Surface-treated copper foil, copper-clad laminate, and printed wiring board
The surface-treated copper foil with a nickel alloy layer addresses the magnetization issue in nickel layers during heat treatment, achieving superior transmission characteristics and heat resistance by controlling magnetic flux densities, thus improving the performance of printed wiring boards.
Patent Information
- Application Number
- PCT/JP2024/012204
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-03
AI Technical Summary
The existing surface-treated copper foils used in printed wiring boards face challenges with nickel layers becoming magnetized during heat treatment, leading to deteriorated transmission characteristics and heat resistance issues due to the trade-off between these two properties.
A surface-treated copper foil with a nickel alloy layer containing elements like zinc, phosphorus, molybdenum, tungsten, chromium, iron, and cobalt, which suppresses magnetization even after heat treatment, maintaining excellent transmission characteristics and heat resistance by controlling the saturation and residual magnetic flux densities within specific limits.
The solution effectively reduces transmission loss and enhances heat resistance by preventing nickel layer magnetization, ensuring stable high-frequency signal transmission and reliable bonding with resin base materials.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002
Abstract
Description
Surface-treated copper foil, copper-clad laminates and printed wiring boards
[0001] The present invention relates to a surface-treated copper foil, a copper-clad laminate, and a printed wiring board.
[0002] Surface-treated copper foils are used in a variety of applications, such as copper foils for circuits in printed wiring boards and negative electrode current collectors in lithium-ion secondary batteries.
[0003] In particular, in the field of printed wiring boards, the recent trend toward smaller electronic devices and increased performance has led to higher density mounting of mounted components and higher signal frequencies, creating a demand for printed wiring boards with excellent high-frequency compatibility.
[0004] For copper foils for circuits used in such printed wiring boards, the surface condition of the circuit conductor, i.e., the dissimilar metals treated on the surface, becomes increasingly important due to the influence of the skin effect as the frequency increases. In particular, nickel (Ni), which is widely used as a dissimilar metal, is a metal that exhibits ferromagnetic properties at room temperature. Therefore, when nickel is present on the surface of copper foil for circuits, the magnetic effect affects the current distribution and magnetic field distribution within the conductor, resulting in a problem of deterioration of the transmission characteristics of the surface-treated copper foil.
[0005] On the other hand, when producing a printed wiring board, it is necessary to bond a copper foil for circuits to a resin substrate, and in this case, good adhesion is required between the copper foil and the resin substrate, and in particular, heat-resistant adhesion (hereinafter sometimes simply referred to as "heat resistance"). Nickel on the surface of the copper foil for circuits plays an important role in achieving such heat resistance. In other words, the presence of nickel on the surface of the copper foil for circuits is in a trade-off relationship between transmission characteristics and heat resistance.
[0006] Known examples aimed at improving both of the above characteristics include the techniques of Patent Documents 1 and 2. Patent Document 1 proposes controlling the total deposition amount of Co, Ni, and Mo in the surface treatment layer of copper foil to a predetermined amount or less and forming particles of a predetermined shape in the surface treatment layer in order to suppress the influence of ferromagnetic metals on transmission characteristics. Patent Document 2 also proposes a surface-treated copper foil in which the magnetism is controlled to a predetermined condition (demagnetized) by controlling the manufacturing process of the base foil (copper foil substrate) of the surface-treated copper foil.
[0007] Patent No. 7055049 Patent No. 7174869
[0008] However, in both Patent Documents 1 and 2, only the magnetism of the surface-treated copper foil that has no thermal history after production is considered, and no consideration is given to the influence of thermal pressure bonding with a resin substrate or thermal load during solder reflow in the manufacturing process of a printed wiring board.
[0009] In response to this, the present inventors have conducted extensive research and found that even if a surface-treated copper foil having a surface treatment film containing a nickel-containing surface treatment layer (hereinafter, simply referred to as a "nickel layer (Ni layer)") is demagnetized without any thermal history after production, when the surface-treated copper foil serving as a circuit conductor is subjected to heat treatment during the process of producing the above-mentioned printed wiring board, the nickel layer in the surface treatment film of the surface-treated copper foil may subsequently develop magnetism (become magnetized). As described above, if the nickel layer in the surface treatment film of the surface-treated copper foil serving as a circuit conductor is magnetized by the heat treatment received during the process of producing a printed wiring board, this will result in a problem of deterioration in transmission characteristics. Therefore, there is a need for a surface-treated copper foil that can suppress magnetization of the nickel layer even after a predetermined heat treatment and can exhibit excellent transmission characteristics and heat resistance.
[0010] Therefore, an object of the present invention is to provide a surface-treated copper foil, a copper-clad laminate, and a printed wiring board that can suppress magnetization of the nickel layer even after a predetermined heat treatment and exhibit excellent transmission characteristics and heat resistance.
[0011] That is, the gist of the present invention is as follows: [1] A surface-treated copper foil having a surface treatment film including a surface treatment layer containing nickel on at least one surface of a copper foil substrate, wherein the saturation magnetic flux density (Bs) after heat treatment at 300°C for 2 hours is 300 ) is 5.0 x 10 -3 [2] The residual magnetic flux density (Br 300 ) is 5.0 x 10 -4[3] The surface-treated copper foil according to the above [1] or [2], which satisfies the following requirements (I) and (II): Requirement (I): The rate of increase in saturation magnetic flux density Bs after heat treatment at 300°C for 2 hours [{(Bs 300 -Bs 0 ) / Bs 0}×100] is 300% or less. Requirement (II): The increase rate of residual magnetic flux density Br after heat treatment at 300° C. for 2 hours [{(Br 300 -Br 0 ) / Br 0}×100] is 300% or less. 300 is the saturation magnetic flux density after heat treatment at 300°C for 2 hours, Bs 0 is the saturation magnetic flux density before the heat treatment, Br 300 is the residual magnetic flux density after heat treatment at 300°C for 2 hours, Br 0 is the residual magnetic flux density before the heat treatment. [4] On the surface having the surface treatment film, the nickel deposition amount is 0.02 mg / dm 2 3.0 mg / dm or more 2 [5] The surface-treated copper foil according to any one of [1] to [3] above, wherein the surface treatment film comprises, in order from the copper foil substrate side, a roughening treatment layer and the nickel-containing surface treatment layer, and the arithmetic mean height Sa of the surface of the surface treatment film, measured optically in accordance with ISO 25178, is 0.02 μm or more and 0.35 μm or less. [6] The surface-treated copper foil according to any one of [1] to [5] above, wherein the nickel-containing surface treatment layer is made of a nickel alloy containing one or more elements selected from the group consisting of zinc, phosphorus, molybdenum, tungsten, chromium, iron, cobalt, and niobium. [7] A copper-clad laminate comprising the surface-treated copper foil according to any one of [1] to [6] above. [8] A printed wiring board comprising the copper-clad laminate according to [7] above.
[0012] According to the present invention, it is possible to provide a surface-treated copper foil, a copper-clad laminate, and a printed wiring board that can suppress magnetization of the nickel layer even after a predetermined heat treatment and exhibit excellent transmission characteristics and heat resistance.
[0013] The surface-treated copper foil, copper-clad laminate, and printed wiring board according to the present invention will be described in detail below. In this specification, the term "A to B" used to describe numerical values means "A or more and B or less" (when A<B) or "A or less and B or more" (when A>B). In the present invention, a combination of preferred embodiments is a more preferred embodiment.
[0014] [Surface-treated copper foil] The surface-treated copper foil of the present invention has a surface treatment film including a surface treatment layer containing nickel on at least one surface of a copper foil substrate, and has a saturation magnetic flux density (Bs 300 ) is 5.0 x 10 -3 It is below T.
[0015] The surface-treated copper foil of the present invention has the above-mentioned structure, and therefore can suppress the magnetization of the nickel layer even after a predetermined heat treatment, and can exhibit excellent transmission characteristics and heat resistance. Although the detailed reason for such effects is not clear, the following is one possible reason.
[0016] First, in order to solve the above-mentioned problems, the present inventors conducted extensive research, focusing on the suppression of magnetization in the nickel layer after heat treatment. As a result of their research, the present inventors discovered that, in surface-treated copper foils having a conventional surface treatment film containing a nickel layer, (1) the magnetic flux density increases upon undergoing a predetermined heat treatment, and (2) in copper foil types in which the increase is large, the transmission loss in the high-frequency band increases significantly. Although the reason why the magnetic flux density increases in surface-treated copper foils after the predetermined heat treatment is not clear, one possible reason is that the heat treatment promotes crystallization and / or an increase in crystal grain size in the nickel layer, which causes magnetization of the nickel layer after the heat treatment.
[0017] Therefore, the inventors of the present invention have conducted further research and have found that by improving the nickel layer, it is possible to suppress the nickel layer from being magnetized by heat treatment, and that the saturation magnetic flux density (Bs 300 ) is 5.0 x 10 -3 It has been found that a surface-treated copper foil having a saturation magnetic flux density (SMD) of 0.1T or less can be obtained, and that such a surface-treated copper foil can reduce transmission loss and also exhibit excellent heat resistance. While the relationship between saturation magnetic flux density and transmission loss is not entirely clear, it is believed that the higher the frequency band, the greater the influence of the surface condition of the circuit conductor. The adhesion of ferromagnetic metal to the circuit conductor increases the transmission loss of high-frequency signals due to losses caused by the generation of eddy currents (losses resulting from an increase in the electrical resistance of the circuit conductor due to the generation of eddy currents) and magnetic hysteresis loss. Therefore, in the present invention, by controlling the saturation magnetic flux density of the nickel layer to a predetermined value or less, the magnetism of the circuit conductor can be reduced to a level that does not affect transmission loss in the high-frequency band, thereby significantly reducing transmission loss. Furthermore, by including a nickel layer as a surface treatment film, the surface-treated copper foil of the present invention is believed to exhibit excellent heat resistance. Such a surface-treated copper foil of the present invention is suitable for use in, for example, printed wiring boards. The use of the surface-treated copper foil of the present invention can achieve both reduced transmission loss and excellent heat resistance.
[0018] The surface-treated copper foil of the present invention will be described in detail below.
[0019] The surface-treated copper foil of the present invention has a surface treatment film including a nickel-containing surface treatment layer on at least one surface of a copper foil substrate.
[0020] <Copper Foil Substrate> The copper foil substrate serves as the base layer of the surface-treated copper foil. The copper foil substrate may be an electrolytic copper foil or a rolled copper foil, preferably an electrolytic copper foil. The thickness of the copper foil substrate is, for example, 5 to 210 μm, preferably 5 to 100 μm, and more preferably 5 to 40 μm. When the copper foil substrate is an electrolytic copper foil, the surface treatment film may be the surface of the electrolytic copper foil that is peeled from a rotating drum-shaped cathode (hereinafter simply referred to as a "drum-shaped cathode") (hereinafter referred to as the "drum side"), or the surface opposite the drum side (hereinafter referred to as the "non-drum side"), but is preferably the non-drum side. In general, the drum side is sometimes referred to as the glossy side (S side), and the non-drum side is sometimes referred to as the deposit side or matte side (M side).
[0021] <Surface Treatment Film> The surface treatment film is a layer formed on at least one surface of a copper foil substrate and serves to impart a desired function to the surface-treated copper foil. The surface treatment film may be formed on either the front or back surface of the copper foil substrate, or on both surfaces. The surface treatment film also includes a nickel layer. Specifically, the surface treatment film may be composed of only a nickel layer, or may include one or more other surface treatment layers. Examples of other surface treatment layers include a roughening treatment layer formed on the copper foil substrate, intermediate layers such as a zinc (Zn)-containing surface treatment layer (hereinafter sometimes referred to as a "zinc layer (Zn layer)") and a chromium (Cr)-containing surface treatment layer (hereinafter sometimes referred to as a "chromium layer (Cr layer)") formed on a nickel layer, and chemical adhesion layers formed using a silane coupling agent or the like.
[0022] The surface of the surface treatment film is at least one of the front and back surfaces of the surface-treated copper foil, and is the surface of the copper foil substrate having a surface treatment film containing a nickel layer. The surface of such a surface treatment film may be the surface of a nickel layer formed on the copper foil substrate, or the surface of another surface treatment layer (e.g., a chemical adhesion layer formed by a silane coupling agent) formed directly or indirectly on the nickel layer. Furthermore, when the surface-treated copper foil of the present invention is used for the conductor circuit of a printed wiring board, the surface of the surface treatment film, preferably the surface of the surface treatment film further including a roughening treatment layer, serves as the surface (adhesion surface) for adhering and laminating a resin substrate.
[0023] (Surface Treatment Layer Containing Nickel) The surface treatment film includes a surface treatment layer containing nickel (nickel layer). The nickel layer serves as a base layer for the surface-treated copper foil.
[0024] The nickel layer may be any layer containing nickel, and may be a single layer or a multi-layer consisting of two or more layers of different compositions, but is preferably a single layer from the viewpoint of ease of production.
[0025] The nickel layer may be composed of nickel alone or an alloy of nickel and other elements (hereinafter also referred to as "nickel alloy"). However, from the viewpoint of reducing transmission loss while exhibiting excellent heat resistance, a nickel alloy is preferable. The nickel alloy is preferably a nickel alloy containing one or more elements selected from the group consisting of zinc (Zn), phosphorus (P), molybdenum (Mo), tungsten (W), chromium (Cr), iron (Fe), cobalt (Co), and niobium (Nb), more preferably a nickel alloy containing one or more elements selected from the group consisting of Zn, P, Mo, W, Cr, and Co. More specifically, the nickel alloy is preferably one or more elements selected from the group consisting of Ni—P, Ni—Zn, Ni—Mo, Ni—W, Ni—Cr, Ni—Co, Ni—Zn—P, Ni—Zn—Mo, and Ni—Zn—Cr. The metal or alloy composition constituting the nickel layer can be confirmed by the method described in the Examples.
[0026] On the surface having the surface treatment film, the amount of nickel deposited is preferably 0.02 mg / dm 2 3.5mg / dm or more 2 or less, more preferably 0.02 mg / dm 2 3.0 mg / dm or more 2 More preferably, 0.02 mg / dm 2 2.0 mg / dm or more 2 More preferably, 0.02 mg / dm or less 2 More than 1.0 mg / dm 2 By setting the content within the above range, it is possible to reduce transmission loss while exhibiting excellent heat resistance. The amount of nickel deposited on the surface having the surface treatment film can be measured by the method described in the Examples.
[0027] (Other Surface Treatment Layers) The surface treatment film may further include other surface treatment layers in addition to the nickel layer, as necessary. Examples of other surface treatment layers include a roughening layer formed on the copper foil substrate, an intermediate layer such as a Zn layer or a Cr layer formed on the Ni layer, and a chemical adhesion layer formed by a silane coupling agent.
[0028] <Magnetic Properties of Surface-Treated Copper Foil> The surface-treated copper foil of the present invention has a saturation magnetic flux density (Bs 300 ) is 5.0 × 10 -3 T or less, preferably 2.0 × 10 -3 T or less, more preferably 7.0 × 10 -4 By setting the saturation magnetic flux density (Bs) within the above range, the magnetism caused by heating can be reduced, the transmission loss can be reduced, and excellent heat resistance can also be exhibited. 300 ) is preferably 1.0 × 10 from the viewpoint of productivity, for example. -6 T or more, more preferably 5.0 × 10 -6 T or more, more preferably 2.0 × 10 -5 T or above.
[0029] The surface-treated copper foil of the present invention has a residual magnetic flux density (Br 300 ) is preferably 6.0 × 10-4 T or less, more preferably 5.0 × 10 -4 T or less, more preferably 4.0 × 10 -4 T or less. By keeping it within the above range, it is possible to effectively reduce the development of magnetism due to heat treatment, and to further reduce transmission loss. In particular, it is thought that the higher the residual magnetic flux density, the greater the loss due to the generation of eddy currents and the magnetic hysteresis loss, and the greater the transmission loss of high frequency signals. Therefore, it is thought that by reducing the above-mentioned predetermined residual magnetic flux density, it is possible to further reduce transmission loss significantly. Note that the residual magnetic flux density (Br 300 ) is preferably 1.0 × 10 from the viewpoint of productivity, for example. -7 T or more, more preferably 5.0 × 10 -7 T or more, more preferably 3.0 × 10 -6 T or above.
[0030] The surface-treated copper foil of the present invention preferably satisfies the following requirements (I) and (II): Requirement (I): The increase rate of saturation magnetic flux density Bs after heat treatment at 300°C for 2 hours [{(Bs 300 -Bs 0 ) / Bs 0}×100] is preferably 310% or less, more preferably 300% or less, even more preferably 200% or less, and even more preferably 100% or less. Requirement (II): The increase rate of residual magnetic flux density Br after heat treatment at 300° C. for 2 hours [{(Br 300 -Br 0 ) / Br 0}×100] is preferably 310% or less, more preferably 300% or less, even more preferably 200% or less, and even more preferably 100% or less. 300 is the saturation magnetic flux density after heat treatment at 300°C for 2 hours, Bs 0 is the saturation magnetic flux density before the heat treatment, Br 300 is the residual magnetic flux density after heat treatment at 300°C for 2 hours, Br 0is the residual magnetic flux density before the heat treatment. By satisfying the above requirements, the increase in each magnetic flux density after heat treatment can be kept within a predetermined range, thereby further reducing transmission loss. In particular, with surface-treated copper foils with a large increase in magnetic flux density after heat treatment, the waveform of the high-frequency signal tends to become unstable when measuring transmission loss. It is believed that this phenomenon occurs because, when the thermal load during the manufacturing process of a printed wiring board is distributed in the plane, changes in the magnetization distribution occur within the plane of the printed wiring board. Therefore, it is believed that the quality of high-frequency signals can be improved by controlling the increase in magnetic flux density after heat treatment within a certain range.
[0031] The saturation magnetic flux density Bs and residual magnetic flux density Br before and after the predetermined heat treatment can be measured by the following method. First, the surface-treated copper foil after the predetermined heat treatment is obtained by heating the surface-treated copper foil at 300°C for 2 hours. The surface-treated copper foil before and after the heat treatment is cut into a size of 10 mm x 10 mm, respectively, and the saturation magnetic flux density Bs and residual magnetic flux density Br are measured using a vibrating sample magnetometer (VSM) under the following conditions: Applied magnetic field range: ±10,000 [Oe] Sweep rate: 50 [Oe / s] More specifically, the magnetic properties can be measured by the method described in the examples.
[0032] <Surface Roughness of Surface-Treated Copper Foil> When the surface treatment film of the surface-treated copper foil of the present invention includes, in order from the copper foil substrate side, a roughened layer and the nickel layer, the arithmetic mean height Sa of the surface of the surface treatment film, measured optically in accordance with ISO 25178, is preferably 0.02 μm or more and 0.50 μm or less, more preferably 0.02 μm or more and 0.35 μm or less, even more preferably 0.02 μm or more and 0.30 μm or less, and even more preferably 0.02 μm or more and 0.20 μm or less. This configuration can reduce transmission loss while exhibiting excellent heat resistance. In particular, in the surface-treated copper foil, by including a roughened layer below the nickel layer (on the copper foil substrate side), adhesion to the resin substrate can be improved. In this case, by having the uneven shape on the surface of the surface treatment film within the above-mentioned specified range, adhesion to the resin substrate can be improved without adversely affecting transmission loss. The arithmetic mean height Sa can be measured by the method described in the examples.
[0033] <Method for producing surface-treated copper foil> Next, an example of a preferred method for producing the surface-treated copper foil of the present invention will be described. A preferred method for producing the surface-treated copper foil of the present invention includes a step of forming a surface treatment film containing a nickel layer on at least one surface of a copper foil substrate, more specifically, a step of forming a nickel layer directly or indirectly on at least one surface of the copper foil substrate.
[0034] (Copper Foil Substrate) As the copper foil substrate, it is preferable to use an electrolytic copper foil or a rolled copper foil having a smooth and glossy surface without large irregularities. Among them, it is preferable to use an electrolytic copper foil from the viewpoint of productivity and cost, and it is particularly preferable to use the non-drum side of the electrolytic copper foil as the side on which the surface treatment film is formed. In addition, it is preferable that the surface of the drum-shaped cathode used in the production of the electrolytic copper foil is polished with a buff of #1000 to #2500.
[0035] The copper foil substrate preferably has a ten-point average roughness Rzjis of 2 μm or less, more preferably 1 μm or less, and even more preferably 0.8 μm or less, at least on the surface on which the surface treatment film is formed. By ensuring a roughness within the above range, adhesion to the resin substrate can be improved and transmission loss does not deteriorate. Furthermore, the copper foil substrate preferably has a ten-point average roughness Rzjis of 2 μm or less, more preferably 1 μm or less, and even more preferably 0.8 μm or less on both sides. The lower limit of the ten-point average roughness Rzjis on each surface of the copper foil substrate is, for example, 0.1 μm or more, from the viewpoint of ease of production or availability. The ten-point average roughness Rzjis can be measured using a contact surface roughness measuring instrument according to the method specified in JIS B0601:2001. Specifically, it can be measured by the method described in the examples.
[0036] The thickness of the copper foil substrate is, for example, 5 to 210 μm, preferably 5 to 100 μm, and more preferably 5 to 40 μm.
[0037] (Nickel Treatment) The surface-treated copper foil of the present invention forms a nickel layer by nickel treatment. The nickel treatment is a treatment for directly or indirectly forming a nickel layer on at least one surface of a copper foil substrate. An object of the present invention is to obtain a surface-treated copper foil that can suppress magnetization of the nickel layer even after a predetermined heat treatment. In response to this, the present inventors conducted extensive research and concluded that the increase in magnetic flux density in surface-treated copper foil after a predetermined heat treatment is due to the progress of crystallization of the nickel layer and / or an increase in crystal grain size caused by the heat treatment. Focusing on this phenomenon, they investigated nickel treatments that can suppress this. Below, the following nickel treatments (A) and (B) are described in detail as suitable examples of the nickel treatments investigated by the present inventors.
[0038] Nickel Treatment (A) Nickel treatment (A) is an example of a nickel treatment that can suppress an increase in the crystal grain size in the nickel layer after a predetermined heat treatment, and is performed by pulse electrolysis with flow rate control.
[0039] Generally, pulse electrolysis allows for instantaneous application of a higher current density than conventional DC electrolysis, making it possible to form a plating film with a dense microcrystalline structure. However, because reactive species near the electrode are lost due to the instantaneous application of a high current density, pulse electrolysis requires alternating periods of current application and rest. To obtain a dense crystalline structure, the duty ratio (current application time / [current application time + current rest time]) must be reduced. However, reducing the duty ratio results in a large portion of the time during which no current is applied, raising concerns about reduced productivity. Furthermore, discontinuous multi-step plating makes it easier for impurities to be incorporated into the nickel layer, raising concerns about reduced heat resistance, which poses manufacturing challenges.
[0040] Therefore, the inventors conducted extensive research and found that the above-mentioned problems could be solved by controlling the liquid flow rate in the tank to increase the stirring speed in the liquid and supply sufficient reactive species near the electrodes, which serve as the reaction field. That is, by performing pulse electrolysis in a reaction field where the liquid flow rate is controlled, reactive species can be immediately supplied near the electrodes immediately after current application, making it possible to efficiently deposit nickel under conditions with a higher duty ratio than conventional methods. This also reduces the amount of impurities trapped between the nickel layers and makes it possible to electroplat a nickel layer with a fine crystal grain size.
[0041] In such pulse electrolysis, the duty ratio is preferably 0.1 to 0.9, more preferably 0.1 to 0.8, and the solution flow rate is preferably 15 to 110 L / min, more preferably 20 to 100 L / min. By keeping the duty ratio and solution flow rate within the above ranges, it is possible to efficiently deposit microcrystalline nickel, resulting in a microcrystalline nickel layer. Therefore, even after a predetermined heat treatment, the crystal grain size does not fully increase, and it is thought that magnetization of the nickel layer can be suppressed. On the other hand, if the duty ratio is too small, productivity tends to deteriorate, and if the duty ratio is too large, reactive species are not sufficiently supplied to the electrode surface, resulting in poor plating appearance on the electrode surface. Furthermore, if the flow rate is too small, reactive species are not sufficiently supplied to the electrode surface, and if the flow rate is too large, poor plating appearance on the electrode surface tends to occur due to reasons such as the inclusion of air bubbles in the solution.
[0042] Below, an example of the plating bath composition and electrolysis conditions suitable for nickel treatment (A) is shown. Note that the following conditions are a preferred example, and the type and amount of additives, electrolysis conditions, etc. can be appropriately changed and adjusted as needed within the range that does not impair the effects of the present invention. <Plating bath composition> Nickel sulfate hexahydrate: 10 to 80 g / L in terms of nickel (atom) Boric acid: 5 to 40 g / L pH: 3.0 to 5.0 <Pulse electrolysis conditions> Bath temperature: 10 to 60°C Current density: 1 to 15 A / dm 2 Current application time: 5 to 100 milliseconds Duty ratio: 0.1 to 0.9 Total charge: 0.5 to 30 A·S / dm 2 Liquid flow rate: 15-110L / min
[0043] Nickel Treatment (B) Nickel treatment (B) is an example of a nickel treatment that can suppress an increase in the crystal grain size in the nickel layer after a predetermined heat treatment, and is carried out by an electrochemical reduction reaction of nickel hydroxide. Specifically, it is as follows.
[0044] First, a nickel layer is formed on the surface of a copper foil substrate. Then, nickel hydroxide is deposited on the surface of the copper foil substrate by methods such as alkaline immersion, anodic oxidation, or nickel plating under alkaline pH conditions (hereinafter sometimes referred to as "hydroxide treatment"). The nickel hydroxide is then reduced to nickel by electrochemical reduction (hereinafter sometimes referred to as "reduction treatment"), reforming the nickel layer. It is believed that performing the reduction treatment under appropriate conditions can form a mixture of nickel hydroxide and metallic nickel in the nickel layer, resulting in random crystallinity and making the nickel layer amorphous. Furthermore, the presence of some oxygen atoms incorporated into the hydroxide at grain boundaries is believed to have the effect of suppressing the growth of crystal grain size during heating.
[0045] In such an electrochemical reduction reaction of nickel hydroxide, the current density is preferably 0.1 to 2.7 A / dm 2 , more preferably 0.2 to 2.5 A / dm 2 It is believed that the above-mentioned effects can be obtained by keeping the current density within the above range. On the other hand, if the current density is too low, the reduction of nickel hydroxide tends to be insufficient, and if the current density is too high, the crystal grain size tends to increase, and magnetism tends to be exhibited.
[0046] Below are examples of electroplating conditions, hydroxide treatment conditions, and reduction treatment conditions suitable for nickel treatment (B). Note that the following conditions are preferred examples, and the type and amount of additives, electrolysis conditions, etc. can be appropriately changed and adjusted as needed within the scope that does not impair the effects of the present invention. (1) First, it is preferable to perform electroplating under the following conditions. <Plating solution composition> Nickel sulfate hexahydrate: 20 to 60 g / L in terms of nickel (atom) Boric acid: 5 to 40 g / L pH: 3.0 to 5.0 <Electrolysis conditions> Bath temperature: 20 to 60°C Current density: 0.1 to 2.7 A / dm 2 Current application time: 1.5 to 30 seconds
[0047] (2) Next, it is preferable to sequentially perform a hydroxide treatment and a reduction treatment on the surface of the nickel layer obtained in (1) above under the following conditions: <Conditions for the hydroxide treatment> Aqueous sodium hydroxide solution: sodium hydroxide concentration 5 to 50 g / L Immersion time: 10 to 60 seconds <Conditions for the reduction treatment> Current density: 0.1 to 2.7 A / dm 2 Current application time: 10 to 60 seconds
[0048] Furthermore, alloying the nickel layer with dissimilar metals such as Zn, P, Mo, W, Cr, Fe, Co, and Nb can further suppress the increase in magnetization and improve heat resistance. The reaction mechanism for suppressing the magnetism of nickel as described above has a similar effect in plating baths containing dissimilar metals. For example, in nickel treatment (A), a finely crystallized nickel layer can be formed by adding elements such as a Zn source or a P source to the nickel plating bath used in pulse electrolysis.
[0049] In this embodiment, it is considered that the increase in magnetic flux density in the surface-treated copper foil after the predetermined heat treatment is due to the progress of crystallization of the nickel layer and / or an increase in the crystal grain size caused by the heat treatment, and the nickel treatments (A) and (B) are preferably exemplified as a means for improving this. However, the increase in magnetic flux density in the surface-treated copper foil after the predetermined heat treatment may be suppressed by means other than those described above.
[0050] (Roughening Treatment) The surface of the surface-treated copper foil of the present invention may be roughened to form a roughened layer on the surface of the copper foil substrate before nickel treatment. In this case, examples of the roughened layer include electrolytic deposition of copper particles and etching using hydrogen peroxide solution.
[0051] Furthermore, when a roughened layer is formed, it is desirable to control the treatment conditions so that the arithmetic mean height Sa of the surface of the surface treatment film including the roughened layer and the nickel layer, measured optically in accordance with ISO 25178, is preferably 0.02 μm or more and 0.50 μm or less, more preferably 0.02 μm or more and 0.35 μm or less, even more preferably 0.02 μm or more and 0.30 μm or less, and even more preferably 0.02 μm or more and 0.20 μm or less. By controlling the surface condition of the obtained surface-treated copper foil as described above, it is possible to further improve adhesion to the surface of the resin substrate while reducing transmission loss. Note that methods for controlling the treatment conditions include, for example, adjusting the current flow time or current flow amount if the roughened particles are formed by copper electrodeposition, or adjusting the treatment time if the roughened particles are formed by etching.
[0052] As the roughening treatment, it is preferable to perform the following roughening plating treatment (1) on the copper foil substrate surface before nickel treatment. If necessary, a fixed plating treatment (2) may be combined. Roughening Plating Treatment (1) <Plating Bath Composition> Copper sulfate pentahydrate: 3 to 20 g / L in terms of copper (atom) Sulfuric acid: 100 to 250 g / L Ammonium molybdate: 400 to 1200 mg / L in terms of molybdenum (atom) <Electroplating Treatment Conditions> Bath temperature: 5 to 20°C Current density: 5 to 55 A / dm 2 Current application time: 0.5 to 15 seconds Fixed plating process (2) <Plating bath composition> Copper sulfate pentahydrate: 40 to 70 g / L in terms of copper (atom) Sulfuric acid: 100 to 250 g / L <Electroplating process conditions> Bath temperature: 15 to 30°C Current density: 2 to 10 A / dm 2 Current application time: 0.5 to 5 seconds
[0053] (Other Treatments) The surface-treated copper foil of the present invention may further have a chemical adhesion layer such as a silane coupling agent layer formed on the nickel layer, either directly or via an intermediate layer such as a heat-resistant treatment layer containing zinc (Zn) or a rust-proofing treatment layer containing chromium (Cr). The intermediate layer and the chemical adhesion layer are so thin that they do not affect the roughness of the surface treatment surface and have little effect on the magnetism.
[0054] The heat-resistant layer is preferably formed when it is necessary to further improve the heat resistance of the surface treatment film. The heat-resistant layer is preferably formed, for example, from zinc or an alloy containing zinc. Examples of alloys containing zinc include zinc-tin (Sn) alloy, zinc-cobalt (Co) alloy, zinc-copper (Cu) alloy, zinc-molybdenum (Mo) alloy, zinc-chromium (Cr) alloy, and zinc-vanadium (V) alloy.
[0055] The rust prevention layer is preferably formed when it is necessary to further improve the corrosion resistance of the surface treatment film. Examples of the rust prevention layer include a chrome layer formed by chrome plating and a chromate layer formed by chromate treatment.
[0056] When both the heat-resistant treatment layer and the rust-proofing treatment layer are formed, it is preferable to form them on the surface treatment layer in this order. That is, when all of them are provided, the order is copper foil substrate-roughened treatment layer-nickel layer-heat-resistant treatment layer-rust-proofing treatment layer. Furthermore, depending on the application and the desired properties, only one or two of the heat-resistant treatment layer and the rust-proofing treatment layer may be formed.
[0057] Examples of methods for forming the chemical adhesion layer include a method in which a silane coupling agent solution is applied directly or via an intermediate layer to the surface of the nickel layer of the surface-treated copper foil, followed by air drying (natural drying) or heat drying. The silane coupling agent layer is formed when the water in the applied coupling agent solution evaporates. In particular, from the viewpoint of further promoting the dehydration reaction of the silane coupling agent, it is preferable to dry by heat drying at 100 to 220°C.
[0058] Furthermore, the silane coupling agent layer preferably contains one or more agents selected from the group consisting of epoxy-based silane coupling agents, amino-based silane coupling agents, vinyl-based silane coupling agents, methacrylic-based silane coupling agents, acrylic-based silane coupling agents, azole-based silane coupling agents, styryl-based silane coupling agents, ureido-based silane coupling agents, mercapto-based silane coupling agents, sulfide-based silane coupling agents, and isocyanate-based silane coupling agents.
[0059] [Uses] The surface-treated copper foil of the present invention is suitable for use in the manufacture of copper-clad laminates and further for the manufacture of printed wiring boards. That is, the copper-clad laminate of the present invention comprises the surface-treated copper foil of the present invention, and preferably further comprises a resin substrate laminated onto the surface treatment layer of the surface-treated copper foil. Furthermore, the printed wiring board of the present invention comprises the copper-clad laminate of the present invention. When a copper-clad laminate or a printed wiring board is manufactured using such a surface-treated copper foil, magnetization of the nickel layer can be suppressed even after a predetermined heat treatment. Therefore, the resulting copper-clad laminate or printed wiring board can reduce transmission loss and also exhibit good heat resistance due to the nickel layer.
[0060] In next-generation wireless transmission applications, the magnetism of circuit boards can itself pose a major problem. For example, telemedicine is one of the technologies expected to be realized in the next generation of 5G and 6G. However, when considering the use of printed wiring boards in magnetically-based testing devices such as MRI, the magnetization of the printed wiring board itself may cause problems such as inaccurate test results. Another example is wearable devices such as smartwatches. However, as these devices become more highly functional, problems such as improper operation due to magnetic defects may also arise. As the frequency of high-frequency signals increases in the future, the impact of magnetic metals on magnetic fields is expected to become greater. Therefore, in addition to reducing transmission loss, there is a demand for the use of nonmagnetic surface-treated copper foils as circuit conductors for printed wiring boards. From this perspective, the surface-treated copper foil of the present invention is extremely useful.
[0061] That is, the printed wiring board having the surface-treated copper foil of the present invention is suitable as a printed wiring board for use in a high frequency band (particularly a high frequency band of 1 to 100 GHz) and as a printed wiring board where the influence of a magnetic field is a concern.
[0062] A copper-clad laminate comprising the surface-treated copper foil of the present invention can be formed by a known method. Specifically, a copper-clad laminate is generally produced by laminating and adhering a surface-treated copper foil and a resin substrate (insulating substrate) so that the roughened surface (adhesion surface) of the surface-treated copper foil faces the resin substrate. In particular, when producing a copper-clad laminate using the surface-treated copper foil of the present invention, it is preferable to use the surface having a predetermined surface treatment film as the adhesion surface to the resin substrate. This reduces transmission loss and also provides good heat resistance due to the nickel layer.
[0063] The resin substrate may be, for example, a flexible resin substrate or a rigid resin substrate, and the surface-treated copper foil of the present invention is particularly suitable for use in combination with a rigid resin substrate, which requires high transmission characteristics and high adhesion in the high frequency band. Examples of resins that can form the resin substrate include epoxy resin, polyphenylene ether, phenol resin, bis(phenoxyphenoxy)benzene, polyimide, liquid crystal polymer, and fluororesin (e.g., polytetrafluoroethylene).
[0064] In addition, when producing a copper clad laminate for printed wiring boards, it may be produced by laminating a surface-treated copper foil having a silane coupling agent layer and a resin substrate by hot pressing. Note that a copper clad laminate for printed wiring boards produced by applying a silane coupling agent to a resin substrate, and laminating the resin substrate coated with the silane coupling agent and a surface-treated copper foil having a rust prevention treatment layer on the outermost surface by hot pressing also has the same effect as when using the surface-treated copper foil having the above-mentioned silane coupling agent layer.
[0065] Furthermore, a printed wiring board including the surface-treated copper foil of the present invention can be formed by a known method. Specifically, it may be formed using the above-mentioned copper-clad laminate for printed wiring boards. Such a printed wiring board preferably includes the above-mentioned copper-clad laminate for printed wiring boards.
[0066] The printed wiring board according to this embodiment can be obtained by, for example, etching the surface-treated copper foil of a copper-clad laminate to form a circuit, and then laminating another resin substrate to cover the circuit. The resin substrate to be laminated to cover the circuit may be of the same type as or a different type from the resin substrate of the copper-clad laminate.
[0067] The surface-treated copper foil of the present invention can also be suitably used as a negative electrode current collector for lithium ion secondary batteries, etc. The negative electrode current collector including the surface-treated copper foil of the present invention can be formed by a known method. Specifically, the negative electrode current collector is formed by applying carbon particles or the like as a negative electrode active material layer to the surface of the copper foil, drying the coated surface, and then pressing the coated surface.
[0068] Although the embodiments of the present invention have been described above, the above embodiments are merely examples of the present invention. The present invention includes all aspects encompassed by the concept of the present invention and the scope of the claims, and various modifications can be made within the scope of the present invention.
[0069] The present invention will be described in more detail below based on examples, which are merely examples of the present invention.
[0070] (Production Example 1: Preparation of copper foil substrate) A roll of electrolytic copper foil (double-sided glossy foil) having a ten-point average roughness Rzjis of 0.8 μm on the M side and a thickness of 18 μm was produced using the following cathode and anode as a copper foil substrate serving as a substrate for forming a surface treatment film, and a copper sulfate electrolyte of the following composition under the following electrolysis conditions. The ten-point average roughness Rzjis on the M side is a value measured under the following measurement conditions.
[0071] <Cathode and anode> Cathode: Titanium rotating drum with surface roughness adjusted by buffing with #1000 to #2000 grit Anode: Dimensionally stable anode DSA (registered trademark) <Electrolyte composition> Copper sulfate pentahydrate: 75 g / L in terms of copper (atom) Sulfuric acid: 65 g / L Chlorine concentration: 20 mg / L (Additives) ・3-mercapto-1-propanesulfonic acid sodium: 2 mg / L ・Hydroxyethyl cellulose: 10 mg / L ・Low molecular weight glue (molecular weight 3000): 50 mg / L <Electrolysis conditions> Solution temperature: 55°C Current density: 45 A / dm 2
[0072] <Ten-point average roughness Rzjis> On the M side of the electrodeposited copper foil, a contact surface roughness measuring instrument (manufactured by Kosaka Laboratory Co., Ltd., "Surfcorder SE1700") was used to measure the ten-point average roughness Rzjis (µm) defined in JIS B 0601:2001 in the direction (TD direction) perpendicular to the longitudinal direction (machine direction, MD direction) of the electrodeposited copper foil, i.e., the ten-point average roughness Rzjis (µm) in the TD.
[0073] (Examples 1 to 10, 48 to 51, and Comparative Examples 4 and 5) In Examples 1 to 10, 48 to 51, and Comparative Examples 4 and 5, the electrolytic copper foil produced in Production Example 1 was used as the copper foil substrate, and the copper foil substrate was subjected to the following steps [1] to [3] to obtain surface-treated copper foils. These are explained in detail below.
[0074] [1] Formation of nickel layer A nickel layer was formed on the M side of the electrodeposited copper foil by electroplating (nickel treatment (A)) using a pulse electrolysis device. A bath capable of circulating the plating solution was used, and plating was performed while controlling the flow rate. The plating bath composition and pulse electrolysis conditions were as follows. <Plating bath composition> Nickel sulfate hexahydrate: 50 g / L in terms of nickel (atom) Boric acid: 20 g / L pH: 4.3 <Pulse electrolysis conditions> Bath temperature: 20°C Current density: 10 A / dm 2Current application time: 10 milliseconds Duty ratio: See Tables 1 and 2 Total charge: 4 A·S / dm 2 Liquid flow rate: shown in Tables 1 and 2.
[0075] [2] Formation of intermediate layer Subsequently, the surface of the nickel layer formed in [1] above was subjected to zinc plating and chromium plating in this order under the following conditions to form an intermediate layer. The compositions of the plating baths and the electrolysis conditions for the zinc plating and chromium plating were as follows:
[0076] Zinc plating treatment <Plating bath composition> Zinc sulfate heptahydrate: 2.5 g / L in terms of zinc (atom) Sodium hydroxide: 25 g / L pH: 10-12 <Electrolysis conditions> Bath temperature: 20°C Current density: 0.7 A / dm 2 Processing time: 4 seconds
[0077] Chrome plating treatment <Plating bath composition> Chromium (VI) oxide: 8 g / L in terms of chromium (atom) pH: 2.4 <Electrolysis conditions> Bath temperature: 30°C Current density: 5 A / dm 2 Processing time: 4 seconds
[0078] [3] Formation of chemical adhesion layer Finally, a 0.8% by mass aqueous solution of 3-aminopropyltrimethoxysilane was applied onto the intermediate layer (particularly the outermost chromium plating layer) formed in [2] above, and dried at 200°C to form a chemical adhesion layer using a silane coupling agent.
[0079] In Examples 11 to 17 and Comparative Example 6, surface-treated copper foils were obtained in the same manner as in Example 1, except that in the above [1], instead of the nickel treatment (A), an electrochemical reduction reaction of nickel hydroxide (nickel treatment (B)) was carried out under the conditions shown below. Specifically, the following procedure was followed.
[0080] (1) First, a nickel layer was formed on the M side of the electrodeposited copper foil by the following electrolytic plating. The plating bath composition and electrolysis conditions were as follows: <Plating bath composition> Nickel sulfate hexahydrate: 40 g / L in terms of nickel (atom) Boric acid: 20 g / L pH: 4.2 <Electrolysis conditions> Bath temperature: 30°C Current density: 0.5 A / dm 2 Power-on time: 5 seconds
[0081] (2) Next, the surface of the nickel layer obtained in (1) above was immersed in a sodium hydroxide aqueous solution (sodium hydroxide concentration: 30 g / L) for 30 seconds to perform hydroxide treatment on the nickel layer. Thereafter, an electrochemical reduction reaction of nickel hydroxide was carried out in the sodium hydroxide aqueous solution under the following conditions to obtain a nickel layer. <Conditions for reduction treatment> Current density: shown in Tables 1 and 2. Current application time: 30 seconds
[0082] (Examples 18 to 35) In Examples 18 to 35, surface-treated copper foils were obtained in the same manner as in Example 3, except that each component was added to the plating bath in the above [1] at the following concentrations so that the composition of the Ni-containing surface treatment layer would be the alloy composition shown in Table 1.・In the case of Ni-P, sodium hypophosphite monohydrate: 15 g / L converted to phosphorus (atom) ・In the case of Ni-Zn, zinc sulfate heptahydrate: 5 g / L converted to zinc (atom) ・In the case of Ni-Mo, sodium molybdate dihydrate: 5 g / L converted to molybdenum (atom) ・In the case of Ni-W, sodium tungstate dihydrate: 5 g / L converted to tungsten (atom) ・In the case of Ni-Cr, chromium (VI) oxide: 4 g / L converted to chromium (atom) ・In the case of Ni-Co, cobalt chloride hexahydrate: 4 g / L converted to cobalt (atom) ・In the case of Ni-Zn-P, zinc sulfate heptahydrate: 5 g / L converted to zinc (atom) Sodium hypophosphite monohydrate: 15 g / L converted to phosphorus (atom)・In the case of Ni-Zn-Mo Zinc sulfate heptahydrate: 5 g / L in terms of zinc (atom) Sodium molybdate dihydrate: 5 g / L in terms of molybdenum (atom) ・In the case of Ni-Zn-Cr Zinc sulfate heptahydrate: 5 g / L in terms of zinc (atom) Chromium (VI) oxide: 4 g / L in terms of chromium (atom)
[0083] (Examples 36 to 40) In Examples 36 to 40, a surface-treated copper foil was obtained in the same manner as in Example 3, except that a roughened layer was formed in advance on a copper foil substrate under the following conditions, and a surface-treated layer containing Ni was formed on the roughened layer.
[0084] [Formation of Roughened Layer] Before the nickel treatment described in [1] above, a roughened layer was formed on the M side of the electrolytic copper foil by roughening plating. At this time, by changing the current application time, roughening particles of different shapes were formed on the surface of the copper foil substrate. The plating bath composition and plating conditions were as follows. <Plating bath composition> Copper sulfate pentahydrate: 10 g / L in terms of copper (atom) Sulfuric acid: 150 g / L Ammonium molybdate: 600 mg / L in terms of molybdenum (atom) <Electroplating treatment conditions> Bath temperature: 12°C Current density: 20 A / dm2 Current application time: 2 to 8 seconds
[0085] (Examples 41 to 47) In Examples 41 to 47, the total charge amount of Ni plating was set to 1 to 20 A·S / dm 2 A surface-treated copper foil was obtained in the same manner as in Example 3, except that the temperature was changed within the range of .
[0086] (Comparative Examples 1 to 3) In Comparative Examples 1 to 3, surface-treated copper foils were obtained in the same manner as in Example 1, except that in the above [1], nickel treatment (A) was replaced by nickel treatment under the following conditions as a general nickel plating method. The plating bath composition and electrolysis conditions were as follows. <Plating bath composition> Nickel sulfate hexahydrate: 45 g / L in terms of nickel (atom) Boric acid: 20 g / L pH: 3.5 <Electrolysis conditions> Bath temperature: 20°C Current density: 0.5 A / dm 2 Power-on time: 9 seconds
[0087] Comparative Example 7 In Comparative Example 7, a surface-treated copper foil was obtained in the same manner as in Example 1, except that Ni plating was not performed.
[0088] Comparative Example 8 In Comparative Example 8, a surface-treated copper foil was obtained in the same manner as in Example 1, except that a surface treatment layer containing Ni was formed under the same Ni—Co treatment conditions as in Example 4 of Patent Document 1.
[0089] Comparative Example 9 In Comparative Example 9, a surface-treated copper foil was obtained in the same manner as in Example 1 of Patent Document 2.
[0090] (Evaluation) The surface-treated copper foils according to the above Examples and Comparative Examples were evaluated for the following properties. The evaluation conditions for each property were as follows, and unless otherwise specified, each measurement was carried out at room temperature (20°C ± 5°C). The results are shown in Tables 1 and 2.
[0091] [Composition of Ni-Containing Surface Treatment Layer] The composition of the nickel layer of the surface-treated copper foil was analyzed by X-ray photoelectron spectroscopy (XPS) using an X-ray photoelectron spectrometer (ULVAC-PHI, Inc., "PHI Quants"). Monochromated Al-Kα rays (hν = 1486.6 eV) were used as incident X-rays, and the escape angle was 45°. The surface of the surface treatment film including the nickel layer of the surface-treated copper foil was measured in an analysis area of 100 μmφ, and depth direction analysis was performed by Ar sputtering. At this time, if one or more elements selected from the group consisting of Zn, P, Mo, W, Cr, and Co were detected in the same depth region as the depth region where nickel was detected, it was determined that nickel was alloyed, and the alloy composition was estimated to be an alloy of nickel and the detected elements.
[0092] [Ni deposition amount] The surface of the surface-treated copper foil having a surface treatment film containing a nickel layer was analyzed by X-ray fluorescence analysis using a scanning X-ray fluorescence analyzer (ZSX Primus IV, manufactured by Rigaku Corporation) to determine the Ni deposition amount (mg / dm 2 The amount of Ni attached was determined using a calibration curve obtained using known standard samples.
[0093] [Magnetic Properties] The magnetic properties of the surface-treated copper foil were measured before and after the following specified heat treatment by the following method: (Heat Treatment) The surface-treated copper foil was cut into a size of 40 mm x 80 mm, and the cut foil was heat-treated in an oven at 300°C in an inert atmosphere for 2 hours to prepare a surface-treated copper foil after heat treatment.
[0094] (Measurement of Magnetic Properties) The magnetic properties of the surface-treated copper foil before and after the heat treatment were measured by the following method. (1) First, the surface-treated copper foil to be measured was cut into ten 10 mm x 10 mm measurement samples. (2) The magnetic properties of the measurement samples obtained in (1) above were measured under the following conditions. A vibrating sample magnetometer (manufactured by Tamagawa Seisakusho Co., Ltd., "TM-VSM211483-HGC type") was used for the measurement. First, the measurement sample was placed in a sample holder. While vibrating the measurement sample, a magnetic field was applied up to +10,000 Oe at a sweep rate of 50 Oe / s, then down to -10,000 Oe at a sweep rate of 50 Oe / s, and then down to +10,000 Oe at a sweep rate of 50 Oe / s. This resulted in a B-H curve with magnetic flux density on the vertical axis and magnetic field on the horizontal axis. (3) Based on the B-H curve obtained in (2) above, the magnetic flux density at a magnetic field of +10,000 Oe and the magnetic flux density at a magnetic field of 0 Oe were read, and these were defined as the saturation magnetic flux density Bs [T] and the residual magnetic flux density Br [T]. Note that this method results in two magnetic flux density values for each magnetic field. Normally, if the magnetic property measurement is performed properly, the B-H curve will be a vertically symmetrical graph, and the absolute values of the two values calculated for each magnetic field will be nearly identical. In this example, it was confirmed that the B-H curve was vertically symmetrical, and the previously calculated values were adopted. (4) The above measurement was performed once for each measurement sample, and the measured values of the 10 measurement samples were averaged to determine the magnetic flux density of the surface-treated copper foil to be measured. The saturation magnetic flux density Bs and residual magnetic flux density Br of the surface-treated copper foil before the above heat treatment were defined as "Bs 0 " and "Br 0 " and the saturation magnetic flux density Bs and residual magnetic flux density Br of the surface-treated copper foil after the heat treatment are "Bs 300 " and "Br 300 ". Also, "A x 10^-B" in the table means "A x 10 -B (5) Furthermore, the saturation magnetic flux density Bs of the surface-treated copper foil before the heat treatment obtained by the above measurement 0 and residual magnetic flux density Br 0and the saturation magnetic flux density Bs of the surface-treated copper foil after the heat treatment. 300 and residual magnetic flux density Br 300 Based on the values of Bs and Br, the increase rate of the saturation magnetic flux density Bs and the increase rate of the residual magnetic flux density Br after the heat treatment were calculated using the following formulas (I) and (II). Increase rate of the saturation magnetic flux density Bs after the heat treatment (%) = [{(Bs 300 -Bs 0 ) / Bs 0}×100] ... (I) Increase rate (%) of residual magnetic flux density Br after heat treatment = [{(Br 300 -Br 0 ) / Br 0}×100] ...(II)
[0095] [Surface roughness (arithmetic mean height Sa)] The arithmetic mean height Sa was measured on the surface of the surface-treated copper foil having a surface treatment film including a nickel layer using a confocal laser microscope (manufactured by Keyence Corporation, "VK-X1050" and "VK-X1000"). The objective lens magnification of the confocal laser microscope was 100x, the scan mode was laser confocal, the measurement size was 2048 x 1536, the measurement quality was High Precision, and the pitch was 0.08 μm. The calculations of Vvc and Sa were performed under the following filter processing and calculation conditions. <Filter processing and calculation conditions> Image processing: averaging, 3 x 3, median S filter: none F-operation: plane tilt correction L filter: 0.025 μm Calculation target area: 100 μm x 100 μm
[0096] [Transmission Characteristics] To evaluate high-frequency characteristics, transmission loss in the high-frequency band was measured. Details are described below. Two low-dielectric polyphenylene ether resin films (MEGTRON7, a multilayer substrate material manufactured by Panasonic Corporation, 60 μm thick) were stacked on top of each other, and surface-treated copper foil was attached to both sides of the stack to produce a copper-clad laminate. The resin film and the surface of the nickel-containing surface treatment film of the surface-treated copper foil were positioned facing each other, and the two films were pressed together at a surface pressure of 3.5 MPa and 210°C for 2 hours to produce a double-sided copper-clad laminate. Circuit processing was performed on the resulting copper-clad laminate, producing a printed wiring board with a stripline having a transmission path width of 140 μm and a circuit length of 1000 mm. A high-frequency signal was transmitted through the transmission path of this printed wiring board using a network analyzer ("N5291A" manufactured by Keysight Technologies, Inc.), and the transmission loss was measured. The characteristic impedance was 50Ω. The above measurement was performed three times for one copper-clad laminate, and the average value was taken as the measured value. The smaller the absolute value of the measured transmission loss, the smaller the transmission loss and the better the high-frequency characteristics. Using the obtained measured value as an index, the high-frequency characteristics were evaluated according to the following evaluation criteria. S: Absolute value of transmission loss at 40 GHz is less than 41.5 dB A: Absolute value of transmission loss at 40 GHz is 41.5 dB or more and less than 43.0 dB B: Absolute value of transmission loss at 40 GHz is 43.0 dB or more and less than 45.0 dB C: Absolute value of transmission loss at 40 GHz is 45.0 dB or more
[0097] [Heat Resistance] Double-sided copper-clad laminates were produced using the same method as described in [Evaluation of High-Frequency Characteristics] above. The obtained double-sided copper-clad laminates were cut into pieces measuring 5 cm x 5 cm to prepare 10 test pieces. The obtained 10 test pieces were heat-treated in an oven at 290°C under an atmospheric condition for 1 hour. Thereafter, the heat-treated test pieces were removed, and each test piece was visually inspected for the presence or absence of peeling between the copper foil and the resin. Based on the evaluation results of the 10 test pieces, the heat-resistant adhesion was evaluated according to the following evaluation criteria. <Evaluation Criteria for Heat-Resistant Adhesion> A: Peeling occurred in 0 or 1 test piece B: Peeling occurred in 2 or 3 test pieces C: Peeling occurred in 4 or more test pieces
[0098]
[0099]
[0100] As shown in Tables 1 and 2, the saturation magnetic flux density (Bs 300 ) is 5.0 x 10 -3 It was confirmed that the surface-treated copper foils having a hardness of 0.1T or less can suppress the nickel layer from being magnetized even after heat treatment, and therefore have excellent transmission characteristics and heat resistance (Examples 1 to 51).
[0101] In contrast, the saturation magnetic flux density (Bs 300 ) is 5.0 x 10 -3 It was confirmed that the surface-treated copper foils having a nickel layer thickness exceeding T (Comparative Examples 1 to 6, 8, and 9) were inferior in transmission characteristics to the surface-treated copper foils of Examples 1 to 51 because the nickel layer was magnetized after heat treatment. Furthermore, it was confirmed that the surface-treated copper foil (Comparative Example 7) which did not have a surface treatment film including a nickel-containing surface treatment layer on at least one side of the copper foil substrate had good transmission characteristics but was inferior in heat resistance to the surface-treated copper foils of Examples 1 to 51.
Claims
1. A surface-treated copper foil having a surface treatment film including a surface treatment layer containing nickel on at least one surface of a copper foil substrate, the saturation magnetic flux density (Bs) after heat treatment at 300°C for 2 hours 300 ) is 5.0 x 10 -3 T or less.
2. Residual magnetic flux density (Br 300 ) is 5.0 x 10 -4 The surface-treated copper foil according to claim 1, wherein the surface tension is T or less.
3. The surface-treated copper foil according to claim 1 or 2, which satisfies the following requirements (I) and (II): Requirement (I): The increase rate of saturation magnetic flux density Bs after heat treatment at 300° C. for 2 hours [{(Bs 300 -Bs 0 ) / Bs 0 }×100] is 300% or less. Requirement (II): The increase rate of residual magnetic flux density Br after heat treatment at 300° C. for 2 hours [{(Br 300 -Br 0 ) / Br 0 }×100] is 300% or less. 300 is the saturation magnetic flux density after heat treatment at 300° C. for 2 hours, Bs 0 is the saturation magnetic flux density before the heat treatment, Br 300 is the residual magnetic flux density after heat treatment at 300° C. for 2 hours, and B 0 is the residual magnetic flux density before the heat treatment.
4. The amount of nickel deposited on the surface having the surface treatment film is 0.02 mg / dm 2 More than 3.0 mg / dm 2 The surface-treated copper foil according to any one of claims 1 to 3, wherein:
5. The surface-treated copper foil according to any one of claims 1 to 4, wherein the surface treatment film comprises, in this order from the copper foil substrate side, a roughening treatment layer and a surface treatment layer containing nickel, and the surface of the surface treatment film has an arithmetic mean height Sa of 0.02 μm or more and 0.35 μm or less as measured optically in accordance with ISO 25178.
6. The surface-treated copper foil according to any one of claims 1 to 5, wherein the nickel-containing surface treatment layer is composed of a nickel alloy containing one or more elements selected from the group consisting of zinc, phosphorus, molybdenum, tungsten, chromium, iron, cobalt, and niobium.
7. A copper-clad laminate comprising the surface-treated copper foil according to any one of claims 1 to 6.
8. A printed wiring board comprising the copper clad laminate according to claim 7.
Citation Information
Patent Citations
Nickel-plated copper material and preparation method and application thereof
CN105063699A
Composite copper member
WO2020226160A1
Cited By
Surface-treated copper foil and copper-clad laminate
WO2026203730A1