Adhesive electrode for biological signal acquisition, electrode strip, biological sensor, and method for manufacturing adhesive electrode for biological signal acquisition
The adhesive electrode with a conductive polymer and additional compounds in a water-based adhesive addresses the issue of skin deformation and noise in conventional electrodes by maintaining connectivity and flexibility, enabling stable biological signal acquisition.
Patent Information
- Application Number
- PCT/JP2024/012936
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional biological signal acquisition electrodes lack self-adhesive properties, leading to skin deformation during movement, increased resistance, and noise interference, making stable signal acquisition difficult.
An adhesive electrode with a conductive material containing a conductive polymer and additional conductive compounds dispersed in a water-based adhesive, forming a sea-island structure to maintain connectivity and flexibility, ensuring close skin contact and stable signal acquisition.
The electrode effectively suppresses resistance changes and noise generation, allowing for stable and reliable acquisition of biological signals even during skin deformation, with improved adhesion and conductivity.
Smart Images

Figure JP2024012936_03102024_PF_FP_ABST
Abstract
Description
Adhesive electrode for acquiring biological signals, electrode piece, biosensor, and method for manufacturing adhesive electrode for acquiring biological signals
[0001] The present invention relates to an adhesive electrode for acquiring a biological signal, an electrode piece, a biosensor, and a method for manufacturing an adhesive electrode for acquiring a biological signal.
[0002] BACKGROUND ART In the fields of medicine and monitoring, when a biosensor is used to measure bioinformation such as an electrocardiogram waveform, pulse wave, electroencephalogram, and electromyography, an adhesive electrode for acquiring biosignals (bioelectrode) is used, which is brought into contact with the skin of a subject to acquire electrical signals related to the bioinformation.
[0003] As a bioelectrode for such a biosensor, for example, a stretchable electrode formed in a sheet shape by laminating a stretchable conductor layer containing at least conductive particles in a flexible resin onto a first insulating layer has been disclosed (see, for example, Patent Document 1).
[0004] Japanese Patent Application Publication No. 2019-141594
[0005] However, conventional electrodes for acquiring biological signals, such as the stretchable electrode of Patent Document 1, are not self-adhesive. Therefore, when the surface of the skin is deformed due to body movement during measurement and the electrode undergoes an elongation change, the resistance value increases, making it easier to detect noise, and making it difficult to stably acquire biological signals.
[0006] In order for a biosignal acquisition electrode to stably acquire biosignals, it is important that it adheres as tightly as possible to the skin and that it follows the deformation of the skin that occurs due to human movement, keeping changes in resistance as small as possible.
[0007] An object of one aspect of the present invention is to provide an adhesive electrode for acquiring a biological signal that can suppress resistance changes and stably acquire a biological signal.
[0008] One aspect of the adhesive electrode for acquiring a biological signal according to the present invention comprises: a conductive material containing a conductive polymer and one or more conductive compounds other than the conductive polymer; and a water-dispersible adhesive.
[0009] One aspect of the adhesive electrode for acquiring a biological signal according to the present invention can suppress resistance changes and acquire a biological signal stably.
[0010] 1 is a diagram showing an example of a cross section of a configuration of an adhesive electrode for acquiring a biological signal according to an embodiment of the present invention.
[0011] Hereinafter, embodiments of the present invention will be described in detail. In this specification, unless otherwise specified, the term "to" indicating a range of values means that the range includes the values before and after it as the lower and upper limits.
[0012] <Adhesive electrode for acquiring biological signals> An adhesive electrode for acquiring biological signals according to this embodiment will be described. Note that a living body refers to the human body (person) and animals such as cows, horses, pigs, chickens, dogs, and cats. The biosensor according to this embodiment can be suitably used for living bodies, particularly for the human body. In this embodiment, a case where the living body is a human will be described as an example.
[0013] The adhesive electrode for acquiring a biological signal according to this embodiment is a biological electrode that is attached to a part of a living body (for example, the skin, scalp, or forehead) to detect biological information. In this embodiment, a case will be described in which the adhesive electrode for acquiring a biological signal is attached to human skin to acquire electrical signals (biological signals) related to the human biological information. The biological signals are, for example, electrical signals that represent an electrocardiogram waveform, an electroencephalogram, a pulse rate, etc.
[0014] The adhesive electrode for acquiring a biological signal according to this embodiment has a sheet-like shape, and in a plan view, one longitudinal end (one end) of the adhesive electrode for acquiring a biological signal may be formed into a substantially rectangular shape, and the other longitudinal end (the other end) may be formed into a substantially arc-shaped shape. The adhesive electrode for acquiring a biological signal can be used to detect an electrical signal (biological signal) relating to the biological information of a subject by, for example, attaching it to and contacting the skin, which is an example of a living body, to measure a potential difference (polarization voltage) between the skin and the adhesive electrode for acquiring a biological signal.
[0015] The adhesive electrode for acquiring a biological signal may have other shapes besides a sheet shape, such as a rod shape, etc. The shape of the adhesive electrode for acquiring a biological signal in a plan view is not limited to the above shapes, and may be designed into any shape appropriate depending on the application, etc., and may be formed into any shape such as a substantially rectangular, substantially polygonal, substantially circular, or substantially elliptical shape.
[0016] The thickness of the adhesive electrode for acquiring a biological signal according to the present embodiment may be any appropriate thickness depending on the application, size, etc., as long as it can ensure strength, flexibility, low resistance, and conductivity. The thickness of the adhesive electrode for acquiring a biological signal refers to the length in a direction perpendicular to the surface of the adhesive electrode for acquiring a biological signal. The thickness of the adhesive electrode for acquiring a biological signal is, for example, the thickness measured at an arbitrary location on the cross section of the adhesive electrode for acquiring a biological signal. When measurements are taken at multiple locations at the same location, the thickness may be the average value of the thicknesses measured at these locations.
[0017] The adhesive electrode for acquiring biological signals according to this embodiment is an electrode (adhesive electrode) having adhesive properties, and includes a conductive material including a conductive polymer and a conductive compound, and a water-dispersible adhesive, and may also include moisturizers, additives, etc. as optional components.
[0018] FIG. 1 shows an example of a cross-section of the configuration of the adhesive electrode for acquiring a biosignal according to this embodiment. As shown in FIG. 1 , in the adhesive electrode for acquiring a biosignal 1, a conductive material 11 is dispersed in a particulate water-dispersible adhesive 12. A humectant 13 is also present in the gaps between the conductive material 11 and the water-dispersible adhesive 12 in the water-dispersible adhesive 12. Of the conductive material 11, a conductive polymer 111 is dispersed in its aggregates in the water-dispersible adhesive 12, forming a so-called sea-island structure in which the water-dispersible adhesive 12 corresponds to the "sea" and the conductive polymer 111 corresponds to the "islands." Of the conductive material 11, a conductive compound 112 is present so as to be interposed between the water-dispersible adhesives 12 and connects the conductive polymers 111 dispersed in the water-dispersible adhesive 12.
[0019] The present inventors have noticed that in an adhesive electrode for acquiring a biological signal containing a conductive polymer and a water-dispersible adhesive, a phase-separated structure between the conductive polymer and the water-dispersible adhesive is likely to form, and a sea-island structure in which domains of the conductive polymer are dispersed in the water-dispersible adhesive is likely to form. After extensive research, the present inventors have found that if another conductive compound is included as a conductive material in addition to the conductive polymer, the domains of the conductive polymer dispersed in the water-dispersible adhesive can be connected to each other by the conductive compound. This allows the adhesive electrode for acquiring a biological signal to be easily stretched while suppressing an increase in resistance due to deformation such as stretching, thereby suppressing noise generation and enabling stable measurement of biological signals.
[0020] [Conductive Material] The conductive material contained in the adhesive electrode for acquiring a biological signal according to this embodiment includes a conductive polymer and one or more types of conductive compounds other than the conductive polymer.
[0021] Examples of the conductive polymer contained in the conductive material include polythiophene-based conductive polymers, polyaniline-based conductive polymers, polypyrrole-based conductive polymers, polyacetylene-based conductive polymers, polyphenylene-based conductive polymers, derivatives thereof, and composites thereof. These may be used alone or in combination of two or more.
[0022] Examples of polythiophene-based conductive polymers include polythiophene, poly3-methylthiophene, poly3-ethylthiophene, poly3-propylthiophene, poly3-butylthiophene, poly3-hexylthiophene, poly3-heptylthiophene, poly3-octylthiophene, poly3-decylthiophene, poly3-dodecylthiophene, poly3-octadecylthiophene, poly3-bromothiophene, poly3-chlorothiophene, poly3-iodothiophene, poly3-cyanothiophene, poly3-phenylthiophene, poly3,4-dimethylthiophene, poly3,4-dibutylthiophene, poly3-hydroxythiophene, poly3-methoxythiophene, poly3-ethoxythiophene, poly3-butoxythiophene, poly3-hexyloxythiophene, poly3-heptyloxythiophene, poly3-octyloxythiophene, poly3-decyloxythiophene, poly3-dodecyloxythiophene, poly Examples of the thiophene include 3-octadecyloxythiophene, poly3,4-dihydroxythiophene, poly3,4-dimethoxythiophene, poly3,4-diethoxythiophene, poly3,4-dipropoxythiophene, poly3,4-dibutoxythiophene, poly3,4-dihexyloxythiophene, poly3,4-diheptyloxythiophene, poly3,4-dioctyloxythiophene, poly3,4-didecyloxythiophene, poly3,4-didodecyloxythiophene, poly3,4-ethylenedioxythiophene (also referred to as "PEDOT"), poly3,4-propylenedioxythiophene, poly3,4-butenedioxythiophene, poly3-methyl-4-methoxythiophene, poly3-methyl-4-ethoxythiophene, poly3-carboxythiophene, poly3-methyl-4-carboxythiophene, poly3-methyl-4-carboxyethylthiophene, and poly3-methyl-4-carboxybutylthiophene.
[0023] Examples of polyanionic conductive polymers include polymers having sulfonic acid groups such as polystyrene sulfonic acid (also referred to as "PSS"), polyvinyl sulfonic acid, polyallyl sulfonic acid, polyacrylic sulfonic acid, polymethacrylic sulfonic acid, poly(2-acrylamido-2-methylpropanesulfonic acid), polyisoprene sulfonic acid, polysulfoethyl methacrylate, poly(4-sulfobutyl methacrylate), and polymethacryloxybenzenesulfonic acid, as well as polymers having carboxylic acid groups such as polyvinyl carboxylic acid, polystyrene carboxylic acid, polyallyl carboxylic acid, polyacrylic carboxylic acid, polymethacrylic carboxylic acid, poly(2-acrylamido-2-methylpropanecarboxylic acid), polyisoprene carboxylic acid, and polyacrylic acid. These may be used as homopolymers obtained by polymerizing one type alone, or as copolymers of two or more types. Among these polyanions, polymers having sulfonic acid groups are preferred because they can achieve higher conductivity, and polystyrene sulfonic acid is more preferred.
[0024] Examples of polypyrrole-based conductive polymers include polypyrrole, poly(N-methylpyrrole), poly(3-methylpyrrole), poly(3-ethylpyrrole), poly(3-n-propylpyrrole), poly(3-butylpyrrole), poly(3-octylpyrrole), poly(3-decylpyrrole), poly(3-dodecylpyrrole), poly(3,4-dimethylpyrrole), poly(3,4-dibutylpyrrole), poly(3-carboxypyrrole), poly(3-methyl-4-carboxypyrrole), poly(3-methyl-4-carboxyethylpyrrole), poly(3-methyl-4-carboxybutylpyrrole), poly(3-hydroxypyrrole), poly(3-methoxypyrrole), poly(3-ethoxypyrrole), poly(3-butoxypyrrole), poly(3-hexyloxypyrrole), and poly(3-methyl-4-hexyloxypyrrole).
[0025] Examples of polyacetylene-based conductive polymers include polyacetylenes having polar groups, such as polyphenylacetylene monoesters having an ester at the para-position of phenylacetylene, and polyphenylacetylene monoamides having an amide at the para-position of phenylacetylene.
[0026] Examples of polyphenylene-based conductive polymers include polyphenylene vinylene.
[0027] As these composites, a composite in which polythiophene is doped with polyaniline as a dopant is preferred, etc. Among composites of polythiophene and polyaniline, it is more preferred to use PEDOT / PSS in which PEDOT is doped with PSS, because it has a lower contact impedance with a living body and high conductivity.
[0028] The content of the conductive polymer is preferably 0.20 parts by mass to 20 parts by mass, more preferably 2.5 parts by mass to 15 parts by mass, and even more preferably 3.0 parts by mass to 12 parts by mass, relative to 100 parts by mass of the conductive composition. When the content is within the above preferred range relative to 100 parts by mass of the conductive composition, the conductive composition can have excellent conductivity, toughness, and flexibility.
[0029] The conductive polymer may be used as an aqueous solution dissolved in a solvent. In this case, the solvent may be an organic solvent or an aqueous solvent. Examples of organic solvents include ketones such as acetone and methyl ethyl ketone (MEK); esters such as ethyl acetate; ethers such as propylene glycol monomethyl ether; and amides such as N,N-dimethylformamide. Examples of aqueous solvents include water; and alcohols such as methanol, ethanol, propanol, and isopropanol. Of these, it is preferable to use an aqueous solvent.
[0030] The conductive compound contained in the conductive material is not particularly limited in type as long as it is a compound other than a conductive polymer and has conductivity. Examples of the conductive compound include carbon materials such as graphite, carbon black, carbon nanotubes, carbon nanohorns, and carbon fibers; metals such as aluminum, gold, silver, copper, iron, platinum, chromium, tin, indium, antimony, titanium, and nickel; and so-called ABO 3Examples of the conductive ceramics include perovskite-type composite oxides. These conductive compounds may be used alone or in combination of two or more. From the viewpoint of durability, it is preferable to use a carbon material.
[0031] The shape of the conductive compound is not particularly limited as long as it can be dispersed in the water-dispersible PSA and can connect domains of the conductive polymer dispersed in the water-dispersible PSA so as to form a sea-island structure, and the shape of the conductive compound may be particulate, fibrous, a structure having a higher-order chain structure, or the like.
[0032] The content of the conductive compound is preferably 0.1 wt% to 50 wt%, more preferably 0.5 wt% to 40 wt%, and even more preferably 1.0 wt% to 30 wt%, relative to 100 wt% of the conductive polymer. When the content of the conductive compound is 0.1 wt% to 50 wt%, relative to 100 wt% of the conductive polymer, the conductive compound can connect the conductive polymers in the aqueous dispersion adhesive and exhibit sufficient conductivity. Furthermore, the adhesive electrode for acquiring biosignals is prevented from becoming hard and brittle, thereby maintaining good workability and adhesiveness of the adhesive electrode for acquiring biosignals.
[0033] [Water-Dispersed Adhesive] As the water-dispersed adhesive contained in the adhesive electrode for acquiring a biological signal according to this embodiment, a water-based emulsion adhesive or the like is used.
[0034] The aqueous emulsion adhesive is used as a binder resin for the adhesive electrode for acquiring a biological signal. The aqueous emulsion adhesive has the function of improving the adhesiveness and flexibility of the adhesive electrode for acquiring a biological signal. Therefore, by including the aqueous emulsion adhesive in the adhesive electrode for acquiring a biological signal, the adhesive electrode for acquiring a biological signal can have low elasticity and can improve its ability to conform to the unevenness of the skin surface.
[0035] As the aqueous emulsion pressure-sensitive adhesive, it is preferable to use an acrylic emulsion pressure-sensitive adhesive.
[0036] The acrylic emulsion pressure-sensitive adhesive is preferably a silane emulsion pressure-sensitive adhesive containing a water-dispersible copolymer and an organic liquid component that is compatible with the water-dispersible copolymer.
[0037] The water-dispersible copolymer is a polymer obtained by copolymerizing a monomer mixture containing a (meth)acrylic acid alkyl ester with a silane-based monomer copolymerizable with the (meth)acrylic acid alkyl ester.
[0038] The monomer mixture containing a (meth)acrylic acid alkyl ester is a monomer mixture containing a (meth)acrylic acid alkyl ester as a main component, preferably in an amount of 50 wt % to 100 wt %.
[0039] As the (meth)acrylic acid alkyl ester, a straight-chain or branched alkyl ester having an alkyl group of 1 to 15 carbon atoms, preferably 1 to 9 carbon atoms, is used. Specific examples include (meth)acrylic acid alkyl esters having a straight-chain or branched alkyl group, such as methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, undecyl (meth)acrylate, and tridecyl (meth)acrylate. These may be used alone or in combination of two or more.
[0040] The monomer mixture containing the (meth)acrylic acid alkyl ester may contain a carboxyl group-containing monomer copolymerizable with the (meth)acrylic acid alkyl ester.
[0041] The carboxyl group-containing monomer copolymerizable with the (meth)acrylic acid alkyl ester is not particularly limited as long as it is a polymerizable compound containing a carboxyl group in its structure and is copolymerizable with the (meth)acrylic acid alkyl ester, and examples thereof include (meth)acrylic acid, itaconic acid, maleic acid, maleic anhydride, 2-methacryloyloxyethyl succinic acid, etc. Acrylic acid is particularly preferred.
[0042] From the viewpoint of hydrolysis of the silane-based monomer and adjustment of the resulting adhesiveness, the carboxyl group-containing monomer is preferably contained in an amount of 0.1 wt % to 10 wt % relative to 100 wt % of the monomer mixture containing the (meth)acrylic acid alkyl ester.
[0043] The silane monomer copolymerizable with (meth)acrylic acid alkyl ester is not particularly limited as long as it is a polymerizable compound having a silicon atom and is copolymerizable with (meth)acrylic acid alkyl ester, but silane compounds having a (meth)acryloyl group, such as (meth)acryloyloxyalkylsilane derivatives, are preferred because of their excellent copolymerizability with (meth)acrylic acid alkyl ester. Examples of silane monomers include 3-(meth)acryloyloxypropyltrimethoxysilane, 3-(meth)acryloyloxypropyltriethoxysilane, 3-(meth)acryloyloxypropylmethyldimethoxysilane, and 3-(meth)acryloyloxypropylmethyldiethoxysilane. These silane monomers can be used alone or in combination of two or more.
[0044] Furthermore, other silane-based monomers that can be used include, for example, vinyltrimethoxysilane, vinyltriethoxysilane, 4-vinylbutyltrimethoxysilane, 4-vinylbutyltriethoxysilane, 8-vinyloctyltrimethoxysilane, 8-vinyloctyltriethoxysilane, 10-methacryloyloxydecyltrimethoxysilane, 10-acryloyloxydecyltrimethoxysilane, 10-methacryloyloxydecyltriethoxysilane, and 10-acryloyloxydecyltriethoxysilane.
[0045] It is preferable that the silane-based monomer is copolymerized with the monomer mixture containing the (meth)acrylic acid alkyl ester in an amount of 0.005 wt % to 2 wt % relative to 100 wt % of the monomer mixture containing the (meth)acrylic acid alkyl ester.
[0046] By copolymerizing a silane monomer with a monomer mixture containing a (meth)acrylic acid alkyl ester, the silane compounds that serve as crosslinking points are uniformly distributed within the molecules of the resulting copolymer. As a result, the aqueous emulsion pressure-sensitive adhesive, despite being a water-dispersible type, has excellent cohesion because the inside and outside of the particles are uniformly crosslinked, and the addition of an organic liquid component not only provides low skin irritation but also excellent fixation and sweat-resistant fixation.
[0047] The aqueous dispersion copolymer may be a copolymer of a monomer copolymerizable with a (meth)acrylic acid alkyl ester other than the above-mentioned silane-based monomer and carboxyl group-containing monomer, if necessary. The monomer copolymerizable with a (meth)acrylic acid alkyl ester other than the silane-based monomer and the carboxyl group-containing monomer can be used for the purpose of adjusting the cohesive force of the adhesive electrode for acquiring biological signals when the aqueous emulsion adhesive is formed into a sheet or the like, or improving compatibility with organic liquid components, and the amount used can be set arbitrarily depending on the purpose by replacing a part of the content of the (meth)acrylic acid alkyl ester.
[0048] Examples of monomers copolymerizable with (meth)acrylic acid alkyl esters other than silane-based monomers and carboxyl group-containing monomers include sulfoxyl group-containing monomers such as styrenesulfonic acid, allylsulfonic acid, sulfopropyl(meth)acrylate, (meth)acryloyloxynaphthalenesulfonic acid, and acrylamidomethylpropanesulfonic acid; hydroxyl group-containing monomers such as (meth)acrylic acid hydroxyethyl ester and (meth)acrylic acid hydroxypropyl ester; amide group-containing monomers such as (meth)acrylamide, dimethyl(meth)acrylamide, N-butylacrylamide, N-methylol(meth)acrylamide, and N-methylolpropane(meth)acrylamide; (meth)acrylic acid alkylaminoalkyl esters such as (meth)acrylic acid aminoethyl ester, (meth)acrylic acid dimethylaminoethyl ester, and (meth)acrylic acid tert-butylaminoethyl ester; and (meth)acrylic acid methoxy. Examples thereof include (meth)acrylic acid alkoxyalkyl esters such as (meth)acrylic acid diethyl ester and (meth)acrylic acid ethoxyethyl ester, (meth)acrylic acid methoxyethylene glycol ester, (meth)acrylic acid tetrahydrofurfuryl ester, (meth)acrylic acid methoxyethylene glycol ester, (meth)acrylic acid methoxydiethylene glycol ester, (meth)acrylic acid methoxypolyethylene glycol ester, and (meth)acrylic acid methoxypolypropylene glycol ester, and vinyl monomers such as (meth)acrylonitrile, vinyl acetate, vinyl propionate, N-vinyl-2-pyrrolidone, methylvinylpyrrolidone, vinylpyridine, vinylpiperidine, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, vinylimidazole, vinylcaprolactam, vinyloxazole, and vinylmorpholine. These can be used alone or in combination of two or more.
[0049] The water-dispersible polymer can be prepared as a water dispersion of a (meth)acrylic acid alkyl ester copolymer, for example, by subjecting a mixture of a monomer mixture containing a (meth)acrylic acid alkyl ester and a silane-based monomer to conventional emulsion polymerization.
[0050] As the polymerization method, general batch polymerization, continuous dropwise polymerization, divided dropwise polymerization, etc. can be adopted, and the polymerization temperature is, for example, 20°C to 100°C.
[0051] The polymerization initiator used in the polymerization is not particularly limited, and a general component used as a polymerization initiator can be used.
[0052] A chain transfer agent may be used in the polymerization to adjust the degree of polymerization. The chain transfer agent is not particularly limited, and a general component used as a chain transfer agent can be used.
[0053] In addition to the above-mentioned method, the water-dispersible copolymer may also be prepared by obtaining a copolymer of a monomer mixture containing a (meth)acrylic acid ester and a silane-based monomer by a method other than emulsion polymerization, and then dispersing the copolymer in water with an emulsifier.
[0054] The organic liquid component contained in the acrylic emulsion adhesive, when blended with the water-dispersible copolymer, not only maintains good adhesion to the skin surface, but also reduces damage to the keratin when peeled from the skin surface, and also reduces pain when peeled.
[0055] The organic liquid component is preferably liquid at room temperature and has good compatibility with the water-dispersible copolymer. Here, "compatibility" refers to the state in which the organic liquid component is uniformly dissolved and incorporated into the water-dispersible copolymer, and separation cannot be confirmed visually.
[0056] Examples of the organic liquid component include esters of monobasic or polybasic acids having 8 to 18 carbon atoms and branched alcohols having 14 to 18 carbon atoms, and esters of unsaturated fatty acids or branched acids having 14 to 18 carbon atoms and tetrahydric or lower alcohols.
[0057] Examples of esters of monobasic or polybasic acids having 8 to 18 carbon atoms with branched alcohols having 14 to 18 carbon atoms include isostearyl laurate, isocetyl myristate, octyldodecyl myristate, isostearyl palmitate, isocetyl stearate, octyldodecyl oleate, diisostearyl adipate, diisocetyl sebacate, trioleyl trimellitate, and triisocetyl trimellitate.
[0058] Examples of unsaturated fatty acids or branched acids having 14 to 18 carbon atoms include myristoleic acid, oleic acid, linoleic acid, linolenic acid, isopalmitic acid, and isostearic acid.
[0059] Examples of tetrahydric or lower alcohols include ethylene glycol, propylene glycol, glycerin, trimethylolpropane, pentaerythritol, and sorbitan.
[0060] The content of the organic liquid component can be appropriately set according to the type of water-dispersible copolymer and the organic liquid component, and may be, for example, 20 wt % to 80 wt % relative to 100 wt % of the water-dispersible copolymer.
[0061] When the acrylic emulsion pressure-sensitive adhesive is a silane emulsion pressure-sensitive adhesive, specifically, a silane emulsion pressure-sensitive adhesive containing 2-ethylhexyl acrylate, methyl methacrylate, acrylic acid, and 3-methacryloxypropyltrimethoxysilane can be used as the acrylic emulsion pressure-sensitive adhesive.
[0062] The acrylic emulsion pressure-sensitive adhesive may be a two-component or three-component acrylic emulsion pressure-sensitive adhesive containing a monomer mixture containing a (meth)acrylic acid alkyl ester and a carboxyl group-containing monomer, and may contain a solvent and / or other components in a predetermined amount within a range in which the solvent and / or other components can exhibit their performance.
[0063] The monomer mixture containing the (meth)acrylic acid alkyl ester contained in the two-component or three-component acrylic emulsion pressure-sensitive adhesive is similar to the monomer mixture containing the (meth)acrylic acid alkyl ester contained in the above-mentioned silane-based emulsion pressure-sensitive adhesive, so details will be omitted.
[0064] The carboxyl group-containing monomer is preferably a carboxyl group-containing monomer copolymerizable with a (meth)acrylic acid alkyl ester. The carboxyl group-containing monomer copolymerizable with a (meth)acrylic acid alkyl ester is the same as the carboxyl group-containing monomer contained in the above-mentioned monomer mixture containing a (meth)acrylic acid alkyl ester, and therefore details thereof are omitted.
[0065] Specifically, the two-component acrylic emulsion adhesive may be an adhesive containing 2-ethylhexyl acrylate, which is a monomer mixture containing a (meth)acrylic acid alkyl ester, and acrylic acid, which is a carboxyl group-containing monomer mixture.
[0066] Specifically, the three-component acrylic emulsion pressure-sensitive adhesive may be a pressure-sensitive adhesive containing 2-ethylhexyl acrylate and methyl methacrylate, which are a monomer mixture containing a (meth)acrylic acid alkyl ester, and acrylic acid, which is a carboxyl group-containing monomer mixture.
[0067] The average particle size of the aqueous emulsion adhesive is preferably 100 nm to 1.0 μm, more preferably 100 nm to 500 nm, and even more preferably 100 nm to 300 nm. When the average particle size is within the above preferred range, adhesive strength and water resistance can be imparted to the adhesive electrode for acquiring biological signals.
[0068] The shape of the aqueous emulsion pressure-sensitive adhesive is not particularly limited, and may be, for example, spherical, ellipsoidal, spindle-like, crushed, plate-like, columnar, or the like.
[0069] The average particle size refers to the volume-average particle size based on the effective diameter. The average particle size is the particle size (median diameter) at which the cumulative amount of particles, accumulated from the smallest to the largest, accounts for 50% by volume on a particle size distribution curve obtained by measuring the particle size distribution of a polymer emulsion pressure-sensitive adhesive or an acrylic emulsion pressure-sensitive adhesive by, for example, laser diffraction / scattering or dynamic light scattering.
[0070] The content of the aqueous emulsion adhesive is preferably 35 wt % to 90 wt %, more preferably 40 wt % to 85 wt %, and even more preferably 50 wt % to 80 wt %, relative to 100 wt % of the adhesive electrode for acquiring biological signals. When the content of the aqueous emulsion adhesive is within the above preferred range, adhesive strength and flexibility can be imparted to the adhesive electrode for acquiring biological signals, and a decrease in conductivity can be suppressed.
[0071] As described above, the adhesive electrode for acquiring a biological signal may contain a moisturizer, an additive, and the like as optional components.
[0072] The moisturizing agent has the function of improving the conductivity of the adhesive electrode for acquiring a biological signal, as well as improving the adhesive strength and flexibility.
[0073] Examples of moisturizing agents include polyol compounds such as glycerin, ethylene glycol, propylene glycol, sorbitol, and polymers thereof, and aprotic compounds such as N-methylpyrrolidone (NMP), dimethylformaldehyde (DMF), N-N'-dimethylacetamide (DMAc), and dimethyl sulfoxide (DMSO). These may be used alone or in combination of two or more. Among these, glycerin is preferred from the viewpoint of compatibility with other components.
[0074] The content of the moisturizer is preferably 2 wt% to 60 wt%, more preferably 3 wt% to 50 wt%, and even more preferably 5 wt% to 35 wt%, relative to 100 wt% of the adhesive electrode for acquiring biological signals. If the content of the moisturizer falls within the above preferred range, the adhesive strength of the adhesive electrode for acquiring biological signals can be improved, maintaining high adhesion to the skin surface, and the storage modulus can be reduced and viscoelasticity can be increased, thereby reducing the amount of noise generated during use. Furthermore, the adhesive electrode for acquiring biological signals can be prevented from absorbing water from the outside and suppressing swelling.
[0075] The additive has a neutralizing effect on the conductive polymer, neutralizing the conductive polymer and improving its flexibility. For example, when the conductive polymer is PEDOT-PSS, the additive forms an organic salt when neutralized with PSS, which is a strong acid, and can improve water absorbency and at the same time, can make the conductive polymer insoluble in water.
[0076] Preferred examples of the additive include imidazole compounds.
[0077] The imidazole compound is an organic structure having an imidazole group. The imidazole group of the imidazole compound acts as an additive, for example, in the pH range of 3.5 to 6.5. Examples of the imidazole compound include heterocyclic amines.
[0078] Examples of heterocyclic amines include imidazole, 2-methylimidazole, 2-propylimidazole, 2-undecylimidazole, 2-phenylimidazole, N-methylimidazole, 1-(2-hydroxyethyl)imidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-methylimidazole, and 1-cyanoethyl Examples of suitable additives include 4,5-imidazole dicarboxylic acid, 4,5-imidazoledicarboxylate dimethyl, benzimidazole, 2-aminobenzimidazole, 2-aminobenzimidazole-2-sulfonic acid, 2-amino-1-methylbenzimidazole, 2-hydroxybenzimidazole, and 2-(2-pyridyl)benzimidazole. Among these, imidazole is preferred. The additive may be an imidazole compound, and may be used alone or in combination of two or more.
[0079] The content of the additive is preferably 0.5 wt % to 2.4 wt %, more preferably 0.7 wt % to 2.2 wt %, and even more preferably 0.8 wt % to 2.0 wt %, relative to 100 wt % of the adhesive electrode for acquiring biological signals.
[0080] The method for manufacturing the adhesive electrode for acquiring a biological signal according to the present embodiment is not particularly limited. An example of the method for manufacturing the adhesive electrode for acquiring a biological signal will be described. For example, first, a conductive polymer and water are mixed to prepare an aqueous solution containing the conductive polymer (a step of preparing an aqueous solution containing the conductive polymer).
[0081] The mixing ratio of the conductive polymer to water, mixing conditions such as mixing time, temperature of the conductive polymer-containing solution, etc. are not particularly limited, and may be set to any appropriate size as long as the conductive polymer can be sufficiently mixed in the conductive polymer-containing solution.
[0082] Next, a water-dispersible pressure-sensitive adhesive and, if necessary, other additives such as a moisturizer are mixed with the conductive polymer-containing aqueous solution to prepare a pressure-sensitive adhesive composition aqueous solution (first mixing step).
[0083] The mixing ratio of the conductive polymer-containing aqueous solution, the water-dispersible adhesive, the moisturizer, etc., the mixing conditions such as the mixing time, the temperature of the aqueous pressure-sensitive adhesive composition, etc. are not particularly limited, and may be set to any appropriate size as long as the water-dispersible adhesive and the moisturizer, etc. can be sufficiently mixed into the conductive polymer-containing aqueous solution.
[0084] Next, the aqueous solution of the adhesive composition is mixed with an aqueous solution of a conductive compound containing a conductive compound to prepare an aqueous solution of the conductive composition (second mixing step). The aqueous solution of the conductive composition is used as a composition for forming an adhesive electrode.
[0085] There are no particular limitations on the mixing conditions, such as the mixing ratio of the aqueous pressure-sensitive adhesive composition solution and the aqueous conductive compound-containing solution, the stirring speed, acceleration, temperature, etc. For example, as long as the conductive compound can be mixed into the aqueous pressure-sensitive adhesive composition solution to such an extent that the bond between the conductive polymer contained in the aqueous pressure-sensitive adhesive composition solution and the conductive compound contained in the aqueous conductive compound-containing solution is not broken, each of the mixing conditions may be appropriately set to any value.
[0086] Among the mixing conditions, it is preferable to mix and stir the aqueous solution containing the conductive composition at a stirring speed and acceleration that are such that the bonds between the conductive polymer and the conductive compound contained in the aqueous solution containing the conductive composition are not broken. The stirring speed may be set appropriately depending on the size of the stirring vessel used, etc. The acceleration may also be set appropriately depending on the size of the stirring vessel used, etc., and may be, for example, within the range of 300 G to 500 G.
[0087] Next, the aqueous solution containing the conductive composition is applied to the surface (coating surface) of the release substrate, and then dried to evaporate the water contained in the aqueous solution containing the conductive composition (coating and drying step). Because the aqueous pressure-sensitive adhesive has a particulate shape, by applying the aqueous solution containing the conductive composition to the coating surface of the release substrate, the aqueous pressure-sensitive adhesive particles bond and fuse together to form a coating film, which is a cured product of the adhesive electrode-forming composition.
[0088] The release substrate may be a release liner or a core material. The release liner may be a resin film such as a polyethylene terephthalate (PET) film, a polyethylene (PE) film, a polypropylene (PP) film, a polyamide (PA) film, a polyimide (PI) film, or a fluororesin film. The core material may be a resin film such as a PET film or a PI film; a ceramic sheet; a metal film such as aluminum foil; a resin substrate reinforced with glass fiber, plastic nonwoven fiber, or the like; a silicone substrate or a glass substrate.
[0089] The method for applying the aqueous solution containing the conductive composition to the application surface of the release substrate is not particularly limited as long as it is possible to apply the aqueous solution containing the conductive composition to the release substrate, and a general application method may be used.
[0090] Examples of the coating method include roll coating, screen coating, gravure coating, spin coating, reverse coating, bar coating, blade coating, spray coating, air knife coating, dipping, dispensing, etc., and a method in which a small amount of an aqueous solution containing a conductive composition is dropped onto the surface to be coated of the substrate and spread with a doctor blade, etc. By these coating methods, the aqueous solution containing the conductive composition can be uniformly applied onto the surface to be coated.
[0091] The drying conditions for the aqueous solution containing the conductive composition applied to the coating surface of the release substrate are not particularly limited as long as they are conditions that allow the aqueous solution containing the conductive composition applied to the release substrate to be dried, and general drying conditions may be used.
[0092] The drying may be performed at room temperature or by heating using a dryer. Examples of the dryer that can be used include general dryers such as a drying oven, a vacuum oven, an air circulation oven, a hot air dryer, a far-infrared dryer, a microwave reduced-pressure dryer, and a high-frequency dryer. The aqueous solution containing the conductive composition applied to the surface of the substrate using these dryers may be dried by, for example, heating the interior of the dryer to a high temperature, heating the substrate, blowing hot air onto the aqueous solution containing the conductive composition, or irradiating the aqueous solution containing the conductive composition with far-infrared rays, microwaves, or high frequencies.
[0093] The heating temperature and heating time when heating the conductive composition-containing aqueous solution using a dryer are set to a temperature and time that can evaporate the water contained in the conductive composition-containing aqueous solution. The heating temperature may be, for example, 100°C to 200°C. When the conductive composition contains a crosslinking agent, a heating temperature within the range of 100°C to 200°C can promote the evaporation of the water contained in the conductive composition-containing aqueous solution. The heating time of the conductive composition-containing aqueous solution may be, for example, 0.5 minutes to 300 minutes. A heating time of 0.5 minutes to 300 minutes can sufficiently evaporate the water contained in the conductive composition-containing aqueous solution.
[0094] Next, the obtained cured product is punched (pressed) using a press or the like as needed to form the outer shape of the cured product into a predetermined shape (forming step), thereby obtaining an adhesive electrode for acquiring a biological signal, which is a molded product having the outer shape of the predetermined shape.
[0095] It should be noted that molding may be performed using a laser processing machine instead of a press. Furthermore, the obtained cured product may be molded into a predetermined shape only in terms of its outer shape. Furthermore, when the cured product can be used as an adhesive electrode for acquiring a biological signal as is, the cured product may be used as an adhesive electrode for acquiring a biological signal without being molded or otherwise processed.
[0096] The method for manufacturing an adhesive electrode for acquiring a biological signal according to this embodiment includes a step of preparing an aqueous solution containing a conductive polymer, a first mixing step, and a second mixing step, which are carried out separately. In the step of preparing an aqueous solution containing a conductive polymer and the first mixing step, a conductive polymer is dispersed in the aqueous solution containing a conductive polymer to obtain an aqueous solution containing a conductive compound. Then, in the second mixing step, an aqueous solution of an adhesive composition is mixed with the aqueous solution containing a conductive polymer, and the mixture is stirred and mixed. This produces a composition for forming an adhesive electrode in which the conductive polymer and the conductive compound are present in a linked state. The obtained composition for forming an adhesive electrode is applied to a release substrate and cured to produce an adhesive electrode for acquiring a biological signal.
[0097] In the obtained adhesive electrode for acquiring a biological signal, the conductive polymer and the conductive compound can exist in a linked state. Therefore, even if the domains of the conductive polymer are dispersed in a particulate aqueous dispersion adhesive to form an island-sea structure, the conductive polymer and the conductive compound can exist in a linked state. Therefore, when the adhesive electrode for acquiring a biological signal is attached to the surface of a living body, even if it is deformed by elongation or the like due to deformation of the surface of the living body, resistance change is suppressed and the biological signal can be stably acquired.
[0098] As described above, the adhesive electrode for acquiring a biosignal according to the present embodiment includes a conductive material and a water-dispersible adhesive, and the conductive material includes both a conductive polymer and a conductive compound. Because the adhesive electrode for acquiring a biosignal according to the present embodiment uses a water-dispersible adhesive as a binder resin, it easily conforms to deformations in the skin, such as warping and elongation. Therefore, the adhesive electrode for acquiring a biosignal according to the present embodiment can adhere closely to the skin without gaps and can maintain close contact even when deformations in the skin surface occur due to human movement, thereby acquiring a biosignal. Because the conductive polymer domains are dispersed in the water-dispersible adhesive to form a sea-island structure, stretching the adhesive electrode for acquiring a biosignal can easily break the connections between the conductive polymers, resulting in a decrease in the conductivity of the adhesive electrode for acquiring a biosignal. This can increase the resistance of the adhesive electrode for acquiring a biosignal, making noise more likely to occur and reducing sensitivity.
[0099] In the adhesive electrode for acquiring a biological signal according to this embodiment, domains of a conductive polymer dispersed in a water-dispersible adhesive to form an island-in-a-sea structure can be connected to each other via a conductive compound. Therefore, even if the adhesive electrode for acquiring a biological signal is stretched due to deformation of the skin caused by body movement while measuring biological information using a biosensor equipped with the adhesive electrode for acquiring a biological signal, the conductive polymers dispersed in the water-dispersible adhesive can remain connected to each other via the conductive compound. Therefore, even if the adhesive electrode for acquiring a biological signal is stretched due to deformation of the surface of the skin caused by body movement, the adhesive electrode for acquiring a biological signal according to this embodiment can maintain a state susceptible to stretching, suppress resistance changes, and suppress noise generation, thereby enabling stable acquisition of biological signals.
[0100] Furthermore, the adhesive electrode for acquiring a biological signal can exhibit conductivity by including a conductive polymer. Furthermore, the adhesive electrode for acquiring a biological signal can exhibit adhesive strength, self-adhesiveness, and softness by including a water-dispersible adhesive. Therefore, the adhesive electrode for acquiring a biological signal can exhibit adhesive strength to the skin while having high conformability to deformations on the skin surface, so that even if the skin surface deforms due to body movement, the electrode can remain attached to the skin and maintain low contact impedance, which can be kept below a predetermined value.
[0101] Furthermore, the adhesive electrode for acquiring biological signals according to this embodiment contains a conductive compound, which can increase the elastic modulus and sensitivity to biological signals, thereby improving sensing performance, handling properties, and ease of use.
[0102] The method for measuring the contact impedance of the adhesive electrode for acquiring a biological signal is not particularly limited, and can be measured by any appropriate method. For example, 2 ) is prepared as a test piece, and an end of a copper foil tape having a predetermined size (e.g., 5 mm wide x 10 cm long) is attached to the end of the electrode. The side of the copper foil tape opposite the side attached to the electrode is fixed with a clip connected to a cable. The clip on the other side of the cable is connected to an impedance analyzer, and the adhesive electrode for acquiring biosignals is attached to a part of the skin, and the contact impedance with the skin surface is measured for a predetermined time (e.g., 1 minute). Alternatively, a method for measuring the contact impedance of the adhesive electrode for acquiring biosignals may be used. Instead of using the adhesive electrode for acquiring biosignals as a test piece, a biosensor may be fabricated in which the adhesive electrode for acquiring biosignals is arranged on the attachment surface so that the adhesive electrode for acquiring biosignals can come into contact with the skin, and the contact impedance may be measured using the biosensor.
[0103] The resistance of the adhesive electrode for acquiring a biosignal can be evaluated by measuring the sheet resistance (unit: Ω / □) of the adhesive electrode for acquiring a biosignal. The sheet resistance is the surface resistance of the adhesive electrode for acquiring a biosignal. The sheet resistance can be measured using a common resistance measurement method, for example, by an eddy current measurement method using a non-contact resistance measuring device in accordance with JIS Z 2316-1:2014. The measurement range may be a predetermined range on the main surface of the adhesive electrode for acquiring a biosignal. The above-mentioned method for measuring the resistance of the adhesive electrode for acquiring a biosignal may be used either when the adhesive electrode for acquiring a biosignal is in its initial state (before extension) or when it is extended.
[0104] The resistance of the adhesive electrode for acquiring a biological signal when stretched may be measured in the same manner as in the example of the method for measuring contact impedance described above. That is, a predetermined area (for example, 4 cm 2 ) is prepared as a test piece, and the end of a copper foil tape having a predetermined size (e.g., 5 mm wide x 10 cm long) is attached to the end of the electrode, and the side of the copper foil tape opposite to the side attached to the electrode is fixed with a clip connected to a cable. The clip on the other side of the cable is connected to an impedance analyzer, and the adhesive electrode for acquiring biosignals is attached to a part of the living body, and the contact impedance with the skin is measured for a predetermined time (e.g., 1 minute).
[0105] The method for measuring the adhesive strength of the adhesive electrode for acquiring a biological signal is not particularly limited, and can be measured by any appropriate method. For example, the adhesive strength of the adhesive electrode for acquiring a biological signal may be determined by performing a 180° peel test and measuring the 180° peel strength. For example, the adhesive strength of the adhesive electrode for acquiring a biological signal may be determined by measuring the 180° peel strength of an area of a predetermined size (for example, 4 cm 2) is prepared as a test piece, and the electrode sheet is attached to a support substrate (e.g., a PET film, etc.) to form a backing, thereby preparing a measurement sample. The measurement sample is cut to a predetermined size (e.g., 5 cm x 1 cm) and attached to an adherend (e.g., a stainless steel plate, a bakelite plate, etc.) and fixed. Then, using a tensile tester, the load when the measurement sample is peeled from the adherend under peel conditions of a peel angle of 180° and a predetermined peel speed (e.g., 300 mm / min) is measured, and the adhesive strength (unit: N / 10 mm) is measured.
[0106] The adhesive electrode for acquiring a biological signal according to this embodiment can have a storage modulus G' of 3 MPa to 15 MPa in the room temperature range (e.g., 25°C ± 5°C). The storage modulus G' may be measured using a commonly used method. Note that, since the base material of the adhesive electrode for acquiring a biological signal is a water-dispersible adhesive, the storage modulus G' of the adhesive electrode for acquiring a biological signal can be regarded as the storage modulus G' of the water-dispersible adhesive. Therefore, the storage modulus G' of the water-dispersible adhesive may be used as the storage modulus G' of the adhesive electrode for acquiring a biological signal. As a method for measuring the storage modulus G' of the water-dispersible adhesive, for example, the water-dispersible adhesive is applied to a substrate to a predetermined thickness (e.g., 500 μm), followed by autoclaving to prepare a measurement sample. This measurement sample is punched into a predetermined shape (for example, a disk with a diameter of 5 mm), and the viscoelastic properties are measured using a commonly used viscoelasticity measuring device while raising the temperature from -50°C to 150°C at a rate of 5°C / min. The value at 25°C from the storage modulus G' value may be used as an index of hardness in the normal use range of the electrode.
[0107] The adhesive electrode for acquiring a biological signal can use at least one conductive polymer selected from the group consisting of a polythiophene-based conductive polymer, a polyaniline-based conductive polymer, and a polyacetylene-based conductive polymer as the conductive polymer, thereby ensuring that the adhesive electrode for acquiring a biological signal exhibits conductivity.
[0108] The adhesive electrode for acquiring a biological signal can have a conductive compound content of 0.1 wt % to 50 wt % relative to 100 wt % of the conductive polymer, which allows the adhesive electrode for acquiring a biological signal to maintain conductivity and more reliably suppress resistance changes even when the adhesive electrode for acquiring a biological signal is stretched, thereby reliably suppressing noise generation.
[0109] The adhesive electrode for acquiring a biological signal can use a water-based emulsion adhesive as the water-dispersion adhesive. This allows the adhesive electrode for acquiring a biological signal to suppress a decrease in adhesive strength while maintaining resistance and to improve conformability to the skin surface. Therefore, the adhesive electrode for acquiring a biological signal can improve adhesive strength and conformability to the skin surface.
[0110] The adhesive electrode for acquiring a biological signal can use an acrylic emulsion adhesive instead of an aqueous emulsion adhesive. This allows the adhesive electrode for acquiring a biological signal to further suppress a decrease in adhesive strength while maintaining resistance, and to reliably improve conformability to the skin surface. As a result, the adhesive electrode for acquiring a biological signal can have high adhesive strength and conformability to the skin surface.
[0111] The adhesive electrode for acquiring biological signals can use a silane-based emulsion adhesive containing a water-dispersible copolymer and an organic liquid component in addition to the acrylic emulsion adhesive. This reliably reduces the viscoelasticity of the adhesive electrode for acquiring biological signals, thereby increasing adhesive strength and further improving conformability to the skin surface. This further increases flexibility of the adhesive electrode for acquiring biological signals and more reliably maintains adhesiveness.
[0112] The adhesive electrode for acquiring a biological signal may contain a moisturizing agent. This allows the adhesive electrode for acquiring a biological signal to have improved dispersibility of the conductive polymer in the aqueous adhesive and to have increased conductivity, thereby reducing resistance and improving conductivity and suppressing noise. The adhesive electrode for acquiring a biological signal may also have improved adhesive strength and flexibility.
[0113] Furthermore, the adhesive electrode for acquiring a biological signal can use glycerin as a moisturizing agent. By including glycerin as a moisturizing agent in the adhesive electrode for acquiring a biological signal, the glycerin functions as a dispersant for PEDOT, which is used as a conductive polymer, and can increase the dispersibility of PEDOT and reduce resistance. Furthermore, glycerin can increase the crystallization of PEDOT, which is used as a conductive polymer, and increase conductivity. Therefore, the adhesive electrode for acquiring a biological signal can improve conductivity and further reduce noise.
[0114] As described above, the adhesive electrode for acquiring a biological signal according to this embodiment can be formed into a film, and therefore can be used as an electrode piece in which the adhesive electrode for acquiring a biological signal is provided on a substrate. The electrode piece has higher rigidity than when the adhesive electrode for acquiring a biological signal is used alone, and therefore can be easier to handle.
[0115] The substrate used for the electrode piece can be formed using any appropriate material. Examples of the substrate used for the electrode piece include polyolefin resins such as polyethylene (PE) and polyethylene naphthalate (PEN), polyester resins such as polyethylene terephthalate (PET), acrylic resins, polyurethane resins, polystyrene resins, silicone resins, acrylic resins, vinyl chloride resins, plastic substrates such as polyimide (PI) and polycarbonate (PC), metal plates, and glass substrates. The substrate used for the electrode piece may be a substrate without a porous structure or a substrate (porous body) with a porous structure such as a nonwoven fabric sheet.
[0116] As described above, the adhesive electrode for acquiring a biological signal according to this embodiment exhibits high flexibility and maintains adhesion to the skin, suppresses resistance changes even when the skin surface deforms due to body movement, and can acquire a biological signal stably with low resistance. Therefore, the adhesive electrode for acquiring a biological signal can be effectively used as an electrode (biological electrode) for a biosensor, in particular, a stick-on type biosensor that requires stable acquisition of a biological signal, adhesion to the living body, high flexibility, and safety for the living body.
[0117] Although the embodiments have been described above, they are presented as examples and the present invention is not limited to the above embodiments. The above embodiments can be implemented in various other forms, and various combinations, omissions, substitutions, modifications, etc. can be made without departing from the spirit of the invention. These embodiments and their modifications are included within the scope and spirit of the invention, and are also included in the scope of the invention and its equivalents as set forth in the claims.
[0118] Hereinafter, the embodiment will be described in more detail with reference to examples and comparative examples, but the embodiment is not limited to these examples and comparative examples.
[0119] <Preparation of Conductive Composition> [Preparation of Conductive Composition Aqueous Solution A] 0.8 g of PEDOT / PSS as a conductive polymer and 15 g of water were added to a container and mixed using a stirring mixer (Thinky Corporation) at a rotation speed of 2000 rpm for 10 minutes. Next, 12 g of an emulsion-based adhesive (2EHA / MMA / AA / =90 / 10 / 4, solids concentration 52%) as a binder resin and 2 g of glycerin as a humectant were added, and the mixture was stirred and degassed for 10 minutes using the stirring mixer at 2200 rpm. Furthermore, 3 g of a conductive carbon black aqueous dispersion (solids concentration 6%, product name: CCT-061, Taisei Kako Co., Ltd.) was added as a second conductive material, and the mixture was further mixed and dispersed using the stirring mixer at 2000 rpm for 5 minutes to obtain a conductive composition aqueous solution A.
[0120] [Preparation of conductive composition aqueous solution B] The preparation of the conductive composition aqueous solution A was carried out in the same manner as in Example 1, except that a multi-layered CNT aqueous dispersion (solid content concentration 6%, product name: F9106S, KJ Specialty Paper Co., Ltd.) was used as the second conductive material, to obtain a conductive composition aqueous solution B.
[0121] [Preparation of Conductive Composition Aqueous Solution C] The preparation of the conductive composition aqueous solution A was carried out in the same manner as in Example 1, except that 15 g of a single-layer CNT aqueous dispersion (solid content concentration 0.2%, product name: eDIPS INK, Meijo Nanocarbon Co., Ltd.) was added as the second conductive material, thereby obtaining a conductive composition aqueous solution C.
[0122] [Preparation of Conductive Composition Aqueous Solution D] The preparation of the conductive composition aqueous solution A was carried out in the same manner as in Example 1, except that 0.2 g of silver-plated filler (powder, product name: TFM-S05P, Toyo Aluminum K.K.) was added as the second conductive material, thereby obtaining a conductive composition aqueous solution D.
[0123] [Preparation of Conductive Composition Aqueous Solution E] The preparation of the conductive composition aqueous solution A was carried out in the same manner as in Example 1, except that 1.3 g of a conductive carbon black aqueous dispersion (solid content concentration 6%, product name: CCT-061, Taisei Kako Co., Ltd.) was added as the second conductive material, to obtain a conductive composition aqueous solution E.
[0124] [Preparation of conductive composition aqueous solution F] A conductive composition aqueous solution F was obtained in the same manner as in Example 1, except that in preparing the conductive composition aqueous solution A, 0.8 g of PEDOT / PSS pellets ("Orgacon DRY", manufactured by Agfa Materials Japan, Inc.) and 6 g of a conductive carbon black aqueous dispersion (solid content concentration 6%, product name: CCT-061, Taisei Kako Co., Ltd.) were used as the second conductive material.
[0125] [Preparation of Aqueous Conductive Composition Solution G] Aqueous conductive composition solution G was obtained in the same manner as in Example 1, except that the aqueous conductive composition solution A was prepared without adding the second conductive material.
[0126] [Preparation of conductive composition aqueous solution H] The preparation of the conductive composition aqueous solution A was carried out in the same manner as in Example 1, except that in the preparation of the conductive composition aqueous solution A, 12 g of the carbon black aqueous dispersion used in Example 1 was used as the first conductive material, and 10.0 g of an emulsion-based pressure-sensitive adhesive (2EHA / MMA / AA / =90 / 10 / 4, solid content concentration 52%) was used, and 4 g of the multi-layered CNT aqueous dispersion used in Example 2 was used as the second conductive material, to obtain a conductive composition aqueous solution H.
[0127] <Preparation of Electrode Sheet> [Example 1] The prepared aqueous conductive composition solution A was applied using an applicator to a polyethylene terephthalate (PET) film (PET-50-SCA1, manufactured by Fujiko Co., Ltd., thickness 50 μm) that had been surface-treated with a silicone-based release agent. The PET film coated with the aqueous conductive composition solution was then transported to a drying oven (SPHH-201, manufactured by ESPEC Corporation), and the aqueous conductive composition solution A was heated and dried at 130°C for 3 minutes to prepare a cured product of the conductive composition. The cured product was punched (pressed) into a desired shape to form a sheet, thereby preparing an electrode sheet (bioelectrode) with a thickness of 30 μm.
[0128] [Examples 2 to 6, Comparative Examples 1 and 2] Electrode sheets were prepared in the same manner as in Example 1, except that the conductive composition aqueous solution A in Example 1 was changed to one of the conductive composition aqueous solutions B to F.
[0129] Table 1 shows the types of coordination liquid, types of conductive materials, and conductive material ratios used to prepare the electrode sheets in the above-mentioned Examples and Comparative Examples.
[0130] <Evaluation of Electrode Sheet> The electrode sheets obtained in each of the Examples and Comparative Examples were measured for contact impedance, sheet resistance, resistance during elongation, adhesive strength, elongation at break, and storage modulus G'.
[0131] [Measurement of contact impedance] The electrode sheet was placed at a 2 An electrode sheet test specimen was prepared by cutting the electrode sheet to an area of 100 mm. The end of a copper foil tape cut to a width of 5 mm and a length of 10 cm was attached to the end of the test specimen, and the side of the copper foil tape opposite the surface attached to the test specimen was fixed with an alligator clip attached to one end of a cable. The clip on the other end of the cable was connected to an impedance analyzer (product name: IM3570, manufactured by Hioki E.E. Corporation, frequency set to 1 kHz), and the electrode sheet was then attached to the subject's inner arm, and the contact impedance with the skin was measured for 1 minute. The measurement results of the contact impedance of the electrode sheets of each Example and Comparative Example are shown in Table 1.
[0132] [Sheet Resistance] Using a non-contact resistance measuring instrument (NC-80NC, manufactured by Napson Corporation), the sheet resistance was measured as the surface resistance of the electrode sheet by an eddy current measurement method in accordance with JIS Z 2316-1:2014. The measurement range was 0.5 mm to 150 mm from the main surface of the electrode sheet. The measurement results of the sheet resistance of the electrode sheets of each example and comparative example are shown in Table 1.
[0133] [Resistance during stretching] The electrode sheet was cut to a length of 11 cm and a width of 1 cm, and both ends of the cut electrode sheet were fixed to a stretching device at a width of 5 mm each (fixed within 5 mm from each end). Both ends of the electrode sheet were fixed with alligator clips attached to one end of a cable. The clip on the other end of the cable was connected to an impedance analyzer (product name: IM3570, manufactured by Hioki E.E. Corporation). A voltage of 2 V was applied to the electrode sheet using the impedance analyzer, and the current value was measured while the electrode sheet was stretched by 10% at a time, thereby measuring the resistance change of the electrode sheet. Table 1 shows the resistance measurement results when the electrode sheets of each example and comparative example were stretched by 20% (at 20% stretch) and 100% (at 100% stretch).
[0134] [Adhesive Strength] The electrode sheet was cut into a length of 5 cm and a width of 1 cm and backed with a PET film (Lumirror S10, 25 μm thick) to prepare a measurement sample. The measurement sample was then attached to the adherend, a bakelite board, and fixed by rolling it back and forth with a 2 kg roller. Using a tensile tester (AGS-J, manufactured by Shimadzu Corporation), the load when the measurement sample was peeled from the adherend was measured under peel conditions of a peel angle of 180° and a peel rate (tensile speed) of 300 mm / min, and the adhesive strength (unit: N / 10 mm) was measured. The measurement results of the adhesive strength of the electrode sheets of each example and comparative example are shown in Table 1.
[0135] [Elongation at break] The electrode sheet was cut into a length of 5 cm and a width of 1 cm, and each of the cut electrode sheets was reinforced with paper at both ends for 2 cm. The cut electrode sheet was then set in a tensile tester (AGS-J, manufactured by Shimadzu Corporation) so that the measurement section was 1 cm long. The set electrode sheet was pulled at a speed (tensile speed) of 50 mm / min, and the elongation at break was measured. The electrode sheet was pulled up to a maximum of 500%.
[0136] [Elastic Modulus at 25°C] The aqueous PSA was applied to a substrate to a thickness of 500 μm, and then autoclaved to prepare a measurement sample. The measurement sample was punched out to a diameter of 5 mm using a punch, and the viscoelasticity was measured using a viscoelasticity measuring device (ARES-G2) while the temperature was raised from -50°C to 150°C at a rate of 5°C / min. The elastic modulus at 25°C obtained from the data on the storage modulus G' was used as an index of the hardness of the electrode during normal use.
[0137]
[0138] As can be seen from Table 1, the increase in resistance during stretching relative to the initial resistance (before stretching) was suppressed in each example compared to each comparative example. Therefore, it was confirmed that the electrode sheets of the above examples can suppress resistance changes by including a conductive polymer and a conductive compound other than the conductive polymer as the conductive material. Therefore, it can be said that the adhesive electrode for acquiring biosignals according to this embodiment can be effectively used for stably measuring bioinformation over a long period of time, even when attached to the skin of a subject for a long period of time (e.g., 24 hours).
[0139] Note that, for example, aspects of the present invention are as follows. <1> An adhesive electrode for acquiring a biological signal, comprising: a conductive material containing a conductive polymer and one or more conductive compounds other than the conductive polymer; and an aqueous dispersion-based adhesive. <2> The adhesive electrode for acquiring a biological signal according to <1>, wherein the conductive polymer is at least one of a polythiophene-based conductive polymer, a polyaniline-based conductive polymer, and a polyacetylene-based conductive polymer. <3> The adhesive electrode for acquiring a biological signal according to <1> or <2>, wherein the content of the conductive compound is 0.1 wt % to 50 wt % relative to 100 wt % of the conductive polymer. <4> The adhesive electrode for acquiring a biological signal according to any one of <1> to <3>, wherein the aqueous dispersion-based adhesive is an aqueous emulsion adhesive. <5> The adhesive electrode for acquiring a biological signal according to <4>, wherein the aqueous emulsion adhesive is an acrylic emulsion adhesive. <6> The adhesive electrode for acquiring a biological signal according to <5>, wherein the acrylic emulsion adhesive is a silane emulsion adhesive containing a water-dispersible copolymer and an organic liquid component compatible with the water-dispersible copolymer. <7> The adhesive electrode for acquiring a biological signal according to any one of <1> to <6>, which contains a humectant. <8> The adhesive electrode for acquiring a biological signal according to <7>, wherein the humectant is glycerin. <9> An electrode piece comprising the adhesive electrode for acquiring a biological signal according to any one of <1> to <8> provided on a substrate. <10> A biosensor comprising the adhesive electrode for acquiring a biological signal according to any one of <1> to <8>.
[0140] <11> A method for manufacturing an adhesive electrode for acquiring a biological signal, comprising: a step of mixing an aqueous adhesive composition solution containing a conductive polymer and a water-dispersible adhesive with an aqueous conductive compound-containing solution containing a conductive compound to prepare an aqueous conductive composition solution; and a step of drying the aqueous conductive composition solution to evaporate water contained in the aqueous conductive composition solution, thereby obtaining a cured product of an adhesive electrode-forming composition having a conductive material containing the conductive polymer and the conductive compound, and the water-dispersible adhesive.
[0141] This application claims priority based on Japanese Patent Application No. 2023-54112, filed with the Japan Patent Office on March 29, 2023, and incorporates the entire contents of said application by reference.
[0142] REFERENCE SIGNS LIST 1 adhesive electrode for acquiring biological signals 11 conductive material 12 water-dispersible adhesive 13 moisturizer 111 conductive polymer 112 conductive compound
Claims
1. An adhesive electrode for acquiring biological signals, comprising: a conductive material containing a conductive polymer and one or more conductive compounds other than the conductive polymer; and a water-dispersible adhesive.
2. An adhesive electrode for acquiring biological signals as described in claim 1, wherein the conductive polymer is at least one type of conductive polymer selected from the group consisting of polythiophene-based conductive polymers, polyaniline-based conductive polymers, and polyacetylene-based conductive polymers.
3. An adhesive electrode for acquiring biological signals as described in claim 1, wherein the content of the conductive compound is 0.1 wt % to 50 wt % relative to 100 wt % of the conductive polymer.
4. An adhesive electrode for acquiring biological signals as described in claim 1, wherein the water-dispersed adhesive is a water-based emulsion adhesive.
5. The adhesive electrode for acquiring biological signals according to claim 4, wherein the aqueous emulsion adhesive is an acrylic emulsion adhesive.
6. An adhesive electrode for acquiring biological signals as described in claim 5, wherein the acrylic emulsion adhesive is a silane emulsion adhesive containing a water-dispersible copolymer and an organic liquid component that is compatible with the water-dispersible copolymer.
7. The adhesive electrode for acquiring biological signals according to claim 1, which contains a moisturizing agent.
8. An adhesive electrode for acquiring biological signals as described in claim 7, wherein the moisturizer is glycerin.
9. An electrode piece comprising the adhesive electrode for acquiring biosignals according to claim 1 provided on a substrate.
10. A biosensor comprising the adhesive electrode for acquiring biosignals according to claim 1.
11. A method for manufacturing an adhesive electrode for acquiring a biological signal, comprising: a step of mixing an aqueous adhesive composition solution containing a conductive polymer and a water-dispersible adhesive with an aqueous conductive compound-containing solution containing a conductive compound to prepare an aqueous conductive composition solution; and a step of drying the aqueous conductive composition solution to evaporate water contained in the aqueous conductive composition solution, thereby obtaining a cured product of an adhesive electrode-forming composition having a conductive material containing the conductive polymer and the conductive compound, and the water-dispersible adhesive.
Citation Information
Patent Citations
Biological electrode composition, biological electrode, and biological electrode manufacturing method
JP2020031722A
Self-adhesive electrode patch
JP2020527974A
Hydrogel
WO2018062030A1
Biosensor
WO2021200806A1
Cited By
Electrode material with both electronic conduction and interface adhesion and preparation method thereof
CN119798900A