Surface-treated steel sheet
The surface-treated steel sheet with a zinc-nickel plating layer, chromium-containing composite layer, and a specialized coating film addresses the need for improved adhesion and corrosion resistance, enhancing its suitability for fuel tanks by optimizing layer thickness and composition.
Patent Information
- Application Number
- PCT/JP2024/013186
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-03
AI Technical Summary
Existing surface-treated steel sheets used for fuel tanks face challenges in achieving both formability and corrosion resistance, particularly when exposed to fuels like gasoline, as they require improved adhesion and corrosion resistance to prevent corrosion.
A surface-treated steel sheet with a specific laminated structure, including a plating layer of zinc and nickel, a chromium-containing composite layer, and a coating film containing epoxy resin, isocyanate resin, silica particles, and polyethylene wax, which enhances adhesion and corrosion resistance by optimizing the thickness and composition of these layers.
The proposed solution significantly improves the adhesion and corrosion resistance of the steel sheets, ensuring they can withstand fuel exposure without compromising formability or weldability, thus making them suitable for fuel tank applications.
Smart Images

Figure JP2024013186_03102024_PF_FP_ABST
Abstract
Description
Surface-treated steel sheet
[0001] The present invention relates to a surface-treated steel sheet.
[0002] Various types of plated steel sheets are used as materials for manufacturing motorcycle fuel tanks. When manufacturing a fuel tank, the plated steel sheet material must be processed into the desired shape. Furthermore, the surface of the plated steel sheet that is exposed to fuels such as gasoline must be corrosion-resistant to prevent corrosion by the fuel. Therefore, plated steel sheets used as fuel tank materials must be both formable and corrosion-resistant.
[0003] In order to achieve both formability and corrosion resistance, for example, Patent Document 1 listed below discloses an organic composite plated steel sheet in which a chromate film and a film made of a paint composition are formed on the surface of a zinc, aluminum, or zinc-based alloy plated steel sheet.
[0004] Special Publication No. 4-28539
[0005] Here, the present inventors have further studied the organic composite plated steel sheet disclosed in Patent Document 1 and have found that there is room for further improvement in terms of both the adhesion of the coating after forming and the corrosion resistance.
[0006] Therefore, the present invention has been made in consideration of the above-mentioned points, and an object of the present invention is to provide a surface-treated steel sheet that can further improve the adhesion and corrosion resistance of the coating after forming.
[0007] In order to solve the above problems, the present inventors conducted extensive research and discovered that by appropriately forming a specific composite layer in the laminate structure realized in the surface-treated steel sheet, it is possible to further improve the adhesion and corrosion resistance of the coating after forming. The gist of the present invention, which was completed based on this finding, is as follows.
[0008] (1) A steel sheet having a zinc- and nickel-containing plating layer located on at least one surface thereof, a first composite layer containing Fe, Zn, and Ni located between the steel sheet and the plating layer, a chromium-containing composite layer containing at least Cr located on the plating layer, and a coating film containing an epoxy resin, an isocyanate resin, and silica particles located on the chromium-containing composite layer, wherein the coating weight of the plating layer is 2 to 50 g / m per side. 2 The chromium-containing composite layer includes a second composite layer containing Cr, Zn, and Ni located on the plating layer side, and a third composite layer containing Si, N, and Cr located on the coating film side, and the coating amount of the chromium-containing composite layer is 10 to 200 mg / m in terms of metal Cr. 2(2) The surface-treated steel sheet according to (1), wherein a ratio (d2 / d1) of an average thickness d2 of the second composite layer to an average thickness d1 of the first composite layer is 0.2 to 150.0, and a ratio (d3 / d1) of an average thickness d3 of the third composite layer to an average thickness d1 of the first composite layer is 0.2 to 150.0. (3) The surface-treated steel sheet according to (1) or (2), wherein the coating contains polyethylene wax in a proportion of 0.1 to 10.0 mass% based on the coating solid content, the epoxy resin content is 30.0 mass% or more based on the coating solid content, the isocyanate resin content is 0.10 to 2.00 in terms of mass ratio based on the epoxy resin, and the silica particles content is 5.0 to 50.0 mass% based on the coating solid content, and the coating contains the epoxy resin, the isocyanate resin, the silica particles, and the polyethylene wax in a total amount of 100 mass% or less. (4) The surface-treated steel sheet according to (1) or (2), wherein the epoxy resin is a bisphenol A-type epoxy resin having a number average molecular weight of 300 to 100,000. (5) The surface-treated steel sheet according to (1) or (2), wherein the silica particles are at least one of fumed silica and colloidal silica, the fumed silica having an average particle size of 5 to 40 nm, and the colloidal silica having an average particle size of 5 to 200 nm. (6) The surface-treated steel sheet according to (1) or (2), which is used as a material for a fuel tank.
[0009] As described above, according to the present invention, it is possible to further improve the adhesion and corrosion resistance of the coating after forming in a surface-treated steel sheet.
[0010] FIG. 1 is an explanatory diagram schematically showing the structure of a surface-treated steel sheet according to an embodiment of the present invention. FIG. 2 is an explanatory diagram for explaining a first composite layer in the surface-treated steel sheet according to the embodiment. FIG. 3 is an explanatory diagram for explaining the first composite layer in the surface-treated steel sheet according to the embodiment. FIG. 4 is an explanatory diagram for explaining a chromium-containing composite layer in the surface-treated steel sheet according to the embodiment. FIG. 5 is an explanatory diagram for explaining the chromium-containing composite layer in the surface-treated steel sheet according to the embodiment. FIG. 6 is an explanatory diagram for explaining the chromium-containing composite layer in the surface-treated steel sheet according to the embodiment. FIG. 7 is a flow chart showing an example of a flow of a manufacturing method of a surface-treated steel sheet according to the embodiment.
[0011] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings. In this specification and drawings, components having substantially the same functional configurations are designated by the same reference numerals, and redundant explanations will be omitted.
[0012] <Overall Configuration of Surface-Treated Steel Sheet> First, the overall configuration of the surface-treated steel sheet according to this embodiment will be described with reference to Fig. 1. Fig. 1 is an explanatory view schematically showing the structure of the surface-treated steel sheet according to this embodiment.
[0013] As shown in Figure 1, the surface-treated steel sheet 1 according to this embodiment includes a steel sheet 10, a plating layer 20, a chromium-containing composite layer 30, and a coating film 40. Such a surface-treated steel sheet 1 can be suitably used as a material for fuel tanks of various automobiles (particularly motorcycles).
[0014] Although FIG. 1 illustrates a case in which the plating layer 20, the chromium-containing composite layer 30, and the coating film 40 are provided on one surface of the steel sheet 10, the plating layer 20, the chromium-containing composite layer 30, and the coating film 40 may be provided on both surfaces of the steel sheet 10.
[0015] [Regarding the Steel Plate 10] The steel plate 10 is the base material of the surface-treated steel plate 1 according to this embodiment, and various steel plates can be used depending on the strength (e.g., tensile strength) required of the surface-treated steel plate 1. Examples of such steel plates include ordinary steel, low-carbon steel, and high-strength steel.
[0016] However, when manufacturing a fuel tank, which is one of the important applications of the surface-treated steel sheet 1 according to this embodiment, a high degree of workability is required for the steel sheet used as the raw material. Therefore, it is preferable to use IF steel, which has excellent workability, as the steel sheet 10 according to this embodiment, and furthermore, it is more preferable to use a steel sheet containing several ppm or more of boron (B) in order to ensure airtightness after welding, secondary workability, etc.
[0017] The thickness of the steel plate 10 may also be set appropriately depending on the strength required of the surface-treated steel plate 1 and the allowable mass of the article manufactured by processing the surface-treated steel plate 1, etc.
[0018] [Regarding the plating layer 20] The plating layer 20 in the surface-treated steel sheet 1 is a layer provided to ensure the corrosion resistance of the base material, the steel sheet 10. The plating layer 20 according to this embodiment is located on at least one surface of the steel sheet 10, and is a plating layer containing zinc (Zn) and nickel (Ni).
[0019] By providing the plating layer 20 containing zinc and nickel, the plating layer 20 exhibits excellent resistance weldability, workability, and corrosion resistance (particularly, gasoline resistance). In the plating layer 20, the Ni content is preferably within a range of 5 to 15 mass %, with the remainder being Zn and impurities.
[0020] By setting the Ni content to 5% by mass or more, it is possible to further improve corrosion resistance without causing a decrease in resistance weldability and workability. The Ni content is more preferably 8% by mass or more. On the other hand, by setting the Ni content to 15% by mass or less, it is possible to further suppress the occurrence of large cracks in the plating layer 20 and further ensure the adhesion of the plating layer 20. The Ni content is more preferably 13% by mass or less.
[0021] The coating weight of the plating layer 20 is 2 to 50 g / m per side. 2 The coating weight of the plating layer 20 is within the range of 2 g / m 2 By setting the coating weight to 5 g / m or more, it is possible to fully exhibit the various properties of the plating layer 20, such as resistance weldability, workability, and corrosion resistance. 2 On the other hand, when the coating weight of the plating layer 20 is 50 g / m 2 By setting the coating weight of the plating layer 20 to 40 g / m or less, it is possible to achieve resistance weldability, workability, and corrosion resistance in a favorable state. 2 The following is the result.
[0022] The deposition mass of the plating layer 20 can be calculated from the difference in mass before and after physical or chemical removal of a known area of the plating layer 20 from the steel sheet 10. The method for removing the plating layer 20 from the steel sheet 10 is not particularly limited, but examples of physical methods include blasting, and examples of chemical methods include acid dissolution treatment. The Ni content of the plating layer 20 can be determined by measuring the plating layer 20 removed from the steel sheet 10 as described above using an X-ray fluorescence analyzer.
[0023] [Regarding the chromium-containing composite layer 30] The chromium-containing composite layer 30 according to this embodiment is located on the plating layer 20 and is a composite layer containing at least chromium (Cr). The chromium-containing composite layer 30 improves the adhesion between the plating layer 20 described above and the coating film 40 described below, and also contributes to improving the corrosion resistance of the surface-treated steel sheet 1.
[0024] The amount of the chromium-containing composite layer 30 deposited is 10 to 200 mg / m in terms of metal Cr. 2 The deposition amount of the chromium-containing composite layer 30 is 10 mg / m 2 If the coating weight of the chromium-containing composite layer 30 is less than 10 mg / m, the coating weight of the chromium-containing composite layer 30 becomes too small, making it difficult to achieve the effect of improving adhesion as described above. 2This makes it possible to improve the adhesion between the plating layer 20 and the coating film 40 described below. The coating amount of the chromium-containing composite layer 30 is preferably 20 mg / m 2 More preferably, 30 mg / m 2 That's all.
[0025] On the other hand, the deposition amount of the chromium-containing composite layer 30 is 200 mg / m 2 If the adhesion amount of the chromium-containing composite layer 30 exceeds 200 mg / m, the adhesion amount of the chromium-containing composite layer 30 becomes too large, and the coating film 40 described below may easily peel off. 2 By satisfying the above condition, it is possible to stably improve the adhesion between the plating layer 20 and the coating film 40 described later. The coating amount of the chromium-containing composite layer 30 is preferably 150 mg / m 2 or less, more preferably 100 mg / m 2 The following is the result.
[0026] In the surface-treated steel sheet 1 according to this embodiment, a layer satisfying the following conditions is defined as the chromium-containing composite layer 30. For example, when a depth profile relating to the distribution of elements is obtained from the surface of the coating film 40 (described below) by radio frequency glow discharge optical emission spectrometry (RF-GD-OES), the chromium-containing composite layer 30 can be identified from the chromium depth profile. That is, when the position where the intensity of elemental chromium is maximum in the depth profile of chromium located between the coating film 40 and the plating layer 20 is defined as the peak intensity position, the position where the peak intensity of chromium is halved on the coating film 40 side can be defined as the interface position of the chromium-containing composite layer 30 on the coating film 40 side, and the position where the peak intensity of chromium is halved on the plating layer 20 side can be defined as the interface position of the chromium-containing composite layer 30 on the plating layer 20 side.
[0027] The RF-GD-OES measurement may be carried out using a glow discharge optical emission surface analyzer (for example, a Marcus-type high-frequency glow discharge optical emission surface analyzer GD-Profiler 2 manufactured by Horiba Jobin Yvon K.K.) under conditions of a gas replacement time of 30 seconds, a pre-sputtering time of 30 seconds, a pressure of 600 Pa, and an output of 35 W, until the intensity of the spectrum of iron derived from the underlying steel is detected.
[0028] The deposition weight of the chromium-containing composite layer 30 can be calculated from a calibration curve that shows the relationship between the fluorescent X-ray intensity and the deposition weight of chromium, for example, by quantitative analysis using fluorescent X-ray analysis. The deposition weight of the chromium-containing composite layer 30 can also be calculated by analyzing an aqueous solution in which the chromium-containing composite layer 30 is dissolved using inductively coupled plasma (ICP) emission spectroscopy.
[0029] Here, when determining the deposition amount of the chromium-containing composite layer 30 from a surface-treated steel sheet that has already been processed into various parts such as a fuel tank, a test piece can be cut from a portion of the part of interest that has not been subjected to joining processes such as welding, drawing, bending, or other processes, and used as the analysis target. In this case, the size of the cut test piece can be, for example, approximately 50 x 50 mm when the test piece is in a flat plate shape. Using a portion of the obtained test piece, measurement by RF-GD-OES as described above is performed, and the portion of the test piece corresponding to the chromium-containing composite layer 30 is identified. Then, X-ray fluorescence analysis or ICP atomic emission spectroscopy can be performed on the portion of the obtained test piece that corresponds to the chromium-containing composite layer 30.
[0030] The detailed configuration of the chromium-containing composite layer 30 will be described later.
[0031] [Regarding the coating film 40] The coating film 40 according to this embodiment is located on the chromium-containing composite layer 30 and is a resin layer containing an epoxy resin, an isocyanate resin, and silica particles. The coating film 40 preferably further contains polyethylene wax in addition to the above components. By providing the coating film 40, the surface-treated steel sheet 1 according to this embodiment exhibits excellent corrosion resistance, processability, and electrodeposition coatability.
[0032] <Epoxy Resin> The epoxy resin contained in the coating film 40 according to this embodiment is a resin that functions as a binder resin. By containing an epoxy resin in the coating film 40, the water resistance and alkali resistance of the coating film are improved, and adhesion to other layer structures is also improved. In the coating film 40 according to this embodiment, it is preferable to use, for example, a bisphenol A-type epoxy resin as the epoxy resin.
[0033] The number average molecular weight of the epoxy resin contained in the coating film 40 according to this embodiment is preferably within the range of 300 to 100,000.
[0034] By setting the number average molecular weight of the epoxy resin to 300 or more, the resin can be sufficiently polymerized by a crosslinking reaction, thereby further improving the corrosion resistance of the coating film. The number average molecular weight of the epoxy resin is more preferably 1,000 or more, and even more preferably 2,000 or more. On the other hand, by setting the number average molecular weight of the epoxy resin to 100,000 or less, the resin can be sufficiently polymerized by a crosslinking reaction, thereby further improving the corrosion resistance of the coating film. The number average molecular weight of the epoxy resin is more preferably 20,000 or less, and even more preferably 10,000 or less.
[0035] Furthermore, among epoxy resins having a number-average molecular weight within the above range, it is even more preferable to use those having an epoxy equivalent in the range of 1000 to 3500. By setting the epoxy equivalent of the epoxy resin to 1000 or more, it is possible to more appropriately crosslink the epoxy resin and further improve the corrosion resistance of the coating film. The epoxy equivalent of the epoxy resin is more preferably 1500 or more, and even more preferably 2000 or more. On the other hand, by setting the epoxy equivalent of the epoxy resin to 3500 or less, it is possible to suppress excessive polymerization of the epoxy resin, thereby maintaining the processability of the coating film 40 and further improving the corrosion resistance of the coating film. The epoxy equivalent of the epoxy resin is more preferably 3000 or less, and even more preferably 2500 or less.
[0036] <Isocyanate Resin> The isocyanate resin contained in the coating film 40 according to this embodiment is a resin that functions as a curing agent, and is able to appropriately cure the coating film 40 to exhibit excellent corrosion resistance, processability, and adhesion. Here, the isocyanate resin according to this embodiment refers to a resin having an isocyanate group or a low-molecular-weight compound having an isocyanate group, and examples of such isocyanate resins include polyisocyanate compounds and blocked polyisocyanate compounds.
[0037] Examples of the polyisocyanate compound include an aliphatic or alicyclic diisocyanate compound, an aromatic diisocyanate compound, and a triisocyanate compound.
[0038] Examples of aliphatic or alicyclic diisocyanate compounds include hexamethylene diisocyanate, isophorone diisocyanate, hydrogenated diphenylmethane diisocyanate, etc. Examples of aromatic diisocyanate compounds include tolylene diisocyanate, diphenylmethane-4,4'-diisocyanate, etc. Examples of triisocyanate compounds include adducts of 1 mole of trimethylolpropane and 3 moles of the above diisocyanates, and trimers of diisocyanates such as hexamethylene diisocyanate and tolylene diisocyanate.
[0039] The blocked polyisocyanate compound is a polyisocyanate compound such as those exemplified above that is blocked with a blocking agent. Preferably, the blocking agent is one that, when added to an isocyanate group, produces an adduct that is stable at room temperature and dissociates to regenerate free isocyanate groups when the coating film is baked.
[0040] Examples of such blocking agents include lactam-based blocking agents, oxime-based blocking agents, alcohol-based blocking agents, phenol-based blocking agents, and ester-based blocking agents.
[0041] Here, examples of lactam-based blocking agents include ε-caprolactam and γ-butyrolactam. Examples of oxime-based blocking agents include methyl ethyl ketoxime and cyclohexanone oxime. Examples of alcohol-based blocking agents include methanol, ethanol, and isobutyl alcohol. Examples of phenol-based blocking agents include phenol, p-tert-butylphenol, and cresol. Examples of ester-based blocking agents include ethyl acetoacetate and methyl acetoacetate. Among the above-mentioned blocking agents, methyl ethyl ketoxime and ethyl acetoacetate are particularly preferred, from the viewpoints that they dissociate particularly at low temperatures and are stable during storage of the coating material for forming a coating film.
[0042] In the coating film 40 according to this embodiment, the polyisocyanate compounds and blocked polyisocyanate compounds described above can be used alone or in combination of two or more. The compounds exemplified above are merely examples of isocyanate resins, and isocyanate resins other than those described above can also be used.
[0043] <Silica Particles> The silica particles contained in the coating film 40 according to this embodiment are components contained to prevent components in the coating film 40 from eluting out of the coating film, while further improving the corrosion resistance of the coating film 40. Examples of such silica particles include fumed silica and colloidal silica. At least one of these silica particles is used in the coating film 40 according to this embodiment.
[0044] Here, the average particle size of the fumed silica is preferably within the range of 5 to 40 nm. By setting the average particle size of the fumed silica to 5 nm or more, it is possible to further improve the corrosion resistance and adhesion of the coating film 40. The average particle size of the fumed silica is more preferably 7 nm or more. On the other hand, by setting the average particle size of the fumed silica to 40 nm or less, it is possible to further improve the corrosion resistance while maintaining the smoothness of the coating film 40. The average particle size of the fumed silica is more preferably 16 nm or less.
[0045] Furthermore, the average particle size of the colloidal silica is preferably within the range of 5 to 200 nm. By setting the average particle size of the colloidal silica to 5 nm or more, it is possible to further improve the corrosion resistance and adhesion of the coating film 40. The average particle size of the colloidal silica is more preferably 9 nm or more, and even more preferably 12 nm or more. On the other hand, by setting the average particle size of the colloidal silica to 200 nm or less, it is possible to further improve the corrosion resistance while maintaining the smoothness of the coating film 40. The average particle size of the colloidal silica is more preferably 60 nm or less, and even more preferably 22 nm or less.
[0046] <Polyethylene Wax> The polyethylene wax contained in the coating film 40 according to this embodiment functions as a lubricant and further improves the workability of the surface-treated steel sheet 1 according to this embodiment. In particular, it is preferable to use, as this polyethylene wax, a polyethylene wax having a density of 0.94 or more, a molecular weight in the range of 1,000 to 10,000, and an acid value of 15 KOHmg / g or less. By using a polyethylene wax having the above-mentioned density, molecular weight, and acid value, it is possible to further improve the workability of the surface-treated steel sheet 1.
[0047] Furthermore, in addition to the polyethylene wax, the coating film 40 according to this embodiment may contain various lubricants such as polyolefin-based lubricants, carboxylic acid ester-based lubricants, metal carboxylic acid salts, and polyalkylene glycol-based lubricants, as well as various lubricant powders such as molybdenum disulfide, silicone compounds, and fluorine compounds.
[0048] <Contents of the Above Components> In the coating film 40 according to the present embodiment, the contents of the epoxy resin, isocyanate resin, silica particles, and polyethylene wax preferably satisfy the following conditions: the epoxy resin content is 30.0 mass % or more relative to the coating solid content (i.e., relative to the total mass of the coating film 40), the isocyanate resin content is 0.10 to 2.00 in mass ratio relative to the epoxy resin, the silica particle content is 5.0 to 50.0 mass % relative to the coating solid content (i.e., relative to the total mass of the coating film 40), and the polyethylene wax content is 0.1 to 10.0 mass % relative to the coating solid content (i.e., relative to the total mass of the coating film 40), and the epoxy resin, isocyanate resin, silica particles, and polyethylene wax are preferably contained in a total amount of 100 mass % or less.
[0049] By setting the epoxy resin content to 30.0% by mass or more relative to the total mass of the coating film solids (i.e., the coating film 40), it is possible to suppress embrittlement of the coating film 40 and further improve the processing adhesion of the coating film 40. The epoxy resin content is more preferably 45.0% by mass or more, and even more preferably 50.0% by mass or more, relative to the coating film solids.
[0050] By setting the mass ratio of the isocyanate resin to the epoxy resin to be 0.10 or more, the epoxy resin and the isocyanate resin can be crosslinked in a favorable state, thereby achieving a coating film with excellent corrosion resistance. The mass ratio of the isocyanate resin to the epoxy resin is more preferably 0.15 or more, and even more preferably 0.20 or more. On the other hand, by setting the mass ratio of the isocyanate resin to the epoxy resin to be 2.00 or less, the water resistance and alkali resistance of the coating film 40 can be maintained while further improving the adhesion of the coating film 40. The mass ratio of the isocyanate resin to the epoxy resin is more preferably 0.90 or less, and even more preferably 0.50 or less.
[0051] By setting the content of silica particles to 5.0% by mass or more relative to the total mass of the coating solids (i.e., the coating 40), it is possible to further improve the corrosion resistance of the coating 40. The content of silica particles is more preferably 18.0% by mass or more, and even more preferably 23.0% by mass or more, relative to the coating solids. On the other hand, by setting the content of silica particles to 50.0% by mass or less, relative to the total mass of the coating solids, it is possible to prevent a decrease in the processing adhesion of the coating 40. The content of silica particles is more preferably 38.0% by mass or less, and even more preferably 33.0% by mass or less, relative to the coating solids.
[0052] By setting the polyethylene wax content to 0.1% by mass or more relative to the total mass of the coating solids (i.e., the coating 40), it is possible to reduce the frictional resistance of the surface of the coating 40 and prevent peeling of the coating during processing. The polyethylene wax content is more preferably 1.0% by mass or more, and even more preferably 1.5% by mass or more, relative to the coating solids. On the other hand, by setting the polyethylene wax content to 10.0% by mass or less relative to the total mass of the coating solids, it is possible to prevent the occurrence of shrinkage unevenness of the polyethylene wax and achieve a coating 40 with excellent appearance. The polyethylene wax content is more preferably 3.0% by mass or less, and even more preferably 2.5% by mass or less, relative to the coating solids.
[0053] <<Regarding Other Components>> In addition to the components described above, the coating film 40 according to this embodiment may further contain a resol-type phenolic resin. By further containing a resol-type phenolic resin in the coating film 40, the coating film formation reaction can be promoted at lower temperatures (for example, a maximum temperature of approximately 100 to 130°C). In this case, the content of the resol-type phenolic resin relative to the content of the isocyanate resin is preferably, for example, within a range of 0.1 to 10.0 in terms of mass ratio. This makes it possible to promote the coating film formation reaction at lower temperatures while suppressing a decrease in the alkali resistance of the coating film 40.
[0054] Furthermore, the coating film 40 according to this embodiment may further contain, in addition to the components described above, an anti-rust pigment, an extender pigment, a coloring pigment, an anti-rust agent, a dispersion stabilizer, and the like.
[0055] <<About Thickness>> In the coating film 40 according to this embodiment, the thickness of the coating film 40 is within the range of 0.5 to 2.0 μm. If the thickness of the coating film 40 is less than 0.5 μm, the coating film 40 is too thin, and the surface-treated steel sheet 1 cannot exhibit sufficient corrosion resistance. By making the thickness of the coating film 40 0.5 μm or more, the surface-treated steel sheet 1 can exhibit excellent corrosion resistance even when exposed to various fuels including gasoline. The thickness of the coating film 40 is preferably 0.6 μm or more, and more preferably 0.7 μm or more.
[0056] On the other hand, if the thickness of the coating film 40 exceeds 2.0 μm, this is not preferred because it may deteriorate the spot weldability and appearance of the surface-treated steel sheet 1. By setting the thickness of the coating film 40 to 2.0 μm or less, it is possible to suppress deterioration in spot weldability and appearance while achieving excellent corrosion resistance. The thickness of the coating film 40 is preferably 1.5 μm or less.
[0057] Here, the thickness of the coating film 40 can be measured by direct observation of the cross section. Specifically, the surface-treated steel sheet of interest is embedded in a room-temperature drying epoxy resin so that the cross section in the thickness direction can be observed, and the embedded surface is mechanically polished and further polished to a mirror finish, and then observed with a scanning electron microscope (SEM). The thickness can be measured at any number of positions (e.g., 10 positions), and the average value of the obtained thicknesses can be used as the thickness of the coating film 40. In this case, the coating film 40 may be identified by combining this with elemental mapping using energy dispersive X-ray spectrometry (EDS) or an electron probe microanalyzer (EPMA).
[0058] Furthermore, the film thickness can be converted into the thickness of the coating film 40 per unit sputtering time by measuring the depth profile from the surface side of the surface-treated steel sheet to the steel sheet side using radio frequency glow discharge optical emission spectroscopy (RF-GD-OES) and comparing the sputtering time corresponding to the depth profile of the coating film 40 with the thickness of the coating film 40 observed by SEM from the cross section described above.
[0059] In addition, in a depth profile obtained by radio frequency glow discharge optical emission spectroscopy, the position of the interface of the coating film 40 on the chromium-containing composite layer 30 side can also be grasped by the method described above. That is, in the depth profile of chromium, attention is focused on an intensity peak within the range corresponding to the chromium-containing composite layer 30, and the position where the chromium intensity is reduced to half of the peak value from the position of the peak toward the coating film 40 can be determined to be the position of the interface between the coating film 40 and the chromium-containing composite layer 30.
[0060] Here, when identifying the details of the coating film 40 from a surface-treated steel sheet that has already been processed into various parts such as a fuel tank, a test piece can be cut out from a portion of the part of interest that has not been subjected to joining processes such as welding or processing processes such as drawing or bending, and used as the object of analysis. In this case, the size of the test piece to be cut out can be the size of the test piece when made into a flat plate, for example, about 50 x 50 mm. Various measurements can then be carried out using the obtained test piece.
[0061] For example, when determining the content of the above-mentioned components in a portion of a test piece corresponding to the coating film 40, the portion corresponding to the coating film 40 can be analyzed by Fourier transform infrared spectroscopy (FT-IR) and the components can be determined based on whether or not peaks derived from epoxy groups or isocyanate groups are detected in the resulting infrared absorption spectrum. If peaks derived from epoxy groups are detected in the resulting infrared absorption spectrum, it can be determined that the coating film 40 of interest contains an epoxy resin. Furthermore, if peaks derived from isocyanate groups are detected in the resulting infrared absorption spectrum, it can be determined that the coating film 40 of interest contains an isocyanate resin.
[0062] The contents of the epoxy resin and isocyanate resin can be determined by preparing an epoxy resin / isocyanate resin mixed coating film in advance, the mixing ratio of which is known, and creating a calibration curve of the peak intensity of the peak derived from the epoxy group and the peak intensity of the peak derived from the isocyanate group for the mixed coating film by FT-IR.Then, in the analysis by FT-IR obtained as described above, the contents of the epoxy resin and isocyanate resin can be specified from the peak intensity of each peak obtained.
[0063] The number average molecular weight of the epoxy resin can be determined as follows: A sample is taken from the portion of the test piece corresponding to the coating film 40, and the molecular structure of the resin is divided into units and analyzed by field desorption-mass spectrometry (FD-MS) to determine the molecular weight distribution.
[0064] The presence or absence of polyethylene wax can be determined by immersing a test piece in a heated solvent (more specifically, 2-butanone heated to approximately 80°C) to dissolve and separate the polyethylene wax in the solvent, analyzing the resulting extract by FT-IR, and determining whether or not a peak derived from a methylene group is detected in the resulting infrared absorption spectrum. If a peak derived from a methylene group is detected in the resulting infrared absorption spectrum, it can be determined that the coating film 40 of interest contains polyethylene wax. The content ratio of polyethylene wax can be determined from the difference in mass between before and after extraction of the polyethylene wax as described above.
[0065] Furthermore, the presence or absence of silica particles can be identified, for example, by confirming the presence of elements Si and O by elemental analysis such as X-ray fluorescence analysis for a portion of the test piece corresponding to the coating film 30, and then analyzing the portion corresponding to the coating film 30 by FT-IR, based on whether or not a peak derived from an Si—O bond is detected in the resulting infrared absorption spectrum. If the presence of elements Si and O is confirmed by elemental analysis and a peak derived from an Si—O bond is detected in the infrared absorption spectrum, it can be determined that the coating film 30 of interest contains silica particles.
[0066] The overall configuration of the surface-treated steel sheet 1 according to this embodiment has been described above with reference to FIG.
[0067] <Regarding the first composite layer 50> Next, the first composite layer of the surface-treated steel sheet 1 according to this embodiment will be described in detail with reference to Fig. 2 and Fig. 3. Fig. 2 and Fig. 3 are explanatory diagrams for describing the first composite layer in the surface-treated steel sheet according to this embodiment.
[0068] In the surface-treated steel sheet 1 according to this embodiment, a first composite layer is located between the steel sheet 10 and the plating layer 20. Here, Fig. 2 shows an enlarged schematic view of the layer structure of the surface-treated steel sheet 1 in the region R surrounded by the dashed line in Fig. 1 (in other words, the layer structure in the vicinity of the interface between the steel sheet 10 and the plating layer 20).
[0069] In Fig. 2, the layer located between the steel sheet 10 and the plating layer 20 is the first composite layer 50. This first composite layer 50 is a composite layer containing iron (Fe) derived from the steel sheet 10 and Zn and Ni derived from the plating layer 20. The first composite layer 50 is a layer produced by interdiffusion and compounding of the Fe derived from the steel sheet 10 and the Zn and Ni derived from the plating layer 20 through a manufacturing method described below.
[0070] The presence of the first composite layer 50 improves the adhesion between the steel sheet 10 and the plating layer 20. In combination with the detailed configuration of the chromium-containing composite layer 30, which will be described in detail below, the surface-treated steel sheet 1 according to this embodiment can further improve the adhesion and corrosion resistance of the coating after forming.
[0071] Here, the average thickness of the first composite layer 50 (thickness d1 in FIG. 2) is preferably within the range of 0.01 to 0.50 μm. By setting the average thickness d1 of the first composite layer 50 to 0.01 μm or more, it is possible to further improve the adhesion between the steel sheet 10 and the plating layer 20. The average thickness d1 of the first composite layer 50 is more preferably 0.03 μm or more, and even more preferably 0.05 μm or more. On the other hand, by setting the average thickness d1 of the first composite layer 50 to 0.50 μm or less, it is possible to obtain sufficient formability. The average thickness d1 of the first composite layer 50 is more preferably 0.40 μm or less, and even more preferably 0.30 μm or less.
[0072] Here, a method for identifying the first composite layer 50 and a method for measuring the average thickness will be described in detail with reference to Fig. 3. In this embodiment, with regard to the method for identifying the first composite layer 50 and the method for measuring the average thickness, attention is focused on the depth profiles of iron, zinc, and nickel measured by radio frequency glow discharge optical emission spectroscopy (RF-GD-OES) from near the interface of the plating layer 20 to near the interface of the steel sheet 10.
[0073] That is, in the depth profile of iron, zinc, and nickel obtained by RF-GD-OES from near the interface of the plating layer 20 to near the interface of the steel sheet 10, the position where the peak of zinc or nickel, an element derived from the plating layer 20, is reduced by half is defined as the position of the interface of the plating layer 20 side of the first composite layer 50. In this case, of the positions defined by zinc and the positions defined by nickel, the position closer to the steel sheet 10 is defined as the position of the interface of the plating layer 20 side of the first composite layer 50. For example, in the example shown in FIG. 3 , if the peak intensity of Zn or Ni closer to the steel sheet 10 is Ia, the position corresponding to the sputtering time t1 at which the intensity of the element of interest becomes 0.5 × Ia is the position of the interface of the first composite layer 50 on the plating layer 20 side.
[0074] In this embodiment, the position where the peak of iron, an element derived from the steel sheet 10, is reduced by half is defined as the position of the interface of the first composite layer 50 on the steel sheet 10 side. For example, in the example shown in Fig. 3, when the peak intensity of Fe is Ib, the position corresponding to the sputtering time t2 at which the intensity of Fe becomes 0.5 x Ib is the position of the interface of the first composite layer 50 on the steel sheet 10 side.
[0075] Based on the above definitions, the range located between the two defined interfaces is the range of the first composite layer 50. In the example shown in Figure 3, the position corresponding to sputtering time t1 to t2 is the position of the first composite layer 50, and the thickness corresponding to sputtering time t1 to t2 is the average thickness of the first composite layer 50. Here, since knowledge regarding the thickness per unit sputtering time can be obtained from the time required to sputter a layer whose average thickness is known, it is possible to convert the sputtering time into thickness.
[0076] When identifying the first composite layer 50 from a surface-treated steel sheet that has already been processed into various parts such as a fuel tank, a test piece may be cut out from a portion of the part of interest that has not been subjected to joining processes such as welding or processing processes such as drawing or bending, and used as the object of analysis. In this case, the size of the test piece to be cut out may be the size of the test piece when it is in a flat plate shape, for example, about 50 × 50 mm.
[0077] <Detailed Structure of Chromium-Containing Composite Layer 30> Next, the detailed structure of the chromium-containing composite layer 30 according to this embodiment will be described with reference to Fig. 4 and Fig. 5. Fig. 4 and Fig. 5 are explanatory diagrams for describing the chromium-containing composite layer in the surface-treated steel sheet according to this embodiment.
[0078] As will be described in detail in the manufacturing method below, the chromium-containing composite layer 30 according to this embodiment is a layer produced by combining a portion of the plating layer, a chromate film formed on the plating layer, and a portion of the coating film formed on the chromate film through the steps of the manufacturing method.
[0079] 4, the chromium-containing composite layer 30 has a second composite layer 60 located on the plating layer 20 side and a third composite layer 70 located on the coating film 40 side. The second composite layer 60 is a composite layer containing chromium (Cr), Zn, and Ni, and the third composite layer 70 is a composite layer containing silicon (Si), nitrogen (N), and Cr.
[0080] As can be inferred from the fact that the second composite layer 60 is a composite layer containing Cr, Zn, and Ni, it is a composite layer derived from the Cr present in the chromate film before being compounded and the Zn and Ni present in the plating layer before being compounded.
[0081] Furthermore, as can be inferred from the fact that the third composite layer 70 is a composite layer containing Si, N, and Cr, it is a composite layer derived from the Cr present in the chromate film before being compounded, and the Si contained in the silica particles and the N contained in the isocyanate resin in the coating film before being compounded.
[0082] As shown in FIG. 4, a layer 80 different from the second composite layer 60 and the third composite layer 70 may be provided between these two composite layers.
[0083] Possible examples of the layer 80 that may be present between the second composite layer 60 and the third composite layer 70 include a layer derived from a chromate film that remains uncomposite, and a composite layer containing Cr, Zn, Ni, Si, and N (in other words, a layer in which the second composite layer 60 and the third composite layer 70 are further combined). The chromium-containing composite layer 30 may be a layer composed of the second composite layer 60 and the third composite layer 70, without the presence of the layer 80 described above. The second composite layer 60 and the third composite layer 70 may also overlap.
[0084] The presence of the second composite layer 60 and the third composite layer 70 as described above improves the adhesion between the chromium-containing composite layer 30 and the plating layer 20, and the adhesion between the chromium-containing composite layer 30 and the coating film 40. In combination with the first composite layer 50 described above, the surface-treated steel sheet 1 according to this embodiment can further improve the adhesion and corrosion resistance of the coating after forming.
[0085] Here, the average thickness of the second composite layer 60 (thickness d2 in FIG. 4) is preferably within the range of 0.1 to 1.5 μm. By setting the average thickness d2 of the second composite layer 60 to 0.1 μm or more, it is possible to further improve the adhesion between the plating layer 20 and the chromium-containing composite layer 30. The average thickness d2 of the second composite layer 60 is more preferably 0.2 μm or more, and even more preferably 0.5 μm or more. On the other hand, by setting the average thickness d2 of the second composite layer 60 to 1.5 μm or less, it is possible to appropriately distribute the stress applied to the steel sheet during forming. The average thickness d2 of the second composite layer 60 is more preferably 1.2 μm or less, and even more preferably 1.0 μm or less.
[0086] Furthermore, the average thickness of the third composite layer 70 (thickness d3 in FIG. 4 ) is preferably within the range of 0.1 to 1.5 μm. By setting the average thickness d3 of the third composite layer 70 to 0.1 μm or more, it is possible to further improve the adhesion between the chromium-containing composite layer 30 and the coating film 40. The average thickness d3 of the third composite layer 70 is more preferably 0.2 μm or more, and even more preferably 0.5 μm or more. On the other hand, by setting the average thickness d3 of the third composite layer 70 to 1.5 μm or less, it is possible to appropriately distribute the stress applied to the steel sheet during forming. The average thickness d3 of the third composite layer 70 is more preferably 1.2 μm or less, and even more preferably 1.0 μm or less.
[0087] Furthermore, the ratio (d2 / d1) of the average thickness d2 of the second composite layer to the average thickness d1 of the first composite layer is preferably 0.2 to 150.0, and the ratio (d3 / d1) of the average thickness d3 of the third composite layer to the average thickness d1 of the first composite layer is preferably 0.2 to 150.0.
[0088] When the ratio (d2 / d1) is 0.2 or more, it is possible to further improve the adhesion between the plating layer 20 and the chromium-containing composite layer 30. The ratio (d2 / d1) is more preferably 0.5 or more, and even more preferably 1.7 or more. On the other hand, when the ratio (d2 / d1) is 150.0 or less, it is possible to appropriately distribute the stress applied to the steel sheet during forming. The ratio (d2 / d1) is more preferably 40.0 or less, and even more preferably 20.0 or less.
[0089] When the ratio (d3 / d1) is 0.2 or more, it is possible to further improve the adhesion between the chromium-containing composite layer 30 and the coating film 40. The ratio (d3 / d1) is more preferably 0.5 or more, and even more preferably 1.7 or more. On the other hand, when the ratio (d3 / d1) is 150.0 or less, it is possible to appropriately distribute the stress applied to the steel sheet during forming. The ratio (d3 / d1) is more preferably 40.0 or less, and even more preferably 20.0 or less.
[0090] Here, a method for distinguishing the second composite layer 60 and the third composite layer 70 and a method for measuring the average thicknesses d2 and d3 of the composite layers will be described in detail with reference to FIGS.
[0091] In this embodiment, with regard to the method for identifying the second composite layer 60 and the method for measuring the average thickness, attention is focused on the depth profile of chromium, zinc, and nickel measured by radio frequency glow discharge optical emission spectroscopy (RF-GD-OES) from near the interface of the coating film 40 to near the interface of the plating layer 20.
[0092] That is, in the depth profile of chromium, zinc, and nickel obtained by RF-GD-OES from near the interface of the coating film 40 to near the interface of the plating layer 20, the position where the peak of chromium, an element derived from the chromium-containing composite layer 30, is reduced by half is defined as the position of the interface of the second composite layer 60 on the plating layer 20 side. For example, in the example shown in Figure 5, if the peak intensity of Cr is Ic, the position corresponding to sputtering time t3 at which the intensity of Cr becomes 0.5 × Ic is the position of the interface of the second composite layer 60 on the plating layer 20 side.
[0093] In this embodiment, the position where the peak of zinc or nickel, an element derived from the plating layer 20, is reduced by half is defined as the position of the interface of the second composite layer 60 on the coating layer 40 side. In this case, of the positions defined by zinc and the positions defined by nickel, the position closer to the coating 40 side is defined as the position of the interface of the second composite layer 60 on the coating layer 40 side. For example, in the example shown in Figure 5, if the peak intensity of Zn or Ni closer to the coating 40 is Id, the position corresponding to the sputtering time t4 at which the intensity of the element of interest becomes 0.5 × Id is the position of the interface of the second composite layer 60 on the coating layer 40 side.
[0094] Based on the above definitions, the range located between the two defined interfaces is the range of the second composite layer 60. In the example shown in Figure 5, the position corresponding to sputtering times t3 to t4 is the position of the second composite layer 60, and the thickness corresponding to sputtering times t3 to t4 is the average thickness of the second composite layer 60. Here, since knowledge regarding the thickness per unit sputtering time can be obtained from the time required to sputter a layer with a known thickness, it is possible to convert the sputtering time into thickness.
[0095] Furthermore, in this embodiment, with regard to the method for identifying the third composite layer 70 and the method for measuring the average thickness, attention is focused on the depth profile of silicon and chromium measured by radio frequency glow discharge optical emission spectroscopy (RF-GD-OES) from near the interface of the coating film 40 to near the interface of the plating layer 20.
[0096] That is, in the depth profile of silicon and chromium obtained by RF-GD-OES from near the interface of the coating film 40 to near the interface of the plating layer 20, the position where the peak of silicon, an element derived from the coating film 40, is reduced by half is defined as the position of the interface of the third composite layer 70 on the plating layer 20 side. For example, in the example shown in Figure 6, when the peak intensity of Si is Ie, the position corresponding to the sputtering time t5 at which the Si intensity becomes 0.5 × Ie is the position of the interface of the third composite layer 70 on the plating layer 20 side.
[0097] In this embodiment, the position where the peak of chromium, an element derived from the chromium-containing composite layer 30, is reduced by half is defined as the position of the interface of the third composite layer 70 on the coating film 40 side. For example, in the example shown in Fig. 6, when the peak intensity of Cr is If, the position corresponding to the sputtering time t6 at which the intensity of Cr becomes 0.5 × If is the position of the interface of the third composite layer 70 on the coating film 40 side.
[0098] Based on the above definitions, the range located between the two defined interfaces is the range of the third composite layer 70. In the example shown in Figure 6, the position corresponding to sputtering times t5 to t6 is the position of the third composite layer 70, and the thickness corresponding to sputtering times t5 to t6 is the average thickness of the third composite layer 70. Here, since knowledge regarding the thickness per unit sputtering time can be obtained from the time required to sputter a layer with a known thickness, it is possible to convert the sputtering time into thickness.
[0099] When identifying the detailed structure of the chromium-containing composite layer 30 from a surface-treated steel sheet that has already been processed into various parts such as a fuel tank, a test piece may be cut out from a portion of the part of interest that has not been subjected to joining processes such as welding or processing processes such as drawing or bending, and used as the analysis target. In this case, the size of the test piece cut out may be the size of the test piece when made into a flat plate, for example, about 50 × 50 mm. The obtained test piece may then be used to carry out the above-mentioned measurements.
[0100] The surface-treated steel sheet according to this embodiment has been described in detail above with reference to FIGS.
[0101] (Regarding the manufacturing method of the surface-treated steel sheet) Next, the manufacturing method of the surface-treated steel sheet according to the present embodiment as described above will be described with reference to Fig. 7. Fig. 7 is a flow chart showing an example of the flow of the manufacturing method of the surface-treated steel sheet according to the present embodiment.
[0102] As shown in FIG. 7 , the method for producing a surface-treated steel sheet according to this embodiment includes a pretreatment step (step S11), an electroplating step (step S13), a cleaning step (step S15), an electrolytic chromate treatment step (step S17), a cleaning step (step S19), and a coating film formation step (step S21).
[0103] The pretreatment step (step S11) is a step for cleaning the surface of the steel sheet by subjecting the steel sheet, which serves as the base material, to various pretreatments, including alkaline degreasing, water washing, pickling, etc. There are no particular restrictions on the pretreatment step, and it is sufficient to follow a conventional treatment method.
[0104] The electroplating step (step S13) is a step of forming a plating layer on the surface of a steel sheet as a base material by electroplating. In this electroplating step, a plating bath containing components capable of realizing a desired plating composition (a plating bath containing Ni and, as necessary, other elements, with the balance being Zn) is prepared, and electroplating is performed using this plating bath and the steel sheet at a predetermined current density and for a predetermined current flow time.
[0105] The plating bath temperature is preferably 50 to 70°C. The current density is preferably 5 to 100 A / dm 2 The current application time is preferably 10 to 100 seconds, and more preferably 12 to 50 seconds.
[0106] As described above, in the electroplating step (step S13) according to this embodiment, a longer current application time is used compared to conventional zinc-nickel electroplating. This increases the immersion time of the steel sheet in the plating bath, resulting in increased diffusion of Fe in the steel sheet. This allows for more regions to be combined than usual, and the first composite layer 50 according to this embodiment can be formed with an appropriate thickness.
[0107] The plating deposition amount in this electroplating step is set to 2 to 50 g / m so that the deposition amount of the plating layer 20 as previously explained can be realized. 2 It is preferable that the range is within the range.
[0108] The cleaning step (step S15) is a step of subjecting the steel sheet after the electroplating step to a cleaning treatment. The cleaning step is not particularly specified, and may be performed according to a conventional treatment method.
[0109] The electrolytic chromate treatment step (step S17) is a step of performing an electrolytic chromate treatment on the steel sheet (more specifically, the steel sheet on which the plating layer has been formed) that has been subjected to the cleaning step.
[0110] The electrolytic bath for electrolytic chromate treatment is Cr 6+ The main component contains sulfuric acid and halogen ions, or the above components further contain SiO 2 and TiO 2 It is preferable to use inorganic colloids such as those containing metal ions such as Co and Zn. Cr ions are electrodeposited in a trivalent state using such an electrolytic chromate bath, and Cr 3+ The formation of a poorly soluble chromate film mainly composed of chromium makes it possible to prevent chromium from eluting into the treatment solution used for subsequent chemical conversion treatments and electrodeposition coatings on the surface-treated steel sheet.
[0111] The temperature of the electrolytic chromate bath is preferably 50 to 70°C. The current density is preferably 5 to 100 A / dm 2 The current application time is preferably 1 to 10 seconds, and more preferably 2 to 8 seconds.
[0112] In the method for producing a surface-treated steel sheet according to this embodiment, the chromate treatment is performed by electrolytic chromate treatment at the specific current density and current flow time as described above. This promotes dissolution of components from the pre-formed plating layer, and in combination with the coating film formation process described below, the chromium-containing composite layer 30 according to this embodiment is formed.
[0113] The amount of chromate film deposited in the electrolytic chromate treatment step is set to 10 to 200 mg / m in terms of metal Cr so that the amount of Cr deposited can be achieved as previously explained. 2 It is preferable that the range is within the range.
[0114] The cleaning step (step S19) is a step of cleaning the steel sheet after the electrolytic chromate treatment step. The cleaning step is not particularly specified, and may be performed according to a conventional treatment method.
[0115] The coating film forming step (step S21) is a step of performing a treatment for forming a coating film on the steel sheet (more specifically, the steel sheet on which the plating layer and the chromate film have been formed) that has been subjected to the cleaning step.
[0116] In this process, a paint for forming the coating film is prepared so as to realize the content of the components of the coating film 40 as described above. In such a paint, each of the components of the coating film 40 as described above is dissolved or dispersed in an organic solvent.
[0117] In the coating film forming step according to this embodiment, it is preferable to use a ketone organic solvent as the organic solvent. By adding the ketone organic solvent to the coating material in an amount of 40 mass% or more and adjusting the coating material solids concentration to 10 to 50 mass%, it becomes possible to easily form a uniform coating film.
[0118] Examples of such ketone organic solvents include methyl isobutyl ketone, acetone cyclohexanone, isophorone, etc., but other ketone organic solvents can also be used. However, when selecting such a solvent, it is important to avoid selecting a solvent that can react with the isocyanate resin.
[0119] The paint prepared as described above is applied to the surface of the steel sheet after the cleaning process by various methods such as roll coating, curtain flow coating, etc. At this time, it is preferable to appropriately adjust the thickness of the applied paint, taking into consideration the formation of the third composite layer 70, so that the thickness of the coating film 40 after drying is within the range of 0.5 to 2.0 μm.
[0120] Next, the steel sheet after coating with the paint is held, for example, at a maximum temperature in the range of 100 to 200°C for 10 to 60 seconds, thereby volatilizing the solvent in the paint and drying and solidifying the paint solids to form the coating film 40. During this heat treatment process, the components contained in the paint and the chromate film (and, in some cases, further components contained in the first composite layer and plating layer) thermally diffuse, ultimately forming the chromium-containing composite layer 30 as previously described.
[0121] By going through the above steps, the surface-treated steel sheet 1 according to this embodiment as previously described is manufactured.
[0122] The method for manufacturing a surface-treated steel sheet according to this embodiment has been described in detail above with reference to FIG.
[0123] The surface-treated steel sheet according to the present invention will be specifically described below with reference to examples and comparative examples. Note that the examples shown below are merely examples of the surface-treated steel sheet according to the present invention, and the surface-treated steel sheet according to the present invention is not limited to the examples below.
[0124] (1) Zinc-nickel plated steel sheet The plated steel sheet used was a cold-rolled steel sheet (manufactured by Nippon Steel Corporation) on which a zinc-nickel plating was formed by electroplating to have a predetermined nickel content. The coating weight is the coating weight per side. The plating layer of the zinc-nickel plated steel sheet was spray degreased for 5 seconds using a commercially available sodium orthosilicate alkaline cleaning solution, then rinsed with water and dried.
[0125] (2) Chemical conversion treatment and painting treatment Chromate chemical conversion treatment solution and paint were prepared. In the chromate chemical conversion treatment, electrolytic chromate treatment was performed at a solution temperature of 50 to 70°C and a current density of 5 to 100 A / dm 2 Electrolysis was carried out within the range of 1000 ppm for the times shown in Tables 1-1 to 1-3 below. Thereafter, each plated steel sheet was washed with water and dried.
[0126] In addition, the following epoxy resin, isocyanate resin, silica particles, and polyethylene wax were mixed in the specified proportions to prepare paints. The contents shown in Tables 1-1 to 1-3 are the contents in the coating film (solid content).
[0127] [Epoxy Resins] Epoxy Resin A: No. 1007 manufactured by Mitsubishi Chemical Corporation, molecular weight: 2900, epoxy equivalent: 1750-2200 Epoxy Resin B: No. 827 manufactured by Mitsubishi Chemical Corporation, molecular weight: 360, epoxy equivalent: 180-190 Epoxy Resin C: No. 1001 manufactured by Mitsubishi Chemical Corporation, molecular weight: 900, epoxy equivalent: 450-500 Epoxy Resin D: H-360 manufactured by DIC Corporation, molecular weight: 25000 Epoxy Resin E: No. 4250 manufactured by Mitsubishi Chemical Corporation, molecular weight: 60000, epoxy equivalent: 7500-8900
[0128] [Isocyanate resin] Isocyanate A: hexamethylene diisocyanate manufactured by Tosoh Corporation Isocyanate B: ethyl acetoacetate block compound
[0129] [Silica particles] <Fume silica> Fumed silica A: Aerosil 300 (average particle size: 7 nm) manufactured by Nippon Aerosil Co., Ltd. Fumed silica B: Aerosil 200 (average particle size: 12 nm) manufactured by Nippon Aerosil Co., Ltd. Fumed silica C: Aerosil R972CF (average particle size: 16 nm) manufactured by Nippon Aerosil Co., Ltd. Fumed silica D: Aerosil MOX80 (average particle size: 30 nm) manufactured by Nippon Aerosil Co., Ltd. Fumed silica E: Aerosil OX50 (average particle size: 40 nm) <Colloidal silica> Colloidal silica A: Snowtex N manufactured by Nissan Chemical Co., Ltd. (average particle size: 12 nm) Colloidal silica B: Snowtex ST-NXS manufactured by Nissan Chemical Co., Ltd. (average particle size: 5 nm) Colloidal silica C: Snowtex ST-NS manufactured by Nissan Chemical Co., Ltd. (average particle size: 9 nm) Colloidal silica D: Snowtex ST-N-40 (average particle size: 22 nm) manufactured by Nissan Chemical Industries, Ltd. Colloidal silica E: Snowtex ST-YL (average particle size: 60 nm) manufactured by Nissan Chemical Industries, Ltd. Colloidal silica F: Snowtex MP-2040 (average particle size: 200 nm) manufactured by Nissan Chemical Industries, Ltd. Colloidal silica G: Snowtex MP-454M (average particle size: 450 nm) manufactured by Nissan Chemical Industries, Ltd.
[0130] [Polyethylene wax] CERIDUST 3620 manufactured by Clariant Chemicals Co., Ltd.
[0131] The coating material prepared as described above was applied using a roll coater and dried and solidified by holding it at a maximum temperature (PMT) of 165 to 185°C for 10 to 60 seconds. The coating thickness after drying and solidification is shown in Tables 1-1 to 1-3.
[0132] For each of the surface-treated steel sheets obtained as described above, depth profiles of the elements Fe, Zn, Ni, Cr, Si, and N were measured by RF-GD-OES using the method previously described. This confirmed whether or not the specified elements were contained in each composite layer. The results obtained are shown in Tables 1-1 to 1-3.
[0133]
[0134]
[0135]
[0136] Furthermore, the obtained surface-treated steel sheets were evaluated for adhesion at the processed portion, corrosion resistance at the processed portion, corrosion resistance on a flat surface, and corrosion resistance after degreasing. The evaluation methods and evaluation criteria for each evaluation were as follows. The obtained results are summarized in Tables 2-1 to 2-3 below.
[0137] <Post-Processing Adhesion> Test specimens were cut from each surface-treated steel sheet and subjected to cylindrical cup drawing under the following conditions: punch diameter: 50 mmφ, punch shoulder R: 5 mm, blank diameter: 100 mmφ, drawing ratio: 2.0, and pressure: 1 ton. For the molded products obtained by the above cylindrical cup drawing, cross cuts were made in the barrel of the cylindrical cup, and then the molded products were immersed in boiling water for 1 hour to evaluate post-processing adhesion. The cross cuts were made in two opposing positions in the barrel of the cylindrical cup drawn part, midway between the rolling direction (L direction) of the steel sheet and the perpendicular direction (C direction) (positions at 45° from the L direction and C direction). The cross cuts were made starting at a height of 5 mm from the drawn end surface of the barrel, extending toward the bottom of the cylindrical cup, with one cut 40 mm long and two cuts perpendicular to each other at 90°. Two cross cuts were made on the barrel after drawing, and the peeled width of the coating film from the cut was measured, and the maximum peeled width was given a rating. A rating of 2 or higher was considered to be acceptable. [Evaluation criteria] Rating 5: 0.1 mm or less 4: More than 0.1 mm and less than 0.2 mm 3: More than 0.2 mm and less than 0.3 mm 2: More than 0.3 mm and less than 0.4 mm 1: More than 0.4 mm
[0138] <Corrosion resistance after processing> Test specimens were cut out from each surface-treated steel sheet, and after being subjected to a ball-head protrusion to a height of 7 mm using an Erichsen testing machine, a salt spray test (JIS Z 2371:2015) was conducted for 500 hours, and the area ratio of white rust occurring on the ball-head protrusion was evaluated. The end faces and back surfaces were sealed before evaluation. A score of 2 or higher was considered a pass. [Evaluation criteria] Score 5: 5% or less 4: More than 5% and 7% or less 3: More than 7% and 10% or less 2: More than 10% and 12% or less 1: More than 12%
[0139] <Flat surface corrosion resistance> Test specimens were cut out from each surface-treated steel sheet, and subjected to a salt spray test (JIS Z 2371:2015) for 500 hours, and evaluated based on the area ratio of white rust formation. The end faces and back surfaces were sealed before evaluation. A score of 2 or higher was considered a pass. [Evaluation criteria] Score 5: 1% or less 4: More than 1% and 3% or less 3: More than 3% and 5% or less 2: More than 5% and 10% or less 1: More than 10%
[0140] <Corrosion resistance after degreasing> Test specimens were cut out from each surface-treated steel sheet, and after spray degreasing using a commercially available sodium orthosilicate alkaline cleaning solution at 60°C for 2 minutes, a salt spray test (JIS Z 2371:2015) was performed for 500 hours, and the corrosion resistance was evaluated based on the area ratio of white rust on the flat surface. The end faces and back surfaces were sealed before evaluation. A score of 2 or higher was considered to be pass. [Evaluation criteria] Score 5: 5% or less 4: More than 5% and 7% or less 3: More than 7% and 10% or less 2: More than 10% and 12% or less 1: More than 12%
[0141]
[0142]
[0143]
[0144] As is clear from Tables 2-1 to 2-3 above, the surface-treated steel sheets corresponding to the examples of the present invention showed pass results for the adhesion of the processed part, the corrosion resistance of the processed part, the flat surface corrosion resistance, and the corrosion resistance after degreasing, while the surface-treated steel sheets corresponding to the comparative examples of the present invention showed fail results for at least one of the adhesion of the processed part, the corrosion resistance of the processed part, the flat surface corrosion resistance, and the corrosion resistance after degreasing.
[0145] For example, in Comparative Examples No. 1 and 8, the Cr deposition amount in the chromium-containing composite layer was outside the range of the present invention due to the current flow time in the electrolytic chromate treatment, so the processed part adhesion, processed part corrosion resistance, flat surface corrosion resistance, and post-degreasing corrosion resistance were unsatisfactory. In Comparative Examples No. 9 and 16, the Cr deposition amount in the chromium-containing composite layer was outside the range of the present invention due to the chromium concentration in the electrolytic bath used, so the processed part adhesion, processed part corrosion resistance, flat surface corrosion resistance, and post-degreasing corrosion resistance were unsatisfactory. In Comparative Examples No. 17 and 24, the roll coater conditions when applying the paint were inappropriate, so the coating film thickness was outside the range of the present invention, so the processed part adhesion, processed part corrosion resistance, flat surface corrosion resistance, and post-degreasing corrosion resistance were unsatisfactory.
[0146] In Comparative Example No. 98, the coating weight of the Zn—Ni plating layer was outside the range of the present invention, and therefore the adhesion of the processed portion, the corrosion resistance of the processed portion, the flat corrosion resistance, and the corrosion resistance after degreasing were unacceptable. In Comparative Example No. 99, the coating weight of the Zn—Ni plating layer was outside the range of the present invention, and therefore the adhesion of the processed portion was unacceptable.
[0147] In Comparative Example No. 100, the Cr deposition amount in the chromium-containing composite layer was outside the range of the present invention due to the chromium concentration in the electrolytic bath used, and therefore the processed portion corrosion resistance, flat surface corrosion resistance, and post-degreasing corrosion resistance were unacceptable. In Comparative Example No. 101, the Cr deposition amount in the chromium-containing composite layer was outside the range of the present invention due to the chromium concentration in the electrolytic bath used, and therefore the processed portion adhesion was unacceptable. Furthermore, in Comparative Example No. 102, the bath temperature of the electrolytic bath used was 40°C, and therefore the Cr deposition amount in the chromium-containing composite layer was outside the range of the present invention, and therefore the processed portion corrosion resistance, flat surface corrosion resistance, and post-degreasing corrosion resistance were unacceptable.
[0148] Although the preferred embodiments of the present invention have been described in detail above with reference to the accompanying drawings, the present invention is not limited to these examples. It is clear that a person skilled in the art to which the present invention pertains can conceive of various modifications and alterations within the scope of the technical ideas set forth in the claims, and it is understood that these also naturally fall within the technical scope of the present invention.
[0149] The embodiments disclosed herein are illustrative in all respects and are not limiting. The above-described embodiments may be omitted, substituted, or modified in various ways without departing from the scope of the appended claims, the technical scope of the present invention as described below, and the spirit thereof. For example, the components of the above-described embodiments may be arbitrarily combined within the scope that does not impair the effects of the components. Furthermore, such an arbitrary combination naturally provides the functions and effects of each of the components involved in the combination, and also provides other functions and effects that are apparent to those skilled in the art from the description of this specification.
[0150] Furthermore, the effects described in this specification are merely descriptive or exemplary and are not limiting. In other words, the technology according to the present invention may achieve other effects that will be apparent to those skilled in the art from the description of this specification, in addition to or in place of the above-described effects.
[0151] The following configuration also falls within the technical scope of the present invention: (1) A steel sheet having a plating layer containing zinc and nickel located on at least one surface thereof, a first composite layer containing Fe, Zn, and Ni located between the steel sheet and the plating layer, a chromium-containing composite layer containing at least Cr located on the plating layer, and a coating film containing epoxy resin, isocyanate resin, and silica particles located on the chromium-containing composite layer, wherein the coating weight of the plating layer is 2 to 50 g / m per side. 2the chromium-containing composite layer comprises: a second composite layer containing Cr, Zn, and Ni located on the plating layer side; and a third composite layer containing Si, N, and Cr located on the coating film side; and the coating weight of the chromium-containing composite layer is 10 to 200 mg / m in terms of metallic Cr. 2 (2) The surface-treated steel sheet according to (1), wherein a ratio (d2 / d1) of an average thickness d2 of the second composite layer to an average thickness d1 of the first composite layer is 0.2 to 150.0, and a ratio (d3 / d1) of an average thickness d3 of the third composite layer to an average thickness d1 of the first composite layer is 0.2 to 150.0. (3) The surface-treated steel sheet according to (1) or (2), wherein the coating film contains polyethylene wax in a proportion of 0.1 to 10.0 mass% based on the coating film solid content, the epoxy resin content is 30.0 mass% or more based on the coating film solid content, the isocyanate resin content is 0.10 to 2.00 in terms of mass ratio based on the epoxy resin, and the silica particle content is 5.0 to 50.0 mass% based on the coating film solid content, and the coating film contains the epoxy resin, the isocyanate resin, the silica particles, and the polyethylene wax in a total amount of 100 mass% or less. (4) The surface-treated steel sheet according to any one of (1) to (3), wherein the epoxy resin is a bisphenol A-type epoxy resin having a number average molecular weight of 300 to 100,000. (5) The surface-treated steel sheet according to any one of (1) to (4), wherein the silica particles are at least either fumed silica or colloidal silica, the fumed silica has an average particle size of 5 to 40 nm, and the colloidal silica has an average particle size of 5 to 200 nm. (6) The surface-treated steel sheet according to any one of (1) to (5), which is used as a material for a fuel tank.
[0152] REFERENCE SIGNS LIST 1 Surface-treated steel sheet 10 Steel sheet 20 Plated layer 30 Chromium-containing composite layer 40 Coating film 50 First composite layer 60 Second composite layer 70 Third composite layer
Claims
1. A steel sheet having a plating layer containing zinc and nickel located on at least one surface thereof, a first composite layer containing Fe, Zn, and Ni located between the steel sheet and the plating layer, a chromium-containing composite layer containing at least Cr located on the plating layer, and a coating film containing epoxy resin, isocyanate resin, and silica particles located on the chromium-containing composite layer, wherein the coating weight of the plating layer is 2 to 50 g / m per side. 2 the chromium-containing composite layer includes: a second composite layer containing Cr, Zn, and Ni located on the plating layer side; and a third composite layer containing Si, N, and Cr located on the coating film side; and the coating amount of the chromium-containing composite layer is 10 to 200 mg / m in terms of metallic Cr. 2 and the coating film has a thickness of 0.5 to 2.0 μm.
2. The surface-treated steel sheet according to claim 1, wherein the ratio (d2 / d1) of the average thickness d2 of the second composite layer to the average thickness d1 of the first composite layer is 0.2 to 150.0, and the ratio (d3 / d1) of the average thickness d3 of the third composite layer to the average thickness d1 of the first composite layer is 0.2 to 150.
0.
3. A surface-treated steel sheet according to claim 1 or 2, wherein the coating contains polyethylene wax in a proportion of 0.1 to 10.0% by mass relative to the coating solid content, the epoxy resin content is 30.0% by mass or more relative to the coating solid content, the isocyanate resin content is 0.10 to 2.00 in terms of mass ratio relative to the epoxy resin, and the silica particle content is 5.0 to 50.0% by mass relative to the coating solid content, and the coating contains the epoxy resin, the isocyanate resin, the silica particles and the polyethylene wax in a total amount of 100% by mass or less.
4. The surface-treated steel sheet according to claim 1 or 2, wherein the epoxy resin is a bisphenol A type epoxy resin having a number average molecular weight of 300 to 100,000.
5. The surface-treated steel sheet according to claim 1 or 2, wherein the silica particles are at least one of fumed silica and colloidal silica, the average particle size of the fumed silica is 5 to 40 nm, and the average particle size of the colloidal silica is 5 to 200 nm.
6. The surface-treated steel sheet according to claim 1 or 2, which is used as a material for a fuel tank.
Citation Information
Patent Citations
Manufacture of organic composite plated steel sheet
JP1992180574A