Alloy material

The alloy material's tailored chemical composition addresses weld hot cracking and hot workability issues by stabilizing grain boundaries and preventing cracking, achieving high creep strength and resistance in high-temperature environments.

WO2024204622A1PCT designated stage expired Publication Date: 2024-10-03NIPPON STEEL CORPORATION

Patent Information

Application Number
PCT/JP2024/012847
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-03-28
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Alloy materials used in high-temperature environments, such as steam reformers and petrochemical plants, face challenges with weld hot cracking resistance and hot workability, particularly due to the embrittlement and segregation of elements like P, S, and Mg, which reduce creep strength and increase the likelihood of cracking during welding and hot working.

Method used

A specific chemical composition for the alloy material is developed, including elements like C, Si, Mn, Cr, Ni, Al, Ti, B, Nb, Mo, Ca, and Ta, which control the formation of Ti-based precipitates and grain boundary segregation, enhancing creep strength, weld hot cracking resistance, and hot workability by adjusting the content of these elements within specific ranges to stabilize grain boundaries and prevent compositional liquefaction.

Benefits of technology

The alloy material achieves high creep strength, excellent weld hot cracking resistance, and improved hot workability by stabilizing grain boundaries and preventing cracking, making it suitable for high-temperature applications in environments like steam reformers and petrochemical plants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

Provided is an alloy material that exhibits a high creep strength, an excellent resistance to weld hot cracking, and an excellent hot workability. An alloy material according to the present disclosure contains, in mass%, C: 0.050-0.100%, Si: 1.00% or less, Mn: 1.50% or less, Cr: 19.00-23.00%, Ni: 30.00-35.00%, N: 0.010% or less, Al: 0.15-0.70%, Ti: 0.15-0.70%, B: 0.0001-0.0030%, Nb: 0.0010-0.5000%, Mo: 0.01-1.00%, and Ca: 0.0001-0.0200%, with the balance being Fe and impurities; satisfies formula (1) and formula (2); and further satisfies formula (3) when B ≤ 0.0010%. (1): 0.60 < Al + Ti < 1.20 (2): 3.3 - 41C - Si + 2Mo + 3Ti + 245B - 12Nb ≤ 2.00 (3): 0.4 + 67C + 1.3Si + 5.5Mo + 5.2Ti + 13.4Nb ≤ 8.25
Need to check novelty before this filing date? Find Prior Art

Description

alloy materials

[0001] The present disclosure relates to alloy materials, and more particularly to alloy materials that can be used in high-temperature environments.

[0002] Alloy materials used in steam reformers, ethylene cracking furnaces, heating furnace tubes for oil refineries and petrochemical plants, polycrystalline silicon manufacturing equipment, etc. are used in high-temperature environments of 500 to 1000°C. Therefore, alloy materials used in such high-temperature environments are required to have excellent corrosion resistance and high creep strength in high-temperature environments. Known alloy materials used in such high-temperature environments include Alloy 800, Alloy 800H, and Alloy 800HT.

[0003] Alloy 800, Alloy 800H, and Alloy 800HT contain large amounts of Cr and Ni. Therefore, these alloys have excellent corrosion resistance at high temperatures. These alloys also contain Al and Ti. Therefore, these alloys tend to develop a gamma prime (γ') phase (Ni) during use in high-temperature environments. 3 The precipitation strengthening due to the γ' phase gives these alloys high creep strength.

[0004] Incidentally, Alloy 800, Alloy 800H, and Alloy 800HT, which contain Al and Ti, are prone to weld hot cracking in the heat-affected zone (HAZ) during welding. These alloy materials are manufactured by hot working in a temperature range of around 900°C, and cracking is likely to occur due to embrittlement during hot working. Therefore, these alloy materials are required to have excellent resistance to weld hot cracking and excellent hot workability.

[0005] Techniques for improving the resistance to weld hot cracking of alloy materials containing Al and Ti are disclosed in Japanese Patent Laid-Open No. 2022-163425 (Patent Document 1), Japanese Patent Laid-Open No. 2022-163585 (Patent Document 2), and Japanese Patent Laid-Open No. 2022-163586 (Patent Document 3).

[0006] The alloy material disclosed in Patent Document 1 has a chemical composition containing, by mass%, C: 0.15% or less, Si: 0.05 to 2.0%, Mn: 0.05 to 2.0%, P: 0.035% or less, S: 0.0015% or less, Cr: 16 to 30%, Ni: 18 to 50%, Al: 0.01 to 1.0%, Ti: 0.01 to 1.5%, N: 0.35% or less, O: 0.003% or less, Mo: 8% or less, Cu: 4% or less, Co: 3% or less, Ca: 0.0003 to 0.0050%, and Mg: 0.0045% or less, with the balance being Fe and impurities. Furthermore, the concentrations of CaO, MgO, and Al in the inclusions in which O or S was detected were calculated from the average Ca concentration, average Mg concentration, and average Al concentration of the inclusions. 2 O 3 The mass ratio of [CaO-0.6×MgO] / [CaO+MgO+Al 2 O 3 ]≧0.20. In Patent Document 1, oxide inclusions (CaO, MgO, and AlO) in the alloy material are 2 O 3 ) is appropriately controlled to suppress the formation of coarse TiC and improve the resistance to hot welding cracking of the alloy material.

[0007] The alloy material disclosed in Patent Document 2 has a chemical composition containing, by mass%, C: 0.15% or less, Si: 0.05 to 2.0%, Mn: 0.05 to 2.0%, P: 0.035% or less, S: 0.0015% or less, Cr: 16 to 30%, Ni: 18 to 50%, Al: 0.01 to 1.0%, Ti: 0.01 to 1.5%, N: 0.35% or less, O: 0.003% or less, Mo: 8% or less, Cu: 4% or less, Co: 3% or less, Ca: 0.0003 to 0.0050%, and Mg: 0.0060% or less, with the balance being Fe and impurities. Furthermore, the number density of TiC-based precipitates having a circle equivalent diameter of 1.0 μm or more and the Mg content in the steel are compared to the number density of TiC (particles / mm 2 )≦463−9.5×Mg concentration in steel (ppm by mass). In Patent Document 2, the amount of coarse TiC precipitates is appropriately controlled according to the Mg concentration in the alloy material. This improves the resistance to weld hot cracking of the alloy material.

[0008] The alloy material disclosed in Patent Document 3 has a chemical composition containing, in mass%, C: 0.15% or less, Si: 0.05 to 2.0%, Mn: 0.05 to 2.0%, P: 0.035% or less, S: 0.0015% or less, O: 0.0020% or less, with the total of O+S being 0.0020% or less, Cr: 16 to 30%, Ni: 18 to 50%, Al: 0.01 to 1.0%, Ti: 0.01 to 1.5%, N: 0.02% or less, Mo: 8% or less, Cu: 4% or less, Co: 3% or less, Ca: 0.0010 to 0.0050%, and Mg: 0.0010 to 0.0050%, with the balance being Fe and impurities. Furthermore, the average concentration of S in the oxide-based inclusions and sulfide-based inclusions is 0.70% by mass or more. In Patent Document 3, S, which reduces the grain boundary strength and the melting point of the grain boundary, is fixed in the inclusions, thereby improving the weld hot cracking resistance of the alloy material.

[0009] Furthermore, a technology for improving the hot workability of an alloy material containing Al and Ti is disclosed in Japanese Patent Laid-Open No. 2021-070838 (Patent Document 4).

[0010] The alloy material disclosed in Patent Document 4 has a chemical composition, by mass%, of 0.10% or less of C, 0.05 to 1.0% of Si, 0.05 to 2.0% of Mn, 0.035% or less of P, 0.0015% or less of S, 18 to 25% of Cr, 18 to 50% of Ni, 0.05 to 1.0% of Al, 0.15 to 1.5% of Ti, 0.02% or less of N, 0.003% or less of O, 5% or less of Mo, 2% or less of W, 3% or less of Cu, 2.0% or less of Co, 0.0003 to 0.005% of Ca, and 0.006% or less of Mg, with the balance being Fe and unavoidable impurities. Furthermore, the Ca / Al mass ratio in the oxide-based inclusions is 1.0 to 15. Furthermore, the excess Ca (ΔCa) calculated using ΔCa=Ca-1.25×S-K(Ca / O)×O is 0.0003 to 0.0030%. In Patent Document 4, ΔCa in the alloy material is appropriately controlled, thereby improving the hot workability of the alloy material.

[0011] JP 2022-163425 A JP 2022-163585 A JP 2022-163586 A JP 2021-070838 A

[0012] The alloy materials described in Patent Documents 1 to 3 exhibit excellent resistance to weld hot cracking, but these documents do not consider the hot workability of the alloy materials. The alloy material described in Patent Document 4 exhibits excellent hot workability, but does not consider the resistance to weld hot cracking.

[0013] An object of the present disclosure is to provide an alloy material that has high creep strength, and further has excellent resistance to weld hot cracking and excellent hot workability.

[0014] The alloy material according to the present disclosure has a chemical composition, in mass %, of C: 0.050 to 0.100%, Si: 1.00% or less, Mn: 1.50% or less, P: 0.035% or less, S: 0.0015% or less, Cr: 19.00 to 23.00%, Ni: 30.00 to 35.00%, N: 0.010% or less, Al: 0.15 to 0.70%, Ti: 0.15 to 0.70%, B: 0.0001 to 0.0030%, Nb: 0.0010 to 0.5000%, Mo: 0.01 to 1.00%, Ca: 0.0001 to 0.0200%, Ta: 0 to 0.50%, V: 0 to 1.00%, Zr: 0 to 0.100%, Hf: 0 to 0.10%, Cu: 0 to 1.00%, W: 0 to 1.00%, Co: 0 to 1.00%, rare earth elements: 0 to 0.1000%, Mg: 0 to 0.0200%, and the balance being Fe and impurities, satisfying formulas (1) and (2), and when the B content in the chemical composition is 0.0010% or less, further satisfying formula (3). 0.60<Al+Ti<1.20 (1) 3.3-41C-Si+2Mo+3Ti+245B-12Nb≦2.00 (2) 0.4+67C+1.3Si+5.5Mo+5.2Ti+13.4Nb≦8.25 (3) Here, the element symbols in formulas (1) to (3) are substituted with the content of the corresponding element in the chemical composition in mass %.

[0015] The alloy material according to the present disclosure provides high creep strength, and further provides excellent resistance to weld hot cracking and excellent hot workability.

[0016] The present inventors first investigated an alloy material that can provide high creep strength, excellent resistance to weld hot cracking, and excellent hot workability from the viewpoint of chemical composition, and as a result, the present inventors found an alloy material containing, in mass %, C: 0.050 to 0.100%, Si: 1.00% or less, Mn: 1.50% or less, P: 0.035% or less, S: 0.0015% or less, Cr: 19.00 to 23.00%, Ni: 30.00 to 35.00%, N: 0.010% or less, Al: 0.15 to 0.70%, Ti: 0.15 to 0.70%, B: 0.0001 to 0.0030%, Nb: 0.0010 to 0.5000%, Mo: 0.01 to 1.00%, Ca: 0.01 to 1.00%, and Cr: 0.050 to 0.100%. It was considered that an alloy material having a chemical composition consisting of: 0.0001-0.0200%, Ta: 0-0.50%, V: 0-1.00%, Zr: 0-0.100%, Hf: 0-0.10%, Cu: 0-1.00%, W: 0-1.00%, Co: 0-1.00%, rare earth elements: 0-0.1000%, Mg: 0-0.0200%, and the balance being Fe and impurities, could be used in high temperature environments and could potentially obtain excellent resistance to weld hot cracking and excellent hot workability.

[0017] Therefore, the present inventors further investigated the creep strength, resistance to weld hot cracking, and hot workability of alloy materials satisfying the above-mentioned chemical composition, and as a result, the present inventors obtained the following findings.

[0018] [Regarding Creep Strength] The present inventors have investigated means for increasing the creep strength in high-temperature environments in alloy materials that satisfy the above-mentioned chemical composition. As described above, Al and Ti form a gamma prime (γ') phase (Ni) in the alloy material during use in a high-temperature environment. 3 The γ' phase increases creep strength. Therefore, the total content of Al and Ti affects creep strength. Specifically, in an alloy material having the above chemical composition, sufficient creep strength can be obtained if the following formula (1) is satisfied: 0.60<Al+Ti<1.20 (1) Here, the content of the corresponding element in the chemical composition of the alloy material is substituted for each element symbol in formula (1) in mass %.

[0019] [Regarding resistance to weld hot cracking and hot workability] Among the elements in the above-mentioned chemical composition, elements such as P, S, and Mg are likely to segregate to grain boundaries. If these elements segregate, the grain boundaries become embrittled, and hot workability at around 900°C decreases. B suppresses the decrease in hot workability due to the segregation of these elements to grain boundaries. Specifically, B segregates to grain boundaries and suppresses the segregation of elements other than B to grain boundaries. Therefore, the segregation of B strengthens the grain boundaries. As a result, the hot workability of the alloy material is improved.

[0020] However, if B is contained, the solidification temperature of the grain boundary of the HAZ of the alloy material melted during the temperature rise process during welding will decrease, and therefore, although B improves the hot workability, it will decrease the resistance to weld hot cracking.

[0021] Therefore, the present inventors have investigated means for improving resistance to weld hot cracking while improving hot workability by including B. As a result, the present inventors have found that in order to further improve resistance to weld hot cracking while including B, it is effective to (A) increase the melting temperature and solidification temperature of Ti-based precipitates that precipitate at grain boundaries, and (B) increase the solidification temperature of the grain boundaries that have melted due to the constitutional liquation phenomenon during the temperature rise process during welding.

[0022] [(A) Increasing the melting temperature and solidification temperature of Ti-based precipitates precipitated at grain boundaries] In this specification, Ti-based precipitates refer to precipitates containing Ti. The Ti-based precipitates are mainly carbides containing Ti. The Ti-based precipitates may contain elements other than Ti (e.g., Si, Nb, etc.).

[0023] C, Si, and Nb increase the melting temperature and solidification temperature of Ti-based precipitates. Specifically, C and Si increase the stability of Ti-based precipitates at high temperatures. Therefore, the melting temperature and solidification temperature of Ti-based precipitates increase. Furthermore, Nb is contained in Ti-based precipitates and increases the melting temperature and solidification temperature of Ti-based precipitates. Therefore, C, Si, and Nb are elements that increase the melting temperature and solidification temperature of Ti-based precipitates precipitated at grain boundaries.

[0024] [(B) Increasing the solidification temperature of grain boundaries melted by constitutional liquefaction during the heating process during welding] Even if the melting and solidification temperatures of Ti-based precipitates are high, the occurrence of constitutional liquefaction reduces weld hot cracking resistance. Specifically, during welding heating, the alloy material is rapidly heated locally. In this case, in the heated portion of the alloy material (HAZ), a eutectic melting reaction occurs between the Ti precipitates at the grain boundaries and the grain boundary region, causing the Ti-based precipitates and the grain boundaries to liquefy at a temperature lower than their melting points. This phenomenon is called constitutional liquefaction.

[0025] Grain boundaries where constitutional liquefaction occurs serve as the initiation point for cracks. Therefore, in order to improve resistance to weld hot cracking, it is effective not only to increase the melting temperature and solidification temperature of Ti-based precipitates but also to increase the solidification temperature of grain boundaries where constitutional liquefaction occurs. Therefore, the present inventors investigated means for increasing the solidification temperature of grain boundaries where constitutional liquefaction occurs. As a result, they found that Mo, Ti, and B promote constitutional liquefaction at grain boundaries. When Mo, Ti, or B is contained in grain boundaries where constitutional liquefaction occurs, the solidification temperature of grain boundaries where constitutional liquefaction occurs decreases. If the solidification temperature of grain boundaries where constitutional liquefaction occurs decreases, weld hot cracking becomes more likely to occur.

[0026] Based on the above findings, the inventors believed that resistance to weld hot cracking could be improved by increasing the C, Si, and Nb contents to increase the melting and solidification temperatures of Ti-based precipitates in the alloy, and by reducing the Mo, Ti, and B contents to increase the solidification temperature of the grain boundaries where constitutional liquation occurs. Further investigation was then conducted into the relationship between these elements and resistance to weld hot cracking. As a result, it was discovered that excellent resistance to weld hot cracking and excellent hot workability can be obtained in an alloy having the above chemical composition if the following formula (2) is further satisfied: 3.3-41C-Si+2Mo+3Ti+245B-12Nb≦2.00 (2) Here, the element symbols in formula (2) are substituted with the content of the corresponding element in the chemical composition of the alloy, in mass percent.

[0027] [When the B content is 0.0010% or less] However, even in an alloy material that satisfies the above-mentioned chemical composition and formulas (1) and (2), if the B content is 0.0010% or less, there are cases in which sufficient hot workability is not obtained even if excellent resistance to weld hot cracking is obtained. Therefore, the present inventors further investigated means for achieving both excellent hot workability and excellent resistance to weld hot cracking when the B content is low. As a result, the present inventors have obtained the following findings.

[0028] In alloy materials having the above-described chemical composition, Ti-based precipitates may be present within the crystal grains during hot working at approximately 900°C. The Ti-based precipitates harden the alloy material. As a result, the hot workability of the alloy material decreases. Therefore, in order to improve the hot workability at approximately 900°C, it is effective to suppress the hardening of the alloy material due to Ti-based precipitates.

[0029] Therefore, the present inventors have investigated means for sufficiently suppressing hardening of the alloy material due to Ti-based precipitates during hot working when the B content is 0.0010% or less, and as a result, the present inventors have obtained the following findings.

[0030] In the above-mentioned hot working temperature range, C, Ti, Si, and Nb promote the formation of Ti-based precipitates. C and Ti directly contribute to the formation of Ti-based precipitates. Si increases the diffusion rate of C and Ti, contributing to the formation of Ti-based precipitates. Nb substitutes for the Ti sites of Ti-based precipitates (i.e., lattice points occupied by Ti atoms in Ti-based precipitates), promoting the formation of Nb-containing Ti-based precipitates (composite precipitates). Furthermore, among the above-mentioned chemical compositions, Mo solid-solution strengthens the grain interior, hardening the alloy material even in the hot working temperature range.

[0031] Based on the above findings, the present inventors considered that when the B content is 0.0010% or less, the hot workability at about 900°C can be improved by appropriately controlling the C content, Ti content, Si content, Nb content, and Mo content.

[0032] Based on the above findings, further investigation was conducted into the relationship between the contents of the above elements (C, Si, Mo, Ti, and Nb) and hot workability when the B content is 0.0010% or less. As a result, it was found that in an alloy material that satisfies the above chemical composition and formulas (1) and (2), when the B content is 0.0010% or less, excellent resistance to weld hot cracking and excellent hot workability can be achieved by further satisfying formula (3): 0.4 + 67C + 1.3Si + 5.5Mo + 5.2Ti + 13.4Nb ≦ 8.25 (3) Here, the content of each element in formula (3) is substituted with the content of the corresponding element in the chemical composition in mass %.

[0033] The alloy material of this embodiment has been completed based on the above findings and has the following configuration.

[0034] The alloy material of the first configuration has a chemical composition, in mass %, of C: 0.050 to 0.100%, Si: 1.00% or less, Mn: 1.50% or less, P: 0.035% or less, S: 0.0015% or less, Cr: 19.00 to 23.00%, Ni: 30.00 to 35.00%, N: 0.010% or less, Al: 0.15 to 0.70%, Ti: 0.15 to 0.70%, B: 0.0001 to 0.0030%, Nb: 0.0010 to 0.5000%, Mo: 0.01 to 1.00%, Ca: 0.0001 to 0.0200%, Ta: 0 to 0.50%, V: 0 to 1.00%, Zr: 0 to 0.100%, Hf: 0 to 0.10%, Cu: 0 to 1.00%, W: 0 to 1.00%, Co: 0 to 1.00%, rare earth elements: 0 to 0.1000%, Mg: 0 to 0.0200%, and the balance being Fe and impurities, satisfying formulas (1) and (2), and when the B content in the chemical composition is 0.0010% or less, further satisfying formula (3). 0.60<Al+Ti<1.20 (1) 3.3-41C-Si+2Mo+3Ti+245B-12Nb≦2.00 (2) 0.4+67C+1.3Si+5.5Mo+5.2Ti+13.4Nb≦8.25 (3) Here, the element symbols in formulas (1) to (3) are substituted with the content of the corresponding element in the chemical composition in mass %.

[0035] The alloy material of the second configuration is the alloy material of the first configuration, and the chemical composition contains, in mass %, one or more elements selected from the group consisting of Ta: 0.01 to 0.50%, V: 0.01 to 1.00%, Zr: 0.001 to 0.100%, Hf: 0.01 to 0.10%, Cu: 0.01 to 1.00%, W: 0.01 to 1.00%, Co: 0.01 to 1.00%, rare earth elements: 0.0001 to 0.1000%, and Mg: 0.0001 to 0.0200%.

[0036] The alloy material of the third configuration is the alloy material of the first or second configuration, and the chemical composition contains, in mass%, B: more than 0.0010 to 0.0030%, and the Ti content [Ti] in mass% in the residue obtained by the extraction residue method is less than 0.020%, or the [Ti] is 0.020% or more, the Nb content [Nb] in mass% in the residue is 0.015% or more, and the [Ti] and the [Nb] satisfy the formula (4): [Ti] + [Nb] ≧ 0.050 (4)

[0037] The alloy material of the fourth configuration is an alloy material of the first or second configuration, and the chemical composition contains, in mass%, B: 0.0001 to 0.0010%, and the Ti content [Ti] in mass% in the residue obtained by the extraction residue method is 0.031% or less, or the [Ti] is more than 0.031%, and the Nb content [Nb] in mass% in the residue is 0.3 x [Ti]% or more.

[0038] The alloy material of this embodiment will be described in detail below. Note that "%" regarding elements means mass % unless otherwise specified.

[0039] [Features of the alloy material of this embodiment] The alloy material of this embodiment satisfies the following features 1 to 4. (Feature 1) The chemical composition, in mass %, is: C: 0.050 to 0.100%, Si: 1.00% or less, Mn: 1.50% or less, P: 0.035% or less, S: 0.0015% or less, Cr: 19.00 to 23.00%, Ni: 30.00 to 35.00%, N: 0.010% or less, Al: 0.15 to 0.70%, Ti: 0.15 to 0.70%, B: 0.0001 to 0.0030%, and Nb: 0.00 10-0.5000%, Mo: 0.01-1.00%, Ca: 0.0001-0.0200%, Ta: 0-0.50%, V: 0-1.00%, Zr: 0-0.100%, Hf: 0-0.10%, Cu: 0-1.00%, W: 0-1.00%, Co: 0-1.00%, rare earth elements: 0-0.1000%, Mg: 0-0.0200%, and the balance consisting of Fe and impurities. (Feature 2) The chemical composition of Feature 1 further satisfies formula (1): 0.60<Al+Ti<1.20 (1) Here, for each element symbol in formula (1), the content of the corresponding element in the chemical composition of the alloy material is substituted in mass%. (Feature 3) The chemical composition of Feature 1 further satisfies formula (2): 3.3 - 41C - Si + 2Mo + 3Ti + 245B - 12Nb ≦ 2.00 (2) where, for each element symbol in formula (2), the content of the corresponding element in the chemical composition of the alloy material is substituted in mass %. (Feature 4) When the B content in the chemical composition of Feature 1 is 0.0010% or less, formula (3) is further satisfied: 0.4 + 67C + 1.3Si + 5.5Mo + 5.2Ti + 13.4Nb ≦ 8.25 (3) where, for each element symbol in formula (3), the content of the corresponding element in the chemical composition of the alloy material is substituted in mass %.

[0040] The alloy material of this embodiment satisfies the above-mentioned Features 1 to 4. Therefore, the alloy material of this embodiment has high creep strength, and further has excellent resistance to weld hot cracking and excellent hot workability. Features 1 to 4 will be described below.

[0041] [(Feature 1) Chemical Composition] The chemical composition of the alloy material of this embodiment contains the following elements.

[0042] C: 0.050 to 0.100% Carbon (C) increases the creep strength of the alloy material in a high-temperature environment. If the C content is less than 0.050%, the above effect cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the C content exceeds 0.100%, M is formed at the grain boundary. 23 C 6 This produces a Cr-type carbide. In this case, Cr-depleted regions are formed at the grain boundaries. Therefore, even if the contents of other elements are within the ranges of this embodiment, the stress relaxation cracking resistance of the alloy material decreases. Therefore, the C content is 0.050 to 0.100%. A preferred lower limit of the C content is 0.055%, more preferably 0.060%, even more preferably 0.065%, and even more preferably 0.070%. A preferred upper limit of the C content is 0.097%, more preferably 0.095%, even more preferably 0.093%, even more preferably 0.090%, even more preferably 0.085%, and even more preferably 0.080%.

[0043] Si: 1.00% or less Silicon (Si) deoxidizes the alloy during the steelmaking process. Si also enhances the oxidation resistance of the alloy material in high-temperature environments. Even if even a small amount of Si is contained, the above effects can be achieved to some extent, even if the contents of other elements are within the ranges of this embodiment. However, if the Si content exceeds 1.00%, weld hot cracking resistance and hot workability will decrease, even if the contents of other elements are within the ranges of this embodiment. Therefore, the Si content is 1.00% or less. The preferred lower limit of the Si content is greater than 0%, more preferably 0.01%, even more preferably 0.05%, even more preferably 0.10%, even more preferably 0.15%, and even more preferably 0.20%. The preferred upper limit of the Si content is 0.90%, even more preferably 0.80%, even more preferably 0.70%, even more preferably 0.65%, even more preferably 0.60%, even more preferably 0.55%, and even more preferably 0.50%.

[0044] Mn: 1.50% or less Manganese (Mn) deoxidizes the welded portion of the alloy material during welding. Mn also stabilizes austenite. Even if even a small amount of Mn is contained, the above effect can be obtained to some extent. However, if the Mn content exceeds 1.50%, sigma phase (σ phase) is likely to be formed when used in a high-temperature environment. The σ phase reduces the toughness and creep ductility of the alloy material in a high-temperature environment. Therefore, the Mn content is 1.50% or less. The preferred lower limit of the Mn content is more than 0%, more preferably 0.01%, even more preferably 0.05%, even more preferably 0.10%, even more preferably 0.40%, even more preferably 0.50%, and even more preferably 0.60%. The upper limit of the Mn content is preferably 1.45%, more preferably 1.40%, even more preferably 1.35%, even more preferably 1.30%, even more preferably 1.25%, and even more preferably 1.20%.

[0045] P: 0.035% or less Phosphorus (P) is an unavoidable impurity. In other words, the P content is greater than 0%. P segregates at grain boundaries during welding, reducing stress relaxation cracking resistance. P also segregates at grain boundaries, reducing hot workability. Therefore, the P content is 0.035% or less. The lower the P content, the better. However, excessive reduction in the P content significantly increases manufacturing costs. Therefore, considering normal industrial production, the preferred lower limit of the P content is 0.001%, more preferably 0.002%, and even more preferably 0.005%. The preferred upper limit of the P content is 0.030%, more preferably 0.025%, even more preferably 0.020%, and even more preferably 0.015%.

[0046] S: 0.0015% or less Sulfur (S) is an unavoidable impurity. In other words, the S content is greater than 0%. S segregates at grain boundaries of alloy materials during welding and hot working, reducing welding hot cracking resistance and hot workability. Therefore, the S content is 0.0015% or less. The lower the S content, the better. However, excessive reduction in the S content significantly increases manufacturing costs. Therefore, considering normal industrial production, the preferred lower limit of the S content is greater than 0%, more preferably 0.0001%, and even more preferably 0.0002%. The preferred upper limit of the S content is 0.0012%, more preferably 0.0010%, even more preferably 0.0008%, and even more preferably 0.0006%.

[0047] Cr: 19.00 to 23.00% Chromium (Cr) enhances the corrosion resistance of alloy materials in high-temperature environments. If the Cr content is less than 19.00%, the above effect cannot be fully achieved even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Cr content exceeds 23.00%, the stability of austenite in high-temperature environments decreases. In this case, the creep strength of the alloy material decreases even if the contents of other elements are within the ranges of this embodiment. Therefore, the Cr content is 19.00 to 23.00%. A preferred lower limit of the Cr content is 19.20%, more preferably 19.40%, and even more preferably 19.60%. A preferred upper limit of the Cr content is 22.50%, more preferably 22.00%, even more preferably 21.50%, even more preferably 21.00%, even more preferably 20.50%, and even more preferably 20.00%.

[0048] Ni: 30.00 to 35.00% Nickel (Ni) stabilizes austenite and increases the creep strength of the alloy material in high-temperature environments. If the Ni content is less than 30.00%, the above effect cannot be fully achieved even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Ni content exceeds 35.00%, the above effect saturates. Furthermore, raw material costs increase. Therefore, the Ni content is 30.00 to 35.00%. The preferred lower limit of the Ni content is 30.20%, more preferably 30.40%, even more preferably 30.60%, and even more preferably 30.80%. The upper limit of the Ni content is preferably 34.70%, more preferably 34.50%, even more preferably 34.00%, even more preferably 33.50%, even more preferably 33.00%, even more preferably 32.50%, even more preferably 32.00%, even more preferably 31.50%, and even more preferably 31.00%.

[0049] N: 0.010% or less Nitrogen (N) is an impurity. N dissolves in the matrix (parent phase) to stabilize austenite. The dissolved N also forms fine nitrides in the alloy during use in high-temperature environments. The fine nitrides strengthen Cr-deficient regions, thereby improving the stress relaxation cracking resistance of the alloy. The fine nitrides formed during use in high-temperature environments further improve creep strength through precipitation strengthening. Even if even a small amount of N is contained, the above effects can be achieved to some extent. However, if the N content exceeds 0.010%, Ti nitrides are excessively formed and coarsened. In this case, the weld hot cracking resistance of the alloy is reduced, and further, the toughness and hot workability are also reduced. Therefore, the N content is 0.010% or less. The preferred lower limit of the N content is 0.001%. The preferred upper limit of the N content is 0.007%, more preferably 0.006%, and even more preferably 0.005%.

[0050] Al: 0.15 to 0.70% Aluminum (Al) deoxidizes the alloy during the steelmaking process. Al also enhances the oxidation resistance of the alloy material in high-temperature environments. Al also generates the γ' phase in high-temperature environments, thereby enhancing the creep strength of the alloy material in high-temperature environments. If the Al content is less than 0.15%, the above effects cannot be fully achieved, even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Al content exceeds 0.70%, a large amount of γ' phase is generated during the manufacturing process of the alloy material. In this case, the hot workability during the manufacturing process of the alloy material is reduced, even if the contents of other elements are within the ranges of this embodiment. Therefore, the Al content is 0.15 to 0.70%. The preferred lower limit of the Al content is 0.17%, more preferably 0.19%, even more preferably 0.21%, even more preferably 0.23%, and even more preferably 0.30%. The upper limit of the Al content is preferably 0.65%, more preferably 0.60%, even more preferably 0.57%, even more preferably 0.55%, even more preferably 0.53%, even more preferably 0.51%, even more preferably 0.45%, and even more preferably 0.40%. The Al content is the so-called total Al content (mass%).

[0051] Ti: 0.15 to 0.70% Titanium (Ti) combines with Ni and Al to form the γ' phase in high-temperature environments, thereby enhancing the creep strength of the alloy material in high-temperature environments. If the Ti content is less than 0.15%, the above effects cannot be fully achieved, even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Ti content exceeds 0.70%, Ti-based precipitates become coarse, or a large amount of γ' phase is formed during the manufacturing process of the alloy material. In this case, even if the contents of other elements are within the ranges of this embodiment, the weld hot cracking resistance and hot workability may be reduced. Therefore, the Ti content is 0.15 to 0.70%. The preferred lower limit of the Ti content is 0.16%, more preferably 0.17%, even more preferably 0.18%, and even more preferably 0.20%. The upper limit of the Ti content is preferably 0.65%, more preferably 0.60%, even more preferably 0.57%, even more preferably 0.55%, even more preferably 0.50%, and even more preferably 0.45%.

[0052] B: 0.0001 to 0.0030% Boron (B) segregates to grain boundaries in high-temperature environments of approximately 900°C, increasing grain boundary strength. This improves the hot workability of the alloy material. If the B content is less than 0.0001%, the above effects cannot be fully achieved, even if the contents of other elements are within the ranges specified in this embodiment. On the other hand, if the B content exceeds 0.0030%, B lowers the solidification temperature of the grain boundaries melted during welding heating. In this case, resistance to weld hot cracking decreases, even if the contents of other elements are within the ranges specified in this embodiment. Therefore, the B content is 0.0001 to 0.0030%. The preferred lower limit of the B content is 0.0003%, more preferably 0.0005%, and even more preferably 0.0010%. The preferred upper limit of the B content is 0.0028%, more preferably 0.0025%, even more preferably 0.0023%, and even more preferably 0.0020%.

[0053] Nb: 0.0010 to 0.5000% When contained in Ti-based precipitates, niobium (Nb) increases the melting temperature and solidification temperature of the Ti-based precipitates. As a result, the weld hot cracking resistance of the alloy material is improved. Nb also forms fine precipitates in the alloy material in high-temperature environments, thereby improving the creep strength of the alloy material. If the Nb content is less than 0.0010%, the above effects cannot be fully achieved even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Nb content exceeds 0.5000%, the hot workability of the alloy material is reduced even if the contents of other elements are within the ranges of this embodiment. Therefore, the Nb content is 0.0010 to 0.5000%. The preferred lower limit of the Nb content is 0.0020%, more preferably 0.0050%, even more preferably 0.0080%, and even more preferably 0.0100%. The upper limit of the Nb content is preferably 0.4500%, more preferably 0.4000%, even more preferably 0.3000%, even more preferably 0.2500%, and still more preferably 0.2400%.

[0054] Mo: 0.01 to 1.00%. Molybdenum (Mo), when contained together with B, strengthens grain boundaries through co-segregation, improving the hot workability of the alloy material. Even if the B content exceeds 0.0010%, the above effect is not fully achieved if the Mo content is less than 0.01%. On the other hand, if the Mo content exceeds 1.00%, intermetallic compounds such as LAVES phases are formed within the crystal grains. In this case, the strength difference between the crystal grains and the grain boundaries increases. As a result, hot workability is reduced. Furthermore, if the B content is 0.0010% or less, not only is the above effect of Mo reduced, but the hardness within the grains increases due to solid solution strengthening of Mo. As a result, hot workability at around 900°C is reduced. Therefore, the Mo content is 0.01 to 1.00%. The lower limit of the Mo content is preferably 0.02%, more preferably 0.03%, even more preferably 0.04%, and still more preferably 0.05%. The upper limit of the Mo content is preferably 0.90%, even more preferably 0.80%, even more preferably 0.70%, even more preferably 0.60%, and still more preferably 0.50%.

[0055] Ca: 0.0001 to 0.0200% Calcium (Ca) fixes S (sulfur) as inclusions, improving the hot workability of the alloy material. Ca also fixes S and suppresses its grain boundary segregation. In this case, resistance to weld hot cracking is improved. If the Ca content is less than 0.0001%, the above effects cannot be fully achieved even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Ca content exceeds 0.0200%, the cleanliness of the alloy material decreases. In this case, the hot workability of the alloy material decreases even if the contents of other elements are within the ranges of this embodiment. Therefore, the Ca content is 0.0001 to 0.0200%. The preferred lower limit of the Ca content is 0.0002%, more preferably 0.0005%, and even more preferably 0.0010%. The upper limit of the Ca content is preferably 0.0150%, more preferably 0.0100%, still more preferably 0.0080%, still more preferably 0.0050%, still more preferably 0.0040%, and still more preferably 0.0030%.

[0056] The balance of the chemical composition of the alloy material according to this embodiment is composed of Fe and impurities. Here, the impurities in the chemical composition refer to those that are mixed in from raw materials such as ore, scrap, or the manufacturing environment during industrial production of the alloy material, and are acceptable within a range that does not adversely affect the alloy material according to this embodiment. Typical examples of impurities are Sn, As, Zn, Pb, Sb, Bi, and O (oxygen). The total content of these impurities is 0.10% or less.

[0057] [Optional Elements] The chemical composition of the alloy material of this embodiment may further contain, in place of a portion of Fe, one or more elements selected from the group consisting of Ta: 0-0.50%, V: 0-1.00%, Zr: 0-0.100%, Hf: 0-0.10%, Cu: 0-1.00%, W: 0-1.00%, Co: 0-1.00%, rare earth elements: 0-0.1000%, and Mg: 0-0.0200%. These optional elements will be described below.

[0058] [First Group: Ta, V, Zr, and Hf] The chemical composition of the alloy material according to this embodiment may further contain, in place of a portion of Fe, one or more elements selected from the group consisting of Ta, V, Zr, and Hf. These elements are optional elements. All of these elements increase the melting temperature of Ti carbide, stabilize the Ti carbide, and improve resistance to weld hot cracking.

[0059] Ta: 0 to 0.50% Tantalum (Ta) is an optional element and does not necessarily need to be contained. That is, the Ta content may be 0%. When Ta is contained, that is, when the Ta content exceeds 0%, Ta combines with Ti and C and is contained in Ti-based precipitates. The melting and solidification temperatures of Ti-based precipitates containing Ta are increased. Therefore, the solidification temperature of the grain boundaries melted during welding is increased. As a result, resistance to weld hot cracking is improved. Even if even a small amount of Ta is contained, the above effects can be obtained to some extent. However, if the Ta content exceeds 0.50%, resistance to weld hot cracking is reduced in the weld heat-affected zone of the alloy material during welding. If the Ta content exceeds 0.50%, hot workability is further reduced. Therefore, the Ta content is 0 to 0.50%. The lower limit of the Ta content is preferably 0.01%, more preferably 0.02%, even more preferably 0.05%, and still more preferably 0.08%. The upper limit of the Ta content is preferably 0.45%, more preferably 0.40%, even more preferably 0.35%, and still more preferably 0.30%.

[0060] V: 0 to 1.00% Vanadium (V) is an optional element and may not be contained. That is, the V content may be 0%. When V is contained, that is, when the V content exceeds 0%, V is combined with Ti and C and contained in Ti carbide. The melting and solidification temperatures of Ti-based precipitates containing V are increased. Therefore, the solidification temperature of the molten grain boundaries during welding is increased. As a result, resistance to weld hot cracking is improved. Even if even a small amount of V is contained, the above effects can be obtained to some extent. However, if the V content exceeds 1.00%, resistance to weld hot cracking in the weld heat-affected zone of the alloy material decreases during welding. Therefore, the V content is 0 to 1.00%. The preferred lower limit of the V content is 0.01%, more preferably 0.02%, even more preferably 0.04%, and even more preferably 0.06%. The upper limit of the V content is preferably 0.80%, more preferably 0.50%, even more preferably 0.40%, even more preferably 0.35%, and still more preferably 0.30%.

[0061] Zr: 0 to 0.100% Zirconium (Zr) is an optional element and does not necessarily need to be contained. That is, the Zr content may be 0%. When Zr is contained, that is, when the Zr content exceeds 0%, Zr combines with Ti and C and is contained in Ti carbide. The melting and solidification temperatures of Ti-based precipitates containing Zr are increased. Therefore, the solidification temperature of the molten grain boundaries during welding is increased. As a result, resistance to weld hot cracking is improved. Even if even a small amount of Zr is contained, the above effects can be achieved to some extent. However, if the Zr content exceeds 0.100%, resistance to weld hot cracking in the weld heat-affected zone of the alloy material during welding actually decreases. Therefore, the Zr content is 0 to 0.100%. The preferred lower limit of the Zr content is 0.001%, and more preferably 0.002%. The upper limit of the Zr content is preferably 0.090%, more preferably 0.080%, even more preferably 0.050%, even more preferably 0.030%, and still more preferably 0.010% or less.

[0062] Hf: 0 to 0.10% Hafnium (Hf) is an optional element and may not be contained. That is, the Hf content may be 0%. When Hf is contained, that is, when the Hf content exceeds 0%, Hf is combined with Ti and C and contained in Ti-based precipitates. The melting and solidification temperatures of Ti-based precipitates containing Hf are increased. Therefore, the solidification temperature of the molten grain boundaries during welding is increased. As a result, resistance to weld hot cracking is improved. Even if even a small amount of Hf is contained, the above effects can be obtained to some extent. However, if the Hf content exceeds 0.10%, resistance to weld hot cracking in the weld heat-affected zone of the alloy material during welding actually decreases. Therefore, the Hf content is 0 to 0.10%. The preferred lower limit of the Hf content is 0.01%, and more preferably 0.02%. The upper limit of the Hf content is preferably 0.09%, more preferably 0.08%, even more preferably 0.07%, and still more preferably 0.06%.

[0063] [Second Group: Cu, W, and Co] The chemical composition of the alloy material according to this embodiment may further contain, in place of a portion of Fe, one or more elements selected from the group consisting of Cu, W, and Co. These elements are optional elements, and all of them increase the creep strength of the alloy material.

[0064] Cu: 0 to 1.00% Copper (Cu) is an optional element and does not necessarily need to be contained. That is, the Cu content may be 0%. When Cu is contained, that is, when the Cu content exceeds 0%, Cu precipitates as a Cu phase within grains during use of the alloy material in a high-temperature environment. This precipitation strengthening increases the creep strength of the alloy material. Even if even a small amount of Cu is contained, the above effect can be achieved to some extent. However, when the Cu content exceeds 1.00%, excessive Cu phase precipitates within the crystal grains. In this case, the difference in strength between the crystal grains and the grain boundaries increases. As a result, stress relaxation cracking resistance decreases. Therefore, the Cu content is 0 to 1.00%. The preferred lower limit of the Cu content is 0.01%, more preferably 0.02%, even more preferably 0.05%, even more preferably 0.10%, even more preferably 0.15%, and even more preferably 0.20%. The upper limit of the Cu content is preferably 0.90%, more preferably 0.80%, even more preferably 0.70%, even more preferably 0.60%, even more preferably 0.55%, and even more preferably 0.50%.

[0065] W: 0 to 1.00% Tungsten (W) is an optional element and does not necessarily need to be included. In other words, the W content may be 0%. When W is included, i.e., when the W content exceeds 0%, W enhances the creep strength of the alloy material through solid solution strengthening during use in high-temperature environments. Even if even a small amount of W is included, the above effect can be achieved to some extent. However, when the W content exceeds 1.00%, intermetallic compounds such as LAVES phases are formed within the crystal grains. In this case, secondary induced precipitation hardening increases, increasing the difference in strength between the crystal grains and the grain boundaries. As a result, stress relaxation cracking resistance decreases. Therefore, the W content is 0 to 1.00%. The preferred lower limit of the W content is 0.01%, more preferably 0.02%, even more preferably 0.03%, even more preferably 0.04%, even more preferably 0.05%, and even more preferably 0.10%. The upper limit of the W content is preferably 0.90%, more preferably 0.80%, even more preferably 0.70%, even more preferably 0.65%, even more preferably 0.60%, and even more preferably 0.50%.

[0066] Cobalt (Co): 0 to 1.00% Cobalt (Co) is an optional element and does not necessarily need to be contained. In other words, the Co content may be 0%. When Co is contained, that is, when the Co content exceeds 0%, Co stabilizes austenite and increases the creep strength of the alloy material in high-temperature environments. Even if even a small amount of Co is contained, the above effect can be obtained to some extent. However, if the Co content exceeds 1.00%, the raw material cost increases. Therefore, the Co content is 0 to 1.00%. The preferred lower limit of the Co content is 0.01%, more preferably 0.02%, even more preferably 0.03%, even more preferably 0.05%, and even more preferably 0.10%. The preferred upper limit of the Co content is 0.90%, even more preferably 0.80%, even more preferably 0.70%, even more preferably 0.60%, and even more preferably 0.50%.

[0067] [Third Group: Rare Earth Elements (REM)] The chemical composition of the alloy material according to this embodiment may further contain rare earth elements (REM) in place of a portion of Fe.

[0068] Rare Earth Elements: 0 to 0.1000% Rare earth elements (REM) are optional elements and do not necessarily need to be present. That is, the REM content may be 0%. When REM is present, that is, when the REM content exceeds 0%, the REM fixes S (sulfur) as inclusions, improving the hot workability of the alloy material. The REM further fixes S and suppresses its grain boundary segregation. In this case, resistance to weld hot cracking is improved. Even if even a small amount of REM is present, the above effects can be achieved to some extent. However, if the REM content exceeds 0.1000%, the cleanliness of the alloy material decreases. In this case, the hot workability of the alloy material actually decreases. Therefore, the REM content is 0 to 0.1000%. The preferred lower limit of the REM content is 0.0001%, more preferably 0.0005%, even more preferably 0.0010%, and even more preferably 0.0020%. The upper limit of the REM content is preferably 0.0800%, more preferably 0.0600%, and even more preferably 0.0400%.

[0069] In this specification, REM includes at least one element selected from Sc, Y, and lanthanoids (La with atomic number 57 to Lu with atomic number 71), and the REM content means the total content of these elements.

[0070] [Fourth Group: Mg] The chemical composition of the alloy material according to this embodiment may further contain Mg in place of a portion of Fe.

[0071] Mg: 0 to 0.0200% Magnesium (Mg) is an impurity and may not be present. In other words, the Mg content may be 0%. If the Mg content exceeds 0.0200%, Mg segregates to grain boundaries in high-temperature environments of approximately 900°C, embrittling the grain boundaries. In this case, the hot workability of the alloy material is reduced. Therefore, the Mg content is 0 to 0.0200%. The lower the Mg content, the better. However, excessive reduction in the Mg content significantly increases manufacturing costs. Therefore, considering normal industrial production, the preferred lower limit of the Mg content is greater than 0%, more preferably 0.0001%, and even more preferably 0.0002%. The preferred upper limit of the Mg content is 0.0150%, more preferably 0.0100%, even more preferably 0.0080%, even more preferably 0.0050%, and even more preferably 0.0040%.

[0072] [(Feature 2) Regarding Formula (1)] The chemical composition of the alloy material of the present embodiment further satisfies Formula (1): 0.60<Al+Ti<1.20 (1) Here, for each element symbol in Formula (1), the content of the corresponding element in the chemical composition of the alloy material is substituted in mass %.

[0073] F1 is defined as Al + Ti. F1 is an index of the amount of γ' phase generated during use of the alloy material of this embodiment in a high-temperature environment. In the alloy material of this embodiment, the γ' phase is generated during use in a high-temperature environment. This γ' phase increases the creep strength of the alloy material in a high-temperature environment.

[0074] Even when an alloy material satisfies Features 1, 3, and 4, if F1 is 0.60 or less, a sufficient amount of γ' phase will not be formed in the alloy material in a high-temperature environment. In this case, the creep strength of the alloy material in a high-temperature environment will be reduced. On the other hand, even when an alloy material satisfies Features 1, 3, and 4, if F1 is 1.20 or more, an excessive amount of γ' phase will be formed in the alloy material. In this case, the weld hot cracking resistance will be reduced. Therefore, F1 is greater than 0.60 and less than 1.20.

[0075] The lower limit of F1 is preferably 0.61, more preferably 0.62, even more preferably 0.64, even more preferably 0.66, even more preferably 0.68, and even more preferably 0.70. The upper limit of F1 is preferably 1.15, more preferably 1.10, even more preferably 1.05, even more preferably 1.00, and even more preferably 0.95. The numerical value of F1 is rounded to one decimal place.

[0076] [(Feature 3) Regarding Formula (2)] The chemical composition of the alloy material of the present embodiment further satisfies Formula (2): 3.3-41C-Si+2Mo+3Ti+245B-12Nb≦2.00 (2) Here, for each element symbol in Formula (2), the content of the corresponding element in the chemical composition of the alloy material is substituted in mass %.

[0077] F2 is defined as 3.3 - 41C - Si + 2Mo + 3Ti + 245B - 12Nb. F2 is an index of resistance to welding hot cracking. The alloy material of this embodiment contains B to improve hot workability when hot working is performed at approximately 900°C. However, in an alloy material having a chemical composition satisfying Feature 1, the segregation of B to the grain boundaries lowers the solidification temperature of the grain boundaries of the alloy material. This makes it easy for resistance to welding hot cracking to decrease. Therefore, as described above, the alloy material of this embodiment (A) increases the melting temperature and solidification temperature of Ti-based precipitates precipitated at grain boundaries, and (B) increases the solidification temperature of the grain boundaries melted by the constitutional liquation phenomenon during the heating process during welding. As a result, resistance to welding hot cracking is improved.

[0078] Specifically, in a chemical composition satisfying Feature 1, C, Si, and Nb increase the solidification temperature of Ti-based precipitates after melting. On the other hand, Mo, Ti, and B promote the constitutional liquefaction phenomenon and lower the solidification temperature of the grain boundary after melting. Therefore, by appropriately controlling the C content, Si content, Nb content, Mo content, Ti content, and B content, the above (A) and (B) are simultaneously achieved, increasing the solidification temperature of the grain boundary after melting during welding, and as a result, improving resistance to weld hot cracking. Even if the alloy material satisfies Features 1, 2, and 4, if F2 exceeds 2.00, the above effects cannot be sufficiently obtained. Therefore, F2 is 2.00 or less.

[0079] The upper limit of F2 is preferably 1.97, more preferably 1.95, even more preferably 1.93, and even more preferably 1.90. The lower limit of F2 is not particularly limited, but is preferably -7.00, more preferably -6.00, even more preferably -5.00, and even more preferably -4.00. The numerical value of F2 is the value obtained by rounding off to one decimal place.

[0080] [(Feature 4) Regarding Formula (3)] When the B content in the chemical composition that satisfies Feature 1 is 0.0010% or less, the chemical composition of the alloy material of this embodiment also satisfies Formula (3): 0.4 + 67C + 1.3Si + 5.5Mo + 5.2Ti + 13.4Nb≦8.25 (3) Here, for each element symbol in Formula (3), the content of the corresponding element in the chemical composition of the alloy material is substituted in mass %.

[0081] F3 is defined as 0.4 + 67C + 1.3Si + 5.5Mo + 5.2Ti + 13.4Nb. F3 is an index of hot workability when hot working is performed at about 900°C.

[0082] As described above, B segregates at the grain boundaries of the alloy material and lowers the solidification temperature of the grain boundaries. Therefore, in an alloy material that satisfies Feature 1 and contains B, resistance to weld hot cracking is likely to be reduced. Therefore, in this embodiment, the chemical composition of the alloy material is set to satisfy formula (2), thereby increasing the solidification temperature of the grain boundaries after melting during welding and improving resistance to weld hot cracking.

[0083] When welding extremely thick materials or welding with a large heat input is performed, an alloy material with high resistance to weld hot cracking is used. In this case, the B content in the alloy material may be adjusted to 0.0010% or less.

[0084] When the B content is 0.0010% or less, the reduction in the B content improves resistance to weld hot cracking. However, a reduction in the B content tends to reduce hot workability. Therefore, when the B content in the chemical composition is 0.0010% or less, the alloy material of this embodiment improves hot workability by suppressing hardening of the alloy material due to Ti-based precipitates. C, Si, Mo, Ti, and Nb promote the formation of Ti-based precipitates. Therefore, when the B content in the chemical composition is 0.0010% or less, the value of F3, which is composed of the C content, Si content, Mo content, Ti content, and Nb content, is appropriately adjusted to suppress the formation of Ti-based precipitates. This improves hot workability at around 900°C. Even if the alloy material satisfies Features 1 to 3, if F3 exceeds 8.25, the above effects cannot be fully achieved. Therefore, F3 is 8.25 or less.

[0085] The upper limit of F3 is preferably 8.20, more preferably 8.15, even more preferably 8.13, and even more preferably 8.10. The lower limit of F3 is not particularly limited, but is preferably 4.60, more preferably 4.80, even more preferably 5.00, and even more preferably 5.50. The numerical value of F3 is the value obtained by rounding off to one decimal place.

[0086] [Effects of Alloy Material] The alloy material of this embodiment satisfies the above-mentioned Features 1 to 4. As a result, the alloy material of this embodiment has sufficient creep strength in high-temperature environments, and can achieve both excellent resistance to weld hot cracking and excellent hot workability.

[0087] [Microstructure and Shape of Alloy Material] The microstructure of the alloy material of this embodiment is made of austenite. The shape of the alloy material of this embodiment is not particularly limited. The alloy material may be an alloy pipe or an alloy plate. The alloy material may be rod-shaped. Preferably, the alloy material of this embodiment is an alloy pipe or an alloy plate.

[0088] [Preferred embodiment of the alloy material of this embodiment when the B content exceeds 0.0010%] In a chemical composition that satisfies Features 1 to 3, when the B content is greater than 0.0010% and less than 0.0030%, preferably, the alloy material of this embodiment further satisfies the following Feature 5. (Feature 5) The Ti content [Ti] in mass% in the residue obtained by the extraction residue method is less than 0.020%, or [Ti] is 0.020% or more, and the Nb content [Nb] in mass% in the residue is 0.015% or more, and [Ti] and [Nb] satisfy the formula (4): [Ti] + [Nb] ≧ 0.050 (4) Feature 5 will now be described.

[0089] [(Feature 5) Relationship between Ti content [Ti] and Nb content [Nb] in residue (part 1)] In the alloy material of this embodiment, when the B content in the chemical composition is more than 0.0010% to 0.0030%, by satisfying Features 1 to 3, the alloy material has sufficient creep strength in high-temperature environments and can achieve both excellent resistance to weld hot cracking and excellent hot workability.

[0090] The alloy material of this embodiment contains a certain amount of Ti-based precipitates before welding. Therefore, during the heating process when welding the alloy material, the Ti-based precipitates trapped at the grain boundaries undergo eutectic melting. Because the alloy material of this embodiment contains B, B segregates at the grain boundaries. Therefore, the solidification temperature of the grain boundaries after melting is lowered by B. As a result, resistance to weld hot cracking is reduced. Therefore, when the B content of the alloy material of this embodiment is greater than 0.0010% and less than 0.0030%, it is preferable to adopt one of the following two measures, Measure I and Measure II. (Measure I) Minimize the amount of Ti-based precipitates already present in the alloy material. This suppresses eutectic melting at the grain boundaries at low temperatures and increases the solidification temperature of the grain boundaries. (Measure II) Add Nb to the Ti-based precipitates to stabilize them up to high temperatures. In this case, the eutectic melting temperature of the grain boundaries containing Ti-based precipitates increases, and the solidification temperature of the grain boundaries also increases.

[0091] Therefore, when the B content is more than 0.0010% to 0.0030%, the alloy material of this embodiment preferably satisfies either of the following requirements I and II. (Requirement I) The Ti content [Ti] in the residue is less than 0.020%. (Requirement II) The [Ti] in the residue obtained by the extraction residue method is 0.020% or more, the Nb content [Nb] in the residue is 0.015% or more, and [Ti] and [Nb] satisfy the formula (4). [Ti] + [Nb] ≧ 0.050 (4)

[0092] [Regarding Requirement I] When the B content is more than 0.0010% to 0.0030%, if the amount of Ti-based precipitates formed is small, hot welding cracking due to eutectic melting between Ti-based precipitates and grain boundaries is unlikely to occur. Requirement I requires that the Ti content [Ti] in the residue be less than 0.020%. In this case, the amount of Ti-based precipitates formed in the alloy material is sufficiently suppressed. Therefore, even better resistance to hot welding cracking can be obtained.

[0093] In the case of requirement I, the upper limit of the Ti content [Ti] in the residue is preferably 0.019%, and more preferably 0.017%.

[0094] [Regarding Requirement II] When the B content is more than 0.0010% to 0.0030%, if a certain amount of Ti-based precipitates are formed, it is preferable to increase the solidification temperature after eutectic melting of the Ti-based precipitates and grain boundaries. If the Ti-based precipitates in the alloy material contain Nb, the Ti-based precipitates are stabilized at high temperatures. Therefore, it is possible to increase the solidification temperature of the grain boundaries after eutectic melting of the Ti-based precipitates and grain boundaries. In Requirement II, [Ti] in the residue is 0.020% or more, the Nb content [Nb] in the residue is 0.015% or more, and [Ti] and [Nb] satisfy the formula (4). [Ti] + [Nb] ≧ 0.050 (4)

[0095] In this case, the proportion of Ti-based precipitates containing Nb is high among the Ti-based precipitates present in the alloy material, and therefore the solidification temperature of the grain boundary after eutectic melting of the Ti-based precipitates and the grain boundary is sufficiently high, resulting in even better resistance to weld hot cracking.

[0096] In the case of requirement II, the lower limit of [Ti] + [Nb] in the residue is preferably 0.052%, more preferably 0.060%, even more preferably 0.070%, even more preferably 0.080%, and even more preferably 0.090%.

[0097] [Preferred embodiment of the alloy material of this embodiment when the B content is 0.0010% or less] In a chemical composition that satisfies Features 1 to 4, when the B content is 0.0001 to 0.0010%, the alloy material of this embodiment further satisfies the following Feature 6. (Feature 6) The Ti content [Ti] in mass% in the residue obtained by the extraction residue method is 0.031% or less, or [Ti] is more than 0.031% and the Nb content [Nb] in mass% in the residue is 0.3 × [Ti]% or more. Feature 6 will be described below.

[0098] [(Feature 6) Relationship between [Ti] and [Nb] in the residue (part 2)] When the B content is 0.0001 to 0.0010%, preferably, either of the following requirements III and IV is satisfied. (Requirement III) The Ti content [Ti] in the residue is 0.031% or less. (Requirement IV) The [Ti] in the residue is more than 0.031%, and the Nb content [Nb] in the residue is 0.3 × [Ti]% or more.

[0099] [Regarding Requirement III] When the B content is 0.0010% or less, the decrease in weld hot cracking resistance due to the B content is suppressed compared to Requirement (I). Therefore, when [Ti] in the residue is 0.031% or less, the formation of Ti precipitates in the alloy material is sufficiently suppressed, and even better weld hot cracking resistance is obtained.

[0100] [Regarding Requirement (IV)] Even when the B content is 0.0010% or less, if Ti-based precipitates are formed in a certain amount, the high-temperature stability of the Ti-based precipitates is increased to raise the solidification temperature of the grain boundaries after eutectic melting of the Ti-based precipitates and the grain boundaries. Specifically, the proportion of Nb-containing Ti-based precipitates in the alloy material is increased. If the [Ti] in the residue is more than 0.031% and the Nb content [Nb] in the residue is 0.3 × [Ti]%, the proportion of Nb-containing Ti-based precipitates is sufficiently high. As a result, even better resistance to weld hot cracking is obtained.

[0101] [Method for measuring Ti content [Ti] and Nb content [Nb] in residue] [Ti] and [Nb] in the residue of an alloy material are determined by the following extraction residue method. A test piece is taken from the alloy material. The cross section perpendicular to the longitudinal direction of the test piece may be circular or rectangular. When the alloy material is an alloy pipe, the test piece is taken so that the center of the cross section perpendicular to the longitudinal direction of the test piece is at the center of the wall thickness of the alloy pipe, and the longitudinal direction of the test piece is in the axial direction of the alloy pipe. When the alloy material is an alloy plate, the test piece is taken so that the center of the cross section perpendicular to the longitudinal direction of the test piece is at the center of the plate width and the center of the plate thickness of the alloy plate, and the longitudinal direction of the test piece is in the longitudinal direction of the alloy plate. When the alloy material is a round bar, the test piece is taken so that the center of the cross section perpendicular to the longitudinal direction of the test piece is at the R / 2 position of the round bar (the center of the radius in the cross section perpendicular to the longitudinal direction of the round bar), and the longitudinal direction of the test piece is in the longitudinal direction of the round bar.

[0102] The surface of the collected test piece is polished to about 50 μm by preliminary electrolytic polishing to obtain a new surface. The electrolytically polished test piece is electrolyzed (main electrolysis) in an electrolyte (10% acetylacetone + 1% tetraammonium chloride + methanol). The electrolyte after the main electrolysis is passed through a 0.2 μm filter to capture the residue. The obtained residue is acid-decomposed, and the mass of Ti and the mass of Nb in the residue are determined by ICP (inductively coupled plasma) optical emission spectrometry. Furthermore, the mass of the electrolyzed alloy material is determined. Specifically, the mass of the test piece before the main electrolysis and the mass of the test piece after the main electrolysis are measured. The value obtained by subtracting the mass of the test piece after the main electrolysis from the mass of the test piece before the main electrolysis is defined as the mass of the electrolyzed alloy material.

[0103] The Ti content [Ti] (mass %) in the residue is determined by dividing the Ti mass in the residue by the mass of the electrolyzed alloy material, and the Nb content [Nb] (mass %) in the residue is determined by dividing the Nb mass in the residue by the mass of the electrolyzed alloy material.

[0104] [Method for manufacturing alloy material] A method for manufacturing the alloy material of this embodiment will be described. The manufacturing method described below is one example of a method for manufacturing the alloy material of this embodiment. Therefore, the alloy material of this embodiment may be manufactured by a manufacturing method other than the manufacturing method described below. However, the manufacturing method described below is a preferred example of a method for manufacturing the alloy material of this embodiment.

[0105] The method for manufacturing an alloy material according to this embodiment includes the following steps: (Step 1) Preparation step (Step 2) Hot working step (Step 3) Cold working step (Step 4) Heat treatment step Step 3 (cold working step) is an optional step and may not be performed. Each step will be described below.

[0106] [(Step 1) Preparation Step] In the preparation step, a material having a chemical composition that satisfies the above-described features 1 to 4 is prepared. The material may be supplied from a third party or may be manufactured. The material may be an ingot, slab, bloom, or billet.

[0107] When manufacturing a material, the material is manufactured by the following method. A molten alloy having the above-described chemical composition is manufactured. The manufactured molten alloy is used to manufacture an ingot by ingot casting. The manufactured molten alloy may be used to manufacture a slab, bloom, or billet by continuous casting. The manufactured ingot, slab, or bloom may be hot worked to manufacture a billet. For example, the ingot may be hot forged to manufacture a cylindrical billet, and this billet may be used as the material. In this case, the temperature of the material immediately before the start of hot forging is not particularly limited, but is, for example, 1100 to 1300°C. The method of cooling the material after hot forging is not particularly limited.

[0108] [(Step 2) Hot Working Step] In the hot working step, the raw material prepared in the preparation step is hot worked to produce an intermediate alloy material. The intermediate alloy material may be, for example, an alloy pipe, an alloy plate, or an alloy round bar.

[0109] When the intermediate alloy material is an alloy pipe, the hot working step involves the following processes: First, a cylindrical material is prepared. A through hole is formed along the central axis of the cylindrical material by machining. The cylindrical material with the through hole formed is heated. The heated cylindrical material is subjected to hot extrusion, typically the Ugine-Séjournet process, to produce the intermediate alloy material (alloy pipe).

[0110] Alternatively, instead of hot extrusion, an alloy pipe may be produced by piercing-rolling according to the Mannesmann process. In this case, a cylindrical blank is heated. The heating temperature is not particularly limited, but is, for example, 1100 to 1300°C. The heated cylindrical blank is then subjected to piercing-rolling using a piercing mill. When piercing-rolling is performed, the piercing ratio is not particularly limited, but is, for example, 1.0 to 4.0. The piercing-rolled cylindrical blank is then further hot-rolled using a mandrel mill, a reducer, a sizing mill, or the like to produce a hollow blank (alloy pipe). The cumulative area reduction rate in the hot working step is not particularly limited, but is, for example, 20 to 80%. When an alloy pipe is produced by hot working, the temperature (finishing temperature) of the hollow blank immediately after the hot working is preferably 800°C or higher. Note that the hot working step includes hot working at approximately 900°C.

[0111] When the intermediate alloy material is an alloy plate, the hot working step uses, for example, one or more rolling mills equipped with a pair of work rolls. A material such as a slab is heated. The heated material is hot rolled using the rolling mill to produce an alloy plate. The heating temperature of the material before hot rolling is not particularly limited, but is, for example, 1100 to 1300°C. The hot working step includes hot working at about 900°C.

[0112] When the intermediate alloy material is a round bar, the hot working process uses, for example, one or more rolling mills equipped with a pair of work rolls. The pair of work rolls has a groove formed therein. A material such as a bloom is heated. The heated material is hot rolled using the rolling mill to produce a round bar. The heating temperature of the material before hot rolling is not particularly limited, but is, for example, 1100 to 1300°C. The hot working process includes hot working at about 900°C.

[0113] [(Step 3) Cold Working Step] The cold working step is performed as needed. In other words, the cold working step does not have to be performed. When the cold working step is performed, the intermediate alloy material is subjected to pickling treatment and then cold working. When the intermediate alloy material is an alloy pipe or alloy bar, the cold working is, for example, cold drawing. When the intermediate alloy material is an alloy plate, the cold working is, for example, cold rolling. By performing the cold working step, recrystallization can be initiated and grain regulation can be achieved. The area reduction rate in the cold working step is not particularly limited, but is, for example, 10 to 90%.

[0114] [(Step 4) Heat Treatment Step] In the heat treatment step, the intermediate alloy material after the hot working step or the cold working step is subjected to heat treatment to adjust the amount of solute Ti in the alloy material and the size of the crystal grains. The heat treatment temperature T1 is 1170 to 1300°C. The holding time at the heat treatment temperature T1 is not particularly limited, but is, for example, 5 to 30 minutes. After the holding time has elapsed, the intermediate alloy material is quenched.

[0115] The alloy material of this embodiment can be manufactured through the above steps. The manufacturing method described above is one example of a manufacturing method for the alloy material of this embodiment. Therefore, the manufacturing method for the alloy material of this embodiment is not limited to the manufacturing method described above. As long as Features 1 to 4 are satisfied, the manufacturing method for the alloy material is not limited to the manufacturing method described above.

[0116] [Preferable Conditions in the Heat Treatment Step] Preferably, the heat treatment temperature T1 in the heat treatment step satisfies the following formula (X): T1≦1600+33011×(Nb) 2 −6995×(Nb) (X) Here, the Nb content in mass % in the chemical composition of the alloy material is substituted for (Nb) in formula (X).

[0117] FA is defined as follows: FA = 1600 + 33011 × (Nb) 2 −6995×(Nb) FA is an index that affects the composition of precipitates in an alloy material, and more specifically, is an index that affects the Ti content [Ti] and Nb content [Nb] in the residue.

[0118] If the heat treatment temperature T1 is FA or less, and the B content in the alloy material is more than 0.0010% to 0.0030%, Feature 5 (requirement (I) or requirement (II)) is likely to be satisfied. Also, if the B content in the alloy material is 0.0001 to 0.0010%, Feature 6 (requirement (III) or requirement (IV)) is likely to be satisfied.

[0119] [Method for manufacturing a welded joint of an alloy material] The welded joint of an alloy material of this embodiment can be manufactured by the following method.

[0120] The alloy material of this embodiment is prepared as a base material. A groove is formed in the prepared base material. Specifically, the groove is formed at the end of the base material by a known processing method. The groove shape may be V-shaped, U-shaped, X-shaped, or any other shape other than V-shaped, U-shaped, or X-shaped.

[0121] Welding is performed on prepared base materials to produce a welded joint. Specifically, two base materials with grooves formed therein are prepared. The grooves of the prepared base materials are butted together. Then, welding is performed on the pair of butted grooves using a known welding material to form a weld metal having the above-mentioned chemical composition. An example of the welding material is AWS standard name: ER NiCr-3. However, the welding material is not limited to this.

[0122] The welding method may be a single layer of weld metal or multi-layer welding. Examples of the welding method include TIG welding (GTAW), shielded metal arc welding (SMAW), flux-cored wire arc welding (FCAW), gas metal arc welding (GMAW), and submerged arc welding (SAW). The welded joint of the alloy material of this embodiment can be manufactured by the above manufacturing process.

[0123] The effects of the alloy material of this embodiment will be explained more specifically using examples. The conditions in the following examples are one example of conditions adopted to confirm the feasibility and effects of the alloy material of this embodiment. Therefore, the alloy material of this embodiment is not limited to this one example of conditions.

[0124] [Production of Alloy Material] Ingots were produced having the chemical compositions shown in Tables 1A and 1B. The ingots were cylindrical with an outer diameter of 120 mm and a mass of 30 kg.

[0125]

[0126]

[0127] In Table 1B, "-" means that the content of the corresponding element was below the impurity level.

[0128] Gleeble test pieces, which will be described later, were taken from the produced ingots. The ingots from which the Gleeble test pieces were taken were hot forged to produce materials (alloy plates) with a thickness of 30 mm. The heating temperature of the ingots in the hot forging was 1100 to 1300°C. The produced materials were subjected to a hot working process. Specifically, the materials were heated in a heating furnace. The heating temperature in the hot working process was 1200°C. The heated materials were hot rolled to produce intermediate alloy materials (alloy plates) with a thickness of 15 mm.

[0129] A heat treatment process was carried out on the intermediate alloy material. The heat treatment temperature T1 (°C) in the heat treatment process was as shown in the "T1 (°C)" column in Table 2. The holding time at the heat treatment temperature was 30 minutes. After the holding time had elapsed, the intermediate alloy material was water-cooled to room temperature. Through the above process, alloy materials (alloy plates) of each test number were produced.

[0130]

[0131] In Table 2, in the "B content type" column, "H" indicates that the B content of the alloy material was more than 0.0010% to 0.0030%. "L" indicates that the B content of the alloy material was 0.0001 to 0.0010%. The "F1", "F2", and "F3" columns show the F1 value, F2 value, and F3 value of each test number. The "FA" column shows the FA value of each test number. The "T1≦FA" column shows "T (True)" when T1 satisfies formula (X), and shows "F (False)" when T1 does not satisfy formula (X).

[0132] [Evaluation Tests] The following evaluation tests were carried out using the manufactured alloy material: (Test 1) Measurement test of Ti content [Ti] and Nb content [Nb] in the residue of the alloy material (Test 2) Gleeble test (evaluation of hot workability) (Test 3) Evaluation test of weld hot cracking resistance (Test 4) Evaluation test of creep strength Each test will be explained below.

[0133] [(Test 1) Measurement test of Ti content [Ti] and Nb content [Nb] in residue of alloy material] Based on the method described in the above [Method for measuring Ti content [Ti] and Nb content [Nb] in residue], the Ti content [Ti] (mass %) and Nb content [Nb] (mass %) in the residue were determined. Note that the test specimens were taken so that the center of a cross section perpendicular to the longitudinal direction of the test specimen was the center of the plate width and the plate thickness of the alloy material (alloy plate), and the longitudinal direction of the test specimen was the longitudinal direction of the alloy material (alloy plate). The size of the test specimen was 10 mm × 30 mm × plate thickness (15 mm). The obtained Ti content [Ti] (mass %) and Nb content [Nb] (mass %) are shown in the "[Ti] (mass %)" and "[Nb] (mass %)" columns in Table 3. The 0.3×[Ti] value and the [Ti]+[Nb] value are shown in the “0.3×[Ti]” and "[Ti]+[Nb]” columns in Table 3.

[0134]

[0135] In Table 3, in the "B content type" column, "H" indicates that the B content of the alloy material was more than 0.0010% to 0.0030%. "L" indicates that the B content of the alloy material was 0.0001 to 0.0010%. In the "Requirement I" column, if the B content of the alloy material was more than 0.0010 to 0.0030% and requirement I was satisfied, "T (True)" was indicated. In the "Requirement II" column, if the B content of the alloy material was more than 0.0010 to 0.0030% and requirement II was satisfied, "T (True)" was indicated. In the "Requirement III" column, if the B content of the alloy material was 0.0001 to 0.0010% and requirement III was satisfied, "T (True)" was indicated. In the "Requirement IV" column, if the B content of the alloy material is 0.0001 to 0.0010% and the requirement IV is satisfied, "T (True)" is shown.

[0136] [(Test 2) Gleeble Test (Evaluation of Hot Workability)] To evaluate the hot workability of the alloy material of each test number, the fracture reduction of area at 900°C was measured using a Gleeble tester. A Gleeble test specimen was taken from the R / 2 position of the ingot (a cylinder with an outer diameter of 120 mm) of each test number. Here, the R / 2 position refers to the center position of the radius in a cross section perpendicular to the axial direction of the ingot. The Gleeble test specimen was a cylindrical test specimen with a radius of 10 mm and a length of 120 mm. The central axis of the Gleeble test specimen was parallel to the axial direction of the ingot. Using the Gleeble tester, the Gleeble test specimen was heated from room temperature to 1200°C in 60 seconds and then held at 1200°C for 300 seconds. Then, it was cooled to 900°C at a cooling rate of 100°C / min using He gas and held at 900°C for 10 seconds. After the holding time had elapsed, the Gleeble test specimen was subjected to a tensile test at a displacement rate of 10 mm / sec to break the Gleeble test specimen. After the break, the dimensions of the cross section of the Gleeble test specimen were measured to determine the reduction in area (%).

[0137] When the reduction of area was 60% or more, the hot workability was evaluated as excellent (shown as "E (Excellent)" in the "Greeble test" column in Table 3). On the other hand, when the reduction of area was less than 60%, the hot workability was evaluated as poor (shown as "B (Bad)" in the "Greeble test" column in Table 3).

[0138] [(Test 3) Evaluation Test for Weld Hot Cracking Resistance] Two test pieces, each having a thickness of 12 mm, a width of 40 mm, and a length of 300 mm, were taken from the alloy material (alloy plate) of each test number, with the center at the center of the plate width. The two test pieces were subjected to the following longitudinal Varestraint test.

[0139] Specifically, TIG fillet welding (bead-on welding) was performed in the longitudinal direction of the widthwise center of each test piece under the conditions of a welding current of 200 A, a voltage of 12 V, and a welding speed of 15 cm / min. During the TIG welding, a bending stress was momentarily applied parallel to the welding direction so as to apply a 2% strain to the surface layer.

[0140] A portion containing a weld crack caused by the application of bending stress was cut out to a size that could be observed with an optical microscope. The cut sample had a thickness of 12 mm, a width of 30 mm, and a length of 30 mm.

[0141] The scale on the weld surface of the cut-out sample was removed by buffing. Then, using a 100x optical microscope, the presence or absence of cracks in the HAZ and, if cracks were present, their lengths were measured. Specifically, the length of cracks that propagated in a direction perpendicular to the welding direction from the boundary between the weld metal and the HAZ (the length perpendicular to the welding direction) was measured. The length of all cracks that occurred in the test piece in the direction perpendicular to the welding direction was determined. The sum of these crack lengths was defined as the total crack length (mm). The total crack length was determined for each of the two test pieces. The arithmetic mean value of the determined total crack lengths was defined as the average total crack length.

[0142] The average total crack length was evaluated as follows: Evaluation E: The average total crack length was 1.5 mm or less. Evaluation G (Good): The average total crack length was more than 1.5 mm and 2.0 mm or less. Evaluation B: The average total crack length was more than 2.0 mm. Evaluation G or E indicated that the specimen had excellent resistance to welding hot cracking (indicated by "G" or "E" in the "resistance to welding hot cracking" column in Table 3). On the other hand, evaluation B indicated that sufficient resistance to welding hot cracking was not obtained (indicated by "B" in the "resistance to welding hot cracking" column in Table 3).

[0143] [(Test 4) Creep Strength Evaluation Test] The following creep evaluation test was conducted on the alloy material (alloy plate) of each test number. A creep rupture test specimen conforming to JIS Z2271:2019 was taken from the center of the plate width and the center of the plate thickness of the alloy material (alloy plate) of each test number. The cross section of the parallel portion of the creep rupture test specimen perpendicular to the axial direction was circular. The outer diameter of the parallel portion was 6 mm, and the length was 30 mm. The longitudinal direction of the creep rupture test specimen was parallel to the rolling direction of the alloy plate.

[0144] The collected creep rupture test specimens were used to conduct creep rupture tests in accordance with JIS Z2271:2019. Specifically, the creep rupture test specimens were heated to 700°C. Then, creep rupture tests were conducted. The test stress was 80 MPa. In the test, the creep rupture time (hours) was determined.

[0145] When the creep rupture time was 2000 hours or more, the creep strength was evaluated as excellent (indicated by "E" in the "Creep Strength" column in Table 3). On the other hand, when the creep rupture time was less than 2000 hours, the creep strength was evaluated as low (indicated by "B" in the "Creep Strength" column in Table 3).

[0146] [Test Results] Referring to Tables 1A, 1B, 2, and 3, in Test Nos. 1 to 30, when the B content was more than 0.0010% but not more than 0.0030%, the alloy materials satisfied Features 1 to 3, and when the B content was 0.0001% to 0.0010%, the alloy materials satisfied Features 1 to 4. Therefore, sufficient creep strength was obtained in high-temperature environments. Furthermore, excellent resistance to weld hot cracking and excellent hot workability were obtained.

[0147] Among Test Nos. 1 to 13 in which the B content was more than 0.0010% to 0.0030%, Test Nos. 2 and 3 further satisfied Requirement I of Feature 5, and Test Nos. 4 to 13 satisfied Requirement II of Feature 5. Therefore, compared with Test No. 1 which did not satisfy Feature 5, the weld hot cracking resistance was even better.

[0148] Among test numbers 14 to 30 in which the B content was 0.0001 to 0.0010%, test numbers 15 to 29 satisfied requirement III of characteristic 6, and test number 30 satisfied requirement IV of characteristic 6. Therefore, compared with test number 14, which did not satisfy characteristic 6, the weld hot cracking resistance was even better.

[0149] On the other hand, in test numbers 31 to 34, although the content of each element in the chemical composition was appropriate, F1 was too low, and therefore sufficient creep strength was not obtained.

[0150] In test numbers 35 to 38, although the content of each element in the chemical composition was appropriate, F1 was too high, and therefore sufficient resistance to weld hot cracking was not obtained.

[0151] In test numbers 39 to 43, the content of each element in the chemical composition was appropriate, but the F2 content was too high, so sufficient resistance to weld hot cracking was not obtained.

[0152] In test numbers 44 and 45, the contents of each element in the chemical composition were appropriate, but the B content was 0.0010% or less and F3 was too high, so sufficient hot workability was not obtained.

[0153] The embodiments of the present invention have been described above. However, the above-described embodiments are merely examples for carrying out the present invention. Therefore, the present invention is not limited to the above-described embodiments, and the above-described embodiments can be appropriately modified and carried out without departing from the spirit of the present invention.

Claims

1. Chemical composition, by mass%, is: C: 0.050-0.100%, Si: 1.00% or less, Mn: 1.50% or less, P: 0.035% or less, S: 0.0015% or less, Cr: 19.00-23.00%, Ni: 30.00-35.00%, N: 0.010% or less, Al: 0.15-0.70%, Ti: 0.15-0.70%, B: 0.0001-0.0030%, Nb: 0.0010-0.5000%, Mo: 0.01-1.00%, Ca: 0.0001-0.0200%, Ta: 0-0.50%, V: 0-1.00%, An alloy material comprising Zr: 0-0.100%, Hf: 0-0.10%, Cu: 0-1.00%, W: 0-1.00%, Co: 0-1.00%, rare earth elements: 0-0.1000%, Mg: 0-0.0200%, and the balance being Fe and impurities, and satisfying formulas (1) and (2), and further satisfying formula (3) when the B content in the chemical composition is 0.0010% or less. 0.60<Al+Ti<1.20 (1) 3.3-41C-Si+2Mo+3Ti+245B-12Nb≦2.00 (2) 0.4+67C+1.3Si+5.5Mo+5.2Ti+13.4Nb≦8.25 (3) Here, the content of the corresponding element in the chemical composition is substituted for each element symbol in formulas (1) to (3) in mass %.

2. The alloy material according to claim 1, wherein the chemical composition contains, in mass%, one or more elements selected from the group consisting of Ta: 0.01-0.50%, V: 0.01-1.00%, Zr: 0.001-0.100%, Hf: 0.01-0.10%, Cu: 0.01-1.00%, W: 0.01-1.00%, Co: 0.01-1.00%, rare earth elements: 0.0001-0.1000%, and Mg: 0.0001-0.0200%.

3. The alloy material according to claim 1 or 2, wherein the chemical composition contains, in mass%, B: more than 0.0010% to 0.0030%, and the Ti content [Ti] in mass% in the residue obtained by the extraction residue method is less than 0.020%, or the [Ti] is 0.020% or more, the Nb content [Nb] in mass% in the residue is 0.015% or more, and the [Ti] and the [Nb] satisfy the formula (4). [Ti] + [Nb] ≧ 0.050 (4) 4. An alloy material according to claim 1 or 2, wherein the chemical composition contains, in mass%, B: 0.0001 to 0.0010%, and the Ti content [Ti] in mass% in the residue obtained by the extraction residue method is 0.031% or less, or the [Ti] is more than 0.031%, and the Nb content [Nb] in mass% in the residue is 0.3 x [Ti]% or more.

Citation Information

Patent Citations

  • HIGH Ni ALLOY AND METHOD FOR PRODUCING HIGH Ni ALLOY

    JP2021070838A

  • HIGH Ni ALLOY EXCELLENT IN WELD HOT CRACKING RESISTANCE

    JP2022163425A

  • HIGH Ni ALLOY EXCELLENT IN WELD HOT CRACKING RESISTANCE

    JP2022163585A

  • HIGH Ni ALLOY EXCELLENT IN WELD HOT CRACKING RESISTANCE

    JP2022163586A

  • Austenite heat-resisting steel and heat treatment technology thereof

    CN106399800A

Cited By

  • Alloy material

    WO2026075177A1