Separation method and separation device

The use of an amorphous silica molecular sieve membrane formed by chemical vapor deposition addresses the challenges of separating fluorocarbon mixed gases by leveraging molecular size differences, achieving high selectivity and efficiency while reducing energy and equipment costs.

WO2024204658A1PCT designated stage expired Publication Date: 2024-10-03KOGAKUIN UNIVERSITY +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012913
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-07-07
Filing Date
2024-03-28
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Current methods for separating fluorocarbon mixed gases, such as refrigerant gases, face challenges due to azeotropy and the small difference in molecular size, making efficient separation and regeneration difficult, especially with membrane separation techniques which require high energy consumption and large equipment investments.

Method used

A molecular sieve membrane containing amorphous silica formed by chemical vapor deposition is used to separate fluorocarbon mixed gases by exploiting the difference in molecular diameters, with the membrane being formed on a porous ceramic support and utilizing a counter-diffusion CVD method to achieve high selectivity and efficiency.

Benefits of technology

The method achieves high selectivity and efficiency in separating fluorocarbon gases like difluoromethane and pentafluoroethane, with a transmittance ratio of difluoromethane being over 100 times higher than pentafluoroethane, and shows temperature-dependent but pressure-independent performance, reducing energy consumption and equipment costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012913_03102024_PF_FP_ABST
    Figure JP2024012913_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a method for separating a fluorocarbon mixture gas, the method comprising a gas separation step for bringing a mixture gas x comprising at least two fluorocarbon gases having mutually different molecular diameters into contact with a molecular sieve membrane 20 containing amorphous silica and formed by a chemical vapor deposition method, thereby separating the mixture gas x into a gas a and a gas b each having a different mixing ratio from that of the mixture gas. Also provided is a separation device which is provided with a porous membrane containing amorphous silica and formed by a chemical vapor deposition method, the separation device employing the porous membrane to separate, from a mixture gas comprising at least two fluorocarbon gases having mutually different molecular diameters, a gas composition in which the mixing ratio of one of the fluorocarbon gases is improved, or a single-component gas.
Need to check novelty before this filing date? Find Prior Art

Description

Separation method and separation device

[0001] The present disclosure relates to a method and apparatus for separating fluorocarbon gas mixtures.

[0002] Distillation is a technique for separating a specific refrigerant gas from a mixed refrigerant gas. However, evaporation requires a large amount of energy and capital investment. Therefore, a low-cost technique for separating and recovering each refrigerant gas from a mixed refrigerant gas is desired.

[0003] For example, Patent Document 1 discloses a method for separating and recovering fluorocarbons from a gas mixture containing fluorocarbons, which comprises contacting the gas mixture containing fluorocarbons with a selectively permeable composite membrane having an active thin film formed by crosslinking a crosslinkable silicone resin on a porous support membrane made of polyimide or polysulfone, allowing the fluorocarbons to selectively permeate through the membrane and then separating them.

[0004] In addition, Non-Patent Document 1 describes the use of difluoromethane (HFC-32, CH 2 F 2 ) 50% and pentafluoroethane (HFC-125, CHF 2 CF 3 It has been reported that when a mixture of R410A consisting of 50% perfluoro(butenyl vinyl ether) and 50% perfluoro(2,2-dimethyl-1,3-dioxole) was separated using a fluorine-based amorphous polymer membrane consisting of polydimethylsiloxane and 5 mol % perfluoro(butenyl vinyl ether) and 95 mol % perfluoro(2,2-dimethyl-1,3-dioxole), the permeability of HFC-32 was higher than that of HFC-125.

[0005] Patent Document 1: Japanese Patent Application Laid-Open No. 1-42444

[0006] Non-patent document 1: Abby N. Harders et al. , J. Member. Sci. , 652, 120467 (2022)

[0007] Fluorocarbons are used as mixed gases in refrigerants, etc., but separation is difficult due to azeotropy, etc., and the small difference in molecular diameter makes it difficult to efficiently separate and regenerate them even with membrane separation. In the fluorocarbon gas separation techniques disclosed in Patent Document 1 and Non-Patent Document 1, the ratio of the permeability of each fluorocarbon gas is several to 20 times, and a separation technique with higher selectivity is desired.

[0008] The present disclosure aims to provide a new method and apparatus for separating fluorocarbons.

[0009] Means for solving the above problems include the following aspects. <1> A method for separating a fluorocarbon mixed gas, comprising: a molecular sieve membrane preparation step of preparing a molecular sieve membrane containing amorphous silica formed by a chemical vapor deposition method; and a gas separation step of contacting a mixed gas containing two or more fluorocarbon gases having different molecular diameters with the molecular sieve membrane to separate the two or more fluorocarbon gases into gases whose mixing ratio differs from that in the mixed gas before contacting the molecular sieve membrane. <2> The method for separating a fluorocarbon mixed gas according to <1>, wherein the molecular sieve membrane is an amorphous silica membrane having a structure containing —Si—O—Si— bonds. <3> The method for separating a fluorocarbon mixed gas according to <1> or <2>, wherein the gas separation step is performed in an environment of 20°C to 300°C. <4> The method for separating a fluorocarbon mixed gas according to any one of <1> to <3>, wherein the gas separation step is performed in an environment of 0.1 MPa or more. <5> The method for separating a fluorocarbon mixed gas according to any one of <1> to <4>, wherein the molecular sieve membrane is a molecular sieve membrane formed using dimethoxydiphenylsilane as a chemical vapor deposition material in the chemical vapor deposition method. <6> The method for separating a fluorocarbon mixed gas according to any one of <1> to <5>, wherein the chemical vapor deposition method is a counter-diffusion method. <7> The method for separating a fluorocarbon mixed gas according to any one of <1> to <6>, wherein the molecular sieve membrane is formed on a ceramic porous support. <8> The method for separating a fluorocarbon mixed gas according to any one of <1> to <7>, wherein the fluorocarbon mixed gas is a mixed gas of difluoromethane and pentafluoroethane. <9> A separation device comprising a porous membrane containing amorphous silica formed by a chemical vapor deposition method, which separates a gas composition or a single gas in which the mixing ratio of one fluorocarbon gas is increased from a mixed gas containing two or more fluorocarbon gases having different molecular diameters using the porous membrane.

[0010] According to the present disclosure, a new method and apparatus for separating fluorocarbons is provided.

[0011] 1 is a schematic diagram showing an example of the configuration of a molecular sieve membrane used in the fluorocarbon mixed gas separation method and separation apparatus of the present disclosure. It is a schematic diagram showing a gas separator, which is a main part of one embodiment of an apparatus for carrying out the fluorocarbon mixed gas separation method of the present disclosure. It is a schematic cross-sectional view showing a cross section of the molecular sieve membrane and housing taken along line C-C in FIG. 2. It is a schematic diagram showing the configuration of a membrane production apparatus and gas permeation test apparatus used in the examples. It is a diagram showing Arrhenius plots of each single component gas in the examples. It is a diagram showing the temperature dependence of ideal selectivity in the examples. It is a diagram showing the pressure dependence of the permeability at 200°C of each single component gas of HFC-32 and HFC-125. It is a diagram showing the pressure dependence of the permeability at 100°C of each single component gas of HFC-32 and HFC-125. It is a diagram showing the pressure dependence of the permeability at 25°C of each single component gas of HFC-32 and HFC-125.

[0012] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. In this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits. The term "process" in this specification includes not only an independent process, but also a process that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved. In this disclosure, a combination of two or more preferred aspects is a more preferred aspect. Components indicated by the same reference numerals in the drawings are the same components. Reference numerals may be omitted for components with the same function in the drawings. Reference numerals may also be omitted in the following description. The dimensional ratios in the drawings do not necessarily represent the actual dimensional ratios.

[0013] The inventors of the present disclosure have conducted extensive research and experiments into methods for separating refrigerant gases containing a mixture of two or more fluorocarbon gases with different molecular sizes (sometimes referred to as "fluorocarbon mixed gases" in this disclosure) with high selectivity, and have found that by taking advantage of the differences in the physical properties (size, etc.) of the various gases and using a molecular sieve membrane containing amorphous silica formed by chemical vapor deposition (also known as chemical vapor deposition, hereinafter sometimes referred to as CVD), high selectivity separation is possible. For example, the activated thin film formed by crosslinking a crosslinkable silicone resin disclosed in Patent Document 1 and the fluorine-based amorphous polymer membrane disclosed in Non-Patent Document 1 are not porous membranes, but separate gases by a solution-diffusion effect that utilizes differences in the solubility and diffusivity of gases in the membrane. On the other hand, the CVD amorphous silica film used in the present disclosure mainly utilizes the difference in size of each gas molecule, and separates gases by the molecular sieve effect achieved by controlling the pore size.

[0014] For example, R410A, a mixed refrigerant of difluoromethane (sometimes referred to as HFC-32 or R32) and pentafluoroethane (sometimes referred to as HFC-125 or R125), is used as a refrigerant in air conditioners and refrigeration, but there is a shift toward R32, which has a lower global warming potential. The CVD amorphous silica film used in the present disclosure has a transmittance for difluoromethane (R32, molecular diameter: 0.363 nm) that is more than 100 times higher than the transmittance for pentafluoroethane (R125, molecular diameter: 0.447 nm). Furthermore, the transmittance ratio was found to be temperature-dependent in the range from room temperature (e.g., 25°C) to 200°C, with higher temperatures indicating a higher transmittance ratio and greater suitability for separation. Furthermore, almost no pressure dependence of the transmittance was observed. That is, the method for separating a fluorocarbon mixed gas (sometimes simply referred to as a "mixed gas" in the present disclosure) according to the present disclosure includes a molecular sieve membrane preparation step of preparing a molecular sieve membrane containing amorphous silica formed by a chemical vapor deposition method, and a gas separation step of contacting a mixed gas containing two or more fluorocarbon gases having different molecular diameters with the molecular sieve membrane to separate the two or more fluorocarbon gases into gases whose mixing ratio differs from the mixing ratio in the mixed gas before contacting the molecular sieve membrane.

[0015] <Molecular sieve membrane> First, the molecular sieve membrane used in the fluorocarbon mixed gas separation method of the present disclosure will be described. Fig. 1 is a cross-sectional view schematically showing one embodiment of a gas separation member equipped with a molecular sieve membrane used in the fluorocarbon mixed gas separation method of the present disclosure. The gas separation member 30 shown in Fig. 1 includes a porous support 10 and an amorphous silica layer (amorphous silica membrane) 20 formed as a molecular sieve membrane on one surface of the porous support 10. The amorphous silica layer 20 has the function of selectively or preferentially allowing permeation of fluorocarbon gases with relatively small molecular diameters among two or more fluorocarbon gases contained in the fluorocarbon mixed gas by the molecular sieve.

[0016] The molecular sieve membrane of the present disclosure may be composed of a CVD amorphous silica layer alone, but from the viewpoints of strength as a molecular sieve membrane, ease of membrane formation, etc., it is preferable that the molecular sieve membrane be in the form of a gas separation member 30 having a structure in which an amorphous silica layer 20 serving as a molecular sieve membrane is supported on a porous support 10 as shown in Fig. 1. Note that the amorphous silica layer 20 may be formed not only on the surface of the porous support 10 but also within the pores of the porous support 10, as will be described later.

[0017] (Porous Support) As the porous support 10 supporting the amorphous silica layer 20, a porous support having pores permeable to the fluorocarbon gas to be separated can be used. In the embodiment shown in FIG. 1, the porous support 10 has a two-layer structure consisting of a support layer 12 and an intermediate layer 14, each of which is porous. From the viewpoint of more stably immobilizing the amorphous silica layer 20 and ensuring that the amorphous silica layer 20 remains stable for a longer period of time, it is preferable to use a porous support 10 having a two-layer structure, as shown in FIG. 1, in which the support layer 12 has good strength and gas permeability and is cost-effective, and the intermediate layer 14 has smaller pores than the support layer 12 and better retains the amorphous silica layer 20. In the present disclosure, the surface of the intermediate layer 14 opposite to the surface in contact with the support layer 12 may be referred to as the "surface of the intermediate layer."

[0018] The two-layer porous support 10 has an amorphous silica layer 20 at least on the surface of the intermediate layer 14. The amorphous silica layer 20 may be formed only on the surface of the intermediate layer 14, or may be formed not only on the surface of the intermediate layer 14 but also extending into the pores of the intermediate layer 14. In particular, the two-layer porous support 10 preferably has an amorphous silica layer 20 inside the pores of the intermediate layer 14 and on the surface of the intermediate layer 14. By having the amorphous silica layer 20 inside the pores of the intermediate layer 14, the amorphous silica layer 20 is more densely packed in the pores and more stably present. This further improves the function of the amorphous silica layer 20 as a molecular sieve, and it is believed that the amorphous silica layer 20 functions as a separation active region with excellent separation function for fluorocarbon mixed gases. The separation active region will be described later.

[0019] Here, "having an amorphous silica layer inside the pores" refers to both a state in which an amorphous silica layer is formed on the inner wall surface of the pores, and a state in which the pores are filled with amorphous silica so that a portion of the fluorocarbon mixed gas can permeate. When an amorphous silica layer is formed by the chemical vapor deposition method described below, a silica precursor in a gaseous phase penetrates into the pores of the porous support and is converted to amorphous silica on the inner wall surface of the pores. If the chemical vapor deposition is continued, the thickness of the amorphous silica layer formed on the inner wall surface of the pores increases, and the pores of the porous support may be filled with the amorphous silica layer. Both of these states are referred to as having an amorphous silica layer inside the pores. A preferred embodiment of the molecular sieve membrane used in the method for separating fluorocarbon mixed gases of the present disclosure is one having an amorphous silica layer inside the pores of the intermediate layer and on the surface of the intermediate layer, the thickness of the fluorocarbon gas separation active region in the amorphous silica layer being 5 nm to 15 nm, and the membrane length (length in the longitudinal direction) of the amorphous silica layer being 6 cm or more.

[0020] Examples of materials for the porous support include porous ceramics from the viewpoints of pore size and availability, and metal oxides, metal nitrides, and metal nitrides are preferred from the viewpoint of heat resistance. More specifically, porous supports such as alumina, silica, titania, zirconia, and magnesia are more preferred, with α-alumina supports being particularly preferred. In the case of tubular porous supports, the size is not particularly limited, but examples include porous tubular supports having an outer diameter of about 3 mm to 20 mm, an inner diameter of about 1 mm to 15 mm, and a wall thickness of about 1 mm to 3 mm. The average pore diameter of the porous support is preferably in the range of 30 nm to 1000 nm, more preferably in the range of 50 nm to 500 nm, and even more preferably in the range of 80 nm to 180 nm.

[0021] A preferred porous support having a two-layer structure is one in which the support layer 12 is a tubular α-alumina layer having an average pore size of 20 nm to 1000 nm, preferably 80 nm to 180 nm, and the intermediate layer 14 on the outer surface of the tubular support layer 12 is a γ-alumina layer having an average pore size of 1 nm to 20 nm, preferably 3 nm to 5 nm.

[0022] The average pore size of the porous support can be determined by measuring the pore size distribution using a through-pore size evaluation device based on the bubble point method of ASTM F316-86 (JIS K 3832). Examples of devices used for the measurement include a Perm Porometer manufactured by Seika Digital Image Co., Ltd.

[0023] The thickness of the support layer 12 can be selected arbitrarily depending on the purpose. From the viewpoint of the balance between strength and gas permeability, the thickness of the support layer 12 can be, for example, 0.5 mm to 3 mm, and preferably in the range of 1 mm to 2 mm. The thickness of the intermediate layer 14 can be, for example, 0.5 μm to 10 μm, and preferably in the range of 1 μm to 5 μm.

[0024] The thicknesses of the support layer 12 and intermediate layer 14 in the porous support 10 can be measured by platinum sputtering a cross section and observing it with a field emission scanning electron microscope (FE-SEM). An example of an FE-SEM device is the JSM-6701F (manufactured by JEOL Ltd.). The acceleration voltage of the FE-SEM can be, for example, 10.0 kV.

[0025] There are no particular limitations on the method for providing the intermediate layer 14 on the support layer 12 serving as a porous support, and any known method for manufacturing a porous layer can be applied as appropriate. In particular, when the support layer 12 is made of a material with good heat resistance, such as alumina, a method in which an intermediate layer-forming material containing boehmite sol, which will be described later, is coated on the support layer 12 and then fired is preferred. According to the method for forming the intermediate layer 14 using the intermediate layer-forming material containing boehmite sol, an intermediate layer 14 of any desired thickness can be formed by adjusting the coating amount of the intermediate layer-forming material, the firing temperature, and by performing coating and firing multiple times, for example.

[0026] One example of a method for producing a two-layer porous support is to dip-coat the outer surface of a tubular porous support layer made of α-alumina with boehmite sol, which is an intermediate layer-forming material, two to three times, followed by calcination to form a γ-alumina intermediate layer having an average pore size of 3 nm to 5 nm. When coating the tubular support layer with the intermediate layer-forming material, it is preferable to seal the ends of the tubular body to prevent the intermediate layer-forming material from penetrating into the interior of the tubular body that is the support layer 12. The boehmite sol can be produced by a conventional method, for example, using aluminum s-butoxide (sometimes abbreviated as ALSB), 2-propanol, and gallium (III) nitrate octahydrate, or aluminum s-butoxide (ALSB), 2-propanol, and nitric acid.

[0027] (Amorphous Silica Layer) The amorphous silica layer 20 has the function of selectively separating the fluorocarbon gases contained in the fluorocarbon mixed gas by molecular sieving, that is, according to the molecular diameter (molecular size). The amorphous silica layer 20 preferably has an amorphous structure in which siloxane bonds represented by -Si-O-Si- form a three-dimensional network. It is believed that the three-dimensionally formed network structure of silicon dioxide plays the role of a molecular sieve.

[0028] The thickness of the amorphous silica layer 20 is not particularly limited. A thick amorphous silica layer serving as a molecular sieve membrane improves fluorocarbon gas separation efficiency, but tends to lower gas permeability. From this perspective, the thickness of the separation active region in the amorphous silica layer is, for example, 5 nm to 100 nm, preferably in the range of 5 nm to 15 nm. Here, the separation active region in the amorphous silica layer refers to a region in the amorphous silica layer that is dense and contributes to the separation of fluorocarbon gas. It is presumed that a region of the amorphous silica layer formed inside the pores of the intermediate layer, which has a denser structure, functions as a separation active region with higher fluorocarbon gas separation activity than a silica film formed on the surface of the intermediate layer, and this region is referred to as the separation active region in the amorphous silica layer. The separation active region in the amorphous silica layer can be identified as a region where Al2p is increased and Si2p is decreased based on the elemental composition in the depth direction of the formed amorphous silica layer, as a result of analysis by X-ray photoelectron spectroscopy (XPS) described below.

[0029] The thickness of the amorphous silica layer and the thickness of the separation active region in the amorphous silica layer can be measured by performing elemental composition analysis of the amorphous silica layer in the gas separation member from the surface opposite to the porous support side in the depth direction of the film by X-ray photoelectron spectroscopy (hereinafter referred to as XPS). In the present disclosure, an XPS VG ESCALAB 250 spectrometer (manufactured by Thermo Fisher Scientific) equipped with an Al Kα radiation source is used, and the chamber pressure is set to 10-8 The values ​​measured at a pressure of less than Pa and an etching rate of 0.05 nm / s can be used. The elements and electron orbitals analyzed by XPS are Si: 2p, Al: 2p, O: 1s, and C: 1s.

[0030] When the fluorocarbon mixed gas to be separated contains two fluorocarbon gases with different molecular diameters, the amorphous silica layer 20 preferably has an average pore diameter larger than that of the fluorocarbon gas with the smaller molecular diameter and smaller than that of the fluorocarbon gas with the larger molecular diameter. For example, when separating a mixed gas of R32 (molecular diameter: 0.363 nm) and R125 (molecular size: 0.447 nm), setting the average pore diameter of the pores formed by the silicon dioxide network structure in the amorphous silica layer 20 to approximately 0.38 to 0.42 nm allows R32 to easily permeate and R125 to hardly permeate, thereby enabling efficient separation of the fluorocarbon mixed gas with high gas selectivity. Note that even if the average pore diameter of the amorphous silica layer 20 is larger than the molecular diameter of R125, R32 permeates more easily than R125, so the average pore diameter of the amorphous silica layer 20 may be larger than the molecular diameter of R125.

[0031] The amorphous silica membrane used in the present disclosure has a pore size distribution, and since the pore size is 1 nm or less, there is no quantitative pore size distribution measurement method, but the pore size can be analytically estimated by the normalized Knudsen-based permeance (NKP) method using permeation data for single-component gases. Specifically, in the present disclosure, an amorphous silica membrane whose average pore size is estimated to be 0.3 to 0.6 nm using the NKP method (200°C) described in the following document can be used. <Documents related to NKP method> Evaluation and fabrication of pore-size-tuned silica membranes with tetraethoxydimethyl disiloxane for gas separation Hye Ryeon Lee, Masakoto Kanezashi, Yoshihiro Shimomura, Tomohisa Yoshioka, Toshinori Tsuru AIChE Journal, 57(10) 2755-2765 (2011)

[0032] The molecular sieve membrane used in the method for separating fluorocarbon mixed gases of the present disclosure can be produced by chemical vapor deposition (CVD), which allows the formation of a highly durable amorphous silica layer 20 on the porous support 10.

[0033] CVD methods used to form the amorphous silica layer 20 include, for example, one-way diffusion CVD, in which a silica precursor derived from a silica source and an oxidizing agent, preferably oxygen, are supplied to one side of a porous support to form an amorphous silica layer, and counter-diffusion CVD, in which a silica precursor derived from a silica source is supplied to one side of the porous support and an oxidizing agent is supplied to the other side of the porous support. In the counter-diffusion CVD method, by maintaining equal pressure on both sides of the porous support, the silica precursor diffused into the pores of the porous support and the oxidizing agent come into contact within the pores to produce amorphous silica. An amorphous silica layer is formed on the pore walls of the pores of the porous support, and the reaction automatically terminates when the pores are filled with the silica layer. Meanwhile, the reaction between the silica precursor and oxygen continues in pores in the porous support that are not filled with the silica layer. Therefore, the reaction continues until the pores are filled with the amorphous silica layer, making it easy to obtain a high-performance amorphous silica layer with good reproducibility. That is, by the counter diffusion CVD method, an amorphous silica layer can be easily produced not only on the surface of the intermediate layer of the porous support having a double structure, which is the preferred embodiment described above, but also inside the pores of the intermediate layer.

[0034] Taking the counter-diffusion CVD method as an example for forming the amorphous silica layer 20, the porous support 10 is placed in a housing. Meanwhile, a silicon compound, which is the silica source, is placed in a bubbler and heated while supplying nitrogen gas, and the silicon compound vapor is supplied into the housing. The temperature inside the housing is set to 300°C to 650°C. The silicon compound vapor, which serves as the silica source inside the housing, is supplied to one surface (e.g., the outer peripheral surface side) of the porous support, and oxygen is circulated to the other surface (e.g., the inner peripheral surface side) to cause a reaction between the two within the porous support. For example, when an amorphous silica layer is formed on the outer surface of a tubular porous support having a length of 10 mm to 100 mm, the concentration of the silicon compound vapor is set to about 0.93 mol / m 3 If the oxygen flow rate is about 200 mL / min, a sufficient amount of amorphous silica layer is formed in about 60 minutes. Thereafter, the supply of silicon compound vapor is stopped, the inside of the housing is purged with oxygen, the supply of oxygen is stopped, and nitrogen is supplied into the inside of the porous support to purge, thereby obtaining an amorphous silica layer.

[0035] Examples of chemical vapor deposition materials (silica sources) that can be used to manufacture the amorphous silica layer 20 include dimethoxydimethylsilane (DMDMS), tetraethylorthosilicate (TEOS), hexamethyldisiloxane (HMDS), tetramethylorthosilicate (TMOS), trimethyloxy(methyl)silicate (TMMS), methoxytrimethylsilicate (MTMS), phenyltrimethoxysilane (PTMS), dimethoxydiphenylsilane (DMDPS), triethoxyethylsilane, diethoxydiethylsilane, ethoxytriethylsilane, methoxytriphenylsilane, etc. The abbreviation for the compound is given in parentheses following the compound name, and hereinafter, each compound may be referred to by the abbreviation in parentheses.

[0036] The silica source is preferably DMDMS, TMOS, HMDS, TEOS, TMMS, MTMS, DMDPS, etc., and more preferably DMDPS. That is, the amorphous silica layer is more preferably an amorphous silica layer derived from a silica source containing DMDPS.

[0037] A method for producing a molecular sieve membrane for use in the separation method for fluorocarbon mixed gases of the present disclosure preferably includes, for example, using a silica source containing dimethoxydiphenylsilane (DMDPS) on an aluminum oxide porous support having an average pore diameter of 30 nm to 1000 nm, and forming an amorphous silica layer having an average pore diameter of 0.3 nm to 0.6 nm by the NKP method (200 ° C.). As described above, the porous support has a two-layer structure comprising at least a support layer 12 and an intermediate layer 14, the support layer 12 being a porous body having an average pore diameter of 50 nm to 200 nm, and the intermediate layer 14 being a porous body having an average pore diameter of 3 nm to 5 nm. It is more preferable to form an amorphous silica layer 20 not only on the surface of the intermediate layer 14 but also in the pores of the intermediate layer 14 of the two-layer porous support 10 by a counter-diffusion CVD method.

[0038] <Fluorocarbon Mixed Gas Separation Method> Next, a method for separating a fluorocarbon mixed gas by the fluorocarbon mixed gas separation method of the present disclosure will be described with reference to the drawings. FIG. 2 is a schematic diagram showing a gas separator, which is a main component of one embodiment of an apparatus for carrying out the fluorocarbon mixed gas separation method of the present disclosure. FIG. 3 is a schematic cross-sectional view taken along line CC in FIG. 2. The gas separator 50 shown in FIG. 2 has a tubular gas separation member 30 disposed inside a tubular housing 32, and both ends are sealed by sealing members 33A and 33B. A pipe 28 is connected to the center of the sealing member 33A, which communicates with the inside A of the gas separation member 30 and through which a mixed gas x is introduced. Meanwhile, a pipe 28A that leads to the inside A of the gas separation member 30 and is used to discharge gas that has passed through the gas separation member 30 without permeating it is connected to the center of the sealing member 33B, and a pipe 28B that leads to the space B between the gas separation member 30 and the housing 32 and is used to discharge gas that has permeated the gas separation member 30 is connected near the outer periphery of the sealing member 33B. The gas separation member 30 has the layer structure shown in Fig. 1, and a CVD amorphous silica layer (silica membrane) 20 is formed as the outermost layer as a molecular sieve membrane.

[0039] By connecting a vacuum pump (not shown) to pipe 28B and applying suction, gas permeation through molecular sieve membrane 20 can be promoted. In addition, by providing valves (not shown) to each of pipes 28, 28A, and 28B, the gas flow rate and pressure can be adjusted. The diameter of pipe 28A, which discharges gas from gas separation member 30, may be made smaller than that of pipe 28, which introduces the mixed gas, to increase the pressure inside gas separation member 30 and promote gas permeation through molecular sieve membrane 20.

[0040] When a gas separation apparatus including a gas separator 50 having such a configuration is used to separate a fluorocarbon gas mixture, for example, a mixture of R125 and R32, the mixed gas x is supplied to the interior (inside A) of the gas separation member 30 through the pipe 28. As the mixed gas x passes through the gas separation member 30, it comes into contact with the amorphous silica layer 20 via the porous support 10, and at least a portion of the R32, which has a relatively small molecular diameter, permeates the amorphous silica layer 20 and moves to the space B between the gas separation member 30 and the housing 32. As a result, gas a, which has a lower R32 concentration than the mixed gas x before introduction, is discharged from the pipe 28A, and gas b, which has a higher R32 concentration than the mixed gas x before introduction, is discharged from the pipe 28B. For example, a gas separation apparatus including multiple gas separators 50 can be used to increase separation efficiency by passing the mixed gas x through the gas separators 50 multiple times. The gas separation apparatus according to the present disclosure can also perform multi-stage separation of the mixed gas x. The gas separation device according to the present disclosure can separate a gas composition or a single gas in which one fluorocarbon gas is mixed at an increased ratio from a mixed gas containing two or more fluorocarbon gases with different molecular diameters. Alternatively, the mixed gas x may be supplied to the outside (space B) of the gas separation member 30, and at least a portion of the R32, which has a relatively small molecular diameter, may be allowed to permeate into the interior (inside A) of the gas separation member 30, so that a gas having a higher R32 concentration than the mixed gas x before introduction is discharged from pipe 28A, and a gas having a lower R32 concentration is discharged from pipe 28B.

[0041] The environment in which gas separation is performed using the fluorocarbon mixed gas separation method of the present disclosure is not particularly limited. However, since the gas separation member 30 used in the present disclosure is made of an inorganic material, it has high heat resistance. Furthermore, according to a fluorocarbon gas permeation experiment described later in the present disclosure, it was found that a higher gas selectivity is exhibited at 100°C to 200°C than at room temperature (e.g., 25°C). Therefore, it is preferable to perform gas separation in an environment of, for example, 20°C to 300°C. On the other hand, according to a fluorocarbon gas permeation experiment described later, almost no pressure dependence of the permeability is observed. Therefore, it is preferable to perform gas separation in an environment with a pressure of 0.1 MPa or higher.

[0042] The permeation amount of the gas to be separated is not particularly limited, and may be set according to the type of gas. For example, the permeation amount of R32 ([mol / (m 2 sPa)]) is preferably 1.0 × 10 -4 ~1.0 x 10 -10 and more preferably 1.0 × 10 -5 ~1.0 x 10 -9 and more preferably 1.0 × 10 -6 ~1.0 x 10 -8 is.

[0043] The fluorocarbon mixed gas separation method of the present disclosure will be described in more detail below with reference to examples, although the following examples do not limit the fluorocarbon mixed gas separation method of the present disclosure.

[0044] [Formation of Amorphous Silica Film] An amorphous silica film was formed by the following procedure. A Ga-doped γ-alumina intermediate layer was coated on the outer peripheral surface of a tubular α-alumina substrate by a sol-gel method. Next, amorphous silica was deposited inside the pores of the Ga-doped γ-alumina intermediate layer by a counter-diffusion CVD method, thereby forming an amorphous silica film (hereinafter sometimes referred to as a "silica film"). This process is described in detail below.

[0045] (1) Preparation of porous support (Substrate) A tubular α-alumina substrate (manufactured by Noritake Co., Ltd.) was used as the substrate for the support layer. The specifications of the α-alumina substrate are shown in Table 1. Note that the "pore diameter" refers to the average pore diameter.

[0046]

[0047] The α-alumina substrate was cut to a total length of 120 mm using a diamond cutter, and both ends of 20 mm were glass-sealed. The length of the amorphous film formed on the substrate was 80 mm, which was not glass-sealed.

[0048] (γ-alumina Coating) γ-alumina coating was performed only on the outer surface of the substrate. The procedure was as follows: preparation of Ga-doped boehmite sol (hereinafter sometimes referred to as "boehmite sol"), preparation of a coating solution, and dip coating and firing.

[0049] (Preparation of Ga-Doped Boehmite Sol) The following reagents were prepared: Aluminum s-butoxide (ALSB) 500 g, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. 2-propanol 500 mL, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. Gallium (III) nitrate octahydrate 25 g, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.

[0050] <Preparation Procedure> ALSB, 2-propanol, a 50 mL beaker, a stirring bar, a pass pipette, a 100 mL dropping bottle, a nitrogen balloon, an electronic balance, and a stirrer were placed in a glove box (manufactured by AS ONE Corporation), and the box was then closed. The nitrogen balloon was prepared before closing the glove box.

[0051] The glove box was purged with nitrogen for 15 minutes. After purging with nitrogen, 3.60 g (0.06 mol) of 2-propanol was placed in a beaker and the inner wall of the beaker was wetted. 24.6 g (0.10 mol) of ALSB was added directly from the reagent bottle to the beaker whose wall had been wetted with 2-propanol and stirred for 1 hour. 360 mL of pure water was placed in a 500 mL beaker and heated to 90°C on a hot stirrer. Pure water at 90°C was prepared next to the beaker to adjust the liquid level, and the 500 mL beaker was replenished with pure water as needed. The openings of each beaker were covered with aluminum foil when not in use. Inside the glove box, the mixture of ALSB and 2-propanol was placed in a 100 mL dropping bottle, and a nitrogen balloon was attached to the top of the dropping bottle.

[0052] A dropping bottle with a nitrogen balloon attached was removed from the glove box, and the 90°C pure water prepared on a hot stirrer was vigorously stirred. The ALSB and 2-propanol mixture was added dropwise. The beaker's mouth was not covered with aluminum foil, and stirring was continued at 90°C until the 2-propanol evaporated (until the alcohol odor disappeared). The liquid volume was maintained at 340 mL. 17.14 g (0.04 mol) of gallium(III) nitrate octahydrate was added to 108 g (6 mol) of pure water, and the beaker's mouth was covered with parafilm and stirred for over 1 hour to prepare an aqueous gallium nitrate solution. After the 2-propanol evaporated, the solution was transferred to a 500 mL Erlenmeyer flask. If a white precipitate was present, this was also transferred as much as possible. The Erlenmeyer flask's mouth was covered with aluminum foil and allowed to cool. After cooling, the gallium nitrate aqueous solution was slowly added dropwise with vigorous stirring. After stirring for 12 hours or more, a boehmite sol was obtained and stored in a plastic bottle.

[0053] (Preparation of Coating Solution) In addition to the boehmite sol prepared above, the following chemicals were prepared: 1 mol / L nitric acid, 500 mL, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. Polyvinyl alcohol 500, fully saponified type, 500 g, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.

[0054] <Preparation procedure> 1) Add 47.5 mL of pure water and 1 M HNO to a 50 mL measuring cylinder. 3 2.5 mL of the solution was added. This solution was transferred to a 100 mL Erlenmeyer flask and a stir bar was added. 2) While gently stirring to avoid foaming, 1.75 g of polyvinyl alcohol 500 (fully saponified type) (PVA) was added to the 100 L Erlenmeyer flask. 3) Because PVA is difficult to dissolve, the 100 mL Erlenmeyer flask was moved to a hot plate stirrer, the Erlenmeyer flask's mouth was sealed with aluminum foil, and the mixture was stirred while heated to 90°C. After 40 minutes, the mixture was allowed to cool while still stirring, completing the PVA solution. 4) 20 mL of the prepared PVA solution and 30 mL of boehmite sol were placed in a 50 mL beaker, a stir bar was added, the mouth of the beaker was covered with parafilm, and the mixture was stirred for 15 minutes to complete the coating solution.

[0055] (Dip Coating and Firing) <Operation Procedure> 1) To coat only the outer surface of the substrate, the opening on one end of the substrate (the lower side during dipping) was sealed with sealing tape to prevent the coating solution from penetrating the inside of the substrate. 2) The coating solution was poured into a test tube, taking care to prevent air bubbles from entering, and the remaining coating solution was stored while stirring. A substrate with a total length of 120 mm was dipped into the coating solution from the side sealed with sealing tape and dipped for 5 seconds. Care was taken not to touch the wall of the test tube when inserting or removing the substrate. 3) The dipped substrate was placed in an electric muffle furnace KM-600 (manufactured by Advantec Co., Ltd.) and dried and fired using a specified temperature program (hold at 60°C for 3 hours, then heat to 600°C over 6 hours, hold for another 6 hours, and then cool to room temperature over 6 hours). When placing the substrate in the electric muffle furnace, the glass seal portion of the substrate was placed on the base so that it did not come into contact with the film-forming portion. 4) Dip coating and firing (the above steps 2) to 3) were repeated three times to produce a porous support (hereinafter, sometimes referred to as a "γ / α-alumina substrate" or simply as a "substrate") in which a Ga-doped γ-alumina layer (intermediate layer) was formed on the outer peripheral surface of a tubular α-alumina substrate (substrate layer).

[0056] (2) Formation of Amorphous Silica Layer (Silica Film) An amorphous silica layer (silica film) was formed on the outer peripheral surface of the double-structure porous support (γ / α-alumina substrate) manufactured as described above by counter-diffusion CVD. The schematic configuration of the apparatus 100 used for forming the silica film is shown in FIG. 4. The apparatus 100 shown in FIG. 4 contains a gas tank 24 containing oxygen used for film formation, as well as R125, R32, H 2 , N 2 The gas separator 40 is also equipped with gas tanks 13, 16, 18, and 22 containing the above gases, and is configured so that each gas permeation test can be performed by adjusting valves 38 and the like provided on each pipe 28. MFC stands for mass flow controller. SUS pipes are used for the pipes 28. Similar to the configuration shown in FIG. 3, the gas separator 40 has a glass tube housing 32 arranged outside the gas separation member 30, with a space B provided for the gas that has permeated the gas separation member 30 to pass through. An electric furnace 34 equipped with a thermocouple 36 is arranged outside the housing 32.

[0057] The substrate 10 was joined to SUS pipe joints using graphite ferrules (manufactured by GL Sciences Inc.) and unions (manufactured by Swagelok) 31A, 31B at the glass seal portions at both ends exposed from the housing 32. Pressure gauges 44, 48, a soap film flowmeter 52, a pressure transducer 54, and a vacuum pump 58 were connected to each pipe 28.

[0058] When an amorphous silica layer was formed on a porous support (γ / α-alumina substrate) 10 using the apparatus 100 configured as described above, a silica precursor was placed in a bubbler 26, and nitrogen was supplied to the bubbler 26 at a flow rate of 200 mL / min, and bubbling was performed to supply silica precursor vapor to the housing 32. A ribbon heater 42 was wrapped around the pipe 28 to prevent condensation of the precursor, and the pipe temperature was maintained at 180°C. Unreacted precursor was collected using an ice-water cold trap 46. The temperature of the bubbler 26 was controlled by wrapping it in a mantle heater (not shown).

[0059] The silica precursor vapor concentration before film formation was measured by trapping the silica precursor in the nitrogen carrier gas for a certain period of time in an ice-water cold trap 46 using a gas line that did not pass through the housing 32, and measuring the silica precursor vapor concentration (mol / m 3 ) was calculated.

[0060] (Formation of Silica Film by Counter-Diffusion CVD Method) DMDPS (dimethoxydiphenylsilane, manufactured by Tokyo Chemical Industry Co., Ltd.) represented by the following structural formula was used as a precursor.

[0061]

[0062] The physical properties of DMDPS are shown in Table 2.

[0063]

[0064] <Film Formation Procedure> The power for the temperature controls of the electric furnace 34, ribbon heater 42, and bubbler 26, which are located outside the housing, were turned on. The furnace 34 was heated from room temperature to 600°C over 1.5 hours, and the ribbon heater 42 was set to 180°C. Once all temperatures had stabilized, an ice-water cold trap 46 was prepared. The DMDPS vapor concentration was measured using a gas line that did not pass through the housing 32, and the DMDPS vapor concentration was found to be approximately 0.08 mol / m 3 The bubbler temperature was adjusted so that the temperature was around 0.05°C. After adjusting the bubbler temperature, DMDPS vapor was supplied to the housing 32 (substrate outside B), and after 2 minutes, oxygen was circulated to the substrate inside A at 200 mL / min, and film formation was started. After 60 minutes, the supply of DMDPS vapor was stopped, and nitrogen was circulated to the substrate outside B at a full flow rate, and oxygen was circulated to the substrate inside A at 200 mL / min, and the inside of the housing 32 was purged. After 1 hour, the oxygen supply was stopped, and nitrogen was purged to the substrate inside A at a full flow rate for several minutes, completing the film formation.

[0065] <Gas Permeability Evaluation> (Single Component Gas Permeation Test 1) After forming the silica membrane, a gas permeation test was performed using the apparatus 100 shown in FIG. 4. Gas was supplied to the supply side (outside the substrate), and pressure was applied to the supply side by closing the valve 38B at the membrane outlet. The supply side pressure at this time was set to 0.20 to 0.40 MPa, and the gas was permeated using a dead-end method in which the transmembrane pressure difference was 0.20 to 0.40 MPa, and the flow rate of the permeated gas obtained from the permeation side was measured using a Bubble Flowmeter (BFM) 52 (manufactured by HORIBA). Usually, when the permeation side gas flow rate is large, it is measured using a BMF 52. When the permeation side gas flow rate is small and measurement using a BMF is not possible, the permeation side gas flow rate was measured using a pressure change method. In the pressure change method, the supply side pressure was set to 0.20 MPa, and the permeation side was evacuated for 2 hours using an oil rotary vacuum pump 58 (manufactured by ULVAC, Inc.), creating a transmembrane pressure difference of approximately 0.35 MPa. When gas was supplied to the supply side, permeation occurred, and the pressure on the permeation side began to rise. The pressure was measured over time to determine the rate of pressure rise, and the permeation gas flow rate was calculated from the permeation side volume.

[0066] (Temperature Dependence) H of a silica film with a film length of 80 mm formed on a Ga-doped γ / α-alumina substrate 2 , N2 The temperature dependence of the transmittance of each of HFC-125, HFC-32, and HFC-32 is shown in Figure 5. In Figure 5, "E" on the vertical axis means a power of 10, for example, "E-10" means "10 -10 "The temperature dependence of ideal selectivity is shown in Figure 6. According to the NKP method (200°C) mentioned above, the average pore size of the silica membrane is thought to be about 0.40 to 0.55 nm, which is suitable for separating HFC-32 and HFC-125. The transmittance and transmittance ratio of HFC-32 and HFC-125 at 200°C, 100°C, and 25°C are shown in Table 3 below.

[0067]

[0068] The ideal selectivity calculated by dividing the permeability of HFC-32 by the permeability of HFC-125 was 1026 at 200°C, 1623 at 100°C, and 617 at 25°C. 2 Transmittance / N 2 The ideal selectivity calculated from the permeability was about 10 at all temperatures. This also shows that this method is particularly suitable for separating HFC-32 and HFC-125.

[0069] (Single Component Gas Permeation Test 2) After forming the silica membrane, a gas permeation test was performed using the apparatus 100 shown in FIG. 4. Gas was supplied to the supply side (outside the substrate), and pressure was applied to the supply side by closing the valve 38B at the membrane outlet. The supply side pressure at this time was set to 0.20 to 0.60 MPa, and the gas was permeated using a dead-end method in which the transmembrane pressure difference was 0.10 to 0.50 MPa, and the flow rate of the permeated gas obtained from the permeation side was measured using a Bubble Flowmeter (BFM) 52 (manufactured by HORIBA). Usually, when the permeation side gas flow rate is large, it is measured using a BMF 52. When the permeation side gas flow rate is small and measurement using a BMF is not possible, the permeation side gas flow rate was measured using a pressure change method. For the pressure change method, the feed side pressure was set to 0.20 to 0.60 MPa, and the permeation side was evacuated for two hours using an oil rotary vacuum pump 58 (manufactured by ULVAC, Inc.), creating a transmembrane pressure difference of approximately 0.20 to 0.60 MPa. When gas was supplied to the feed side, permeation occurred, and the pressure on the permeation side began to rise. The pressure was measured over time to determine the rate of pressure rise, and the permeate gas flow rate was calculated from the permeation side volume. The relationships between feed side pressure and permeability for HFC-32 and HFC-125 at 200°C, 100°C, and 25°C are shown in Figures 7, 8, and 9, respectively. At any of the temperatures tested, no significant differences (pressure dependence) were observed in the permeabilities of HFC-32 and HFC-125 due to differences in pressure.

[0070] The method for separating fluorocarbon mixed gases according to the present disclosure can achieve energy-saving separation compared to separation by distillation, and is expected to have significant economic benefits. Furthermore, it can contribute to the regulation of refrigerant gases, which have been pointed out to have a greenhouse effect 100 times greater than that of carbon dioxide.

[0071] The disclosures of Japanese Patent Application No. 2023-059439 filed on March 31, 2023 and Japanese Patent Application No. 2023-112649 filed on July 7, 2023 are incorporated herein by reference in their entirety. All documents, patent applications, and technical standards mentioned herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard was specifically and individually indicated to be incorporated herein by reference.

[0072] REFERENCE SIGNS LIST 10 Porous support 13, 16, 18, 22 Gas tank 12 Support layer 14 Intermediate layer 20 Amorphous silica layer (molecular sieve membrane) 24 Gas tank 26 Bubbler 28, 28A, 28B Piping 30 Gas separation member 32 Housing 33A, 33B Sealing member 34 Electric furnace 36 Thermocouple 38, 38B Valve 40 Gas separator 42 Ribbon heater 44 Pressure gauge 46 Ice water cold trap 50 Gas separator 52 Soap film flowmeter 54 Pressure transducer 58 Vacuum pump 100 Film forming apparatus and gas permeation test apparatus

Claims

1. A method for separating a fluorocarbon mixed gas, comprising: a molecular sieve membrane preparation step of preparing a molecular sieve membrane containing amorphous silica formed by a chemical vapor deposition method; and a gas separation step of contacting a mixed gas containing two or more fluorocarbon gases having different molecular diameters with the molecular sieve membrane, thereby separating the two or more fluorocarbon gases into a gas having a mixing ratio different from that in the mixed gas before contacting with the molecular sieve membrane.

2. The method for separating a fluorocarbon mixed gas according to claim 1, wherein the molecular sieve membrane is an amorphous silica membrane having a structure containing --Si--O--Si-- bonds.

3. The method for separating fluorocarbon mixed gases according to claim 1, wherein the gas separation step is carried out in an environment of 20°C to 300°C.

4. The method for separating a fluorocarbon mixed gas according to claim 1, wherein the gas separation step is carried out in an environment of 0.1 MPa or more.

5. The method for separating a fluorocarbon mixed gas according to claim 1, wherein the molecular sieve membrane is a molecular sieve membrane formed using dimethoxydiphenylsilane as a chemical vapor deposition material in the chemical vapor deposition method.

6. The method for separating fluorocarbon mixed gases according to claim 1, wherein said chemical vapor deposition method is a counter diffusion method.

7. The method for separating fluorocarbon mixed gases according to claim 1, wherein the molecular sieve membrane is formed on a porous ceramic support.

8. A method for separating a fluorocarbon mixed gas according to any one of claims 1 to 7, wherein the fluorocarbon mixed gas is a mixed gas of difluoromethane and pentafluoroethane.

9. A separation device comprising a porous membrane containing amorphous silica formed by a chemical vapor deposition method, which separates a gas composition or a single gas by using the porous membrane to improve the mixture ratio of one fluorocarbon gas from a mixed gas containing two or more fluorocarbon gases having different molecular diameters.

Citation Information

Patent Citations

  • Method for separating and recovering flon

    JP1989042444A

  • Reflection member for antenna, manufacturing method of reflection member for antenna, and terahertz wave observation antenna

    JP2023059349A

  • Deformable toy and building toy

    JP2023112649A

  • Organic gas separating filter and organic gas separating method using the same

    JP2000157851A

  • Filter for separating perfluorinated compound and its production

    JP2001062241A