Optical film, optically anisotropic film, laminate, and display device

The optical film with a changing region and a laminate configuration addresses light leakage in virtual reality display devices by controlling in-plane retardation and slow axis direction changes, effectively reducing optical differences and improving display quality.

WO2024204762A1PCT designated stage expired Publication Date: 2024-10-03FUJIFILM CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/013180
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-29
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Virtual reality display devices with pancake lens type configurations experience light leakage due to variations in in-plane retardation and direction of the in-plane slow axis when laminated optical films with retardation layers are curved, leading to optical differences and leakage issues.

Method used

An optical film with a changing region where in-plane retardation and the direction of the in-plane slow axis change, specifically designed to suppress variations by gradually decreasing or increasing retardation and axis direction from the center, and a laminate incorporating this film with an absorption polarizer to control the angle between their slow axes, effectively reducing light leakage.

Benefits of technology

The solution significantly reduces light leakage in virtual reality display devices by minimizing variations in in-plane retardation and slow axis direction, ensuring consistent optical performance across the curved surface, thereby enhancing the display quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024013180_03102024_PF_FP_ABST
    Figure JP2024013180_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides: an optical film used for manufacturing an optically anisotropic film for which the occurrence of light leakage is suppressed when applied to a pancake-lens virtual reality display device; an optically anisotropic film; a laminate; and a display device. This optical film has a change region in which at least one of the in-plane retardation and the direction of an in-plane slow axis changes. If the in-plane retardation changes in the change region, the in-plane retardation gradually changes outward from the center of the change region, and if the direction of the in-plane slow axis changes in the change region, the in-plane slow axis in the change region satisfies a prescribed requirement.
Need to check novelty before this filing date? Find Prior Art

Description

Optical film, optically anisotropic film, laminate, display device

[0001] The present invention relates to an optical film, an optically anisotropic film, a laminate, and a display device.

[0002] A virtual reality display device is a display device that allows a user to feel as if they are immersed in a virtual world by wearing a dedicated headset on their head and viewing images displayed through lenses. For example, a configuration called a pancake lens has been proposed for a virtual reality display device, which has an image display device, a reflective polarizer, a half mirror, and a retardation layer, and which reduces the overall thickness of the headset by directing light emitted from the image display device back and forth between the reflective polarizer and the half mirror.

[0003] Patent Document 1 discloses a laminated optical film including a retardation layer that converts circularly polarized light into linearly polarized light, and describes that this laminated optical film can be applied to a virtual reality display device.

[0004] International Publication No. 2022 / 075475

[0005] As described in Patent Document 1, when a laminated optical film is applied to a virtual reality display device, the laminated optical film may be formed into a non-planar shape such as a curved shape in accordance with the shape of a lens, etc. The present inventors have found that when a laminated optical film including a retardation layer as described in Patent Document 1 is formed into a curved shape and applied to a pancake lens type virtual reality display device, light leakage is observed and that it is necessary to suppress this.

[0006] In view of the above circumstances, an object of the present invention is to provide an optical film used in manufacturing an optically anisotropic film that suppresses the generation of leaked light when applied to a pancake lens-type virtual reality display device. Another object of the present invention is to provide an optically anisotropic film that suppresses the generation of leaked light when applied to a pancake lens-type virtual reality display device. Another object of the present invention is to provide a laminate and a display device.

[0007] The present inventors have conducted extensive research into the above-mentioned problems and have found that the above problems can be solved by the following configuration.

[0008] (1) An optical film having a change region in which at least one of the in-plane retardation and the direction of the in-plane slow axis changes, wherein when the in-plane retardation changes in the change region, the in-plane retardation changes gradually from the center of the change region toward the outside, and when the direction of the in-plane slow axis changes in the change region, the direction of the in-plane slow axis at the center is parallel to the average direction of the in-plane slow axis of the change region, and the direction of the in-plane slow axis on the third reference line changes gradually from the center of the change region toward the outside, when a line passing through the center of the change region and parallel to the average direction of the in-plane slow axis of the change region is defined as a first reference line, a line passing through the center of the change region and intersecting the first reference line is defined as a second reference line, and two lines passing through the center of the change region and forming an angle of 45° with the first and second reference lines are defined as third reference lines. (2) The optical film according to (1), wherein the average in-plane retardation at a wavelength of 550 nm in the change region is 100 to 300 nm. (3) The optical film according to (1) or (2), wherein, when the in-plane retardation changes in the change region, the in-plane retardation gradually decreases from the center of the change region toward the outside. (4) The optical film according to any one of (1) to (3), wherein, in two adjacent divided regions surrounded by a first reference line and a third reference line in the change region, points P1 and P2 that satisfy the relationship of Requirement 1 described below are present, and in two adjacent divided regions surrounded by a second reference line and a third reference line in the change region, points P3 and P4 that satisfy the relationship of Requirement 2 described below are present. (5) A laminate including the optical film according to any one of (1) to (4) and an absorptive polarizer, wherein the angle formed by the average direction of the in-plane slow axes of the change region of the optical film and the absorption axis of the absorptive polarizer is within a range of 40 to 50°. (6) An optically anisotropic film having a convex curved surface portion, the optically anisotropic film satisfying the relationships of the following formulas (1) and (2). (7) A display device including the optically anisotropic film according to (6). (8) The display device according to (7), which is a virtual reality display device.

[0009] According to the present invention, an optical film can be provided that is used to manufacture an optically anisotropic film that suppresses the generation of leaked light when applied to a pancake lens type virtual reality display device. According to the present invention, an optically anisotropic film can be provided that suppresses the generation of leaked light when applied to a pancake lens type virtual reality display device. According to the present invention, a laminate and a display device can be provided.

[0010] FIG. 1 is a top view of an example of a first embodiment of the optical film of the present invention. FIG. 2 is a diagram illustrating the procedure for molding a film using a mold having a concave molding surface. FIG. 3 is a diagram illustrating the procedure for molding a film using a mold having a concave molding surface. FIG. 4 is a top view of a film used for molding. FIG. 5 is a diagram illustrating the procedure for molding a film using a mold having a convex molding surface. FIG. 6 is a diagram illustrating the procedure for molding a film using a mold having a convex molding surface. FIG. 7 is a top view of another example of the first embodiment of the optical film of the present invention. FIG. 8 is a top view of an example of a second embodiment of the optical film of the present invention. FIG. 9 is a top view of a film used for molding. FIG. 10 is a schematic diagram illustrating an example of a manufacturing procedure for the optical film of the present invention. FIG. 11 is a schematic diagram illustrating an example of a manufacturing method for an alignment film used in manufacturing the optical film of the present invention. FIG. 12 is a partially enlarged schematic diagram of FIG. 11. FIG. 13 is a top view of an example of an optically anisotropic film. FIG. 14 is a cross-sectional view taken along line A-A in FIG. 13. Fig. 15 is a top view showing another example of an optically anisotropic film. Fig. 16 is a cross-sectional view showing an example of a laminate of the present invention. Fig. 17 is a cross-sectional view showing another example of a laminate of the present invention. Fig. 18 is a cross-sectional view showing an example of a composite lens of the present invention. Fig. 19 is a diagram showing an example of a virtual reality display device of the present invention, showing an example of a light ray of a main image. Fig. 20 is a diagram plotting the results of Examples and Comparative Examples.

[0011] The present invention will be described in detail below. The following description of the constituent elements may be based on representative embodiments and specific examples, but the present invention is not limited to such embodiments. In this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits.

[0012] In this specification, "absorption axis" refers to the polarization direction in which absorbance is maximized in the plane when linearly polarized light is incident. "Reflection axis" refers to the polarization direction in which reflectance is maximized in the plane when linearly polarized light is incident. "Transmission axis" refers to the direction in the plane that is perpendicular to the absorption axis or reflection axis. "In-plane slow axis" refers to the direction in the plane in which refractive index is maximized.

[0013] In this specification, Re(λ) and Rth(λ) represent the in-plane retardation and the thickness retardation, respectively, at a wavelength λ. Unless otherwise specified, the wavelength λ is 550 nm. In the present invention, Re(λ) and Rth(λ) are values ​​measured at a wavelength λ using an AxoScan (manufactured by Axometrics). By inputting the average refractive index ((nx + ny + nz) / 3) and film thickness (d) into AxoScan, the following in-plane slow axis direction (°) is calculated: Re(λ) = R0(λ) Rth(λ) = ((nx + ny) / 2 - nz) × d. Note that R0(λ) is displayed as a numerical value calculated by AxoScan, but it means Re(λ).

[0014] In this specification, the refractive indices nx, ny, and nz are measured using an Abbe refractometer (NAR-4T, manufactured by Atago Co., Ltd.) with a sodium lamp (λ = 589 nm) as a light source. When measuring wavelength dependency, measurements can be made using a multi-wavelength Abbe refractometer DR-M2 (manufactured by Atago Co., Ltd.) in combination with an interference filter. Values ​​from the Polymer Handbook (John Wiley & Sons, Inc.) and catalogs of various optical films can also be used. Examples of average refractive index values ​​for major optical films are listed below: cellulose acylate (1.48), cycloolefin polymer (1.52), polycarbonate (1.59), polymethyl methacrylate (1.49), and polystyrene (1.59).

[0015] In this specification, A plates and C plates are defined as follows. There are two types of A plates: positive A plates (positive A plates) and negative A plates (negative A plates). When the refractive index in the in-plane slow axis direction of the film (the direction in which the in-plane refractive index is maximum) is nx, the refractive index in the direction perpendicular to the in-plane slow axis is ny, and the refractive index in the thickness direction is nz, the positive A plates satisfy the relationship of formula (A1), and the negative A plates satisfy the relationship of formula (A2). Note that the positive A plates have a positive Rth, and the negative A plates have a negative Rth. Formula (A1) nx>ny≒nz Formula (A2) ny<nx≒nz Note that the above "≒" encompasses not only the case where the two are completely identical, but also the case where the two are substantially identical. "Substantially the same" means, for example, that "ny ≒ nz" also includes cases where (ny - nz) x d (where d is the film thickness) is -10 to 10 nm, preferably -5 to 5 nm, and "nx ≒ nz" also includes cases where (nx - nz) x d is -10 to 10 nm, preferably -5 to 5 nm. There are two types of C plates: positive C plates (positive C plates) and negative C plates (negative C plates). Positive C plates satisfy the relationship of formula (C1), while negative C plates satisfy the relationship of formula (C2). Note that positive C plates have a negative Rth value, and negative C plates have a positive Rth value. Formula (C1) nz > nx ≒ ny Formula (C2) nz < nx ≒ ny Note that the above "≒" includes not only cases where the two are completely identical, but also cases where the two are substantially identical. The term "substantially the same" includes, for example, the case where (nx-ny) x d (where d is the thickness of the film) is 0 to 10 nm, preferably 0 to 5 nm, in "nx≈ny".

[0016] A characteristic feature of the optical film of the present invention is that it has a change region in which at least one of the in-plane retardation and the direction of the in-plane slow axis changes. The present inventors investigated the cause of light leakage when a laminated optical film including the retardation layer described in Patent Document 1 is curved and applied to a pancake lens-type virtual reality display device, and found that light leakage occurs due to variations in the in-plane retardation and / or the direction of the in-plane slow axis within the curved retardation layer. More specifically, when the retardation layer is molded into a curved shape, there are locations where the magnitude of the in-plane retardation and / or the orientation of the in-plane slow axis are likely to differ between before and after molding, and therefore variations in the in-plane retardation and / or the direction of the in-plane slow axis occur in the molded product, and these variations are responsible for light leakage. Based on the above findings, the present inventors have discovered that by providing a change region in which at least one of the in-plane retardation and the direction of the in-plane slow axis is changed in the optical film itself used for molding, the occurrence of variations in in-plane retardation and / or variations in the direction of the in-plane slow axis in the optically anisotropic film (molded product) obtained by molding can be suppressed.

[0017] The present invention also finds that the generation of leakage light can be suppressed by applying an optically anisotropic film having a convex curved surface portion that satisfies certain requirements (the relationship between equations (1) and (2) described below) to a virtual reality display device.

[0018] In the following, the optical film will be described in detail first, and then the optically anisotropic film will be described in detail.

[0019] <First Embodiment of Optical Film> FIG. 1 is a top view of an example of a first embodiment of the optical film of the present invention. The optical film 10A has a change region 12A in which the in-plane retardation changes. The change region 12A is a region extending in the in-plane direction of the optical film 10A and is circular in FIG. 1 . As will be described later, the change region 12A is a region formed into a convex curved surface by molding. In the change region 12A, as indicated by the white arrows, the in-plane retardation gradually decreases from the center C of the change region 12A toward the outer edge. More specifically, in the change region 12A, the in-plane retardation gradually decreases from the center C toward the periphery of the change region 12A. In other words, as indicated by the dashed lines in FIG. 1 , the in-plane retardation continuously decreases concentrically. The center of the change region 12A corresponds to the center of gravity of the change region 12A. In other words, in this specification, the center of the change region refers to the center of gravity of the change region. In Fig. 1, the in-plane retardation changes continuously from the center C of the change region 12A toward the outside, but is not limited to this form and may decrease stepwise. In Fig. 1, the region other than the change region 12A in the optical film 10A may have optical anisotropy or may be isotropic.

[0020] The decrease in in-plane retardation from the center C of the change region 12A to the periphery of the change region 12A is not particularly limited, and an optimal value is selected as appropriate depending on molding conditions, etc. In particular, when the in-plane retardation gradually decreases outward from the center C as described above, the absolute value of the difference between the in-plane retardation at a wavelength of 550 nm at the center C of the change region 12A and the in-plane retardation at a wavelength of 550 nm at a position on the periphery of the change region 12A (hereinafter simply referred to as "specific difference 1") is preferably 5 to 100 nm, more preferably 10 to 50 nm. Furthermore, the decrease rate of the in-plane retardation from the center C of the change region 12A to the periphery of the change region 12A is not particularly limited, and an optimal value is selected as appropriate depending on molding conditions, etc. In particular, the ratio of the specific difference 1 to the distance (mm) from the center C of the change area 12A to the periphery of the change area 12A (specific difference 1 / distance (nm / mm)) is preferably 0.2 to 4 (nm / mm), and more preferably 0.4 to 2 (nm / mm).

[0021] The in-plane retardation at a wavelength of 550 nm at the center C of the change region 12A is not particularly limited, and an optimum value is selected depending on the purpose of use. For example, when an optically anisotropic film that functions as a λ / 4 plate is manufactured using the optical film, the in-plane retardation at a wavelength of 550 nm at the center C of the change region 12A is preferably 130 to 250 nm, more preferably 140 to 200 nm. Furthermore, when an optically anisotropic film that functions as a λ / 4 plate is manufactured using the optical film, the in-plane retardation at a wavelength of 550 nm at a position on the periphery of the change region 12A is preferably 120 to 200 nm, more preferably 130 to 180 nm.

[0022] 1, the change region 12A corresponds to a partial region in the in-plane direction of the optical film 10A, but the present invention is not limited to this embodiment, and the change region may cover the entire in-plane region of the optical film 10A. In particular, the equivalent circle diameter of the change region 12A is preferably 20 to 80 mm, and more preferably 30 to 70 mm. The equivalent circle diameter is the diameter of a perfect circle having the same area as the area of ​​the change region 12A.

[0023] In FIG. 1, the shape of the change area 12A is a perfect circle, but the present invention is not limited to this form, and the shape of the change area may be an ellipse or an irregular shape.

[0024] The reason why variations in in-plane retardation are suppressed by producing an optically anisotropic film having a convexly curved surface portion using the optical film 10A having the above-described change region 12A will be explained below. First, as an example, a phenomenon that occurs when a film is molded using a mold having a concave molding surface will be explained below with reference to FIGS. 2 to 4. FIGS. 2 and 3 show the procedure for molding a film using a mold having a concave molding surface, and FIG. 4 shows the film used for molding. As shown in FIG. 2, a circular film 22 is placed on a mold 20 having a concave molding surface. As shown in FIG. 3, the film 22 is deformed so as to conform to the molding surface of the mold 20, thereby obtaining a film 24 (which also corresponds to a film having a convexly curved surface portion) onto which the concave shape has been transferred. Typically, when a mold having such a concave molding surface is used, differences in the stretching ratio occur between the central portion 22C of the film 22 and the peripheral portion 22R surrounding the central portion 22C, as shown in FIGS. 2 and 4. More specifically, the central portion 22C of the film 22 is more easily stretched than the peripheral portion 22R of the film 22. As a result, in the film 24 to which the concave shape has been transferred, the thickness of the central portion 24C is thinner than the thickness of the peripheral portion 24R. As a result, after molding, the in-plane retardation of the central portion 24C is smaller than the in-plane retardation of the peripheral portion 24R.

[0025] In contrast, when a molding die having a concave molding surface is used to transfer a concave shape to the change region 12A in the optical film 10A described above, similar to that of the film 22, the decrease in in-plane retardation before and after molding is large at a position near the center C of the change region 12A, and small at a position near the periphery of the change region 12A. As described above, in-plane retardation in the change region 12A inherently decreases gradually from the center to the outside. Therefore, the in-plane retardation after molding near the center of the change region 12A and the in-plane retardation after molding near the periphery of the change region 12A are approximately the same. As a result, in the state of the change region 12A after molding, the in-plane retardation is approximately the same at all positions, thereby suppressing the occurrence of variations in in-plane retardation in the in-plane direction.

[0026] 1, the in-plane retardation gradually decreases from the center C of the change region 12A toward the outside, but the present invention is not limited to this embodiment, and the in-plane retardation may gradually increase from the center of the change region toward the outside. When the in-plane retardation gradually increases, it may increase continuously or stepwise.

[0027] When the in-plane retardation gradually increases from the center of the change region toward the outside as described above, the increase in in-plane retardation from the center of the change region to the periphery of the change region is not particularly limited, and an optimal value is selected as appropriate depending on molding conditions, etc. In particular, the absolute value of the difference between the in-plane retardation at a wavelength of 550 nm at the center of the change region and the in-plane retardation at a wavelength of 550 nm at a position on the periphery of the change region (hereinafter simply referred to as "specific difference 2") is preferably 5 to 100 nm, more preferably 10 to 50 nm. Furthermore, the rate of increase in in-plane retardation from the center of the change region to the periphery of the change region is not particularly limited, and an optimal value is selected as appropriate depending on molding conditions, etc. In particular, the ratio of specific difference 2 to the distance (mm) from the center of the change region to the periphery of the change region (specific difference 2 / distance (nm / mm)) is preferably 0.2 to 4 (nm / mm), more preferably 0.4 to 2 (nm / mm).

[0028] When the in-plane retardation gradually increases from the center of the change region toward the outside as described above, the in-plane retardation at a wavelength of 550 nm at the center of the change region is not particularly limited, and an optimal value is selected depending on the purpose of use. For example, when an optically anisotropic film functioning as a λ / 4 plate is produced using the optical film, the in-plane retardation at a wavelength of 550 nm at the center of the change region is preferably 120 to 200 nm, more preferably 130 to 180 nm. Furthermore, when an optically anisotropic film functioning as a λ / 4 plate is produced using the optical film, the in-plane retardation at a wavelength of 550 nm at a position on the periphery of the change region is preferably 130 to 250 nm, more preferably 140 to 200 nm.

[0029] As described above, when the in-plane retardation gradually increases from the center toward the outside in the transition region, molding is preferably performed using a mold having a convex molding surface. Below, we first explain the phenomenon that occurs when molding a film using a mold having a convex molding surface, using FIGS. 4 to 6. FIGS. 5 and 6 show the procedure for molding a film using a mold having a convex molding surface, and FIG. 4 shows the film used for molding. As shown in FIG. 5, a circular film 22 is placed on a mold 26 having a convex molding surface, and as shown in FIG. 6, the film 22 is deformed to fit the molding surface of the mold 26, thereby obtaining a film 28 with a transferred convex shape. Typically, when using a mold having such a convex molding surface, differences in the stretching ratio occur between the central portion 22C and the peripheral portion 22R of the film 22, as shown in FIGS. 5 and 6. More specifically, the peripheral portion 22R of the film 22 is more easily stretched than the central portion 22C of the film 22. As a result, in the film 28 to which the convex surface shape has been transferred, the film thickness of the peripheral portion 28R is thinner than the film thickness of the central portion 28C, and as a result, after molding, the in-plane retardation of the peripheral portion 28R is smaller than the in-plane retardation of the central portion 28C.

[0030] In contrast, if a molding die having a convex molding surface is used to transfer a convex shape, similar to that of the above-mentioned film 22, to a change region portion in which the in-plane retardation gradually increases from the center toward the periphery of the change region, the decrease in in-plane retardation will be small near the center of the change region and large near the periphery of the change region. Therefore, the in-plane retardation after molding near the center of the change region and the in-plane retardation after molding near the periphery of the change region will be approximately the same. In other words, in the state after molding of the change region in which the in-plane retardation gradually increases from the center toward the periphery, the in-plane retardation will be approximately the same at all positions, and the occurrence of variation in in-plane retardation in the in-plane direction can be suppressed.

[0031] Although FIG. 1 illustrates an embodiment in which the in-plane retardation in the change region 12A changes concentrically, the embodiment is not limited thereto as long as the in-plane retardation gradually changes from the center toward the outside. For example, as shown in FIG. 7 , an optical film 10B has a change region 12B, and as indicated by the dashed line, the in-plane retardation may gradually change in a concentric elliptical shape from the center C of the change region 12B toward the outside. The in-plane retardation gradually changing concentrically may be either a gradual decrease or a gradual increase. When the in-plane retardation gradually changes concentrically, the angle between the major axis of the ellipse and the average direction of the in-plane slow axes of the change region is preferably in the range of 70 to 110°, more preferably 80 to 100°. When the change region is molded to be extended further near the center, a gradual change in the in-plane retardation in a concentric circular shape is preferred. Furthermore, when the transition region is formed by extending the peripheral area of ​​the transition region more significantly, it is preferable that the in-plane retardation gradually changes in the shape of a concentric ellipse. The average direction of the in-plane slow axis of the transition region can be measured by the method described later.

[0032] <Second Embodiment of Optical Film> FIG. 8 is a top view of an example of a second embodiment of the optical film of the present invention. The optical film 10C has a change region 12C in which the direction of the in-plane slow axis changes. The change region 12C is a region extending in the in-plane direction of the optical film 10C and is circular in FIG. 8 . As described below, the change region 12C is a region formed into a convex curved surface by molding. In FIG. 8 , regions other than the change region 12C in the optical film 10C may be optically anisotropic or isotropic. In FIG. 8 , the solid line SX in the change region 12C represents the direction of the in-plane slow axis at each position. As shown in FIG. 8 , the direction of the in-plane slow axis changes in the change region 12C. Note that the direction indicated by the hollow arrow in FIG. 8 is the average direction of the in-plane slow axis of the change region 12C. The average direction is the direction obtained by averaging the directions of the in-plane slow axes at 1,000 or more locations in the change region 12C. The average direction of the in-plane slow axis can be determined using a known device, for example, a polarization camera. A polarization camera is a camera capable of acquiring polarization information possessed by a subject. The type of polarization camera is not particularly limited, and examples include devices in which a polarizing filter containing multiple polarizers is mounted on a sensor array (image sensor). The measurement can also be performed using a two-dimensional birefringence evaluation system. Examples of the two-dimensional birefringence evaluation system used in the present invention include the two-dimensional birefringence evaluation system (WPA-200) manufactured by Photonic Lattice Inc. For example, the above-mentioned two-dimensional birefringence evaluation system can determine the direction of the absorption axis at 10,000 to 200,000 positions. When measuring the direction of the in-plane slow axis at each position within the change region using a device such as a polarization camera or a two-dimensional birefringence evaluation system, the device is positioned in a direction corresponding to the normal direction of the optical film, and the measurement is performed.

[0033] 8, a line that passes through the center C of the change region 12C and is parallel to the average direction of the in-plane slow axes of the change region 12C (the direction of the outline arrow in FIG. 8) is referred to as a first reference line L1, a line that passes through the center C of the change region 12C and is perpendicular to the first reference line is referred to as a second reference line L2, and two lines that pass through the center C of the change region 12C and form a 45° angle with the first reference line L1 and the second reference line L2 are referred to as a third reference line L3. Note that the center of the change region 12C corresponds to the center of gravity of the change region 12C.

[0034] In the change region 12C, the direction of the in-plane slow axis at the center C is parallel to the average direction of the in-plane slow axes of the change region 12C. The term "parallel" is intended to include the range of error acceptable in the technical field to which the present invention pertains, and in the present invention, the angle formed between the in-plane slow axis at the center C and the average direction of the in-plane slow axes of the change region 12C may be within a range of 0 to 5°. In particular, the angle is preferably within a range of 0 to 3°.

[0035] Furthermore, within the change region 12C, the direction of the in-plane slow axis on the third reference line L3 gradually changes from the center C of the change region 12C toward the outside. More specifically, in the direction from the center C of the change region 12C toward the top of the paper in FIG. 8 , the third reference line L3 intersects with the in-plane slow axis represented by the three solid lines in the figure, and the angle (acute angle) between the in-plane slow axis and the third reference line L3 gradually increases as one moves outward from the center C. In other words, the angle (acute angle) between the in-plane slow axis at each position on the third reference line L3 and the third reference line gradually increases toward the outside from the center C. Note that, even in the direction from the center C of the change region 12C toward the bottom of the paper in FIG. 8 , the angle (acute angle) between the in-plane slow axis at each position on the third reference line L3 and the third reference line gradually increases toward the outside from the center C. Also in the direction from the center C of the change region 12C in Fig. 8 toward the right on the paper, the angle (acute angle) formed between the in-plane slow axis at each position on the third reference line L3 and the third reference line gradually increases outward from the center C. Also in the direction from the center C of the change region 12C in Fig. 8 toward the left on the paper, the angle (acute angle) formed between the in-plane slow axis at each position on the third reference line L3 and the third reference line gradually increases outward from the center C. In Fig. 8 , the angle formed between the direction of the in-plane slow axis at each position and the third reference line continuously changes outward from the center C of the change region 12C on the third reference line, but is not limited to this mode and may decrease stepwise.

[0036] The angle between the in-plane slow axis at the center C of the change region 12C and the in-plane slow axis at a position on the third reference line and on the periphery of the change region is not particularly limited, but is often 0.4 to 5°, and more often 0.4 to 3°.

[0037] The reason why variations in the direction of the in-plane slow axis are suppressed by producing an optically anisotropic film having a convexly curved surface portion using the optical film 10C having the above-described change region 12C will be explained below. First, as an example, a phenomenon that occurs when a film is molded using a mold having a concave molding surface will be explained below with reference to FIGS. 2, 3, and 9. FIGS. 2 and 3 show the procedure for molding a film using a mold having a concave molding surface, and FIG. 9 shows the film used for molding. In FIG. 9, the direction of the white arrow indicates the average direction of the in-plane slow axis, and two third reference lines L3 drawn by the above-described procedure are shown. As shown in FIG. 2, a circular film 22 is placed on a mold 20 having a concave molding surface, and as shown in FIG. 3, the film 22 is deformed so as to conform to the molding surface of the mold 20, thereby obtaining a film 24 with a transferred concave shape. When a film is molded using a mold having a concave molding surface as shown in Figures 2 and 3, the stretching direction varies depending on the position of the film 22. More specifically, as shown in Figure 9, the central portion 22C of the film 22 is stretched in various directions as indicated by the arrows during molding, so that the direction of the in-plane slow axis is unlikely to shift before and after molding. In contrast, the four end regions 22E near the periphery of the film and near the two third reference lines L3 are likely to be stretched in only one specific direction, so that the direction of the in-plane slow axis is likely to shift before and after molding. In other words, the likelihood of the direction of the in-plane slow axis shifting during molding varies depending on the position on the film being molded.

[0038] In contrast, if an attempt is made to transfer a concave shape to the change region 12C in the above-described optical film 10C using a mold having a concave molding surface in the same manner as in the above-described film 22, the direction of the in-plane slow axis at the position corresponding to the vicinity of the edge region 22E described in FIG. 9 is originally deviated from the direction of the in-plane slow axis at the center. Therefore, when molding is performed using a mold having the above-described concave molding surface, the direction of the in-plane slow axis will be the same at all positions after molding, and deviation in the direction of the in-plane slow axis is unlikely to occur.

[0039] 8, in the change region 12C, the direction of the in-plane slow axis at each position on the first reference line and the second reference line is preferably parallel to the direction of the in-plane slow axis at the center C of the change region 12C. Note that the above-mentioned "parallel" includes the range of error allowable in the technical field to which the present invention pertains, and in the present invention, the angle formed between the in-plane slow axis at each position on the first reference line and the second reference line and the in-plane slow axis at the center C of the change region 12C may be in the range of 0 to 5°. In particular, the above-mentioned angle is preferably in the range of 0 to 3°.

[0040] In the change region of the optical film of the present invention, when the two lines forming an angle of 22.5° between the first reference line and the third reference line are defined as a fourth reference line, it is preferable that the direction of the in-plane slow axis on the fourth reference line gradually changes from the center of the change region toward the outside. For example, in the change region 12C shown in FIG. 8, it is preferable that the angle (acute angle) between the in-plane slow axis at each position on the fourth reference line (not shown) and the fourth reference line gradually increases from the center C toward the outside. When the angle gradually increases, it may increase continuously or in steps. Furthermore, in the change region of the optical film of the present invention, when the two lines forming an angle of 22.5° between the second reference line L2 and the third reference line L3 are defined as a fifth reference line, it is preferable that the direction of the in-plane slow axis on the fifth reference line gradually changes from the center of the change region toward the outside. For example, in the transition region 12C shown in Fig. 8, it is preferable that the angle (acute angle) formed between the in-plane slow axis at each position on the fifth reference line (not shown) and the fifth reference line gradually increases outward from the center C. When the angle gradually increases, it may increase continuously or in steps.

[0041] In the transition region 12C, two adjacent divided regions surrounded by the first reference line L1 and the third reference line L3 (the combination of divided region R1 and divided region R2, and the combination of divided region R5 and divided region R6) have points P1 and P2 that satisfy the relationship of Requirement 1. Requirement 1: The tilt direction of the in-plane slow axis at point P1, which exists in one of the two adjacent divided regions surrounded by the first reference line and the third reference line, with respect to the first reference line is opposite to the tilt direction of the in-plane slow axis at point P2, which exists in the other of the two divided regions, is located on a line that passes through point P1 and is perpendicular to the first reference line, and is the same distance from the first reference line on the perpendicular line as point P1. It is preferable that the optical film of the present invention satisfy this Requirement 1.

[0042] Requirement 1 will be described in detail below using point P1 located within divided region R1 and point P2 located within divided region R2 shown in FIG. 8 as representative examples. As shown in FIG. 8 , divided region R1, surrounded by a first reference line L1 and one of the third reference lines L3, is a sector-shaped region with a central angle of 45°. Similarly, divided region R2, surrounded by the first reference line L1 and the other of the third reference lines L3, is also a sector-shaped region with a central angle of 45°. The divided regions R1 and R2 are adjacent to each other via the first reference line L1. In the transition region 12C, points P1 and P2 exist in divided regions R1 and R2, respectively, such that the tilt direction of the in-plane slow axis at point P1 located within divided region R1 relative to the first reference line L1 is opposite to the tilt direction of the in-plane slow axis at point P2 located within divided region R2 and having a predetermined positional relationship with point P1 relative to the first reference line L1. The position of point P2 is located on a line (dashed line in FIG. 8 ) that passes through point P1 and is perpendicular to the first reference line L1. Furthermore, the position of point P2 is located at the same distance from the first reference line L1 on the perpendicular line (dashed line in FIG. 8 ) as point P1. In other words, the straight line (dashed line in FIG. 8 ) connecting points P1 and P2 is perpendicular to the first reference line L1, and the length of the straight line from point P1 to the first reference line L1 is equal to the length of the straight line from point P2 to the first reference line L1. Furthermore, the in-plane slow axis at point P1 has one end on the center C side inclined in a direction away from the first reference line L1, and the in-plane slow axis at point P2 also has one end on the center C side inclined in a direction away from the first reference line L1, with the two inclination directions being opposite to each other. 8, the in-plane slow axis at point P1 is located at a position rotated clockwise with respect to the first reference line L1, and the in-plane slow axis at point P2 is located at a position rotated counterclockwise with respect to the first reference line L1. Note that the angle of inclination of the in-plane slow axis at point P1 with respect to the first reference line L1 is the same as the angle of inclination of the in-plane slow axis at point P2 with respect to the first reference line L1. In other words, the angle of clockwise rotation of the in-plane slow axis at point P1 with respect to the first reference line L1 is the same as the angle of counterclockwise rotation of the in-plane slow axis at point P1 with respect to the first reference line L1.

[0043] 8, there is a combination of divided regions R5 and R6 as two adjacent divided regions surrounded by the first reference line L1 and the third reference line L3. Although not shown in FIG. 8, points P1 and P2 that satisfy the relationship of requirement 1 above also exist within divided regions R5 and R6.

[0044] Furthermore, in two adjacent divided regions (combination of divided regions R3 and R4, and combination of divided regions R7 and R7) within the transition region 12C surrounded by the second reference line L2 and the third reference line L3, there are points P3 and P4 that satisfy the relationship of Requirement 2. Requirement 2: The tilt direction of the in-plane slow axis at point P3, which exists in one of the two adjacent divided regions surrounded by the second reference line and the third reference line, with respect to the second reference line is opposite to the tilt direction of the in-plane slow axis at point P4, which exists in the other of the two divided regions, is located on a line that passes through point P3 and is perpendicular to the second reference line, and is the same distance from the second reference line on the perpendicular line as point P3. It is preferable that the optical film of the present invention satisfy this Requirement 2.

[0045] Requirement 2 will be described in detail below using point P3 located within divided region R3 and point P4 located within divided region R4 shown in FIG. 8 as representative examples. As shown in FIG. 8 , divided region R3, surrounded by the second reference line L2 and one of the third reference lines L3, is a sector-shaped region with a central angle of 45°. Similarly, divided region R4, surrounded by the second reference line L2 and the other of the third reference lines L3, is also a sector-shaped region with a central angle of 45°. The divided regions R3 and R4 are adjacent to each other via the second reference line L2. In the transition region 12C, points P3 and P4 exist in divided regions R3 and R4, respectively, such that the tilt direction of the in-plane slow axis at point P3 located within divided region R3 relative to the second reference line L2 is opposite to the tilt direction of the in-plane slow axis at point P4 located within divided region R4 and having a predetermined positional relationship with point P3, relative to the second reference line L2. The position of point P4 is located on a line (dashed line in FIG. 8 ) that passes through point P3 and is perpendicular to the second reference line L2. Furthermore, the distance from point P4 to the second reference line L2 on the perpendicular line (dashed line in FIG. 8 ) is equal to that of point P3. In other words, the line (dashed line in FIG. 8 ) connecting points P3 and P4 is perpendicular to the second reference line L2, and the length of the line from point P3 to the second reference line L2 is equal to the length of the line from point P4 to the second reference line L2. Furthermore, the in-plane slow axis at point P3 has one end on the center C side inclined in a direction away from the second reference line L2, and the in-plane slow axis at point P4 also has one end on the center C side inclined in a direction away from the second reference line L2, with the two inclination directions being opposite to each other. 8, the in-plane slow axis at point P3 is located at a position rotated clockwise with respect to the second reference line L2, and the in-plane slow axis at point P4 is located at a position rotated counterclockwise with respect to the second reference line L2. Note that the angle of inclination of the in-plane slow axis at point P3 with respect to the second reference line L2 is the same as the angle of inclination of the in-plane slow axis at point P4 with respect to the second reference line L2. In other words, the angle of clockwise rotation of the in-plane slow axis at point P3 with respect to the second reference line L2 is the same as the angle of counterclockwise rotation of the in-plane slow axis at point P4 with respect to the second reference line L2.

[0046] 8, there is a combination of divided regions R7 and R8 as two adjacent divided regions surrounded by the second reference line L2 and the third reference line L3. Although not shown in FIG. 8, points P3 and P4 that satisfy the relationship of requirement 2 above also exist within divided regions R7 and R8.

[0047] As described above, in FIG. 8 , the angle A1 between the in-plane slow axis and the first reference line L1 at point P1 is the same as the angle A2 between the in-plane slow axis and the first reference line L1 at point P2. However, the present invention is not limited to this example. The absolute value of the difference between the angles A1 and A2 is preferably within 5°, more preferably within 3°. The lower limit is not particularly limited, and an example of this is 0°. Furthermore, as described above, in FIG. 8 , the angle A3 between the in-plane slow axis and the second reference line L2 at point P3 is the same as the angle A4 between the in-plane slow axis and the second reference line L2 at point P4. However, the present invention is not limited to this example. The absolute value of the difference between the angles A3 and A4 is preferably within 5°, more preferably within 3°. The lower limit is not particularly limited, and an example of this is 0°.

[0048] Although FIG. 8 illustrates only one point P1 and one point P2 satisfying the relationship of Requirement 1, the present invention is not limited to this embodiment, and it is preferable that there are multiple points P1 and P2 that satisfy the relationship of Requirement 1. In particular, it is preferable that two positions located within two adjacent divided regions surrounded by the first and third reference lines, on the two fourth reference lines described above, and facing each other across the first reference line, correspond to points P1 and P2 that satisfy Requirement 1. Furthermore, FIG. 8 illustrates only one point P3 and one point P4 that satisfy the relationship of Requirement 2, but the present invention is not limited to this embodiment, and it is preferable that there are multiple points P3 and P4 that satisfy the relationship of Requirement 2. In particular, it is preferable that two positions located within two adjacent divided regions surrounded by the second and third reference lines, on the two fifth reference lines described above, and facing each other across the second reference line, correspond to points P3 and P4 that satisfy Requirement 2.

[0049] In the transition region 12C, the inclination of the in-plane slow axis with respect to the first reference line L1 at each position in two adjacent divided regions (the combination of divided regions R1 and R2, and the combination of divided regions R5 and R6) surrounded by the first reference line L1 and the third reference line L3 preferably increases with increasing distance from the first reference line L1. For example, in Fig. 8, the inclination of the in-plane slow axis with respect to the first reference line L1 at a position farther from the first reference line L1 than point P1 is preferably greater than the inclination of the in-plane slow axis with respect to the first reference line L1 at point P1. Furthermore, in the transition region 12C, the inclination of the in-plane slow axis with respect to the second reference line L2 at each position in two adjacent divided regions (the combination of divided region R3 and divided region R4, and the combination of divided region R7 and divided region R7) surrounded by the second reference line L2 and the third reference line L3 preferably decreases with increasing distance from the second reference line L2. For example, in Fig. 8, the inclination of the in-plane slow axis with respect to the second reference line L2 at a position farther from the second reference line L2 than point P3 is preferably smaller than the inclination of the in-plane slow axis with respect to the second reference line L2 at point P3.

[0050] <Third embodiment of optical film> The third embodiment of the optical film is a film that combines the features of the first embodiment and the second embodiment described above. That is, the third aspect of the optical film is a film having a change region in which both the in-plane retardation and the direction of the in-plane slow axis change. The aspect in which the in-plane retardation changes in the change region and the aspect in which the direction of the in-plane slow axis changes in the deformation region are as explained in the first embodiment and the second embodiment, respectively, and therefore will not be explained here.

[0051] <Other Properties of Optical Film> The film thickness of the optical film (first to third embodiments) is not particularly limited, but is preferably 0.5 to 5.0 μm, and more preferably 1.0 to 3.0 μm, from the viewpoint of further suppressing the occurrence of leaked light in a virtual reality display device (hereinafter simply referred to as "the viewpoint of the superior effects of the present invention"). Note that the above film thickness is an average value obtained by measuring the film thickness of the optical film at 10 points and arithmetically averaging the measurements.

[0052] The average value of the in-plane retardation at a wavelength of 550 nm in the change region of the optical film is not particularly limited, but is preferably 120 to 200 nm, more preferably 130 to 170 nm, from the viewpoint of applications as various retardation plates such as a λ / 4 plate. The average value of the in-plane retardation is an average value obtained by measuring the in-plane retardation at a wavelength of 550 nm at 50 or more positions in the change region of the optical film and arithmetically averaging the measured values.

[0053] At any position in the change region of the optical film, it is preferable that the relationship of the following formula (X) be satisfied: Re(450)≦Re(550)≦Re(650) Formula (X) Furthermore, at any position in the change region of the optical film, it is preferable that the relationship of the following formula (Y) be satisfied: 0.72≦Re(450) / Re(550)≦0.92 Formula (Y).

[0054] <Materials contained in optical film> The materials contained in the above-mentioned optical films (first to third embodiments) are not particularly limited, and examples thereof include liquid crystal compounds. As will be described later, the optical film is preferably formed using a composition containing a liquid crystal compound having a polymerizable group.

[0055] As the liquid crystal compound, either a polymer liquid crystal compound or a low molecular weight liquid crystal compound can be used, with the polymer liquid crystal compound being preferred because it can increase the degree of orientation. Furthermore, as the liquid crystal compound, a polymer liquid crystal compound and a low molecular weight liquid crystal compound may be used in combination. The liquid crystal compound may be fixed in the optically anisotropic film. Here, "polymer liquid crystal compound" refers to a liquid crystal compound having a repeating unit in its chemical structure. Furthermore, "low molecular weight liquid crystal compound" refers to a liquid crystal compound having no repeating unit in its chemical structure.

[0056] The low molecular weight liquid crystal compound is not particularly limited, and examples thereof include rod-shaped liquid crystal compounds and discotic liquid crystal compounds. Furthermore, a liquid crystal compound with reverse wavelength dispersion may also be used as the low molecular weight liquid crystal compound. The low molecular weight liquid crystal compound preferably has a polymerizable group. The polymerizable group is preferably a polymerizable group capable of radical polymerization or cationic polymerization. Specific examples of the polymerizable group include an acryloyloxy group, a methacryloyloxy group, an alicyclic ether group, a cyclic acetal group, a cyclic lactone group, a cyclic thioether group, a spiro orthoester group, and a vinyloxy group.

[0057] Examples of polymer liquid crystal compounds include the thermotropic liquid crystalline polymers described in JP 2011-237513 A. When the optically anisotropic film contains a polymer liquid crystal compound, the polymer liquid crystal compound preferably forms a nematic liquid crystal phase. The temperature range in which the nematic liquid crystal phase is exhibited is preferably room temperature (23°C) to 450°C, and from the viewpoints of handling and manufacturing suitability, preferably 50 to 400°C.

[0058] As will be described later, the optical film is preferably formed using a liquid crystal compound having a polymerizable group.

[0059] In addition to the above-mentioned components, the optical film may contain an adhesion improver, a plasticizer, a polymer, etc. Here, examples of the adhesion improver include the reactive additives listed in paragraphs

[0123] to

[0129] of JP 2019-91088 A and the boronic acid monomers listed in paragraphs

[0015] to

[0028] of WO 2015 / 053359 A.

[0060] <Method for producing optical film> The method for producing an optical film is not particularly limited, and known methods can be used. As a method for producing the first embodiment of the optical film described above, for example, a method (Method 1) can be used, in which a coating film is formed using a composition containing a liquid crystal compound having a polymerizable group, the liquid crystal compound in the coating film is aligned, and the coating film is irradiated with light so as to have an irradiation amount distribution in the in-plane direction of the coating film, thereby producing an optical film. Hereinafter, the above-mentioned Method 1 will be described in detail.

[0061] In Method 1, a coating film is first formed using a composition containing a liquid crystal compound having a polymerizable group. The composition used in Method 1 contains a liquid crystal compound having a polymerizable group. The liquid crystal compound having a polymerizable group is as described above. The composition may contain components other than the liquid crystal compound (e.g., a solvent and a polymerization initiator) as necessary.

[0062] A method for forming a coating film includes a method of applying the composition onto a substrate. The substrate to be used is not particularly limited, and any known planar substrate can be used. Furthermore, an alignment film may be provided on the substrate as needed. By providing the alignment film, the liquid crystal compound can be aligned. An example of the alignment film is a photo-alignment film.

[0063] Examples of methods for applying the composition include known methods such as roll coating, gravure printing, spin coating, wire bar coating, extrusion coating, direct gravure coating, reverse gravure coating, die coating, spraying, and inkjet printing.

[0064] Next, a treatment is carried out to align the liquid crystal compound in the coating film. The alignment treatment may include a drying treatment. Components such as the solvent can be removed from the coating film by the drying treatment. The drying treatment may be carried out by leaving the coating film at room temperature for a predetermined time (for example, natural drying), or by heating and / or blowing air. Here, the liquid crystal compound contained in the composition may be aligned by the above-mentioned coating treatment or drying treatment. When the drying treatment is carried out at a temperature equal to or higher than the temperature at which the liquid crystal compound contained in the coating film transitions from a liquid crystal phase to an isotropic phase, the heating treatment described below may not be carried out.

[0065] The alignment treatment preferably includes a heat treatment, which allows the liquid crystal compound contained in the coating film to be aligned. From the viewpoint of manufacturability, the heat treatment is preferably performed at a temperature of 10 to 250°C, more preferably 25 to 190°C. The heating time is preferably 1 to 300 seconds, more preferably 1 to 60 seconds.

[0066] The alignment treatment may include a cooling treatment carried out after the heating treatment. The cooling treatment is a treatment for cooling the coating film after heating. This can fix the alignment of the liquid crystal compound contained in the coating film. The cooling method is not particularly limited and can be carried out by a known method. The optimal cooling temperature is selected depending on the liquid crystal compound used.

[0067] Next, the coating film is irradiated with light so as to have a distribution of the irradiation amount in the in-plane direction of the coating film. A more specific method, for example, when producing an optical film having a change region in which the in-plane retardation gradually decreases from the center to the periphery, includes irradiating the coating film with light so that the irradiation amount gradually decreases from the center to the periphery within a predetermined range while maintaining the temperature during the cooling treatment performed in the orientation treatment described above, and then performing a heat treatment. In this procedure, the degree of polymerization of the liquid crystal compound is adjusted by changing the irradiation amount during light irradiation. The degree of polymerization of the liquid crystal compound is high in the center where the irradiation amount is high, and low near the periphery where the irradiation amount is low. When the coating film irradiated with light as described above is subjected to a heat treatment, the orientation of the liquid crystal compound near the center where the polymerization degree is high remains almost unchanged, but the orientation of the liquid crystal compound near the periphery where the polymerization degree is low becomes disordered, resulting in a decrease in in-plane retardation. An example of a method for irradiating the coating film with light so as to have a distribution of the irradiation amount in the in-plane direction of the coating film as described above is a method using a filter whose transmittance varies from the center to the periphery. For example, as shown in Figure 10, one method involves exposing the coating film 30 through a filter 32 having a light-transmitting region 34 and a light-shielding region 36. In the light-transmitting region 34, the transmittance gradually decreases concentrically from the center outward. When exposure is performed from the direction indicated by the white arrow in Figure 10, a distribution of the amount of transmitted light occurs due to the light-transmitting region 34, and as a result, a distribution of the amount of exposure occurs from the center outward within the irradiation region IA of the coating film 30.

[0068] Light irradiation may also be performed during the heat treatment. Light irradiation during the heat treatment may be performed so as to create a distribution of the irradiation dose, or so as to make the irradiation dose uniform across the entire surface. When light irradiation is performed during the heat treatment so as to create a distribution of the irradiation dose, it is preferable to perform light irradiation so that the irradiation dose gradually increases from the center toward the outside. Such a distribution of the irradiation dose during the heat treatment makes it more likely that the alignment of the liquid crystal compound will be disturbed at positions where the irradiation dose is high. In other words, a greater difference in in-plane retardation can be achieved between the center and the periphery of the irradiated region.

[0069] The type of light used in the light irradiation is not particularly limited, and various types of light such as infrared light, visible light, and ultraviolet light can be used, but ultraviolet light is preferred. The temperature of the heat treatment carried out together with the light irradiation is not particularly limited, but is preferably 10 to 250°C, more preferably 25 to 190°C.

[0070] In addition to the above-mentioned method 1, a distribution of in-plane retardation can also be generated by, for example, providing a temperature distribution during light irradiation. More specifically, when a heat treatment is performed in which the heating temperature is gradually increased from the center toward the outside in the region where light is irradiated, polymerization of the liquid crystal compound proceeds while maintaining the orientation of the liquid crystal compound in the region where the heating temperature is low, but polymerization of the liquid crystal compound proceeds while disturbing the orientation of the liquid crystal compound in the region where the heating temperature is high. Therefore, a change region can be formed in which the in-plane retardation is high near the center and gradually decreases toward the outside.

[0071] Although the manufacturing method of the first embodiment of the optical film has been described in detail above, the second embodiment of the optical film can also be manufactured by a known method. For example, an optical film can be manufactured by forming an alignment film capable of aligning a liquid crystal compound in a predetermined direction and then aligning the liquid crystal compound on the alignment film. The alignment film can be a photo-alignment film that has been subjected to a predetermined photo-alignment treatment. One method for preparing such a photo-alignment film is to use a wire grid and a mask having predetermined openings. This method will be described in detail below.

[0072] As shown in FIG. 11 , a mask 42 and a wire grid 44 are placed on an alignment film 40 containing photoalignable groups. The mask 42 is an annular mask having openings 46 and light-shielding portions 48. The wire grid 44 transmits light parallel to the direction indicated by the diagonal lines in FIG. 11 . The mask 42 and wire grid 44 are placed on the alignment film 40, and exposure is performed from the wire grid 44 side. FIG. 12 is a partial enlarged view of the optical system shown in FIG. 11 when exposure is performed. Of the polarized light that passes through the wire grid 44, polarized light traveling in the normal direction of the wire grid 44, as indicated by the white arrows, is directly irradiated onto the alignment film 40, imparting an alignment restriction force to the alignment film 40 that can align the liquid crystal compound in a specific direction, as indicated by the black arrows. On the other hand, of the polarized light that passes through the wire grid 44, some polarized light is emitted obliquely relative to the wire grid 44, as indicated by the black arrows, and slips under the light-shielding portions 48 of the mask 42. The polarization direction of such polarized light is shifted by a predetermined angle from the polarization direction of polarized light emitted in the direction indicated by the white arrow. Therefore, due to the influence of polarized light that has slipped under such light-shielding portion 48, the direction of the alignment control force indicated by the black arrow at the position where such polarized light is irradiated differs from the direction of the alignment control force at the position where polarized light traveling in the direction indicated by the white arrow is irradiated. In particular, as shown in Figures 11 and 12, because mask 42 is annular, the deviation in the direction of the alignment control force increases as it moves outward from the center, resulting in an alignment film that can form the change region of the optical film of the second embodiment described above.

[0073] The above describes an embodiment in which a specific mask is used, but it is also possible to produce a photo-alignment film having an alignment control force in a specific direction at each position by irradiating light onto an alignment film containing photo-alignable groups by direct imaging.

[0074] The second embodiment of the optical film described above can be produced by applying a composition containing a liquid crystal compound having a polymerizable group onto the photo-alignment film obtained by the above-mentioned method to align the liquid crystal compound in the coating film, and then subjecting the coating film to a light irradiation treatment. The method and conditions for aligning the liquid crystal compound and the light irradiation treatment can be appropriately selected from those described in Method 1 above.

[0075] <Laminate> The optical film described above may be laminated as another member. For example, it may be a laminate including the optical film and an absorptive polarizer. In the laminate, the angle formed between the average direction of the in-plane slow axes of the change regions of the optical film and the absorption axis of the absorptive polarizer is preferably within a range of 40 to 50°. The average direction of the in-plane slow axes of the change regions is as described above.

[0076] Examples of absorption-type polarizers include iodine-based polarizers, dye-based polarizers using dichroic dyes, and polyene-based polarizers. Iodine-based polarizers and dye-based polarizers include coated polarizers and stretched polarizers, both of which are applicable. As the coated polarizers, polarizers in which a dichroic organic dye is oriented by utilizing the orientation of a liquid crystal compound are preferred, and as the stretched polarizers, polarizers produced by adsorbing iodine or a dichroic dye into polyvinyl alcohol and stretching it are preferred. The thickness of the absorption-type polarizer is not particularly limited, but is preferably 3 to 60 μm, more preferably 5 to 20 μm.

[0077] <Method for molding optical film> An optically anisotropic film having a convex curved surface portion can be produced using the optical film having the above-mentioned changed region. The method for molding the optical film is not particularly limited, and a known method can be used. For example, the changed region can be molded into a convex curved surface portion using a mold having a concave molding surface as shown in Figures 2 and 3, or the changed region can be molded into a convex curved surface portion using a mold having a convex molding surface as shown in Figures 6 and 7.

[0078] When molding the first embodiment of the optical film described above, a method of adjusting the heating conditions of the optical film during molding can be used. For example, when molding a film using a mold having a concave molding surface as shown in Figures 2 and 3, the stretching direction varies depending on the position of the film, as described above. In particular, as described above, as shown in Figure 9, the central portion 22C of the film 22 is stretched in various directions as indicated by the arrows during molding, so the direction of the in-plane slow axis is less likely to shift before and after molding. In contrast, the edge region 22E is stretched only in a specific direction, so the direction of the in-plane slow axis is more likely to shift before and after molding depending on the position. In other words, the likelihood of the direction of the in-plane slow axis shifting during molding varies depending on the position on the film being molded. To address the above problem, a method of adjusting the heating conditions of the molded film can be used.

[0079] Specifically, this is a method of heating and molding an optical film so that the heating temperature is distributed in the in-plane direction. More specifically, in the case of the concave molding described above, a manufacturing method includes a step of heating the change region of the optical film so that the heating temperature of the peripheral portion surrounding the change region of the optical film is lower than the heating temperature of the center of the change region of the optical film, and then deforming the heated change region of the optical film along the molding surface using a molding die having a concave molding surface. In this procedure, by lowering the heating temperature of the peripheral portion than the heating temperature of the center of the change region of the optical film placed on the molding die having a concave molding surface, when the change region of the optical film is deformed along the molding surface, the central portion is made more easily stretched and the peripheral portion is made less easily stretched. That is, as described above, when molding using a molding die having a concave molding surface, the in-plane slow axis direction usually shifts more in the peripheral portion than in the central portion. However, by changing the heating conditions for the central portion and the peripheral portion, the central portion, where the in-plane slow axis direction is less likely to shift due to stretching, is more likely to stretch, and the peripheral portion, where the in-plane slow axis direction is more likely to shift due to stretching, is more likely to stretch. As a result, the in-plane slow axis direction shift is suppressed in the change region of the deformed optical film. As described above, by adopting a predetermined method when molding the first embodiment of the optical film, it is possible to suppress both the occurrence of variations in in-plane retardation and the occurrence of variations in the in-plane slow axis direction.

[0080] The optimum heating conditions for the optical film are appropriately selected depending on the type of material of the optical film used, the shape of the convex curved surface portion, and the molding method. In particular, the heating temperature is preferably equal to or higher than the glass transition temperature of the optical film. The upper limit of the heating temperature is not particularly limited, but is preferably within (the glass transition temperature of the optical film + 100°C).

[0081] The heating method is not particularly limited, and examples thereof include heating by contact with a heated solid, heating by contact with a heated liquid, heating by contact with a heated gas, heating by infrared radiation, heating by microwave radiation, etc. Among these, heating by infrared radiation is preferred.

[0082] The wavelength of the infrared rays used for heating is preferably 1.0 to 30.0 μm, more preferably 1.5 to 5 μm. Examples of IR (infrared) light sources include near-infrared lamp heaters with a tungsten filament sealed in a quartz tube, and wavelength-controlled heaters with multiple quartz tubes and a mechanism for cooling a portion of the space between the quartz tubes with air. Methods for creating an intensity distribution of infrared radiation include varying the density of IR light sources and placing a filter with a patterned infrared transmittance between the IR light source and the planar optical film. Examples of filters with a patterned transmittance include glass with metal vapor deposition, filters with an infrared reflection band of a cholesteric liquid crystal layer, filters with an infrared reflection band using a dielectric multilayer film, and ink that absorbs infrared. The temperature of the optical film is controlled by the intensity of infrared radiation, and by the infrared radiation duration and illuminance. The temperature of the planar optical film can be monitored using a non-contact radiation thermometer, a thermocouple, or the like, and molded at the desired temperature.

[0083] Although the above describes a method of heating the optical film so as to have a heating temperature distribution in the in-plane direction, the method is not limited to the above as long as a temperature distribution is generated in the in-plane direction of the optical film during molding, and for example, a process may be performed in which the optical film is uniformly heated in the in-plane direction, and then cooled before molding so that the temperature of the peripheral portion is lower than that of the center portion, thereby generating a temperature distribution in the in-plane direction of the optical film, and then molding. The cooling process is not particularly limited, and examples include a method of lowering the temperature of the peripheral portion by adjusting the speed of pressure application when pressing the film against a molding die, and a method of contacting only the peripheral portion with a refrigerant.

[0084] When molding the first embodiment of the optical film described above, by increasing the radius of curvature, it is possible to suppress the occurrence of deviation in the direction of the in-plane slow axis in the resulting molded product.

[0085] Although the method for forming an optical film has been described above, the above-described laminate may be formed in the same manner to form an optically anisotropic film having a convex curved surface portion.

[0086] <Optically Anisotropic Film> The optically anisotropic film of the present invention is an optically anisotropic film having a convex curved surface portion, and satisfies the relationship of formula (1) and formula (2). Formula (1) (ΔRe) 1/2 + (Δaxis) 1/2 ≦10×(L / R−0.1) Equation (2) L / R≧0.30 R represents the numerical value R when R (mm) is the minimum radius of curvature of the convexly curved surface portion. L represents the numerical value L when L (mm) is half the value of the circle-equivalent diameter of the convexly curved surface portion when observed from the normal direction of the tangent plane at the apex of the convexly curved surface portion. ΔRe represents the numerical value ΔRe when ΔRe (nm) is the largest in-plane retardation difference between the differences in in-plane retardation at a wavelength of 550 nm at two positions on the convexly curved surface portion. Δaxis represents the numerical value Δaxis when Δaxis (°) is the largest angle between the in-plane slow axes at two positions on the convexly curved surface portion when observed from the normal direction of the tangent plane at the apex of the convexly curved surface portion. The above formulas (1) and (2) will be explained below with reference to FIGS. 13 and 14, which show examples of optically anisotropic films.

[0087] FIG. 13 shows an example of an optically anisotropic film of the present invention. FIG. 13 is a top view of the optically anisotropic film, and FIG. 14 is a cross-sectional view taken along line A-A in FIG. 1. Note that line A-A is a line passing through the center C of the optically anisotropic film 50, which is circular when viewed in plan. As shown in FIGS. 13 and 14, the optically anisotropic film 50 has a convex curved shape. More specifically, as shown in FIG. 14, the optically anisotropic film 50 has a shape (convex shape) that is convexly curved toward the upper side of the paper. In other words, the optically anisotropic film 50 has a convex shape that protrudes toward one surface. Note that the optically anisotropic film 50 can also be said to have a concave shape in which the other surface is recessed. In the optically anisotropic film 50 shown in FIGS. 13 and 14, the entire film corresponds to a convex curved portion. 14, the optically anisotropic film 50 has two opposing surfaces, a first surface 50A and a second surface 50B, where the first surface 50A is a curved surface that is convex upward in the plane of the drawing, and the second surface 50B is a curved surface that is convex upward in the plane of the drawing. Note that the curved surface of the optically anisotropic film 10 shown in FIGS. 13 and 14 is a paraboloid of revolution, but it may also be a spherical or spheroidal shape.

[0088] 14 , when the optically anisotropic film 50 is observed from the normal direction of the tangent plane to the center C (corresponding to the apex of the convex portion) of the optically anisotropic film 50 (when the optically anisotropic film 50 is viewed in plan), the shape of the optically anisotropic film 50 is a perfect circle. Note that the center C of the optically anisotropic film 50 is the intersection point between the axis of the paraboloid of revolution and the optically anisotropic film 50, and corresponds to the position where it intersects with the normal to the center of the exit surface of the image display panel when the optically anisotropic film 50 is incorporated into a virtual reality display device described below. Furthermore, when the optically anisotropic film 50 is incorporated into a virtual reality display device described below, the optically anisotropic film 50 is positioned so that it is convex toward the image display panel.

[0089] In formula (1), R represents the numerical value R when the minimum radius of curvature of the convexly curved surface portion is R (mm). For example, if R (mm) is 40 mm, R is 40. The minimum radius of curvature (R (mm)) of the convexly curved surface portion is not particularly limited, and an optimal value is selected depending on the intended use of the optically anisotropic film. However, it is often 25 to 200 mm, and more often 35 to 100 mm. The radius of curvature of the convexly curved surface portion of the optically anisotropic film may be constant or may vary at any position on the convexly curved surface portion. If the radius of curvature varies depending on the position on the convexly curved surface portion, the smallest value among them is selected and used as the minimum radius of curvature. The method for measuring the radius of curvature is not particularly limited, and examples include methods using devices such as a spherometer and a laser interferometer.

[0090] In formula (1), L represents the numerical value L (mm) when half the circle-equivalent diameter of the convex curved surface portion when observed from the normal direction of the tangent plane at the apex of the convex curved surface portion. For example, when L (mm) is 25 mm, L is 25. The half circle-equivalent diameter (L (mm)) of the convex curved surface portion is not particularly limited, and an optimal value is selected depending on the intended use of the optically anisotropic film. However, it is often 5 to 50 mm, and more often 15 to 35 mm. Figure 13 corresponds to a view of the convex curved surface portion of the optically anisotropic film 50 observed from the normal direction of the tangent plane at the apex of the convex curved surface portion. As described above, since the optically anisotropic film 50 itself is perfectly circular, in the embodiment shown in Figure 13, the distance from the center C to the outer edge corresponds to the above-mentioned L.

[0091] In formula (1), ΔRe represents the numerical value ΔRe (nm) when the largest difference in in-plane retardation between the differences in in-plane retardation at a wavelength of 550 nm at two positions on the convexly curved surface portion is taken as ΔRe (nm). For example, when ΔRe (nm) is 1.0 nm, ΔRe is 1.0. The largest difference in in-plane retardation (ΔRe (nm)) is not particularly limited, and an optimal value is selected depending on the intended use of the optically anisotropic film. However, it is often 0 to 12 nm, and from the viewpoint of achieving superior effects of the present invention, a difference of 0 to 5 nm is preferred. The in-plane retardation at a wavelength of 550 nm at each position on the convexly curved surface portion can be measured using a known device, such as a two-dimensional birefringence evaluation system (WPA-200) from Photonic Lattice Co., Ltd. The measurement is performed from the normal direction of the tangent plane at the vertex of the convexly curved surface portion. It should be noted that a range of 2.5 cm from the periphery of the projection of the convex curved surface portion when observed from the normal direction of the tangent plane at the apex of the convex curved surface portion has a large measurement error, and is therefore excluded from the measurement range of ΔRe.

[0092] In formula (1), Δaxis represents the numerical value Δaxis (°) when the largest angle between the in-plane slow axes at two positions on the convexly curved surface portion when observed from the normal direction of the tangent plane at the vertex of the convexly curved surface portion is taken as Δaxis (°). For example, when Δaxis (°) is 0.1°, Δaxis is 0.1. The largest angle (Δaxis (°)) is not particularly limited, and an optimum value is selected appropriately depending on the intended use of the optically anisotropic film. However, it is often 0 to 3.0°, and more often 0 to 2.0°. Of these, a value of 0 to 1.5° is preferred in terms of achieving superior effects of the present invention. The in-plane slow axes at each position on the convexly curved surface portion can be measured using a known device, such as a two-dimensional birefringence evaluation system (WPA-200) from Photonic Lattice, Inc. The measurement is performed from the normal direction of the tangent plane at the apex of the convex curved surface portion. Note that a range of 2.5 cm from the periphery of the projection of the convex curved surface portion when observed from the normal direction of the tangent plane at the apex of the convex curved surface portion has a large measurement error, so this range is excluded from the measurement range of Δaxis.

[0093] The following formula (1) is a formula including the variables ΔRe, Δaxis, L, and R, and formula (2) is a formula including the variables L and R. Through various studies, the inventors have found that when the relationships of formula (1) and formula (2) below are satisfied, the occurrence of light leakage, which is an issue of the present invention, can be suppressed. Formula (1) (ΔRe) 1/2 + (Δaxis) 1/2 ≦10×(L / R−0.1) Equation (2) L / R≧0.30 (ΔRe) 1/2 + (Δaxis) 1/2 The difference between L / R and 10×(L / R−0.1) is not particularly limited, but is preferably 0 to 9, and more preferably 4 to 9. The upper limit of L / R is not particularly limited, but is often 0.80 or less, and more often 0.70 or less.

[0094] In a cut surface of the optically anisotropic film 50 taken along a plane including the normal to the tangent plane to the center C of the optically anisotropic film 50, the outer contour of the optically anisotropic film 50 (the contour corresponding to the first surface 50A of the optically anisotropic film 50) is a parabola. When the optically anisotropic film 50 is cut along any plane parallel to the tangent plane to the center C of the optically anisotropic film 50, the outer contour of the optically anisotropic film 50 (the contour corresponding to the first surface 50A of the optically anisotropic film 50) is a circle. When the normal to the tangent plane to the center C of the optically anisotropic film 50 is directed from the first surface 50A to the second surface 50B (the direction of the white arrow in FIG. 14 ), the diameter of the circle formed by the outer contour of the optically anisotropic film 50 when the optically anisotropic film 50 is cut along a plane parallel to the tangent plane to the center C of the optically anisotropic film 50 gradually increases.

[0095] 13 and 14, the entire optically anisotropic film 50 corresponds to the convexly curved portion, but the present invention is not limited to this embodiment, and only a part of the optically anisotropic film may be the convexly curved portion. For example, the optically anisotropic film 52 shown in Fig. 15 has a convexly curved portion 54 and a flat portion 56, and the convexly curved portion satisfies the above-mentioned requirements 1 and 2.

[0096] The shape of the convex curved surface portion of the optically anisotropic film is preferably a spherical shape, a spheroid shape, or a paraboloid of revolution. That is, the convex curved surface portion is preferably a spherical shape portion, a spheroid shape portion, or a radial surface of revolution. As described above, the shape of the convex curved surface portion of the optically anisotropic film is preferably a solid of revolution.

[0097] In Figures 13 and 14, we have described an embodiment in which the convex curved portion of the optically anisotropic film has a perfect circular shape when viewed in a plane, but the present invention is not limited to this embodiment, and the shape of the convex curved portion of the optically anisotropic film when viewed in a plane may be elliptical or another shape.

[0098] The thickness of the optically anisotropic film is not particularly limited, but is preferably 0.5 to 50 μm, more preferably 1 to 10 μm, from the viewpoint of achieving better effects of the present invention. The thickness of the optically anisotropic layer is an average value, and is determined by measuring the thickness of the optically anisotropic film at 10 or more positions and arithmetically averaging the results.

[0099] Examples of materials contained in the optically anisotropic film include the liquid crystal compounds described above. The liquid crystal compound may be fixed in the optically anisotropic film. In particular, the optically anisotropic film is preferably a film formed using a composition containing a liquid crystal compound, and more preferably a film formed using a composition containing a liquid crystal compound having a polymerizable group.

[0100] The method for producing an optically anisotropic film is not particularly limited, and known methods can be used. For example, as described above, a method can be used in which the change region of an optical film having a change region is molded using the predetermined method described above. When only the change region of the optical film is molded, other portions that are not molded can be cut out and removed as necessary. More specifically, for example, only the change region of an optical film having a change region can be molded to produce an optically anisotropic film 52 as shown in FIG. 15, and then the flat portion 56 can be removed to produce an optically anisotropic film 50 as shown in FIG. 13.

[0101] <Laminate> The optically anisotropic film of the present invention may be combined with other components to form a laminate. The other components are not particularly limited, and examples thereof include a linear polarizer, a cholesteric liquid crystal layer, a linear polarization type reflective polarizer, a surface antireflection layer, a pressure-sensitive adhesive layer, a support, and an alignment film. FIG. 16 shows an example of a laminate. The laminate 60A shown in FIG. 16 includes an absorptive polarizer 62, an optically anisotropic film 64, a positive C plate 66, and a cholesteric liquid crystal layer 68, in this order. FIG. 17 shows another example of a laminate of the present invention. The laminate 60B shown in FIG. 17 includes an absorptive polarizer 62, a linear polarization type reflective polarizer 70, an optically anisotropic film 64, and a positive C plate 66, in this order. The optically anisotropic film 64 is the optically anisotropic film having a convex curved surface portion of the present invention described above. As shown in Figures 16 and 17, all of the components included in the laminate 60A and the laminate 60B have a curved surface similar to that of the optically anisotropic film 64 of the present invention. The laminate 60A and the laminate 60B each include two retardation layers: an optically anisotropic film 64 and a positive C plate 66. A retardation layer having the function of converting linearly polarized light into circularly polarized light may be disposed on the side of the absorptive polarizer 62 of the laminate 60A opposite the optically anisotropic film 64. Furthermore, a retardation layer having the function of converting linearly polarized light into circularly polarized light may be disposed on the side of the absorptive polarizer 62 of the laminate 60B opposite the linearly polarized reflective polarizer 70. The laminates 60A and 60B are suitable for use in the virtual reality display devices described below.

[0102] The optically anisotropic film 64 is the optically anisotropic film of the present invention described above. The optically anisotropic film 64 functions as a λ / 4 plate. The λ / 4 plate is a plate having a λ / 4 function, specifically, a plate having the function of converting linearly polarized light of a certain wavelength (preferably visible light) into circularly polarized light (or circularly polarized light into linearly polarized light). The angle between the average direction of the in-plane slow axis of the optically anisotropic film 64 and the transmission axis of the absorptive polarizer 62 is preferably within the range of 45°±10°. The average direction of the in-plane slow axis of the optically anisotropic film 64 is the direction obtained by averaging the directions of the in-plane slow axes at 1,000 or more locations on the optically anisotropic film 64. Hereinafter, other components other than the optically anisotropic film included in the laminate will be described in detail.

[0103] (Absorptive Polarizer) The absorptive polarizer may have the same structure as that described above for the absorptive polarizer that can be laminated with the optical film.

[0104] (Retardation layer having the function of converting linearly polarized light into circularly polarized light) A retardation layer having the function of converting linearly polarized light into circularly polarized light (hereinafter also simply referred to as "specific retardation layer") is a type of retardation layer. The specific retardation layer is not particularly limited as long as it has the function of converting linearly polarized light into circularly polarized light, and for example, a λ / 4 plate can be mentioned. The λ / 4 plate is as described above.

[0105] Specific retardation layer can have reverse wavelength dispersion.Having reverse wavelength dispersion means that with wavelength increasing, the retardation value at this wavelength increases.In addition, specific retardation layer can be multi-layer structure, and as the embodiment of this case, specifically, can be made up of lambda / 4 plate and lambda / 2 plate stacked together to make a broadband lambda / 4 plate.

[0106] The angle formed by the in-plane slow axis of the specific retardation layer and the absorption axis of the absorptive polarizer is not particularly limited, but is preferably within the range of 45°±10°.

[0107] The specific retardation layer may be the layer that is made by fixing the liquid crystal compound that is twisted and aligned with the thickness direction as the helical axis.For example, as disclosed in Japanese Patent No. 05753922 and Japanese Patent No. 05960743, the retardation layer that has the layer that is made by fixing the rod-shaped liquid crystal compound or discotic liquid crystal compound that is twisted and aligned with the thickness direction as the helical axis can be enumerated.

[0108] The thickness of the specific retardation layer is not particularly limited, but is preferably 0.1 to 8 μm, more preferably 0.3 to 5 μm.

[0109] (Positive C Plate) The positive C plate functions as an optical compensation layer for increasing the degree of polarization of transmitted light with respect to obliquely incident light. The in-plane retardation of the positive C plate at a wavelength of 550 nm is preferably 10 nm or less. The retardation in the thickness direction of the positive C plate at a wavelength of 550 nm is preferably −600 to −40 nm.

[0110] The material for forming the positive C plate is not particularly limited, but it is preferably formed from a composition containing a liquid crystal compound. Such a positive C plate can typically be obtained by vertically aligning a rod-shaped polymerizable liquid crystal compound contained in a polymerizable liquid crystal composition and fixing the alignment state by polymerization. Alternatively, the positive C plate can be formed from a composition containing a side-chain polymer liquid crystal compound as the liquid crystal compound.

[0111] The thickness of the positive C plate is not particularly limited, but from the viewpoint of thinning, it is preferably 0.5 to 10 μm, and more preferably 0.5 to 5 μm.

[0112] (Cholesteric Liquid Crystal Layer) A cholesteric liquid crystal layer is an optical component that separates incident light into right-handed circularly polarized light and left-handed circularly polarized light, specularly reflecting one circularly polarized light and transmitting the other circularly polarized light. Examples of cholesteric liquid crystal layers include cholesteric liquid crystal layers formed by fixing a cholesteric liquid crystal phase. Cholesteric liquid crystal layers are preferred as optical films used for curved surface molding because they suppress a decrease in the degree of polarization and distortion of the polarization axis when stretched or molded into a three-dimensional shape. Furthermore, they are less likely to experience a decrease in the degree of polarization due to distortion of the polarization axis.

[0113] The cholesteric liquid crystal layer preferably includes a blue light-reflecting layer having a reflectance of 40% or more at a wavelength of 460 nm, a green light-reflecting layer having a reflectance of 40% or more at a wavelength of 550 nm, a yellow light-reflecting layer having a reflectance of 40% or more at a wavelength of 600 nm, and a red light-reflecting layer having a reflectance of 40% or more at a wavelength of 650 nm. This configuration is preferable because it can exhibit high reflection characteristics over a wide wavelength range in the visible range. The reflectances mentioned above are those when unpolarized light is incident on the cholesteric liquid crystal layer at each wavelength. The cholesteric liquid crystal layer may also have a pitch gradient structure in which the helical pitch of the cholesteric liquid crystal phase is continuously varied in the thickness direction.

[0114] It is also preferable to use, as the cholesteric liquid crystal layer, a cholesteric liquid crystal layer formed by fixing a cholesteric liquid crystal phase containing a rod-shaped liquid crystal compound and a cholesteric liquid crystal layer formed by fixing a cholesteric liquid crystal phase containing a discotic liquid crystal compound in combination. In this configuration, the cholesteric liquid crystal phase containing the rod-shaped liquid crystal compound has a positive Rth, while the cholesteric liquid crystal phase containing the discotic liquid crystal compound has a negative Rth, so that the Rths cancel each other out, thereby preventing color unevenness from occurring even with respect to light incident from an oblique direction, which is preferable.

[0115] The thickness of the cholesteric liquid crystal layer is not particularly limited, but is preferably 30 μm or less, more preferably 15 μm or less, from the viewpoint of thinning. There is no particular lower limit, and it is often 1 μm or more.

[0116] (Linearly Polarized Reflective Polarizer) A linearly polarized reflective polarizer is a polarizer that reflects one of mutually orthogonal linearly polarized light beams and transmits the other linearly polarized light beam. Examples of linearly polarized reflective polarizers include a film obtained by stretching a dielectric multilayer film and a wire grid polarizer. Commercially available products include a reflective polarizer (product name APF) manufactured by 3M Corporation and a wire grid polarizer (product name WGF) manufactured by Asahi Kasei Corporation. The angle between the transmission axis of the linearly polarized reflective polarizer and the transmission axis of the absorptive polarizer is preferably within the range of 0 to 10°.

[0117] (Surface Antireflection Layer) The laminate of the present invention may have a surface antireflection layer. In the laminate of the present invention, the surface antireflection layer is preferably disposed on the surface-most side. The surface antireflection layer may be disposed on only one surface side of the laminate, or on both surfaces. The type of surface antireflection layer is not particularly limited, but from the viewpoint of further reducing the reflectance, a moth-eye film and an AR (Anti-Reflection) film are preferred. Furthermore, a moth-eye film is preferred because it can maintain high antireflection performance even if the film thickness varies due to stretching and molding.

[0118] (Adhesive Layer) The laminate of the present invention may or may not have an adhesive layer. When the laminate has an adhesive layer, the number of adhesive layers is preferably one or two. Examples of adhesives constituting the adhesive layer include pressure-sensitive adhesives and adhesives. Examples of adhesives include rubber-based adhesives, acrylic-based adhesives, silicone-based adhesives, urethane-based adhesives, vinyl alkyl ether-based adhesives, polyvinyl alcohol-based adhesives, polyvinylpyrrolidone-based adhesives, polyacrylamide-based adhesives, and cellulose-based adhesives, with acrylic-based adhesives (pressure-sensitive adhesives) being preferred. Examples of adhesives include aqueous adhesives, solvent-based adhesives, emulsion-based adhesives, solventless adhesives, active energy ray-curable adhesives, and heat-curable adhesives. Examples of active energy ray-curable adhesives include electron beam-curable adhesives, ultraviolet-curable adhesives, and visible light-curable adhesives, with ultraviolet-curable adhesives being preferred.

[0119] The thickness of the pressure-sensitive adhesive layer is not particularly limited, but from the viewpoint of thinning, it is preferably 25 μm or less, more preferably 15 μm or less, and even more preferably 5 μm or less. The lower limit is not particularly limited, and it is often 0.1 μm or more.

[0120] (Support) The laminate of the present invention may have a support. The support can be placed in any location. For example, when the cholesteric liquid crystal layer and the retardation layer are films to be transferred from a temporary support, the support can be used as the transfer destination. The type of support is not particularly limited, but a transparent support is preferred. Examples include films such as cellulose acylate, polycarbonate, polysulfone, polyethersulfone, polyacrylate, polymethacrylate, cyclic polyolefin, polyolefin, polyamide, polystyrene, and polyester. Among these, the support is preferably a cellulose acylate film, a cyclic polyolefin film, a polyacrylate film, or a polymethacrylate film. Commercially available cellulose acetate films (e.g., "TD80U" or "Z-TAC" manufactured by Fujifilm Corporation) can also be used. Furthermore, it is preferable that the support have a small retardation. Specifically, the in-plane retardation at a wavelength of 550 nm is preferably 10 nm or less, and the absolute value of the retardation in the thickness direction at a wavelength of 550 nm is preferably 50 nm or less.

[0121] The thickness of the support is not particularly limited, but is preferably from 5 to 300 μm, more preferably from 5 to 100 μm, and even more preferably from 5 to 30 μm.

[0122] (Method for manufacturing laminate) The method for manufacturing the laminate of the present invention is not particularly limited, and may be a known method.For example, a laminate may be manufactured by laminating another member onto the surface of the optically anisotropic film having a convexly curved surface portion via a pressure-sensitive adhesive layer, or a moldable laminate may be manufactured by laminating another member onto the surface of the above-mentioned optical film via a pressure-sensitive adhesive layer, and then the moldable laminate may be molded into a predetermined shape by carrying out the above-mentioned optical film molding method using the moldable laminate, thereby manufacturing a laminate including an optically anisotropic film having a convexly curved surface portion.

[0123] <Composite Lens> The composite lens of the present invention comprises the above-described laminate, a lens, and a half mirror, in this order. FIG. 18 shows an example of the composite lens of the present invention. A composite lens 72 comprises a laminate 74, a lens 76, and a half mirror 78, in this order. As shown in FIG. 18, all of the components included in the composite lens 72 have the same curved surface shape as the optically anisotropic film. The configuration of the laminate 74 is as described above, and includes an optically anisotropic film having a convex curved surface portion. The components other than the laminate included in the composite lens will be described in detail below.

[0124] (Lens) A compound lens has a lens. Examples of lenses include convex lenses and concave lenses. Examples of convex lenses include biconvex lenses, plano-convex lenses, and convex meniscus lenses. Examples of concave lenses include biconcave lenses, plano-concave lenses, and concave meniscus lenses. As lenses used in virtual reality display devices, convex meniscus lenses or concave meniscus lenses are preferred in terms of expanding the viewing angle, and concave meniscus lenses are more preferred in terms of minimizing chromatic aberration. Lens materials that are transparent to visible light, such as glass, crystal, and plastic, can be used. Since birefringence in lenses can cause rainbow unevenness and light leakage, the smaller the birefringence, the more preferable, and materials with zero birefringence are more preferred.

[0125] (Half Mirror) The composite lens of the present invention has a half mirror. The half mirror is a conventionally known half mirror that transmits approximately half of incident light and reflects the remaining approximately half. The transmittance of the half mirror is preferably 50±30%, more preferably 50±10%. The type of half mirror is not particularly limited, but examples include a reflective layer made of a metal. Examples of metals include silver and aluminum. The thickness of the reflective layer is preferably 1 to 20 nm, more preferably 2 to 10 nm, and even more preferably 3 to 6 nm.

[0126] <Virtual reality display device> The virtual reality display device of the present invention has the optically anisotropic film, laminate, or composite lens described above. FIG. 19 is a schematic diagram showing an example of the configuration of a virtual reality display device. The virtual reality display device 80 shown in FIG. 19 has, from the right side of the figure, an image display panel 82, a circular polarizer 84, a half mirror 86, a lens 88, and a laminate 90 of the present invention. Note that the laminate 90 used in FIG. 19 has a configuration similar to the laminate 60A described above, with the optically anisotropic film 64 positioned closer to the image display panel 82 than the absorptive polarizer 62. The laminate 90, lens 88, and half mirror 86 shown in FIG. 19 constitute the composite lens described above. In the virtual reality display device 80 shown in FIG. 19, a light ray 92 emitted from the image display panel 82 passes through the circular polarizer 84 to become circularly polarized light, and then passes through the half mirror 86. The light ray 92 then passes through the lens 88, enters the laminate 90 from the cholesteric liquid crystal layer side, is reflected, passes through the lens 88 again, is reflected again by the half mirror 86, passes through the lens 88 again, and enters the laminate 90. At this time, the circular polarization state of the light ray 92 does not change when reflected by the laminate 90, but when reflected by the half mirror 86, it changes to circular polarization in the opposite direction to the circular polarization when it entered the laminate 90. Therefore, the light ray 92 passes through the laminate 90 and is visible to the user. Furthermore, when the light ray 92 is reflected by the half mirror 86, the image is magnified because the half mirror 86 has a concave mirror shape, allowing the user to view the magnified virtual image. The above-mentioned mechanism is called a round-trip optical system or a folded optical system. The optically anisotropic film of the present invention included in the laminate 90 functions as a so-called linear polarizer, blocking light that unnecessarily passes through the cholesteric liquid crystal layer and preventing it from leaking and being observed by the user of the virtual reality display device. In the optically anisotropic film of the present invention, the in-plane retardation and / or the in-plane slow axis direction of the convex curved surface portion varies little, so that the occurrence of leaked light can be further suppressed.

[0127] The image display panel 82 is a known image display panel (display panel) such as an organic electroluminescence display panel. In the illustrated example, the image display panel 82 emits an unpolarized image (image light). The unpolarized image emitted by the image display panel 82 passes through the circular polarizer 84 and is converted into circularly polarized light.

[0128] The features of the present invention will be explained in more detail below with reference to examples and comparative examples. The materials, amounts used, ratios, treatment details, and treatment procedures shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be construed as being limited by the specific examples shown below.

[0129] Example 1 (Preparation of Optically Anisotropic Film A1) [Preparation of Substrate] The following composition was placed in a mixing tank, stirred, and heated at 90°C for 10 minutes. The resulting composition was then filtered through a filter paper with an average pore size of 34 μm and a sintered metal filter with an average pore size of 10 μm to prepare a dope. The solid content of the dope was 23.5% by mass, the amount of plasticizer added was the ratio relative to the cellulose acylate, and the solvent for the dope was methylene chloride / methanol / butanol = 81 / 18 / 1 (mass ratio).

[0130] ------------------------------------------------ Cellulose acylate dope -------------------------------------------------- Cellulose acylate (degree of acetyl substitution: 2.86, viscosity average degree of polymerization: 310) 100 parts by mass Sugar ester compound 1 (formula (S4) below) 3.0 parts by mass Sugar ester compound 2 (formula (S5) below) 1.0 part by mass Silica particle dispersion (AEROSIL R972, manufactured by Nippon Aerosil Co., Ltd.) 0.1 part by mass Solvent (methylene chloride / methanol / butanol) 351.9 parts by mass --------------------------------------------------

[0131]

[0132]

[0133] The dope prepared above was cast using a drum film-forming machine. The dope was cast from a die onto a metal support cooled to 0°C, and the resulting web (film) was then peeled off from the drum. The drum was made of SUS (stainless steel).

[0134] The web (film) obtained by casting was peeled from the drum and then dried for 20 minutes in a tenter apparatus, in which both ends of the web were clipped with clips while the film was being transported at 30 to 40°C. Subsequently, the web was post-dried by zone heating while being transported with rolls. The obtained web was knurled and then wound up to obtain cellulose acylate film 1. The obtained cellulose acylate film 1 had a thickness of 40 μm, an in-plane retardation Re(550) of 1 nm at a wavelength of 550 nm, and a thickness direction retardation Rth(550) of 23 nm at a wavelength of 550 nm.

[0135] [Preparation of Photo-Alignment Film 1] A coating solution E1 for forming a photo-alignment film having the following composition was continuously applied onto the above-mentioned cellulose acylate film 1 using a wire bar. The support on which the coating film was formed was dried with hot air at 134°C for 75 seconds, and then the coating film was irradiated with polarized ultraviolet light (8 mJ / cm 2 , using an ultra-high pressure mercury lamp) to form a photo-alignment film 1. The film thickness of the photo-alignment film 1 was 0.5 μm.

[0136] -------------------------------------------------- Coating liquid E1 for forming photoalignment film -------------------------------------------------- Polymer PA-1 (shown below) 100.00 parts by mass Acid generator PAG-1 (shown below) 6.00 parts by mass DIPEA 0.60 parts by mass Butyl acetate 625.4 parts by mass Methyl ethyl ketone 156.3 parts by mass --------------------------------------------------

[0137] Polymer PA-1 (In the formula below, the numerical value for each repeating unit represents the content (% by mass) of each repeating unit relative to all repeating units; weight average molecular weight: 45,000)

[0138]

[0139] Acid generator PAG-1

[0140]

[0141] DIPEA

[0142]

[0143] [Preparation of Optically Anisotropic Film A1] The following composition F1 was applied onto the above-mentioned photo-alignment film 1 using a bar coater. The coating film formed on the photo-alignment film 1 was heated to 125°C with hot air, then cooled to 60°C, and then irradiated with 200 mJ / cm at a wavelength of 365 nm using a high-pressure mercury lamp in a nitrogen atmosphere. 2 The coating film was irradiated with ultraviolet light of 200 mJ / cm 2 while being heated to 120°C. 2The coating film was irradiated with ultraviolet light at 100°C, thereby fixing the alignment of the liquid crystal compound and producing an optically anisotropic film A1, a positive A plate. During ultraviolet irradiation, a mask with a linearly varying ultraviolet transmittance was placed between the coating film and the high-pressure mercury lamp (see Figure 10). When irradiating at 60°C, a mask with a 100% transmittance at the center and a 0% transmittance on the circumference was placed, while when irradiating at 120°C, a mask with a 0% transmittance at the center and a 100% transmittance on the circumference was placed. This optically anisotropic film A1 corresponds to the optical film having the aforementioned varying region. The resulting optically anisotropic film A1 had a thickness of 3.5 μm and was a patterned retardation film in which the in-plane retardation continuously decreased concentrically from the center toward the 50 mm diameter circumference (see Figure 1). The Re(550) at the center was 180 nm, and the Re(550) on the circumference 50 mm diameter from the center was 142 nm. The average in-plane retardation at a wavelength of 550 nm in the change region of the optically anisotropic film A1 was 160 nm. The relationship Re(450)≦Re(550)≦Re(650) was satisfied at any position in the change region of the optically anisotropic film A1. The ratio Re(450) / Re(550) was 0.82 at any position in the change region of the optically anisotropic film A1.

[0144] - 45.36 parts by mass of polymerizable liquid crystal compound LA-1 described below - 21.84 parts by mass of polymerizable liquid crystal compound LA-2 described below - 20.00 parts by mass of polymerizable liquid crystal compound LA-3 described below - 5.00 parts by mass of polymerizable liquid crystal compound LA-4 described below - 7.80 parts by mass of mixture of polymerizable liquid crystal compounds LA-5 described below - 0.50 parts by mass of polymerization initiator PI-1 described below - 0.09 parts by mass of leveling agent T-1 described below - 180.73 parts by mass of cyclopentanone - 53.98 parts by mass of methyl ethyl ketone

[0145] Polymerizable liquid crystal compound LA-1 (tBu represents a tertiary butyl group)

[0146]

[0147] Polymerizable liquid crystal compound LA-2

[0148]

[0149] Polymerizable liquid crystal compound LA-3

[0150]

[0151] Polymerizable liquid crystal compound LA-4 (Me represents a methyl group)

[0152]

[0153] Polymerizable liquid crystal compound mixture LA-5 (a mixture of the following liquid crystal compounds (RA), (RB), and (RC) in a mass ratio of 84:14:2)

[0154]

[0155] Polymerization initiator PI-1

[0156]

[0157] Leveling agent T-1 (in the formula below, the numerical value for each repeating unit represents the content (mass %) of each repeating unit relative to all repeating units; weight average molecular weight: 25,000)

[0158]

[0159] (Preparation of optically anisotropic film C1) Optically anisotropic film C1 was prepared by referring to the method described in paragraphs 0069 to 0077 of WO 2018 / 174194. The thickness of the optically anisotropic film C1 was 0.5 μm and Rth(550) was −60 nm.

[0160] [Formation of Half Mirror on Lens] Aluminum was vapor-deposited on the convex side of a lens (a convex meniscus lens LE1076-A (diameter 2 inches, focal length 100 mm) manufactured by Thorlab) to give a reflectance of 40%, forming a half mirror.

[0161] (Preparation of Optical Laminate 1) An adhesive (SK-2057, manufactured by Soken Chemical & Engineering Co., Ltd.) was applied to the side of the optically anisotropic film A1 opposite to the cellulose acylate film 1 side to form an adhesive layer, and the optically anisotropic film C1 was attached thereto so that the adhesive layer and the coating layer were in close contact with each other. Thereafter, the cellulose acylate film 1 and the photo-alignment film 1 were peeled off to obtain a laminate. Next, an adhesive (SK-2057, manufactured by Soken Chemical & Engineering Co., Ltd.) was applied to one side of a linear polarization type reflective polarizer (APF: 53 μm, manufactured by 3M Corporation) to form an adhesive layer, and the laminate was attached to the optically anisotropic film A1 in a direction in which the optically anisotropic film A1 and the APF were in close contact with each other, such that the average direction of the in-plane slow axis of the optically anisotropic film A1 and the reflection axis of the linear polarization type reflective polarizer formed an angle of 45°. The support was peeled off to obtain an optical laminate 1. The optical laminate 1 had an APF, an optically anisotropic film A1, and an optically anisotropic film C1 in this order.

[0162] [Preparation of Molded Body 1] The optical laminate 1 was set in a molding device. At this time, it was positioned so that the optically anisotropic film C1 was on the bottom side. The molding space in the molding device consisted of box 1 and box 2, separated by the optical laminate 1. A meniscus lens (diameter 50 mm, radius of curvature on the concave side 40 mm) with aluminum vapor deposition on the convex side was placed as a mold in box 1 below the optical laminate 1, with the concave side facing up. In addition, a transparent window was installed on the top of box 2 above the optical laminate 1, and an IR light source for heating the optical laminate 1 was installed outside this window. Between the IR light source and the optical laminate 1, a ring-shaped patterned infrared reflection filter was placed. The filter was cut out to fit the outer peripheral shape of the mold from a cholesteric liquid crystal layer that reflects infrared light with a wavelength of 2.2 μm to 3.0 μm at a reflectance of approximately 50%, and the center was further cut out into a circle with a diameter of 1 inch. At this time, when viewed from directly above, the center of the patterned infrared reflection filter, the center of the mold, and the center of the pattern of the optically anisotropic film A1 were arranged so as to be in the same position. Next, a vacuum pump was used to evacuate the inside of box 1 and box 2 to 0.1 atmospheres or less. Next, as a process for heating the optical laminate 1, infrared rays were irradiated and the optical laminate 1 was heated until the center reached 108°C and the end reached 99°C. Next, as a process for pressing the optical laminate 1 against the mold and deforming it according to the shape of the mold, gas was flowed into box 2 from a gas cylinder to pressurize it to 300 kPa, and the optical laminate 1 was pressed against the mold. This resulted in a molded product 1 molded into a convex curved shape. Note that, by the above procedure, the change region in the optically anisotropic film A1 was molded into a convex curved shape.

[0163] Example 2 Molded product 2 was produced in the same manner as in Example 1, except that the optically anisotropic film A1 was replaced with the optically anisotropic film A2 below and the radius of curvature of the meniscus lens during curved surface molding was set to 45 mm.

[0164] [Preparation of Optically Anisotropic Film A2] The above-described composition F1 was applied onto the above-described photo-alignment film 1 using a bar coater. The coating film formed on the photo-alignment film 1 was heated to 125°C with hot air, then cooled to 60°C, and then irradiated with 200 mJ / cm at a wavelength of 365 nm using a high-pressure mercury lamp in a nitrogen atmosphere. 2The coating film was irradiated with ultraviolet light of 200 mJ / cm 2 while being heated to 120°C. 2 The coating film was irradiated with ultraviolet light at 100°C, thereby fixing the alignment of the liquid crystal compound and producing an optically anisotropic film A2, a positive A plate. During irradiation at 60°C, a mask with a linearly varying ultraviolet transmittance in a concentric pattern of 50 mm diameter was placed between the coating film and the high-pressure mercury lamp, and ultraviolet irradiation was performed. During irradiation at 60°C, a mask with a transmittance of 100% at the center and 0% on the circumference was used. No mask was used during irradiation at 120°C. This optically anisotropic film A2 corresponds to the optical film having the aforementioned varying region. The resulting optically anisotropic film A2 had a thickness of 3.6 μm and was a patterned retardation film in which the Re continuously decreased concentrically from the center toward the circumference with a diameter of 50 mm (see FIG. 1). The Re(550) at the center was 171 nm, and the Re(550) on the circumference with a diameter of 50 mm from the center was 142 nm. The average in-plane retardation at a wavelength of 550 nm in the change region of the optically anisotropic film A2 was 156 nm. The relationship Re(450)≦Re(550)≦Re(650) was satisfied at any position in the change region of the optically anisotropic film A2. The ratio Re(450) / Re(550) was 0.82 at any position in the change region of the optically anisotropic film A2.

[0165] Example 3 Molded product 3 was produced in the same manner as in Example 1, except that the optically anisotropic film A1 was replaced with the following optically anisotropic film A3 and the radius of curvature of the meniscus lens during curved surface molding was set to 36 mm.

[0166] [Preparation of Optically Anisotropic Film A3] Composition F1 having the following composition was applied onto the above-mentioned photo-alignment film 1 using a bar coater. The coating film formed on the photo-alignment film 1 was heated to 125°C with hot air, then cooled to 50°C, and then irradiated with 200 mJ / cm at a wavelength of 365 nm using a high-pressure mercury lamp under a nitrogen atmosphere. 2 The coating film was irradiated with ultraviolet light of 200 mJ / cm 2 while being heated to 120°C. 2The coating film was irradiated with ultraviolet light at 100°C, thereby fixing the alignment of the liquid crystal compound and producing an optically anisotropic film A3, a positive A plate. A mask with a linearly varying ultraviolet transmittance was placed between the coating film and the high-pressure mercury lamp, and ultraviolet irradiation was performed. When irradiating at 50°C, a mask with a 100% transmittance at the center and a 0% transmittance on the circumference was placed, while when irradiating at 120°C, a mask with a 0% transmittance at the center and a 100% transmittance on the circumference was placed. This optically anisotropic film A3 corresponds to the optical film having the aforementioned change region. The resulting optically anisotropic film A3 had a thickness of 3.5 μm and was a patterned retardation film in which the Re continuously decreased concentrically from the center to the 50 mm diameter circumference (see FIG. 1). The Re(550) at the center was 193 nm, and the Re(550) on the circumference 50 mm diameter from the center was 142 nm. The average in-plane retardation at a wavelength of 550 nm in the change region of the optically anisotropic film A3 was 166 nm. The relationship Re(450)≦Re(550)≦Re(650) was satisfied at any position in the change region of the optically anisotropic film A3. The ratio Re(450) / Re(550) was 0.82 at any position in the change region of the optically anisotropic film A3.

[0167] Example 4 Molded body 4 was produced in the same manner as in Example 1, except that the optically anisotropic film A1 was replaced with the optically anisotropic film A4 described below, and no ring-shaped patterned infrared reflective filter was placed during curved surface molding.

[0168] [Fabrication of Wire Grid Polarizer 1] Wire grid polarizer 1 was fabricated with reference to JP 2012-118438 A. Note that wire grid 1 transmits only light polarized in a specific direction, and when a photo-alignment film is irradiated through wire grid polarizer 1, an alignment film having an alignment control force that generates an in-plane slow axis direction in the change region as shown in FIG.

[0169] [Preparation of Photo-Alignment Film 2] The above-mentioned coating solution E1 for forming a photo-alignment film was continuously applied onto the above-mentioned cellulose acylate film 1 using a wire bar, and the support on which the coating film was formed was dried for 75 seconds with hot air at 134°C. Subsequently, ultraviolet light generated using an ultra-high pressure mercury lamp was collimated using a collimating lens, and then polarized through the above-mentioned wire grid polarizer 1, and the coating film was irradiated with polarized ultraviolet light (8 mJ / cm 2 ) to form a photo-alignment film 2. The thickness of the photo-alignment film 2 was 0.5 μm.

[0170] [Preparation of Optically Anisotropic Film A4] The above-described composition F1 was applied onto the above-described photo-alignment film 2 using a bar coater. The coating film formed on the photo-alignment film 2 was heated to 125°C with hot air, then cooled to 60°C, and then irradiated with 200 mJ / cm at a wavelength of 365 nm using a high-pressure mercury lamp in a nitrogen atmosphere. 2 The coating film was irradiated with ultraviolet light of 200 mJ / cm 2 while being heated to 120°C. 2 The coating film was irradiated with ultraviolet light of 1000 nm, thereby fixing the alignment of the liquid crystal compound and producing an optically anisotropic film A4, a positive A plate. During ultraviolet irradiation, a mask with a linearly varying ultraviolet transmittance in a concentric ellipse with a diameter of 50 mm was placed between the coating film and the high-pressure mercury lamp. For irradiation at 60°C, a mask with a transmittance of 60% at the center and 30% on the circumference was placed, while for irradiation at 120°C, a mask with a transmittance of 40% at the center and 70% on the circumference was placed. This optically anisotropic film A4 corresponds to the optical film having the aforementioned change region. The resulting optically anisotropic film A4 had a thickness of 3.5 μm and was a patterned retardation film in which Re continuously decreased in a concentric ellipse from the center toward the circumference with a diameter of 50 mm (see FIG. 7 ). Furthermore, the average in-plane retardation at a wavelength of 550 nm in the change region of the optically anisotropic film A4 was 160 nm. In addition, the relationship Re(450)≦Re(550)≦Re(650) was satisfied at any position in the change region of the optically anisotropic film A4. In addition, Re(450) / Re(550) was 0.82 at any position in the change region of the optically anisotropic film A4.

[0171] Example 5 A molded body 5 was produced in the same manner as in Example 4, except that the photo-alignment film 3 described below was used instead of the photo-alignment film 2 used in the optically anisotropic film A4. The average in-plane retardation at a wavelength of 550 nm in the change region of the optically anisotropic film A5 obtained in Example 5 was 160 nm. This optically anisotropic film A5 corresponds to the optical film having the change region described above.

[0172] [Preparation of Photo-Alignment Film 3] The above-mentioned coating solution E1 for forming a photo-alignment film was continuously applied onto the above-mentioned cellulose acylate film 1 using a wire bar. The support on which the coating film was formed was dried with hot air at 134°C for 75 seconds. Subsequently, ultraviolet light generated using an ultra-high pressure mercury lamp was collimated using a collimating lens, and then polarized through a wire grid that transmits only polarized light in one direction, and the coating film was irradiated with polarized ultraviolet light (8 mJ / cm). 2 A photo-alignment film 3 was formed by irradiating the film with polarized light (using an ultra-high pressure mercury lamp) (see Figures 11 and 12). A mask with a donut-shaped shielding portion with an outer diameter of 75 mm and an inner diameter of 25 mm was placed between the coating film and the wire grid, and polarized light was irradiated. The distance between the coating film and the mask was 34 mm, the distance between the mask and the wire grid was 34 mm, and the distance between the wire grid and the mercury lamp was 10 mm. The photo-alignment film 3 was an alignment film having an alignment control force that caused the in-plane slow axis direction of the change region to be as shown in Figure 8. The film thickness of the photo-alignment film 3 was 0.5 μm.

[0173] Example 6 Molded body 6 was produced in the same manner as in Example 4, except that optically anisotropic film A4 was replaced with the optically anisotropic film A6 below and the radius of curvature of the meniscus lens during curved surface molding was set to 60 mm.

[0174] [Preparation of Optically Anisotropic Film A6] The above-described composition F1 was applied onto the above-described photo-alignment film 1 using a bar coater. The coating film formed on the photo-alignment film 1 was heated to 125°C with hot air, then cooled to 60°C, and then irradiated with 200 mJ / cm at a wavelength of 365 nm using a high-pressure mercury lamp in a nitrogen atmosphere. 2 The coating film was irradiated with ultraviolet light of 200 mJ / cm 2 while being heated to 120°C. 2The coating film was irradiated with ultraviolet light of 1000 nm, thereby fixing the alignment of the liquid crystal compound and producing an optically anisotropic film A6, a positive A plate. During ultraviolet irradiation, a mask with a linearly varying ultraviolet transmittance in a concentric ellipse with a diameter of 50 mm was placed between the coating film and the high-pressure mercury lamp. For irradiation at 60°C, a mask with a transmittance of 20% at the center and 10% on the circumference was placed, while for irradiation at 120°C, a mask with a transmittance of 80% at the center and 90% on the circumference was placed. This optically anisotropic film A6 corresponds to the optical film having the aforementioned change region. The resulting optically anisotropic film A6 had a thickness of 3.5 μm and was a patterned retardation film in which Re continuously decreased in a concentric ellipse from the center toward the circumference with a diameter of 50 mm (see FIG. 7 ). Furthermore, the average in-plane retardation at a wavelength of 550 nm in the change region of the optically anisotropic film A6 was 149 nm. In addition, the relationship Re(450)≦Re(550)≦Re(650) was satisfied at any position in the change region of the optically anisotropic film A6. In addition, Re(450) / Re(550) was 0.82 at any position in the change region of the optically anisotropic film A6.

[0175] Example 7 Molded product 7 was produced in the same manner as in Example 6, except that optically anisotropic film A6 was replaced with the following optically anisotropic film A7.

[0176] [Preparation of Optically Anisotropic Film A7] The above-described composition F1 was applied onto the above-described photo-alignment film 1 using a bar coater. The coating film formed on the photo-alignment film 1 was heated to 125°C with hot air, then cooled to 60°C, and then irradiated with 200 mJ / cm at a wavelength of 365 nm using a high-pressure mercury lamp in a nitrogen atmosphere. 2 The coating film was irradiated with ultraviolet light of 200 mJ / cm 2 while being heated to 120°C. 2The coating film was irradiated with ultraviolet light of 1000 nm, thereby fixing the alignment of the liquid crystal compound and producing an optically anisotropic film A7, a positive A plate. During ultraviolet irradiation, a mask with a linearly varying ultraviolet transmittance in a concentric ellipse with a diameter of 50 mm was placed between the coating film and the high-pressure mercury lamp. For irradiation at 60°C, a mask with a transmittance of 70% at the center and 30% on the circumference was placed, while for irradiation at 120°C, a mask with a transmittance of 30% at the center and 60% on the circumference was placed. This optically anisotropic film A7 corresponds to the optical film having the aforementioned change region. The resulting optically anisotropic film A7 had a thickness of 3.1 μm and was a patterned retardation film in which Re continuously decreased in a concentric ellipse from the center toward the circumference with a diameter of 50 mm (see FIG. 7 ). Furthermore, the average in-plane retardation at a wavelength of 550 nm in the change region of the optically anisotropic film A7 was 149 nm. In addition, the relationship Re(450)≦Re(550)≦Re(650) was satisfied at any position in the change region of the optically anisotropic film A7. In addition, Re(450) / Re(550) was 0.82 at any position in the change region of the optically anisotropic film A7.

[0177] Example 8 Molded product 8 was produced in the same manner as in Example 6, except that optically anisotropic film A6 was replaced with the following optically anisotropic film A8.

[0178] [Preparation of Optically Anisotropic Film A8] The above-described composition F1 was applied onto the above-described photo-alignment film 3 using a bar coater. The coating film formed on the photo-alignment film 3 was heated to 125°C with hot air, then cooled to 60°C, and then irradiated with 80 mJ / cm at a wavelength of 365 nm using a high-pressure mercury lamp in a nitrogen atmosphere. 2 The coating film was irradiated with ultraviolet light of 200 mJ / cm 2 while being heated to 120°C. 2The coating film was irradiated with ultraviolet light of 1000 nm, thereby fixing the alignment of the liquid crystal compound, and an optically anisotropic film A8, a positive A plate, was produced. This optically anisotropic film A8 corresponds to the optical film having the above-mentioned change region. The thickness of the obtained optically anisotropic film A8 was 3.2 μm, and the average in-plane retardation at a wavelength of 550 nm in the change region of the optically anisotropic film A8 was 151 nm. Furthermore, at every position in the change region of the optically anisotropic film A8, the relationship Re(450)≦Re(550)≦Re(650) was satisfied. Furthermore, at every position in the change region of the optically anisotropic film A8, Re(450) / Re(550) was 0.82.

[0179] Example 9 Molded product 9 was produced in the same manner as in Example 4, except that optically anisotropic film A4 was replaced with the following optically anisotropic film A9 and the radius of curvature of the meniscus lens during curved surface molding was set to 75 mm.

[0180] [Preparation of Optically Anisotropic Film A9] The above-described composition F1 was applied onto the above-described photo-alignment film 1 using a bar coater. The coating film formed on the photo-alignment film 1 was heated to 125°C with hot air, then cooled to 60°C, and then irradiated with 200 mJ / cm at a wavelength of 365 nm using a high-pressure mercury lamp in a nitrogen atmosphere. 2 The coating film was irradiated with ultraviolet light of 200 mJ / cm 2 while being heated to 120°C. 2The coating film was irradiated with ultraviolet light of 1000 nm, thereby fixing the alignment of the liquid crystal compound, and an optically anisotropic film A9 having a positive A plate layer was produced. Here, a mask with a linearly varying ultraviolet transmittance in a concentric ellipse with a diameter of 50 mm was placed between the coating film and the high-pressure mercury lamp, and ultraviolet irradiation was performed. When irradiating at 60°C, a mask with a transmittance of 15% at the center and 10% on the circumference was placed, and when irradiating at 120°C, a mask with a transmittance of 85% at the center and 90% on the circumference was placed. The resulting optically anisotropic film A9 had a thickness of 3.5 μm, and was a patterned retardation film in which Re continuously decreased in a concentric ellipse from the center toward the circumference with a diameter of 50 mm (see FIG. 7). The average in-plane retardation at a wavelength of 550 nm in the change region of the optically anisotropic film A9 was 146 nm. In addition, at any position in the change region of the optically anisotropic film A9, the relationship Re(450)≦Re(550)≦Re(650) was satisfied. In addition, at any position in the change region of the optically anisotropic film A9, Re(450) / Re(550) was 0.82.

[0181] Comparative Example 1 A molded body 10 was produced in the same manner as in Example 4, except that the optically anisotropic film A4 was replaced with the following optically anisotropic film A10.

[0182] [Preparation of Optically Anisotropic Film A10] The above-described composition F1 was applied onto the above-described photo-alignment film 1 using a bar coater. The coating film formed on the photo-alignment film 1 was heated to 125°C with hot air, then cooled to 60°C, and then irradiated with 80 mJ / cm at a wavelength of 365 nm using a high-pressure mercury lamp in a nitrogen atmosphere. 2 The coating film was irradiated with ultraviolet light of 200 mJ / cm 2 while being heated to 120°C. 2 The coating film was irradiated with ultraviolet light of 1000 nm, thereby fixing the alignment of the liquid crystal compound, and an optically anisotropic film A10, a positive A plate, was produced. The thickness of the obtained optically anisotropic film A10 was 3.5 μm, and the average in-plane retardation at a wavelength of 550 nm was 166 nm. Furthermore, at any position in the change region of the optically anisotropic film A10, the relationship Re(450)≦Re(550)≦Re(650) was satisfied. Furthermore, at any position in the change region of the optically anisotropic film A10, Re(450) / Re(550) was 0.82.

[0183] Comparative Example 2 A molded article 11 was produced in the same manner as in Example 1, except that the optically anisotropic film A1 was replaced with the following optically anisotropic film A11.

[0184] [Preparation of Optically Anisotropic Film A11] The above-described composition F1 was applied onto the above-described photo-alignment film 1 using a bar coater. The coating film formed on the photo-alignment film 1 was heated to 125°C with hot air, then cooled to 60°C, and then irradiated with 80 mJ / cm at a wavelength of 365 nm using a high-pressure mercury lamp in a nitrogen atmosphere. 2 The coating film was irradiated with ultraviolet light of 200 mJ / cm 2 while being heated to 120°C. 2 The coating film was irradiated with ultraviolet light of 1000 nm, thereby fixing the alignment of the liquid crystal compound, and an optically anisotropic film A11, which is a positive A plate, was produced. The thickness of the obtained optically anisotropic film A11 was 3.8 μm, and the average in-plane retardation at a wavelength of 550 nm was 180 nm. Furthermore, at any position in the change region of the optically anisotropic film A11, the relationship Re(450)≦Re(550)≦Re(650) was satisfied. Furthermore, at any position in the change region of the optically anisotropic film A11, Re(450) / Re(550) was 0.82.

[0185] Comparative Example 3 A molded body 12 was produced in the same manner as in Example 1, except that the optically anisotropic film A1 was replaced with the optically anisotropic film A12 described below and the radius of curvature of the meniscus lens during curved surface molding was set to 60 mm.

[0186] [Preparation of Optically Anisotropic Film A12] The above-described composition F1 was applied onto the above-described photo-alignment film 1 using a bar coater. The coating film formed on the photo-alignment film 1 was heated to 125°C with hot air, then cooled to 60°C, and then irradiated with 80 mJ / cm at a wavelength of 365 nm using a high-pressure mercury lamp in a nitrogen atmosphere. 2 The coating film was irradiated with ultraviolet light of 200 mJ / cm 2 while being heated to 120°C. 2The coating film was irradiated with ultraviolet light of 1000 nm, thereby fixing the alignment of the liquid crystal compound, and an optically anisotropic film A12, a positive A plate, was produced. The thickness of the obtained optically anisotropic film A12 was 3.3 μm, and the average in-plane retardation at a wavelength of 550 nm was 156 nm. Furthermore, at any position in the change region of the optically anisotropic film A12, the relationship Re(450)≦Re(550)≦Re(650) was satisfied. Furthermore, at any position in the change region of the optically anisotropic film A12, Re(450) / Re(550) was 0.82.

[0187] Comparative Example 4 A molded body 13 was produced in the same manner as in Example 1, except that the optically anisotropic film A1 was replaced with the optically anisotropic film A13 described below, and the ring-shaped patterned infrared reflection filter used during curved surface molding was changed to a circular patterned infrared reflection filter obtained by cutting out a circle with a diameter of 2.5 cm from a cholesteric liquid crystal layer that reflects infrared rays with wavelengths of 2.2 μm to 3.0 μm at a reflectance of approximately 50%.

[0188] [Preparation of Optically Anisotropic Film A13] The above-described composition F1 was applied onto the above-described photo-alignment film 1 using a bar coater. The coating film formed on the photo-alignment film 1 was heated to 125°C with hot air, then cooled to 60°C, and then irradiated with 80 mJ / cm at a wavelength of 365 nm using a high-pressure mercury lamp in a nitrogen atmosphere. 2 The coating film was irradiated with ultraviolet light of 200 mJ / cm 2 while being heated to 120°C. 2 The coating film was irradiated with ultraviolet light of 1000 nm, thereby fixing the alignment of the liquid crystal compound, and an optically anisotropic film A13, a positive A plate, was produced. The thickness of the obtained optically anisotropic film A13 was 3.4 μm, and the average in-plane retardation at a wavelength of 550 nm was 159 nm. Furthermore, at any position in the change region of the optically anisotropic film A13, the relationship Re(450)≦Re(550)≦Re(650) was satisfied. Furthermore, at any position in the change region of the optically anisotropic film A13, Re(450) / Re(550) was 0.82.

[0189] <Optical Evaluation of Optically Anisotropic Films> In each example and comparative example, the adhesive used to form the APF was changed to the water-soluble adhesive SK Dyne 1193 (manufactured by Soken Chemical & Engineering Co., Ltd.), the meniscus lens used in curved surface molding was changed to a plano-concave lens (made of optical glass) made of optical glass, and no optically anisotropic film C1 was attached. A molded body having a convex curved surface was produced according to the same procedures as in each example and comparative example. The obtained molded body was immersed in water for 8 hours to dissolve the water-soluble adhesive and peel off the APF. The in-plane retardation and in-plane slow axis of the convex curved surface of the obtained optically anisotropic film were measured using a two-dimensional birefringence measurement system WPA-200. The optically anisotropic films produced above were produced under the same molding conditions as the optically anisotropic films in molded bodies 1 to 13 and had the same shape. In other words, the optically anisotropic films produced above exhibit the same optical properties as the optically anisotropic films in molded bodies 1 to 13, respectively. The measurement results of the above-mentioned ΔRe and Δaxis are shown in Table 1. During the measurement, a plano-convex lens (made of optical glass) having the same diameter and radius of curvature as the plano-concave lens used in forming the curved surface was placed on top of the concave surface of the molded article with its convex side in contact with the concave surface of the molded article, thereby canceling the effect of refraction due to the concave surface of the molded article and enabling measurement of the in-plane retardation and in-plane slow axis of the optically anisotropic film.

[0190] [Preparation of composite lenses] The APF sides of the molded articles 1 to 13 obtained above were bonded to the photo-alignment film side of the absorptive polarizer film 1S described below using an adhesive. The layers were laminated so that the transmission axis of the APF coincided with the transmission axis of the light-absorbing anisotropic layer. This resulted in composite lenses 1 to 13, each consisting of a half mirror / meniscus lens / positive C plate / adhesive / optically anisotropic film of the present invention / adhesive layer / APF / adhesive layer / absorptive polarizer.

[0191] [Preparation of Absorptive Polarizer Film 1S Having Light Absorption Anisotropic Layer] [Preparation of Substrate] Cellulose acylate film A2 was prepared in the same manner as cellulose acylate film A1, except that the film thickness was set to 60 μm.

[0192] [Formation of Photo-Alignment Film B1] The composition B1 for forming a photo-alignment film, which will be described later, was continuously applied onto the cellulose acylate film A2 using a wire bar. The support on which the coating film was formed was dried with hot air at 140°C for 120 seconds, and then the coating film was irradiated with polarized ultraviolet light (10 mJ / cm 2 A photo-alignment film B1 was formed by irradiating the substrate with a TAC (triacetyl cellulose) film having a photo-alignment film B1. The photo-alignment film B1 had a thickness of 1.5 μm. ------------------------------------------------ Composition of composition B1 for forming a photo-alignment film------------------------------------------------ Photo-alignment compound PA-1 below: 100.00 parts by mass EPICLON N-695 (manufactured by DIC Corporation) 55.74 parts by mass jER YX7400 (manufactured by Mitsubishi Chemical Corporation) 18.75 parts by mass Polymerizable polymer PA-2 below: 8.01 parts by mass Thermal cationic polymerization initiator PAG-1 below: 16.75 parts by mass Stabilizer DIPEA below: 1.06 parts by mass Butyl acetate 1230.49 parts by mass

[0193] Photoalignment compound PA-1 (wherein the numerical value for each repeating unit represents the content (mass%) of each repeating unit relative to all repeating units; weight average molecular weight: 32,000)

[0194]

[0195] Thermal cationic polymerization initiator PAG-1

[0196]

[0197] Stabilizer DIPEA

[0198]

[0199] Polymerizable polymer PA-2 [Weight average molecular weight: 18000]

[0200]

[0201] [Formation of Optically Absorbent Anisotropic Film C1] A composition for forming an optically absorptive anisotropic film C1 having the following composition was continuously applied to the obtained photo-alignment film B1 using a wire bar to form a coating film. Next, the coating film was heated at 130°C for 15 seconds and cooled to room temperature (23°C). Next, the coating film was heated at 75°C for 10 seconds and cooled to room temperature again. Thereafter, an optically absorptive anisotropic film C1 (polarizer) (thickness: 1.8 μm) was formed on the photo-alignment film B1 by irradiating it with light using an LED (light emitting diode) lamp (center wavelength 365 nm) at an irradiation condition of 300 mJ. The absorption axis of the optically absorptive anisotropic film C1 was in the plane of the optically absorptive anisotropic film C1 and perpendicular to the width direction of the cellulose acylate film A2.

[0202] 0.70 parts by mass of the liquid crystal compound L-3 described above; 0.06 parts by mass of the adhesion improver A-1 described above; 0.18 parts by mass of polymerization initiator IRGACUREOXE-02 (manufactured by BASF); 0.009 parts by mass of the surfactant F-3 described below; Cyclopentanone 91.75 parts by mass ・Benzyl alcohol 2.35 parts by mass ----------------------------------------------------------------

[0203] Dichroic substance Dye-C1

[0204]

[0205] Dichroic substance Dye-C2

[0206]

[0207] Dichroic substance Dye-M1

[0208]

[0209] Dichroic substance Dye-Y2

[0210]

[0211] Liquid crystal compound L-1 (In the formula below, the numerical values ​​("59", "15", "26") shown for each repeating unit represent the content (% by mass) of each repeating unit relative to all repeating units. Weight average molecular weight: 18,000)

[0212]

[0213] Liquid crystal compound L-2 (a mixture of the following liquid crystal compounds (RA), (RB), and (RC) in a mass ratio of 84:14:2)

[0214]

[0215] Liquid crystal compound L-3

[0216]

[0217] Adhesion improver A-1

[0218]

[0219] Surfactant F-3 (wherein the numerical value for each repeating unit represents the content (mass%) of each repeating unit relative to the total repeating units. Ac represents —C(O)CH 3 Weight average molecular weight: 15,000

[0220]

[0221] [Formation of Protective Layer D1] Coating Solution D2 having the following composition was continuously applied onto the optically absorptive anisotropic film C1 using a wire bar. Thereafter, the coating was dried with hot air at 80°C for 5 minutes and irradiated with 300 mJ of light using an LED (light emitting diode) lamp (center wavelength 365 nm) to obtain a laminate having a 0.6 μm-thick protective layer D1 made of polyvinyl alcohol (PVA), i.e., an absorptive polarizer film 1 having a cellulose acylate film A1 (substrate), a photo-alignment film B1, an optically absorptive anisotropic film C1, and a protective layer D1 adjacent to each other in this order. -------------------------------------------------- Composition of coating liquid D1 for forming protective layer -------------------------------------------------- 3.31 parts by mass of modified polyvinyl alcohol shown below 0.17 parts by mass of initiator IRGACURE 2959 (manufactured by BASF) 0.07 parts by mass of glutaraldehyde 0.07 parts by mass of pyridinium paratoluenesulfonate 0.05 parts by mass of surfactant F-9 shown below 74.0 parts by mass of water 22.4 parts by mass of ethanol --------------------------------------------------

[0222] Modified polyvinyl alcohol (in the formula below, the numerical value for each repeating unit represents the content (mass%) of each repeating unit relative to all repeating units; weight average molecular weight: 14,000)

[0223]

[0224] Surfactant F-9

[0225]

[0226] [Preparation of Absorptive Polarizer Film 1S Molded to a Curved Surface] The protective layer side of the absorptive polarizer film 1 was bonded to a PMMA film via an adhesive sheet, and only the substrate was peeled off to form the absorptive polarizer film 2, which was then set in a molding device. The PMMA film side was positioned on the upper side. The molding space in the molding device consisted of box 1 and box 2, separated by the absorptive polarizer film 2. A meniscus lens (diameter 50 mm) was placed as a mold in box 1 below the absorptive polarizer film 2, with the concave surface facing up. The radius of curvature of the concave surface was set to be the same as the radius of curvature of each of the molded bodies 1 to 13 to be bonded. A transparent window was installed on the top of box 2 above the absorptive polarizer film 2, and an IR light source for heating the absorptive polarizer film 2 was installed outside the window. Between the IR light source and the absorptive polarizer film 2, a ring-shaped patterned infrared reflection filter was placed by cutting a cholesteric liquid crystal layer that reflects infrared light with wavelengths of 2.2 μm to 3.0 μm at a reflectance of approximately 50% to fit the outer periphery of the mold and further cutting out a circle with a diameter of 1 inch in the center. The patterned infrared reflection filter was positioned so that the center of the filter was at the center of the mold when viewed from directly above. Next, a vacuum pump was used to evacuate the insides of boxes 1 and 2 to a pressure of 0.1 atmospheres or less. Next, in the heating step, the absorptive polarizer film 2 was heated by irradiating it with infrared rays until the center of the absorptive polarizer film 2 reached 108°C and the edges reached 99°C. The glass transition temperature Tg of the PMMA film used as the support was 105°C, so that the center would easily stretch and the edges would not easily stretch during molding. Next, in a step of pressing the absorptive polarizer film 2 against the mold and deforming it to conform to the shape of the mold, gas was flowed into the box 2 from a gas cylinder to pressurize it to 300 kPa, and the absorptive polarizer film 2 was pressure-bonded to the mold. Finally, the absorptive polarizer film 2 was removed from the lens mold, thereby obtaining an absorptive polarizer film 1S molded to a curved surface.

[0227] [Fabrication of Virtual Reality Display Devices] A virtual reality display device "Huawei VR Glass" manufactured by Huawei, which is a virtual reality display device that uses a reciprocating optical system, was disassembled, and all of the compound lenses were removed. Compound lenses 1 to 13 were then incorporated into the main body, with the light absorption anisotropic layer facing the eye, to fabricate virtual reality display devices 1 to 13.

[0228] <Evaluation of Light Leakage> In the manufactured virtual reality display devices 1 to 13, a black and white checkered pattern was displayed on the image display panel, and the degree of light leakage was visually evaluated using the following three levels. If there is light leakage, a double image is visible and the contrast of the relevant part decreases. A rating of B or higher is preferable. A: No double image is visible at all B: A slight double image is visible but not bothersome C: A clear double image The results are shown in Table 1.

[0229] In Table 1, the "Re" column indicates that the above-mentioned requirement "in-plane retardation gradually decreases from the center of the change region toward the outside" is met, and "B" indicates that the requirement is not met. In Table 1, the "Axis" column indicates that the above-mentioned requirement "the direction of the in-plane slow axis at the center of the change region is parallel to the average direction of the in-plane slow axes, and the direction of the in-plane slow axis on the third reference line gradually increases from the center of the change region toward the outside" is met, and "B" indicates that the requirement is not met. In Table 1, the "Shift Angle" column indicates the angle between the in-plane slow axis at the center of the change region and the in-plane slow axis at a position on the third reference line at the periphery of the change region. In Table 1, the "Requirement 1 and Requirement 2" column indicates that both the above-mentioned requirements 1 and 2 are met, and "A" indicates that either one or both are not met. In Table 1, the "Radius of curvature R (mm)" and "Lens radius L (mm)" columns respectively represent the minimum radius of curvature (mm) of the convexly curved surface portion and half the equivalent circle diameter (mm) of the convexly curved surface portion, as described above. In Table 1, the "ΔRe (nm)" column represents the largest in-plane retardation difference (nm) among the differences in in-plane retardation at a wavelength of 550 nm at two positions on the convexly curved surface portion, as described above. In Table 1, the "Δaxis (°)" column represents the largest angle (°) among the angles formed between the in-plane slow axes at two positions on the convexly curved surface portion when observed from the normal direction of the tangent plane at the vertex of the convexly curved surface portion, as described above. In Table 1, the "Formula (1)" column represents "A" if the requirement of the above-described formula (1) is met, and "B" if it is not met. In Table 1, the "Formula (2)" column represents "A" if the requirement of the above-described formula (2) is met, and "B" if it is not met.

[0230] The change regions of the optical films of Examples 4, 5, and 8 satisfied the various requirements described above. More specifically, the change regions of the optical films of Examples 4, 5, and 8 included points P1 and P2, and the angle A1 between the in-plane slow axis and the first reference line at point P1 was the same as the angle A2 between the in-plane slow axis and the first reference line at point P2. The change regions of the optical films of Examples 4, 5, and 8 included points P3 and P4, and the angle A3 between the in-plane slow axis and the second reference line at point P3 was the same as the angle A4 between the in-plane slow axis and the second reference line at point P4. The change regions of the optical films of Examples 4, 5, and 8 also included points P3 and P4, and the direction of the in-plane slow axis at each position on the first reference line and the second reference line was parallel to the direction of the in-plane slow axis at the center of the change region. In the change regions of the optical films of Examples 4, 5, and 8, when the two lines forming an angle of 22.5° between the first reference line and the third reference line were defined as a fourth reference line, the angle (acute angle) formed by the in-plane slow axis at each position on the fourth reference line and the fourth reference line gradually increased outward from the center C. In the change regions of the optical films of Examples 4, 5, and 8, when the two lines forming an angle of 22.5° between the second reference line and the third reference line were defined as a fifth reference line, the angle (acute angle) formed by the in-plane slow axis at each position on the fifth reference line and the fifth reference line gradually increased outward from the center C. In addition, in the changed regions of the optical films of Examples 4, 5, and 8, any two positions located within two adjacent divided regions surrounded by the first reference line and the third reference line and on the two fourth reference lines described above, and facing each other across the first reference line, corresponded to points P1 and P2 satisfying the above-mentioned requirement 1. In addition, in the changed regions of the optical films of Examples 4, 5, and 8, any two positions located within two adjacent divided regions surrounded by the second reference line and the third reference line and on the two fifth reference lines described above, and facing each other across the second reference line, corresponded to points P3 and P4 satisfying the above-mentioned requirement 2.In the change regions of the optical films of Examples 4, 5, and 8, the inclination of the in-plane slow axis with respect to the first reference line at each position in two adjacent divided regions surrounded by the first reference line and the third reference line (the combination of divided regions R1 and R2, and the combination of divided regions R5 and R6 in FIG. 8 ) increased with increasing distance from the first reference line. In the change regions of the optical films of Examples 4, 5, and 8, the inclination of the in-plane slow axis with respect to the second reference line at each position in two adjacent divided regions surrounded by the second reference line and the third reference line (the combination of divided regions R3 and R4, and the combination of divided regions R7 and R7 in FIG. 8 ) decreased with increasing distance from the second reference line.

[0231]

[0232] As shown in the table above, it was confirmed that the optically anisotropic film of the present invention exhibits the desired effects. It was also confirmed that by using the optical film having a change region of the present invention, an optically anisotropic film exhibiting the desired effects can be formed. A comparison of Examples 1 to 9 confirmed that better effects can be obtained when ΔRe is 0 to 5 nm and Δaxis is 0 to 1.5°. Note that Figure 20 is a diagram plotting the results of the above Examples and Comparative Examples, and it was confirmed that all Examples satisfied the relationships of Equations (1) and (2).

[0233] 10A, 10B, 10C Optical film 12A, 12B, 12C Change region 20 Mold having a concave molding surface 22 Film 24 Film to which a concave shape has been transferred 26 Mold having a convex molding surface 28 Film to which a convex shape has been transferred 30 Coating film 32 Filter 34 Transmitting region 36 Light-shielding region 40 Alignment film containing a photo-alignable group 42 Mask 44 Wire grid 46 Opening 48 Light-shielding portion 50, 52 Optically anisotropic film 54 Convex curved portion 56 Planar portion 60A, 60B Laminate 62 Absorptive polarizer 64 Optically anisotropic film 66 Positive C plate 68 Cholesteric liquid crystal layer 70 Linear polarization type reflective polarizer 72 Composite lens 74, 90 Laminate 76, 88 Lens 78, 86 Half mirror 80 Virtual reality display device 82 Image display device 84 Circular polarizer 92 Light ray

Claims

1. An optical film having a change region in which at least one of the in-plane retardation and the direction of the in-plane slow axis changes, wherein when the in-plane retardation changes in the change region, the in-plane retardation changes gradually from the center of the change region toward the outside, and when the direction of the in-plane slow axis changes in the change region, the direction of the in-plane slow axis at the center is parallel to the average direction of the in-plane slow axis of the change region, and the direction of the in-plane slow axis on the third reference line changes gradually from the center of the change region toward the outside.

2. The optical film according to claim 1, wherein the average in-plane retardation at a wavelength of 550 nm in the changed region is 100 to 300 nm.

3. The optical film according to claim 1, wherein when the in-plane retardation changes in the change region, the in-plane retardation gradually decreases from the center of the change region toward the outside.

4. The optical film according to claim 1, wherein, in two adjacent divided regions in the change region surrounded by the first reference line and the third reference line, there are points P1 and P2 that satisfy the relationship of Requirement 1 below, and, in two adjacent divided regions in the change region surrounded by the second reference line and the third reference line, there are points P3 and P4 that satisfy the relationship of Requirement 2 below. Requirement 1: The direction of inclination of the in-plane slow axis at point P1 present in one of the two adjacent divided regions surrounded by the first reference line and the third reference line, relative to the first reference line, is opposite to the direction of inclination of the in-plane slow axis at point P2 present in the other of the two divided regions, which is located on a line that passes through point P1 and is perpendicular to the first reference line, and is at a distance from the first reference line on the perpendicular line equal to that of point P1, relative to the first reference line. Requirement 2: The direction of inclination of the in-plane slow axis at point P3, which exists in one of two adjacent divided regions surrounded by the second reference line and the third reference line, with respect to the second reference line is opposite to the direction of inclination of the in-plane slow axis at point P4, which exists in the other of the two divided regions, is located on a line that passes through point P3 and is perpendicular to the second reference line, and is at a distance from the second reference line on the perpendicular line equal to that of point P3, with respect to the second reference line.

5. A laminate comprising the optical film according to claim 1 and an absorptive polarizer, wherein the angle between the average direction of the in-plane slow axes of the change regions of the optical film and the absorption axis of the absorptive polarizer is within the range of 40 to 50°.

6. An optically anisotropic film having a convex curved surface portion, the optically anisotropic film satisfying the relationship of formula (1) and formula (2). Formula (1) (ΔRe) 1/2 + (Δaxis) 1/2 ≦10×(L / R−0.1) Equation (2) L / R≧0.30 R represents a numerical value R when the minimum radius of curvature of the convex curved surface portion is R (mm). L represents a numerical value L when half the value of the circle equivalent diameter of the convex curved surface portion when observed from the normal direction of the tangent plane at the apex of the convex curved surface portion is L (mm). ΔRe represents a numerical value ΔRe when the largest in-plane retardation difference among the differences in in-plane retardation at a wavelength of 550 nm at two positions on the convex curved surface portion is ΔRe (nm). Δaxis represents a numerical value Δaxis when the largest angle between the in-plane slow axes at two positions on the convex curved surface portion when observed from the normal direction of the tangent plane at the apex of the convex curved surface portion is Δaxis (°).

7. A display device comprising the optically anisotropic film according to claim 6.

8. The display device of claim 7 which is a virtual reality display device.

Citation Information

Patent Citations

  • Polymer film, retardation film, method for producing retardation film and optical compensation polarizing plate by using the retardation film

    JP2007131681A

  • curved optical filter

    JP2011501821A

  • Optical element and method of manufacturing the same

    JP2022020360A

  • Optical film, polarizing plate, and liquid crystal display

    WO2010095317A1