrolyte permeability.

WO2024204284A1PCT designated stage expired Publication Date: 2024-10-03KURARAY CO LTD

Patent Information

Application Number
PCT/JP2024/012122
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-08-25
Filing Date
2024-03-26
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Current electrochemical devices, particularly non-aqueous electrolyte secondary batteries, face challenges in achieving optimal capacity retention rates due to limitations in the design of current collectors with three-dimensional porous structures, which affect the permeability and resistance of electrodes.

Method used

The development of an electrode configuration featuring a current collector with a three-dimensional porous structure and an active material, where the average opening diameter and median diameter of the active material satisfy a specific ratio, and the current collector is filled with an active material component to achieve a high filling rate, enhancing the capacity retention rate of electrochemical devices.

Benefits of technology

This configuration improves the capacity retention rate of electrochemical devices by optimizing the interaction between the current collector and active material, reducing electrode resistance, and ensuring effective electrolyte permeability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012122_03102024_PF_FP_ABST
    Figure JP2024012122_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides an electrode comprising an active material and a current collector that has a three-dimensional porous structure, said electrode satisfying one or both of the following conditions (i) and (ii). (i) When the average opening diameter of the current collector is regarded as A (μm) and the median diameter (D50) of the active material is regarded as B (μm), A and B satisfy the relationship of expression (1). (1): 0.10 ≤ B / A ≤ 2.00 (ii) The current collector is filled with an active material component containing the active material, and the filling rate (%) defined by formula (2) is not less than 37%. (2): Filling rate (%) = β / (α-γ) × 100, wherein α represents the observed area of the current collector which is determined from an electron micrograph of a cross section of the electrode in the thickness direction, and β and γ respectively represent the projected areas of the active material and the current collector in the observed area which are calculated using image analysis software.
Need to check novelty before this filing date? Find Prior Art

Description

Electrode, method of manufacturing electrode, and electrochemical device Related Applications

[0001] This application claims priority to Japanese Patent Application No. 2023-056012 filed on March 30, 2023 and Japanese Patent Application No. 2023-137490 filed on August 25, 2023, the entire contents of which are incorporated herein by reference.

[0002] The present invention relates to an electrode useful for electrochemical devices and the like, a method for producing the same, and an electrochemical device.

[0003] In recent years, various electrochemical devices have been developed in response to the widespread use of small terminals such as smartphones and laptop computers, as well as electric and hybrid vehicles. In particular, the use of non-aqueous electrolyte secondary batteries, typified by lithium-ion secondary batteries, has become widespread, and efforts are being made to reduce their size and weight for in-vehicle applications.

[0004] For example, Patent Document 1 (WO 2022 / 118692) describes a conductive material having a three-dimensional porous structure, and an air permeability of 0.1 to 600 cc / cm 2 This publication discloses an electrode using a current collector having a current density of 100 μm / s and a thickness of less than 100 μm. This electrode can be made thin, the electrode resistance can be sufficiently reduced, and good charge / discharge characteristics can be obtained.

[0005] International Publication No. 2022 / 118692

[0006] However, although Patent Document 1 describes that the air permeability of the current collector is controlled from the viewpoint of improving the permeability of the electrolyte solution, and that the resistance of the electrode is reduced by making the current collector thinner, there is still room for improvement in order to obtain practical output performance in the current collector, particularly in a current collector having a three-dimensional porous structure.

[0007] In view of the above problems, an object of the present invention is to provide an electrode that can improve the capacity retention rate of an electrochemical device.

[0008] As a result of extensive research, the present inventors have found that the above-mentioned problems can be solved by constructing an electrode having the following configuration, and have completed the present invention through further research based on this finding. That is, the present invention may include the following aspects.

[0009] [Aspect 1] An electrode including a current collector and an active material, wherein the current collector has a three-dimensional porous structure with an average pore size A, and the active material has a median pore size (D 50 ) B, and the average opening diameter A (μm) and the median diameter (D 50 ) B (μm) satisfies the relationship of the following formula (1): 0.10≦B / A≦2.00 (1) (B / A is preferably 0.13 or more, more preferably 0.15 or more, and preferably 1.96 or less, more preferably 1.70 or less, even more preferably 1.50 or less, and particularly preferably 1.20 or less.) [Aspect 2] The electrode according to aspect 1, wherein the current collector is filled with an active material component containing the active material, and the filling rate (%) determined by the following formula (2) is 37% or more: Filling rate (%)=β / (α−γ)×100 (2) In the formula, α represents the observation area, which is determined by multiplying the thickness of the current collector by the observation length, as determined from an electron microscope photograph (SEM image) of a cross section of the electrode in the thickness direction, and β and γ represent the projected areas of the active material and the current collector (solid phase portion of the current collector) within the observation area, respectively, as calculated using image analysis software.

[0010] [Embodiment 3] An electrode comprising a current collector having a three-dimensional porous structure, the current collector being filled with an active material component containing an active material, and having a filling rate (%) determined by the following formula (2) of 37% or more (preferably 45% or more): Filling rate (%) = β / (α - γ) × 100 (2) In the formula, α represents the observed area, which is determined by multiplying the current collector thickness by the observed length, as determined from an electron microscope photograph of a cross section of the electrode in the thickness direction, and β and γ represent the projected areas of the active material and the current collector (solid phase portion of the current collector), respectively, within the observed area, as calculated using image analysis software.

[0011] [Aspect 4] In the electrode according to aspect 3, the current collector has an average opening diameter A, and the active material has a median diameter (D 50 ) B, and the average opening diameter A (μm) and the median diameter (D 50 ) An electrode in which B (μm) satisfies the relationship of the following formula (1): 0.10≦B / A≦2.00 (1) (B / A is preferably 0.13 or more, more preferably 0.15 or more, and preferably 1.96 or less, more preferably 1.70 or less, even more preferably 1.50 or less, and particularly preferably 1.20 or less).

[0012] [Aspect 5] The electrode according to any one of Aspects 1 to 4, wherein the current collector has a thickness of 100 μm or less (e.g., 5 to 80 μm, more preferably 5 to 60 μm, even more preferably 5 to 45 μm, and particularly preferably 10 to 30 μm). [Aspect 6] The current collector has an air permeability of 0.1 to 600 cc / cm 2 / sec (preferably 1 cc / cm 2 / sec or more, more preferably 10 cc / cm 2 / sec or more, and preferably 500 cc / cm 2 / sec or less, more preferably 400 cc / cm 2 6. The electrode of any one of aspects 1 to 5, wherein the electrical resistance is less than or equal to 1 / second.

[0013] [Aspect 7] The electrode according to any one of Aspects 1 to 6, wherein the current collector comprises a non-conductive structure and a metal coating. [Aspect 8] The electrode according to Aspect 7, wherein the non-conductive structure comprises a fiber assembly having an average fiber diameter of 10 μm or less. [Aspect 9] The electrode according to Aspect 8, wherein the fiber assembly is a non-woven fabric.

[0014] [Aspect 10] The electrode according to any one of Aspects 7 to 9, wherein the metal coating comprises at least one metal selected from the group consisting of aluminum, copper, nickel, gold, and silver. [Aspect 11] The electrode according to any one of Aspects 1 to 10, wherein the active material is capable of absorbing and releasing electrolyte ions.

[0015] [Aspect 12] The electrode according to any one of Aspects 1 to 11, further comprising a conductive material. [Aspect 13] The electrode according to any one of Aspects 1 to 12, wherein the active material has a median diameter of 0.1 to 100 μm, for example, 0.1 to 16 μm. [Aspect 14] The electrode according to any one of Aspects 1 to 13, wherein the current collector is filled with an active material component comprising the active material and a water-insoluble binder.

[0016] Aspect 15: A method for producing an electrode according to any one of Aspects 1 to 14, comprising at least the steps of: preparing a current collector having a three-dimensional porous structure with an average pore size A; and forming an active material layer containing an active material with a median size B on the current collector, wherein the average pore size A and the median size B satisfy the following formula (1): 0.10≦B / A≦2.00 (1) (B / A is preferably 0.13 or more, more preferably 0.15 or more, and preferably 1.96 or less, more preferably 1.70 or less, even more preferably 1.50 or less, and particularly preferably 1.20 or less).

[0017] [Aspect 16] The method for producing an electrode according to any one of Aspects 1 to 14, comprising at least the step of filling an active material component into a current collector having a three-dimensional porous structure. [Aspect 17] The air permeability of the current collector before filling with the active material component is 0.1 to 600 cc / cm 2 A method for producing an electrode according to Aspect 16, wherein the current collector has a thickness of 100 μm or less before being filled with an active material component. Aspect 18: A method for producing an electrode according to Aspect 16 or Aspect 17, wherein the current collector has a thickness of 100 μm or less before being filled with an active material component. Aspect 19: An electrochemical device comprising the electrode according to any one of Aspects 1 to 14.

[0018] It should be noted that any combination of at least two elements disclosed in the claims and / or the specification is included in the present invention, and in particular any combination of two or more of the claims described in the claims is included in the present invention.

[0019] According to the electrode of the present invention, the capacity retention rate of an electrochemical device including this electrode can be improved.

[0020] The present invention will be more clearly understood from the following description of preferred examples taken in conjunction with the accompanying drawings. However, the examples and drawings are merely for illustration and explanation purposes and should not be used to define the scope of the present invention. The scope of the present invention is defined by the appended claims.

[0023] Figure 1 is a micrograph (200x magnification) illustrating a method for measuring the average opening diameter in a current collector according to a first embodiment of the present invention.

[0024] Figure 2 is a scanning electron micrograph (2000x magnification) of an electrode cross section to illustrate a method for measuring the packing ratio in an electrode according to a second embodiment of the present invention.

[0025] Figure 3 is a schematic diagram illustrating the location of a current collector and active material in the observation area in the scanning electron micrograph of Figure 2.

[0026] Figure 4 is a schematic cross-sectional view showing an example of the configuration of an electrochemical device.

[0021] The electrode of the present invention is an electrode including a current collector having a three-dimensional porous structure and an active material, and satisfies either one or both of the following conditions (i) and (ii): (i) the average pore size of the current collector is A (μm), and the median diameter of the active material (D 50 ) is B (μm), A and B satisfy the relationship of the following formula (1): 0.10≦B / A≦2.00 (1) (ii) The current collector is filled with an active material component containing an active material, and the filling rate (%) determined by the following formula (2) is 37% or more: Filling rate (%)=β / (α−γ)×100 (2) In the formula, α represents the observed area of ​​the current collector determined from an electron microscope photograph (SEM image) of a cross section in the thickness direction of the electrode, and β and γ represent the projected areas of the active material and the current collector (solid phase portion of the current collector) within the observed area, respectively, calculated using image analysis software.

[0022] The electrode of the present invention is suitable as an electrode for an electrochemical device. Electrochemical devices include secondary batteries such as lithium ion secondary batteries, nickel-metal hydride secondary batteries, and nickel-cadmium secondary batteries, and capacitors such as electric double layer capacitors. Among these, the electrochemical device may particularly be a nonaqueous electrolyte secondary battery (e.g., a lithium ion secondary battery, a sodium ion battery, a lithium-sulfur battery, a lithium-air battery, an all-solid-state battery, an organic radical battery, etc.), and more preferably a lithium ion secondary battery. The following description will be given using an electrode for a nonaqueous electrolyte secondary battery as an example.

[0023] First Embodiment [Current Collector] The current collector is a conductive body having a three-dimensional porous structure (hereinafter, sometimes referred to as a three-dimensional porous structure or simply a porous structure), where the three-dimensional porous structure means a structure having porosity in which voids are distributed in a three-dimensional space. The current collector has an average opening diameter A, which is the average of the opening diameters of a plurality of openings formed by this porous structure.

[0024] (Three-dimensional porous structure) To realize a three-dimensional porous structure, the current collector can be constructed using a fibrous structure (fiber aggregate) such as a woven fabric or nonwoven fabric (including paper), or a resin foam such as urethane foam. There is no limitation on the method for obtaining a conductive body having a porous structure as the current collector, and the porous conductive body may be formed from a known conductive material used in electrodes. The porous conductive body may be in the form of a nonwoven fabric. Furthermore, when the conductive body having a three-dimensional porous composite structure is composed of a non-conductive structure and a metal coating formed on the non-conductive structure, the non-conductive structure is not particularly limited and may be a known resin foam or a fiber structure (e.g., a woven fabric or non-woven fabric) made of non-conductive fibers.

[0025] FIG. 1 is a micrograph illustrating a method for measuring the average pore size of a current collector according to one embodiment of the present invention. For a three-dimensional porous structure, a sample is first cut out to a predetermined shape in the plane direction of the current collector. Taking into account the penetration of the active material into the current collector, a portion of the current collector from its surface to a predetermined depth (e.g., 100 μm or less) in the thickness direction may be peeled off and measured, but typically the thickness of the current collector itself may also be measured. The cut-out sample can then be placed on a base (e.g., a black flat plate) and photographed to obtain a magnified image.

[0026] Using Figure 1 as an example, Figure 1 is an enlarged photograph showing a cut-out sample sandwiched between glass slides and then placed on a black flat plate. As shown in the photograph, the fiber materials constituting the sample overlap each other in the depth (thickness) direction. On the other hand, spaces where no fiber material is present, i.e., spaces where the base portion can be seen, can function as through-holes in the depth direction. In this case, the average opening diameter of the current collector is determined by considering the space in the base portion surrounded by the fiber material as the through-hole. Therefore, the diameter of a circle having the area determined by the image of each through-hole can be calculated, and the average of the diameters of the through-holes can be considered as the average opening diameter.

[0027] The number of through holes to be measured is determined appropriately depending on the size of the through holes in the sample, and if large through holes are present in the image, the number of through holes used for measurement will be reduced. Typically, an average value is calculated using 500 to 5,000 through holes.

[0028] The area of ​​the through-hole is set to 2 μm in order to reduce measurement errors. 2The average area value of the through holes observed in an area of ​​0.5 μm or more may be adopted. Furthermore, when the current collector is a fiber structure, the fibers themselves may be shiny and black in some cases. In such a case, in order to distinguish the shiny black part of the fiber from the through holes that are recognizable by the black color of the flat black plate on the black background, the area of ​​a square having a length of 0.5 times the average fiber diameter of the fibers as a threshold may be used, and the area of ​​the black part larger than this may be used as the area of ​​the through holes. For example, when the average fiber diameter of the fibers constituting the fiber structure is 4 μm, a 4 μm square corresponding to a square area of ​​2 μm on a side may be used. 2 The average area value of the through holes observed in the above area may be used.

[0029] When measuring the image of an enlarged photograph, it is preferable to binarize the image. For example, an image analysis software (Keyence Corporation's "Multi-File Analysis Application") can be used to distinguish between black parts and other parts, thereby making it possible to use a binarized image.

[0030] Preferably, from the viewpoint of improving the permeability of the electrolyte, the air permeability of the current collector is 0.1 to 600 cc / cm 2 / second. Since there is thought to be a correlation between the air permeability of the current collector and the permeability of the electrolyte, if the air permeability of the current collector is high, the permeability of the electrolyte can be improved, ionic conductivity can be ensured, and as a result, the electrode resistance can be reduced. On the other hand, if the air permeability of the current collector is low, the mechanical strength of the porous structure can be improved, and the durability of the current collector and the stability of electrode production can be improved.

[0031] The air permeability of the current collector is 0.1 cc / cm 2 / sec or more is preferable, and 1 cc / cm 2 / sec or more is more preferable, and 10 cc / cm 2 On the other hand, the air permeability of the current collector is preferably 600 cc / cm 2 / sec or less is preferable, and 500cc / cm 2 / sec or less is more preferable, and 400 cc / cm 2 For example, the air permeability of the current collector is 0.1 to 600 cc / cm 2 / sec, preferably 1 to 500 cc / cm2 / sec, and more preferably 10 to 400 cc / cm 2 The air permeability of the current collector can be measured by the method described in the Examples below. When measuring the air permeability of a current collector disposed inside an electrode, the air permeability may be measured after removing the active material components and the like from the current collector using a solvent or the like.

[0032] The current collector may have a thickness of 100 μm or less. A thin current collector can produce a battery with a high charge / discharge capacity per unit volume. Therefore, the current collector thickness is preferably 80 μm or less, more preferably 60 μm or less, even more preferably 45 μm or less, even more preferably 40 μm or less, and most preferably 30 μm or less. While there is no particular lower limit for the current collector thickness, from the viewpoint of avoiding breakage during battery manufacturing and handling, a thickness of 5 μm or more is preferred, and 10 μm or more is even more preferred. For example, the current collector thickness may be preferably 5 to 80 μm, more preferably 5 to 60 μm, even more preferably 5 to 45 μm, and particularly preferably 10 to 30 μm. Here, the current collector thickness can be measured, for example, from a scanning electron microscope (SEM) image of a cross section of the electrode in the thickness direction. Specifically, it can be a value measured by the method described in the Examples below.

[0033] The weight of the current collector is, for example, 1.0 to 50 g / m 2 The smaller the basis weight of the current collector, the higher the air permeability and the thinner the current collector can be made. 2 Preferably, the weight is 12 g / m or less. 2 More preferably, it is 10 g / m or less. 2 From the viewpoint of the mechanical strength of the current collector, the larger the basis weight, the more preferable. 2 More than 2.0 g / m is preferable. 2 More preferably, 3.0 g / m or more 2 Therefore, the weight per unit area of ​​the current collector is 1.0 to 30 g / m 2is preferable, and more preferably 1.0 to 20 g / m 2 and more preferably 1.0 to 15 g / m 2 and particularly preferably 2.0 to 12 g / m 2 and more preferably 3.0 to 10 g / m 2 may be.

[0034] The current collector may be a structure having a non-conductive porous structure (hereinafter, sometimes referred to as a non-conductive porous structure) that is composited with a metal coating formed by a technique such as plating, thereby imparting conductivity to the non-conductive porous structure.

[0035] When the conductive body having a three-dimensional porous composite structure is composed of a non-conductive structure and a metal coating, the non-conductive structure is not particularly limited and may be a known resin foam or a fiber structure made of non-conductive fibers. Preferably, the conductive body as a current collector may be a conductive body having a three-dimensional porous composite structure in which a metal coating is formed on a non-conductive porous structure (particularly a non-conductive fiber structure) to form a composite.

[0036] Examples of non-conductive fibers include polyolefin fibers, cellulose fibers, (meth)acrylic fibers, polyvinyl alcohol fibers, vinyl chloride fibers, styrene fibers, polyester fibers, polyamide fibers, polycarbonate fibers, and urethane fibers. Among these fibers, from the viewpoint of exhibiting the aforementioned strength, polyester fibers such as polyethylene terephthalate fibers, polybutylene terephthalate fibers, polytrimethylene terephthalate fibers, and melt-liquid crystal-forming aromatic polyester fibers are preferably used. Among these, polyester fibers such as melt-liquid crystal-forming aromatic polyester fibers (e.g., melt-liquid crystal-forming wholly aromatic polyester fibers) are particularly preferably used.

[0037] The liquid-crystalline aromatic polyesters constituting the liquid-crystalline aromatic polyester fibers, particularly the liquid-crystalline wholly aromatic polyesters, are resins with excellent heat resistance and chemical resistance. In this specification, "liquid-crystalline" refers to the property of exhibiting optical anisotropy (liquid crystallinity) in the molten phase, and "liquid-crystalline aromatic polyesters" refers to polyesters that exhibit liquid-crystalline properties. The "liquid-crystalline" property can be confirmed, for example, by placing a sample on a hot stage, heating it under a nitrogen atmosphere, and observing the transmitted light through the sample. Liquid-crystalline aromatic polyesters are composed of repeating structural units derived from, for example, aromatic diols, aromatic dicarboxylic acids, aromatic hydroxycarboxylic acids, etc., and the structural units derived from aromatic diols, aromatic dicarboxylic acids, and aromatic hydroxycarboxylic acids are not particularly limited in terms of their chemical structure, as long as the effects of the present invention are not impaired. Furthermore, the liquid-crystalline aromatic polyesters may contain structural units derived from aromatic diamines, aromatic hydroxyamines, or aromatic aminocarboxylic acids, provided that the effects of the present invention are not impaired. For example, preferred structural units are shown in Table 1.

[0038]

[0039] Each Y is independently a substituent that may be substituted in the range of 1 to the maximum number that can be substituted on the aromatic ring or cyclo ring, and specifically, each Y is independently a substituent selected from a hydrogen atom, a halogen atom (e.g., a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, etc.), an alkyl group (e.g., an alkyl group having 1 to 4 carbon atoms such as a methyl group, an ethyl group, an isopropyl group, a t-butyl group, etc.), an alkoxy group (e.g., a methoxy group, an ethoxy group, an isopropoxy group, a n-butoxy group, etc.), an aryl group (e.g., a phenyl group, a naphthyl group, etc.), an aralkyl group [e.g., a benzyl group (phenylmethyl group), a phenethyl group (phenylethyl group), etc.], an aryloxy group (e.g., a phenoxy group), and an aralkyloxy group (e.g., a benzyloxy group, etc.).

[0040] More preferred structural units include the structural units described in Examples (1) to (18) shown in the following Tables 2, 3, and 4. When the structural unit in the formula is a structural unit that can exhibit multiple structures, two or more of such structural units may be combined and used as a structural unit that constitutes the polymer.

[0041]

[0042] In the structural units of Tables 2, 3 and 4, n is an integer of 1 or 2, and each structural unit n=1 and n=2 may exist alone or in combination; Y 1 and Y 2 may each independently represent a hydrogen atom, a halogen atom (e.g., a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, etc.), an alkyl group (e.g., an alkyl group having 1 to 4 carbon atoms such as a methyl group, an ethyl group, an isopropyl group, a t-butyl group, etc.), an alkoxy group (e.g., a methoxy group, an ethoxy group, an isopropoxy group, an n-butoxy group, etc.), an aryl group (e.g., a phenyl group, a naphthyl group, etc.), an aralkyl group [e.g., a benzyl group (phenylmethyl group), a phenethyl group (phenylethyl group), etc.], an aryloxy group (e.g., a phenoxy group), an aralkyloxy group (e.g., a benzyloxy group, etc.), etc. Among these, preferred Y 1 and Y 2 Examples of the aryl group include a hydrogen atom, a chlorine atom, a bromine atom, and a methyl group.

[0043] Examples of Z include substituents represented by the following formulas.

[0044]

[0045] Among these, the melt liquid crystalline wholly aromatic polyester used in the present invention preferably has a composition containing parahydroxybenzoic acid and 6-hydroxy-2-naphthoic acid as main components, or a composition containing parahydroxybenzoic acid, 6-hydroxy-2-naphthoic acid, terephthalic acid, and biphenol as main components.

[0046] The nonwoven fabric containing the molten liquid-crystalline aromatic polyester is preferably a meltblown nonwoven fabric obtained by the meltblown method. The meltblown method can be a known method, for example, in which a molten molten liquid-crystalline aromatic polyester is discharged as a molten polymer from a plurality of nozzle holes arranged in a row, high-temperature, high-velocity air is sprayed from a gas injection port installed adjacent to an orifice die to finely fiberize the discharged molten polymer, and the fiber stream is then collected on a conveyor net or other collector to produce a nonwoven fabric. To impart heat resistance, the resulting nonwoven fabric can also be subjected to a heat treatment. The heating temperature is preferably at least the melting point of the molten liquid-crystalline wholly aromatic polyester minus 40°C and not more than the melting point of the molten liquid-crystalline wholly aromatic polyester plus 20°C, and the heat treatment is preferably carried out for at least 3 hours. The gas used as the heating medium during the heat treatment can be a mixture of nitrogen, oxygen, argon, carbon dioxide, or air, but oxygen or air is more preferred from a cost perspective. The heat treatment may be carried out either under tension or without tension, depending on the purpose.

[0047] The melt viscosity of the molten liquid crystal-forming aromatic polyester at 310 ° C is preferably 20 Pa s or less. If the melt viscosity at 310 ° C exceeds 20 Pa s, it is difficult to form ultrafine fibers, and this is not preferred due to the generation of oligomers during polymerization, and problems during polymerization and granulation. On the other hand, if the melt viscosity is too low, it is also difficult to form fibers, and it is desirable for the melt viscosity to be 5 Pa s or more at 310 ° C. The melt viscosity of this molten liquid crystal-forming aromatic polyester at 310 ° C refers to a value measured using, for example, a melt indexer (manufactured by Takara Kogyo Co., Ltd.: L244).

[0048] If necessary, commonly used additives such as colorants, inorganic fillers, antioxidants, and ultraviolet absorbers, as well as thermoplastic elastomers, may be added to the above-mentioned liquid crystalline aromatic polyester within the range that does not impair the functions of the present invention (for example, 10% by weight or less).

[0049] Among the fiber structures, nonwoven structures are preferred from the viewpoints of avoiding complex manufacturing processes, maintaining strength and flexibility, and controlling contact points during metal coating formation. Examples of nonwoven fabrics include nonwoven fabrics formed by wet or dry methods, meltblown nonwoven fabrics, spunlace nonwoven fabrics, thermally bonded nonwoven fabrics, and nonwoven fabrics formed by needle punching. Among these nonwoven fabrics, it is preferable to use long fibers with a small fiber diameter, and meltblown nonwoven fabrics are preferred. In particular, when a conductive nonwoven fabric comprising a meltblown nonwoven fabric formed using a molten liquid-crystalline aromatic polyester and a metal coating formed on the nonwoven fabric is used as a conductive body, the aforementioned thin current collector can be obtained.

[0050] Specifically, the average fiber diameter of the fibers constituting the nonwoven fabric is preferably 10 μm or less, for example, in the range of 0.1 to 10 μm. If the average fiber diameter is less than 0.1 μm, fly lint is likely to occur and form fiber clumps, while if the average fiber diameter exceeds 10 μm, the fabric texture becomes coarse, resulting in insufficient conductivity when metal coated. When a meltblown nonwoven fabric is used as the nonwoven fabric, the average fiber diameter of the fibers constituting the meltblown nonwoven fabric is preferably in the range of 0.5 to 8 μm, more preferably in the range of 0.5 to 7 μm, and even more preferably in the range of 1 to 6 μm. The average fiber diameter of the fibers constituting the meltblown nonwoven fabric in the present invention refers to the average value of the diameters of 100 randomly selected fibers measured in a magnified photograph of the nonwoven fabric taken with a scanning electron microscope.

[0051] When a nonwoven fabric is used in a three-dimensional porous structure, it is preferable to use a melt-blown nonwoven fabric containing such a liquid crystal-forming aromatic polyester as a main component.

[0052] (Metal Coating) When the conductive body of the present invention is a non-conductive structure provided with a metal coating, the metal coating is preferably a metal coating coated on a fiber structure, particularly a nonwoven fabric-like structure (specifically, coated on fibers constituting a fiber structure such as a nonwoven fabric), from the viewpoints of avoiding complex manufacturing processes, maintaining strength and flexibility, and controlling contact points during metal coating formation. The metal coating preferably contains copper, nickel, gold, silver, or aluminum. These metals may be used alone or in combination. Among these, laminated coatings containing copper, nickel, gold, or aluminum are particularly preferred in terms of high conductivity and ease of forming a metal coating. Among these, copper, nickel, and aluminum are particularly preferred metal coatings in terms of economy and high conductivity. These metal coatings may be formed in multiple layers. For example, a first metal layer may be formed on the non-conductive structure, and a second metal layer may be further formed on the first metal layer.

[0053] The surface resistance of the conductive body of the present invention may vary depending on the type and thickness of the metal coating. However, from the viewpoint of ensuring sufficient conductivity, the surface resistance is set to 10 -3 ~10 0 It is preferably in the range of 10 -3 ~10 -1 It is more preferable that the resistance is in the range of Ω / □.

[0054] As a method for forming a metal coating, conventionally known methods such as electroplating, electroless plating, sputtering, and vacuum deposition can be used, but electroless plating is preferred from the viewpoint of easily obtaining high conductivity. As a method for electroless plating, conventionally known methods can be used and are not particularly limited, but a common method is to apply a catalyst to a non-conductive structure (e.g., the fiber surface of a nonwoven fabric) that serves as a substrate, and then immerse the structure in a chemical plating bath in which a metal salt, a reducing agent, and a buffer agent are dissolved, thereby forming a metal coating.

[0055] The thickness of the metal coating in the current collector (electrically conductive material) of the present invention may be, for example, in the range of 0.05 to 10 μm, or in the range of 0.1 to 5 μm, but from the viewpoint of controlling the air permeability of the current collector while imparting the above-mentioned surface resistivity, it is more preferably 4 μm or less, or 2 μm or less. If the thickness of the metal coating is less than 0.05 μm, sufficient conductivity cannot be obtained, while if the thickness of the metal coating is more than 10 μm, the flexibility and pliability of the current collector are impaired, which is undesirable.

[0056] When forming a metal coating, for example, the air permeability is 0.2 to 800 cc / cm 2 / sec., a metal film is formed on a non-conductive structure having an air permeability of 0.1 to 600 cc / cm 2 / sec.

[0057] For example, the non-conductive structure (for example, a non-conductive meltblown nonwoven fabric) has an air permeability of 0.2 to 800 cc / cm 2 It is preferable that the air permeability of the non-conductive structure is 800 cc / cm 2 If the air permeability exceeds 800 cc / cm / s, it becomes difficult to set the air permeability of the current collector within the above range, and as a result, it becomes difficult to achieve the desired reduction in resistance. 2 / sec or less, and 700 cc / cm 2 / sec or less, and more preferably 600 cc / cm 2 Further, the lower limit of the air permeability of the non-conductive structure is not particularly limited, but from the viewpoint of ensuring mechanical strength and electrical conductivity after metal coating, it is preferable that the lower limit be 0.2 cc / cm 2 / sec or more, and 1 cc / cm 2 More preferably, it is equal to or greater than 1 / second.

[0058] Furthermore, the thickness of the non-conductive structure (e.g., a non-conductive meltblown nonwoven fabric) is preferably in the range of 5 μm or more and less than 100 μm. If the thickness of the non-conductive structure is less than 5 μm, it tends to be easily broken during battery manufacturing and handling, and if the thickness of the non-conductive structure is 100 μm or more, the demand for a thinner current collector cannot be met. Therefore, the thickness of the non-conductive structure is preferably in the range of 5 μm or more and less than 100 μm, more preferably in the range of 7 to 30 μm, and even more preferably in the range of 9 to 20 μm. The above description of the current collector also applies to the electrode of the second embodiment.

[0059] [Active Material] The electrode of the present invention includes a current collector and an active material, and may include a conductive agent and / or a binder as needed. The active material is capable of absorbing and releasing electrolyte ions and has a predetermined median diameter (D 50 ) has a median diameter (D 50 ) represents the particle diameter at which the cumulative volume from the fine particle side in the particle size distribution measured by laser scattering method is 50%, and particles with larger particle diameters and particles with smaller particle diameters exist in equal volumes across this particle diameter boundary. The preferred median diameter of the active material varies depending on the embodiment of the electrode, but may be 0.1 to 100 μm from the viewpoint of achieving both suppression of side reactions during charge and discharge, electrode formability, and coatability of the active material layer (sometimes referred to as the active material component layer). The above explanation is also applicable to the electrode of the second embodiment.

[0060] [First Embodiment of Electrode] In one embodiment of the electrode of the present invention, it is preferable that the average opening diameter of the current collector and the median diameter of the active material satisfy a predetermined relationship. That is, when the average opening diameter of the current collector is A (μm) and the median diameter of the material is B (μm), if B / A satisfies the relationship of the following formula (1), the active material can be efficiently inserted into the openings of the current collector, and the capacity retention rate of the resulting electrochemical device can be improved: 0.10≦B / A≦2.00 (1)

[0061] The smaller the B / A value, the larger the average opening diameter of the current collector relative to the particle size of the active material, allowing for a larger proportion of the active material to penetrate the openings of the current collector, resulting in a larger contact area between the active material and the current collector. This reduces the resistance of the electrochemical device and improves the capacity retention rate. However, if B / A is too small, the active material will clog the current collector excessively, increasing the electrolyte transfer resistance. This will increase the resistance of the electrochemical device and reduce the capacity retention rate. Therefore, it is undesirable for B / A to be below the lower limit of 0.10.

[0062] The larger the B / A value, the more effectively the electrochemical device resistance can be reduced by preventing increases in the interfacial resistance between the active materials and the electrolyte transfer resistance for a current collector with the same opening diameter. However, if the B / A value exceeds the upper limit of 2.00, the proportion of active material that penetrates the openings in the current collector decreases, and the contact area with the current collector decreases. As a result, it becomes difficult to improve the capacity retention rate of the electrochemical device.

[0063] The value of B / A may be preferably 0.13 or more, more preferably 0.15 or more, and even more preferably 0.20 or more. On the other hand, the value of B / A may be preferably 1.96 or less, more preferably 1.70 or less, even more preferably 1.50 or less, and particularly preferably 1.20 or less. For example, B / A may be 0.13 to 1.96, 0.15 to 1.70, 0.20 to 1.50, or 0.20 to 1.20.

[0064] The preferred range varies as appropriate depending on the relationship with the median diameter of the active material, but the average opening diameter A may be, for example, 1 to 100 μm, more preferably 5 to 50 μm, and even more preferably 10 to 20 μm, in terms of ease of forming a metal film and permeability of the electrolyte.

[0065] In the present embodiment, the preferred range of the median diameter B of the active material varies as appropriate depending on the relationship with the average opening diameter of the current collector. However, from the viewpoint of suppressing side reactions during charge and discharge, and achieving both electrode formability and coatability of the active material layer, for example, the median diameter B of the active material may be 0.1 to 100 μm, more preferably 1 to 50 μm, and even more preferably 2 to 30 μm.

[0066] [Positive Electrode] The positive electrode active material is not particularly limited as long as it has a predetermined average diameter in relation to the current collector, and known positive electrode active materials can be used. Positive electrode active materials capable of absorbing and releasing electrolyte ions include layered oxides (LiMO). 2 or NaMO 2 where M is a metal, for example, LiCoO 2 , LiNiO 2 , LiMnO 2 , NaFeO 2 , NaNiO 2 , NaCoO 2 , NaMnO 2 , NaVO 2 or LiNixCoyMnO 2 , NaNixMnzO 2 (where x, y, and z represent the composition ratio), olivine-based (LiMPO 4 or NaMPO 4 where M is a metal, for example LiFePO 4 , NaFePO 4 etc.), spinel type (LiM 2 O 4 or NaM 2 O 4 where M is a metal, for example LiMn 2 O 4 , NaMn 2 O 4 complex metal chalcogen compounds such as Li 1+x Mn 2-x O 4 (0<x<2) Lithium-rich spinel compounds represented by Li[Ni 0.17 Li 0.2 Co 0.07 Mn 0.56 ]O 2 , LiNi0.5 Mn 1.5 O 4 Examples of the positive electrode active material include organic radicals such as metal oxides such as those mentioned above, phosphate-containing compounds, polyanion-containing compounds, Prussian blue analogs, sulfur, compounds or polymers having a nitroxyl radical, compounds or polymers having an oxy radical, compounds or polymers having a nitrogen radical, and compounds or polymers having a fulvalene skeleton. These positive electrode active materials can be used alone or in combination of two or more. Among these, composite metal chalcogen compounds are preferred. Furthermore, when constructing a battery using electrostatic adsorption such as a lithium ion capacitor, examples of the positive electrode active material include carbon materials and inorganic materials having a high specific surface area, such as activated carbon, mesoporous carbon, and conductive ceramics such as defective titanium oxide.

[0067] The positive electrode active material may be applied to a current collector as a positive electrode slurry to form a positive electrode active material layer. The content of the positive electrode active material in the positive electrode active material layer is preferably 80.0 to 99.9 wt %, more preferably 90 to 99.5 wt %, based on the total weight of the positive electrode active material layer (or the total weight of the solid content of the slurry).

[0068] The positive electrode active material layer may include the positive electrode active material described above, a binder, and optionally a conductive material (conductive additive). The content of the binder in the positive electrode active material layer may be 1 wt % to 5 wt % based on the total weight of the positive electrode active material layer. When a conductive material is further included, the positive electrode active material may be used in an amount of 90 wt % to 98 wt %, 1 wt % to 5 wt % of the binder, and 1 wt % to 5 wt % of the conductive material. When the positive electrode active material layer includes a binder, a conductive material (conductive additive), and the like in addition to the positive electrode active material, the solid components including these may be referred to as a positive electrode active material component, and the positive electrode active material layer may be referred to as a positive electrode active material component layer.

[0069] The binder serves to effectively adhere the positive electrode active material particles to each other and to the current collector. The binder may be a water-insoluble binder, a water-soluble binder, or a combination thereof.

[0070] Examples of the water-insoluble binder include polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamideimide, polyimide, styrene-butadiene rubber, acrylated styrene-butadiene rubber, copolymers of (meth)acrylic acid and (meth)acrylic acid alkyl esters, copolymers of olefins having 2 to 8 carbon atoms and maleic acid, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, copolymers of propylene and olefins having 2 to 8 carbon atoms, polyamideimide, polyimide, and combinations thereof.

[0071] Examples of the water-soluble binder include polyvinyl alcohol, a copolymer of vinyl alcohol and an ethylenically unsaturated carboxylic acid and an alkali metal modified product thereof, an alkali metal modified copolymer of an alkene having 2 to 4 carbon atoms and an ethylenically unsaturated carboxylic acid, an alkali metal modified copolymer of an alkene having 2 to 4 carbon atoms and maleic anhydride, and sodium poly(meth)acrylate.

[0072] The positive electrode may further include a cellulose-based compound as a thickener, which can impart viscosity. The cellulose-based compound may be a mixture of one or more of carboxymethyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose, or alkali metal salts thereof. The alkali metal may be sodium, potassium, or lithium. The amount of the thickener used may be 0.1 to 3 parts by weight per 100 parts by weight of the active material.

[0073] The conductive material is used to impart conductivity to the electrode, and any electron-conductive material that does not undergo chemical change in the battery that is constructed can be used. Examples of such a conductive material include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, and carbon fiber; metal-based materials such as metal powder or metal fiber of copper, nickel, aluminum, silver, and the like; conductive polymers such as polyphenylene derivatives; and conductive materials containing mixtures of these.

[0074] As the solvent used for the positive electrode slurry, for example, an organic solvent can be used, and among them, a polar organic solvent capable of dissolving the binder described below is preferred. Specifically, as the organic solvent, acetonitrile, N-methylpyrrolidone, acetylpyridine, cyclopentanone, N,N-dimethylacetamide, dimethylformamide, dimethyl sulfoxide, methylformamide, methyl ethyl ketone, furfural, ethylenediamine, etc. can be used. Among these, N-methylpyrrolidone (NMP) is most preferred from the viewpoints of ease of handling, safety, ease of synthesis, etc. Note that these organic solvents may be used alone or in combination of two or more.

[0075] The amount of the solvent used is such that the solid content concentration in the positive electrode slurry is preferably 1 to 80 wt %, more preferably 5 to 70 wt %, and even more preferably 10 to 60 wt %. By setting the solid content concentration within the above range, the positive electrode active material and other components contained therein can be uniformly dispersed, which is preferable.

[0076] The positive electrode slurry can be produced by mixing the positive electrode active material and other components, if necessary, in the solvent. There are no particular limitations on the mixing method, and a general mixing device such as a disperser, mill, or kneader can be used. For example, stirring for 20 minutes to 120 minutes is preferred.

[0077] The temperature at which the mixture is mixed is not particularly limited, and is, for example, in the range of 0° C. to 160° C., more preferably in the range of 20° C. to 80° C. An excessively low temperature is undesirable because the viscosity becomes too high and coating becomes impossible, while an excessively high temperature is undesirable from the viewpoints of safety and equipment operability because of the evaporation of the organic solvent and the accompanying viscosity changes.

[0078] The positive electrode is prepared using a positive electrode slurry and includes a current collector and a positive electrode active material layer. The positive electrode active material layer can be formed by kneading the active material and, if necessary, a conductive material, a binder, etc., and forming the mixture into a sheet, which is then placed on the current collector as the positive electrode active material layer, or by applying (coating) the positive electrode slurry onto the current collector and drying it to form the positive electrode active material layer.

[0079] The method for applying the positive electrode slurry to the current collector is not particularly limited, and known methods can be used. Specifically, examples of the application method include a doctor blade method, a dipping method, a reverse roll method, a direct roll method, a gravure method, an extrusion method, and a brush coating method. In this case, the positive electrode slurry may be applied to only one side of the current collector, or may be applied to both sides. The thickness of the slurry film on the current collector after application and before drying can be appropriately set depending on the thickness of the positive electrode composite layer obtained by drying.

[0080] The method for drying the positive electrode slurry on the current collector is not particularly limited and may be a known method, for example, drying with warm air, hot air, or low-humidity air, vacuum drying, or drying by irradiation with infrared rays or electron beams, etc. By drying the electrochemical element positive electrode slurry on the current collector in this manner, a positive electrode active material layer can be formed on the current collector, and a positive electrode including the current collector and the positive electrode active material layer can be obtained.

[0081] Preferably, the drying step is carried out by drying the positive electrode slurry on the current collector at a drying temperature of 100° C. or higher and 160° C. or lower under atmospheric pressure or reduced pressure for 1 hour to 12 hours.

[0082] After the drying step, the positive electrode active material layer may be subjected to pressure treatment using a mold press, a roll press, etc. Pressure treatment can improve the adhesion between the positive electrode active material layer and the current collector.

[0083] The thickness of the positive electrode active material is not limited because it differs depending on the manufacturing method and the desired battery performance, but is usually formed to 10 μm to 200 μm, more preferably 20 μm to 150 μm, and 25 μm to 130 μm taking into consideration the electric capacity of the battery and the blend with the negative electrode.

[0084] [Negative Electrode] The negative electrode active material is not particularly limited as long as it has a predetermined average diameter in relation to the current collector, and known negative electrode active materials can be used. The negative electrode active material includes a substance capable of absorbing and releasing electrolyte ions, alkali metals (Li, Na, K, Rb, Cs), alkaline earth metals (Be, Mg, Ca, Sr, Ba), alloys of alkali metals and alkaline earth metals, substances capable of doping and dedoping alkali metals and alkaline earth metals, and transition metal oxides.

[0085] The material capable of absorbing and releasing electrolyte ions is preferably a carbonaceous material, and any commonly used carbon-based negative electrode active material can be used. Representative examples include crystalline carbon, amorphous carbon, or a combination of these. Examples of crystalline carbon include graphite, such as amorphous, plate-like, flake-like, spherical, or fibrous natural or artificial graphite. Examples of amorphous carbon include soft or hard carbon, mesophase pitch carbide, and calcined coke. These materials can also be used in a state in which lithium is pre-absorbed.

[0086] As the alloy of the alkali metal or alkaline earth metal, an alloy of an alkali metal or alkaline earth metal and a metal selected from the group consisting of Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al and Sn may be used.

[0087] As a substance capable of doping and dedoping alkali metals and alkaline earth metals, Si, SiOx (0<x<2), Si-Q alloy (wherein Q is an element selected from the group consisting of alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, Group 15 elements, Group 16 elements, transition metals, rare earth elements, and combinations thereof, and is not Si), Sn, SnO 2 , Sn-R (wherein R is an element selected from the group consisting of alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, Group 15 elements, Group 16 elements, transition metals, rare earth elements, and combinations thereof, and is not Sn), and the like, and at least one of these and SiO 2 The elements Q and R may be selected from the group consisting of Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ti, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof.

[0088] Examples of the transition metal oxide include vanadium oxide and lithium vanadium oxide.

[0089] When constructing a battery that uses electrostatic adsorption of electrolyte ions, such as an electric double layer capacitor or a lithium ion capacitor, examples of the material include carbon materials and inorganic materials with a large specific surface area, such as activated carbon, mesoporous carbon, and conductive ceramics, such as defective titanium oxide.

[0090] The negative electrode active material may be applied to a current collector as a negative electrode slurry to form a negative electrode active material layer. The content of the negative electrode active material in the negative electrode active material layer is preferably 80.0 to 99.9 wt %, more preferably 90 to 99.5 wt %, based on the total weight of the negative electrode active material layer (or the total weight of the solid content of the slurry).

[0091] The negative electrode active material layer may include the negative electrode active material described above, a binder if necessary, and optionally a conductive material (conductive additive). The content of the binder in the negative electrode active material layer may be 1 wt % to 5 wt % based on the total weight of the negative electrode active material layer. When a conductive material is further included, the negative electrode active material may be used in an amount of 90 wt % to 98 wt %, the binder in an amount of 1 wt % to 5 wt %, and the conductive material in an amount of 1 wt % to 5 wt %.

[0092] The binder serves to effectively adhere the negative electrode active material particles to each other and to effectively adhere the negative electrode active material to the current collector. The binder may be a water-insoluble binder, a water-soluble binder, or a combination thereof. Examples of the water-insoluble binder and the water-soluble binder exemplified in the description of the positive electrode active material layer may be used.

[0093] Furthermore, the negative electrode active material layer may use a conductive material, and as the conductive material, those exemplified in the description of the positive electrode active material layer may be used. When the negative electrode active material layer contains a binder, a conductive material (conductive additive), and the like in addition to the negative electrode active material, the solid components containing these are sometimes referred to as negative electrode active material components, and the negative electrode active material layer is sometimes referred to as a negative electrode active material component layer.

[0094] The negative electrode active material layer may be formed from a negative electrode slurry, and the solvent used for the negative electrode slurry may be any of those exemplified in the description of the positive electrode active material layer.

[0095] As with the above-described positive electrode, the negative electrode may be prepared by preparing a negative electrode slurry with a solvent and applying it to the current collector, or, for example, by kneading the active material and, if necessary, a conductive material, a binder, etc., and forming it into a sheet, which is then placed on the current collector as a negative electrode active material layer. Alternatively, an ink-like slurry of the active material, conductive material, and binder may be applied to the current collector and dried to form a negative electrode active material layer. The thickness of the negative electrode active material layer is not limited, as it varies depending on the manufacturing method and the desired battery performance. It is usually formed to be 10 μm to 200 μm, more preferably 20 μm to 150 μm, and is usually formed to be 25 μm to 130 μm, taking into account the battery's electrical capacity and the blend with the positive electrode.

[0096] As will be described later, in this embodiment as well, it is preferable that at least a portion of the pores of the current collector be filled with components (active material components) including active materials (positive electrode active material, negative electrode active material) and, as necessary, binders, conductive agents, etc. In the electrode of this embodiment, the average opening diameter A of the current collector and the median diameter (D 50 ) B satisfies the predetermined relationship, so that in the process of forming the active material layer, the slurry containing the active material can penetrate into the voids of the current collector and fill the voids with the active material component.

[0097] The electrode includes a current collector and an electrode material layer provided on at least one surface of the current collector. Here, "the electrode material layer is provided on the surface of the current collector" means that the electrode material layer has a portion adjacent to the current collector, and also includes the case where a portion of the electrode material layer penetrates into the current collector.

[0098] Second Embodiment In the second embodiment of the present invention, the configuration of the current collector and the definition of the median diameter of the active material, as described in the first embodiment, can also be applied. Therefore, the following first describes the relationship between the porous structure of the current collector and the active material in the electrode of the second embodiment. [Second Embodiment of Electrode] In this embodiment, the electrode preferably includes a current collector having a three-dimensional porous structure and active material components filled into the current collector, and the filling rate of the active material components relative to the current collector is controlled within a predetermined range. Here, the active material components refer to solid components based on the active material, including the active material and, optionally, a binder, a conductive additive, and the like. The filling rate of the active material components relative to the current collector is preferably 37% or more, and more preferably 45% or more. Here, the filling rate is defined as the ratio of the area occupied by the active material components to the area of ​​the voids in the current collector in a cross section of the current collector filled with the active material components. By increasing the packing ratio, the contact area between the solid phase portion of the current collector (e.g., fibers on which a metal coating is formed) and the active material can be increased, thereby improving the capacity retention rate of the electrochemical device. Hereinafter, the method for measuring the packing ratio will be described with reference to Figures 2 and 3.

[0099] Figure 2 is a scanning electron microscope (SEM) image of a cross section of the electrode in the thickness direction. In the image, the highest and lowest points where the projected portion of the current collector is present were identified, and straight lines L1 and L2 were drawn perpendicular to the thickness direction and passing through these points. The distance between these lines was determined as the thickness T of the current collector.

[0100] Next, the leftmost and rightmost positions of the projected portion of the current collector in the photograph are determined, and lines L3 and L4 are drawn parallel to the thickness direction, including these positions, and the distance between these lines is defined as the observation length of the current collector (width of the observation region) W. Thus, the observation area is determined as observation area (α) = current collector thickness × observation length.

[0101] Next, using image analysis software (Keyence Corporation's "Multi-File Analysis Application"), the image was binarized by setting it so that the black parts were distinguished from the other parts, and the projected areas of the active material and current collector within the observation area were calculated as (β) and (γ), respectively.

[0102] Figure 3 is a schematic diagram illustrating the locations of the current collector and active material in the observation area of ​​Figure 2. In Figure 3, the area occupied by the active material 2 is indicated by dots, and the area occupied by the current collector 1 is indicated by diagonal lines. Furthermore, the portions where the active material 2 and current collector 1 are not present represent voids 3. That is, the observation area (α) is formed by the total area of ​​the current collector (solid phase portion of the current collector) 1, the active material 2, and the voids 3, and the area where the active material 2 is present corresponds to the projected area (β) of the active material, and the area where the current collector 1 is present corresponds to the projected area (γ) of the current collector.

[0103] By subtracting the portion where the current collector 1 is present from the observation area (α), the area that can be filled with the active material in the observation area (α) can be determined. That is, the value (α-γ) obtained by subtracting the projected area (γ) of the current collector from the observation area (α) corresponds to the area that can be filled with the active material in the observation area, which in Figure 3 is the area occupied by the active material 2 and voids 3.

[0104] Then, by expressing the ratio of the area (β) occupied by the active material 2 to the area (α-γ) that can be filled with the active material 2 by the formula: β / (α-γ)×100, the ratio of the area (β) actually filled with the active material to the area (α-γ) that can be filled with the active material in the observed area can be defined as the filling rate (%) expressed as a percentage.

[0105] The filling rate may be 37% or more, preferably 45% or more, more preferably 50% or more, and even more preferably 60% or more. The upper limit of the filling rate is not particularly set and may be 100%, but in order to ensure permeability of the electrolyte, it is preferably 90% or less. Therefore, the filling rate may be, for example, 45% or more and 90% or less.

[0106] The active material component may be present at a filling rate of 37% or more, preferably 45% or more, of the interior of the current collector, and an active material component layer may be formed on the surface of the current collector as needed.

[0107] The thickness of the entire electrode is not limited because it differs depending on the manufacturing method of the electrode and the desired battery performance, and may be, for example, 20 μm to 500 μm, preferably 30 μm to 400 μm, and more preferably 40 μm to 300 μm. The thickness of the active material component layer is a value measured by the method described in the examples below.

[0108] The thickness of the active material component layer is not limited, as it varies depending on the manufacturing method of the electrode and the desired battery performance, and may be, for example, 5 μm to 200 μm, preferably 10 μm to 150 μm, and more preferably 20 μm to 130 μm. The thickness of the active material component layer refers to the total thickness in the electrode, and is the thickness of one layer when the active material component layer is provided on only one side, and is the total thickness of two layers when the active material component layer is provided on both sides. The thickness of the active material component layer is a value measured by the method described in the Examples below.

[0109] By increasing the filling rate of the active material component in the current collector, the ratio of the thickness of the active material component layer to the thickness of the current collector can be reduced, and for example, the ratio (thickness of the active material component layer) / (thickness of the current collector) may be, for example, 0.5 to 8, preferably 0.6 to 7. The thickness of the active material component layer is a value measured by the method described in the examples below.

[0110] The electrode density is not limited because it is determined depending on the filling rate and the ratio of the active material component layer, but is, for example, 1.00 to 2.00 g / cm 3 , preferably 1.05 to 1.80 g / cm 3 The electrode density is a value measured by the method described in the examples below.

[0111] [Positive Electrode] The positive electrode active material is not particularly limited as long as it has a predetermined average diameter in relation to the current collector, and known positive electrode active materials can be used. Positive electrode active materials capable of absorbing and releasing electrolyte ions include layered oxides (LiMO). 2 or NaMO 2 where M is a metal, for example, LiCoO 2 , LiNiO 2 , LiMnO 2 , NaFeO 2 , NaNiO 2 , NaCoO 2 , NaMnO 2 , NaVO 2 or LiNixCoyMnO 2 , NaNixMnzO 2 (where x, y, and z represent the composition ratio), olivine-based (LiMPO 4 or NaMPO 4 where M is a metal, for example LiFePO 4 , NaFePO 4 etc.), spinel type (LiM 2 O 4 or NaM 2 O 4 where M is a metal, for example LiMn 2 O 4 , NaMn 2 O 4 complex metal chalcogen compounds such as Li1+x Mn 2-x O 4 (0<x<2) Lithium-rich spinel compounds represented by Li[Ni 0.17 Li 0.2 Co 0.07 Mn 0.56 ]O 2 , LiNi 0.5 Mn 1.5 O 4 Examples of the positive electrode active material include organic radicals such as metal oxides such as those mentioned above, phosphate-containing compounds, polyanion-containing compounds, Prussian blue analogs, sulfur, compounds or polymers having a nitroxyl radical, compounds or polymers having an oxy radical, compounds or polymers having a nitrogen radical, and compounds or polymers having a fulvalene skeleton. These positive electrode active materials can be used alone or in combination of two or more. Among these, composite metal chalcogen compounds are preferred. Furthermore, when constructing a battery using electrostatic adsorption such as a lithium ion capacitor, examples of the positive electrode active material include carbon materials and inorganic materials having a high specific surface area, such as activated carbon, mesoporous carbon, defective titanium oxide, and conductive ceramics.

[0112] The positive electrode active material may be applied to the current collector as a positive electrode slurry to form a positive electrode active material portion. The content of the positive electrode active material in the positive electrode active material portion is preferably 80.0 to 99.9 wt %, more preferably 90 to 99.5 wt %, based on the total weight of the positive electrode active material portion (or the total weight of the solid content of the slurry).

[0113] The positive electrode active material portion may further include the positive electrode active material described above, a binder as needed, and optionally a conductive material (conductive additive). The content of the binder in the positive electrode active material portion may be 1 wt% to 5 wt% based on the total weight of the positive electrode active material portion. When a conductive material is further included, the positive electrode active material may be used in an amount of 90 wt% to 98 wt%, the binder may be 1 wt% to 5 wt%, and the conductive material may be 1 wt% to 5 wt%.

[0114] The binder serves to effectively adhere the positive electrode active material particles to each other and to the current collector. The binder may be a water-insoluble binder, a water-soluble binder, or a combination thereof.

[0115] Examples of the water-insoluble binder include polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamideimide, polyimide, styrene-butadiene rubber, acrylated styrene-butadiene rubber, copolymers of (meth)acrylic acid and (meth)acrylic acid alkyl esters, copolymers of olefins having 2 to 8 carbon atoms and maleic acid, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, copolymers of propylene and olefins having 2 to 8 carbon atoms, polyamideimide, polyimide, and combinations thereof.

[0116] Examples of the water-soluble binder include polyvinyl alcohol, a copolymer of vinyl alcohol and an ethylenically unsaturated carboxylic acid and an alkali metal modified product thereof, an alkali metal modified copolymer of an alkene having 2 to 4 carbon atoms and an ethylenically unsaturated carboxylic acid, an alkali metal modified copolymer of an alkene having 2 to 4 carbon atoms and maleic anhydride, and sodium poly(meth)acrylate.

[0117] The positive electrode binder may further include a cellulose-based compound as a thickener, which can impart viscosity. The cellulose-based compound may be a mixture of one or more of carboxymethyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose, or alkali metal salts thereof. For example, a binder may be prepared by adding carboxymethyl cellulose to styrene-butadiene rubber. The alkali metal may be sodium, potassium, or lithium. The amount of the thickener used may be 0.1 to 3 parts by weight per 100 parts by weight of the active material.

[0118] The conductive material is used to impart conductivity to the electrode, and any electron-conductive material that does not undergo chemical change in the battery that is constructed can be used. Examples of such a conductive material include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, and carbon fiber; metal-based materials such as metal powder or metal fiber of copper, nickel, aluminum, silver, and the like; conductive polymers such as polyphenylene derivatives; and conductive materials containing mixtures of these.

[0119] Examples of solvents that can be used in the positive electrode slurry include water and various organic solvents (e.g., amide compounds, hydrocarbons, alcohols, ketones, esters, amine compounds, lactones, sulfoxides, sulfone compounds, etc.). These solvents may be used alone or in combination of two or more. The organic solvent is preferably a polar organic solvent capable of dissolving the binder. For example, preferred polar organic solvents include acetonitrile, N-methylpyrrolidone, acetylpyridine, cyclopentanone, N,N-dimethylacetamide, dimethylformamide, dimethylsulfoxide, methylformamide, methyl ethyl ketone, furfural, and ethylenediamine. Among these, N-methylpyrrolidone (NMP) is most preferred from the viewpoints of ease of handling, safety, ease of synthesis, and the like.

[0120] The amount of the solvent used is such that the solid content concentration in the positive electrode slurry is preferably in the range of 1 to 80% by weight, more preferably 5 to 70% by weight, and even more preferably 10 to 60% by weight. By setting the solid content concentration in the above range, the positive electrode active material and other components contained therein can be uniformly dispersed, which is preferable.

[0121] The electrode manufacturing method includes at least a step of filling a current collector having a three-dimensional porous structure with active material components. When filling the current collector with the active material components, the filling rate of the active material components can be improved by, for example, (i) adjusting the slurry viscosity to an appropriate range, (ii) adjusting the surface tension of the slurry to an appropriate range, and / or (iii) optimizing the application method. The above (i) to (iii) may be performed alone or in combination. The active material components refer to the solid content of the slurry, and include, for example, an active material, a binder, a conductive material, and the like.

[0122] The positive electrode slurry can be produced by mixing the positive electrode active material and other components, if necessary, in the solvent. There are no particular limitations on the mixing method, and a general mixing device such as a disperser, mill, or kneader can be used. For example, stirring for 20 minutes to 120 minutes is preferred.

[0123] The temperature at which the mixture is mixed is not particularly limited, and is, for example, in the range of 0° C. to 160° C., more preferably in the range of 20° C. to 80° C. An excessively low temperature is undesirable because the viscosity becomes too high and coating becomes impossible, while an excessively high temperature is undesirable from the viewpoints of safety and equipment operability because of the evaporation of the organic solvent and the accompanying viscosity changes.

[0124] (i) The slurry viscosity may be, for example, 10,000 mPa·s or less, preferably 7,000 mPa·s or less, and more preferably 5,000 mPa·s or less. If the slurry viscosity is too high, it becomes difficult for the slurry containing the active material components to penetrate into the current collector. The lower limit of the slurry viscosity is not particularly limited, but may be 50 mPa·s or more from the viewpoint of efficiently filling the active material components.

[0125] (ii) When water, which has a high surface tension, is used as the solvent, it is preferable to adjust the surface tension of the slurry. For example, water may be used as the solvent in combination with a surface conditioner for reducing the surface tension of water. Examples of the surface conditioner include lower alcohols such as methanol and ethanol (preferably C 1-3 Examples of suitable surface conditioners include alcohols), various surfactants, and antifoaming agents such as silicone oils. The proportion of the surface conditioner relative to water can be appropriately selected depending on the type of surface conditioner used. For example, in the case of a lower alcohol, the proportion may be 0.1 to 20 parts by weight, preferably 0.5 to 15 parts by weight, per 100 parts by weight of water. In the case of an antifoaming agent, the proportion may be 0.005 to 2 parts by weight, preferably 0.01 to 1.5 parts by weight, per 100 parts by weight of water. The surface conditioner may be used either mixed with water or without being mixed with water.

[0126] (iii) The application method is broadly divided into application by coating and application by dipping. The method for coating the positive electrode slurry onto the current collector is not particularly limited, and known methods can be used. Specifically, examples of the coating method include a doctor blade method, a dipping method, a reverse roll method, a direct roll method, a gravure method, an extrusion method, and a brush coating method. In this case, the positive electrode slurry may be coated on only one side of the current collector, or may be coated on both sides. When coating, for example, by adjusting the slurry to be coated by the above (i) and / or (ii), it is possible to improve the filling rate.

[0127] In the case of application by dipping, the current collector may be immersed in the slurry and held there, pressurized, or vibrated by ultrasonic waves, etc., to promote the defoaming action and expel air from the current collector, thereby enabling the slurry to be effectively filled toward the inside of the current collector.

[0128] Thereafter, the slurry may be dried as necessary. The drying method is not particularly limited and any known method can be used, such as drying with warm air, hot air, or low-humidity air, vacuum drying, or drying by irradiation with infrared rays or electron beams.

[0129] Preferably, the drying step is carried out by drying the positive electrode slurry on the current collector at a drying temperature of 60° C. or higher and 160° C. or lower under atmospheric pressure or reduced pressure for 1 hour to 12 hours.

[0130] After the drying step, the positive electrode active material portion may be subjected to pressure treatment using a mold press, a roll press, or the like, as needed. Pressure treatment can improve the adhesion between the positive electrode active material portion and the current collector.

[0131] [Negative Electrode] The negative electrode active material is not particularly limited as long as it has a predetermined average diameter in relation to the current collector, and known negative electrode active materials can be used. The negative electrode active material includes a substance capable of absorbing and releasing electrolyte ions, alkali metals (Li, Na, K, Rb, Cs), alkaline earth metals (Be, Mg, Ca, Sr, Ba), alloys of alkali metals and alkaline earth metals, substances capable of doping and dedoping alkali metals and alkaline earth metals, and transition metal oxides.

[0132] The material capable of absorbing and releasing electrolyte ions is preferably a carbonaceous material, and any commonly used carbon-based negative electrode active material can be used. Representative examples include crystalline carbon, amorphous carbon, or a combination of these. Examples of crystalline carbon include graphite, such as amorphous, plate-like, flake-like, spherical, or fibrous natural or artificial graphite. Examples of amorphous carbon include soft or hard carbon, mesophase pitch carbide, and calcined coke. These materials can also be used in a state in which lithium is pre-absorbed.

[0133] As the alloy of the alkali metal or alkaline earth metal, an alloy of an alkali metal or alkaline earth metal and a metal selected from the group consisting of Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al and Sn may be used.

[0134] As a substance capable of doping and dedoping alkali metals and alkaline earth metals, Si, SiO x (0<x<2), Si-Q alloy (wherein Q is an element selected from the group consisting of alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, Group 15 elements, Group 16 elements, transition metals, rare earth elements, and combinations thereof, and is not Si), Sn, SnO 2 , Sn-R (wherein R is an element selected from the group consisting of alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, Group 15 elements, Group 16 elements, transition metals, rare earth elements, and combinations thereof, and is not Sn), and the like, and at least one of these and SiO 2 The elements Q and R may be selected from the group consisting of Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ti, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof.

[0135] Examples of the transition metal oxide include vanadium oxide and lithium vanadium oxide.

[0136] When constructing a battery that uses electrostatic adsorption of electrolyte ions, such as an electric double layer capacitor or a lithium ion capacitor, examples of the material include carbon materials and inorganic materials with a large specific surface area, such as activated carbon, mesoporous carbon, and conductive ceramics, such as defective titanium oxide.

[0137] The negative electrode active material may be applied to the current collector by the same application method as described for the positive electrode active material portion. Therefore, the negative electrode active material may be applied to the current collector as a negative electrode slurry to form the negative electrode active material portion. The content of the negative electrode active material in the negative electrode active material portion is preferably 80.0 to 99.9 wt %, more preferably 90 to 99.5 wt %, based on the total weight of the negative electrode active material portion (or the total weight of the solids in the slurry).

[0138] The negative electrode active material portion may further include the negative electrode active material described above, a binder as needed, and optionally a conductive material (conductive additive). The content of the binder in the negative electrode active material portion may be 1 wt% to 5 wt% based on the total weight of the negative electrode active material portion. When the negative electrode active material portion further includes a conductive material, the negative electrode active material may be used in an amount of 90 wt% to 98 wt%, the binder may be used in an amount of 1 wt% to 5 wt%, and the conductive material may be used in an amount of 1 wt% to 5 wt%.

[0139] The binder serves to effectively adhere the negative electrode active material particles to each other and to the current collector. The binder may be a water-insoluble binder, a water-soluble binder, or a combination thereof. Examples of the water-insoluble binder and the water-soluble binder exemplified in the description of the positive electrode active material may be used.

[0140] Furthermore, a conductive material may be used for the negative electrode active material portion, and as the conductive material, those exemplified in the description of the positive electrode active material portion may be used.

[0141] The negative electrode active material portion may be formed from a negative electrode slurry, and the solvent used for the negative electrode slurry may be any of those exemplified in the description of the positive electrode active material portion.

[0142] In the negative electrode, similarly to the positive electrode described above, an active material component is filled into a current collector having a three-dimensional porous structure.

[0143] With regard to the relationship that must be satisfied between the current collector and the active material in the electrode as explained above, the electrode of the present invention may satisfy the conditions of either the first embodiment or the second embodiment, but preferably the electrode of the present invention may satisfy the conditions of both the first embodiment and the second embodiment.

[0144] That is, in the electrode of the first embodiment, the current collector may be filled with an active material component containing the active material, and the filling rate (%) determined by the following formula (2) may be 37% or more: Filling rate (%) = β / (α - γ) × 100 (2) In the formula, α represents the observation area, which is determined by multiplying the thickness of the current collector by the observation length, as determined from an electron microscope photograph of a cross section of the electrode in the thickness direction, and β and γ represent the projected areas of the active material and current collector, respectively, within the observation area, as calculated using image analysis software. Alternatively, in the electrode of the second embodiment, the average opening diameter A (μm) of the current collector and the median diameter (D 50 ) B (μm) may satisfy the relationship of the following formula (1): 0.10≦B / A≦2.00 (1)

[0145] [Electrochemical Device] FIG. 4 is a schematic cross-sectional view showing an example of the configuration of an electrochemical device 10 (a nonaqueous electrolyte secondary battery). In the electrochemical device 10, a positive electrode 4 and a negative electrode 5 are disposed opposite each other with a separator 6 interposed therebetween. The positive electrode 4 comprises a positive electrode current collector 4a and a positive electrode active material component layer 4b, and the negative electrode 5 comprises a negative electrode current collector 5a and a negative electrode active material component layer 5b. These may be housed in a case (not shown). The electrochemical device 10 of the present invention includes an electrode according to the first or second embodiment of the present invention. The electrode of the present invention may be used for both the positive electrode 4 and the negative electrode 5, or for either one of them. When the electrode of the present invention is used for only one of the electrodes, the other electrode may use a known or commonly used current collector (e.g., copper foil, nickel foil, aluminum foil, etc.) that is electrically conductive and electrochemically durable as the current collector. For example, when the electrochemical device 10 of the present invention is a non-aqueous electrolyte secondary battery, other materials constituting the battery, such as the separator 6 and the electrolyte (not shown), are not particularly limited, and various materials that have conventionally been used or proposed for non-aqueous electrolyte secondary batteries can be used.

[0146] [Electrolyte] The electrolyte may be any known electrolyte that can be used in electrochemical devices. When used as a nonaqueous electrolyte battery, it is preferable that the electrolyte contains at least a nonaqueous organic solvent and an alkali metal salt such as a lithium salt.

[0147] The non-aqueous organic solvent serves as a medium through which ions involved in the electrochemical reaction of the battery can migrate.

[0148] The non-aqueous organic solvent may be a carbonate, ester, ether, ketone, alcohol, or aprotic solvent. Examples of the carbonate solvent include dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate (BC). Examples of the ester solvent include methyl acetate, ethyl acetate, n-propyl acetate, dimethyl acetate, methyl propionate, ethyl propionate, γ-butyrolactone, decanolide, valerolactone, mevalonolactone, and caprolactone. Examples of the ether solvent that can be used include dibutyl ether, tetraglyme, diglyme, dimethoxyethane, 2-methyltetrahydrofuran, and tetrahydrofuran. Examples of the ketone solvent that can be used include cyclohexanone. Examples of the alcohol solvent that can be used include ethyl alcohol and isopropyl alcohol. Examples of the aprotic solvent that can be used include nitriles such as R—CN (where R is a linear, branched, or cyclic hydrocarbon group having 2 to 20 carbon atoms, which may contain an aromatic ring or an ether bond), amides such as dimethylformamide, dioxolanes such as 1,3-dioxolane, and sulfolanes.

[0149] The non-aqueous organic solvents may be used alone or in combination of two or more. When two or more organic solvents are used in combination, the mixing ratio may be appropriately adjusted depending on the desired battery performance.

[0150] In addition, in the case of the carbonate-based solvent, it is preferable to use a mixture of a cyclic carbonate and a chain carbonate, and in this case, the cyclic carbonate and the chain carbonate may be mixed in a volume ratio of 1:1 to 1:9 to exhibit better electrolyte performance.

[0151] The alkali metal salt (e.g., lithium salt) is a substance that is dissolved in an organic solvent and acts as a source of alkali metal ions (e.g., lithium ions) in a battery, enabling basic operation of an alkali metal ion secondary battery (e.g., a lithium ion secondary battery), and promoting the movement of alkali metal ions between the positive electrode and the negative electrode. A representative example of such an alkali metal salt is LiPF 6 , LiBF 4 , LiSbF 6 , LiAsF 6 , LiCF 3 SO 3 , LiN(SO 2 C 2 F 5 ) 2 , Li(CF 3 SO 2 ) 2 N, LiC 4 F 9 SO 3 , LiClO 4 , LiAlO 4 , LiAlCl 4 , LiN(C x F 2x+1 SO 2 ) (C y F 2y+1 SO 2 ) (where x and y are natural numbers), LiCl, LiI and LiB(C 2 O 4 ) 2 (Lithium bis(oxalato)borate (LiBOB), NaClO 4 , NaPF 6 , NaBF 4 , NaCF 3 SO 3 , NaN(CF 3 SO 2 ) 2 , NaN(FSO 2 ) 2 , NaN(C 2 F 5 SO 2 ) 2 , NaC(CF 3 SO 2 ) 3 , NaAsF 6 , NaPF6 , NaB(C 6 H 5 ) 4 , C.H. 3 SO 3 Na, CF 3 SO 3 Examples of alkali metal salts include Na, NaCl, and NaBr. These may be used alone or in combination. Preferably, the concentration of the alkali metal salt is in the range of 0.1 to 2.0 M. If the concentration of the alkali metal salt is less than 0.1 M, the conductivity of the electrolyte tends to decrease, resulting in a decrease in electrolyte performance. If the concentration exceeds 2.0 M, the viscosity of the electrolyte tends to increase, resulting in a decrease in the mobility of the alkali metal ions.

[0152] The electrolyte may further contain a vinylene carbonate or ethylene carbonate compound as a life-promoting agent to improve the battery life.

[0153] Representative examples of the ethylene carbonate-based compound include difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, cyanoethylene carbonate, fluoroethylene carbonate, etc. When such a life-promoting agent is further used in the electrolyte, the amount used may be appropriately adjusted.

[0154] [Separator] In the electrochemical device of the present invention, a separator may be present between the positive electrode and the negative electrode. Such a separator may be any known or commonly used separator, such as a polyethylene film, a polypropylene film, a polyvinylidene fluoride film, or a multilayer film of two or more of these layers. Alternatively, a mixed multilayer film such as a polyethylene / polypropylene two-layer separator, a polyethylene / polypropylene / polyethylene three-layer separator, or a polypropylene / polyethylene / polypropylene three-layer separator may be used.

[0155] The present invention will be explained in more detail below with reference to examples, but the present invention is not limited to these examples. The physical properties of the examples and comparative examples in the present invention were measured by the following methods.

[0156] [Median diameter D 50 (μm)] Median diameter D of carbon precursor and carbonaceous material 50 The particle size distribution was measured by a laser scattering method as follows. The active material samples of the examples and comparative examples described below were placed in an aqueous solution containing 0.3 wt % of a surfactant ("Polyoxyethylene (10) Octylphenyl Ether" manufactured by Wako Pure Chemical Industries, Ltd.), treated in an ultrasonic cleaner for 10 minutes or more, and dispersed in the aqueous solution. The particle size distribution was measured using this dispersion. The particle size distribution was measured using a particle size / particle size distribution measuring instrument ("MT3000II" manufactured by Microtrac Bell Co., Ltd.), with a solvent refractive index of 1.33 and particle permeability as absorption. The particle diameter at which the cumulative volume reached 50% was defined as the average particle diameter D 50 It was decided.

[0157] [Average Opening Diameter (μm)] The current collector was cut into a 2 × 2 cm sample in the planar direction, and the cut sample was sandwiched between glass slides and placed on a black flat plate. The placed sample was then observed at 200x magnification using a shape analysis laser microscope (VK-X1000, manufactured by Keyence Corporation).

[0158] Next, the observation image obtained, measuring 0.75 x 1.00 mm, was binarized using image analysis software (Keyence Corporation's "Multi-File Analysis Application") by setting a threshold value so as to distinguish between the black parts originating from the plate and the other parts, and the black parts where the base could be seen were designated as individual through holes.

[0159] From the observation image obtained by image processing, the area was 2 μm 2 The diameter of a circle having the same area as each cross-sectional area was used for the above through holes, and the opening diameter was calculated by taking the diameter of the circle having the same area as each through hole as the equivalent diameter of the circle of each through hole. The average value of the opening diameters of 500 to 5,000 through holes obtained from the observation image was calculated, and this was used as the average opening diameter of each sample.

[0160] [Average Fiber Diameter (μm)] An arbitrary point in a sample piece (nonwoven fabric) was photographed at 1000x magnification using a scanning electron microscope, and the average value of the measured fiber diameters of 100 fibers was taken as the average fiber diameter of the sample piece.

[0161] [Basis weight (g / m 2 ) ] In accordance with JIS L 1906, three sample pieces measuring 20 cm long x 20 cm wide were taken from each meter of width of the sample (nonwoven fabric) produced in the Examples and Comparative Examples, the mass of each sample piece was measured using an electronic balance, and the average value of the masses of the three sample pieces was calculated based on the test piece area of ​​400 cm. 2 The mass per unit area was calculated by dividing the mass by 1 / 2, and this was taken as the basis weight of the nonwoven fabric.

[0162] [Thickness (μm)] In accordance with JIS L 1906, the same three sample pieces as those prepared for the basis weight measurement were used, and each sample piece was measured under a diameter of 16 mm and a load of 20 gf / cm. 2 The thickness was measured at five points using a digital thickness gauge (B1 type, manufactured by Toyo Seiki Seisakusho Co., Ltd.), and the average value of the 15 points was taken as the thickness of the nonwoven fabric or the current collector before being made into an electrode.

[0163] [Air permeability (cc / cm 2 / sec.)] In accordance with JIS L 1096, 6.27.1 (Method A: Frazier method), the same three sample pieces as those prepared for the basis weight measurement were used, and each sample piece was measured using an air permeability measuring device (FX3300 manufactured by TEXTEST (Switzerland) with a measurement area of ​​38 cm 2 The air permeability was measured under the condition of a measuring pressure of 125 Pa, and the average value of the air permeabilities measured for each of the three sheets was taken as the air permeability of the nonwoven fabric or current collector.

[0164] [Surface Resistivity (Ω / □)] The surface resistance of the current collector was measured by a four-terminal four-probe method in accordance with JIS-K-7194 using a resistance measuring device (MULTIMETER 3478A, manufactured by Hewlett-Packard Company).

[0165] [Slurry Viscosity] The viscosity of the slurry was measured 2 minutes after the start of measurement using a Brookfield viscometer (DV2T, manufactured by Eiko Seiki Co., Ltd.) at 25°C, a spindle CPA-52Z, and a rotation speed of 5 rpm.

[0166] [Filling rate] The electrode was cut to an appropriate size, embedded in G2 epoxy resin, and then cross-sectioned using CP. The cross-section of this electrode was observed using a scanning electron microscope (SU8200, manufactured by Hitachi High-Technologies Corporation) at 15 kV and 2000x magnification. Next, a projection of the current collector was cut out from the obtained observation image using image analysis software ("PopImaging" manufactured by Digital Being Kids, Inc.) so that it matched the thickness of the current collector alone (Figure 2).

[0167] First, the highest and lowest positions of the projected portion of the current collector were determined in the obtained projection image, and straight lines L1 and L2 perpendicular to the thickness direction were drawn, including these positions, and the distance between these lines was determined as the thickness of the current collector. Next, the leftmost and rightmost positions of the projected portion of the current collector in the photograph were determined, and straight lines L3 and L4 parallel to the thickness direction were drawn, including these positions, and the distance between these lines was determined as the observation length of the current collector. The observation area (α) was then calculated as the current collector thickness x the observation length.

[0168] The observed area (α) was binarized by setting a threshold value so as to distinguish between the white portion originating from the current collector and the other portion, and the white portion was designated as the current collector portion. The area (γ) of the current collector portion was calculated from the observed image obtained by image processing. Next, the portion other than the current collector in the current collector projection was binarized by setting a threshold value so as to distinguish between the portion where the active material was present and the portion where the active material was not present, and the area (β) of the active material-filled portion was calculated.

[0169] From the observation image obtained by image processing, the value (α-γ) obtained by subtracting the area (γ) of the current collector portion from the observation area (α) corresponds to the area that can be filled with active material in the observation area. The ratio of the area (β) actually filled with active material to the area (α-γ) that can be filled with active material in the observation area was calculated using the following formula to calculate the filling rate. The average value of the ratios for five points obtained in the same manner from the observation image was calculated and used as the filling rate for each sample. [Formula] Filling rate (%) = β / (α-γ) × 100

[0170] [Thickness of Electrode and Active Material Layer] Three sample pieces were used as electrodes for coin batteries. Each sample piece was measured in accordance with JIS L1906, with a diameter of 16 mm and a load of 20 gf / cm. 2 The thickness was measured at three points using a digital pressure measuring instrument (B1 type, manufactured by Toyo Seiki Seisakusho Co., Ltd.), and the average value of the nine points was taken as the electrode thickness. The thickness of the active material component layer was calculated by subtracting the thickness of the current collector measured when measuring the packing rate from the electrode thickness.

[0171] [Electrode Density] The electrode density was calculated by multiplying the weight (g) of graphite mixed in the slurry by the volume (cm) of the electrode produced when producing an electrode for a coin battery. 3 ) divided by (g / cm 3 The volume of the electrode was calculated using the thickness and diameter (14 mm) of the electrode.

[0172] [Powder Falling] The surface of the produced electrode was observed to visually check for the presence or absence of active material that had fallen off or been detached from the current collector. ◯: No active material that had fallen off or been detached from the current collector was observed. ×: Active material that had fallen off or been detached from the current collector was observed.

[0173] Example A1: Preparation of a current collector (1) A molten liquid crystal-forming wholly aromatic polyester (VECTRA-L manufactured by Polyplastics Co., Ltd.) consisting of a copolymer of parahydroxybenzoic acid and 6-hydroxy-2-naphthoic acid, having a melting point of 300°C and a melt viscosity of 15 Pa s at 310°C, was extruded using a twin-screw extruder and supplied to a melt-blown nonwoven fabric manufacturing apparatus having a nozzle with a nozzle hole diameter of 0.15 mm, L / D = 30, and 1,500 holes per meter width (nozzle hole spacing: 0.67 mm). The extrusion rate per hole was 0.10 g / min, the resin temperature was 330°C, the hot air temperature was 330°C, and the nozzle width was 18 Nm. 3 The basis weight is 11g / m 2 After obtaining a nonwoven fabric, it was heat-treated in air at 300°C for 6 hours. Thereafter, the obtained nonwoven fabric was passed between a metal roll heated to 110°C and a resin elastic roll (manufactured by Yuri Roll Co., Ltd.) with a surface Shore D hardness of 86 degrees, and continuously treated using a pressure calendar at a linear pressure of 120 kg / cm. The basis weight was 11 g / m as described above. 2A meltblown nonwoven fabric having an average fiber diameter of 5.1 μm was obtained. (2) A palladium catalyst was applied to the fiber surface of the meltblown nonwoven fabric obtained in (1) above, and the fabric was immersed in an electroless copper plating solution containing copper sulfate and potassium sodium tartrate (Rochelle salt), followed by rinsing with water to form a copper film on the surface of the nonwoven fabric. Subsequently, the fabric was immersed in an electrolytic nickel plating solution to coat the fabric with copper by electroplating, followed by rinsing with water and drying. This resulted in a copper film laminated on the copper film, with an average opening diameter of 18.3 μm, a thickness of 46 μm, and an air permeability of 327 cc / cm. 2 This conductive nonwoven fabric was used as a current collector.

[0174] Preparation of Electrode (Negative Electrode) <Preparation of Slurry for Negative Electrode> 94 parts by weight of artificial graphite having a median diameter of 21.0 μm, 6 parts by weight of polyvinylidene fluoride (KF Polymer #1120 manufactured by Kureha Corporation), and NMP (N-methylpyrrolidone) were placed in a dedicated container and kneaded using a planetary mixer (ARE-250, manufactured by Thinky Co., Ltd.) to obtain a slurry.

[0175] <Preparation of Battery Negative Electrode> The obtained slurry was applied to a current collector made of the conductive nonwoven fabric using a bar coater (T101, manufactured by Matsuo Sangyo Co., Ltd.), allowed to stand for 15 minutes, and then subjected to primary drying at 86°C for 30 minutes in a hot air dryer (manufactured by Yamato Scientific Co., Ltd.). This was then rolled using a roll press (manufactured by Hosen Co., Ltd.). After that, a battery electrode (diameter: 14 mm) was punched out, and secondary drying was performed at 120°C for 3 hours under reduced pressure to prepare a coin battery electrode.

[0176] [Comparative Example A1] Similar to Example A1(1), the basis weight was 4 g / m 2 A meltblown nonwoven fabric having an average fiber diameter of 2.8 μm was produced using this nonwoven fabric in the same manner as in Example A1(2), with an air permeability of 204 cc / cm 2 A conductive nonwoven fabric having a film thickness of 16 μm and an average pore size of 10.1 μm was obtained. A battery negative electrode was produced in the same manner as in Example A1, except that this conductive nonwoven fabric was used as a current collector.

[0177] Comparative Example A2 A negative electrode for a battery was produced in the same manner as in Example A1, except that a rolled copper foil (thickness: 10 μm) was used as the negative electrode current collector.

[0178] [Example A2] A battery negative electrode was produced in the same manner as in Example A1, except that the meltblown nonwoven fabric of Comparative Example A1 was used as the nonwoven fabric and 94 parts by weight of artificial graphite having a median diameter of 5.0 μm was used to produce a negative electrode slurry.

[0179] <Fabrication of Battery> The battery electrode obtained above was transferred to a glove box (manufactured by Miwa Seisakusho) under an argon gas atmosphere. Metallic lithium foil (thickness 0.2 mm, diameter 15 mm) was used as the positive electrode. A polypropylene separator (Celgard #2400, manufactured by Polypore) was used, and lithium hexafluorophosphate (LiPF 6 ) in a mixed solvent system (1M-LiPF F) containing ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) with vinylene carbonate (VC). 6 , EC / EMC / DMC=3 / 3 / 4 vol%, VC 1 wt%) were used to inject the electrolyte, and a coin battery (2032 type) was fabricated.

[0180] <Charge / Discharge Characteristics Test> The prepared coin batteries were subjected to a charge / discharge test using a commercially available charge / discharge tester (TOSCAT3100, manufactured by Toyo Systems). The coin batteries were placed in a thermostatic chamber at 25°C and charged to 0 V relative to the lithium potential at 0.2 C (approximately 0.50 mA / cm) with respect to the amount of active material. 2 ), and then constant voltage charging was performed at 0 V down to a current of 0.0385 mA relative to the lithium potential. The capacity at this time was recorded as the charge capacity (mAh / g). Next, constant current charging was performed at 0.2 C (approximately 0.50 mA / cm) relative to the lithium potential. 2 The battery was discharged at a constant current of 1.5 V at 200 V, and the capacity at this time was defined as the discharge capacity (mAh / g). The discharge capacity x electrode density was defined as the volumetric capacity. The percentage of the discharge capacity / charge capacity was defined as the charge / discharge efficiency, which was used as an index of the utilization efficiency of lithium ions in the battery.

[0181] <Rate characteristic test> The coin battery used in the charge / discharge test was placed in a thermostatic chamber at 25°C, and charging was performed at a current of 0.2 C (approximately 0.50 mA / cm) relative to the amount of active material until the battery reached 0 V relative to the lithium potential. 2) was charged, and then constant voltage charging was performed from 0 V to a current of 0.0385 mA relative to the lithium potential. 2 The coin battery was then charged again under the same conditions at a constant current of 3 C (approximately 7.5 mA / cm) to the lithium potential, and the capacity at which it reached 0.4 V was taken as the 0.5 C discharge capacity (mAh / g). 2 ) was discharged at a constant current of 3C down to 1.5V, and the capacity at the time when it reached 0.4V was defined as the 3C discharge capacity (mAh / g). The capacity retention rate was calculated using the following formula: Capacity retention rate [%] = 3C discharge capacity / 0.5C discharge capacity × 100

[0182] The evaluation results of the physical properties of the current collector and the evaluation results of the electrode and battery characteristics for each example and comparative example are shown in Tables 5 to 8 below, respectively.

[0183]

[0184]

[0185]

[0186]

[0187] As shown in Tables 5 to 8, in Comparative Example A1, although a current collector having a three-dimensional porous structure was used, the median diameter of the active material relative to the average opening diameter of the current collector was large, and therefore the filling rate of the voids in the current collector was small, and the capacity retention rate (3C / 0.5C) of the battery was small. This capacity retention rate was approximately the same as the capacity retention rate (3C / 0.5C) of the battery in Comparative Example A2, which used rolled copper foil as the current collector.

[0188] On the other hand, in Examples A1 and A2, a current collector having a three-dimensional porous structure is used, and the median diameter of the active material relative to the average pore diameter of the current collector is controlled within a predetermined range. This allows the battery capacity retention rate (3C / 0.5C) to be significantly improved compared to Comparative Examples A1 and A2.

[0189] [Example A3] Preparation of Negative Electrode Active Material <Preparation of Carbon Precursor> Coconut shells were crushed and dry distilled at 500°C to obtain coconut shell char (containing 98% by weight of particles with a particle size of 0.850 to 2.360 mm). Nitrogen gas containing 1% by volume of hydrogen chloride gas was supplied at a flow rate of 10 L / min to 100 g of coconut shell char. After heating at 950°C for 80 minutes, the supply of hydrogen chloride gas was stopped, and the carbon precursor was further heat-treated at 950°C for 30 minutes. The material was then coarsely crushed to an average particle size of 10 μm in a ball mill, and then crushed in a compact jet mill (Seishin Enterprise Co., Ltd.'s "Cojet System α-mkIII"). The material was further classified using Labocruseal N-01 (Seishin Enterprise Co., Ltd.) to obtain a carbon precursor with a specific surface area of ​​400 m. 2 / g, a carbon precursor having a predetermined particle size was obtained.

[0190] <Preparation of Carbonaceous Material> 9.1 g of carbon precursor was mixed with 0.9 g of polystyrene (manufactured by Sekisui Plastics Co., Ltd., average particle size 400 μm, residual carbon rate 1.2%). 10 g of the mixture was placed in a high-speed heating furnace manufactured by Motoyama Corporation, heated to 1290°C under a nitrogen flow rate of 6 L / min, held at that temperature for 10 minutes, and then naturally cooled. After confirming that the temperature inside the furnace had dropped to 200°C or less, the carbonaceous material was removed from the furnace to obtain hard carbon (median diameter D 50 : 1.3 μm).

[0191] A negative electrode for a battery and a battery were produced in the same manner as in Example A2, except that the obtained hard carbon was used as the negative electrode active material instead of the artificial graphite.

[0192] Examples A4, A5, and A6 A negative electrode for a battery and a battery were produced in the same manner as in Example A3, except that hard carbon having a median diameter shown in Table 10 was used as the negative electrode active material.

[0193] Comparative Example A3 A battery negative electrode and a battery were produced in the same manner as in Example A3, except that the meltblown nonwoven fabric produced in Example A1 was used as the nonwoven fabric.

[0194] The evaluation results of the physical properties of the current collector, the physical properties of the active material and the slurry, and the evaluation results of the electrode and battery characteristics for each Example and Comparative Example are shown in Tables 9 to 12 below, respectively.

[0195]

[0196]

[0197]

[0198]

[0199] As shown in Tables 9 to 12, in Examples A3 to A6, the median diameter of the active material relative to the average pore size of the current collector was controlled within a predetermined range regardless of the median diameter of the active material, so the battery capacity retention rate (3C / 0.5C) was able to be 90% or higher. On the other hand, in Comparative Example A3, although a current collector having a three-dimensional porous structure was used, the median diameter of the active material relative to the average pore size of the current collector was small, so the capacity retention rate was lower than in Examples A3 to A6 despite using the same active material as in Example A3.

[0200] [Example A7] Preparation of current collector (Al plating) (2) Both fiber surfaces of the meltblown nonwoven fabric obtained in (1) of Example 1 were coated with Al by vapor deposition. 2 A conductive nonwoven fabric having a conductivity of 1 / second was obtained.

[0201] Preparation of Electrode (Positive Electrode) <Preparation of Positive Electrode Slurry> Using a planetary mixer (ARE-250, manufactured by Thinky Corporation), the mixture was kneaded while appropriately adding N-methylpyrrolidone, and the slurry viscosity was adjusted to about 1500 mPa·s to prepare a positive electrode slurry. 3 parts by weight of polyvinylidene fluoride (KF Polymer 1700, manufactured by Kureha Corporation) was used as a binder, and LiNi with a median diameter of 10 μm was used as a positive electrode active material. 1/3 Co 1/3 M.N. 1/3 93 parts by weight of O2 ("Cellseed C-5H" manufactured by Nippon Chemical Industry Co., Ltd.) and 2 parts by weight of Super-P (manufactured by Timcal Corporation) as a conductive material were added. That is, the composition ratio of the active material, conductive additive, and binder in the positive electrode slurry was NCM powder:conductive additive:binder=95:2:3 (mass ratio) in terms of solid content.

[0202] <Preparation of Battery Positive Electrode> The obtained slurry was applied to a current collector made of the conductive nonwoven fabric using a bar coater (T101, manufactured by Matsuo Sangyo Co., Ltd.), left to stand for 5 minutes, and then transferred to a hot plate heated to 80°C for primary drying for 30 minutes. Next, a rolling process was performed using a roll press (manufactured by Hosen Co., Ltd.). After that, a battery electrode (diameter: 15 mm) was punched out, and then secondary drying was performed at 140°C for 3 hours under reduced pressure to prepare a coin battery electrode.

[0203] Comparative Example A4 A positive electrode for a battery was produced in the same manner as in Example A7, except that an aluminum foil (thickness: 20 μm) was used as the positive electrode current collector.

[0204] <Fabrication of Battery> The battery electrode obtained above was transferred to a glove box (manufactured by Miwa Manufacturing Co., Ltd.) under an argon gas atmosphere. Metallic lithium foil (thickness 0.2 mm, diameter 15 mm) was used as the negative electrode. A glass fiber nonwoven fabric (TGP-020A, manufactured by Nippon Sheet Glass Co., Ltd.) was used as the separator, and lithium hexafluorophosphate (LiPF 6 ) in a mixed solvent system (1M-LiPF F) containing ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) with vinylene carbonate (VC). 6 , EC / EMC / DMC=1 / 1 / 1 vol %, VC 1 wt %) were used to inject the electrolyte, and a coin battery (2032 type) was fabricated.

[0205] <Charge / Discharge Characteristics Test> The prepared coin battery was subjected to a charge / discharge test using a commercially available charge / discharge tester (TOSCAT3100, manufactured by Toyo Systems). The coin battery was placed in a thermostatic chamber at 25°C, and a current of 0.2 C (approximately 0.70 mA / cm) was applied to the lithium potential. 2 The battery was then charged at a constant current of 0.2 C (approximately 0.70 mA / cm) relative to the weight of the active material until the potential of the battery reached 3.0 V relative to the lithium potential. 2 The battery was charged at a constant current of 1000 mAh / g, and the capacity at this time was defined as the discharge capacity (mAh / g). The discharge capacity x electrode density was defined as the volumetric capacity. The percentage of the discharge capacity / charge capacity was defined as the charge / discharge efficiency, which was used as an index of the utilization efficiency of lithium ions in the battery.

[0206] <Discharge rate characteristic test> The coin battery used in the charge / discharge test was placed in a thermostatic chamber at 25°C, and charging was performed at a current of 0.2 C (approximately 0.70 mA / cm) relative to the weight of the active material until the voltage reached 4.2 V relative to the lithium potential. 2 ) was charged at a constant current of 0.5 C (about 1.75 mA / cm) relative to the lithium potential. 2 The coin battery was then charged again under the same conditions at a constant current of 3 C (approximately 10.5 mA / cm) to the lithium potential, and the capacity at which 3.0 V was reached was taken as the 0.5 C discharge capacity (mAh / g). 2 ) was discharged at a constant current of 3C up to 3.0V, and the capacity at the time when 3.0V was reached was defined as the 3C discharge capacity (mAh / g). The capacity retention rate was calculated using the following formula: Capacity retention rate [%] = 3C discharge capacity / 0.5C discharge capacity × 100

[0207] The evaluation results of the physical properties of the current collectors, the physical properties of the active materials and the slurries, and the evaluation results of the electrode and battery characteristics in Example A7 and Comparative Example A4 are shown in Tables 13 to 16 below, respectively.

[0208]

[0209]

[0210]

[0211]

[0212] As shown in Tables 13 to 16, in Example A7, the median diameter of the active material relative to the average opening diameter of the current collector was controlled within a predetermined range, and the filling rate was also high, so the capacity retention rate was higher than that of Comparative Example A4, in which aluminum foil was used as the current collector.

[0213] Example B1 Preparation of a current collector (1) A molten liquid crystal-forming wholly aromatic polyester (VECTRA-L manufactured by Polyplastics Co., Ltd.) consisting of a copolymer of parahydroxybenzoic acid and 6-hydroxy-2-naphthoic acid, having a melting point of 300°C and a melt viscosity of 15 Pa s at 310°C, was extruded using a twin-screw extruder and supplied to a melt-blown nonwoven fabric manufacturing apparatus having a nozzle with a nozzle hole diameter of 0.15 mm, L / D = 30, and 1,500 holes per meter width (nozzle hole spacing: 0.67 mm). The extrusion rate per hole was 0.10 g / min, the resin temperature was 330°C, the hot air temperature was 330°C, and the nozzle width was 18 Nm. 3 Sprayed at 4g / m 2 After obtaining a nonwoven fabric, it was heat-treated in air at 300°C for 6 hours. Thereafter, the obtained nonwoven fabric was passed between a metal roll heated to 110°C and a resin elastic roll (manufactured by Yuri Roll Co., Ltd.) with a surface Shore D hardness of 86 degrees, and continuously treated using a pressure calendar at a linear pressure of 120 kg / cm. The basis weight was 4 g / m as described above. 2 A meltblown nonwoven fabric having an average fiber diameter of 2.8 μm was obtained. (2) A palladium catalyst was applied to the fiber surface of the meltblown nonwoven fabric obtained in (1) above, and the fabric was immersed in an electroless copper plating solution containing copper sulfate and potassium sodium tartrate (Rochelle salt), followed by rinsing with water to form a copper film on the surface of the nonwoven fabric. Subsequently, the fabric was immersed in an electrolytic nickel plating solution to coat the fabric with copper by electrolytic plating, followed by rinsing with water and drying. This resulted in a copper film laminated on the copper film, with a thickness of 16 μm and an air permeability of 204 cc / cm. 2 This conductive nonwoven fabric was used as a current collector.

[0214] Preparation of Electrode (Negative Electrode) <Preparation of Negative Electrode Slurry> 96.5 parts by weight of artificial graphite with a median diameter of 5.0 μm, styrene-butadiene rubber (SBR: "TRD2001" manufactured by JSR Corporation) 2.0 parts by weight, carboxymethyl cellulose (CMC: "Cellogen BSH-6" manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) 1.0 parts by weight, carbon black (CB: "Super P" manufactured by MTI Co., Ltd.) 0.5 parts by weight were kneaded with 106.3 parts by weight of ion-exchanged water. Furthermore, to this kneaded mixture, 2.1 parts by weight of ethanol ("Ethanol (99.5)" manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added as a surface conditioner and kneaded to obtain a slurry with a viscosity of approximately 3000 mPa s (ratio of ethanol to the total weight of the slurry: 1 wt%). The solvent in the obtained slurry is referred to as an aqueous solvent (water containing 1 wt% ethanol).

[0215] <Preparation of Battery Negative Electrode> The obtained slurry was applied to a current collector made of the conductive nonwoven fabric using a bar coater (T101, manufactured by Matsuo Sangyo Co., Ltd.), allowed to stand for 15 minutes, and then subjected to primary drying at 86°C for 30 minutes in a hot air dryer (manufactured by Yamato Scientific Co., Ltd.). This was then rolled using a roll press (manufactured by Hosen Co., Ltd.). After that, a battery electrode (diameter: 14 mm) was punched out, and secondary drying was performed at 120°C for 3 hours under reduced pressure to prepare a coin battery electrode.

[0216] [Example B2] A battery negative electrode was produced in the same manner as in Example B1(2), except that 104.2 parts by weight of ion-exchanged water and 4.2 parts by weight of ethanol ("Ethanol (99.5)" manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were used in Example B1, thereby using an aqueous solvent (water containing 2 wt % ethanol) as the slurry solvent.

[0217] [Example B3] A battery negative electrode was produced in the same manner as in Example B1, except that 97.9 parts by weight of ion-exchanged water and 10.4 parts by weight of ethanol ("Ethanol (99.5)" manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were used in Example B1, thereby using an aqueous solvent (water containing 5 wt % ethanol) as the slurry solvent.

[0218] [Example B4] As in Example B1(1), a fabric having a basis weight of 11 g / m 2A meltblown nonwoven fabric having an average fiber diameter of 5.1 μm was prepared, and an aqueous solvent (water containing 5 wt% ethanol) was used as the slurry solvent. A battery negative electrode was prepared in the same manner as in Example B1, except that the meltblown nonwoven fabric of Example B9 was used as the nonwoven fabric, and 94 parts by weight of artificial graphite having a median diameter of 5.0 μm was used to prepare a negative electrode slurry.

[0219] [Example B5] A battery negative electrode was produced in the same manner as in Example B1, except that 108.1 parts by weight of ion-exchanged water and 0.2 parts by weight of antifoaming agent were used, thereby using an aqueous solvent (water containing 0.1 wt % of antifoaming agent) as the slurry solvent. "Noptex E-D54" manufactured by San Nopco Ltd. was used as the antifoaming agent.

[0220] [Example B6] A negative electrode slurry was prepared in the same manner as in Example B1, except that 108.3 parts by weight of ion-exchanged water was used in Example B1 and kneading was performed without adding ethanol, and the resulting slurry was applied to the current collector obtained in Example B1 by dipping. A battery negative electrode was prepared in the same manner as in Example B1, except that ultrasonic degassing treatment was performed during impregnation.

[0221] Example B7 A battery negative electrode was produced in the same manner as in Example B1, except that the negative electrode slurry was prepared using 100 parts by weight of artificial graphite having a median diameter of 5.0 μm, 3.125 parts by weight of a 10 wt % aqueous solution of polyvinyl alcohol (PVA215 (manufactured by Kuraray Co., Ltd.): polymerization degree 1700, saponification degree 88) as a solid content, and ion-exchanged water added to give a slurry viscosity of approximately 10,000 mPa s.

[0222] [Example B8] A battery negative electrode was produced in the same manner as in Example B1, except that the negative electrode slurry was prepared using 100 parts by weight of artificial graphite having a median diameter of 5.0 μm, 3.125 parts by weight of a 10 wt % aqueous solution of polyvinyl alcohol (PVA235 (manufactured by Kuraray Co., Ltd.): polymerization degree 3500, saponification degree 88) as a solid content, and ion-exchanged water added to give a slurry viscosity of approximately 3000 mPa s.

[0223] Example B9 A battery negative electrode was produced in the same manner as in Example B1, except that the negative electrode slurry was prepared using 100 parts by weight of artificial graphite having a median diameter of 5.0 μm, 3.125 parts by weight of a 10 wt % aqueous solution of polyvinyl alcohol (PVA235 (manufactured by Kuraray Co., Ltd.): polymerization degree 3500, saponification degree 88) as a solid content, and ion-exchanged water added to give a slurry viscosity of approximately 10,000 mPa s.

[0224] Example B10 A negative electrode for a battery was produced in the same manner as in Example B2, except that the slurry viscosity was set to about 10,000 Pa·s.

[0225] Example B11 A negative electrode for a battery was produced in the same manner as in Example B1, except that the amount of ion-exchanged water was changed to 108.3 parts by weight and kneading was performed without adding ethanol.

[0226] Comparative Example B1 A negative electrode for a battery was produced in the same manner as in Example B5, except that a rolled copper foil (thickness: 10 μm) was used as the negative electrode current collector.

[0227] [Comparative Example B2] A slurry was prepared in the same manner as in Example B9, except that the particle size of the artificial graphite was changed to 21 μm. The viscosity of the slurry was about 3000 Pa. A battery negative electrode was produced using this slurry in the same manner as in Example B1.

[0228] <Fabrication of Battery> The battery electrode obtained above was transferred to a glove box (manufactured by Miwa Seisakusho) under an argon gas atmosphere. Metallic lithium foil (thickness 0.2 mm, diameter 15 mm) was used as the positive electrode. A polypropylene separator (Celgard #2400, manufactured by Polypore) was used, and lithium hexafluorophosphate (LiPF 6 ) in a mixed solvent system (1M-LiPF F) containing ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) with vinylene carbonate (VC). 6 , EC / EMC / DMC=3 / 3 / 4 vol%, VC 1 wt%) were used to inject the electrolyte, and a coin battery (2032 type) was fabricated.

[0229] <Charge / Discharge Characteristics Test> The prepared coin batteries were subjected to a charge / discharge test using a commercially available charge / discharge tester (TOSCAT3100, manufactured by Toyo Systems). The coin batteries were placed in a thermostatic chamber at 25°C and charged at 0.2 C (approximately 0.50 mA / cm) relative to the weight of the active material until the charge reached 0 V relative to the lithium potential. 2 ), and then constant voltage charging was performed at 0 V down to a current of 0.0385 mA relative to the lithium potential. The capacity at this time was recorded as the charge capacity (mAh / g). Next, constant current charging was performed at 0.2 C (approximately 0.50 mA / cm) relative to the lithium potential. 2 The battery was discharged at a constant current of 1.5 V at 200 V, and the capacity at this time was defined as the discharge capacity (mAh / g). The discharge capacity x electrode density was defined as the volumetric capacity. The percentage of the discharge capacity / charge capacity was defined as the charge / discharge efficiency, which was used as an index of the utilization efficiency of lithium ions in the battery.

[0230] <Discharge rate characteristic test> The coin battery used in the charge / discharge test was placed in a thermostatic chamber at 25°C, and charging was performed at a current of 0.2 C (approximately 0.50 mA / cm) relative to the weight of the active material until the battery reached 0 V relative to the lithium potential. 2 ) was charged, and then constant voltage charging was performed from 0 V to a current of 0.0385 mA relative to the lithium potential. 2 The coin battery was then charged again under the same conditions at a constant current of 3 C (approximately 7.5 mA / cm) to the lithium potential, and the capacity at which it reached 0.4 V was taken as the 0.5 C discharge capacity (mAh / g). 2 ) was discharged at a constant current of 3C down to 1.5V, and the capacity at the time when it reached 0.4V was defined as the 3C discharge capacity (mAh / g). The capacity retention rate was calculated using the following formula: Capacity retention rate [%] = 3C discharge capacity / 0.5C discharge capacity × 100

[0231] The evaluation results of the physical properties of the current collector and the evaluation results of the electrode and battery characteristics for each Example and Comparative Example are shown in Tables 17 to 20 below, respectively.

[0232]

[0233]

[0234]

[0235]

[0236] In Comparative Example B1, copper foil was used as the current collector, and therefore the volumetric capacity in the initial charge-discharge characteristics and the capacity retention rate in the discharge rate characteristics could not be improved.

[0237] Comparative Example B2 corresponds to Example 3 of Patent Document 1, but the median diameter D of the active material relative to the average opening diameter of the current collector is 50 The filling rate in the current collector is 35%, and the volumetric capacity in the initial charge-discharge characteristics and the capacity retention rate in the discharge rate characteristics cannot be improved.

[0238] In contrast to this, as shown in Tables 17 to 20, in Examples B1 to B11, the particle size of the graphite active material was reduced, thereby enabling a significant improvement in charge capacity.

[0239] However, while the capacity retention rates of Examples B9 to B11, in which the current collector packing rate was less than 45%, remained below 80%, Examples B1 to B8, in which the packing rate was 45% or more, showed higher capacity retention rates of over 80%. In Example B9, not only was the slurry viscosity high but the surface tension of the slurry was also high, making it impossible to increase the packing rate inside the current collector, and the volumetric capacity in the initial charge-discharge characteristics and the capacity retention rate in the discharge rate characteristics were not as improved as in Examples B1 to B9.

[0240] In Example B10, although the surface tension is reduced by using an aqueous solvent containing ethanol, the high viscosity of the slurry makes it impossible to increase the filling rate inside the current collector, and the volumetric capacity in the initial charge-discharge characteristics and the capacity retention rate in the discharge rate characteristics are not as improved as in Examples B1 to B9.

[0241] Although the slurry viscosity was reduced in Example B11, the surface tension of the slurry was high, so the filling rate inside the current collector could not be increased, and the volumetric capacity in the initial charge-discharge characteristics and the capacity retention rate in the discharge rate characteristics were not improved as much as in Examples B1 to B9.

[0242] In contrast, in Examples B1 to B5, the slurry viscosity and surface tension of the slurry were adjusted, so that the filling rate in the current collector could be increased to 45% or more. As a result, the volumetric capacity in the initial charge-discharge characteristics was further improved, and the capacity retention rate in the discharge rate characteristics was also improved.

[0243] In Example B6, even when the same slurry as in Example B10 was used, the filling rate was improved compared to Example B10 by dip-coating the slurry while applying ultrasonic waves during application. As a result, the volumetric capacity in the initial charge-discharge characteristics was improved, and the capacity retention rate in the discharge rate characteristics was also improved.

[0244] In addition, by reducing the molecular weight of the binder component in Example B7 and by reducing the concentration of the binder component in the slurry in Example B8, the packing ratio was improved compared to Example B11 even when the surface tension of the slurry was high, resulting in improved volumetric capacity in the initial charge-discharge characteristics and improved capacity retention in the discharge rate characteristics. However, in Examples B6 and B7, some powder falling occurred due to the low viscosity of the binder component.

[0245] In the above examples, the electrode according to the present invention is applied to the negative electrode of a button battery, but the present invention is not limited to this. Alternatively, the electrode according to the present invention may be applied to the positive electrode of a button battery. Furthermore, the nonaqueous electrolyte battery is not limited to a "button battery" and may be a battery of other shapes, such as a cylindrical shape.

[0246] Furthermore, in the above embodiment, the electrolyte is in a liquid state, but this is not limiting, and electrolytes in other forms such as gel may also be used.

[0247] The electrode of the present invention can improve the capacity retention rate of various electrochemical devices, and the electrochemical devices can be used in, for example, mobile terminals such as smartphones and laptop computers, and various vehicles that use the electrochemical device as a power supply (e.g., electric vehicles, hybrid vehicles, etc.).

[0248] While the preferred embodiments of the present invention have been described above with reference to the drawings, those skilled in the art will readily recognize various changes and modifications within the scope of the present invention upon reading the specification. Accordingly, such changes and modifications are to be interpreted as falling within the scope of the invention as defined by the claims.

[0249] 1 Current collector 2 Active material 3 Gap 4 Positive electrode 4a Positive electrode current collector 4b Positive electrode active material component layer 5 Negative electrode 5a Negative electrode current collector 5b Negative electrode active material component layer 6 Separator

Claims

1. An electrode including a current collector and an active material, the current collector having a three-dimensional porous structure with an average opening diameter A, the active material having a median diameter (D50) B, and the average opening diameter A (μm) and the median diameter (D50) B (μm) satisfy the relationship of the following formula (1): 0.10≦B / A≦2.00 (1) 2. The electrode according to claim 1, wherein the current collector is filled with an active material component containing the active material, and the filling rate (%) defined by the following formula (2) is 37% or more: Filling rate (%) = β / (α-γ) x 100 (2) In the formula, α represents the observation area, which is determined by multiplying the thickness of the current collector by the observation length, determined from an electron microscope photograph of a cross section in the thickness direction of the electrode, and β and γ represent the projected areas of the active material and current collector, respectively, within the observation area, which are calculated using image analysis software.

3. An electrode comprising a current collector having a three-dimensional porous structure, the current collector being filled with an active material component containing an active material, and the filling rate (%) defined by the following formula (2) is 37% or more: Filling rate (%) = β / (α-γ) × 100 (2) In the formula, α represents the observation area, which is determined by multiplying the thickness of the current collector by the observation length, which is determined from an electron microscope photograph of a cross section in the thickness direction of the electrode, and β and γ represent the projected areas of the active material and current collector, respectively, within the observation area, which are calculated using image analysis software.

4. The electrode according to claim 3, wherein the filling rate is 45% or more.

5. The electrode according to any one of claims 1 to 4, wherein the current collector has a thickness of 100 µm or less.

6. The air permeability of the current collector is 0.1 to 600 cc / cm 2 5. The electrode according to claim 1 , wherein the electrical resistance is 1 / sec.

7. The electrode according to any one of claims 1 to 4, wherein the current collector comprises a non-conductive structure and a metal coating.

8. The electrode according to claim 7, wherein the non-conductive structure is a fiber assembly having an average fiber diameter of 10 μm or less.

9. The electrode according to claim 8, wherein the fiber assembly is a nonwoven fabric.

10. The electrode of claim 7, wherein the metal coating comprises at least one metal selected from the group consisting of aluminum, copper, nickel, gold, and silver.

11. The electrode according to any one of claims 1 to 4, wherein the active material is capable of absorbing and releasing electrolyte ions.

12. The electrode of any one of claims 1 to 4, wherein the electrode further comprises a conductive material.

13. The electrode according to any one of claims 2 to 4, wherein the median diameter of the active material is 0.1 to 16 μm.

14. The electrode of any one of claims 2 to 4, wherein the active material components include a water-insoluble binder.

15. A method for producing an electrode according to claim 1 or 2, comprising at least the steps of: preparing a current collector having a three-dimensional porous structure with an average opening size A; and forming an active material layer containing an active material with a median size B on the current collector, wherein the average opening size A and the median size B satisfy formula (1).

16. A method for producing an electrode according to any one of claims 2 to 4, comprising at least a step of filling an active material component into a current collector having a three-dimensional porous structure.

17. The air permeability of the current collector before being filled with the active material component is 0.1 to 600 cc / cm 2 The method for producing an electrode according to claim 16, wherein the electrochemical reaction is carried out at a rate of 1 / second.

18. The method for producing an electrode according to claim 16, wherein the thickness of the current collector before being filled with active material components is 100 μm or less.

19. An electrochemical device comprising an electrode according to any one of claims 1 to 14.

Citation Information

Patent Citations

  • Manufacturing method of battery electrode

    JP2010092721A

  • Conductive nonwoven fabric and secondary battery using it

    JP2012109224A

  • Positive electrode for lithium ion secondary battery, method for manufacturing the same, and lithium ion secondary battery formed by use thereof

    JP2014197479A

  • Electrode for non-aqueous electrolyte secondary cell and non-aqueous electrolyte secondary cell using same

    WO2013145752A1

  • Current collector, electrode, and non-aqueous electrolyte battery

    WO2022118692A1

Cited By

  • Three dimensional composite copper foil for solid lithium battery and method for manufacturing the same

    JP2026076935A