Decorative sheet, resin-impregnated decorative panel, and method for manufacturing resin-impregnated decorative panel

The decorative sheet with a porous base material, design layer, and release layer with specific parameters addresses the balance of releasability and gloss-matte design in resin-impregnated boards, achieving effective peeling and aesthetic retention.

WO2024204587A1PCT designated stage expired Publication Date: 2024-10-03DAI NIPPON PRINTING CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012745
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-28
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional decorative sheets for resin-impregnated decorative boards face challenges in balancing the functions of selective peeling of the cured resin layer and expressing a gloss-matte design, as the release layer's composition and structure trade off between releasability and matte finish, and the matte feel can be lost during the pressurizing process.

Method used

A decorative sheet comprising a porous base material, a design layer, and a release layer with specific parameters such as a 60° gloss value, pure water contact angle, and Spc (arithmetic mean curvature) within predetermined ranges, allowing for both good releasability and maintenance of the gloss-matte design after curing.

Benefits of technology

The solution enables the selective peeling of the cured resin layer while maintaining a gloss-matte design, ensuring both functional releasability and aesthetic appeal of the resin-impregnated decorative boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012745_03102024_PF_FP_ABST
    Figure JP2024012745_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure provides a decorative sheet used to manufacture a resin-impregnated decorative panel, the decorative sheet comprising a porous substrate, a design layer, and a release layer having a pattern shape in this order in the thickness direction, wherein: the 60º gloss value of the release layer is at most 10; the pure water contact angle of the release layer is at least 85º; and the Spc (arithmetic mean peak curvature) of the release layer is at least 80 mm-1.
Need to check novelty before this filing date? Find Prior Art

Description

Decorative sheet, resin-impregnated decorative board, and method for manufacturing resin-impregnated decorative board

[0001] The present disclosure relates to a decorative sheet used in the manufacture of a resin-impregnated decorative board, a resin-impregnated decorative board, and a method for manufacturing a resin-impregnated decorative board.

[0002] Resin-impregnated decorative boards have been known, which are obtained by impregnating a porous substrate with a precursor such as a melamine resin and then curing the resin precursor. Resin-impregnated decorative boards are used on walls, furniture, floors, and the like in homes, stores, public facilities, and the like.

[0003] Melamine decorative boards that express a glossy matte design are known. For example, Patent Document 1 discloses a decorative board that has a release layer in harmony with a pattern on a partial area of ​​the surface of a porous substrate, and a thermosetting resin layer containing a melamine resin on the remaining area of ​​the surface that does not have the release layer, and the thermosetting resin is impregnated into the porous substrate and cured.

[0004] Patent No. 6716877

[0005] The release layer of a decorative sheet used in the manufacture of resin-impregnated decorative laminates is required to simultaneously have two functions: 1) the function of selectively releasing the cured resin layer cured by a heat and pressure process, and 2) the function of expressing a good gloss / matt design by providing a difference in gloss from the cured resin layer. However, there is still room for improvement in the design of a decorative sheet that stably balances these two functions.

[0006] The present disclosure has been made in consideration of the above-mentioned situation, and its main object is to provide a decorative sheet used in the manufacture of resin-impregnated decorative panels, in which the cured resin layer cured by a heating and pressurizing process can be selectively peeled off, and which can express a gloss-matte design due to the difference in gloss between the release layer and the cured resin layer.

[0007] In the present disclosure, there is provided a decorative sheet used in the manufacture of a resin-impregnated decorative board, the decorative sheet having a porous substrate, a design layer, and a release layer having a pattern shape, in this order in the thickness direction, the 60° gloss value of the release layer being 10 or less, the pure water contact angle of the release layer being 85° or more, and the Spc (arithmetic mean curvature of peaks) of the release layer being 80 mm -1 The decorative sheet is as described above.

[0008] In the present disclosure, there is provided a resin-impregnated decorative board, comprising: a decorative sheet having a porous substrate, a design layer, and a release layer having a pattern, in that order in the thickness direction; a core substrate arranged in the decorative sheet so as to face the porous substrate; and a cured resin layer arranged between the patterns of the release layer, the cured resin layer being thicker than the release layer and containing a cured product of curable resin Y, wherein the core substrate and the porous substrate contain the cured product of the curable resin Y, the pure water contact angle of the release layer is 85° or more, and the Spc (arithmetic mean peak curvature) of the release layer is 10 mm. -1 As described above, a resin-impregnated decorative board is provided.

[0009] The present disclosure also provides a method for producing a resin-impregnated decorative board, the method comprising: a preparation step of preparing the decorative sheet described above; a laminate formation step of forming a laminate having, in this order in the thickness direction, (i) a core substrate, the decorative sheet, a curable resin layer containing curable resin Y, and a release film, (ii) the surface of the decorative sheet facing the porous substrate is arranged opposite the core substrate, and (iii) the decorative sheet is impregnated with the curable resin Y; a heating and pressurizing step of heating and pressurizing the laminate to cure the curable resin Y and form a cured resin layer from the curable resin layer to obtain a cured laminate; and a peeling step of peeling the release film from the cured laminate to remove the cured resin layer arranged in a position overlapping with the release layer in the thickness direction, while leaving the cured resin layer arranged between the patterns of the release layer.

[0010] The present disclosure has the effect of providing a decorative sheet in which the cured resin layer cured by the heating and pressurizing process can be selectively peeled off, and which can express a gloss matte design due to the difference in gloss between the release layer and the cured resin layer.

[0011] Fig. 1 is a schematic cross-sectional view illustrating a decorative sheet according to the present disclosure. Fig. 2 is a schematic cross-sectional view illustrating a decorative sheet according to the present disclosure. Fig. 3 is a schematic cross-sectional view illustrating a resin-impregnated decorative board according to the present disclosure. Fig. 4 is a schematic cross-sectional view illustrating a method for manufacturing a resin-impregnated decorative board using a decorative sheet according to the present disclosure. Fig. 5 is a schematic cross-sectional view illustrating a method for manufacturing a resin-impregnated decorative board using a decorative sheet according to the present disclosure. Fig. 6 is a view illustrating a method for manufacturing a backing plate used when measuring the 60° gloss value of a release layer in the examples.

[0012] Below, embodiments will be described with reference to the drawings etc. However, the present disclosure can be implemented in many different forms and is not limited to the description of the embodiments exemplified below. Furthermore, to clarify the explanation, the drawings may show the width, thickness, and shape of each part schematically compared to the actual form, but this is merely an example and should not be construed as limiting.

[0013] In this specification, when describing a mode in which another component is disposed on a certain component, the term "above" or "below" refers to both a case in which another component is disposed directly above or below the certain component so as to be in contact with the component, and a case in which another component is disposed above or below the certain component with another component interposed therebetween, unless otherwise specified. Also, in this specification, when describing a mode in which another component is disposed on the surface of a certain component, the term "on the surface" refers to both a case in which another component is disposed directly above or below the certain component so as to be in contact with the component, and a case in which another component is disposed above or below the certain component with another component interposed therebetween, unless otherwise specified.

[0014] A. Decorative Sheet The decorative sheet of the present disclosure will be described in detail below. Fig. 1 is a schematic cross-sectional view illustrating an example of a decorative sheet of the present disclosure. The decorative sheet 10 shown in Fig. 1 is a decorative sheet used in the manufacture of a resin-impregnated decorative board, and comprises a porous substrate 1, a design layer 2, a release layer 3 having a pattern shape, and a thickness direction D T In the present disclosure, the 60° gloss value of the release layer 3 is 10 or less, the pure water contact angle of the release layer 3 is 85° or more, and the Spc (arithmetic mean peak curvature) of the release layer 3 is 80 mm -1 That's all.

[0015] The release layer contains, for example, a matting agent and a release agent. To improve the release layer's releasability from the cured resin layer, methods such as increasing the release agent content, reducing the matting agent content, reducing the particle size of the matting agent, or increasing the film thickness of the release layer are conceivable. However, these methods result in a lower matte finish and a lower gloss / matte design. On the other hand, methods such as reducing the release agent content, increasing the matting agent content, increasing the particle size of the matting agent, or thinning the release layer film thickness improve the gloss / matte design but reduce the release layer's releasability. As such, the release layer's releasability from the cured resin layer and the gloss / matte design are in a trade-off relationship, making it difficult to fully control these two functions solely through the composition and structure. Furthermore, because a pressure step is involved in the production process of resin-impregnated decorative boards, even if the release layer has a sufficient matte finish in the decorative sheet state, the matte finish may be lost after the pressure step. Therefore, there is still room for further study in designing decorative sheets that stably balance these two functions.

[0016] The inventors of the present application have discovered that by controlling the parameters of the release layer, namely the 60° gloss value, the pure water contact angle, and the Spc (arithmetic mean curvature of the peaks), within a predetermined range, it is possible for the release layer to have both releasability from the cured resin layer and a gloss matte design with the cured resin layer.

[0017] 1. Release Layer The release layer in the present disclosure is disposed on the surface of the design layer opposite the porous substrate and has a pattern shape. In the area where the design layer is present on the porous substrate, at least a portion of the release layer is disposed on the surface of the design layer opposite the porous substrate side, and in the area where the design layer is not present on the porous substrate, the porous substrate and the release layer may be in contact.

[0018] I. Properties The release layer in the present disclosure has a 60° gloss value of 10 or less, a pure water contact angle of 85° or more, and an Spc (arithmetic mean peak curvature) of 80 mm -1 If the 60° gloss value, pure water contact angle, and Spc of the release layer are adjusted to fall within the above-mentioned ranges, the cured resin layer can be selectively peeled off, and a gloss matte design can be achieved due to the difference in gloss from the cured resin layer.

[0019] (1) 60° Gloss Value The release layer in the present disclosure typically has a 60° gloss value of 10 or less, preferably 6.5 or less, more preferably 5.5 or less, and even more preferably 4.0 or less. When the 60° gloss value is within the above range, the release layer imparts a matte design feel, thereby enabling a gloss-matte design feel to be expressed. On the other hand, the 60° gloss value is, for example, 0.5 or more, preferably 1.0 or more, more preferably 1.2 or more, and even more preferably 2.0 or more.

[0020] In the present disclosure, the 60° gloss value of the release layer refers to the 60° specular gloss measured in accordance with Method 3 of JIS Z 8741:1997, and is a value measured by the following method. The decorative sheet is placed with the release layer side facing up, and the 60° specular gloss is measured from the release layer side using a gloss meter in accordance with Method 3 of JIS Z 8741:1997. The 60° gloss value of the release layer is the average value of measurements taken at any 10 locations. At each measurement location, the release layer is located in the center of the measurement area of ​​the gloss meter, and the measurement is performed after confirming that the area of ​​the release layer accounts for 30% or more, preferably 50% or more, of the area of ​​the measurement area. As a specific method for this, the method described in the examples can be adopted.

[0021] The 60° gloss value of the release layer can be adjusted by the average particle size of the matting agent, the content of the matting agent, and the thickness of the release layer. For example, the 60° gloss value can be reduced by reducing the thickness of the release layer. For example, the 60° gloss value can be reduced by increasing the content of the matting agent. For example, the 60° gloss value can be reduced by increasing the average particle size of the matting agent.

[0022] (2) Pure Water Contact Angle The pure water contact angle of the release layer in the present disclosure is typically 85° or more, preferably 90° or more, more preferably 100° or more, and even more preferably 110° or more. When the pure water contact angle of the release layer is in the above range, the releasability of the cured resin layer is improved. In addition, the contamination resistance is improved. On the other hand, the pure water contact angle of the release layer is, for example, 130° or less, and preferably 125° or less.

[0023] In the present disclosure, the pure water contact angle of the release layer is a value obtained by measurement using the following method. Specifically, a decorative sheet is placed on a horizontal surface with the release layer facing up. Next, a water droplet (pure water, 2.0 μL) is dropped onto the release layer from a direction perpendicular to the horizontal surface. The water droplet is dropped so that it is not dropped at the boundary between the design layer and the release layer, but is dropped so that the entire droplet is in contact with the release layer. After dropping the water droplet, a one-second wait is performed, and the contact angle between the release layer and pure water is measured using a contact angle meter. The above measurement is performed at 10 random locations, and the average value is taken as the pure water contact angle.

[0024] The pure water contact angle can be adjusted by the content of the release agent and the thickness of the release layer. For example, the pure water contact angle can be increased by increasing the content of the release agent. For example, the pure water contact angle can be increased by increasing the thickness of the release layer.

[0025] (3) Spc (arithmetic mean curvature of peaks) The release layer in the present disclosure typically has an Spc (arithmetic mean curvature of peaks) of 80 mm. -1 or more, and 100 mm -1 It is preferable that the length is 120 mm or more. -1 More preferably, it is 150 mm or more.-1 By setting the Spc of the release layer within the above range, the matte surface finish is not lost even after the heating and pressing process, and a glossy matte design can be achieved. On the other hand, the Spc (arithmetic mean curvature of the peaks) is 300 mm or more. -1 It is preferable that the length is 200 mm or less. -1 More preferably, it is:

[0026] Spc (arithmetic mean curvature of the peaks) is one of the three-dimensional surface texture parameters defined in ISO 25178, and is the mean curvature (average sharpness) of the tip of the peaks, calculated from the arithmetic mean value of the curvature radii of the peaks (peaks) of the parts classified as peaks (convex parts) in the feature image included in the reference area. Therefore, Spc (arithmetic mean curvature of the peaks) is the reciprocal (mm) of the radius (mm -1 )

[0027] The larger the value of Spc (arithmetic mean curvature of the peaks), the greater the curvature of the tip of the peak (protrusion) (the reciprocal of the curvature radius is smaller, and the tip shape is sharper). On the other hand, the smaller the value of Spc (arithmetic mean curvature of the peaks), the smaller the curvature of the peak (protrusion apex) (the reciprocal of the curvature radius is larger, and the tip shape is blunter).

[0028] In the present disclosure, the Spc (arithmetic mean curvature of peaks) of the release layer is the average value of measurements taken on the surface of the release layer of a decorative sheet using a laser microscope manufactured by Keyence Corporation, with measurement points selected so that all of the measurement points are within the release layer, at 10 arbitrary points, under the following conditions: (Measurement conditions) Objective lens: 5x Laser wavelength: 661 nm Measurement area at each point: 500 μm × 500 μm

[0029] The Spc can be adjusted, for example, by adjusting the average particle size of the matting agent. Specifically, the Spc can be increased by increasing the average particle size of the matting agent. Furthermore, the Spc can be increased by increasing the content of the matting agent.

[0030] II. Composition (1) Resin Component The release layer contains a resin component. The resin component is typically a cured product (crosslinked structure) of curable resin X. On the other hand, the resin component may be a thermoplastic resin. In particular, it is preferable that the release layer contains a cured product of curable resin X. This is because a release layer with good abrasion resistance can be obtained. Furthermore, when the release layer contains a cured product of curable resin X, the release layer has good releasability from the cured resin layer.

[0031] Examples of the curable resin X include ionizing radiation curable resins and thermosetting resins. Examples of the ionizing radiation curable resin include electron beam curable resins and ultraviolet ray curable resins.

[0032] The ionizing radiation curable resin (ionizing radiation curable compound) is not limited as long as it undergoes a crosslinking polymerization reaction upon irradiation with ionizing radiation and changes into a three-dimensional polymer structure. Examples of the ionizing radiation curable resin include prepolymers, oligomers, and monomers having a polymerizable unsaturated bond or epoxy group in the molecule that can be crosslinked upon irradiation with ionizing radiation. In the present disclosure, only one type of ionizing radiation curable resin may be used, or two or more types may be used. Among these, it is preferable to use at least one of a polyfunctional monomer and an oligomer as the ionizing radiation curable resin.

[0033] Examples of ionizing radiation curable resins include (meth)acrylate resins such as urethane (meth)acrylate, ester (meth)acrylate, and epoxy (meth)acrylate; silicon resins such as siloxane; ester resins; and epoxy resins. (Meth)acrylate resins refer to acrylate resins or methacrylate resins.

[0034] The weight-average molecular weight of the ionizing radiation curable resin is, for example, 500 to 80,000, or may be 1,000 to 50,000. The weight-average molecular weight is a value measured by gel permeation chromatography (GPC) using polystyrene as a standard substance.

[0035] The ionizing radiation curable resin preferably contains at least a polyfunctional monomer or oligomer having a weight-average molecular weight of at least 500. Examples of such polyfunctional monomers or oligomers include (meth)acrylate resins such as dipentaerythritol hexa(meth)acrylate, dipentaerythritol penta(meth)acrylate, urethane(meth)acrylate, ester(meth)acrylate, and epoxy(meth)acrylate.

[0036] On the other hand, examples of thermosetting resins include unsaturated ester resins, urethane resins (including two-component curing polyurethanes), epoxy resins, aminoalkyd resins, phenolic resins, urea resins, diallyl phthalate resins, melamine resins, guanamine resins, melamine urea co-condensation resins, silicon resins, and siloxane resins.

[0037] (2) Matting Agent The release layer preferably contains a matting agent. Examples of the matting agent include inorganic particles and synthetic resin particles. Examples of the inorganic particles include silica, alumina, calcium carbonate, magnesium carbonate, calcium sulfate, barium sulfate, and kaolin. Examples of the synthetic resin particles include acrylic beads, urethane beads, nylon beads, silicone beads, silicone rubber beads, polycarbonate beads, and polyolefin wax (e.g., polypropylene wax and polyethylene wax).

[0038] The average particle size of the matting agent is, for example, 0.3 μm or more and 10 μm or less, or 0.5 μm or more and 7 μm or less, or 1 μm or more and 5 μm or less. The average particle size is D50 according to the volume-based particle size distribution measured by a laser diffraction scattering method.

[0039] The content of the matting agent is preferably 5 parts by mass or more, more preferably 8 parts by mass or more, and particularly preferably 10 parts by mass or more, relative to 100 parts by mass of the release layer. 100 parts by mass of the release layer means that the total solid content of the release layer is 100 parts by mass. On the other hand, the content of the matting agent is preferably 20 parts by mass or less, more preferably 18 parts by mass or less, and particularly preferably 15 parts by mass or less, relative to 100 parts by mass of the release layer.

[0040] (3) Release Agent The release layer may contain a release agent. Addition of a release agent improves releasability. Examples of release agents include silicone-based release agents such as silicone oil, wax-based release agents such as polyolefin wax, and fluorine-based release agents. Among these, silicone oil is preferred because it has excellent heat resistance in the heating and pressurizing process. The silicone oil may be reactive or non-reactive, but reactive silicone oil is preferred because it has even better heat resistance.

[0041] Reactive silicone oil refers to the modified silicone oil that has organic group introduced into side chain or end, and has reactivity due to the nature of the organic group that is introduced.Specifically, reactive silicone oil can be exemplified as modified silicone oil side chain type, modified silicone oil both ends type, modified silicone oil one end type, modified silicone oil side chain both ends type, and the organic group that is introduced is amino-modified, epoxy-modified, mercapto-modified, carboxyl-modified, carbinol-modified, phenol-modified, methacrylic-modified, heterogeneous functional group-modified, etc.These reactive silicone oils can be used alone or in combination of two or more.

[0042] The non-reactive silicone oil is not particularly limited as long as it does not have a reactive functional group such as an amino group, an epoxy group, a mercapto group, a carboxy group, a hydroxy group, a (meth)acryloyl group, or an allyl group. Examples of the non-reactive silicone oil include silicone oils made of polysiloxane, as well as polyether-modified silicone oils, aralkyl-modified silicone oils, fluoroalkyl-modified silicone oils, long-chain alkyl-modified silicone oils, higher fatty acid ester-modified silicone oils, higher fatty acid amide-modified silicone oils, and phenyl-modified silicone oils. These non-reactive silicone oils can be used alone or in combination of two or more.

[0043] The content of the release agent is, for example, 1 part by mass or more and 10 parts by mass or less, preferably 2 parts by mass or more and 9 parts by mass or less, and more preferably 3 parts by mass or more and 8 parts by mass or less, per 100 parts by mass of the release layer.

[0044] The release layer may be colorless or colored. In the latter case, the release layer preferably contains a colorant. The colorant may be the same as the colorant used in the design layer described below.

[0045] The release layer may contain additives such as ultraviolet absorbers, infrared absorbers, light stabilizers, polymerization inhibitors, crosslinking agents, antistatic agents, antioxidants, leveling agents, coupling agents, plasticizers, antifoaming agents, fillers, thermal radical generators, aluminum chelating agents, etc. The weather resistance of the release layer can be improved by adding ultraviolet absorbers or light stabilizers.

[0046] III. Thickness and Ratio The thickness of the release layer is not particularly limited, but is, for example, 0.1 μm or more and 20 μm or less, preferably 0.3 μm or more and 10 μm or less, and more preferably 0.5 μm or more and 8 μm or less. The thickness of the release layer is the thickness T of the release layer 3 shown in FIG. 3 As shown in Fig. 1, the thickness of the portion of the decorative layer 2 that does not penetrate into the decorative layer 2 and protrudes from the surface of the decorative layer 2 opposite to the substrate 1 is the thickness of the portion of the decorative layer 2 that does not penetrate into the decorative layer 2 and protrudes from the surface of the decorative layer 2 opposite to the substrate 1. Also, the area of ​​the release layer is S when the decorative sheet is viewed from the pattern thickness direction. 1The area of ​​the porous substrate is S 2 In this case, S 2 S against 1 The ratio (S 1 / S 2 ) is, for example, 5% or more, and may be 10% or more. 1 / S 2 is, for example, 80% or less, may be 70% or less, or may be 60% or less.

[0047] IV. Formation Method The release layer can be obtained, for example, by applying a release layer-forming ink containing a curable resin X to the surface of the design layer opposite the porous substrate and curing it. Since a portion of the release layer-forming ink penetrates the porous substrate, as shown in the examples described below, the porosity of the porous substrate affects the pure water contact angle, 60 ° gloss value, and SPC. In addition, the composition of the release layer-forming ink (e.g., the proportion of weathering agents such as light stabilizers and UV absorbers) mainly affects the 60 ° gloss value and SPC, as shown in the examples described below. In the present disclosure, by taking these effects into consideration and adjusting the pure water contact angle, 60 ° gloss value, and SPC within a predetermined range, good releasability and good gloss matte design can be obtained.

[0048] When the ink for forming a release layer contains an electron beam curable resin as the curable resin X, a cured product of the electron beam curable resin is usually obtained by irradiating it with an electron beam. Examples of the electron beam source include various electron beam accelerators such as Cockcroft-Waldt type, Van de Graaf type, resonant transformer type, insulating core transformer type, linear type, dynamitron type, and high frequency type. The energy of the electron beam is, for example, 100 kV or more and 1000 kV or less, or may be 100 kV or more and 300 kV or less. The irradiation dose of the electron beam is, for example, 2 Mrad or more and 15 Mrad or less.

[0049] When the ink for forming a release layer contains an ultraviolet-curable resin as the curable resin X, a cured product of the ultraviolet-curable resin is usually obtained by irradiating the ink with ultraviolet light. Examples of ultraviolet light sources include ultra-high pressure mercury lamps, high pressure mercury lamps, low pressure mercury lamps, carbon arc lamps, black light fluorescent lamps, and metal halide lamps. The wavelength of the ultraviolet light is, for example, 190 nm or more and 380 nm or less.

[0050] When the ink for forming a release layer contains a thermosetting resin as the curable resin X, it is usually heated to obtain a cured product of the thermosetting resin. The heating temperature is set appropriately depending on the type of thermosetting resin. The ink for forming a release layer may contain a curing agent such as a crosslinking agent or a polymerization initiator, and a polymerization accelerator, in addition to the thermosetting resin. Examples of curing agents include isocyanates, organic sulfonates, organic amines, peroxides (e.g., methyl ethyl ketone peroxide), and radical initiators (azoisobutylnitrile).

[0051] The ink for forming the release layer may contain a solvent, if necessary. Examples of the solvent include water; hydrocarbon compounds such as toluene and xylene; alcohol compounds such as methanol, ethanol, and methyl glycol; ketone compounds such as acetone and methyl ethyl ketone; ester compounds such as methyl formate and ethyl acetate; nitrogen-containing compounds such as N-methylpyrrolidone and N,N-dimethylformamide; ether compounds such as tetrahydrofuran and dioxane; halogenated hydrocarbon compounds such as methylene chloride and chloroform; and dimethyl sulfoxide.

[0052] V. Other The release layer has releasability with respect to the cured resin layer located between the release layer and the release film during the manufacturing process of the resin-impregnated decorative board described below. By having such releasability, in the resin-impregnated decorative board 100 shown in Figure 3 manufactured using the decorative sheet of the present disclosure, the release layer 3 imparts a matte design feel, and the cured resin layer 32 imparts a glossy design feel, thereby achieving a gloss-matte design feel.

[0053] Furthermore, as shown in Figure 2, it is preferable that the release layer 3 is arranged so as to synchronize with the pattern of the design layer 2. "Synchronization" means that the shapes and positions of the two target patterns generally match. Specifically, it means that the shapes and positions of the release layer pattern and at least a portion of the pattern constituting the design layer's design match to an extent that does not impair realism and a sense of luxury. In Figure 2, the design layer 2 has design layers y1 and y2, and the release layer 3 is synchronized with the design layer y1. By arranging the pattern of the release layer so as to synchronize with the design layer's design, a high-quality texture can be obtained. On the other hand, the release layer does not have to be arranged so as to synchronize with the design layer's design.

[0054] 2. Design Layer The design layer in the present disclosure is disposed on one surface of the porous substrate. The design layer preferably has a pattern.

[0055] Examples of patterns for the design layer include organic patterns, inorganic patterns, and abstract patterns. Organic patterns are patterns derived from the life activities of living organisms such as animals and plants. Inorganic patterns are patterns that do not fall under the category of organic patterns. Abstract patterns are patterns that interpret objects (such as images found in nature) abstractly and do not represent a clear shape. Examples of organic patterns include wood grain patterns, leather patterns, floral patterns, and botanical patterns. Examples of inorganic patterns include stone patterns, concrete patterns, sand patterns, fabric patterns, metal patterns, tile patterns, and brickwork patterns. Examples of abstract patterns include flickering patterns (such as ink flickering patterns), smoke patterns, and marble patterns.

[0056] The design layer has, for example, a pattern layer. The design layer may also have a solid layer on the porous substrate side of the pattern layer. In the present disclosure, the pattern layer refers to a layer formed partially (particularly in a pattern) on one side of the porous substrate. The solid layer refers to a layer formed over the entire surface of one side of the porous substrate.

[0057] The design layer contains, for example, a colorant and a resin component. Examples of the colorant include inorganic pigments such as carbon black, titanium white, zinc white, red iron oxide, Prussian blue, and cadmium red; organic pigments such as azo pigments, lake pigments, anthraquinone pigments, quinacridone pigments, phthalocyanine pigments, isoindolinone pigments, and dioxazine pigments; metal powder pigments such as aluminum powder and bronze powder; pearlescent pigments such as titanium oxide-coated mica and bismuth oxide chloride; fluorescent pigments; and luminous pigments. Dyes may also be used as the colorant.

[0058] Examples of the resin component include (meth)acrylic resins, ester urethane resins, acrylamide resins, ethylene oxide resins, N-vinylpyrrolidone resins, ester resins, amide resins, vinyl acetate resins, vinyl chloride resins, urethane (meth)acrylic resins, natural rubber, and synthetic rubber. Of these, (meth)acrylic resins and urethane (meth)acrylic resins are preferred.

[0059] The resin component preferably contains a resin having one or more polar groups selected from the group consisting of a hydroxy group, an amino group, and a carboxy group. By containing the resin having the polar group, the impregnation of the curable resin Y into the porous substrate is improved.

[0060] The resin having a polar group has a hydroxy group (-OH), an amino group (-NH 2 ), or a carboxy group (—COOH). The polar group may be ionized and stabilized, for example, by the influence of a solvent or other functional groups. Therefore, the "hydroxy group (—OH)" is in the ionized state, "—O - " is a concept that includes the above "amino group (-NH 2 ) is in the ionized state "-NH 3 + " is a concept that includes "carboxy group (-COOH)" in the ionized state "-COO - " is a concept that includes

[0061] Hydroxy group (-OH), amino group (-NH 2Examples of resins having one or more polar groups, either a carboxy group (—COOH), an aqueous protein such as casein, cellulose, acetyl cellulose, cellulose nitrate, hydroxypropyl cellulose, carboxymethyl cellulose and the like, polyvinyl alcohol derivatives such as polyvinyl alcohol and polyvinyl butyral resin, amino resins such as melamine resin, (meth)acrylic acid resins, phenolic resins, acrylic polyols, natural polymers (for example, polynucleotides, polypeptides, polysaccharides), and the like.

[0062] The design layer in the present disclosure preferably contains one or more of casein, melamine-based resin, polyvinyl alcohol, polyvinyl alcohol derivative, cellulose, and cellulose derivative as a resin having a polar group, and more preferably contains casein. As casein, α-casein, β-casein, γ-casein, or a mixture thereof can be used. Furthermore, casein derivatives such as sodium caseinate and ammonium caseinate can be used alone or in combination.

[0063] The ratio of the resin having the polar group to the resin components contained in the design layer is, for example, 20% by mass or more, 30% by mass or more, 40% by mass or more, or 50% by mass or more. On the other hand, the ratio of the resin having the polar group is, for example, 100% by mass or less, or 90% by mass or less. If the content of the resin having the polar group is within the above range, the penetration of the ink of the release layer into the porous substrate can be further suppressed without inhibiting the penetration of the curable resin Y into the porous substrate.

[0064] The design layer may contain additives such as fillers (e.g., silica), extender pigments (e.g., organic beads), neutralizers, surfactants, etc. The thickness of the design layer is not particularly limited, but is, for example, 0.1 μm or more and 20 μm or less.

[0065] The design layer can be formed, for example, by coating an ink containing a colorant, a binder resin, and a solvent (or a dispersion medium). For example, the ink is applied to one side of the porous substrate and then dried to obtain the design layer.

[0066] Examples of the solvent (or dispersion medium) include petroleum-based organic solvents such as hexane, heptane, octane, toluene, xylene, ethylbenzene, cyclohexane, and methylcyclohexane; ester-based organic solvents such as ethyl acetate, butyl acetate, 2-methoxyethyl acetate, and 2-ethoxyethyl acetate; alcohol-based organic solvents such as methyl alcohol, ethyl alcohol, normal propyl alcohol, isopropyl alcohol, isobutyl alcohol, ethylene glycol, and propylene glycol; ketone-based organic solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ether-based organic solvents such as diethyl ether, dioxane, and tetrahydrofuran; chlorine-based organic solvents such as dichloromethane, carbon tetrachloride, trichloroethylene, and tetrachloroethylene; and inorganic solvents such as water.

[0067] Examples of the coating method include printing. Examples of printing methods include gravure printing, offset printing, screen printing, flexographic printing, electrostatic printing, and inkjet printing. Examples of coating methods for forming a solid layer include various coating methods such as roll coating, knife coating, air knife coating, die coating, lip coating, comma coating, kiss coating, flow coating, and dip coating.

[0068] 3. Porous Substrate The porous substrate in the present disclosure is a substrate impregnated with curable resin Y during the production of the resin-impregnated decorative board. Examples of porous substrates include permeable fibrous substrates. Examples of permeable fibrous substrates include paper, synthetic paper, nonwoven fabrics, and woven fabrics. Examples of the paper include titanium paper, tissue paper, kraft paper, linter paper, paperboard, gypsum board paper, fine paper, coated paper, parchment paper, and Japanese paper. Vinyl wallpaper rolls (paper dry-laminated with polyvinyl chloride resin) can also be used as the fibrous substrate. Other examples of fibrous substrates include nonwoven fabrics or woven fabrics containing inorganic fibers such as glass fiber, asbestos, potassium titanate fiber, alumina fiber, silica fiber, and carbon fiber. Other examples of fibrous substrates include nonwoven fabrics or woven fabrics containing synthetic resin fibers such as polyester, vinylon, polyethylene, and polypropylene. Among these porous substrates, titanium paper, tissue paper, kraft paper, coated paper, art paper, parchment paper, glassine paper, parchment paper, paraffin paper, and Japanese paper are preferred in terms of impregnation with the curable resin Y. Titanium paper is particularly preferred as a porous substrate because it has excellent impregnation with the curable resin Y and also has excellent hiding power.

[0069] The porous substrate may be colored. For example, a colored porous substrate can be obtained by blending a colorant during the manufacturing stage of the porous substrate. For example, when the porous substrate is paper, colored paper can be obtained by blending a colorant during the papermaking stage. Examples of colorants include inorganic pigments such as titanium dioxide, carbon black, and iron oxide, organic pigments such as phthalocyanine blue, and various dyes. The amount of colorant blended is appropriately set according to the desired color tone. The porous substrate may also contain various additives such as fillers, matting agents, foaming agents, flame retardants, lubricants, antistatic agents, antioxidants, UV absorbers, and light stabilizers, as needed.

[0070] The basis weight of the porous substrate is not particularly limited, but is, for example, 40 g / m 2 Above, 150g / m 2The thickness of the porous substrate is not particularly limited, but is, for example, 50 μm or more and 170 μm or less. For example, in order to improve the adhesion of the ink that forms the design layer, the surface of the porous substrate facing the design layer may be subjected to a corona discharge treatment.

[0071] 4. Decorative Sheet The decorative sheet of the present disclosure is used to manufacture a resin-impregnated decorative board. A method for manufacturing a resin-impregnated decorative board using the decorative sheet of the present disclosure will be described later.

[0072] B. Resin-impregnated decorative board The resin-impregnated decorative board of the present disclosure will be described in detail below. Figure 3 is a schematic cross-sectional view illustrating a resin-impregnated decorative board of the present disclosure. The resin-impregnated decorative board 100 shown in Figure 3 includes a decorative sheet 10 having a porous substrate 1, a design layer 2, and a release layer 3 having a patterned shape, in this order in the thickness direction; a core substrate 20 arranged to face the porous substrate 1 in the decorative sheet 10; and a cured resin layer 32 arranged between the patterns of the release layer 3, thicker than the release layer 3, and containing a cured product of curable resin Y. The porous substrate contains the cured product of the curable resin Y. The pure water contact angle of the release layer 3 is within a predetermined range, and the Spc (arithmetic mean curvature of the peaks) of the release layer 3 is within a predetermined range.

[0073] According to the resin-impregnated decorative board of the present disclosure, since the pure water contact angle of the release layer is equal to or greater than a predetermined value and the Spc (arithmetic mean peak curvature) of the release layer is equal to or greater than a predetermined value, the cured resin layer arranged in a position overlapping the release layer is peeled off well, and the resin-impregnated decorative board has a good gloss matte design between the release layer and the cured resin layer.

[0074] 1. Decorative Sheet The decorative sheet of the present disclosure has a porous substrate, a design layer, and a release layer having a pattern shape, in this order in the thickness direction.

[0075] (1) Release Layer In the resin-impregnated decorative board of the present disclosure, the pure water contact angle of the release layer is typically 85° or more, preferably 90° or more, more preferably 100° or more, and even more preferably 110° or more. When the pure water contact angle of the release layer in the resin-impregnated decorative board is within the above range, the releasability of the cured resin layer is improved. Furthermore, the contamination resistance is improved. Meanwhile, the pure water contact angle of the release layer in the resin-impregnated decorative board is, for example, 130° or less, and preferably 125° or less.

[0076] The pure water contact angle of the release layer in the resin-impregnated decorative laminate is a value measured by completely removing the cured resin layer remaining on the release layer to expose the release layer, and then using the same method as the method for measuring the pure water contact angle of the release layer detailed above in "A. Decorative Sheet." Examples of methods for removing the cured resin layer remaining on the release layer include the same method as the method for the cellophane tape resistance test in the examples.

[0077] The method for adjusting the pure water contact angle of the release layer is the same as that described in detail above in "A. Decorative sheet."

[0078] The Spc (arithmetic mean curvature of peaks) of the release layer in the resin-impregnated decorative board is 10 mm -1 or more, and 15 mm -1 More than 20 mm is preferable. -1 More preferably, 40 mm or more -1 More preferably, 60 mm or more -1 The above is particularly preferred. If the Spc of the release layer is within the above range, the release layer imparts a matte design feel to the resin-impregnated decorative board, thereby enabling a glossy matte design feel to be expressed. On the other hand, the Spc (arithmetic mean curvature of the peaks) of the release layer in the resin-impregnated decorative board is, for example, 140 mm -1 is less than or equal to 120 mm -1 Preferably less than 100 mm -1 The following is more preferred:

[0079] In the resin-impregnated decorative board, the method of measuring and adjusting the Spc of the release layer is the same as that detailed above in "A. Decorative sheet."

[0080] The 60° gloss value of the release layer of the resin-impregnated decorative board is preferably 10 or less, more preferably 8 or less, and particularly preferably 7.5 or less. When the 60° gloss value of the release layer is within the above range, the release layer imparts a matte design feel, thereby enabling a gloss-matte design feel to be expressed. On the other hand, the 60° gloss value of the release layer of the resin-impregnated decorative board is, for example, 2.0 or more, and preferably 3.0 or more.

[0081] The methods for measuring and adjusting the 60° gloss of the release layer in the resin-impregnated decorative board are the same as those detailed above in "A. Decorative sheet."

[0082] (2) Porous substrate and decorative layer The porous substrate and decorative layer in the present disclosure are the same as those described in detail in "A. Decorative sheet" above. In addition, in the resin-impregnated decorative board, the porous substrate contains a cured product of curable resin Y.

[0083] 2. Cured Resin Layer The resin-impregnated decorative board of the present disclosure has a cured resin layer disposed between the patterns of the release layer and thicker than the release layer. The 60° gloss value of the cured resin layer is preferably greater than the 60° gloss value of the release layer. This is because a glossy matte design can be achieved. The 60° gloss value of the cured resin layer is, for example, 11 or more, or may be 15 or more, or may be 20 or more. On the other hand, the 60° gloss value of the cured resin layer is, for example, 60 or less, or may be 55 or less, or may be 50 or less.

[0084] In the resin-impregnated decorative board, the difference between the 60° gloss value of the release layer and the 60° gloss value of the cured resin layer is preferably 1.0 or more, and more preferably 3.0 or more, because this allows for a more pronounced gloss matte effect.

[0085] In the resin-impregnated decorative board, the ratio (G32 / G3) of the 60° gloss value G32 of the cured resin layer 32 to the 60° gloss value G3 of the release layer 3 is preferably 1.2 or more, and more preferably 1.5 or more, because this allows for a more pronounced matte gloss effect.

[0086] The cured resin layer contains a cured product of the curable resin Y. Among the curable resins Y, a thermosetting resin is preferred. A wide variety of thermosetting resins can be used as the thermosetting resin. Examples of thermosetting resins include melamine-based resins (melamine-based resin precursors), melamine-urea co-condensation resins, unsaturated polyester-based resins, polyurethane-based resins (including two-component curing polyurethanes), epoxy-based resins, aminoalkyd-based resins, phenol-based resins, urea-based resins, diallyl phthalate-based resins, guanamine-based resins, silicon-based resins, and polysiloxane-based resins. Examples of methods for impregnating the decorative sheet with the thermosetting resin include immersing the decorative sheet in a bath containing the thermosetting resin; applying the thermosetting resin to the decorative sheet using a coater such as a kiss coater or a comma coater; and spraying the thermosetting resin onto the decorative sheet using a spray device or shower device.

[0087] In the present disclosure, the thickness T of the cured resin layer 32 32 is the thickness T of the release layer 3 3 The thickness of the cured resin layer T is thicker than the thickness of the cured resin layer T. The uneven surface makes it easier to improve the surface design. 32 is not particularly limited, but may be, for example, 1 μm or more, or 10 μm or more. 32 is, for example, 500 μm or less, and may be 300 μm or less. 32 The thickness T may be less than 30 μm. 32 By reducing the thickness T of the cured resin layer, the processability when peeling the release film from the cured resin layer is improved. 32 may be 28 μm or less, may be 25 μm or less, or may be 20 μm or less.

[0088] In this embodiment, the difference between the top position of the release layer and the top position of the cured resin layer (surface height difference of the resin-impregnated decorative laminate) is, for example, preferably 0.5 μm or more and 45.0 μm or less, more preferably 2.0 μm or more and 35.0 μm or less, and even more preferably 3.0 μm or more and 30.0 μm or less. Furthermore, the difference may be 0.5 μm or more and 25 μm or less, 2.0 μm or more and 25 μm or less, or 3.0 μm or more and 20 μm or less.

[0089] 3. Core Substrate The resin-impregnated decorative board of the present disclosure has a porous core substrate 20 on the surface of the decorative sheet 10 facing the porous substrate 1 (the surface of the decorative sheet 10 located on the porous substrate 1 side relative to the design layer 2). Having a core substrate can increase the mechanical strength of the resin-impregnated decorative board. Examples of the core substrate 20 include phenolic resin-impregnated paper. Phenolic resin-impregnated paper is paper obtained by impregnating kraft paper, which serves as core paper, with phenolic resin and drying it. The core substrate may contain a cured product of curable resin Y.

[0090] 4. Cured Product of Curable Resin The porous substrate in the present disclosure contains a cured product of curable resin Y. As will be described later, the cured product of curable resin Y filled in the porous substrate and the cured product of curable resin Y contained in the cured resin layer are formed from the same curable resin Y. These cured products are, for example, cured products of thermosetting resins.

[0091] The resin-impregnated decorative board of the present disclosure preferably has a total light transmittance as defined in JIS K7361-1:1997 of 10% or less, more preferably 5% or less, and even more preferably 1% or less.

[0092] 5. Resin-Impregnated Decorative Boards The resin-impregnated decorative boards of the present disclosure are used, for example, by being placed on the surface of a substrate. Examples of substrates include wood members, resin members, metal members, and ceramic members. Examples of wood members include wood veneers, wood plywood, particle boards, and wood fiberboards. Examples of wood used for wood members include cedar, cypress, pine, and lauan. Examples of resins used for resin members include vinyl chloride resins, (meth)acrylic resins, ester resins, styrene resins, olefin resins, acrylonitrile-butadiene-styrene copolymers (ABS resins), phenolic resins, cellulose resins, carbonate resins, melamine resins, and rubber. Examples of metals used for metal members include iron and aluminum. The material of the ceramic member may be ceramics such as glass or porcelain, non-cement ceramic materials such as gypsum, or non-ceramic ceramic materials such as ALC (lightweight aerated concrete).

[0093] Examples of applications of the resin-impregnated decorative boards of the present disclosure include building materials and furniture. Building materials may be interior or exterior materials. Building materials include, for example, walls, floors, ceilings, doors, and shelves. Furniture includes, for example, tables, desks, and cabinets.

[0094] 4(a) to (d) and 5(a) and (b) are schematic cross-sectional views illustrating a method for manufacturing a resin-impregnated decorative board according to the present disclosure. The method for manufacturing a resin-impregnated decorative board according to the present disclosure includes a preparation step (FIG. 4(a)) of preparing the decorative sheet 10 described above, and a laminate forming step of forming a laminate 52 having, in this order in the thickness direction, (i) a core substrate 20, a decorative sheet 10, a curable resin layer 30 containing a curable resin Y, and a release film 40, (ii) the surface of the decorative sheet 10 on the porous substrate 1 side is arranged opposite the core substrate 20, and (iii) the decorative sheet 10 is impregnated with the curable resin Y. 4(b) to 4(d)), a heating and pressurizing step (FIG. 5(a)) of heating and pressurizing the laminate 52 to harden the curable resin Y and form a cured resin layer 31 from the curable resin layer 30 to obtain a cured laminate 53, and a peeling step (FIG. 5(b)) of peeling the release film 40 from the cured laminate 53 to remove the cured resin layer 31 arranged in a position overlapping with the release layer 3 in the thickness direction, while leaving the cured resin layer 31 arranged between the patterns of the release layer 3.

[0095] 1. Preparation Step This step is a step of preparing a decorative sheet. Details of the decorative sheet are as described above.

[0096] 2. Laminate Formation Step This step is a step of forming a laminate 52, as shown in FIG. 4(d), which includes (i) a core substrate 20, a decorative sheet 10, a curable resin layer 30 containing curable resin Y, and a release film 40, in that order in the thickness direction, (ii) the surface of the decorative sheet 10 facing the porous substrate 1 faces the core substrate 20, and (iii) the decorative sheet 10 is impregnated with the curable resin Y.

[0097] The method for forming such a laminate is not particularly limited. For example, as shown in Fig. 4(b), a decorative sheet 10 is impregnated with a curable resin Y, and a curable resin layer 30 containing the curable resin Y is formed to cover the design layer 2 and the release layer 3, thereby obtaining a precursor laminate 51 (Fig. 4(c)). Next, the release film 40 is placed on the surface of the precursor laminate facing the curable resin layer 30, and a core substrate 20 is placed on the side of the precursor laminate 51 opposite the side having the release layer. This allows a laminate 52 to be obtained.

[0098] Details of the core substrate and the curable resin Y are as described above.

[0099] In this step, for example, the decorative sheet is immersed in a curable resin composition containing curable resin Y. After immersion, it is preferable to dry the sheet. At this time, the curable resin may be partially cured to give a semi-cured state.

[0100] The curable resin composition is a curable resin composition containing a curable resin Y. The proportion of the curable resin Y in the curable resin composition is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more. The curable resin composition may contain water, alcohol, an organic solvent, or the like as a solvent.

[0101] Examples of the release film include films containing polyester resins such as polyethylene terephthalate and polybutylene terephthalate, polyolefin resins such as polyethylene and polypropylene, acrylic resins, etc. The release film may also have a release layer containing a cured product of the ionizing radiation-curable resin composition on the surface facing the curable resin layer.

[0102] Another method for forming the laminate in this step is, for example, to place a core substrate opposite the porous substrate of the decorative sheet, and while impregnating the core substrate and porous substrate with curable resin Y, form a curable resin layer that covers the design layer and release layer and contains curable resin Y. Then, a release film 40 is placed on the surface on the curable resin layer side. This also allows the production of a laminate.

[0103] 3. Heating and Pressurizing Step This step is a step in which the laminate 52 is heated and pressurized to cure the curable resin Y, thereby forming the cured resin layer 31 from the curable resin layer 30, and obtaining the cured laminate 53.

[0104] The heating temperature is, for example, 90° C. or higher and 160° C. or lower, and the heating time is, for example, 30 seconds or higher and 30 minutes or lower.

[0105] 4. Peeling Step This step involves peeling the release film from the cured laminate 53, thereby removing the cured resin layer 31 arranged in a position overlapping the release layer 3 in the thickness direction, while leaving the cured resin layer 31 arranged between the patterns of the release layer 3. This results in a resin-impregnated decorative board 100 having a porous substrate 1, a design layer 2 arranged on one side of the porous substrate 1, a release layer 3 having a pattern shape arranged on the side of the design layer 2 opposite the porous substrate 1, and a cured resin layer 32 arranged between the patterns of the release layer 3 of the decorative sheet.

[0106] The resin-impregnated decorative board obtained by this method for producing a resin-impregnated decorative board can have the Spc and pure water contact angle of the release layer within the ranges described above in "B. Resin-impregnated decorative board." Therefore, the cured resin layer arranged in a position overlapping the release layer can be easily peeled off, and a resin-impregnated decorative board with a good gloss-matt design between the release layer and the cured resin layer can be produced.

[0107] The present disclosure is not limited to the above-described embodiments. The above-described embodiments are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present disclosure and exhibits similar effects is included within the technical scope of the present disclosure.

[0108] [Example 1] (Preparation of decorative sheet) A paper substrate (basis weight 80 g / m) was used as a porous substrate. 2Titanium base paper for building materials (PM-77P manufactured by KJ Specialty Paper Co., Ltd.) was prepared. The ash content of the paper substrate was measured in accordance with JIS-P8252 and found to be 26%. A design layer (picture layer) with a thickness of 2 μm was partially laminated on the paper substrate so as to create a stone grain design by gravure printing using the printing ink described below. Furthermore, the release layer forming ink 1 described below was laminated on the picture layer in sync with the picture layer, and then an electron beam irradiation of 3 Mrad was performed at an acceleration voltage of 165 kV to form a release layer with a thickness of 2 μm. In this way, a decorative sheet was produced in which a porous substrate, a design layer, and a release layer were laminated in this order.

[0109] <Printing ink> Pigment (azo, quinacridone, carbon black, etc.) 10 parts by weight Casein / acrylic resin 10 parts by weight Water 70 parts by weight Dipropyl glycol 5 parts by weight Isopropyl alcohol 5 parts by weight

[0110] <Ink 1 for forming release layer> Ionizing radiation curable monomer (Aronix M-400, manufactured by Toagosei Co., Ltd.) 48 parts by mass Reactive silicone (X-22-164B, manufactured by Shin-Etsu Chemical Co., Ltd.) 4 parts by mass (6.7 parts by mass per 100 parts by mass of total solids) Silane coupling treated silica (particle size 2 μm) 8 parts by mass (13.3 parts by mass per 100 parts by mass of total solids) Methyl ethyl ketone 40 parts by mass

[0111] (Production of melamine decorative board) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, Nikaledin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The impregnation was carried out so that the ratio of the acrylic resin to the acrylic resin was 100% (when dried), and the resulting mixture was dried to produce an impregnated decorative sheet (precursor laminate).

[0112] The impregnated decorative sheet was produced by impregnating kraft paper with phenolic resin liquid, with a basis weight of 245 g / m 2The impregnated decorative sheet was laminated on a core substrate consisting of three sheets of phenolic resin-impregnated core paper (obtained by impregnating core kraft paper with a liquid uncured resin composition consisting of phenolic resin), and the following release film was further laminated on top of the impregnated decorative sheet so that the peeling layer of the release film was in contact with the printed surface of the impregnated decorative sheet, thereby obtaining a laminate.

[0113] (Preparation of Release Film) A coating liquid containing 100 parts by mass of an ionizing radiation curable monomer (Aronix M-350, manufactured by Toagosei Co., Ltd.), 2 parts by mass of a reactive silicone (X-22-164B, manufactured by Shin-Etsu Chemical Co., Ltd.), 8 parts by mass of silica particles (product name "Sylysia 450", manufactured by Fuji Silysia Chemical Ltd., average particle size: 8.0 μm), and 50 parts by mass of ethyl acetate was applied at a rate of 5 g / m to the readily adhesive surface of a 50 μm-thick PET film (Cosmoshine (registered trademark) A4160, manufactured by Toyobo Co., Ltd.). 2 (when dry) and then cured by irradiating with an electron beam of 5 Mrad at an acceleration voltage of 165 kV to produce a release film having a peeling layer.

[0114] The formed laminate was sandwiched between two mirror-finished plates and subjected to a pressure of 100 kg / cm using a heat press. 2 The uncured melamine resin composition was then heat-molded at a molding temperature of 150°C for 10 minutes to thermally cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured melamine resin, thereby obtaining the melamine decorative board of Example 1. When the release film was peeled off from the cured laminate, the cured resin layer on the release layer was removed along with the release film, leaving the cured resin layer formed in the area without the release layer.

[0115] [Example 2] (Preparation of decorative sheet) A paper substrate (titanium base paper for building materials, PM-77P manufactured by KJ Specialty Paper Co., Ltd.) was prepared as a porous substrate. By gravure printing using the above printing ink, a design layer (pattern layer) having a thickness of 2 μm was partially laminated on the paper substrate so as to form a stone grain pattern design. Furthermore, the following release layer forming ink 2 was laminated on the pattern layer in synchronization with the pattern layer, and then an electron beam irradiation of 3 Mrad was performed at an acceleration voltage of 165 kV to form a release layer having a thickness of 2 μm. In this way, a decorative sheet was produced in which a porous substrate, a design layer, and a release layer were laminated in this order.

[0116] <Ink 2 for forming release layer> Ionizing radiation curable monomer (Aronix M-400, manufactured by Toagosei Co., Ltd.) 50.6 parts by mass Reactive silicone (X-22-164B, manufactured by Shin-Etsu Chemical Co., Ltd.) 4 parts by mass (6.7 parts by mass per 100 parts by mass of total solids) Silane coupling treated silica (particle size 2 μm) 5.4 parts by mass (9.0 parts by mass per 100 parts by mass of total solids) Methyl ethyl ketone 40 parts by mass

[0117] (Production of melamine decorative board) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, Nikaledin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The impregnation was carried out so that the ratio of the acrylic resin to the acrylic resin was 100% (when dried), and the resulting mixture was dried to produce an impregnated decorative sheet (precursor laminate).

[0118] The impregnated decorative sheet was laminated on the above core substrate, and the above release film was further laminated on the impregnated decorative sheet so that the peel layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.

[0119] The formed laminate was sandwiched between two mirror-finished plates and subjected to a pressure of 100 kg / cm using a heat press. 2The uncured melamine resin composition was then heat-molded at a molding temperature of 150°C for 10 minutes to thermally cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured melamine resin, yielding the melamine decorative board of Example 2.

[0120] [Example 3] (Preparation of decorative sheet) A paper substrate (titanium base paper for building materials, PM-77P manufactured by KJ Specialty Paper Co., Ltd.) was prepared as a porous substrate. By gravure printing using the above printing ink, a design layer (picture layer) having a thickness of 2 μm was partially laminated on the paper substrate so as to form a stone grain pattern design. Furthermore, the following release layer forming ink 3 was laminated on the picture layer in synchronization with the picture layer, and then an electron beam irradiation of 3 Mrad was performed at an acceleration voltage of 165 kV to form a release layer having a thickness of 2 μm. In this way, a decorative sheet was produced in which a porous substrate, a design layer, and a release layer were laminated in this order.

[0121] <Ink 3 for forming release layer> Ionizing radiation curable monomer (Aronix M-400, manufactured by Toagosei Co., Ltd.) 45.4 parts by mass Reactive silicone (X-22-164B, manufactured by Shin-Etsu Chemical Co., Ltd.) 4 parts by mass (6.7 parts by mass per 100 parts by mass of total solids) Silane coupling treated silica (particle size 2 μm) 10.6 parts by mass (17.7 parts by mass per 100 parts by mass of total solids) Methyl ethyl ketone 40 parts by mass

[0122] (Production of melamine decorative board) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, Nikaledin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The impregnation was carried out so that the ratio of the acrylic resin to the acrylic resin was 100% (when dried), and the resulting mixture was dried to produce an impregnated decorative sheet (precursor laminate).

[0123] The impregnated decorative sheet was laminated on the above core substrate, and the above release film was further laminated on the impregnated decorative sheet so that the peel layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.

[0124] The formed laminate was sandwiched between two mirror-finished plates and subjected to a pressure of 100 kg / cm using a heat press. 2 The uncured melamine resin composition was then heat-molded at a molding temperature of 150°C for 10 minutes to thermally cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured melamine resin, yielding the melamine decorative board of Example 3.

[0125] [Example 4] (Preparation of decorative sheet) A paper substrate (titanium base paper for building materials, PM-77P manufactured by KJ Specialty Paper Co., Ltd.) was prepared as a porous substrate. By gravure printing using the above printing ink, a design layer (picture layer) having a thickness of 2 μm was partially laminated on the paper substrate so as to form a stone grain pattern design. Furthermore, the following release layer forming ink 4 was laminated on the picture layer in synchronization with the picture layer, and then an electron beam irradiation of 3 Mrad was performed at an acceleration voltage of 165 kV to form a release layer having a thickness of 2 μm. In this way, a decorative sheet was produced in which a porous substrate, a design layer, and a release layer were laminated in this order.

[0126] <Ink 4 for forming release layer> Ionizing radiation curable monomer (Aronix M-400, manufactured by Toagosei Co., Ltd.) 50.6 parts by mass Reactive silicone (X-22-164B, manufactured by Shin-Etsu Chemical Co., Ltd.) 1.4 parts by mass (2.3 parts by mass per 100 parts by mass of total solids) Silane coupling treated silica (particle size 2 μm) 8 parts by mass (13.3 parts by mass per 100 parts by mass of total solids) Methyl ethyl ketone 40 parts by mass

[0127] (Production of melamine decorative board) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, Nikaledin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The impregnation was carried out so that the ratio of the acrylic resin to the acrylic resin was 100% (when dried), and the resulting mixture was dried to produce an impregnated decorative sheet (precursor laminate).

[0128] The impregnated decorative sheet was laminated on the above core substrate, and the above release film was further laminated on the impregnated decorative sheet so that the peel layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.

[0129] The formed laminate was sandwiched between two mirror-finished plates and subjected to a pressure of 100 kg / cm using a heat press. 2 The uncured melamine resin composition was then heat-molded at a molding temperature of 150°C for 10 minutes to thermally cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured melamine resin, yielding the melamine decorative board of Example 4.

[0130] [Example 5] (Preparation of decorative sheet) A paper substrate (titanium base paper for building materials, PM-77P manufactured by KJ Specialty Paper Co., Ltd.) was prepared as a porous substrate. By gravure printing using the above printing ink, a design layer (pattern layer) having a thickness of 2 μm was partially laminated on the paper substrate so as to form a stone grain pattern design. Furthermore, the following release layer forming ink 5 was laminated on the pattern layer in synchronization with the pattern layer, and then an electron beam irradiation of 3 Mrad was performed at an acceleration voltage of 165 kV to form a release layer having a thickness of 2 μm. In this way, a decorative sheet was produced in which a porous substrate, a design layer, and a release layer were laminated in this order.

[0131] <Ink 5 for forming release layer> Ionizing radiation curable monomer (Aronix M-400, manufactured by Toagosei Co., Ltd.) 46.6 parts by mass Reactive silicone (X-22-164B, manufactured by Shin-Etsu Chemical Co., Ltd.) 5.4 parts by mass (9.0 parts by mass per 100 parts by mass of total solids) Silane coupling treated silica (particle size 2 μm) 8 parts by mass (13.3 parts by mass per 100 parts by mass of total solids) Methyl ethyl ketone 40 parts by mass

[0132] (Production of melamine decorative board) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, Nikaledin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The impregnation was carried out so that the ratio of the acrylic resin to the acrylic resin was 100% (when dried), and the resulting mixture was dried to produce an impregnated decorative sheet (precursor laminate).

[0133] The impregnated decorative sheet was laminated on the above core substrate, and the above release film was further laminated on the impregnated decorative sheet so that the peel layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.

[0134] The formed laminate was sandwiched between two mirror-finished plates and subjected to a pressure of 100 kg / cm using a heat press. 2 The uncured melamine resin composition was then heat-molded at a molding temperature of 150°C for 10 minutes to thermally cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured melamine resin, yielding the melamine decorative board of Example 5.

[0135] [Example 6] (Preparation of decorative sheet) A paper substrate (titanium base paper for building materials, PM-77P manufactured by KJ Specialty Paper Co., Ltd.) was prepared as a porous substrate. By gravure printing using the above printing ink, a design layer (pattern layer) having a thickness of 2 μm was partially laminated on the paper substrate so as to form a stone grain pattern design. Furthermore, the following release layer forming ink 6 was laminated on the pattern layer in synchronization with the pattern layer, and then an electron beam of 3 Mrad was irradiated at an acceleration voltage of 165 kV to form a release layer having a thickness of 2 μm. In this way, a decorative sheet was produced in which a porous substrate, a design layer, and a release layer were laminated in this order.

[0136] <Ink 6 for forming release layer> Ionizing radiation curable monomer (Aronix M-400, manufactured by Toagosei Co., Ltd.) 50.6 parts by mass Reactive silicone (X-22-164B, manufactured by Shin-Etsu Chemical Co., Ltd.) 4 parts by mass (6.7 parts by mass per 100 parts by mass of total solids) Silane coupling treated silica (particle size 5 μm) 5.4 parts by mass (9.0 parts by mass per 100 parts by mass of total solids) Methyl ethyl ketone 40 parts by mass

[0137] (Production of melamine decorative board) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, Nikaledin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The impregnation was carried out so that the ratio of the acrylic resin to the acrylic resin was 100% (when dried), and the resulting mixture was dried to produce an impregnated decorative sheet (precursor laminate).

[0138] The impregnated decorative sheet was laminated on the above core substrate, and the above release film was further laminated on the impregnated decorative sheet so that the peel layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.

[0139] The formed laminate was sandwiched between two mirror-finished plates and subjected to a pressure of 100 kg / cm using a heat press. 2The uncured melamine resin composition was then heat-molded at a molding temperature of 150°C for 10 minutes to thermally cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured melamine resin, yielding the melamine decorative board of Example 6.

[0140] [Example 7] (Preparation of decorative sheet) A paper substrate (titanium base paper for building materials, PM-77P manufactured by KJ Specialty Paper Co., Ltd.) was prepared as a porous substrate. By gravure printing using the above printing ink, a design layer (picture layer) having a thickness of 2 μm was partially laminated on the paper substrate so as to form a stone grain pattern design. Furthermore, the following release layer forming ink 7 was laminated on the picture layer in synchronization with the picture layer, and then an electron beam irradiation of 3 Mrad was performed at an acceleration voltage of 165 kV to form a release layer having a thickness of 2 μm. In this way, a decorative sheet was produced in which a porous substrate, a design layer, and a release layer were laminated in this order.

[0141] <Ink 7 for forming release layer> Ionizing radiation curable monomer (Aronix M-400, manufactured by Toagosei Co., Ltd.) 45.4 parts by mass Reactive silicone (X-22-164B, manufactured by Shin-Etsu Chemical Co., Ltd.) 4 parts by mass (6.7 parts by mass per 100 parts by mass of total solids) Silane coupling treated silica (particle size 1 μm) 10.6 parts by mass (17.7 parts by mass per 100 parts by mass of total solids) Methyl ethyl ketone 40 parts by mass

[0142] (Production of melamine decorative board) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, Nikaledin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The impregnation was carried out so that the ratio of the acrylic resin to the acrylic resin was 100% (when dried), and the resulting mixture was dried to produce an impregnated decorative sheet (precursor laminate).

[0143] The impregnated decorative sheet was laminated on the above core substrate, and the above release film was further laminated on the impregnated decorative sheet so that the peel layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.

[0144] The formed laminate was sandwiched between two mirror-finished plates and subjected to a pressure of 100 kg / cm using a heat press. 2 The uncured melamine resin composition was then heat-molded at a molding temperature of 150°C for 10 minutes to thermally cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured melamine resin, yielding the melamine decorative board of Example 7.

[0145] [Example 8] (Preparation of decorative sheet) A paper substrate (titanium base paper for building materials, PM-77P manufactured by KJ Specialty Paper Co., Ltd.) was prepared as a porous substrate. By gravure printing using the above printing ink, a design layer (pattern layer) having a thickness of 2 μm was partially laminated on the paper substrate so as to form a stone grain pattern design. Furthermore, the following release layer forming ink 8 was laminated on the pattern layer in synchronization with the previously formed pattern layer, and then irradiated with an electron beam of 3 Mrad at an acceleration voltage of 165 kV to form a release layer having a thickness of 6 μm. In this way, a decorative sheet was produced in which a porous substrate, a design layer, and a release layer were laminated in this order.

[0146] <Ink 8 for forming release layer> Ionizing radiation curable monomer (Aronix M-400, manufactured by Toagosei Co., Ltd.) 45.4 parts by mass Reactive silicone (X-22-164B, manufactured by Shin-Etsu Chemical Co., Ltd.) 4 parts by mass (6.7 parts by mass per 100 parts by mass of total solids) Silane coupling treated silica (particle size 2 μm) 10.6 parts by mass (17.7 parts by mass per 100 parts by mass of total solids) Methyl ethyl ketone 40 parts by mass

[0147] (Production of melamine decorative board) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, Nikaledin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The impregnation was carried out so that the ratio of the acrylic resin to the acrylic resin was 100% (when dried), and the resulting mixture was dried to produce an impregnated decorative sheet (precursor laminate).

[0148] The impregnated decorative sheet was laminated on the above core substrate, and the above release film was further laminated on the impregnated decorative sheet so that the peel layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.

[0149] The formed laminate was sandwiched between two mirror-finished plates and subjected to a pressure of 100 kg / cm using a heat press. 2 The uncured melamine resin composition was then heat-molded at a molding temperature of 150°C for 10 minutes to thermally cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured melamine resin, yielding the melamine decorative board of Example 8.

[0150] [Comparative Example 1] (Preparation of decorative sheet) A paper substrate (titanium base paper for building materials, PM-77P manufactured by KJ Specialty Paper Co., Ltd.) was prepared as a porous substrate. By gravure printing using the above printing ink, a design layer (pattern layer) having a thickness of 2 μm was partially laminated on the paper substrate so as to form a stone grain pattern design. Furthermore, the following release layer forming ink 9 was laminated on the pattern layer in synchronization with the pattern layer, and then an electron beam irradiation of 3 Mrad was performed at an acceleration voltage of 165 kV to form a release layer having a thickness of 2 μm. In this way, a decorative sheet was produced in which a porous substrate, a design layer, and a release layer were laminated in this order.

[0151] <Ink 9 for forming release layer> Ionizing radiation curable monomer (Aronix M-400, manufactured by Toagosei Co., Ltd.) 53.4 parts by mass Reactive silicone (X-22-164B, manufactured by Shin-Etsu Chemical Co., Ltd.) 4 parts by mass (6.7 parts by mass per 100 parts by mass of total solids) Silane coupling treated silica (particle size 2 μm) 2.6 parts by mass (4.3 parts by mass per 100 parts by mass of total solids) Methyl ethyl ketone 40 parts by mass

[0152] (Production of melamine decorative board) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, Nikaledin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The impregnation was carried out so that the ratio of the acrylic resin to the acrylic resin was 100% (when dried), and the resulting mixture was dried to produce an impregnated decorative sheet (precursor laminate).

[0153] The impregnated decorative sheet was laminated on the above core substrate, and the above release film was further laminated on the impregnated decorative sheet so that the peel layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.

[0154] The formed laminate was sandwiched between two mirror-finished plates and subjected to a pressure of 100 kg / cm using a heat press. 2 The uncured melamine resin composition was heat-molded at a molding temperature of 150°C for 10 minutes to thermally cure the composition, thereby forming a cured resin layer containing a cured melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured melamine resin, yielding the melamine decorative board of Comparative Example 1.

[0155] [Comparative Example 2] (Preparation of decorative sheet) A paper substrate (titanium base paper for building materials, PM-77P manufactured by KJ Specialty Paper Co., Ltd.) was prepared as a porous substrate. By gravure printing using the above printing ink, a design layer (picture layer) having a thickness of 2 μm was partially laminated on the paper substrate so as to form a stone grain pattern design. Furthermore, the following release layer forming ink 10 was laminated on the picture layer in synchronization with the picture layer, and then an electron beam irradiation of 3 Mrad was performed at an acceleration voltage of 165 kV to form a release layer having a thickness of 2 μm. In this way, a decorative sheet was produced in which the paper substrate, design layer, and release layer were laminated in this order.

[0156] <Ink 10 for forming release layer> Ionizing radiation curable monomer (Aronix M-400, manufactured by Toagosei Co., Ltd.) 51.4 parts by mass Reactive silicone (X-22-164B, manufactured by Shin-Etsu Chemical Co., Ltd.) 0.6 parts by mass (1.0 part by mass per 100 parts by mass of total solids) Silane coupling treated silica (particle size 2 μm) 8.0 parts by mass (13.3 parts by mass per 100 parts by mass of total solids) Methyl ethyl ketone 40 parts by mass

[0157] (Production of melamine decorative board) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, Nikaledin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The impregnation was carried out so that the ratio of the acrylic resin to the acrylic resin was 100% (when dried), and the resulting mixture was dried to produce an impregnated decorative sheet (precursor laminate).

[0158] The impregnated decorative sheet was laminated on the above core substrate, and the above release film was further laminated on the impregnated decorative sheet so that the peel layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.

[0159] The formed laminate was sandwiched between two mirror-finished plates and subjected to a pressure of 100 kg / cm using a heat press. 2The uncured melamine resin composition was then heat-molded at a molding temperature of 150°C for 10 minutes to thermally cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured melamine resin, yielding the melamine decorative board of Comparative Example 2.

[0160] [Comparative Example 3] (Preparation of decorative sheet) A paper substrate (titanium base paper for building materials, PM-77P manufactured by KJ Specialty Paper Co., Ltd.) was prepared as a porous substrate. By gravure printing using the above printing ink, a design layer (picture layer) having a thickness of 2 μm was partially laminated on the paper substrate so as to form a stone grain pattern design. Furthermore, the following release layer forming ink 11 was laminated on the picture layer in synchronization with the picture layer, and then an electron beam irradiation of 3 Mrad was performed at an acceleration voltage of 165 kV to form a release layer having a thickness of 2 μm. In this way, a decorative sheet was produced in which the paper substrate, design layer, and release layer were laminated in this order.

[0161] <Ink 11 for forming release layer> Ionizing radiation curable monomer (Aronix M-400, manufactured by Toagosei Co., Ltd.) 48 parts by mass Reactive silicone (X-22-164B, manufactured by Shin-Etsu Chemical Co., Ltd.) 4 parts by mass (6.7 parts by mass per 100 parts by mass of total solids) Silane coupling treated silica (particle size 5 μm) 8 parts by mass (13.3 parts by mass per 100 parts by mass of total solids) Methyl ethyl ketone 40 parts by mass

[0162] (Production of melamine decorative board) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, Nikaledin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The impregnated decorative sheet was produced by impregnating the sheet with the resin to a ratio of 1:1 (when dry) and then drying.

[0163] The impregnated decorative sheet was laminated on the above core substrate, and the above release film was further laminated on the impregnated decorative sheet so that the peel layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.

[0164] The formed laminate was sandwiched between two mirror-finished plates and subjected to a pressure of 100 kg / cm using a heat press. 2 The uncured melamine resin composition was then heat-molded at a molding temperature of 150°C for 10 minutes to thermally cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured melamine resin, yielding the melamine decorative board of Comparative Example 3.

[0165] [Comparative Example 4] (Preparation of decorative sheet) A paper substrate (titanium base paper for building materials, PM-77P manufactured by KJ Specialty Paper Co., Ltd.) was prepared as a porous substrate. By gravure printing using the above printing ink, a design layer (pattern layer) having a thickness of 2 μm was partially laminated on the paper substrate so as to form a stone grain pattern design. Furthermore, the following release layer forming ink 12 was laminated on the pattern layer in synchronization with the pattern layer, and then an electron beam irradiation of 3 Mrad was performed at an acceleration voltage of 165 kV to form a release layer having a thickness of 2 μm. In this way, a decorative sheet was produced in which a porous substrate, a design layer, and a release layer were laminated in this order.

[0166] <Ink 12 for forming release layer> Ionizing radiation curable monomer (Aronix M-400, manufactured by Toagosei Co., Ltd.) 48 parts by mass Reactive silicone (X-22-164B, manufactured by Shin-Etsu Chemical Co., Ltd.) 4 parts by mass (6.7 parts by mass per 100 parts by mass of total solids) Silane coupling treated silica (particle size 1 μm) 8 parts by mass (13.3 parts by mass per 100 parts by mass of total solids) Methyl ethyl ketone 40 parts by mass

[0167] (Production of melamine decorative board) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, Nikaledin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The impregnated decorative sheet was produced by impregnating the sheet with the resin to a ratio of 1:1 (when dry) and then drying.

[0168] The impregnated decorative sheet was laminated on the above core substrate, and the above release film was further laminated on the impregnated decorative sheet so that the peel layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.

[0169] The formed laminate was sandwiched between two mirror-finished plates and subjected to a pressure of 100 kg / cm using a heat press. 2 The uncured melamine resin composition was then heat-molded at a molding temperature of 150°C for 10 minutes to thermally cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured melamine resin, yielding the melamine decorative board of Comparative Example 4.

[0170] [Comparative Example 5] (Preparation of decorative sheet) A paper substrate (titanium base paper for building materials, PM-77P manufactured by KJ Specialty Paper Co., Ltd.) was prepared as a porous substrate. By gravure printing using the above printing ink, a design layer (picture layer) having a thickness of 2 μm was partially laminated on the paper substrate so as to form a stone grain pattern design. Furthermore, release layer forming ink 1 was laminated on the picture layer in synchronization with the previously formed picture layer, and then an electron beam irradiation of 3 Mrad was performed at an acceleration voltage of 165 kV to form a release layer having a thickness of 6 μm. In this way, a decorative sheet was produced in which the paper substrate, design layer, and release layer were laminated in this order.

[0171] (Production of melamine decorative board) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, Nikaledin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The impregnated decorative sheet was produced by impregnating the sheet with the resin to a ratio of 1:1 (when dry) and then drying.

[0172] The impregnated decorative sheet was laminated on the above core substrate, and the above release film was further laminated on the impregnated decorative sheet so that the peel layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.

[0173] The formed laminate was sandwiched between two mirror-finished plates and subjected to a pressure of 100 kg / cm using a heat press. 2 The uncured melamine resin composition was then heat-molded at a molding temperature of 150°C for 10 minutes to thermally cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured melamine resin, yielding the melamine decorative board of Comparative Example 5.

[0174] [Pure Water Contact Angle of Release Layer of Decorative Sheet] The pure water contact angle of the release layer of the decorative sheets obtained in Examples 1 to 8 and Comparative Examples 1 to 5 was measured by the following method. The decorative sheet was placed on a horizontal surface with the release layer facing up. Next, a water droplet (pure water, 2.0 μL) was dropped onto the release layer from a direction perpendicular to the horizontal surface. At this time, the water droplet was not dropped at the boundary between the design layer and the release layer, but was dropped so that the entire water droplet came into contact with the release layer. After dropping the water droplet, a one-second wait was held, and the contact angle between the release layer and pure water was measured using a contact angle meter (fully automatic contact angle meter DMo-702, manufactured by Kyowa Interface Science Co., Ltd.). The above measurement was performed at 10 random locations, and the average value was taken as the pure water contact angle. The results are shown in Tables 1 and 2. The pure water contact angle of the release layer of a resin-impregnated decorative board can basically be measured using the same method as above, but when dropping water droplets onto the release layer, the water droplets are not dropped at the boundary between the cured resin layer and the release layer, but are dropped so that the entire water droplet comes into contact with the release layer.

[0175] [60° Gloss Value of Release Layer of Decorative Sheet] The 60° gloss value of the release layer in the decorative sheets obtained in Examples 1 to 8 and Comparative Examples 1 to 5 was measured by the following method. The decorative sheet was placed with the release layer side facing up, and the 60° specular gloss was measured from the release layer side using a gloss meter (Micro Trigloss (Cat. No. 4563) manufactured by BYK Gardner) in accordance with Method 3 of JIS Z 8741:1997 as follows. 1) Paper (Tencolor <400> A4 black manufactured by Oji F-Tex) was prepared and cut into a size of 180 mm x 60 mm as shown in Figure 6(a). 2) A gloss meter was placed on the cut-out paper, and an impression of the gloss meter was made with a pencil (dotted frame in Figure 6(b)). 3) A 15 mm x 9 mm hole C was cut out in the center as shown in Figure 6(c), to prepare a backing plate 61. 4) The prepared backing plate was placed on the measurement sample, and the cutout portion (hole C) was visually inspected to confirm that the release layer was in the center and that the ratio of the area of ​​the release layer to the area of ​​the cutout portion (hole C) was 50% or more. 5) Carefully positioning the backing plate as set in 4), the gloss meter was placed in line with the molded portion, and the 60° gloss was measured. 6) The operations 4) and 5) were repeated, increasing the number of samples, and the average value of the measurements at 10 locations was taken as the 60° gloss value of the release layer. The results are shown in Tables 1 and 2.

[0176] [Spc of release layer of decorative sheet and melamine decorative board] The Spc (arithmetic mean curvature of peaks) of the release layer of the decorative sheets and melamine decorative boards obtained in Examples 1 to 8 and Comparative Examples 1 to 5 was measured by the following method. The value was measured on the surface of the release layer of the decorative sheet using a laser microscope (VK-X3000, manufactured by Keyence Corporation) under the following conditions. Note that Spc is the average value of measurements taken at 10 arbitrary points, with measurement points selected so that all of the measurement points fall within the release layer. The results are shown in Tables 1 and 2. (Measurement conditions) Objective lens: 5x Laser wavelength: 661 nm Measurement area at each point: 500 μm × 500 μm

[0177] [Melamine Peelability Evaluation] Using the melamine decorative boards obtained in Examples 1 to 8 and Comparative Examples 1 to 5, a Scotch tape resistance test was conducted on the area containing the release layer, and melamine peelability was evaluated according to the following evaluation criteria. The results are shown in Tables 1 and 2. (Scotch tape resistance test method) 1) Nichiban Scotch tape (registered trademark) (No. 405 (industrial use), 24 mm wide) was pulled out 15 to 30 cm, and except for the end 5 cm, the adhesive surfaces of the remaining sections were bonded together (this area serves as a grip for peeling). 2) The adhesive surface of the edge was attached to the test area and rubbed from above with a cloth or similar to ensure strong adhesion. 3) The area where the adhesive cotton was bonded together in 1) was gripped and pulled forcefully in a 45-degree direction. 4) The melamine layer of the adhesive area and the surface of the test area were visually inspected and rated according to the A, B, and C criteria. 5) 1) to 4) were performed on 10 random locations on the release layer, and the most common evaluation was judged as the melamine release property (in the case of the same number of evaluations, the worst result was used).

[0178] (Evaluation criteria) A: Almost no peeling of melamine is observed, and no melamine remains on the release layer. B: Significant peeling of melamine is observed, but it can be peeled off by testing. C: No peeling of melamine is observed, and melamine remains on most of the release layer even after testing. (Most of the melamine on the release layer (more than 90% of the area of ​​the release layer) cannot be peeled off by testing.)

[0179] [Evaluation of Gloss Matte Design] The gloss matte design of the melamine decorative boards obtained in Examples 1 to 8 and Comparative Examples 1 to 5 was evaluated visually. Specifically, under a light source of a natural color fluorescent lamp color rendering AA (manufactured by Panasonic Corporation, model number: FLR40S·D-SDL / M), the obtained decorative boards were each visually observed from a position 50 cm away, and the gloss matte design and the state of the matte portion (release layer) were confirmed.

[0180] The observers scored the gloss matte design on a scale of 1 to 5 (1 being the worst and 5 being the best). The scale was rated as follows: 1 point if most of the melamine remained peeled or significant whitening was observed in the matte area and surrounding areas, and a sufficient gloss matte design could not be confirmed; 5 points if no peeled melamine was found in the matte area and a sufficient gloss matte design could be confirmed. Ten observers each conducted the test, and the average score was calculated to evaluate the gloss matte design according to the following criteria. The results are shown in Tables 1 and 2. (Evaluation criteria) A: The average score when evaluating the gloss matte design was 3 points or more B: The average score when evaluating the gloss matte design was 2 points or more but less than 3 points C: The average score when evaluating the gloss matte design was less than 2 points

[0181]

[0182]

[0183] As shown in Table 1, when the decorative sheets obtained in Examples 1 to 8 were used, the results were excellent in both melamine releasability and gloss matte design. On the other hand, as shown in Table 2, the decorative sheet obtained in Comparative Example 1 had a high 60° gloss value and a low Spc value, and was therefore confirmed to have poor gloss matte design. Furthermore, the decorative sheets obtained in Comparative Examples 2 and 3 had low pure water contact angles and were confirmed to have poor melamine releasability. The decorative sheets obtained in Comparative Examples 4 and 5 were confirmed to have poor gloss matte design due to their low Spc.

[0184] [Example 9] (Preparation of decorative sheet) A paper substrate (basis weight 80 g / m) was used as a porous substrate. 2Titanium base paper for building materials (PM-83P manufactured by KJ Specialty Paper Co., Ltd.) was prepared. The ash content of the paper substrate was measured in accordance with JIS-P8252 and found to be 18%. A design layer (picture layer) with a thickness of 2 μm was partially laminated on the paper substrate by gravure printing using the above printing ink to form a stone grain pattern. Furthermore, release layer forming ink 1 was laminated on the picture layer in sync with the picture layer, and then electron beam irradiation of 3 Mrad was performed at an acceleration voltage of 165 kV to form a release layer with a thickness of 2 μm. In this way, a decorative sheet was produced in which a porous substrate, a design layer, and a release layer were laminated in this order.

[0185] (Production of melamine decorative board) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, Nikaledin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The impregnation was carried out so that the ratio of the acrylic resin to the acrylic resin was 100% (when dried), and the resulting mixture was dried to produce an impregnated decorative sheet (precursor laminate).

[0186] The impregnated decorative sheet was laminated on the above core substrate, and the above release film was further laminated on the impregnated decorative sheet so that the peel layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.

[0187] The formed laminate was sandwiched between two mirror-finished plates and subjected to a pressure of 100 kg / cm using a heat press. 2 The uncured melamine resin composition was then heat-molded at a molding temperature of 150°C for 10 minutes to thermally cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured melamine resin, yielding the melamine decorative board of Example 9.

[0188] [Example 10] (Preparation of decorative sheet) A paper substrate (titanium base paper for building materials, PM-83P manufactured by KJ Specialty Paper Co., Ltd.) was prepared as a porous substrate. By gravure printing using the above printing ink, a design layer (pattern layer) having a thickness of 2 μm was partially laminated on the paper substrate so as to form a stone grain pattern design. Furthermore, release layer forming ink 3 was laminated on the pattern layer in synchronization with the pattern layer, and then an electron beam irradiation of 3 Mrad was performed at an acceleration voltage of 165 kV to form a release layer having a thickness of 2 μm. In this way, a decorative sheet was produced in which a porous substrate, a design layer, and a release layer were laminated in this order.

[0189] (Production of melamine decorative board) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, Nikaledin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The impregnation was carried out so that the ratio of the acrylic resin to the acrylic resin was 100% (when dried), and the resulting mixture was dried to produce an impregnated decorative sheet (precursor laminate).

[0190] The impregnated decorative sheet was laminated on the above core substrate, and the above release film was further laminated on the impregnated decorative sheet so that the peel layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.

[0191] The formed laminate was sandwiched between two mirror-finished plates and subjected to a pressure of 100 kg / cm using a heat press. 2 The uncured melamine resin composition was then heat-molded at a molding temperature of 150°C for 10 minutes to thermally cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured melamine resin, yielding the melamine decorative board of Example 10.

[0192] [Example 11] (Preparation of decorative sheet) A paper substrate (titanium base paper for building materials, PM-77P manufactured by KJ Specialty Paper Co., Ltd.) was prepared as a porous substrate. By gravure printing using the above printing ink, a design layer (pattern layer) having a thickness of 2 μm was partially laminated on the paper substrate so as to form a stone grain pattern design. Furthermore, the following release layer forming ink 13 was laminated on the pattern layer in synchronization with the pattern layer, and then irradiated with an electron beam of 3 Mrad at an acceleration voltage of 165 kV to form a release layer having a thickness of 2 μm. In this way, a decorative sheet was produced in which a porous substrate, a design layer, and a release layer were laminated in this order.

[0193] <Ink 13 for forming release layer> Ionizing radiation curable monomer (Aronix M-400, manufactured by Toagosei Co., Ltd.) 46.8 parts by mass Reactive silicone (X-22-164B, manufactured by Shin-Etsu Chemical Co., Ltd.) 4 parts by mass (6.7 parts by mass per 100 parts by mass of total solids) Silane coupling treated silica (particle size 2 μm) 8 parts by mass (13.3 parts by mass per 100 parts by mass of total solids) Hindered amine light stabilizer (Tinuvin 123, manufactured by BASF Corporation) 1.2 parts by mass (2.0 parts by mass per 100 parts by mass of total solids) Methyl ethyl ketone 40 parts by mass

[0194] (Production of melamine decorative board) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, Nikaledin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The impregnation was carried out so that the ratio of the acrylic resin to the acrylic resin was 100% (when dried), and the resulting mixture was dried to produce an impregnated decorative sheet (precursor laminate).

[0195] The impregnated decorative sheet was laminated on the above core substrate, and the above release film was further laminated on the impregnated decorative sheet so that the peel layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.

[0196] The formed laminate was sandwiched between two mirror-finished plates and subjected to a pressure of 100 kg / cm using a heat press. 2The uncured melamine resin composition was then heat-molded at a molding temperature of 150°C for 10 minutes to thermally cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured melamine resin, yielding the melamine decorative board of Example 11.

[0197] [Example 12] (Preparation of decorative sheet) A paper substrate (titanium base paper for building materials, PM-77P manufactured by KJ Specialty Paper Co., Ltd.) was prepared as a porous substrate. By gravure printing using the above printing ink, a design layer (pattern layer) having a thickness of 2 μm was partially laminated on the paper substrate so as to form a stone grain pattern design. Furthermore, the following release layer forming ink 14 was laminated on the pattern layer in synchronization with the pattern layer, and then an electron beam irradiation of 3 Mrad was performed at an acceleration voltage of 165 kV to form a release layer having a thickness of 2 μm. In this way, a decorative sheet was produced in which a porous substrate, a design layer, and a release layer were laminated in this order.

[0198] <Ink 14 for forming release layer> Ionizing radiation curable monomer (Aronix M-400, manufactured by Toagosei Co., Ltd.) 45 parts by mass Reactive silicone (X-22-164B, manufactured by Shin-Etsu Chemical Co., Ltd.) 4 parts by mass (6.7 parts by mass per 100 parts by mass of total solids) Silane coupling treated silica (particle size 2 μm) 8 parts by mass (13.3 parts by mass per 100 parts by mass of total solids) Hindered amine light stabilizer (Tinuvin 123, manufactured by BASF Corporation) 3 parts by mass (5.0 parts by mass per 100 parts by mass of total solids) Methyl ethyl ketone 40 parts by mass

[0199] (Production of melamine decorative board) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, Nikaledin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The impregnation was carried out so that the ratio of the acrylic resin to the acrylic resin was 100% (when dried), and the resulting mixture was dried to produce an impregnated decorative sheet (precursor laminate).

[0200] The impregnated decorative sheet was laminated on the above core substrate, and the above release film was further laminated on the impregnated decorative sheet so that the peel layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.

[0201] The formed laminate was sandwiched between two mirror-finished plates and subjected to a pressure of 100 kg / cm using a heat press. 2 The uncured melamine resin composition was then heat-molded at a molding temperature of 150°C for 10 minutes to thermally cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured melamine resin, yielding the melamine decorative board of Example 12.

[0202] [Example 13] (Preparation of decorative sheet) A paper substrate (titanium base paper for building materials, PM-77P manufactured by KJ Specialty Paper Co., Ltd.) was prepared as a porous substrate. By gravure printing using the above printing ink, a design layer (pattern layer) having a thickness of 2 μm was partially laminated on the paper substrate so as to form a stone grain pattern design. Furthermore, the following release layer forming ink 15 was laminated on the pattern layer in synchronization with the pattern layer, and then an electron beam of 3 Mrad was irradiated at an acceleration voltage of 165 kV to form a release layer having a thickness of 2 μm. In this way, a decorative sheet was produced in which a porous substrate, a design layer, and a release layer were laminated in this order.

[0203] <Ink 15 for forming release layer> Ionizing radiation curable monomer (Aronix M-400, manufactured by Toagosei Co., Ltd.) 44 parts by mass Reactive silicone (X-22-164B, manufactured by Shin-Etsu Chemical Co., Ltd.) 4 parts by mass (6.7 parts by mass per 100 parts by mass of total solids) Silane coupling treated silica (particle size 2 μm) 9 parts by mass (15.0 parts by mass per 100 parts by mass of total solids) Hindered amine light stabilizer (Tinuvin 123, manufactured by BASF Corporation) 3 parts by mass (5.0 parts by mass per 100 parts by mass of total solids) Methyl ethyl ketone 40 parts by mass

[0204] (Production of melamine decorative board) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, Nikaledin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The impregnation was carried out so that the ratio of the acrylic resin to the acrylic resin was 100% (when dried), and the resulting mixture was dried to produce an impregnated decorative sheet (precursor laminate).

[0205] The impregnated decorative sheet was laminated on the above core substrate, and the above release film was further laminated on the impregnated decorative sheet so that the peel layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.

[0206] The formed laminate was sandwiched between two mirror-finished plates and subjected to a pressure of 100 kg / cm using a heat press. 2 The uncured melamine resin composition was then heat-molded at a molding temperature of 150°C for 10 minutes to thermally cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured melamine resin, yielding the melamine decorative board of Example 13.

[0207] [Comparative Example 6] (Preparation of decorative sheet) As a porous substrate, a paper substrate (basis weight 100 g / m 2 Titanium paper (KW-1002P manufactured by KJ Specialty Paper Co., Ltd.) was prepared. The ash content of the paper substrate was measured in accordance with JIS-P8252 and found to be 36%. A 2 μm-thick design layer (picture layer) was partially laminated on the paper substrate by gravure printing using the above printing ink to create a stone-grain design. Furthermore, release layer-forming ink 1 was laminated on the picture layer in sync with the picture layer, and then electron beam irradiation of 3 Mrad was performed at an acceleration voltage of 165 kV to form a 2 μm-thick release layer. This produced a decorative sheet in which a porous substrate, a design layer, and a release layer were laminated in this order.

[0208] (Production of melamine decorative board) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, Nikaledin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The impregnation was carried out so that the ratio of the acrylic resin to the acrylic resin was 100% (when dried), and the resulting mixture was dried to produce an impregnated decorative sheet (precursor laminate).

[0209] The impregnated decorative sheet was laminated on the above core substrate, and the above release film was further laminated on the impregnated decorative sheet so that the peel layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.

[0210] The formed laminate was sandwiched between two mirror-finished plates and subjected to a pressure of 100 kg / cm using a heat press. 2 The uncured melamine resin composition was then heat-molded at a molding temperature of 150°C for 10 minutes to thermally cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured melamine resin, yielding the melamine decorative board of Comparative Example 6.

[0211] [Comparative Example 7] (Preparation of decorative sheet) A paper substrate (titanium base paper for building materials, PM-77P manufactured by KJ Specialty Paper Co., Ltd.) was prepared as a porous substrate. By gravure printing using the above printing ink, a design layer (pattern layer) having a thickness of 2 μm was partially laminated on the paper substrate so as to form a stone grain pattern design. Furthermore, the following release layer forming ink 16 was laminated on the pattern layer in synchronization with the pattern layer, and then irradiated with an electron beam of 3 Mrad at an acceleration voltage of 165 kV to form a release layer having a thickness of 2 μm. In this way, a decorative sheet was produced in which a porous substrate, a design layer, and a release layer were laminated in this order.

[0212] <Ink 16 for forming release layer> Ionizing radiation curable monomer (Aronix M-400, manufactured by Toagosei Co., Ltd.) 42 parts by mass Reactive silicone (X-22-164B, manufactured by Shin-Etsu Chemical Co., Ltd.) 4 parts by mass (6.7 parts by mass per 100 parts by mass of total solids) Silane coupling treated silica (particle size 2 μm) 8 parts by mass (13.3 parts by mass per 100 parts by mass of total solids) Hindered amine light stabilizer (Tinuvin 123, manufactured by BASF Corporation) 6 parts by mass (10.0 parts by mass per 100 parts by mass of total solids) Methyl ethyl ketone 40 parts by mass

[0213] (Production of melamine decorative board) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, Nikaledin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The impregnation was carried out so that the ratio of the acrylic resin to the acrylic resin was 100% (when dried), and the resulting mixture was dried to produce an impregnated decorative sheet (precursor laminate).

[0214] The impregnated decorative sheet was laminated on the above core substrate, and the above release film was further laminated on the impregnated decorative sheet so that the peel layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.

[0215] The formed laminate was sandwiched between two mirror-finished plates and subjected to a pressure of 100 kg / cm using a heat press. 2 The uncured melamine resin composition was then heat-molded at a molding temperature of 150°C for 10 minutes to thermally cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured melamine resin, yielding the melamine decorative board of Comparative Example 7.

[0216] [Pure Water Contact Angle of Release Layer of Decorative Sheet] The pure water contact angle of the release layer of the decorative sheets obtained in Examples 9 to 12 and Comparative Examples 6 and 7 was measured. The measurement method was the same as above. The results are shown in Table 3.

[0217] [60° Gloss Value of Release Layer of Decorative Sheet] The 60° gloss values ​​of the release layers of the decorative sheets obtained in Examples 9 to 12 and Comparative Examples 6 and 7 were measured. The measurement method was the same as above. The results are shown in Table 3.

[0218] [Spc of release layer of decorative sheet and melamine decorative board] The Spc (arithmetic mean curvature of peaks) of the release layer of the decorative sheets and melamine decorative boards obtained in Examples 9 to 12 and Comparative Examples 6 and 7 was measured. The measurement method was the same as above. The results are shown in Table 3.

[0219] [Evaluation of Melamine Removal Property] Melamine removability was evaluated using the melamine decorative boards obtained in Examples 9 to 12 and Comparative Examples 6 and 7. The evaluation criteria were the same as above. The results are shown in Table 3.

[0220] [Evaluation of Gloss and Matte Design] The gloss and matte design of the melamine decorative boards obtained in Examples 9 to 12 and Comparative Examples 6 and 7 was evaluated. The evaluation criteria were the same as above. The results are shown in Table 3.

[0221]

[0222] As shown in Table 3, for example, Example 9 and the above-described Example 1 both use the release layer-forming ink 1, but the type of porous substrate is different. Specifically, the porous substrate (PM-83P) used in Example 9 has a lower ash content than the porous substrate (PM-77P) used in Example 1, making the release layer-forming ink 1 less permeable. As a result, the pure water contact angle and 60° gloss value of Example 9 increased compared to Example 1, and the Spc decreased slightly. Thus, the type of porous substrate affects the pure water contact angle, 60° gloss value, and Spc. Therefore, it is necessary to adjust the pure water contact angle, 60° gloss value, and Spc within a predetermined range while taking into account the type of porous substrate. In the present disclosure, good releasability and good gloss-matt design properties can be obtained by adjusting the pure water contact angle, 60° gloss value, and Spc within a predetermined range while taking into account the type of porous substrate. A similar relationship was also confirmed between Example 10 and Example 3.

[0223] On the other hand, both Comparative Example 6 and the above-described Example 1 use the release layer-forming ink 1, but the type of porous substrate is different. Specifically, the porous substrate (KW-1002P) used in Comparative Example 6 has a higher ash content than the porous substrate (PM-77P) used in Example 1, and the release layer-forming ink 1 is more easily permeable. As a result, in Comparative Example 6, the pure water contact angle and 60° gloss value decreased, and Spc increased, compared to Example 1. Thus, the type of porous substrate affects the pure water contact angle, 60° gloss value, and Spc. In Comparative Example 6, the pure water contact angle was low, and therefore the releasability was poor.

[0224] In addition, Examples 11 and 12 and the above-mentioned Example 1 both use the same porous substrate, but the amount of light stabilizer added to the ink for forming the release layer is different. The amount of light stabilizer added does not have a significant effect on the pure water contact angle, but as the amount of light stabilizer added increases, the 60° gloss value tends to increase and the Spc tends to decrease. As such, the presence or absence of a light stabilizer and the amount of light stabilizer added affect the 60° gloss value and Spc. Therefore, it is necessary to adjust the pure water contact angle, 60° gloss value, and Spc within a predetermined range while taking into account the presence or absence of a light stabilizer added and the amount of light stabilizer added. In the present disclosure, good releasability and good gloss matte design can be obtained by adjusting the pure water contact angle, 60° gloss value, and Spc within a predetermined range while taking into account the presence or absence of a light stabilizer added and the amount of light stabilizer added.

[0225] On the other hand, Comparative Example 7, Example 11, and Example 12 all use the same porous substrate, but the amount of light stabilizer added to the ink for forming the release layer is different. When the amount of light stabilizer added is increased, the 60 ° gloss value tends to increase and the Spc tends to decrease. In Comparative Example 7, the 60 ° gloss value was high, so the gloss matte design was poor. Furthermore, when comparing Example 12 and Example 13, Example 13, by increasing the proportion of the matting agent compared to Example 12, had a lower 60 ° gloss value and an increased Spc, resulting in better gloss matte design.

[0226] Thus, the present disclosure provides, for example, the following inventions.

[0227] [1] A decorative sheet used in the manufacture of a resin-impregnated decorative board, the decorative sheet having a porous substrate, a design layer, and a release layer having a pattern shape, in this order in the thickness direction, the 60° gloss value of the release layer is 10 or less, the pure water contact angle of the release layer is 85° or more, and the Spc (arithmetic mean curvature of peaks) of the release layer is 80 mm -1 That's it, decorative sheet.

[0228] [2] The decorative sheet according to [1], wherein the release layer has a pure water contact angle of 100° or more.

[0229] [3] The decorative sheet according to [1] or [2], wherein the 60° gloss value of the release layer is 6.5 or less.

[0230] [4] The Spc (arithmetic mean curvature of peaks) of the release layer is 120 mm -1 The decorative sheet according to any one of [1] to [3] above.

[0231] [5] The decorative sheet according to any one of [1] to [4], wherein the release layer contains a release agent.

[0232] [6] The decorative sheet according to [5], wherein the release agent contains reactive silicone oil.

[0233] [7] The decorative sheet according to [5] or [6], wherein the content of the release agent is 1 part by mass or more and 10 parts by mass or less per 100 parts by mass of the release layer.

[0234] [8] The decorative sheet according to any one of [1] to [7], wherein the release layer contains a matting agent.

[0235] [9] The decorative sheet according to [8], wherein the matting agent contains inorganic particles.

[0236]

[10] The decorative sheet according to [8] or [9], wherein the content of the matting agent is 5 parts by mass or more and 20 parts by mass or less per 100 parts by mass of the release layer.

[0237]

[11] The decorative sheet according to any one of [8] to

[10] , wherein the average particle size of the matting agent is 1 μm or more and 5 μm or less.

[0238]

[12] The decorative sheet according to any one of [1] to

[11] , wherein the thickness of the release layer is 0.5 μm or more and 8 μm or less.

[0239]

[13] The decorative sheet according to any one of [1] to

[12] , wherein the release layer contains a cured product of curable resin X.

[0240]

[14] The decorative sheet according to

[13] , wherein the curable resin X in the release layer is an ionizing radiation curable resin.

[0241]

[15] The decorative sheet according to any one of [1] to

[14] , wherein the resin-impregnated decorative board is a melamine decorative board.

[0242]

[16] A resin-impregnated decorative board comprising: a decorative sheet having a porous substrate, a design layer, and a release layer having a pattern in this order in the thickness direction; a core substrate arranged so as to face the porous substrate in the decorative sheet; and a cured resin layer arranged between the patterns of the release layer, thicker than the release layer, and containing a cured product of curable resin Y, wherein the porous substrate contains the cured product of the curable resin Y, the pure water contact angle of the release layer is 85° or more, and the Spc (arithmetic mean peak curvature) of the release layer is 10 mm. -1 That's it, resin-impregnated decorative panel.

[0243]

[17] The resin-impregnated decorative board according to

[16] , wherein the 60° gloss value of the release layer is 10 or less.

[0244]

[18] The resin-impregnated decorative board according to

[16] or

[17] , wherein the ratio of the 60° gloss value of the cured resin layer to the 60° gloss value of the release layer is 1.2 or more.

[0245]

[19] A method for producing a resin-impregnated decorative board, comprising: a preparation step of preparing the decorative sheet according to any one of [1] to

[15] ; (i) a laminate formation step of forming a laminate having a core substrate, the decorative sheet, a curable resin layer containing curable resin Y, and a release film, in this order in the thickness direction, (ii) a surface of the decorative sheet facing the porous substrate facing the core substrate, and (iii) the decorative sheet impregnated with the curable resin Y; a heating and pressurizing step of heating and pressurizing the laminate to cure the curable resin Y and form a cured resin layer from the curable resin layer to obtain a cured laminate; and a peeling step of peeling the release film from the cured laminate to remove the cured resin layer arranged in a position overlapping with the release layer in the thickness direction, while leaving the cured resin layer arranged between the patterns of the release layer.

[0246] DESCRIPTION OF SYMBOLS 1...Porous substrate 2...Design layer 3...Matte layer 10...Decorative sheet 20...Core substrate 30...Curable resin layer 40...Release film 100...Resin-impregnated decorative sheet

Claims

1. A decorative sheet used in the manufacture of a resin-impregnated decorative board, the decorative sheet having a porous substrate, a design layer, and a release layer having a pattern shape, in that order in the thickness direction, the 60° gloss value of the release layer is 10 or less, the pure water contact angle of the release layer is 85° or more, and the Spc (arithmetic mean curvature of the peaks) of the release layer is 80 mm -1 That's it, the decorative sheet.

2. The decorative sheet according to claim 1, wherein the contact angle of said release layer with pure water is 100° or more.

3. The decorative sheet according to claim 1, wherein the 60° gloss value of said release layer is 6.5 or less.

4. The Spc (arithmetic mean curvature of peaks) of the release layer is 120 mm -1 The decorative sheet according to claim 1 .

5. The decorative sheet according to claim 1, wherein said release layer contains a release agent.

6. The decorative sheet according to claim 5, wherein the release agent comprises a reactive silicone oil.

7. The decorative sheet according to claim 5, wherein the content of said release agent is 1 part by mass or more and 10 parts by mass or less per 100 parts by mass of said release layer.

8. The decorative sheet according to claim 1, wherein said release layer contains a mattifying agent.

9. The decorative sheet according to claim 8, wherein the mattifying agent comprises inorganic particles.

10. The decorative sheet according to claim 8, wherein the content of the matting agent is 5 parts by mass or more and 20 parts by mass or less per 100 parts by mass of the release layer.

11. The decorative sheet according to claim 8, wherein the average particle size of said mattifying agent is 1 μm or more and 5 μm or less.

12. The decorative sheet according to claim 1, wherein the thickness of said release layer is 0.5 μm or more and 8 μm or less.

13. The decorative sheet according to claim 1, wherein the release layer contains a cured product of curable resin X.

14. The decorative sheet according to claim 13, wherein said curable resin X in said release layer is an ionizing radiation curable resin.

15. The decorative sheet according to claim 1, wherein the resin-impregnated decorative board is a melamine decorative board.

16. A resin-impregnated decorative board comprising: a decorative sheet having a porous substrate, a design layer, and a release layer having a pattern shape, in that order in the thickness direction; a core substrate arranged to face the porous substrate in the decorative sheet; and a cured resin layer arranged between the patterns of the release layer, thicker than the release layer, and containing a cured product of curable resin Y; the porous substrate contains the cured product of curable resin Y; the pure water contact angle of the release layer is 85° or more; and the Spc (arithmetic mean curvature of peaks) of the release layer is 10 mm. -1 That is all about the resin-impregnated decorative panel.

17. The resin-impregnated decorative board according to claim 16, wherein the 60° gloss value of the release layer is 10 or less.

18. The resin-impregnated decorative board according to claim 16, wherein the ratio of the 60° gloss value of the cured resin layer to the 60° gloss value of the release layer is 1.2 or greater.

19. A method for producing a resin-impregnated decorative board, comprising: a preparation step of preparing a decorative sheet according to any one of claims 1 to 15; a laminate formation step of forming a laminate having, in this order in the thickness direction, a core substrate, the decorative sheet, a curable resin layer containing curable resin Y, and a release film, (ii) a surface of the decorative sheet facing the porous substrate is arranged to face the core substrate, and (iii) the decorative sheet is impregnated with the curable resin Y; a heating and pressurizing step of heating and pressurizing the laminate to form a cured resin layer from the curable resin layer while curing the curable resin Y, thereby obtaining a cured laminate; and a peeling step of peeling the release film from the cured laminate, removing the cured resin layer arranged in a position overlapping with the release layer in the thickness direction, while leaving the cured resin layer arranged between the patterns of the release layer.

Citation Information

Patent Citations

  • decorative panels

    JP6716877B2

  • Thermosetting resin decorative panel and method for manufacturing the same

    JP2002166501A

  • Decorative sheet and decorative material

    JP2023049868A

  • Decorative panel and manufacturing method for same

    WO2016148091A1