Catalyst, method for producing catalyst, and method for producing bis (aminomethyl) cyclohexane
The use of a catalyst with ruthenium on alumina and specific alkali metal content, optimized through ammonia temperature-programmed desorption, addresses the selectivity limitations of existing catalysts, achieving improved BAC selectivity and yield by reducing impurity production and deammonization reactions.
Patent Information
- Application Number
- PCT/JP2024/012867
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-03
AI Technical Summary
Existing catalysts for the catalytic hydrogenation of xylylene diamine to produce bis(aminomethyl)cyclohexane have limitations in selectivity, with low-boiling impurities as byproducts and acid sites on the catalyst surface influencing impurity production, limiting further improvement in BAC selectivity.
A catalyst with specific physical properties, including a desorption peak amount of 0.020 mmol/g-cat or less, comprising ruthenium (Ru) as the catalyst component supported on alumina, with an alkali metal content of 0.1-10% by mass, and an alkali metal such as sodium (Na), potassium (K), or lithium (Li), is used, along with a method involving ammonia temperature-programmed desorption to optimize hydrogenation conditions.
The catalyst exhibits excellent BAC selectivity, reducing deammonization reactions and improving yield, with a desorption peak amount of 0.015 mmol/g-cat or less, enhancing the hydrogenation ability and selectivity of bis(aminomethyl)cyclohexane production.
Smart Images

Figure JP2024012867_03102024_PF_FP_ABST
Abstract
Description
Catalyst, catalyst production method, and method for producing bis(aminomethyl)cyclohexane
[0001] The present invention relates to a catalyst, a method for producing the catalyst, and a method for producing bis(aminomethyl)cyclohexane.
[0002] Bis(aminomethyl)cyclohexane (hereinafter also referred to as "BAC") is an industrially important compound used as a raw material for polyamides, bis(isocyanatomethyl)cyclohexane, and the like. BAC can be obtained, for example, by catalytic hydrogenation of xylylenediamine. Regarding such catalytic hydrogenation, for example, Patent Document 1 proposes the use of a catalyst prepared by adding an alkali metal modifier as an auxiliary to a ruthenium / alumina catalyst component.
[0003] Chinese Patent Application Publication No. 112473663
[0004] Although the catalyst described in Patent Document 1 is said to improve selectivity, there is a recent trend toward even higher catalytic performance, and therefore there is room for further improvement.
[0005] The present invention has been made in view of the above problems, and an object of the present invention is to provide a catalyst and the like that exhibits excellent BAC selectivity.
[0006] As a result of extensive investigations, the present inventors have found that the above problems can be solved by using a catalyst having predetermined physical properties, and have thus completed the present invention.
[0007] That is, the present invention encompasses the following aspects. [1] A catalyst having hydrogenation ability for producing bis(aminomethyl)cyclohexane, wherein the catalyst has a desorption peak amount of 0.020 mmol / g-cat or less as measured by the ammonia temperature programmed desorption method described below. (Ammonia temperature programmed desorption method) He gas is contacted with 150 mg of the catalyst at 500°C and a gas flow rate of 20 sccm for 30 minutes. Then, 5% by volume of NH 3A mixed gas of He and the remainder He is contacted with the catalyst at 50°C and a gas flow rate of 20 sccm for 10 minutes. Thereafter, while He gas is contacted with the catalyst at a gas flow rate of 20 sccm, the temperature is increased at 10°C / min, and the desorption peak is detected with a thermal conductivity detector. [2] The catalyst according to [1], wherein the catalyst comprises a catalytic component and a support supporting the catalytic component, and the catalytic component comprises Ru. [3] The catalyst according to [1] or [2], wherein the Ru content in the catalyst is 0.1 to 10.0 mass% relative to 100 mass% of the catalyst, and the Na content in the catalyst is 0.1 to 10.0 mass% relative to 100 mass% of the catalyst. [4] The catalyst according to [2] or [3], wherein the support comprises alumina. [5] A method for producing a catalyst according to any one of [1] to [4], comprising: step (a) of reacting a catalyst component with a support to obtain a first reactant; and step (b) of adding an alkali metal to the first reactant to obtain a second reactant. [6] A method for producing a catalyst according to [5], further comprising step (c) of reducing the second reactant to obtain a third reactant, wherein the desorption peak amount of the third reactant measured by the ammonia temperature programmed desorption method is 0.020 mmol / g-cat or less. [7] A method for producing a catalyst according to [6], wherein step (c) is carried out at a temperature of 160 to 360°C. [8] A method for producing a catalyst according to any one of [5] to [7], wherein step (a) comprises adsorbing a Ru raw material solution onto a support, drying the support, and contacting the support with a basic aqueous solution. [9] A method for producing a catalyst according to any one of [5] to [7], wherein the alkali metal comprises at least one selected from the group consisting of Na, K, and Li.
[10] A method for producing bis(aminomethyl)cyclohexane, comprising a hydrogenation step of continuously contacting xylylenediamine with hydrogen in the presence of a catalyst having hydrogenation ability to obtain bis(aminomethyl)cyclohexane, wherein the catalyst exhibits a desorption peak amount of 0.020 mmol / g-cat or less as measured by the ammonia temperature-programmed desorption method described below. (Ammonia temperature-programmed desorption method) He gas is contacted with 150 mg of the catalyst at 500°C and a gas flow rate of 20 sccm for 30 minutes. Then, 5% by volume of NH 3and the remainder He, is contacted with the catalyst at 50°C and a gas flow rate of 20 sccm for 10 minutes. Thereafter, while He gas is contacted with the catalyst at a gas flow rate of 20 sccm, the temperature is increased at a rate of 10°C / min, and the desorption peak is detected with a thermal conductivity detector.
[11] The catalyst includes a catalytic component and a support that supports the catalytic component, and the catalytic component contains Ru.
[12] The catalyst is obtained by production method (A), and the production method (A) includes: a step (a) of reacting the catalytic component with the support to obtain a first reactant; and a step (b) of adding an alkali metal to the first reactant to obtain a second reactant.
[13] The method for producing bis(aminomethyl)cyclohexane according to
[12] , wherein the production method (A) further comprises step (c) of reducing the second reactant to obtain a third reactant, and wherein the desorption peak amount of the third reactant measured by the ammonia temperature programmed desorption method is 0.020 mmol / g-cat or less.
[14] The method for producing bis(aminomethyl)cyclohexane according to
[13] , wherein step (c) is carried out at a temperature of 160 to 360°C.
[15] The method for producing bis(aminomethyl)cyclohexane according to any of
[12] to
[14] , wherein step (a) comprises adsorbing a Ru raw material solution onto a support, drying the adsorbed Ru raw material solution, and contacting the adsorbed Ru raw material solution with a basic aqueous solution.
[16] The method for producing bis(aminomethyl)cyclohexane according to any of
[12] to
[15] , wherein the alkali metal comprises at least one selected from the group consisting of Na, K, and Li.
[17] The method for producing bis(aminomethyl)cyclohexane according to any one of
[10] to
[16] , wherein the Ru content in the catalyst is 0.1 to 10.0 mass% relative to 100 mass% of the catalyst, and the Na content in the catalyst is 0.1 to 10.0 mass% relative to 100 mass% of the catalyst.
[18] The method for producing bis(aminomethyl)cyclohexane according to any one of
[11] to
[17] , wherein the support contains alumina.
[0008] According to the present invention, a catalyst or the like that exhibits excellent BAC selectivity can be provided.
[0009] 7 is a graph showing the results of TPD measurement of the catalyst obtained in Example 1. FIG. 8 is a graph showing the results of multi-point baseline correction of the graph of FIG. 1. FIG. 9 is a graph showing the results of TPD measurement of the catalyst obtained in Comparative Example 1. FIG. 10 is a graph showing the results of multi-point baseline correction of the graph of FIG. 3. FIG. 11 is a graph showing the results of TPD measurement of the catalyst obtained in Comparative Example 2. FIG. 12 is a graph showing the results of multi-point baseline correction of the graph of FIG. 5. FIG. 13 is a graph showing the results of TPD measurement of the catalyst obtained in Comparative Example 3. FIG. 14 is a graph showing the results of multi-point baseline correction of the graph of FIG.
[0010] Hereinafter, a mode for carrying out the present invention (hereinafter referred to as "the present embodiment") will be described in detail. The following present embodiment is an example for explaining the present invention, and is not intended to limit the present invention to the following content. The present invention can be carried out by appropriately modifying it within the scope of its gist.
[0011] <Catalyst> The catalyst of this embodiment is a catalyst for producing bis(aminomethyl)cyclohexane, which has hydrogenation ability, and the catalyst has a desorption peak amount of 0.020 mmol / g-cat or less, as measured by the ammonia temperature-programmed desorption method (hereinafter also referred to as "TPD") described below (hereinafter also referred to as "TPD measurement"). (Ammonia temperature-programmed desorption method) He gas is contacted with 150 mg of the catalyst for 30 minutes at 500°C and a gas flow rate of 20 sccm. Next, 5% by volume of NH 3 A mixed gas of 1,000 sulphite and the remainder He is contacted with the catalyst at 50°C and a gas flow rate of 20 sccm for 10 minutes. Thereafter, while contacting the catalyst with He gas at a gas flow rate of 20 sccm, the temperature is increased at 10°C / min, and the desorption peak is detected with a thermal conductivity detector. The catalyst of this embodiment, configured as described above, exhibits excellent BAC selectivity.
[0012] (TPD Measurement) The catalyst of this embodiment exhibits excellent BAC selectivity because the desorption peak amount measured by the TPD measurement is 0.020 mmol / g-cat or less. The reason for this is not entirely clear, and while it is not intended to limit the reason here, it is speculated as follows. The inventors investigated conventional hydrogenation catalysts for producing BAC and found that low-boiling-point impurities are likely to be generated as by-products in the hydrogenation reaction, which limits the improvement of BAC selectivity. The inventors further investigated the cause of this problem and speculated that, particularly in the hydrogenation reaction for producing BAC, the acid sites on the catalyst surface have a significant impact and are strongly related to the generation of these impurities. Therefore, they speculated that reducing these acid sites would further improve BAC selectivity. Based on this speculation, the inventors continued their investigations and found that, using the desorption peak amount obtained by this measurement as an indicator, BAC selectivity tends to be particularly improved when this value is 0.020 mmol / g-cat or less. Although the detailed mechanism is not entirely clear, the inventors speculate as follows. That is, the reaction substrate and product in this case contain amino groups in their structures, and it is thought that these react strongly with the active sites on the catalyst surface. Specifically, it is thought that the deammonia reaction occurs, which leads to the production of the above impurities (by-products). Therefore, the desorption peak amount obtained in this measurement is used as an index, and by sufficiently reducing this value, it is possible to obtain NH 3 It is believed that this is because the active sites on the catalyst surface that react strongly with the hydroxybenzoate disappear, resulting in the suppression of the deammoniation reaction and improved selectivity. However, the above description merely describes one possible factor that may explain why the catalyst of this embodiment exhibits excellent BAC selectivity, and the mechanism of action of this embodiment is not limited to this. In addition to the above-mentioned viewpoints, from the viewpoint of further improving the BAC yield, the desorption peak amount is preferably 0.015 mmol / g-cat or less. More specifically, the desorption peak amount can be measured based on the method described in the Examples below. The desorption peak amount can be adjusted to the above range, for example, by producing a catalyst based on the production method described below.
[0013] From the viewpoint of catalyst strength, the catalyst of the present embodiment preferably contains a catalyst component and a carrier that supports the catalyst component.
[0014] (Catalyst Component) The catalyst component in this embodiment is not particularly limited, and various known catalyst components can be used. Examples of the catalyst component in this embodiment include Ru, Rh, and Ni, and these can be used alone or in combination of two or more. In this embodiment, from the viewpoint of hydrogenation ability, the catalyst component preferably contains Ru. The catalyst of this embodiment particularly contains a catalyst component and a support that supports the catalyst component, and it is preferable that the catalyst component contains Ru.
[0015] When the catalyst of this embodiment contains Ru, from the viewpoint of hydrogenation ability, the Ru content is preferably 0.1 to 10.0 mass% relative to 100 mass% of the catalyst. The Ru content can be measured by X-ray fluorescence analysis (XRF). Alternatively, the Ru content can be determined as the raw material charging ratio during catalyst production.
[0016] (Carrier) The carrier in this embodiment is not particularly limited as long as it can support the catalyst component, and various known carriers can be used. Examples of the carrier in this embodiment include alumina, diatomaceous earth, and carbon, and these can be used alone or in combination of two or more. In this embodiment, from the viewpoint of catalyst strength, it is preferable that the carrier contains alumina.
[0017] (Alkali Metal) From the viewpoint of hydrogenation ability, the catalyst of this embodiment preferably contains an alkali metal. The alkali metal in this embodiment is distinct from the above-described catalyst components, and its type is not particularly limited, and examples thereof include Li, Na, K, Rb, and Cs. These may be used alone or in combination. From the viewpoint of hydrogenation ability, the alkali metal in this embodiment preferably contains at least one selected from the group consisting of Na, K, and Li. In addition to the above viewpoints, from the viewpoint of further improving the BAC yield, the alkali metal in this embodiment more preferably contains at least one selected from the group consisting of Na and K. When the catalyst of this embodiment contains an alkali metal, from the viewpoint of hydrogenation ability, the content of the alkali metal is preferably 0.1 to 10.0 mass% relative to 100 mass% of the catalyst. In particular, when the catalyst of this embodiment contains Na, from the viewpoint of hydrogenation ability, the content of Na is preferably 0.1 to 10.0 mass% relative to 100 mass% of the catalyst. In particular, the catalyst of this embodiment preferably has a Ru content of 0.1 to 10.0 mass% relative to 100 mass% of the catalyst, and a Na content of 0.1 to 10.0 mass% relative to 100 mass% of the catalyst. The Na content and other alkali metal content can be measured based on the method described in the Examples below. The Na content and other alkali metal content can also be determined as the raw material charging ratio during catalyst production.
[0018] <Method for Producing Catalyst> The method for producing the catalyst of this embodiment is not particularly limited as long as it can produce the catalyst of this embodiment, but it is preferably obtained by the following method. That is, a preferred method for producing the catalyst of this embodiment (hereinafter also referred to as "Production Method (A)") is a method for producing the catalyst of this embodiment, and includes step (a) of reacting a catalyst component with a support to obtain a first reactant, and step (b) of adding an alkali metal to the first reactant to obtain a second reactant. Because Production Method (A) is configured as described above, it can efficiently produce a catalyst that exhibits excellent BAC selectivity.
[0019] (Step (a)) In step (a), a catalyst component and a support are reacted to obtain a first reactant. The catalyst component and support may be appropriately selected from those exemplified in <Catalyst>. The reaction between the catalyst component and the support may be carried out, for example, by the incipient wetness (IW) method under various known conditions, without being limited thereto. In this embodiment, from the viewpoint of the hydrogenation ability of the resulting catalyst, step (a) preferably includes adsorbing a Ru raw material solution onto a support, drying the support, and contacting the support with a basic aqueous solution. The Ru raw material solution may preferably contain, for example, ruthenium chloride n-hydrate, without being limited thereto. The basic aqueous solution may preferably contain, for example, sodium hydroxide, without being limited thereto.
[0020] (Step (b)) In step (b), an alkali metal is added to the first reactant to obtain a second reactant. The second reactant can be used as the catalyst of this embodiment by itself, or can be used as the catalyst of this embodiment after further adjusting performance such as hydrogenation ability through step (c) described below. As the alkali metal, those exemplified in <Catalyst> can be appropriately used. The addition of the alkali metal can be carried out, for example, by the incipient wetness (IW) method under various known conditions, but is not limited to the following. The alkali metal may be added as, for example, a carbonate, hydrogencarbonate, nitrate, hydroxide, or the like, but is not limited to the following. In terms of the hydrogenation ability of the resulting catalyst, the alkali metal in this embodiment preferably includes at least one selected from the group consisting of Na, K, and Li.
[0021] (Step (c)) It is preferable that the production method (A) further includes step (c) of reducing the second reactant to obtain a third reactant. When the third reactant is used as the catalyst of this embodiment, the hydrogenation ability tends to be higher. From the same viewpoint as above, in the production method (A), the desorption peak amount of the third reactant measured by the ammonia temperature programmed desorption method is preferably 0.020 mmol / g-cat or less, more preferably 0.015 mmol / g-cat or less. The temperature condition of step (c) is not particularly limited, but from the viewpoint of the hydrogenation ability of the resulting catalyst, step (c) is preferably carried out at a temperature of 160 to 360°C.
[0022] <Method for Producing Bis(aminomethyl)cyclohexane> The method for producing bis(aminomethyl)cyclohexane of this embodiment (hereinafter also referred to as the "production method of this embodiment") includes a hydrogenation step in which xylylenediamine is continuously contacted with hydrogen in the presence of a catalyst having hydrogenation ability to obtain bis(aminomethyl)cyclohexane, and the catalyst exhibits a desorption peak amount of 0.020 mmol / g-cat or less as measured by the ammonia temperature programmed desorption method described below. (Ammonia temperature programmed desorption method) He gas is contacted with 150 mg of the catalyst at 500°C and a gas flow rate of 20 sccm for 30 minutes. Next, 5% by volume of NH 3 A mixed gas of 1,000 sulphite and the remainder He is contacted with the catalyst at 50°C and a gas flow rate of 20 sccm for 10 minutes. Thereafter, while contacting the catalyst with He gas at a gas flow rate of 20 sccm, the temperature is increased at 10°C / min, and desorption peaks are detected with a thermal conductivity detector. Because the production method of this embodiment is configured as described above, BAC can be produced with high BAC selectivity.
[0023] (Hydrogenation Step) In the hydrogenation step of the present embodiment, bis(aminomethyl)cyclohexane is obtained by continuously contacting xylylenediamine with hydrogen in the presence of a catalyst having hydrogenation ability. That is, continuous hydrogenation of xylylenediamine is carried out. The bis(aminomethyl)cyclohexane obtained by the production method of the present embodiment may be 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, or a mixture thereof.
[0024] In the production method of this embodiment, xylylenediamine, which is one of the raw materials, exists as three isomers: ortho-, meta-, and para-. These isomers can be used alone or as a mixture. In the production method of this embodiment, meta- and para-isomers can be preferably used. That is, the xylylenediamine preferably includes meta-xylylenediamine (hereinafter also referred to as "MXDA") and / or para-xylylenediamine (hereinafter also referred to as "PXDA").
[0025] In the production method of this embodiment, the solvent that can be used is not particularly limited, and various known solvents can be employed. Examples of solvents in this embodiment include, but are not limited to, alkylamines and alkylenediamines. These can be used alone, or two or more can be used in combination. When alkylamines and alkylenediamines are included as solvents, they are separated by distillation from the reaction product and recycled. Therefore, it is preferable to select a solvent having 1 to 18 carbon atoms that is liquid at room temperature for easy recycling in continuous production methods in industrial scale. In this case, the production of by-products tends to be further suppressed and the yield of the target product tends to be further increased. Examples of alkylamines in this embodiment include, but are not limited to, methylamine, dimethylamine, trimethylamine, ethylamine, diethylamine, triethylamine, propylamine, dipropylamine, isopropylamine, diisopropylamine, butylamine, dibutylamine, tributylamine, hexylamine, cyclohexylamine, 2-ethylhexylamine, etc. These can be used alone, or two or more can be used in combination. Examples of alkylenediamines in this embodiment include, but are not limited to, ethylenediamine, propylenediamine, 1,4-butylenediamine, hexamethylenediamine, and bis(aminomethyl)cyclohexane. These may be used alone or in combination of two or more. In this embodiment, bis(aminomethyl)cyclohexane obtained by catalytic reduction can be recycled and reused, and therefore, the solvent in this embodiment preferably contains 1,3-bis(aminomethyl)cyclohexane and / or 1,4-bis(aminomethyl)cyclohexane.
[0026] In the production method of the present embodiment, the mixing weight ratio of the alkylamines and alkylenediamines to the raw material xylylenediamine (amount of xylylenediamine:total amount of alkylamines and alkylenediamines) is not particularly limited, but is preferably 1:30 to 1:1.
[0027] The alkylamines and alkylenediamines may be used alone, as a mixture of the amines and alkylenediamines, or as a mixture with other organic solvents. Examples of organic solvents that can be mixed include, but are not limited to, alcohols such as methanol, ethanol, isopropyl alcohol, and n-propyl alcohol.
[0028] In the hydrogenation step of this embodiment, the hydrogen supply conditions are not particularly limited, but the hydrogen pressure is preferably 5 MPa to 15 MPa, and the hydrogen supply rate per mL of catalyst is preferably 0.5 NmL / min to 2.5 NmL / min. The hydrogen pressure can be specified as a gauge pressure.
[0029] From the viewpoint of hydrogenation ability, the catalyst used in the production method of this embodiment has a desorption peak amount measured by the ammonia temperature programmed desorption method of 0.020 mmol / g-cat or less, and preferably 0.015 mmol / g-cat or less. As the catalyst, those described in the <Catalyst> section can be appropriately used.
[0030] The catalyst in the production method of this embodiment can include a catalyst component and a carrier that supports the catalyst component, and the catalyst component and carrier can be selected from those exemplified in <Catalyst>. From the viewpoint of hydrogenation ability, the catalyst in the production method of this embodiment includes a catalyst component and a carrier that supports the catalyst component, and the catalyst component preferably contains Ru. In the catalyst in the production method of this embodiment, the carrier preferably contains alumina.
[0031] The catalyst used in the production method of this embodiment preferably contains an alkali metal in addition to the catalyst components and the carrier. The alkali metal may be any of those exemplified in the <Catalyst> section, and from the viewpoint of hydrogenation ability, it is preferable that the catalyst contains at least one selected from the group consisting of Na, K, and Li. The catalyst used in the production method of this embodiment preferably has a Ru content of 0.1 to 10.0 mass% relative to 100 mass% of the catalyst, and an alkali metal content of 0.1 to 10.0 mass% relative to 100 mass% of the catalyst. The catalyst used in the production method of this embodiment preferably has a Ru content of 0.1 to 10.0 mass% relative to 100 mass% of the catalyst, and a Na content of 0.1 to 10.0 mass% relative to 100 mass% of the catalyst.
[0032] The catalyst in the production method of this embodiment is obtained by production method (A), which preferably includes step (a) of reacting the catalyst component with the support to obtain a first reactant, and step (b) of adding an alkali metal to the first reactant to obtain a second reactant. The second reactant can be used as the catalyst in the production method of this embodiment, or it can be used as the catalyst in the production method of this embodiment after further adjusting its performance, such as hydrogenation ability, through step (c) described below. Here, production method (A) can be appropriately adopted from those described in the <Catalyst Production Method> section. That is, from the viewpoint of the hydrogenation ability of the resulting catalyst, production method (A) further includes step (c) of reducing the second reactant to obtain a third reactant, and the desorption peak amount of the third reactant measured by the ammonia temperature programmed desorption method is preferably 0.020 mmol / g-cat or less, more preferably 0.015 mmol / g-cat or less. From the viewpoint of the hydrogenation ability of the resulting catalyst, step (a) preferably comprises adsorbing a Ru raw material solution onto a carrier, drying the carrier, and contacting the carrier with a basic aqueous solution. From the viewpoint of the hydrogenation ability of the resulting catalyst, the alkali metal in step (b) preferably comprises at least one selected from the group consisting of Na, K, and Li. From the viewpoint of the hydrogenation ability of the resulting catalyst, step (c) is preferably carried out at a temperature of 160 to 360°C.
[0033] The amount of catalyst used in the production method of this embodiment is not particularly limited, but can be 0.1 to 5.0, preferably 0.1 to 2.0, in terms of WHSV relative to the feed amount of the raw material xylylenediamine. The above amount can be preferably adopted when using a catalyst of this embodiment that supports approximately 2 mass % of ruthenium, but these conditions can also be adopted for other catalysts of this embodiment.
[0034] In the hydrogenation step of this embodiment, the reaction temperature is not particularly limited, but is 50 to 150°C, preferably 80 to 130°C.
[0035] The reactor for carrying out the hydrogenation step in this embodiment is not particularly limited, and for example, a fixed-bed reactor can be used. When the reactor in this embodiment is carried out continuously using a solvent, it may be configured so that dissolved gases are separated from the reaction product using a gas-liquid separator, and then the BAC obtained by catalytic hydrogenation is separated and recycled. Alternatively, it may be configured so that the reaction product after gas-liquid separation can be distilled and separated to remove the solvent in a solvent recovery facility and recycled. In this embodiment, the BAC obtained by catalytic hydrogenation can also be used as a solvent. In this case, it is preferable to separate dissolved gases from the reaction product using a gas-liquid separator and then directly recycle the BAC.
[0036] (Optional Steps) The production method of this embodiment may include an optional step other than the hydrogenation step. The production method of this embodiment may further include, for example, a purification step, although this is not limited to the following. Examples of the purification step include distilling off alkylamines, alkylenediamines, and an organic solvent at normal pressure, followed by vacuum distillation, and the like, which allows the target compound (BAC) to be preferably separated from the reaction product.
[0037] The present embodiment will be described in more detail below with reference to examples, but the scope of the present embodiment is not limited to these examples.
[0038] [Example 1] (Production of catalyst) Using 20 g of alumina, 1 g of ruthenium chloride n-hydrate, and 8 g of water, the catalyst components were supported on the alumina by the incipient wetness (IW) method, and then dried at 120°C to obtain Support 1. Support 1 was subjected to a base treatment using 60 g of 1 M sodium hydroxide and 300 g of water (i.e., Support 1 was contacted with sodium hydroxide and water), and then dried at 110°C to obtain Support 2. To this, 1.0 g of NaHCO 3 and 8 g of water were added by the IW method, and the mixture was dried at 110° C. to obtain the catalyst of Example 1.
[0039] (Amount of alkali metal in catalyst) The amount of alkali metal (amount of Na) contained in the catalyst was analyzed by X-ray fluorescence (XRF) analysis, and was found to be 1.7% by mass, based on 100% by mass of the catalyst. In other words, the amount of alkali metal (amount of Na) was 0.8 mmol / g-cat.
[0040] (TPD Measurement) 150 mg of catalyst was brought into contact with He gas at 500° C. and a gas flow rate of 20 sccm for 30 minutes. Then, 5% by volume of NH 3 A mixed gas of NH and the balance He was contacted with the catalyst at a gas flow rate of 20 sccm at 50°C for 10 minutes. Thereafter, while He gas was contacted with the catalyst at a gas flow rate of 20 sccm, the temperature was raised at 10°C / min, and desorption peaks were detected with a thermal conductivity detector (Microtrac-Bell "BEL-CAT B"). Specifically, the desorption peaks were calculated from the area of the high-temperature peaks vertically divided after multipoint baseline correction of the peaks appearing between 50 and 350°C, and the multipoint baseline correction was performed by a known method using the start and end points of the peaks. The amount of desorption peak (mmol / g-cat) was calculated by multipoint baseline correction of the peaks appearing between 50 and 350°C. 3 That is, the value was calculated using the calibration factor value based on the method described in the "BEL-CAT B" manual (the gas species of the desorption peak was NH 3 It was assumed that the desorption peak amount of Example 1 was 0.005 (mmol / g-cat). The TPD measurement results of the catalyst of Example 1 are shown in Figure 1 (before multi-point baseline correction) and Figure 2 (after multi-point baseline correction). The arrows in each figure correspond to the positions corrected by multi-point baseline correction (selected peak start and end points). As a result of the above, the desorption peak amount of Example 1 was 0.005 (mmol / g-cat).
[0041] (Production of BAC) The following hydrogenation reaction was carried out using a fixed-bed, externally heated flow reactor with an inner diameter of 17 mm and a length of 320 mm. First, hydrogen gas was contacted with 16 mL of catalyst at 260°C and a gas flow rate of 100 mL / min for 7 hours to reduce the catalyst. Next, in the presence of the reduced catalyst, a mixture consisting of meta-xylylenediamine (4% by mass) as a raw material and 1,3-bis(aminomethyl)cyclohexane (96% by mass) as a solvent was supplied to the reactor at a rate of 45 g / hr under the following conditions: catalyst amount 16 mL, reaction temperature 100°C, hydrogen pressure 8.7 MPa (gauge pressure), and hydrogen supply rate 25 NmL / min (1.6 NmL / min per mL of catalyst).
[0042] (Reaction Results) 24 hours after the start of the reaction, the reaction product was collected for 1 hour and analyzed by gas chromatography. The BAC selectivity was 94.2%. The MXDA conversion was 88.9%. The gas chromatographic analysis conditions were as follows, and quantification was performed by the area percentage method. GC apparatus: Shimadzu GC2030 Column: HP-1MS (column with a length of 30 m, an inner diameter of 0.25 mm, and a film thickness of 0.25 μm) Sample introduction temperature: 300°C Split ratio: 10 Temperature program: After holding at 150°C for 5 minutes, the temperature was increased to 300°C (10 minutes), and then held at 300°C for 10 minutes Detector and detection temperature: Flame ionization detector (FID), 300°C Carrier gas: He (46.2 mL / min) Injection amount: 0.2 μL
[0043] (Reduction of catalyst and TPD measurement) Separately, 150 mg of the catalyst obtained in the above "Production of catalyst" (i.e., the catalyst before use in the above "Production of BAC") was contacted with hydrogen gas at 260°C and a gas flow rate of 50 sccm for 30 minutes to reduce the catalyst. Next, the reduced catalyst was contacted with He gas at 500°C and a gas flow rate of 20 sccm for 30 minutes. Next, 5% by volume of NH 3A mixed gas of 1000 ppm ...
[0044] [Example 2] In the preparation of the catalyst of Example 1, 1.0 g of NaHCO 3 Instead of 1.0 g of K 2 CO 3 The catalyst of Example 2 was obtained in the same manner as in Example 1, except that the catalyst used was a catalyst having a MXDA selectivity of 94.2%. The amount of alkali metal and TPD measurement were also carried out for the obtained catalyst in the same manner as in Example 1. As a result, the desorption peak amount for Example 2 was 0.002 (mmol / g-cat). Furthermore, BAC was produced in the same manner as in Example 1 using the catalyst of Example 2, and the reaction results were evaluated. The BAC selectivity was 94.2%. The MXDA conversion was 90.7%. The above results are shown in Table 1.
[0045] [Example 3] In the production of the catalyst of Example 1, 1.0 g of NaHCO 3 A catalyst of Example 3 was obtained in the same manner as in Example 1, except that 1.0 g of LiOH was used instead of 1.0 g of HCl. The amount of alkali metal in the obtained catalyst was measured in the same manner as in Example 1, and TPD measurement was also carried out. As a result, the desorption peak amount in Example 3 was 0.019 (mmol / g-cat). Furthermore, BAC was produced using the catalyst of Example 3 in the same manner as in Example 1, and the reaction results were evaluated. The BAC selectivity was 94.0%. The above results are shown in Table 1.
[0046] [Example 4] In the production of the catalyst of Example 1, 1.0 g of NaHCO 3 Instead, 4.0 g of LiNO 3The catalyst of Example 4 was obtained in the same manner as in Example 1, except that the catalyst used was a catalyst containing 100% methyl methacrylate (MSM). The alkali metal content of the obtained catalyst was measured in the same manner as in Example 1, and TPD measurement was also performed. As a result, the desorption peak amount of Example 4 was 0.001 (mmol / g-cat). Furthermore, BAC was produced using the catalyst of Example 4 in the same manner as in Example 1, and the reaction results were evaluated. The BAC selectivity was 94.3%. The BAC yield was higher than that of Example 3. The above results are shown in Table 1. Furthermore, the catalyst of Example 4 was reduced and TPD measurement was performed in the same manner as in Example 1. As a result, the desorption peak amount of the catalyst after reduction was 0.001 (mmol / g-cat), which was in good agreement with the value before reduction.
[0047] [Comparative Example 1] In the production of the catalyst of Example 1, 1.0 g of NaHCO 3 The obtained support 2 was used as the catalyst of Comparative Example 1 without adding any alkali metals. The amount of alkali metals was measured for the catalyst of Comparative Example 1 in the same manner as in Example 1, and TPD analysis was also performed. As a result, the desorption peak amount for Comparative Example 1 was 0.036 (mmol / g-cat). Furthermore, BAC was produced using the catalyst of Comparative Example 1 in the same manner as in Example 1, and the reaction results were evaluated. The BAC selectivity was 91.8%. The BAC yield was lower than that of Example 1. The above results are shown in Table 1. The TPD analysis results for the catalyst of Comparative Example 1 are shown in Figure 3 (before multi-point baseline correction) and Figure 4 (after multi-point baseline correction). The arrows in each figure correspond to the positions corrected by multi-point baseline correction (selected peak start and end points).
[0048] [Comparative Example 2] A catalyst was produced under the same production conditions as in Example 10 of Patent Document 1, and designated the catalyst of Comparative Example 2. That is, using 10 g of alumina, 1 g of ruthenium chloride n-hydrate, and 200 g of water, the catalytic components were supported on the alumina by equilibrium adsorption (12-hour immersion), and then dried at 100°C for 12 hours to obtain supported material a. Supported material a was calcined at 500°C in air to obtain supported material b. Supported material b was contacted with 10% hydrogen / nitrogen gas at 150°C for 10 hours to obtain supported material c. Supported material c was then contacted with 0.5 g of Na 2 CO 3Na was added by equilibrium adsorption using 200 g of HCl and water, and the mixture was dried to obtain a catalyst of Comparative Example 2. TPD measurement was performed on the catalyst of Comparative Example 2 in the same manner as in Example 1. The TPD measurement results for the catalyst of Comparative Example 2 are shown in Figure 5 (before multi-point baseline correction) and Figure 6 (after multi-point baseline correction). The arrows in each figure correspond to the positions corrected by multi-point baseline correction (selected peak start and end points). As a result, the desorption peak amount for Comparative Example 2 was 0.054 (mmol / g-cat).
[0049] Comparative Example 3 A catalyst was produced under the same production conditions as Comparative Example 1 of Patent Document 1, and designated as the catalyst of Comparative Example 3. TPD measurement was carried out on the catalyst of Comparative Example 3 in the same manner as in Example 1. The TPD measurement results for the catalyst of Comparative Example 3 are shown in Figure 7 (before multi-point baseline correction) and Figure 8 (after multi-point baseline correction). The arrows in each figure correspond to the positions corrected by multi-point baseline correction (selected peak start and end points). As a result, the desorption peak amount of Comparative Example 3 was 0.023 (mmol / g-cat).
[0050]
[0051] It was evaluated that the catalyst production methods of Comparative Examples 2 and 3, in which the alkali metal is added by the equilibrium adsorption method, make it difficult to control the amount of alkali metal taken into the catalyst, and as a result, it also tends to be difficult to control the desorption peak amount. In contrast, the catalyst production methods of Examples 1 to 4, in which the alkali metal is added by the IW method after the base treatment, make it easier to control the amount of alkali metal taken into the catalyst than in Comparative Examples 2 and 3, and as a result, it also tends to be easier to control the desorption peak amount.
[0052] It was confirmed that the BAC selectivity was higher in all of Examples 1 to 4 compared to Comparative Example 1. Furthermore, the BAC yield in Examples 1 and 2 was higher than that in Examples 3 and 4, and there was a tendency for the alkali metals Na and K to further improve not only the selectivity but also the yield. In this comparison, in light of the level of performance currently required of catalysts, a difference in BAC selectivity or BAC yield of more than 0.1 was evaluated as being significant.
[0053] Comparative Example 4 BAC was produced in the same manner as in Comparative Example 1, except that in the production of BAC in Comparative Example 1, the raw material was changed from meta-xylylenediamine (4 mass%) to para-xylylenediamine (4 mass%) and the solvent was changed from 1,3-bis(aminomethyl)cyclohexane to 1,4-bis(aminomethyl)cyclohexane, and the reaction results were evaluated (BAC selectivity and PXDA conversion were calculated).
[0054] [Example 5] BAC was produced in the same manner as in Comparative Example 4, except that the catalyst of Example 1 was used instead of the catalyst of Comparative Example 4, and the reaction results were evaluated. The BAC selectivity of Example 5 was 0.5% higher than the BAC selectivity of Comparative Example 4. The PXDA conversion of Example 5 was 4.0% higher than the PXDA conversion of Comparative Example 4. The yield of Example 5 was 4.2% higher than the yield of Comparative Example 4.
[0055] [Example 6] BAC was produced in the same manner as in Comparative Example 4, except that the catalyst of Example 2 was used instead of the catalyst of Comparative Example 4, and the reaction results were evaluated. The BAC selectivity of Example 6 was 1.1% higher than the BAC selectivity of Comparative Example 4. The PXDA conversion of Example 6 was 4.2% higher than the PXDA conversion of Comparative Example 4. The yield of Example 6 was 5.0% higher than the yield of Comparative Example 4.
[0056] Comparing Examples 5 and 6 with Comparative Example 4, it can be seen that the catalysts of Examples 1 and 2 exhibit higher catalytic performance than the catalyst of Comparative Example 1, even when PXDA is used as a raw material for BAC production.
[0057] This application is based on a Japanese patent application (Patent Application No. 2023-058039) filed on March 31, 2023, the contents of which are incorporated herein by reference.
Claims
1. A catalyst having hydrogenation ability for producing bis(aminomethyl)cyclohexane, the catalyst having a desorption peak amount of 0.020 mmol / g-cat or less as measured by the following ammonia temperature programmed desorption method. (Ammonia temperature programmed desorption method) He gas is contacted with 150 mg of the catalyst at 500° C. and a gas flow rate of 20 sccm for 30 minutes. Then, 5% by volume of NH 3 and the remainder He, is contacted with the catalyst at a gas flow rate of 20 sccm for 10 minutes at 50° C. Thereafter, while contacting the catalyst with He gas at a gas flow rate of 20 sccm, the temperature is increased at 10° C. / min, and the desorption peak is detected with a thermal conductivity detector.
2. The catalyst according to claim 1, wherein the catalyst comprises a catalyst component and a support for supporting the catalyst component, and the catalyst component comprises Ru.
3. The catalyst according to claim 2, wherein the Ru content in the catalyst is 0.1 to 10.0 mass % relative to 100 mass % of the catalyst, and the Na content in the catalyst is 0.1 to 10.0 mass % relative to 100 mass % of the catalyst.
4. The catalyst of claim 3, wherein the support comprises alumina.
5. A method for producing the catalyst according to claim 1, comprising: a step (a) of reacting a catalyst component with a support to obtain a first reactant; and a step (b) of adding an alkali metal to the first reactant to obtain a second reactant.
6. The method for producing a catalyst according to claim 5, further comprising a step (c) of reducing the second reactant to obtain a third reactant, wherein the desorption peak amount of the third reactant measured by the ammonia temperature programmed desorption method is 0.020 mmol / g-cat or less.
7. The method for producing a catalyst according to claim 6, wherein the step (c) is carried out at a temperature of 160 to 360°C.
8. The method for producing a catalyst according to claim 5, wherein the step (a) comprises adsorbing the Ru raw material solution onto a support, drying the support, and contacting the support with a basic aqueous solution.
9. The method for producing a catalyst according to claim 5, wherein the alkali metal comprises at least one selected from the group consisting of Na, K and Li.
10. A method for producing bis(aminomethyl)cyclohexane, comprising a hydrogenation step of continuously contacting xylylenediamine with hydrogen in the presence of a catalyst having hydrogenation ability to obtain bis(aminomethyl)cyclohexane, wherein the catalyst has a desorption peak amount of 0.020 mmol / g-cat or less as measured by the ammonia temperature programmed desorption method described below. (Ammonia temperature programmed desorption method) He gas is contacted with 150 mg of the catalyst at 500° C. and a gas flow rate of 20 sccm for 30 minutes. Then, 5% by volume of NH 3 and the remainder He, is contacted with the catalyst at a gas flow rate of 20 sccm for 10 minutes at 50° C. Thereafter, while contacting the catalyst with He gas at a gas flow rate of 20 sccm, the temperature is increased at 10° C. / min, and the desorption peak is detected with a thermal conductivity detector.
11. The method for producing bis(aminomethyl)cyclohexane according to claim 10, wherein the catalyst comprises a catalyst component and a support for supporting the catalyst component, and the catalyst component comprises Ru.
12. The method for producing bis(aminomethyl)cyclohexane according to claim 11, wherein the catalyst is obtained by a production process (A), the production process (A) comprising: a step (a) of reacting the catalyst component with the support to obtain a first reactant; and a step (b) of adding an alkali metal to the first reactant to obtain a second reactant.
13. The method for producing bis(aminomethyl)cyclohexane according to claim 12, wherein the production method (A) further comprises a step (c) of reducing the second reactant to obtain a third reactant, and the amount of desorption peak of the third reactant measured by the ammonia temperature programmed desorption method is 0.020 mmol / g-cat or less.
14. The method for producing bis(aminomethyl)cyclohexane according to claim 13, wherein step (c) is carried out at a temperature of 160 to 360°C.
15. The method for producing bis(aminomethyl)cyclohexane according to claim 14, wherein the step (a) comprises adsorbing the Ru raw material solution onto a carrier, drying the carrier, and contacting the carrier with a basic aqueous solution.
16. The method for producing bis(aminomethyl)cyclohexane according to claim 15, wherein the alkali metal comprises at least one selected from the group consisting of Na, K and Li.
17. The method for producing bis(aminomethyl)cyclohexane according to claim 16, wherein the Ru content in the catalyst is 0.1 to 10.0 mass % relative to 100 mass % of the catalyst, and the Na content in the catalyst is 0.1 to 10.0 mass % relative to 100 mass % of the catalyst.
18. The method for producing bis(aminomethyl)cyclohexane according to claim 17, wherein the support comprises alumina.
Citation Information
Patent Citations
Transmitting device, receiving device and program
JP2023058039A
Catalyst for preparing 1,3-cyclohexane dimethylamine through m-xylylenediamine selective hydrogenation
CN109772312A
Catalyst for synthesis of bis(aminomethyl)cyclohexane and preparation method and application thereof
CN110433823A
Catalyst for preparing alicyclic amine from aromatic amine as well as preparation method and application of catalyst
CN112473663A
Anti-deamination hydrogenation catalyst as well as preparation method and application thereof
CN114160127A
Cited By
Catalyst, method for producing catalyst, and method for producing bis (aminomethyl) cyclohexane
WO2026204668A1
Catalyst, method for producing catalyst, and method for producing bis(aminomethyl)cyclohexane
WO2026204669A1