Photoelectric conversion element and production method for same
The photoelectric conversion element employs a metal layer as a light shielding layer between substrates to prevent UV-induced deterioration, addressing the cost and efficiency issues in dye-sensitized solar cells by maintaining power generation characteristics and reducing manufacturing costs.
Patent Information
- Application Number
- PCT/JP2024/012880
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-03
AI Technical Summary
Dye-sensitized solar cells face deterioration in power generation characteristics due to ultraviolet irradiation during the curing of the sealing material, which increases manufacturing costs and reduces workability due to the need for masking equipment.
A photoelectric conversion element with a transparent first and second substrate, a metal layer between the substrates, and conductive layers to prevent ultraviolet rays from reaching the porous semiconductor layer, using a metal layer as a light shielding layer to block UV rays during curing.
Suppresses deterioration of power generation characteristics and reduces manufacturing costs by eliminating the need for UV masking, while enhancing photoelectric conversion efficiency through improved light management.
Smart Images

Figure JP2024012880_03102024_PF_FP_ABST
Abstract
Description
Photoelectric conversion element and its manufacturing method
[0001] The present disclosure relates to a photoelectric conversion element and a method for manufacturing the photoelectric conversion element.
[0002] Solar cells using crystalline silicon substrates and thin-film silicon solar cells are known as solar cells that convert sunlight into electricity. Crystalline silicon solar cells use silicon substrates, while thin-film silicon solar cells require various semiconductor manufacturing gases and equipment, which increases the manufacturing costs of both. In response to this, it has been proposed to use photoelectric conversion elements that utilize photoinduced electron transfer in metal complexes in dye-sensitized solar cells, without using silicon substrates or other materials that increase manufacturing costs.
[0003] In this type of photoelectric conversion element, oxide semiconductor particles are sensitized by a sensitizing dye that absorbs incident light such as sunlight, and can convert light energy into electricity. For example, Patent Document 1 discloses a dye-sensitized solar cell that includes a first substrate, a counter electrode disposed on the first substrate, a current extraction electrode, a porous semiconductor layer disposed on the current extraction electrode, an electrolyte solution containing a redox electrolyte dissolved therein, a second substrate disposed above the porous semiconductor layer with a predetermined gap therebetween, and a sealant disposed between the first and second substrates and sealing the electrolyte solution. It also discloses the use of an ultraviolet-curable resin as the sealant.
[0004] JP 2014-203539 A
[0005] In the manufacturing process of a dye-sensitized solar cell having the above-described configuration, the first and second substrates are placed facing each other and bonded together with a sealant. After bonding, ultraviolet (UV) light is irradiated from the outside of the first substrate side to cure the UV-curable resin that constitutes the sealant. However, if the UV light strikes the porous semiconductor layer of the working electrode during this curing process, the sensitizing dye may deteriorate, resulting in a decrease in power generation characteristics. While masking the working electrode during UV irradiation is considered, this approach requires special equipment for masking and the work of removing the masking material, which increases manufacturing costs and reduces workability, making it undesirable.
[0006] In view of the above-mentioned problems, the present disclosure has an object to provide a photoelectric conversion element capable of suppressing a decrease in power generation characteristics caused by curing a sealing material by ultraviolet irradiation, and a method for manufacturing the same.
[0007] The solution of the present disclosure for achieving the above object is a photoelectric conversion element having a first substrate having optical transparency, a second substrate having optical transparency and disposed opposite the first substrate, a sealant that seals the gap between the first substrate and the second substrate, and an electrolyte medium filled between the first substrate and the second substrate sealed with the sealant, wherein the element includes a first conductive layer disposed on the electrolyte medium side of the first substrate, a porous semiconductor layer that is disposed on the electrolyte medium side of the first conductive layer and supports a sensitizing dye, a second conductive layer disposed on the electrolyte medium side of the second substrate, and a catalyst layer that is disposed on the electrolyte medium side of the second conductive layer, and wherein a metal layer is stacked between the second substrate and the second conductive layer, and the metal layer is covered by the second conductive layer.
[0008] In the photoelectric conversion element, the metal layer is preferably disposed in a range overlapping the porous semiconductor layer in a plan view.
[0009] In the photoelectric conversion element, the metal layer is preferably a layer containing one or more metals selected from the group consisting of aluminum, copper, molybdenum, tantalum, titanium, and tungsten, or a metal nitride of the metal.
[0010] In the photoelectric conversion element, the metal layer includes a first metal layer provided on the second substrate side and a second metal layer stacked on the first metal layer on the side opposite to the second substrate side, the first metal layer being preferably formed of one or more metals selected from the group consisting of aluminum, copper, molybdenum, tantalum, titanium, and tungsten, and the second metal layer preferably containing silver. The second metal layer may also be configured to contain a metal having a higher reflectivity than the first metal layer.
[0011] In the photoelectric conversion element, it is preferable that the second substrate has at least one alignment mark on a plane thereof, and that the alignment mark is made of the same material as the constituent material of the metal layer.
[0012] The present disclosure also encompasses a method for manufacturing a photoelectric conversion element according to each of the above-described solutions, which is characterized in that, in the step of forming the metal layer, the metal layer is formed on the second substrate and at least one alignment mark is formed on the second substrate.
[0013] According to the present disclosure, it is possible to suppress a decrease in power generation characteristics caused by curing the sealing material by ultraviolet irradiation.
[0014] FIG. 1 is a cross-sectional view schematically showing a photoelectric conversion element according to a first embodiment of the present disclosure. FIG. 2 is a plan view showing a second substrate of the photoelectric conversion element. FIG. 3 is a plan view showing the positional relationship between a metal layer and a porous semiconductor layer on a second substrate included in the photoelectric conversion element. FIG. 4 is a cross-sectional view schematically showing a photoelectric conversion element according to a second embodiment of the present disclosure. FIG. 5 is a cross-sectional view schematically showing a photoelectric conversion element according to a third embodiment of the present disclosure. FIG. 6 is a table showing configuration examples of examples and comparative examples of photoelectric conversion elements according to the present disclosure.
[0015] Hereinafter, a photoelectric conversion element according to an embodiment of the present disclosure will be described with reference to the drawings.
[0016] The photoelectric conversion element according to this embodiment includes at least a first substrate and a second substrate that are optically transparent and face each other, a sealing material that seals the gap between the first substrate and the second substrate, an electrolyte medium that is filled between the first substrate and the second substrate, a first conductive layer provided on the electrolyte medium side of the first substrate, a porous semiconductor layer provided on the electrolyte medium side of the first conductive layer, a second conductive layer provided on the electrolyte medium side of the second substrate, and a catalyst layer provided on the electrolyte medium side of the second conductive layer.
[0017] In the photoelectric conversion element, the first substrate and the first conductive layer constitute one electrode (first electrode), which is an electrode substrate having a porous semiconductor layer carrying at least a photosensitizing dye. This first electrode is also called a photoelectrode. The second substrate and the second conductive layer constitute the other electrode (second electrode), which functions as a counter electrode of the first electrode, the photoelectrode.
[0018] In the following embodiments, common components are designated by common reference numerals, and redundant explanations are omitted.
[0019] First Embodiment FIG. 1 is a cross-sectional view schematically showing a photoelectric conversion element 1 according to a first embodiment.
[0020] As shown in the figure, the photoelectric conversion element 1 includes a first substrate 21, a second substrate 31 disposed opposite the first substrate 21, a sealant 41 that seals the gap between the first substrate 21 and the second substrate 31, and an electrolyte medium 43 filled between the first substrate 21 and the second substrate 31. Furthermore, a first conductive layer 23 is provided on the first substrate 21 facing the electrolyte medium 43, and a porous semiconductor layer 25 carrying a sensitizing dye is provided on the first conductive layer 23 facing the electrolyte medium 43. Furthermore, a second conductive layer 33 is provided on the second substrate 31 facing the electrolyte medium 43, and a catalyst layer 37 is provided on the second conductive layer 33 facing the electrolyte medium 43.
[0021] On the first electrode side, which serves as the negative electrode, a first substrate 21, a first conductive layer 23, and a porous semiconductor layer 25 are provided in this order, and on the second electrode side, which serves as the positive electrode, a second substrate 31, a second conductive layer 33, and a catalyst layer 37 are provided in this order. A metal layer 35 is further provided between the second substrate 31 and the second conductive layer 33.
[0022] The first substrate 21 is a non-conductive plate-like or sheet-like member that is light-transmitting (optically transparent), and a transparent glass substrate, plastic substrate, or the like can be used. The first substrate 21 is preferably selected so as to sufficiently transmit light of a wavelength that excites the sensitizing dye in the porous semiconductor layer 25. The glass substrate can be, for example, a glass substrate made of soda glass, fused silica glass, or crystalline silica glass.
[0023] The second substrate 31 of the counter electrode is a non-conductive plate-like or sheet-like member having light transmissivity (light transparency), and may be a transparent glass substrate, a plastic substrate, etc. The second substrate 31 is preferably selected so as to sufficiently transmit light of a wavelength for curing the sealing material 41 described below.
[0024] In the description of the photoelectric conversion element according to the present disclosure, the term "transparent" refers to a transmittance of about 50% or more, and is also used to mean colorless and transparent to visible light. Visible light has a wavelength of about 360 nm to 830 nm, and corresponds to an energy of about 3.45 eV to 1.49 eV. A material having a transmittance of 50% or more in this range is considered transparent.
[0025] The first conductive layer 23 is made of a material that is transparent to visible light and has electrical conductivity, such as fluorine-doped tin oxide (FTO), indium-tin composite oxide (ITO), or tin oxide (SnO 2 ), and is preferably formed of a transparent conductive oxide (TCO) such as zinc oxide (ZnO).
[0026] The thickness (average film thickness) of the first conductive layer 23 is preferably, for example, 20 nm or more and 5000 nm or less, and more preferably 100 nm or more. If the thickness of the first conductive layer 23 is 100 nm or more, the electrical resistance value of the first conductive layer 23 is reduced, thereby increasing the amount of current that can be extracted to the outside of the photoelectric conversion layer. If the thickness of the first conductive layer 23 is 5000 nm or less, a decrease in the amount of light passing through the first conductive layer 23 is prevented, thereby achieving high photoelectric conversion efficiency. The lower the electrical resistance value of the first conductive layer 23, the more preferable it is, and for example, 40 Ω / sq or less is preferable.
[0027] The second conductive layer 33 on the second substrate 31 can be configured in the same manner as the first conductive layer 23. The thickness of the second conductive layer 33 is preferably set to, for example, 20 nm or more and 5000 nm or less.
[0028] The porous semiconductor layer 25 can have various shapes, such as a bulk shape, a particulate shape, or a layer shape having many fine pores, but preferably has a porous structure capable of supporting a sensitizing dye. Examples of semiconductor materials constituting the porous semiconductor layer 25 include titanium oxide, zinc oxide, tin oxide, iron oxide, niobium oxide, cerium oxide, tungsten oxide, barium titanate, strontium titanate, cadmium sulfide, lead sulfide, zinc sulfide, indium phosphide, copper indium sulfide (CuInS 2 ), CuAlO 2 , and SrCu 2 O 2 From the viewpoint of high stability, the porous semiconductor layer 25 is preferably made of titanium oxide.
[0029] The titanium oxide used to form the porous semiconductor layer 25 may be, for example, anatase titanium oxide, rutile titanium oxide, amorphous titanium oxide, various titanium oxides in the narrow sense such as metatitanic acid and orthotitanic acid, titanium hydroxide, or hydrous titanium oxide, either alone or in combination. The two types of crystalline titanium oxide, anatase and rutile, can take either form depending on the production method and thermal history, but crystalline titanium oxide is generally of the anatase type.
[0030] The semiconductor may be in the form of either a single crystal or a polycrystal. From the standpoints of stability, ease of crystal growth, and manufacturing costs, polycrystals are preferred, and it is preferable to use nanoscale or microscale semiconductor particles made of polycrystals. Therefore, it is preferable to use titanium oxide particles as the material for the porous semiconductor layer 25. Titanium oxide particles can be manufactured by, for example, a liquid-phase method such as hydrothermal synthesis or sulfuric acid synthesis, or a gas-phase method. They can also be manufactured by high-temperature hydrolysis of chlorides, a method developed by Degussa.
[0031] The semiconductor fine particles may be a mixture of two or more different particle sizes of the same or different semiconductor compounds. It is believed that semiconductor fine particles with a large particle size contribute to improving the light absorption rate by scattering incident light, while semiconductor fine particles with a small particle size contribute to improving the amount of sensitizing dye adsorbed by increasing the surface area.
[0032] The thickness of the porous semiconductor layer 25 is preferably, for example, 0.1 μm or more and 100 μm or less. The specific surface area of the porous semiconductor layer 25 is preferably 10 m 2 / g or more 200m 2 The porosity of the porous semiconductor layer 25 is preferably, for example, 40% or more and 75% or less.
[0033] The porous semiconductor layer 25 may be composed of multiple layers of semiconductor particles with different particle diameters. A layer of large particles with an average particle diameter, for example, 100 nm to 500 nm, may be stacked on a layer of small particles with an average particle diameter, for example, 5 nm to 50 nm. In this case, the ratio of the average particle diameters of the layers is preferably 10 times or more.
[0034] As the sensitizing dye carried on the porous semiconductor layer 25, one or more of various organic dyes and metal complex dyes that have absorption in the visible light region or infrared light region can be selectively used.
[0035] The organic dye may be, for example, at least one selected from the group consisting of azo dyes, quinone dyes, quinoneimine dyes, quinacridone dyes, squarylium dyes, cyanine dyes, merocyanine dyes, triphenylmethane dyes, xanthene dyes, porphyrin dyes, perylene dyes, indigo dyes, and naphthalocyanine dyes. The absorption coefficient of an organic dye is generally greater than that of a metal complex dye in which a molecule is coordinately bonded to a transition metal.
[0036] Metal complex dyes are formed by a metal being coordinately bonded to a molecule. Examples of the molecule include porphyrin dyes, phthalocyanine dyes, naphthalocyanine dyes, and pyridine dyes. Examples of the metal include at least one selected from the group consisting of Cu, Ni, Fe, Co, V, Sn, Si, Ti, Ge, Cr, Zn, Ru, Mg, Al, Pb, Mn, In, Mo, Y, Zr, Nb, Sb, La, W, Pt, Ta, Ir, Pb, Os, Ga, Tb, Eu, Rb, Bi, Se, As, Sc, Ag, Cd, Hf, Re, Au, Ac, Tc, Te, and Rh. Among these, metal complex dyes preferably include those in which a metal is coordinated to a phthalocyanine dye or a pyridine dye, and particularly preferably include Ru metal complex dyes. As the Ru metal complex dye, for example, Ru metal complex dyes such as Ruthenizer 535 dye, Ruthenizer 535-bisTBA dye, or Ruthenizer 620-1H3TBA dye, which are trade names of Solaronix, can be used.
[0037] A co-adsorbent may also be supported on the porous semiconductor layer 25. The co-adsorbent suppresses association and aggregation with the sensitizing dye, and allows the sensitizing dye to be adsorbed in a uniformly dispersed state on the porous semiconductor layer 25. The co-adsorbent can be appropriately selected from common materials in the field in accordance with the sensitizing dye to be combined.
[0038] The electrolyte medium 43 is typically an electrolytic solution and includes a carrier transport material. The carrier transport material is preferably a conductive material capable of transporting ions, such as a liquid electrolyte, a solid electrolyte, a gel electrolyte, or a molten salt gel electrolyte. The electrolytic solution is a liquid containing a redox pair, and can be a liquid consisting of a redox pair and a solvent capable of dissolving the pair, a liquid consisting of a redox pair and a molten salt capable of dissolving the pair, or a liquid consisting of a redox pair, a solvent capable of dissolving the pair, and a molten salt.
[0039] The liquid electrolyte is preferably a liquid containing redox species, and is not particularly limited as long as it can generally be used in batteries, solar cells, etc. Specifically, the liquid electrolyte is preferably one consisting of a redox species and a solvent capable of dissolving the redox species, one consisting of a redox species and a molten salt capable of dissolving the redox species, or one consisting of a redox species, the solvent, and the molten salt.
[0040] The redox species is, for example, I - / I 3 - System, Br 2 - / Br 3 - system, Fe 2+ / Fe 3+ system, Co 2+ / Co 3+ Cu system + / Cu 2+ Specifically, the redox species include metal iodides and iodine (I 2 ), a salt consisting of iodide ions and iodine (I 2 ) or a combination of a metal bromide and bromine (Br 2 As the metal iodide, for example, lithium iodide (LiI), sodium iodide (NaI), potassium iodide (KI), and calcium iodide (CaI) are preferably used in combination. 2 ) can be used.
[0041] As the salt consisting of iodide ions, for example, at least one of ammonium salts and imidazolium salts can be used. As the ammonium salt, for example, at least one of tetraethylammonium iodide (TEAI), tetrapropylammonium iodide (TPAI), tetrabutylammonium iodide (TBAI), and tetrahexylammonium iodide (THAI) can be used. As the imidazolium salt, for example, at least one of dimethylpropylimidazole iodide (DMPII), methylpropylimidazole iodide (MPII), ethylmethylimidazole iodide (EMII), ethylimidazole iodide (EII), and hexylmethylimidazole iodide (HMII) can be used.
[0042] Examples of the solvent include carbonate solvents such as propylene carbonate, nitrile solvents such as acetonitrile, alcohol solvents such as ethanol, and lactone solvents such as gamma-butyrolactone. Two or more of these solvents can also be mixed and used. The solvent is selected comprehensively from the viewpoints of solvent viscosity, electrolyte solubility, etc., depending on the temperature environment in which the dye-sensitized solar cell using the photoelectric conversion element 1 is installed.
[0043] The catalyst layer 37 is formed, for example, from a thin film of Pt, carbon, or a conductive polymer. The conductive polymer may be, for example, PEDOT or PEDOT:PSS. Pt can be formed by methods such as screen printing, sputtering, thermal decomposition of chloroplatinic acid, and electrodeposition. From the viewpoint of minimizing the use of expensive Pt, a layer formed by thermal decomposition of chloroplatinic acid is particularly preferred. The thickness of the catalyst layer 37 is not particularly limited, but when Pt is used, a thickness of 1 nm to 300 nm is preferred. Alternatively, the catalyst layer 37 can be formed by dispersing the material in any solvent into a paste form and applying it by screen printing or the like.
[0044] The sealant 41 seals and bonds the first substrate 21 and the second substrate 31. In this embodiment, as shown in FIG. 1 , the sealant 41 is provided between the first conductive layer 23 on the first substrate 21 and the second conductive layer 33 on the second substrate 31 to seal and bond the first substrate 21 and the second substrate 31. The sealant 41 can be formed using, for example, a material including at least one selected from the group consisting of silicone resin, acrylic resin, epoxy resin, polyisobutylene-based resin, hot-melt resin, and glass-based resins such as glass frit. In particular, it is preferable to use an ultraviolet-curable resin for the sealant 41 because it has a fast curing rate and reduces working time.
[0045] A metal layer 35 is provided between the second conductive layer 33 and the second substrate 31. As shown in Fig. 1 , the metal layer 35 is laminated on the surface of the second substrate 31 facing the second conductive layer 33 (the surface facing the electrolyte medium 43), and the second conductive layer 33 is laminated on the metal layer 35 facing the electrolyte medium 43. The metal layer 35 is provided on the inner side (the second substrate 31 side) of the second conductive layer 33, and the surface of the metal layer 35 that is not in contact with the second substrate 31 is entirely covered with the second conductive layer 33.
[0046] The metal layer 35 is a layer containing one metal selected from the group consisting of aluminum, copper, molybdenum, tantalum, titanium, and tungsten, or a metal nitride of one metal selected from the group. The metal layer 35 may be a combination of two or more metals selected from the group, or a multi-layer structure containing one or two metals selected from the group and the metal nitride. Therefore, the metal layer 35 may be a single layer structure of the metal, a single layer structure of the metal nitride, or a multi-layer structure of the metal and the metal nitride. Such a metal layer 35 can be formed by a method such as sputtering, thermal CVD, or vapor deposition.
[0047] For example, the metal layer 35 may have a single layer structure of molybdenum tungsten (MoW). Alternatively, the metal layer 35 may contain the metal nitride, for example, a multi-layer structure of titanium nitride (TiN), aluminum (Al), and titanium (Ti). In this case, the metal layer 35 is stacked in the order titanium nitride, aluminum, and titanium from the second substrate 31 side.
[0048] 2 is a plan view showing the second substrate 31 in one step of the manufacturing process of the photoelectric conversion element 1. During manufacturing, alignment marks are formed on the first substrate 21 and the second substrate 31. For example, as shown in FIG. 2, two second alignment marks 52 are formed at diagonally opposite corners on the plane of the rectangular second substrate 31. Similarly, first alignment marks 51 are formed at diagonally opposite corners on the plane of the first substrate 21.
[0049] These first alignment marks 51 and second alignment marks 52 are provided, for example, at positions that enable alignment between the first substrate 21 and the second substrate 31. The first alignment marks 51 and the second alignment marks 52 can be used for alignment when the first substrate 21 and the second substrate 31 are bonded together.
[0050] As described above, the metal layer 35 is provided on the second substrate 31. In this case, if the metal layer 35 and the second alignment mark 52 formed on the second substrate 31 are made of the same material, the metal layer 35 can be formed simultaneously in the step of forming the second alignment mark 52 on the second substrate 31. In other words, in the step of forming the metal layer 35, the metal layer 35 can be formed on the second substrate 31 while the second alignment mark 52 is also formed on the second substrate 31.
[0051] 3 is a plan view showing the positional relationship between the metal layer 35 on the second substrate 31 and the porous semiconductor layer 25. The metal layer 35 is arranged in a range that overlaps with the porous semiconductor layer 25 in a plan view. The area of the metal layer 35 on the second substrate 31 is set to be equal to or larger than the area (installation area) of the porous semiconductor layer 25 on the first conductive layer 23. As also shown in FIG. 1 , in the cross section of the photoelectric conversion element 1, the metal layer 35 and the porous semiconductor layer 25 are arranged in a position that overlaps with each other in the thickness direction (the vertical direction in the figure).
[0052] 3, the size of the metal layer 35 is preferably such that the metal layer 35 of the second substrate 31 covers the entire porous semiconductor layer 25 in a plan view and does not overlap with the sealing material 41. The thickness of the metal layer 35 is preferably 20 nm to 300 nm.
[0053] 1, when the first substrate 21 and the second substrate 31 are integrated, ultraviolet light is irradiated onto the sealing material 41 from the side of the second substrate 31. In the area where the metal layer 35 is provided on the sealing material 41 made of ultraviolet curing resin, the metal layer 35 and the porous semiconductor layer 25 overlap in the direction of incidence of the ultraviolet light. Ultraviolet light of, for example, 200 nm to 400 nm used to cure the sealing material 41 is blocked by the metal layer 35, and is prevented from entering the porous semiconductor layer 25.
[0054] This allows the metal layer 35 to function as a light-shielding layer for the porous semiconductor layer 25, preventing ultraviolet light from entering the porous semiconductor layer 25, and also allows the ultraviolet-curable resin constituting the sealing material 41 to be cured well, thereby integrating the first substrate 21 and the second substrate 31. This also makes it possible to prevent situations in which the molecular structure of the sensitizing dye in the porous semiconductor layer 25 is denatured or the photoelectric conversion efficiency is reduced due to ultraviolet light irradiation.
[0055] Furthermore, since the metal layer 35 blocks ultraviolet light from entering the porous semiconductor layer 25, there is no need to use a mask for blocking ultraviolet light in the manufacturing process of the photoelectric conversion element 1. When the photoelectric conversion element 1 is used to form a dye-sensitized solar cell, the manufacturing cost can be reduced.
[0056] In addition, providing the metal layer 35 in the photoelectric conversion element 1 can increase the conductivity of the second electrode including the second substrate 31. Because the metal layer 35 is covered with the second conductive layer 33, corrosion is suppressed even when the electrolyte medium 43 contains iodine.
[0057] By using a material with high reflectivity for the metal layer 35, light that is not completely absorbed by the sensitizing dye in the porous semiconductor layer 25 and that passes through is reflected by the metal layer 35 and absorbed again by the porous semiconductor layer 25, thereby making it possible to increase the photoelectric conversion efficiency.
[0058] It should be noted that the first alignment mark 51 and the second alignment mark 52 do not necessarily have to be provided in positions that allow them to be aligned with each other, and may be used for purposes other than aligning the first substrate 21 and the second substrate 31.
[0059] 4 is a cross-sectional view that schematically shows a photoelectric conversion element 1 according to embodiment 2. In the photoelectric conversion element 1 according to this embodiment, the porous semiconductor layer 25 has a laminated structure.
[0060] The porous semiconductor layer 25 is laminated on the electrolyte medium 43 side of the first conductive layer 23, and an absorption layer 26 and a reflection layer 27 are laminated on top of each other in this order. The reflection layer 27 is made of fine particles having a larger particle diameter than the absorption layer 26. The average particle diameter of the reflection layer 27 can be, for example, 100 nm or more and 500 nm or less. The absorption layer 26 is made of fine particles having a smaller particle diameter than the reflection layer 27, and the average particle diameter can be, for example, 5 nm or more and 50 nm or less. The ratio of the average particle diameter of the reflection layer 27 to that of the absorption layer 26 is preferably 10 times or more.
[0061] When the sealing material 41 is cured by ultraviolet irradiation, the reflective layer having a large particle size can protect the sensitizing dye adsorbed in the absorption layer. Therefore, by providing the reflective layer 27 in addition to the configuration shown in the first embodiment, it is possible to cure the sealing material 41 without reducing the photoelectric conversion efficiency.
[0062] The absorption layer 26 and the reflection layer 27 may be made of the same material as the porous semiconductor layer 25. The absorption layer 26 and the reflection layer 27 may be made of the same material or different materials.
[0063] 5 is a cross-sectional view schematically illustrating a photoelectric conversion element 1 according to embodiment 3. In the photoelectric conversion element 1 according to this embodiment, the metal layer 35 has a multi-layer structure including a first metal layer 351 provided on the second substrate 31 side and a second metal layer 352 stacked on the first metal layer 351 on the side opposite to the second substrate 31 side. That is, within the second conductive layer 33 provided on the second substrate 31, the first metal layer 351 and the second metal layer 352, which are in contact with the second substrate 31, are provided in this order, and are covered with the second conductive layer 33.
[0064] The first metal layer 351 is formed of one or more metals selected from the group consisting of aluminum, copper, molybdenum, tantalum, titanium, and tungsten, or a combination thereof, while the second metal layer 352 is configured as a reflective layer containing a metal having a higher reflectivity than the first metal layer 351. The thickness of each of the first metal layer 351 and the second metal layer 352 is preferably 50 nm.
[0065] The first metal layer 351 and the second metal layer 352 are less susceptible to corrosion because they are covered with the second conductive layer 33, and for example, silver (Ag) can be used for the second metal layer 352. This increases the reflectance of the second metal layer 352 and improves the conductivity, thereby further increasing the photoelectric conversion efficiency.
[0066] 6 is a table showing the configurations of examples and comparative examples of photoelectric conversion elements. As examples of photoelectric conversion elements according to the present disclosure, the thicknesses of the metal layers were varied as follows, and a power consumption of 1 kW / m was applied to each photoelectric conversion element. 2 The photoelectric conversion efficiency was measured by irradiating the device with light (AM1.5 solar simulator) with an intensity of 1000 kJ / cm.
[0067] In Example 1, a first conductive layer made of ITO (average film thickness: 300 nm) was formed on a transparent glass substrate. A commercially available titanium oxide paste (manufactured by JGC Catalysts and Chemicals, product name: PST-18NR) with an average particle size of 18 nm was applied onto the first conductive layer using a screen plate and a screen printer, and leveling was carried out at room temperature for 10 minutes. The resulting coating was dried for 20 minutes in an oven set at 120°C, and then baked in air for 60 minutes in a baking furnace set at 500°C. This formed a porous semiconductor layer.
[0068] Next, a dye adsorption solution was prepared. Specifically, a mixed solvent of anhydrous acetonitrile and anhydrous t-butanol in a volume ratio of 1:1 was prepared. A dye (manufactured by Solaronix, trade name: Ruthenizer, 620-1H3TBA) was dissolved in the solvent for the dye adsorption solution thus prepared at 3 × 10 mol / L.
[0069] Next, the first substrate on which the porous semiconductor layer was formed was immersed in the prepared dye adsorption solution at room temperature for 24 hours. Thereafter, it was washed with ethanol and dried at 60° C. for about 5 minutes. This allowed the dye contained in the dye adsorption solution to be adsorbed into the porous semiconductor layer.
[0070] On another glass substrate, a second alignment mark and a metal layer were formed by sputtering, and on the metal layer, a second conductive layer made of ITO (thickness: approximately 300 nm) and a catalyst layer made of Pt (thickness: approximately 50 nm) were formed by sputtering.
[0071] An ultraviolet curing resin (ThreeBond Corporation, THREEBOND 3035B) was used as the sealing material. After the sealing material was applied to the first substrate, the first and second substrates were bonded in place by aligning the first and second alignment marks. The sealing material was then cured by irradiating it with ultraviolet light from the second substrate side.
[0072] Next, an electrolyte solution (electrolyte medium) was injected through holes previously formed on the second substrate, and the holes were then sealed with the above-described ultraviolet curable resin, thereby filling the gap between the dye-adsorbed porous semiconductor layer and the catalyst layer, thereby producing the photoelectric conversion element of Example 1.
[0073] The electrolyte solution was prepared as follows: Methylpropylimidazolium iodide was dissolved in acetonitrile as a solvent to a concentration of 0.6 mol / L, and I was added to the solvent to a concentration of 0.05 mol / L. 2 Further, t-butylpyridine was dissolved in the above solvent to a concentration of 0.5 mol / L, and LiI was dissolved in the above solvent to a concentration of 0.1 mol / L.
[0074] In Example 1, a photoelectric conversion element was manufactured using MoW as the metal layer with a thickness of 50 nm. The photoelectric conversion efficiency (hereinafter simply referred to as conversion efficiency) was 7.80%.
[0075] In Example 2, a photoelectric conversion element was manufactured with a metal layer having a thickness of 100 nm, and the conversion efficiency was 7.86%.
[0076] In Example 3, a photoelectric conversion element was manufactured with a metal layer having a thickness of 200 nm, and the conversion efficiency was 7.95%.
[0077] As a comparative example, a photoelectric conversion element was manufactured without forming a metal layer, and the conversion efficiency was 7.16%.
[0078] It was confirmed that the photoelectric conversion elements of Examples 1 to 3 had higher conversion efficiencies than the comparative example. The reason for the decrease in conversion efficiency in the comparative example is thought to be the absence of a metal layer. It was confirmed that the decrease in conversion efficiency was suppressed in Examples 1 to 3, which had a metal layer.
[0079] The above-disclosed embodiments are illustrative in all respects and are not intended to be limiting. Therefore, the technical scope of the present disclosure should not be interpreted solely by the above-disclosed embodiments, but should be defined by the claims. Furthermore, all modifications within the scope and meaning equivalent to the claims are included.
[0080] This application claims priority from Japanese Patent Application No. 2023-058705, filed in Japan on March 31, 2023, the entire contents of which are incorporated herein by reference.
[0081] REFERENCE SIGNS LIST 1 Photoelectric conversion element 21 First substrate 23 First conductive layer 25 Porous semiconductor layer 26 Absorption layer 27 Reflection layer 31 Second substrate 33 Second conductive layer 35 Metal layer 351 First metal layer 352 Second metal layer 37 Catalyst layer 41 Sealant 43 Electrolyte medium 51 First alignment mark 52 Second alignment mark
Claims
1. A photoelectric conversion element having a first substrate having optical transparency, a second substrate having optical transparency and disposed opposite the first substrate, a sealant that seals the gap between the first substrate and the second substrate, and an electrolyte medium filled between the first substrate and the second substrate sealed with the sealant, the photoelectric conversion element including a first conductive layer disposed on the electrolyte medium side of the first substrate, a porous semiconductor layer that is disposed on the electrolyte medium side of the first conductive layer and supports a sensitizing dye, a second conductive layer disposed on the electrolyte medium side of the second substrate, and a catalyst layer disposed on the electrolyte medium side of the second conductive layer, wherein a metal layer is laminated between the second substrate and the second conductive layer, and the metal layer is covered by the second conductive layer.
2. A photoelectric conversion element according to claim 1, characterized in that the metal layer is arranged in a range overlapping the porous semiconductor layer in a plan view.
3. A photoelectric conversion element according to claim 1 or 2, characterized in that the metal layer is a layer containing one or more metals selected from the group consisting of aluminum, copper, molybdenum, tantalum, titanium and tungsten, or a metal nitride of the metal.
4. A photoelectric conversion element as described in claim 1 or 2, characterized in that the metal layer includes a first metal layer provided on the second substrate side and a second metal layer stacked on the first metal layer on the side opposite the second substrate side, the first metal layer being formed from one or more metals selected from the group consisting of aluminum, copper, molybdenum, tantalum, titanium, and tungsten, and the second metal layer containing silver.
5. A photoelectric conversion element as described in claim 1 or 2, characterized in that the metal layer includes a first metal layer provided on the second substrate side and a second metal layer stacked on the first metal layer on the opposite side to the second substrate side, and the second metal layer has a higher reflectivity than the first metal layer.
6. A photoelectric conversion element as described in claim 1, characterized in that the second substrate has at least one alignment mark on a flat surface, and the alignment mark is made of the same material as the constituent material of the metal layer.
7. A method for manufacturing a photoelectric conversion element as described in claim 6, characterized in that in the step of forming the metal layer, the metal layer is formed on the second substrate and at least one alignment mark is formed on the second substrate.
Citation Information
Patent Citations
Dye-sensitized solar cell and electrode therefor
JP2004296669A
Dye sensitized solar battery and module thereof
JP2005056613A
Dye-sensitized solar cell
JP2005142090A
Mesh electrode substrate, organic solar cell element, and organic solar cell element module
JP2012221814A
Solar cell and manufacturing method for dye-sensitized solar cell
WO2014157060A1