Rubber composition for tire and rubber material for tire

The use of fumed silica with controlled silane coupling agents and diols in the tire rubber composition addresses the balance between fuel efficiency, wear resistance, and heat aging resistance, resulting in a superior tire material with enhanced performance.

WO2024204394A1PCT designated stage expired Publication Date: 2024-10-03TOKUYAMA CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012328
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-27
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing rubber materials for tires face challenges in achieving a balance between low fuel consumption, wear resistance, and heat aging resistance, with previous compositions either compromising on abrasion resistance or fuel efficiency when using wet silica or carbon black as fillers.

Method used

A rubber composition for tires is developed using fumed silica as a filler, with specific surface area-controlled silane coupling agents and diols, which enhances the fuel efficiency, abrasion resistance, and heat aging resistance by optimizing the content of these additives based on the BET specific surface area of the fumed silica.

Benefits of technology

The composition results in a tire rubber material with improved fuel efficiency, wear resistance, and heat aging resistance, suitable for various tire applications, including passenger cars and trucks, by ensuring uniform dispersion of fumed silica and reducing the amount of filler needed.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

[Problem] To provide a rubber material for a tire having excellent fuel economy, wear resistance, and heat aging resistance, and a rubber composition for a tire suitable for manufacturing such a tire. [Solution] A rubber composition for a tire that contains a diene rubber, fumed silica having a surface silanol group density of 3 / nm2 or less, a silane coupling agent, and a diol, in which the silane coupling agent content is from 0.50 μmol / m2 to 3.9 μmol / m2 relative to the BET specific surface area per gram of fumed silica, and the diol content is from 3 μmol / m2 to 14 μmol / m2 relative to the BET specific surface area per gram of fumed silica.
Need to check novelty before this filing date? Find Prior Art

Description

Rubber composition for tires and rubber material for tires

[0001] The present invention relates to a rubber composition for tires and a rubber material for tires. Specifically, the present invention relates to a rubber material for tires that is particularly excellent in fuel economy, abrasion resistance, and heat aging resistance, and a composition suitable for producing the rubber material for tires.

[0002] Automobile tires are required to have not only low fuel consumption but also a long life. To achieve a long life, it is necessary to improve the abrasion resistance and heat aging resistance of tires. To improve abrasion resistance, carbon black has been compounded as a reinforcing filler into rubber compositions for tires.

[0003] On the other hand, it is known that wet silica is effective in improving fuel economy, but the abrasion resistance when wet silica is blended is inferior to the abrasion resistance when carbon black is blended. Therefore, when wet silica is used as a reinforcing filler, part of the carbon black blended amount is replaced by wet silica, and the amount of carbon black blended is relatively reduced, so it is known that a decrease in the abrasion resistance of the tire rubber material is unavoidable.

[0004] Patent Document 1 proposes a rubber material for tires that contains a rubber component, carbon black and wet silica as fillers, and an inorganic compound powder, with the aim of obtaining a rubber material for tires that is excellent in fuel economy and wet grip performance without reducing abrasion resistance.

[0005] Furthermore, Patent Document 2 proposes replacing a portion of wet silica with dry silica, and describes that dry silica can improve fuel economy and suppress a decrease in rubber hardness more than wet silica.

[0006] Furthermore, Patent Document 3 discloses a rubber composition for tires containing predetermined amounts of organic cobalt or a cobalt complex, a phenol derivative, a cyclic polysulfide, and polymethylolmelamine in order to improve heat aging resistance.

[0007] JP 2005-213353 A JP 2016-104840 A JP 2021-172733 A

[0008] However, the rubber materials for tires described in Patent Documents 1 to 3 have the problem that they are not materials that can simultaneously achieve low fuel consumption, abrasion resistance, and heat aging resistance.

[0009] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a rubber material for tires that is excellent in fuel economy, abrasion resistance, and heat aging resistance, and a rubber composition for tires that is suitable for producing the same.

[0010] The present inventors have discovered that by blending fumed silica as a filler in a rubber composition for tires and further controlling the contents of predetermined additives depending on the specific surface area of ​​the fumed silica, a rubber material for tires excellent in fuel economy, abrasion resistance, and heat aging resistance can be obtained, and have completed the present invention.

[0011] From the above, the aspects of the present invention are as follows.

[0012] [1] Diene rubber and a surface silanol group density of 3 / nm 2 a silane coupling agent and a diol, wherein the content of the silane coupling agent is 0.50 μmol / m relative to the BET specific surface area per 1 g of the fumed silica. 2 3.9 μmol / m or more 2 The diol content is 3 μmol / m or less relative to the BET specific surface area per 1 g of fumed silica. 2 14 μmol / m or more 2 The rubber composition for tires is as follows:

[0013] [2] The rubber composition for a tire according to [1], wherein the silane coupling agent is a sulfide-based silane coupling agent.

[0014] [3] The rubber composition for a tire according to [1] or [2], which contains 10 parts by mass or more and 70 parts by mass or less of fumed silica per 100 parts by mass of the diene rubber.

[0015] [4] The BET specific surface area of ​​the fumed silica is 180 m 2 / g or more 500m 2 / g or less.

[0016] [5] The rubber composition for a tire according to any one of [1] to [4], wherein the fumed silica is untreated fumed silica.

[0017] [6] A rubber material for a tire obtained by vulcanizing the rubber composition for a tire according to any one of [1] to [5].

[0018] According to the present invention, it is possible to provide a rubber material for tires that is excellent in fuel economy, abrasion resistance, and heat aging resistance, and a rubber composition for tires that is suitable for producing the same.

[0019] The present invention will be described in detail below based on specific embodiments in the following order: 1. Rubber composition for tires 1.1. Diene rubber 1.2. Fumed silica 1.3. Silane coupling agent 1.4. Diol 1.5. Other components 2. Method for producing rubber composition for tires 3. Rubber material for tires

[0020] (1. Rubber Composition for Tire) The rubber composition for tire according to the present embodiment is a rubber composition comprising a diene rubber and a silanol group having a surface silanol group density of 3 / nm 2 The composition includes the following: fumed silica, a silane coupling agent, and a diol.

[0021] (1.1. Diene Rubber) The diene rubber contained in the rubber composition for a tire according to this embodiment is preferably at least one selected from natural rubber, isoprene rubber, butadiene rubber, styrene-butadiene rubber, acrylonitrile-butadiene rubber, butyl rubber, ethylene-propylene-diene rubber, and chloroprene rubber. The content of each of the above rubbers constituting the diene rubber may be determined appropriately depending on the application, etc. Among these, at least one selected from natural rubber and styrene-butadiene rubber is preferred.

[0022] Examples of natural rubber include natural rubber (NR) and modified natural rubbers such as epoxidized natural rubber (ENR), hydrogenated natural rubber (HNR), deproteinized natural rubber (DPNR), and high-purity natural rubber (HPNR). These natural rubbers may be used alone or in combination of two or more. In this embodiment, unmodified NR is preferred as the natural rubber.

[0023] Examples of styrene-butadiene rubber (SBR) include unmodified solution-polymerized SBR (S-SBR), unmodified emulsion-polymerized SBR (E-SBR), and modified SBRs thereof (modified S-SBR, modified E-SBR).

[0024] (1.2. Fumed Silica) Fumed silica is fine particle silicon dioxide produced by high-temperature hydrolysis of silicon tetrachloride in an oxyhydrogen flame. Therefore, fumed silica is also called dry silica because its production method differs from that of wet silica, which is produced by wet methods such as precipitation and gelation. Fumed silica has a smaller primary particle size of primary aggregates (smallest constituents) and a larger nitrogen adsorption BET specific surface area than wet silica. Fumed silica particles are aggregated and fused together in a beaded shape, forming bulky aggregates.

[0025] Fumed silica has siloxane bonds, but on the surface of the fumed silica, in addition to the siloxane groups, there are silanol groups in which hydroxy groups are bonded to silicon atoms. The density of silanol groups on the surface of fumed silica (surface silanol group density) is lower than that of wet silica due to differences in the manufacturing method. In this embodiment, the surface silanol group density of the fumed silica is 3 groups / nm 2 By keeping the surface silanol group density within the above range, the amount of silanol groups, which are reaction sites with the silane coupling agent described below, can be maintained, while preventing a decrease in wettability with rubber due to water being adsorbed onto the silica surface, which has the advantage of enabling even finer dispersion to be expected.

[0026] The surface silanol group density may be measured by, for example, the Karl Fischer method, the Igros method, or active hydrogen titration using a Grignard reagent.

[0027] In addition, silanol groups tend to adsorb water. Therefore, surface treatments are sometimes performed to reduce water adsorption by reacting the silanol groups with other substances. Surface-treated fumed silica is called surface-treated fumed silica, while untreated fumed silica is called untreated fumed silica.

[0028] In this embodiment, surface-treated fumed silica and untreated fumed silica are distinguished by the degree of modification hydrophobicity (M value) shown below. The degree of modification hydrophobicity (M value) is a value obtained by a measurement method utilizing the fact that surface-treated fumed silica floats in water but is completely suspended in methanol. The method described in the examples of WO 2004 / 099075 can be used to measure the M value. When surface-treated fumed silica and untreated fumed silica are represented by the M value, the M value of surface-treated fumed silica is 1 or more, and the M value of untreated fumed silica is less than 1.

[0029] In this embodiment, from the viewpoint that the silane coupling agent has a bulky molecular structure and can react in sufficient amounts with the silica surface, it is preferable that the fumed silica be untreated fumed silica that has a small amount of moisture that induces self-condensation of the coupling agent and that has a sufficient number of silanol groups, which serve as reaction sites.

[0030] A relatively high tap density of fumed silica is preferable from the viewpoint of industrial productivity. Specifically, the tap density of fumed silica is preferably 200 g / L or more. As described above, fumed silica is bulky, so when the tap density is to be 200 g / L or more, it is preferable to compress the fumed silica.

[0031] Examples of methods for compressing fumed silica include a method of compressing it with a ball mill and a method of compressing it with a vibration mill.

[0032] In this embodiment, the tap density of the fumed silica may be less than 200 g / L.

[0033] In this embodiment, the BET specific surface area of ​​the fumed silica is 200 m 2 / g or more, 250m 2 / g or more, 300m 2 When the BET specific surface area of ​​the fumed silica is within the above range, the number of silanol groups in the fumed silica that serve as reaction sites with the diene rubber or the silane coupling agent can be sufficiently secured.

[0034] The upper limit of the BET specific surface area of ​​the fumed silica is not particularly limited, but for example, it is 500 m 2 / g. If the BET specific surface area of ​​the fumed silica is too small, the flame temperature during production of the fumed silica must be increased, which tends to result in the loss of the structure unique to fumed silica and the inability to produce fumed silica stably. If the BET specific surface area of ​​the fumed silica is too large, it tends to result in the inability to produce fumed silica stably.

[0035] The true density of fumed silica is 2.0 g / cm 3 2.4g / cm or more 3 It is preferable that the density is 2.1 g / cm or less. 3 2.3g / cm or more 3 More preferably, it is 2.15 g / cm or less. 3 2.25g / cm or more 3 When the true density of the fumed silica is within the above range, the elastic modulus of the silica becomes higher than when the true density is lower than 2.0, and the reinforcing effect in the rubber composition is more likely to be exhibited.

[0036] One of the reasons why the true density is lower than the commonly known 2.2 of amorphous silica is the presence of pores inside the silica. According to MacKenzie, E = E0(1-P) 2 It is known that the elastic modulus drops sharply as the pores increase, as shown in the formula: E0 = elastic modulus of solid material, P = pore volume, E = elastic modulus of material with pore volume P

[0037] If a filler with a low modulus of elasticity is used, the reinforcing effect tends to decrease. On the other hand, if the true density is too high, the surface free energy of the silica particle surface increases, which tends to increase the difference in surface free energy with the rubber, and this may result in poor dispersibility. In addition, since the reinforcing effect generally increases with the volume fraction of the filler, filling a material with too high a density makes it difficult to achieve the effect of improving the modulus of elasticity.

[0038] Known methods for producing amorphous silica with high true density include synthesis under high pressure and rapid cooling during melting. The true density of fumed silica can be measured, for example, by the pycnometer method.

[0039] The amount of fumed silica blended is preferably 10 parts by mass or more and 70 parts by mass or less per 100 parts by mass of diene rubber. By blending the amount of fumed silica within the above range, a rubber material for tires excellent in fuel economy and wear resistance can be obtained. If the blending amount of fumed silica is too high, the viscosity increases, so the fumed silica is not sufficiently dispersed in the rubber component, and a good kneaded product tends not to be obtained.

[0040] The amount of fumed silica is more preferably 20 parts by mass or more, and even more preferably 32 parts by mass or more, per 100 parts by mass of diene rubber, while the amount of fumed silica is more preferably 60 parts by mass or less, and even more preferably 50 parts by mass or less, per 100 parts by mass of diene rubber.

[0041] (1.3. Silane Coupling Agent) Hydrophobic diene rubber and fumed silica having hydrophilic silanol groups have low affinity, making them difficult to mix during kneading. Therefore, by incorporating a silane coupling agent, a crosslinked structure between the diene rubber and the fumed silica is easily formed via the silane coupling agent, making it easier for the fumed silica to disperse uniformly in the diene rubber. As a result, the presence of coarse fumed silica that does not disperse in the rubber can be suppressed in the tire rubber material, thereby improving the abrasion resistance of the tire rubber material.

[0042] As the silane coupling agent, a sulfur-containing silane coupling agent is preferred. Examples of sulfur-containing silane coupling agents include bis-(3-triethoxysilylpropyl)tetrasulfide, bis(3-triethoxysilylpropyl)disulfide, 3-trimethoxysilylpropylbenzothiazole tetrasulfide, γ-mercaptopropyltriethoxysilane, 3-octanoylthiopropyltriethoxysilane, and mercapto-thiocarboxylate oligomer. In this embodiment, from the viewpoint of the heat resistance (thermal aging resistance) of the rubber composition for tires, a sulfide-based silane coupling agent is preferred.

[0043] In order for fumed silica to be uniformly dispersed in diene rubber, the silanol groups of the fumed silica must bond with a silane coupling agent to enhance affinity with the hydrophobic diene rubber. Therefore, the silane coupling agent must be blended in an amount that reacts with the silanol groups in the right amount. Since the surface silanol group density corresponds to the BET specific surface area per gram of fumed silica, the amount of silane coupling agent to be blended can be determined according to the BET specific surface area per gram of fumed silica.

[0044] Therefore, from the viewpoint of enhancing the dispersibility of the fumed silica, the blending amount of the silane coupling agent (the content of the silane coupling agent in the rubber composition for tires) is set to 0.50 μmol / m relative to the BET specific surface area per 1 g of the fumed silica. 2 3.9 μmol / m or more 2 The following is the result.

[0045] The blending amount is 0.7 μmol / m 2 On the other hand, the blending amount is preferably 2.0 μmol / m or more. 2 It is preferably 1.5 μmol / m or less, 2 More preferably, it is:

[0046] (1.4. Diol) A diol is a dihydric alcohol, a hydrocarbon having two hydroxy groups. By incorporating a diol, the Mooney viscosity of the tire rubber composition is reduced, but the A hardness of the tire rubber material is increased, allowing the amount of fumed silica to be reduced. As a result, the fuel economy and abrasion resistance of the tire rubber material are improved. Furthermore, by incorporating a diol together with the above-mentioned silane coupling agent, a tire rubber material with good heat aging resistance can be obtained. Note that the above effects tend not to be obtained with monohydric alcohols and trihydric or higher alcohols.

[0047] In this embodiment, preferred examples of the diol include propylene glycol, 1,3-propanediol, dipropylene glycol, diethylene glycol, and polyethylene glycol having a degree of polymerization of about 200 to 1000, and propylene glycol, 1,3-propanediol, dipropylene glycol, diethylene glycol, and polyethylene glycol having a degree of polymerization of 300 to 500 are more preferred.

[0048] Similarly to the silane coupling agent, the effect obtained by blending the diol may be determined depending on the density of the surface silanol groups. Therefore, the blending amount of the diol (the content of the diol in the rubber composition for tires) is set to 3 μmol / m with respect to the BET specific surface area per 1 g of the fumed silica. 2 14 μmol / m or more 2 The following is the result.

[0049] The blending amount is 3.4 μmol / m 2 It is preferable that the concentration is 6.8 μmol / m or more. 2 On the other hand, the blending amount is more preferably 11 μmol / m or more. 2 It is preferable that:

[0050] (1.5. Other Components) In this embodiment, the rubber composition for a tire may contain components that are blended into rubber compositions in addition to the above-described components (diene rubber, fumed silica, silane coupling agent, and diol). An example of such a component is a lubricant. Blending a lubricant improves the kneadability of each component, making it easier to obtain a rubber composition for a tire in which each component is well dispersed.

[0051] Examples of lubricants include process oils such as stearic acid, mineral oil, and chemically synthesized oil. A single lubricant may be used, or two or more types may be used in combination. Examples of process oils include aromatic oils, paraffin oils, and naphthenic oils. These may be used alone, or two or more types may be used in combination.

[0052] The amount of lubricant blended (the content of lubricant in the rubber composition for tires) is not limited as long as the effects of the present invention can be obtained. For example, the amount of lubricant blended is preferably 2 parts by mass or more and 60 parts by mass or less, and more preferably 4 parts by mass or more and 50 parts by mass or less, per 100 parts by mass of diene rubber. Specifically, the amount of lubricant blended may be determined depending on the type of diene rubber. For example, when the diene rubber is NR, the amount of lubricant blended is relatively small, and when the diene rubber is SBR, the amount of lubricant blended is relatively large, including the lubricant contained in the SBR itself.

[0053] If the amount of lubricant is too small, the viscosity becomes high and kneading becomes poor, which may result in an insufficient improvement in the abrasion resistance of the resulting tire rubber material, whereas if the amount of lubricant is too large, shearing is not applied during kneading, which may result in an insufficient dispersion of the fumed silica in the diene rubber.

[0054] Furthermore, the rubber composition for tires may contain a reinforcing filler other than hydrophilic fumed silica. Examples of reinforcing fillers include carbon black, wet silica, clay, mica, talc, calcium carbonate, aluminum hydroxide, aluminum oxide, and titanium oxide. When a reinforcing filler is compounded, an appropriate amount of a filler coupling agent may also be compounded. The amount of the reinforcing filler to be compounded is not limited as long as the effects of the present invention can be obtained, and a general compounding amount may be used.

[0055] Furthermore, the rubber composition for a tire may contain various additives such as zinc oxide, an antioxidant, a plasticizer, a processing aid, a liquid polymer, a thermosetting resin, etc. The amount of these additives to be added is not limited as long as the effects of the present invention can be obtained, and may be a general amount.

[0056] (2. Method for producing rubber composition for tire) The rubber composition for tire according to this embodiment is obtained by kneading the diene rubber, the fumed silica, the silane coupling agent, the diol, and, if necessary, other components.

[0057] In this embodiment, the rubber composition for a tire may be produced by kneading predetermined components to prepare a master batch, and then blending and kneading the remaining components into the master batch, or by kneading all of the components together.

[0058] When preparing the masterbatch, it is preferable to knead the above-mentioned diene rubber, the above-mentioned fumed silica, the above-mentioned silane coupling agent, the above-mentioned diol, and, if necessary, other components.

[0059] As a kneading device for preparing the masterbatch, for example, a known kneading device such as a Banbury mixer or a kneader can be used.

[0060] After preparing the masterbatch, other components are blended with the masterbatch and kneaded to obtain a rubber composition for tires. The masterbatch and other components can be kneaded using a known kneading device such as a Banbury mixer or a kneader.

[0061] When all the components are kneaded to produce a rubber composition for tires, a known kneading device such as a Banbury mixer or a kneader can be used.

[0062] The kneading conditions may be set so that the components are thoroughly kneaded.

[0063] (3. Rubber Material for Tire) The rubber material for tire according to this embodiment is a material obtained by vulcanizing the rubber composition for tire described above.

[0064] In order to improve the dispersibility of fumed silica in a rubber composition for tires, the content of the silane coupling agent is set according to the BET specific surface area of ​​the fumed silica, so that the silane coupling agent can crosslink the diene rubber and the fumed silica in an appropriate amount. As a result, the fumed silica is uniformly mixed in the rubber composition for tires, and the generation of coarse particles in the rubber material for tires is suppressed. This effect is particularly noticeable when the fumed silica is compressed to form compressed fumed silica.

[0065] Furthermore, diols are blended into rubber materials for tires. The inclusion of diols increases the A hardness of the rubber after vulcanization, allowing the amount of filler to be reduced. As a result, fuel economy, abrasion resistance, and heat aging resistance can be improved.

[0066] Therefore, the rubber material for a tire according to the present embodiment is excellent in fuel economy, abrasion resistance, and heat aging resistance. Such a rubber material for a tire can be suitably used for tires for passenger cars, trucks, buses, etc. It can be suitably used for various tire components, particularly for treads, base treads, sidewalls, clinches, etc.

[0067] Although the embodiments of the present invention have been described above, the present invention is not limited to the above-described embodiments and may be modified in various ways within the scope of the present invention.

[0068] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0069] (Experiment 1) (Preparation of Rubber Composition for Tires) In Experiment 1, the diene rubber was SBR rubber. The following components (A) to (D) and (E-1) to (E-4) were charged into a 0.6 L volume Plastomill (Model BB600, manufactured by Toyo Seiki Seisaku-sho, Ltd.) so that the compounding amounts per 100 parts by mass of SBR rubber were as shown in Table 1. After charging, the rotor rotation speed was adjusted within a range of 20 to 100 rpm so that the temperature of the kneaded mixture was within a range of 140 to 150°C, and the mixture was kneaded for 5 minutes after the temperature was reached. The air cylinder pressure was 0.5 MPa. After kneading was completed, the mixture was cooled to room temperature and removed to obtain a kneaded mixture. (A) Diene rubber (A-1) SBR (S-SBR E-581 manufactured by Asahi Kasei Corporation) (A-2) BR (BR01 manufactured by ENEOS Materials Corporation) (B) Filler (B-1) Carbon black (Seast 6 manufactured by Tokai Carbon, nitrogen adsorption BET specific surface area: 120 m 2 / g, tap density: 400 g / L) (B-2) Wet silica (manufactured by Tosoh Silica, Nipsil AQ, nitrogen adsorption BET specific surface area: 200 m 2 / g, tap density: 300 g / L, silanol group density: 6 / nm 2 , pycnometer method true density 2.1 g / cm 3 (B-3) Hydrophilic fumed silica (manufactured by Tokuyama, Reolosil QS-40, nitrogen adsorption BET specific surface area: 380 m 2 / g, tap density: 50 g / L, silanol group density: 2.3 / nm 2 , pycnometer method true density 2.2 g / cm 3 (B-4) Hydrophilic fumed silica (manufactured by Tokuyama, Reolosil QS-30C, nitrogen adsorption BET specific surface area: 300 m 2 / g, tap density: 70 g / L, silanol group density: 2.1 / nm 2 , pycnometer method true density 2.2 g / cm 3 (B-5) (B-4) was compressed in a ball mill to obtain a highly compressed fumed silica having a tap density of 200 g / L (silanol group density: 2.5 / nm 2, pycnometer method true density 2.2 g / cm 3 (B-6) (B-4) was compressed in a ball mill to obtain a highly compressed fumed silica having a tap density of 250 g / L (silanol group density: 3 / nm 2 , pycnometer method true density 2.2 g / cm 3 (B-7) Hydrophilic fumed silica (manufactured by Tokuyama, Reolosil CP-102, nitrogen adsorption BET specific surface area: 200 m 2 / g, tap density: 100 g / L, silanol group density: 1.8 / nm 2 , pycnometer method true density 2.2 g / cm 3 (B-8) (B-7) was compressed in a ball mill to obtain a highly compressed fumed silica having a tap density of 250 g / L (silanol group density: 3 / nm 2 , pycnometer method true density 2.2 g / cm 3 ) (C) Silane coupling agent (C-1) Polysulfide coupling agent (Si69, manufactured by EVONIK) (D) Diol (D-1) 1,3-propanediol (E) Other components (E-1) Lubricant (stearic acid, NOF Corp., Beads Stearic Acid YR) (E-2) Lubricant (zinc oxide, Seido Chemical Co., Ltd., Zinc Oxide Type 2) (E-3) Antioxidant (Ozonone 6C, manufactured by Seiko Chemical Co., Ltd.) (E-4) Process oil (Aromax 3 (TDAE Oil) manufactured by Fuji Industries Co., Ltd.)

[0070] The surface silanol group density of the fumed silica was measured using a coulometric titrator (MKC-610, manufactured by Kyoto Electronics Manufacturing Co., Ltd.) equipped with a moisture vaporizer (ADP-512, manufactured by Kyoto Electronics Manufacturing Co., Ltd.). That is, the temperature was raised to 130°C in the low-temperature furnace of the moisture vaporizer, and the amount of moisture equivalent to the loss on drying of the silica was measured by coulometric titration using the MKC-610 model. Thereafter, the amount of moisture equivalent to the loss on ignition was measured in the high-temperature furnace heated to 1000°C in the same manner by coulometric titration. The amount of moisture equivalent to the loss on ignition generated between 130°C and 1000°C was converted to silanol group density using the following formula: silanol group density (number / nm 2 ) = 668.9 × H2O (%) / specific surface area (m 2 / g)

[0071] The kneaded product obtained above was mixed with the following components (E-5), (E-6), and (E-7) using a 6-inch roll tester to obtain a rubber composition for tires. The amount of sulfur added was determined taking into consideration the amount of sulfur contained in the other additive components. (E) Other Components (E-5) Sulfur (5% oil-containing fine sulfur powder manufactured by Tsurumi Chemical Industry Co., Ltd.) (E-6) Vulcanization accelerator (Sansera CM-G, N-cyclohexyl-2-benzothiazole sulfamide (CBS) manufactured by Sanshin Chemical Industry Co., Ltd.) (E-7) Vulcanization accelerator (Sansera D-G, 1,3-diphenylguanidine (DPG) manufactured by Sanshin Chemical Industry Co., Ltd.)

[0072] The compressed fumed silica (B-5) was obtained by adding 200 g of the fumed silica (B-4) to a 7 L ball mill (ball diameter: φ32 mm, ball filling rate: 30%) and grinding at room temperature for about 5 hours at a rotation speed of 300 rpm. The tap density of the compressed fumed silica (B-6) and the compressed fumed silica (B-8) was adjusted by changing the grinding time.

[0073] The nitrogen adsorption BET specific surface area of ​​each of the fillers (B-1) to (B-8) was measured by the nitrogen adsorption BET method using a BELSOP MINI X manufactured by Microtrac. The tap density of each of the fillers (B-1) to (B-8) was measured as follows. First, a 1 L resin graduated cylinder was placed on an electronic balance, tared, and filled with approximately 1 L of filler, and the weight M (g) was recorded. After that, the cylinder was manually tapped 30 times from a height of approximately 10 cm, after which the volume V (ml) was measured, and the tap density ρ was calculated using the following formula: Tap density ρ = 1000 × M / V (g / L)

[0074]

[0075] Test specimens were prepared from the resulting rubber compositions for tires to evaluate the following properties. The resulting test specimens were used to evaluate the following physical properties.

[0076] (Processability: Mooney Viscosity) For test pieces of the obtained rubber composition for tires, the Mooney viscosity at 100°C (ML1+4 100°C) was measured in accordance with JIS K6300-1 using a Mooney viscometer (VR-1132 manufactured by Ueshima Seisakusho). When the Mooney viscosity is low, the processability of the rubber composition for tires tends to be good. The results are shown in Table 1.

[0077] (Preparation of tire rubber material test pieces) Subsequently, the obtained tire rubber composition was press-vulcanized for T90+1 minute, determined under conditions of 160°C for 30 minutes according to JIS K6300-2, to obtain a tire rubber material. Test pieces for the following evaluations were prepared from the obtained tire rubber material. The obtained test pieces were used to evaluate the following physical properties.

[0078] (A Hardness) The hardness (Shore A hardness) of the test specimens of the obtained tire rubber material was measured using a durometer in accordance with JIS K6253 Type A. Since the target A hardness of the tire rubber material is 65, it is preferable that the A hardness of the test specimens is also around 65. The results are shown in Table 1.

[0079] (Fuel efficiency performance: tan δ at 60°C) Test pieces of the obtained rubber material for tires were measured in accordance with JIS K6394 using a dynamic viscoelasticity tester (VR-7130 manufactured by Ueshima Seisakusho) under the following conditions. Tan δ (60°C) was calculated from the measured value at 60°C. Measurement temperature: 60°C Static strain: 10% Dynamic strain: ±2% Frequency: 10 Hz

[0080] The rolling resistance index was calculated using the following formula, with the calculated tan δ (60°C) of Standard Example 1 (Comparative Example 1) set to 1.0. The higher the index, the better the rolling resistance. The results are shown in Table 1. (Rolling resistance index) = (tan δ (60°C) of Standard Example 1) / (tan δ (60°C) of Example)

[0081] (Wear resistance performance: FPS abrasion volume) For the test pieces of the obtained rubber material for tires, the FPS abrasion volume was measured using an FPS abrasion tester (AB-2012 manufactured by Ueshima Seisakusho) under conditions of a temperature of 35°C, a load of 40 N, a slip ratio of 10%, and a test time of 2 minutes. The volume loss was calculated from the FPS abrasion volume, and the abrasion index was calculated using the following formula, with the loss volume of Standard Example 1 (Comparative Example 1) set at 1.0. The higher the index, the better the abrasion resistance performance. The results are shown in Table 1. (Wear index) = (loss volume of Standard Example 1) / (loss volume of Example)

[0082] (Heat Aging Resistance) The obtained rubber composition for tires was vulcanized at 160°C for T90+1 minute using a 2 mm thick mold, and the obtained vulcanized rubber sheet was punched out using a JIS No. 3 dumbbell to prepare a sample. The sample was heat aged for 5 days (120 hours) in a Geer oven set at 80°C, and then the strength at break (breaking strength) of the sample, together with an unaged sample, was measured using a tensile tester in accordance with JIS K6251. The ratio of the unaged breaking strength to the breaking strength after aging was calculated as an index of heat aging resistance. The heat resistance index was calculated using the following formula. A heat resistance index of 1 or more indicates excellent heat aging resistance, while a heat resistance index of less than 1 indicates poor heat aging resistance due to a decrease in breaking strength caused by thermal degradation. The results are shown in Table 1. (Heat resistance index) = {(breaking strength after heat aging) / (breaking strength of unaged sample)}

[0083] Furthermore, for the samples before the heat aging test, the strength index was calculated using the following formula, with the breaking strength of Standard Example 1 (Comparative Example 1) set at 1.00. The higher the strength index, the better the strength. The results are shown in Table 1. (Strength index) = (Breaking strength of Example) / (Breaking strength of Standard Example 1)

[0084] From Table 1, it was confirmed that when the diene rubber is an SBR rubber, a tire rubber material in which the amounts of the silane coupling agent and the diol added are within the above-mentioned ranges has higher abrasion resistance than a tire rubber material produced by kneading carbon black or wet silica. It was also confirmed that the tire rubber material has high heat aging resistance.

[0085] (Experiment 2) In Experiment 2, the diene rubber was NR rubber. The following components (A) to (D) and (E-1) to (E-4) were charged into a 0.5 L Moriyama pressure kneader so that the compounding amounts per 100 parts by mass of NR rubber were as shown in Table 2. After the materials were charged one by one, the rotor rotation speed was 30 rpm, and once the temperature of the kneaded mixture reached a range of 140 to 150°C, the mixture was kneaded for 5 minutes. The ram pressure during kneading was in the range of 0.4 to 0.5 MPa. After kneading was completed, the mixture was cooled to room temperature to obtain a kneaded mixture. (A) Diene rubber (A-3) Vietnam-made natural rubber: SVR (B) Filler (B-1) Carbon black (Tokai Carbon, Seast 6, nitrogen adsorption BET specific surface area: 120 m 2 / g, tap density: 400 g / L) (B-2) Wet silica (manufactured by Tosoh Silica, Nipsil AQ, nitrogen adsorption BET specific surface area: 200 m 2 / g, tap density: 300 g / L, silanol group density: 6 / nm 2 (B-4) Hydrophilic fumed silica (manufactured by Tokuyama, Reolosil QS-30C, nitrogen adsorption BET specific surface area: 300 m 2 / g, tap density: 70g / L) (B-5) Highly compressed fumed silica having a tap density of 200g / L obtained by compressing (B-4) with a ball mill. (B-6) Highly compressed fumed silica having a tap density of 250g / L obtained by compressing (B-4) with a ball mill. (C) Silane coupling agent (C-1) Polysulfide coupling agent (Si69, manufactured by EVONIK Corporation) (D) Diol (D-1) 1,3-propanediol (E) Other components (E-1) Lubricant (stearic acid, manufactured by NOF Corp., Beads Stearic Acid YR) (E-2) Lubricant (zinc oxide, manufactured by Seido Chemical Industries, Zinc Oxide Type 2) (E-3) Antioxidant (Ozonone 6C, manufactured by Seiko Chemical Industries) (E-4) Process oil (Aromax 3 (TDAE Oil) manufactured by Fuji Industries)

[0086] The kneaded product thus obtained was mixed with the following components (E-5) and (E-8) using a 6-inch roll tester to obtain a rubber composition for tires. (E) Other Components (E-5) Sulfur (5% oil-containing fine sulfur powder manufactured by Tsurumi Chemical Industry Co., Ltd.) (E-8) Vulcanization accelerator (N-(tert-butyl)-2-benzothiazole sulfenamide (TBBS), Sansera NS-G manufactured by Sanshin Chemical Industry Co., Ltd.)

[0087]

[0088] For the obtained rubber composition for a tire, test specimens were prepared to perform the same evaluations as in Experiment 1. The obtained test specimens were used to evaluate the physical properties (Mooney viscosity) evaluated in Experiment 1. The results are shown in Table 2.

[0089] (Preparation of Rubber Material for Tire) Subsequently, the obtained rubber composition for tire was press-vulcanized for T90+1 minute, determined under conditions of 150°C for 60 minutes according to JIS K6300-2, to obtain a rubber material for tire. Test specimens were prepared from the obtained rubber material for tire to perform the same evaluations as in Experiment 1. Using the obtained test specimens, some of the physical properties evaluated in Experiment 1 were evaluated. Note that the strength index was based on that of Standard Example 2 (Comparative Example 5). The results are shown in Table 2.

[0090] From Table 2, it was confirmed that even if the diene rubber is NR, a tire rubber material in which the amounts of silane coupling agent and diol added are within the above-mentioned ranges also has higher heat aging resistance than a tire rubber material produced by kneading carbon black or wet silica.

Claims

1. Diene rubber and surface silanol group density of 3 / nm 2 or less, a silane coupling agent, and a diol, wherein the content of the silane coupling agent is 0.50 μmol / m2 or less relative to the BET specific surface area per 1 g of the fumed silica. 2 3.9 μmol / m or more 2 The content of the diol is 3 μmol / m or less relative to the BET specific surface area per gram of the fumed silica. 2 14 μmol / m or more 2 A rubber composition for tires, comprising:

2. The rubber composition for tires according to claim 1, wherein the silane coupling agent is a sulfide-based silane coupling agent.

3. A rubber composition for tires according to claim 1 or 2, comprising 10 parts by mass or more and 70 parts by mass or less of said fumed silica per 100 parts by mass of said diene rubber.

4. The BET specific surface area of ​​the fumed silica is 180 m 2 / g or more 500m 2 The rubber composition for a tire according to any one of claims 1 to 3, wherein the viscosity is 1 / g or less.

5. A rubber composition for tires according to any one of claims 1 to 4, wherein the fumed silica is untreated fumed silica.

6. A rubber material for tires obtained by vulcanizing the rubber composition for tires according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Method for producing rubber composition for tire, and pneumatic tire

    JP2012144619A

  • Method of producing rubber composition for tire

    JP2015183061A

  • Tire rubber composition

    JP2019157042A

  • Method for producing rubber composition for tires, and pneumatic tire

    WO2016009776A1

  • Masterbatch, method for producing masterbatch, rubber composition for tires, method for producing rubber composition for tires, and rubber material for tires

    WO2023054510A1