Coating solution for preparation of reforming catalyst to which insulation support is applied, and reforming catalyst preparation method

The reforming catalyst using an insulating material support coated with silica and alumina sols addresses the high-cost and inefficiency issues of conventional catalysts by reducing catalyst amounts and enhancing thermal stability, achieving cost-effective and durable performance at high temperatures.

WO2024205353A1PCT designated stage expired Publication Date: 2024-10-03JOONG IL MATERIALS INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/095224
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2024-02-15
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional reforming catalysts require expensive equipment and have high production costs due to the need for large amounts of catalyst, and they exhibit low start-up time and thermal efficiency due to the use of alumina-based supports, which are not suitable for high-temperature reactions.

Method used

A reforming catalyst is developed using an insulating material support coated with a pre-coating solution containing silica sol, alumina sol, and catalyst powder, followed by a firing step to enhance mechanical strength and durability, allowing for the use of less catalyst while maintaining stability at high temperatures.

Benefits of technology

The catalyst is manufactured economically in various shapes, reduces catalyst usage, and maintains stability and durability during high-temperature reactions, offering improved thermal efficiency and cost-effectiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024095224_03102024_PF_FP_ABST
    Figure KR2024095224_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The objective of the present invention is to provide a reforming catalyst that can be simply and economically prepared in various forms, enables catalyst usage amount to be reduced, is stable even in high-temperature reactions and has excellent durability, and thus the present invention provides: a pre-coating solution comprising a catalyst and a reinforcing solution, which comprises a silica sol, an alumina sol and a solvent; a catalyst coating solution comprising a catalyst aqueous solution and an inorganic binder, which comprises a silica sol and an alumina sol; and a reforming catalyst preparation method comprising: a pre-coating step of manufacturing a pre-coating insulation support by using the pre-coating solution; a firing step of heating and firing the pre-coating insulation support; and a catalyst coating step of coating the pre-coating insulation support with a catalyst coating solution, thereby preparing a reforming catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Coating solution for manufacturing a reforming catalyst with an insulating support and a manufacturing method for the reforming catalyst

[0001] The present invention relates to a reforming catalyst to which an insulating support is applied, and more particularly, to a coating solution composition for producing a reforming catalyst to which an insulating support is applied and a method for producing a reforming catalyst to which an insulating support is applied.

[0002]

[0003] Recently, countries and companies are making significant efforts to address environmental pollution and global warming. Fossil fuels, while currently the most widely used energy source, are significantly contributing to environmental pollution and global warming. Therefore, significant efforts are being made to secure alternative energy sources. One method for producing hydrogen, a promising alternative energy source, involves using a reformer to convert fossil fuels such as methane, methanol, gasoline, and natural gas into hydrogen. This process includes steam reforming, partial oxidation, and autothermal reforming.

[0004] These reforming reactions typically utilize nickel (Ni), a low-cost transition metal, as the catalyst. However, when nickel is used as the catalytically active material, CO adsorbs on the nickel surface, resulting in carbon deposition. To address this issue, noble metals can be supported or impregnated onto alumina (Al2O3, alumina), which has a large surface area, to enhance efficiency and stability. However, noble metals are typically more expensive than nickel.

[0005] Typically, catalysts are manufactured as powders, and depending on the reaction conditions and state, the catalysts are molded and processed into spherical, cylindrical, or pellet shapes, and then compressed into spherical or pellet shapes of a certain size for use. However, reforming catalysts processed in this way require expensive equipment for the molding process, and the large amount of catalyst input increases the production cost. To compensate for these drawbacks, alumina-based catalyst supports are used, coating the catalyst on the surface and using it in pellet form. However, reforming reactions are extremely endothermic or exothermic reactions that occur at high temperatures, and alumina-based support catalysts have the disadvantage of slow heat transfer, resulting in low start-up time and thermal efficiency.

[0006] Accordingly, there is a need for the development of a reforming catalyst that can be easily and economically manufactured in various shapes suitable for the reaction, is economical because it reduces the amount of catalyst used, is stable even in high-temperature reactions, and has excellent durability.

[0007]

[0008] The present invention aims to provide a reforming catalyst that can be easily and economically manufactured in various shapes, can reduce the amount of catalyst used, is stable even in high-temperature reactions, and has excellent durability in order to solve the above problems.

[0009]

[0010] The present invention provides a pre-coating solution comprising a reinforcing solution including silica sol, alumina sol, and a solvent, and a catalyst powder, which is coated on an insulating support including silica and alumina to provide a reforming catalyst applied to an insulating support.

[0011] In addition, the present invention provides a catalyst coating solution comprising an inorganic binder including silica sol and alumina sol, and a catalyst powder, which is coated on a pre-coated insulation support to provide a reforming catalyst to which an insulation support is applied, and wherein the pre-coated insulation support is formed by coating a pre-coating solution including silica sol and alumina sol on an insulation support including silica and alumina.

[0012] In addition, the present invention provides a method for producing a reforming catalyst, comprising: a pre-coating step of forming a pre-coated insulating material support by coating a pre-coating solution containing silica sol and alumina sol on an insulating material support containing silica and alumina to produce a pre-coated insulating material support; a firing step of heating and firing the pre-coated insulating material support; and a catalyst coating step of coating a catalyst coating solution containing an inorganic binder containing silica sol and alumina sol and a catalyst powder on the pre-coated insulating material support to produce a reforming catalyst.

[0013]

[0014] According to one embodiment of the present invention, a reforming catalyst having an insulating support applied thereto can be manufactured in a simple and economical manner in various shapes.

[0015] Additionally, according to one embodiment of the present invention, when an insulating support is applied, the amount of catalyst used in the production of a reforming catalyst can be reduced.

[0016] In addition, according to one embodiment of the present invention, by using a reforming catalyst to which an insulating support is applied, a catalytic reaction can proceed stably even at high temperature.

[0017] In addition, according to one embodiment of the present invention, a reforming catalyst having an insulating support with excellent durability can be provided.

[0018]

[0019] Figure 1 is a schematic diagram of a method for manufacturing a reforming catalyst using an insulating support according to one embodiment of the present invention.

[0020] Figure 2 is a graph showing the CH4 reforming reaction measured for 350 hours using a reforming catalyst manufactured according to Example 1.

[0021]

[0022]

[0023] Hereinafter, embodiments of the present invention are described in detail. However, the present invention is not limited to the embodiments disclosed below and may be implemented in various different forms. These embodiments are provided solely to ensure complete disclosure of the present invention and to more fully inform those skilled in the art of the present invention.

[0024]

[0025] The present invention relates to a method for producing a reforming catalyst applied with an insulating material support, comprising: providing a pre-coating solution for improving the strength of the insulating material support; and a catalyst coating solution for coating the insulating material support with a catalyst; and providing a method for producing a reforming catalyst applied with the insulating material support using the pre-coating solution and the catalyst coating solution. Accordingly, the strength is secured so that an insulating material having low density and low mechanical strength can be used as a support for a reforming catalyst, thereby providing a reforming catalyst with excellent durability. In addition, by applying the insulating material support, it is possible to provide an economical reforming catalyst that is stable even in high-temperature reactions and can reduce the amount of catalyst used.

[0026] At this time, it is preferable that the insulating material support be an insulating material that has a large surface area, low thermal conductivity, is physically / chemically stable, is made of a safe material, is easy to process, and has a low unit price. In particular, an insulating material that uses silica with excellent thermal stability and alumina with excellent strength is preferable. For example, the insulating material may be an insulating material formed of Al2O3: 46-85%, SiO2: 10-52%, and a density of 350 ± 35 kg / ㎥, but is not limited thereto.

[0027]

[0028] Hereinafter, the pre-coating solution and catalyst coating solution of the present invention will be described in detail.

[0029]

[0030] The pre-coating solution according to the present invention comprises a reinforcing solution including silica sol, alumina sol, and a solvent, and a catalyst powder.

[0031] The above pre-coating solution may be mixed with the reinforcing solution and the catalyst powder in a weight ratio of 98.0 to 100: 0 to 2.0. The main purpose of the above pre-coating solution is to manufacture a pre-coated insulating material support using the reinforcing solution. At this time, the pre-coating solution may improve the mechanical strength and durability of the outer surface of the manufactured pre-coated insulating material support by densifying some of the surface pores of the insulating material support. Accordingly, the strength and durability of the reforming catalyst to which the insulating material support is applied may be improved.

[0032] In addition, in the above pre-coating solution, increasing the proportion of reinforcing solution is advantageous in securing the strength and durability of the reforming catalyst, and by adding a small amount of the catalyst powder, the catalyst powder can be pre-distributed on the surface of the pre-coating insulation support, thereby enabling the performance of the reforming catalyst to be effectively and stably exhibited.

[0033] The above reinforcing solution may contain 45.0 to 55.0 wt% of the silica sol, 32.5 to 42.5 wt% of the alumina sol, and the remainder of the solvent. Accordingly, since the reinforcing solution and the insulating support, which are mainly composed of Al2O3 and SiO2, have the same components, the pre-coating solution can be well coated on the surface of the insulating support.

[0034] For example, the silica sol may be a dispersion in which SiO2 particles are dispersed at a content of 27 to 33 wt%, and the size of the SiO2 particles may be 8 to 25 nm. In addition, the alumina sol may be a dispersion in which Al2O3 particles are dispersed at a content of 5 to 20 wt%, and the size of the Al2O3 particles may be 15 to 170 nm.

[0035] In the above reinforcing solution, if the ratio of the silica sol and the alumina sol is low, the surface coating ability of the insulating material support may be reduced. For example, if the reinforcing solution contains less than 45.0 wt% of the silica sol and 32.5 wt% of the alumina sol, when the silica sol and the alumina sol are coated on the surface of the insulating material support, the ability to densify a portion of the surface pores is reduced, and the mechanical strength and durability of the outer surface of the pre-coated insulating material support may be adversely affected.

[0036] In addition, in the reinforcing solution, if the silica sol ratio increases, the strength of the pre-coated insulation support may decrease. For example, if the silica sol exceeds 55.0 wt%, the surface of the insulation support may be excessively coated with silica particles, causing the outer surface of the pre-coated insulation support to be easily broken by external impact, which may adversely affect the mechanical strength and durability.

[0037] In addition, in the above reinforcing solution, if the alumina sol ratio increases, the thermal stability of the pre-coated insulation support may decrease. For example, if the alumina sol exceeds 42.5 wt%, the surface of the insulation support may be excessively coated with alumina particles, which may increase the thermal conductivity of the surface of the pre-coated insulation support, thereby adversely affecting the thermal stability of the catalyst formed on the surface of the pre-coated insulation support.

[0038] The solvent may be water. Examples include, but are not limited to, distilled water and DI water. This avoids environmental and safety issues that may arise when using organic solvents, and also prevents increased calcination and drying times required to completely remove the organic solvent.

[0039] In addition, the solvent may be an aqueous solution containing 0 to 2% of an organic substance in distilled water and DI water. For example, the organic substance may include, but is not limited to, methyl cellulose and PVA. Accordingly, the SiO2 particles and the Al2O3 particles of the silica sol and the alumina sol may be well attached to the surface of the insulating support by the organic substance. At this time, if the organic substance exceeds 2%, the viscosity is high, the dispersing power of the powder inside the reinforcing liquid is reduced, making it difficult to achieve a consistent coating, and the firing and drying time required to completely remove the organic substance may increase, which is not preferable.

[0040] The above catalyst powder may be a catalyst based on Ni, Zn, Al, Zr, or Ce, but is not limited thereto. Furthermore, the catalyst powder may be processed into a powder form of less than 10 μm and mixed. Accordingly, the catalyst powder may be uniformly dispersed in the solvent and uniformly coated on the surface of the insulating support.

[0041] The above pre-coating solution may further include an additive containing SiO2 having a particle size of 4 μm or less. For example, the additive may be further added in an amount of 0.1 to 3.0% by weight based on the weight of the reinforcing solution. Accordingly, on the surface of the insulating material support made of a porous material, even in areas with large pore sizes or on the surface of the insulating material support processed into various shapes, it is possible to effectively densify the surface, thereby improving the mechanical strength and durability of the pre-coated insulating material support.

[0042] At this time, if the amount of the additive input is excessively high, the strength of the pre-coated insulation support may be reduced. For example, if the amount of the additive input exceeds 3.0% of the weight of the reinforcing liquid, the surface of the insulation support may be excessively coated with silica particles, causing the outer surface of the pre-coated insulation support to exhibit properties that are easily broken by external impact, which may adversely affect the mechanical strength and durability.

[0043]

[0044] The catalyst coating solution according to the present invention comprises an inorganic binder including silica sol and alumina sol, a catalyst aqueous solution including a solvent and a catalyst powder.

[0045] The catalyst coating solution may contain 2.6 to 5.2 wt% of the inorganic binder and the remainder being an aqueous catalyst solution. The main purpose of the catalyst coating solution is to manufacture the reforming catalyst by coating the surface of the pre-coated insulation support with a catalyst. For example, if the content of the inorganic binder in the catalyst coating solution is less than 2.6 wt%, the ratio of the inorganic binder to the catalyst powder decreases, which may adversely affect the stable attachment of the catalyst powder to the surface of the pre-coated insulation support, and may adversely affect the mechanical strength and durability. In addition, if the content of the inorganic binder in the catalyst coating solution exceeds 5.2 wt%, the ratio of the inorganic binder on the surface of the pre-coated insulation support increases, and the ratio of the catalyst powder relatively decreases, which may cause a decrease in the fuel conversion rate, and a decrease in the efficiency relative to the amount of the catalyst powder introduced.

[0046] The above-mentioned inorganic binder can be mixed with the above-mentioned silica sol and the above-mentioned alumina sol in a weight ratio of 1 to 5: 0 to 4. Accordingly, since the above-mentioned insulating material support, in which Al2O3 and SiO2 are the main components, and the above-mentioned inorganic binder have the same components, the above-mentioned catalyst coating liquid can be well coated on the surface of the above-mentioned pre-coated insulating material support, and the above-mentioned catalyst powder particles can be well attached to the surface of the above-mentioned pre-coated insulating material support.

[0047] For example, the silica sol may be a dispersion in which SiO2 particles are dispersed at a content of 27 to 33%, and the size of the SiO2 particles may be 8 to 25 nm. In addition, the alumina sol may be a dispersion in which Al2O3 particles are dispersed at a content of 5 to 20%, and the size of the Al2O3 particles may be 15 to 170 nm. Accordingly, the catalyst powder may be stably attached to the surface of the pre-coated insulating material support by the inorganic binder.

[0048] The above catalyst solution may be a mixture of the solvent and the catalyst powder in a weight ratio of 89 to 91: 9 to 11. For example, if the catalyst powder is contained in the solvent in an amount less than 9 weight ratio, or if the catalyst powder is contained in the solvent in an amount greater than 11 weight ratio, the catalyst powder may not be evenly coated on the surface of the pre-coated insulation support.

[0049] The above catalyst powder may be a catalyst based on Ni, Zn, Al, Zr, or Ce, but is not limited thereto. Furthermore, the catalyst powder may be processed into a powder form of less than 10 μm and mixed. Accordingly, the catalyst powder may be uniformly dispersed in the solvent and uniformly coated on the surface of the pre-coated insulating material support.

[0050] The solvent may be water. For example, distilled water and DI-water may be used, but are not limited thereto.

[0051] In addition, the solvent may be an aqueous solution containing 0 to 2% of an organic substance in distilled water or DI water. For example, the organic substance may include, but is not limited to, methyl cellulose and PVA. Accordingly, the catalyst powder particles may be well attached to the surface of the pre-coated insulation support due to the organic substance. At this time, if the organic substance exceeds 2%, the viscosity increases, which reduces the dispersibility of the catalyst powder within the reinforcing liquid, making it difficult to achieve a consistent coating, and the firing and drying time required to completely remove the organic substance may increase, which is not preferable.

[0052]

[0053] Hereinafter, with reference to FIG. 1, a method for manufacturing a reforming catalyst using the pre-coating solution and the catalyst coating solution and an insulating material support is described in detail.

[0054] Figure 1 is a schematic diagram of a method for manufacturing a reforming catalyst using an insulating support according to one embodiment of the present invention.

[0055] The method for manufacturing a reforming catalyst using an insulating support according to the present invention includes an insulating support preparation step (S1), a pre-coating step (S2), a calcination step (S3), and a catalyst coating step (S4).

[0056]

[0057] The above insulating material support preparation step (S1) is a step of preparing an insulating material support of the reforming catalyst, and may include an insulating material support processing step and a dust removal step.

[0058] The above-mentioned insulating material support processing step is a step of processing the insulating material support into various shapes. At this time, the insulating material support can be processed into various shapes. For example, it can be processed into a cube, rectangular parallelepiped, sphere, pellet shape, cylinder, and cylindrical shape, but is not limited thereto. Various uneven processing is also possible on the surface of the insulating material support, but is not limited thereto.

[0059] In addition, the size of the insulating support may be 5 mm or more in the long side. At this time, in order to maximize the effect of the insulating support, it is advantageous if the difference between the long side and the short side is not large, such as a sphere or a cube. For example, if the insulating support is processed into a shape with a large difference between the long side and the short side, the insulating support may not form a sufficient volume, and thus the insulating effect may not be sufficiently exerted, resulting in reduced thermal stability and reduced catalytic reaction efficiency. In addition, if the size of the insulating support is processed to be less than 5 mm, it is difficult to obtain the same shape due to durability, resulting in a low processing yield, which is not preferable.

[0060] The above dust removal step is a step for removing foreign substances attached to the surface of the insulating material support. For example, dust generated during the processing of the insulating material support may remain attached to the surface of the insulating material support, and this can be removed using various methods such as a brush or blower. Accordingly, when coating the insulating material support, it is possible to prevent uneven coating areas or uncoated areas from forming on the coating surface due to foreign substances attached to the surface of the insulating material support.

[0061]

[0062] The above pre-coating step (S2) is a step of creating a pre-coated insulation support by coating the insulation support using the pre-coating solution, and may include a pre-coating impregnation step and a pre-coating drying step.

[0063] The above-described pre-coating impregnation step is a step of impregnating a plurality of the insulating material supports with the pre-coating solution. At this time, the pre-coating solution and the insulating material support are preferably prepared in a volume ratio of 1.8 to 2.2:1. For example, if the pre-coating solution ratio is less than 1.8, the surface coating ability of the insulating material support may be reduced. In addition, if the pre-coating solution ratio exceeds 2.2, the pre-coating solution may be wasted.

[0064] In the above pre-coating impregnation step, when impregnating a plurality of the insulating material supports with the pre-coating liquid, the insulating material supports may be impregnated while the pre-coating liquid is being stirred. For example, a plurality of the insulating material supports may be placed in a 1,000 to 2,000 mesh sieve and impregnated in a mixing tank in which the pre-coating liquid is being stirred. Accordingly, the insulating material supports can be stably impregnated without moving within the mixing tank as the pre-coating liquid is stirred, and damage to the insulating material supports due to stirring can be prevented.

[0065] The stirring conditions of the pre-coating solution in the above pre-coating impregnation step are preferably 100 to 300 RPM at room temperature. For example, if the stirring conditions are less than 100 RPM, the plurality of insulating material supports may not be evenly coated, and if the stirring conditions exceed 300 RPM, foaming may occur or the surface coating ability of the insulating material supports may be reduced due to excessive mixing.

[0066] The above pre-coating drying step is a step of taking out the insulating material support after the pre-coating impregnation step is completed and drying it. For example, hot air drying, infrared drying, and a combination thereof can be applied, but are not limited thereto. In addition, in order for the insulating material support to be evenly dried, it is preferable to evenly spread out the insulating material support so that it does not overlap with each other and dry it. Accordingly, in the pre-coating drying step, SiO2 and Al2O3 that were mixed with the solvent on the surface of the insulating material support are attached to the surface of the insulating material support to form a coating film, and the solvent and organic substances can be removed.

[0067] In addition, since the SiO2 and Al2O3 are integrated into the surface of the insulating material support, the strength of the surface of the insulating material support can be improved, and dust generated on the surface of the insulating material support can be prevented, thereby preventing the catalyst coated on the pre-coated insulating material support from being easily peeled off due to dust.

[0068] The above pre-coating drying step is preferably performed at a drying temperature of 180 to 220°C for 0.5 to 1.5 hours. For example, if the drying temperature is lower than 180°C, insufficient heat may be applied, making it difficult for the pre-coating solution to stably form a coating film on the surface of the insulating material support. In addition, if the drying temperature exceeds 220°C, heat more than sufficient for the pre-coating solution to form a coating film on the surface of the insulating material support may be applied, resulting in unnecessary energy consumption and a decrease in process efficiency.

[0069] In addition, if the drying time is less than 0.5 hours, a coating film by the pre-coating solution may not be stably formed on the surface of the insulating material support, and if it exceeds 1.5 hours, a decrease in process efficiency due to unnecessary energy use may occur after the coating film by the pre-coating solution is sufficiently formed on the surface of the insulating material support.

[0070] The above pre-coating step (S2) may repeat the pre-coating impregnation step and the pre-coating drying step one or more times. For example, the pre-coating impregnation step and the pre-coating drying step may be repeated one or more times until the coating amount calculated by calculating the density difference based on the weight difference between the pre-coating insulation support after the pre-coating drying step and the insulation support before the pre-coating step (S2) is entered becomes 150 to 300 kg / ㎥ (0.15 to 0.30 g / ㎤). At this time, since the pre-coating solution penetrates and coats the pores of the insulation support in the pre-coating step (S2), the change in volume can be ignored when calculating the density. Accordingly, a pre-coating insulation support can be effectively produced.

[0071]

[0072] The above-mentioned firing step (S3) is a step of heating and firing the pre-coated insulation support that completed the above-mentioned pre-coating step (S2). For example, the above-mentioned firing step (S3) may be applied to various heating furnaces that apply hot air heating, infrared heating, and combinations thereof, but is not limited thereto. At this time, the heating conditions are preferably such that the target temperature is increased to 700 to 1,000°C at a heating rate of 5 to 10°C and then maintained for 6 to 12 hours.

[0073] The above-mentioned firing step (S3) is a process of forming a coating film on the surface of the pre-coated insulation support from which both solvent and organic substances have been removed while increasing to a target temperature, and shrinking the pre-coated insulation support including pores in advance at a high temperature before coating a catalyst, so that the reaction area of ​​the pre-coated insulation support can be properly utilized. Accordingly, if the target temperature is less than 700°C, additional shrinkage may occur when the reforming catalyst to which the pre-coated insulation support is applied is used at a high temperature, which may lower the efficiency of the reforming catalyst, and if the target temperature exceeds 1000°C, it may be higher than a temperature sufficient to shrink the pre-coated insulation support, which may result in a decrease in process efficiency due to unnecessary energy use.

[0074] In addition, if the heating rate is less than 5°C, it may take too long to reach the target temperature, which may result in a decrease in process efficiency, and if the heating rate exceeds 10°C / min, deformation of the pre-coated insulation support may occur due to rapid temperature increase.

[0075] If the above firing step (S3) is performed for less than 6 hours after reaching the target temperature, firing may not be completed, and if it exceeds 12 hours, a decrease in process efficiency may occur due to unnecessary energy and time consumption after firing is completed.

[0076]

[0077] The above catalyst coating step (S4) is a step of producing the reforming catalyst by coating the pre-coated insulating material support that has completed the firing step (S3) using the catalyst coating solution, and may include a catalyst coating impregnation step and a catalyst coating drying step.

[0078] The above catalyst coating impregnation step is a step of impregnating a plurality of the pre-coated insulation supports that have completed the firing step (S3) with the catalyst coating solution. At this time, it is preferable that the catalyst coating solution and the pre-coated insulation support be prepared in a volume ratio of 1.8 to 2.2: 1. For example, when the catalyst coating solution ratio is less than 1.8, the coating ability on the surface of the pre-coated insulation support may be reduced. In addition, when the catalyst coating solution ratio exceeds 2.2, waste of the catalyst coating solution may occur.

[0079] In the catalyst coating impregnation step, when impregnating a plurality of the pre-coated insulation supports with the catalyst coating solution, the pre-coated insulation supports may be impregnated while the catalyst coating solution is being stirred. For example, a plurality of the pre-coated insulation supports may be placed in a 1,000 to 2,000 mesh strainer and impregnated in a mixing tank in which the catalyst coating solution is being stirred. Accordingly, the pre-coated insulation supports may be stably impregnated without moving within the mixing tank in response to the stirring of the catalyst coating solution, and damage to the pre-coated insulation supports may be prevented.

[0080] The stirring conditions of the catalyst coating solution in the catalyst coating impregnation step are preferably 100 to 300 RPM at room temperature. For example, if the stirring conditions are less than 100 RPM, the plurality of pre-coated insulation supports may not be evenly coated, and if the stirring conditions exceed 300 RPM, foaming may occur or the surface coating ability of the pre-coated insulation supports may be reduced due to excessive mixing.

[0081] The above catalyst coating drying step is a step in which the pre-coated insulation support is removed and dried after the catalyst coating impregnation step is completed. For example, hot air drying, infrared drying, and combinations thereof may be used, but are not limited thereto. Furthermore, to ensure even drying of the insulation support, it is preferable to evenly spread the insulation support out so that it does not overlap with one another during drying.

[0082] Accordingly, in the catalyst coating drying step, the SiO2, Al2O3 and the catalyst powder that were present on the surface of the pre-coated insulation support together with the solvent are attached to the surface of the pre-coated insulation support to form a coating film, and the solvent and organic substances can be removed. In addition, since the SiO2, the Al2O3 and the catalyst powder are integrally attached to the surface of the pre-coated insulation support, the catalyst powder can be stably attached to the surface of the pre-coated insulation support.

[0083] The above catalyst coating drying step is preferably performed at a drying temperature of 180 to 220°C and for a drying time of 0.5 to 1.5 hours. For example, when the drying temperature is less than 180°C, sufficient heat may not be applied, making it difficult for a coating film by the catalyst coating solution to be stably formed on the surface of the pre-coated insulation support. In addition, when the drying temperature exceeds 220°C, heat more than sufficient for the catalyst coating solution to form a coating film on the surface of the pre-coated insulation support may be applied, which may result in a decrease in process efficiency due to unnecessary energy consumption. In addition, when the drying time is less than 0.5 hours, a coating film by the catalyst coating solution may not be stably formed on the surface of the pre-coated insulation support, and when it exceeds 1.5 hours, after a coating film by the catalyst coating solution has been sufficiently formed on the surface of the pre-coated insulation support, a decrease in process efficiency due to unnecessary energy consumption may occur.

[0084] In the catalyst coating step (S4), the catalyst coating impregnation step and the catalyst coating drying step may be repeated one or more times. For example, the catalyst coating impregnation step and the catalyst coating drying step may be repeated one or more times until the coating amount calculated by calculating the density difference based on the weight difference between the pre-coated insulation support on which the catalyst coating drying step has been completed and the pre-coated insulation support before entering the catalyst coating step (S4) becomes 20 to 40 kg / ㎥ (0.02 to 0.04 g / ㎤). At this time, since the thickness coated on the pre-coated insulation support in the catalyst coating step (S4) is very low, the change in volume can be ignored when calculating the density difference. Accordingly, the reforming catalyst can be effectively produced.

[0085] By performing the catalyst coating step (S4) after the pre-coating step (S2), the strength of the insulating support can be secured, thereby providing a catalyst with excellent durability. For example, if only the catalyst coating step (S4) is performed without the pre-coating step (S2), sufficient strength of the insulating support cannot be secured. In addition, if only the pre-coating step (S2) is performed, the catalyst material required for the reforming catalyst cannot be provided, and thus the reforming catalyst cannot be used as a catalyst.

[0086] In addition, in the pre-coating step (S2) and the catalyst coating step (S4), by using the pre-coating solution and the catalyst coating solution having the same main components as the insulating material support, the insulating material support can be efficiently coated while maintaining the characteristics of the insulating material support, such as heat resistance and stable properties even in high-temperature reactions.

[0087]

[0088] The organic matter removal step is a step for removing residual organic matter that may be contained in the reforming catalyst that has completed the catalyst coating step (S4). In particular, when an aqueous solution containing organic matter is used in the pre-coating solution and the catalyst coating solution, it is preferable to apply the organic matter removal step.

[0089] The organic matter removal step may be performed using various heating methods such as hot air heating, infrared heating, and combinations thereof, but is not limited thereto. At this time, the heating conditions are preferably maintained at 550 to 750°C for 2 to 4 hours. For example, if the temperature is lower than 550°C, the organic matter contained in the reforming catalyst may not be sufficiently removed, and if the temperature exceeds 750°C, the temperature may be higher than sufficient to remove the organic matter contained in the reforming catalyst, resulting in unnecessary energy consumption and a decrease in process efficiency. In addition, if the organic matter removal step is performed for less than 2 hours, the organic matter contained in the reforming catalyst may not be sufficiently removed, and if it exceeds 4 hours, the time required to remove the organic matter contained in the reforming catalyst may be higher than sufficient, resulting in a decrease in process efficiency due to unnecessary energy consumption and excessive time consumption.

[0090]

[0091] Hereinafter, the present invention will be described in more detail through manufacturing examples, working examples, comparative examples, and experimental examples. However, the following working examples are intended only to aid understanding of the present invention and are not intended to limit the scope of the present invention in any way.

[0092]

[0093] Manufacturing example: Manufacturing of pre-coated insulation support

[0094]

[0095] Insulation support: Use insulation material processed into a cube shape with a side length of 6 mm, with a density of 350±10% kg / ㎥, Al2O3 46~85%, SiO2 25~54%.

[0096] Silica sol: Mix and use silica sol SS-30SG (Schemtech), SS-30A (Schemtech) and SS-30 (Schemtech) with SiO2 particle content of 29-31 wt% and SiO2 particle size of 10-20 nm.

[0097] Alumina sol: Use alumina sol (Alintec) with Al2O3 particle content of 5 to 20 wt% and Al2O3 particle size of 20 to 150 nm.

[0098] Water: distilled water

[0099] Catalyst powder: Al-Ru 3% (alumina - ruthenium 3%), processed into powder form of less than 10㎛

[0100]

[0101] Pre-coating impregnation stage conditions: Pre-coating solution: insulation support = 2:1 volume ratio, stirring speed 150 RPM, impregnation temperature 20℃, impregnation is performed until no bubbles are generated in the insulation.

[0102] Pre-coating drying stage conditions: hot air drying, temperature 180~220℃, drying time 1 hour

[0103]

[0104] Using the above insulation support, the silica sol, the alumina sol, the water, and the catalyst powder, and based on the pre-coating liquid content described in Table 1, a pre-coating step satisfying the pre-coating impregnation step conditions and the pre-coating drying step conditions was performed so that the coating amount on the insulation support reached 250 kg / ㎥, thereby manufacturing a pre-coated insulation support.

[0105]

[0106] Classification Free coating solution content Silica sol (g) Alumina sol (g) Water (g) Catalyst powder (g) Manufacturing example 1 100 75 252 Manufacturing example 2 90 85 252 Manufacturing example 3 110 65 252 Manufacturing example 4 100 75 250

[0107] Example: Preparation of reforming catalyst

[0108]

[0109] Silica sol: Mix and use silica sol SS-30SG (Schemtech), SS-30A (Schemtech) and SS-30 (Schemtech) with SiO2 particle content of 29-31 wt% and SiO2 particle size of 10-20 nm.

[0110] Alumina sol: Use alumina sol (Alintec) with Al2O3 particle content of 5 to 20 wt% and Al2O3 particle size of 20 to 150 nm.

[0111] Water: distilled water

[0112] Catalyst powder: Al-Ru 3% (alumina - ruthenium 3%), processed into powder form of less than 10㎛

[0113] Firing stage conditions: hot air drying, temperature 850℃, firing time 6hr

[0114] Catalyst coating mixing conditions: Catalyst coating solution: Insulation support = 2:1 volume ratio, stirring speed 150 RPM, impregnation temperature 20℃, impregnation proceeds until no bubbles are generated in the insulation.

[0115] Catalyst coating drying conditions: hot air drying, temperature 200℃, drying time 1 hour

[0116]

[0117] A firing step satisfying the firing step conditions was performed on the pre-coated insulation support manufactured in Manufacturing Examples 1 to 4. Next, a catalyst coating step satisfying the catalyst coating impregnation step conditions and the catalyst coating drying step conditions was performed on the pre-coated insulation support that completed the firing step using the silica sol, the alumina sol, the water, and the catalyst powder based on the catalyst coating liquid content described in Table 2, so that the coating amount on the pre-coated insulation support reached 30 kg / ㎥ (0.03 g / cm3), thereby manufacturing a reforming catalyst.

[0118]

[0119] Classification Free coating insulation support catalyst coating solution content Silica sol (g) Alumina sol (g) Water (g) Catalyst powder (g) Example 1 Manufacturing example 1 1 2 10 0 10 Example 2 Manufacturing example 3 2 4 10 0 10 Example 3 Manufacturing example 2 4 2 10 0 10 Example 4 Manufacturing example 4 1 2 10 0 10

[0120]

[0121] Comparative Examples 1-5: Manufacturing of reforming catalyst

[0122]

[0123] Using the same silica sol, alumina sol, water, and catalyst powder as in the above manufacturing example, and based on the pre-coating liquid content described in Table 3, a pre-coating step satisfying the same pre-coating impregnation step conditions and pre-coating drying step conditions as in the above manufacturing example was performed to manufacture a pre-coated insulation support.

[0124] Next, a firing step satisfying the same firing step conditions as in the above example was performed on the pre-coated insulation support, and a catalyst coating step satisfying the same catalyst coating impregnation step conditions and catalyst coating drying step conditions as in the above example was performed on the pre-coated insulation support that completed the firing step using the same silica sol, alumina sol, water, and catalyst powder as in the above example based on the catalyst coating liquid content described in Table 3, thereby manufacturing a reforming catalyst.

[0125]

[0126] ClassificationFree coating solution contentCatalyst coating solution contentSilica sol (g)Alumina sol (g)Water (g)Catalyst powder (g)Silica sol (g)Alumina sol (g)Water (g)Catalyst powder (g)Comparative example 1 150 25 25 21 2 10 0 10Comparative example 2 17 50 25 21 2 10 0 10Comparative example 3 12 5 50 25 21 2 10 0 10Comparative example 4 7 5 10 0 25 21 2 10 0 10Comparative example 5 87.5 87.5 25 21 2 10 0 10

[0127]

[0128] Experimental Example 1: CH4 reforming reaction using a reforming catalyst

[0129] Using the reforming catalysts manufactured through the above Examples 1 to 4 and Comparative Examples 1 to 5, CH4 reforming reaction was performed under the same SCR (Steam to Carbon Ratio) reaction conditions, GHSV (Gas Hourly Space Velocity) 2000, and reforming reaction temperature 750°C. In order to compare the catalytic effect and stability over time, CH4 gas (mol%) was measured and shown in Table 4.

[0130]

[0131] CH4gas (mol%)5 hours10 hours15 hours20 hoursExample 10.210.220.210.23Example 20.470.470.470.46Example 30.690.690.690.69Example 40.330.380.370.38Comparative Example 10.410.450.490.51Comparative Example 20.430.460.490.51Comparative Example 30.340.370.440.47Comparative Example 40.280.240.240.34Comparative Example 50.610.590.590.65

[0132] Referring to Table 4, it can be confirmed that when the reforming catalyst according to the present invention was applied (Examples 1 to 4), the change in CH4 gas (mol%) concentration over time was very small. Accordingly, the stability over time of the reforming catalyst applied with the insulating support can be confirmed.

[0133] In contrast, it can be confirmed that the change in the CH4gas (mol%) concentration over time in Comparative Examples 1 to 5, which deviate from the appropriate ratio of silica sol and alumina sol, increases over time, confirming that the thermal stability deteriorates.

[0134] In addition, when comparing Example 1, in which the pre-coating liquid contains catalyst powder, with Example 4, in which the pre-coating liquid does not contain catalyst powder, among the reforming catalysts according to the present invention, it can be confirmed that the CH4gas (mol%) value is stably maintained over time in both Examples 1 and 4, but the CH4gas (mol%) value of Example 1 is relatively low, so it can be confirmed that there is a difference in the reaction amount. Accordingly, it can be confirmed that when the catalyst powder is applied to the pre-coating liquid, the catalytic reaction of the reforming catalyst to which the insulation support is applied can occur more effectively.

[0135]

[0136] Comparative Example 7: Pellet-type catalyst

[0137] Application of pellet-type catalyst containing 30g of Al-Ru 3% (alumina-ruthenium 3%) catalyst processed into pellets of 2~3mm in size.

[0138]

[0139] Experimental Example 2: CH4 reforming reaction using a reforming catalyst

[0140] Using the reforming catalyst (9 g based on catalyst amount) manufactured through the above Example 1 and the pellet-type catalyst of the above Comparative Example 7, CH4 reforming reaction was performed under the same SCR (Steam to Carbon Ratio) reaction conditions, GHSV (Gas Hourly Space Velocity) 2000, and reforming reaction temperature 750°C. In order to compare the catalytic effect and stability over time, CH4 gas (mol%) was measured and shown in Table 5.

[0141]

[0142] CH4gas (mol%)5 hours10 hours15 hours20 hoursExample10.210.220.210.23Comparative example70.310.330.330.34

[0143] Referring to Table 5, it can be confirmed that when the reforming catalyst according to the present invention was applied (Example 1) and when the conventional catalyst type pellet-type catalyst (Comparative Example 7) was applied, the CH4gas (mol%) concentration over time was maintained constant, and the reaction amount was also similar.

[0144] However, in order to obtain a similar reaction amount, the conventional pellet-type catalyst (Comparative Example 7) required about 70% more catalyst than the reforming catalyst to which the insulating support according to the present invention was applied. This means that, in order to produce 1 kW of power based on a fuel cell, the reforming catalyst to which the insulating support according to the present invention was applied required about 90 g of catalyst, whereas the conventional pellet-type catalyst required about 300 g of catalyst. Accordingly, when the reforming catalyst to which the insulating support according to the present invention was applied, the amount of expensive catalyst used can be reduced, thereby securing price competitiveness.

[0145]

[0146] Experimental Example 3: Long-term implementation of CH4 reforming reaction using reforming catalyst

[0147] Using the reforming catalyst manufactured through the above Example 1, CH4 reforming reaction was performed under the same SCR (Steam to Carbon Ratio) reaction conditions, GHSV (Gas Hourly Space Velocity) 2000, and reforming reaction temperature 750°C. In order to compare the catalytic effect and stability over time, H2, CO, CO2, and CH4 gas mol% were measured for 350 hours, and the results are shown in Fig. 2.

[0148] Referring to FIG. 2, it can be confirmed that when the reforming catalyst according to the present invention is applied (Example 1), the reaction occurs stably even when the reaction is performed at a high temperature for a long time.

[0149]

[0150] Through the above Experimental Examples 1 to 3, it is possible to confirm the effective composition of the coating solution of the reforming catalyst to which the insulating material support according to the present invention is applied, and it is possible to confirm that it is performed more effectively and stably than the conventional pellet-type catalyst.

[0151]

[0152] As described above, the specific description of the present invention has been made by way of embodiments with reference to the attached drawings, but the above-described embodiments have only been described as preferred examples of the present invention, and therefore, the present invention should not be understood as being limited to the above-described embodiments, and the scope of the rights of the present invention should be understood by the claims described below and their equivalent concepts.

Claims

1. Coated on an insulating support containing silica and alumina, A reinforcing solution comprising silica sol, alumina sol and a solvent; and catalyst; A pre-coating solution containing .

2. In claim 1, The above reinforcing liquid and the above catalyst are mixed in a weight ratio of 98.0 to 100: 0 to 2.0, Pre-coating solution.

3. In claim 1, The above reinforcing agent is, 45.0 to 55.0 wt% of the above silica sol, 32.5 to 42.5 wt% of the above aluminasol, and Containing the solvent as a remainder, Pre-coating solution.

4. A pre-coated insulation support formed by coating a pre-coating solution containing silica sol and alumina sol on an insulation support containing silica and alumina.

5. Coated on a pre-coated insulation support, Inorganic binder comprising silica sol and alumina sol; and Catalytic solution; Including, The above pre-coated insulation support is formed by coating a pre-coating solution containing silica sol and alumina sol on an insulation support containing silica and alumina. Catalytic coating solution.

6. In claim 5, The above catalyst solution is a mixture of solvent and catalyst in a weight ratio of 89 to 91: 9 to 11. Catalytic coating solution.

7. In claim 5, The above catalyst coating liquid 2.6 to 5.2 wt% of the above-mentioned inorganic binder, and Including the above catalyst solution as a residual amount, The above-mentioned inorganic binder is a mixture of the above-mentioned silica sol and the above-mentioned alumina sol in a weight ratio of 1 to 5: 0 to 4. Catalytic coating solution.

8. It is formed by coating a catalyst coating solution containing an inorganic binder including silica sol and alumina sol and a catalyst aqueous solution on a pre-coated insulation support. A reforming catalyst, wherein the above pre-coated insulation support is formed by coating a pre-coating solution containing silica sol and alumina sol on an insulation support containing silica and alumina.

9. In the method for manufacturing a reforming catalyst, A pre-coating step for manufacturing a pre-coated insulation support by coating a pre-coating solution containing silica sol and alumina sol on an insulation support containing silica and alumina; A firing step of heating and firing the above-mentioned pre-coated insulation support; and A catalyst coating step for manufacturing a reforming catalyst by coating a catalyst coating solution containing an inorganic binder including silica sol and alumina sol and a catalyst aqueous solution on the above-mentioned pre-coated insulation support; A method for producing a reforming catalyst, comprising:

10. In claim 9, The above pre-coating step is, A pre-coating impregnation step of impregnating the above insulation support with the pre-coating solution; and Including a pre-coating drying step for drying the insulation support after the above pre-coating step is completed; The above pre-coating impregnation step and the above pre-coating drying step are included at least once, Method for manufacturing a reforming catalyst.

11. In claim 9, The above firing step is, The above pre-coated insulation support is heated, and the temperature is increased to 700 to 1,000°C at a rate of 5 to 10°C, and then maintained for 6 to 12 hours. Method for manufacturing a reforming catalyst.

12. In claim 9, The above catalyst coating step is, A catalyst coating impregnation step of impregnating the above pre-coated insulation support with the catalyst coating solution; and Including a catalyst coating drying step for drying the pre-coated insulation support after the above catalyst coating step is completed; The catalyst coating impregnation step and the catalyst coating drying step are included at least once. Method for manufacturing a reforming catalyst.

13. In claim 9, Further comprising an organic matter removal step of removing residual organic matter by heating the above-mentioned reforming catalyst at 550 to 750°C for 2 to 4 hours. Method for manufacturing a reforming catalyst.

Citation Information

Patent Citations

  • Photocatalytic hydrosols and aqueous photocatalytic coating agents

    JP5252876B2

  • Cobalt-based catalyst on basis of metal structure for fischer-tropsch reaction for manufacturing selective synthetic oil, manufacturing method thereof, and method for manufacturing selective synthetic oil using cobalt-based catalyst on basis of metal structure

    KR101373823B1

  • A novel catalyst carrier and a supported-type catalyst prepared by using the same

    KR1020080113676A

  • Composition for optoelectronic device and organic optoelectronic device and display device

    KR102555494B1

  • Coating solution and manufacturing method for producing catalyst for reforming with insulation support material

    KR102600234B1