Thermoelectric wafer and method for manufacturing same
The thermoelectric wafer design with a thicker end region and specific thickness ratio addresses mechanical strength issues, enhancing durability and productivity by using a semiconductor material coating and firing process, resulting in improved thermoelectric module performance.
Patent Information
- Application Number
- PCT/JP2024/012228
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional thermoelectric wafers lack mechanical strength, leading to cracks and fractures during handling and post-processing, which affects their performance and productivity in thermoelectric conversion modules.
The thermoelectric wafer design features an end region with a greater thickness than the recessed region, with a specific thickness ratio to enhance mechanical strength and prevent cracks, and a manufacturing method involving a coating film of thermoelectric semiconductor material, binder resin, and ionic compound, followed by heating and pressurizing to form a concave region and subsequent firing to create a thermoelectric element layer.
The enhanced mechanical strength of the thermoelectric wafer reduces the occurrence of cracks and fractures, improving its durability and suitability for mass production and post-processing, resulting in higher-quality thermoelectric chips for conversion modules.
Smart Images

Figure JP2024012228_03102024_PF_FP_ABST
Abstract
Description
Thermoelectric wafer and method of manufacturing same
[0001] The present invention relates to a thermoelectric wafer and a method for manufacturing the same.
[0002] As one of the means for effectively utilizing energy, there have been devices that directly convert thermal energy into electrical energy and vice versa using thermoelectric conversion modules with thermoelectric effects such as the Seebeck effect and the Peltier effect. For example, a so-called π-type thermoelectric conversion element configuration is known as a thermoelectric conversion module. A π-type thermoelectric conversion element is configured by providing a pair of spaced-apart electrodes on a substrate, with, for example, a P-type thermoelectric element layer on one electrode and an N-type thermoelectric element layer on the other electrode, also spaced apart from each other, and connecting the top surfaces of both thermoelectric element layers to a common electrode on the opposing substrate. Recently, in order to improve thermoelectric performance and mass productivity, thin-film P-type and N-type thermoelectric element layers have been formed into wafers, and thermoelectric conversion modules have been mass-produced. Patent Document 1, for example, discloses a structure in which a film of fibrous semiconductor material (usable for high-performance devices such as thermoelectric conversion elements, light-emitting elements, and nanowire solar cells) is provided on a substrate (wafer), and further a bank made of an addition-curing silicone resin is provided at the edge of the substrate (wafer).
[0003] JP 2018-85441 A
[0004] However, in Patent Document 1, the banks made of addition-curing silicone resin at the ends of the substrate (wafer) are provided to fill the spaces between the formed films of multiple fibrous semiconductor materials (A) with filler (C), and no consideration is given to the mechanical strength of the substrate (wafer).
[0005] In view of the above, an object of the present invention is to provide a thermoelectric wafer having excellent mechanical strength and a method for manufacturing the same.
[0006] As a result of extensive research aimed at solving the above-mentioned problems, the inventors discovered that by making the thickness of the edge region of a thermoelectric wafer greater than the thickness of the recessed region surrounded by the edge region, it is possible to suppress cracks, breakage, and the like that occur in the thermoelectric wafer due to mechanical strength, and thus completed the present invention. Specifically, the present invention provides the following [1] to [5]. [1] A thermoelectric wafer comprising a thermoelectric element layer containing a thermoelectric semiconductor material, the thermoelectric wafer comprising an edge region and a recessed region surrounded by the edge region, the thickness of the edge region being greater than the thickness of the recessed region. [2] The thermoelectric wafer according to [1] above, in which the ratio of the length of the edge region of the thermoelectric wafer in the direction of the recessed region to the maximum distance from the edge to approximately the center of the thermoelectric wafer is 0.001 or greater. [3] The thermoelectric wafer according to [1] or [2] above, in which the ratio of the thickness of the edge region to the minimum thickness of the recessed region is 1.01 or greater. [4] A method for manufacturing a thermoelectric wafer, comprising the following steps (A) to (C): (A) obtaining a coating film formed from a thermoelectric semiconductor composition containing a thermoelectric semiconductor material, (B) heating and pressurizing an area other than an edge area of the coating film to form a recessed area surrounded by the edge area, thereby obtaining a thermoelectric wafer precursor, and (C) firing the thermoelectric wafer precursor to obtain a thermoelectric wafer comprising a thermoelectric element layer, the thermoelectric wafer comprising the edge area of the thermoelectric wafer and a recessed area surrounded by the edge area, the thickness of the edge area being greater than the thickness of the recessed area. [5] A method for manufacturing a thermoelectric wafer according to above [4], wherein the thermoelectric element layer is made of a thermoelectric semiconductor composition containing the thermoelectric semiconductor material, a binder resin, and an ionic compound.
[0007] According to the present invention, it is possible to provide a thermoelectric wafer having excellent mechanical strength and a method for manufacturing the same.
[0008] 1A and 1B are explanatory views showing an example of a thermoelectric wafer according to the present invention, and FIG. 1C are explanatory views showing an example of steps according to a method for manufacturing a thermoelectric wafer according to the present invention in the order of steps.
[0009] [Thermoelectric Wafer] The thermoelectric wafer of the present invention is a thermoelectric wafer made of a thermoelectric element layer containing a thermoelectric semiconductor material, and is characterized in that the thermoelectric wafer has an edge region and a recessed region surrounded by the edge region, and the thickness of the edge region is greater than the thickness of the recessed region. In the present invention, by making the thickness of the edge region of the thermoelectric wafer greater than the thickness of the recessed region surrounded by the edge region, the mechanical strength of the edge region can be increased, and cracks and breakages that occur in the thermoelectric wafer due to mechanical damage that occurs, for example, during handling in the manufacturing process or during processing in later processes can be suppressed.
[0010] In this specification, a film made of a thermoelectric semiconductor composition before drying may be simply referred to as a "composition film," and a film after drying may be simply referred to as a "coated film." Furthermore, a film obtained by compressing after heating and pressurizing treatment may be simply referred to as a "thermoelectric wafer precursor." Furthermore, a film obtained after firing a thermoelectric wafer precursor may be simply referred to as a "thermoelectric element layer" or a "thermoelectric wafer." Furthermore, chips obtained by singulating a thermoelectric wafer may be simply referred to as a "thermoelectric chip" or "chip."
[0011] In this specification, preferred definitions can be selected arbitrarily, and it can be said that a combination of preferred definitions is more preferable. In this specification, the expression "XX to YY" means "XX or more and YY or less." In this specification, for preferred numerical ranges (for example, ranges of content, etc.), lower and upper limits described in stages can be independently combined. For example, from the description "preferably 10 to 90, more preferably 30 to 60," the "preferable lower limit (10)" and the "more preferable upper limit (60)" can be combined to form "10 to 60."
[0012] 1 is an explanatory diagram showing an example of a thermoelectric wafer of the present invention, where (a) is a plan view of the thermoelectric wafer 1 and (b) is a cross-sectional view of the thermoelectric wafer 1. The thermoelectric wafer 1 is a circular wafer and includes an edge region 2 and a recessed region 3 surrounded by the edge region 2, where D is the diameter, P is the length of the edge region 2, and C is the length of the recessed region 3. 1 is the thickness of the end region 2, Q is the diameter of the recessed region 3, C 2denotes the thickness of the recessed region 3.
[0013] The ratio of the length of the end region of the thermoelectric wafer in the direction of the recessed region to the maximum distance from the edge of the thermoelectric wafer to the approximate center of the thermoelectric wafer is preferably 0.001 or more, more preferably 0.01 to 0.20, and even more preferably 0.03 to 0.10. When the ratio of the length of the end region of the thermoelectric wafer in the direction of the recessed region to the maximum distance from the edge of the thermoelectric wafer to the approximate center is within this range, the reduction in the effective area of the thermoelectric wafer is suppressed, and the number of thermoelectric chips (with identical specifications) obtained by singulating the thermoelectric wafer can be maintained. Here, the "maximum distance from the edge of the thermoelectric wafer to the approximate center" refers to the distance from the circumferential edge of the circle to the center of the circle, for example, when the thermoelectric wafer is circular as shown in FIG. 1 . Furthermore, for example, when the thermoelectric wafer is rectangular, as described below, it refers to the distance from each corner of the rectangle to the intersection of the diagonal lines.
[0014] The ratio of the thickness of the edge region to the minimum thickness of the recessed region of the thermoelectric wafer is preferably 1.01 or more, more preferably 1.01 to 3.00, even more preferably 1.10 to 2.50, and particularly preferably 1.20 to 2.00. When the ratio of the thickness of the edge region to the minimum thickness of the recessed region of the thermoelectric wafer is within this range, it becomes easier to improve the mechanical strength of the edge of the thermoelectric wafer.
[0015] When the ratio of the thickness of the edge region to the minimum thickness of the recessed region of the thermoelectric wafer and the ratio of the length of the edge region of the thermoelectric wafer in the direction of the recessed region to the maximum distance from the edge to approximately the center of the thermoelectric wafer are both within the above ranges, it is possible to maintain the number of thermoelectric chips (with identical specifications) obtained by dicing the thermoelectric wafer, and to suppress the occurrence of cracks and breakage at the edge of the thermoelectric wafer.
[0016] The thickness of the thermoelectric wafer made of the thermoelectric element layer obtained by the firing treatment described below, i.e., the thickness of the recessed region of the thermoelectric wafer, is preferably 10 to 800 μm, more preferably 15 to 600 μm, and even more preferably 20 to 420 μm. If the thickness of the thermoelectric wafer is within this range, the thermoelectric wafer is mechanically stable and the occurrence of defects such as cracks and warpage is easily suppressed.
[0017] The shape of the thermoelectric wafer is not particularly limited, but examples thereof include a circle, an ellipse, a square, a rectangle, etc. The size of the thermoelectric wafer is not particularly limited, but from the viewpoint of mass-producing a plurality of chips at once, a circle has a diameter of 30 mm to 500 mm, and a square or rectangle has a side of 10 mm to 500 mm.
[0018] (Support) In the present invention, a support is preferably used as a support for the coating film. Examples of the support include, but are not limited to, glass, silicon, ceramics, and resin films. Resin films are preferred from the viewpoint of flexibility, and heat-resistant resin films are more preferred from the viewpoint of heat resistance. The heat-resistant resin film is not particularly limited, but is preferably a polyimide film, a polyamide film, a polyetherimide film, a polyaramid film, a polyamideimide film, or a fluorine-based film (polytetrafluoroethylene, tetrafluoroethylene-hexafluoropropylene copolymer, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer), and polyimide film is particularly preferred from the viewpoint of high versatility. The thickness of the heat-resistant resin film is preferably 50 to 1000 μm, more preferably 75 to 500 μm, and even more preferably 100 to 200 μm, from the viewpoints of flexibility, heat resistance, and dimensional stability. The glass transition temperature (Tg) of the heat-resistant resin film is preferably 200° C. or higher, more preferably 220° C. or higher, and even more preferably 250° C. or higher. Here, Tg refers to the temperature at the maximum point of tan δ (loss modulus / storage modulus) obtained by a differential scanning calorimeter (measured in the range of 0 to 500° C. at a heating rate of 5° C. / min).
[0019] <Thermoelectric element layer> The thermoelectric wafer used in the present invention is composed of a thermoelectric element layer. The thermoelectric element layer is preferably formed from a thermoelectric semiconductor composition containing a thermoelectric semiconductor material (hereinafter sometimes referred to as "thermoelectric semiconductor particles"), a binder resin, and an ionic compound (ionic liquid, inorganic ionic compound).
[0020] (Filling Rate) The thermoelectric element layer constituting the thermoelectric wafer of the present invention may contain voids containing air entrapped during coating film formation and gas components derived from the binder resin during heating. When the filling rate is defined as the ratio of the area of the thermoelectric conversion material to the area of a longitudinal cross section including the center of the thermoelectric element layer (the remaining area is considered to be voids), the filling rate is preferably 0.900 to 0.999, more preferably 0.920 to 0.990, and even more preferably 0.940 to 0.980. A filling rate within this range can reduce the electrical resistivity of the thermoelectric conversion material in the thermoelectric element layer, thereby improving the thermoelectric performance of the thermoelectric element layer. Note that in the definition of filling rate, the thermoelectric conversion material refers to the thermoelectric element layer excluding voids. The filling rate can be measured using the filling rate evaluation described in the Examples.
[0021] (Thermoelectric Semiconductor Material) The thermoelectric semiconductor material is preferably pulverized to a predetermined size using, for example, a pulverizer or the like and used as thermoelectric semiconductor particles. The particle size of the thermoelectric semiconductor particles is preferably 10 nm to 100 μm, more preferably 50 nm to 50 μm, and even more preferably 3 μm to 30 μm. The average particle size of the thermoelectric semiconductor particles is obtained by measurement using a laser diffraction particle size analyzer (Malvern, Mastersizer 3000), and is taken as the median of the particle size distribution.
[0022] The thermoelectric semiconductor material used in the present invention is not particularly limited as long as it is a material that can generate thermoelectric power by applying a temperature difference, and examples thereof include bismuth-tellurium-based thermoelectric semiconductor materials such as P-type bismuth telluride and N-type bismuth telluride; telluride-based thermoelectric semiconductor materials such as GeTe and PbTe; antimony-tellurium-based thermoelectric semiconductor materials; ZnSb, Zn 3 Sb 2、 Zn 4 Sb3 Zinc-antimony based thermoelectric semiconductor materials such as silicon-germanium based thermoelectric semiconductor materials such as silicon germanium; Bi 2 Se 3 Bismuth selenide-based thermoelectric semiconductor materials such as β-FeSi 2 , CrSi 2 , MnSi 1.73 , Mg 2 Silicide-based thermoelectric semiconductor materials such as Si; oxide-based thermoelectric semiconductor materials; Heusler materials such as FeVAl, FeVAlSi, and FeVTiAl; TiS 2 Sulfide-based thermoelectric semiconductor materials such as the above are used.
[0023] Among these, the thermoelectric semiconductor material used in the present invention is preferably a bismuth-tellurium-based thermoelectric semiconductor material such as P-type bismuth telluride or N-type bismuth telluride. The P-type bismuth telluride has positive holes as carriers and a positive Seebeck coefficient, for example, Bi X Te 3 Sb 2-X In this case, X is preferably 0<X≦0.8, and more preferably 0.4≦X≦0.6. When X is greater than 0 and not greater than 0.8, the Seebeck coefficient and electrical conductivity are increased, and the properties as a P-type thermoelectric conversion material are maintained, which is preferable. In addition, the N-type bismuth telluride has electrons as carriers and a negative Seebeck coefficient, for example, Bi 2 Te 3-Y Se Y In this case, Y is preferably 0≦Y≦3 (when Y=0: Bi 2 Te 3 ) and more preferably 0.1<Y≦2.7. When Y is 0 to 3, the Seebeck coefficient and electrical conductivity become large, and the properties as an N-type thermoelectric conversion material are maintained, which is preferable.
[0024] The content of the thermoelectric semiconductor particles in the thermoelectric semiconductor composition is preferably 30 to 99% by mass, more preferably 50 to 96% by mass, and even more preferably 70 to 95% by mass. When the content of the thermoelectric semiconductor particles is within the above range, the Seebeck coefficient (absolute value of the Peltier coefficient) is large, and a decrease in electrical conductivity is suppressed, with only the thermal conductivity decreasing, so that a film exhibiting high thermoelectric performance and having sufficient film strength and flexibility is obtained, which is preferable.
[0025] The thermoelectric semiconductor particles are preferably subjected to an annealing treatment (hereinafter, sometimes referred to as "annealing treatment A"). By performing annealing treatment A, the crystallinity of the thermoelectric semiconductor particles is improved, and further, the surface oxide film of the thermoelectric semiconductor particles is removed, thereby increasing the Seebeck coefficient (absolute value of the Peltier coefficient) of the thermoelectric conversion material and further improving the thermoelectric figure of merit.
[0026] (Binder Resin) The binder resin used in the present invention has the effect of physically binding thermoelectric semiconductor materials (thermoelectric semiconductor particles) together, and can increase the flexibility of the thermoelectric conversion module and facilitate the formation of a thin film by coating or the like.
[0027] The binder resin is appropriately selected depending on the heat treatment temperature and the firing (annealing) temperature of the thermoelectric semiconductor material. It is preferable to heat-treat the binder resin at a temperature higher than its decomposition temperature. Furthermore, a resin that maintains its physical properties, such as mechanical strength and thermal conductivity, without being impaired when a coating film made of a thermoelectric semiconductor composition is subjected to heat treatment or the like to cause crystal growth of thermoelectric semiconductor particles is more preferable. In this specification, the "decomposition temperature" refers to the temperature at which the mass loss rate measured by thermogravimetry (TG) is 100% (the mass after decomposition is less than 1% of the mass before decomposition). The decomposition temperature of the binder resin is preferably 150 to 400°C.
[0028] Thermoplastic resins and curable resins can be used as such binder resins. Examples of thermoplastic resins include polyolefin resins such as polyethylene, polypropylene, polyisobutylene, and polymethylpentene; polycarbonate; thermoplastic polyester resins such as polyethylene terephthalate and polyethylene naphthalate; polyvinyl polymers such as polystyrene, acrylonitrile-styrene copolymer, polyvinyl acetate, ethylene-vinyl acetate copolymer, vinyl chloride, polyvinylpyridine, polyvinyl alcohol, and polyvinylpyrrolidone; polyurethane; and cellulose derivatives such as ethyl cellulose. Examples of curable resins include thermosetting resins and photocurable resins. Examples of thermosetting resins include epoxy resins and phenolic resins. Examples of photocurable resins include photocurable acrylic resins, photocurable urethane resins, and photocurable epoxy resins. These resins may be used alone or in combination of two or more. Among these, thermoplastic resins are preferred, with polycarbonate and cellulose derivatives such as ethyl cellulose being more preferred, and polycarbonate being particularly preferred.
[0029] The content of the binder resin in the thermoelectric semiconductor composition is preferably 0.1 to 20% by mass, more preferably 0.5 to 15% by mass, and even more preferably 1.0 to 10% by mass.
[0030] <Ionic Compounds> (Ionic Liquids) The ionic liquids that can be contained in the thermoelectric semiconductor composition are molten salts formed by combining cations and anions, and refer to salts that can exist in liquid form at temperatures ranging from −50°C to less than 400°C. Ionic liquids have characteristics such as extremely low vapor pressure and nonvolatility, excellent thermal stability and electrochemical stability, low viscosity, and high ionic conductivity. Therefore, as a conductive additive, they can effectively suppress a decrease in electrical conductivity between thermoelectric semiconductor materials. In addition, ionic liquids exhibit high polarity due to their aprotic ionic structure and excellent compatibility with binder resins, thereby enabling the electrical conductivity of the thermoelectric element layer to be uniform.
[0031] The ionic liquid may be a known or commercially available one. For example, a nitrogen-containing cyclic cationic compound such as pyridinium, pyrimidinium, pyrazolium, pyrrolidinium, piperidinium, or imidazolium, or a derivative thereof; a tetraalkylammonium-based amine-based cation and a derivative thereof; a phosphine-based cation such as phosphonium, trialkylsulfonium, or tetraalkylphosphonium, or a derivative thereof; a lithium cation and a derivative thereof; or a mixture of a cation component and Cl - ,Br - , I - , AlCl 4 - , Al 2 Cl 7 - , B.F. 4 - , P.F. 6 - , ClO 4 - , NO 3 - , C.H. 3 COO - , C.F. 3 COO - , C.H. 3 SO 3 - , C.F. 3 SO 3 - , (FSO 2 ) 2 N - , (CF 3 SO 2 ) 2 N - , (CF 3 SO 2 ) 3 C - , AsF 6 - , SbF 6 - , NbF 6 - , TaF 6 - , F(HF) n - , (CN) 2 N - , C 4 F 9 SO 3- , (C 2 F 5 SO 2 ) 2 N - , C 3 F 7 COO - , (CF 3 SO 2 ) (CF 3 CO)N - and an anion component such as the above.
[0032] The ionic liquid preferably has a decomposition temperature of 300° C. or higher. If the decomposition temperature is within the above range, the effect as a conductive additive can be maintained even when a coating film made of the thermoelectric semiconductor composition is annealed, as will be described later.
[0033] The content of the ionic liquid in the thermoelectric semiconductor composition is preferably 0.01 to 50 mass %, more preferably 0.4 to 30 mass %, and even more preferably 0.8 to 20 mass %. When the content of the ionic liquid is within the above range, a decrease in electrical conductivity is effectively suppressed, and a film with high thermoelectric performance is obtained.
[0034] (Inorganic ionic compound) The inorganic ionic compound that can be contained in the thermoelectric semiconductor composition is a compound composed of at least a cation and an anion. Inorganic ionic compounds exist in a solid state over a wide temperature range from 400 to 900°C and have characteristics such as high ionic conductivity, so that they can act as a conductive additive to suppress a decrease in electrical conductivity between thermoelectric semiconductor materials.
[0035] The content of the inorganic ionic compound in the thermoelectric semiconductor composition is preferably 0.01 to 50% by mass, more preferably 0.5 to 30% by mass, and even more preferably 1.0 to 10% by mass. When the content of the inorganic ionic compound is within the above range, a decrease in electrical conductivity can be effectively suppressed, resulting in a film with improved thermoelectric performance. When an inorganic ionic compound and an ionic liquid are used in combination as the ionic compound, the total content of the inorganic ionic compound and the ionic liquid in the thermoelectric semiconductor composition is preferably 0.01 to 50% by mass, more preferably 0.5 to 30% by mass, and even more preferably 1.0 to 10% by mass.
[0036] The thickness of the coating film made of the thermoelectric semiconductor composition is preferably 10 to 1000 μm, more preferably 20 to 800 μm, and even more preferably 30 to 650 μm.
[0037] <Solder Receiving Layer> The solder receiving layer has a function of joining the thermoelectric element layer and the solder material layer on the opposing electrode side that constitutes the thermoelectric conversion module, and is directly joined to the thermoelectric element layer.
[0038] The solder-receiving layer preferably contains a metal material. The metal material is preferably at least one selected from gold, silver, nickel, aluminum, rhodium, platinum, chromium, palladium, tin, and an alloy containing any of these metal materials. Among these, a gold, silver, nickel, aluminum, or two-layer structure of tin and gold is preferred, and silver, nickel, and aluminum are more preferred from the viewpoints of material cost, high thermal conductivity, and bonding stability.
[0039] The thickness of the solder-receiving layer is preferably 10 nm to 50 μm, more preferably 50 nm to 16 μm, even more preferably 200 nm to 4 μm, and particularly preferably 500 nm to 3 μm. When the thickness of the solder-receiving layer is within this range, adhesion to the surface of the thermoelectric element layer and to the surface of the solder material layer on the electrode side that constitutes the thermoelectric conversion module is excellent, resulting in a highly reliable bond. Furthermore, high electrical conductivity as well as thermal conductivity can be maintained, resulting in the thermoelectric performance of the thermoelectric conversion module being maintained without any deterioration. The solder-receiving layer may be formed as a single layer using a metal material, or may be formed as a multilayer by laminating two or more metal materials.
[0040] [Method for manufacturing a thermoelectric wafer] The method for manufacturing a thermoelectric wafer of the present invention is a method for manufacturing a thermoelectric wafer, comprising the following steps (A) to (C): (A) obtaining a coating film formed from a thermoelectric semiconductor composition containing a thermoelectric semiconductor material; (B) heating and pressurizing an area other than the edge area of the coating film to form a recessed area surrounded by the edge area, thereby obtaining a thermoelectric wafer precursor; and (C) firing the thermoelectric wafer precursor to obtain a thermoelectric wafer made of a thermoelectric element layer. The thermoelectric wafer is characterized in that it comprises the edge area of the thermoelectric wafer and a recessed area surrounded by the edge area, and the thickness of the edge area is greater than the thickness of the recessed area.
[0041] In the following description, steps (A), (B), and (C) may also be referred to as the "coating step," the "heating and pressurizing step," and the "firing step," respectively, in that order. The method for manufacturing a thermoelectric wafer of the present invention will now be described with reference to the drawings.
[0042] 2A and 2B are explanatory views showing, in order of steps, an example of a method for producing a thermoelectric wafer according to the present invention, in which (a) is a cross-sectional structural view including a coating film 12 formed from a thermoelectric semiconductor composition on a support 11, (b) is a cross-sectional structural view showing an embodiment in which the coating film 12 and a heating and pressing jig 13 are opposed to each other, (c) is a cross-sectional structural view showing an embodiment in which the coating film 12 is heated and pressed from both sides of the support 11 and the coating film 12 using a heating and pressing device (not shown), (d) is a cross-sectional structural view showing an embodiment including a thermoelectric wafer precursor 14 obtained by the heating and pressing treatment, (e) is a cross-sectional structural view showing an embodiment after the heating and pressing jig 13 has been released from the thermoelectric wafer precursor 14, and (f) is a cross-sectional structural view of a thermoelectric wafer 15 obtained after the support 11 has been peeled off and the thermoelectric wafer precursor 14 has been subjected to a firing treatment.
[0043] Step (A): Coating Step The method for manufacturing a thermoelectric wafer of the present invention includes a coating step. The coating step is a step of forming a composition film from a thermoelectric semiconductor composition containing a thermoelectric semiconductor material on a support and drying the composition film to obtain a coated film. For example, in the above-mentioned FIG. 2( a), this is a step of obtaining a coated film 12 formed from the thermoelectric semiconductor composition on the support 11.
[0044] The details of the thermoelectric semiconductor composition containing the thermoelectric semiconductor material used to form the coating film are as described above.
[0045] Methods for applying the thermoelectric semiconductor composition as a composition film include, but are not limited to, well-known methods such as screen printing, flexographic printing, gravure printing, spin coating, dip coating, die coating, spray coating, bar coating, applicator coating, and doctor blade coating. The resulting composition film is then dried to form a coating film. Conventional drying methods, such as hot air drying, hot roll drying, and infrared irradiation, can be used as the drying method. The heating temperature is typically 80 to 150°C, and the heating time, although varying depending on the heating method, is typically several seconds to several tens of minutes. Furthermore, when a solvent is used in preparing the thermoelectric semiconductor composition, the heating temperature is not particularly limited as long as it is within a temperature range that can dry the solvent used.
[0046] The thermoelectric wafer may be further annealed (hereinafter sometimes referred to as "annealing treatment B") as needed, even after the firing treatment described below. By performing annealing treatment B, the thermoelectric performance can be further stabilized and the thermoelectric semiconductor particles in the thermoelectric wafer can undergo further crystal growth, thereby further improving the thermoelectric performance. Although there are no particular limitations on annealing treatment B, it is usually performed in an inert gas atmosphere such as nitrogen or argon, in a reducing gas atmosphere, or under vacuum conditions with a controlled gas flow rate, and is performed at 100 to 500°C for several minutes to several tens of hours, depending on the heat resistance temperature of the thermoelectric semiconductor composition used.
[0047] Step (B): Heating and Pressuring Step The thermoelectric wafer manufacturing method of the present invention includes a heating and pressing step. The heating and pressing step is a step of subjecting the coating film to a heating and pressing treatment. For example, in (b) and (c) of FIG. 2 described above, a heating and pressing device (not shown) is used to perform a heating and pressing treatment on the coating film 12 from both sides of the support 11 and the coating film 12 with a heating and pressing jig 13 interposed therebetween, forming a recessed region surrounded by an edge region of the coating film 12, and in (c), further pressure compression is performed to obtain a thermoelectric wafer precursor 14 in which the thickness of the coating film is reduced.
[0048] The heating and pressurizing treatment in the heating and pressurizing step can be carried out by a known method, for example, using a hydraulic press, a vacuum press, etc. The heating temperature is 100 to 400°C, and the pressure is 40 to 300 MPa. The heating and pressurizing treatment time is not particularly limited, but is preferably several seconds to several hours, and more preferably several minutes to several tens of minutes.
[0049] Step (C): Firing Step The method for producing a thermoelectric wafer of the present invention includes a firing step. The firing step is a step of firing the thermoelectric wafer precursor formed from the coating film compressed in step (B) to obtain a thermoelectric wafer comprising a thermoelectric element layer. For example, in (d) of FIG. 2 described above, the thermoelectric wafer precursor 14 obtained by the heating and pressurizing treatment and compression is peeled from the support 11, and in (e) the thermoelectric wafer precursor 14 is fired to obtain a thermoelectric wafer 15 comprising a thermoelectric element layer. The firing step stabilizes the thermoelectric performance and allows the thermoelectric semiconductor particles in the thermoelectric semiconductor composition in the coating film to undergo crystal growth, further improving the thermoelectric performance of the thermoelectric wafer comprising a thermoelectric element layer.
[0050] The firing treatment is not particularly limited, but is usually carried out under an inert gas atmosphere such as nitrogen or argon, under a reducing gas atmosphere, or under vacuum conditions, with the gas flow rate controlled. The firing temperature depends on the thermoelectric semiconductor particles, resin, ionic compound (ionic liquid, inorganic ionic compound), etc. used in the thermoelectric semiconductor composition, and is adjusted appropriately, but is usually carried out at 260 to 600°C, preferably 280 to 550°C. The firing time is not particularly limited, but is usually several minutes to several tens of hours, preferably several minutes to several hours.
[0051] The method for manufacturing a thermoelectric wafer of the present invention preferably further includes a solder-receiving layer forming step as a post-step. The solder-receiving layer forming step is a step of obtaining a solder-receiving layer by performing a plating process or the like on the thermoelectric wafer, i.e., the thermoelectric element layer. The solder-receiving layer has the function of joining the thermoelectric element layer and the solder material layer on the opposing electrode side that constitutes the thermoelectric conversion module, and is directly joined to the thermoelectric element layer.
[0052] The metal material used to form the solder-receiving layer, the thickness of the solder-receiving layer, etc. are as described above.
[0053] The solder-receiving layer is preferably formed using the above-mentioned metal material. Since the solder-receiving layer is required to have high electrical conductivity and high thermal conductivity in order to maintain thermoelectric performance, it is preferable to use a solder-receiving layer formed by electroplating, electroless plating, or vacuum deposition.
[0054] A thermoelectric wafer produced by the thermoelectric wafer manufacturing method of the present invention, or a thermoelectric wafer having a solder-receiving layer formed thereon, may be further singulated in a dicing step. The dicing step is a step of singulating the thermoelectric wafer into thermoelectric chips. From the viewpoints of processing accuracy and process stability, singulation is preferably performed using a dicing blade with dicing tape attached. The thermoelectric wafer of the present invention and the thermoelectric wafer manufactured by the manufacturing method thereof suffers from little chip flying during dicing, improving the manufacturing yield of the resulting thermoelectric chips.
[0055] (Manufacturing of Thermoelectric Conversion Module) A thermoelectric conversion module can be manufactured by combining a plurality of thermoelectric chips (P-type thermoelectric chips, N-type thermoelectric chips) described above obtained by dicing a thermoelectric wafer manufactured by the thermoelectric wafer manufacturing method of the present invention or a thermoelectric wafer having a solder-receiving layer formed on the thermoelectric wafer. From the viewpoint of thermoelectric performance, the thermoelectric conversion module can be manufactured by mounting (arranging) the P-type thermoelectric chips and the N-type thermoelectric chips so that they are connected via electrodes to form a so-called π-type or in-plane type thermoelectric conversion module.
[0056] Next, the present invention will be described in more detail with reference to examples, but the present invention is not limited to these examples in any way.
[0057] The occurrence of edge cracks in the thermoelectric wafers produced in the examples and comparative examples and the suitability of the thermoelectric wafers including the solder-receiving layer for post-processing were evaluated by the following methods.
[0058] (a) Edge Crack Evaluation For the thermoelectric wafers obtained in the Examples and Comparative Examples, edge cracks were measured using an ultrasonic flaw detection device (manufactured by Nippon Burns Co., Ltd., model name "C-SAM D9600"), and the obtained analytical image was binarized using image processing software (manufactured by National Institutes of Health, ImageJ ver. 1.44P) by setting the contrast from "Brightness / Contrast" to the maximum value, and dark areas in the binarization process were considered to be crack areas and bright areas were considered to be the thermoelectric semiconductor material in the thermoelectric element layer, and edge cracks were evaluated according to the following criteria. A: No cracks (edge cracks) were found in the edge region of the thermoelectric wafer. B: One or more cracks (edge cracks) were found in the edge region of the thermoelectric wafer.
[0059] (b) Evaluation of Post-Process Suitability Thermoelectric wafers having two solder-receiving layers were fabricated by electroless plating the thermoelectric wafers obtained in the Examples and Comparative Examples, sequentially providing a nickel layer (thickness: 5 μm) as the first layer and a gold layer (thickness: 40 nm) as the second layer. The thermoelectric wafers with the solder-receiving layers were attached to dicing tape, and cracks in the thermoelectric wafers were observed using a digital microscope (manufactured by Keyence Corporation, model name: VHX-5000, magnification: 20x), and the results were evaluated according to the following criteria: P: No cracks (edge cracks) were found in the edge region of the thermoelectric wafer, and the thermoelectric wafer was suitable for post-processing. Q: One or more cracks (edge cracks) were found in the edge region of the thermoelectric wafer, and the thermoelectric wafer was not suitable for post-processing.
[0060] (c) Filling rate evaluation The thermoelectric wafers obtained in the examples and comparative examples were divided into rectangular parallelepipeds (10 mm x 10 mm) to form thermoelectric element layers. Each was cut into a longitudinal section including the center of the thermoelectric element layer using a polishing machine (manufactured by Refine Tech Co., Ltd., model name: Refine Polisher HV). The longitudinal section was observed using a scanning electron microscope (SEM) (manufactured by Keyence Corporation). Then, image processing software (manufactured by National Institutes of Health, ImageJ ver. 1.44P) was used to calculate the ratio (filling rate) of the area of the thermoelectric conversion material to the area of the longitudinal section of the thermoelectric element layer. In measuring the filling rate, a 500x magnification SEM image (longitudinal section) was used to measure a range surrounded by 1280 pixels in the width direction and 220 pixels in the thickness direction at any position on the thermoelectric element layer, and the image was cut out. The cut-out image was binarized by setting the contrast to the maximum value in "Brightness / Contrast," and the dark areas in the binarization process were considered to be voids and the bright areas were considered to be thermoelectric conversion material, and the filling rate of the thermoelectric conversion material was calculated using "Threshold." The filling rate was calculated for three SEM images and used as the average value.
[0061] (Example 1) <Preparation of Thermoelectric Wafer> (1) Preparation of Thermoelectric Semiconductor Composition Coating Solution P-type bismuth telluride Bi 0.4 Te 3.0 Sb 1.6A coating liquid was prepared from a thermoelectric semiconductor composition comprising 78.5 parts by mass of particles (average particle size 16.0 μm), 15.5 parts by mass of polyethylene carbonate (decomposition temperature: 250°C) as a binder resin, 0.8 parts by mass of N-butylpyridinium bromide as an ionic liquid (an ionic compound), and 5.18 parts by mass of N-methylpyrrolidone as a solvent. The average particle size of the particles was determined by particle size distribution measurement using a laser diffraction particle size analyzer (Malvern, Mastersizer 3000). (2) Preparation of Thermoelectric Wafer The coating liquid prepared in (1) was applied to a polyimide film (Ube Industries, trade name "Kapton 500H", 100 mm x 160 mm x 125 μm thick) using a screen printer and dried at 110°C for 20 minutes to form a coating film with a thickness of 600 μm. Next, using a hand press (manufactured by Dumbbell, model number: SDL-100), the coating film together with the polyimide film was punched into a circle with a diameter of 60 mm (radius of 30 mm). Next, a SUS plate (SUS304, thickness: 20 mm) with a diameter of 60 mm and a 100 μm deep groove in a 1 mm area around the periphery was placed opposite to the surface of the coating film that was in contact with the polyimide film, and then heated and pressurized at 250°C and 50 MPa for 15 minutes using an electric heater press (heating and pressing device) (manufactured by Sansho Industry, model number: 500kN). The thickness of the 1 mm area around the periphery of the coating film was reduced to 380 μm, and the thickness of the recessed area surrounded by the 1 mm area around the periphery was reduced to 285 μm, thereby obtaining a thermoelectric wafer precursor. Furthermore, the thermoelectric wafer precursor peeled from the polyimide film was heated at a heating rate of 5 K / min in an atmosphere of a mixed gas of hydrogen and argon (hydrogen:argon=3% by volume:97% by volume), and was maintained at a baking (annealing) temperature of 430°C for 30 minutes, thereby producing a thermoelectric wafer.
[0062] Comparative Example 1 A thermoelectric wafer was produced in the same manner as in Example 1, except that a SUS plate having a diameter of 60 mm and a 100 μm deep groove in a 1 mm region on the periphery was replaced with a SUS plate of the same specifications but without a groove, and the thermoelectric wafer precursor was subjected to a heating and pressurizing treatment to compress the thickness of the 1 mm edge region, which is the periphery, of the thermoelectric wafer precursor to 283 μm and the thickness of the region surrounded by the edge region to 289 μm.
[0063] The results of the edge crack evaluation, post-processing suitability evaluation, and filling rate evaluation of the thermoelectric wafers obtained in Example 1 and Comparative Example 1 are shown in Table 1.
[0064]
[0065] The thermoelectric wafer of Example 1, which satisfies the specification of the present invention that the thickness of the edge region is greater than the thickness of the recessed region, does not suffer from edge cracks and is well suited to subsequent processes such as the process of forming a solder-receiving layer and the process of attaching to a dicing tape, compared to the thermoelectric wafer of Comparative Example 1, which does not satisfy the specification of the present invention.
[0066] The thermoelectric wafer of the present invention has excellent mechanical strength and is suitable for post-processing, allowing it to be mass-produced and diced into individual pieces for use as thermoelectric chips in thermoelectric conversion modules. For example, it can be used in power generation applications, such as converting exhaust heat from various combustion furnaces, including factories, waste incineration furnaces, and cement combustion furnaces, as well as exhaust heat from automobile combustion gases and electronic devices, into electricity. Cooling applications include temperature control for various sensors, such as CPUs (Central Processing Units) used in smartphones and various computers, image sensors (e.g., CMOSs) and CCDs (Charge Coupled Devices), and microelectromechanical systems (MEMSs) and light-receiving elements.
[0067] 1: Thermoelectric wafer (thermoelectric element layer) 2: Edge region 3: Recessed region 4: Thermoelectric wafer (thermoelectric element layer) 11: Support 12: Coating film 13: Heating and pressing jig 14: Thermoelectric wafer precursor 15: Thermoelectric wafer D: Diameter of thermoelectric wafer Q: Diameter of recessed region P: Length of edge region C 1 : Thickness of the end region C 2 : thickness of the recessed area
Claims
1. A thermoelectric wafer comprising a thermoelectric element layer including a thermoelectric semiconductor material, the thermoelectric wafer having an edge region and a recessed region surrounded by the edge region, the thickness of the edge region being greater than the thickness of the recessed region.
2. The thermoelectric wafer according to claim 1, wherein the ratio of the length of the end region of the thermoelectric wafer in the direction of the recessed region to the maximum distance from the end of the thermoelectric wafer to approximately the center of the thermoelectric wafer is 0.001 or more.
3. The thermoelectric wafer of claim 1, wherein the ratio of the thickness of said edge region to the minimum thickness of said recessed region is 1.01 or greater.
4. A method for producing a thermoelectric wafer, comprising the following steps (A) to (C): (A) obtaining a coating film formed from a thermoelectric semiconductor composition containing a thermoelectric semiconductor material; (B) heating and pressurizing an area other than the edge area of the coating film to form a recessed area surrounded by the edge area, thereby obtaining a thermoelectric wafer precursor; and (C) firing the thermoelectric wafer precursor to obtain a thermoelectric wafer consisting of a thermoelectric element layer. The method for producing a thermoelectric wafer, wherein the thermoelectric wafer comprises an edge area of the thermoelectric wafer and a recessed area surrounded by the edge area, and the thickness of the edge area is greater than the thickness of the recessed area.
5. The method for producing a thermoelectric wafer according to claim 4, wherein the thermoelectric element layer is made of a thermoelectric semiconductor composition containing the thermoelectric semiconductor material, a binder resin and an ionic compound.
Citation Information
Patent Citations
Thermoelectric device and its manufacture
JP1994085332A
Thermoelectric conversion material, circuit manufacturing method and thermoelectric conversion module
JP2015122464A
Thermoelectric Devices and Methods for Forming Thermoelectric Devices
US20190131508A1