Low temperature formation of transition metal disulfide thin films

WO2024211486A3PCT designated stage expired Publication Date: 2024-11-14RGT UNIV OF CALIFORNIA
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/US2024/022946
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-07
Filing Date
2024-04-04
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Current methods for forming transition metal disulfide thin films, such as MoS2, face challenges in achieving scalable, low-temperature deposition compatible with CMOS processes, with existing techniques requiring high temperatures, sulfur-rich environments, and resulting in defects and poor electronic properties due to misalignment of flakes and post-annealing steps.

Method used

A spin-coating-thermolysis hybrid method using a high-sulfur content molecular precursor with an 8:1 sulfur-to-transition metal atomic ratio, allowing for the formation of uniform, crystalline MoS2 films at temperatures up to 450°C, eliminating the need for post-sulfurization and high-temperature annealing, and enabling integration into CMOS back-end-of-line processing.

Benefits of technology

This approach enables the production of high-quality, large-area, crystalline transition metal disulfide films with improved electronic properties, reduced defects, and compatibility with CMOS processes, while maintaining energy efficiency and scalability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure US2024022946_14112024_PF_FP_ABST
    Figure US2024022946_14112024_PF_FP_ABST
Patent Text Reader

Abstract

A structure having a film of transition metal disulfide (TMS2) on a substrate. A method of forming a transition metal disulfide film includes forming a solution from at least a sulfur-rich precursor soluble in organic solvents and a transition metal, coating a layer of the solution onto a substrate for a first period of time while heating the substrate at a first temperature, while ramping the temperature to an annealing temperature for a second period of time, and continuing to heat the substrate at the annealing temperature for a third period of time. A method comprises forming a solution from at least a sulfur-rich precursor soluble in organic solvents and a transition metal, coating a layer of solution onto a substrate to form an amorphous film, and applying a laser to the amorphous film in a predetermined pattern to form transition metal disulfide in the predetermined pattern.
Need to check novelty before this filing date? Find Prior Art

Description

LOW TEMPERATURE FORMATION OF TRANSITION METAL DISULFIDE THIN FILMSRELATED APPLICATIONS

[0001] This disclosure is a non-provisional of and claims benefit from US Provisional Application No. 63 / 457,846, titled “LOW TEMPERATURE FORMATION OF TRANSITION METAL DISULFIDE THIN FILMS,” filed on April 7. 2023, the disclosure of which is incorporated herein by reference in its entirety.TECHNICAL FIELD

[0002] This disclosure relates to formation of amorphous-to-crystalline transition metal disulfide films, more particularly to the large-area formation of mono-to-many layer transition metal sulfides via spin coating-thermolysis hybrid methods with a single source precursor.BACKGROUND

[0003] One typical transition metal disulfide is molybdenum disulfide, or MoS2. This material is a two-dimensional semiconductor with a direct band gap of 1.84 eV in the monolayer limit and possesses improved carrier mobility over silicon at nanometer-scale thicknesses. These properties make thin-film MoS2especially interesting for potential applications in optoelectronic devices, logic transistors, and flexible electronics, in addition to catalysis and energy storage. However, integrating MoS2into complementary-metal-oxide- semiconductor (CMOS) processes, specifically back-end-of-line, or BEOL, processing requires the development of a scalable deposition technique occurring at temperatures no higher than approximately 450° C. Two common methods of producing thin MoS2films are chemical vapor deposition (CVD) and mechanical exfoliation. However, CVD generallyrequires a large thermal budget (elevated temperatures above 450° C over a period of several hours). Mechanical exfoliation is not a commercially scalable process. Instead, solution processing techniques, and in particular spin coating, are able to rapidly produce consistent wafer-scale thin films.

[0004] In general, spin coating is highly beneficial for quickly producing uniform films with thicknesses on the order of tens of nanometers. Compared to CVD, spin coating can be performed at lower temperatures and more quickly, providing increased energy efficiency. Compared to mechanical exfoliation, spin coating can produce films of consistent thicknesses, and is commercially scalable. However, the disadvantage of spin coating is that it cannot produce films of MoS2as thin as CVD or mechanical exfoliation, which are capable of producing monolayer films. More importantly, it can never achieve single or polycrystallinity and nm-thick layered structures throughout entire surfaces. Most studies on solution processed MoS2growth have focused on the use of dispersed flakes produced via exfoliation of a bulk crystal, of sizes ranging from several hundred nanometers to several microns. However, these flakes are not soluble in common solvents, and it is challenging to control flake size and thickness. The misalignment between flakes after adhering to the substrate produces defects in the film and leads to a large sheet resistance and poor electronic properties. In addition, these other processes require a high-temperature post-annealing step (up to 800° C) to heal these defects, sometimes in a sulfur-rich environment.BRIEF DESCRIPTION OF THE DRAWINGS

[0005] FIG. 1 shows the molecular structure of an example of a molybdenum and sulfur xanthate precursor.

[0006] FIG. 2 shows a graph of themiogravimetric analysis of a molybdenum and sulfur xanthate precursor.

[0007] FIG. 3 shows a graphical representation of an embodiment of spin coating procedure using different temperatures.

[0008] FIG. 4 shows images of a precursor solution and a spin coater with an integrated heater.

[0009] FIG. 5 shows images of 3 4-inch silicon wafers having MoS2films of varying thicknesses.

[0010] FIG. 6 shows Raman spectra of annealed sample showing a conversion to MoS2.

[0011] FIG. 7 shows Raman and photoluminescence data for formation of a tungsten sulfide.

[0012] FIG. 8 shows results of X-ray photoelectron spectroscopy (XPS) of spin coated films.

[0013] FIG. 9 shows scanning transmission electron microscopy (STEM) and energydispersion X-ray spectroscopic (EDS) images of an embodiment of a molybdenum disulfide film.

[0014] FIG. 10 shows an atom force microscopy micrograph of a molybdenum disulfide film having an rms surface roughness of 0.6 nanometers.

[0015] FIG. 11 shows Raman spectra showing conversion to molybdenum disulfide in embodiments of films with varying thicknesses.

[0016] FIG. 12 shows schematics of an embodiment of a system for laser-induced molybdenum disulfide film formation, Raman spectra of molybdenum disulfide as a function of laser power, and images of molybdenum disulfide films.

[0017] FIG. 13 shows schematics of embodiments for laser direct writing of amorphous molybdenum disulfur films encapsulated with aluminum oxide, and analysis results comparing encapsulated and un-encapsulated films.

[0018] FIG. 14 shows spectra resulting from an embodiment of forming molybdenum disulfide films with additives in the process.DETAILED DESCRIPTION OF THE EMBODIMENTS

[0019] The embodiments here use a high-sulfur content molecular precursor, meaning a precursor having an 8:1 sulfur-to- transition metal atomic ratio per molecule, that is soluble in organic solvents to form a homogenous solution with the precursor and a transition metal - sulfur containing molecule. The embodiments involve use of this solution to produce thin, uniform films. Further, since the precursor solution contains sulfur it eliminates the need for a post-sulfurization step. The embodiments involve lower temperatures than other transition metal disulfide film formation processes, allowing the ability to integrate transition metal disulfide films into typical CMOS back-end processes.

[0020] The below discussion focuses on molybdenum disulfide films, but any transition metal may be used to form a transition metal sulfide (TMS2) film. The focus on molybdenum is based on experimental examples and data, but one should note that this is only for ease of discussion and understanding.

[0021] Several CVD- and PVD-based deposition processes have been developed to grow MoS2films at low temperatures, and these are contained below in Table 1, reproduced from (Park, J.-H., et al. Synthesis of High-Performance Monolayer Molybdenum Disulfide at Low Temperature. Small Methods 5, 2000720 (2021). One should note that, while the existing studies claim low temperatures as growth temperatures, the processes in Table I and those like them require high temperatures and / or energies to dissociate precursors in the CVD or PVD systems. Some embodiments use a two-step spin-coating and thermolysis using sulfur- rich precursors with a low complete decomposition temperature. Growth temperatures in the embodiments may range up to 450-750° C, compatible with CMOS processes. While the below discussion focuses on spin coating, other forms of coating the substrate may be used . These include slot-die coating, spray coating, dip coating, blade coating, etc. The substrate, however coated, may then be subjected to the temperature annealing process as discussed above.

[0022] Although the spin coating process of the embodiments occurs at temperatures comparable to these other deposition techniques, it can be performed rapidly in comparison. Further, the embodiments do not require additional H2S gas-involved high-temperature annealing (or other sulfur rich gas phase, liquid, or solid phase chemistries) to form large-area crystalline MoS2. Additionally, the embodiments may form the large-area crystalline transition metal disulfide on any wafers size, limited only by the size of the spin coater.

[0023]

[0024] To produce the films, the embodiments utilize a single-source molybdenum and sulfur xanthate precursor chemical. The term “xanthate” typically refers to a salt with the formula ROCS-2M+, where R refers to an alkyl group and M+is either a Na+or K+ion. The chemical formula of the particular compound used is Mo(S2COEt)4, where Et represents the ethyl group, CH2CH3. FIG. 1 shows the molecular structure of Mo(S2COEt)4. Other transition metals can be formed with a similar chemical formula. For example, the formation of WS2from W(S2COEt)4. FIG. 1 shows molybdenum as 10, sulfur as 12, oxygen as 14, carbon as 16, and the hydrogens on the ends as 18.

[0025] Prior thermogravimetric analysis (TGA) has shown decomposition of this chemical to about 50% mass at a temperature of 200° C and complete decomposition by -300° C. FIG. 2 shows the inventors’ TGA analysis of the xanthate molecule. This corroborates that complete decomposition occurs by -300° C.

[0026] FIG. 3 shows a graphic representation of the times and temperatures of an embodiment of a procedure to form MoS2films. The process may start with dissolving the precursor molecule in a solvent. Further processing may be needed to ensure that the precursor molecule breaks up completely. This may include room-temperature or cryogenic temperature sonication and / or ultrasonication and filtration. Once prepared, in one embodiment the process involves placing the substrate of any size or geometry into a spin coater, which may have an integrated heater, and pipetting the solution onto the substrate. The spin coater may perform an initial rotation step w'ith a first, low temperature, anneal. The spin coater integrated heater, or other heat source, may hold at the first, lower temperature, or it may just ramp up to the necessary heat level for the high temperature anneal and the low temperature anneal may occur as a by-product of the ramping up. The discussion may refer to this embodiment as a ramping anneal process, and the annealing that occurs at the lower temperatures as a soft anneal at a soft annealing temperature. For embodiments that apply the coating in other ways, the process involves the heating, either to a first low'er temperature, then to a higher temperature. Alternatively, as mentioned above, the first lower temperature may just occur as part of the heating ramp up.

[0027] In the spin coating embodiments, the rotational speed then ramps up to a constant speed, while the heater ramps up to a temperature, referred to here as the annealing temperature, high enough to remove the solvent of the solution. Without spinning, the heater will ramp up to the temperature needed to remove the solvent. The process may then stop therotation while continuing the heating. As discussed above, both the temperatures will be in a range compatible with CMOS BEOL processing.

[0028] The 8-to-l atomic ratio of sulfur to molybdenum in the xanthate molecule eliminates the need for a post sulfurization step. The process generally involves preparing a solution of the precursor molecule in a solvent. In one embodiment a 0.25 M solution of Mo(S2COEt)4in dimethylformamide (DMF) is prepared, which is then ultrasonicated for 1 hour to break down large particles that may be in the solution. The solution then passes through a syringe filter with pore size of 0.10 μm to remove any additional particles that remain. Substrates may range from 1 .5 cm squares, such as sapphire, mica, and silicon with 300 nm SiO2, to 4” wafers, such as Si and 300 nm SiO2, extendable to larger wafer sizes.

[0029] For the spin coating process, after the substrate is placed inside the spin coater, enough precursor solution is pipetted to cover the entire substrate surface. The spin coating procedure consists of an initial rotation step to form the film along with a low temperature anneal via an integrated heater. In one embodiment, the spin coater accelerated the substrate to a target rotation speed of 1000-3000 rpm over a period of 5 seconds, after which it holds the rotation speed constant for 30 seconds. During this time, the integrated heater may ramp up to a predetermined temperature, in one embodiment 60° C, and then holds.

[0030] After 30 seconds of rotation at a constant speed, the spin coater shuts off while the temperature ramps up to an annealing temperature, in one embodiment the annealing temperature equals 200° C, but any temperature high enough to remove the solvent in which the xanthate resides will work. In one embodiment, the substrate and newly deposited film are annealed at a constant 200° C for 2 minutes, after which the heater turns off. The substrate and film then cool to room temperature. FIG. 4 shows a photograph of the solution in vials such as 20 and the spin coater 22 with integrated heater 26 and vacuum chuck 24.

[0031] For the embodiments that do not employ a spin coating, the filtered solution may be applied to the substrate by slot-die coating, spray coating, dip coating, blade coating, or any other method of applying a uniform coating to a substrate.

[0032] FIG. 5 shows a photograph of four-inch silicon wafers 30, 32, and 34, with deposited MoS2films of varying thicknesses, with the inset showing a low-magnification optical micrograph of the center of a wafer. As mentioned above, the low-temperature anneal may occur during the ramping up of the heater temperature to the higher temperature.

[0033] Immediately after the spin coating and initial annealing step, the film has composition MoSx, x > 2, due to the excess sulfur in the xanthate precursor solution. However, inert annealing at elevated temperatures of 250° C - 450° C removes excess sulfur and forms MoS2. The temperatures remain in a range safe for CMOS BEOL processing. FIG. 6 shows the appearance of clear MoS2peaks at wavenumbers of -385 cm-1and -405 cm-1in Raman spectroscopy of samples annealed in argon at temperatures of 350° C and 450° C. As mentioned previously, other transition metals including tungsten (W) can also be used. Raman and photoluminescence data on the formation of monolayer WS2 monolayer from W(S2COEt)4molecule is also shown in FIG. 7.

[0034] These results are further supported by x-ray photoelectron spectroscopy (XPS) results shown in FIG. 8, which illustrate both the emergence of clear peaks corresponding to MoS2as well as the attenuation of peaks corresponding to unwanted MoSx and MoOxcompounds after annealing at 350° C.

[0035] Further structural and compositional analysis was carried out on samples before and after the second annealing step, using transmission electron microscopy (TEM) and energy dispersive x-ray spectroscopy (EDS). Before annealing, the atomic ratio of sulfur to molybdenum is > 2.25, as shown in FIG. 9, which also contains EDS composition maps of a cross-section of the film, substrate, and protective platinum (Pt) layer. In FIG. 9, the upperleft photograph is a high-angle annular dark field (HAADF) scanning TEM (STEM) crosssection image of the film and substrate. The substrate 40 is typically S1O2. the film 42, and, in this embodiment, a protective layer 44. The upper right shows an EDS composition map of the cross-section. The lower left shows elemental composition maps, with the accompanying EDS compositional maps on the lower right. Of note is the limited amount of oxygen present in the spin-coated film., in agreement with XPS results mentioned above.

[0036] Atomic force microscopy (AFM) measurements were performed on the films to determine the surface roughness, as shown in FIG. 10. A typical central section of a film spin coated onto a 4” silicon wafer has an RMS roughness of 0.6 nm. “RMS” roughness is a root mean square measurement of surfaces across their microscopic peaks and valleys.

[0037] FIG. 11 shows Raman spectra demonstrate that the conversion to MoS2via thermal annealing can be observed in films with varying thickness. Varying thickness can result from different rotation speeds and different precursor solution concentrations, with the precursor concentration providing the most dominant parameter to control thickness, examples of which are shown to the left.

[0038] In addition to the spin coating and annealing, the MoS2could be formed via direct laser-direct writing 54 of spin-coated 52 amorphous MoSx (α-MoSx) 50 as shown in FIG. 12a. This may also comprise spin-coated amorphous transition metal (α-TMSx) at 50. Lasers provide one of the most feasible means to supply local energy for materials transformation in a temporally and spatially controlled manner. Without using wet photolithography processes, arbitrary shapes and patterns could be site-specifically produced on micro-second timescales. Other energy and heating sources, such as electron beams, ion beams and extreme ultraviolet light EUV can also be utilized for the transformation process.

[0039] In the embodiments here, the amorphous molybdenum sulfur film, (α -MoSx), undergoes writing with a laser to form the MoS2crystalline structure. The film prior toannealing is referred to as a molybdenum sulfur film, as the formation of specific compounds has not yet occurred. The process may use a low-temperature, soft anneal similar to the options in the ramping anneal embodiments discussed above. The soft annealing temperature removes the solvents and causes the amorphous film to form MoS.i. However, this represents an option, as the laser process can accomplish the same result.

[0040] In one embodiment, the amorphous film may have a protective coating of aluminum oxide (AI2O3). The laser then writes the desired pattern into the amorphous film, converting it to the molybdenum sulfide (MoS2) form in regions where the film is desired. The oxide protective layer, such as the aluminum oxide layer shown, allows the formation of semiconductor-insulator interfaces and avoids oxidation during the laser-induced thermolysis. The oxide can serve as a gate-dielectric layer. The layer may comprise other oxides transparent to the laser wavelength used in the annealing step.

[0041] In the embodiments here, MoS2formation requires a specific activate energy to break sulfur-rich molecules apart and make the resultant MoS2crystalline. FIG. 12b and its inset present Raman spectra, and FIGs. 12c and 12d show optical images of MoS2by a 488-nm laser as a function of incident powers (Pine), where a maximum Pineis 79,652 W / m2. The conversion into MoS2relies on laser powers. Crystalline MoS2is successfully obtained with a moderate Pinerange of up to 40%, whereas molybdenum oxide, including m-MoO2, is co- formed with MoS2at a Pinerange from 60 to 100 %. In addition, such a site-selective transformation scheme allowed the formation of MoS2patterns of arbitrary shapes. A 3 μm x 3 μm square of MoS2was written, as shown in FIG. 12c. Individual points where the 488-nm laser irradiated exhibit highly uniform Algmodes of MoS2, indicating that the laser could convert the film into MoS2in a well-controlled manner. This implies that the laser-assisted MoS2direct formation is highly compatible with existing CMOS manufactures.

[0042] As shown in FIG. 13 a. AI2O3, or other oxide protective layer 60is pre-deposited on the spin-coated α-MoSx62 before the encapsulated films are converted by a laser 64 or a hot plate 66 in the air to construct well-ordered, defect-free semiconductor-insulator interfaces 68 as well as avoid oxidation during thermolysis to MoS2. FIGs. 13a and 13b illustrate schematics of laser direct writing and annealing methods of AI2O3-encapsulated α -MoSx. FIG. 13c presents Raman spectra of MoS2with and without AI2O3capping layers after annealing by a hot plate at 300 °C in the air. MoS2with AI2O3, the solid red line in FIG. 13c, exhibits E2gand Algmodes of multilayer MoS2, although the conversion was carried out in the air. FIGs. 13d and 13e show optical images of MoS2with and without AI2O3capping layers. The AI2O3capping layer may also serve as a gate oxide for CMOS-compatible MoS2- based field-effect transistors.

[0043] The amorphous film portions that do not undergo the laser conversion to MoS2may remain to become part of the ultimate device that uses the MoS2film. The remaining amorphous film is conductive, so it could become an ohmic contact for the semiconductor comprised of the converted portions of the film. Otherwise, the process may include etching the unconverted portions or dissolving it in common solvents or by using standard lithographic techniques, etc.

[0044] In another embodiment, one variation of the ramping annealing process utilizes additives during the annealing process to accelerate thermolysis as well as enhance the MoS2crystallinity, producing mono to few-layer crystalline MoS2over a large area. FIGs. 14a and 14b present Raman and PL spectra of MoS2w'ith and without additives. In MoS2without additives, the frequency differences between Algand E2g(Δk) is more than 24 cm-1, and no PL signal is shown, indicating typical multilayers. However, MoS2annealed with additives has frequency differences (Δk) of less than 20 cm-1, consistent wdth mono- or bilayer MoS2. It also has a strong PL signal at 680 nm (« 1 ,88eV). In one embodiment, the additives mayinclude sodium chloride (NaCl) and / or tellurium (Te). These only provide examples of additives, the process may use one or more of many other additives.

[0045] Additionally, the FWHM of Raman modes generally reveals crystallinity: small FWHM could be associated with high crystallinity. In the use of additives, resultant MoS2exhibits superior crystallinity even in relatively low temperatures, as shown in FIG. 14c.

[0046] Potential uses of MoS2films and coatings include but not limited to direct integration into CMOS electronic devices (transistors, memory, etc.), and direct integration onto flexible substrates for flexible / wearable sensors and electronics. In many current processes, formation of some films may occur on a first substrate and then transferred to some substrates, such as sapphire. Using the techniques here, the films may be formed directly on substrates.

[0047] Other examples may include e-skin, ocular electronics, etc. Other uses include optoelectronic devices such as photovoltaics, light emitters, sensors and detectors, and gas / chemical sensors. Even further examples include textile electronics, and related applications in the microelectronics and coating industries. In addition, films or coatings of the amorphous trisulfide or disulfide of the transition metal or the crystalline transition metal disulfide can be used electrochemical processes, catalysts as well as a membrane for filtration, for example filtration of heavy metal ions from wastewater.

[0048] Additionally, this written description makes reference to particular features. It is to be understood that the disclosure in this specification includes all possible combinations of those particular features. For example, where a particular feature is disclosed in the context of a particular aspect, that feature can also be used, to the extent possible, in the context of other aspects.

[0049] Also, when reference is made in this application to a method having two or more defined steps or operations, the defined steps or operations can be carried out in any order or simultaneously, unless the context excludes those possibilities.

[0050] All features disclosed in the specification, including the claims, abstract, and drawings, and all the steps in any method or process disclosed, may be combined in any combination, except combinations where at least some of such features and / or steps are mutually exclusive. Each feature disclosed in the specification, including the claims, abstract, and drawings, can be replaced by alternative features seiwing the same, equivalent, or similar purpose, unless expressly stated otherwise.

[0051] Although specific embodiments have been illustrated and described for purposes of illustration, it will be understood that various modifications may be made without departing from the spirit and scope of the disclosure. Accordingly, the invention should not be limited except as by the appended claims.

Claims

WHAT IS CLAIMED IS:

1. A structure having a film comprised of a transition metal and sulfide on a substrate.

2. The structure as claimed in claim 1, further comprising a protective layer on a surface of the film.

3. The structure as claimed in claim 1, wherein the transition metal comprises one of molybdenum, or tungsten.

4. The structure as claimed in claim 1, wherein the protective layer comprises aluminum oxide AI2O3.

5. The structure as claimed in claim 1, wherein the film further comprises one or more of sodium chloride (NaCl) or tellurium (Te).

6. A method of forming a transition metal disulfide film, comprising: forming a solution from at least a sulfur-rich precursor soluble in organic solvents and a transition metal: coating a layer of the solution onto a substrate for a first period of time while heating the substrate at a first temperature; ramping the temperature to an annealing temperature for a second period of time; and continuing to heat the substrate at the annealing temperature for a third period of time.

7. The method as claimed in claim 6, wherein the solution comprises the sulfur-rich precursor in organic solvents, an organic solvent, the transition metal and one or more additives.

8. The method as claimed in claim 7, wherein the one or more additives comprise one or more of sodium chloride (NaCl) and tellurium (Te).

9. The method as claimed in claim 6, wherein the film further comprises aluminum oxide (AI2O3).

10. The method a claimed in claim 6. wherein coating the substrate comprises one of slotdie coating, spray coating, dip coating, blade coating, or spin-coating.11 . The method as claimed in claim 6, wherein the annealing temperature comprises a temperature high enough to remove the solvents.

12. The method as claimed in claim 6, wherein the annealing temperature comprises one of 200 °C, or a temperature having a range of 250 - 400 °C.

13. The method as claimed in claim 6, ramping the temperature to an annealing temperature occurs in argon.

14. A method of forming a transition metal disulfide film, comprising: forming a solution from at least a sulfur-rich precursor soluble in organic solvents and a transition metal; coating a layer of solution onto a substrate to form an amorphous film; and applying a laser to the amorphous film in a predetermined pattern to form transition metal disulfide in the predetermined pattern.

15. The method as claimed in claim 14, further comprising heating the substrate to a soft annealing temperature either during or after the coating.

16. The method as claimed in claim 14, further comprising coating a layer of aluminum oxide onto the amorphous film prior to applying the laser.

17. The method as claimed in claim 16, wherein applying a laser in the predetermined pattern converts the aluminum oxide to a semiconductor- insulator interface.

18. The method as claimed in claim 17, further comprising one of either leaving uncoverted portions of the aluminum oxide on the film, or removing the unconverted portions of the aluminum oxide from the film.

19. The method as claimed in claim 14, wherein the solution comprises the sulfur-rich precursor in organic solvents, an organic solvent, the transition metal and one or more additives.

20. The method as claimed in claim 14, wherein the one or more additives comprises one or more of sodium chloride (NaCl) and tellurium (Te).

Citation Information

Patent Citations

  • Sulfur-containing thin films

    US20150170907A1

  • Method of forming a transition metal containing film on a substrate by a cyclical deposition process, a method for supplying a transition metal halide compound to a reaction chamber, and related vapor deposition apparatus

    US20190249300A1

  • Method and system for depositing molybdenum layers

    US20220018016A1