Reactor, method for producing metal nitride catalyst, and method for synthesizing ammonia
The use of a metal nitride catalyst in a reactor with specific properties allows for efficient ammonia synthesis at low temperatures and pressures, addressing the inefficiencies of existing methods and providing a cost-effective and stable solution for ammonia production.
Patent Information
- Application Number
- PCT/JP2024/012909
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-03
AI Technical Summary
Current ammonia synthesis methods using the Haber-Bosch process require high temperature and high pressure, leading to increased equipment costs and power consumption, and existing catalysts face issues with stability, oxidation resistance, and cost-effectiveness, making it difficult to achieve efficient ammonia production at lower reaction temperatures and pressures.
A reactor using a metal nitride catalyst with a specific formula (MNx) where M is a metal element with a Fermi energy higher than -4.4 eV and x allows a rock salt structure, supported with transition metal elements, and an oxygen content of 15 at% or less, which is heat-treated and used in a honeycomb structure for ammonia synthesis at 300°C or lower and 0.9 MPa or lower pressure.
The solution enables stable, industrially viable ammonia synthesis at normal pressure and low temperature, reducing equipment costs and power consumption while maintaining high reaction efficiency, with the metal nitride catalyst effectively activating nitrogen and hydrogen to produce ammonia.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure 00000020_0000 
Figure 00000020_0001
Abstract
Description
Reactor, method for producing metal nitride catalyst, and method for synthesizing ammonia
[0001] The present invention relates to a reactor, a method for producing a metal nitride catalyst, and a method for synthesizing ammonia.
[0002] Ammonia is an important chemical substance used in the synthesis of chemical fertilizers, acrylonitrile, nitric acid, and other products, and is produced by the Haber-Bosch process. The Haber-Bosch process uses nitrogen and hydrogen as raw materials and a catalyst to synthesize ammonia. However, this synthesis requires high temperature and pressure conditions, which increases equipment costs and power consumption, and requires complex processes to reduce energy loss.
[0003] If ammonia synthesis under low-pressure and low-temperature conditions were possible, it would be possible to reduce equipment costs and power consumption and simplify the process. Therefore, the development of catalysts for synthesizing ammonia under low-pressure and low-temperature conditions is underway.
[0004] For example, Patent Document 1 proposes a catalyst containing one element selected from the group consisting of molybdenum, tungsten, rhenium, iron, cobalt, ruthenium, and osmium, or a combination of iron and ruthenium, ruthenium and rhenium, or iron and molybdenum, potassium or sodium, and alumina, thoria, zirconia, or silica, in which the transition metal and alkali metal are substantially in a metallic state. The conditions for synthesizing ammonia using this catalyst are a reaction temperature of 150 to 450°C and a reaction pressure of 50 to 2000 kg / cm. 2 (about 5 to about 200 MPa).
[0005] Patent Document 2 describes 15 cm -3A catalyst has been proposed in which a metal element of Groups 6 to 9 (e.g., Ru) is supported on a mayenite-type compound (e.g., electride) containing the above conduction electrons. The conditions for ammonia synthesis using this catalyst are described as a reaction temperature of 100 to 600°C and a reaction pressure of 10 kPa to 30 MPa. Patent Document 3 proposes a catalyst in which a transition metal (e.g., Ru) is supported on a metal oxyhydride. The conditions for ammonia synthesis using this catalyst are described as a reaction temperature of 200 to 600°C and a reaction pressure of 0.01 to 20 MPa.
[0006] Non-Patent Document 1 proposes a catalyst in which Ni is supported on a metal nitride (CeN), and describes that the nitrogen vacancies in the metal nitride activate both nitrogen and hydrogen. The conditions for ammonia synthesis using this catalyst are a reaction pressure of 0.1 to 0.9 MPa and a reaction temperature of 150 to 400°C. However, considering the amount of ammonia produced, a reaction temperature of 300 to 400°C is presumed to be appropriate.
[0007] Japanese Patent Publication No. 51-47674 International Publication No. 2012 / 077658 International Publication No. 2021 / 006136
[0008] Tian-Nan Ye and 6 others, “Contribution of Nitrogen Vacancies to Ammonia Synthesis over Metal Nitride Catalysts”, JACS, 2020, 142, 14374-14383
[0009] Although the catalyst of Patent Document 1 can synthesize ammonia under conditions of lower pressure and temperature than conventional conditions, these levels cannot be said to be sufficient. 15 cm -3The production of the mayenite type compound containing the above-mentioned conduction electrons is costly and time-consuming, and control of the production conditions is difficult, so it is not suitable for mass production. The catalyst of Patent Document 3 is an unstable material with insufficient oxidation resistance, making it difficult to handle industrially. The catalyst of Non-Patent Document 1 still requires a high reaction temperature among the ammonia synthesis conditions. Note that, although the above explanations of the problems of the prior art have focused on ammonia synthesis, it is also desirable to reduce the reaction temperature and reaction pressure in syntheses other than ammonia synthesis from the viewpoint of reducing facility costs and power consumption.
[0010] The present invention has been made to solve the above-mentioned problems, and aims to provide a reactor that uses a metal nitride catalyst that can be supplied industrially and stably, and that is capable of carrying out a predetermined reaction even at low reaction temperatures and reaction pressures. Another aim of the present invention is to provide a method for producing a metal nitride catalyst that can be supplied industrially and stably, and that is capable of carrying out a predetermined reaction even at low reaction temperatures and reaction pressures. A further aim of the present invention is to provide a method for synthesizing ammonia that is capable of synthesizing ammonia even at atmospheric pressure and at a reaction temperature of 300°C or less.
[0011] The present inventors have conducted extensive research to solve the above problems and have found that certain metal nitrides are useful as catalysts, leading to the completion of the present invention. That is, the present invention is exemplified as follows.
[0012] [1] A reactor comprising a metal nitride catalyst represented by the general formula MNx (M is a metal element having a Fermi energy higher than −4.4 eV vs. LV, and x is a range in which a rock salt structure can be formed).
[0013] [2] The reactor according to [1], wherein M is at least one metal element selected from Ti, Hf, Ta, Mo, Cr, V, and Zr.
[0014] [3] The reactor according to [1] or [2], wherein x is 0.4 or more and less than 1.0.
[0015] [4] The metal nitride catalyst has a specific surface area of 0.1 m 2 / g or more.
[0016] [5] The reactor according to any one of [1] to [4], wherein the oxygen content of the metal nitride catalyst is 15 atomic % or less.
[0017] [6] The reactor according to any one of [1] to [5], wherein at least one transition metal element selected from transition metal elements of groups 6, 7, 8, 9, 10, 11, and 12 is supported on the metal nitride catalyst.
[0018] [7] The reactor according to [6], wherein the supported transition metal element is at least one selected from Ru, Ni, and Fe.
[0019] [8] The reactor according to [6] or [7], wherein the supported amount of the transition metal element is 0.1 mass% or more.
[0020] [9] The reactor according to any one of [1] to [5], which is used for ammonia synthesis.
[0021]
[10] The reactor according to any one of [6] to [8], which is used for ammonia synthesis.
[0022]
[11] The reactor according to any one of [1] to
[10] , further comprising a honeycomb structure having an outer peripheral wall and partition walls disposed inside the outer peripheral wall and defining a plurality of cells extending from a first end face to a second end face, wherein the metal nitride catalyst is held in the partition walls of the honeycomb structure.
[0023]
[12] The reactor according to
[11] , wherein the honeycomb structure is made of cordierite or a Si—SiC-based material.
[0024]
[13] A method for producing a metal nitride catalyst, comprising heat-treating a metal nitride represented by the general formula MN (M is a metal element having a Fermi energy higher than −4.4 eV vs. LV) at 1200 to 1800° C. under vacuum conditions.
[0025]
[14] A method for synthesizing ammonia, comprising reacting nitrogen and hydrogen over the metal nitride catalyst using the reactor according to any one of [1] to
[12] .
[0026]
[15] The method for synthesizing ammonia according to
[14] , which is carried out at a temperature of 300°C or less and a pressure of 0.9 MPa or less.
[0027]
[16] 5,000hr -1 The method for synthesizing ammonia according to
[14] or
[15] , which is carried out under the above space velocity.
[0028] According to the present invention, it is possible to provide a reactor that uses a metal nitride catalyst that can be supplied industrially in a stable manner and that is capable of carrying out a predetermined reaction even at low reaction temperatures and reaction pressures. Furthermore, according to the present invention, it is possible to provide a method for producing a metal nitride catalyst that can be supplied industrially in a stable manner and that is capable of carrying out a predetermined reaction even at low reaction temperatures and reaction pressures. Furthermore, according to the present invention, it is possible to provide a method for synthesizing ammonia that is capable of synthesizing ammonia even at atmospheric pressure and at a reaction temperature of 300°C or less.
[0029] 1 is a schematic diagram of a cross section of a reactor having a honeycomb structure, the cross section being parallel to the direction in which cells extend. FIG. 2 is a schematic diagram of a cross section of the reactor of FIG. 1 taken along line aa'.
[0030] The following is a detailed description of the embodiments of the present invention. The present invention is not limited to the following embodiments, and it should be understood that modifications and improvements made to the following embodiments based on the ordinary knowledge of those skilled in the art without departing from the spirit of the present invention are also within the scope of the present invention.
[0031] (1. Reactor) The reactor according to the embodiment of the present invention is equipped with a metal nitride catalyst. The metal nitride catalyst used in the reactor according to the embodiment of the present invention can activate nitrogen and hydrogen, and can therefore be used as a catalyst in various reaction systems that use nitrogen and / or hydrogen as raw materials. In particular, the metal nitride catalyst used in the reactor according to the embodiment of the present invention is suitable for use as a catalyst for ammonia synthesis using nitrogen and hydrogen as raw materials.
[0032] The metal nitride catalyst used in the reactor according to the embodiment of the present invention is represented by the general formula MNx (M is a metal element having a Fermi energy higher than −4.4 eV vs. L.V., and x is a range in which a rock salt structure can be formed). When such a metal nitride catalyst is brought into contact with nitrogen and hydrogen, it can activate the nitrogen and hydrogen, and therefore can carry out a predetermined reaction even at low reaction temperatures and pressures (particularly, it can synthesize ammonia even at atmospheric pressure and at a reaction temperature of 300° C. or less).
[0033] M in the general formula MNx is not particularly limited as long as it is a metal element whose Fermi energy is higher than -4.4 eV vs. L.V., but can be, for example, at least one metal element selected from Ti, Hf, Ta, Mo, Cr, V, and Zr. When M is one of these exemplified metal elements, MN is expressed as TiN, HfN, TaN, MoN, CrN, VN, or ZrN. The Fermi energies of these MNs are as follows: TiN: -4.1 eV HfN: -4.3 eV TaN: -4.4 eV MoN: -4.2 eV CrN: -4.0 eV VN: -3.9 eV ZrN: -4.1 eV
[0034] Furthermore, M in the general formula MNx is preferably Ti from the viewpoints of stability at room temperature and in the atmosphere, stable industrial supply, etc. That is, MN is preferably TiN.
[0035] The value of x in the general formula MNx is not particularly limited as long as it is within a range that allows a rock salt structure to be formed. When M in the general formula MNx is one of the metal elements exemplified above, the range of x that allows a rock salt structure to be formed is 0.4 to 1.2, and preferably 0.5 to 1.1.
[0036] The metal nitride catalyst represented by the general formula MNx is preferably anion deficient. The anion deficient metal nitride catalyst converts hydrogen into hydride ions (H -) due to its strong reducing properties. Hydride ions can easily react with N to produce specific compounds such as ammonia. When a metal nitride catalyst is anion-deficient, x in the general formula MNx is 0.4 or more and less than 1.0, preferably 0.5 to 0.9, and more preferably 0.6 to 0.8. The general formula MNx of a metal nitride catalyst can be identified by measurement using TEM-EDX (energy dispersive X-ray spectroscopy). Specifically, a line analysis is performed from the exterior to the interior of the metal nitride catalyst, and the content [atomic %] of each element (M and N) is measured at a position 10 nm from the surface, and x can be calculated from the element content ratio (N / M).
[0037] The metal nitride catalyst represented by the general formula MNx has a specific surface area of 0.1 m 2 / g or more. If the specific surface area is in this range, a sufficient contact area with hydrogen and nitrogen can be secured, and the production amount of a predetermined compound such as ammonia can be increased. From the viewpoint of stably obtaining this effect, the specific surface area of the metal nitride catalyst is preferably 0.2 to 100 m 2 / g, and more preferably 0.3 to 80m 2 / g. The specific surface area of the metal nitride catalyst can be measured by the BET method. The adsorbed gas molecules used in the BET method can be gas molecules such as nitrogen, argon, and krypton.
[0038] The metal nitride catalyst represented by the general formula MNx preferably has an oxygen content of 15 atomic % or less. With such an oxygen content, hydrogen molecules are more likely to dissociate on the surface of the metal nitride catalyst to generate hydride ions. From the viewpoint of stably obtaining this effect, the oxygen content of the metal nitride catalyst is more preferably 12 atomic % or less, and even more preferably 10 atomic % or less. Here, the oxygen content of the metal nitride catalyst refers to the oxygen content [atomic %] obtained by measuring each element by the above-mentioned TEM-EDX.
[0039] The shape of the metal nitride catalyst represented by the general formula MNx is not particularly limited, and can be in various forms such as a lump such as a pellet, a powder, or a film. When the metal nitride catalyst is in powder form, its average particle size is generally 1 nm to 10 μm. Here, in this specification, the "average particle size" refers to the particle size at 50% of the integrated value (D50) in the particle size distribution determined by a laser diffraction / scattering method.
[0040] The metal nitride catalyst represented by the general formula MNx functions as a catalyst by itself, but may optionally support at least one transition metal element selected from the transition metal elements of groups 6, 7, 8, 9, 10, 11, and 12. These transition metal elements are used as homogeneous and heterogeneous catalysts in various reaction systems. Therefore, by supporting these transition metal elements on a metal nitride catalyst, it can be used as a catalyst in various reaction systems. Examples of transition metal elements in group 6 include Cr, Mo, and W. Examples of transition metal elements in group 7 include Mn, Tc, and Re. Examples of transition metal elements in group 8 include Fe, Ru, and Os. Examples of transition metal elements in group 9 include Co, Rh, and Ir. Examples of transition metal elements in group 10 include Ni, Pd, and Pt. Examples of transition metal elements in group 11 include Cu, Ag, and Au. Examples of transition metal elements in group 12 include Zn, Cd, and Hg. These transition metal elements may be used alone or in combination of two or more thereof. Intermetallic compounds of these transition metal elements may also be used.
[0041] Among the above-mentioned various elements, when used as a catalyst for ammonia synthesis, the transition metal elements are preferably Cr, Mo, Mn, Re, Fe, Ru, Os, Co, Rh, Ni, Pd, and Pt, more preferably Mo, Re, Fe, Ru, Os, Co, and Ni, and even more preferably Ru, Ni, and Fe. These transition metal elements have high bond energy with nitrogen, and can increase the amount of ammonia produced.
[0042] The amount of the transition metal element supported is not particularly limited, but is preferably 0.1 mass% or more, more preferably 0.3 to 40 mass%, and even more preferably 0.5 to 20 mass%. Such a supported amount can fully ensure the effects of supporting the transition metal element. Here, the supported amount of the transition metal element in this specification refers to the ratio of the transition metal element to the total amount of the metal nitride catalyst and the transition metal element.
[0043] The method for producing a metal nitride catalyst represented by the general formula MNx is not particularly limited, and it can be produced according to a known method. Metal nitrides are commercially available, and such commercially available metal nitrides may also be used as catalysts. Anion-deficient metal nitride catalysts (metal nitride catalysts in which x in the general formula MNx is 0.4 or more and less than 1.0) can be produced by heat-treating a metal nitride represented by the general formula MN (M is a metal element whose Fermi energy is higher than 4.4 eV vs. L.V.) under vacuum conditions at 1200 to 1800°C, preferably 1300 to 1700°C. The heat-treatment time is not particularly limited, but is generally 1 to 10 hours, preferably 2 to 5 hours.
[0044] When a predetermined transition metal element is supported on a metal nitride catalyst, the supporting method is not particularly limited, and known methods can be used. For example, when the metal nitride catalyst is in the form of a powder, the transition metal element can be supported by impregnation, physical mixing, or the like. In this case, a transition metal compound may be used as a source of the transition metal element, and the transition metal compound may be impregnated into the metal nitride catalyst or physically mixed with the metal nitride catalyst, and then the transition metal compound may be thermally decomposed to obtain the transition metal element. The thermal decomposition temperature may be set appropriately depending on the type of transition metal compound used, and is not particularly limited. Furthermore, when the metal nitride catalyst is in the form of a block or a film, the transition metal element can be supported by impregnation, CVD, sputtering, or the like.
[0045] The transition metal compound used as a supply source of the transition metal element is not particularly limited as long as it is thermally decomposable, and examples thereof include inorganic transition metal compounds and organic transition metal compounds. 12 ], dichlorotetrakis(triphenylphosphine)ruthenium(II) [RuCl2(PPh3)4], dichlorotris(triphenylphosphine)ruthenium(II) [RuCl2(PPh3)3], tris(acetylacetonato)ruthenium(III) [Ru(acac)3], ruthenocene [Ru(C5H5)], ruthenium chloride [RuCl3], iron pentacarbonyl [Fe(CO)5], iron tetracarbonyl iodide [Fe(CO)4I2], iron chloride [FeCl3], ferrocene [Fe(C5H5)2], tris(acetylacetonato)iron(III) [Fe(acac)3], triiron dodecacarbonyl [Fe3(CO) 12 ], nickel chloride [NiCl2], nickel(II) acetylacetonate [Ni(acac)2], tetracarbonyl nickel [Ni(CO)4], etc. These can be used alone or in combination of two or more.
[0046] A reactor according to an embodiment of the present invention includes the metal nitride catalyst. Therefore, this reactor can perform a predetermined reaction even at low reaction temperatures and reaction pressures (particularly, can synthesize ammonia even at atmospheric pressure and a reaction temperature of 300°C or less). The reactor is not particularly limited as long as it has a structure that can accommodate the metal nitride catalyst and bring the metal nitride catalyst into contact with reaction raw materials (e.g., hydrogen and nitrogen), and existing reactors can be used.
[0047] The reactor preferably includes a honeycomb structure having an outer peripheral wall and partition walls disposed inside the outer peripheral wall and defining a plurality of cells extending from the first end face to the second end face. FIG. 1 shows a schematic cross-sectional view of a reactor including the honeycomb structure, the cross-sectional view being parallel to the direction in which the cells extend. FIG. 2 shows a schematic cross-sectional view of the reactor shown in FIG. 1 taken along line a-a'. As shown in FIGS. 1 and 2, the reactor 100 includes a honeycomb structure 10 having an outer peripheral wall 11 and partition walls 12 disposed inside the outer peripheral wall 11 and defining a plurality of cells 14 extending from the first end face 13a to the second end face 13b. A metal nitride catalyst 20 is supported on the partition walls 12 of the honeycomb structure 10. The metal nitride catalyst 20 may also be supported on the outer peripheral wall 11 facing the cells 14. By holding the metal nitride catalyst 20 on the partition walls 12 of the honeycomb structure 10, the geometric surface area on which the metal nitride catalyst 20 is supported is increased, thereby improving the reaction efficiency and enabling the reactor 100 to be made smaller.
[0048] The shape of the cross section (cross section shown in Figure 2) of the honeycomb structure 10 perpendicular to the extension direction of the cells 14 is not particularly limited, and can be various shapes such as a circle, an ellipse, a triangle, a hexagon, an octagon, etc., in addition to the square shown in Figure 2. The size of the honeycomb structure 10 is not particularly limited, and may be adjusted appropriately depending on the type of reaction, the amount of processing, etc.
[0049] The shape of the cells 14 (the shape of the cells 14 in a cross section perpendicular to the direction in which the cells 14 extend) is not particularly limited, but can be any of various shapes such as a circle, an ellipse, a triangle, a rectangle, a hexagon, or an octagon.
[0050] The size of the cells 14 is not particularly limited, but the diameter of the cells 14 in a cross section perpendicular to the extension direction of the cells 14 is preferably 1 to 3 mm, and more preferably 1.5 to 2.5 mm. By making the diameter of the cells 14 1 mm or more, it is possible to increase the amount of reaction raw material that can be supplied into the cells 14. Furthermore, by making the diameter of the cells 14 3 mm or less, the contact area with the metal nitride catalyst 20 increases, thereby improving the reaction efficiency. Here, the diameter of the cells 14 means the length of the part where the diameter is maximum.
[0051] The thickness of the outer wall 11 is not particularly limited, but is preferably 0.5 to 2.0 mm, and more preferably 0.6 to 1.8 mm. By making the thickness of the outer wall 11 0.5 mm or more, strength against external impacts can be ensured. By making the thickness of the outer wall 11 2.0 mm or less, the amount of reaction raw material that can be supplied to the honeycomb structure 10 can be increased.
[0052] The thickness of the partition walls 12 is not particularly limited, but is preferably 0.05 to 0.3 mm, and more preferably 0.08 to 0.15 mm. By setting the thickness of the partition walls 12 to 0.05 mm or more, it is possible to ensure the strength of the honeycomb structure 10. Furthermore, by setting the thickness of the partition walls 12 to 0.3 mm or less, it is possible to increase the amount of reaction raw material that can be supplied into the cells 14.
[0053] The material of the honeycomb structure 10 (the outer wall 11 and the partition walls 12) is not particularly limited, but is preferably cordierite or a Si-SiC-based material. If the honeycomb structure 10 is made of such a material, the predetermined reaction can be efficiently carried out within the honeycomb structure 10 without being inhibited.
[0054] The metal nitride catalyst 20 held on the partition walls 12 of the honeycomb structure 10 is preferably in a layered form, although there are no particular limitations on the type of catalyst. The thickness of the layered metal nitride catalyst 20 may be appropriately set depending on the processing amount, and is not particularly limited.
[0055] The reactor 100 can carry out a reaction by supplying reaction raw materials into the cells 14. The reactor 100 can be used for either a batch method or a flow method, but is suitable for use in the flow method. When the reactor 100 is used in the batch method, the reaction raw materials can be contained in the cells 14 and a reaction can be carried out by sealing either the first end face 13a or the second end face 13b. When the reactor 100 is used in the flow method, the reaction raw materials can be continuously introduced from the first end face 13a to carry out a reaction in the cells 14, and the reaction product can be continuously discharged from the second end face 13b.
[0056] (2. Method for synthesizing ammonia) The method for synthesizing ammonia according to an embodiment of the present invention uses the above-described metal nitride catalyst and is carried out by reacting nitrogen and hydrogen on the metal nitride catalyst. According to this synthesis method, since the above-described metal nitride catalyst is used, ammonia can be synthesized even at low reaction temperatures and reaction pressures, particularly at atmospheric pressure and at reaction temperatures of 300°C or less.
[0057] The reaction temperature in the ammonia synthesis method according to the embodiment of the present invention is not particularly limited, but is preferably 300°C or lower, more preferably 280°C or lower, and even more preferably 250°C or lower. Since ammonia synthesis is an exothermic reaction, a lower temperature range is more advantageous for ammonia production in terms of chemical equilibrium, and so by setting the temperature within this range, the amount of ammonia produced can be increased. Furthermore, lowering the reaction temperature can reduce equipment costs and power consumption. The lower limit of the reaction temperature is not particularly limited, but is generally 150°C, preferably 200°C.
[0058] The reaction pressure in the ammonia synthesis method according to an embodiment of the present invention is not particularly limited, but is preferably 0.9 MPa or less, and more preferably normal pressure (atmospheric pressure). Such a reaction pressure can reduce equipment costs and power consumption. However, since the amount of ammonia produced increases as the reaction pressure increases, the reaction pressure may be increased to increase the amount of ammonia produced. In this case, the reaction pressure is preferably 20 MPa or less, and more preferably 15 MPa or less. The reaction pressure refers to the pressure of a mixed gas containing nitrogen and oxygen.
[0059] The space velocity (feed rate) of the reaction raw materials in the method for synthesizing ammonia according to the embodiment of the present invention is not particularly limited, but is preferably 5000 h -1 At such a space velocity, nitrogen and oxygen can be reacted efficiently. The upper limit of the space velocity is not particularly limited, but is generally 50,000 hr -1 The following is the result.
[0060] The present invention will be explained in more detail below with reference to examples, but the present invention is not limited to these examples in any way.
[0061] Example 1 Commercially available TiN (average particle size 20 nm) was prepared as a metal nitride and used as a metal nitride catalyst. The specific surface area of this metal nitride catalyst was measured by the BET method (adsorbed gas molecules: krypton) and found to be 57 m 2 / g. The oxygen content of this metal nitride catalyst was measured by TEM-EDX and found to be 0.1 atomic %. In the following examples, the specific surface area and oxygen content were measured in the same manner.
[0062] (Example 2) Commercially available TiN (average particle size: 20 nm) was powder-pressed at 10 kN to form a pellet. The pellet-shaped TiN was then placed in a BN crucible and heat-treated at 1500°C for 3 hours in a vacuum furnace to cause anion deficiency and form the pellet-shaped TiN. 0.8 After that, pellet-shaped TiN was obtained. 0.8 The metal nitride catalyst was prepared by crushing the catalyst in a mortar and pestle. The specific surface area of the catalyst was measured and found to be 0.3 m 2 The oxygen content of this metal nitride catalyst was measured and found to be 11 atomic %. 0.8 The identification was carried out using TEM-EDX according to the above method.
[0063] (Example 3) Ru(CO) was added to commercially available TiN (average particle size 20 nm) so that the amount of Ru metal supported was 1.2 mass %. 12 (Sigma-Aldrich) was added and physically mixed in a mortar to obtain a mixed powder. The mixed powder was then heat-treated under vacuum to obtain Ru(CO). 12 The catalyst was thermally decomposed to support Ru metal, which was used as a metal nitride catalyst. The heat treatment involved raising the temperature from room temperature to 40°C at a rate of 2°C / min and holding for 1 hour, raising the temperature from 40°C to 70°C at a rate of 0.25°C / min and holding for 1 hour, raising the temperature from 70°C to 120°C at a rate of 0.4°C / min and holding for 1 hour, and raising the temperature from 120°C to 250°C at a rate of 0.9°C / min and holding for 2 hours. The specific surface area of this metal nitride catalyst was measured and found to be 57 m 2The oxygen content of this metal nitride catalyst was measured and found to be 12 atomic %.
[0064] (Example 4) TiN prepared in Example 2 0.8 Ru metal was supported by the same method as in Example 3, except that TiN (average particle size: 20 nm) was used instead of commercially available TiN, and this was used to prepare a metal nitride catalyst. The specific surface area of this metal nitride catalyst was measured and found to be 0.3 m 2 The oxygen content of this metal nitride catalyst was measured and found to be 12 atomic %.
[0065] Comparative Example 1 Ru metal was supported in the same manner as in Example 3, except that commercially available γ-AlO (Baikalox CR125 manufactured by Baikowski) was used instead of commercially available TiN (average particle size 20 nm), and this was used as a metal nitride catalyst.
[0066] 0.4 g of each metal nitride catalyst obtained above was packed into a SUS reactor tube, and hydrogen gas at 400°C was passed through it for 1 hour as a pretreatment, followed by ammonia synthesis. Ammonia synthesis was performed by passing hydrogen gas at a flow rate of 150 mL / min and nitrogen gas at a flow rate of 50 mL / min through the reactor tube. The reaction pressure was atmospheric pressure, the reaction temperature was the temperature shown in Table 1 (400°C, 300°C, 250°C, and 200°C), and the reaction time was 30 minutes. Under these conditions, ammonia synthesis was repeated 10 times to measure the amount of ammonia produced, and the average of the last five measurement results was used as the measurement result of the amount of ammonia produced. The amount of ammonia produced was measured by measuring the gas exiting the reactor tube using a gas chromatography system (Agilent Technologies 990 Micro GC System), and a PoraPLOT Q column (Agilent Technologies) was used as the column. Ammonia detection and measurement were performed with a retention time of 63.5. The measurement results of the amount of ammonia produced are shown in Table 1. The measurement results are expressed as the amount of ammonia produced per weight of the metal nitride catalyst, and are expressed as a relative value to the amount of ammonia produced at 400°C in Comparative Example 1.
[0067]
[0068] As shown in Table 1, the metal nitride catalysts of Examples 1 to 4 were able to increase the amount of ammonia produced even at reaction temperatures of 300° C. or less.
[0069] As can be seen from the above results, the present invention can provide a reactor that uses a metal nitride catalyst that can be supplied industrially and stably, and that is capable of carrying out a predetermined reaction even at low reaction temperatures and reaction pressures. The present invention also can provide a method for producing a metal nitride catalyst that can be supplied industrially and stably, and that is capable of carrying out a predetermined reaction even at low reaction temperatures and reaction pressures. Furthermore, the present invention can provide a method for synthesizing ammonia that can synthesize ammonia even at atmospheric pressure and at a reaction temperature of 300°C or less.
[0070] REFERENCE SIGNS LIST 10 honeycomb structure 11 outer peripheral wall 12 partition wall 13a first end face 13b second end face 14 cell 20 metal nitride catalyst 100 reactor
Claims
1. A reactor equipped with a metal nitride catalyst represented by the general formula MNx (M is a metal element having a Fermi energy higher than -4.4 eV vs. LV, and x is a range in which a rock salt structure can be formed).
2. The reactor according to claim 1, wherein M is at least one metal element selected from the group consisting of Ti, Hf, Ta, Mo, Cr, V and Zr.
3. The reactor according to claim 1 or 2, wherein x is equal to or greater than 0.4 and less than 1.
0.
4. The specific surface area of the metal nitride catalyst is 0.1 m 2 4. The reactor of claim 3, wherein the MnO2 content is 1 / g or more.
5. The reactor of claim 3, wherein the oxygen content of said metal nitride catalyst is 15 atomic % or less.
6. The reactor according to claim 1 or 2, wherein at least one transition metal element selected from the group consisting of transition metal elements of groups 6, 7, 8, 9, 10, 11 and 12 is supported on the metal nitride catalyst.
7. The reactor according to claim 6, wherein the supported transition metal element is at least one selected from the group consisting of Ru, Ni and Fe.
8. The reactor according to claim 6, wherein the amount of the transition metal element supported is 0.1 mass % or more.
9. The reactor according to claim 1 or 2, which is used for ammonia synthesis.
10. The reactor of claim 6, used for ammonia synthesis.
11. The reactor according to claim 1 or 2, further comprising a honeycomb structure having an outer peripheral wall and partition walls disposed inside the outer peripheral wall and defining a plurality of cells extending from a first end face to a second end face, wherein the metal nitride catalyst is held in the partition walls of the honeycomb structure.
12. The reactor according to claim 11, wherein the honeycomb structure is made of cordierite or Si-SiC based material.
13. A method for producing a metal nitride catalyst, comprising heat-treating a metal nitride represented by the general formula MN (wherein M is a metal element having a Fermi energy higher than -4.4 eV vs. LV) at 1200 to 1800°C under vacuum conditions.
14. A method for synthesizing ammonia, comprising reacting nitrogen and hydrogen over the metal nitride catalyst, using the reactor according to claim 6.
15. The method for synthesizing ammonia according to claim 14, which is carried out at a temperature of 300° C. or less and a pressure of 0.9 MPa or less.
16. 5,000 hours -1 The method for synthesizing ammonia according to claim 14, wherein the method is carried out under a space velocity of at least 1000 sq. m.
Citation Information
Patent Citations
Magunechitsukuchatsuku
JP1976047674A
Ammonia synthesis catalyst and ammonia synthesis method
WO2012077658A1
Metal oxyhydride production method, metal oxyhydride, and ammonia synthesis method using same
WO2021006136A1
Ceramic body, ceramic carrier having catalyst carrying ability, ceramic catalytic body, and its manufacturing method
JP2006232657A
Catalyst for ammonia synthesis
JP2014171916A
Cited By
Ammonia production system and ammonia production method
WO2026191291A1